Polishing composition, method for producing polishing composition, polishing method, and method for producing semiconductor substrate

By using a polishing composition with negative zeta potential abrasive grains and a bridged bicyclic compound with tertiary nitrogen atoms, the problem of slow polishing speed for polysilicon substrates doped with p-type impurities is solved, and efficient polishing effects are achieved.

CN113388328BActive Publication Date: 2024-10-25FUJIMI INCORPORATED
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110265786.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-03-13
Filing Date
2021-03-11
Publication Date
2024-10-25
Estimated Expiration
2041-03-11

AI Technical Summary

Technical Problem

The existing technology is difficult to efficiently grind polysilicon substrates containing p-type impurities, and fails to meet the grinding needs of new semiconductor substrates.

Method used

A polishing composition containing abrasive grains, a bridged bicyclic compound having a tertiary nitrogen atom and a pH adjuster is used. The zeta potential of the abrasive grains is negative and the pH is less than 5. Polycrystalline silicon is polished through these compositions and the bridge is used. The nucleophilicity of the bicyclic compound acts on the chemical bonds on the membrane surface to achieve efficient scraping.

Benefits of technology

It significantly increases the polishing speed of polysilicon doped with p-type impurities, achieves efficient planarization, and improves the polishing effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002971740830000091
    Figure BDA0002971740830000091
  • Figure BDA0002971740830000101
    Figure BDA0002971740830000101
  • Figure BDA0002971740830000141
    Figure BDA0002971740830000141
Patent Text Reader

Abstract

The present invention relates to a polishing composition, a method for producing a polishing composition, a polishing method, and a method for producing a semiconductor substrate. The polishing composition of the present invention is a polishing composition comprising abrasive grains, an additive, a pH adjuster, and a dispersion medium, wherein the abrasive grains have a negative zeta potential, the additive is a bridged bicyclic compound having a tertiary nitrogen atom, the content of the additive is greater than 0% by mass and less than 0.5% by mass relative to the total mass of the polishing composition, and the pH of the polishing composition is less than 5.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polishing composition, a method for producing the polishing composition, a polishing method, and a method for producing a semiconductor substrate. Background Art

[0002] In recent years, as the surface of semiconductor substrates has become multi-layered, the so-called chemical mechanical polishing (CMP) technology is used to planarize semiconductor substrates by polishing them during device manufacturing. CMP is a method of planarizing the surface of a polishing object (object to be polished) such as a semiconductor substrate using a polishing composition (slurry) containing abrasive particles such as silicon dioxide, aluminum oxide, and cerium oxide, an anticorrosive agent, a surfactant, etc. The polishing object (object to be polished) is silicon, polysilicon, silicon oxide film (silicon oxide), silicon nitride, wiring formed of metal, plugs, etc.

[0003] For example, as a technique for polishing a polysilicon film disposed on a silicon substrate having a separation region, Japanese Patent Application Publication No. 2007-103515 (equivalent to U.S. Patent Application Publication No. 2007 / 077764, Korean Patent Application Publication No. 2007 / 0037409, Chinese Patent Application Publication No. 1939663, and Taiwan Patent Application Publication No. 200725721) discloses a polishing method comprising: a step of performing preliminary polishing using a preliminary polishing composition containing abrasive grains, an alkali, a water-soluble polymer, and water; and a step of performing fine polishing using a fine polishing composition containing abrasive grains, an alkali, a water-soluble polymer, and water. (Prior art document) Summary of the invention

[0004] Problem that the invention aims to solve

[0005] Recently, substrates made of polysilicon doped with impurities have begun to be used as semiconductor substrates, and a new demand for polishing such substrates has arisen. Such a demand has not been studied in the past.

[0006] Therefore, an object of the present invention is to provide a method capable of polishing an object to be polished including polycrystalline silicon doped with p-type impurities at a high polishing rate.

[0007] Solutions for solving problems

[0008] The present inventors have repeatedly conducted intensive studies to solve the above-mentioned new problems. As a result, they found that the above-mentioned problems can be solved by a polishing composition comprising abrasive grains, an additive, a pH adjuster and a dispersion medium, wherein the abrasive grains have a negative zeta potential, the additive is a bridged bicyclic compound having a tertiary nitrogen atom, the content of the additive is greater than 0% by mass and less than 0.5% by mass relative to the total mass of the polishing composition, and the pH of the polishing composition is less than 5, thereby completing the present invention. DETAILED DESCRIPTION

[0009] Hereinafter, embodiments of the present invention will be described. However, the present invention is not limited to the following embodiments.

[0010] In this specification, unless otherwise specified, operations and measurements of physical properties are performed under the conditions of room temperature (20° C. or higher and 25° C. or lower) and relative humidity of 40% RH or higher and 50% RH or lower.

[0011] The present invention is a polishing composition for polishing a polishing object including polycrystalline silicon doped with p-type impurities, the polishing composition including abrasive grains, a pH adjuster, an additive, and a dispersion medium, the abrasive grains having a negative zeta potential, the additive being a bridged bicyclic compound having a tertiary nitrogen atom, the content of the additive being greater than 0 mass % and less than 0.5 mass % relative to the total mass of the polishing composition, and the pH of the polishing composition being less than 5. The polishing composition of the present invention having such a structure can polish a polishing object including polycrystalline silicon doped with p-type impurities at a high polishing rate.

[0012] The mechanism for obtaining such an effect can be considered as follows. However, the following mechanism is only a guess, and the scope of the present invention is not limited to these. The polishing composition of the present invention contains a bridged bicyclic compound having a tertiary nitrogen atom as an additive. The non-shared electron pair present on the tertiary nitrogen atom has nucleophilicity. Therefore, a compound having nucleophilicity is used as an additive. In addition, it is believed that the tertiary nitrogen atom contained in the bridged bicyclic compound has a small steric hindrance near the non-shared electron pair, thereby improving the nucleophilicity. For example, it can be considered that: a B-Si bond is formed on the film surface of polycrystalline silicon doped with boron (B), and the polishing of the film surface of the polishing object is suppressed by the bond. Here, the non-shared electron pair possessed by the tertiary nitrogen atom is nucleophilic with the B atom on the film surface of the polishing object, thereby extending the distance of the B-Si bond formed on the film surface or cutting the B-Si bond. As a result, the film surface (i.e., the polishing surface) of the polishing object is embrittled, and scraping with abrasive grains becomes easy. That is, the bridged bicyclic compound having a tertiary nitrogen atom contained as a component of the polishing composition acts on the chemical bonds formed on the film surface of the polishing object, thereby making it easier for the abrasive contained in the polishing composition to mechanically scrape the polishing surface, thereby achieving efficient polishing.

[0013] [Object to be polished]

[0014] The polishing object of the present invention includes polysilicon doped with p-type impurities. That is, the polishing object of the present invention is used for polishing a polishing object including polysilicon doped with p-type impurities.

[0015] Examples of p-type impurities to be doped into polycrystalline silicon include Group 13 elements such as boron (B), aluminum (Al), gallium (Ga), and indium (In).

[0016] There is no particular restriction on the lower limit of the content (doping amount) of p-type impurities doped in polycrystalline silicon, and it is preferably 2.5 atomic % or more, and more preferably 5 atomic % or more, relative to the total of 100 atomic % of polycrystalline silicon and impurities. In addition, there is no particular restriction on the upper limit of the content (doping amount) of p-type impurities doped in polycrystalline silicon, and it is preferably 20 atomic % or less, and more preferably 15 atomic % or less, relative to the total of 100 atomic % of polycrystalline silicon and impurities. It should be noted that the content of p-type impurities doped in polycrystalline silicon is calculated using a multifunctional scanning X-ray photoelectron spectroscopy device (XPS) by the method described in the embodiments described later.

[0017] The polishing object of the present invention may include other materials besides polysilicon doped with p-type impurities, such as silicon nitride, silicon carbonitride (SiCN), silicon oxide, undoped polysilicon, undoped amorphous silicon, metal, SiGe, etc.

[0018] Examples of polishing objects containing silicon oxide include TEOS-type silicon oxide surfaces (hereinafter also referred to as "TEOS") generated using tetraethyl orthosilicate as a precursor, HDP films, USG films, PSG films, BPSG films, and RTO films.

[0019] Examples of the metal include tungsten, copper, aluminum, cobalt, hafnium, nickel, gold, silver, platinum, palladium, rhodium, ruthenium, iridium, and osmium.

[0020] [Polishing composition]

[0021] [Abrasive grains]

[0022] The polishing composition of the present invention contains abrasive particles. In the polishing composition of the present invention, the abrasive particles have a negative (minus) zeta potential. Here, "zeta (ζ) potential" refers to the potential difference generated at the interface between a solid and a liquid in contact with each other when the solid and the liquid move relative to each other.

[0023] In the polishing composition of the present invention, the zeta potential of the abrasive is preferably from -60 mV to -5 mV, more preferably from -50 mV to -10 mV, further preferably from -45 mV to -15 mV, and particularly preferably from -40 mV to -15 mV. The abrasive having a zeta potential in such a range can further increase the polishing speed.

[0024] Here, the zeta potential of the abrasive in the polishing composition is calculated by supplying a diluted solution of the polishing composition to a zetasizer-nano manufactured by the Malvern Panametrics Division of Spectris Corporation, measuring the zeta potential by a laser Doppler method (electrophoretic light scattering measurement method) using a capillary cell at a measurement temperature of 25°C and analyzing the obtained data using the Smoluchowski equation.

[0025] In the polishing composition of the present invention, the types of abrasive grains include metal oxides such as silicon dioxide, aluminum oxide, zirconium oxide, and titanium oxide. The abrasive grains may be used alone or in combination of two or more. The abrasive grains may be commercially available or synthetic.

[0026] As the type of abrasive grains, silicon dioxide is preferred, and colloidal silicon dioxide is more preferred. As the method for producing colloidal silicon dioxide, sodium silicate method and sol-gel method can be cited, and colloidal silicon dioxide produced by any production method can be suitably used as the abrasive grains of the present invention. However, from the viewpoint of reducing metal impurities, colloidal silicon dioxide produced by sol-gel method which can be produced with high purity is preferred.

[0027] The production of colloidal silica by the sol-gel method can be carried out using a conventionally known method. Specifically, colloidal silica can be obtained by using a hydrolyzable silicon compound (for example, alkoxysilane or a derivative thereof) as a raw material and subjecting it to a hydrolysis / condensation reaction.

[0028] The type of colloidal silica used is not particularly limited, and for example, surface-modified colloidal silica can be used. The surface modification of colloidal silica can be performed, for example, by chemically bonding the functional groups of an organic acid to the surface of the colloidal silica, i.e., by immobilizing the organic acid. Alternatively, the colloidal silica can be surface-modified by mixing a metal such as aluminum, titanium or zirconium, or an oxide thereof, with the colloidal silica and doping it on the surface of the silica particles.

[0029] In a preferred embodiment of the present invention, the colloidal silica contained in the polishing composition is colloidal silica with an organic acid immobilized on the surface. Compared with conventional colloidal silica without an organic acid immobilized on the surface, there is a tendency that the absolute value of the zeta potential in the polishing composition is large. Therefore, it is easy to adjust the zeta potential of the colloidal silica in the polishing composition to a negative value (e.g., a range of more than -45 mV and less than -15 mV).

[0030] As colloidal silica with an organic acid immobilized on the surface, preferably, colloidal silica with an organic acid such as a carboxylic acid group, a sulfonic acid group, a phosphonic acid group, or an aluminic acid group immobilized on the surface can be mentioned. Among these, colloidal silica with a sulfonic acid or a carboxylic acid immobilized on the surface is preferred from the viewpoint of being easy to manufacture, and colloidal silica with a sulfonic acid immobilized on the surface is more preferred.

[0031] The immobilization of organic acid on the surface of colloidal silica cannot be achieved simply by allowing colloidal silica and organic acid to coexist. For example, if sulfonic acid, which is a kind of organic acid, is immobilized on colloidal silica, it can be carried out by the method described in "Sulfonic acid-functionalized silica through of thiol groups", Chem. Commun. 246-247 (2003). Specifically, after coupling a silane coupling agent having a thiol group such as 3-mercaptopropyltrimethoxysilane with colloidal silica, the thiol group is oxidized with hydrogen peroxide, thereby obtaining colloidal silica with sulfonic acid immobilized on the surface (sulfonic acid modified colloidal silica).

[0032] Alternatively, if carboxylic acid, which is a type of organic acid, is immobilized on colloidal silica, it can be carried out, for example, by the method described in "Novel Silane Coupling Agents Containing a Photolabile 2-Nitrobenzyl Ester for Introduction of a Carboxy Group on the Surface of Silica Gel", Chemistry Letters, 3, 228-229 (2000). Specifically, a silane coupling agent containing a photoreactive 2-nitrobenzyl ester is coupled to colloidal silica and then irradiated with light, thereby obtaining colloidal silica with carboxylic acid immobilized on the surface (carboxylic acid-modified colloidal silica).

[0033] Here, the shape of the abrasive grains is not particularly limited, and may be spherical or non-spherical. Specific examples of the non-spherical shape include a triangular prism, a quadrangular prism, and other polygonal prisms; a cylindrical shape, a straw bag shape in which the center of the cylinder is more bulging than the ends, a donut shape in which the center of the disk is penetrated, a plate shape, a so-called cocoon shape with a contraction in the center, a so-called associated spherical shape in which a plurality of particles are integrated, a so-called konpeito shape with a plurality of protrusions on the surface, and a rugby ball shape, and the like, without particular limitation.

[0034] The size of the abrasive is not particularly limited. For example, the average primary particle size of the abrasive is preferably 5 nm or more, more preferably 8 nm or more, further preferably 10 nm or more, and particularly preferably 12 nm or more. As the average primary particle size of the abrasive increases, the polishing speed of the polished object based on the polishing composition increases. In addition, the average primary particle size of the abrasive is preferably 100 nm or less, more preferably 50 nm or less, further preferably 30 nm or less, particularly preferably 20 nm or less, and most preferably 15 nm or less. As the average primary particle size of the abrasive becomes smaller, a surface with few defects can be easily obtained by polishing with the polishing composition. That is, the average primary particle size of the abrasive is preferably 5 nm or more and 100 nm or less, more preferably 8 nm or more and 50 nm or less, further preferably 10 nm or more and 30 nm or less, particularly preferably 12 nm or more and 20 nm or less, and most preferably 12 nm or more and 15 nm or less. It should be noted that the average primary particle size of the abrasive can be calculated, for example, based on the specific surface area (SA) of the abrasive calculated according to the BET method, and assuming that the shape of the abrasive is a true sphere and calculated. In this specification, the average primary particle size of the abrasive grains is a value measured by the method described in Examples.

[0035] In addition, the average secondary particle size of the abrasive is preferably 10 nm or more, more preferably 15 nm or more, further preferably 20 nm or more, and particularly preferably 25 nm or more. As the average secondary particle size of the abrasive increases, the resistance in grinding decreases, and grinding can be performed stably. In addition, the average secondary particle size of the abrasive is preferably 400 nm or less, more preferably 300 nm or less, further preferably 200 nm or less, particularly preferably 100 nm or less, and most preferably 50 nm or less. As the average secondary particle size of the abrasive decreases, the surface area per unit mass of the abrasive increases, the contact frequency with the grinding object increases, and the grinding speed increases. That is, the average secondary particle size of the abrasive is preferably 10 nm or more and 400 nm or less, more preferably 15 nm or more and 300 nm or less, further preferably 20 nm or more and 200 nm or less, particularly preferably 25 nm or more and 100 nm or less, and particularly preferably 25 nm or more and 50 nm or less. It should be noted that the average secondary particle size of the abrasive can be measured, for example, by a dynamic light scattering method represented by a laser diffraction scattering method.

[0036] The average degree of association of the abrasive is preferably 5.0 or less, more preferably 4.0 or less, further preferably 3.0 or less, and particularly preferably 2.5 or less. As the average degree of association of the abrasive decreases, defects can be further reduced. In addition, the average degree of association of the abrasive is preferably 1.0 or more, more preferably 1.5 or more, and further preferably 2.0 or more. The average degree of association can be obtained by dividing the value of the average secondary particle size of the abrasive by the value of the average primary particle size. As the average degree of association of the abrasive increases, there is a favorable effect of increasing the polishing speed of the polishing object using the polishing composition.

[0037] The upper limit of the aspect ratio of the abrasive grains in the grinding composition is not particularly limited, preferably less than 2.0, more preferably below 1.8, and more preferably below 1.5. If it is such a scope, the defects on the surface of the grinding object can be further reduced. It should be noted that the aspect ratio is the smallest rectangle circumscribed with the image of the abrasive grains taken by a scanning electron microscope, and the average of the value obtained by dividing the length of the long side of the rectangle by the length of the short side of the same rectangle, and common image analysis software can be used to obtain. The lower limit of the aspect ratio of the abrasive grains in the grinding composition is not particularly limited, preferably more than 1.0, more preferably more than 1.2.

[0038] In the particle size distribution of the abrasive obtained by the laser diffraction scattering method, the lower limit of the ratio D90 / D10 of the diameter of the particle when the cumulative particle mass from the microparticle side reaches 90% of the total mass of the particles to the diameter of the particle when the total mass of the particles reaches 10% of the total mass of all particles is not particularly limited, preferably 1.1 or more, more preferably 1.4 or more, further preferably 1.7 or more, and most preferably 2.0 or more. In addition, in the particle size distribution of the abrasive in the polishing composition obtained by the laser diffraction scattering method, the upper limit of the ratio D90 / D10 of the diameter of the particle when the cumulative particle mass from the microparticle side reaches 90% of the total mass of the particles to the diameter of the particle when the total mass of the particles reaches 10% of the total mass of the particles is not particularly limited, preferably 3.0 or less, more preferably 2.5 or less. If it is within such a range, the defects on the surface of the polishing object can be further reduced.

[0039] The size of the abrasive grains (average primary grain size, average secondary grain size, aspect ratio, D90 / D10, etc.) can be appropriately controlled by, for example, selecting a method for producing the abrasive grains.

[0040] The content (concentration) of abrasive grains is not particularly limited, and is preferably 0.5% by mass or more, more preferably 0.8% by mass or more, more preferably 1% by mass or more, more preferably greater than 1% by mass, and particularly preferably greater than 1.5% by mass, relative to the gross mass of the grinding composition. In addition, the upper limit of the content of abrasive grains is preferably 20% by mass or less, more preferably 15% by mass or less, more preferably 10% by mass or less, and particularly preferably 5% by mass or less relative to the gross mass of the grinding composition. That is, the content of abrasive grains is preferably 0.5% by mass or more and 20% by mass or less, more preferably 0.8% by mass or more and 20% by mass or less, more preferably 1% by mass or more and 15% by mass or less, further preferably greater than 1% by mass or less and 10% by mass or less, particularly preferably 1.5% by mass or more and 5% by mass or less relative to the gross mass of the grinding composition. If it is such a range, the cost can be suppressed and the grinding speed can be improved. It should be noted that when the grinding composition includes more than two kinds of abrasive grains, the content of abrasive grains refers to their total amount.

[0041] [additive]

[0042] The polishing composition of the present invention contains, as an additive, a bridged bicyclic compound (also referred to as a "bicyclic compound") having a tertiary nitrogen atom. A tertiary nitrogen atom refers to a nitrogen atom (N atom) bonded to three carbon atoms. Therefore, the nitrogen atom present in the bridged bicyclic compound is preferably bonded to an aliphatic hydrocarbon group or an aromatic hydrocarbon group. In the bridged bicyclic compound, the group bonded to the tertiary nitrogen atom is more preferably an aliphatic hydrocarbon group, and further preferably an alkyl (alkylene) group. By making the nitrogen atom present in the bridged bicyclic compound a tertiary nitrogen atom, the nucleophilicity of the nitrogen atom becomes higher. Thus, when polishing is performed using the polishing composition, the additive can effectively act on the film surface of the polished object (specifically, the chemical bonds formed on the film surface).

[0043] Here, if the nitrogen atom present in the bridged bicyclic compound is a tertiary nitrogen atom, it may be one of the atoms forming the bridged ring, or may be included in the substituent possessed by the bridged ring. The nitrogen atom present in the bridged bicyclic compound is preferably one of the atoms forming the bridged ring. Therefore, the bridged bicyclic compound having a tertiary nitrogen atom is preferably an azabicyclic compound in which the nitrogen atom present in the ring is a tertiary nitrogen atom, that is, an azabicyclic compound having a tertiary nitrogen atom as a ring-forming atom is preferred.

[0044] The bridged bicyclic compound may have at least one tertiary nitrogen atom, or may have two or more tertiary nitrogen atoms. For example, the bridged bicyclic compound may have two tertiary nitrogen atoms, because the effect of the present invention can be further exerted, and is therefore preferred. In addition, the bridged bicyclic compound may have nitrogen atoms other than tertiary nitrogen atoms (e.g., secondary nitrogen atoms or primary nitrogen atoms).

[0045] As the bridged bicyclic compound having a tertiary nitrogen atom, the carbon number is preferably 5 to 15, the carbon number is more preferably 6 to 12, the carbon number is further preferably 6 to 10, and the carbon number is particularly preferably 6 to 8. That is, in a more preferred embodiment, the additive used in the present invention is a bridged bicyclic compound having a tertiary nitrogen atom and a carbon number of 6 to 12 (more preferably a carbon number of 6 to 10, and particularly preferably 6 to 8). In addition, in a more preferred embodiment, the additive used in the present invention is an azabicyclic compound having a tertiary nitrogen atom as a ring atom and a carbon number of 6 to 12 (more preferably a carbon number of 6 to 10, and particularly preferably 6 to 8).

[0046] The additive used in the present invention is represented by the following structural formula (1) in a preferred embodiment.

[0047]

[0048] In the above formula (1),

[0049] X is independently a nitrogen atom or CH,

[0050] Y is -NH-, -NR 1 -or-R 2- , at this time, R 1 is a substituted or unsubstituted alkyl group having 1 to 3 carbon atoms, R 2 is a substituted or unsubstituted alkylene group having 1 to 3 carbon atoms,

[0051] n and m are each independently an integer of 0 to 2,

[0052] Wherein, at least one of X is N, or Y is -NR 1 -.

[0053] Here, R 1 and R 2 When the group has a substituent, the substituent is halogen (fluorine, chlorine or bromine), -NR 3 R 4 (R 3 and R 4 are each independently hydrogen or an alkyl group having 1 to 3 carbon atoms), or an alkyl group having 1 to 3 carbon atoms.

[0054] In formula (1), the alkyl group having 1 to 3 carbon atoms may be linear or branched, and is, for example, methyl, ethyl, n-propyl, or isopropyl. 1 In formula (1), the alkylene group having 1 to 3 carbon atoms may be straight chain or branched, for example, methylene, ethylene, trimethylene (-CH2CH2CH2-), or propylene (-CH2CH(CH3)-). 2 In formula (1), n ​​and m are independently 0, 1 or 2.

[0055] In a preferred embodiment, in formula (1), X is independently a nitrogen atom or CH, Y is -NH-, -N(CH3)-, -CH2-, or -CH2CH2-, and n and m are independently integers of 0 to 2, wherein at least one of X is N, or Y is -N(CH3)-.

[0056] Examples of the compound represented by formula (1) include the following compounds.

[0057]

[0058] The compound represented by the above formula (1-1) is 1,4-diazabicyclo[2.2.2]octane (also known as triethylenediamine), and the compound represented by the above formula (1-2) is 1-azabicyclo[2.2.2]octane (also known as quinuclidine). In addition, the compound represented by the above formula (1-3) is 1-azabicyclo[3.2.2]nonane (also known as homoquinuclidine), and the compound represented by the above formula (1-4) is 9-methyl-9-azabicyclo[3.3.1]nonane (also known as granatane). Among these bridged bicyclic compounds, at least one selected from 1,4-diazabicyclo[2.2.2]octane and 1-azabicyclo[2.2.2]octane is preferred for the purpose of increasing the polishing rate.

[0059] The content (concentration) of additive is greater than 0 mass % and less than 0.5 mass % relative to the total mass of the grinding composition (the total mass of the grinding composition). If it is such a scope, the grinding speed can be improved. In addition, the content of additive is preferably more than 0.001 mass % relative to the total mass of the grinding composition, more preferably more than 0.01 mass %, more preferably more than 0.03 mass %, particularly preferably more than 0.06 mass %. In addition, the upper limit of the content of additive is preferably less than 0.45 mass % relative to the total mass of the grinding composition, more preferably less than 0.3 mass %, more preferably less than 0.25 mass %, particularly preferably less than 0.2 mass %. That is, the content of additive is preferably more than 0.001 mass % and less than 0.45 mass % relative to the grinding composition, more preferably more than 0.01 mass % and less than 0.3 mass %, more preferably more than 0.03 mass % and less than 0.25 mass %, particularly preferably more than 0.06 mass % and less than 0.2 mass %. If it is such a scope, cost can be suppressed, and the grinding speed can be improved. When the polishing composition contains two or more additives, the content of the additives refers to the total amount of the additives.

[0060] [pH and pH adjusters]

[0061] The pH of the polishing composition of the present invention is less than 5. If the pH is above 5, the polishing speed of the polishing object cannot be increased. The pH of the polishing composition of the present invention can be less than 5, preferably pH 4.9 or less, more preferably pH 4.5 or less, further preferably pH 4 or less, particularly preferably pH 3 or less, and most preferably pH 2.5 or less. When the pH is less than 5, there is a favorable effect of increasing the polishing speed of the polishing object, especially polycrystalline silicon containing p-type impurities. The lower limit of the pH is preferably 1.0 or more, more preferably 1.5 or more.

[0062] The polishing composition of the present invention contains a pH adjuster. The pH adjuster adjusts the pH of the polishing composition to a desired value.

[0063] The pH adjuster contained in the polishing composition of the present invention includes inorganic acids, organic acids, bases, etc. These may be used alone or in combination of two or more.

[0064] Specific examples of inorganic acids that can be used as pH adjusters include hydrochloric acid, sulfuric acid, nitric acid, hydrofluoric acid, boric acid, carbonic acid, hypophosphorous acid, phosphorous acid, and phosphoric acid. Among them, hydrochloric acid, sulfuric acid, nitric acid, or phosphoric acid is preferred.

[0065] Specific examples of organic acids that can be used as pH adjusters include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, 2-methylbutyric acid, n-hexanoic acid, 3,3-dimethylbutyric acid, 2-ethylbutyric acid, 4-methylvaleric acid, n-heptanoic acid, 2-methylhexanoic acid, n-octanoic acid, 2-ethylhexanoic acid, benzoic acid, glycolic acid, salicylic acid, glyceric acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid, tartaric acid, citric acid, lactic acid, diglycolic acid, 2-furancarboxylic acid, 2,5-furandicarboxylic acid, 3-furancarboxylic acid, 2-tetrahydrofurancarboxylic acid, methoxyacetic acid, methoxyphenylacetic acid, and phenoxyacetic acid. Organic sulfuric acids such as methanesulfonic acid, ethanesulfonic acid, and hydroxyethanesulfonic acid can also be used. Among them, dicarboxylic acids such as malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, maleic acid, phthalic acid, malic acid and tartaric acid, and tricarboxylic acids such as citric acid are preferred.

[0066] Salts such as alkali metal salts of inorganic or organic acids may be used as pH adjusters instead of or in combination with inorganic or organic acids. When a weak acid and a strong base, a strong acid and a weak base, or a weak acid and a weak base are combined, a pH buffering effect can be expected.

[0067] Specific examples of the base that can be used as the pH adjuster include ammonia, sodium hydroxide, potassium hydroxide, tetramethylammonium hydroxide, etc. The content of the pH adjuster can be appropriately selected within a range in which the effects of the present invention are exhibited.

[0068] It should be noted that the pH of the polishing composition can be measured, for example, by a pH meter. Specifically, a pH meter (e.g., manufactured by Horiba, Ltd., model: LAQUA) or the like is used, and after three-point calibration using a standard buffer solution (phthalate pH buffer solution pH: 4.01 (25°C), neutral phosphate pH buffer solution pH: 6.86 (25°C), carbonate pH buffer solution pH: 10.01 (25°C)), a glass electrode is inserted into the polishing composition, and the value after 2 minutes or more and stabilization is measured, thereby the pH of the polishing composition can be measured.

[0069] [Dispersion medium]

[0070] The polishing composition of the present invention includes a dispersion medium for dispersing each component. As a dispersion medium, water can be exemplified; alcohols such as methanol, ethanol, and ethylene glycol; ketones such as acetone, and mixtures thereof. Among these, water is preferred as a dispersion medium. That is, according to a preferred embodiment of the present invention, the dispersion medium includes water. According to a more preferred embodiment of the present invention, the dispersion medium is substantially formed by water. It should be noted that the above-mentioned "substantially" means that as long as the target effect of the present invention can be achieved, a dispersion medium other than water may also be included. More specifically, it is preferably formed by 90% by mass or more and 100% by mass or less of water and 0% by mass or more and 10% by mass or less of a dispersion medium other than water, and more preferably by 99% by mass or more and 100% by mass or less of water and 0% by mass or more and 1% by mass or less of a dispersion medium other than water. The most preferred dispersion medium is water.

[0071] From the viewpoint of not inhibiting the effects of the components contained in the polishing composition, the dispersion medium is preferably water containing as few impurities as possible. Specifically, pure water, ultrapure water, or distilled water from which impurity ions have been removed by an ion exchange resin and foreign matter has been removed by a filter is more preferred.

[0072] [Other ingredients]

[0073] The polishing composition of the present invention may contain known additives that can be used for polishing compositions, such as an oxidizing agent, a complexing agent, an anticorrosive agent, and an antifungal agent, as necessary, within a range that does not significantly impair the effects of the present invention.

[0074] [Method for producing polishing composition]

[0075] The method for producing the polishing composition of the present invention is not particularly limited, and can be obtained, for example, by stirring and mixing abrasive grains, additives, pH adjusting agents, and other components as required in a dispersion medium (e.g., water). The details of each component are as described above. Therefore, the present invention provides a method for producing the polishing composition of the present invention, comprising a step of mixing the abrasive grains, the additives, the pH adjusting agents, and the dispersion medium.

[0076] The temperature when mixing the components is not particularly limited, but is preferably 10° C. or higher and 40° C. or lower, and heating may be performed to increase the dissolution rate. The mixing time is not particularly limited as long as uniform mixing is possible.

[0077] [Polishing method and method for manufacturing semiconductor substrate]

[0078] As described above, the polishing composition of the present invention can be suitably used for polishing a polishing object comprising polycrystalline silicon doped with p-type impurities. Therefore, the present invention provides a polishing method, which uses the polishing composition of the present invention to polish a polishing object comprising polycrystalline silicon doped with p-type impurities. In addition, the present invention provides a method for manufacturing a semiconductor substrate, which includes a step of polishing a semiconductor substrate comprising polycrystalline silicon doped with p-type impurities using the aforementioned polishing method.

[0079] As the polishing device, a general polishing device can be used which is equipped with a holder for holding a substrate having an object to be polished, a motor with a variable rotation speed, etc., and has a polishing plate to which a polishing pad (polishing cloth) can be attached.

[0080] As the polishing pad, ordinary nonwoven fabric, polyurethane, porous fluororesin, etc. can be used without particular limitation. The polishing pad is preferably provided with grooves for accumulating the polishing liquid.

[0081] About grinding conditions, for example, the rotation speed of the grinding plate is preferably more than 10rpm and 500rpm. The pressure (grinding pressure) applied to the substrate with the grinding object is preferably more than 0.5psi and less than 10psi. The method for supplying the grinding composition to the grinding pad is also not particularly limited, for example, a method of continuously supplying with a pump etc. can be adopted. This supply amount is not limited, and the surface of the preferred grinding pad is always covered with the grinding composition of the present invention.

[0082] After polishing, the substrate is washed in running water, and water droplets adhering to the substrate are shaken off with a spin dryer or the like to be dried, thereby obtaining a substrate having a layer containing a metal.

[0083] The polishing composition used in the present invention may be a single component type or a multi-component type including a two-component type. In addition, the polishing composition used in the present invention may be prepared by diluting the stock solution of the polishing composition, for example, 10 times or more, with a diluent such as water.

[0084] Although the embodiments of the present invention have been described in detail, these are merely illustrative and exemplary descriptions and are not restrictive. The scope of the present invention should obviously be interpreted by the appended claims.

[0085] The present invention includes the following aspects and modes.

[0086] 1. A polishing composition comprising abrasive grains, an additive, a pH adjuster and a dispersion medium,

[0087] The zeta potential of the aforementioned abrasive particles is negative.

[0088] The aforementioned additive is a bridged bicyclic compound having a tertiary nitrogen atom,

[0089] The content of the additive is greater than 0% by mass and less than 0.5% by mass relative to the total mass of the polishing composition.

[0090] The polishing composition has a pH of less than 5.

[0091] 2. The polishing composition according to 1. above, wherein the additive is an azabicyclic compound having a tertiary nitrogen atom as a ring atom and having 6 to 12 carbon atoms.

[0092] 3. The polishing composition according to 1. or 2. above, wherein the additive is a compound represented by the following structural formula (1):

[0093]

[0094] In formula (1),

[0095] X is independently a nitrogen atom or CH,

[0096] Y is -NH-, -NR 1 -or-R 2 -, at this time, R 1 is a substituted or unsubstituted alkyl group having 1 to 3 carbon atoms, R 2 is a substituted or unsubstituted alkylene group having 1 to 3 carbon atoms,

[0097] n and m are each independently an integer of 0 to 2,

[0098] Wherein, at least one of X is N, or Y is -NR 1 -.

[0099] 4. The polishing composition according to any one of 1. to 3. above, wherein the content of the abrasive grains is greater than 1% by mass and less than 10% by mass relative to the total mass of the polishing composition.

[0100] 5. The polishing composition according to any one of 1. to 4. above, wherein the abrasive grains are colloidal silica having an organic acid immobilized on the surface.

[0101] 6. The polishing composition according to any one of 1. to 5. above, wherein the abrasive has a zeta potential of -45 mV to -15 mV.

[0102] 7. The polishing composition according to any one of 1. to 6. above, which is used for polishing an object to be polished comprising polycrystalline silicon doped with p-type impurities.

[0103] 8. A polishing method comprising the step of polishing an object to be polished using the polishing composition according to any one of 1. to 7. above.

[0104] 9. A method for manufacturing a semiconductor substrate, comprising the step of polishing a semiconductor substrate including polycrystalline silicon doped with p-type impurities by the polishing method described in 8. above.

[0105] Example

[0106] The present invention is further described in detail using the following examples and comparative examples. However, the technical scope of the present invention is not limited to the following examples. It should be noted that, unless otherwise specified, "%" and "part" represent "mass %" and "mass part" respectively.

[0107] <Preparation of Polishing Composition>

[0108] (Preparation of surface modified colloidal silica)

[0109] As colloidal silica, sulfonic acid-modified colloidal silica having an average primary particle size of 13.5 nm, an average secondary particle size of 31.0 nm, an average degree of association of 2.3, and D90 / D10: 2.3 (D90: 44 nm, D10: 19 nm) prepared by the method described in "Sulfonic acid-functionalized silica through quantitative oxidation of thiol groups", Chem. Commun. 246-247 (2003) was prepared. It should be noted that the average primary particle size and the average secondary particle size of the sulfonic acid-modified colloidal silica were measured according to the following method for measuring the particle size of abrasive particles.

[0110] (Example 1)

[0111] The sulfonic acid-modified colloidal silica (colloidal silica; average primary particle size: 13.5 nm, average secondary particle size: 31.0 nm, average degree of association: 2.3, D90 / D10: 2.3) obtained above as abrasive was added to pure water as a dispersion medium at room temperature (25°C) in a final concentration of 4% by mass and triethylenediamine as an additive was added to a final concentration of 0.1% by mass to obtain a mixed solution.

[0112] Thereafter, maleic acid as a pH adjuster was added to the mixed solution in such a manner that the pH became 2.3, and the mixture was stirred and mixed at room temperature (25°C) for 30 minutes to prepare a polishing composition. The pH of the polishing composition (liquid temperature: 25°C) was confirmed by a pH meter (Model: LAQUA, manufactured by Horiba, Ltd.). In addition, the zeta potential of the sulfonic acid-modified colloidal silica in the obtained polishing composition was measured by the following method for measuring the zeta potential of the abrasive, and the result was -27.8 mV. Triethylenediamine, an additive used in the polishing composition, has a tertiary nitrogen atom. It should be noted that the particle size of the abrasive (sulfonic acid-modified colloidal silica) in the polishing composition is the same as the particle size of the abrasive used.

[0113] Determination method

[0114] [Zeta potential of abrasive particles]

[0115] The polishing composition obtained was diluted so that the abrasive concentration became 0.01 mass %, and the diluted polishing composition was supplied to a zeta potential measuring device (manufactured by Malvern Panametrics Division of Spectris Corporation) zetasizer-nano, and measured by laser Doppler method (electrophoretic light scattering measurement method) using a capillary cell at a measurement temperature of 25° C. The obtained data was analyzed using the Smoluchowski formula, and the zeta potential of the abrasive was calculated.

[0116] [Grit size of abrasive grains]

[0117] The average primary particle size of the abrasive grains was calculated from the specific surface area of ​​the abrasive grains and the density of the abrasive grains measured by the BET method using "FlowSorbII 2300" manufactured by Micromeritics Instrument Corp. The average secondary particle size of the abrasive grains was measured using a dynamic light scattering particle size distribution apparatus UPA-UTI151 manufactured by Nikkiso Co., Ltd.

[0118] (Examples 2 to 11, Comparative Examples 1 to 14)

[0119] The polishing compositions of Examples 2 to 11 and Comparative Examples 1 to 14 were prepared in the same manner as in Example 1, except that the type and content of additives, the type and content of abrasive grains, and the pH (content of pH adjuster) were changed as shown in Tables 1 and 2 below. It should be noted that "-" in Tables 1 and 2 below means that the preparation is not contained. The pH of each polishing composition obtained, the average secondary particle size of the sulfonic acid-modified colloidal silica or the unmodified colloidal silica in each polishing composition, and the zeta potential are shown in Tables 1 and 2 below.

[0120] <Evaluation>

[0121] Using each polishing composition obtained above, the polishing rate when any of the following polishing objects was polished under the following polishing conditions was measured.

[0122] (Grinding equipment and grinding conditions)

[0123] Grinding device: Engis Japan Corporation grinding machine EJ-380IN-CH

[0124] Polishing pad: NITTA HAAS Co., Ltd. hard polyurethane pad IC1010

[0125] Grinding pressure: 3.0psi (1psi = 6894.76Pa)

[0126] Grinding plate speed: 60rpm

[0127] Grinding head (bracket) speed: 60rpm

[0128] Supply of polishing composition: Overflow

[0129] Polishing composition supply amount: 100 mL / min

[0130] Grinding time: 60 seconds.

[0131] (Polishing object)

[0132] Regarding the polishing object, the following 300 mm blank wafers were prepared. Each wafer was cut into 30 mm × 30 mm pieces as test pieces, and the polishing test was carried out. The details of the polishing object used in the test are shown below. It should be noted that the impurity content (doping amount) is the amount relative to the total 100 atomic % of polysilicon and impurities.

[0133] Polysilicon doped with p-type impurities

[0134] (1) Boron-doped polysilicon (boron content: 11.5 atomic %)

[0135] (2) Aluminum-doped polysilicon (aluminum content: 10 atomic %)

[0136] It should be noted that the content of the p-type impurity doped in the polycrystalline silicon was calculated using the following equipment under the following conditions.

[0137] Measurement equipment: Multifunctional scanning X-ray photoelectron spectroscopy (XPS)

[0138] Equipment name and manufacturer: PHI5000 Versa Probe manufactured by ULVAC-PHI, Inc.

[0139] Measurement: In the case of boron-doped polysilicon, the measured elements are boron, silicon, oxygen and carbon. The sweep times of the measuring equipment are set to 10 for each element. The output value of the polysilicon (Poly-Si output value; i.e., the total output value of Si, O and C) and the output value of boron (B output value) are used to calculate the boron content (B content) (atomic %) relative to the total of 100 atomic % of polysilicon and boron by the following formula (i).

[0140] Formula (i)

[0141] B content (atomic %) = B output value (%) / (Poly-Si output value (%) + B output value (%)).

[0142] It should be noted that in the case of aluminum-doped polysilicon, the measured elements are aluminum, silicon, oxygen, and carbon. Except for changing the B output value (%) of the above formula (i) to the output value of aluminum (Al output value), other conditions are the same as those for boron-doped polysilicon, and the aluminum content (Al content) (atomic %) relative to the total of 100 atomic % of polysilicon and aluminum is calculated.

[0143] The polishing objects used in the evaluation of each polishing composition are shown in Table 1 and Table 2. It should be noted that in Table 1 and Table 2, the impurities doped in the polishing object are shown in the column "Doping species of polycrystalline silicon". When the doping species of polycrystalline silicon is boron, it means the boron-doped polycrystalline silicon described above (1), and when it is aluminum, it means the aluminum-doped polycrystalline silicon described above (2).

[0144] (grinding speed)

[0145] The polishing speed (polishing rate) is calculated according to the following formula.

[0146]

[0147] The film thickness was determined using an optical interference film thickness measuring device LAMBDA ACE VM-2030 manufactured by SCREEN SEMICONDUCTOR SOLUTIONS CO., LTD. and evaluated by dividing the difference in film thickness before and after polishing by the polishing time. The results are shown in Tables 1 and 2 below.

[0148] [Table 1]

[0149]

[0150] [Table 2]

[0151]

[0152] As shown in Table 1, when the polishing compositions of Examples 1 to 11 were used, the polishing speed was greater than / min., compared with the polishing compositions of Comparative Examples 1 to 14, polycrystalline silicon doped with p-type impurities can be polished at a higher polishing rate.

[0153] The results of Comparative Example 10 show that when the zeta potential of the abrasive in the polishing composition is positive, the abrasive in the polishing composition aggregates, which is not suitable as a polishing composition. In addition, the results of Comparative Example 11 show that when a bridged bicyclic compound having a tertiary nitrogen atom is used as an additive, if the content of the additive is 0.5% by mass or more relative to the total mass of the polishing composition, the abrasive in the polishing composition aggregates, which is not suitable as a polishing composition.

[0154] Comparison of Examples 1 and 2 with Comparative Examples 12 and 13 shows that polycrystalline silicon doped with p-type impurities can be polished at a high polishing rate by making the nitrogen atom possessed by the bridged bicyclic compound used as an additive a tertiary nitrogen atom.

[0155] This shows that a polishing composition having a negative zeta potential of the abrasive, containing less than 0.5 mass % of a bridged bicyclic compound having a tertiary nitrogen atom, and having a pH of less than 5 improves the polishing rate of polycrystalline silicon doped with p-type impurities.

[0156] This application is based on Japanese Patent Application No. 2020-044292 filed on March 13, 2020, the disclosure of which is incorporated herein in its entirety by reference.

Claims

1. A polishing composition comprising abrasive grains, a bridged bicyclic compound, a pH adjuster, a dispersion medium and optionally an additive, The zeta potential of the abrasive particles is negative. The content of the abrasive grains is 1.5 mass % or more and 20 mass % or less, The bridged bicyclic compound is a bridged bicyclic compound having a tertiary nitrogen atom, The content of the bridged bicyclic compound is 0.03 mass % or more and 0.3 mass % or less relative to the total mass of the polishing composition. The pH of the polishing composition is 4.5 or less, The pH regulator is an inorganic acid or an organic acid. The additives optionally included as needed are at least one selected from the group consisting of an oxidant, a complexing agent, an anticorrosive agent, and an antifungal agent.

2. The polishing composition according to claim 1, wherein The bridged bicyclic compound is an azabicyclic compound having a tertiary nitrogen atom as a ring atom and having 6 to 12 carbon atoms.

3. The polishing composition according to claim 1, wherein The bridged bicyclic compound is a compound represented by the following structural formula (1): In formula (1), X is independently a nitrogen atom or CH, Y is -NH-, -NR 1 -or-R 2 -, at this time, R 1 is a substituted or unsubstituted alkyl group having 1 to 3 carbon atoms, R 2 is a substituted or unsubstituted alkylene group having 1 to 3 carbon atoms, n and m are each independently an integer of 0 to 2, Wherein, at least one of X is N, or Y is -NR 1 -.

4. The polishing composition according to claim 1, wherein The content of the abrasive grains is 1.5 mass % or more and 10 mass % or less relative to the total mass of the polishing composition.

5. The polishing composition according to claim 1, wherein The abrasive grains are colloidal silica with organic acid fixed on the surface.

6. The polishing composition according to claim 1, wherein The abrasive has a zeta potential of not less than -45 mV and not more than -15 mV. 7 . The polishing composition according to claim 1 , which is used for polishing an object to be polished comprising polycrystalline silicon doped with p-type impurities. 8 . A polishing method comprising the step of polishing an object to be polished using the polishing composition according to claim 1 . 9 . A method for manufacturing a semiconductor substrate, comprising the step of polishing a semiconductor substrate including polycrystalline silicon doped with p-type impurities by the polishing method according to claim 8 .