Lightweight broadband absorbing material for high-power microwave darkroom and preparation method thereof

By using non-combustible and high-temperature resistant inorganic fiber cloth and nano-conductive carbon film in high-temperature microwave anechoic chamber absorbing materials, combined with a ceramic protective layer, the problem of oxidation of existing materials at high temperatures is solved, and efficient and durable broadband absorbing is achieved performance, suitable for high temperature and high power testing.

CN113394573BActive Publication Date: 2024-10-01XIAN ANJUDE NANO TECH CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
CN202110840616.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-25
Publication Date
2024-10-01
Estimated Expiration
2041-07-25

AI Technical Summary

Technical Problem

Existing high-frequency and high-power microwave anechoic chamber absorbing materials are oxidized at high temperatures and cannot effectively protect the carbon-based absorbing agent, resulting in a decrease in absorbing performance and unable to meet the needs of high-temperature applications above 300°C.

Method used

Using non-combustible and high-temperature resistant inorganic fiber cloth as the base material, it is coated with a nano-conductive carbon film and covered with a ceramic polymer precursor to form a three-dimensional periodic structure. The design is optimized through electromagnetic simulation to form a lightweight, broadband, high-temperature-resistant and high-performance Power density absorbing material to prevent oxidation of the carbon layer.

Benefits of technology

Achieved long-term use at high temperatures as an absorbing material, with low reflectivity and high oxygen index, able to withstand power density exceeding 10kW/m², reducing the risk of fire caused by microwave energy, with reasonable cost, suitable for high temperature and high power testing scene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113394573B_ABST
    Figure CN113394573B_ABST
Patent Text Reader

Abstract

The present invention provides a lightweight broadband absorbing material for a high-power microwave darkroom, characterized in that the structure of the absorbing material is: a three-dimensional periodic structure composed of non-flammable and high-temperature resistant absorbing sheets, the absorbing sheets are flat, corrugated or three-dimensional honeycomb structures; the height range of the three-dimensional periodic structure is 0.1 to 2m, the period size range is 1cm to 50cm, the absorbing bandwidth range is 0.03GHz to 40GHz, the oxygen index is higher than 60%, the use temperature in the air is not less than 600℃, and the power density that can be tolerated exceeds 10kW / m 2 The absorbing material provided by the present application is a non-combustible material with high temperature resistance and oxygen index better than 60%, and can withstand high power density, light weight and low cost absorbing periodic structure. The product of the present invention can be used in high power and high temperature test darkrooms and other required scenes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of microwave absorbing materials and structures, in particular to a high-temperature and high-power-density broadband absorbing structure, and in particular relates to a lightweight broadband absorbing material for a high-power microwave darkroom and a preparation method thereof. Background Art

[0002] With the increasing demand for high-frequency and high-power testing, the requirements for the power density that absorbing materials can withstand are also increasing. The power density that absorbing materials commonly used in darkrooms can withstand is basically below 6kW / m2; the maximum power density of sponge absorbing cones is below 2.5kW / m2, mainly below 1.5kW / m2, and the maximum operating temperature does not exceed 80℃; the maximum power density of non-woven absorbing cones is below 6kW / m2, and the maximum operating temperature does not exceed 120℃. When absorbing materials absorb high-energy microwaves, they heat themselves, soften, and even catch fire. Although the maximum power density of highly flame-retardant aramid and glass fiber honeycombs can exceed 6kW / m2, their cost is more than 10 times that of sponge and non-woven absorbing materials. The absorbing cone material that can withstand the highest power is silicon carbide ceramic, which can withstand temperatures above 1000°C and high power density of several 10kW / m2. However, the density of silicon carbide exceeds 3g / cm3. To achieve the same absorbing performance, its surface density is more than 10 times that of other absorbing materials. It is very heavy and its price is no lower than that of aramid absorbing honeycomb. At the same time, due to its high dielectric constant, it is difficult to achieve the absorbing performance that other absorbing materials can achieve, that is, a low reflectivity of -40dB.

[0003] As a broadband absorbing material and structure for applications below 180°C, there is already a relatively mature solution, namely the absorbing honeycomb structure. Through proper ventilation and cooling, the aramid honeycomb can withstand a power density of more than 10kW / m2 and an oxygen index greater than 30, meeting the Class B flame retardant requirements. Japan's NEC-Tokin uses ceramic absorbing plates with added absorbing agents to form absorbing cones to achieve higher power density and heat resistance. The price is also relatively reasonable, but the absorbing performance is also compromised.

[0004] The applicant of the present invention has designed absorbing materials using honeycomb and honeycomb-like structures, and applied for multiple broadband absorbing materials for microwave darkrooms (CN201510052941.4, CN201510052941.4, CN201810909123.5, CN2018115342993, CN201910547844.0, CN201911293988.4). Some of the applications have been authorized, but the absorbent is not effectively protected, and the carbon-based absorbent is not prevented from being oxidized in high-temperature air, and cannot meet high-temperature applications above 300°C.

[0005] Non-combustible inorganic fiber cloth is used as the base material of the absorbing material, and a nano-conductive carbon film with good temperature stability is used as the absorbing coating. A ceramic protective layer is coated on the outer surface to prevent the carbon layer from being oxidized in the air, so as to achieve long-term high-temperature use in the air. The absorbing material is combined into a three-dimensional cone and wedge absorbing structure to achieve broadband, long-term high-temperature resistance and high-power density absorbing material for darkrooms. At the same time, it has low surface density and reasonable price, and has broad application prospects to replace sponge and non-woven absorbing materials to reduce fires caused by local high temperatures generated by concentrated microwave energy. Summary of the invention

[0006] The purpose of the embodiment of the present invention is to provide a lightweight broadband absorbing material and preparation method for a high-power microwave darkroom. The absorbing material is a high-temperature resistant, non-flammable, oxygen index better than 60%, high-power density-resistant, lightweight and low-cost absorbing periodic structure. The product of the present invention can be used in high-power and high-temperature test darkrooms and other required scenarios, such as local protection of microwave weapon test field. The specific technical solution is as follows:

[0007] The present application provides a lightweight broadband absorbing material for a high-power microwave darkroom, wherein the structure of the absorbing material is: a three-dimensional periodic structure composed of non-flammable and high-temperature resistant absorbing sheets, wherein the absorbing sheets are flat, corrugated or three-dimensional honeycomb structures;

[0008] The three-dimensional periodic structure has a height range of 0.1 to 2 m, a period size range of 1 cm to 50 cm, an absorption bandwidth range of 0.03 GHz to 40 GHz, an oxygen index higher than 60%, an operating temperature in air of not less than 600°C, a tolerable power density of more than 10 kW / m2, and is made of non-combustible material.

[0009] Optionally, the preparation process of the wave absorbing sheet is as follows: using a non-flammable and high temperature resistant inorganic fiber cloth as a substrate, coating the substrate with carbon and carbonizing it to form a polymer material with a conductive carbon film, then coating it with a layer of a ceramic inert polymer precursor, and sintering it at a high temperature in an inert atmosphere to form the wave absorbing sheet;

[0010] The weight ratio of the combustible carbon component in the absorbing material does not exceed 2%.

[0011] Optionally, the substrate is at least one of glass fiber, basalt ceramic fiber, high silica fiber, alumina fiber, silicon carbide fiber, and quartz fiber;

[0012] The substrate is in the form of woven fabric or non-woven fabric, the thickness of the substrate is in the range of 0.1 to 5 mm, and the surface density is in the range of 50 to 600 g / m 2 .

[0013] Optionally, the material of the conductive carbon film is a polymer material that can be carbonized on the fiber surface to form a conductive carbon film;

[0014] The material of the conductive carbon film is any one of polystyrene, polyimide, epoxy resin, cyanate resin, soluble mesophase asphalt, and phenolic resin;

[0015] The material of the conductive carbon film is a polymer material that can be carbonized at a low temperature of 600°C and can conduct electricity. The material of the conductive carbon film is aromatic hydrocarbon polyimide or soluble mesophase pitch;

[0016] The thickness of the conductive carbon film does not exceed 3 micrometers, and the surface square resistance formed by the conductive carbon film is adjustable between 30 and 1000 ohms.

[0017] Optionally, the material forming the conductive carbon film is a polymer material, and the material forming the conductive carbon film is a polymer material to which at least one conductive nano additive selected from carbon black, carbon nanotubes, and graphene sheets is added;

[0018] The diameter of the carbon black is no greater than 0.06 micrometers, the diameter of the carbon nanotube is no greater than 0.1 micrometers, and the thickness of the graphene sheet is less than 10 nanometers;

[0019] The volume content of the conductive nano additive in the conductive carbon film is in the range of 1 to 30%.

[0020] Optionally, the material of the ceramicizable inert polymer precursor is at least one organic coating material selected from the group consisting of siloxane resin, polycarbosilane, and polycarbonitridosilane;

[0021] Alternatively, the material of the ceramicizable inert polymer precursor is at least one inorganic coating material selected from the group consisting of silicate, silica sol, and phosphate;

[0022] The inert polymer precursor is formed after high-temperature treatment, and the inert polymer precursor is used for bonding the wave absorbing plates to form a three-dimensional honeycomb structure.

[0023] Optionally, the preparation process of the three-dimensional periodic structure is: forming a basic shape by a pointed cone honeycomb or a pointed wedge honeycomb, and putting a cone, square cone or pointed wedge protective cover formed by the same high temperature resistant absorbing sheet on the pointed cone honeycomb or the pointed wedge honeycomb;

[0024] The pointed cone honeycomb and the pointed wedge honeycomb are hexagonal honeycombs formed by bonding absorbing sheets or corrugated tiles, or are square honeycombs formed by embedding absorbing sheets or corrugated tiles.

[0025] The substrate is 0.3 mm thick E glass fiber twill cloth, the conductive carbon film is a conductive carbon film obtained by carbonizing 3-10% graphene soluble mesophase asphalt at 600°C, the inert polymer precursor forms a protective coating, the protective coating is 50% neutral silica sol, the drying and curing temperature is 120°C, and the sintering temperature is 600°C;

[0026] The total height of the three-dimensional periodic structure is 900 mm, the period is 200×200 mm, and the honeycomb holes of 8×8 are formed by an over-stretched honeycomb with a side length of 13.7 mm. The stretched honeycomb is made of corrugated glue and then cut into a square cone with a side length of 200 mm and a height of 900 mm, and a square cone cover with a height of 700 mm. The square cone and cover obtained by cutting are composed of the square cone and the cover.

[0027] Optionally, the shape, size, substrate thickness and surface resistance of the three-dimensional periodic structure and the absorber are optimized by electromagnetic simulation;

[0028] During the optimization process, the shape, arrangement and surface square resistance of each absorber are optimized through simulation according to the requirements of absorbing performance. The absorbers after simulation optimization have the lowest height and use the least materials while meeting the requirements of absorbing performance.

[0029] The software used for electromagnetic simulation is any finite element electromagnetic simulation software such as HFSS, CST or FDTD;

[0030] The substrate is 0.2 mm thick E glass fiber twill cloth, the conductive carbon film is a conductive carbon film obtained by carbonizing 3-10% graphene soluble mesophase pitch at 600° C., the inert polymer precursor forms a protective coating, and the protective coating is 50% neutral silica sol;

[0031] The three-dimensional periodic structure has a total height of 450 mm and a period of 100×100 mm, and is formed by a 100×100 mm cross-section square interlocking pointed cone honeycomb and a conical cover with a diameter of 100 mm and a height of 350 mm;

[0032] The pointed cone honeycomb is composed of 10 wave absorbing sheets, and the honeycomb tip corresponding to the conical cover is made of a 100mm wide and 350mm high pointed cone plus a 100mm high base.

[0033] The present application also provides a method for preparing a lightweight broadband absorbing material for a high-power microwave darkroom, comprising the following steps:

[0034] S1. Using electromagnetic simulation software to optimize the shape, size, substrate thickness and surface square resistance of the honeycomb structure and the protective cover to obtain a simulated structure, and preparing a test sample according to the simulation results, using measured data to feedback and correct the surface square resistance value to optimize the design, and obtaining the final optimization result after several cycles;

[0035] S2. Production of conductive coatings and high temperature resistant protective coatings;

[0036] S3. Spraying or dipping the conductive coating on a substrate, drying and curing the conductive coating and cracking the conductive coating in a furnace at a temperature above 600° C. in an inert atmosphere to form a carbon film, so that the surface of the substrate is covered with a conductive carbon film, and the surface conductivity of the carbon film is changed according to the amount of conductive coating impregnation and the amount of nano-carbon material added to the coating. The change process is based on the principle that the thickness of the carbon film is proportional to the surface conductivity and inversely proportional to the surface resistance;

[0037] S4. spraying or dipping the conductive carbon film with a protective coating, drying and curing the protective coating, extruding the obtained structure into a corrugated shape using a corrugator, and applying the same protective coating to the corrugated part using the attached protective coating as glue to form multi-layer corrugated; stacking the multi-layer corrugated and curing it by heat micro-pressure to form a honeycomb block, and sintering it in a furnace above 600° C. under an inert atmosphere, so that the surface of the substrate is covered with an anti-oxidation protective coating and forms the desired corrugated or honeycomb shape;

[0038] S5. The absorbing sheet is cut into a desired shape, folded into a wedge, a pointed cone or a conical shape, and sewn into a protective cover with glass fiber or quartz fiber, and the protective coating is used as a glue to bond the protective cover together;

[0039] S6. Cut the absorbing sheet or corrugated paper into the required shape, combine them into interlocking honeycombs, and fix them at the intersections of the interlocking honeycombs with high-temperature resistant glue, and cut the interlocking honeycombs into wedges or cone honeycombs with a high-speed saw, thereby obtaining the lightweight broadband absorbing material.

[0040] Optionally, S3 and S4 are implemented according to the following steps:

[0041] The continuous production line is adopted. The rolled substrate is unwound from the unwinder at a uniform speed. The speed range of the production line is 1 to 50 meters per minute. After spraying or dipping the coating, preliminary solvent drying in a low-temperature oven, and drying and curing in a high-temperature oven, it is extruded into a corrugated belt through a corrugator, and then rolled up. The whole roll of the product is placed in a high-temperature furnace for cracking, carbonization and ceramicization.

[0042] The conductive carbon film adopts a graphene-soluble mesophase asphalt conductive coating layer, the asphalt is dissolved in quinoline to form a 20% solution, nanographene powder is added, and the asphalt is dispersed at a high speed or ultrasonically dispersed to obtain the conductive carbon film, wherein the weight ratio of asphalt to graphene is 100:3-10;

[0043] Alternatively, the conductive carbon film uses high ceramic conversion rate silicone resin, the silicone resin is siloxane, the siloxane resin has a high oxygen chemical structure with an O / Si ratio greater than 1.3, the carbon hydrogen content of the siloxane resin is less than 25%, and the concentration of the siloxane resin in chloroform is 15%.

[0044] The present application also provides a widescreen absorbing periodic structure that can be used in a high-power microwave darkroom. The absorbing material is a three-dimensional periodic structure composed of non-flammable and high-temperature resistant absorbing sheets. The absorbing sheets can be flat or corrugated, or can be a three-dimensional honeycomb structure. The three-dimensional broadband absorbing structure has a height of 0.1 to 2m, a periodic size of 1 to 50cm, an absorbing bandwidth of 0.03 to 40GHz, a temperature of more than 600°C, and a power density of more than 10kW / m 2 The high temperature resistant absorber is made of non-combustible high temperature resistant inorganic fiber cloth as the substrate, coated with a polymer material that becomes a conductive carbon film after carbonization and then coated with a layer of inert polymer precursor that can be ceramicized, and then sintered at high temperature in an inert atmosphere. The weight ratio of the combustible carbon component in the absorber material does not exceed 2%.

[0045] Flexible non-combustible substrates are inorganic fiber materials such as glass fiber, basalt ceramic fiber, high silica fiber, alumina fiber, silicon carbide fiber, and quartz fiber. E glass fiber is used at 600°C and below, which is cheap and has a wide range of raw materials. Basalt fiber and high silica fiber can be used between 800 and 1000°C, and the price is acceptable. Quartz fiber, alumina fiber, and silicon carbide fiber can be used for special application scenarios above 1000°C, but the cost is relatively high. The fiber can be in the form of various woven fabrics and non-woven fabrics. Woven fabrics have high tear strength and slightly higher cost. Plain weave and various twill weaves can be used to meet mechanical requirements. There are many types of non-woven fabrics, such as needle felt and non-woven fabrics bonded with a small amount of organic adhesive. The thickness of the substrate is 0.1 to 5 mm, and the surface density is 50 to 600 g / m2. If it is too thin, the mechanical strength and structural rigidity are insufficient, and if it is too thick, the cost and weight will increase. For high-frequency absorbing structures with shorter heights, thinner substrates are used with better flexibility; for low-frequency absorbing structures with higher heights, thicker substrates are used with higher rigidity and strength.

[0046] The conductive layer is any polymer material that can be carbonized on the fiber surface to form a conductive carbon film: for example, polystyrene, polyimide, epoxy resin, cyanate resin, soluble mesophase pitch, phenolic resin, etc. The main structure of aromatic hydrocarbon polyimide and soluble mesophase pitch is a multi-ring benzene ring with a planar molecular structure. After carbonization, it is easy to form a highly conductive graphene structure, which is the preferred conductive carbonized film. The thickness of the carbon film does not exceed 3 microns, preferably does not exceed 1 micron, and more preferably, within 0.5 microns. Its thickness has no significant effect on the flexibility of the fiber cloth. Conductive nano additives such as carbon black, carbon nanotubes and graphene can be added to the polymer material of the conductive layer film to stabilize the conductivity of the coating at different temperatures. In particular, when carbonized at low temperature, the conductivity of the carbonized film is not high and needs to be improved by high conductivity additives. The diameter of the conductive carbon black is not greater than 0.06 microns, the diameter of the carbon nanotube is not greater than 0.1 microns, and the thickness of the nanographene sheet is less than 10 nanometers, preferably less than 3 nanometers, and the diameter is less than 2 microns, preferably less than 500 nanometers. The volume content of conductive carbon black, carbon nanotubes and graphene in the conductive carbon film is 1-30%, preferably 3-10%. The conductive nanocarbon material can be added independently, or two or three carbon materials can be added at the same time. The surface square resistance formed by the carbonized coating is adjustable between 30 and 1000 ohms. The impedance range of the conductive carbon film is suitable for the design of absorbing materials, with high temperature stability, low density, and less weight gain, which is superior to other dielectric absorbing materials.

[0047] Carbon film is easily oxidized at high temperature, losing its conductivity and wave-absorbing properties, and requires a dense protective film to prevent high-temperature oxidation and ablation. The ceramic polymer precursors coated on the outside of the conductive carbon film are: siloxane resin, polycarbosilane, polycarbonitride silane, etc. The ceramicization temperature is relatively high, and sintering above 1000°C is required to achieve high density and stability in high-temperature air. Inorganic coating materials such as silicates, silica sols and phosphates can also be used, and the sintering temperature can be lowered, even not exceeding 350°C. Since there are larger particles in the inorganic raw materials, a thicker coating thickness is required to achieve the same protective performance. Silica sol is preferred, and its particle size is less than 50nm. The inert protective film can also be used for bonding absorbers to form a three-dimensional honeycomb structure.

[0048] The three-dimensional structure is formed by a pointed cone honeycomb or a pointed wedge honeycomb, on which a protective cover of a cone, square cone or pointed wedge formed by the same high-temperature resistant absorbing sheet is put. The honeycomb can be a hexagonal honeycomb formed by bonding the absorbing sheet into a honeycomb block and stretching and heat setting, which has good shape and mechanical stability; it can also be a square or rectangular cross-section honeycomb formed by absorbing sheets or corrugated sheets. Preferably, a pointed cone honeycomb is covered with a conical hat to achieve balanced absorption of electromagnetic waves of various polarizations and incident angles.

[0049] The shape, size, substrate thickness and surface resistance of the high-temperature absorbing three-dimensional periodic structure are optimized by electromagnetic simulation. Finite element electromagnetic simulation software HFSS, CST, FDTD, etc. are used to calculate the reflectivity of the structure, and the minimum height and the least material are achieved according to the requirements of absorbing performance. The optimization range includes the shape, arrangement and surface resistance of each absorbing plate. The surface resistance of the absorbing plate ranges from 30 to 1000 ohms. The optimal value is determined by simulation and corrected according to the actual microwave measurement value of the absorbing plate. The performance of the optimized three-dimensional absorbing structure is similar to that of sponge and non-woven absorbing materials of the same height, and the low-frequency absorbing performance can be improved through optimized design.

[0050] The method for preparing a three-dimensional wave absorbing periodic structure for a high-power darkroom adopts the following steps:

[0051] S1. Use electromagnetic simulation software to optimize the shape, size, substrate thickness and surface square resistance of the honeycomb and protective cover. Prepare test samples based on preliminary simulation results. Use measured data to feedback and correct the surface square resistance value to optimize the design. After several cycles, the final optimization result is obtained.

[0052] S2. Produce conductive coating and high temperature resistant protective layer coating according to the use temperature and simulation results;

[0053] S3. Spraying or dipping a conductive coating on a substrate, drying and curing the conductive coating, and drying and curing the conductive coating and pyrolyzing the conductive coating in a furnace at a temperature above 600° C. in an inert atmosphere to form a carbon film, so that the surface of the substrate is covered with a conductive carbon film, and the surface conductivity of the carbon film is changed according to the amount of conductive coating impregnation and the amount of nano-carbon material added to the coating. The thicker the carbon film, the higher the surface conductivity;

[0054] S4. Spray or dip a protective coating on the conductive carbon film, dry and solidify the protective coating, extrude it into a corrugated shape using a corrugator if necessary, or locally apply the same coating as glue, stack and heat-press multiple layers of fiber cloth to form a honeycomb block, stretch and shape it at high temperature, and sinter it in a furnace above 600°C under an inert atmosphere, so that the surface of the substrate is covered with an anti-oxidation protective coating and forms the desired corrugated or honeycomb shape;

[0055] S5. Cut the absorber into the required shape, fold it into a wedge, a cone or a conical shape, and sew it into a cover with glass fiber or quartz fiber. The protective coating can also be used as glue to bond the cover.

[0056] S6. Cut the absorber or corrugated sheet into the required shape, combine them into interlocking honeycombs, and fix them at the intersection with high temperature resistant glue, or cut the bonded honeycombs into wedges or cones with a high-speed saw;

[0057] In step S2, the method for preparing the graphene composite soluble mesophase asphalt conductive slurry is to dissolve asphalt in quinoline to form a 20% solution, add nanographene powder, and obtain it by high-speed dispersion or ultrasonic dispersion, and the weight ratio of asphalt to graphene is 100:3-10. When using silica sol as a protective coating, its concentration must be higher than 30% and the pH value must be between 6 and 8. When using silicone resin with a high ceramic conversion rate, the silicone resin is siloxane, and the silicone resin has a high oxygen chemical structure with an O / Si ratio greater than 1.3, and the weight of the carbon and hydrogen components in the molecular structure is less than 25%.

[0058] The preparation of the high temperature resistant absorber and the corrugated structure in steps S3 and S4 can be produced by a roll-to-roll continuous production line. The rolled substrate is unwound from the unwinder at a uniform speed. The speed range of the production line is 1 to 50 m / min. After spraying or dipping the coating, preliminary solvent drying in a low-temperature oven, drying and curing in a high-temperature oven or extruding into a corrugated tape by a corrugator, and then winding, the entire roll of the product is placed in a high-temperature furnace for cracking, carbonization and ceramicization.

[0059] The bottom dimensions of the standard absorbing structure are 600×600mm, and the height is optimized according to the requirements of performance and absorbing bandwidth. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0061] Figure 1 This is the design diagram of Example 1; Figure 1 The accompanying drawings are marked as follows: 1. the highest pointed cone absorbing plate, 2. the outer pointed cone absorbing plate, 3. the middle and high pointed cone absorbing plate, 4. the cross-sectional view of the absorbing cone.

[0062] Figure 2 This is the corrugated wave absorbing structure design adopted in Example 2 of the present invention.

[0063] Figure 3 The honeycomb-type wave absorbing structure design adopted in the third embodiment of the present invention is Figure 3 Figures a) to c) are the process of preparing honeycombs by stretching. Figure 3 d) to g) are schematic diagrams of wave-absorbing honeycomb structures. Figure 3 The reference numerals in the drawings are: 1. absorber, 2. node glue. DETAILED DESCRIPTION

[0064] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0065] Example 1

[0066] The base material is 0.2mm thick E glass fiber twill cloth, which can withstand high temperatures above 600℃. Figure 1 As shown in the figure, the total height of the absorbing structure is 450mm, the period is 100X100mm, and the height of the cone with a diameter of 100mm is 350mm. The cone is supported by a square pointed cone honeycomb with a cross section of 100X100mm. The pointed cone honeycomb is composed of 10 absorbing sheets. The honeycomb tip corresponding to the cone is a 100mm wide, 350mm high pointed cone plus a 100mm high base. The honeycomb wall adjacent to the cone at about 25mm is also a 100mm wide, 175mm high pointed cone plus a 100mm high base. The honeycomb wall at 50mm on the left and right is a 100mm wide, 50mm high pointed cone plus a 100mm base. After simulation optimization, the shape achieves a reflectivity better than -40dB in the wide frequency range of 1.5 to 40GHz, a short-term heat resistance temperature of 600℃, a long-term heat resistance temperature of 450℃, and a continuous irradiation microwave power density greater than 10kW / m2. The oxygen index test result of the absorbing sheet is 75%.

[0067] The method for preparing graphene composite soluble mesophase asphalt conductive slurry is to dissolve asphalt in quinoline to form a 20% solution, add nanographene powder with a d50 of 0.7 microns, and obtain it by high-speed dispersion or ultrasonic dispersion. The weight ratio of asphalt to graphene is 100:3-10. The protective coating and adhesive are neutral silica sol with a concentration greater than 30% and a pH value between 6 and 8. The drying and curing temperature is 120°C and the sintering temperature is 600°C.

[0068] The roll-to-roll continuous production line can be used for production. The rolled substrate is released from the unwinder at a uniform speed. The speed range of the production line is 1 to 50 meters per minute. After spraying or dipping in conductive coating, preliminary solvent drying in a low-temperature oven at 80°C, drying and curing in a high-temperature oven at 300°C, and then winding, the whole roll of products is placed in an inert gas protection high-temperature furnace at 600°C for cracking and carbonization, and the carbonization time is 5 hours. The protective coating is also prepared using a continuous production line. The rolled substrate is released from the unwinder at a uniform speed. The speed range of the production line is 1 to 50 meters per minute. After spraying or dipping in protective coating, preliminary moisture drying in a low-temperature oven at 60°C, drying and curing in a high-temperature oven at 120°C, and then winding, the whole roll of products is placed in an inert gas protection high-temperature furnace at 600°C for ceramic densification, and the ceramicization time is 5 hours.

[0069] Preparation of the pointed cone: The length of the pointed cone piece is 600mm and the height is Figure 1 As shown, the absorbers are cut into the required conical shapes, assembled into interlocking honeycombs, and fixed at the intersections with high temperature resistant glue;

[0070] Preparation of cone: Cut the absorber into the required shape, fold it into a cone shape, and sew it into a cover with glass fiber. You can also use the protective coating as glue to glue the cover together. Put the cover on the pointed cone.

[0071] Example 2

[0072] The base material is 0.2mm thick high-silicon cloth, which can withstand high temperatures above 600℃ for long-term use. Figure 2 As shown in the figure, the total height of the absorbing structure is 150mm, the period is 50X50mm, and the height of the cone with a diameter of 50mm is 110mm. The cone is supported by a square pointed cone honeycomb with a cross section of 50X50mm. The pointed cone honeycomb consists of 2 absorbing sheets and 4 corrugated sheets. The depth of the corrugation is 15mm, and the period length is 50mm. The honeycomb tip corresponding to the cone is a 50mm wide, 110mm high pointed cone plus a 40mm base. The corrugated honeycomb wall adjacent to the cone at about 25mm is also a 50mm wide, 25mm high pointed cone plus a 40mm base. After the shape is optimized by simulation, the reflectivity of the wide screen range of 5 to 40GHz is better than -40dB, the short-term heat resistance temperature is 800℃, the long-term heat resistance temperature is 600℃, and the continuous irradiation microwave power density is greater than 15kW / m2. The oxygen index test result of the absorbing sheet is 80%.

[0073] The method for preparing the polyimide conductive paste is to dissolve high molecular weight polyimide in NMP solvent to form a 10% solution, stir and mix to obtain a uniform solution, impregnate the fiber with the polyimide solution, and form a conductive carbon film after carbonization at 1100°C. The protective coating and adhesive are silicone resin with a ceramic conversion rate of 75%, the solvent is chloroform, siloxane with a high ceramic conversion rate, the siloxane resin has a high oxygen chemical structure with an O / Si ratio greater than 1.3, the weight of the carbon and hydrogen components in the molecular structure is less than 25%, the concentration of the siloxane resin in chloroform is 15%, the drying and curing temperature is 180°C, and the sintering temperature is 1000°C.

[0074] The roll-to-roll continuous production line can be used for production. The rolled substrate is unwound from the unwinder at a uniform speed. The speed range of the production line is 1 to 50 m / min. It is sprayed or impregnated with conductive coating, preliminarily dried with solvent in a low-temperature oven at 80°C, and dried and cured in a high-temperature oven at 260°C when preparing flat sheet materials, and then rolled up. When preparing corrugated paper, it is dried and cured in a high-temperature oven at 240°C, and shaped into corrugated paper by a hot roller at 280°C. It is cut into 600 mm long and placed in a graphite box of the same size. The entire box and the entire roll of intermediate products are placed in an inert gas-protected high-temperature furnace for cracking and carbonization at 1100°C, and the carbonization time is 3 hours. The protective coating is also prepared using a continuous production line. For coils, the rolled substrate is unwound at a uniform speed from the unwinder, and the speed range of the production line is 1 to 50 m / min. After spraying or dipping in the protective coating, preliminary solvent drying in a low-temperature oven at 80°C, and drying and curing in a high-temperature oven at 180°C, the substrate is rolled up. For corrugated paper, a whole box of corrugated paper is immersed in the protective coating. After standing for 30 minutes, the excess coating is discharged and dried in a vacuum oven. The drying temperature in the first stage is 80°C, and the drying temperature in the second stage is 180°C. The whole box of corrugated paper and the whole roll of product are placed in an inert gas-protected high-temperature furnace for ceramic densification at 1000°C, and the ceramicization time is 3 hours.

[0075] Preparation of the cone: The length of the cone sheet and the corrugated paper is 600mm, and the height is Figure 2 As shown, the absorber and the corrugated sheet are cut into the required shape, combined into an interlocking honeycomb, and fixed at the intersection with high temperature resistant glue;

[0076] Preparation of cone: Cut the absorber into the required shape, fold it into a cone shape, and sew it into a cover with quartz fiber. Put the cover on the pointed cone.

[0077] Example 3

[0078] The base material is 0.3mm thick E glass fiber twill cloth, which can withstand high temperatures above 600℃. Figure 3 As shown in the figure, the total height of the absorbing structure is 900mm, the period is 200X200mm, and the height of the pointed cone with a side length of 200mm is 700mm. The pointed cone is supported by a square pointed cone honeycomb with a cross section of 200X200mm. The pointed cone honeycomb is composed of an over-stretched honeycomb with a side length of 13.7mm, forming an 8X8 honeycomb hole. After simulation optimization, the shape achieves a reflectivity better than -40dB in the wide frequency range of 0.7 to 40GHz, a short-term heat resistance temperature of 600℃, a long-term heat resistance temperature of 450℃, and a continuous irradiation microwave power density of more than 12kW / m2. The oxygen index test result of the absorber is 75%.

[0079] The method for preparing graphene composite soluble mesophase asphalt conductive slurry is to dissolve asphalt in quinoline to form a 20% solution, add nanographene powder with a d50 of 0.7 microns, and obtain it by high-speed dispersion or ultrasonic dispersion. The weight ratio of asphalt to graphene is 100:3-10. The protective coating and adhesive are neutral silica sol with a concentration greater than 30% and a pH value between 6 and 8. The drying and curing temperature is 120°C and the sintering temperature is 600°C.

[0080] The roll-to-roll continuous production line is adopted. The rolled substrate is unwound from the unwinder at a uniform speed. The speed range of the production line is 1 to 50 m / min. After spraying or dipping with conductive coating, preliminary solvent drying in a low-temperature oven at 80°C, drying and curing in a high-temperature oven at 300°C, and then winding, the whole roll of product is placed in an inert gas-protected high-temperature furnace for cracking and carbonization at 600°C for 5 hours. The protective coating is also prepared using a continuous production line. The rolled substrate is unwound at a uniform speed from the unwinder. The speed range of the production line is 1 to 50 m / min. After spraying or dipping the protective coating, preliminary moisture drying in a low-temperature oven at 60°C, drying and curing in a high-temperature oven at 120°C, and then winding, when preparing corrugated paper, it is dried and cured in a high-temperature oven at 100°C, and shaped into corrugated paper by a hot roller at 150°C. The length of each side of the corrugated paper is 13.7 mm. It is cut into 600 mm long and 900 mm high corrugated sheets and placed in iron boxes of the same size. The entire box and the entire roll of intermediate products are placed in an inert gas-protected high-temperature furnace for ceramic densification at 600°C for 5 hours.

[0081] Preparation of the pointed cone: The length of the corrugated sheet is 600 mm and the height is Figure 3 As shown, the corrugated sheet is cut into the desired shape, and the joints of the corrugated sheets are coated with silica sol (in Figure 3 2) in c, stacked into a honeycomb cone, and cured at 200°C. It can also be made by conventional glass fiber honeycomb preparation process, such as Figure 3 As shown in a to c, the absorber is coated with high temperature glue (protective coating) according to the design, stacked into blocks, hot pressed and glued at 200℃, stretched into a honeycomb, and then shaped at high temperature. It is cut into a pointed cone with a high-speed band saw.

[0082] Preparation of cone: Cut the absorber into the required shape, fold it into a pointed cone, and sew it into a cover with glass fiber, or use silica sol as glue to glue the cover. Put the cover on the pointed cone.

[0083] The above-described embodiment is only a preferred solution of the present invention and does not limit the present invention in any form. There are other variations and modifications without exceeding the technical solution described in the claims.

Claims

1. A lightweight broadband absorbing material for a high-power microwave darkroom, characterized in that: The structure of the absorbing material is: a three-dimensional periodic structure composed of non-flammable and high-temperature resistant absorbing sheets, wherein the absorbing sheets are flat, corrugated or three-dimensional honeycomb structures; The three-dimensional periodic structure has a height range of 0.1 to 2 m, a period size range of 1 cm to 50 cm, a wave absorption bandwidth range of 0.03 GHz to 40 GHz, an oxygen index higher than 60%, an operating temperature in air of not less than 600°C, and a tolerable power density of more than 10 kW / m 2 , and is made of non-combustible material; The preparation process of the absorber is as follows: using non-flammable high temperature resistant inorganic fiber cloth as a substrate, coating carbon on the substrate and carbonizing it to form a polymer material with a conductive carbon film, then coating it with a layer of ceramic inert polymer precursor, and sintering it at high temperature in an inert atmosphere to form the absorber; The weight ratio of the combustible carbon component in the absorbing material does not exceed 2%; The material of the conductive carbon film is a polymer material that can be carbonized on the fiber surface to form a conductive carbon film; The material of the conductive carbon film is any one of polystyrene, polyimide, epoxy resin, cyanate resin, soluble mesophase asphalt, and phenolic resin; The conductive carbon film is made of a polymer material that can be carbonized at a low temperature of 600°C and conduct electricity; The thickness of the conductive carbon film does not exceed 3 micrometers, and the surface square resistance formed by the conductive carbon film is between 30 and 1000 ohms.

2. The absorbing material according to claim 1, characterized in that: The substrate is at least one of glass fiber, basalt ceramic fiber, high silica fiber, alumina fiber, silicon carbide fiber and quartz fiber; The substrate is in the form of woven fabric or non-woven fabric, the thickness of the substrate is in the range of 0.1 to 5 mm, and the surface density is in the range of 50 to 600 g / m 2 .

3. The absorbing material according to claim 1, characterized in that: The conductive carbon film is formed of a polymer material, which is a polymer material to which at least one conductive nano additive selected from carbon black, carbon nanotubes and graphene sheets is added; The diameter of the carbon black is no greater than 0.06 micrometers, the diameter of the carbon nanotube is no greater than 0.1 micrometers, and the thickness of the graphene sheet is less than 10 nanometers; The volume content of the conductive nano additive in the conductive carbon film is in the range of 1 to 30%.

4. The absorbing material according to claim 1, characterized in that: The material of the ceramicizable inert polymer precursor is at least one organic coating material selected from the group consisting of siloxane resin, polycarbosilane, and polycarbonitridosilane; Alternatively, the material of the ceramicizable inert polymer precursor is at least one inorganic coating material selected from the group consisting of silicate, silica sol, and phosphate; The inert polymer precursor is formed after high-temperature treatment, and the inert polymer precursor is used for bonding the wave absorbing plates to form a three-dimensional honeycomb structure.

5. The absorbing material according to any one of claims 1 to 4, characterized in that: The preparation process of the three-dimensional periodic structure is as follows: forming a basic shape with a pointed cone honeycomb or a pointed wedge honeycomb, and putting a cone, square cone or pointed wedge protective cover formed by the same high temperature resistant wave absorbing sheet on the pointed cone honeycomb or the pointed wedge honeycomb; The pointed cone honeycomb and the pointed wedge honeycomb are hexagonal honeycombs formed by bonding absorbing sheets or corrugated tiles, or are square honeycombs formed by embedding absorbing sheets or corrugated tiles. The substrate is 0.3 mm thick E glass fiber twill cloth, the conductive carbon film is a conductive carbon film obtained by carbonizing 3-10% graphene soluble mesophase asphalt at 600°C, the inert polymer precursor forms a protective coating, the protective coating is 50% neutral silica sol, the drying and curing temperature is 120°C, and the sintering temperature is 600°C; The total height of the three-dimensional periodic structure is 900 mm, the period is 200×200 mm, and the honeycomb holes of 8×8 are formed by an over-stretched honeycomb with a side length of 13.7 mm. The stretched honeycomb is made of corrugated glue and then cut into a square cone with a side length of 200 mm and a height of 900 mm, and a square cone cover with a height of 700 mm. The square cone and cover obtained by cutting are composed of the square cone and the cover.

6. The absorbing material according to any one of claims 1 to 4, characterized in that: The shape, size, substrate thickness and surface resistance of the three-dimensional periodic structure and the absorber are optimized by electromagnetic simulation; During the optimization process, the shape, arrangement and surface square resistance of each absorber are optimized through simulation according to the requirements of absorbing performance. The absorbers after simulation optimization have the lowest height and use the least materials while meeting the requirements of absorbing performance. The software used for electromagnetic simulation is any finite element electromagnetic simulation software such as HFSS, CST or FDTD; The substrate is 0.2 mm thick E glass fiber twill cloth, the conductive carbon film is a conductive carbon film obtained by carbonizing 3-10% graphene soluble mesophase pitch at 600° C., the inert polymer precursor forms a protective coating, and the protective coating is 50% neutral silica sol; The three-dimensional periodic structure has a total height of 450 mm and a period of 100×100 mm, and is formed by a 100×100 mm cross-section square interlocking pointed cone honeycomb and a conical cover with a diameter of 100 mm and a height of 350 mm; The pointed cone honeycomb is composed of 10 wave absorbing sheets, and the honeycomb tip corresponding to the conical cover is made of a 100mm wide and 350mm high pointed cone plus a 100mm high base.

7. A method for preparing a lightweight broadband absorbing material for a high-power microwave darkroom, characterized in that: The steps include: S1. Using electromagnetic simulation software to optimize the shape, size, substrate thickness and surface square resistance of the honeycomb structure and the protective cover to obtain a simulated structure, and preparing a test sample according to the simulation results, using measured data to feedback and correct the surface square resistance value to optimize the design, and obtaining the final optimization result after several cycles; S2. Production of conductive coatings and high temperature resistant protective coatings; S3. Spraying or dipping the conductive coating on a substrate, drying and curing the conductive coating and cracking the conductive coating in a furnace at a temperature above 600° C. in an inert atmosphere to form a carbon film, so that the surface of the substrate is covered with a conductive carbon film, and the surface conductivity of the carbon film is changed according to the amount of conductive coating impregnation and the amount of nano-carbon material added to the coating. The change process is based on the principle that the thickness of the carbon film is proportional to the surface conductivity and inversely proportional to the surface resistance; S4. spraying or dipping the conductive carbon film with a protective coating, drying and curing the protective coating, extruding the obtained structure into a corrugated shape using a corrugator, and applying the same protective coating to the corrugated part using the attached protective coating as glue to form multi-layer corrugated; stacking the multi-layer corrugated and curing it by heat micro-pressure to form a honeycomb block, and sintering it in a furnace above 600° C. under an inert atmosphere, so that the surface of the substrate is covered with an anti-oxidation protective coating and forms the desired corrugated or honeycomb shape; S5. The absorbing sheet is cut into a desired shape, folded into a wedge, a pointed cone or a conical shape, and sewn into a protective cover with glass fiber or quartz fiber, and the protective coating is used as a glue to bond the protective cover together; S6. Cut the absorbing sheet or corrugated paper into the required shape, combine them into interlocking honeycombs, and fix them at the intersections of the interlocking honeycombs with high-temperature resistant glue, and cut the interlocking honeycombs into wedges or cone honeycombs with a high-speed saw, thereby obtaining the lightweight broadband absorbing material.

8. The method for preparing a lightweight broadband absorbing material for a high-power microwave darkroom according to claim 7, characterized in that: S3 and S4 are implemented according to the following steps: The continuous production line is adopted. The rolled substrate is unwound from the unwinder at a uniform speed. The speed range of the production line is 1 to 50 meters per minute. After spraying or dipping the coating, preliminary solvent drying in a low-temperature oven, and drying and curing in a high-temperature oven, it is extruded into a corrugated belt through a corrugator, and then rolled up. The whole roll of the product is placed in a high-temperature furnace for cracking, carbonization and ceramicization. The conductive carbon film adopts a graphene-soluble mesophase asphalt conductive coating layer, the asphalt is dissolved in quinoline to form a 20% solution, nanographene powder is added, and the asphalt is dispersed at a high speed or ultrasonically dispersed to obtain the conductive carbon film, wherein the weight ratio of asphalt to graphene is 100:3-10; Alternatively, the conductive carbon film uses high ceramic conversion rate silicone resin, the silicone resin is siloxane, the siloxane resin has a high oxygen chemical structure with an O / Si ratio greater than 1.3, the carbon hydrogen content of the siloxane resin is less than 25%, and the concentration of the siloxane resin in chloroform is 15%.

Citation Information

Patent Citations

  • Super-wide incidence angle microwave absorbing materials and a production method thereof

    CN108966622A

  • Light-weight wave-absorbing darkroom pointed cone material and preparation method thereof

    CN109788728A

  • Microwave-absorbing material for microwave chamber and printing production method thereof

    CN104735964A

  • Ceramic particles with controlled pore and / or microsphere placement and / or size and method of making same

    CN105236947A

  • PIM testing wave-absorbing module for vacuum low-temperature environment

    CN106597124A