Electrophotographic photoreceptor, process cartridge, and image forming device
By reasonably preparing fluorine-containing resin particles and antioxidants on the outermost surface layer of the electrophotographic photoreceptor, the problem of poor charging maintenance is solved, and good initial charging performance and stable charging performance after repeated use is achieved, ensuring the charging potential difference value Within reasonable scope.
Patent Information
- Application Number
- CN202010742967.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-25
- Filing Date
- 2020-07-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-07-29
AI Technical Summary
The existing electrophotographic photoreceptors have poor charging maintenance after repeated use, especially when the number of carboxyl groups of fluorine-containing resin particles is too large or the antioxidant is sublimated at high temperatures, resulting in a charging potential difference value △VH greater than 5V, affecting the performance of the photoreceptor. .
Fluorine-containing resin particles and antioxidants are used on the outermost surface layer of the electrophotographic photoreceptor, and the number of carboxyl groups is controlled within 30 per 106 carbon atoms, the weight reduction of the antioxidant is controlled below 40%, and it is included in the molecule Compounds with more than 2 benzene rings ensure the stability and charging performance of antioxidants.
The initial charging performance of the electrophotographic photoreceptor and the charging maintenance performance after repeated use are improved, and the charging potential difference value △VH is less than 5V, thereby extending the service life of the photoreceptor.
Smart Images

Figure CN113448195B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an electronic photographic photoreceptor, a process cartridge and an image forming device. Background Art
[0002] Japanese Patent Application Laid-Open No. 2004-045858 proposes “an electrophotographic photoreceptor having a photosensitive layer on a conductive support, wherein the photosensitive layer contains a resin and a phenolic antioxidant”.
[0003] Japanese Patent Gazette No. 2004-102158 proposes "a photosensitive body having at least a photosensitive layer formed by sequentially stacking a charge generating layer containing a charge generating material and a charge transporting layer containing a charge transporting material on a conductive support, characterized in that the charge generating layer contains the charge generating material, and the charge transporting layer is formed by a coating liquid containing the charge transporting material, a phenolic antioxidant having a sulfur atom, and a phosphite antioxidant in a non-halogen solvent." Summary of the invention
[0004] Technical problem to be solved by the invention
[0005] The technical problem to be solved by the present invention is to provide an electrophotographic photoreceptor, wherein the number of carboxyl groups contained in the fluorine-containing resin particles per 10 6 The number of carbon atoms is greater than 30; the weight reduction of the antioxidant is greater than 40% by weight after heating at 150°C for 10 minutes in an air atmosphere; or the photosensitive body is assembled in a photosensitive body electrical characteristic evaluation device equipped with a charging device, an exposure device and a static elimination device, and a series of steps of charging, exposing and static elimination are performed for one cycle under the following conditions, and the charging potential after recharging is set to VH1; the above steps are performed for 100 cycles under the following conditions, and the charging potential after recharging is set to VH2. At this time, compared with the case where the absolute value of the difference △VH between the above VH1 and the above VH2 is greater than 5V, the initial charging property is good and the charging maintenance property under repeated use is improved.
[0006] (condition)
[0007] ·Measurement environment: Temperature 20℃ / Humidity 40%RH
[0008] Charging potential: +600V
[0009] Exposure light: 10mJ / m 2
[0010] Exposure wavelength: 780nm
[0011] ·Light source for eliminating static electricity: halogen lamp
[0012] ·Electrostatic light wavelength: above 600nm and below 800nm
[0013] · Anti-static light intensity: 30mJ / m 2
[0014] ·Photoreceptor rotation speed: 66.7rpm
[0015] Means for solving problems
[0016] According to a first aspect of the present invention, there is provided an electrophotographic photoreceptor, wherein:
[0017] The electrophotographic photoreceptor comprises a conductive substrate and a photosensitive layer provided on the conductive substrate.
[0018] The outermost surface layer of the electrophotographic photoreceptor contains fluorine-containing resin particles and an antioxidant.
[0019] The number of carboxyl groups contained in the fluorine-containing resin particles is relative to 10 6 The number of carbon atoms is 0 to 30.
[0020] After heating at 150° C. for 10 minutes in an air atmosphere, the weight loss of the antioxidant is 40% by mass or less.
[0021] According to a second aspect of the present invention, the molecular weight of the antioxidant is 240 or more and 350 or less.
[0022] According to a third aspect of the present invention, the antioxidant having a molecular weight of 240 to 350 is a compound having two or more benzene rings in the molecule.
[0023] According to a fourth aspect of the present invention, the content of the antioxidant is 20 mass % or more and 60 mass % or less relative to the content of the fluorine-containing resin particles.
[0024] According to a fifth aspect of the present invention, the content of the fluorine-containing resin particles is 5 mass % or more and 20 mass % or less based on the outermost surface layer.
[0025] According to a sixth aspect of the present invention, there is provided an electrophotographic photoreceptor, wherein:
[0026] The electrophotographic photoreceptor comprises a conductive substrate and a photosensitive layer provided on the conductive substrate.
[0027] The outermost surface layer of the electrophotographic photoreceptor contains fluorine-containing resin particles and an antioxidant.
[0028] The number of carboxyl groups contained in the fluorine-containing resin particles is relative to 10 6 The number of carbon atoms is 0 to 30.
[0029] The electrophotographic photoreceptor is assembled in a photoreceptor electrical characteristics evaluation device including a charging device, an exposure device, and a static elimination device.
[0030] A series of steps of charging, exposure and neutralization were performed once under the following conditions, and the charging potential after recharging was set to VH1.
[0031] The above process was repeated 100 times under the following conditions, and the charging potential after recharging was set to VH2.
[0032] At this time, the absolute value of the difference ΔVH between the above VH1 and the above VH2 is less than 5V.
[0033] (condition)
[0034] ·Measurement environment: Temperature 20℃ / Humidity 40%RH
[0035] Charging potential: +600V
[0036] Exposure light: 10mJ / m 2
[0037] Exposure wavelength: 780nm
[0038] ·Light source for eliminating static electricity: halogen lamp
[0039] ·Electrostatic light wavelength: above 600nm and below 800nm
[0040] · Anti-static light intensity: 30mJ / m 2
[0041] ·Photoreceptor rotation speed: 66.7rpm
[0042] According to a seventh aspect of the present invention, there is provided a process cartridge that is detachably mounted in an image forming apparatus and includes the above-mentioned electrophotographic photoreceptor.
[0043] According to the 8th scheme of the present invention, the above-mentioned processing box has a cleaning mechanism with a cleaning scraper for cleaning the surface of the above-mentioned electrophotographic photosensitive body, and at least the part of the above-mentioned cleaning scraper that contacts the above-mentioned electrophotographic photosensitive body is composed of a component containing polyurethane rubber and having an endothermic peak temperature in the range of not less than 180°C and not more than 220°C based on differential scanning calorimetry.
[0044] According to a ninth aspect of the present invention, there is provided an image forming apparatus comprising:
[0045] The above-mentioned electrophotographic photoreceptor,
[0046] A charging mechanism is used to charge the surface of the electrophotographic photoreceptor.
[0047] The electrostatic latent image forming mechanism forms an electrostatic latent image on the charged surface of the electrophotographic photoreceptor.
[0048] a developing mechanism for developing the electrostatic latent image formed on the surface of the electrophotographic photoreceptor using a developer containing a toner to form a toner image, and
[0049] The transfer mechanism transfers the toner image to the surface of the recording medium.
[0050] According to the 10th embodiment of the present invention, the image forming device comprises a cleaning mechanism having a cleaning scraper for cleaning the surface of the electrophotographic photosensitive body, and at least the portion of the cleaning scraper in contact with the electrophotographic photosensitive body is composed of a component containing polyurethane rubber and having an endothermic peak temperature in the range of not less than 180°C and not more than 220°C based on differential scanning calorimetry.
[0051] Effects of the Invention
[0052] According to the first embodiment, an electrophotographic photoreceptor can be obtained, wherein the electrophotographic photoreceptor has good initial charging property and improved charging maintenance property under repeated use, compared with the case where the electrophotographic photoreceptor has a conductive substrate and a photosensitive layer provided on the conductive substrate, and the outermost surface layer contains fluorine-containing resin particles and an antioxidant, and the number of carboxyl groups contained in the fluorine-containing resin particles is 10 6 The number of carbon atoms is greater than 30, or the weight loss of the antioxidant after heating at 150° C. for 10 minutes in an air atmosphere is greater than 40% by mass.
[0053] According to the second embodiment, an electrophotographic photoreceptor can be obtained, which has good initial chargeability and improved charge retention during repeated use, compared with the case where the molecular weight of the antioxidant is less than 240 or greater than 350.
[0054] According to the third embodiment, an electrophotographic photoreceptor can be obtained, which has good initial chargeability and improved charge retention during repeated use, compared with the case where the antioxidant is a compound having one benzene ring in the molecule.
[0055] According to the fourth scheme, an electrophotographic photosensitive body can be obtained. Compared with the case where the content of the antioxidant is less than 20% by mass or greater than 60% by mass relative to the content of the fluorine-containing resin particles, the electrophotographic photosensitive body of the fourth scheme has good initial charging properties and improved charging maintenance properties under repeated use.
[0056] According to the fifth scheme, an electrophotographic photosensitive body can be obtained. Compared with the case where the content of the fluorine-containing resin particles relative to the outermost surface layer is less than 5% by mass or greater than 20% by mass, the electrophotographic photosensitive body of the scheme has good initial charging properties and improved charging maintenance properties under repeated use.
[0057] According to the sixth embodiment, an electrophotographic photoreceptor can be obtained, wherein the electrophotographic photoreceptor has good initial charging property and improved charging maintenance property under repeated use, compared with the following case: in an electrophotographic photoreceptor having a conductive substrate and a photosensitive layer provided on the conductive substrate, and the outermost surface layer containing fluorine-containing resin particles and an antioxidant, the number of carboxyl groups contained in the fluorine-containing resin particles is 10 6 The number of carbon atoms is greater than 30; or it is assembled in a photosensitive body electrical characteristics evaluation device equipped with a charging device, an exposure device and a static elimination device, and a series of processes of charging, exposing and static elimination are carried out for one cycle under the following conditions, and the charging potential after recharging is set to VH1, and the above processes are carried out for 100 cycles under the following conditions, and the charging potential after recharging is set to VH2, at this time, the absolute value of the difference △VH between the above VH1 and the above VH2 is greater than 5V.
[0058] According to the seventh or ninth embodiment, a processing box or an image forming apparatus having an electrophotographic photosensitive body can be obtained, and the processing box or the image forming apparatus of the embodiment has good initial charging property and improved charging maintenance property under repeated use compared with the following case: the processing box or the image forming apparatus has a conductive substrate and a photosensitive layer provided on the conductive substrate, the outermost surface layer contains fluorine-containing resin particles and an antioxidant, and the number of carboxyl groups contained in the fluorine-containing resin particles is 10 6 The number of carbon atoms is greater than 30; the weight reduction of the above antioxidant is greater than 40% by weight after heating at 150°C for 10 minutes in an air atmosphere; or it is assembled in a photosensitive body electrical characteristic evaluation device equipped with a charging device, an exposure device and a static elimination device, and a series of steps of charging, exposing and static elimination are carried out for one cycle under the above conditions, and the charging potential after recharging is set to VH1, and the above steps are carried out for 100 cycles under the above conditions, and the charging potential after recharging is set to VH2, at this time, the absolute value of the difference △VH between the above VH1 and the above VH2 is greater than 5V of the electronic photographic photosensitive body.
[0059] According to the eighth or tenth embodiment, a processing box or an image forming apparatus having an electrophotographic photosensitive body can be obtained, and the processing box or the image forming apparatus of the embodiment has good initial charging property and improved charging maintenance property under repeated use compared with the following case: the processing box or the image forming apparatus has a conductive substrate and a photosensitive layer provided on the conductive substrate, and the outermost surface layer contains fluorine-containing resin particles and an antioxidant, and the number of carboxyl groups contained in the fluorine-containing resin particles is 10 6 An electrophotographic photoreceptor having a carbon atom number of not less than 0 and not more than 30 and a weight reduction of the antioxidant after heating at 150°C for 10 minutes in an air atmosphere of not more than 40 mass % (or the electrophotographic photoreceptor is assembled in a photoreceptor electrical characteristic evaluation device having a charging device, an exposure device and a static elimination device, and a series of steps of charging, exposing and static elimination are carried out for one cycle under the above conditions, and the charging potential after recharging is set to VH1, and the above steps are carried out for 100 cycles under the above conditions, and the charging potential after recharging is set to VH2, at this time, the absolute value of the difference △VH between the above VH1 and the above VH2 is not more than 5 V), and a processing box or an image forming device having a cleaning mechanism with a cleaning scraper for cleaning the surface of the above electrophotographic photoreceptor, wherein at least the portion of the cleaning component in contact with the above electrophotographic photoreceptor is composed of a component containing polyurethane rubber and having an endothermic peak top temperature in the range of not less than 180°C and not more than 220°C based on differential scanning calorimetry. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 This is a schematic cross-sectional view showing an example of the layer structure of the electrophotographic photoreceptor according to the present embodiment.
[0061] Figure 2 This is a schematic structural diagram showing an example of the image forming apparatus according to the present embodiment.
[0062] Figure 3 This is a schematic structural diagram showing another example of the image forming apparatus according to the present embodiment. DETAILED DESCRIPTION
[0063] The following is a description of an embodiment of the present invention. These descriptions and examples are for illustrating the embodiment and do not limit the scope of the invention.
[0064] In the numerical range recorded in stages in this specification, the upper limit or lower limit recorded in one numerical range can be replaced by the upper limit or lower limit of the numerical range in other stages recorded. In addition, in the numerical range recorded in this specification, the upper limit or lower limit of the numerical range can be replaced by the value shown in the embodiment.
[0065] Each component may contain two or more corresponding substances.
[0066] When referring to the amount of each component in a composition, if there are two or more substances corresponding to each component in the composition, unless otherwise stated, it refers to the total amount of the two or more substances present in the composition.
[0067] <Electrophotographic Photoreceptor>
[0068] The electrophotographic photoreceptor (hereinafter also referred to as "photoreceptor") of the first embodiment has a conductive substrate and a photosensitive layer provided on the conductive substrate, and the outermost surface layer contains fluorine-containing resin particles and an antioxidant.
[0069] Furthermore, the number of carboxyl groups contained in the fluorine-containing resin particles is relative to 10 6 The number of carbon atoms is 0 to 30, and the weight loss of the antioxidant after heating at 150° C. for 10 minutes in an air atmosphere is 40% by mass or less.
[0070] The photoreceptor of the first embodiment has good initial charging properties due to the above-mentioned configuration, and improves charging retention properties after repeated use. The reason for this is presumably as follows.
[0071] In order to improve the wear resistance of the photoreceptor, a method of adding fluorine-containing resin particles to the outermost surface layer of the photoreceptor is used. 6 Fluorine-containing resin particles containing more than 0 and less than 30 carboxyl groups per carbon atom can improve the chargeability of the photoreceptor, but it is not easy to form hydrogen bonds with the hydroxyl groups contained in the antioxidant contained in the outermost surface layer. Therefore, the interaction between the fluorine-containing resin particles and the antioxidant is reduced, and the antioxidant is easy to sublimate. Due to repeated use, the antioxidant content in the outermost surface layer is reduced. The antioxidant contained in the outermost surface layer can not only prevent the oxidation of the components in the outermost surface layer, but also has the effect of replenishing the charge. Therefore, due to the decrease in the concentration of the antioxidant in the outermost surface layer, the chargeability of the photoreceptor is reduced. That is, even if such a photoreceptor has good initial chargeability, the charge retention will be reduced after repeated use. The photoreceptor is a photoreceptor that contains 10% to 20% antioxidants in the outermost surface layer relative to every 10 6 Fluorine-containing resin particles containing 0 to 30 carboxyl groups per carbon atom.
[0072] On the other hand, the photoreceptor of the first embodiment contains 6The present invention relates to a fluorine-containing resin particle having 0 to 30 carboxyl groups per carbon atom, and an antioxidant having a weight loss of 40% by mass or less after heating at 150° C. for 10 minutes in an air atmosphere. The antioxidant having a weight loss within the above range has the characteristic of not easily sublimating even if it does not interact with the fluorine-containing resin particle. Thus, the reduction in charge replenishment capacity due to sublimation of the antioxidant in the outermost surface layer can be suppressed.
[0073] Therefore, it is estimated that the photoreceptor of the first embodiment has good initial chargeability and improved charge retention during repeated use.
[0074] The photoreceptor according to the second embodiment includes a conductive substrate and a photosensitive layer provided on the conductive substrate, wherein the outermost layer contains fluorine-containing resin particles and an antioxidant.
[0075] Furthermore, the number of carboxyl groups contained in the fluorine-containing resin particles is relative to 10 6 The number of carbon atoms is greater than 0 and less than 30, and the photosensitive body is assembled in a photosensitive body electrical characteristics evaluation device equipped with a charging device, an exposure device and a static elimination device. A series of steps of charging, exposure and static elimination are performed for one cycle under the following conditions, and the charging potential after recharging is set to VH1. The above steps are performed for 100 cycles under the following conditions, and the charging potential after recharging is set to VH2. At this time, the absolute value of the difference △VH between the above VH1 and the above VH2 is less than 5V.
[0076] (condition)
[0077] ·Measurement environment: Temperature 20℃ / Humidity 40%RH
[0078] Charging potential: +600V
[0079] Exposure light: 10mJ / m 2
[0080] Exposure wavelength: 780nm
[0081] ·Light source for eliminating static electricity: halogen lamp
[0082] ·Electrostatic light wavelength: above 600nm and below 800nm
[0083] · Anti-static light intensity: 30mJ / m 2
[0084] ·Photoreceptor rotation speed: 66.7rpm
[0085] The photoreceptor of the second embodiment has good initial charging properties and improved charging retention properties after repeated use due to the above-mentioned configuration. The reason for this is presumably as follows.
[0086] As described above, the outermost surface layer contains 6 In a photosensitive body containing fluorine-containing resin particles having 0 to 30 carboxyl groups per carbon atom and an antioxidant, even if the initial charging property of the photosensitive body is good, the antioxidant content in the outermost surface layer will decrease due to continuous use, and the charging property of the photosensitive body will also decrease accordingly.
[0087] The second embodiment contains 6 In a photoreceptor containing fluorine-containing resin particles having 0 to 30 carboxyl groups per carbon atom and an antioxidant, the photoreceptor is assembled in a photoreceptor electrical characteristic evaluation device equipped with a charging device, an exposure device and a static elimination device, and a series of steps of charging, exposure and static elimination are performed once under the above conditions and the charging potential after recharging is set to VH1, and the charging potential after the above steps are performed 100 times under the above conditions and recharging is set to VH2, and the absolute value of the difference △VH between the above VH1 and the above VH2 is 5V or less. When the photoreceptor of the second embodiment satisfies the above conditions, it means that even if it does not interact with the fluorine-containing resin particles, the antioxidant is not easy to sublime. For example, the antioxidant used in the second embodiment has a weight loss of 40% by mass or less after heating at 150°C for 10 minutes in an air atmosphere. This can suppress the reduction of the charge replenishment capacity due to the sublimation of the antioxidant in the outermost surface layer.
[0088] Therefore, it is estimated that the photoreceptor of the second embodiment has good initial chargeability and improved charge retention during repeated use.
[0089] A photoreceptor that conforms to both the first embodiment and the second embodiment (hereinafter also referred to as "the photoreceptor of the present embodiment") is described in detail below. An example of the photoreceptor of the present invention is a photoreceptor that conforms to either of the first and second embodiments.
[0090] Hereinafter, the electrophotographic photoreceptor according to the present embodiment will be described with reference to the drawings.
[0091] Figure 1 The electrophotographic photoreceptor 7A shown has a structure in which an undercoat layer 1, a charge generating layer 2, and a charge transporting layer 3 are sequentially stacked on a conductive substrate 4. The charge generating layer 2 and the charge transporting layer 3 constitute a photosensitive layer 5.
[0092] It should be noted that the electrophotographic photoreceptor 7A may have a layer structure in which the undercoat layer 1 is not provided.
[0093] The electrophotographic photoreceptor 7A may include a single-layer photosensitive layer integrating the functions of the charge generating layer 2 and the charge transporting layer 3. In the case of a photoreceptor including a single-layer photosensitive layer, the single-layer photosensitive layer constitutes the outermost layer.
[0094] The electrophotographic photoreceptor 7A may be a photoreceptor having a surface protective layer on the charge transport layer 3 or on the single-layer photosensitive layer. In the case of a photoreceptor having a surface protective layer, the surface protective layer constitutes the outermost surface layer.
[0095] Hereinafter, each layer of the electrophotographic photoreceptor of this embodiment will be described in detail. Note that reference numerals will be omitted in the description.
[0096] (Conductive substrate)
[0097] As the conductive substrate, for example, metal plates, metal cylinders, and metal belts containing metals (aluminum, copper, zinc, chromium, nickel, molybdenum, vanadium, indium, gold, platinum, etc.) or alloys (stainless steel, etc.) can be cited. In addition, as the conductive substrate, for example, paper, resin films, and belts coated, vapor-deposited, or laminated with conductive compounds (such as conductive polymers, indium oxide, etc.), metals (such as aluminum, palladium, gold, etc.), or alloys can also be cited. Here, "conductive" means that the volume resistivity is less than 10 13 Ωcm.
[0098] When an electrophotographic photoreceptor is used in a laser printer, the surface of the conductive substrate is preferably roughened to a center line average roughness Ra of 0.04 μm or more and 0.5 μm or less in order to suppress interference fringes generated when irradiating laser. It should be noted that when non-interference light is used as a light source, roughening for preventing interference fringes is not particularly necessary, but since the roughening can suppress the occurrence of defects caused by the unevenness of the conductive substrate surface, it is suitable for further extending the life.
[0099] Examples of the roughening method include wet honing in which an abrasive is suspended in water and sprayed onto the conductive substrate; centerless grinding in which the conductive substrate is pressed against a rotating grindstone and continuously ground; and anodizing.
[0100] As a method for roughening the surface, there is also a method in which, instead of roughening the surface of the conductive substrate, conductive or semiconductive powder is dispersed in a resin to form a layer on the surface of the conductive substrate, and the surface is roughened using particles dispersed in the layer.
[0101] The roughening treatment performed by anodic oxidation is a roughening treatment in which an oxide film is formed on the surface of the conductive substrate by anodizing a conductive substrate made of metal (e.g., aluminum) as an anode in an electrolyte solution. As the electrolyte solution, for example, sulfuric acid solution, oxalic acid solution, etc. can be cited. However, the porous anodic oxide film formed by anodic oxidation is chemically active in its original state, easily contaminated, and the resistance change due to the environment is also large. Therefore, it is preferred that the porous anodic oxide film is subjected to the following sealing treatment: in pressurized steam or boiling water (metal salts such as nickel can also be added), the volume expansion caused by the hydration reaction is utilized to block the micropores of the oxide film, so that it becomes a more stable hydrated oxide.
[0102] The film thickness of the anodic oxide film is preferably, for example, 0.3 μm or more and 15 μm or less. When the film thickness is within the above range, the film tends to exhibit a barrier property against injection and tends to suppress an increase in residual potential due to repeated use.
[0103] The conductive substrate may be subjected to a treatment using an acidic treatment liquid or a boehmite treatment.
[0104] The treatment based on the acidic treatment solution is implemented, for example, as follows. First, an acidic treatment solution containing phosphoric acid, chromic acid and hydrofluoric acid is prepared. The mixing ratio of phosphoric acid, chromic acid and hydrofluoric acid in the acidic treatment solution can be, for example, a range of 10 mass % to 11 mass % for phosphoric acid, a range of 3 mass % to 5 mass % for chromic acid, and a range of 0.5 mass % to 2 mass % for hydrofluoric acid, and the overall concentration of these acids can be in the range of 13.5 mass % to 18 mass %. The treatment temperature is, for example, preferably 42° C. to 48° C. The film thickness of the coating is preferably 0.3 μm to 15 μm.
[0105] The boehmite treatment is carried out, for example, by immersing in pure water at 90°C to 100°C for 5 to 60 minutes or contacting with heated steam at 90°C to 120°C for 5 to 60 minutes. The film thickness of the coating is preferably 0.1 μm to 5 μm. It can also be further anodized using an electrolyte solution with low coating solubility such as adipic acid, boric acid, borate, phosphate, phthalate, maleate, benzoate, tartrate, citrate, etc.
[0106] (Base coating)
[0107] The undercoat layer is, for example, a layer containing inorganic particles and a binding resin.
[0108] Examples of inorganic particles include particles having a powder resistance (volume resistivity) of 10 2 Ωcm or more 10 11 Inorganic particles below Ωcm.
[0109] Among these, examples of the inorganic particles having the above resistance value include metal oxide particles such as tin oxide particles, titanium oxide particles, zinc oxide particles, and zirconium oxide particles, and zinc oxide particles are particularly preferred.
[0110] The specific surface area of the inorganic particles based on the BET method can be, for example, 10 m 2 / g or above.
[0111] The volume average particle size of the inorganic particles can be, for example, 50 nm to 2000 nm (preferably 60 nm to 1000 nm).
[0112] The content of the inorganic particles is, for example, preferably from 10% by mass to 80% by mass, and more preferably from 40% by mass to 80% by mass, based on the binder resin.
[0113] The inorganic particles may be subjected to a surface treatment. Among the inorganic particles, two or more kinds of inorganic particles having different surface treatments or inorganic particles having different particle sizes may be mixed and used.
[0114] Examples of the surface treatment agent include silane coupling agents, titanate coupling agents, aluminum coupling agents, surfactants, etc. Among them, silane coupling agents are preferred, and silane coupling agents having an amino group are more preferred.
[0115] Examples of the silane coupling agent having an amino group include, but are not limited to, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, and N,N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane.
[0116] Silane coupling agents can be used in combination of two or more. For example, a silane coupling agent having an amino group can be used in combination with other silane coupling agents. As other silane coupling agents, for example, vinyl trimethoxysilane, 3-methacryloxypropyl-tris(2-methoxyethoxy)silane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, vinyl triacetoxysilane, 3-mercaptopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N,N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, etc. can be cited, but are not limited to these.
[0117] The surface treatment method using the surface treatment agent may be any method as long as it is a known method, and may be either a dry method or a wet method.
[0118] The treatment amount of the surface treatment agent is preferably, for example, 0.5% by mass or more and 10% by mass or less relative to the inorganic particles.
[0119] Here, from the viewpoint of long-term stability of electrical characteristics and high carrier blocking properties, the undercoat layer may contain an electron accepting compound (acceptor compound) together with the inorganic particles.
[0120] As electron accepting compounds, for example, there can be mentioned: quinone compounds such as chloranil and bromoaniline; tetracyanoquinodimethane compounds; fluorenone compounds such as 2,4,7-trinitrofluorenone and 2,4,5,7-tetranitro-9-fluorenone; oxadiazole compounds such as 2-(4-biphenyl)-5-(4-tert-butylphenyl)-1,3,4-oxadiazole, 2,5-bis(4-naphthyl)-1,3,4-oxadiazole, and 2,5-bis(4-diethylaminophenyl)-1,3,4-oxadiazole; xanthone compounds; thiophene compounds; electron transporting substances such as diphenylquinone compounds such as 3,3',5,5'-tetra-tert-butyldiphenylquinone, and the like.
[0121] In particular, as the electron accepting compound, a compound having an anthraquinone structure is preferred. As the compound having an anthraquinone structure, for example, hydroxyanthraquinone compounds, aminoanthraquinone compounds, aminohydroxyanthraquinone compounds, etc. are preferred, and specifically, for example, anthraquinone, alizarin, quinizarin, anthraquinone, purpurin, etc. are preferred.
[0122] The electron accepting compound may be contained in the undercoat layer in a dispersed state together with the inorganic particles, or may be contained in the undercoat layer in a state of being attached to the surface of the inorganic particles.
[0123] Examples of a method for attaching the electron accepting compound to the surface of the inorganic particles include a dry method and a wet method.
[0124] The dry method is, for example, the following method: while the inorganic particles are stirred using a mixer with a large shear force, an electron accepting compound is directly added dropwise or an electron accepting compound dissolved in an organic solvent is added dropwise, and the electron accepting compound is sprayed together with dry air or nitrogen to attach the electron accepting compound to the surface of the inorganic particles. When the electron accepting compound is added dropwise or sprayed, it is preferably done at a temperature below the boiling point of the solvent. After the electron accepting compound is added dropwise or sprayed, it can be further calcined at more than 100°C. Regarding calcination, there is no particular restriction as long as the temperature and time are such that the electronic photographic properties can be obtained.
[0125] The wet method is, for example, the following method: while the inorganic particles are dispersed in a solvent by stirring, ultrasonic waves, a sand mill, an ultrafine grinder, a ball mill, etc., an electron accepting compound is added, and after stirring or dispersing, the solvent is removed so that the electron accepting compound is attached to the surface of the inorganic particles. The solvent removal method is, for example, filtering or distillation removal by distillation. After the solvent is removed, it can be further roasted at more than 100°C. Regarding roasting, there is no particular limitation as long as the temperature and time are such that the electronic photographic characteristics can be obtained. In the wet method, the water contained in the inorganic particles can be removed before the electron accepting compound is added. As examples thereof, a method of stirring and heating in a solvent and removing it at the same time and a method of removing it by azeotropy with a solvent can be cited.
[0126] The electron accepting compound may be attached before or after the inorganic particles are surface treated with a surface treatment agent, or the electron accepting compound may be attached and the surface treated with a surface treatment agent may be simultaneously performed.
[0127] The content of the electron accepting compound may be, for example, 0.01% by mass to 20% by mass, and preferably 0.01% by mass to 10% by mass, based on the inorganic particles.
[0128] Examples of the adhesive resin used in the primer layer include: acetal resins (e.g., polyvinyl butyral), polyvinyl alcohol resins, polyvinyl acetal resins, casein resins, polyamide resins, cellulose resins, gelatin, polyurethane resins, polyester resins, unsaturated polyester resins, methacrylic resins, acrylic resins, polyvinyl chloride resins, polyvinyl acetate resins, vinyl chloride-vinyl acetate-maleic anhydride resins, silicone resins, silicone-modified alkyd resins, urea resins, phenol resins, phenol-formaldehyde resins, melamine resins, urethane resins, alkyd resins, epoxy resins and other known polymer compounds; zirconium chelate compounds; titanium chelate compounds; aluminum chelate compounds; titanium alkoxide compounds; organic titanium compounds; silane coupling agents and other known materials.
[0129] Examples of the binder resin used in the primer layer include a charge transporting resin having a charge transporting group, and a conductive resin (for example, polyaniline).
[0130] Among these, the binding resin for the primer layer is preferably a resin that is insoluble in the coating solvent of the upper layer, and is particularly preferably a thermosetting resin such as urea resin, phenol resin, phenol-formaldehyde resin, melamine resin, urethane resin, unsaturated polyester resin, alkyd resin, epoxy resin, or a resin obtained by reacting at least one resin selected from the group consisting of polyamide resin, polyester resin, polyether resin, methacrylic resin, acrylic resin, polyvinyl alcohol resin, and polyvinyl acetal resin with a curing agent.
[0131] When two or more of these adhesive resins are used in combination, the mixing ratio thereof is set as necessary.
[0132] The undercoat layer may contain various additives in order to improve electrical characteristics, improve environmental stability, and improve image quality.
[0133] As additives, there can be mentioned known materials such as polycyclic condensed pigments, azo pigments, etc., electron transport pigments, zirconium chelate compounds, titanium chelate compounds, aluminum chelate compounds, titanium alkoxide compounds, organic titanium compounds, silane coupling agents, etc. As mentioned above, silane coupling agents are used for surface treatment of inorganic particles, but can also be further added to the primer layer as an additive.
[0134] Examples of the silane coupling agent as an additive include vinyltrimethoxysilane, 3-methacryloxypropyl-tri(2-methoxyethoxy)silane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, vinyltriacetoxysilane, 3-mercaptopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N,N-bis(2-hydroxyethyl)-3-aminopropyltriethoxysilane, and 3-chloropropyltrimethoxysilane.
[0135] Examples of the zirconium chelate compound include zirconium butoxide, zirconium ethyl acetoacetate, zirconium triethanolamine, zirconium acetylacetonate butoxide, zirconium ethyl acetoacetate butoxide, zirconium acetate, zirconium oxalate, zirconium lactate, zirconium phosphonate, zirconium octanoate, zirconium naphthenate, zirconium laurate, zirconium stearate, zirconium isostearate, zirconium methacrylate butoxide, zirconium stearate butoxide, and zirconium isostearate butoxide.
[0136] Examples of the titanium chelate compound include tetraisopropyl titanate, tetra-n-butyl titanate, butyl titanate dimer, tetra(2-ethylhexyl) titanate, titanium acetylacetonate, titanium polyacetylacetonate, titanium octylene glycollate, ammonium lactate titanium, lactate titanium, ethyl lactate titanium, triethanolamine titanium, and polyhydroxystearate titanium.
[0137] Examples of the aluminum chelate compound include aluminum isopropoxide, aluminum diisopropoxide monobutoxy, aluminum butyrate, aluminum diethylacetoacetate diisopropoxide, and aluminum tris(ethylacetoacetate).
[0138] These additives may be used alone or in the form of a mixture or polycondensate of two or more compounds.
[0139] The Vickers hardness of the primer layer may be 35 or higher.
[0140] The surface roughness (ten-point average roughness) of the undercoat layer can be adjusted to 1 / (4n) to 1 / 2 of the wavelength λ of the exposure laser used (n is the refractive index of the upper layer) in order to suppress the moiré image.
[0141] In order to adjust the surface roughness, resin particles or the like may be added to the primer layer. Examples of the resin particles include silicone resin particles and cross-linked polymethyl methacrylate resin particles. In addition, in order to adjust the surface roughness, the surface of the primer layer may be ground. Examples of the grinding method include polishing, sandblasting, wet honing, grinding, and the like.
[0142] The formation of the undercoat layer is not particularly limited and can be formed by a known formation method. For example, the undercoat layer can be formed by forming a coating film of an undercoat layer-forming coating liquid prepared by adding the above components to a solvent, drying the coating film, and heating as necessary.
[0143] Examples of the solvent used for preparing the coating solution for forming the undercoat layer include known organic solvents such as alcohol solvents, aromatic hydrocarbon solvents, halogenated hydrocarbon solvents, ketone solvents, ketone alcohol solvents, ether solvents, and ester solvents.
[0144] Specific examples of these solvents include common organic solvents such as methanol, ethanol, n-propanol, isopropanol, n-butanol, benzyl alcohol, methyl cellosolve, ethyl cellosolve, acetone, methyl ethyl ketone, cyclohexanone, methyl acetate, ethyl acetate, n-butyl acetate, dioxane, tetrahydrofuran, dichloromethane, chloroform, chlorobenzene, and toluene.
[0145] Examples of the method for dispersing the inorganic particles when preparing the coating liquid for forming an undercoat layer include known methods such as a roll mill, a ball mill, a vibration ball mill, an attritor, a sand mill, a colloid mill, and a paint shaker.
[0146] Examples of a method for applying the coating liquid for forming an undercoat layer onto a conductive substrate include common methods such as blade coating, wire bar coating, spray coating, dip coating, bead coating, air knife coating, and curtain coating.
[0147] The film thickness of the primer layer is set, for example, preferably within the range of 15 μm or more, and more preferably within the range of 20 μm or more and 50 μm or less.
[0148] (Middle layer)
[0149] Although illustration is omitted, an intermediate layer may be further provided between the undercoat layer and the photosensitive layer.
[0150] The intermediate layer is, for example, a layer containing a resin. Examples of the resin used for the intermediate layer include acetal resins (e.g., polyvinyl butyral), polyvinyl alcohol resins, polyvinyl acetal resins, casein resins, polyamide resins, cellulose resins, gelatin, polyurethane resins, polyester resins, methacrylic resins, acrylic resins, polyvinyl chloride resins, polyvinyl acetate resins, vinyl chloride-vinyl acetate-maleic anhydride resins, silicone resins, silicone-modified alkyd resins, phenol-formaldehyde resins, melamine resins and other polymer compounds.
[0151] The intermediate layer may be a layer containing an organic metal compound. Examples of the organic metal compound used for the intermediate layer include organic metal compounds containing metal atoms such as zirconium, titanium, aluminum, manganese, and silicon.
[0152] These compounds for the intermediate layer may be used alone or in the form of a mixture or polycondensate of two or more compounds.
[0153] Among these, the intermediate layer is preferably a layer containing an organic metal compound containing a zirconium atom or a silicon atom.
[0154] The formation of the intermediate layer is not particularly limited and can be performed by a known formation method, for example, by forming a coating film of an intermediate layer-forming coating liquid prepared by adding the above components to a solvent, drying the coating film, and heating as necessary to form the intermediate layer.
[0155] As a coating method for forming the intermediate layer, a common method such as a dip coating method, an extrusion coating method, a wire bar coating method, a spray coating method, a blade coating method, a knife coating method, a curtain coating method, etc. is used.
[0156] The film thickness of the intermediate layer is preferably set within a range of, for example, 0.1 μm or more and 3 μm or less. In addition, the intermediate layer may be used as a primer layer.
[0157] (Charge Generation Layer)
[0158] The charge generating layer is, for example, a layer containing a charge generating material and a binder resin. In addition, the charge generating layer may be a vapor-deposited layer of the charge generating material. The vapor-deposited layer of the charge generating material is suitable for the case where a non-interference light source such as an LED (Light Emitting Diode) or an organic EL (Electro-Luminescence) image array is used.
[0159] Examples of the charge generating material include azo pigments such as disazo and trisazo; condensed ring aromatic pigments such as dibromoanthanthrone; perylene pigments; pyrrolopyrrole pigments; phthalocyanine pigments; zinc oxide; and trigonal selenium.
[0160] Among these, in order to cope with laser exposure in the near-infrared region, metal phthalocyanine pigments or metal-free phthalocyanine pigments are preferably used as charge generating materials. Specifically, for example, hydroxygallium phthalocyanine disclosed in Japanese Patent Publication No. 5-263007, Japanese Patent Publication No. 5-279591, etc.; chlorogallium phthalocyanine disclosed in Japanese Patent Publication No. 5-98181, etc.; dichlorotin phthalocyanine disclosed in Japanese Patent Publication No. 5-140472, Japanese Patent Publication No. 5-140473, etc.; titanyl phthalocyanine disclosed in Japanese Patent Publication No. 4-189873, etc. are more preferred.
[0161] On the other hand, in order to cope with laser exposure in the near-ultraviolet region, preferred charge generating materials include condensed-ring aromatic pigments such as dibromoantanthrone; thioindigo pigments; tetraazaporphyrin compounds; zinc oxide; trigonal selenium; and disazo pigments disclosed in Japanese Patent Publication No. 2004-78147 and Japanese Patent Publication No. 2005-181992.
[0162] When using a non-interference light source such as an LED or an organic EL image array having a central wavelength of light emission between 450nm and 780nm, the above-mentioned charge generating material can also be used. However, from the aspect of resolution, when a photosensitive layer is used as a thin film of less than 20μm, the electric field intensity in the photosensitive layer increases, and it is easy to generate a charge reduction due to the injection of charges from the substrate, that is, to generate image defects called so-called black spots. This situation becomes significant when using a charge generating material that easily generates dark current in a p-type semiconductor, such as trigonal selenium and phthalocyanine pigments.
[0163] In contrast, when an n-type semiconductor such as a condensed aromatic pigment, perylene pigment, or azo pigment is used as a charge generating material, dark current is less likely to be generated, and image defects called black spots can be suppressed even when formed into a thin film. Examples of n-type charge generating materials include compounds (CG-1) to (CG-27) described in paragraphs
[0288] to
[0291] of Japanese Patent Application Laid-Open No. 2012-155282, but are not limited thereto.
[0164] The n-type was determined by using the polarity of the photocurrent flowing using the commonly used time-of-flight method, and the type in which electrons flow more easily as carriers than holes was determined as the n-type.
[0165] The binder resin used in the charge generating layer can be selected from a wide range of insulating resins. Alternatively, the binder resin can be selected from organic photoconductive polymers such as poly-N-vinylcarbazole, polyvinylanthracene, polyvinylpyrene, and polysilane.
[0166] Examples of the adhesive resin include polyvinyl butyral resin, polyarylate resin (condensation product of bisphenol and aromatic divalent carboxylic acid, etc.), polycarbonate resin, polyester resin, phenoxy resin, vinyl chloride-vinyl acetate copolymer, polyamide resin, acrylic resin, polyacrylamide resin, polyvinyl pyridine resin, cellulose resin, urethane resin, epoxy resin, casein, polyvinyl alcohol resin, polyvinyl pyrrolidone resin, etc. Here, "insulating property" means that the volume resistivity is 10 13 Ωcm or more.
[0167] These adhesive resins may be used alone or in combination of two or more.
[0168] It should be noted that the mixing ratio of the charge generating material to the binder resin is preferably within a range of 10:1 to 1:10 in terms of mass ratio.
[0169] The charge generating layer may contain other known additives.
[0170] The formation of the charge generating layer is not particularly limited, and a known formation method can be used. For example, it can be performed as follows: a coating film of a coating liquid for forming a charge generating layer is formed by adding the above-mentioned components to a solvent, the coating film is dried, and heated as needed to form a charge generating layer. It should be noted that the formation of the charge generating layer can also be performed by vapor deposition of the charge generating material. The formation of the charge generating layer based on vapor deposition is particularly suitable for the case where a condensed aromatic pigment or a perylene pigment is used as the charge generating material.
[0171] Examples of the solvent used for preparing the charge generating layer-forming coating solution include methanol, ethanol, n-propanol, n-butanol, benzyl alcohol, methyl cellosolve, ethyl cellosolve, acetone, methyl ethyl ketone, cyclohexanone, methyl acetate, n-butyl acetate, dioxane, tetrahydrofuran, dichloromethane, chloroform, chlorobenzene, toluene, etc. These solvents may be used alone or in combination of two or more.
[0172] As a method for dispersing particles (e.g., charge generating materials) in a coating liquid for forming a charge generating layer, for example, a medium disperser such as a ball mill, a vibrating ball mill, an ultrafine grinder, a sand mill, a horizontal sand mill, etc.; a medium-free disperser such as a stirring, ultrasonic disperser, a roller mill, a high-pressure homogenizer, etc. As a high-pressure homogenizer, for example, a collision method in which the dispersion liquid is dispersed by liquid-liquid collision or liquid-wall collision under high pressure; a penetration method in which the dispersion liquid is dispersed by penetrating through a fine flow path under high pressure, etc. can be cited.
[0173] In the dispersion, it is effective that the average particle size of the charge generating material in the charge generating layer forming coating liquid is 0.5 μm or less, preferably 0.3 μm or less, and more preferably 0.15 μm or less.
[0174] Examples of a method for applying the coating liquid for forming a charge generating layer onto the undercoat layer (or the intermediate layer) include common methods such as blade coating, wire rod coating, spray coating, dip coating, bead coating, air knife coating, and curtain coating.
[0175] The film thickness of the charge generating layer is set, for example, preferably within the range of 0.1 μm to 5.0 μm, more preferably within the range of 0.2 μm to 2.0 μm.
[0176] (Charge Transport Layer)
[0177] The charge transport layer is, for example, a layer containing a charge transport material and a binder resin. The charge transport layer may also be a layer containing a polymer charge transport material.
[0178] When the charge transport layer is the outermost surface layer, the charge transport layer contains fluorine-containing resin particles and an antioxidant in addition to the binder resin and the charge transport material.
[0179] It should be noted that, when other layers (such as a protective layer, etc.) are provided on the charge transport layer and the charge transport layer is not the outermost surface layer, the charge transport layer may contain at least a binding resin and a charge transport material, and may contain other additives as required. The binding resin, charge transport material and other additives are the same as when the charge transport layer is the outermost surface layer.
[0180] Next, components contained in the charge transport layer as the outermost layer will be described.
[0181] - Adhesive resin -
[0182] The adhesive resin used in the charge transport layer can include polycarbonate resin, polyester resin, polyarylate resin, methacrylic resin, acrylic resin, polyvinyl chloride resin, polyvinylidene chloride resin, polystyrene resin, polyvinyl acetate resin, styrene-butadiene copolymer, vinylidene chloride-acrylonitrile copolymer, vinyl chloride-vinyl acetate copolymer, vinyl chloride-vinyl acetate-maleic anhydride copolymer, silicone resin, silicone-modified alkyd resin, phenol-formaldehyde resin, styrene-modified alkyd resin, poly-N-vinyl carbazole, polysilane, etc. Among these, polycarbonate resin or polyarylate resin is preferred as the adhesive resin. These adhesive resins are used alone or in combination of two or more.
[0183] It should be noted that the mixing ratio of the charge transport material to the binder resin is preferably 10:1 to 1:5 in terms of mass ratio.
[0184] Here, the content of the binder resin is preferably 10% by mass to 90% by mass, more preferably 30% by mass to 90% by mass, and further preferably 50% by mass to 90% by mass, relative to the total solid content of the photosensitive layer (charge transport layer).
[0185] - Charge transport materials -
[0186] As charge transport materials, there can be cited quinone compounds such as para-benzoquinone, chloranil, bromoquinone, anthraquinone, etc.; tetracyanoquinodimethane compounds; fluorenone compounds such as 2,4,7-trinitrofluorenone; xanthone compounds; benzophenone compounds; cyanovinyl compounds; vinyl compounds and other electron transport compounds. As charge transport materials, there can also be cited hole transport compounds such as triarylamine compounds, benzidine compounds, arylalkane compounds, aryl-substituted vinyl compounds, isophenylethylene compounds, anthracene compounds, hydrazone compounds, etc. These charge transport materials can be used alone or in combination of two or more, but are not limited to these.
[0187] As the charge transport material, from the viewpoint of charge mobility, a triarylamine derivative represented by the following structural formula (a-1) and a benzidine derivative represented by the following structural formula (a-2) are preferred.
[0188] [Chemistry 1]
[0189]
[0190] In the structural formula (a-1), Ar T1,Ar T2 and Ar T3 Each independently represents: substituted or unsubstituted aryl, -C6H4-C(R T4 )=C(R T5 )(R T6 ) or -C6H4-CH=CH-CH=C(R T7 )(R T8 ). T4 , R T5 , R T6 , R T7 and R T8 Each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group.
[0191] Examples of the substituents of the above groups include halogen atoms, alkyl groups having 1 to 5 carbon atoms, and alkoxy groups having 1 to 5 carbon atoms. Examples of the substituents of the above groups include substituted amino groups substituted with alkyl groups having 1 to 3 carbon atoms.
[0192] [Chemistry 2]
[0193]
[0194] In the structural formula (a-2), R T91 and R T92 Each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 5 carbon atoms, or an alkoxy group having 1 to 5 carbon atoms. T101 , R T102 , R T111 and R T112 Each independently represents a halogen atom, an alkyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms, an amino group substituted by an alkyl group having 1 to 2 carbon atoms, a substituted or unsubstituted aryl group, -C(R T12 )=C(R T13 )(R T14 ) or -CH=CH-CH=C(R T15 )(R T16 ), R T12 , R T13 , R T14 , R T15 and R T16 Each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, or a substituted or unsubstituted aryl group. Tm1, Tm2, Tn1, and Tn2 each independently represent an integer of 0 or more and 2 or less.
[0195] Examples of the substituents of the above groups include halogen atoms, alkyl groups having 1 to 5 carbon atoms, and alkoxy groups having 1 to 5 carbon atoms. Examples of the substituents of the above groups include substituted amino groups substituted with alkyl groups having 1 to 3 carbon atoms.
[0196] Here, among the triarylamine derivatives represented by the structural formula (a-1) and the benzidine derivatives represented by the structural formula (a-2), the one having "-C6H4-CH=CH-CH=C(R T7 )(R T8 )" and triarylamine derivatives having "-CH=CH-CH=C(R T15 )(R T16 )" benzidine derivatives.
[0197] As the polymer charge transport material, known materials having charge transport properties such as poly-N-vinyl carbazole and polysilane are used. In particular, polyester-based polymer charge transport materials disclosed in Japanese Patent Publication No. 8-176293 and Japanese Patent Publication No. 8-208820 are particularly preferred. It should be noted that the polymer charge transport material can be used alone or in combination with a binding resin.
[0198] - Fluorine-containing resin particles -
[0199] Examples of the fluorine-containing resin particles include particles of a homopolymer of a fluoroolefin and particles of a copolymer of two or more fluoroolefins, that is, a copolymer of one or more fluoroolefins and a non-fluorine-containing monomer (that is, a monomer having no fluorine atom).
[0200] Examples of the fluoroolefin include perhaloolefins such as tetrafluoroethylene (TFE), perfluorovinyl ether, hexafluoropropylene (HFP), and chlorotrifluoroethylene (CTFE), and non-perfluoroolefins such as vinylidene fluoride (VdF), trifluoroethylene, and vinyl fluoride. Among these, VdF, TFE, CTFE, and HFP are preferred.
[0201] On the other hand, as non-fluorine-based monomers, for example, hydrocarbon olefins such as ethylene, propylene, and butene can be cited; alkyl vinyl ethers such as cyclohexyl vinyl ether (CHVE), ethyl vinyl ether (EVE), butyl vinyl ether, and methyl vinyl ether; alkenyl vinyl ethers such as polyoxyethylene allyl ether (POEAE) and ethyl allyl ether; organic silicon compounds having reactive α,β-unsaturated groups such as vinyl trimethoxysilane (VSi), vinyl triethoxysilane, and vinyl tri(methoxyethoxy)silane; acrylic acid esters such as methyl acrylate and ethyl acrylate; methacrylic acid esters such as methyl methacrylate and ethyl methacrylate; vinyl esters such as vinyl acetate, vinyl benzoate, and "VeoVA" (trade name, vinyl ester manufactured by Shell); etc. Among these, alkyl vinyl ethers, allyl vinyl ethers, vinyl esters, and organic silicon compounds having reactive α,β-unsaturated groups are preferred.
[0202] Among these, as fluorine-containing resin particles, particles with a high fluorination rate are preferred, and particles of polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), tetrafluoroethylene-perfluoro(alkyl vinyl ether) copolymer (PFA), ethylene-tetrafluoroethylene copolymer (ETFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE) and the like are more preferred, and particles of PTFE, FEP, and PFA are particularly preferred.
[0203] In the fluorine-containing resin particles, every 10 6 The number of carboxyl groups is 0 or more and 30 or less per carbon atom.
[0204] When the number of carboxyl groups in the fluorine-containing resin particles is within the above range, the charging performance can be improved.
[0205] The number of carboxyl groups in the fluorine-containing resin particles is preferably 0 to 20 from the viewpoint of improving the charging property.
[0206] Here, the carboxyl group of the fluorine-containing resin particles is, for example, a carboxyl group derived from a terminal carboxylic acid contained in the fluorine-containing resin particles.
[0207] Examples of methods for reducing the carboxyl group content of the fluorine-containing resin particles include: 1) not irradiating the particles during the particle production process; and 2) irradiating the particles in the absence of oxygen or at a reduced oxygen concentration.
[0208] The carboxyl group content of the fluorine-containing resin particles is measured as follows according to the description in Japanese Unexamined Patent Application Publication No. 4-20507.
[0209] The fluorine-containing resin particles were preformed using a press to produce a film with a thickness of about 0.1 mm. The produced film was subjected to infrared absorption spectrum measurement. The fluorine-containing resin particles whose carboxylic acid ends were completely fluorinated by contacting fluorine gas with the fluorine-containing resin particles were also subjected to infrared absorption spectrum measurement. The number of terminal carboxyl groups (per 10 6 number of carbon atoms) = (l×K) / t
[0210] l: absorbance
[0211] K: Correction coefficient
[0212] t: film thickness (mm)
[0213] Assume that the absorption wave number of carboxyl is 3560 cm -1 , assume the correction factor is 440.
[0214] Here, the fluorine-containing resin particles include particles obtained by irradiation with radiation (also referred to as "radiation-irradiated fluorine-containing resin particles" in this specification) and particles obtained by polymerization (also referred to as "polymerized fluorine-containing resin particles" in this specification).
[0215] The radiation-irradiated fluororesin particles (fluororesin particles obtained by irradiation) are fluororesin particles obtained by radiation polymerization and granulation, or fluororesin particles obtained by decomposing the polymerized fluororesin by radiation irradiation to reduce the molecular weight and granulate the polymerized fluororesin.
[0216] The radiation-irradiated fluorine-containing resin particles generate a large amount of carboxylic acid by irradiation with radiation in the air, and therefore also contain a large amount of carboxyl groups.
[0217] On the other hand, polymerized fluorine-containing resin particles (fluorine-containing resin particles obtained by a polymerization method) refer to fluorine-containing resin particles which are granulated while being polymerized by a suspension polymerization method, an emulsion polymerization method or the like and which are not irradiated with radiation.
[0218] The fluorine-containing resin particles may be polymerizable fluorine-containing resin particles. As described above, the polymerizable fluorine-containing resin particles are granulated while being polymerized by suspension polymerization, emulsion polymerization, or the like and are not irradiated with radiation.
[0219] Here, the production of fluorine-containing resin particles by suspension polymerization is, for example, a method in which monomers for forming fluorine-containing resins are suspended in a dispersion medium together with additives such as a polymerization initiator and a catalyst, and the polymer is granulated while polymerizing the monomers.
[0220] The production of fluorine-containing resin particles by emulsion polymerization is, for example, a method in which monomers for forming fluorine-containing resins are emulsified together with additives such as polymerization initiators and catalysts in a dispersion medium using a surfactant (i.e., an emulsifier), and then the polymer is granulated while the monomers are polymerized.
[0221] In particular, the fluorine-containing resin particles may be particles obtained without irradiation with radiation in the production process.
[0222] Among these, radiation-irradiated fluororesin particles obtained by irradiating fluororesin particles in the absence of oxygen or under conditions where the oxygen concentration is reduced may also be used.
[0223] The average particle size of the fluorine-containing resin particles is not particularly limited, but is preferably 0.2 μm or more and 4.5 μm or less, and more preferably 0.2 μm or more and 4 μm or less.
[0224] The average particle size of the fluorine-containing resin particles is a value measured by the following method.
[0225] The maximum diameter of the fluorine-containing resin particles (secondary particles formed by agglomeration of primary particles) is measured by SEM (scanning electron microscope) at a magnification of 5000 or more, and the measurement is performed on 50 particles and the average value obtained is used as the average particle size of the fluorine-containing resin particles. It should be noted that JSM-6700F manufactured by JEOL Ltd. is used as SEM, and secondary electron images with an acceleration voltage of 5 kV are observed.
[0226] From the viewpoint of dispersion stability, the specific surface area (BET specific surface area) of the fluorine-containing resin particles is preferably 5 m 2 / g above 15m 2 / g or less, more preferably 7m 2 / g above 13m 2 / g or less.
[0227] In addition, the specific surface area is a value measured by the nitrogen replacement method using a BET type specific surface area measuring instrument (manufactured by Shimadzu Corporation: FlowsoapII2300).
[0228] From the viewpoint of dispersion stability, the apparent density of the fluorine-containing resin particles is preferably from 0.2 g / ml to 0.5 g / ml, more preferably from 0.3 g / ml to 0.45 g / ml.
[0229] In addition, the apparent density is a value measured according to JIS K6891 (1995).
[0230] The melting temperature of the fluorine-containing resin particles is preferably 300°C or higher and 340°C or lower, more preferably 325°C or higher and 335°C or lower.
[0231] In addition, the melting temperature is a melting point measured according to JIS K6891 (1995).
[0232] From the perspective of improving the charging properties of the photoreceptor, the content of the fluorine-containing resin particles is preferably 5% by mass to 20% by mass, more preferably 5% by mass to 15% by mass, and further preferably 8% by mass to 10% by mass, relative to the outermost layer.
[0233] - Antioxidants -
[0234] The photoreceptor of this embodiment contains an antioxidant in the outermost layer.
[0235] Examples of the antioxidant include substances having a property of preventing or suppressing the action of oxygen on oxidizing substances present inside or on the surface of the electrophotographic photoreceptor under conditions of light, heat, discharge, or the like.
[0236] As the antioxidant, specifically, free radical inhibitors, peroxide decomposers, etc. can be cited. As the free radical inhibitor, for example, known antioxidants such as hindered phenol antioxidants, hindered amine antioxidants, diallylamine antioxidants, diallyldiamine antioxidants, and hydroquinone antioxidants can be cited. As the peroxide decomposer, known antioxidants such as organic sulfur antioxidants (for example, thioether antioxidants), phosphoric acid antioxidants, dithiocarbamate antioxidants, thiourea antioxidants, and benzimidazole antioxidants can be cited.
[0237] The antioxidant contained in the outermost surface layer has a weight loss of 40% by mass or less after heating at 150° C. for 10 minutes.
[0238] By setting the weight reduction amount of the antioxidant to be within the above range, sublimation of the antioxidant from the photosensitive layer can be suppressed.
[0239] From the viewpoint of suppressing sublimation of the antioxidant from the photosensitive layer, the weight loss of the antioxidant after heating at 150° C. for 10 minutes is preferably 0 mass % to 20 mass %, more preferably 0 mass % to 5 mass %.
[0240] The weight loss was measured by measuring the mass of the antioxidant before and after heating at 150° C. for 10 minutes, and calculating the weight loss rate.
[0241] In order to make the weight reduction of the antioxidant within the above range, it is preferable to use the antioxidant described below.
[0242] The molecular weight of the antioxidant is preferably 240 to 350, more preferably 270 to 350, and even more preferably 300 to 350.
[0243] By setting the molecular weight of the antioxidant to be within the above range, it is possible to suppress the antioxidant from sublimating from the photosensitive layer when contained in the photosensitive layer, which is preferred.
[0244] As the antioxidant, a compound having two or more benzene rings in the molecule is preferred.
[0245] The antioxidant preferably has two or more benzene rings in the molecule because sublimation of the antioxidant from the photosensitive layer when the antioxidant is contained in the photosensitive layer can be suppressed.
[0246] As the antioxidant, a hindered phenol antioxidant is preferred. A hindered phenol antioxidant is a compound having a hindered phenol ring.
[0247] In the hindered phenol antioxidant, the hindered phenol ring is, for example, a phenol ring substituted with at least one alkyl group having 4 to 8 carbon atoms (e.g., a branched alkyl group having 4 to 8 carbon atoms). More specifically, the hindered phenol ring is, for example, a phenol ring in which the ortho position of the phenolic hydroxyl group is substituted with a tertiary alkyl group (e.g., tert-butyl group).
[0248] Examples of hindered phenol antioxidants include:
[0249] 1) Antioxidants having one hindered phenol ring;
[0250] 2) an antioxidant having 2 or more but less than 4 hindered phenol rings connected by a linking group, wherein the linking group is a linking group formed by a straight-chain or branched aliphatic hydrocarbon group having a valency of 2 or more but less than 4, or a linking group in which an ester bond (-C(=O)O-) and / or an ether bond (-O-) is inserted between carbon-carbon bonds of an aliphatic hydrocarbon group having a valency of 2 or more but less than 4;
[0251] 3) An antioxidant having 2 or more but less than 4 hindered phenol rings and one benzene ring (unsubstituted or substituted by an alkyl group or the like) or an isocyanurate ring, or 2 or more but less than 4 hindered phenol rings connected to a benzene ring or an isocyanurate ring via an alkylene group; etc.
[0252] From the viewpoint of suppressing sublimation of the antioxidant from the photosensitive layer, the hindered phenol antioxidant is preferably 2) or 3) above.
[0253] Specifically, as the hindered phenol-based antioxidant, an antioxidant represented by the following formula (HP) is preferred from the viewpoint of suppressing sublimation of the antioxidant from the photosensitive layer.
[0254] [Chemistry 3]
[0255]
[0256] In the formula (HP), R H1 and R H2 Each independently represents a branched alkyl group having 4 to 8 carbon atoms.
[0257] R H3 and R H4 Each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms.
[0258] R H5 It represents an alkylene group having 1 to 10 carbon atoms.
[0259] In the formula (HP), R H1 and R H2 The alkyl group represented by the above-mentioned group includes a branched alkyl group having 4 to 8 carbon atoms (preferably 4 to 6 carbon atoms).
[0260] Specific examples of the branched alkyl group include isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, tert-pentyl, isohexyl, sec-hexyl, tert-hexyl, isoheptyl, sec-heptyl, tert-heptyl, isooctyl, sec-octyl and tert-octyl.
[0261] Among these, the alkyl group is preferably a tert-butyl group or a tert-amyl group, and more preferably a tert-butyl group.
[0262] In the formula (HP), R H3 and R H4 , examples include linear or branched alkyl groups having 1 to 10 carbon atoms (preferably 1 to 4 carbon atoms).
[0263] Specific examples of the linear alkyl group include methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decyl groups.
[0264] Specific examples of the branched alkyl group include isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, neopentyl, tert-pentyl, isohexyl, sec-hexyl, tert-hexyl, isoheptyl, sec-heptyl, tert-heptyl, isooctyl, sec-octyl, tert-octyl, isononyl, sec-nonyl, tert-nonyl, isodecyl, sec-decyl, and tert-decyl.
[0265] Among these, the alkyl group is preferably a lower alkyl group such as a methyl group or an ethyl group.
[0266] In the formula (HP), R H5 It represents a linear or branched alkylene group having 1 to 10 carbon atoms (preferably 1 to 4 carbon atoms).
[0267] Specific examples of the linear alkylene group include a methylene group, an ethylene group, a n-propylene group, a n-butylene group, a n-pentylene group, a n-hexylene group, a n-heptylene group, a n-octylene group, a n-nonylene group, and a n-decylene group.
[0268] Specific examples of the branched alkylene group include isopropylene, isobutylene, secondary butylene, tertiary butylene, isopentylene, neopentylene, tertiary pentylene, isohexylene, secondary hexylene, tertiary hexylene, isoheptylene, secondary heptylene, tertiary heptylene, isooctylene, secondary octylene, tertiary octylene, isononylene, secondary nonylene, tertiary nonylene, isodecylene, secondary decylene, and tertiary decylene.
[0269] Among these, the alkylene group is preferably a lower alkylene group such as a methylene group, an ethylene group, and a butylene group.
[0270] It should be noted that in formula (HP), R H1 , R H2 , R H3 , R H4 and R H5 Each of the above substituents includes a group further having a substituent. Examples of such substituents include halogen atoms (e.g., fluorine atoms, chlorine atoms), alkoxy groups (e.g., alkoxy groups having 1 to 4 carbon atoms), and aryl groups (e.g., phenyl groups, naphthyl groups, etc.).
[0271] In formula (HP), from the perspective of suppressing the sublimation of the antioxidant from the photosensitive layer, R H1 and R H2 represents tert-butyl, more preferably R H1 and R H2 Represents tert-butyl, R H3 and R H4 represents an alkyl group having 1 to 3 carbon atoms (especially a methyl group), R H5 It represents an alkylene group having 1 to 4 carbon atoms (particularly a methylene group).
[0272] Specifically, the hindered phenol antioxidant is particularly preferably a hindered phenol antioxidant represented by the exemplary compound (HP-3).
[0273] Specific examples of the hindered phenol-based antioxidant are shown below, but the present invention is not limited thereto.
[0274] [Chemistry 4]
[0275]
[0276] [Chemistry 5]
[0277]
[0278] The hindered phenol antioxidant may be used alone or in combination of two or more.
[0279] From the viewpoint of suppressing sublimation of the antioxidant from the photosensitive layer, the content of the antioxidant is preferably 20 mass % to 60 mass %, and preferably 30 mass % to 50 mass %, based on the content of the fluorine-containing resin particles.
[0280] -Additives, Formation Methods and Film Thickness-
[0281] The charge transport layer may contain other known additives.
[0282] The charge transport layer can be formed by any known method without particular limitation. For example, the charge transport layer can be formed by forming a coating film of a charge transport layer-forming coating liquid prepared by adding the above components to a solvent, drying the coating film, and heating as necessary.
[0283] As the solvent for preparing the coating solution for forming the charge transport layer, there can be mentioned aromatic hydrocarbons such as benzene, toluene, xylene, and chlorobenzene; ketones such as acetone and 2-butanone; halogenated aliphatic hydrocarbons such as dichloromethane, chloroform, and vinyl chloride; cyclic or linear ethers such as tetrahydrofuran and diethyl ether, and other common organic solvents. These solvents can be used alone or in combination of two or more.
[0284] Examples of a coating method for coating the charge transport layer-forming coating liquid on the charge generating layer include common methods such as blade coating, wire bar coating, spray coating, dip coating, bead coating, air knife coating, and curtain coating.
[0285] The film thickness of the charge transport layer is set, for example, preferably within the range of 5 μm to 50 μm, more preferably within the range of 10 μm to 30 μm.
[0286] (Protective layer)
[0287] The protective layer is provided on the photosensitive layer as required. The protective layer is provided, for example, to prevent chemical changes in the photosensitive layer during charging or to further improve the mechanical strength of the photosensitive layer.
[0288] Therefore, the protective layer may be a layer composed of a cured film (crosslinked film). Examples of these layers include the layers described in the following 1) or 2).
[0289] 1) A layer consisting of a cured film of a composition comprising a reactive group-containing charge transport material having a reactive group and a charge transport skeleton in the same molecule (i.e., a layer comprising a polymer or a crosslinked body of the reactive group-containing charge transport material)
[0290] 2) A layer composed of a cured film of a composition comprising a non-reactive charge transport material and a reactive group-containing non-charge transport material having no charge transport skeleton but having a reactive group (i.e., a layer comprising a non-reactive charge transport material and a polymer or a crosslinked body of the reactive group-containing non-charge transport material)
[0291] Examples of the reactive group of the reactive group-containing charge transport material include chain polymerizable groups, epoxy groups, -OH, -OR [wherein R represents an alkyl group], -NH2, -SH, -COOH, -SiR Q1 3-Qn (OR Q2 ) Qn [Among them, R Q1 represents a hydrogen atom, an alkyl group, or a substituted or unsubstituted aryl group, R Q2 represents a hydrogen atom, an alkyl group, a trialkylsilyl group, Qn represents an integer of 1 to 3] and the like.
[0292] As the chain polymerizable group, there is no particular limitation as long as it is a functional group that can be subjected to free radical polymerization, and for example, it is a functional group having a group containing at least a carbon double bond. Specifically, it can be mentioned: a group containing at least one selected from a vinyl group, a vinyl ether group, a vinyl sulfide group, a styryl group (vinyl phenyl group), an acryloyl group, a methacryloyl group, and derivatives thereof. Among them, for the reason of its excellent reactivity, as the chain polymerizable group, it is preferably a group containing at least one selected from a vinyl group, a styryl group (vinyl phenyl group), an acryloyl group, a methacryloyl group, and derivatives thereof.
[0293] The charge transport skeleton of the reactive group-containing charge transport material is not particularly limited as long as it is a known structure in an electrophotographic photoreceptor, and examples thereof include a structure in which the skeleton is derived from a nitrogen-containing hole transport compound such as a triarylamine compound, a benzidine compound, a hydrazone compound, and is conjugated with a nitrogen atom. Among these, a triarylamine skeleton is preferred.
[0294] The reactive group-containing charge transport material, the non-reactive charge transport material, and the reactive group-containing non-charge transport material having a reactive group and a charge transport skeleton may be selected from known materials.
[0295] The protective layer may contain other known additives.
[0296] The protective layer can be formed by any known method without particular limitation. For example, the protective layer can be formed by forming a coating film of a protective layer-forming coating liquid prepared by adding the above components to a solvent, drying the coating film, and performing a curing treatment such as heating as required.
[0297] Examples of the solvent used to prepare the protective layer-forming coating solution include aromatic solvents such as toluene and xylene; ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ester solvents such as ethyl acetate and butyl acetate; ether solvents such as tetrahydrofuran and dioxane; cellosolve solvents such as ethylene glycol monomethyl ether; alcohol solvents such as isopropyl alcohol and butanol, etc. These solvents may be used alone or in combination of two or more.
[0298] In addition, the coating liquid for forming a protective layer may be a solvent-free coating liquid.
[0299] Examples of a method for applying the protective layer-forming coating liquid onto a photosensitive layer (e.g., a charge transport layer) include common methods such as dip coating, extrusion coating, wire rod coating, spray coating, blade coating, knife coating, and curtain coating.
[0300] The film thickness of the protective layer is set, for example, preferably within the range of 1 μm to 20 μm, more preferably within the range of 2 μm to 10 μm.
[0301] (Single-layer photosensitive layer)
[0302] The single-layer photosensitive layer (charge generation / charge transport layer) is, for example, a layer containing a charge generation material and a charge transport material and, if necessary, a binding resin and other known additives. It should be noted that these materials are the same as those described for the charge generation layer and the charge transport layer.
[0303] Furthermore, in the single-layer photosensitive layer, the content of the charge generating material can be 0.1% by mass to 10% by mass, preferably 0.8% by mass to 5% by mass, relative to the total solid content. In addition, in the single-layer photosensitive layer, the content of the charge transport material can be 5% by mass to 50% by mass, relative to the total solid content.
[0304] The method for forming the single-layer photosensitive layer is the same as the method for forming the charge generating layer and the charge transporting layer.
[0305] The film thickness of the single-layer photosensitive layer may be, for example, 5 μm to 50 μm, and preferably 10 μm to 40 μm.
[0306] (Difference in charging potential △VH)
[0307] The photosensitive body of the present embodiment is assembled in a photosensitive body electrical characteristics evaluation device equipped with a charging device, an exposure device and a static elimination device. The charging potential after performing a series of processes of charging, exposure and static elimination for one cycle under the following conditions and charging again is set to VH1. The charging potential after performing the above processes for 100 cycles under the following conditions and charging again is set to VH2. At this time, the absolute value of the difference △VH between the above VH1 and the above VH2 is less than 5V.
[0308] The photoreceptor of this embodiment has the above-mentioned structure, and can suppress the sublimation of the antioxidant from the photosensitive layer.
[0309] In order to make the absolute value of the difference ΔVH of the charging potential fall within the above range, the outermost surface layer of the photoreceptor preferably contains: the number of carboxyl groups contained is 10 6 Fluorine-containing resin particles having a carbon number of 0 to 30; and an antioxidant having a weight loss of 40% by mass or less after heating at 150° C. for 10 minutes.
[0310] From the viewpoint of improving the initial chargeability of the photoreceptor and the charge maintenance property during repeated use, the absolute value of the difference ΔVH between VH1 and VH2 is more preferably 4 V or less, and further preferably 3.5 V or less.
[0311] The absolute value of the difference ΔVH in the charging potential of the photoreceptor is measured as follows.
[0312] The photoreceptor was assembled in a photoreceptor electrical characteristics evaluation device manufactured by Fuji Xerox Co., Ltd., which was equipped with a charging device, an exposure device, and a static elimination device. After a series of steps of charging, exposure, and static elimination were performed for one cycle under the following conditions, charging was further performed, and the charge potential on the surface of the photoreceptor was measured, and the potential value was taken as VH1. Next, after a series of steps of charging, exposure, and static elimination were performed for a total of 100 cycles under the following conditions, charging was further performed, and the charge potential on the surface of the photoreceptor was measured, and the potential value was taken as VH2, and the absolute value of the difference △VH between the above VH1 and the above VH2 was calculated.
[0313] In addition, regarding the measurement of the charge potential of the photoreceptor surface, a surface potentiometer (manufactured by Trek, Trek334) was used to measure the charge potential at a position 1 mm away from the photoreceptor surface.
[0314] (condition)
[0315] ·Measurement environment: Temperature 20℃ / Humidity 40%RH
[0316] Charging potential: +600V
[0317] Exposure light: 10mJ / m2
[0318] Exposure wavelength: 780nm
[0319] · Anti-static light source: Halogen lamp (manufactured by Hayashi Watch Industry Co., Ltd.)
[0320] ·Electrostatic light wavelength: above 600nm and below 800nm
[0321] · Anti-static light intensity: 30mJ / m 2
[0322] ·Photoreceptor rotation speed: 66.7rpm
[0323] <Image Forming Apparatus (and Process Cartridge)>
[0324] The image forming apparatus of the present embodiment comprises: an electrophotographic photoreceptor; a charging mechanism for charging the surface of the electrophotographic photoreceptor; an electrostatic latent image forming mechanism for forming an electrostatic latent image on the surface of the charged electrophotographic photoreceptor; a developing mechanism for developing the electrostatic latent image formed on the surface of the electrophotographic photoreceptor with a developer containing a toner to form a toner image; and a transfer mechanism for transferring the toner image to the surface of a recording medium. In addition, as the electrophotographic photoreceptor, the electrophotographic photoreceptor of the present embodiment described above is applied.
[0325] The image forming device of this embodiment can apply the following well-known image forming devices: a device equipped with a fixing mechanism for fixing the toner image transferred to the surface of a recording medium; a device for a direct transfer method for directly transferring the toner image formed on the surface of an electrophotographic photosensitive body to a recording medium; a device for an intermediate transfer method for transferring the toner image formed on the surface of an electrophotographic photosensitive body once to the surface of an intermediate transfer body, and then transferring the toner image transferred to the surface of the intermediate transfer body to the surface of a recording medium for a second time; a device equipped with a cleaning mechanism for cleaning the surface of an electrophotographic photosensitive body after the toner image is transferred but before charging; a device equipped with a de-staticizing mechanism for de-staticizing the surface of an electrophotographic photosensitive body by irradiating de-staticizing light to the surface of an electrophotographic photosensitive body after the toner image is transferred but before charging; a device equipped with an electrophotographic photosensitive body heating component for increasing the temperature of the electrophotographic photosensitive body and lowering the relative temperature; and the like.
[0326] In the case of an intermediate transfer type device, the transfer mechanism, for example, comprises an intermediate transfer body for transferring a toner image on a surface, a primary transfer mechanism for transferring a toner image formed on a surface of an electronic photographic photosensitive body to a surface of the intermediate transfer body, and a secondary transfer mechanism for secondary transferring the toner image transferred to the surface of the intermediate transfer body to a surface of a recording medium.
[0327] The image forming apparatus of the present embodiment may be any of a dry developing system image forming apparatus and a wet developing system (development system using a liquid developer) image forming apparatus.
[0328] It should be noted that, in the image forming apparatus of the present embodiment, for example, the portion having the electrophotographic photoreceptor may be a box structure (processing box) that can be loaded and unloaded relative to the image forming apparatus. As the processing box, for example, a processing box having the electrophotographic photoreceptor of the present embodiment is suitable for use. It should be noted that, in addition to the electrophotographic photoreceptor, the processing box may also have, for example, at least one selected from the group consisting of a charging mechanism, an electrostatic latent image forming mechanism, a developing mechanism, and a transfer mechanism.
[0329] An example of the image forming apparatus according to the present embodiment is shown below, but the present invention is not limited thereto. It should be noted that the main parts shown in the drawings will be described, and the description of other parts will be omitted.
[0330] Figure 2 This is a schematic structural diagram showing an example of the image forming apparatus according to the present embodiment.
[0331] like Figure 2 As shown, the image forming apparatus 100 of the present embodiment includes: a process box 300 including an electrophotographic photoreceptor 7; an exposure device 9 (an example of an electrostatic latent image forming mechanism); a transfer device 40 (a primary transfer device); and an intermediate transfer body 50. It should be noted that in the image forming apparatus 100, the exposure device 9 is arranged at a position where the electrophotographic photoreceptor 7 can be exposed through the opening of the process box 300, and the transfer device 40 is arranged at a position opposite to the electrophotographic photoreceptor 7 across the intermediate transfer body 50, and the intermediate transfer body 50 is arranged so that a part of it contacts the electrophotographic photoreceptor 7. Although not shown in the figure, there is also a secondary transfer device for transferring the toner image transferred to the intermediate transfer body 50 to a recording medium (e.g., paper). It should be noted that the intermediate transfer body 50, the transfer device 40 (a primary transfer device), and the secondary transfer device (not shown) are equivalent to an example of a transfer mechanism.
[0332] Figure 2 The process box 300 in the embodiment integrally supports the electrophotographic photoreceptor 7, the charging device 8 (an example of a charging mechanism), the developing device 11 (an example of a developing mechanism), and the cleaning device 13 (an example of a cleaning mechanism) in a housing. The cleaning device 13 has a cleaning blade (an example of a cleaning member) 131, and the cleaning blade 131 is configured to contact the surface of the electrophotographic photoreceptor 7. It should be noted that the cleaning member may be a conductive or insulating fibrous member other than the cleaning blade 131, and may be used alone or in combination with the cleaning blade 131.
[0333] It should be noted that Figure 2 In the example, the image forming apparatus includes a fibrous member 132 (rolled) for supplying the lubricant 14 to the surface of the electrophotographic photoreceptor 7 and a fibrous member 133 (flat brush) for assisting cleaning, but these members are arranged as needed.
[0334] Next, each structure of the image forming apparatus according to this embodiment will be described.
[0335] -Charging device-
[0336] As the charging device 8, for example, a contact charger using a conductive or semi-conductive charging roller, a charging brush, a charging film, a charging rubber blade, a charging tube, etc. can be used. In addition, a non-contact roller charger, a scorotron charger using corona discharge, a corotron charger, or other known chargers can also be used.
[0337] -Exposure device-
[0338] As the exposure device 9, for example, an optical device that uses semiconductor laser, LED light, liquid crystal shutter light and other light to expose the surface of the electrophotographic photoreceptor 7 according to a predetermined image can be cited. The wavelength of the light source is set to be within the spectral sensitivity area of the electrophotographic photoreceptor. As the wavelength of the semiconductor laser, near-infrared with an oscillation wavelength near 780nm is the mainstream. However, it is not limited to this wavelength, and a laser with an oscillation wavelength of approximately 600nm or a laser with an oscillation wavelength of more than 400nm and less than 450nm as a blue laser can also be used. In addition, in order to form a color image, a surface-emitting laser source that can output a multi-beam type is also effective.
[0339] -Developing device-
[0340] As the developing device 11, for example, a common developing device that performs development in contact with or without contact with a developer can be cited. As the developing device 11, there is no particular limitation as long as it has the above-mentioned function, and it can be selected according to the purpose. For example, a known developer having a function of attaching a single-component developer or a two-component developer to the electrophotographic photoreceptor 7 using a brush, a roller, etc. can be cited. Among them, it is preferable to use a developing roller having a developer retained on the surface.
[0341] The developer used in the developing device 11 may be a one-component developer containing only a toner or a two-component developer containing a toner and a carrier. The developer may be magnetic or non-magnetic. These developers may be known developers.
[0342] -Cleaning device-
[0343] The cleaning device 13 is a cleaning blade type device including a cleaning blade 131 .
[0344] Here, a member constituting a region including a portion of the cleaning blade 131 that contacts the electrophotographic photoreceptor 7 is referred to as a “contact member”.
[0345] In the cleaning blade 131, when the contact member and the region other than the contact member are made of different materials, the region other than the contact member is referred to as a "non-contact member". The non-contact member may be made of one material or two or more members of different materials.
[0346] It should be noted that the cleaning blade 131 of the present embodiment may be composed only of the above-mentioned contact member.
[0347] In the cleaning blade 131 , at least the portion (ie, the contact member) that contacts the electrophotographic photoreceptor 7 is preferably made of a member containing polyurethane rubber and having an endothermic peak top temperature in the range of 180° C. to 220° C. as measured by differential scanning calorimetry.
[0348] By making at least the contact part of the cleaning blade 131 contain polyurethane rubber and the endothermic peak temperature measured by differential scanning calorimetry within the above range, the polyurethane can be appropriately given high crystallinity, thereby improving the wear resistance of the cleaning blade. As a result, even if the antioxidant on the surface layer side of the photoreceptor sublimates, the antioxidant can be kept on the surface side of the photoreceptor because the surface of the photoreceptor is moderately worn due to contact with the cleaning blade, which is preferred.
[0349] The lower limit of the endothermic peak top temperature (melting temperature) is more preferably 185° C. or higher, and further preferably 190° C. or higher. The upper limit of the endothermic peak top temperature (melting temperature) is more preferably 215° C. or lower, and further preferably 210° C. or lower.
[0350] The endothermic peak top temperature of the cleaning blade 131 is measured in accordance with ASTM D2418-99.
[0351] The measurement was performed using Diamond-DSC manufactured by Perkin Elmer. The melting temperatures of indium and zinc were used for temperature correction of the device detection unit, and the heat of fusion of indium was used for heat correction. An aluminum pan was used as the measurement sample, and an empty pan was set as a reference for measurement. At this time, the heating rate during DSC measurement was set to 3°C / min, and the measurement temperature range was set to 20°C to 250°C.
[0352] As a method for controlling the endothermic peak temperature within the above range, for example, a method for further growing the hard segment aggregates in the polyurethane can be cited. Specifically, when the cross-linked structure in the polyurethane is formed, it is adjusted in a manner that physical cross-linking (cross-linking of hard segments with each other through hydrogen bonds) is more effective than chemical cross-linking (cross-linking through a cross-linking agent), thereby creating an environment in which the hard segment aggregates are more likely to grow. It should be noted that when the polyurethane is polymerized, the lower the polymerization temperature is set, the longer the aging time becomes, and as a result, there is a tendency for more physical cross-linking to be performed.
[0353] Here, the "hard segment" refers to a relatively harder material in the polyurethane rubber material. On the other hand, the "soft segment" refers to a relatively softer material in the polyurethane rubber material.
[0354] Polyurethane rubber is usually synthesized by polymerizing polyisocyanate and polyol. In addition, in addition to polyol, resins having functional groups that can react with isocyanate groups can also be used. It should be noted that polyurethane rubber preferably has a hard segment and a soft segment.
[0355] The combination of the material constituting the hard segment (hard segment material) and the material constituting the soft segment (soft segment material) is not particularly limited, and can be selected from known resin materials in such a way that one is relatively harder than the other and the other is relatively softer than the one. In the present embodiment, the following combination is suitable.
[0356] Soft segment materials
[0357] First, regarding the soft segment material, as polyols, polyester polyols obtained by dehydration condensation of diols and dibasic acids, polycarbonate polyols obtained by reaction of diols and alkyl carbonates, polycaprolactone polyols, polyether polyols, etc. It should be noted that commercial products of the above-mentioned polyols used as soft segment materials include, for example, PRAXCELL 205 and PRAXCELL 240 manufactured by Daicel.
[0358] Hard segment materials
[0359] In addition, as a hard segment material, a resin having a functional group that can react with an isocyanate group is preferably used. In addition, a resin having flexibility is preferred, and from the aspect of flexibility, an aliphatic resin having a straight-chain structure is more preferred. As a specific example, an acrylic resin containing two or more hydroxyl groups, a polybutadiene resin containing two or more hydroxyl groups, an epoxy resin having two or more epoxy groups, etc. are preferably used.
[0360] When using hard segment materials and soft segment materials, the mass ratio of the material constituting the hard segment relative to the total amount of the hard segment material and the soft segment material (hereinafter referred to as the "hard segment material ratio") is preferably in the range of 10 mass % to 30 mass %, more preferably in the range of 13 mass % to 23 mass %, and further preferably in the range of 15 mass % to 20 mass %.
[0361] By making the hard segment material ratio more than 10 mass %, wear resistance and good long-term maintenance of cleanliness can be obtained. On the other hand, by making the hard segment material ratio less than 30 mass %, flexibility and expansibility can be obtained without excessive hardening, the generation of notches can be suppressed, and good long-term maintenance of cleanliness can be achieved.
[0362] Polyisocyanate
[0363] Examples of the polyisocyanate used for synthesis of the polyurethane rubber include 4,4′-diphenylmethane diisocyanate (MDI), 2,6-toluene diisocyanate (TDI), 1,6-hexane diisocyanate (HDI), 1,5-naphthalene diisocyanate (NDI), and 3,3-dimethylphenyl-4,4-diisocyanate (TODI).
[0364] In addition, from the viewpoint of easily forming hard segment aggregates of a desired size (particle diameter), as the polyisocyanate, 4,4′-diphenylmethane diisocyanate (MDI), 1,5-naphthalene diisocyanate (NDI), and hexamethylene diisocyanate (HDI) are more preferred.
[0365] The amount of the polyisocyanate mixed is preferably 20 to 40 parts by mass, more preferably 20 to 35 parts by mass, and even more preferably 20 to 30 parts by mass, relative to 100 parts by mass of the resin having a functional group reactive with an isocyanate group.
[0366] By making the mixing amount 20 parts by mass or more, the amount of urethane bonding can be ensured to be large, so that the hard segment grows and the required hardness is obtained. On the other hand, by making it 40 parts by mass or less, the hard segment does not become too large, and expandability can be obtained, thereby suppressing the generation of notches in the cleaning blade.
[0367] Cross-linking agent
[0368] As the crosslinking agent, diol (2-functional), triol (3-functional), tetraol (4-functional) and the like can be mentioned, and they can be used in combination. In addition, amine compounds can also be used as crosslinking agents. It should be noted that it is preferred to use a crosslinking agent with more than 3 functions for crosslinking. As a trifunctional crosslinking agent, for example, trimethylolpropane, glycerol, triisopropanolamine and the like can be mentioned.
[0369] The mixing amount of the crosslinking agent is preferably 2 parts by mass or less relative to 100 parts by mass of the resin having a functional group reactive with an isocyanate group. By setting the mixing amount to 2 parts by mass or less, the molecular motion is not restricted by chemical crosslinking, and the hard segment derived from the urethane bond grows significantly by aging, making it easy to obtain the required hardness.
[0370] ·Production method of polyurethane rubber
[0371] The polyurethane rubber member constituting the contact member in this embodiment is manufactured by common polyurethane manufacturing methods such as the prepolymer method and the one-step method. The prepolymer method can obtain polyurethane with excellent strength and wear resistance, so it is suitable for this embodiment, but it is not limited to the manufacturing method.
[0372] It should be noted that as a means for controlling the endothermic peak top temperature (melting temperature) in the contact member within the above range, there can be cited a method of increasing the crystallinity of the polyurethane member while controlling it within an appropriate range, for example, a method of further growing the hard segment aggregates in the polyurethane. Specifically, there can be cited an adjustment such that when the crosslinked structure in the polyurethane is formed, physical crosslinking (crosslinking between hard segments based on hydrogen bonds) is more effectively performed than chemical crosslinking (crosslinking based on a crosslinking agent), and when the polyurethane is polymerized, the lower the polymerization temperature is set, the longer the aging time becomes, and as a result, there is a tendency for more physical crosslinking to be performed.
[0373] The polyurethane rubber part is molded by mixing an isocyanate compound, a crosslinking agent and the like with the above-mentioned polyol, and molding under molding conditions that can suppress uneven molecular arrangement.
[0374] Specifically, when preparing the polyurethane composition, the crosslinking is delayed by lowering the temperature of the polyol or prepolymer or lowering the curing / molding temperature. By setting these temperatures (polyol or prepolymer temperature, curing / molding temperature) to a low level to reduce reactivity, the urethane bonded portion can be aggregated to obtain a hard segment crystal, so the temperature can be adjusted so that the particle size of the hard segment aggregate reaches the desired crystal size.
[0375] Thus, a polyurethane rubber part can be molded in which the molecules contained in the polyurethane composition are arranged side by side and which includes a crystal having an endothermic peak top temperature of crystal melting energy within the above range when measured by DSC.
[0376] The amounts of the polyol, polyisocyanate and cross-linking agent, the ratio of the cross-linking agent and the like are adjusted to fall within a desired range.
[0377] In the molding of the cleaning blade, the cleaning blade-forming composition prepared by the above method is formed into a sheet by centrifugal molding, extrusion molding, etc., and then cut to produce a cleaning blade.
[0378] The weight average molecular weight of the polyurethane rubber member in the present embodiment is preferably within a range of 1,000 to 4,000, and more preferably within a range of 1,500 to 3,500.
[0379] (Non-contact parts)
[0380] The non-contact member in the cleaning blade of the present embodiment can be made of any known material without particular limitation.
[0381] As the material used in the non-contact component, for example, polyurethane rubber, silicone rubber, fluororubber, chloroprene rubber, butadiene rubber, etc. can be cited. Among these, polyurethane rubber is preferred. As polyurethane rubber, ester polyurethane and ether polyurethane can be cited, and ester polyurethane is particularly preferred.
[0382] In addition, when manufacturing polyurethane rubber, there is a method using polyol and polyisocyanate.
[0383] Examples of the polyol include polytetramethyl ether glycol, polyethylene adipate, and polycaprolactone.
[0384] Examples of the polyisocyanate include 2,6-toluene diisocyanate (TDI), 4,4′-diphenylmethane diisocyanate (MDI), p-phenylene diisocyanate (PPDI), 1,5-naphthalene diisocyanate (NDI), and 3,3-dimethyldiphenyl-4,4′-diisocyanate (TODI). Among them, MDI is preferred.
[0385] Furthermore, examples of the curing agent for curing polyurethane include curing agents such as 1,4-butanediol, trimethylolpropane, ethylene glycol, and mixtures thereof.
[0386] As a specific example, it is preferable to use a prepolymer (the prepolymer is produced by mixing diphenylmethane-4,4-diisocyanate into dehydrated polytetramethyl ether glycol and reacting them) with 1,4-butanediol and trimethylolpropane as a curing agent. It should be noted that additives such as a reaction regulator may also be added.
[0387] The non-contact component is produced by a conventionally known method, such as centrifugal molding, extrusion molding, etc., according to the raw materials used in the production, and cut into a predetermined shape, etc., thereby producing the component.
[0388] (Manufacture of cleaning blades)
[0389] In the case where the cleaning scraper includes a contact component and a non-contact component, the first layer as the contact component and the second layer as the non-contact component (in the case of a layer structure of more than three layers, two or more layers) are bonded to each other to produce the cleaning scraper. As the above bonding method, double-sided tape, various adhesives, etc. are preferably used. In addition, a time difference can be set during molding so that the materials of each layer flow into the mold, and two or more layers can be bonded by bonding between the materials without setting an adhesive layer.
[0390] It should be noted that in addition to the cleaning blade method, a brush cleaning method and a simultaneous development and cleaning method may also be used.
[0391] -Transfer device-
[0392] Examples of the transfer device 40 include known transfer chargers such as a contact transfer charger using a belt, a roller, a film, a rubber blade, or the like, a scorotron transfer charger using corona discharge, and a corona transfer charger.
[0393] -Intermediate transfer body-
[0394] A belt-shaped transfer body (intermediate transfer belt) made of polyimide, polyamideimide, polycarbonate, polyarylate, polyester, rubber, etc. imparted with semiconductivity is used as the intermediate transfer body 50. In addition, a drum-shaped transfer body can be used as the intermediate transfer body in addition to a belt-shaped transfer body.
[0395] Figure 3 This is a schematic structural diagram showing another example of the image forming apparatus according to the present embodiment.
[0396] Figure 3 The image forming apparatus 120 shown is a multi-color image forming apparatus of a tandem type equipped with four process cartridges 300. In the image forming apparatus 120, the four process cartridges 300 are arranged in parallel on the intermediate transfer body 50, and a configuration is formed in which one electrophotographic photoreceptor is used for each color. It should be noted that the image forming apparatus 120 has the same configuration as the image forming apparatus 100 except that it is a tandem type.
[0397] [Example]
[0398] The following examples are described, but the present invention is not limited to the following examples. It should be noted that in the following description, "parts" and "%" are all based on mass unless otherwise specified.
[0399] <Production of fluorine-containing resin particles>
[0400] (Production of fluorine-containing resin particles (1))
[0401] The fluorine-containing resin particles (1) were produced as follows.
[0402] 3 liters of deionized water, 3.0 g of ammonium perfluorooctanoate, and 110 g of solid paraffin (manufactured by Nippon Oil Corporation) as an emulsion stabilizer were added to the autoclave, and the system was replaced with nitrogen three times and TFE (tetrafluoroethylene) twice to remove oxygen. Then, the internal pressure was set to 1.0 MPa using TFE, and the internal temperature was maintained at 70°C while stirring at 250 rpm. Then, 150 cc of ethane (as a chain transfer agent) and 20 ml of an aqueous solution containing 300 mg of ammonium persulfate (as a polymerization initiator) were added to the system to initiate the reaction. During the reaction, the temperature in the system was maintained at 70°C, and TFE was continuously supplied in such a manner that the internal pressure of the autoclave was always maintained at 1.0 ± 0.05 MPa. After the initiator was added, the supply and stirring of TFE were stopped when the TFE consumed in the reaction reached 1000 g, and the reaction was terminated. The particles were then separated by centrifugation, and 400 parts by mass of methanol were collected and washed with a stirrer at 250 rpm for 10 minutes while irradiating with ultrasonic waves, and the supernatant was filtered out. This operation was repeated three times, and the filtrate was dried at 60° C. for 17 hours under reduced pressure.
[0403] Through the above steps, fluorine-containing resin particles (1) are produced.
[0404] (Production of fluorine-containing resin particles (C1))
[0405] The fluorine-containing resin particles (C1) were produced as follows.
[0406] 100 parts by mass of commercially available homopolytetrafluoroethylene fine powder (standard specific gravity 2.175 measured according to ASTM D 4895 (2004)) and 2.4 parts by mass of ethanol as an additive were added to a bag made of barrier nylon. The bag was then irradiated with 150 kGy of cobalt-60 gamma rays in air at room temperature to obtain a low molecular weight polytetrafluoroethylene powder. The obtained powder was crushed to obtain fluorine-containing resin particles (C1).
[0407] <Manufacturing of cleaning blade>
[0408] (Manufacture of cleaning blade (1))
[0409] A cleaning blade (1) was manufactured as follows.
[0410] First, polycaprolactone polyol (manufactured by Daicel, PRAXCELL 205, average molecular weight 529, hydroxyl value 212KOHmg / g) and polycaprolactone polyol (manufactured by Daicel, PRAXCELL 240, average molecular weight 4155, hydroxyl value 27KOHmg / g) were used as soft segment materials of the polyol component. In addition, an acrylic resin containing two or more hydroxyl groups (manufactured by Soken Chemical Co., Ltd., ACTFLOWUMB-2005B) was used as a hard segment material, and the soft segment material and the hard segment material were mixed at a ratio of 8:2 (mass ratio).
[0411] Next, 6.26 parts of 4,4'-diphenylmethane diisocyanate (Millionate MT manufactured by Nippon Polyurethane Industry Co., Ltd.) as an isocyanate compound was added to 100 parts of the mixture of the soft segment material and the hard segment material, and the mixture was reacted at 70°C for 3 hours under a nitrogen atmosphere. It should be noted that the amount of the isocyanate compound used in the reaction was selected so that the ratio of the isocyanate group to the hydroxyl group contained in the reaction system (isocyanate group / hydroxyl group) was 0.5.
[0412] Next, 34.3 parts of the isocyanate compound was further added, and the mixture was reacted at 70° C. for 3 hours under a nitrogen atmosphere to obtain a prepolymer. The total amount of the isocyanate compound used in the preparation of the prepolymer was 40.56 parts.
[0413] Next, the prepolymer was heated to 100° C. and degassed under reduced pressure for 1 hour. Thereafter, 7.14 parts of a mixture of 1,4-butanediol and trimethylolpropane (mass ratio = 60 / 40) was added to 100 parts of the prepolymer and mixed for 3 minutes without foaming to prepare a cleaning blade forming composition A1.
[0414] Next, the cleaning blade forming composition A1 was poured into a centrifugal molding machine whose mold was adjusted to 140°C, and a curing reaction was performed for 1 hour. Then, it was aged and heated at 110°C for 24 hours, cooled, and cut to obtain a cleaning blade (1) (referred to as "BLD1" in Table 2).
[0415] (Manufacture of cleaning blade (2))
[0416] The cleaning blade (2) was manufactured as follows.
[0417] In the preparation of the cleaning blade 1, a cleaning blade (2) (referred to as "BLD2" in Table 2) was obtained in the same manner as the cleaning blade (1) except that the aging heating temperature was changed to 75°C.
[0418] (Manufacture of cleaning blade (3))
[0419] The cleaning blade (3) was manufactured as follows.
[0420] In the preparation of the cleaning blade (1), a cleaning blade (3) (referred to as "BLD3" in Table 2) was obtained in the same manner as the cleaning blade (1) except that the aging heating temperature was changed to 75°C and the aging heating time was changed to 32 hours.
[0421] (Manufacturing of cleaning blade (4))
[0422] The cleaning blade (4) was manufactured as follows.
[0423] In the preparation of the cleaning blade (1), a cleaning blade (4) (referred to as "BLD4" in Table 2) was obtained in the same manner as the cleaning blade (1) except that the aging heating temperature was changed to 75°C and the weight ratio of the mixture of 1,4-butanediol and trimethylolpropane was changed to 70 / 30.
[0424] (Manufacturing of cleaning blade (5))
[0425] The cleaning blade (5) was manufactured as follows.
[0426] In the preparation of the cleaning blade (1), a cleaning blade (5) (referred to as "BLD5" in Table 2) was obtained in the same manner as the cleaning blade (1) except that the soft segment material was changed to 1,9-ND adipate having a molecular weight of 2000 obtained from 1,9-nonanediol and adipic acid.
[0427] <Example 1>
[0428] (Production of Photoreceptor)
[0429] A photoreceptor was prepared as follows.
[0430] Zinc oxide (average particle size 70 nm: manufactured by TAYCA; specific surface area 15 m 2 / g) and 500 parts of tetrahydrofuran were stirred and mixed, and 1.4 parts of a silane coupling agent (KBE503: manufactured by Shin-Etsu Chemical Co., Ltd.) were added and stirred for 2 hours. The tetrahydrofuran was then distilled off by reduced pressure distillation, and the mixture was calcined at 120°C for 3 hours to obtain zinc oxide surface treated with a silane coupling agent.
[0431] 110 parts of the surface-treated zinc oxide and 500 parts of tetrahydrofuran were stirred and mixed, and a solution prepared by dissolving 0.6 parts of alizarin in 50 parts of tetrahydrofuran was added, followed by stirring at 50° C. for 5 hours. The zinc oxide to which alizarin was imparted was then filtered out by vacuum filtration, and further dried under reduced pressure at 60° C. to obtain zinc oxide with alizarin.
[0432] 60 parts of the zinc oxide with alizarin, 13.5 parts of a curing agent (blocked isocyanate Sumidur 3175, manufactured by Sumitomo-Bayer Urethane Co., Ltd.), 15 parts of a butyral resin (S-LECBM-1, manufactured by Sekisui Chemical Co., Ltd.), and 85 parts of methyl ethyl ketone were mixed to obtain a mixed solution. 38 parts of the mixed solution was mixed with 25 parts of methyl ethyl ketone and the mixture was stirred for 2 hours. The glass beads were dispersed using a sand mill for 2 hours to obtain a dispersion.
[0433] 0.005 parts of dioctyltin dilaurate and 30 parts of silicone resin particles (TOSPEARL 145, Momentive Performance Materials Japan) were added to the obtained dispersion as a catalyst to obtain a primer coating solution. The coating solution was applied to a cylindrical aluminum substrate by dip coating and dried and cured at 170° C. for 30 minutes to obtain a primer layer with a thickness of 24 μm.
[0434] Next, 1 part of hydroxygallium phthalocyanine (which has strong diffraction peaks at Bragg angles (2θ±0.2°) of 7.5°, 9.9°, 12.5°, 16.3°, 18.6°, 25.1°, and 28.3° in its X-ray diffraction spectrum) was mixed with 1 part of polyvinyl butyral (S-LECBM-5, manufactured by Sekisui Chemical Co., Ltd.) and 80 parts of n-butyl acetate, and the mixture was dispersed together with glass beads using a paint shaker for 1 hour to prepare a coating liquid for a charge generation layer. The obtained coating liquid was dip-coated on the conductive substrate on which the primer layer was formed, and dried by heating at 130°C for 10 minutes to form a charge generation layer having a film thickness of 0.15 μm.
[0435] 45 parts of a benzidine compound represented by the following formula (CTM1) as a charge transport material and 55 parts of a polymer compound (viscosity-average molecular weight: 40,000) having a repeating unit represented by the following formula (PCZ1) as a binder resin were dissolved in 350 parts of toluene and 150 parts of tetrahydrofuran, 11.2 parts of fluorine-containing resin particles (1) and 3 parts of a compound represented by the formula (HP-2) as a hindered phenol-based antioxidant in the antioxidant (Add1) (ADKSTABAO-20, manufactured by Adeka Corporation) were added, and the mixture was treated five times using a high-pressure homogenizer to prepare a coating liquid for a charge transport layer.
[0436] The obtained coating liquid was applied onto the charge generating layer by dip coating, and heated at 130° C. for 45 minutes to form a charge transporting layer having a film thickness of 31 μm.
[0437] [Chemistry 6]
[0438]
[0439] [Chemistry 7]
[0440]
[0441] Each photoreceptor is manufactured through the above steps.
[0442] (Processing Box Production)
[0443] The prepared photoreceptor was installed in a process cartridge equipped with a cleaning blade (1) of an image forming apparatus (DocuCentre-V C7775, manufactured by Fuji Xerox Corporation) to obtain a process cartridge.
[0444] <Examples 2 to 17, Comparative Examples 1 to 8>
[0445] A photoreceptor and a process cartridge were prepared in the same manner as in Example 1 except that the type and amount of fluorine-containing resin particles, the type and amount of antioxidant, and the type of cleaning blade were changed as shown in Tables 1 and 2.
[0446] <Evaluation>
[0447] (Lubricity Evaluation)
[0448] The friction coefficient of the outermost surface layer of the photoreceptor obtained in each example was measured 30 times in succession by the HEIDON impedance measurement method under the following measurement conditions, and the average of the measured values from the 10th to the 20th time was calculated. It should be noted that the friction coefficient is the motion friction coefficient of the measurement needle. The name of the measuring device used in the measurement of the friction coefficient is as follows.
[0449] TRIBOGEAR (load-variable friction and wear testing system) manufactured by Shinto Scientific Co., Ltd.: TYPEHHS2000 (using standard analysis software)
[0450] ·Measurement conditions
[0451] Needle material: diamond, needle tip shape: R = 0.2mm, load: 20g, needle contact angle: 90° (perpendicular to the photosensitive surface), needle movement distance: one-way 10mm round trip, number of round trips: 30 times
[0452] -Lubricity Evaluation Criteria-
[0453] A(○): less than 0.6
[0454] B(△): 0.6 or more and less than 0.7
[0455] C(×): 0.7 or more
[0456] (Determination of the absolute value of △VH)
[0457] The photoreceptor obtained in each example was assembled in a photoreceptor electrical characteristics evaluation apparatus manufactured by Fuji Xerox Co., Ltd., and the absolute value of the difference ΔVH between the VH1 and VH2 was measured according to the above-described procedure.
[0458] (Actual machine evaluation)
[0459] -Evaluation Image Forming Device-
[0460] The process cartridge obtained in each example was installed in DocuCentre-VC7775 manufactured by Fuji Xerox Co., Ltd. A surface potential meter (Trek 334 manufactured by Trek Co., Ltd.) was used, and a surface potential probe was set at a position 1 mm from the photoreceptor surface in the measurement target area.
[0461] This apparatus was used as an image forming apparatus for evaluating initial chargeability and charge retention performance described below.
[0462] (Evaluation of initial chargeability)
[0463] The surface potential after charging was set to -700 V using an evaluation image forming apparatus, and then a halftone image with an image density of 30% was output on A4 paper in a high temperature and high humidity environment (temperature 28°C, humidity 85% RH). The surface potential was then measured using a surface potentiometer and evaluated according to the following evaluation criteria.
[0464] A(○): Surface potential is -700 V or more and less than -680 V
[0465] B(△): Surface potential is above -680V and less than -660V
[0466] C(×): Surface potential is -660V or above
[0467] (Charge retention evaluation)
[0468] The surface potential after charging was set to -700 V using an evaluation image forming apparatus, and then 70,000 sheets of halftone images with an image density of 30% were output on A4 paper in a high temperature and high humidity environment (temperature 28°C, humidity 85% RH). The surface potential was then measured using a surface potentiometer and evaluated according to the following evaluation criteria.
[0469] A(○): Surface potential is -700 V or more and less than -680 V
[0470] B(△): Surface potential is above -680V and less than -660V
[0471] C(×): Surface potential is -660V or above
[0472] The records in the following table are explained below.
[0473] The antioxidant species "Add1" represents a compound represented by the formula (HP-2) (ADKSTABAO-20, manufactured by Adeka Corporation).
[0474] The antioxidant species "Add2" represents 2,2'-methylenebis(6-tert-butyl-p-cresol (product name: Sumilizer MDP-S, manufactured by Sumitomo Chemical Co., Ltd.) (a compound represented by the formula (HP-3)).
[0475] The antioxidant species "Add3" represents tris(nonylphenyl)phosphite (product name: Sumilizer TNP, manufactured by Sumitomo Chemical Co., Ltd.).
[0476] The antioxidant "Add4" represents butylated hydroxyanisole.
[0477] The antioxidant "Add5" represents butylated hydroxytoluene.
[0478] The antioxidant species "Add6" represents the compound name 2-phenylethyl (E)-cinnamate (manufactured by Tokyo Chemical Industry Co., Ltd.).
[0479] “-” indicates that the fluorine-containing resin particles are not contained or the value of the corresponding item cannot be calculated due to the absence of the fluorine-containing resin particles.
[0480] The "content of the fluorine-containing resin particles to the charge transport layer (mass %)" means the content of the fluorine-containing resin particles relative to the charge transport layer, and the unit is mass %.
[0481] The "content to particles (mass %)" of the antioxidant means the content of the antioxidant relative to the content of the fluorine-containing resin particles contained in the charge transport layer, and the unit is mass %.
[0482] The “number of benzene rings” of an antioxidant refers to the number of benzene rings contained in one molecule of the antioxidant.
[0483] “|ΔVH|(V)” represents the absolute value of the difference ΔVH between VH1 and VH2.
[0484] [Table 1]
[0485]
[0486]
[0487] The above results show that the photoreceptor of this example has good initial chargeability and improved charge retention after repeated use.
Claims
1. An electrophotographic photoreceptor, in, The electrophotographic photoreceptor comprises a conductive substrate and a photosensitive layer provided on the conductive substrate. The outermost surface layer of the electrophotographic photoreceptor contains fluorine-containing resin particles and an antioxidant. The number of carboxyl groups contained in the fluorine-containing resin particles is relative to 10 6 The number of carbon atoms is 0 to 30. After heating at 150° C. for 10 minutes in an air atmosphere, the weight loss of the antioxidant is 40% by mass or less.
2. The electrophotographic photoreceptor according to claim 1, in, The molecular weight of the antioxidant is 240 or more and 350 or less.
3. The electrophotographic photoreceptor according to claim 2, in, The antioxidant having a molecular weight of 240 or more and 350 or less is a compound having two or more benzene rings in the molecule.
4. The electrophotographic photoreceptor according to any one of claims 1 to 3, in, The content of the antioxidant is 20% by mass or more and 60% by mass or less relative to the content of the fluorine-containing resin particles.
5. The electrophotographic photoreceptor according to claim 4, in, The content of the fluorine-containing resin particles is 5% by mass or more and 20% by mass or less with respect to the outermost surface layer.
6. An electrophotographic photoreceptor, in, The electrophotographic photoreceptor comprises a conductive substrate and a photosensitive layer provided on the conductive substrate. The outermost surface layer of the electrophotographic photoreceptor contains fluorine-containing resin particles and an antioxidant. The number of carboxyl groups contained in the fluorine-containing resin particles is relative to 10 6 The number of carbon atoms is 0 to 30. The electrophotographic photoreceptor is assembled in a photoreceptor electrical characteristics evaluation device including a charging device, an exposure device, and a static elimination device. A series of steps of charging, exposure and neutralization were performed once under the following conditions, and the charging potential after recharging was set to VH1. The above process was repeated 100 times under the following conditions, and the charging potential after recharging was set to VH2. At this time, the absolute value of the difference △VH between the above VH1 and the above VH2 is less than 5V. The conditions are: ·Measurement environment: Temperature 20℃ / Humidity 40%RH Charging potential: +600V Exposure light: 10mJ / m 2 Exposure wavelength: 780nm ·Light source for eliminating static electricity: halogen lamp ·Electrostatic light wavelength: above 600nm and below 800nm · Anti-static light intensity: 30mJ / m 2 · Rotation speed of photoreceptor: 66.7 rpm 7 . A process cartridge that is detachably mounted in an image forming apparatus, comprising the electrophotographic photoreceptor according to claim 1 .
8. A process cartridge according to claim 7, in, The processing box is provided with a cleaning mechanism, and the cleaning mechanism has a cleaning blade for cleaning the surface of the above-mentioned electrophotographic photoreceptor. At least a portion of the cleaning blade that contacts the electrophotographic photoreceptor is composed of a member containing polyurethane rubber and having an endothermic peak top temperature in a range of 180° C. to 220° C. as measured by differential scanning calorimetry.
9. An image forming apparatus comprising: The electrophotographic photoreceptor according to any one of claims 1 to 6, A charging mechanism is used to charge the surface of the electrophotographic photoreceptor. The electrostatic latent image forming mechanism forms an electrostatic latent image on the charged surface of the electrophotographic photoreceptor. a developing mechanism for developing the electrostatic latent image formed on the surface of the electrophotographic photoreceptor using a developer containing a toner to form a toner image, and The transfer mechanism transfers the toner image to the surface of the recording medium.
10. The image forming apparatus according to claim 9, in, The image forming apparatus comprises a cleaning mechanism having a cleaning blade for cleaning the surface of the electrophotographic photoreceptor. At least a portion of the cleaning blade that contacts the electrophotographic photoreceptor is composed of a member containing polyurethane rubber and having an endothermic peak top temperature in a range of 180° C. to 220° C. as determined by differential scanning calorimetry.
Citation Information
Patent Citations
Oxytitanium phthalocyanine hydrate crystal and electronic photograph photosensitizer using the same
JP1992189873A
Production of new dichloro-tin phthalocyanine crystal and electrophotographic photoreceptor made by using the crystal
JP1993140472A
New crystal of dichloro-tin phthalocyanine, its production and electophotgraphic photoreceptor and coating fluid for the photoreceptor which are made therefrom
JP1993140473A
Preparation of novel crystal of hydroxygallium phthalocyanine and electrophotographic photoreceptor made using the same
JP1993279591A
Novel charge transfer polymer, preparation thereof, and organic electronic device made using the same