Semiconductor packages
By designing a T-shaped bump pad and setting an undercut structure with a metal seed layer underneath, the peeling problem between the bump pad and the lower protective layer was solved, improving the reliability and productivity of semiconductor packages.
Patent Information
- Application Number
- CN202110249687.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-03-27
- Filing Date
- 2021-03-08
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2041-03-08
AI Technical Summary
Existing technologies in semiconductor packages suffer from delamination between bump pads and the underlying protective layer, leading to bump structure detachment and affecting package reliability and manufacturing productivity.
By designing the bump pads as T-shaped and placing a metal seed layer between them and the lower protective layer, the undercut structure of the metal seed layer is used to improve the bonding strength between the bump pads and the bump structure, and reduce peeling defects.
This improved the reliability of semiconductor packages and increased manufacturing productivity while reducing overall costs.
Smart Images

Figure CN113451257B_ABST
Abstract
Description
[0001] Cross-references to related applications
[0002] Priority is claimed to Korean Patent Application No. 10-2020-0037361, filed on March 27, 2020, with the Korean Intellectual Property Office, the entire contents of which are incorporated herein by reference. Technical Field
[0003] This disclosure relates to semiconductor packages, and more particularly to semiconductor packages including redistribution layers. Background Technology
[0004] With the rapid development of the electronics industry and to meet user demands, electronic devices are becoming increasingly compact and multifunctional. Consequently, the need for miniaturization and multifunctionality of semiconductor chips used in electronic devices is growing. This necessitates semiconductor chips with finely pitched connection terminals and microelectrode pads to mount high-capacity semiconductor chips within structures with limited semiconductor package dimensions. Therefore, a redistribution layer is needed to electrically connect external connection terminals to microelectrode pads included in the semiconductor package. Summary of the Invention
[0005] Embodiments of the present invention provide a semiconductor package and a method thereof that improve reliability and manufacturing productivity by reducing defects caused by bump pads.
[0006] An embodiment of the present invention provides a semiconductor package comprising: a semiconductor chip; a redistribution layer structure disposed below the semiconductor chip; a bump pad disposed below the redistribution layer structure, the bump pad having an upper structure and a lower structure, the upper structure having a first width and the lower structure having a second width less than the first width; a metal seed layer disposed along the lower surface of the upper structure and the side surface of the lower structure; an insulating layer surrounding the redistribution layer structure and the bump pad; and a bump structure disposed below the bump pad. A first undercut is disposed at one end of the metal seed layer that contacts the upper structure, and a second undercut is disposed at the other end of the metal seed layer that contacts the lower structure.
[0007] An embodiment of the present invention provides a semiconductor package comprising: a first sub-package including a first semiconductor chip; a second sub-package disposed on the first sub-package and including a second semiconductor chip; and an inter-package connection structure connecting the first sub-package to the second sub-package. Both the first and second sub-packages include: a lower redistribution layer structure; a bump pad disposed below the lower redistribution layer structure, the bump pad having an upper structure and a lower structure, the upper structure having a first width and the lower structure having a second width less than the first width; a metal seed layer disposed along the lower surface of the upper structure and the side surface of the lower structure; a lower insulating layer surrounding the lower redistribution layer structure and the bump pad; and a bump structure disposed below the bump pad. The first undercut is located at the end of the metal seed layer that contacts the upper structure, and the second undercut is located at the other end of the metal seed layer that contacts the lower structure.
[0008] An embodiment of the present invention provides a semiconductor package comprising: a bump structure; a T-shaped bump pad disposed on the bump structure, the T-shaped bump pad having an upper structure and a lower structure with a step difference between the upper structure and the lower structure; a redistribution layer structure disposed on the bump pad and having multiple redistribution layer lines; multiple insulating layers surrounding the redistribution layer structure and the bump pad; a metal seed layer conformally disposed between the lower surface of the upper structure and the lowermost insulating layer of the multiple insulating layers, and between the side surface of the lower structure and the lowermost insulating layer; and a semiconductor chip disposed on the redistribution layer structure and electrically connected to the bump structure. A first undercut is disposed at one end of the metal seed layer, and a second undercut is disposed at the other end of the metal seed layer, and the first undercut and the second undercut extend orthogonally to each other.
[0009] Embodiments of the present invention also provide a semiconductor package comprising a redistribution layer structure having a first main surface and a second main surface opposite to the first main surface, the redistribution layer structure including a redistribution layer line and an insulating layer; a semiconductor chip located on the first main surface of the redistribution layer structure and connected to the redistribution layer line; a bump pad located on the second main surface of the redistribution layer structure, the bump pad including a first structure embedded in the redistribution layer structure and connected to the redistribution layer line, and a second structure protruding from the first structure, the second structure having a pad surface exposed from the insulating layer at the second main surface of the redistribution layer structure; and a metal seed layer disposed between the insulating layer and the bottom surface of the first structure and between the insulating layer and the side surface of the second structure, the metal seed layer having a first undercut and a second undercut at its opposite ends. Attached Figure Description
[0010] The embodiments of the inventive concept will become clearer from the following detailed description taken in conjunction with the accompanying drawings, in which:
[0011] Figure 1 A cross-sectional view of a semiconductor package according to an embodiment of the present invention is shown;
[0012] Figure 2 It shows Figure 1 Enlarged cross-sectional view of region AA;
[0013] Figure 3 It shows Figure 2 A bottom view of the bump pads;
[0014] Figure 4 It shows Figure 2 Enlarged cross-sectional view of region BB;
[0015] Figure 5 An enlarged cross-sectional view of a portion of a semiconductor package according to an embodiment of the present invention is shown;
[0016] Figure 6 An enlarged cross-sectional view of a portion of a semiconductor package according to another embodiment of the present invention is shown;
[0017] Figure 7 An enlarged cross-sectional view of a portion of a semiconductor package according to yet another embodiment of the concept of the present invention is shown;
[0018] Figure 8 A cross-sectional view of a semiconductor package according to an embodiment of the present invention is shown;
[0019] Figure 9 A cross-sectional view of a semiconductor package according to another embodiment of the present invention is shown;
[0020] Figure 10 A cross-sectional view of a semiconductor package according to another embodiment of the present invention is shown;
[0021] Figure 11 A cross-sectional view of a semiconductor package according to yet another embodiment of the concept of the present invention is shown;
[0022] Figure 12 A block diagram illustrating a method for manufacturing a semiconductor package according to an embodiment of the concept of the present invention is shown;
[0023] Figure 13 , Figure 14 , Figure 15 , Figure 16 , Figure 17 , Figure 18 , Figure 19 , Figure 20 , Figure 21 , Figure 22 , Figure 23 , Figure 24 , Figure 25 , Figure 26 , Figure 27 , Figure 28 and Figure 29 A cross-sectional view is shown of a method for manufacturing a semiconductor package according to an embodiment of the present invention, based on a process sequence; and
[0024] Figure 30 A structural diagram is shown that schematically illustrates the construction of a semiconductor package according to an embodiment of the present invention. Detailed Implementation
[0025] In the following, embodiments of the inventive concept will be described in detail with reference to the accompanying drawings.
[0026] Figure 1 A cross-sectional view of a semiconductor package according to an embodiment of the present invention is shown. Figure 2 It shows Figure 1 Enlarged cross-sectional view of region AA. Figure 3 It shows Figure 2 A bottom view of the bump pads. Figure 4 It shows Figure 2 A magnified cross-sectional view of region BB.
[0027] Refer to together Figures 1 to 4The semiconductor package 10 includes one or more semiconductor chips 170, one or more redistribution layer structures 140 disposed below the one or more semiconductor chips 170, one or more bump pads 123 disposed below the one or more redistribution layer structures 140, one or more seed metal layers 121 disposed along a portion of the side surface of the one or more bump pads 123, an insulating layer 130 surrounding the one or more redistribution layer structures 140 and the one or more bump pads 123, and one or more bump structures 191 disposed below the one or more bump pads 123.
[0028] If the size of the semiconductor chip 170 is reduced or the number of input / output terminals of the semiconductor chip 170 is increased, the semiconductor package 10 may not be able to accommodate all external connection terminals (e.g., input / output terminals) within the main surface of the semiconductor chip 170. Therefore, the semiconductor package 10 can have a fan-out wafer-level package (FO-WLP) or fan-out panel-level package (FO-PLP) structure that includes external connection terminals by extending the redistribution layer structure 140 to the molding member 181 forming the outer peripheral surface of the semiconductor chip 170.
[0029] Furthermore, in FO-WLP, the semiconductor package 10 according to an embodiment of the present invention can be implemented by a chip-last manufacturing method, in which the supporting substrate 101 (see...) is first... Figure 13 A redistribution layer structure 140 is formed on the redistribution layer structure 140, and then a semiconductor chip 170 is mounted on the formed redistribution layer structure 140. However, for ease of understanding, regardless of the formation order of the semiconductor chip 170 relative to the redistribution layer structure 140, the semiconductor chip 170 will be described first below.
[0030] Semiconductor chip 170 may include, for example, logic chips or memory chips. Logic chips may include, for example, microprocessors, analog elements, or digital signal processors. Furthermore, memory chips may include volatile memory chips such as dynamic random access memory (DRAM) or static RAM (SRAM), or non-volatile memory chips such as phase-change RAM (PRAM), magnetoresistive RAM (MRAM), resistive RAM (RRAM), or ferroelectric RAM (FeRAM). In some embodiments, semiconductor chip 170 may include high-bandwidth memory chips. Semiconductor package 10 may include a plurality of semiconductor chips 170.
[0031] Semiconductor chip 170 can be understood as including a semiconductor device having an integrated circuit. For example, semiconductor chip 170 may include a semiconductor substrate 171 having active and passive surfaces facing each other. Circuit portions for implementing the integrated circuit functions of semiconductor chip 170 can be formed on the active surface of semiconductor substrate 171 by semiconductor manufacturing processes. That is, wiring layers such as conductive wiring, interlayer insulating films disposed between wiring layers, and individual unit elements can be formed on semiconductor substrate 171.
[0032] Furthermore, the semiconductor chip 170 may include electrode pads 173 formed in the semiconductor substrate 171 to extend the functionality of the circuitry portion externally. The peripheral portions (e.g., side surfaces) of the electrode pads 173 may be covered by a protective layer formed on the active surface of the semiconductor substrate 171, and the central portion of the electrode pads 173 may be exposed from the protective layer. The protective layer may physically and chemically protect the semiconductor device on the active surface of the semiconductor substrate 171. The protective layer may include, for example, inorganic insulating materials such as silicon oxide, silicon nitride, and silicon oxynitride, or organic insulating materials such as insulating polymers, or insulating materials composed of combinations thereof.
[0033] The electrode pad 173 may have a polygonal shape, such as a square, hexagon, or octagon, or it may be circular or elliptical. The electrode pad 173 may be formed to have a predetermined size or larger to withstand electrical and mechanical stresses. Hereinafter, the surface on which the electrode pad 173 is formed will be referred to as the lower surface of the semiconductor chip 170. Solder bumps 175 may be disposed below the electrode pad 173.
[0034] The molding member 181 can protect the semiconductor chip 170 from external influences such as contaminants and impacts. To perform this function, the molding member 181 can be made of epoxy molding compound, resin, or the like. Alternatively, the molding member 181 can be formed by processes such as compression molding, lamination, or screen printing. In some embodiments, the molding member 181 can cover the side surfaces of the semiconductor chip 170 and can expose the upper surface of the semiconductor chip 170 (i.e., the main surface opposite the aforementioned lower surface) to the outside. The molding member 181 can form the external shape of the semiconductor package 10, and the redistribution layer structure 140 can extend from the molding member 181.
[0035] The upper pad 161 and the upper protective layer 151 surrounding the upper pad 161 may be disposed below the solder bump 175. The upper pad 161 may be located in an opening in the upper protective layer 151. In some embodiments, the upper protective layer 151 may comprise an inorganic insulating material, an organic insulating material, or an insulating material composed of a combination thereof.
[0036] The redistribution layer structure 140 may include a single layer or multiple layers of metal wiring. For example, the redistribution layer structure 140 may be formed of copper (Cu), nickel (Ni), gold (Au), chromium (Cr), titanium (Ti), or palladium (Pd) or alloys thereof. In some embodiments, the redistribution layer structure 140 may be formed by an electroplating process.
[0037] The redistribution layer structure 140 may include a gradually narrowing inverted trapezoidal passage and redistribution layer lines 141 to 144 (e.g., 141, 142, 143, and 144) in contact with the upper surface of the passage. Each of the redistribution layer lines 141 to 144 may be arranged along a plane formed in a first direction (X direction) and a second direction (Y direction) perpendicular to the first direction (X direction). Additionally, the redistribution layer lines 141 to 144 may be arranged as multiple layers in a third direction (Z direction) perpendicular to both the first direction (X direction) and the second direction (Y direction). The width of the passage may be formed in a shape that narrows away from the semiconductor chip 170 along the third direction (Z direction). This may be based on the characteristics of a post-chip manufacturing method in which the semiconductor chip 170 is subsequently mounted on the redistribution layer structure 140.
[0038] The redistribution layer structure 140 may include redistribution layer lines 141 to 144 consisting of four layers between insulating layers 130. However, the redistribution layer structure 140 may include more or fewer layers than redistribution layer lines 141 to 144.
[0039] Redistribution line lines 141 to 144 electrically connect the bump pad 123 to the electrode pad 173 of the semiconductor chip 170. For example, solder bumps 175 are disposed between the electrode pad 173 and the upper pad 161 of the semiconductor chip 170, such that the electrode pad 173 and the upper pad 161 can be electrically connected to each other. The first redistribution line 141 is disposed below the upper pad 161, and the upper pad 161 and the first redistribution line 141 can be directly connected to each other. The second redistribution line 142 can be disposed below the first redistribution line 141, and the first redistribution line 141 and the second redistribution line 142 can be directly connected to each other. In the same manner, the third redistribution line 143 is disposed below the second redistribution line 142, and the fourth redistribution line 144 is disposed below the third redistribution line 143, so as to be directly connected to each other. Here, the bump pad 123 is located below the fourth redistribution layer line 144, and the fourth redistribution layer line 144 and the bump pad 123 can be directly connected to each other.
[0040] Additionally, insulating layer 130 may include one or more insulating layers surrounding redistribution layer structure 140. Insulating layer 130 may be formed, for example, of a polymer, benzocyclobutene, or resin, and may be formed of photosensitive polyimide. Therefore, insulating layer 130 may be referred to as a polymer layer. However, the materials constituting insulating layer 130 are not limited thereto. For example, insulating layer 130 may be made of silicon oxide or silicon nitride.
[0041] Regarding insulating layer 130, a first insulating layer 131 is disposed below the upper protective layer 151, and the first insulating layer 131 may include an opening exposing a portion of the upper surface of the first redistribution layer line 141. A second insulating layer 132 is disposed below the first insulating layer 131, and the second insulating layer 132 may include an opening exposing a portion of the upper surface of the second redistribution layer line 142. Similarly, a third insulating layer 133 may be disposed below the second insulating layer 132, a fourth insulating layer 134 may be disposed below the third insulating layer 133, and a fifth insulating layer 135 may be disposed below the fourth insulating layer 134. A lower protective layer 111 is disposed below the fifth insulating layer 135, and the lower protective layer 111 may include an opening exposing the lower surface of the bump pad 123.
[0042] Bump pads 123 are electrically connected to individual unit elements of semiconductor chip 170 via redistribution layer structure 140, allowing the functionality of the circuit portion of semiconductor chip 170 to be electrically connected to bump structure 191. That is, bump pads 123 may also be referred to as under-bump metal (UBM). In some embodiments, bump pads 123 may be copper (Cu) pads. Furthermore, the thickness 123H of bump pads 123 may be from approximately 3 μm to approximately 15 μm, but is not limited thereto. Semiconductor package 10 may include a plurality of bump pads 123.
[0043] The bump pad 123 may include an upper structure 123T and a lower structure 123B. The upper structure 123T may contact the fourth redistribution layer line 144 of the redistribution layer structure 140, and the lower structure 123B may contact the bump structure 191. The first width W1 of the upper structure 123T in the bump pad 123 may be greater than the second width W2 of the lower structure 123B. That is, the bump pad 123 has a T-shape, and the side surfaces of the bump pad 123 may have a step difference. In some embodiments, the value of the first width W1 may be determined to be within a range that satisfies the condition of being greater than the value of the second width W2 plus approximately 2 μm and less than four times the value of the second width W2. However, the value of the first width W1 is not limited to this. The lower (second) structure 123B is characterized in that it may extend or protrude from the upper (first) structure 123T.
[0044] The upper structure 123T and lower structure 123B of the bump pad 123 may have the same central axis 123C. That is, the center of the upper structure 123T and the center of the lower structure 123B may be aligned in the third direction (Z direction). Additionally, the horizontal level of the lower surface of the lower structure 123B may be substantially the same as the horizontal level of the lowest surface of the lower protective layer 111. That is, the lower surface of the lower structure 123B and the lowest surface of the lower protective layer 111 may be substantially coplanar. In some embodiments, each of the upper structure 123T and lower structure 123B of the bump pad 123 may have a cylindrical shape. In other embodiments, each of the upper structure 123T and lower structure 123B of the bump pad 123 may have any shape, for example, a quadrilateral prism shape.
[0045] A metal seed layer 121 may be disposed between the bump pad 123 and the lower protective layer 111. Specifically, the metal seed layer 121 may be conformally disposed on a portion of the side surface of the bump pad 123 and a portion of the upper surface of the lower protective layer 123. The metal seed layer 121 may be formed by a physical vapor deposition process to have a thickness of approximately 100 Å to approximately 20,000 Å. The metal seed layer 121 may be formed of, for example, at least one metal selected from titanium (Ti), titanium-tungsten (TiW), and chromium (Cr), or alloys thereof.
[0046] The metal seed layer 121 can be used as a seed for forming the bump pad 123. That is, the metal seed layer 121 provides a path through which current can flow when the bump pad 123 is formed by an electroplating process, thereby forming the bump pad 123 on the metal seed layer 121. In some embodiments, the metal seed layer 121 and the bump pad 123 can be made of different materials. For example, the metal seed layer 121 can be formed of titanium (Ti), and the bump pad 123 can be formed of copper (Cu). In this case, the metal seed layer 121 and the bump pad 123 can form an interface.
[0047] The metal seed layer 121 can be disposed along the lower surface of the upper structure 123T and the side surface of the lower structure 123B of the bump pad 123. A first undercut 121C1 can be formed at one end of the metal seed layer 121 that contacts the upper structure 123T, and a second undercut 121C2 can be formed at the other end of the metal seed layer 121 that contacts the lower structure 123B. The first undercut 121C1 can be formed along (or along) a first direction (X direction), and the second undercut 121C2 can be formed along (or along) a third direction (Z direction). That is, the first undercut 121C1 and the second undercut 121C2 can be perpendicular to each other, or in other words, extend orthogonally to each other. Here, the first length C1 of the first undercut 121C1 can reach approximately 2 μm, and the second length C2 of the second undercut 121C2 can reach approximately 3 μm. However, in other embodiments, the first undercut and the second undercut can have different lengths.
[0048] The bump structure 191 may include solder balls or solder bumps. In some embodiments, for example, lead-free solder comprising tin (Sn) may be used as the material constituting the bump structure 191. The semiconductor package 10 can be connected to an external device such as a printed circuit board (PCB) via the bump structure 191. The bump structure 191 may be electrically connected to the redistribution layer structure 140 via bump pads 123.
[0049] In some embodiments, the third width W3 of the bump structure 191 may be greater than the second width W2 of the lower structure 123B. In this case, the first undercut 121C1 may be filled by the insulating layer 130, and the second undercut 121C2 may be filled by the bump structure 191. The bump structure 191 may be configured to contact the lower surface of the lower structure 123B, but may be configured not to contact the lower surface of the lower protective layer 111. Furthermore, the bump structure 191 may contact the side surfaces of the lower structure 123B and the side surfaces of the lower protective layer 111 via the second undercut 121C2.
[0050] In response to the rapid development of the electronics industry and to meet user demands, electronic devices are becoming increasingly compact and multifunctional. Consequently, the demand for miniaturization and multifunctionality of semiconductor chips, such as semiconductor chip 170, used in electronic devices is also increasing. As a result, semiconductor chips, such as semiconductor chip 170, are required to have fine (or reduced) pitch connection terminals and micro electrode pads 173 to mount high-capacity semiconductor chips 170 within the structure of a semiconductor package 10 with limited dimensions. Therefore, a redistribution layer structure 140 with fine (or small) dimensions is needed to electrically connect bump structures 191 (which are external connection terminals) to the electrode pads 173 included in the semiconductor package 10. However, during the recent development of manufacturing semiconductor packages 10 using ultra-fine processes, a problem has arisen where bump structures 191 detach due to peeling between bump pads 123 and the lower protective layer 111.
[0051] In embodiments of the present invention, peeling defects that may occur between the bump pad 123 and the lower protective layer 111 in the semiconductor package 10 can be reduced by forming the bump pad 123 into a T-shape and forming a metal seed layer 121 between the bump pad 123 and the lower protective layer 111. Additionally, the bonding strength between the bump pad 123 and the bump structure 191 can be improved by a second undercut 121C2 of the metal seed layer 121.
[0052] Therefore, the semiconductor package 10 according to the embodiment of the present invention can have improved reliability and can increase manufacturing productivity while reducing overall cost.
[0053] Figure 5 , Figure 6 and Figure 7 An enlarged cross-sectional view of a portion of a semiconductor package according to another embodiment of the present invention is shown.
[0054] Most of the components constituting the semiconductor packages 20, 30, and 40 described below, and the materials constituting these components, are referenced. Figures 1 to 4 The descriptions are substantially the same or similar. Therefore, for convenience, the following description will focus primarily on the differences between semiconductor packages 20, 30, and 40 and semiconductor package 10.
[0055] Reference Figure 5 The semiconductor package 20 includes a bump structure 291 attached to the lower surface of the bump pad 123 as shown in the figure.
[0056] The bump structure 291 included in the semiconductor package 20 may include solder balls or solder bumps. Through the bump structure 291, the semiconductor package 20 can be connected to an external device such as a PCB. The bump structure 291 can be electrically connected to the redistribution layer structure 140 (see [link to documentation]) via bump pads 123. Figure 1 ).
[0057] In some embodiments, the fourth width W4 of the bump structure 291 may be equal to or less than the second width W2 of the lower structure 123B. In this case, the first undercut 121C1 may be filled by the insulating layer 130, and the second undercut 121C2 may remain empty. The bump structure 291 may be configured to contact the lower surface of the lower structure 123B, but may be configured not to contact the lower protective layer 111. Additionally, the bump structure 291 may be spaced apart from the side surfaces of the lower structure 123B and the lower protective layer 111 by the second undercut 121C2.
[0058] Reference Figure 6 The semiconductor package 30 includes a bump pad 323 having a recessed circular upper surface, as shown in the figure.
[0059] Bump pad 323 may include redistribution layer structure 140 (see...) Figure 1 The bump pad 323 has an upper structure 323T that contacts the bump structure 191 and a lower structure 323B that contacts the bump structure 191. The width of the upper structure 323T of the bump pad 323 can be greater than the width of the lower structure 323B. That is, the bump pad 323 has a T-shape, and the side surface of the bump pad 323 can have a step difference.
[0060] The upper structure 323T of the bump pad 323 can be formed to have a concave surface 323R. That is, a portion of the upper surface of the upper structure 323T can be concave. This is likely a characteristic resulting from the process of forming the bump pad 323.
[0061] Reference Figure 7 The semiconductor package 40 includes a bump pad 423 having a raised circular upper surface, as shown in the figure.
[0062] Bump pad 423 may include redistribution layer structure 140 (see...) Figure 1 The bump pad 423 has an upper structure 423T that contacts the bump structure 191 and a lower structure 423B that contacts the bump structure 191. The width of the upper structure 423T of the bump pad 423 can be greater than the width of the lower structure 423B of the bump pad 423. That is, the bump pad 423 has a T-shape, and the side surface of the bump pad 423 can have a step difference.
[0063] The upper structure 423T of the bump pad 423 can be formed to have a convex surface 423R. That is, the upper surface of the upper structure 423T can be convex. This is likely a characteristic resulting from the process of forming the bump pad 423.
[0064] Figure 8 , Figure 9 , Figure 10 and Figure 11 A cross-sectional view of a semiconductor package according to another embodiment of the present invention is shown.
[0065] Most of the components constituting the semiconductor packages 50, 60, 70 and 80 described below, and the materials constituting these components, are referenced. Figures 1 to 4 Those described are substantially the same or similar. Therefore, for convenience, the following description will focus primarily on the differences between semiconductor packages 50, 60, 70, and 80 and semiconductor package 10.
[0066] Reference Figure 8 The semiconductor package 50 includes an upper redistribution layer structure 540 formed on the upper surface of the semiconductor chip 170 and a second semiconductor chip 570 mounted on the upper redistribution layer structure 540.
[0067] The semiconductor package 50 may include a through electrode 163 passing through a molding member 181. The side surfaces of the semiconductor chip 170 and the through electrode 163 are covered by the molding member 181, and the top surfaces of the semiconductor chip 170 and the through electrode 163 are exposed. In some embodiments, after the molding member 181 is formed to cover the semiconductor chip 170 and the through electrode 163, the top surface of the molding member 181 may be ground to expose the top surfaces of the semiconductor chip 170 and the through electrode 163 to the outside. In other embodiments, after the molding member 181 is formed to cover the semiconductor chip 170, a via is then formed in the molding member 181 by an exposure process and an etching process, and the through electrode 163 is formed to fill the via.
[0068] The semiconductor package 50 may include passive components 560 and second semiconductor chips 570. After forming an upper redistribution layer structure 540 electrically connected to the through electrode 163, the passive components 560 and second semiconductor chips 570 may be mounted on the upper redistribution layer structure 540. The semiconductor package 50 may include a plurality of second semiconductor chips 570 and a plurality of passive components.
[0069] The upper insulating layer 530 may be configured to surround the upper redistribution layer structure 540, and the second molding member 581 may be configured to surround the passive element 560 and the second semiconductor chip 570.
[0070] Reference Figure 9 The semiconductor package 60 includes a second semiconductor chip 670 mounted on the upper part of the semiconductor chip 170 in the form of a sub-package.
[0071] Semiconductor package 60 includes both fan-out panel-level package (FO-PLP) and stacked package (PoP) structures. That is, a first sub-package SP1 including a semiconductor chip 170 and a second sub-package SP2 including a second semiconductor chip 670 are connected via an inter-package connection structure 691 to form a single semiconductor package. For example, semiconductor chip 170 may include a controller semiconductor chip, and the second semiconductor chip 670 may include a memory semiconductor chip.
[0072] The first sub-package SP1 may include a frame structure 160 surrounding the side surface of the semiconductor chip 170. The frame structure 160 is a configuration for supporting the semiconductor package 60, and by means of this configuration, rigidity can be maintained and thickness uniformity can be ensured. The frame structure 160 has an upper surface and a lower surface facing the upper surface, and a through region is formed to penetrate between its upper and lower surfaces. In the through region, the semiconductor chip 170 is positioned spaced apart from the frame structure 160, resulting in the periphery of the side surface of the semiconductor chip 170 being surrounded by the frame structure 160.
[0073] The material of the frame structure 160 is not particularly limited, as long as it can support the semiconductor package 60. For example, insulating materials, metals with excellent rigidity and thermal conductivity, glass, ceramics, plastics, etc., can be used. The thickness of the frame structure 160 is not particularly limited and can be designed according to the thickness of the semiconductor chip 170. For example, depending on the type of semiconductor chip 170, the thickness of the frame structure 160 can be approximately 100 μm to approximately 500 μm. The frame structure 160 can be large in size, having multiple through areas for mass production of the semiconductor package 60, and therefore the frame structure 160 can be manufactured by individualizing the semiconductor package 60 using a sawing process after manufacturing multiple semiconductor packages 60.
[0074] The frame structure 160 may include through electrodes 165 and 167 penetrating its interior. Through electrodes 165 and 167 may penetrate the main body of the frame structure 160. Through electrodes 165 and 167 may include a lower through electrode 167 and an upper through electrode 165, but the specific number, spacing, arrangement type, etc., are not particularly limited and can be fully modified according to the design. The frame structure 160 can therefore be characterized as including through electrodes that are multiple wiring layers formed as a multi-level structure.
[0075] Through electrodes 165 and 167 can be electrically connected to the inter-package connection structure 691.
[0076] The second sub-package SP2 may include a second semiconductor chip 670, a second redistribution layer structure 640 disposed beneath the second semiconductor chip 670, a second bump pad 623 disposed beneath the second redistribution layer structure 640, a second seed metal layer 621 disposed along a portion of the side surface of the second bump pad 623, and a second insulating layer 630 surrounding the second redistribution layer structure 640 and the second bump pad 623. Additionally, the second sub-package SP2 may include an underfill 683 to enhance the connection between the second semiconductor chip 670 and the solder balls, and may include a molding member 681 to protect the second semiconductor chip 670 from external influences such as contaminants and impact forces.
[0077] The second bump pad 623 may be substantially the same as the bump pad 123, and the second metal seed layer 621 may be substantially the same as the metal seed layer 121. That is, in the semiconductor package 60 of the embodiment of the present invention, the features included in the first sub-package SP1 may also be applied to the second sub-package SP2.
[0078] Reference Figure 10 The semiconductor package 70 includes a package substrate 720, an interposer 710 disposed on the package substrate 720, and one or more semiconductor chips 770 disposed on the interposer 710.
[0079] The packaging substrate 720 included in the semiconductor package 70 can be a PCB, a wafer substrate, a ceramic substrate, a glass substrate, etc. In the semiconductor package 70 of the present invention, the packaging substrate 720 can be a PCB.
[0080] External terminals 791 can be disposed on the lower surface of the package substrate 720. The semiconductor package 70 can be electrically connected to and mounted on the module board or system board of an electronic product via the external terminals 791.
[0081] Intermediate layer 710 may include redistribution layer structure 140, bump pads 123 connected to the lower part of redistribution layer structure 140, and through electrode 711 connected to the upper part of redistribution layer structure 140.
[0082] One or more semiconductor chips 770 may be mounted on the interposer 710. The semiconductor package 70 may include a molding member 781 surrounding the semiconductor chip 770 and a heat dissipation member 783 located on the molding member 781. In addition, the semiconductor package 70 may include a seal 785 surrounding the interposer 710, the molding member 781 and the heat dissipation member 783.
[0083] One or more semiconductor chips 770 may include a first semiconductor chip 771 and a second semiconductor chip 772. The first semiconductor chip 771 includes a single logic chip and may be implemented, for example, as a microprocessor, graphics processor, signal processor, network processor, chipset, audio codec, video codec, application processor, or system-on-a-chip (SoC). The second semiconductor chip 772 may include a high-bandwidth memory chip in which multiple slices are stacked. In some embodiments, one or more semiconductor chips 770 may include any number of first semiconductor chips 771 and second semiconductor chips 772.
[0084] Reference Figure 11 The semiconductor package 80 includes a package substrate 820, a first semiconductor chip 871 disposed on the package substrate 820, and a plurality of second semiconductor chips 872 and 873 disposed on the first semiconductor chip 871.
[0085] The packaging substrate 820 included in the semiconductor package 80 can be a PCB, a wafer substrate, a ceramic substrate, a glass substrate, etc. In the semiconductor package 80 of the embodiment of the present invention, the packaging substrate 820 can be a PCB.
[0086] External terminals 891 can be disposed on the lower surface of the package substrate 820. The semiconductor package 80 can be electrically connected to and mounted on the module board or system board of an electronic product via the external terminals 891.
[0087] One or more semiconductor chips 870 may include a first semiconductor chip 871 and a plurality of second semiconductor chips 872 and 873. The first semiconductor chip 871 may include a redistribution layer structure 140. Additionally, the first semiconductor chip 871 may include bump pads 123 connected to the lower portion of the redistribution layer structure 140 and through electrodes 861 connected to the upper portion of the redistribution layer structure 140. The plurality of second semiconductor chips 872 and 873 may be mounted on the first semiconductor chip 871, and the side surfaces of the plurality of second semiconductor chips 872 and 873 may be surrounded by a molding member 881.
[0088] The first semiconductor chip 871 includes a single logic chip and can be implemented, for example, as a microprocessor, graphics processor, signal processor, network processor, chipset, audio codec, video codec, application processor, or system-on-a-chip. The plurality of second semiconductor chips 872 and 873 may, for example, include volatile memory chips and / or non-volatile memory chips.
[0089] Figure 12 A block diagram illustrating a method for manufacturing a semiconductor package according to an embodiment of the present invention is shown.
[0090] Reference Figure 12 The method for manufacturing a semiconductor package (S10) may include a process sequence of steps one through nine (S110 to S190).
[0091] A method (S10) for manufacturing a semiconductor package according to an embodiment of the present invention may include: a first step (S110) of forming an adhesive layer and a lower protective layer on a support substrate; a second step (S120) of forming a preliminary seed layer on the upper surface of the adhesive layer and the exposed surface of the lower protective layer; a third step (S130) of forming bump pads on the preliminary seed layer; a fourth step (S140) of forming a metal seed layer by wet etching of the preliminary seed layer; a fifth step (S150) of forming a redistribution layer structure on the bump pads; a sixth step (S160) of mounting a semiconductor chip and forming a molding member surrounding the semiconductor chip; a seventh step (S170) of attaching a carrier substrate and removing the support substrate; an eighth step (S180) of removing the adhesive layer by wet etching; and a ninth step (S190) of forming a bump structure under the bump pads and removing the carrier substrate.
[0092] In some embodiments, Figure 12 The specific process sequence of the steps shown may differ from the sequence described above. For example, where appropriate, two processes described successively may be performed substantially simultaneously, or may be performed in the reverse order of the described sequence.
[0093] Reference Figures 13 to 29 The technical features of each step in steps one through nine (S110 to S190) are described in detail.
[0094] Figures 13 to 29 A cross-sectional view is shown of a method for manufacturing a semiconductor package according to an embodiment of the present invention, based on a process sequence.
[0095] Reference Figure 13 An adhesive layer AL and a preliminary protective layer 111P are sequentially formed on a support substrate 101.
[0096] In forming semiconductor package 10 (see Figure 1 When the support substrate 101 is used to support various material layers, it can later be removed from the semiconductor package 10 (see...). Figure 1 Remove from ).
[0097] The support substrate 101 can support the insulating layer and the conductive layer, and can be made of a material that is stable to baking and etching processes. In some embodiments, the support substrate 101 can be a translucent substrate when it is subsequently separated and removed by laser ablation. In other embodiments, the support substrate 101 can be a heat-resistant substrate when it is later separated and removed by heating.
[0098] In some embodiments, the support substrate 101 may be a glass substrate. In other embodiments, the support substrate 101 may be made of a heat-resistant organic polymer material such as polyimide, polyetheretherketone, polyethersulfone, polyphenylene sulfide, etc., but is not limited to such materials.
[0099] An adhesive layer AL can be provided on the support substrate 101. The adhesive layer AL enables the support substrate 101 to bond with the semiconductor package 10 (see [reference]). Figure 1 Separated by a layer of metal material. The adhesive layer AL may include a layer of metallic material. The adhesive layer AL may be formed, for example, of a metal or an alloy thereof, including at least one selected from titanium (Ti), titanium-tungsten (TiW), and chromium (Cr).
[0100] Subsequently, a preliminary protective layer 111P can be formed on the adhesive layer AL. The preliminary protective layer 111P prevents contamination caused by material diffusion between the adhesive layer AL and various material layers added in subsequent processes. Furthermore, the preliminary protective layer 111P prevents interference with various material layers added in subsequent processes during the separation of the support substrate 101. The preliminary protective layer 111P may include a photosensitive insulating film such as silicon oxide, silicon nitride, or a photoimageable dielectric (PID).
[0101] Reference Figure 14 In the initial protective layer 111P (see Figure 13 A mask pattern (not shown) is formed on the surface, and the mask pattern is used as an etching mask to etch the initial protective layer (111P, see [reference]). Figure 13 It is part of the lower protective layer 111.
[0102] After the lower protective layer 111 is formed, the mask pattern is removed by an ashing and stripping process. Etching can be dry etching. Dry etching forms the lower protective layer 111, which includes a plurality of first openings 111H. The first openings 111H may have sidewalls substantially perpendicular to the upper surface of the supporting substrate 101. In this case, the first openings 111H may have a rectangular cross-sectional shape. In other embodiments, due to the nature of the dry etching process, the first openings 111H may have gradually narrowing sidewalls that taper in width instead of vertical sidewalls.
[0103] The first opening 111H partially exposes the upper surface of the adhesive layer AL. Furthermore, viewed from above, the exposed portion of the adhesive layer AL can have a circular shape. That is, the lower protective layer 111 can include a plurality of first openings 111H having a cylindrical shape.
[0104] Reference Figure 15 A preliminary seed layer 121P is formed on the exposed upper surface of the exposed adhesive layer AL and the exposed surface of the lower protective layer 111 by a physical vapor deposition process, having a thickness in the range of about 100 Å to about 20,000 Å.
[0105] The preliminary seed layer 121P can be formed of, for example, a metal or alloy thereof containing at least one selected from titanium (Ti), titanium-tungsten (TiW), and chromium (Cr). That is, the preliminary seed layer 121P can be formed of substantially the same material as the adhesive layer AL. Therefore, an interface is shown between the preliminary seed layer 121P and the adhesive layer AL, but this interface can be shown differently. Figure 15 As shown in the figure.
[0106] The initial seed layer 121P can be used to form the bump pad 123 (see...). Figure 17 Seed crystals. That is, when bump pads 123 (see...) are formed by electroplating... Figure 17 During this process, the initial seed layer 121P provides a path through which current can flow, thereby allowing bump pads 123 to be formed on the initial seed layer 121P (see...). Figure 17 ).
[0107] The initial seed layer 121P can be formed to conformally cover the first opening 111H of the lower protective layer 111. The upper surface of the adhesive layer AL exposed by the first opening 111H corresponds to the portion that is in direct contact with the initial seed layer 121P.
[0108] Reference Figure 16 A mask pattern MP is formed on the initial seed layer 121P.
[0109] The mask pattern MP can be formed as a pattern that exposes a portion of the initial seed layer 121P. This is because the portion exposed by the mask pattern MP corresponds to the formation of the bump pad 123 in subsequent processes (see...). Figure 17 The part is part of the bump pad 123, so when multiple bump pads 123 are formed (see...) Figure 17 When multiple portions of the mask pattern MP are exposed, they can be formed to correspond to multiple bump pads 123 (see...). Figure 17 In the following text, for ease of description, the multiple bump pads 123 may be simply referred to as bump pads 123.
[0110] Reference Figure 17A bump pad 123 is formed on a preliminary seed layer 121P on which a mask pattern MP is formed.
[0111] The bump pad 123 can be formed as the upper surface of the mask pattern MP that directly contacts the preliminary seed layer 121P. The bump pad 123 can be formed by performing an electroplating process.
[0112] To form the bump pad 123, a support substrate 101 on which a mask pattern MP is formed can be placed in a plating bath and electroplating can be performed. The bump pad 123 can be made of a metal, such as copper (Cu), nickel (Ni), and gold (Au), or an alloy thereof.
[0113] The bump pad 123 can be formed to not completely fill the area defined by the mask pattern MP, but only partially fill the area. That is, the height of the bump pad 123 can be formed to be lower than the height of the mask pattern MP.
[0114] Reference Figure 18 Perform ashing and stripping processes, and remove the mask pattern MP (see [link]). Figure 17 ).
[0115] The bump pad 123 may include the superstructure 123T (see Figure 20 ) and substructure 123B (see Figure 20 The upper structure 123T of the bump pad 123 (see...) Figure 20 The width of the bump pad 123 can be greater than the lower structure 123B of the bump pad 123 (see [link]). Figure 20 The width of the bump pad 123. That is, the bump pad 123 has a T-shape, and the side surface of the bump pad 123 may have a step difference.
[0116] Refer to together Figure 19 and Figure 20 By using bump pad 123 as an etching mask, the exposed preliminary seed layer 121P (see [reference]) is etched to the outside. Figure 18 Wet etching (WE) is performed to form a metal seed layer 121.
[0117] The metal seed layer 121 can be disposed along the lower surface of the upper structure 123T and the side surface of the lower structure 123B of the bump pad 123.
[0118] When the initial seed layer 121P is selectively etched using isotropic wet etching (WE) (see...) Figure 18When the bump pad 123 is in contact with the upper structure 123T, a first undercut 121C1 can be formed at the metal seed layer 121 located between the bump pad 123 and the lower protective layer 111. That is, the first undercut 121C1 can be formed at the end of the metal seed layer 121 that contacts the upper structure 123T. The first undercut 121C1 can be formed along (or along) a first direction (X direction).
[0119] Reference Figure 21 An insulating layer 130 is formed on the lower protective layer 111 to fill the periphery of the bump pad 123 and includes a second opening 130H that partially exposes the upper surface of the bump pad 123. A plurality of second openings 130H may be formed, and for ease of description, the plurality of second openings 130H may be referred to as second openings 130H hereinafter.
[0120] The insulating layer 130 may be made of silicon oxide or silicon nitride. In some embodiments, the insulating layer 130 may include a photosensitive insulating film such as a PID. The photosensitive insulating film is characterized in that it can be formed with a flat upper surface that does not reflect or have the shape of the underlying layer. Therefore, regardless of the shape of the bump pad 123, the insulating layer 130 can have a flat profile. Moreover, the insulating layer 130 can fill the first undercut 121C1.
[0121] A second opening 130H is formed by etching a portion of the insulating layer 130 using a mask pattern (not shown) as an etching mask, and the mask pattern is removed by an ashing and stripping process.
[0122] Etching can be dry etching. Dry etching forms an insulating layer 130 comprising a plurality of second openings 130H. Due to the nature of the etching process, the second openings 130H can have downwardly narrowing sidewalls instead of vertical sidewalls.
[0123] The second opening 130H partially exposes the upper surface of the bump pad 123. Additionally, when viewed from above, the exposed portion of the bump pad 123 may have a circular shape.
[0124] Reference Figure 22 A redistribution layer structure 140 and an upper pad 161 are sequentially formed on the bump pad 123.
[0125] The redistribution layer structure 140 and the upper pad 161 can be formed, for example, of copper (Cu), nickel (Ni), gold (Au), chromium (Cr), titanium (Ti), or palladium (Pd) or alloys thereof. In some embodiments, the redistribution layer structure 140 can be formed by a mosaic process. Because mosaic processes are well known, their detailed description is omitted.
[0126] When a similar process is repeated, all of the following can be formed: redistribution layer structure 140, insulating layer 130 surrounding redistribution layer structure 140, upper pad 161 on redistribution layer structure 140, and upper protective layer 151 surrounding upper pad 161.
[0127] Reference Figure 23 Semiconductor chip 170 is mounted to be electrically connected to upper pad 161.
[0128] Semiconductor chip 170 can be electrically connected to upper pad 161 using solder bumps. Semiconductor chip 170 can be a custom semiconductor die or a sub-package in which a semiconductor die is molded. Semiconductor chip 170 is mounted such that the active surface on which the connection pads are formed can face downwards, and the connection pads of semiconductor chip 170 can be aligned with the upper surface of upper pad 161.
[0129] Multiple semiconductor chips 170 can be installed. Some of the semiconductor chips 170 may be logic chips, while others may be memory chips. For convenience, the following description may refer to semiconductor chip 170 rather than multiple semiconductor chips 170.
[0130] In the process of electrically connecting the semiconductor chip 170 and the solder bumps, a gap may be formed between the semiconductor chip 170 and the solder bumps. Such a gap may cause problems with the reliability of the connection between the semiconductor chip 170 and the solder bumps. To ensure reliability, an underfill (not shown) may be injected and cured to enhance the connection.
[0131] The semiconductor chip 170 is more stably secured to the solder bump by the underfill, and electrical separation of the semiconductor chip 170 from the solder bump is prevented despite the difference in thermal expansion coefficients between the two. In some embodiments, the molding member 181 (see...) Figure 24 It can be directly filled into the gap between the semiconductor chip 170 and the solder bump, and in this case, no underfill is required.
[0132] Reference Figure 24 The molded component 181 is formed to surround the side surface and top surface of the semiconductor chip 170.
[0133] The molded component 181 can protect the semiconductor chip 170 from external influences such as impact forces. To perform this function, the molded component 181 can be made of epoxy molding compound, resin, etc.
[0134] In some embodiments, the molding member 181 may cover only the side surface of the semiconductor chip 170 and may expose the upper surface of the semiconductor chip 170 to the outside.
[0135] Reference Figure 25 The carrier substrate 102 is attached to the molding member 181 so as to face the support substrate 101 (see...). Figure 24 ), and remove the support substrate 101 (see Figure 24 ).
[0136] The carrier substrate 102 may include, for example, glass or alumina. To facilitate the attachment of the carrier substrate 102, a second adhesive layer (not shown) may be formed between the carrier substrate 102 and the molding member 181. The second adhesive layer may be in the form of a liquid or gel that can be easily deformed under a predetermined pressure.
[0137] In order to separate and remove the support substrate 101 (see...) Figure 24 The support substrate 101 can be irradiated with a laser (see...) Figure 24 Adhesive layer AL and support substrate 101 (see) Figure 24 The bonding force between the components can be weakened by laser irradiation, and the support substrate 101 (see [reference]) can be strengthened. Figure 24 ) separated out.
[0138] Refer to together Figure 26 and Figure 27 The exposed adhesive layer AL is removed by wet etching (WE) (see Figure 25 ).
[0139] Due to wet etching (WE), the lower surface of the bump pad 123 and the lower surface of the lower protective layer 111 can be exposed. The horizontal height of the lower surface of the bump pad 123 can be substantially the same as the horizontal height of the lowest surface of the lower protective layer 111.
[0140] When using wet isotropic etching (WE) to etch the adhesive layer AL (see... Figure 25 When forming the lower protective layer 111, a second undercut 121C2 can be formed at the metal seed layer 121 located between the bump pad 123 and the lower protective layer 111. That is, the second undercut 121C2 can be formed at the other end of the metal seed layer 121 that contacts the lower structure 123B. The second undercut 121C2 can be formed along (or along) a third direction (Z direction).
[0141] Refer to together Figure 28 and Figure 29 A bump structure 191, serving as an external connection terminal, is formed on the lower surface of the bump pad 123.
[0142] In some embodiments, the bump structure 191 may be formed as a solder ball. The solder ball is spherically formed and may be attached to the lower surface of the bump pad 123. In other embodiments, with respect to the bump structure 191, a solder layer may be formed on the lower surface of the bump pad 123, and the solder layer may be melted by a reflow process to form a reflow solder layer.
[0143] In some embodiments, the bump structure 191 may have a third width W3, which is greater than the second width W2 of the lower structure 123B (see [link]). Figure 3 and Figure 4 According to such an embodiment, the first undercut 121C1 can be filled by the insulating layer 130, and the second undercut 121C2 can be filled by the bump structure 191. The bump structure 191 can be configured to contact the lower surface of the lower structure 123B, and can be configured not to contact the lower surface of the lower protective layer 111. Furthermore, the bump structure 191 can contact the side surfaces of the lower structure 123B and the side surfaces of the lower protective layer 111 through the second undercut 121C2.
[0144] Refer again Figure 1 The carrier substrate 102 can be removed to complete the manufacturing of the semiconductor package 10. As a result, with respect to the semiconductor package 10 according to an embodiment of the present invention, peeling defects between the bump pad 123 and the semiconductor package 10 can be prevented by forming a T-shaped bump pad 123 and forming a metal seed layer 121 between the bump pad 123 and the lower protective layer 111.
[0145] Figure 30 A configuration diagram is shown that schematically illustrates the arrangement of a semiconductor package according to an embodiment of the present invention.
[0146] Reference Figure 30 The semiconductor package 1000 may include a microprocessor unit (MPU) 1010, a memory 1020, an interface 1030, a graphics processing unit (GPU) 1040, and a functional block 1050 interconnected via a bus 1060. The semiconductor package 1000 may include both the MPU 1010 and the GPU 1040, or may include only one of the MPU 1010 and the GPU 1040.
[0147] The MPU 1010 may include cores and a cache memory. For example, the MPU 1010 may include multiple cores. Each core in the multiple cores may have the same or different performance. In addition, each core in the multiple cores may be activated simultaneously or at different times.
[0148] Memory 1020 can store the results processed by function block 1050 under the control of MPU 1010. Interface 1030 can exchange information or signals with external devices. GPU 1040 can perform graphics functions. For example, GPU 1040 can be used as a video codec or can process 3D graphics. Function block 1050 can perform various functions. For example, when semiconductor package 1000 is an application processor used in a mobile device, some function blocks 1050 can perform communication functions.
[0149] Semiconductor package 1000 may include the above reference Figures 1 to 11 The semiconductor package described is any one of 10, 20, 30, 40, 50, 60, 70 and 80.
[0150] Although the inventive concept has been specifically shown and described with reference to embodiments thereof, it should be understood that various changes in form and detail may be made herein without departing from the spirit and scope of the appended claims.
Claims
1. A semiconductor package, comprising: Semiconductor chips; A redistribution layer structure is disposed beneath the semiconductor chip; A bump pad is disposed below the redistribution layer structure. The bump pad has an upper structure and a lower structure. The upper structure has a first width, and the lower structure has a second width that is smaller than the first width. A metal seed layer is provided along the lower surface of the upper structure and the side surface of the lower structure; An insulating layer surrounding the redistribution layer structure and the bump pads; and A bump structure is provided below the bump pad. The first undercut is located at the end of the metal seed layer that contacts the upper structure, and the second undercut is located at the other end of the metal seed layer that contacts the lower structure. The first undercut is filled with the insulating layer.
2. The semiconductor package according to claim 1, wherein, The redistribution layer structure includes: Multiple redistribution lines; and Multiple pathways, the multiple pathways being connected to the multiple redistribution layer lines, The plurality of channels have a gradually narrowing shape that narrows away from the semiconductor chip.
3. The semiconductor package according to claim 1, wherein, The first undercut and the second undercut extend orthogonally to each other.
4. The semiconductor package according to claim 3, wherein, The second undercut is filled by the bump structure.
5. The semiconductor package according to claim 4, wherein, The bump structure has a third width, which is greater than the second width of the lower structure.
6. The semiconductor package according to claim 3, wherein, The second undercut is empty.
7. The semiconductor package according to claim 6, wherein, The bump structure has a third width, and the second width of the lower structure is greater than or equal to the third width of the bump structure.
8. The semiconductor package according to claim 1, wherein, The metal seed layer includes at least one of titanium, titanium-tungsten, and chromium.
9. The semiconductor package according to claim 1, wherein, The horizontal height of the lower surface of the lower structure is the same as the horizontal height of the lowest surface of the insulating layer. The bump structure contacts the lower surface and the side surface of the lower structure, and The bump structure contacts the side surface of the insulating layer but not the lower surface of the insulating layer.
10. The semiconductor package according to claim 1, wherein, The upper surface of the superstructure is either convex upwards or concave downwards.
11. A semiconductor package, comprising: A first sub-package, the first sub-package including a first semiconductor chip; A second sub-package is disposed on the first sub-package and includes a second semiconductor chip; and An inter-package connection structure connects the first sub-package to the second sub-package. Both the first sub-package and the second sub-package include: Lower redistribution layer structure, A bump pad is disposed below the lower redistribution layer structure. The bump pad has an upper structure and a lower structure. The upper structure has a first width, and the lower structure has a second width smaller than the first width. A metal seed layer is provided along the lower surface of the upper structure and the side surface of the lower structure. A lower insulating layer, the lower insulating layer surrounding the lower redistribution layer structure and the bump pads, and A bump structure is provided below the bump pad. The first undercut is located at the end of the metal seed layer that contacts the upper structure, and the second undercut is located at the other end of the metal seed layer that contacts the lower structure. The first undercut is filled by the lower insulating layer.
12. The semiconductor package of claim 11, wherein, The first sub-package also includes a frame structure disposed around the side surface of the first semiconductor chip, and The frame structure and the lower redistribution layer structure of the first sub-package are electrically connected to each other through through electrodes disposed inside the frame structure.
13. The semiconductor package according to claim 12, wherein, The inter-package connection structure connects the frame structure of the first sub-package to the lower redistribution layer structure of the second sub-package.
14. The semiconductor package of claim 11, wherein, The first undercut and the second undercut extend orthogonally to each other.
15. The semiconductor package of claim 14, wherein, The bump structure has a third width, which is greater than the second width of the lower structure, and The second undercut is filled by the bump structure.
16. The semiconductor package of claim 14, wherein, The bump structure has a third width, and the second width of the lower structure is greater than or equal to the third width of the bump structure. The second undercut is empty.
17. The semiconductor package of claim 11, wherein, The horizontal height of the lower surface of the lower structure is the same as the horizontal height of the lowest surface of the lower insulating layer. The bump structure contacts the lower surface and the side surface of the lower structure, and The bump structure contacts the side surface of the lower insulating layer, but does not contact the lower surface of the insulating layer.
18. A semiconductor package, comprising: Bump structure; T-shaped bump pads are disposed on the bump structure. The T-shaped bump pads have an upper structure and a lower structure, and there is a step difference between the upper structure and the lower structure. A redistribution layer structure is disposed on the T-shaped bump pad and has multiple redistribution layer lines; Multiple insulating layers surround the redistribution layer structure and the T-shaped bump pad; A metal seed layer is conformally disposed between the lower surface of the upper structure and the lowermost insulating layer among the plurality of insulating layers, and between the side surface of the lower structure and the lowermost insulating layer; and A semiconductor chip, disposed on the redistribution layer structure and electrically connected to the bump structure. The first undercut is located at one end of the metal seed layer, and the second undercut is located at the other end of the metal seed layer, with the first and second undercuts extending orthogonally to each other. The first undercut is filled by an insulating layer located on the lowest insulating layer among the plurality of insulating layers.
19. The semiconductor package of claim 18, further comprising: The additional semiconductor chip is disposed on the redistribution layer structure; and A molded component surrounding the semiconductor chip and the additional semiconductor chip.
20. The semiconductor package of claim 18, wherein, The thickness of the metal seed layer between the T-shaped bump pad and the bottommost insulating layer is 100 Å to 20,000 Å, and The metal seed layer includes at least one of titanium, tungsten titanium, and chromium.
Citation Information
Patent Citations
Organic molecules, particularly those for use in optoelectronic devices
KR1020200037361A
Semiconductor package
KR1020170034211A
Semiconductor packages
KR1020180049336A
Semiconductor packages and methods of forming same
KR1020190038357A