Polarizing film, polarizing plate, and method for producing the polarizing film

By introducing high-boiling alcohol into the polarizing film and carrying out specific manufacturing treatments, the shrinkage and cracking problems of the thin polarizing film in high-temperature environments are solved, and higher durability and optical performance are achieved.

CN113508317BActive Publication Date: 2024-11-19NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080017275.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-08
Filing Date
2020-02-18
Publication Date
2024-11-19
Estimated Expiration
2040-02-18

AI Technical Summary

Technical Problem

The existing thin polarizing films are prone to shrink and cracks in high temperature environments, which affects their stability and service life.

Method used

A polyvinyl alcohol-based resin film containing iodine was used, and 0.1% to 1.0% by weight of alcohols having a boiling point of 100°C or above, such as glycerol and ethylene glycol were introduced, and a polarizing film was formed by stretching and dyeing treatment, and the Water stretching and drying shrinkage are performed during the manufacturing process to improve softness and durability.

Benefits of technology

It effectively suppresses the shrinkage and cracks of the polarizing film in a high-temperature environment, improves its durability and optical characteristics, and ensures excellent performance in a high-temperature and high-humidity environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113508317B_ABST
    Figure CN113508317B_ABST
Patent Text Reader

Abstract

Provided is a polarizing film that suppresses shrinkage and cracking in a high temperature environment. The polarizing film of the present invention is composed of a polyvinyl alcohol-based resin film containing iodine, and contains 0.1 wt% to 1.0 wt% of an alcohol having a boiling point of 100°C or more. In one embodiment, the alcohol having a boiling point of 100°C or more is glycerol and / or ethylene glycol. The polarizing plate of the present invention comprises: the above-mentioned polarizing film, and a protective layer disposed on at least one side of the polarizing film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polarizing film, a polarizing plate, and a method for manufacturing the polarizing film. Background Art

[0002] In a liquid crystal display device, which is a representative image display device, polarizing films are arranged on both sides of the liquid crystal unit due to its image forming method. As a method for manufacturing a polarizing film, for example, the following method is proposed: a laminate having a resin substrate and a polyvinyl alcohol (PVA) resin layer is stretched, and then dyed to obtain a polarizing film on the resin substrate (for example, Patent Document 1). Using such a method, a thin polarizing film can be obtained, and therefore it has attracted attention as a method that contributes to the thinning of image display devices in recent years. However, thin polarizing films have the problem of large shrinkage and easy cracking in a high temperature environment.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2001-343521 Summary of the invention

[0006] Problem that the invention aims to solve

[0007] The present invention has been made to solve the above-mentioned conventional problems, and a main object of the present invention is to provide a polarizing film and a polarizing plate in which shrinkage and cracking in a high-temperature environment are suppressed, and a method for producing such a polarizing film.

[0008] Solutions for solving problems

[0009] The polarizing film of the present invention is composed of a polyvinyl alcohol-based resin film containing iodine, and contains 0.1 wt % to 1.0 wt % of an alcohol having a boiling point of 100° C. or higher.

[0010] In one embodiment, the alcohol having a boiling point of 100° C. or higher is at least one selected from the group consisting of glycerin and ethylene glycol.

[0011] In one embodiment, the polarizing film has a thickness of 8 μm or less.

[0012] According to another aspect of the present invention, a polarizing plate is provided, which comprises: the polarizing film described above, and the protective layer disposed on at least one side of the polarizing film.

[0013] According to another aspect of the present invention, a method for manufacturing the polarizing film is provided. The method comprises: forming a polyvinyl alcohol-based resin layer on one side of a long thermoplastic resin substrate to form a laminate; stretching and dyeing the laminate to form the polyvinyl alcohol-based resin layer into a polarizing film; and introducing an alcohol having a boiling point of 100° C. or higher into the polarizing film.

[0014] In one embodiment, the production method includes immersing the polarizing film in a treatment liquid containing the alcohol having a boiling point of 100° C. or higher.

[0015] In one embodiment, the production method further includes heating the laminate after introducing the alcohol having a boiling point of 100° C. or higher into the polarizing film.

[0016] In one embodiment, the stretching includes underwater stretching.

[0017] Effects of the Invention

[0018] According to the present invention, by introducing alcohol having a boiling point of 100° C. or higher into a polarizing film, a polarizing film in which shrinkage and cracking are suppressed in a high temperature environment can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 This is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention.

[0020] Figure 2 This is a schematic diagram showing an example of a drying shrinkage process using a heating roller.

[0021] Figure 3 (a) is a conceptual diagram for explaining the test samples of the shrinkage test of Examples 1 to 2 and Comparative Example 1, and (b) is a conceptual diagram for explaining the test samples of the shrinkage test of Examples 3 to 6 and Comparative Examples 2 and 3.

[0022] Figure 4 This is a conceptual diagram explaining the measurement method of the guitar pick test. DETAILED DESCRIPTION

[0023] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0024] A.Polarizing film

[0025] The polarizing film of the embodiment of the present invention is composed of a polyvinyl alcohol (PVA) resin film containing iodine, and contains 0.1% by weight to 1.0% by weight of an alcohol having a boiling point of 100°C or more (hereinafter sometimes referred to as a high-boiling alcohol). The polarizing film contains such a high-boiling alcohol in a specified amount, so that shrinkage and cracking in a high-temperature environment can be suppressed. For such a high-boiling alcohol, as described in item C later about the manufacturing method, it is representative that it can be introduced into the polarizing film between the stretching treatment in water and the drying shrinkage treatment. It is speculated that by introducing such a high-boiling alcohol, the high-boiling alcohol functions as a plasticizer, and the softness of the polarizing film finally obtained is improved, so that shrinkage in a high-temperature environment can be suppressed, and cracking can also be suppressed as a result. The content of the high-boiling alcohol in the polarizing film is preferably 0.1% by weight to 0.9% by weight, more preferably 0.1% by weight to 0.8% by weight, further preferably 0.2% by weight to 0.7% by weight, and particularly preferably 0.2% by weight to 0.6% by weight. If the content is too small, the effect of the high-boiling-point alcohol may not be obtained, and if the content is too large, the decrease in polarization degree in a high-temperature and high-humidity environment may become greater.

[0026] The boiling point of the high-boiling-point alcohol is 100° C. or higher as described above, preferably 150° C. or higher, more preferably 180° C. or higher, and further preferably 250° C. or higher. The upper limit of the boiling point may be 310° C., for example.

[0027] Representative examples of high boiling point alcohols include higher alcohols, alcohols with ring structures (e.g., aromatic alcohols, alicyclic alcohols), and polyols. Specific examples include glycerol, ethylene glycol, butanol, phenol, and amyl alcohol. High boiling point alcohols can be used alone or in combination of two or more. Glycerol and ethylene glycol are preferred. They impart good flexibility to the obtained polarizing film, and as a result, shrinkage and cracking in a high temperature environment can be suppressed.

[0028] The thickness of the polarizing film is, for example, 8 μm or less, preferably 7 μm or less, more preferably 5 μm or less, and further preferably 3 μm or less. The lower limit of the thickness of the polarizing film may be 1 μm in one embodiment, and may be 2 μm in another embodiment.

[0029] The polarizing film preferably shows absorption dichroism at any wavelength of 380nm to 780nm. The monomer transmittance of the polarizing film is preferably 42.0% or more, more preferably 42.5% or more, and further preferably 43.0% or more. On the other hand, the monomer transmittance is preferably 47.0% or less, more preferably 46.0% or less. The polarization degree of the polarizing film is preferably 99.90% or more, more preferably 99.95% or more. On the other hand, the polarization degree is preferably 99.998% or less. According to an embodiment of the present invention, it is possible to take into account both high monomer transmittance and high polarization degree in this way, and it is possible to achieve excellent durability in a high temperature and high humidity environment as described above. The above-mentioned monomer transmittance is representatively a Y value obtained by measuring using an ultraviolet visible spectrophotometer and performing visual sensitivity correction. In addition, the monomer transmittance is a value when the refractive index of one surface of the polarizing plate is converted to 1.50 and the refractive index of the other surface is converted to 1.53. The polarization degree is typically determined by the following equation based on the parallel transmittance Tp and the orthogonal transmittance Tc obtained by measuring with an ultraviolet-visible spectrophotometer and performing sensitivity correction.

[0030] Polarization degree (%) = {(Tp-Tc) / (Tp+Tc)} 1 / 2 ×100

[0031] The shrinkage rate of the polarizing film in the absorption axis direction after heating at a temperature of 85°C for 120 hours is preferably 0.20% or less, more preferably 0.18% or less, further preferably 0.16% or less, and particularly preferably 0.14% or less. According to an embodiment of the present invention, a polarizing film with a small shrinkage rate in such a high temperature environment can be obtained. It should be noted that the shrinkage rate is the shrinkage rate of a sample with a size of 10 cm in the absorption axis direction and 10 cm in the transmission axis direction.

[0032] The polarizing film can be made using a single resin film or a laminate of two or more layers. As a specific example of a polarizing film obtained using a laminate, a polarizing film obtained using a laminate of a resin substrate and a PVA-based resin layer formed on the resin substrate can be cited. The polarizing film obtained using a laminate of a resin substrate and a PVA-based resin layer formed on the resin substrate can be made, for example, as follows: a PVA-based resin solution is applied to a resin substrate and dried to form a PVA-based resin layer on the resin substrate, thereby obtaining a laminate of a resin substrate and a PVA-based resin layer; the laminate is stretched and dyed to make the PVA-based resin layer into a polarizing film. In an embodiment of the present invention, a high-boiling alcohol is introduced into the polarizing film. Thus, a polarizing film in which shrinkage and cracking are suppressed under high temperature environments as described above can be obtained. It is preferred that a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is formed on one side of the resin substrate. Stretching typically includes immersing the laminate in a boric acid aqueous solution and stretching it. Furthermore, stretching may also include stretching the laminate at a high temperature (for example, above 95°C) in the air before stretching in the boric acid aqueous solution as required. Moreover, in the present embodiment, the laminate is preferably provided for a drying shrinkage treatment in which the laminate is heated while being transported in the length direction so as to shrink the width direction by more than 2%. Typically, the manufacturing method of the present embodiment includes: sequentially performing an air auxiliary stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment on the laminate. By introducing auxiliary stretching, the crystallinity of PVA can be improved even if PVA is coated on a thermoplastic resin, and high optical properties can be achieved. In addition, by simultaneously improving the orientation of PVA in advance, the problems of reduction in orientation and dissolution of PVA can be prevented when immersed in water in the subsequent dyeing process and stretching process, and high optical properties can be achieved. Furthermore, when the PVA-based resin layer is immersed in a liquid, the disorder of the orientation of the polyvinyl alcohol molecules and the reduction of the orientation can be suppressed compared to the case where the PVA-based resin layer does not contain a halide. Thus, the optical properties of the polarizing film obtained by the treatment process of immersing the laminate in a liquid such as dyeing treatment and underwater stretching treatment can be improved. Furthermore, by shrinking the laminate in the width direction by drying shrinkage treatment, the optical properties can be improved. The obtained resin substrate / polarizing film laminate can be used directly (that is, the resin substrate can be used as a protective layer of the polarizing film), or the resin substrate can be peeled off from the resin substrate / polarizing film laminate and any appropriate protective layer that meets the purpose can be stacked on the peeling surface. Details of the method for manufacturing the polarizing film will be described later in item C.

[0033] B.Polarizing plate

[0034] Figure 11 is a schematic cross-sectional view of a polarizing plate according to an embodiment of the present invention. The polarizing plate 100 comprises: a polarizing film 10, a first protective layer 20 disposed on one side of the polarizing film 10, and a second protective layer 30 disposed on the other side of the polarizing film 10. The polarizing film 10 is the polarizing film of the present invention described in the above-mentioned item A. One of the first protective layer 20 and the second protective layer 30 may be omitted. It should be noted that, as described above, one of the first protective layer and the second protective layer may be a resin substrate used in the manufacture of the above-mentioned polarizing film.

[0035] The first and second protective layers are formed by any appropriate film that can be used as a protective layer of a polarizing film. For the specific example of the material as the main component of the film, cellulose resins such as triacetyl cellulose (TAC), polyester resins, polyvinyl alcohol resins, polycarbonate resins, polyamide resins, polyimide resins, polyethersulfone resins, polysulfone resins, polystyrene resins, polynorbornene resins, polyolefin resins, (meth) acrylic acid resins, acetate resins, etc. can be listed. In addition, thermosetting resins or ultraviolet curing resins such as (meth) acrylic acid resins, carbamate resins, (meth) acrylic acid carbamate resins, epoxy resins, and silicone resins can also be listed. In addition, for example, glassy polymers such as siloxane polymers can also be listed. In addition, the polymer film described in Japanese Patent Publication No. 2001-343529 (WO01 / 37007) can also be used. As the material of the film, for example, a resin composition containing a thermoplastic resin having a substituted or unsubstituted imide group in the side chain and a thermoplastic resin having a substituted or unsubstituted phenyl group and a nitrile group in the side chain can be used, for example, a resin composition containing an alternating copolymer formed by isobutylene and N-methylmaleimide and an acrylonitrile-styrene copolymer can be cited. The polymer film can be, for example, an extrusion molding of the above resin composition.

[0036] When the polarizing plate 100 is applied to an image display device, the thickness of the protective layer (outer protective layer) disposed on the side opposite to the display panel is typically 300 μm or less, preferably 100 μm or less, more preferably 5 μm to 80 μm, and further preferably 10 μm to 60 μm. It should be noted that, when the surface treatment is performed, the thickness of the outer protective layer is the thickness including the thickness of the surface treatment layer.

[0037] When the polarizing plate 100 is applied to an image display device, the thickness of the protective layer (inner protective layer) disposed on the display panel side is preferably 5 μm to 200 μm, more preferably 10 μm to 100 μm, and further preferably 10 μm to 60 μm. In one embodiment, the inner protective layer is a phase difference layer having any appropriate phase difference value. In this case, the in-plane phase difference Re (550) of the phase difference layer is, for example, 110 nm to 150 nm. "Re (550)" is the in-plane phase difference measured at 23 ° C with light of a wavelength of 550 nm, and is calculated by the formula: Re = (nx-ny) × d. Here, "nx" is the refractive index in the direction where the refractive index in the plane is the largest (ie, the slow axis direction), "ny" is the refractive index in the direction orthogonal to the slow axis in the plane (ie, the fast axis direction), "nz" is the refractive index in the thickness direction, and "d" is the thickness (nm) of the layer (film).

[0038] C. Method for manufacturing polarizing film

[0039] The manufacturing method of the polarizing film of one embodiment of the present invention comprises: applying a PVA-based resin solution on one side of a long thermoplastic resin substrate and drying it to form a PVA-based resin layer to form a laminate; stretching and dyeing the laminate to form the PVA-based resin layer into a polarizing film; and introducing a high-boiling alcohol into the polarizing film. By introducing a high-boiling alcohol, a polarizing film in which shrinkage and cracking are suppressed under a high-temperature environment can be achieved. Preferably, the PVA-based resin solution also contains a halide. Preferably, the above-mentioned manufacturing method includes sequentially performing an air auxiliary stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment on the laminate, wherein the drying shrinkage treatment is performed by heating while conveying the laminate in the length direction so as to shrink the width direction by more than 2%. In this case, the introduction of the high-boiling alcohol can be preferably performed between the underwater stretching treatment and the drying shrinkage treatment. The content of the halide in the PVA-based resin solution (resulting in the PVA-based resin layer) is preferably 5 to 20 parts by weight relative to 100 parts by weight of the PVA-based resin. The drying shrinkage treatment is preferably carried out using a heating roller, and the temperature of the heating roller is preferably 60°C to 120°C. The shrinkage rate of the laminate in the width direction caused by the drying shrinkage treatment is preferably 2% or more. According to such a manufacturing method, the polarizing film described in the above-mentioned item A can be obtained. In particular, by preparing a laminate having a PVA-based resin layer containing a halide, stretching the laminate as a multi-stage stretching including air auxiliary stretching and underwater stretching, and heating the stretched laminate with a heating roller, a polarizing film having excellent optical properties (representatively, monomer transmittance and unit absorbance) can be obtained.

[0040] C-1. Preparation of laminate

[0041] As a method for producing a laminate of a thermoplastic resin substrate and a PVA-based resin layer, any appropriate method may be adopted. Preferably, a coating solution containing a halide and a PVA-based resin is applied to the surface of the thermoplastic resin substrate and dried to form a PVA-based resin layer on the thermoplastic resin substrate. As described above, the content of the halide in the PVA-based resin layer is preferably 5 to 20 parts by weight relative to 100 parts by weight of the PVA-based resin.

[0042] As a coating method of the coating liquid, any appropriate method can be adopted. For example, roll coating, spin coating, wire bar coating, dip coating, die coating, curtain coating, spray coating, knife coating (comma coating, etc.) and the like can be listed. The coating and drying temperature of the above-mentioned coating liquid is preferably 50° C. or above.

[0043] The thickness of the PVA-based resin layer is preferably 3 μm to 40 μm, more preferably 3 μm to 20 μm.

[0044] Before forming the PVA-based resin layer, the thermoplastic resin substrate may be subjected to a surface treatment (e.g., corona treatment), or an easy-adhesive layer may be formed on the thermoplastic resin substrate. By carrying out such a treatment, the adhesion between the thermoplastic resin substrate and the PVA-based resin layer can be improved.

[0045] C-1-1. Thermoplastic resin substrate

[0046] As the thermoplastic resin substrate, any appropriate thermoplastic resin film may be used. Details of the thermoplastic resin substrate are described in, for example, Japanese Patent Application Laid-Open No. 2012-73580. The entire contents of the publication are incorporated herein by reference.

[0047] C-1-2. Coating liquid

[0048] The coating liquid contains a halide and a PVA-based resin as described above. The coating liquid is typically a solution formed by dissolving the halide and the PVA-based resin in a solvent. As the solvent, for example, water, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, N-methylpyrrolidone, various glycols, polyols such as trimethylolpropane, amines such as ethylenediamine and diethylenetriamine can be cited. These can be used alone or in combination of two or more. Among these, water is preferred. The PVA-based resin concentration of the solution is preferably 3 to 20 parts by weight relative to 100 parts by weight of the solvent. At such a resin concentration, a uniform coating film that is closely attached to the thermoplastic resin substrate can be formed. The content of the halide in the coating liquid is preferably 5 to 20 parts by weight relative to 100 parts by weight of the PVA-based resin.

[0049] The coating liquid may be mixed with additives. As additives, for example, plasticizers, surfactants, etc. may be cited. As plasticizers, for example, polyols such as ethylene glycol and glycerol may be cited. As surfactants, for example, nonionic surfactants may be cited. These may be used for the purpose of further improving the uniformity, dyeability, and stretchability of the obtained PVA-based resin layer.

[0050] As the above-mentioned PVA-based resin, any appropriate resin can be used. For example, polyvinyl alcohol and ethylene-vinyl alcohol copolymer can be listed. Polyvinyl alcohol is obtained by saponifying polyvinyl acetate. Ethylene-vinyl alcohol copolymer is obtained by saponifying ethylene-vinyl acetate copolymer. The saponification degree of PVA-based resin is usually 85 mol% to 100 mol%, preferably 95.0 mol% to 99.95 mol%, and more preferably 99.0 mol% to 99.93 mol%. The saponification degree can be calculated according to JIS K 6726-1994. By using a PVA-based resin with such a saponification degree, a polarizing film with excellent durability can be obtained. When the saponification degree is too high, there is a concern that gelation will occur.

[0051] The average polymerization degree of the PVA-based resin can be appropriately selected depending on the purpose. The average polymerization degree is usually 1000 to 10000, preferably 1200 to 4500, and more preferably 1500 to 4300. The average polymerization degree can be determined in accordance with JIS K 6726-1994.

[0052] As the above-mentioned halide, any appropriate halide can be used. For example, iodide and sodium chloride can be listed. As the iodide, for example, potassium iodide, sodium iodide, and lithium iodide can be listed. Among these, potassium iodide is preferred.

[0053] The amount of the halide in the coating solution is preferably 5 to 20 parts by weight, more preferably 10 to 15 parts by weight, based on 100 parts by weight of the PVA resin. If the amount of the halide exceeds 20 parts by weight, the halide may bleed out, and the resulting polarizing film may become cloudy.

[0054] Generally, by stretching the PVA resin layer, the orientation of the polyvinyl alcohol molecules in the PVA resin will become higher, but if the stretched PVA resin layer is immersed in a liquid containing water, the orientation of the polyvinyl alcohol molecules is sometimes disordered and the orientation is reduced. In particular, when a laminate of a thermoplastic resin and a PVA resin layer is stretched in boric acid water, in order to stabilize the stretching of the thermoplastic resin, when the laminate is stretched in boric acid water at a relatively high temperature, the tendency for the above-mentioned orientation to decrease is significant. For example, the stretching of the PVA film itself in boric acid water is usually carried out at 60°C, while the stretching of the laminate of A-PET (thermoplastic resin substrate) and the PVA resin layer is carried out at a high temperature of about 70°C. In this case, the orientation of the PVA at the initial stage of stretching will decrease in the stage before it rises by stretching in water. In this regard, by preparing a laminate of a PVA-based resin layer containing a halide and a thermoplastic resin substrate, and performing high-temperature stretching (auxiliary stretching) in air before stretching the laminate in boric acid water, the crystallization of the PVA-based resin in the PVA-based resin layer of the laminate after auxiliary stretching can be promoted. As a result, when the PVA-based resin layer is immersed in a liquid, the disorder of the orientation of the polyvinyl alcohol molecules and the reduction of the orientation can be suppressed compared to the case where the PVA-based resin layer does not contain a halide. As a result, the optical properties of the polarizing film obtained by the treatment process of immersing the laminate in a liquid such as dyeing treatment and underwater stretching treatment can be improved.

[0055] C-2. Aerial assisted stretching treatment

[0056] In order to obtain high optical properties in particular, a two-stage stretching method combining dry stretching (auxiliary stretching) and boric acid water stretching is selected. By introducing auxiliary stretching as in the two-stage stretching, it is possible to stretch while suppressing the crystallization of the thermoplastic resin substrate, and it is possible to solve the problem of reduced stretchability due to excessive crystallization of the thermoplastic resin substrate in the subsequent boric acid water stretching, and the laminate is stretched at a high ratio. Furthermore, in the case of coating a PVA-based resin on a thermoplastic resin substrate, in order to suppress the influence of the glass transition temperature of the thermoplastic resin substrate, it is necessary to lower the coating temperature compared to the case where the PVA-based resin is usually coated on a metal roller, and as a result, the crystallization of the PVA-based resin becomes relatively low and the problem of insufficient optical properties is obtained. In response to this, by introducing auxiliary stretching, even in the case of coating a PVA-based resin on a thermoplastic resin, the crystallinity of the PVA-based resin can be improved, and high optical properties can be achieved. Furthermore, by improving the orientation of the PVA-based resin in advance, it is possible to prevent problems such as a decrease in the orientation and dissolution of the PVA-based resin when immersed in water in the subsequent dyeing and stretching steps, thereby achieving high optical properties.

[0057] The stretching method of aerial auxiliary stretching can be fixed-end stretching (for example, a method of stretching using a tenter stretching machine) or free-end stretching (for example, a method of uniaxially stretching the laminate by passing it between rollers with different circumferential speeds). In order to obtain high optical properties, free-end stretching can be actively adopted. In one embodiment, the aerial stretching process includes a heating roller stretching process, and the heating roller stretching process is stretched by transporting the above-mentioned laminate along its length direction while utilizing the circumferential speed difference between the heating rollers. The aerial stretching process typically includes a regional stretching process and a heating roller stretching process. It should be noted that the order of the regional stretching process and the heating roller stretching process is not limited, and the regional stretching process can be performed first, or the heating roller stretching process can be performed first. The regional stretching process can also be omitted. In one embodiment, the regional stretching process and the heating roller stretching process are performed sequentially. In addition, in another embodiment, in the tenter stretching machine, stretching is performed by holding the end of the film and expanding the distance between the tenters along the flow direction (the expansion of the distance between the tenters is the stretching ratio). At this time, the distance between the tenters in the width direction (perpendicular to the flow direction) is set in an arbitrarily close manner. It is preferred to set the stretch ratio in the flow direction in a manner closer to free-end stretching. In the case of free-end stretching, the shrinkage ratio in the width direction = (1 / stretch ratio) 1 / 2 to calculate.

[0058] The auxiliary stretching in the air can be carried out in one stage or in multiple stages. When it is carried out in multiple stages, the stretching ratio is the product of the stretching ratios of each stage. The stretching direction in the auxiliary stretching in the air is preferably substantially the same as the stretching direction in the underwater stretching.

[0059] The stretching ratio of the auxiliary stretching in the air is preferably 2.0 to 3.5 times. The maximum stretching ratio when the auxiliary stretching in the air and the stretching in the water are combined is preferably 5.0 times or more, more preferably 5.5 times or more, and further preferably 6.0 times or more relative to the original length of the laminate. In this specification, the "maximum stretching ratio" refers to the stretching ratio before the laminate is about to break, and refers to the stretching ratio at which the laminate is separately confirmed to break and is 0.2 lower than its value.

[0060] The stretching temperature of the aerial auxiliary stretching can be set to any appropriate value according to the forming material of the thermoplastic resin substrate, the stretching method, etc. The stretching temperature is preferably above the glass transition temperature (Tg) of the thermoplastic resin substrate, more preferably above the glass transition temperature (Tg) of the thermoplastic resin substrate + 10 ° C, and particularly preferably above Tg + 15 ° C. On the other hand, the upper limit of the stretching temperature is preferably 170 ° C. By stretching at such a temperature, the crystallization of the PVA-based resin can be suppressed from proceeding rapidly, thereby suppressing the adverse conditions caused by the crystallization (for example, hindering the orientation of the PVA-based resin layer caused by stretching).

[0061] C-3. Insolubilization, dyeing and cross-linking

[0062] As needed, an insolubilization treatment is performed after the auxiliary stretching treatment in the air and before the stretching treatment in the water and the dyeing treatment. The above-mentioned insolubilization treatment is typically performed by immersing the PVA-based resin layer in an aqueous solution of boric acid. The above-mentioned dyeing treatment is typically performed by dyeing the PVA-based resin layer with a dichroic substance (typically iodine). As needed, a cross-linking treatment is performed after the dyeing treatment and before the stretching treatment in the water. The above-mentioned cross-linking treatment is typically performed by immersing the PVA-based resin layer in an aqueous solution of boric acid. Details about the insolubilization treatment, the dyeing treatment and the cross-linking treatment are recorded, for example, in Japanese Patent Gazette No. 2012-73580 (mentioned above).

[0063] C-4. Underwater stretching

[0064] The underwater stretching treatment is performed by immersing the laminate in a stretching bath. Through the underwater stretching treatment, the laminate can be stretched at a temperature lower than the glass transition temperature (typically about 80° C.) of the thermoplastic resin substrate and the PVA resin layer, and the PVA resin layer can be stretched at a high ratio while suppressing crystallization. As a result, a polarizing film with excellent optical properties can be manufactured.

[0065] The stretching method of the laminate can adopt any appropriate method. Specifically, it can be fixed end stretching or free end stretching (for example, a method of uniaxially stretching the laminate by passing the laminate between rollers with different circumferential speeds). Preferably, free end stretching is selected. The stretching of the laminate can be carried out in one stage or in multiple stages. In the case of multiple stages, the stretching ratio (maximum stretching ratio) of the laminate described later is the product of the stretching ratios of each stage.

[0066] The underwater stretching is preferably performed by immersing the laminate in a boric acid aqueous solution (boric acid underwater stretching). By using a boric acid aqueous solution as a stretching bath, the PVA-based resin layer can be given rigidity that can withstand the tension applied during stretching and water resistance that is insoluble in water. Specifically, boric acid generates tetrahydroxyborate anions in an aqueous solution and cross-links with the PVA-based resin through hydrogen bonds. As a result, the PVA-based resin layer can be given rigidity and water resistance so that it can be stretched well, and a polarizing film with excellent optical properties can be manufactured.

[0067] The above-mentioned boric acid aqueous solution is preferably obtained by dissolving boric acid and / or a borate in water as a solvent. The boric acid concentration is preferably 1 to 10 parts by weight, more preferably 2.5 to 6 parts by weight, and particularly preferably 3 to 5 parts by weight relative to 100 parts by weight of water. By setting the boric acid concentration to 1 part by weight or more, the dissolution of the PVA-based resin layer can be effectively suppressed, and a polarizing film with higher characteristics can be obtained. It should be noted that an aqueous solution obtained by dissolving a boron compound such as borax, glyoxal, glutaraldehyde, etc. in a solvent other than boric acid or a borate can also be used.

[0068] It is preferred to mix an iodide in the stretching bath (boric acid aqueous solution). By mixing an iodide, the dissolution of iodine adsorbed on the PVA-based resin layer can be suppressed. Specific examples of iodide are as described above. The concentration of iodide is preferably 0.05 to 15 parts by weight, more preferably 0.5 to 8 parts by weight relative to 100 parts by weight of water.

[0069] The stretching temperature (liquid temperature of the stretching bath) is preferably 40°C to 85°C, more preferably 60°C to 75°C. At such a temperature, it is possible to stretch at a high ratio while suppressing the dissolution of the PVA-based resin layer. Specifically, as described above, the glass transition temperature (Tg) of the thermoplastic resin substrate is preferably above 60°C in terms of its relationship with the formation of the PVA-based resin layer. In this case, if the stretching temperature is lower than 40°C, there is a concern that stretching cannot be performed well even if the plasticization of the thermoplastic resin substrate brought about by water is taken into account. On the other hand, the higher the temperature of the stretching bath, the higher the solubility of the PVA-based resin layer becomes, and there is a concern that excellent optical properties cannot be obtained. The immersion time of the laminate in the stretching bath is preferably 15 seconds to 5 minutes.

[0070] The stretching ratio based on underwater stretching is preferably 1.5 times or more, more preferably 3.0 times or more. The total stretching ratio of the laminate is preferably 5.0 times or more, more preferably 5.5 times or more relative to the original length of the laminate. By achieving such a high stretching ratio, a polarizing film with excellent optical properties can be manufactured. Such a high stretching ratio can be achieved by adopting an underwater stretching method (boric acid underwater stretching).

[0071] C-5. Introduction of high boiling point alcohol

[0072] In an embodiment of the present invention, a high-boiling alcohol is introduced after the stretching treatment in water (and typically before the drying shrinkage treatment described later). The introduction of the high-boiling alcohol can be carried out in any appropriate manner. For example, the laminate can be immersed in a treatment solution containing a high-boiling alcohol, or a treatment solution containing a high-boiling alcohol can be coated on the surface of the polarizing film of the laminate. Typically, the introduction of the high-boiling alcohol can be carried out by immersion. The immersion can be carried out in any appropriate manner. For example, a high-boiling alcohol can be added to a cleaning bath in a cleaning treatment to prepare a bath of a treatment liquid, a bath of a treatment liquid can be used instead of a cleaning bath, or a bath of a treatment liquid can be set separately from the cleaning bath. Typically, a high-boiling alcohol can be added to a cleaning bath (cleaning liquid) in a cleaning treatment. The concentration of the high-boiling alcohol in the treatment liquid (cleaning liquid) is preferably 0.03 wt% to 1.0 wt%.

[0073] C-6. Drying shrinkage treatment

[0074] The drying shrinkage treatment may be preferably performed after the introduction of the high boiling point alcohol. By performing the drying shrinkage treatment after the introduction of the high boiling point alcohol, the high boiling point alcohol acts as a plasticizer during the drying shrinkage treatment, thereby improving the flexibility of the polarizing film finally obtained.

[0075] The drying shrinkage treatment can be carried out by heating the region as a whole, or by heating the conveying roller (using the so-called heating roller) (heating roller drying method). Preferably, both are used. By using a heating roller for drying, the heating curling of the laminate can be effectively suppressed to manufacture a polarizing film with excellent appearance. Specifically, by drying the laminate along the heating roller, the crystallization of the above-mentioned thermoplastic resin substrate can be effectively promoted to increase the crystallinity, and even at a lower drying temperature, the crystallinity of the thermoplastic resin substrate can be well increased. As a result, the rigidity of the thermoplastic resin substrate increases, thereby becoming a state that can withstand the shrinkage of the PVA-based resin layer caused by drying, and curling can be suppressed. In addition, by using a heating roller, the laminate can be dried while maintaining a flat state, so that not only curling but also wrinkles can be suppressed. At this time, the laminate is shrunk in the width direction by the drying shrinkage treatment, thereby improving the optical properties. This is because the orientation of PVA and PVA / iodine complex can be effectively improved. The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment is preferably 1% to 10%, more preferably 2% to 8%, and particularly preferably 4% to 6%.

[0076] Figure 2Schematic diagram showing an example of drying shrinkage treatment. In the drying shrinkage treatment, the laminate 200 is dried while being transported by the transport rollers R1 to R6 and the guide rollers G1 to G4 heated to a predetermined temperature. In the example shown in the figure, the transport rollers R1 to R6 are arranged in a manner to alternately and continuously heat the surface of the PVA resin layer and the surface of the thermoplastic resin substrate, but, for example, the transport rollers R1 to R6 may be arranged in a manner to continuously heat only one surface of the laminate 200 (for example, the surface of the thermoplastic resin substrate).

[0077] The drying conditions can be controlled by adjusting the heating temperature of the conveying roller (the temperature of the heating roller), the number of heating rollers, the contact time with the heating roller, etc. The temperature of the heating roller is preferably 60°C to 120°C, more preferably 65°C to 100°C, and particularly preferably 70°C to 80°C. An optical laminate can be manufactured that can well increase the crystallinity of the thermoplastic resin, thereby well suppressing curling, and has very excellent durability. It should be noted that the temperature of the heating roller can be measured by a contact thermometer. Six conveying rollers are provided in the example shown in the figure, but there is no particular limitation as long as there are multiple conveying rollers. Conveying rollers are usually provided in 2 to 40 numbers, preferably 4 to 30 numbers. The contact time (total contact time) between the laminate and the heating roller is preferably 1 second to 300 seconds, more preferably 1 to 20 seconds, and more preferably 1 to 10 seconds.

[0078] The heating roller can be set in a heating furnace (such as an oven) or in a normal production line (under room temperature environment). It is preferably set in a heating furnace equipped with air supply means. By combining the drying based on the heating roller and the hot air drying, the rapid temperature change between the heating rollers can be suppressed, and the shrinkage in the width direction can be easily controlled. The temperature of the hot air drying is preferably 30°C to 100°C. The hot air drying time is preferably 1 second to 300 seconds. The wind speed of the hot air is preferably about 10m / s to 30m / s. It should be noted that the wind speed is the wind speed in the heating furnace and can be measured by a mini blade type digital anemometer.

[0079] C-7. Others

[0080] The laminate of thermoplastic resin substrate / polarizing film obtained as described above can be directly used as a polarizing plate (the thermoplastic resin substrate can be used as a protective layer); or the thermoplastic resin substrate can be peeled off after the protective layer is adhered to the polarizing film surface of the laminate, and used as a polarizing plate having a structure of protective layer / polarizing film; or another protective layer can be adhered to the peeled surface of the thermoplastic resin substrate, and used as a polarizing plate having a structure of protective layer / polarizing film / protective layer.

[0081] Example

[0082] The present invention is described in detail below by way of examples, but the present invention is not limited to these examples. The measuring methods of various properties are as follows. It should be noted that, unless otherwise specified, the "parts" and "%" in the examples and comparative examples are by weight.

[0083] (1) Thickness

[0084] The measurement was performed using an interferometer film thickness meter (manufactured by Otsuka Electronics Co., Ltd., product name: "MCPD-3000").

[0085] (2) Alcohol concentration of polarizing film

[0086] The polarized film obtained in the examples and comparative examples was frozen and crushed, and about 0.02 g was taken into a threaded tube. After adding 0.5 ml of methanol for permeation extraction for more than one night, the extract was filtered with a 0.45 μm membrane filter, and 1 μL of the filtrate was injected into a gas chromatograph (manufactured by Agilent Technologies, product name "6890N"). The alcohol content was calculated using the following standard curve based on the peak area corresponding to each alcohol type.

[0087] Glycerol standard curve

[0088] y=5.666E -01 x+1.833E -00

[0089] Ethylene glycol standard curve

[0090] y=2.478E -01 x+1.315E -00

[0091] (3) Single body transmittance

[0092] The single transmittance Ts of the polarizing plates (protective films / polarizing films) of Examples and Comparative Examples measured using an ultraviolet-visible spectrophotometer (LPF-200 manufactured by Otsuka Electronics) was defined as the single transmittance of the polarizing film.

[0093] (4) Contractility

[0094] A test sample with a size of 10 cm in the absorption axis direction and 10 cm in the transmission axis direction was cut out from the polarizing plate (protective film / polarizing film) of the embodiment and the comparative example. The test sample was attached to a glass plate with an adhesive and imaged using a CNC image measuring instrument (QickVision (QV606) manufactured by Mitutoyo Corporation). Figure 3The film was then placed in a heating oven (85°C) for 120 hours, taken out of the oven and accurately measured again, and the shrinkage in the absorption axis direction was calculated based on the initial length. The evaluation was performed as follows based on Comparative Example 1.

[0095] ◎: Smaller shrinkage rate than Comparative Example 1 (smaller absolute value in the negative direction)

[0096] △: The shrinkage ratio is equivalent to that of Comparative Example 1

[0097] ×: The shrinkage rate is larger than that of Comparative Example 1 (the absolute value in the negative direction is larger)

[0098] (5) Crack (nano-slit): guitar pick test

[0099] The polarizing plates (protective films / polarizing films) of Examples and Comparative Examples were cut into a size of 50 mm×150 mm (absorption axis direction: 50 mm), and a surface protection film prepared by the following method was bonded to the protection film side.

[0100] (Surface protection film for test samples)

[0101] In a four-necked flask equipped with a stirring blade, a thermometer, a nitrogen inlet tube, and a condenser, 94 parts by mass of 2-ethylhexyl acrylate (2EHA), 1 part by mass of N,N-diethylacrylamide (DEAA), 1 part by mass of ethoxydiethylene glycol acrylate (EDE), 4 parts by mass of 4-hydroxybutyl acrylate (HBA), 0.2 parts by mass of 2,2'-azobisisobutyronitrile as a polymerization initiator, and 150 parts by mass of ethyl acetate were added, and nitrogen was introduced while slowly stirring, and the liquid temperature in the flask was maintained at about 60°C for 5 hours to perform a polymerization reaction to prepare an acrylic polymer solution (40% by mass). The weight average molecular weight of the acrylic polymer is 570,000, and the glass transition temperature (Tg) is -68°C. The acrylic polymer solution (40% by mass) was diluted to 20% by mass with ethyl acetate, and 2 parts by mass (2 parts by mass of solid content) of isocyanurate of hexamethylene diisocyanate (CORONATE HX: C / HX manufactured by Nippon Polyurethane Industry Co., Ltd.) and 2 parts by mass (0.02 parts by mass of solid content) of dibutyltin dilaurate (1% by mass ethyl acetate solution) as a crosslinking catalyst were added to 500 parts by mass (100 parts by mass of the solution), and the mixture was stirred to prepare an acrylic adhesive solution. The acrylic adhesive solution was applied to a transparent polyethylene terephthalate (PET) film (polyester film) having a thickness of 38 μm, and heated at 130° C. for 1 minute to form an adhesive layer having a thickness of 15 μm, thereby preparing a surface protection film.

[0102] Next, the polarizing plate with the surface protection film attached thereto was attached to a glass plate by means of an adhesive to prepare a test sample. Figure 4 A load of 200 g was applied with a guitar pick (manufactured by HISTORY, model "HP2H (HARD)"), and the load was repeated 50 times at a distance of 100 mm in a direction perpendicular to the absorption axis of the polarizer. The above load was applied at one location. In addition, the above load was applied at high speed (5 m / min) and low speed (1 m / min), respectively. Next, the test sample was placed in an environment of 80°C for 1 hour, and the number of cracks was counted using a differential interference microscope. Evaluation was performed as follows based on Comparative Example 1.

[0103] ◎: Fewer than in Comparative Example 1

[0104] △: The number is the same as that of Comparative Example 1

[0105] ×: The number is larger than that of Comparative Example 1.

[0106] [Example 1]

[0107] As the thermoplastic resin substrate, a long amorphous polyethylene terephthalate copolymer film (thickness: 100 μm) having a Tg of about 75° C. was used. One surface of the resin substrate was subjected to a corona treatment.

[0108] To 100 parts by weight of a PVA-based resin prepared by mixing polyvinyl alcohol (polymerization degree 4200, saponification degree 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "GOHSEFIMER Z410") in a ratio of 9:1, 13 parts by weight of potassium iodide was added to prepare a PVA aqueous solution (coating solution).

[0109] The PVA aqueous solution was applied onto the corona-treated surface of the resin substrate and dried at 60° C. to form a 13 μm-thick PVA-based resin layer, thereby producing a laminate.

[0110] The obtained laminate was subjected to free-end uniaxial stretching to 2.4 times in the longitudinal direction (longitudinal direction) between rolls having different peripheral speeds in an oven at 130° C. (in-air auxiliary stretching treatment).

[0111] Next, the laminate was immersed in an insolubilization bath (boric acid aqueous solution prepared by mixing 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (insolubilization treatment).

[0112] Next, the film was immersed in a dyeing bath (an iodine aqueous solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 relative to 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the final single body transmittance (Ts) of the polarizing film obtained was 45.0%±0.2% (dyeing treatment).

[0113] Next, the film was immersed in a crosslinking bath (boric acid aqueous solution prepared by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 40° C. for 30 seconds (crosslinking treatment).

[0114] Thereafter, the laminate was immersed in an aqueous boric acid solution (boric acid concentration: 4.0 wt %, potassium iodide: 5.0 wt %) at a liquid temperature of 70°C and uniaxially stretched (underwater stretching treatment) in the longitudinal direction (length direction) between rollers with different peripheral speeds to a total stretching ratio of 5.5 times.

[0115] Thereafter, the laminate was immersed in a treatment bath (aqueous solution of 4 wt % potassium iodide and 0.23 wt % glycerin) at a liquid temperature of 20° C. to be cleaned, and glycerin was introduced into the PVA-based resin layer (polarizing film) (cleaning treatment and introduction of glycerin).

[0116] Thereafter, the film was dried in an oven maintained at 90° C. for 4 minutes (drying treatment).

[0117] In this way, a polarizing film with a thickness of 5.0 μm was formed on the resin substrate. A cycloolefin film (manufactured by ZEON, product name "G-Film") as a protective layer (protective film) was attached to the surface of the polarizing film using a UV curable adhesive (thickness 1.0 μm), and then the resin substrate was peeled off to obtain a polarizing plate having a protective layer / polarizing film structure. The glycerol concentration in the polarizing film of the obtained polarizing plate was 0.30% by weight.

[0118] The single-body transmittance of the obtained polarizing plate (substantially, a polarizing film) is shown in Table 1. Furthermore, Table 1 also shows the evaluation results of (4) and (5) above.

[0119] [Example 2]

[0120] A polarizing plate was produced in the same manner as in Example 1 except that the glycerin concentration of the treatment bath was 0.68% by weight. The obtained polarizing plate (or polarizing film) was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0121] [Example 3]

[0122] A polarizing plate (protective film / polarizing film) was prepared in the same manner as in Example 1. The polarizing plate was cut into a size of 10 cm in the absorption axis direction and 10 cm in the transmission axis direction, and the cut piece was directly (i.e., attached to a glass plate without an adhesive) as a test sample. The test sample was imaged using a CNC image measuring instrument (QickVision (QV606) manufactured by Mitutoyo Corporation). Figure 3 The length is measured at 4 points (b) excluding the edge of the film, and the size is accurately measured. Then, it is placed in a heating oven (85°C) for 120 hours, taken out of the oven and the size is accurately measured again. The shrinkage rate in the absorption axis direction is calculated based on the initial length, and the evaluation is performed as follows based on Comparative Example 2 (described later). The results are shown in Table 1.

[0123] ◎: Smaller shrinkage rate than Comparative Example 2 (smaller absolute value in the negative direction)

[0124] △: The shrinkage ratio is equivalent to that of Comparative Example 2

[0125] ×: The shrinkage rate is larger than that of Comparative Example 2 (the absolute value in the negative direction is larger)

[0126] [Example 4]

[0127] A polarizing plate was produced in the same manner as in Example 2. The obtained polarizing plate was subjected to the same evaluation as in Example 3. The results are shown in Table 1.

[0128] [Example 5]

[0129] A laminate of resin substrate / PVA-based resin layer was prepared in the same manner as in Example 1, and the laminate was subjected to an aerial auxiliary stretching treatment in the same manner as in Example 1.

[0130] Next, the laminate was cut into 15 cm × 10 cm in the auxiliary stretching axis direction, the short side of the sample was fixed with a special stretching jig and immersed in an insolubilization bath (a boric acid aqueous solution obtained by mixing 3 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 30°C for 30 seconds (insolubilization treatment).

[0131] Next, the film was immersed in a dyeing bath (an iodine aqueous solution obtained by mixing iodine and potassium iodide in a weight ratio of 1:7 relative to 100 parts by weight of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single body transmittance (Ts) of the final polarizing film became 42.0%±0.2% (dyeing treatment).

[0132] Next, the sample was immersed in a crosslinking bath (boric acid aqueous solution prepared by mixing 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with respect to 100 parts by weight of water) at a liquid temperature of 30° C. for 30 seconds (crosslinking treatment).

[0133] Thereafter, the laminate was immersed in a boric acid aqueous solution (boric acid concentration 4.0 wt %, potassium iodide 5.0 wt %) at a liquid temperature of 70° C. and uniaxially stretched in the longitudinal direction (length direction) to a total stretch ratio of 5.5 times (underwater stretching treatment).

[0134] Thereafter, the laminate is immersed in a treatment bath (aqueous solution of 3 wt % potassium iodide and 1 wt % ethylene glycol) at a liquid temperature of 20°C for 3 seconds to clean the laminate, and ethylene glycol is introduced into the PVA-based resin layer (polarizing film) (cleaning treatment and introduction of ethylene glycol).

[0135] Thereafter, the film was dried in an oven maintained at 60° C. for 4 minutes (drying treatment).

[0136] In this way, a polarizing film with a thickness of 5.0 μm was formed on the resin substrate. A cycloolefin film (manufactured by ZEON, product name "G-Film") as a protective layer (protective film) was adhered to the surface of the polarizing film using a UV curable adhesive (thickness 1.0 μm), and then the resin substrate was peeled off to obtain a polarizing plate having a protective layer / polarizing film structure.

[0137] A test sample with a size of 4 cm in the absorption axis direction and 4 cm in the transmission axis direction was cut out from the obtained polarizing plate. The test sample was attached to a glass plate with an adhesive and imaged using a CNC image measuring instrument (QickVision (QV606) manufactured by Mitutoyo Corporation). Figure 3 The length was measured at 4 points (b) excluding the film edge, and the size was accurately measured. The film was then placed in a heating oven (85°C) for 120 hours, taken out of the oven and the size was accurately measured again, and the shrinkage in the absorption axis direction was calculated based on the initial length. The evaluation was performed as follows based on Comparative Example 3 (described later). The results are shown in Table 1.

[0138] ◎: Smaller shrinkage rate than Comparative Example 3 (smaller absolute value in the negative direction)

[0139] △: The shrinkage rate is equivalent to that of Comparative Example 3

[0140] ×: The shrinkage rate is larger than that of Comparative Example 3 (the absolute value in the negative direction is larger)

[0141] It should be noted that the evaluation of (5) was not performed.

[0142] [Example 6]

[0143] A polarizing plate was produced in the same manner as in Example 5 except that the ethylene glycol concentration of the treatment bath was 3% by weight. The obtained polarizing plate (or polarizing film) was subjected to the same evaluation as in Example 5. The results are shown in Table 1.

[0144] [Comparative Example 1]

[0145] A polarizing plate was produced in the same manner as in Example 1 except that no high-boiling alcohol was added to the cleaning bath (cleaning liquid). The obtained polarizing plate (or polarizing film) was subjected to the same evaluation as in Example 1. The results are shown in Table 1.

[0146] [Comparative Example 2]

[0147] A polarizing plate was produced in the same manner as in Example 3 except that no high-boiling alcohol was added to the cleaning bath (cleaning liquid). The obtained polarizing plate (or polarizing film) was subjected to the same evaluation as in Example 3. The results are shown in Table 1.

[0148] [Comparative Example 3]

[0149] A polarizing plate was produced in the same manner as in Example 5 except that no high-boiling alcohol was added to the cleaning bath (cleaning liquid). The obtained polarizing plate (or polarizing film) was subjected to the same evaluation as in Example 5. The results are shown in Table 1.

[0150] [Table 1]

[0151]

[0152] * Boiling point of glycerol: 290℃

[0153] * Boiling point of ethylene glycol: 197.6℃

[0154] As is clear from Table 1, the polarizing plates (polarizing films) of Examples of the present invention can suppress shrinkage in a high temperature environment by containing a predetermined amount of high boiling point alcohol. Furthermore, the polarizing plates (polarizing films) of Examples 1 and 2 significantly suppress cracking compared to Comparative Example 1.

[0155] Industrial Applicability

[0156] The polarizing film and polarizing plate of the present invention are suitable for use in liquid crystal display devices.

[0157] Description of Reference Numerals

[0158] 10 polarizing film

[0159] 20 1st protection layer

[0160] 30 Second protection layer

[0161] 100 polarizing plate

Claims

1. A method for manufacturing a polarizing film, The polarizing film is composed of a polyvinyl alcohol-based resin film containing iodine, and contains 0.30 wt % to 1.0 wt % of an alcohol having a boiling point of 100° C. or higher. The manufacturing method comprises: A polyvinyl alcohol-based resin layer is formed on one side of a long thermoplastic resin substrate to prepare a laminate; The laminate is subjected to an aerial auxiliary stretching treatment, a dyeing treatment, an underwater stretching treatment and a drying shrinkage treatment in sequence, and the polyvinyl alcohol resin layer is made into a polarizing film, wherein the drying shrinkage treatment is performed by heating the laminate while conveying the laminate in the length direction so as to shrink the laminate in the width direction by more than 2%; and After the underwater stretching treatment and before the drying shrinkage treatment, a treatment solution containing an alcohol having a boiling point of 100° C. or higher is used to introduce the alcohol having a boiling point of 100° C. or higher into the polyvinyl alcohol-based resin layer by dipping or coating, The concentration of the alcohol having a boiling point of 100° C. or higher in the treatment liquid is 0.03% by weight to 1.0% by weight. The alcohol having a boiling point of 100° C. or higher is glycerin or ethylene glycol. 2 . The production method according to claim 1 , comprising immersing the polyvinyl alcohol-based resin layer in the treatment liquid. 3 . The production method according to claim 1 , further comprising heating the laminate after introducing the alcohol having a boiling point of 100° C. or higher into the polyvinyl alcohol-based resin layer.

4. The manufacturing method according to claim 1 or 2 comprises applying a coating liquid comprising 100 parts by weight of a polyvinyl alcohol-based resin and 5 to 20 parts by weight of an iodide or sodium chloride on one side of the long strip of thermoplastic resin substrate and drying the coating liquid to form a polyvinyl alcohol-based resin layer comprising iodide or sodium chloride and a polyvinyl alcohol-based resin, thereby producing the laminate.