Solid oxide fuel cell air electrode powder and its manufacturing method

By using perovskite single-phase metal composite oxide powder in the air electrode of the solid oxide fuel cell, the problem of conductivity and open porosity in the prior art is solved, and the performance and stability of the single cell are improved , reduces costs.

CN113574705BActive Publication Date: 2024-12-03SAKAI CHEM IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980094134.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-19
Filing Date
2019-07-18
Publication Date
2024-12-03
Estimated Expiration
2039-07-18

AI Technical Summary

Technical Problem

The prior art is difficult to take into account the high conductivity and high opening porosity of the air electrode of the solid oxide fuel cell, resulting in insufficient performance of the single cell and high cost.

Method used

Using metal composite oxide powder with perovskite type single-phase crystal structure, through specific slurry preparation, drying and sintering processes, ensure the uniform distribution of element B and the stability of perovskite phase, improve the conductivity and Open porosity.

Benefits of technology

The air pole with high conductivity and high opening porosity is achieved, which improves the power generation performance of the single cell and the stability of the perovskite phase, and reduces the number and cost of the single cell.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113574705B_ABST
    Figure CN113574705B_ABST
Patent Text Reader

Abstract

This invention relates to a powder for the air electrode of a solid oxide fuel cell, which is formulated with the following general formula: A1 1‑x A2 x BO 3‑δ (wherein, element A1 is at least one selected from La and Sm, element A2 is at least one selected from Ca, Sr and Ba, element B is at least one selected from Mn, Fe, Co and Ni, 0 < x < 1, and δ is the amount of oxygen vacancies) The cross-section of a molded body obtained by pressing the powder is observed at a magnification of 500x, and the intensity of the characteristic X-rays of element B is measured by energy dispersive X-ray analysis. The number of regions with an intensity of 50% or more of the maximum intensity of the characteristic X-rays and an area ratio of 0.04% or more of the field of view is 5 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a powder for air electrode of a solid oxide fuel cell and a method for producing the same. Background Art

[0002] In recent years, fuel cells have attracted attention as a clean energy source. Among them, solid oxide fuel cells (SOFCs) that use ion-conductive solid oxides as electrolytes have excellent power generation efficiency. SOFCs have an operating temperature of up to 700°C to 1000°C and can also use exhaust heat. In addition, SOFCs can use a variety of fuels such as hydrocarbons and carbon monoxide gas, so they are expected to be widely used from household use to large-scale power generation.

[0003] SOFC usually has multiple cells, which have a porous air electrode (cathode) and a fuel electrode (anode), and an electrolyte layer between them. If air is supplied to the air electrode, a reduction reaction of the oxygen contained in the air occurs to generate oxygen ions. The oxygen ions pass through the electrolyte layer and reach the fuel electrode, reacting with the hydrogen supplied to the fuel electrode to generate water. At this time, electrons are generated at the fuel electrode and consumed at the air electrode.

[0004] In terms of commercialization of SOFC, it is hoped that the performance of a single cell will be improved and the number of cells used will be reduced to reduce costs. In order to improve the performance of a single cell, for example, high conductivity and high open porosity are required for the air electrode. In Patent Documents 1 to 4, various studies have been conducted on metal composite oxides having a perovskite crystal structure represented by ABO3 used as air electrode materials.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2009-035447

[0008] Patent Document 2: Japanese Patent Application Publication No. 2015-201440

[0009] Patent Document 3: Japanese Patent Application Publication No. 2016-139523

[0010] Patent Document 4: Japanese Patent No. 5140787 Summary of the invention

[0011] Problems to be solved by the invention

[0012] Even when the metal composite oxides described in Patent Documents 1 to 4 are used, it is difficult to obtain an air electrode having both high electrical conductivity and high open porosity.

[0013] Means for solving problems

[0014] In view of the above, one aspect of the present invention relates to a solid oxide fuel cell air electrode powder, which is of the following general formula:

[0015] A1 1-x A2 x BO 3-δ

[0016] (wherein the element A1 is at least one selected from La and Sm, the element A2 is at least one selected from Ca, Sr and Ba, the element B is at least one selected from Mn, Fe, Co and Ni, 0<x<1, δ is the oxygen vacancy amount) a powder of a metal composite oxide having a perovskite-type single-phase crystal structure represented by

[0017] When the cross-section of the molded body obtained by press-molding the powder is observed at a magnification of 500 times and the intensity of the characteristic X-ray of the element B is measured by energy dispersive X-ray analysis, the number of regions having an intensity of more than 50% of the maximum intensity of the characteristic X-ray and an area ratio of more than 0.04% of the observation field is less than 5.

[0018] Another aspect of the present invention relates to a method for producing a powder for a solid oxide fuel cell air electrode, which is produced according to the following general formula:

[0019] A1 1-x A2 x BO 3-δ

[0020] (wherein element A1 is at least one selected from La and Sm, element A2 is at least one selected from Ca, Sr and Ba, element B is at least one selected from Mn, Fe, Co and Ni, 0<x<1, δ is the oxygen vacancy amount) A method for producing a solid oxide fuel cell air electrode powder having a perovskite-type single-phase crystal structure represented by:

[0021] a slurry preparation step of mixing a plurality of metal compounds in powder form respectively including the element A1, the element A2 and the element B, and a dispersion medium to prepare a slurry having an average particle size of the metal compounds of not less than 0.5 μm and not more than 2 μm;

[0022] an adding step of adding a granulating agent to the slurry;

[0023] a drying step of removing the dispersion medium in the slurry after the adding step to obtain a dry powder; and

[0024] A calcining step, wherein the dry powder is calcined; wherein:

[0025] The total concentration of the plurality of metal compounds in the slurry supplied to the drying step is 10% by mass or more and less than 25% by mass.

[0026] Effects of the Invention

[0027] According to the present invention, an air electrode having both high electrical conductivity and high open porosity can be obtained.

[0028] The novel features of the present invention are described in the appended claims, but the present invention, both in terms of configuration and content, together with other objects and features of the present invention, will be more clearly understood from the following detailed description with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1A This is an example of a mapping image after binarization processing of the cross section of the molded body.

[0030] Figure 1B for Figure 1A Magnified view of the marked area in .

[0031] Figure 2 This is a flowchart showing an example of a production method according to one embodiment of the present invention.

[0032] Figure 3 This is the X-ray diffraction pattern of the fired powder prepared in Example 1.

[0033] Figure 4 This is a SEM image of a cross section of the molded body produced in Example 1.

[0034] Figure 5 This is a SEM image of a cross section of the molded body produced in Comparative Example 3.

[0035] Figure 6 This is a distribution image of the cross section of the molded body produced in Example 1.

[0036] Figure 7 This is a distribution image of the cross section of the molded body produced in Comparative Example 3.

[0037] Figure 8 This is a distribution image of the cross section of the molded body produced in Example 1 after binarization processing.

[0038] Fig. 9 This is a distribution image of the cross section of the molded body produced in Comparative Example 3 after binarization processing. DETAILED DESCRIPTION

[0039] The B site of the perovskite crystal structure represented by ABO3 is occupied by a transition metal that may have multiple valences. Therefore, the conductivity of the metal composite oxide having the perovskite crystal structure is easily affected by the metal element that enters the B site.

[0040] However, in terms of the analysis of the crystal structure, the X-ray diffraction method is generally used. Even in the case of a metal composite oxide that is evaluated as being composed of only a phase having a perovskite-type crystal structure (hereinafter sometimes referred to as a perovskite phase) by the X-ray diffraction method, if an electron microscope is used for fine analysis, it is sometimes possible to confirm that the metal composite oxide contains a transition metal and has a region of a crystal structure other than the perovskite phase (hereinafter sometimes referred to as a non-perovskite region). For example, in the case of using a raw material containing manganese (Mn) as a transition metal element, in the metal composite oxide, there may be a region containing spinel-type crystals caused by manganese oxide together with the perovskite phase. This is because in the process of mixing and sintering a plurality of raw materials (metal compounds) to make a metal composite oxide, a part of the raw material containing the transition metal does not contribute to the generation of the perovskite phase, but generates a non-perovskite region. It has been determined that the reduction in the electrical conductivity of the metal composite oxide is caused by: such a non-perovskite region containing a transition metal (element B) that can enter the B site occupies a certain degree of region in the metal composite oxide powder and is unevenly distributed.

[0041] The non-perovskite region of the solid oxide fuel cell air electrode powder (hereinafter sometimes referred to as air electrode powder) according to the present embodiment is uniformly dispersed to such an extent that even analysis using an electron microscope cannot confirm uneven distribution.

[0042] That is, the present embodiment relates to an air electrode powder, which is of the following general formula:

[0043] A1 1-x A2 x BO 3-δ

[0044] (wherein element A1 is at least one selected from La and Sm, element A2 is at least one selected from Ca, Sr and Ba, element B is at least one selected from Mn, Fe, Co and Ni, 0<x<1, δ is the amount of oxygen vacancy) a powder of a metal composite oxide having a perovskite-type single-phase crystal structure, wherein, when a cross-section of a molded body obtained by press-molding the powder is observed at a magnification of 500 times, and the intensity of the characteristic X-ray of element B is measured by energy dispersive X-ray analysis, the number of regions having an intensity of more than 50% of the maximum intensity of the characteristic X-ray and an area ratio of more than 0.04% of the observation field is less than 5.

[0045] The so-called air electrode powder has a perovskite single-phase crystal structure, which means that in the X-ray diffraction diagram, no peaks other than the peaks derived from the perovskite crystal phase are observed. The so-called no peaks are observed, typically, means that the intensity of the peaks other than the peaks derived from the perovskite crystal phase is below the detection limit of X-ray diffraction.

[0046] The distribution of the non-perovskite region containing the element B can be confirmed by performing elemental analysis using an electron microscope on the cross section of a molded body obtained by pressure-molding the air electrode powder. Specifically, it is as follows.

[0047] Weigh 2g of air electrode powder and 0.4g of polyvinyl alcohol aqueous solution (concentration: 10% by mass), and mix them in a mortar. Then, use a box-type dryer to stand at 110°C for 1 hour to evaporate the water, and pass it through a sieve with a mesh of 150μm to obtain a granulated powder. 0.5g of the obtained granulated powder is filled in a 10mm×5mm rectangular mold, and press-formed for 60 seconds at a molding pressure of 100MPa to obtain a molded body. At this time, the density of the molded body is preferably 3.5g / cm 3 Above and 4.5g / cm 3 When the density of the molded body is within this range, a sufficient amount of the air electrode powder can be contained in the field of observation using a scanning electron microscope, while excessive compression is suppressed to maintain the shape of the powder.

[0048] The obtained molded body is subjected to Ar ion etching for 20 hours at a voltage of 5.0 kV using a cross-section grinder (e.g., SM-09010 manufactured by JEOL Ltd.) to expose the cross section of the sample. The exposed cross section is observed using a scanning electron microscope (SEM) at a magnification of 500 times to determine the observation field (an area of ​​180 μm×240 μm). In this observation field, an energy dispersive X-ray detector (e.g., INCA X-sight manufactured by Oxford) is used to obtain a distribution image with enhanced brightness and darkness based on the intensity of the characteristic X-ray Kα of element B under the conditions shown below.

[0049] Accelerating voltage: 15 kV

[0050] Processing time: 4

[0051] Dead time: 30-40%

[0052] Resolution: 128 x 96 pixels

[0053] Scan times: 10 times

[0054] In the obtained distribution image, pixels Pa having an intensity of 50% or more of the maximum intensity and pixels Pb having an intensity of less than 50% are distinguished to obtain a binarized distribution image. In the binarized distribution image, regions R where pixels Pa have a common edge and are connected to more than 5 pixels are determined. An area ratio of 0.04% of the observation field is equivalent to 5 pixels in a distribution image of 128×96 pixels. In the observation field, when there are more than 5 regions R, it is defined that the element B is unevenly distributed.

[0055] The element B that does not contribute to the formation of the perovskite phase is not unevenly distributed but finely dispersed, so the conductivity is improved. As a result, the power generation performance of each single cell is improved. In addition, the stability of the perovskite phase at high temperatures is improved. Therefore, it can be expected that the durability of the fuel cell unit will be improved.

[0056] Figure 1A This is an example of the distribution image after binarization obtained in the above manner. Figure 1B For Figure 1A Magnified image of the marked area in . Figure 1B There are two regions R having an intensity of 50% or more of the maximum intensity and an area ratio of 0.04% or more of the observation field: a region R1 having 8 connected pixels and a region R2 having 7 connected pixels.

[0057] Element A1 is at least one selected from La (lanthanum) and Sm (samarium). Element A2 is at least one selected from Ca (calcium), Sr (strontium), and Ba (barium). Element B is at least one selected from Mn (manganese), Fe (iron), Co (cobalt), and Ni (nickel). 0<x<1 is satisfied, and δ is the oxygen vacancy amount.

[0058] Element A1 preferably contains La. The proportion of La in element A1 may also be 90 atomic % or more. Element A2 preferably contains Sr. Element A2 may also contain Sr and Ca. The proportion of Sr in element A2, or their total proportion when Sr and Ca are contained, may also be 90 atomic % or more. The atomic ratio of Ca to Sr: Ca / Sr may be greater than 0.2 and less than 4.0, or greater than 0.6 and less than 1.5. There is no particular limitation on x, for example, it may be 0.2≤x≤0.6, or it may be 0.3≤x≤0.5. Element B preferably contains Mn. The proportion of Mn in element B may also be 90 atomic % or more.

[0059] Specifically, examples of metal composite oxides include lanthanum strontium cobalt ferrite (LSCF, La 1-x1 Sr x1 Co 1- y1 Fey1 O 3-δ , 0<x1<1, 0<y1<1), lanthanum strontium hydromanganite (LSM, La 1-x2 Sr x2 MnO 3-δ , 0<x2<1), lanthanum strontium cobaltite (LSC, La 1-x3 Sr x3 CoO 3-δ , 0<x3<1), samarium strontium cobaltite (SSC, Sm 1-x4 Sr x4 CoO 3-δ , 0<x4<1), lanthanum strontium calcium manganite (LSCM, La 1-x5-y2 Sr x5 Ca y2 MnO 3-δ , 0<x5<1, 0<y2<1), etc. In particular, from the viewpoint of electrical conductivity and thermal expansion coefficient, LSM and LSCM in which element A1 is La, element A2 is Sr (and Ca), and element B is Mn are preferred.

[0060] The specific surface area of ​​the air electrode powder is not particularly limited, but the specific surface area of ​​the air electrode powder based on the BET method (BET specific surface area) is preferably 0.05 m 2 / g or more and 0.3m 2 / g or less. The specific surface area of ​​the powder used in the air electrode is less than 0.05m 2 When the air electrode powder has a BET specific surface area of ​​0.07 m / s, sintering becomes difficult during heat treatment to form the air electrode, and the strength of the electrode may be insufficient. 2 / g or more, more preferably 0.09m 2 / g or more. In addition, the specific surface area of ​​the powder used in the air electrode exceeds 0.3m 2 When the air electrode is sintered to a certain extent, the sintering may be excessive when the heat treatment is performed to form the air electrode. Therefore, the open porosity of the obtained air electrode is likely to be low, and the air diffusibility may be insufficient. The BET specific surface area of ​​the air electrode powder is more preferably 0.25 m 2 / g or less, more preferably 0.20m 2 The BET specific surface area is measured by a BET flow method in accordance with JIS Z 8830:2013.

[0061] The average particle size of the powder for the air electrode (hereinafter referred to as the sintered product D50) is not particularly limited, but is preferably greater than 10 μm and less than 35 μm. When the sintered product D50 is less than 10 μm, sintering is sometimes excessive during heat treatment to form the air electrode. Therefore, the open porosity of the obtained air electrode tends to be low, and the air diffusibility sometimes becomes insufficient. The sintered product D50 is more preferably greater than 13 μm, and further preferably greater than 16 μm. In addition, when the sintered product D50 exceeds 35 μm, sintering becomes difficult, and the strength as an electrode is sometimes insufficient. The sintered product D50 is more preferably less than 31 μm, and further preferably less than 27 μm.

[0062] The average particle size is the particle size when the cumulative volume reaches 50% in the volume-based particle size distribution measured by the laser diffraction method (the same applies below). That is, in the volume-based cumulative particle amount curve obtained by the particle size distribution measurement based on the laser diffraction method, the particle size when the cumulative amount accounts for 50% is the average particle size.

[0063] There is no particular limitation on the D10 and D90 particle sizes of the air electrode powder. D10 is the particle size when the cumulative amount accounts for 10% in the cumulative particle amount curve obtained by operating in the above manner. D90 is the particle size when the cumulative amount accounts for 90% in the cumulative particle amount curve obtained by operating in the above manner. The closer the value obtained by dividing D90 by D10 (D90 / D10) is to 1, the sharper the particle size distribution is.

[0064] D90 / D10 is not particularly limited, but is preferably 5 or less. When D90 / D10 exceeds 5, sintering becomes difficult to be performed uniformly during heat treatment to form an air electrode, and cracks may occur. Therefore, the yield rate is easily reduced. D90 / D10 is more preferably 4 or less, and further preferably 3.5 or less.

[0065] (Method for producing air electrode powder)

[0066] The air electrode powder is manufactured, for example, by the following steps: a step of uniformly mixing a plurality of metal compounds in powder form respectively containing element A1, element A2 and element B, and a dispersion medium (a slurry preparation step); a step of adding a granulating agent (an addition step); a step of removing the dispersion medium to obtain a dry powder having a uniform dispersion state and uniform particle size of the plurality of metal compounds (a drying step); and a step of reacting the plurality of metal compounds by calcining to obtain a calcined powder having a crystal structure of perovskite (a calcining step). The total concentration of the plurality of metal compounds in the slurry (the concentration of the second slurry described later) supplied to the drying step is 10% by mass or more and less than 25% by mass.

[0067] Figure 2 This is a flowchart showing an example of the manufacturing method according to the present embodiment.

[0068] Hereinafter, the manufacturing method of this embodiment will be described step by step.

[0069] (1) Slurry preparation process

[0070] The slurry is prepared by mixing a plurality of metal compounds in powder form each containing element A1, element A2, and element B, and a dispersion medium.

[0071] As metal compounds (first compounds) containing element A1, for example, lanthanum carbonate (La2(CO3)3), lanthanum hydroxide (La(OH)3), lanthanum oxide (La2O3), samarium carbonate (Sm2(CO3)3), samarium hydroxide (Sm(OH)3), samarium oxide (Sm2O3), etc. can be listed.

[0072] As metal compounds (second compounds) containing element A2, for example, strontium carbonate (SrCO3), strontium hydroxide (Sr(OH)2), calcium carbonate (CaCO3), calcium hydroxide (Ca(OH)2), barium carbonate (BaCO3), barium hydroxide (Ba(OH)2), etc. can be listed.

[0073] As metal compounds containing element B (third compounds), for example, manganese oxide (MnO2, Mn3O4, etc.), manganese carbonate (MnCO3), iron oxide (Fe2O3), cobalt oxide (Co3O4), cobalt carbonate (CoCO3), nickel oxide (NiO), nickel carbonate (NiCO3), etc. can be listed.

[0074] The dispersion medium is not particularly limited. From the viewpoint of handleability and reduction of impurities, the main component (component accounting for 50% or more of the total mass) of the dispersion medium may be water (deionized water), and preferably only water (deionized water).

[0075] The average particle size (hereinafter referred to as dispersion D50) of the metal compound contained in the slurry prepared in this step (hereinafter referred to as first slurry) is 0.5 μm or more and 2.0 μm or less.

[0076] If the dispersion D50 is less than 0.5 μm, the various metal compounds tend to segregate. Therefore, the composition of the obtained air electrode powder becomes uneven and an uneven distribution of element B occurs. The dispersion D50 is more preferably 0.7 μm or more, and further preferably 0.9 μm or more. In addition, when the dispersion D50 exceeds 2.0 μm, even after the calcination process, the reaction between the various metal compounds becomes difficult to proceed uniformly, and an uneven distribution of element B occurs in the obtained air electrode powder. The dispersion D50 is more preferably less than 1.7 μm, and further preferably less than 1.5 μm.

[0077] The dispersion D50 is calculated from the particle size distribution measured for all particles in the first slurry (that is, not distinguishing between a plurality of metal compounds and their reactants, complexes, etc.).

[0078] The viscosity of the first slurry is not particularly limited. The viscosity of the first slurry measured using a B-type viscometer at a temperature of 23°C to 27°C and a rotation speed of 60 rpm may be 1 mPa.s or more, or 3 mPa.s or more. The viscosity of the first slurry measured by the above method may be 500 mPa.s or less, or 100 mPa.s or less. The above viscosity is measured in accordance with JIS Z 8803.

[0079] In the slurry preparation step, the metal compound may be pulverized so that the dispersion D50 is within the above range. The mixing and pulverization are performed by, for example, a medium stirring type fine pulverizer such as a planetary mill.

[0080] In this step, a dispersant may be further mixed, whereby the dispersion D50 can be easily adjusted to a desired range.

[0081] The dispersant is not particularly limited, and any conventionally known dispersant may be used.

[0082] When the dispersion medium is mainly composed of water, examples of the dispersant include anionic dispersants such as polycarboxylates, polyacrylates, naphthalenesulfonic acid formalin condensate salts, alkyl sulfonates, and polyphosphates; nonionic dispersants such as polyalkylene oxides and polyoxyalkylene fatty acid esters; and cationic dispersants such as quaternary ammonium salts.

[0083] Among them, anionic dispersants are preferred. For example, polyacrylates can be used. Examples of cations that form salts include sodium ions, potassium ions, magnesium ions, ammonium ions, and calcium ions.

[0084] The amount of the dispersant added is not particularly limited. In consideration of the dispersion effect, the amount of the dispersant added is preferably 0.001 parts by mass or more and 0.075 parts by mass or less, and more preferably 0.0015 parts by mass or more and 0.01 parts by mass or less, based on 100 parts by mass of the total metal compound.

[0085] (2) Adding process

[0086] A granulating agent is added to the first slurry to prepare a second slurry.

[0087] The granulating agent makes it easy for the powders of each metal compound to stick to each other. In the slurry preparation process, the metal compound is micronized until the dispersion D50 is within the above range. That is, since the various metal compounds that have been fully micronized become easy to agglomerate with each other, the average particle size of the obtained dry powder (hereinafter referred to as the dry product D50) is controlled within the desired range, and the ratio of each metal compound contained in the obtained dry powder becomes uniform. In addition, the granulating agent makes it easy for the dry powder to become spherical. As a result, the uneven distribution of element B in the air electrode powder obtained in the subsequent calcination process is suppressed.

[0088] The granulating agent may be added before the dispersion medium in the second slurry is removed in the drying step, and may be added in the slurry preparation step. The dispersion D50 is the average particle size of the metal compound contained in the first slurry before the granulating agent is added.

[0089] The granulating agent is not particularly limited, and any conventionally known granulating agent may be used.

[0090] Examples of the granulating agent include polyvinyl alcohol, gelatin, methyl cellulose, carboxymethyl cellulose, polyvinyl pyrrolidone, and polyethylene glycol.

[0091] The amount of the granulating agent added is not particularly limited. In consideration of the granulation effect, the amount of the granulating agent added is preferably 0.2 parts by mass or more and 4 parts by mass or less, and more preferably 0.5 parts by mass or more and 3 parts by mass or less, based on 100 parts by mass of the total of the metal compound.

[0092] (3) Drying process

[0093] The second slurry is dried to remove the dispersion medium.

[0094] The total concentration of the plurality of metal compounds in the slurry (ie, the second slurry) supplied to the drying step is 10% by mass or more and less than 25% by mass relative to the total of the dispersion medium and the metal compounds.

[0095] If the total concentration of the metal compounds is less than 10% by mass, the amount of solvent relative to the metal compounds is large, so the particle size distribution of the dried product becomes broad. Thus, after the obtained dry powder is sintered, when heat treatment is performed to form an air electrode, sintering becomes difficult to be carried out uniformly, resulting in cracking. The total concentration of the metal compounds is more preferably 15% by mass or more, and more preferably 20% by mass or more. In addition, if the total concentration of the metal compounds is 25% by mass or more, the composition of the obtained air electrode powder becomes uneven, and an uneven distribution of element B occurs. The total concentration of the metal compounds is more preferably 24% by mass or less, and more preferably 23% by mass or less.

[0096] The method of drying the second slurry is not particularly limited, and may be spray drying, hot air drying, vacuum drying, evaporative drying, etc. Among them, spray drying is preferred in that the obtained dry powder is easy to become spherical. In addition, according to spray drying, the metal compound powders contained in the dry powder become more accessible to each other. Generally speaking, in the case of synthesizing a composite oxide from a mixture of multiple metal compound powders by a solid phase method, the atoms contained in each metal compound diffuse due to thermal energy, thereby obtaining a composite oxide with a novel composition and crystal structure. At this time, if the metal compound powders are closer to each other, the atoms become easier to diffuse, and it is easy to obtain a composite oxide with a uniform composition.

[0097] In the second slurry supplied to the spray dryer, the viscosity measured by using a B-type viscometer at a temperature of 23°C to 27°C and a rotation speed of 60 rpm may be, for example, 1 mPa.s or more, or 3 mPa.s or more. The above-mentioned viscosity of the second slurry may be 100 mPa.s or less, or 50 mPa.s or less.

[0098] The dried product D50 is not particularly limited, but is preferably greater than 10 μm and less than 50 μm. When the dried product D50 is less than 10 μm, the sintering of the dry powder in the sintering process tends to be excessive. Therefore, it is difficult to obtain an appropriate average particle size or particle size distribution as an air electrode powder. The dried product D50 is more preferably greater than 15 μm, and further preferably greater than 25 μm. In addition, when the dried product D50 exceeds 50 μm, the composition of the metal compounds in the dry powder will be uneven. Therefore, the composition of the obtained air electrode powder is also prone to become uneven, and uneven distribution of element B is prone to occur. The dried product D50 is more preferably less than 48 μm, and further preferably less than 45 μm.

[0099] There is no particular limitation on the ratio of the dispersion D50 to the dry matter D50. In order to easily obtain the desired dry matter D50, the ratio of the dispersion D50 to the dry matter D50: the dispersion D50 / the dry matter D50 is preferably 0.015 or more and 0.05 or less. If the dispersion D50 / the dry matter D50 is within this range, in the subsequent sintering process, the solid phase reaction between the metal compounds and the sintering between the dry powders become easy to proceed appropriately. As a result, it becomes easy to suppress the uneven distribution of the element B, and it becomes easy to suppress the open porosity of the air electrode obtained using this powder from becoming too small. The dispersion D50 / the dry matter D50 is more preferably 0.019 or more and 0.043 or less, and further preferably 0.023 or more and 0.035 or less.

[0100] The ratio of the burned product D50 to the dried product D50 is not particularly limited. The ratio of the burned product D50 to the dried product D50: burned product D50 / dried product D50 is preferably 1 or less. If the burned product D50 / dried product D50 is 1 or less, in the subsequent calcination step, it is more accurate to say that the sintering of the metal compounds contained in the dried powder is performed rather than the sintering of the dried powders. Therefore, the composition of the obtained burned powder can be expected to be more uniform.

[0101] (4) Firing process

[0102] The dried powder is calcined to obtain a metal composite oxide (powder for air electrode) containing the metal elements contained in each metal compound.

[0103] The sintering temperature is not particularly limited. From the viewpoint of promoting the diffusion of each metal element, the sintering temperature may be 1200°C or higher, or 1350°C or higher. In order to easily suppress rapid and excessive sintering, the sintering temperature may be 1500°C or lower, 1450°C or lower, or 1400°C or lower. The sintering temperature is, for example, 1350°C or higher and 1450°C or lower. If the sintering temperature is within this range, sintering between the metal compounds contained in the dry powder becomes easier than sintering between the dry powders.

[0104] Example

[0105] Hereinafter, the present invention will be specifically described by giving examples of the present invention, but these examples are not intended to limit the present invention.

[0106] First, the method of measuring or calculating the physical properties of the air electrode powder and the like will be described.

[0107] (a) Specific surface area

[0108] The specific surface area was measured by the BET flow method using a specific surface area measuring device (Flowsorb II manufactured by Micromeritics). The heat treatment was performed at 230° C. for 30 minutes in a pure nitrogen gas stream, using a mixed gas of 30% nitrogen and 70% helium as carrier gas.

[0109] (b) Particle size distribution and particle size D50, D90, D10

[0110] The sample was added to a 0.025 wt% sodium hexametaphosphate aqueous solution to adjust the concentration to a laser transmittance of 80 to 90%, and the particle size distribution was measured using a laser diffraction-scattering particle size distribution analyzer (Microtrac Bel Co., Ltd., MT-3300EXII).

[0111] In addition, in the measurement of the particle size distribution of the dispersion D50 and the calcined product D50, after the sample was added to the above-mentioned sodium hexametaphosphate aqueous solution and the concentration was adjusted in the above-mentioned manner, before the measurement, an ultrasonic homogenizer (manufactured by Nippon Seiki Seisaku-sho, US-600T) was used to perform a dispersion treatment with an output of 300 μA for 3 minutes.

[0112] The measurement conditions are as follows.

[0113] Measurement mode: MT-3300

[0114] Particle refractive index: 2.40

[0115] Solvent refractive index: 1.333

[0116] Particle shape: non-spherical

[0117] Dispersion medium: 0.025 wt% sodium hexametaphosphate aqueous solution

[0118] (c) X-ray diffraction

[0119] A diffraction pattern was obtained under the following conditions using an X-ray diffraction apparatus (RINT TTRIII manufactured by Rigaku Co., Ltd., X-ray source CuKα, tube voltage 50 kV, current 300 mA, long slit: PSA200 (total length 200 mm, resolution: 0.057 degrees).

[0120] Optical system: Parallel optical system

[0121] Measurement method: continuous measurement

[0122] Scanning speed: 5 degrees / minute

[0123] Sampling width: 0.04 degrees

[0124] Scanning range (2θ): 20 to 60 degrees

[0125] Example 1

[0126] (1) Slurry preparation process

[0127] 49.97 g of lanthanum oxide (La2O3, manufactured by Fuji Film & Wako Pure Chemical Industries, Ltd., purity 98%), 31.14 g of strontium carbonate (SrCO3, manufactured by Fuji Film & Wako Pure Chemical Industries, Ltd., purity 95%) and 68.89 g of manganese carbonate (MnCO3, manufactured by Fuji Film & Wako Pure Chemical Industries, Ltd., purity 88%) were weighed into a 500 ml resin container.

[0128] 300 ml of deionized water, 0.75 g of ammonium polyacrylate (manufactured by Fuji Film & Wako Pure Chemical Industries, Ltd., Wako Grade 1) as a dispersant, and 150 ml of zirconium oxide beads with a diameter of 1 mm were added to the above resin container, and mixed and pulverized at 180 rpm for 75 minutes using a planetary ball mill (Fritsch, P-5). Then, the beads were removed to obtain a first slurry.

[0129] In the first slurry, the dispersion D50 was 1.0 μm. The viscosity of the first slurry measured using a B-type viscometer at a temperature of 23° C. to 27° C. and a rotation speed of 60 rpm was 44 mPa·s.

[0130] (2) Adding process

[0131] Deionized water was added to the first slurry to adjust the concentration of the metal compound to 23% by mass, and then 1.50 g of polyvinyl alcohol (Fuji Film & Wako Pure Chemical Industries, Ltd., reagent special grade) was added as a granulating agent and dissolved. The viscosity of the prepared second slurry under the above measurement conditions was 7 mPa.s.

[0132] (3) Drying process

[0133] The second slurry was dried using a spray dryer (Ohkawara Chemical Industry Co., Ltd., BDP-10 Spray Bag Dryer) under the conditions of inlet temperature: 210° C., outlet temperature: 100° C., and atomizer rotation speed: 15000 rpm to obtain a dry powder.

[0134] The D50 of the dried product was 31 μm.

[0135] (4) Firing process

[0136] The dried powder was filled in an alumina crucible, and the crucible was placed in an electric furnace (SB-2025 manufactured by Motoyama Co., Ltd.), and fired at 1400°C for 2 hours at a temperature rise and fall rate of 100°C / h. Thereafter, the powder was crushed in an alumina mortar and passed through a sieve with a mesh size of 500 μm to obtain a fired powder.

[0137] From the X-ray diffraction pattern, it can be confirmed that the calcined powder has only the composition formula: La 0.6 Sr 0.4 Perovskite crystal structure represented by MnO3. Figure 3 This is an X-ray diffraction pattern of the fired powder prepared in Example 1. The peak pattern of the obtained fired powder is consistent with the peak pattern of the perovskite phase, and the peak pattern derived from other crystal phases is not observed.

[0138] The specific surface area of ​​the sintered powder is 0.18 m 2 / g, the D50 of the sintered product is 17μm, and the D90 / D10 is 3.4.

[0139] Example 2

[0140] (1) Slurry preparation process

[0141] 43.60 g of lanthanum oxide (La2O3, manufactured by Fuji Film Wako Pure Chemical Industries, Ltd., purity 98%), 20.38 g of strontium carbonate (SrCO3, manufactured by Fuji Film Wako Pure Chemical Industries, Ltd., purity 95%), 13.89 g of calcium carbonate (CaCO3, manufactured by Fuji Film Wako Pure Chemical Industries, Ltd., purity 99.5%) and 72.13 g of manganese carbonate (MnCO3, manufactured by Fuji Film Wako Pure Chemical Industries, Ltd., purity 88%) were weighed into a 500 ml resin container.

[0142] 300 ml of deionized water, 0.75 g of ammonium polyacrylate (Fuji Film Wako Pure Chemical Industries, Ltd., Wako Grade 1) as a dispersant, and 150 ml of zirconium oxide beads with a diameter of 1 mm were added to the above resin container, and mixed and pulverized at 180 rpm for 60 minutes using a planetary ball mill (Fritsch, P-5). Then, the beads were removed to obtain the first slurry.

[0143] In the first slurry, the dispersion D50 was 1.0 μm. The viscosity of the first slurry under the above-mentioned measurement conditions was 41 mPa·s.

[0144] (2) Adding process

[0145] Deionized water was added to the first slurry to adjust the concentration of the metal compound to 23% by mass, and then 1.50 g of polyvinyl alcohol (Fuji Film & Wako Pure Chemical Industries, Ltd., reagent special grade) was added as a granulating agent and dissolved. The viscosity of the prepared second slurry under the above measurement conditions was 5 mPa.s.

[0146] (3) Drying process

[0147] The second slurry was dried using a spray dryer (Ohkawara Chemical Industry Co., Ltd., BDP-10 Spray Bag Dryer) under the conditions of inlet temperature: 210° C., outlet temperature: 100° C., and atomizer rotation speed: 15000 rpm to obtain a dry powder.

[0148] The D50 of the dried product was 41 μm.

[0149] (4) Firing process

[0150] The dried powder was filled in an alumina crucible, and the crucible was placed in an electric furnace (SB-2025 manufactured by Motoyama Co., Ltd.), and fired at 1400°C for 2 hours at a temperature rise and fall rate of 100°C / h. Thereafter, the powder was crushed in an alumina mortar and passed through a sieve with a mesh size of 500 μm to obtain a fired powder.

[0151] From the X-ray diffraction pattern, it can be confirmed that the calcined powder has only the composition formula: La 0.5 Sr 0.25 Ca 0.25 Perovskite crystal structure represented by MnO3.

[0152] The specific surface area of ​​the sintered powder is 0.10 m 2 / g, D50 of the fired product was 26 μm, and D90 / D10 of the fired product was 2.7.

[0153] Comparative Example 1

[0154] (1) Slurry preparation process

[0155] A first slurry was obtained in the same manner as in Example 2 except that the amount of deionized water was changed to 64 ml and the treatment time using the planetary ball mill was changed to 185 minutes.

[0156] In the first slurry, the dispersion D50 was 1 μm. The viscosity of the first slurry under the above-mentioned measurement conditions was 23 mPa·s.

[0157] (2) Drying process

[0158] Deionized water was added to the first slurry to adjust the concentration of the metal compound to 63% by mass. No granulating agent (polyvinyl alcohol) was added to the first slurry. The viscosity of the prepared slurry under the above-mentioned measurement conditions was 13 mPa·s.

[0159] The slurry was dried in the same manner as in Example 2, except that the outlet temperature of the spray dryer was set to 75° C. and the atomizer rotation speed was set to 20,000 rpm, thereby obtaining a dry powder.

[0160] The D50 of the dried product was 36 μm.

[0161] (3) Firing process

[0162] The dry powder was calcined, crushed and screened in the same manner as in Example 2 to obtain a calcined powder.

[0163] From the X-ray diffraction pattern, it can be confirmed that the calcined powder has only the composition formula: La 0.5 Sr 0.25 Ca 0.25 Perovskite crystal structure represented by MnO3.

[0164] The specific surface area of ​​the above powder is 0.15m 2 / g, D50 of the fired product was 20 μm, and D90 / D10 of the fired product was 5.6.

[0165] Comparative Example 2

[0166] (1) Slurry preparation process

[0167] A first slurry was obtained in the same manner as in Example 2 except that the amount of deionized water added was 150 ml and zirconia beads having a diameter of 3 mm were used.

[0168] In the first slurry, the dispersion D50 was 2.2 μm. The viscosity of the first slurry under the above-mentioned measurement conditions was 31 mPa·s.

[0169] (2) Adding process

[0170] Deionized water was added to the first slurry to adjust the solid content concentration to 23% by mass, and then 1.50 g of polyvinyl alcohol (Fuji Film & Wako Pure Chemical Industries, Ltd., reagent special grade) was added as a granulating agent and dissolved. The viscosity of the prepared second slurry under the above measurement conditions was 5 mPa.s.

[0171] (3) Drying process

[0172] A dry powder was obtained in the same manner as in Example 2 except that the outlet temperature of the spray dryer was set to 75°C.

[0173] The D50 of the dried product was 41 μm.

[0174] (4) Firing process

[0175] The dry powder was calcined, crushed and screened in the same manner as in Example 2 to obtain a calcined powder.

[0176] From the X-ray diffraction pattern, it can be confirmed that the calcined powder has only the composition formula: La 0.5 Sr 0.25 Ca 0.25 Perovskite crystal structure represented by MnO3.

[0177] The specific surface area of ​​the above powder is 0.19m 2 / g, the D50 of the fired product was 27 μm, and the D90 / D10 of the fired powder was 3.0.

[0178] Comparative Example 3

[0179] 54.28 g of lanthanum carbonate (La2(CO3)3, manufactured by Fuji Film Wako Pure Chemical Industries, Ltd., purity 99.5%), 18.33 g of strontium carbonate (SrCO3, manufactured by Fuji Film Wako Pure Chemical Industries, Ltd., purity 95%), 12.49 g of calcium carbonate (CaCO3, manufactured by Fuji Film Wako Pure Chemical Industries, Ltd., purity 99.5%) and 64.89 g of manganese carbonate (MnCO3, manufactured by Fuji Film Wako Pure Chemical Industries, Ltd., purity 88%) were weighed into the reaction container of a sample mill (SK-M10, manufactured by Kyoritsu Chemical Industry Co., Ltd.), mixed and pulverized at a motor speed of 14000 rpm for 60 seconds to obtain a raw material mixed powder.

[0180] The average particle size (dried product D50) of the raw material mixed powder was 13 μm.

[0181] The raw material mixed powder was fired, crushed and screened in the same manner as in Example 2 except that the firing temperature was set to 1450° C., thereby obtaining a fired powder.

[0182] From the X-ray diffraction pattern, it can be confirmed that the calcined powder has only the composition formula: La 0.5 Sr 0.25 Ca 0.25 Perovskite crystal structure represented by MnO3.

[0183] The specific surface area of ​​the above powder is 0.20m 2 / g, the D50 of the calcined product was 32 μm, and the D90 / D10 of the calcined powder was 6.1.

[0184] Comparative Example 4

[0185] (1) Slurry preparation process

[0186] The same operation as in Example 2 was carried out to obtain a first slurry.

[0187] In the first slurry, the dispersion D50 was 1.0 μm. The viscosity of the first slurry under the above-mentioned measurement conditions was 41 mPa·s.

[0188] (2) Drying process

[0189] Deionized water was added to the first slurry to adjust the concentration of the metal compound to 23% by mass. No granulating agent (polyvinyl alcohol) was added to the slurry. The viscosity of the prepared slurry under the above-mentioned measurement conditions was 4 mPa·s.

[0190] The prepared slurry was dried in the same manner as in Example 2 to obtain a dry powder.

[0191] The D50 of the dried product was 4.1 μm.

[0192] (3) Firing process

[0193] The dry powder was calcined, crushed and screened in the same manner as in Example 2 to obtain a calcined powder.

[0194] From the X-ray diffraction pattern, it can be confirmed that the calcined powder has only the composition formula: La 0.5 Sr 0.25 Ca 0.25 Perovskite crystal structure represented by MnO3.

[0195] The specific surface area of ​​the above powder is 0.34m 2 / g, the D50 of the fired product was 13 μm, and the D90 / D10 of the fired powder was 10.4.

[0196] The following evaluations were performed on the fired powders obtained in Examples 1 and 2 and Comparative Examples 1 to 4. The results are shown in Table 1.

[0197] (A) Segregation state of Mn

[0198] Weigh 2 g of the calcined powder and 0.4 g of a polyvinyl alcohol aqueous solution (concentration: 10% by mass), and mix them in a mortar. Then, use a box-type dryer to stand at 110°C for 1 hour to evaporate the water, and pass it through a sieve with a mesh of 150 μm to obtain a granulated powder. Fill 0.5 g of the obtained granulated powder into a 10 mm × 5 mm rectangular mold, and press mold for 60 seconds at a molding pressure of 100 MPa to obtain a molded body. The density of the molded body is 3.6 to 4.1 g / cm 3 .

[0199] The molded body was subjected to Ar ion etching for 20 hours at a voltage of 5.0 kV using a cross-section grinder (SM-09010 manufactured by JEOL Ltd.) to expose the cross section of the sample.

[0200] The exposed cross section was observed using a SEM at a magnification of 500 times, and the observation field (area of ​​180 μm×240 μm) was determined. The SEM image of Example 1 is shown in FIG. Figure 4 , the SEM image of Comparative Example 3 is shown in Figure 5 In this observation field, an energy dispersive X-ray detector (Inca X-sight manufactured by Oxford) was used to obtain a distribution image with emphasized brightness and darkness based on the intensity of the characteristic X-rays of Mn-Kα under the following conditions. The distribution image of Example 1 is displayed on Figure 6 , the distribution image of Comparative Example 3 is displayed on Figure 7 .

[0201] Accelerating voltage: 15 kV

[0202] Processing time: 4

[0203] Dead time: 30-40%

[0204] Resolution: 128 x 96 pixels

[0205] Scan times: 10 times

[0206] In the obtained distribution image, pixels Pa having an intensity of 50% or more of the maximum intensity and pixels Pb having an intensity of less than 50% are distinguished to obtain a binarized distribution image. The binarized distribution image of Example 1 is displayed on Figure 8 , the binarized distribution image of Comparative Example 3 is displayed on Fig. 9 In the binarized distribution image, regions R where pixels Pa share an edge and are connected to five or more pixels are identified as locations where Mn is unevenly distributed, and their number is counted.

[0207] (B) Open porosity

[0208] Weigh 10g of the calcined powder and 0.2g of a polyvinyl alcohol aqueous solution (concentration: 10% by mass) and mix them in a mortar. Then, use a box-type dryer to stand at 110°C for 1 hour to evaporate the water, and pass through a sieve with a mesh of 150μm to obtain a granulated powder. The obtained granulated powder is filled in a 46mm×6mm rectangular mold, and pressure-formed for 60 seconds at a molding pressure of 100MPa to obtain a molded body of 46mm in length×6mm in width×6mm in height. The obtained molded body is placed on an alumina plate, and an electric furnace is used to sinter it in the atmosphere at 1200°C for 2 hours to obtain a sintered sample.

[0209] The open porosity (P) of the sintered sample was measured according to JIS R 1634. Specifically, the dry weight, the weight in water, and the weight saturated with water of the sintered sample were measured by the method described in JIS R 1634, and the open porosity was calculated using the following formula.

[0210] P=(W3-W1) / (W3-W2)×100

[0211] Where, P: open porosity (%)

[0212] W1: dry weight (g)

[0213] W2: Weight in water (g)

[0214] W3: Full water weight (g)

[0215] (C) Electrical conductivity

[0216] The electrical conductivity (S1) at 800° C. of the sintered sample obtained in the same manner as above was measured by a four-probe method in accordance with JIS R 1661.

[0217] Specifically, platinum paste (TR-7907 manufactured by Tanaka Precious Metals Co., Ltd.) is applied symmetrically along the width direction of the sintered sample relative to the center line that bisects the length direction to make two voltage terminals. The coating width is 2 mm, and the separation distance between the voltage terminals is set to 20 mm. Next, the same platinum paste as above is applied from a position 5 mm away from the voltage terminal to the end in the length direction to make two current terminals. Furthermore, a platinum wire with a diameter of 0.3 mm is wound around each terminal to make a lead-out electrode. The sintered sample with each terminal formed thereon is mounted on a heating sample holder (probostat manufactured by Norex) and heated at 800°C for 2 hours in an electric furnace. Thereby, the platinum paste is sintered to the sintered sample to obtain a four-terminal unit. The obtained four-terminal unit is used to measure the conductivity (S1) at 800°C by an electrochemical measurement system (ModuLab XM manufactured by Solartron).

[0218] The electrical conductivity (S) of the sintered sample was calculated by the following formula using the open porosity (P) and the electrical conductivity (S1) measured at 800°C.

[0219] S=S1 / ﹛(100-P)×100﹜

[0220] Where, S: conductivity

[0221] S1: Electrical conductivity measured at 800°C

[0222] P: Open porosity (%)

[0223] Table 1

[0224]

[0225] In the table, the numerical values ​​described as the viscosity of the second slurry in Comparative Examples 1 and 4 are the viscosities of the slurries containing no granulating agent prepared in the drying step.

[0226] As can be seen from Table 1, the number of regions R of uneven distribution of Mn in the molded body obtained from the fired powder (powder for air electrode) obtained in Examples 1 and 2 is less than 5. In addition, the open porosity P of the sintered sample obtained from the above-mentioned fired powder is 29-30%, and the electrical conductivity S is 183-193S / cm, which has both good open porosity and high electrical conductivity. In addition, the specific surface area of ​​the above-mentioned fired powder satisfies 0.05m 2 / g or more and 0.3m 2 / g or less, and the fired product D50 is 10 μm or more and 35 μm or less. In addition, since the fired product D50 / dried product D50 is less than 1, it is considered that the reaction inside the dry powder mainly proceeds in the firing step.

[0227] The specific surface area and average particle size of the fired powder obtained in Comparative Example 1 are equivalent to those of the fired powder obtained in Examples 1 and 2. However, it is found that the molded body obtained from the fired powder obtained in Comparative Example 1 has more than 5 regions R where Mn is unevenly distributed, and the non-perovskite region is unevenly distributed. In addition, the electrical conductivity S of the sintered sample obtained from the fired powder is lower than that of Examples 1 and 2.

[0228] In Comparative Example 1, in the slurry preparation process, the metal compound is fully mixed until it becomes 1 μm, and on the other hand, no granulating agent is added, and the slurry with a concentration of the metal compound of 25% by mass or more is supplied to the drying process. Therefore, it is believed that the ratio of each metal compound contained in the dry powder becomes uneven. In addition, the adhesion between the metal compound powders in the dry powder is also weak. Therefore, it is believed that in the subsequent calcination process, a sufficient solid phase reaction to make the composition uniform is not carried out.

[0229] The molded bodies obtained from the fired powders obtained in Comparative Examples 2 and 3 also have more than 5 regions R where Mn is unevenly distributed, and the non-perovskite regions are unevenly distributed. In addition, the electrical conductivity S of the sintered samples obtained from these fired powders is lower than that of Examples 1 and 2.

[0230] The reason for Comparative Example 2 is that the average particle size of the dispersion in the slurry preparation step was larger than 2 μm. In other words, the metal compound was not sufficiently refined in the slurry preparation step, so the composition of the obtained fired powder was considered to be non-uniform.

[0231] In Comparative Example 3, the metal compounds were mixed by a dry method without preparing a slurry, so the metal compounds were not sufficiently refined and mixed, and as a result, it is considered that the composition of the obtained fired powder became uneven. In addition, in Comparative Example 3, the firing temperature was made higher than that of Examples 1 and 2, so that a perovskite-type crystal structure was obtained. That is, it is also shown that the solid-phase reactivity of the dry powder obtained in Comparative Example 3 is low.

[0232] The molded body obtained from the fired powder obtained in Comparative Example 4 also has more than 5 regions R where Mn is unevenly distributed, and the non-perovskite region is unevenly distributed. In addition, the electrical conductivity S and open porosity of the sintered sample obtained from the fired powder are lower than those of Examples 1 and 2.

[0233] In Comparative Example 4, fine mixing is performed in the slurry preparation process until the metal compound becomes 1 μm, and on the other hand, no granulating agent is added. Therefore, in the dry powder, the adhesion between the metal compounds is weak, and it is believed that in the subsequent firing process, a sufficient solid phase reaction to make the composition uniform is not carried out. In addition, the fired product D50 / dried product D50 is greater than 1, so it is believed that sintering between the dry powders occurs in the firing process. That is, it is believed that in the firing process, the heat energy given to the dry powder is not only used for the solid phase reaction between the metal compounds, but also for the sintering between the dry powders. As a result, the composition of the obtained fired powder becomes uneven, and at the same time, D90 / D10 is large, and the particle size distribution of the fired powder becomes wide. If a fired powder with a wide particle size distribution is used to make an air electrode, the fired powder is sintered in a dense state where small particles are filled in the gaps between large particles, so the open porosity tends to become low.

[0234] Possibility of industrial application

[0235] The metal composite oxide of the present invention has excellent electrical conductivity and is therefore suitable as a powder for an air electrode of a solid oxide fuel cell.

[0236] Although the present invention has been described with respect to the present preferred embodiments, such disclosure is not to be construed as limiting. A person skilled in the art of the art to which the present invention belongs will be able to accurately understand various modifications and changes by reading the above disclosure. Therefore, the appended claims should be interpreted as including all modifications and changes without departing from the true spirit and scope of the present invention.

Claims

1. A powder for air electrode of a solid oxide fuel cell, which is a powder of a metal composite oxide having a perovskite-type single-phase crystal structure represented by the following general formula: <h2 style=";text-align:left;direction:ltr">A1<h2 style=";text-align:left;direction:ltr"> 1-x <h2 style=";text-align:left;direction:ltr"> A2<h2 style=";text-align:left;direction:ltr"> x <h2 style=";text-align:left;direction:ltr"> BO<h2 style=";text-align:left;direction:ltr"> 3-δ in, Element A1 is at least one selected from La and Sm, element A2 is at least one selected from Ca, Sr and Ba, element B is at least one selected from Mn, Fe, Co and Ni, 0<x<1, δ is the oxygen vacancy amount; When the intensity of the characteristic X-ray of the element B is measured by energy dispersive X-ray analysis when observing the cross section of the molded body obtained by press-molding the powder at a magnification of 500 times, the number of regions having an intensity of 50% or more of the maximum intensity of the characteristic X-ray and having an area ratio of 0.04% or more of the observation field is 5 or less; The molded body is obtained by the following method: 2 g of the powder and 0.4 g of a polyvinyl alcohol aqueous solution with a concentration of 10% by mass are weighed, mixed in a mortar, and then allowed to stand at 110°C for 1 hour in a box-type dryer to evaporate the water, and granulated powder is obtained by passing through a sieve with a mesh of 150 μm. 0.5 g of the obtained granulated powder is filled in a 10 mm×5 mm rectangular mold, and press-molded for 60 seconds at a molding pressure of 100 MPa.

2. The solid oxide fuel cell air electrode powder according to claim 1, in, The element A1 includes La, The element A2 contains Sr, The element B includes Mn.

3. The solid oxide fuel cell air electrode powder according to claim 1, in, The specific surface area of ​​the powder based on the BET method is 0.05 m 2 / g or more and 0.3m 2 / g or less.

4. The solid oxide fuel cell air electrode powder according to any one of claims 1 to 3, in, The average particle size of the powder is 10 μm or more and 35 μm or less.

5. A method for producing a powder for a solid oxide fuel cell air electrode, which is a method for producing a powder for a solid oxide fuel cell air electrode according to any one of claims 1 to 4; The manufacturing method comprises: a slurry preparation step of mixing a plurality of metal compounds in powder form respectively including the element A1, the element A2 and the element B, and a dispersion medium to prepare a slurry having an average particle size of the metal compounds of not less than 0.5 μm and not more than 2 μm; an adding step of adding a granulating agent to the slurry; a drying step of removing the dispersion medium in the slurry after the adding step to obtain a dry powder; and A calcining step, which is to calcine the dry powder; in, The total concentration of the plurality of metal compounds in the slurry supplied to the drying step is 10% by mass or more and less than 25% by mass.

6. The method for producing a powder for a solid oxide fuel cell air electrode according to claim 5, in, In the slurry preparation step, a dispersant is further mixed.

7. The method for producing a powder for a solid oxide fuel cell air electrode according to claim 5, in, The average particle size of the dry powder obtained in the drying step is 10 μm or more and 50 μm or less.

8. The method for producing a powder for a solid oxide fuel cell air electrode according to claim 5, in, A ratio of an average particle size of the metal compound contained in the slurry obtained in the slurry preparation step to an average particle size of the dry powder obtained in the drying step is 0.015 or more and 0.05 or less.

9. The method for producing a powder for a solid oxide fuel cell air electrode according to claim 5, in, The firing temperature in the firing step is 1200° C. or higher and 1500° C. or lower.

10. The method for producing a powder for a solid oxide fuel cell air electrode according to any one of claims 5 to 9, in, In the drying step, the dispersion medium is removed by spray drying.