All-solid-state secondary battery
By adding boron to the 3LiOH·Li2SO4 solid electrolyte, the problem of reducing lithium ion conductivity at high temperature is solved, and a stable lithium ion conductivity from room temperature to high temperature is achieved, which is suitable for all-solid secondary batteries.
Patent Information
- Application Number
- CN201980092643.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-26
- Filing Date
- 2019-10-24
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2039-10-24
AI Technical Summary
The existing Li2SO4-LiOH solid electrolytes are prone to decrease in lithium ion conductivity at high temperatures, and cannot maintain sufficient lithium ion conductivity from room temperature to high temperature range.
The 3LiOH·Li2SO4 solid electrolyte containing boron was used to identify by X-ray diffraction and maintain the lithium ion conductivity for a long time, thereby improving the maintenance of the ion conductivity.
It significantly suppresses the reduction of lithium ion conductivity at high temperatures, ensures the stability and efficiency of lithium ion conductivity, and is suitable for lithium ion secondary batteries and capacitors.
Smart Images

Figure GDA0004877057850000081
Abstract
Description
Technical Field
[0001] The present invention relates to an all-solid secondary battery. Background Art
[0002] In recent years, research and development of solid electrolytes used in storage elements such as lithium-ion secondary batteries and capacitors has been actively carried out. In particular, it is expected to develop a solid electrolyte that can maintain sufficient lithium ion conductivity from room temperature to high temperature. Here, the following scheme is proposed in non-patent document 1, that is, Li2SO4 and LiOH are homogeneously melted, quenched, and a solidified body is obtained, and the solidified body is used as a solid electrolyte. In particular, the solid electrolyte can be used for devices that operate at low temperatures.
[0003] Prior art literature
[0004] Non-patent literature
[0005] Non-patent document 1: VKDESHPANDE, FCRAGHUWANSHI AND K. SINGH, "ELECTRICAL CONDUCTIVITY OF THE Li2SO4-LiOH SYSTEM", Solid State Ionics 18&19 (1986) 378-381 Summary of the invention
[0006] However, it cannot be said that the lithium ion conductivity of the solid electrolyte described in non-patent document 1 is sufficiently high at room temperature. In addition, the temperature dependence of the conductivity of the solid electrolyte of non-patent document 1 is low, and the conductivity increase effect brought about by the temperature increase cannot be expected. That is, the solid electrolyte cannot be said to be a material with sufficient lithium ion conductivity from room temperature to high temperature. In response to these problems, the inventors of the present invention have obtained the following insight, namely, the solid electrolyte represented by 3LiOH·Li2SO4 exhibits a higher lithium ion conductivity at 25°C. However, it is known that there are other problems, namely, when the material of the above composition is kept at high temperature for a long time, the lithium ion conductivity is easily reduced.
[0007] The inventors of the present invention have recently found that by further containing boron in a solid electrolyte identified as 3LiOH·Li 2 SO 4 , a decrease in lithium ion conductivity can be significantly suppressed even after being kept at a high temperature for a long period of time.
[0008] Therefore, an object of the present invention is to provide an all-solid secondary battery having a 3LiOH·Li 2 SO 4 -based solid electrolyte capable of significantly suppressing a decrease in lithium ion conductivity even after being kept at a high temperature for a long period of time.
[0009] According to one aspect of the present invention, there is provided an all-solid secondary battery, wherein a solid electrolyte identified as 3LiOH·Li 2 SO 4 by X-ray diffraction is used, and the solid electrolyte further contains boron. DETAILED DESCRIPTION
[0010] Solid Electrolyte
[0011] The solid electrolyte used in the all-solid secondary battery of the present invention is a solid electrolyte identified as 3LiOH·Li2SO4 by X-ray diffraction. And, the solid electrolyte also contains boron. By making the solid electrolyte identified as 3LiOH·Li2SO4 further contain boron, the reduction of lithium ion conductivity can be significantly suppressed even after being kept at high temperature for a long time. That is, as described above, the inventors of the present invention have obtained the following insight, that is, the solid electrolyte represented by 3LiOH·Li2SO4 exhibits a higher lithium ion conductivity at 25°C. However, it is known that there are other problems, that is, when the above composition is kept at high temperature for a long time, the lithium ion conductivity is easily reduced. In this regard, the above problem can be solved by making the solid electrolyte identified as 3LiOH·Li2SO4 further contain boron. The mechanism by which the ion conductivity maintenance degree can be improved by containing boron is still uncertain. According to X-ray diffraction measurement, the diffraction peak of 3LiOH·Li2SO4 is slightly shifted to the high-angle side by containing boron. From this point, it is speculated that boron enters any site in the crystal structure of 3LiOH·Li2SO4, thereby improving the stability of the crystal structure with respect to temperature.
[0012] Therefore, the solid electrolyte used in the present invention is preferably used for storage elements such as lithium ion secondary batteries and capacitors, and is particularly preferably used for lithium ion secondary batteries. The lithium ion secondary battery can be an all-solid battery (for example, an all-solid lithium ion secondary battery). In addition, the lithium ion secondary battery can be a liquid battery (for example, a lithium-air battery) using a solid electrolyte as a separator and having an electrolyte between the separator and the opposing electrode.
[0013] As described above, the solid electrolyte used in the present invention is a solid electrolyte identified as 3LiOH·Li2SO4 by X-ray diffraction. That is, the solid electrolyte contains 3LiOH·Li2SO4 as the main phase. Whether 3LiOH·Li2SO4 is contained in the solid electrolyte can be confirmed by identifying it using 032-0598 of the ICDD database in the X-ray diffraction pattern. Here, "3LiOH·Li2SO4" means: a substance whose crystal structure is considered to be the same as 3LiOH·Li2SO4, and the crystal composition does not necessarily need to be the same as 3LiOH·Li2SO4. That is, it is sufficient to have a crystal structure equivalent to 3LiOH·Li2SO4, and substances whose composition deviates from LiOH:Li2SO4=3:1 are also included in the solid electrolyte of the present invention. Therefore, even if it is a solid electrolyte containing boron (for example, 3LiOH·Li2SO4 in which boron solid solution causes the X-ray diffraction peak to move to the high angle side), as long as the crystal structure is considered to be the same as 3LiOH·Li2SO4, it is 3LiOH·Li2SO4 mentioned in this specification. Likewise, the solid electrolyte used in the present invention is also allowed to contain inevitable impurities.
[0014] Therefore, in addition to 3LiOH·Li2SO4 as the main phase, the solid electrolyte may also contain a heterogeneous phase. The heterogeneous phase may contain a plurality of elements selected from Li, O, H, S and B, or may be composed only of a plurality of elements selected from Li, O, H, S and B. As examples of heterogeneous phases, LiOH, Li2SO4 and / or Li3BO3 derived from raw materials can be cited. These heterogeneous phases are considered to be substances remaining from unreacted raw materials when 3LiOH·Li2SO4 is formed. However, since they are not helpful for conducting lithium ions, their amount is expected to be small except for Li3BO3. However, considering that it may help to improve the maintenance of lithium ion conductivity after high temperature and long-term maintenance, a heterogeneous phase containing boron such as Li3BO3 may be contained in a desired amount. However, the solid electrolyte may also be composed of a single phase of 3LiOH·Li2SO4 in which boron is solid-dissolved.
[0015] The solid electrolyte used in the present invention also contains boron. The molar ratio (B / S) of boron B contained in the solid electrolyte to sulfur S is preferably greater than 0.002 and less than 1.0, more preferably 0.003 or more and 0.9 or less, and further preferably 0.005 or more and 0.8 or less. If the boron content is a small amount, the maintenance rate of lithium ion conductivity at high temperature is reduced, but if the B / S is within the above range, the maintenance rate of lithium ion conductivity can be improved. In addition, if the boron content is high, it is possible to reduce the absolute value of lithium ion conductivity, but if the B / S is within the above range, the content of unreacted heterogeneous phases containing boron is reduced, and therefore, the absolute value of lithium ion conductivity can be increased.
[0016] The solid electrolyte used in the present invention is identified as 3LiOH·Li2SO4 in the X-ray diffraction pattern with CuKα as the radiation source. The half-value width of the peak near 2θ=18.4° is preferably 0.500° or less, more preferably 0.400° or less, and further preferably 0.200° or less. If it is in such a range, the lithium ion conductivity maintenance rate after high temperature and long-term maintenance can be further improved. The smaller the above half-value width, the higher the crystallinity, so it is preferred that the lower limit is not particularly limited, and is typically 0.08° or more, and more typically 0.1° or more.
[0017] The solid electrolyte used in the present invention is identified as a peak intensity I near 2θ=20.5° of LiOH in the X-ray diffraction pattern using CuKα as the radiation source. LiOH The peak intensity I near 2θ=18.4° identified as 3LiOH·Li2SO4 LHS The ratio of I LiOH / I LHS It is preferably less than 0.234, more preferably 0.230 or less, and further preferably 0.200 or less. If LiOH is high, the absolute value of lithium ion conductivity may decrease, but if it is within the above range, the content of LiOH decreases, so the absolute value of lithium ion conductivity can be increased.
[0018] The solid electrolyte of the present invention is identified as having a peak intensity I near 2θ=22.2° of Li2SO4 in the X-ray diffraction pattern using CuKα as the radiation source. Li2SO4 The peak intensity I near 2θ=18.4° identified as 3LiOH·Li2SO4 LHS The ratio of I Li2SO4 / I LHS It is preferably less than 1.10, more preferably less than 0.50, and further preferably less than 0.20. If Li2SO4 is high, the absolute value of lithium ion conductivity may decrease, but if it is within the above range, the content of Li2SO4 decreases, thereby increasing the absolute value of lithium ion conductivity.
[0019] The solid electrolyte used in the present invention may be a powder compact obtained by pulverizing a molten solidified body, and is preferably a molten solidified body (ie, a substance obtained by heating, melting, and then solidifying).
[0020] Manufacturing method
[0021] According to a preferred embodiment of the present invention, the solid electrolyte used in the present invention can be manufactured by the following process, that is, a raw material containing LiOH, Li2SO4 and Li3BO3 is melted and cooled to form a solidified body. From the viewpoint of ionic conductivity, the raw material used at this time preferably has a composition represented by xLiOH·Li2SO4·yLi3BO3 (wherein, 2.0≤x≤4, 0.002≤y≤1), as long as the desired characteristics are obtained, and it is not limited to this (for example, it can be 1.0≤x≤4). For example, the manufacture of the solid electrolyte can be carried out as follows, that is, (a) a solidified body is formed by cooling a melt of a raw material containing LiOH, Li2SO4 and Li3BO3 (preferably a raw material of the above composition); (b) a solid electrolyte powder is made by pulverizing the solidified body; (c) a solid electrolyte is formed by molding the solid electrolyte powder or by cooling and solidifying the solid electrolyte powder after melting it again. The cooling of the melt in (a) above can be any of quenching or annealing (for example, furnace cooling). The pulverization method in the above (b) can be carried out by placing spherical stones such as zirconia balls and a solid electrolyte in a container and pulverizing them according to known methods and conditions. The molding in the above (c) step can be carried out by various methods such as pressing (for example, metal mold pressing, cold isostatic pressing), preferably metal mold pressing. The cooling rate when cooling after re-melting the solid electrolyte powder in the above (c) step is preferably 10 to 1000°C / h, more preferably 10 to 100°C / h.
[0022] All-solid-state secondary battery
[0023] As described above, the solid electrolyte used in the present invention is preferably used in an all-solid secondary battery. That is, according to a preferred embodiment of the present invention, an all-solid secondary battery using the above-mentioned solid electrolyte is provided. The all-solid secondary battery has the solid electrolyte of the present invention between the positive electrode and the negative electrode. Moreover, at least a part or all of the solid electrolyte constitutes a lithium ion conductive material layer.
[0024] The positive electrode may be a positive electrode commonly used in lithium secondary batteries, preferably comprising a lithium composite oxide. The lithium composite oxide is composed of Li x An oxide represented by MO2 (0.05<x<1.10, M is at least one transition metal, M typically includes one or more of Co, Ni, Mn and Al). The lithium composite oxide preferably has a layered rock salt structure or a spinel structure. Examples of lithium composite oxides having a layered rock salt structure include: Li x CoO2 (lithium cobalt oxide), Li x NiO2 (lithium nickel oxide), Li x MnO2 (lithium manganate), Li x NiMnO2 (nickel manganese oxide), Lix NiCoO2 (lithium nickel cobalt oxide), LixCoNiMnO2 (lithium cobalt nickel manganese oxide), Li x CoMnO2 (lithium cobalt manganese oxide), Li2MnO3 and solid solutions thereof. Li x CoNiMnO2 (Cobalt Nickel Manganese Oxide) and Li x CoO2 (lithium cobalt oxide, typically LiCoO2). Examples of lithium composite oxides having a spinel structure include LiMn2O4-based materials, LiNi 0.5 Mn 1.5 O4 series materials, etc.
[0025] The lithium composite oxide may contain one or more elements selected from Mg, Al, Si, Ca, Ti, V, Cr, Fe, Cu, Zn, Ga, Ge, Sr, Y, Zr, Nb, Mo, Ag, Sn, Sb, Te, Ba, Bi and W. In addition, LiMPO4 (wherein M is at least one selected from Fe, Co, Mn and Ni) having an olivine structure may also be preferably used.
[0026] The positive electrode may be a mixture of a positive electrode active material, an electron conduction aid, a lithium ion conductive material, and a binder, which is generally referred to as a composite electrode, or may be a sintered plate obtained by sintering a positive electrode raw material powder. The sintered plate may be a dense body or a porous body, and may also contain a solid electrolyte in the pores of the porous body. In addition, a protective layer for suppressing the reaction between the positive electrode and the solid electrolyte or a layer for reducing the interface resistance may be introduced between the positive electrode active material and the solid electrolyte.
[0027] As the negative electrode, a negative electrode commonly used in lithium secondary batteries can be used. Examples of such common negative electrode materials include: carbon-based materials; metals or semimetals such as Li, In, Al, Sn, Sb, Bi, and Si; or alloys containing any of them. In addition, an oxide-based negative electrode can be used.
[0028] A particularly preferred negative electrode comprises a + ) The material for inserting and deintercalating lithium ions preferably contains Ti. The negative electrode active material that meets the above conditions is preferably an oxide containing at least Ti. As a preferred example of such a negative electrode active material, there can be cited: lithium titanate Li4Ti5O 12(hereinafter referred to as LTO), niobium titanium composite oxide Nb2TiO7, titanium oxide TiO2, more preferably LTO and Nb2TiO7, and even more preferably LTO. It should be noted that LTO is known to be a material with a typical spinel structure, and other structures can also be used during charging and discharging. For example, LTO is Li4Ti5O 12 (spinel structure) and Li7Ti5O 12 Therefore, LTO is not limited to the spinel structure.
[0029] The negative electrode may be a mixture of a negative electrode active material, an electron conduction aid, a lithium ion conductive material, and a binder, which is generally referred to as a composite electrode, or may be a sintered plate obtained by sintering a negative electrode raw material powder. The sintered plate may be a dense body or a porous body, and may contain a solid electrolyte in the pores of the porous body. In addition, a protective layer for suppressing the reaction between the negative electrode and the solid electrolyte, or a layer for reducing the interface resistance may be introduced between the negative electrode active material and the solid electrolyte.
[0030] The manufacture of an all-solid secondary battery can be carried out as follows, for example, i) preparing a positive electrode with a current collector and a negative electrode with a current collector; and ii) sandwiching a solid electrolyte between the positive electrode and the negative electrode, applying pressure, heating, etc., to integrate the positive electrode, the solid electrolyte and the negative electrode. The positive electrode, the solid electrolyte and the negative electrode can also be combined by other methods. In this case, as an example of a method for forming a solid electrolyte between the positive electrode and the negative electrode, there can be cited: a method of placing a molded body or powder of a solid electrolyte on one electrode, a method of applying a paste of a solid electrolyte powder on an electrode by screen printing, a method of using an electrode as a substrate and using an aerosol deposition method to solidify the powder of the solid electrolyte, and a method of depositing a solid electrolyte powder on an electrode by electrophoresis to form a film, etc.
[0031] Example
[0032] The present invention will be further specifically described by the following examples.
[0033] Examples 1 to 17
[0034] (1) Preparation of raw material powder
[0035] Li2SO4 powder (commercial product, purity 99% or more), LiOH powder (commercial product, purity 98% or more) and Li3BO3 (commercial product, purity 99% or more) were mixed in the molar ratio shown in Table 1 to obtain a raw material mixed powder. These powders were handled in an Ar atmosphere with a dew point of -50°C or less, and sufficient care was taken to prevent moisture absorption and other deterioration.
[0036] (2) Melt synthesis
[0037] The raw material mixed powder was placed in a crucible made of high-purity alumina in an Ar atmosphere, and the crucible was placed in an electric furnace and heat treated at 430° C. for 2 hours to produce a melt. The melt was then cooled at 100° C. / h in the electric furnace to form a solid.
[0038] (3) Mortar grinding
[0039] The obtained solidified product was pulverized in an Ar atmosphere using a mortar, thereby obtaining a solid electrolyte powder having an average particle size D50 of 5 to 50 μm.
[0040] (4) Melting
[0041] In a glove box in an Ar atmosphere, the solid electrolyte powder was pressed into a metal mold at a pressure of 250 MPa to form a granular solid electrolyte with a diameter of 10 mm. The granular solid electrolyte was sandwiched between two stainless steel (SUS) electrodes with a diameter of 10 mm and a thickness of 0.5 mm, and a 15 g weight was placed on the obtained stack, and heated at 400 ° C for 45 minutes to melt the solid electrolyte. Then, the melt was cooled at 100 ° C / h to form a solidified body.
[0042] (5) Evaluation
[0043] The obtained solidified body (solid electrolyte) was evaluated as follows.
[0044] <X-ray diffraction>
[0045] The solid electrolyte is analyzed using an X-ray diffraction device (XRD, X-ray source: CuKα rays) to obtain an X-ray diffraction pattern. It should be noted that metal Si powder is added as an internal standard and aligned to the 2θ position. The obtained X-ray diffraction pattern is compared with 032-0598 of the ICDD database to identify the 3LiOH·Li2SO4 crystal phase and determine the presence or absence of 3LiOH·Li2SO4. In addition, based on the XRD spectrum obtained above, the half-value width of the peak near 2θ=18.4° identified as 3LiOH·Li2SO4 is calculated. Furthermore, the peak intensity I near 2θ=20.5° identified as LiOH is calculated. LiOH The peak intensity I near 2θ=18.4° identified as 3LiOH·Li2SO4 LHS The ratio (I LiOH / I LHS ). Similarly, the peak intensity I near 2θ = 22.2° identified as Li2SO4 was calculated. Li2SO4The peak intensity I near 2θ=18.4° identified as 3LiOH·Li2SO4 LHS The ratio (I Li2SO4 / I LHS ). The results are shown in Table 1.
[0046] <Ionic conductivity and conductivity retention after 100 hours at 150°C>
[0047] The lithium ion conductivity of the solid electrolyte is measured by conventional AC impedance measurement as follows. First, in an Ar atmosphere, the solid electrolyte is clamped between two stainless steel (SUS) electrodes and placed in a battery (manufactured by Hohsen Co., Ltd., button battery CR2032) for sealing to make a battery for ion conductivity measurement. The battery for ion conductivity measurement is placed in a constant temperature dryer at 150°C, and the conductivity (1 / r) is measured using an AC impedance measurement device (manufactured by BioLogic, VMP3) using the AC impedance method. Based on the measured value and the formula of lithium ion conductivity σ=L / r(1 / A), the initial lithium ion conductivity C0 is calculated.
[0048] In addition, after the solid electrolyte was kept at 150° C. for 100 hours in the above-mentioned battery for measuring ion conductivity, the lithium ion conductivity C1 was measured in the same manner as above. The lithium ion conductivity C1 of the solid electrolyte after being kept at 150° C. for 100 hours was divided by the initial lithium ion conductivity C0 and multiplied by 100 to obtain the conductivity retention rate (%) after being kept at 150° C. for 100 hours.
[0049] <Chemical Analysis>
[0050] The solid electrolyte obtained in each example was subjected to quantitative analysis of boron and sulfur. Boron and sulfur were quantitatively analyzed by ICP atomic emission spectrometry (ICP-AES) using the calibration curve method. Each analysis value of boron and sulfur was converted into moles and calculated as B / S.
[0051] result
[0052] The preparation conditions and evaluation results of the solid electrolytes of Examples 1 to 17 are summarized in Table 1. In Examples 1 to 17, in the process of synthesizing the solid electrolyte by melting the raw material mixed powder containing LiOH, Li2SO4 and Li3BO3 and the process of melting the solid electrolyte powder again, the weight loss was very small, as low as less than 1%, and it is estimated that the composition of Li, O, H, S and B constituting the solid electrolyte was almost unchanged compared with the composition at the time of preparation.
[0053] [Table 1]
[0054]
[0055] The results of Table 1 are described in detail. The main phases of the X-ray diffraction patterns of Examples 1 to 17 are consistent with 032-0598 of the ICDD database, which shows that there is a 3LiOH·Li2SO4 crystal phase. The main phase referred to here refers to: peaks that are not attributed to LiOH, Li2SO4 and Li3BO3. It should be noted that, in particular, in examples containing boron at high concentrations, high-angle shifts in the X-ray diffraction pattern of the 3LiOH·Li2SO4 crystal phase are seen. For example, the peak of 2θ=18.43° of 3LiOH·Li2SO4 in Example 5 where Li3BO3 is not added is 18.46° in Example 2 where Li3BO3 is added. The peak shifts to the high-angle side, and it is inferred that boron is dissolved in the skeleton of the 3LiOH·Li2SO4 crystal phase. In addition to the high-angle shift, it is consistent with 032-0598 of the ICDD database, and it can be seen that it contains a solid electrolyte identified as 3LiOH·Li2SO4. In addition, in Examples 1 to 4, 6 to 10, and 12 to 17 in which Li 3 BO 3 was added for synthesis, chemical analysis showed that B / S was a value greater than 0, which shows that the solid electrolyte contained boron.
[0056] It can be seen that the ion conductivity maintenance rate of Examples 5 and 11 without boron is as low as 75% or less, and the ion conductivity maintenance rate is increased to 80% or more by setting B / S to 0.002 or more as in Example 10. In addition, the ion conductivity of Examples 1 and 3 after being kept at 150°C for 100 hours is compared, and it can be seen that the conductivity of Example 1 is lower. It is speculated that this is because the content of unreacted heterogeneous phases increases due to the large amount of Li3BO3 added, and it can be seen that B / S, which represents the amount of boron added, is preferably less than 1.0.
[0057] In addition, the ion conductivity of Examples 3, 8, and 12 detected by XRD after being kept at 150°C for 100 hours is compared. It can be seen that the ion conductivity of Examples 3 and 8 is higher than that of Example 12. If we focus on the peak intensity ratio (I LiOH / I LHS ), and the value in Example 12 is larger, from which it is inferred that LiOH remains as a different phase, and it is inferred that this hinders ion conduction. Based on the above, it is believed that: when LiOH is detected as a different phase, the peak intensity ratio (I LiOH / I LHS ) is preferably less than 0.234. In addition, by comparing the ion conductivity of Example 14 and Example 17 after holding at 150°C, in which Li2SO4 was detected by XRD, it can be seen that the ion conductivity of Example 14 is higher than that of Example 17. If we focus on the peak intensity ratio (I Li2SO4 / I LHS), and the value of Example 17 is larger, which indicates that Li2SO4 remains as a heterogeneous phase, and it is assumed that this hinders ion conduction. It is therefore believed that when Li2SO4 is detected as a heterogeneous phase, the peak intensity ratio (I Li2SO4 / I LHS ) is preferably less than 1.1.
[0058] In addition, if we focus on Examples 3, 8, 14, and 17, we can see the following. Here, the raw material mixing ratios of these examples are all in the range represented by xLiOH·Li2SO4·yLi3BO3 (wherein, 1.0≤x≤4, 0.002≤y≤1), and the Li2SO4:Li3BO3 ratio is 1:0.05, so it is possible to see the change in characteristics caused by changing only the molar ratio of LiOH (x in the above formula). Then, it can be seen that although Examples 3, 8, 14, and 17 all obtain the desired results in terms of conductivity retention after being kept at 150°C for 100 hours, the ion conductivity of Examples 3, 8, and 14 with x=3, 2.6, and 2 is higher than the ion conductivity of Example 17 with x=1.0. Therefore, it can be said that from the perspective of ion conductivity, the range of 2.0≤x≤4, 0.002≤y≤1 is an ideal range.
[0059] <Production of all-solid-state secondary batteries>
[0060] All-solid secondary batteries were made using the solid electrolytes of Examples 3 and 5, and the resistance increase rate after being kept at 150°C for 100 hours was confirmed. As the positive electrode, a dense sintered plate of lithium cobalt oxide with a collector layer formed on one side was prepared, and as the negative electrode, a dense sintered plate of lithium titanate with a collector layer formed on one side was prepared. The powder compact of the solid electrolyte was sandwiched between the above-mentioned positive and negative plates, and the battery was formed while being pressurized. The obtained battery was left to stand at 150°C and AC impedance was measured. As the resistance of the solid electrolyte part, the resistance R0 just after the temperature was raised to 150°C and the resistance R1 after being kept at 150°C for 100 hours were measured. The resistance increase rate R1 / R0 was calculated based on the obtained resistance value. As a result, it was 1.0 in Example 3 (an example in which boron was added), and 1.3 in Example 5 (a comparative example in which boron was not added). It can be seen that the resistance increase in the all-solid secondary battery using the electrolyte in which boron was added to 3LiOH·Li2SO4 was smaller. From this, it can be seen that in the battery of Example 5, after 100 hours at 150°C, the charge and discharge capacity decreases due to the increase in resistance of the solid electrolyte part. However, in the battery of Example 3, even after 100 hours at 150°C, there is no decrease in capacity due to the increase in resistance of the solid electrolyte part, and charging and discharging can be carried out.
Claims
1. An all-solid secondary battery, wherein: A solid electrolyte identified as 3LiOH·Li2SO4 by X-ray diffraction is used, and the solid electrolyte also contains boron. The raw material used to manufacture the solid electrolyte has a composition represented by xLiOH·Li2SO4·yLi3BO3, where 1.0≤x≤4 and 0.002≤y≤1.
2. The all-solid secondary battery according to claim 1, wherein: A molar ratio of the boron B to sulfur S contained in the solid electrolyte, namely, B / S, exceeds 0.002 and is less than 1.
0.
3. The all-solid secondary battery according to claim 1 or 2, wherein: In the X-ray diffraction pattern of the solid electrolyte using CuKα as a radiation source, the half-value width of the peak near 2θ=18.4° identified as 3LiOH·Li2SO4 is 0.500° or less.
4. The all-solid secondary battery according to claim 1 or 2, wherein: The solid electrolyte was identified as having a peak intensity I near 2θ=20.5° of LiOH in the X-ray diffraction pattern using CuKα as the radiation source. LiOH The peak intensity I near 2θ=18.4° identified as 3LiOH·Li2SO4 LHS The ratio of I LiOH / I LHS Less than 0.
234.
5. The all-solid secondary battery according to claim 1 or 2, wherein: The solid electrolyte was identified as having a peak intensity I near 2θ=22.2° of Li2SO4 in the X-ray diffraction pattern using CuKα as the radiation source. Li2SO4 The peak intensity I near 2θ=18.4° identified as 3LiOH·Li2SO4 LHS The ratio of I Li2SO4 / I LHS Less than 1.
10.
6. The all-solid secondary battery according to claim 1 or 2, wherein: The solid electrolyte is a molten solid.
7. The all-solid secondary battery according to claim 1 or 2, wherein: The solid electrolyte is provided between the positive electrode and the negative electrode.