Organic-inorganic composite resin and method for producing the same
A composite resin of poly(meth)acrylic acid chain and polyorganosiloxane chain is formed by using alkoxysilane with low radical reactivity functional group and (meth)acrylate monomer to perform hydrolysis/dehydration condensation and free radical polymerization. , solves the gelation and stability problems and achieves high-quality coating performance.
Patent Information
- Application Number
- CN202080024097.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-28
- Filing Date
- 2020-03-26
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2040-03-26
AI Technical Summary
The existing organic-inorganic composite resin composed of polysiloxane and acrylic silicone resin has difficulty in gelling during the manufacturing process and lacks storage stability, transparency or gloss, and performs poorly in paints containing pigments.
Alkoxysilane with low radical reactivity functional group and (meth)acrylate monomer are used to carry out hydrolysis/dehydration condensation reaction and free radical polymerization to form an organic combination of poly(meth)acrylic acid chain and polyorganosiloxane chain. Inorganic composite resin, bonded through hydrocarbon groups and controlling reaction conditions to inhibit gelation.
It achieves a coating film that is easy to manufacture, has excellent storage stability, has good transparency or gloss, has high miscibility with pigments, and has excellent toning properties and weather resistance.
Smart Images

Figure BDA0003276961310000251 
Figure BDA0003276961310000252 
Figure BDA0003276961310000261
Abstract
Description
Technical Field
[0001] The present invention relates to an organic-inorganic composite resin, a method for producing the same, a curable resin composition containing the composite resin, and a cured product thereof. Background Art
[0002] As a resin component constituting a curable composition that can be used as a coating and showing curability, various resins have been studied. Among them, as a coating for the purpose of realizing the long life of the coating, particularly high weather resistance, high heat resistance, known polysiloxane-based coatings. Polysiloxane refers to a curable resin formed by hydrolyzing / dehydration condensation reaction of an organic alkoxysilane. The siloxane bond forming the resin is energetically strong, so polysiloxane has the characteristic of being difficult to decompose due to heat or ultraviolet rays. However, the softness of the coating obtained is low, and there is a problem of cracks being easily generated due to the curing shrinkage of the coating, and a problem of low adhesion for various substrates.
[0003] On the other hand, acrylic silicone coatings based on acrylic resins having hydrolyzable silyl groups are also known. The coating film obtained by acrylic silicone coatings is flexible and does not easily crack. However, the coating film has a problem of low weather resistance.
[0004] In order to provide a coating that has both the advantages of polysiloxane-based coatings and the advantages of acrylic silicon-based coatings, it is considered to mix the two coatings. However, if only polysiloxane-based coatings and acrylic silicon-based coatings are mixed, the compatibility of the two resins is low, so there are difficulties such as reduced storage stability of the coating, or phase separation of the coating film formed by the mixed coating, and the coating film becomes cloudy and the transparency is reduced. In this case, the interface generated inside the coating film becomes a cause, and there is also a problem of easy deterioration.
[0005] Therefore, studies have been conducted on the formation of composites of polysiloxane and acrylic silicon. For example, Patent Document 1 describes a method for producing a composite resin by reacting organopolysiloxane and acrylic silicon in the presence of an acid catalyst through a hydrolysis / dehydration condensation reaction of reactive silicon groups of both resins.
[0006] Patent Document 2 discloses that a composite resin is produced by hydrolyzing and condensing a silane compound having a polymerizable unsaturated group such as a (meth)acryloyl group and a silane compound having an epoxy group, and reacting the resulting cocondensate with a polymerizable monomer such as a (meth)acrylic monomer.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: International Publication No. 2017 / 169459
[0010] Patent Document 2: International Publication No. 2016 / 052636 Summary of the invention
[0011] Problems to be solved by the invention
[0012] Patent Document 1 describes an organic-inorganic composite resin obtained by compounding a polysiloxane resin with an acrylic resin. The production of the composite resin involves a reaction of bonding different polymers. Therefore, the grafting rate cannot be sufficiently increased, and the storage stability, transparency and gloss of the coating film cannot be sufficiently improved. In particular, when the coating is made into a pigment-containing coating, the gloss of the coating film cannot be sufficiently improved. In addition, the acrylic resin as a raw material must have a reactive silicon group. In addition, in order to prepare a composition of an acrylic resin with high compatibility with the polysiloxane resin, methyl methacrylate must be used as a main monomer, and there is a tendency that the types of monomers constituting the acrylic resin are limited.
[0013] In addition, in Patent Document 2, an alkoxysilane having a (meth)acryloyl group is used to form a polyorganosiloxane chain, and therefore, the radical reactivity of the group is too high, and therefore, gelation is easily performed during radical polymerization, which tends to make manufacturing difficult. In addition, the organic-inorganic composite resin described in Patent Document 2 has an epoxy group as an essential functional group, and therefore, exhibits curability by being used in combination with a photoacid generator.
[0014] In view of the above-mentioned current situation, an object of the present invention is to provide a novel organic-inorganic composite resin which can suppress gelation during production, is easy to produce, has excellent storage stability, and can form a coating film with excellent transparency or gloss, and a method for producing the same.
[0015] Solutions to the problem
[0016] The inventors of the present invention have conducted in-depth research to solve the above problems. As a result, it was found that a radical reactive functional group having a radical reactivity lower than the growth reactivity of a methacryloyl group in a radical polymerization without a (meth)acryloyl group as disclosed in Patent Document 2 was used in a manner that satisfies a specific range of the radical reactive functional group equivalent, and a polyorganosiloxane was obtained. In the presence of the polyorganosiloxane, a radical polymerizable monomer such as a (meth)acrylate monomer was subjected to radical polymerization, thereby enabling the manufacture of a novel organic-inorganic composite resin. It was also found that in the manufactured novel organic-inorganic composite resin, the poly(meth)acrylic acid chain and the polyorganosiloxane chain were bonded only via a hydrocarbon group, and there was a reactive silicon group on the polyorganosiloxane chain. It was found that the above problems could be solved by the above method, and the present invention was completed.
[0017] That is, the present invention relates to a method for producing an organic-inorganic composite resin, the method comprising:
[0018] A step of subjecting the alkoxysilane component to hydrolysis and dehydration condensation reaction in the presence of water and a condensation catalyst to obtain polyorganosiloxane; and
[0019] a step of subjecting a radically polymerizable monomer component containing a (meth)acrylate monomer to radical polymerization in the presence of the polyorganosiloxane;
[0020] The above alkoxysilane component contains:
[0021] a monoorganotrialkoxysilane and / or a diorganodialkoxysilane (a-1) having a radical-reactive functional group showing a radical reactivity lower than the growth reactivity of a methacryloyl group in radical polymerization, and
[0022] a monoorganotrialkoxysilane and / or a diorganodialkoxysilane (a-2) having no radically reactive functional group,
[0023] The radical reactive functional group showing a radical reactivity lower than the growth reactivity of the methacryloyl group in radical polymerization contains at least a vinyl group,
[0024] The ratio of (a-2) to the total of (a-1) and (a-2) is 70% by weight or more and 99% by weight or less, and 50% by weight or more of the organic groups contained in (a-2) are at least one selected from the group consisting of methyl, ethyl, and phenyl groups,
[0025] The radical reactive functional group equivalent calculated from the alkoxysilane component is within the range of 280 or more and less than 5000,
[0026] The amount of water added is 30 mol% or more and 60 mol% or less relative to 100% of the total molar number of alkoxy groups directly bonded to silicon atoms contained in the alkoxysilane component,
[0027] The organic-inorganic composite resin contains a poly(meth)acrylic acid chain and a polyorganosiloxane chain.
[0028] It is preferred that 50% by weight or more of the organic groups contained in (a-2) are methyl groups.
[0029] It is preferred that the ratio of the monoorganotrialkoxysilane and / or diorganodialkoxysilane having a vinyl group to the entire alkoxysilane component is 2% by weight or more and 30% by weight or less.
[0030] It is preferred that the polyorganosiloxane having a reactive silicon group is obtained by the above-mentioned hydrolysis and dehydration condensation reaction.
[0031] It is preferred that the weight ratio of the polyorganosiloxane chain to the entire organic-inorganic composite resin is 20% by weight or more and 80% by weight or less.
[0032] It is preferred that the temperature of the reaction system be controlled so that the temperature does not substantially decrease from the hydrolysis and dehydration condensation reaction to the completion of the radical polymerization.
[0033] The above-mentioned free radical polymerization is preferably carried out in the presence of a β-dicarbonyl compound.
[0034] The hydrolysis and dehydration condensation reactions and the radical polymerization are preferably carried out in an atmosphere substantially free of oxygen molecules.
[0035] The present invention also relates to an organic-inorganic composite resin comprising: a poly(meth)acrylic acid chain; and a polyorganosiloxane chain bonded to the poly(meth)acrylic acid chain.
[0036] The weight ratio of the polyorganosiloxane chain to the total weight of the organic-inorganic composite resin is 20% by weight or more and 80% by weight or less.
[0037] The polyorganosiloxane chain is a hydrolysis condensation product of an alkoxysilane component containing 70 to 100 mol % of a monoorganotrialkoxysilane and 30 to 0 mol % of a diorganodialkoxysilane.
[0038] The polyorganosiloxane chain has a reactive silicon group.
[0039] The carbon atoms in the monomer units constituting the poly(meth)acrylic acid chain and the silicon atoms in the polyorganosiloxane chain are bonded only via hydrocarbon groups.
[0040] The above hydrocarbon group contains at least ethylene,
[0041] The ratio of the monoorganotrialkoxysilane and / or diorganodialkoxysilane (a-2) having no radical reactive functional group to the total of the monoorganotrialkoxysilane and the diorganodialkoxysilane is 70% by weight or more and 99% by weight or less,
[0042] 50% by weight or more of the organic groups contained in (a-2) are at least one selected from the group consisting of a methyl group, an ethyl group, and a phenyl group.
[0043] It is preferred that the structural units derived from the monoorganotrialkoxysilane be classified into structural units T1 having one siloxane bond, structural units T2 having two siloxane bonds, and structural units T3 having three siloxane bonds, and 29When the ratio (%) of each mole number of T1, T2, and T3 to the total mole number of T1, T2, and T3 measured by Si-NMR is X, Y, and Z, respectively, the siloxane bond formation rate calculated by the following formula is 60% or more and 80% or less:
[0044] (1×X+2×Y+3×Z) / 3.
[0045] It is preferred that the solubility parameter value (SP value) of the poly(meth)acrylic acid chain is 9.0 to 11.0 (cal / cm 3 ) 1 / 2 .
[0046] Furthermore, the present invention relates to a curable resin composition containing the above-mentioned organic-inorganic composite resin, or a cured product obtained by curing the curable resin composition.
[0047] Effects of the Invention
[0048] According to the present invention, there can be provided a novel organic-inorganic composite resin which can suppress gelation during production, is easy to produce, has excellent storage stability, and can form a coating film having excellent transparency or gloss, and a method for producing the same.
[0049] The organic-inorganic composite resin according to a preferred embodiment of the present invention has a reactive silicon group and can therefore be cured by a hydrolysis / dehydration condensation reaction of the reactive silicon group.
[0050] The organic-inorganic composite resin of the preferred embodiment of the present invention generally has excellent storage stability even when constituting a coloring paint containing a pigment whose gloss and storage stability of the coating film are easily reduced, and can form a coating film with excellent gloss. In addition, the organic-inorganic composite resin of the preferred embodiment of the present invention has high miscibility with pigments and dyes, and can achieve excellent color matching properties.
[0051] Furthermore, according to the present invention, the type of monomer constituting the poly(meth)acrylic acid chain can be selected from a plurality of options, and there is also an advantage that the degree of freedom in designing the poly(meth)acrylic acid chain is high.
[0052] Furthermore, in the organic-inorganic composite resin of a preferred embodiment of the present invention, the poly(meth)acrylic acid chain and the polyorganosiloxane chain are bonded only via a hydrocarbon group, not via a heteroatom-containing group such as an ester group such as a (meth)acryloyl group. Therefore, the resin is not easily affected by main chain cleavage caused by hydrolysis or photooxidation, and excellent weather resistance can be expected. DETAILED DESCRIPTION
[0053] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to these embodiments.
[0054] (Method for producing organic-inorganic composite resin)
[0055] First, a method for producing an organic-inorganic composite resin according to an embodiment of the present invention will be described.
[0056] (Hydrolysis and dehydration condensation reaction)
[0057] In the production method of the present invention, firstly, the hydrolysis and dehydration condensation reaction of the alkoxysilane component is carried out to obtain a polyorganosiloxane. The alkoxysilane component used in the present invention contains at least a monoorganotrialkoxysilane and / or a diorganodialkoxysilane (a-1) having a free radical reactive functional group, and a monoorganotrialkoxysilane and / or a diorganodialkoxysilane (a-2) not having a free radical reactive functional group. Hereinafter, they are sometimes referred to as alkoxysilane (a-1) and alkoxysilane (a-2), respectively.
[0058] Alkoxysilane (a-1) is an alkoxysilane having a radical reactive functional group but not having an acryloyl group or a methacryloyl group as an organic group on a silicon atom. As the radical reactive functional group, a radical reactive functional group showing a radical reactivity lower than the growth reactivity of a methacryloyl group in radical polymerization is selected. By using such a radical reactive functional group, bonding of a poly(meth)acrylic acid chain and a polyorganosiloxane chain can be achieved, gelation during the manufacture of an organic-inorganic composite resin can be suppressed, and the storage stability of the organic-inorganic composite resin can be improved.
[0059] The radical reactive functional group showing a radical reactivity lower than the growth reactivity of the methacryloyl group in the free radical polymerization contains at least a vinyl group. It should be noted that the vinyl group described here refers to a vinyl group directly bonded to the silicon atom, not to the vinyl group contained in the allyl group and the p-phenylene group. The radical reactive functional group can be only a vinyl group, or a vinyl group and at least one group selected from the allyl group, the p-phenylene group, and the thiol group can be used in combination. Such a radical reactive functional group is preferably directly bonded to the silicon atom of the alkoxysilane (a-1). By using such a radical reactive functional group, it is possible to realize the bonding of the poly (meth) acrylic acid chain and the polyorganosiloxane chain only via the hydrocarbon group, and the gelation during manufacture is suppressed, and the storage stability of the organic-inorganic composite resin can be improved. In order to realize the bonding of the poly (meth) acrylic acid chain and the polyorganosiloxane chain only via the hydrocarbon group, it is preferred not to use an alkoxysilane containing an ester group such as an acryl group, a methacryloyl group, an ether bond group such as an ethyleneoxy group, etc.
[0060] In addition, the alkoxysilane (a-1) may be a monoorganotrialkoxysilane, a diorganodialkoxysilane, or both, but preferably a monoorganotrialkoxysilane. Here, the monoorganotrialkoxysilane refers to a silane compound having one organic group and three alkoxy groups as substituents on the silicon atom, and the diorganodialkoxysilane refers to a silane compound having two organic groups and two alkoxy groups as substituents on the silicon atom.
[0061] The organic group possessed by the alkoxysilane (a-1) refers to an organic group other than an alkoxy group, and its specific examples are not particularly limited. For example, in addition to the above-mentioned vinyl, allyl, p-phenylene group, and mercapto group, alkyl groups having 1 to 6 carbon atoms, aryl groups having 6 to 12 carbon atoms such as phenyl, etc. can also be listed. The above-mentioned alkyl and aryl groups may be unsubstituted groups, or may have non-radical reactive substituents such as glycidyloxy and epoxycyclohexyl. The above-mentioned alkyl group having 1 to 6 carbon atoms refers to methyl, ethyl, propyl, butyl, pentyl, or hexyl. The number of carbon atoms of the above-mentioned alkyl group is preferably 1 to 5, more preferably 1 to 4, further preferably 1 to 3, and further preferably 1 to 2. As the above-mentioned organic group, only one type may be present, or two or more types may be mixed.
[0062] The alkoxy group of the alkoxysilane (a-1) is not particularly limited, and examples thereof include alkoxy groups having 1 to 3 carbon atoms. Specifically, methoxy groups, ethoxy groups, and propoxy groups are preferred, and methoxy groups and ethoxy groups are more preferred, with methoxy groups being more preferred. The alkoxy groups may be present alone or in combination of two or more.
[0063] Specific examples of alkoxysilane (a-1) are not particularly limited, and examples thereof include vinyl trimethoxysilane, vinyl triethoxysilane, vinyl methyl dimethoxysilane, vinyl methyl diethoxysilane, divinyl dimethoxysilane, divinyl diethoxysilane; allyl trimethoxysilane, allyl triethoxysilane, allyl methyl dimethoxysilane, allyl methyl diethoxysilane; p-phenylene trimethoxysilane, p-phenylene triethoxysilane, p-phenylene methyl dimethoxysilane, p-phenylene methyl diethoxysilane; 3-mercaptopropyl trimethoxysilane, 3-mercaptopropyl triethoxysilane, 3-mercaptopropyl methyl dimethoxysilane, 3-mercaptopropyl methyl diethoxysilane, etc. Among them, monoorganotrialkoxysilane and / or diorganodialkoxysilane having a vinyl group are preferred, and vinyltrialkoxysilane is more preferred.
[0064] When the amount of the monoorganotrialkoxysilane and / or diorganodialkoxysilane having a vinyl group is small, gelation during production can be suppressed, and when the amount is large, the grafting rate of the poly(meth)acrylic acid chain and the polyorganosiloxane chain can be increased, thereby improving the transparency and gloss of the coating film. From these viewpoints, the proportion of the monoorganotrialkoxysilane and / or diorganodialkoxysilane having a vinyl group relative to the overall alkoxysilane component is preferably 2% by weight or more and 30% by weight or less, more preferably 3% by weight or more and 28% by weight or less, and further preferably 4% by weight or more and 25% by weight or less.
[0065] The alkoxysilane (a-2) is an alkoxysilane having no radically reactive functional group such as a (meth)acryloyl group or a vinyl group, and may be a monoorganotrialkoxysilane, a diorganodialkoxysilane, or both, but is preferably a monoorganotrialkoxysilane.
[0066] The organic group as a substituent on the silicon atom in the alkoxysilane (a-2) refers to an organic group other than an alkoxy group that does not contain a radically reactive functional group. Specific examples thereof are not particularly limited, and examples thereof include: an alkyl group having 1 to 6 carbon atoms, an aryl group having 6 to 12 carbon atoms such as a phenyl group, and the like. The above-mentioned alkyl group and aryl group may be an unsubstituted group, or may have a non-radical reactive substituent such as a glycidyloxy group and an epoxycyclohexyl group. The above-mentioned alkyl group having 1 to 6 carbon atoms refers to a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, or a hexyl group. The number of carbon atoms of the above-mentioned alkyl group is preferably 1 to 5, more preferably 1 to 4, further preferably 1 to 3, and further preferably 1 to 2. As the above-mentioned organic group, there may be only one kind, or two or more kinds may be mixed.
[0067] As the organic group possessed by alkoxysilane (a-2), it is preferably selected from at least one of methyl, ethyl and phenyl. In this case, the total of methyl, ethyl and phenyl possessed by (a-2) is preferably 50% by weight or more, more preferably 70% by weight or more, and more preferably 80% by weight or more relative to the overall proportion of the organic group. The upper limit of this ratio can be 100% by weight. For the purpose of curability increasing when the organic-inorganic composite resin manufactured is used as the main component of the coating liquid, the organic group possessed by (a-2) more preferably contains methyl and / or ethyl, and more preferably contains methyl. And then preferably contains methyl and / or ethyl and phenyl, particularly preferably contains methyl and phenyl. By using phenyl in combination, it is easy to suppress the gelation during the free radical polymerization described later, and the storage stability of the organic-inorganic composite resin and the transparency and gloss of the coating film can be taken into account at a high level.
[0068] In a particularly preferred embodiment, from the viewpoint of curability, the proportion of the methyl group possessed by (a-2) relative to the organic group as a whole is preferably 50% by weight or more, more preferably 70% by weight or more, and further preferably 80% by weight or more. The upper limit of the proportion of the methyl group can be 100% by weight, but when an ethyl group and / or a phenyl group are used in combination as described above, it is preferably 99% by weight or less. When an ethyl group and / or a phenyl group are used in combination, the proportion of the ethyl group and / or a phenyl group possessed by (a-2) relative to the organic group as a whole is preferably 0 to 45% by weight.
[0069] Examples of the alkoxy group which the alkoxysilane (a-2) has as a substituent on the silicon atom include the same groups as those mentioned above with respect to the alkoxysilane (a-1).
[0070] Specific examples of the alkoxysilane (a-2) include, but are not particularly limited to, methyltrimethoxysilane, methyltriethoxysilane, methyltriisopropoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, ethyltriisopropoxysilane, propyltrimethoxysilane, propyltriethoxysilane, propyltriisopropoxysilane, butyltrimethoxysilane, butyltriethoxysilane, butyltriisopropoxysilane, hexyltrimethoxysilane, hexyltriethoxysilane, hexyltriisopropoxysilane, etc. Examples of the diorganodialkoxysilane include, for example, dimethyldimethoxysilane, dimethyldiethoxysilane, methylphenyldimethoxysilane, methylphenyldiethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, vinylmethyldimethoxysilane, vinylmethyldiethoxysilane, cyclohexylmethyldimethoxysilane, cyclohexylmethyldiethoxysilane, etc.
[0071] As a specific example of the alkoxysilane (a-2) with the above-mentioned glycidyloxy group, epoxycyclohexyl group, etc., epoxy group, for example, 3-glycidyloxypropyl trimethoxysilane, 3-glycidyloxypropyl triethoxysilane, 3-glycidyloxypropyl methyl dimethoxysilane, 8-glycidyloxyoctyl trimethoxysilane, 2-(3,4-epoxycyclohexyl) ethyl trimethoxysilane, etc. can be cited. By using such an alkoxysilane with an epoxy group, the molecular weight of the obtained organic-inorganic composite resin can be increased. In the case of using an alkoxysilane with an epoxy group, its amount is preferably 0.1% by weight or more in terms of the ratio relative to the overall alkoxysilane component. Moreover, its amount is preferably 20% by weight or less, more preferably 15% by weight or less, and further preferably 10% by weight or less. However, it is also possible not to use an alkoxysilane with an epoxy group, in which case the transparency and gloss of the coating film obtained using the organic-inorganic composite resin can be improved.
[0072] As the alkoxysilane (a-2), it is particularly preferred to use at least one selected from methyltrialkoxysilane, ethyltrialkoxysilane, and phenyltrialkoxysilane. In this case, the total proportion of methyltrialkoxysilane, ethyltrialkoxysilane, and phenyltrialkoxysilane relative to the entire alkoxysilane component is preferably 70% by weight or more, more preferably 80% by weight or more.
[0073] In addition, as alkoxysilane (a-2), methyltrialkoxysilane is particularly preferably used. In this case, relative to the overall alkoxysilane component, the proportion occupied by methyltrialkoxysilane is preferably more than 40% by weight and less than 100% by weight, more preferably more than 40% by weight and less than 95% by weight, further preferably more than 45% by weight and less than 95% by weight, particularly preferably more than 50% by weight and less than 95% by weight, most preferably more than 50% by weight and less than 90% by weight. Since in organic alkoxysilane, the silicon content of the condensate of methyltrialkoxysilane is the highest, therefore, the more methyltrialkoxysilane is relative to the overall content of the alkoxysilane component, the easier it is for the polyorganosiloxane chain manufactured to show the effect peculiar to inorganic resins, thus preferably. In the past, when the content of methyltrialkoxysilane became more, it became easy to gel during manufacturing, but according to the manufacturing method of the present invention, the gelation can be suppressed.
[0074] The alkoxysilane component used in the present invention contains the radical reactive functional group possessed by the alkoxysilane (a-1) and the alkoxy group on the silicon atom possessed by the alkoxysilane (a-1) and the alkoxysilane (a-2), but the content ratio of the compound of the alkoxysilane component is set in a manner that its content ratio is within a specific range. In the present invention, the radical reactive functional group equivalent is used as an indicator representing the content ratio of the radical reactive functional group and the alkoxy group in the alkoxysilane component. Under the assumption that all the alkoxy groups on the silicon atoms contained in the alkoxysilane component are converted into siloxane bonds by hydrolysis / dehydration condensation reaction to generate polysiloxane, the radical reactive functional group equivalent is a value calculated in the form of the molecular weight of the polysiloxane per one radical reactive functional group. The specific calculation method is described in one of the embodiments described later.
[0075] In the present invention, the free radical reactive functional group equivalent calculated according to the alkoxysilane component used as a raw material satisfies more than 280 and less than 5000. It should be noted that the free radical reactive functional group equivalent has a small value, which means that the relative amount of the free radical reactive functional group is large. On the contrary, the free radical reactive functional group equivalent has a large value, which means that the relative amount of the free radical reactive functional group is small. When the free radical reactive functional group equivalent is less than the above range, during the free radical polymerization described later, gelation is carried out and the manufacture of the organic-inorganic composite resin becomes difficult. Even if it can be manufactured, there is a tendency that the storage stability of the resin is reduced. On the contrary, when the free radical reactive functional group equivalent is greater than the above range, although the molecular weight of the organic-inorganic composite resin obtained can be reduced, in the free radical polymerization described later, the bonding of the poly(methyl)acrylic acid chain and the polyorganosiloxane chain cannot be fully carried out, and phase separation occurs in the coating film, and there is a tendency that the transparency and gloss of the coating film are reduced.
[0076] Within the above range, the smaller the free radical reactive functional group equivalent is, the higher the grafting rate of the poly(meth)acrylic acid chain and the polyorganosiloxane chain is, which can improve the compatibility of the organic resin and the inorganic resin, the storage stability of the coating, and the gloss of the coating. In addition, within the above range, the larger the free radical reactive functional group equivalent is, the more the gelation during manufacturing is suppressed, and the reproducibility of production can be improved. From the above viewpoints, the free radical reactive functional group equivalent is preferably 300 or more, more preferably 500 or more, further preferably 800 or more, and particularly preferably 1000 or more. In addition, the free radical reactive functional group equivalent is preferably 4000 or less, more preferably 3000 or less, further preferably 2500 or less, and particularly preferably 2000 or less.
[0077] The usage ratio of alkoxysilane (a-1) and alkoxysilane (a-2) can be appropriately set in consideration of the above free radical reactive functional group equivalent, the molecular weight of the polyorganosiloxane chain, etc. Specifically, relative to the total of alkoxysilane (a-1) and alkoxysilane (a-2), preferably, the ratio occupied by (a-1) is 1% by weight or more and 30% by weight or less, and the ratio occupied by (a-2) is preferably 70% by weight or more and 99% by weight or less, more preferably, the ratio occupied by (a-1) is 5% by weight or more and 25% by weight or less, and the ratio occupied by (a-2) is 75% by weight or more and 95% by weight or less. In addition, relative to the total alkoxysilane component, the proportion of (a-1) is preferably from 1% by weight to 30% by weight, and the proportion of (a-2) is preferably from 70% by weight to 99% by weight, and more preferably the proportion of (a-1) is from 5% by weight to 25% by weight, and the proportion of (a-2) is from 75% by weight to 95% by weight.
[0078] The alkoxysilane component may be composed of only alkoxysilane (a-1) and alkoxysilane (a-2). In addition to these, it may further contain an alkoxysilane (a-3) that is neither an alkoxysilane (a-1) nor an alkoxysilane (a-2). As alkoxysilane (a-3), for example: an alkoxysilane having a (meth)acryloyl group, a triorganomonoalkoxysilane, a tetraalkoxysilane, etc. may be cited. Alkoxysilane (a-3) may not be used, but when alkoxysilane (a-3) is used, its amount may be determined within the range that does not hinder the effect of the present invention, for example, preferably 10% by weight or less, more preferably 5% by weight or less, and further preferably 1% by weight or less in proportion to the entire alkoxysilane component.
[0079] The polyorganosiloxane can be formed by subjecting the alkoxysilane component described above to hydrolysis and dehydration condensation reaction in the presence of water and a condensation catalyst. The produced polyorganosiloxane has a radically reactive functional group derived from the alkoxysilane (a-1).
[0080] In addition, according to a preferred embodiment, a part of the alkoxy groups contained in the alkoxysilane component remain unreacted, or the alkoxysilane component does not undergo a dehydration condensation reaction after undergoing a hydrolysis reaction and remains in the form of a silanol group, and the polyorganosiloxane produced thereby may further have a reactive silyl group. Here, the reactive silyl group refers to a concept including both an alkoxysilyl group and a silanol group.
[0081] In the above-mentioned hydrolysis and dehydration condensation reaction, water is added to make the reaction proceed. At this time, by controlling the amount of water, gelation during free radical polymerization can be suppressed, and the storage stability of the organic-inorganic composite resin can be improved. From this point of view, the total molar number of alkoxy groups directly bonded to the silicon atoms contained in the alkoxysilane component is set to 100%, relative to which the amount of water is 30 mol% or more and 60 mol% or less. The upper limit is preferably 55 mol% or less. The lower limit is preferably 35 mol% or more, more preferably 40 mol% or more, and particularly preferably 45 mol% or more.
[0082] In the above-mentioned hydrolysis and dehydration condensation process, in addition to water, an organic solvent other than water can also be used. As such an organic solvent, a water-soluble organic solvent is preferably used in combination with water. In addition, in order to ensure the solubility of the alkoxysilane component, an organic solvent with more than 4 carbon atoms is preferably used. From the above viewpoints, preferred organic solvents include, for example, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, polyethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monoisopropyl ether, diethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether, ethylene glycol monoisobutyl ether, diethylene glycol monoisobutyl ether, propylene glycol monomethyl ether, propylene glycol dimethyl ether, dipropylene glycol monomethyl ether, tripropylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, diethylene glycol diethyl ether, and ethylene glycol diethyl ether, but are not limited thereto.
[0083] In order to volatilize the organic solvent when forming a coating film after producing the organic-inorganic composite resin, an organic solvent having a boiling point of 150° C. or less under atmospheric pressure is preferred, and specifically, ethylene glycol monoethyl ether, ethylene glycol monoisopropyl ether, propylene glycol monomethyl ether, propylene glycol monopropyl ether, propylene glycol monoethyl ether, and propylene glycol dimethyl ether are particularly preferred.
[0084] In order to promote the reaction, the above-mentioned hydrolysis and dehydration condensation reaction are carried out in the presence of a condensation catalyst. As a condensation catalyst, a known condensation catalyst can be used. There are roughly basic catalysts and acidic catalysts in the condensation catalyst, and the acidic catalyst has the effect of faster hydrolysis compared with condensation, as a result, the polyorganosiloxane obtained has more silanol groups, and the silanol groups are stabilized in an acidic solution, so the storage stability of the organic-inorganic composite resin improves. Therefore, it is preferred to implement the hydrolysis and dehydration condensation process of the present invention under the condition of the presence of an acidic catalyst as a condensation catalyst.
[0085] As the acidic catalyst, organic acids are preferred from the perspective of compatibility with the alkoxysilane component and the organic solvent, and phosphate esters and carboxylic acids are more preferred. Specific examples of organic acids include ethyl acid phosphate, butyl acid phosphate, butyl pyrophosphate (or dibutyl pyrophosphate), butoxyethyl acid phosphate, 2-ethylhexyl acid phosphate, isotridecyl acid phosphate, dibutyl phosphate, bis(2-ethylhexyl) phosphate, formic acid, acetic acid, butyric acid, isobutyric acid, and the like.
[0086] Examples of the basic catalyst include N-ethylmorpholine, N-methyldiethanolamine, N-ethyldiethanolamine, N-n-butyldiethanolamine, N-tert-butyldiethanolamine, triethylamine, n-butylamine, hexylamine, triethanolamine, diazabicycloundecene, amine compounds such as ammonia, and metal hydroxides such as sodium hydroxide and potassium hydroxide.
[0087] In addition, as a condensation catalyst, a neutral salt can also be used. Even if a neutral salt is used, the same effect as that of an acidic catalyst can be obtained. Here, a neutral salt refers to a positive salt formed by a strong acid and a strong base, for example, a salt formed by a combination of any cation selected from the first group element ion, the second group element ion, a tetraalkylammonium ion, and a guanidium ion as a cation, and any anion selected from the seventeenth group element ion, a sulfate ion, a nitrate ion, and a perchlorate ion as an anion except a fluoride ion. In particular, as an anion, the seventeenth group element ion is preferred due to its high nucleophilicity, and as a cation, as an ion that is not high in steric hindrance and does not hinder nucleophilic action, the first group element ion and the second group element ion are preferred.
[0088] There are no particular limitations on specific compounds of the neutral salt, and preferred neutral salts include lithium chloride, sodium chloride, potassium chloride, rubidium chloride, cesium chloride, magnesium chloride, calcium chloride, strontium chloride, lithium bromide, sodium bromide, potassium bromide, rubidium bromide, cesium bromide, magnesium bromide, calcium bromide, strontium bromide, lithium iodide, sodium iodide, potassium iodide, rubidium iodide, cesium iodide, magnesium iodide, calcium iodide, and strontium iodide.
[0089] The amount of the condensation catalyst added can be appropriately adjusted, for example, relative to the alkoxysilane component, it can be about 50ppm to 3% by weight. However, in order to suppress the gelation during the manufacture or storage of the organic-inorganic composite resin, within the range of the effect of shortening the reaction time brought by the condensation catalyst, the less the amount of the condensation catalyst is used, the more preferred.
[0090] The reaction temperature during the hydrolysis and dehydration condensation steps can be appropriately set by a person skilled in the art, and for example, the reaction solution is preferably heated to 50 to 150° C. The reaction time can also be appropriately set by a person skilled in the art, and for example, it can be set to about 10 minutes to 12 hours.
[0091] Preferably, after the above-mentioned hydrolysis and dehydration condensation steps are carried out, a step of removing the alcohol produced in the hydrolysis step from the reaction solution is carried out. By removing the alcohol, the hydrolysis reaction in which alcohol is produced as a by-product can be further promoted. The alcohol removal step can be carried out by distilling off the alcohol by vacuum distillation of the reaction solution after the hydrolysis and dehydration condensation steps. Those skilled in the art can appropriately set the conditions for the vacuum distillation.
[0092] In the hydrolysis and dehydration condensation reactions, the radically reactive functional groups of the alkoxysilane (a-1) are not substantially affected. Therefore, the polyorganosiloxane produced by the reaction has radically reactive functional groups derived from the alkoxysilane (a-1) as described above.
[0093] The number of free radical reactive functional groups per molecule of polyorganosiloxane is not particularly limited, and may be about 1 or more. By setting it to more than 1, the grafting rate of poly(meth)acrylic acid chain and polyorganosiloxane chain can be improved, and good transparency and gloss of the coating film can be achieved. In addition, the above number may exceed 3, or may be more than 4. Even if a polyorganosiloxane having so many free radical reactive functional groups is used, according to the manufacture method of the present invention, gelation during manufacture can also be suppressed. From the viewpoint of suppressing gelation and improving storage stability, the above number is preferably less than 8.
[0094] (Free Radical Polymerization)
[0095] In the present invention, after obtaining polyorganosiloxane by hydrolysis and dehydration condensation reaction of alkoxysilane component, free radical polymerization is carried out on free radical polymerizable monomer component containing (meth) acrylate monomer under the condition of the presence of the polyorganosiloxane, thereby manufacturing organic-inorganic composite resin containing poly(meth) acrylic acid chain and polyorganosiloxane chain. In the free radical polymerization, first, polymerization of free radical polymerizable monomer component containing (meth) acrylic acid ester monomer with high growth reactivity in free radical polymerization is carried out, and after forming poly(meth) acrylic acid chain, free radical reactive functional group showing lower growth reactivity than methacryloyl group in free radical polymerization is reacted with the end of the poly(meth) acrylic acid chain, thereby realizing the composite of poly(meth) acrylic acid chain and polyorganosiloxane chain. However, there may also be a situation where a part of the free radical reactive functional group showing low free radical reactivity is copolymerized with a part that is not the end of the poly(meth) acrylic acid chain. It should be noted that (meth) acrylic acid refers to acrylic acid and / or methacrylic acid.
[0096] The (meth)acrylate monomer is not particularly limited, and examples thereof include: (meth)acrylate alkyl esters having an alkyl group having 1 to 22 carbon atoms, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate; (meth)acrylate aralkyl esters, such as benzyl (meth)acrylate and 2-phenylethyl (meth)acrylate; (meth)acrylate cycloalkyl esters, such as cyclohexyl (meth)acrylate and isobornyl (meth)acrylate; 2-methoxyethyl (meth)acrylate, ω-alkoxyalkyl (meth)acrylates such as 4-methoxybutyl ester; hydroxyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and glyceryl mono(meth)acrylate; silyl (meth)acrylates such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, (meth)acryloxyoctyltrimethoxysilane, and (meth)acryloxyoctyltriethoxysilane. These may be used alone or in combination of two or more.
[0097] The radical polymerizable monomer component for implementing the free radical polymerization may be only the above-mentioned (meth)acrylate monomer, or a (meth)acrylate monomer may be used in combination with other radical polymerizable monomers. The radical polymerizable monomer is not particularly limited, and examples thereof include: unsaturated carboxylic acids such as (meth)acrylic acid; acrylamides such as (meth)acrylamide, α-ethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, N,N-dimethyl (meth)acrylamide, N-methyl (meth)acrylamide, and N-hydroxymethyl (meth)acrylamide; aromatic hydrocarbon vinyl compounds such as styrene, α-methylstyrene, chlorostyrene, styrenesulfonic acid, 4-hydroxystyrene, and vinyltoluene; anhydrides of unsaturated carboxylic acids such as maleic anhydride, and these anhydrides and linear or branched alcohols having 1 to 20 carbon atoms; Esters of unsaturated carboxylic acids such as diesters or half esters formed with or amines; vinyl esters and aromatic compounds such as vinyl acetate, vinyl propionate, and diallyl phthalate; amino vinyl compounds such as vinyl pyridine and aminoethyl vinyl ether; amide-containing vinyl compounds such as itaconic acid diamide, crotonic acid amide, maleic acid diamide, fumaric acid diamide, and N-vinyl pyrrolidone; (meth) acrylonitrile, 2-hydroxyethyl vinyl ether, methyl vinyl ether, cyclohexyl vinyl ether, vinyl chloride, vinylidene chloride, chloroprene, propylene, butadiene, isoprene, fluoroolefin maleimide, N-vinylimidazole, and vinyl sulfonic acid. These may be used alone or in combination of two or more.
[0098] The proportion of the (meth)acrylate monomer to the total free radical polymerizable monomer component can be appropriately set. However, from the viewpoint of the adhesion of the manufactured organic-inorganic composite resin to the substrate, the methacrylate monomer preferably occupies 60% by weight or more, more preferably 65% by weight or more, and further preferably 70% by weight or more relative to the total free radical polymerizable monomer component.
[0099] It is preferred that the solubility parameter value (SP value) of the formed poly(meth)acrylic acid chain be between 9.0 and 11.0 (cal / cm 3 ) 1 / 2 The type and ratio of the monomers constituting the poly(meth)acrylic acid chain are selected in a manner within the range of 9.0 to 10.0 (cal / cm 3 ) 1 / 2The composite of poly(meth)acrylic acid chain and polyorganosiloxane chain within the range of 9.2 to 10.0 (cal / cm 3 ) 1 / 2 , particularly preferably 9.4 to 9.9 (cal / cm 3 ) 1 / 2 .
[0100] The SP value is a value δ calculated by the following formula based on the method described in Fedors [Robert F. Fedors, Polymer Engineering and Science, 14, 147-154 (1974)].
[0101] Fedors formula: δ=(ΣΔei / ΣΔvi) 1 / 2
[0102] In the formula, Δei: represents the evaporation energy of atoms and atomic groups (cal / mol), Δvi: represents the molar volume (cm 3 / mol).
[0103] The number of carbon atoms contained in the monomer units constituting the poly(meth)acrylic acid chain is not particularly limited. For example, when the organic-inorganic composite resin is dissolved in a weak solvent to prepare a coating, the number of carbon atoms in the side chains of the monomer units is preferably in the range of 3 to 7 on average, more preferably in the range of 3.3 to 6.7, and further preferably in the range of 3.5 to 6.2. The number of carbon atoms in the side chains, for example, refers to the number of carbon atoms in the ester portion in the case of (meth)acrylic acid ester monomers, and refers to the number of carbon atoms in the portion other than the carbon-carbon unsaturated bond forming the main chain of the polymer in the case of other monomers. Specifically, the number of carbon atoms in the side chain of methyl methacrylate is 1, the number of carbon atoms in the side chain of butyl methacrylate is 4, the number of carbon atoms in the side chain of cyclohexyl methacrylate is 6, the number of carbon atoms in the side chain of 2-hydroxyethyl methacrylate is 2, the number of carbon atoms in the side chain of 3-methacryloxypropyltrimethoxysilane is 6, and the number of carbon atoms in the side chain of styrene is 6. If a large amount of monomers having a large steric hindrance around the main chain, such as butyl methacrylate and cyclohexyl methacrylate, are used, the compatibility with polyorganosiloxane is reduced. Therefore, it is generally difficult to composite a polyorganosiloxane chain with a poly(meth)acrylic acid chain. However, according to the present invention, even if a large amount of such monomers having a large number of carbon atoms are used, an organic-inorganic composite resin in which a polyorganosiloxane chain and a poly(meth)acrylic acid chain are composited can be produced.
[0104] The radical polymerizable monomer component containing the (meth)acrylate monomer described above is mixed with the polyorganosiloxane to perform radical polymerization. The radical polymerization method can be a conventional method, and a known polymerization method such as bulk radical polymerization, solution radical polymerization, non-aqueous dispersion radical polymerization can be used.
[0105] The free radical polymerization is carried out in the presence of a free radical polymerization initiator. The free radical polymerization initiator is not particularly limited, and examples thereof include 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2-methylbutyronitrile), tert-butyl peroxypivalate, tert-butyl peroxybenzoate, tert-butyl peroxy 2-ethylhexanoate, di-tert-butyl peroxide, cumene hydroperoxide, diisopropyl peroxycarbonate, etc. These may be used alone or in combination of two or more.
[0106] The amount of the radical polymerization initiator is not particularly limited. By adjusting the amount, the molecular weight of the organic-inorganic composite resin produced can be controlled, and gelation during radical polymerization can be suppressed. Specifically, the amount of the radical polymerization initiator can be 0.1 to 10 parts by weight, preferably 0.5 to 7 parts by weight, for example, relative to 100 parts by weight of the radical polymerizable monomer component.
[0107] The free radical polymerization can be preferably carried out by adding a free radical polymerizable monomer component and a free radical polymerization initiator to the system containing the polyorganosiloxane obtained by the hydrolysis / dehydration condensation reaction. That is, it is not necessary to take out the manufactured polyorganosiloxane from the reaction vessel and transfer it to another reaction vessel, and the hydrolysis / dehydration condensation reaction and free radical polymerization can be continuously carried out in one reaction vessel. The manufacturing method of the present invention has the technical advantage of being able to suppress gelation and manufacture an organic-inorganic composite resin by such a simple method.
[0108] The above-mentioned free radical polymerization can be carried out under the condition of the presence of a β-dicarbonyl compound. The β-dicarbonyl compound refers to a compound having a structure in which two carbonyl groups are bonded to one carbon atom. By having a β-dicarbonyl compound in the polymerization system, the dehydration condensation reaction of the silanol group possessed by the polyorganosiloxane can be suppressed during free radical polymerization. As a result, it is easy to maintain the silanol group in the manufactured organic-inorganic composite resin. As a β-dicarbonyl compound, there is no particular limitation, and examples thereof include acetylacetone, dimedone, cyclohexane-1,3-dione, methyl acetoacetate, ethyl acetoacetate, dimethyl malonate, diethyl malonate, Meldrum's acid, etc. The amount of the β-dicarbonyl compound can be set in a manner that can achieve the above-mentioned effect, for example, it can be 0.01 to 10 parts by weight relative to 100 parts by weight of the polyorganosiloxane, or it can be about 0.1 to 5 parts by weight.
[0109] The polymerization temperature during free radical polymerization can be based on the usual method. However, if the temperature of the reaction system is lowered after the polyorganosiloxane containing silanol groups is manufactured by hydrolysis and dehydration condensation reaction, the dehydration condensation reaction between the silanol groups becomes easy to proceed, and the molecular weight of the manufactured organic-inorganic composite resin is easy to change, or it is easy to gel in free radical polymerization. Therefore, from the viewpoint of suppressing the change of molecular weight and the progress of gelation, it is preferred to control the temperature in a manner that the temperature of the reaction system does not substantially decrease from the above-mentioned hydrolysis and dehydration condensation reaction to the end of the above-mentioned free radical polymerization. Here, the temperature of the reaction system does not substantially decrease, which means that the temperature during free radical polymerization is set to be substantially the same as the temperature during hydrolysis and dehydration condensation reaction, or is set to be higher than the temperature during hydrolysis and dehydration condensation reaction. In addition, the term "substantially not reduced" also includes the case where the temperature of the reaction system is only reduced within the range where there is no substantial problem from the viewpoint of suppressing the change of molecular weight and the progress of gelation, specifically, it also includes the case where it is reduced within a range of less than 5°C, preferably less than 3°C.
[0110] In addition, the hydrolysis and dehydration condensation reaction and the free radical polymerization are preferably carried out in an atmosphere substantially free of oxygen molecules. Thus, the reaction of the free radical reactive functional groups showing low free radical reactivity can be promoted, the grafting rate of the poly(meth)acrylic acid chain and the polyorganosiloxane chain can be increased, and the transparency or gloss of the coating film can be improved.
[0111] The poly(meth)acrylic acid chain is formed by the above-mentioned radical polymerization, and the radical reactive functional group having low radical reactivity is reacted with the terminal of the poly(meth)acrylic acid chain to bond polyorganosiloxane, thereby producing an organic-inorganic composite resin containing a poly(meth)acrylic acid chain and a polyorganosiloxane chain.
[0112] According to a preferred embodiment, the polyorganosiloxane chain contained in the produced organic-inorganic composite resin may have a reactive silicon group (alkoxysilyl group and / or silanol group). The reactive silicon allows the organic-inorganic composite resin to exhibit curability utilizing hydrolysis / dehydration reaction of the reactive silicon group.
[0113] In this case, in order to ensure the stability of the reactive silicon, it is preferred to mix a dehydrating agent in the manufactured organic-inorganic composite resin. Thus, the storage stability of the organic-inorganic composite resin having a reactive silicon group in the polyorganosiloxane chain can be improved. As the dehydrating agent, a known dehydrating agent can be used, without particular limitation, and for example, methyltrimethoxysilane, dimethyldimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, vinyltriethoxysilane, methyl orthoformate, ethyl orthoformate, methyl orthoacetate, or ethyl orthoacetate are preferred. Among these, only one type can be used, or multiple types can be used.
[0114] The amount of the dehydrating agent is not particularly limited, and can be appropriately determined by those skilled in the art in consideration of the amount of water contained in the organic-inorganic composite resin before dehydration and the target water content after dehydration. As an example, it is about 0.01 to 20 parts by weight, or about 0.1 to 10 parts by weight, relative to 100 parts by weight of the organic-inorganic composite resin.
[0115] (Organic-inorganic composite resin)
[0116] Next, the organic-inorganic composite resin according to the embodiment of the present invention will be described.
[0117] The organic-inorganic composite resin of the present invention is formed by bonding a poly(meth)acrylic acid chain and a polyorganosiloxane chain, and the bonding of the two chains is achieved by linking the carbon atoms in the monomer units constituting the poly(meth)acrylic acid chain and the silicon atoms in the polyorganosiloxane chain only via hydrocarbon groups without via heteroatom-containing groups such as ester groups, ether groups, amide groups, and imide groups. It should be noted that the carbon atoms in the monomer units constituting the poly(meth)acrylic acid chain refer to the carbon atoms forming the main chain of the poly(meth)acrylic acid chain, and do not refer to the carbon atoms contained in the side chains of the poly(meth)acrylic acid chain.
[0118] The bonding portion of the two chains is shown as the following formula.
[0119] -CR-Si-
[0120] In the formula, C represents a carbon atom contained in a monomer unit constituting a poly(meth)acrylic acid chain. The carbon atom is a carbon atom constituting a carbon-carbon double bond in a monomer before polymerization for producing a poly(meth)acrylic acid chain. R represents a divalent hydrocarbon group. Si represents a silicon atom contained in a polyorganosiloxane chain. In this way, the poly(meth)acrylic acid chain and the polyorganosiloxane chain are not bonded via heteroatom-containing groups such as ester groups and ether groups, but are bonded only via hydrocarbon groups.
[0121] The hydrocarbon group is a divalent bonded group formed by bonding a carbon atom in a monomer unit constituting the poly(meth)acrylic acid chain to a silicon atom in a polyorganosiloxane chain. The number of carbon atoms is not particularly limited, but is preferably 2 to 20, more preferably 2 to 8, further preferably 2 to 4, further preferably 2 to 3, and particularly preferably 2. The hydrocarbon group may be any of an aliphatic hydrocarbon group and an aromatic hydrocarbon group. It may be straight-chain or branched. Specifically, ethylene (including 1,2-ethylene and 1,1-ethylene), propylene (1,3-propylene, 2,3-propylene, etc.), or p-phenyleneethylene (including p-phenylene-1,2-ethylene and p-phenylene-1,1-ethylene) may be mentioned. The hydrocarbon group is preferably derived from a radical-reactive double bond group possessed by the alkoxysilane (a-1). For example, when an alkoxysilane having a vinyl group is used as the alkoxysilane (a-1), an ethylene group is formed as the hydrocarbon group. The hydrocarbon group preferably contains at least an ethylene group. It should be noted that the ethylene group mentioned here does not refer to the ethylene group contained in the propylene group or the p-phenyleneethylene group.
[0122] The poly(meth)acrylic acid chain is a homopolymer or copolymer of a radical polymerizable monomer component containing a (meth)acrylic acid ester monomer. The details of the types and ratios of the monomers forming the poly(meth)acrylic acid chain are as described above.
[0123] The above-mentioned polyorganosiloxane chain refers to a hydrolysis condensate of an alkoxysilane component containing 70 to 100 mol% of a monoorganotrialkoxysilane and 30 to 0 mol% of a diorganodialkoxysilane. The definitions of the above-mentioned monoorganotrialkoxysilane and the above-mentioned diorganodialkoxysilane are as described above. The monoorganotrialkoxysilane is an essential component, but the diorganodialkoxysilane may or may not be used. The proportion of the diorganodialkoxysilane in the total of the monoorganotrialkoxysilane and the diorganodialkoxysilane is 30% by weight or less, preferably 20% by weight or more, more preferably 10% by weight or less, further preferably 5% by weight or less, and further preferably 1% by weight or less.
[0124] In order to realize the bonding of the poly(meth)acrylic acid chain and the polyorganosiloxane chain in the organic-inorganic composite resin of the present invention, as the monoorganotrialkoxysilane and / or the diorganodialkoxysilane, a monoorganotrialkoxysilane and / or the diorganodialkoxysilane (a-1) having a double bond group containing a free radical reaction is used. In addition, it is preferred to use a monoorganotrialkoxysilane and / or the diorganodialkoxysilane (a-2) not having a double bond group containing a free radical reaction in combination with the (a-1). The details of the (a-1) and (a-2) are as described above.
[0125] The polyorganosiloxane chain of the preferred embodiment has a reactive silicon group as described above. The presence of the reactive silicon group enables the organic-inorganic composite resin of the present invention to exhibit curability by a hydrolysis / dehydration condensation reaction.
[0126] In order to make the polyorganosiloxane chain have reactive silicon groups, the siloxane bond formation rate (also called condensation rate) of the polyorganosiloxane chain must be less than 100%. Here, the siloxane bond formation rate refers to a numerical value indicating the conversion rate of alkoxy groups on silicon atoms contained in the alkoxysilane component of the raw material into siloxane bonds, and is 100% when all alkoxy groups are converted into siloxane bonds.
[0127] The siloxane bond formation rate is a value calculated by classifying the structural units derived from monoorganotrialkoxysilane into structural units T1 having one siloxane bond, structural units T2 having two siloxane bonds, and structural units T3 having three siloxane bonds. 29 The value calculated by the following formula is when the ratio (%) of each mole number of T1, T2, and T3 to the total mole number of T1, T2, and T3 measured by Si-NMR is X, Y, and Z, respectively. The total of X, Y, and Z is 100.
[0128] Siloxane bond formation rate = (1×X+2×Y+3×Z) / 3
[0129] When the above-mentioned siloxane bond formation rate is close to a value of 100%, the alkoxy groups are almost completely converted into siloxane bonds, and therefore, the number of reactive silicon groups possessed by the polyorganosiloxane chain decreases. On the contrary, when the siloxane bond formation rate is too low, a polyorganosiloxane chain of sufficient molecular weight cannot be formed, and the organic-inorganic composite resin becomes difficult to exhibit the physical properties derived from the polyorganosiloxane chain. From the above viewpoints, the siloxane bond formation rate of the organic-inorganic composite resin of the present invention is preferably 20% or more and 80% or less. It is more preferably 30% or more, further preferably 40% or more, further preferably 50% or more, particularly preferably 60% or more, and most preferably 65% or more. In addition, from the viewpoint of the reactivity of the reactive silicon groups possessed by the polyorganosiloxane chain, the above-mentioned siloxane bond formation rate is more preferably 75% or less, and further preferably 72% or less.
[0130] The siloxane bond formation rate can be adjusted by adjusting the amount of water used in the hydrolysis / dehydration condensation reaction for forming the polyorganosiloxane chain, the type / amount of the catalyst, or the presence of a component that stabilizes the silanol group in the reaction system.
[0131] In the organic-inorganic composite resin of the present invention, the ratio of the poly(meth)acrylic acid chain to the polyorganosiloxane chain can be set in a manner that can take into account the physical properties of each chain. The ratio of the polyorganosiloxane chain is preferably determined by considering the physical properties of the inorganic chain, and the pigment dispersibility, transparency, gloss, and mechanical properties of the coating film when the organic-inorganic composite resin is used for the coating. Specifically, the weight ratio of the above-mentioned polyorganosiloxane chain relative to the above-mentioned organic-inorganic composite resin as a whole is preferably 20% by weight or more and 80% by weight or less. More preferably, it is 30% by weight or more, and more preferably, it is 40% by weight or more. And it is more preferably 70% by weight or less, more preferably 60% by weight or less, and particularly preferably 50% by weight or less.
[0132] The weight average molecular weight (MW) of the organic-inorganic composite resin of the present invention can be appropriately determined according to the desired physical properties, preferably in the range of 2000 to 500,000, more preferably in the range of 5000 to 300,000. Within this range, gelation during production can be avoided, and the organic-inorganic composite resin can form a coating film with excellent storage stability, transparency or gloss. It should be noted that the weight average molecular weight of the organic-inorganic composite resin can be determined by the method described in Example 1.
[0133] (Coating liquid)
[0134] The organic-inorganic composite resin of the present invention can be used as a curable resin composition for coatings, i.e., the main component of a coating liquid. When constituting the coating liquid, pigments, plasticizers, dispersants, anti-settling agents, anti-skinning agents, desiccants, anti-sagging agents, matting agents, antistatic agents, conductive agents, flame retardants, and other known additives for coatings can be appropriately formulated. The organic-inorganic composite resin of the present invention can be used as a coating liquid, and due to its excellent weather resistance and high transparency, it can also be suitably used as a coating liquid for a transparent coating film without a pigment, or a colored coating liquid containing a pigment or a dye.
[0135] The curable resin composition or coating liquid of the present invention can promote the curing reaction of the coating film in the presence of a curing agent and shorten the operation time when forming the coating film. Therefore, it is preferably a two-component composition or coating liquid containing a curing agent or containing a curing agent in a separate package.
[0136] As the curing agent, a known curing agent can be suitably used as a curing agent for a curable resin composition that utilizes a hydrolysis reaction and a dehydration condensation reaction of a silyl group. Specifically, as the curing agent, the above-mentioned condensation catalyst can be used, and an organic tin compound, a titanium chelate compound, an aluminum chelate compound, an organic amine compound, etc. can be used.
[0137] Specific examples of the above-mentioned organic tin compounds include dioctyltin bis(2-ethylhexylmalate), condensates of dioctyltin oxide or dibutyltin oxide and silicate, dibutyltin dioctoate, dibutyltin dilaurate, dibutyltin distearate, dibutyltin diacetylacetonate, dibutyltin bis(ethylmalate), dibutyltin bis(butylmalate), dibutyltin bis(2-ethylhexylmalate), dibutyltin bis(oleylmalate), stannous octoate, tin stearate, and di-n-butyltin oxide laurate. Specific examples of the organotin compound having an S atom in the molecule include dibutyltin bis-isononyl-3-mercaptopropionate, dioctyltin bis-isononyl-3-mercaptopropionate, octylbutyltin bis-isononyl-3-mercaptopropionate, dibutyltin bis-isooctylmercaptoacetate, dioctyltin bis-isooctylmercaptoacetate, and octylbutyltin bis-isooctylmercaptoacetate.
[0138] Specific examples of the titanium chelate compound include titanium acetylacetonate, titanium tetraacetylacetonate, titanium ethylacetoacetate, titanium phosphate compounds, titanium neoglycolate, titanium ethylacetoacetate, and the like.
[0139] Specific examples of the aluminum chelate compound include ethyl acetoacetate aluminum diisopropionate, aluminum tris(acetoacetate), aluminum tris(ethylacetoacetate), aluminum monoacetylacetonate bis(ethylacetoacetate), and alkyl aluminum acetoacetate diisopropionate.
[0140] Specific examples of the organic amine compound include triethylamine, triethylenediamine, trimethylamine, tetramethylenediamine, N-methylmorpholine, N-ethylmorpholine, N,N′-diethyl-2-methylpiperazine, laurylamine, and dimethyllaurylamine.
[0141] The amount of the curing agent used can be appropriately adjusted according to the curing temperature and curing time, and is, for example, preferably from 0.01 to 20 parts by weight, more preferably from 0.1 to 10 parts by weight, based on 100 parts by weight of the organic-inorganic composite resin.
[0142] The curable resin composition of the present invention can be applied to a substrate and cured to form a coating film. The conditions for application and curing are not particularly limited, but it is preferred to use a heat source to promote evaporation of the solvent during curing.
[0143] The thickness of the formed coating film is not particularly limited. In the present invention, the thickness after drying is preferably 5 μm or more and 100 μm or less. When the thickness is thinner than 5 μm, the water resistance and moisture resistance of the coating film may become insufficient. When the thickness exceeds 100 μm, cracks may be generated due to the curing shrinkage when the coating film is formed. It is more preferably 5 μm or more and 50 μm or less, and further preferably 10 μm or more and 40 μm or less.
[0144] There are no particular restrictions on the substrate to which the curable resin composition of the present invention can be applied, and organic substrates such as polycarbonate (PC), acrylic, ABS, ABS / PC, polyethylene terephthalate (PET), and inorganic substrates such as glass, aluminum, SUS, copper, iron, and stone can be used.
[0145] Example
[0146] The present invention will be described in more detail below with reference to Examples, but the present invention is not limited to these Examples.
[0147] The materials used in Examples and Comparative Examples are as follows.
[0148] Alkoxysilane ingredients
[0149] Vi (A-171: Vinyltrimethoxysilane manufactured by Momentive Performance Materials Japan LLC, molecular weight 148.2)
[0150] Me (OFS-6070: methyltrimethoxysilane manufactured by Dow Toray Co., Ltd., molecular weight 136.2)
[0151] Ph (Z-6124: phenyltrimethoxysilane manufactured by Dow Toray Co., Ltd., molecular weight 198.3)
[0152] MA (A-174: manufactured by Momentive Performance Materials Japan LLC, 3-methacryloxypropyltrimethoxysilane, molecular weight 248.4)
[0153] Ge (OFS-6040: manufactured by Dow Toray Industries, Ltd., 3-glycidyloxypropyltrimethoxysilane, molecular weight 236.3).
[0154] Condensation catalyst
[0155] DBP (manufactured by Johoku Chemical Industry Co., Ltd., dibutyl phosphate, molecular weight 210.2).
[0156] MgCl2 (manufactured by Tokyo Chemical Industry Co., Ltd., magnesium chloride hexahydrate, molecular weight 203.3).
[0157] LiCl (manufactured by Tokyo Chemical Industry Co., Ltd., lithium chloride, molecular weight 42.4).
[0158] Raw monomers and free radical polymerization initiators for (meth)acrylic resins
[0159] MMA (Mitsubishi Gas Chemical Co., Ltd., methyl methacrylate, molecular weight 100.1)
[0160] TSMA (A-174: manufactured by Momentive Performance Materials Japan LLC, 3-methacryloxypropyltrimethoxysilane, molecular weight 248.4)
[0161] BA (manufactured by Nippon Catalyst Co., Ltd., butyl acrylate, molecular weight 128.2)
[0162] CHMA (manufactured by Nippon Catalyst Co., Ltd., cyclohexyl methacrylate, molecular weight 168.0)
[0163] BMA (Mitsubishi Gas Chemical Co., Ltd., butyl methacrylate, molecular weight 142.2)
[0164] AA (manufactured by Nippon Catalyst Co., Ltd., acrylic acid, molecular weight 72.1)
[0165] HEMA (manufactured by Nippon Catalyst Co., Ltd., 2-hydroxyethyl methacrylate, molecular weight 130.1)
[0166] St (manufactured by Sankyo Chemical Co., Ltd., styrene, molecular weight 104.2)
[0167] V59 (manufactured by Wako Pure Chemical Industries, Ltd., 2,2′-azobis(2-methylbutyronitrile), molecular weight 192.3).
[0168] Dehydrating agent
[0169] MOA (manufactured by Tokyo Chemical Industry Co., Ltd., trimethyl orthoformate, molecular weight 106.1).
[0170] Solvents
[0171] S100 (Made by Sanwa Chemical Co., Ltd., a mixture of mineral oil, cumene, xylene and trimethylbenzene)
[0172] LAWS (manufactured by Shell Chemicals Japan Co., Ltd., a mixture of mineral spirit, xylene, trimethylbenzene, and nonane)
[0173] PMA (manufactured by Sankyo Chemical Co., Ltd., propylene glycol monomethyl ether acetate, molecular weight 132.2)
[0174] Stabilizer
[0175] AcAc (produced by Daicel Corporation, acetylacetone, molecular weight 100.1)
[0176] Curing catalyst
[0177] U-20 (Nitto Kasei Co., Ltd., butyltin dilaurate, 631.6)
[0178] (Polysiloxane reaction time)
[0179] After mixing the alkoxysilane component, condensation catalyst, and water at room temperature, the mixture was heated in an oil bath heated to 90°C. The time when the internal temperature reached 70°C was taken as the starting point of the reaction, and the time of heating in the 90°C oil bath was taken as the reaction time. The reaction was carried out for 6 hours.
[0180] (Dealcoholization in polysiloxane synthesis)
[0181] The resin solution obtained by reacting for 6 hours as described above is composed of polysiloxane, alcohol generated during the reaction, and a small amount of residual water. In order to remove volatile components other than polysiloxane by distillation, the resin solution is heated in an oil bath heated to 120°C, slightly pressurized with nitrogen, and the amount of liquid recovered is measured, while distillation is continued until the set content liquid volume is reached.
[0182] The amount of alcohol to be removed by distillation was calculated according to the following formula.
[0183] (When the condensation catalyst is DBP or MgCl2) Amount of water added × 32 / 18 × 2 × 85%
[0184] (When the condensation catalyst is LiCl) Amount of water added × 32 / 18 × 2 × 100%
[0185] The weight of all alcohols that may be produced is calculated in the form of producing 1 mole of alcohol relative to 1 mole of alkoxysilane components used for the reaction. For example, 1 mole of trimethoxydimethylsilyl has 3 moles of methoxysilyl and produces 3 moles of methanol, and 1 mole of methyldimethoxysilyl has 2 moles of methoxysilyl and produces 2 moles of methanol. In addition, 1 mole of water produces 1 mole of silanol group and 1 mole of alcohol from 1 mole of alkoxysilyl. The 1 mole of silanol group produced further reacts with 1 mole of alkoxysilyl to produce 1 mole of alcohol. That is, 2 moles of alcohol are produced from 1 mole of water. The progress of this reaction varies depending on the condensation catalyst. In the case of LiCl, it progresses 100%, while in the case of DBP and MgCl2, it only progresses about 85%. Therefore, considering this point, the calculation formula is corrected as described above.
[0186] (Synthesis of polyorganosiloxane of Example 1)
[0187] In a 300 ml four-necked flask equipped with a condenser, 4.7 g of vinyl trimethoxysilane, 79.7 g of methyl trimethoxysilane, 0.0042 g of dibutyl phosphate, and 12.7 g of pure water were added, and heated in an oil bath set at 90°C to react for 6 hours. The methanol produced by hydrolysis refluxed in the flask, and the internal temperature became about 67°C. Then, while paying attention to heating without substantially lowering the internal temperature, a distillation apparatus was assembled, and the produced methanol and residual water were removed to obtain 59.2 g of a polysiloxane solution. It should be noted that when assembling the distillation apparatus, the mixing of oxygen was avoided as much as possible by setting the nitrogen inlet pipe and nitrogen pressurization, and the distillation was also carried out under the condition of nitrogen bubbling, and the condition of substantially almost no oxygen was maintained after the distillation and during the subsequent free radical polymerization.
[0188] In Examples 2 to 39 and Comparative Examples 1 to 5, polysiloxane solutions were obtained in the same manner as in Example 1 except that the alkoxysilane component, condensation catalyst, and water were used as described in Table 1. In Table 1, the unit of the amount of each component is gram (g).
[0189] (Free Radical Reactive Functional Group Equivalent Weight)
[0190] The free radical reactive functional group equivalent is calculated by the following formula.
[0191] (Molecular weight of alkoxysilane having a radically reactive functional group - molecular weight of the structure separated from the alkoxysilane by hydrolysis / dehydration condensation reaction) ÷ (mol % of alkoxysilane having a radically reactive functional group relative to the total amount of the alkoxysilane component used)
[0192] As an example, the calculation method of the free radical reactive functional group equivalent of Example 1 is described below. "Molecular weight of alkoxysilane having free radical reactive functional groups - molecular weight of the structure separated from alkoxysilane by hydrolysis / dehydration condensation reaction" is 148.23-69=79.23. The number of moles of vinyl trimethoxysilane used is 4.7÷148.23=0.0317, and the number of moles of methyl trimethoxysilane used is 79.7÷136.22=0.585. The free radical reactive functional group equivalent is calculated to be 79.23÷(0.0317÷(0.0317+0.585))≈1542.
[0193] It should be noted that in the above formula, the reason why the "molecular weight of the structure separated from the alkoxysilane by hydrolysis / dehydration condensation reaction" is set to "69" is as follows. In trimethoxysilane: -Si(OCH3)3, when all methoxy groups form siloxane bonds by condensation reaction, -Si(OCH3)3 is formed. 0.5 Correspondingly, the structure separated by the hydrolysis / dehydration condensation reaction is (O 0.5 CH3)3, therefore, its molecular weight is "69".
[0194] (Weight average molecular weight)
[0195] The weight average molecular weight of the polyorganosiloxane was measured by GPC. GPC was performed using HLC-8320GPC manufactured by Tosoh Corporation as a liquid delivery system, TSK-GEL type manufactured by Tosoh Corporation as a chromatographic column, and THF as a solvent. The weight average molecular weight was calculated by polystyrene conversion and is shown in Table 1 as an IP molecular weight.
[0196] [Table 1-1]
[0197]
[0198] [Table 1-2]
[0199]
[0200] [Table 1-3]
[0201]
[0202] [Table 1-4]
[0203]
[0204] [Table 1-5]
[0205]
[0206] (Synthesis of composite resin)
[0207] The apparatus was assembled by changing the condenser and performing reflux from the above distillation apparatus. The oil bath was set to an internal temperature of 110°C while nitrogen was introduced, and the "initial solvent" in Table 2 was added to the polysiloxane solution obtained above, and the internal temperature was set to 110°C.
[0208] Separate from the four-necked flask, a brown bottle was charged with "AC monomers" + "radical generator" + "polymerization solvent" in Table 2 to prepare a monomer solution for pump addition. The prepared monomer solution was added dropwise to the four-necked flask using a diaphragm pump over 3 hours.
[0209] In order to consume the residual monomers, the "free radical generator for residual monomers" + "polymerization solvent for residual monomers" in Table 2 were added to a brown bottle to prepare a free radical generator solution for residual monomers, which was then added dropwise to the reaction solution using a pump over 1 hour. After the addition was completed, the mixture was further heated for 1 hour to obtain the target composite resin solution. The details are as follows.
[0210] (Synthesis of Composite Resin of Example 1)
[0211] 19.7 g of S100 and 46.1 g of LAWS were added to 59.2 g of the polysiloxane solution obtained by the synthesis of the polyorganosiloxane in Example 1, and the mixture was heated to an internal temperature of 110°C.
[0212] In a brown bottle, 5.0 g of MMA, 1.0 g of TSMA, 3.0 g of BA, 41.0 g of BMA, 2.0 g of V59, 2.5 g of S100, and 5.9 g of LAWS were mixed and added by pump over 3 hours.
[0213] A solution containing 0.2 g of V59, 5.6 g of S100, and 13.1 g of LAWS was pumped in for 1 hour and heated for 1 hour to obtain 204.4 g of a composite resin solution. In the obtained composite resin, the carbon atoms in the monomer units constituting the poly(meth)acrylic acid chain and the silicon atoms in the polyorganosiloxane chain are bonded only via ethylene groups, and the polyorganosiloxane chain has a reactive silicon group.
[0214] In Examples 2 to 39 and Comparative Examples 1 to 5 in Table 2, the polysiloxane solutions, solvents, monomers, and free radical generators obtained in Examples 2 to 39 and Comparative Examples 1 to 5 in Table 1 were used as described in Table 2, and a composite resin solution was obtained in the same manner as in the above-mentioned "Synthesis of a composite resin in Example 1". However, in Comparative Examples 2 to 5, gelation occurred during the polymerization of the (meth)acrylate monomer, and a composite resin could not be produced. It should be noted that in Examples 25 and 26, a dehydrating agent was added to the obtained composite resin solution as described in Table 2, and in Examples 37 to 39, a stabilizer was added together with the initial solvent as described in Table 2. It should be noted that in Table 2, the unit of the amount of each component is gram (g).
[0215] (IP volume)
[0216] The IP amount is the weight ratio of the total amount of polyorganosiloxane formed by hydrolysis and dehydration condensation of the alkoxysilane component to the total amount of the polyorganosiloxane and the total amount of the radical polymerizable monomer component.
[0217] (Weight average molecular weight)
[0218] The weight average molecular weight of the organic-inorganic composite resin was measured by GPC using HLC-8320GPC manufactured by Tosoh Corporation as a liquid delivery system, TSK-GEL H type manufactured by Tosoh Corporation as a column, and THF as a solvent, and the weight average molecular weight was calculated by polystyrene conversion.
[0219] ( 29 Si-NMR)
[0220] The structural unit derived from the monoorganotrialkoxysilane was classified into a structural unit T1 having one siloxane bond, a structural unit T2 having two siloxane bonds, and a structural unit T3 having three siloxane bonds. The organic-inorganic composite resin was measured using AVANCE III HD500 manufactured by BRUKER. 29 In Si-NMR, the peak area ratio derived from each structure obtained was taken as the molar ratio of the T1, T2, and T3 structures contained in the organic-inorganic composite resin.
[0221] (Siloxane bond formation rate)
[0222] When the molar ratios of the structures T1, T2, and T3 are X, Y, and Z,
[0223] The value calculated by the formula: (1×X+2×Y+3×Z) / 3 was defined as the siloxane bond formation rate (condensation rate).
[0224] (Storage stability of composite resin solution)
[0225] Two bottles of samples were prepared by sealing the obtained composite resin solution in a sealed glass bottle. One bottle was placed in a 50°C dryer for 4 weeks, and the other bottle was stored in a constant temperature room controlled at 23°C for the same period. The viscosity of the composite resin solution after 4 weeks was evaluated by visual observation. The results are shown in Table 2.
[0226] A: No viscosity change ~ less than 10 times of viscosity increase estimated by naked eye observation; B: more than 10 times of viscosity increase estimated by naked eye observation; C: Gel
[0227] (Preparation and application of clear coating liquid)
[0228] 0.050 g of an organic tin compound U-20 as a curing catalyst and 0.050 g of S-100 as a diluting solvent were mixed with 10.0 g of the composite resin solution obtained in each of Examples and Comparative Examples to prepare a clear coating liquid.
[0229] 6 mil of the prepared clear coating liquid was applied to a 70×150×2 mm float glass plate and a 50×150×1 mm black ABS plate using an applicator to obtain a clear coating film having a thickness of about 0.076 mm when dried.
[0230] (Transparency of clear coating film)
[0231] The clear coating liquid was applied on a glass plate and aged in a thermostatic chamber adjusted to 23° C. for 1 week, and then the haze value of the clear coating film was measured and evaluated using a color / turbidity simultaneous measuring instrument OH400 (manufactured by Nippon Denshoku Industries Co., Ltd.).
[0232] A: no turbidity (haze value <5); B: turbidity (haze value ≥5)
[0233] (Gloss of clear coating)
[0234] The clear coating liquid was applied onto a black ABS plate and aged in a thermostatic chamber adjusted to 23° C. for one week, and then the gloss value of the clear coating film at 60° was measured and evaluated using a gloss meter. The results are shown in Table 2.
[0235] A: 60 or more; B: less than 60
[0236] (Surface drying time)
[0237] After applying the clear coating liquid on a glass plate, the clear coating liquid was aged in a thermostatic chamber adjusted to 23°C, and the time until the surface of the clear coating film was no longer sticky when the index finger was gently pressed and released was measured. The start time was set as the time immediately after application. The results are shown in Table 2.
[0238] (Gel ratio)
[0239] A 0.1 mm thick aluminum sheet was cut into a size of 2.5×2.5×0.1 mm with scissors, and 0.2 g of the clear coating liquid was dripped thereon. After aging in a constant temperature room adjusted to 23°C for 1 week, it was immersed in an acetone bath, and the gel ratio was calculated according to (insoluble part weight) ÷ (coating film weight) × 100. It should be noted that when immersed in the acetone bath, it was immersed in a bag made of 200 mesh wire mesh, and the insoluble part and the eluted part were separated / recovered. The results are shown in Table 2.
[0240] [Table 2-1]
[0241]
[0242] [Table 2-2]
[0243]
[0244] [Table 2-3]
[0245]
[0246] [Table 2-4]
[0247]
[0248] [Table 2-5]
[0249]
[0250] As shown in Table 2, the storage stability of the composite resin obtained in each example is good, and the transparency and gloss of the transparent coating film obtained using the composite resin are good. On the other hand, in Comparative Example 1, the transparency and gloss of the transparent coating film are insufficient. In addition, in Comparative Examples 2 to 5, gelation occurred and the composite resin could not be produced.
[0251] (Production of white enamel paint)
[0252] Titanium oxide fine particles were dispersed in the composite resin solutions obtained in Comparative Example 1 and Examples 9 to 12, 15, 16, 21, 25, and 27 to 39 to obtain a resin solution for a white enamel paint. BYK-142 was added as a dispersant to assist in the dispersion of titanium oxide, MOA was added as a dehydrating agent to remove water from titanium oxide, and glass beads were used to break up the aggregation of titanium oxide fine particles.
[0253] First, titanium oxide fine particles and a small amount of composite resin solution were mixed to obtain a mill base in a manner that allows for easy dispersion at a high concentration. Then, the composite resin solution was further added and diluted to obtain a white enamel paint. The details are as follows.
[0254] [Abrasive]
[0255] In a mayonnaise bottle of 225 ml capacity, 30.15 g of the composite resin solution, 33.50 g of titanium oxide, 0.56 g of a dispersant, 0.50 g of a dehydrating agent, 0.35 g of S100 and 0.15 g of LAWS as dilution solvents, and 50 g of glass beads were added according to the description of "Abrasives" in Table 3, and the mixture was vibrated at high speed for 2 hours using a paint conditioner to obtain abrasives.
[0256] [dilution]
[0257] Next, according to the description of "Dilution" in Table 3, 70.35 g of the composite resin solution, 3.2 g of S100 as a dilution solvent, and 1.37 g of LAWS were added, and the mixture was shaken at high speed for 30 minutes using a paint conditioner to obtain 140.1 g of white enamel paint (excluding the weight of glass beads).
[0258] (Storage stability of white enamel paint)
[0259] Two bottles of the obtained white enamel paint were sealed in a sealed glass bottle. One bottle was placed in a 50°C dryer for 4 weeks, and the other bottle was kept in a constant temperature room controlled at 23°C for the same period. The viscosity of the paint after 4 weeks was evaluated by visual observation. The results are shown in Table 3.
[0260] A: No viscosity change ~ less than 10 times of viscosity increase estimated by naked eye observation; B: more than 10 times of viscosity increase estimated by naked eye observation; C: Gel
[0261] (Preparation and application of white enamel coating liquid)
[0262] 0.060 g of an organic tin compound U-20 as a curing catalyst and 0.060 g of S-100 as a diluting solvent were mixed with 10.0 g of the obtained white enamel paint to prepare a white enamel coating liquid to which a curing catalyst was added.
[0263] 6 mil of the prepared white enamel coating liquid to which a curing catalyst was added was applied to a float glass plate of 70×150×2 mm using an applicator, thereby obtaining a white enamel coating film having a thickness of about 0.090 mm when dried.
[0264] (Gloss of white enamel coating)
[0265] The white enamel coating liquid was applied on a glass plate and aged in a thermostatic chamber adjusted to 23° C. for 1 week, and then the gloss value of the white enamel coating film at 60° was measured and evaluated using a gloss meter.
[0266] A: 60 or more; B: 55 or more and less than 60; C: less than 55
[0267] [Table 3-1]
[0268]
[0269] [Table 3-2]
[0270]
[0271] [Table 3-3]
[0272]
[0273] As shown in Table 3, the white enamel paint obtained in each example has good storage stability, and the gloss of the white enamel coating film obtained using the white enamel paint is also good. In particular, the white enamel coating film obtained in Examples 31 to 33 has the best appearance, good pigment dispersibility, and good color matching properties.
Claims
1. A method for producing an organic-inorganic composite resin, the method comprising: A step of subjecting the alkoxysilane component to a hydrolysis and dehydration condensation reaction in the presence of water and a condensation catalyst to obtain a polyorganosiloxane having a silanol group; as well as a step of subjecting a radically polymerizable monomer component containing a (meth)acrylate monomer to radical polymerization in the presence of the polyorganosiloxane and the β-dicarbonyl compound; The alkoxysilane component contains: a monoorganotrialkoxysilane and / or a diorganodialkoxysilane (a-1) having a radical-reactive functional group having a radical reactivity lower than the growth reactivity of a methacryloyl group in radical polymerization, and a monoorganotrialkoxysilane and / or a diorganodialkoxysilane (a-2) having no radically reactive functional group, The radical reactive functional group showing a radical reactivity lower than the growth reactivity of the methacryloyl group in the radical polymerization is a vinyl group, The alkoxysilane component does not contain an alkoxysilane having a methacryl group, The ratio of (a-2) to the total of (a-1) and (a-2) is 70% by weight or more and 99% by weight or less, and 50% by weight or more of the organic groups contained in (a-2) are at least one selected from the group consisting of methyl, ethyl, and phenyl groups, The free radical reactive functional group equivalent calculated from the alkoxysilane component is within the range of 280 or more and less than 5000, The condensation catalyst is a phosphate ester or a neutral salt as an acidic catalyst, The amount of water added is 30 mol% or more and 60 mol% or less relative to 100% of the total number of moles of alkoxy groups directly bonded to silicon atoms contained in the alkoxysilane component, The organic-inorganic composite resin contains a poly(meth)acrylic acid chain and a polyorganosiloxane chain having a silanol group.
2. The method for producing an organic-inorganic composite resin according to claim 1, wherein: 50% by weight or more of the organic groups contained in (a-2) are methyl groups.
3. The method for producing an organic-inorganic composite resin according to claim 1 or 2, wherein: The proportion of the monoorganotrialkoxysilane and / or diorganodialkoxysilane having a vinyl group to the entire alkoxysilane component is 2% by weight or more and 30% by weight or less.
4. The manufacturing method according to claim 1 or 2, comprising: In the step of obtaining the polyorganosiloxane, the weight average molecular weight of the polyorganosiloxane is 1200, 1300, 1400, 1500, 1600, 1700, 1900, 2100 or 2400.
5. The manufacturing method according to claim 1 or 2, wherein: The weight ratio of the polyorganosiloxane chain to the entire organic-inorganic composite resin is 20% by weight or more and 80% by weight or less.
6. The manufacturing method according to claim 1 or 2, comprising: From the hydrolysis and dehydration condensation reaction to the completion of the radical polymerization, the temperature is controlled so that the temperature of the reaction system does not substantially decrease.
7. The manufacturing method according to claim 1 or 2, wherein: The hydrolysis and dehydration condensation reactions and the radical polymerization are carried out in an atmosphere substantially free of oxygen molecules.