Optical sensor, method for selecting an optical sensor, and detector for optical detection
By using specific structures and materials in optical sensors, combined with technologies such as nanoindentation and microwave reflection methods, the problem of insufficient performance and stability of optical sensors in safety equipment is solved, achieving high performance and long-term stable infrared detection capabilities. .
Patent Information
- Application Number
- CN202080021045.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-15
- Filing Date
- 2020-03-13
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-03-13
AI Technical Summary
It is difficult for existing optical sensors to maintain long-term high performance and stability in safety-related equipment. Especially in applications such as gas sensors, spark sensors, or flame sensors, there are problems with performance degradation and insufficient stability.
An optical sensor stack structure including a substrate, a photoconductive material layer and an amorphous cover is used to ensure that the Young's modulus and hardness are within a specific range through quasi-static nanoindentation measurement, combined with microwave reflection method and wavelength dispersive X-ray spectroscopy. Optimizing static and dielectric properties, using chalcogen compounds of lead as the photoconductive material, and improving long-term stability with amorphous lid encapsulation.
It achieves high performance and long-term stability of optical sensors, meets the application requirements of safety-related equipment, and ensures efficient detection capabilities and durability in the infrared spectrum range.
Smart Images

Figure CN113632242B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an optical sensor and a detector comprising such an optical sensor for optical detection, in particular of optical radiation in the infrared spectral range, in particular with regard to sensing at least one of transmission, absorption, emission and reflection provided by at least one light beam, or for determining the position of at least one object, in particular with regard to the depth or both the depth and the width of the at least one object. Further, the invention relates to a method for manufacturing an optical sensor and various uses of the optical sensor and the detector. Such devices, methods and uses can be used in various fields of safety technology, in particular in the form of safety-related devices, such as gas sensors, spark sensors, or flame sensors. However, further applications, in particular within the field of safety technology, are also possible. Background Art
[0002] A variety of detectors for optically detecting at least one object are known from the perspective of optical sensors.
[0003] WO 2012 / 110924 A1 discloses a detector comprising at least one optical sensor, wherein the optical sensor exhibits at least one sensor area. In this context, the optical sensor is designed to generate at least one sensor signal in a manner that depends on the illumination of the sensor area. According to the FIP effect as described herein, given the same total power of the illumination, the sensor signal here depends on the geometry of the illumination, in particular the beam profile of the illumination on the sensor area. Furthermore, the detector has at least one evaluation device designated to generate at least one geometric information item from the sensor signal, in particular at least one geometric information item about the illumination and / or the object.
[0004] WO 2014 / 097181 A1 discloses a method and a detector for determining the position of at least one object by using at least one transverse optical sensor and at least one longitudinal optical sensor. Preferably, a stack of longitudinal optical sensors is used, in particular to determine the longitudinal position of an object with high accuracy and without ambiguity. Further, WO 2014 / 097181 A1 discloses a human-machine interface, an entertainment device, a tracking system, and a camera, each of which comprises at least one such detector for determining the position of at least one object.
[0005] WO 2016 / 120392 A1 discloses further types of materials suitable as longitudinal optical sensors. In this article, the sensor area of the longitudinal optical sensor includes a photoconductive material, wherein, given the same total power of illumination, the conductivity in the photoconductive material depends on the beam profile of the light beam in the sensor area. Therefore, the longitudinal sensor signal depends on the conductivity of the photoconductive material. Preferably, the photoconductive material is selected from the following: lead sulfide (PbS), lead selenide (PbSe), lead telluride (PbTe), cadmium telluride (CdTe), indium phosphide (InP), cadmium sulfide (CdS), cadmium selenide (CdSe), indium antimonide (InSb), mercury cadmium telluride (HgCdTe; MCT), copper indium sulfide (CIS), copper indium gallium selenide (CIGS), zinc sulfide (ZnS), zinc selenide (ZnSe), or copper zinc tin sulfide (CZTS). Further, solid solutions and / or doped variants thereof are also feasible. Further, a lateral optical sensor having a sensor area is disclosed, wherein the sensor area comprises a layer of photoconductive material, preferably embedded between two layers of transparent conductive oxide and at least two electrodes. Preferably, at least one of the electrodes is a split electrode having at least two partial electrodes, wherein the lateral sensor signal provided by the partial electrodes is indicative of the x and / or y position of an incident light beam within the sensor area.
[0006] WO 2018 / 019921 A1 discloses an optical sensor comprising: at least one layer of photoconductive material; at least two separate electrical contacts contacting the layer of photoconductive material; and a covering layer deposited on the layer of photoconductive material, wherein the covering layer is an amorphous layer comprising at least one metal-containing compound. The optical sensor can be supplied as a non-bulky sealed package, which nevertheless provides a high degree of protection against possible degradation caused by humidity and / or oxygen. In addition, the covering layer is capable of activating the photoconductive material resulting in increased performance of the optical sensor. Further, the optical sensor can be easily manufactured and integrated on a circuit carrier device.
[0007] In addition, European patent application 19 152 511.2 filed on January 18, 2019 discloses an optical sensor comprising: a substrate; at least one layer of photoconductive material applied directly or indirectly to the substrate; at least two separate electrical contacts contacting the layer of photoconductive material; and a cover covering the photoconductive material and accessible surfaces of the substrate, wherein the cover is an amorphous cover comprising at least one metal-containing compound.
[0008] In particular, optical sensors comprising at least one photoconductive material are often used in safety-related devices, such as gas sensors, spark sensors, or flame sensors. In addition, other kinds of applications, in particular in the field of safety technology, are also possible. Therefore, it is desirable to maintain the high performance and stability of the optical sensors for a long time to meet the specific requirements peculiar to these fields of application. Regardless of the advantages suggested by the above-mentioned devices and detectors, which have significantly improved the performance and long-term stability of optical sensors, in particular with regard to the advantages achieved by reactive encapsulation as expressed, for example, in WO 2018 / 019921A1 filed on January 18, 2019 and in European patent application 19 152 511.2, there is still a need for improvements regarding simple, cost-effective and still reliable optical sensors and spatial detectors.
[0009] N.Mukherjee, GGKhan, A.Sinha and A.Mondal, Synthesis of band gapengineered applications and materials science Pb x Cd 1_x Se thin films:Astudy ontheir optical,electrical,structural and localized mechanical properties(Bandgap engineering applications and materials science synthesis of Pb x Cd 1_x Se thin films: studies on their optical, electrical, structural and local mechanical properties), Phys. Status Solidi A 207, No. 8, pp. 1880-1886 (2010) describes a method for preparing Pb x Cd 1-x A novel electrochemical technique for bandgap engineering of Se-type IV-II-VI ternary solid solution systems. We have used a self-contained modified electrochemical cell consisting of a Pb anode and a transparent conductive oxide (TCO)-coated glass cathode, which contains Pb(CH3COO)2, Cd(CH3COO)2, H2SeO3, and Na2EDTA solutions with appropriate concentrations as the working electrolyte. X-ray diffraction (XRD) pattern analysis confirmed that highly crystalline Pb x Cd 1-x Se formation, while scanning electron micrographs (SEM) show uniform deposition with a dense surface morphology. TCO / Pb x Cd 1-xGood rectifying properties of the Se heterojunction were established from current-voltage measurements, indicating the p-type conducting nature of the deposited ternary compound.The mechanical properties of such thin films were measured by nanoindentation.
[0010] MS Darrow, W B White, and R. Roy, Micro-Indentation Hardness Variation as a Function of Composition for Polycrystalline Solutions in the Systems PbS / PbTe, PbSe / PbTe, and PbS / PbSe, Journal of Materials Science 4 (1969) 313-319, describes that the Vickers microindentation hardness as a function of composition has been measured for polycrystalline solutions of lead chalcogenide systems, and the results are compared with the exsolution trends as suggested by the subsolid line features of the same figures. Each system exhibits a positive deviation from the linear hardness relationship between the end-member compounds. The most significant hardening is observed for PbS / PbTe; the maximum hardness occurs at about 30 mole % Pb Te, consistent with a large miscibility interval with a solvus maximum (critical point) of about 30 mol. % Pb Te and about 805°C. The least amount of hardening is observed for the system PbS / PbSe, which has no exsolution at temperatures as low as 300°C. The hardness vs. composition curve is approximately symmetrical about the 50 mol.% composition. In between these two systems, the PbSe / PbTe crystallization solution exhibits an asymmetric hardness / composition curve with a maximum hardness at about 30 mol.% PbTe. Partial phase studies indicate the possibility of a solvus maximum at 500 to 600°C on the PbSe-rich side of the diagram.
[0011] Problems to be solved by the present invention
[0012] The problem solved by the present invention is therefore that of specifying a device and a method for optical detection which at least substantially avoid the disadvantages of known devices and methods of this type.
[0013] In particular, it is desired to provide an optical sensor comprising at least one photoconductive material and a detector for optical detection comprising such an optical sensor, wherein the high performance and stability of the optical sensor can be maintained for a long period of time in order to meet the specific requirements of applications as safety-related devices, such as gas sensors, spark sensors or flame sensors, and applications in the field of safety technology. Summary of the invention
[0014] This problem is solved by the invention having the features of the independent patent claims. Advantageous developments of the invention which can be realized individually or in combination are found in the dependent claims and / or in the following description and detailed examples.
[0015] As used herein, the expressions "have", "include" and "comprise" and grammatical variations thereof are used in a non-exclusive manner. Thus, the expression "A has B" as well as the expression "A includes B" or "A contains B" may refer to the fact that A contains one or more further components and / or members in addition to B, as well as the situation in which no other components, members or elements are present in A in addition to B.
[0016] In a first aspect of the present invention, an optical sensor is disclosed. In this context, the optical sensor according to the present invention comprises a stack: wherein the stack has:
[0017] - substrate,
[0018] - at least one layer of photoconductive material, applied to said substrate,
[0019] - a cover covering the accessible surface of said layer of photoconductive material.
[0020] and at least two separate electrical contacts, spatially separated from the stack and contacting the layer of photoconductive material,
[0021] The optical sensor exhibits a Young's modulus in a quasi-static nanoindenter measurement of the stack.
[0022] 75 GPa to 107 GPa at a penetration depth of 100 nm,
[0023] 47 to 127 GPa at a penetration depth of 300 nm,
[0024] 49 to 119 GPa at a penetration depth of 1000 nm,
[0025] And hardness
[0026] 1.20 GPa to 4.70 GPa at a penetration depth of 100 nm,
[0027] 1.60 GPa to 4.60 GPa at a penetration depth of 300 nm,
[0028] 1.60 GPa to 8.00 GPa at a penetration depth of 1000 nm.
[0029] As used herein, an "optical sensor" is generally a device that is designed to generate at least one sensor signal in a manner that depends on the illumination of a sensor area by a light beam. The sensor signal may generally be any signal that is indicative of at least one of the transmission, absorption, emission and reflection of an incident light beam illuminating the sensor area. As an example, the sensor signal may be or may include a digital and / or analog signal. As an example, the sensor signal may be or may include a voltage signal and / or a current signal. Additionally or alternatively, the sensor signal may be or may include digital data. The sensor signal may include a single signal value and / or a series of signal values. The sensor signal may also include any signal derived by combining two or more separate signals, such as by averaging two or more signals and / or by forming a quotient of two or more signals.
[0030] The "object" may generally be any object selected from a living object and a non-living object. Thus, as an example, the at least one object may include one or more articles and / or one or more parts of articles. Additionally or alternatively, the object may be or may include one or more living beings and / or one or more parts thereof, such as one or more body parts of a human (e.g., a user) and / or an animal.
[0031] As used herein, "position" generally refers to any item of information about the position and / or orientation of an object in space. For this purpose, as an example, one or more coordinate systems may be used, and the position of the object may be determined using one, two, three or more coordinates. In this document, a first coordinate may refer to an object depth, which refers to the distance between the optical sensor and the object, and two other coordinates that may be perpendicular to the first coordinate may refer to the width of the object. As an example, one or more Cartesian coordinate systems and / or other types of coordinate systems may be used. In one example, the coordinate system may be a coordinate system of the detector in which the detector has a predetermined position and / or orientation.
[0032] According to the invention, the optical sensor comprises at least one layer of photoconductive material, wherein the layer of photoconductive material can be used as a sensor area. As used herein, the "sensor area" is considered to be a partition of the optical sensor designed to receive illumination of the optical sensor by the light beam, wherein illumination in the manner as received by the sensor area can trigger the generation of the at least one sensor signal, wherein the generation of the sensor signal can be governed by a defined relationship between the sensor signal and the manner of illumination of the sensor area. According to the invention, the sensor area is formed by the photoconductive layer or a partition thereof. In this context, the sensor area can be formed as a single sensor area. In a particular embodiment, the photoconductive layer may comprise at least two separate sensor areas, preferably an array of separate sensor areas, which are applied directly or indirectly to the same substrate, also indicated as a "common substrate", which can therefore present a considerable area.
[0033] As used herein, the term "photoconductive material" refers to a material that is able to hold an electric current and thus exhibits a certain electrical conductivity, wherein, in particular, the electrical conductivity depends on the illumination of the material. Since resistivity is defined as the reciprocal value of the electrical conductivity, alternatively, the term "photoresistive material" may also be used to name the same class of materials. In materials of this class, the electric current can be conducted through the material via at least one electrical contact to at least one second electrical contact, wherein the first electrical contact is isolated from the second electrical contact, while both the first electrical contact and the second electrical contact are directly connected to the material. For this purpose, the direct connection can be provided by any known measures known from the prior art, such as electroplating, welding, soldering, wire bonding, thermosonic bonding, stitch bonding, ball bonding, wedge bonding, compatibility bonding, thermocompression bonding, anodic bonding, direct bonding, plasma activated bonding, eutectic bonding, glass paste bonding, adhesive bonding, transient liquid phase diffusion bonding, surface activated bonding, surface activated bonding, tape automated bonding, or deposition of highly conductive substances, in particular metals like gold, beryllium-doped gold, copper, aluminum, silver, platinum, or palladium at the contact strips and alloys comprising at least one of the mentioned metals.
[0034] For the purposes of the present invention, the photoconductive material as used in the sensor region of the optical sensor may preferably include an inorganic photoconductive material, and / or a solid solution thereof and / or a doped variant thereof. As used herein, the term "solid solution" refers to a state of a photoconductive material in which at least one solute may be included in a solvent, in which a homogeneous phase is formed, and in which the crystal structure of the solvent may generally be unchanged by the presence of the solute. For example, the binary PbSe may be dissolved in PbS to produce PbS 1-x Se x, where x can vary from 0 to 1. As further used herein, the term "doped variant" can refer to a state of a photoconductive material in which individual atoms other than those constituting the material itself are introduced into sites within the crystal occupied by intrinsic atoms in the undoped state.
[0035] In this aspect, the inorganic photoconductive material may in particular include one or more of the following: selenium, tellurium, selenium-tellurium alloys, metal oxides, group IV elements or compounds (i.e., elements from group IV or compounds having at least one group IV element), group III-V compounds (i.e., compounds having at least one group III element and at least one group V element), group II-VI compounds (i.e., compounds having at least one group II element or at least one group XII element on the one hand and at least one group VI element on the other hand), and / or chalcogenide compounds, which may preferably be selected from the group including the following: sulfide chalcogenide compounds, selenide selenide compounds, ternary chalcogenide compounds, quaternary and higher chalcogenide compounds. As commonly used, the term "chalcogenide compound" refers to compounds of group 16 elements of the periodic table that may include elements other than oxides, i.e., sulfides, selenides, and tellurides. Further, the term "chalcogenide compound" may also refer to mixed chalcogenide compounds, such as sulfoselenides.
[0036] In a particularly preferred embodiment of the present invention, the photoconductive material as used in the optical sensor can be selected from chalcogen compounds of lead, preferably lead sulfide (PbS), solid solutions and / or doped variants thereof. Since the particularly preferred photoconductive materials are generally known to exhibit different absorption characteristics in the infrared spectral range, an optical sensor having a layer comprising the mentioned preferred photoconductive materials can preferably be used as an infrared sensor. However, other embodiments and / or other photoconductive materials such as those disclosed in WO 2018 / 019921 A1 filed on January 18, 2019 and European patent application 19 152 511.2 may also be feasible.
[0037] Regarding the photoconductive material, it includes those material layers that may include at least several crystals exhibiting a size of 15 nm or more. In this article, the layer of the photoconductive material can be manufactured by applying at least one deposition method that can be selected from the group including the following: vacuum evaporation, sputtering, atomic layer deposition, chemical vapor deposition, spray pyrolysis, electrodeposition, anodization, electroconversion, chemical immersion growth, continuous ionic adsorption and reaction, chemical bath deposition, dissolved gas interface technology. Therefore, the layer of the photoconductive material can exhibit a thickness of 10nm to 100μm, preferably 100nm to 10μm, and more preferably 300nm to 5μm. However, other photoconductive materials as mentioned above and / or below may also be feasible for this purpose and may also be processed in the same or similar manner.
[0038] Preferably, the photoconductive material can be manufactured by depositing the corresponding material on an insulating substrate, preferably on a substrate as described in more detail below, in particular for providing mechanical stability to the layer of photoconductive material. In this way, by depositing the selected layer on the appropriate substrate and providing at least two separate electrical contacts, an optical sensor according to the invention can be obtained. In this context, the illumination of the photoconductive material in the sensor area by an incident light beam causes a change in the electrical conductivity in the layer of the illuminated photoconductive material.
[0039] As mentioned above, the layer of photoconductive material can be applied to at least one substrate. As commonly used, the term "substrate" refers to an elongated body suitable for carrying a layer of material (particularly a photoconductive material as used herein), in particular for providing mechanical stability to the layer of photoconductive material. Therefore, the layer of photoconductive material can be applied to the substrate indirectly or preferably directly. In this article, the term "directly" refers to attaching the layer of photoconductive material directly to the substrate, while the term "indirectly" refers to attaching the layer of photoconductive material to the substrate via at least one intermediate layer (such as a bonding layer). Preferably, the substrate can be provided as a layer having a lateral extension that exceeds the thickness of the layer by at least 5 times, preferably at least 25 times, more preferably at least 100 times. In particular, the thickness of the substrate can have a range of 10μm to 2000μm, preferably 50μm to 1000μm, more preferably 100μm to 500μm.
[0040] Preferably, at least one of the substrate and the cover can be optically transparent in a selected wavelength range, in particular in the infrared spectral range or a subregion thereof, as indicated elsewhere herein. Therefore, it can be particularly advantageous to select a material as used for the cover to be preferably optically transparent in the desired wavelength range, in particular, by exhibiting suitable absorption characteristics. Alternatively or in addition, the material applied to the substrate can exhibit optical transparency properties in the desired wavelength range. In particular, this feature can allow the selection of a wider range of materials for the cover material, which may not be optically transparent in the desired wavelength range, as long as the substrate can exhibit sufficient transparency. For this purpose, the substrate can in particular include at least one at least partially transparent insulating material, wherein the insulating material can in particular be selected from at least one of the following: glass, quartz, fused quartz, metal oxides, or ceramic materials, preferably sapphire (Al2O3), wherein glass or quartz are particularly preferred.
[0041] In a particularly preferred embodiment, the substrate may be applied directly or indirectly to a circuit carrier device, such as a printed circuit board (PCB). In this document, the term "printed circuit board", which is usually abbreviated to "PCB", refers to a non-conductive planar board on which at least one thin sheet of conductive material (especially a copper layer) is applied (especially laminated) to the board. Other terms referring to this type of circuit carrier that also includes one or more electronic, electrical, and / or optical elements may also be denoted as a printed circuit assembly, abbreviated to "PCA", a printed circuit board assembly, abbreviated to "PCB assembly" or "PCBA", a circuit card assembly or abbreviated to "CCA" or simply "card". In a PCB, the board may include a glass epoxy board, wherein tissue paper (usually brown or brown) impregnated with phenolic resin may also be used as the board material. Depending on the number of thin sheets, the printed circuit board may be a single-sided PCB, a two-layer or double-sided PCB, or a multi-layer PCB, wherein different thin sheets are connected to each other by using so-called "vias". For the purposes of the present invention, the use of a single-sided PCB may be sufficient; however, other kinds of printed circuit boards may also be applicable. Double-sided PCBs may have metal on both sides, while multi-layer PCBs may be designed by sandwiching additional metal layers between further layers of insulating material. In a multi-layer PCB, the layers may be laminated together in an alternating manner, wherein each metal layer may be etched separately, and wherein internal vias may be plated before the multiple layers are laminated together. Further, the vias may be or include copper plated holes, which may preferably be designed as a conductive path through the insulating board.
[0042] The substrate carrying the layer of photoconductive material, the corresponding electrical contacts and, if applicable, further layers can be arranged on the circuit carrier device, such as the PCB, in particular by gluing, soldering, welding, or depositing them directly or indirectly on adjacent surfaces of the circuit carrier device in another way. For example, the substrate can be attached to the circuit carrier device, such as the PCB, by a film of glue placed between the substrate and the adjacent surface of the circuit carrier device, such as the PCB. For further embodiments of the printed circuit board, it can be https: / / en.wikipedia.org / wiki / Printed_circuit_board Alternatively, however, other kinds of circuit carriers may also be suitable.
[0043] Further, the optical sensor according to the invention comprises a cover covering an accessible surface of the photoconductive material and preferably of the substrate. As commonly used, the phrase "accessible surface" refers to a body, in particular a layer of the photoconductive material or, if applicable, a part of the substrate, which can be reached by the atmosphere surrounding the optical sensor. Preferably, the cover can be applied in such a way that it can directly contact the top and the sides of the layer of photoconductive material and at least the sides of the substrate. As already indicated above, the substrate carries the layer of photoconductive material so that the top of the layer of photoconductive material refers to an extended surface of the photoconductive material which is neither directly nor indirectly applied to the substrate. As commonly used, the term "layer" refers to an elongated body comprising two extended surfaces with a side arranged between them. Since the photoconductive material and the substrate are provided as layers, they each comprise a side.
[0044] In a preferred embodiment, the cover may completely cover the accessible surfaces of the layer of photoconductive material and the sides of the substrate, in particular in a preferred arrangement in which the substrate can be attached to a circuit carrier device, such as a PCB, in particular in the manner as described above. In this preferred embodiment, the cover may be a continuous coating that continuously covers the layer of photoconductive material and the sides of the substrate. Thus, the cover may coat all accessible surfaces of the photoconductive material and the substrate, thereby preventing direct contact between the layer of photoconductive material or the substrate with the surrounding atmosphere, thereby avoiding degradation of the photoconductive material by external influences, such as humidity and / or oxygen. However, as disclosed in WO 2018 / 019921 A1, a cover deposited only on the layer of photoconductive material may already improve the long-term stability of the optical sensor. As a result, the cover helps to reduce or exclude external influences by minimizing or reducing the influence of humidity and / or oxygen on the layer of photoconductive material. Furthermore, a cover that also covers the accessible surface of the substrate may improve such effects by blocking and / or obstructing pathways that might otherwise be able to transmit humidity and / or oxygen to the layer of photoconductive material through or along the surface of the substrate.
[0045] Thus, the cover may be adapted to provide an improved encapsulation for the photoconductive material. As used herein, the term "encapsulation" may refer to a package, preferably an airtight package, in particular so as to avoid as far as possible a partial or complete degradation of the optical sensor or a partition thereof of the photoconductive material comprised within the sensor area of the optical sensor by external influences, such as by humidity and / or by oxygen comprised in the surrounding atmosphere. In this context, the encapsulation may preferably be adapted to cover all accessible surfaces of the photoconductive material, wherein it may be considered that a layer of the photoconductive material may be deposited on a substrate, which substrate may already be adapted to protect partitions of the surface of the photoconductive material. In other words, the substrate and the cover may be adapted in such a way that they may cooperate in order to achieve an improved encapsulation, preferably an improved sealed encapsulation, of the photoconductive material.
[0046] Preferably, at least one deposition method can be used to deposit the cover. For this purpose, the at least one deposition method can be particularly selected from atomic layer deposition, chemical vapor deposition, sputtering process, or a combination thereof. Therefore, in a particularly preferred embodiment, the cover can be or include an atomic deposition coating, a chemical vapor deposition coating, a sputtering coating, or a coating produced by using at least two of the mentioned deposition methods, wherein the atomic deposition coating or the coating produced by using a combination of atomic deposition and sputtering can be particularly preferred. In other words, in this particularly preferred embodiment, the cover can be obtainable by an ALD process, a CVD process, a sputtering process, or a combination thereof, and an ALD process or a combination of ALD and sputtering is particularly preferred. In particular, the cover may include at least one metal-containing compound, wherein the at least one metal can be selected from the group comprising the following: Al, Ti, Ta, Mn, Mo, Zr, Hf, and W. Further, the at least one metal-containing compound can be preferably selected from the group comprising the following: oxides, hydroxides, or a combination thereof. Thus, the metal-containing compound may preferably comprise at least one oxide, at least one hydroxide, or a combination thereof, preferably with Al, Ti, Zr or Hf. In a particularly preferred embodiment of the present invention, the metal-containing compound as comprised by the cover may be a composition comprising aluminum oxide and / or aluminum hydroxide, which, as commonly used, is also referred to as Al2O3 for simplicity's sake. Further, the cover may exhibit a thickness of 10nm to 600nm, preferably 20nm to 200nm, more preferably 40nm to 120nm, most preferably 50nm to 95nm. The thickness may particularly reflect the amount of metal-containing compound within the cover, which may be advantageous for achieving the above-mentioned function of providing encapsulation for the photoconductive material.
[0047] In a further particularly preferred embodiment of the invention, the cover may be conformal with respect to the adjacent surface of the photoconductive material or the substrate. As defined above, the thickness of the conformal cover may therefore follow the corresponding surface of the photoconductive material or the substrate within a deviation of ±50nm, preferably ±20nm, most preferably ±10nm, wherein the deviation may occur at least for at least 90%, preferably for at least 95%, most preferably for at least 99% of the surface of the cover, thereby disregarding any contamination or imperfection that may be present on the surface of the cover.
[0048] In a particularly preferred embodiment, the cover may partially or completely cover the electrical contact, which may be particularly configured to be bondable, such as one or more leads to an external circuit. In this article, the electrical contact may be bondable by wiring, such as gold or aluminum wire, wherein the electrical contact may preferably be bondable by the cover. In a specific embodiment, an adhesive layer may be provided at the electrical contact, wherein the adhesive layer may be particularly suitable for bonding. For this purpose, the adhesive layer may include at least one of the following: Ni, Cr, Ti or Pd.
[0049] According to the invention, the substrate, the layer of photoconductive material and the cover are arranged in the form of a stack, wherein the electrical contact contacting the layer of photoconductive material is spatially separated from the stack. As commonly used, the term "stack" refers to an arrangement comprising at least two individual layers, wherein one of the individual layers is arranged on top of another of the individual layers with respect to a specific direction. With respect to the stack as described herein, a normal vector which may be perpendicular to the extension of the surface of at least one of the individual layers may be used as a specific direction according to which the stack may be arranged. Thus, the substrate may be considered as a base layer, the layer of photoconductive material may be located on top of it, and thus the cover may further be located on top of the layer of photoconductive material. Furthermore, this consideration may be demonstrated by the process of manufacturing the stack as described in more detail below, in particular by providing the substrate as the base layer, and successively depositing further layers, i.e., first, the layer of photoconductive material, and thereafter, the cover. After manufacture, the stack as a whole may be rotated in any direction, which may however have no effect on the arrangement and composition of the stack. Additional covering of the sides of the layer of photoconductive material and, if applicable, additional covering of the substrate by the cover, such as described in more detail elsewhere herein, may be further excluded from consideration in this regard.
[0050] Further according to the invention, the stack as comprised by the optical sensor as indicated above exhibits particularly selected static mechanical properties. As used herein, the term "mechanical properties" of a body such as the stack refers to the response of the body with respect to an incident force applied to the body, also represented by the term "sensitivity". In this document, the static mechanical properties referring to the response or sensitivity of the body with respect to an incident static force applied to the body can be achieved by performing quasi-static nanoindenter measurements on the body. As commonly used, the "quasi-static nanoindenter measurements" involve measurements of the Young's modulus (also represented by any of the terms "elastic modulus" or "elastic modulus") and hardness of the body, which are preferably performed according to standards EN ISO 14577-1:2015 and EN ISO 14577-4:2016. As further commonly used, the term "nanoindenter" refers to a probe having a tip designed to intrude into a very small volume of a sample comprising the stack in order to perform the quasi-static nanoindenter measurements. For this purpose, the tip of the nanoindenter may preferably comprise a cone geometry, wherein a "Bosch tip" according to standard EN ISO 14577-2:2015 may be particularly preferred. For further details about the quasi-static nanoindenter measurements, the probes involved and the results obtained, reference may be made to the standards as mentioned herein.
[0051] Thus, the Young's modulus of the body refers to the tensile elasticity of the body, which is related to the tendency of the body to undergo deformation along an axis under the application of a force along that axis. In particular, the Young's modulus is defined as the ratio of tensile stress to tensile strain, wherein the tensile stress is measured in GPa and relates to the ratio of the deformation caused on the body to the area to which the force is applied, and wherein the tensile strain is the dimensionless ratio of the deformation of the body with respect to a reference dimension on the body. In this context, the modification of the dimensions of the body may include the movement of the body, including the translation and / or rotation of the body, and / or the change of the shape of the body and therefore also the size or volume. According to the present invention, the Young's modulus is measured by using a nanoindenter as defined above. Further, the hardness of the body refers to the resistance of the body to a local deformation of the body, which is caused by a constant compressive load to the body, which can therefore also be measured by applying the nanoindenter. Therefore, the Young's modulus and the hardness can be considered as reliable metrics for determining the static mechanical properties of a stack as comprised by the optical sensor.
[0052] Surprisingly, it has been found that the optical sensor exhibits preferred properties, as shown in more detail below, where the stack comprises the following properties: in a quasi-static nanoindenter measurement of the stack, the Young's modulus
[0053] - 75 GPa to 107 GPa, preferably 80 GPa to 102 GPa, more preferably 86 GPa to 96 GPa at a penetration depth of 100 nm;
[0054] - 47 to 127 GPa, preferably 60 to 114 GPa, more preferably 74 to 100 GPa at a penetration depth of 300 nm; and
[0055] - 49 to 119 GPa, preferably 61 to 107 GPa, more preferably 72 to 96 GPa at a penetration depth of 1000 nm;
[0056] The hardness
[0057] - 1.20 GPa to 4.70 GPa, preferably 1.78 GPa to 4.12 GPa, more preferably 2.37 to 3.53 GPa at a penetration depth of 100 nm;
[0058] - 1.60 GPa to 4.60 GPa, preferably 2.10 GPa to 4.10 GPa, more preferably 2.60 GPa to 3.60 GPa at a penetration depth of 300 nm; and
[0059] At a penetration depth of 1000 nm, it is 1.60 GPa to 8.00 GPa, preferably 2.67 GPa to 6.93 GPa, and more preferably 3.73 GPa to 5.87 GPa.
[0060] Without wishing to be bound by theory, preferably, the above characteristics provide an appropriate description of the selected parameters that are preferably balanced in producing a long-term stable sensor with a desired high quality. In particular, the photoconductivity of the photoconductive sensor may be highly dependent on the crystallinity of the bulk material, preferably selected from the group consisting of crystal structure, crystal size, volume surface ratio and crystal defects. Further, the quality of the cover layer, which may be used as one or both of the active layers to provide surface defects that result in excellent detectivity and encapsulation, is highly dependent on the properties of its amorphous state, particularly including very low levels of crystallinity. In the case where the size of the photoconductive crystals will be small or the cohesion and / or bonding between the crystals will be weak, the hardness and Young's modulus will be small. In the case where the cover layer will have a high degree of crystallinity and / or the photoconductive crystals will be large, the hardness and Young's modulus will be large. Further, the hardness and Young's modulus characterize the connectivity and bonding between the cover layer and the photoconductive crystals. Therefore, the hardness and Young's modulus measured at different penetration depths can be considered as ideal measures for characterizing the complex interaction of microscopic chemical parameters and their connection to the detectivity and long-term stability of the optical sensor.
[0061] In particular, the overall long-term quality of an optical sensor can thus be determined by measuring the sensor parameters a few thousand hours after its production. In order to obtain the selection criteria for high-quality long-term stable sensors according to the invention, the optical sensors and their relative dark resistance change relative to the dark resistance directly after production were measured 4000±50 hours after production, their relative detectivity change relative to the detectivity directly after production, and their absolute maximum deviation from the linear resistivity between -10V and +10V were determined. Therefore, the selection criteria are defined as optical sensors with a relative dark resistance change of less than 0.1% and a relative detectivity change of less than 0.1% and exhibiting an absolute maximum deviation from the linear resistivity between -10V and +10V of less than 0.1% of the dark resistance. For each optical sensor that meets the indicated selection criteria, only one of the following parameters: Young's modulus at a penetration depth of 100nm, 300nm, or 1000nm, or hardness at a penetration depth of 100nm, 300nm, or 1000nm, is determined in the quasi-static nanoindenter measurement of the stack. Each measurement is performed on 30 individual optical sensors. The set of measurements for each parameter yields a mean value μ and a standard deviation σ. Therefore, an optical sensor showing a parameter μ±1.5σ within an interval of 1.5σ around the mean value is considered to be an optical sensor according to the invention. An optical sensor showing a parameter μ±σ within an interval of σ around the mean value is a preferred optical sensor. An optical sensor showing a parameter μ±0.5σ within an interval of 0.5σ around the mean value is particularly preferred.
[0062] In a particularly preferred embodiment of the invention, the stack as comprised by the optical sensor as indicated above may also exhibit particularly selected dielectric properties. Thus, the dielectric properties referring to dielectric parameters such as the dielectric loss of the body with respect to an incident electromagnetic wave applied to the body may be achieved by a microwave reflectometry experiment which may be performed at a microwave frequency of 75 GHz, wherein a "reflectivity factor" denoted by the term "S11" is measured. As commonly used, the "S11 reflectivity factor" is defined in dB as 10 log(P refl / P in ), where P in represents the power of the incident microwave incident on the sample comprising the stack, and wherein, P refl represents the power of reflected microwaves reflected by the sample. Hence, the S11 reflectivity factor can be considered as a reliable measure for determining the dielectric properties of a stack as comprised by the optical sensor.
[0063] Surprisingly, it was further discovered that the optical sensor can exhibit preferred characteristics, as described in more detail below, where the stack includes the following characteristics, in a microwave reflectometry experiment at 75 GHz of the stack, the reflectivity factor S11 can have a range of -6.70 dB to -1.30 dB, preferably -5.80 dB to -2.20 dB, and more preferably -4.90 dB to -3.10 dB.
[0064] Without wishing to be limited by theory, the dielectric properties indicated above provide a further suitable description of the selected parameters that are preferably balanced in producing a long-term stable sensor with a desired high quality. In particular, microwave reflectometry can be used to provide an understanding of the dielectric parameters and effective mobility of defect-based charges in conductive materials. In addition, microwave reflectometry can be used to detect leaks in packages. In addition, microwave reflectometry can also be used to measure humidity. The photoconductive sensor is highly sensitive to humidity because humidity can change its photoconductive properties, which are particularly selected from charge mobility, resistivity, and detectivity. Further, charge mobility, resistivity, detectivity, and / or dielectric losses are particularly dependent on surface defects of the photoconductive crystal, including chemical bonds to the cap layer. Therefore, microwave reflectometry can constitute a preferred combined measurement of microscopic charge mobility, resistivity, detectivity, defect structure and humidity content, which can allow monitoring of a balance of complex and difficult to measure parameters, however, this can be considered to be preferred for obtaining a high performing sensor.
[0065] In particular, the overall long-term quality of the photoconductive sensor can therefore be determined by measuring the sensor parameters several thousand hours after its production. For each optical sensor that meets the indicated selection criteria as defined above, the reflectivity factor S11 of the stack is determined in a microwave reflectometry experiment at 75 GHz. Each measurement is performed on 30 individual optical sensors. The measurement set produces a mean value μ and a standard deviation σ for the reflectivity factor S11. As already indicated above, optical sensors showing a parameter μ±1.5σ within an interval of 1.5σ around the mean value are considered to be optical sensors according to the present invention. Optical sensors showing a parameter μ±σ within an interval of σ around the mean value are preferred optical sensors. Optical sensors showing a parameter μ±0.5σ within an interval of 0.5σ around the mean value are particularly preferred.
[0066] In a particularly preferred embodiment, the stack as comprised by the optical sensor as indicated above may also exhibit a particularly selected composition. As used herein, the term "composition" of the stack refers to the distribution of the composition within the stack. In this particularly preferred embodiment, wavelength dispersive X-ray spectroscopy (WDXS) may be used to determine the characteristics of the composition of the stack. As commonly used, the term "wavelength dispersive X-ray spectroscopy" or "WDXS" refers to a specific method for determining chemical composition and phase composition at a microscopic scale with high sensitivity and resolution. For this purpose, a sample comprising the stack is irradiated by an electron beam, wherein the X-rays emitted by the sample are collimated so as to irradiate a known single crystal at a precise angle, wherein the single crystal diffracts photons for collection by a detector. In this context, the single crystal, the sample and the detector are precisely mounted on a goniometer, wherein the distance between the sample and the single crystal may be equal to the distance between the single crystal and the detector. In a preferred embodiment, an automatic change unit may be used to change the single crystal, particularly depending on the incident energy, thereby allowing analysis of different compositions. Therefore, wavelength dispersive X-ray spectroscopy only counts X-rays of a single wavelength at a time.
[0067] In particular, the photoconductive material that can be used in the optical sensor according to the invention can be in particular a chalcogenide compound of lead, a solid solution thereof and / or a doped variant thereof, wherein, at the same time, the cover can be an amorphous cover comprising an aluminum-containing compound selected from oxides, hydroxides, or combinations thereof, also indicated here as "Al2O3" for simplicity. Thus, the use of the wavelength dispersive X-ray spectrometry allows the composition of a stack of covers comprising Al2O3 covering a PbS layer deposited on a glass substrate to be determined. In this context, the wavelength dispersive X-ray spectrometry measurements are performed using an electron beam microanalyzer as the detector and single crystals of thallium hydrogen phthalate (TAP) or pentaerythritol H (PET H) for WDXS, wherein the WDXS measurements can preferably be performed using an accelerating voltage of 20 kV. Thus, the Al K H and Pb S can be measured at, respectively, 100 kV. α1 Line, Pb M α1 Line and SK α1 The net counts for the WDXS measurement are determined from the peak maximum of the line.
[0068] Surprisingly, it has been further found that the optical sensor can exhibit preferred properties in the following situation: wherein wavelength dispersive X-ray spectroscopy using the stack of the electron beam microanalyzer and an accelerating voltage of 20 kV may result in α1 The net counts / s·nA measured at the peak maximum of the line are similar to those in Pb M α1The ratio of net counts / s·nA measured at the peak maximum of the line is between 0.113 and 0.279, preferably between 0.141 and 0.251, more preferably between 0.168 and 0.224.
[0069] In another particularly preferred embodiment, wherein the lead chalcogenide compound as the photoconductive material used in the optical sensor may be selected as lead sulfide (PbS), it has been further found that the optical sensor may exhibit preferred characteristics in the following case: wherein wavelength dispersive X-ray spectroscopy using the stack of the electron beam microanalyzer and an accelerating voltage of 20 kV may result in the detection of the Al K α1 The net counts / s·nA measured at the peak maximum of the line are similar to those in Pb M α1 Line neutralization in SK α1 Another ratio of the sum of the net counts / s·nA measured in the line has a range of 0.0841 to 0.1456, preferably has a range of 0.0944 to 0.1354, and more preferably has a range of 0.1046 to 0.1251.
[0070] Without wishing to be limited by theory, the dielectric properties indicated above provide a further appropriate description of the selected parameters that are preferably balanced in producing a long-term stable sensor with the desired high quality. In particular, the characteristics of the photoconductive sensor are highly dependent on the interaction of the photoconductive crystal and its interaction with the cover layer. The cover layer can be a conformal layer and thus follow the surface shape of the photoconductive crystal. Therefore, the distribution of chemical elements can vary along the normal to the surface. In this article, close to the substrate, the element distribution can be essentially the same as the element distribution of the photoconductive material, while close to the surface, the element distribution can be essentially the same as the cover layer, and in the middle, the element distribution may be highly dependent on the shape, size and / or agglomeration of the photoconductive crystal and the volume between crystals. For this purpose, known WDX spectra can be used to measure the element distribution not only on top of the surface but also below the surface. Therefore, WDX can be used to obtain an understanding of the complex parameters of the composition of the crystal and the cover layer.
[0071] In particular, the overall long-term quality of a photoconductive sensor can thus be determined by measuring the sensor parameters a few thousand hours after its production. For each optical sensor meeting the indicated selection criteria as defined above, only one of the following parameters was determined: for sensors comprising aluminum in the cap layer and Pb in the photoconductive layer, the Al K α1 The net counts / s·nA measured at the peak maximum of the line are similar to the Pb M α1or, for a sensor comprising Al in the cap layer and Pb and S in the photoconductive layer, the ratio of the net counts / s·nA measured at the peak maximum of the line, α1 The net counts / s·nA measured at the peak maximum of the line are similar to the Pb M α1 line and in the SK α1 The ratio of the sum of the net counts / s·nA measured in the line. Each measurement is performed on 30 individual optical sensors. The set of measurements yields a mean value μ and a standard deviation σ for the reflectivity factor S11. As already indicated above, optical sensors showing a parameter μ±1.5σ within an interval of 1.5σ around the mean value are considered to be optical sensors according to the invention. Optical sensors showing a parameter μ±σ within an interval of σ around the mean value are preferred optical sensors. Optical sensors showing a parameter μ±0.5σ within an interval of 0.5σ around the mean value are particularly preferred.
[0072] For further information about the optical sensor or any of its components (in particular the substrate, the photoconductive material, the cover, or the electrical contacts), reference may be made to WO 2018 / 019921 A1 filed on January 18, 2019 and to European patent application 19 152 511.2.
[0073] In a further aspect of the present invention, a method for selecting an optical sensor having an overall long-term quality is disclosed. In this context, the method comprises the following steps:
[0074] Providing an optical sensor, comprising a stack, wherein the stack has:
[0075] - substrate,
[0076] - at least one layer of photoconductive material, applied to said substrate, and
[0077] - a cover covering the accessible surface of said photoconductive material,
[0078] and at least two separate electrical contacts spaced apart from the stack and contacting the layer of photoconductive material;
[0079] measuring the Young's modulus and hardness of the stack in a quasi-static nanoindenter measurement; and
[0080] Select an optical sensor that exhibits preferred static mechanical properties in quasi-static nanoindenter measurements of the stack, Young's modulus
[0081] 75 GPa to 107 GPa at a penetration depth of 100 nm,
[0082] 47 GPa to 127 GPa at a penetration depth of 300 nm,
[0083] 49 GPa to 119 GPa at a penetration depth of 1000 nm, and
[0084] hardness
[0085] 1.20 GPa to 4.70 GPa at a penetration depth of 100 nm, and
[0086] 1.60 GPa to 4.60 GPa at a penetration depth of 300 nm,
[0087] 1.60 GPa to 8.00 GPa at a penetration depth of 1000 nm,
[0088] wherein the penetration depth is determined with respect to a surface of the stack, or
[0089] In case the Young's modulus and the hardness of the stack deviate from the preferred static mechanical properties of the stack, the optical sensor is rejected.
[0090] For further details concerning methods of selecting an optical sensor having an overall long-term quality, reference may be made to the description of optical sensors herein.
[0091] In a further aspect of the invention, a detector for optical detection, in particular of optical radiation, in particular in the infrared spectral range, in particular sensing at least one of transmission, absorption, emission and reflection provided by at least one light beam, or for determining the position of at least one object, in particular with respect to the depth or depth and width of the at least one object, is disclosed. According to the invention, the detector for optical detection of at least one object comprises:
[0092] - at least one optical sensor as described elsewhere herein, said optical sensor comprising at least one sensor area, wherein said optical sensor is designed to generate at least one sensor signal in a manner dependent on an illumination of said sensor area by a light beam;
[0093] as well as
[0094] - at least one evaluation device, wherein the evaluation device is designed to generate at least one item of information about the optical radiation provided by the light beam by evaluating a sensor signal of the optical sensor.
[0095] In this context, the listed components may be separate components. Alternatively, two or more of the components may be integrated into one component. Further, the at least one evaluation device may be formed as a separate evaluation device independently of the transmission device, preferably selected from at least one of an optical lens, a reflector, a beam splitter, an optical filter and an optical sensor, but may preferably be connected to the optical sensor in order to receive the sensor signal. Alternatively, the at least one evaluation device may be fully or partially integrated into the optical sensor.
[0096] According to the invention, the detector comprises at least one of the optical sensors as described elsewhere in this document. Thus, the detector can preferably be designed for detecting electromagnetic radiation over a fairly wide spectral range, wherein the infrared (IR) spectral range can be particularly preferred. In this context, indium gallium arsenide (InGaAs) can be particularly selected for the photoconductive layer in the sensor region of the optical sensor for wavelengths up to 2.6 μm, indium arsenide (InAs) for wavelengths up to 3.1 μm, lead sulfide (PbS) for wavelengths up to 3.5 μm, lead selenide (PbSe) for wavelengths up to 5 μm, indium antimonide (InSb) for wavelengths up to 5.5 μm; and mercury cadmium telluride (MCT, HgCdTe) for wavelengths up to 16 μm, wherein lead sulfide (PbS), its solid solutions and / or doped variants can be particularly preferred.
[0097] Thus, upon incidence of the sensor area by the light beam, the at least two electrical contacts can provide a sensor signal that depends on the conductivity of the photoconductive material. The term "light beam" generally refers to the amount of light emitted into a specific direction. Thus, the light beam can be a beam of light having a predetermined expansion in a direction perpendicular to the propagation direction of the light beam. Preferably, the light beam can be or can include one or more Gaussian beams, which can be characterized by one or more Gaussian beam parameters, such as a beam waist, a Rayleigh length, or one or more of any other beam parameters or combinations of beam parameters suitable for characterizing the development of the beam diameter in space / or the beam propagation. In this context, the light beam may be allowed by the object itself, i.e., may originate from the object. Additionally or alternatively, another origin of the light beam is feasible. Thus, as will be outlined in more detail below, one or more illumination sources that illuminate the object can be provided, such as by using one or more main rays or light beams, such as one or more main rays or light beams having predetermined characteristics. In the latter case, the light beam propagating from the object to the detector may be a light beam reflected by the object and / or a reflective device connected to the object.
[0098] As used herein, the term "evaluation device" generally refers to any device designed to generate the information item, that is, at least one item of information about sensing at least one of transmission, absorption, emission and reflection or at least one object or for determining the position of at least one object (particularly about the depth or depth and width of the at least one object). As an example, the evaluation device may be or may include one or more integrated circuits, such as one or more application specific integrated circuits (ASICs), and / or one or more digital signal processors (DSPs), and / or one or more field programmable gate arrays (FPGAs), and / or one or more data processing devices, such as one or more computers, preferably one or more microcomputers and / or microcontrollers. Additional components may be included, such as one or more pre-processing devices and / or data acquisition devices, such as one or more devices for receiving and / or pre-processing sensor signals, such as one or more AD converters and / or one or more filters. As used herein, the sensor signal may generally refer to one of the longitudinal sensor signals and, if applicable, the lateral sensor signal. Further, the evaluation device may include one or more data storage devices. Further, as outlined above, the evaluation device may include one or more interfaces, such as one or more wireless interfaces and / or one or more wired interfaces.
[0099] For further information about the detector for optical detection or any components thereof (in particular the evaluation device), reference can be made to WO 2014 / 097181 A and WO 2018 / 019921 A1.
[0100] In a further aspect of the invention, a method for manufacturing an optical sensor is disclosed. The method may preferably be used for manufacturing or producing at least one optical sensor according to the invention, such as at least one optical sensor according to one or more of the embodiments disclosed in more detail elsewhere in this document below. Therefore, for alternative embodiments of the method, reference may be made to the description of the various embodiments of the optical sensor.
[0101] The method comprises the following steps, which may be performed in a given order or in a different order. Further, additional method steps not listed may be provided. Unless otherwise expressly indicated, two or more or even all of the method steps may be performed at least partially simultaneously. Further, two or more or even all of the method steps may be performed repeatedly twice or even more than twice.
[0102] The method according to the invention comprises the following steps:
[0103] a) providing a substrate, at least one layer of photoconductive material applied to said substrate, and at least two separate electrical contacts contacting said layer of photoconductive material; and
[0104] b) thereafter, depositing an amorphous cover on an accessible surface of said layer of photoconductive material, whereby a stack comprising said substrate, obtaining said at least one layer of photoconductive material and said cover;
[0105] as well as
[0106] c) measuring the Young's modulus and hardness of the stack by quasi-static nanoindenter measurement; wherein the method for manufacturing the optical sensor is performed in the following manner: according to step c), the optical sensor exhibits, in the quasi-static nanoindenter measurement of the stack, the Young's modulus
[0107] 75 GPa to 107 GPa at a penetration depth of 100 nm,
[0108] 47 GPa to 127 GPa at a penetration depth of 300 nm,
[0109] 49 GPa to 119 GPa at a penetration depth of 1000 nm, and
[0110] The hardness
[0111] 1.20 GPa to 4.70 GPa at a penetration depth of 100 nm, and
[0112] 1.60 GPa to 4.60 GPa at a penetration depth of 300 nm,
[0113] It has a range of 1.60 GPa to 8.00 GPa at a penetration depth of 1000 nm.
[0114] According to step a), a substrate, at least one layer of photoconductive material and a separate electrical contact are provided. In particular, the respective materials for the substrate, the layer of photoconductive material and the electrical contact may be selected from the list of corresponding materials as set out above.
[0115] According to step b), the cover can be produced by using at least one of the methods as described above. In this context, step b) can be repeated at least once, preferably at least 10 times, more preferably at least 100 times. Preferably, the at least one metal-containing compound, and if applicable, other kinds of compounds, are deposited until they have completed a thickness of 10nm to 600nm, preferably 20nm to 200nm, more preferably 40nm to 100nm, most preferably 50nm to 95nm. In this context, the at least one metal-containing compound, and if applicable, other kinds of compounds, are deposited in such a way that the cover can preferably be conformal with respect to the adjacent surface of the photoconductive material. Thus, the thickness of the conformal cover can follow the corresponding surface of the layer of the photoconductive material or the substrate within a deviation of ±50nm, preferably ±20nm, most preferably ±10nm on at least 90%, preferably at least 95%, most preferably at least 99% of the surface of the conformal cover.
[0116] In a particularly preferred embodiment of the present invention, at least one deposition method is used to deposit the metal-containing compound. Preferably, the deposition method can be selected from at least one of the following: atomic layer deposition (ALD) process, chemical vapor deposition (CVD) process, sputtering process, or a combination thereof. For further details about the ALD process or the CVD process, reference can be made to the above description. For the purpose of providing the metal-containing compound, two different types of precursors can be preferably used, wherein the first precursor can be or include a metal organic precursor, and wherein the second precursor can be or include a fluid. As commonly used, the term "fluid" can refer to the non-solid state of the second precursor. For example, in order to provide an Al-containing compound, the first precursor can be or include TMA, that is, trimethylaluminum Al(CH3)3, and the second precursor can be or include H2O, oxygen, air or a solution thereof, or ozone. In this article, at least one of the precursors can be mixed with an inert gas, particularly N2 or Ar, particularly in order to provide a stable fluid flow.
[0117] As mentioned above, the desired optical sensor is typically designed to generate at least one sensor signal in a manner that depends on the illumination of the sensor area, such as that comprised by the optical sensor, by an incident light beam. For this purpose, at least two electrical contacts suitable for electrically contacting the photoconductive material comprised in the sensor area are also provided. Typically, the electrical contacts may be provided before or during any one of the method steps a) or b). In a particularly preferred embodiment, the electrical contacts may be provided before step b), such as by providing an evaporated metal layer, such as by known evaporation techniques, wherein the metal layer may in particular include one or more of the following: silver, aluminum, platinum, magnesium, chromium, titanium, gold, or graphene. Alternatively, the electrical contacts may be provided by a galvanic or chemical deposition process, such as electroless Ni, electroless Au, galvanic Ni, or galvanic Au. In this context, the cover may be deposited in such a manner that it may also completely or partially cover the electrical contacts. In this particular embodiment, the electrical contact at least partially, preferably completely covered by the cover can therefore be bonded to at least one external connection using a conductive lead, preferably in the form of a wire, in particular an Au, Al, or Cu wire, wherein the conductive lead can in particular be bonded to the electrical contact through the cover. For example, an Au contact applied by the cover can subsequently be contacted by a wire bond.
[0118] According to step c), the Young's modulus and the hardness of the stack are measured in a quasi-static nanoindenter measurement as described above and in more detail below.
[0119] In a particularly preferred embodiment, the method may further comprise the following steps:
[0120] d) determining a reflectivity factor S11 of the stack by applying microwave reflectometry to the stack at 75 GHz,
[0121] As further described above and in more detail below.
[0122] In another particularly preferred embodiment wherein the photoconductive material is selected from the group comprising lead chalcogen compounds, solid solutions and / or doped variants thereof, wherein the lead chalcogen compound may in particular be lead sulfide (PbS), and wherein the cap may be an amorphous cap comprising an aluminum-containing compound selected from oxides, hydroxides or combinations thereof, the method further comprises the following steps:
[0123] e) performing wavelength dispersive X-ray spectroscopy (WDXS) of said stack by using an electron beam microanalyser and an accelerating voltage of 20 kV,
[0124] As also described above and further in more detail below.
[0125] As indicated above, the method for manufacturing the optical sensor is therefore performed in such a way that the stack as comprised by the optical sensor exhibits desired static mechanical properties and preferably also desired dynamic mechanical properties and / or the desired composition.
[0126] Additionally, further details concerning the manufacturing method for the optical sensor may be found elsewhere in this document.
[0127] The device according to the present invention can be used in combination with surface mount technology packages, such as block chip carriers, ceramic leadless chip carriers, leadless chip carriers, leaded chip carriers, leaded ceramic chip carriers, dual leadless chip carriers, plastic leaded chip carriers, packages on packaged chip carriers, etc. Further, the device according to the present invention can be used in combination with standard through-hole or source mount technology semiconductor packages, such as DO-204, DO-213, metal electrode bladeless, DO-214, SMA, SMB, SMC, GF1, SOD, SOT, TSOT, TO-3, TO-5, TO-8, TO-18, TO-39, TO-46, TO-66, TO-92, TO-99, TO-100, TO-126, TO-220, TO-226, TO-247, TO252, TO-263, TO-263THIN, SIP, SIPP, DFN, DIP, DIL, Flat Package (Flat Pack), SO, SOIC, SOP, SSOP, TSOP, TSSOP, ZIP, LCC, PLCC, QFN, QFP, QUIP, QUIL, BGA, eWLB, LGA, PGA, COB, COF, COG, CSP, Flip Chip, PoP, QP, UICC, WL-CSP, WLP, MDIP, PDIP, SDIP, CCGA, CGA, CERPACK, CQGP, LLP, LGA, LTCC, MCM, MICRO SMDXT, etc. Further, the device according to the present invention can be used in combination with a pin grid array (PGA), such as OPGA, FCPGA, PAC, PGA, CPGA, etc. Further, the device according to the present invention can be used in combination with a flat package, such as CFP, CQFP, BQFP, DFN, ETQFP, PQFN, PQFP, LQFP, QFN, QFP, MQFP, HVQFP, SIDEBRAZE, TQFP, TQFN, VQFP, ODFN, etc. Further, the device according to the present invention can be used in combination with a small outline package, such as SOP, CSOP MSOP, PSOP, PSON, PSON, QSOP, SOIC, SSOP, TSOP, TSSOP, TVSOP, μMAX, WSON, etc. Further, the device according to the present invention can be used in combination with a chip-scale package, such as CSP, TCSP, TDSP, MICRO SMD, COB, COF, COG, etc. Furthermore, the device according to the present invention can be used in combination with a ball grid array, such as FBGA, LBGA, TEPBGA, CBGA, OBGA, TFBGA, PBGA, MAP-BGA, UCSP, μBGA, LFBGA, TBGA, SBGA, UFBGA, etc.Further, the device according to the invention may be combined with further electronic devices, such as chips in multi-chip packages, such as SiP, PoP, 3D-SiC, WSI, proximity communications, etc. For additional information concerning integrated circuit packaging, reference may be made to the source at the following address: .
[0128] - https: / / en.wikipedia.org / wiki / List_of_integrated_circuit_packaging_ types or
[0129] - https: / / en.wikipedia.org / wiki / List_of_integrated_circuit_package_ dimensions .
[0130] In a further aspect of the present invention, the use of the detector according to the present invention is disclosed. Wherein, for the purpose of use, the use of the detector is selected from the group including the following: gas sensing, fire detection, flame detection, temperature detection, smoke detection, combustion monitoring, spectroscopy, temperature sensing, motion sensing, industrial monitoring, chemical sensing, exhaust monitoring, safety applications. In particular, the detector can be used for infrared detection applications, heat detection applications, thermometer applications, heat seeking applications, flame detection applications, fire detection applications, smoke detection applications, temperature sensing applications, spectroscopy applications, etc. Further, the detector can be used to monitor exhaust, monitor combustion processes, monitor industrial processes, monitor chemical processes, monitor food processing processes, etc. Further, the detector can be used for temperature control, motion control, exhaust control, gas sensing, gas analysis, motion sensing, chemical sensing, etc. For further use of optical sensors and detectors as disclosed herein, reference can be made to WO2016 / 120392 A1 and WO 2018 / 019921 A1. However, further fields of application may still be conceivable.
[0131] The optical sensor and the detector, the method and the proposed use described above have considerable advantages over the prior art. Therefore, the optical sensor according to the invention can be particularly advantageous because the optical sensor and the stability of the optical sensor can be maintained for a long period of time. Therefore, these advantages are advantageous because they meet the specific requirements for applications as safety-related devices, such as gas sensors, spark sensors, or flame sensors, and for applications in the field of safety technology.
[0132] In summary, in the context of the present invention, the following embodiments are considered to be particularly preferred:
[0133] Embodiment 1: An optical sensor, comprising a stack, wherein the stack has:
[0134] - substrate,
[0135] - at least one layer of photoconductive material, applied to said substrate, and
[0136] - a cover covering the accessible surface of said photoconductive material,
[0137] and at least two separate electrical contacts, spatially separated from the stack and contacting the layer of photoconductive material,
[0138] Wherein, the optical sensor exhibits a Young's modulus in the quasi-static nanoindenter measurement of the stack.
[0139] 75 GPa to 107 GPa at a penetration depth of 100 nm,
[0140] 47 GPa to 127 GPa at a penetration depth of 300 nm,
[0141] 49 GPa to 119 GPa at a penetration depth of 1000 nm, and
[0142] hardness
[0143] 1.20 GPa to 4.70 GPa at a penetration depth of 100 nm,
[0144] 1.60 GPa to 4.60 GPa at a penetration depth of 300 nm,
[0145] 1.60 GPa to 8.00 GPa at a penetration depth of 1000 nm.
[0146] Embodiment 2: The optical sensor according to the above embodiment, wherein the optical sensor exhibits a
[0147] The Young's modulus
[0148] 80 GPa to 102 GPa at a penetration depth of 100 nm,
[0149] 60 GPa to 114 GPa at a penetration depth of 300 nm,
[0150] 61 GPa to 107 GPa at a penetration depth of 1000 nm, and
[0151] The hardness
[0152] 1.78 GPa to 4.12 GPa at a penetration depth of 100 nm,
[0153] 2.10 GPa to 4.10 GPa at a penetration depth of 300 nm,
[0154] 2.67 GPa to 6.93 GPa at a penetration depth of 1000 nm.
[0155] Embodiment 3: The optical sensor according to the above embodiment, wherein the optical sensor exhibits the following characteristics: in the quasi-static nanoindenter measurement of the stack,
[0156] The Young's modulus
[0157] 86 GPa to 96 GPa at a penetration depth of 100 nm,
[0158] 74 GPa to 100 GPa at a penetration depth of 300 nm,
[0159] 72 GPa to 96 GPa at a penetration depth of 1000 nm, and
[0160] The hardness
[0161] 2.37 GPa to 3.53 GPa at a penetration depth of 100 nm,
[0162] 2.60 GPa to 3.60 GPa at a penetration depth of 300 nm,
[0163] 3.73 GPa to 5.87 GPa at a penetration depth of 1000 nm.
[0164] Embodiment 4: The optical sensor according to any one of the preceding embodiments, wherein the optical sensor exhibits a reflectivity factor S11 of -6.70 dB to -1.30 dB in a microwave reflectometry experiment at 75 GHz of the stack.
[0165] Embodiment 5: The optical sensor according to the preceding embodiment, wherein the optical sensor exhibits a reflectivity factor S11 of -5.80 dB to -2.20 dB in a microwave reflectometry experiment at 75 GHz of the stack.
[0166] Embodiment 6: The optical sensor according to the above embodiment, wherein the optical sensor exhibits the following characteristics: in a microwave reflection method experiment at 75 GHz of the stack, the reflectivity factor S11 is -4.90 dB to -3.10 dB.
[0167] Embodiment 7: The optical sensor according to any one of the preceding embodiments, wherein the photoconductive material comprises an inorganic photoconductive material.
[0168] Embodiment 8: An optical sensor according to the above embodiments, wherein the inorganic photoconductive material comprises at least one of the following: selenium, tellurium, selenium-tellurium alloy, photoconductive metal oxide, Group IV element or compound, Group III-V compound, Group II-VI compound, chalcogenide compound, pnictogenide, halide, and solid solution and / or doped variants thereof.
[0169] Embodiment 9: The optical sensor according to the preceding embodiment, wherein the chalcogenide compound is selected from the group consisting of sulfide chalcogenides, selenide chalcogenides, telluride chalcogenides, ternary chalcogenides, quaternary and higher chalcogenides.
[0170] Embodiment 10: An optical sensor according to the above embodiments, wherein the sulfide chalcogenide compound is selected from the group including the following items: lead sulfide (PbS), cadmium sulfide (CdS), zinc sulfide (ZnS), mercury sulfide (HgS), silver sulfide (Ag2S), manganese sulfide (MnS), bismuth trisulfide (Bi2S3), antimony trisulfide (Sb2S3), arsenic trisulfide (As2S3), tin (II) sulfide (SnS), tin (IV) disulfide (SnS2), indium sulfide (In2S3), copper sulfide (CuS), cobalt sulfide (CoS), nickel sulfide (NiS), molybdenum disulfide (MoS2), iron disulfide (FeS2), chromium trisulfide (CrS3), copper indium sulfide (CIS), copper indium gallium selenide (CIGS), copper zinc tin sulfur (CZTS), and their solid solutions and / or doped variants.
[0171] Embodiment 11: An optical sensor according to any one of the two preceding embodiments, wherein the selenide chalcogenide compound is selected from the group consisting of lead selenide (PbSe), cadmium selenide (CdSe), zinc selenide (ZnSe), bismuth triselenide (Bi2Se3), mercury selenide (HgSe), antimony triselenide (Sb2Se3), arsenic triselenide (As2Se3), nickel selenide (NiSe), thallium selenide (TlSe), copper selenide (CuSe), molybdenum diselenide (MoSe2), tin selenide (SnSe), cobalt selenide (CoSe), indium triselenide (In2Se3), copper zinc tin selenide (CZTSe), and solid solutions and / or doped variants thereof.
[0172] Embodiment 12: An optical sensor according to any one of the three preceding embodiments, wherein the telluride chalcogenide compound is selected from the group consisting of lead telluride (PbTe), cadmium telluride (CdTe), zinc telluride (ZnTe), mercury telluride (HgTe), bismuth tritelluride (Bi2Te3), arsenic tritelluride (As2Te3), antimony tritelluride (Sb2Te3), nickel telluride (NiTe), thallium telluride (TlTe), cuprous telluride (CuTe), molybdenum ditelluride (MoTe2), tin telluride (SnTe), and cobalt telluride (CoTe), silver telluride (Ag2Te), indium tritelluride (In2Te3), and solid solutions and / or doped variants thereof.
[0173] Embodiment 13: The optical sensor according to any one of the four preceding embodiments, wherein the ternary chalcogenide is selected from the group consisting of mercury cadmium telluride (HgCdTe), mercury zinc telluride (HgZnTe), mercury cadmium sulfide (HgCdS), lead cadmium sulfide (PbCdS), lead mercury sulfide (PbHgS), copper indium disulfide (CuInS2), cadmium sulfide selenide (CdSSe), zinc sulfide selenide (ZnSSe), thallium sulfide selenide (TlSSe), cadmium zinc sulfide (CdZnS), cadmium chromium sulfide (CdCr2S4), mercury chromium sulfide (HgCr2S4), Copper chromium (CuCr2S4), cadmium lead selenide (CdPbSe), copper indium diselenide (CuInSe2), indium gallium arsenic (InGaAs), lead oxysulfide (Pb2OS), lead oxyselenide (Pb2OSe), lead sulfide selenide (PbSSe), arsenic telluride selenide (As2Se2Te), indium gallium phosphide (InGaP), gallium arsenide phosphide (GaAsP), aluminum gallium phosphide (AlGaP), cadmium selenite (CdSeO3), cadmium zinc telluride (CdZnTe), cadmium zinc selenide (CdZnSe), copper zinc tin sulfur selenide (CZTSSe), and solid solutions and / or doped variants thereof.
[0174] Embodiment 14: The optical sensor according to any of the preceding embodiments, wherein the photoconductive material is selected from chalcogenide compounds of lead, solid solutions and / or doped variants thereof.
[0175] Embodiment 15: The optical sensor according to the preceding embodiments, wherein the photoconductive material is selected from lead sulfide (PbS), its solid solutions and / or doped variants.
[0176] Embodiment 16: The optical sensor according to any of the preceding embodiments, wherein the cover is an amorphous cover comprising at least one metal-containing compound.
[0177] Embodiment 17: An optical sensor according to the preceding embodiments, wherein the at least one metal-containing compound comprises a metal or a semi-metal, wherein the metal is selected from the group consisting of Li, Be, Na, Mg, Al, K, Ca, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Ga, Rb, Sr, Y, Zr, Nb, Mo, Ru, Rh, Pd, Ag, Cd, In, Sn, Cs, Ba, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Tl, and Bi, and wherein the semi-metal is selected from the group consisting of B, Si, Ge, As, Sb, and Te.
[0178] Embodiment 18: The optical sensor of the preceding embodiment, wherein the at least one metal-containing compound comprises a metal selected from the group consisting of Al, Ti, Ta, Mn, Mo, Zr, Hf, and W.
[0179] Embodiment 19: The optical sensor according to any one of the preceding embodiments, wherein the at least one metal-containing compound is selected from the group consisting of oxides, hydroxides, chalcogenides, pnictides, carbides, or combinations thereof.
[0180] Embodiment 20: The optical sensor of any one of the four preceding embodiments, wherein the cover comprises an aluminum-containing compound selected from oxides, hydroxides, or combinations thereof.
[0181] Embodiment 21: The optical sensor according to embodiments 14 and 20, wherein the optical sensor further exhibits a peak in Al K α1 The net counts / s·nA measured at the peak maximum of the line are similar to those in Pb M α1 The ratio of net counts / s·nA measured at the peak maximum of the line ranged from 0.113 to 0.279.
[0182] Embodiment 22: The optical sensor according to the preceding embodiment, wherein the optical sensor further exhibits a wavelength dispersive X-ray spectroscopy using an electron beam microanalyzer and a stacked accelerating voltage of 20 kV at Al K α1 The net counts / s·nA measured at the peak maximum of the line are similar to those in Pb M α1 The ratio of net counts / s·nA measured at the peak maximum of the line ranged from 0.141 to 0.251.
[0183] Embodiment 23: The optical sensor according to the preceding embodiment, wherein the optical sensor further exhibits a wavelength dispersive X-ray spectroscopy using an electron beam microanalyzer and a stacked accelerating voltage of 20 kV at Al K α1 The net counts / s·nA measured at the peak maximum of the line are similar to those in Pb M α1 The ratio of net counts / s·nA measured at the peak maximum of the line ranged from 0.168 to 0.224.
[0184] Embodiment 24: The optical sensor according to embodiments 15 and 20, wherein the optical sensor further exhibits a peak in the AlK α1 The net counts / s·nA measured at the peak maximum of the line are similar to the Pb M α1 Line neutralization in SK α1 Another ratio of the sum of the net counts / s·nA measured in the lines ranged from 0.0841 to 0.1456.
[0185] Embodiment 25: The optical sensor according to the preceding embodiment, wherein the optical sensor further exhibits a peak in the Al K α1 The net counts / s·nA measured at the peak maximum of the line are similar to the Pb M α1 Line neutralization in SK α1 Another ratio of the sum of the net counts / s·nA measured in the lines ranged from 0.0944 to 0.1354.
[0186] Embodiment 26: The optical sensor according to the preceding embodiment, wherein the optical sensor further exhibits a peak in the Al K α1 The net counts / s·nA measured at the peak maximum of the line are similar to the Pb M α1 Line neutralization in SK α1 Another ratio of the sum of the net counts / s·nA measured in the line was 0.1046 to 0.1251.
[0187] Embodiment 27: The optical sensor of any of the preceding embodiments, wherein the cover coats the top and sides of the layer of photoconductive material.
[0188] Embodiment 28: The optical sensor according to the preceding embodiment, wherein the cover further coats at least a side surface of the substrate.
[0189] Embodiment 29: The optical sensor of any one of the preceding embodiments, wherein the cover completely covers the layer of photoconductive material and accessible surfaces of the sides of the substrate.
[0190] Embodiment 30: An optical sensor according to the preceding embodiment, wherein the cover is a continuous coating.
[0191] Embodiment 31: The optical sensor according to any of the preceding embodiments, wherein the cover has a thickness of 10 nm to 600 nm, preferably 20 nm to 200 nm, more preferably 40 nm to 120 nm, most preferably 50 nm to 95 nm.
[0192] Embodiment 32: The optical sensor of any of the preceding embodiments, wherein the cover is a conformal cover about an adjacent surface of the coating.
[0193] Embodiment 33: An optical sensor according to the preceding embodiments, wherein the thickness of the conformal cover follows the corresponding surfaces of the layer of photoconductive material and the substrate within a deviation of ±50 nm, preferably ±20 nm, most preferably ±10 nm over at least 90%, preferably at least 95%, most preferably at least 99% of the surface of the cover.
[0194] Embodiment 34: The optical sensor according to any one of the preceding embodiments, wherein the cover is or includes an atomic deposition coating or a chemical vapor deposition coating.
[0195] Embodiment 35: The optical sensor of any of the preceding embodiments, wherein the cover at least partially covers the electrical contacts.
[0196] Embodiment 36 The optical sensor according to the preceding embodiment, wherein the electrical contact is bondable, in particular by using wires, in particular Au, Al, or Cu wires.
[0197] Embodiment 37: According to any of the preceding embodiments of the optical sensor, the electrical contact is connectable through the cover.
[0198] Embodiment 38: The optical sensor according to any of the preceding embodiments, wherein the at least two electrical contacts are applied at different locations of the layer of photoconductive material.
[0199] Embodiment 39: The optical sensor according to any of the preceding embodiments, wherein the electrical contact comprises at least one electrode material selected from the group consisting of: Ag, Pt, Mo, Al and graphene.
[0200] Embodiment 40: The optical sensor according to the preceding embodiment, wherein an adhesive layer is provided at the electrical contacts, wherein the adhesive layer is suitable for bonding.
[0201] Embodiment 41: The optical sensor according to the preceding embodiment, wherein the bonding layer comprises at least one of the following: Ni, Cr, Ti or Pd.
[0202] Embodiment 42: The optical sensor according to any of the preceding embodiments, wherein the substrate has a thickness of 10 μm to 1000 μm, preferably 50 μm to 500 μm, more preferably 100 μm to 250 μm.
[0203] Embodiment 43: The optical sensor of any of the preceding embodiments, wherein at least one of the cover and the substrate is optically transparent over a range of wavelengths.
[0204] Embodiment 44: An optical sensor according to any one of the preceding embodiments, wherein the substrate is an electrically insulating substrate.
[0205] Embodiment 45: An optical sensor according to any one of the preceding embodiments, wherein the substrate comprises one of glass or quartz.
[0206] Embodiment 46 The optical sensor according to any of the preceding embodiments, wherein the substrate is applied directly or indirectly to a circuit carrier arrangement.
[0207] Embodiment 47 The optical sensor according to any one of the three preceding embodiments, wherein the circuit carrier arrangement is a printed circuit board.
[0208] Embodiment 48: A detector for optical detection of at least one object, comprising:
[0209] - at least one optical sensor according to any of the preceding embodiments, the optical sensor comprising at least one sensor area, wherein the optical sensor is designed to generate at least one sensor signal in a manner dependent on an illumination of the sensor area by a light beam; and
[0210] - at least one evaluation device, wherein the evaluation device is designed to generate at least one item of information about the optical radiation provided by the light beam by evaluating a sensor signal of the optical sensor.
[0211] Embodiment 49: The detector according to the preceding embodiment, wherein the detector is adapted to generate the sensor signal by measuring one or more of the resistance or the conductivity of at least a portion of the sensor area.
[0212] Embodiment 50 The detector according to the preceding embodiment, wherein the detector is adapted to generate the sensor signal by performing at least one current-voltage measurement and / or at least one voltage-current measurement.
[0213] Embodiment 51: A detector according to any one of the preceding embodiments relating to the detector, wherein the detector further comprises at least one transmission device adapted to direct the light beam onto the optical sensor.
[0214] Embodiment 52: A method for manufacturing an optical sensor, the method comprising the following steps:
[0215] a) providing a substrate, at least one layer of photoconductive material applied to said substrate, and at least two separate electrical contacts contacting said layer of photoconductive material; and
[0216] b) thereafter, depositing a cover on an accessible surface of said layer of photoconductive material, thereby obtaining a stack comprising said substrate, said at least one layer of photoconductive material and said cover; and
[0217] c) measuring the Young's modulus and hardness of the stack in a quasi-static nanoindenter measurement; wherein the method for manufacturing the optical sensor is performed in the following manner: according to step c), the optical sensor exhibits, in the quasi-static nanoindenter measurement of the stack, the Young's modulus
[0218] 75 GPa to 107 GPa at a penetration depth of 100 nm,
[0219] 47 GPa to 127 GPa at a penetration depth of 300 nm,
[0220] 49 GPa to 119 GPa at a penetration depth of 1000 nm, and
[0221] hardness
[0222] 1.20 GPa to 4.70 GPa at a penetration depth of 100 nm, and
[0223] 1.60 GPa to 4.60 GPa at a penetration depth of 300 nm,
[0224] 1.60 GPa to 8.00 GPa at a penetration depth of 1000 nm.
[0225] Embodiment 53: The method according to the above embodiment, wherein the Young's modulus
[0226] 80 GPa to 102 GPa at a penetration depth of 100 nm,
[0227] 60 GPa to 114 GPa at a penetration depth of 300 nm,
[0228] 61 GPa to 107 GPa at a penetration depth of 1000 nm, and
[0229] The hardness
[0230] 1.78 GPa to 4.12 GPa at a penetration depth of 100 nm
[0231] 2.10 GPa to 4.10 GPa at a penetration depth of 300 nm,
[0232] 2.67 GPa to 6.93 GPa at a penetration depth of 1000 nm.
[0233] Embodiment 54: The method according to the above embodiment, wherein the Young's modulus
[0234] 86 GPa to 96 GPa at a penetration depth of 100 nm,
[0235] 74 GPa to 100 GPa at a penetration depth of 300 nm,
[0236] 72 GPa to 96 GPa at a penetration depth of 1000 nm, and
[0237] The hardness
[0238] 2.37 GPa to 3.53 GPa at a penetration depth of 100 nm,
[0239] 2.60 GPa to 3.60 GPa at a penetration depth of 300 nm,
[0240] 3.73 GPa to 5.87 GPa at a penetration depth of 1000 nm.
[0241] Embodiment 55: The method according to any one of the preceding embodiments involving methods, wherein the method further comprises the following steps:
[0242] d) experimentally determining the reflectivity factor S11 of the stack by applying microwave reflectometry to the stack (125) at 75 GHz, wherein the reflectivity factor S11 is determined to be -6.70
[0243] dB to -1.30dB.
[0244] Embodiment 56: A method according to the aforementioned embodiment, wherein the reflectivity factor S11 is -5.80 dB to -2.20 dB.
[0245] Embodiment 57: A method according to the aforementioned embodiment, wherein the reflectivity factor S11 is -4.90 dB to -3.10 dB.
[0246] Embodiment 58: The method according to the preceding embodiment, wherein the photoconductive material is selected from the group consisting of chalcogenide compounds of lead, solid solutions and / or doped variants thereof, and wherein the cap is an amorphous cap comprising an aluminum-containing compound selected from oxides, hydroxides, or combinations thereof, the method further comprising the following steps:
[0247] e) performing stacked wavelength dispersive X-ray spectroscopy using an electron beam microanalyser and an accelerating voltage of 20 kV,
[0248] The method for manufacturing the optical sensor is further performed in the following manner: the optical sensor exhibits a wavelength dispersive X-ray spectrometry using the stack of the electron beam microanalyzer and an accelerating voltage of 20 kV at Al K α1 The net counts / s·nA measured at the peak maximum of the line are similar to those in Pb M α1 The ratio of net counts / s·nA measured at the peak maximum of the line ranged from 0.113 to 0.279.
[0249] Embodiment 59: The method according to the above embodiment, wherein in the Al K α1 The net counts / s·nA measured at the peak maximum of the line are similar to the Pb M α1 The ratio of net counts / s·nA measured at the peak maximum of the line ranged from 0.141 to 0.251.
[0250] Embodiment 60: The method according to the above embodiment, wherein in the Al K α1 The net counts / s·nA measured at the peak maximum of the line are similar to the Pb M α1 The ratio of net counts / s·nA measured at the peak maximum of the line ranged from 0.168 to 0.224.
[0251] Embodiment 61: The method according to any one of the three preceding embodiments, wherein the photoconductive material is selected from the group consisting of lead sulfide (PbS), solid solutions and / or doped variants thereof, wherein the method for manufacturing the optical sensor is further performed in the following manner: Further according to step e), the optical sensor exhibits a wavelength dispersive X-ray spectroscopy using the stack of the electron beam microanalyzer and an accelerating voltage of 20 kV in the Al K α1 The net counts / s·nA measured at the peak maximum of the line are similar to the Pb M α1 Line neutralization in SK α1Another ratio of the sum of the net counts / s·nA measured in the lines ranged from 0.0841 to 0.1456.
[0252] Embodiment 62: The method according to the preceding embodiment, wherein in the Al K α1 The net counts / s·nA measured at the peak maximum of the line are similar to the Pb M α1 Line neutralization and in the SK α1 Another ratio of the sum of the net counts / s·nA measured in the lines ranged from 0.0944 to 0.1354.
[0253] Embodiment 63: The method according to the above embodiment, wherein in the Al K α1 The net counts / s·nA measured at the peak maximum of the line are similar to the Pb M α1 Line neutralization and in the SK α1 Another ratio of the sum of the net counts / s·nA measured in the line was 0.1046 to 0.1251.
[0254] Embodiment 64: The method according to any of the preceding embodiments relating to methods, wherein step b) is repeated at least once.
[0255] Embodiment 65: A method according to any one of the preceding embodiments relating to a method, wherein the cap is deposited until it has a completed thickness of 10nm to 600nm, preferably 20nm to 200nm, more preferably 40nm to 120nm, most preferably 50nm to 95nm.
[0256] Embodiment 66: A method according to any one of the preceding embodiments relating to the method, wherein the cover is deposited on the top and sides of the layer of photoconductive material and preferably at least the sides of the substrate in such a manner that it is a conformal cover with respect to the adjacent surfaces of the photoconductive material and the substrate.
[0257] Embodiment 67: A method according to the preceding embodiments, wherein the thickness of the conformal cover follows the corresponding surface of the coating within a deviation of ±50 nm, preferably ±20 nm, most preferably ±10 nm over at least 90%, preferably at least 95%, and most preferably at least 99% of the surface of the cover.
[0258] Embodiment 68: A method according to any one of the preceding embodiments involving a method, wherein at least one deposition method is used to deposit the metal-containing compound, wherein the at least one deposition method is preferably selected from an atomic layer deposition process, a chemical vapor deposition process, a sputtering process, or a combination thereof, preferably the atomic layer deposition process and a combination of the atomic layer deposition process and the sputtering process.
[0259] Embodiment 69: A method according to any one of the preceding embodiments relating to methods, wherein step b) is performed in a vacuum chamber.
[0260] Embodiment 70: The method according to the preceding embodiment, wherein the electrical contacts are provided before step b), wherein the cover is also partially deposited on the electrical contacts.
[0261] Embodiment 71: The method according to the preceding embodiment, wherein the electrical contact is bonded to at least one external connection by using an electrically conductive lead, preferably in the form of a wire, in particular an Au, Al, or Cu wire.
[0262] Embodiment 72: The method of the preceding embodiment, wherein the conductive lead is bonded to the electrical contact through the cover.
[0263] Embodiment 73: The use of the detector according to any one of the preceding embodiments relating to the detector, for the purpose of use, is selected from the group including: gas sensing, fire detection, flame detection, temperature detection, smoke detection, combustion monitoring, spectroscopy, temperature sensing, motion sensing, industrial monitoring, chemical sensing, exhaust gas monitoring, safety applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0264] Further optional details and features of the present invention are apparent from the following description of preferred exemplary embodiments in conjunction with the dependent claims. In this context, specific features can be implemented individually or in combination. The present invention is not limited to exemplary embodiments. Exemplary embodiments are schematically shown in the accompanying drawings. The same reference numerals in the various drawings refer to the same elements or elements with the same function, or elements corresponding to each other with respect to their functions.
[0265] In particular, in the accompanying drawings:
[0266] Figure 1A and 1B shows a preferred exemplary embodiment of an optical sensor according to the present invention;
[0267] Figure 2 shows a preferred exemplary embodiment of an optical detector according to the invention; and
[0268] FIG. 3A to FIG. 3F An exemplary embodiment of a method for manufacturing an optical sensor according to the invention is shown. DETAILED DESCRIPTION
[0269] Figure 1A and Figure 1BExemplary embodiments of an optical sensor 110 according to the invention are each shown in a side view in a highly schematic manner. Thus, the optical sensor 110 comprises at least one layer 112 of a photoconductive material 114. In particular, the layer 112 of the photoconductive material 114 may exhibit a thickness of 10 nm to 100 μm, preferably 100 nm to 10 μm, more preferably 300 nm to 5 μm. In a preferred embodiment, the layer 112 of the photoconductive material 114 may comprise a substantially flat surface, wherein, however, other embodiments that may exhibit variations of the surface of the layer 112, such as gradients or steps, may also be feasible. In this context, the layer 112 of the photoconductive material 114 may preferably be manufactured as described below with respect to FIG. 3 . However, other manufacturing methods may also be feasible.
[0270] In the exemplary embodiment of FIG. 1 , the photoconductive material 114 may be or include at least one chalcogenide compound, which may preferably be selected from the group consisting of sulfide chalcogenides, selenide chalcogenides, telluride chalcogenides, and ternary chalcogenides. In a particularly preferred embodiment as described herein, the photoconductive material 114 is or includes a sulfide, preferably lead sulfide (PbS), a solid solution thereof and / or a doped variant thereof. Since the preferred photoconductive material 114 is generally known to exhibit different absorption characteristics in the infrared spectral range, the optical sensor 110 may preferably be used as an infrared sensor. However, other embodiments and / or other photoconductive materials, in particular, photoconductive materials as described elsewhere in this document for this purpose, may also be feasible.
[0271] Further, the optical sensor 110 according to the present invention comprises a cover 116, wherein the cover 116 preferably completely covers an accessible surface 118 of the photoconductive material 114. As already described above, the cover 116 may therefore be adapted to provide an encapsulation for the photoconductive material 114, in particular as a gas-tight encapsulation, in order to avoid degradation of the optical sensor 110 or its partitions, in particular the photoconductive material 114, by external influences, such as humidity and / or oxygen. As mentioned above, the cover 116 is an amorphous cover, which comprises at least one metal-containing compound 120. In a particularly preferred embodiment as described herein, the metal-containing compound 120 may comprise at least one oxide Al or at least one hydroxide of Al, which may also be represented by the formula AlO x (OH) y, wherein 0≤x≤1.5 and 0≤y≤1.5, wherein x+y=1.5. In this particular embodiment, the cover 116 may exhibit a thickness of 10 nm to 600 nm, preferably 20 nm to 200 nm, more preferably 40 nm to 120 nm, and most preferably 50 nm to 95 nm. This thickness range may particularly reflect the amount of metal-containing compound 120 within the cover 116, which may be advantageous for achieving the above-mentioned function of providing encapsulation for the photoconductive material 114.
[0272] Further, in this particular embodiment, the cover 116 may be a conformal cover with respect to the adjacent surface 118 of the photoconductive material 114. As defined above, the thickness of the conformal cover may therefore follow the corresponding surface 118 of the photoconductive material 114 within a ±50 nm, preferably ±20 nm, most preferably ±10 nm deviation, wherein the deviation may occur at least for at least 90%, preferably for at least 95%, most preferably for at least 99% of the surface 122 of the cover 116, thereby not taking into account any contamination or imperfection that may be present on the surface 122 of the cover 116.
[0273] like Figure 1A and Figure 1B As further shown in each, at least one layer of the photoconductive material 114 is preferably directly applied to at least one substrate 124, wherein the substrate 124 may preferably be or include an insulating substrate. In this context, the thickness of the substrate 124 may have a range of 10 μm to 2000 μm, preferably 50 μm to 1000 μm, more preferably 100 μm to 500 μm. As described in more detail below, the substrate 124 may preferably include an optically transparent material 132, in particular glass or quartz. However, other substrate materials that may be partially or fully optically transparent in the infrared spectral range may also be feasible.
[0274] According to the present invention, a substrate 124, a layer 112 of photoconductive material 114, such as deposited on the substrate 124, and a cover 116 coating at least the layer 112 of photoconductive material 114 form a stack 125. Figure 1A and Figure 1B As schematically shown, a normal vector 126 extending perpendicular to the surface of the substrate 124 can be used as a specific direction according to which the stack 125 can be arranged. Therefore, the substrate 124 can be considered as a base layer, and the layer 112 of the photoconductive material 114 can be located on top of it, and thus the cover 116 can be further located on top of the layer 112 of the photoconductive material 114 within the stack 125.
[0275] In order to allow incident light beam 127 to reach photoconductive material 114 in order to optically modify the conductivity within layer 112 of photoconductive material 114, at least one of cover 116 and substrate 124 may be optically transparent in particular in a desired wavelength range, such as in the infrared spectral range or a subregion thereof. Figure 1A Schematically depicted, a beam path 128 of an incident light beam 127 can be configured to pass through the cover 116 so as to produce a light spot having a diameter 130 within the layer 112 of the photoconductive material 114. Therefore, it can be particularly advantageous to select the metal-containing compound 120 for the cover 116 to be preferably optically transparent in the desired wavelength range, in particular, by exhibiting suitable absorption characteristics. In addition, it can be preferred that one or both of the metal-containing compound 120 for the cover 116 and the material for the substrate 124 can exhibit optical transparency characteristics in the desired wavelength range, such as for allowing sensing of the light beam 127 from two directions of the optical sensor 110.
[0276] The cover 116 may cover the accessible surface 118 of the photoconductive material 114 according to WO 2018 / 019921 A1, but according to European patent application 19 152 511.2 filed on January 18, 2019, additionally covers the accessible surface 134 of the substrate 124. Preferably, the cover 116 may be applied in such a way that it may completely contact all accessible surfaces 118, 134 of the photoconductive material 114 and the substrate 124, respectively, so as to significantly improve the long-term stability of the optical sensor 110. In particular, the cover 116 may be applied in such a way that it may directly contact the top and the sides of the layer 112 of the photoconductive material 114 and at least the sides of the substrate 124. However, other kinds of packaging for providing the photoconductive material 114, in particular as a gas-tight encapsulation, may also be feasible. Thus, the cover 116 may thus prevent direct contact between the layer 112 of the photoconductive material 114 or the substrate 124 with the surrounding atmosphere, thereby avoiding degradation of the photoconductive material 114 by external influences, such as humidity and / or oxygen.
[0277] like Figure 1A and Figure 1BAs further shown, the optical sensor 110 according to the present invention comprises at least two separate electrical contacts 136, 136', namely at least one first electrical contact 136 and at least one second electrical contact 136', wherein the electrical contacts 136, 136' are adapted to contact the layer 112 of the photoconductive material 114, however, in a separate position outside the stack 125. For this purpose, the electrical contacts 136, 136' may be configured and arranged in a certain way so as to be able to conduct an electric current through the layer 112 of the photoconductive material 114 via the first electrical contact 136 to the second electrical contact 136', or vice versa, or to apply a voltage across the layer 112 of the photoconductive material 114 by using the first electrical contact 136 and the second electrical contact 136'. For both purposes, the first electrical contact 136 may be electrically isolated from the second electrical contact 136', while the first electrical contact 136 and the second electrical contact 136' are directly connected to the layer 112 of the photoconductive material 114. As further shown herein, the cover 116 can at least partially coat the electrical contacts 136, 136', which can be particularly configured to be bondable, such as to a connector that may lead to a circuit such as a Figure 1B One or more leads 138, 138' of external circuitry are depicted.
[0278] The direct connection between any of the electrical contacts 136, 136' and the layer 112 of photoconductive material 114 can be provided by any known process capable of providing electrical contact, such as electroplating, welding, soldering, wire bonding, thermosonic bonding, stitch bonding, ball bonding, wedge bonding, compatibility bonding, thermocompression bonding, anodic bonding, direct bonding, plasma activated bonding, eutectic bonding, glass paste bonding, adhesive bonding, transient liquid phase diffusion bonding, surface activated bonding, tape automated bonding, or depositing a highly conductive substance at the contact strip. In order to allow sufficient conductivity through the electrical contacts 136, 136' while providing sufficient mechanical stability of the electrical contacts 136, 136', the electrical contacts 136, 136' may preferably include at least one electrode material selected from the group consisting of metals Ag, Cu, Pt, Al, Mo or Au, alloys comprising at least one of the mentioned metals, and graphene. However, other types of electrode materials may also be feasible.
[0279] like Figure 1B Schematically depicted, the substrate 124 can be attached to a circuit carrier device 142, in particular to a printed circuit board (PCB) 144, preferably via a thin film 140 of glue. For this purpose, wires, such as gold wires, beryllium-doped gold wires, aluminum wires, platinum wires, palladium wires, silver wires, or copper wires, can be used as leads 138, 138' for bonding electrical contacts 136, 136', such as contact pads (not depicted here) on the circuit carrier device 142. In the example Figure 1BIn the particularly preferred embodiment shown, the electrical contacts 136, 136' may be engageable through the cover 116. This feature may in particular allow improving the encapsulation function of the cover 116 and, therefore, provide stability to the electrical contacts 136, 136'.
[0280] Further in accordance with the present invention, the stack 125, as comprised by the optical sensor 110, exhibits a particularly selected static mechanical property 145. In this context, the static mechanical property 145, which refers to the response of the stack 125 to an incident static force applied to the stack 125, can be achieved by performing a quasi-static nanoindenter measurement on the body, as described below with respect to Figure 3C As indicated there, the Young's modulus and the hardness of the stack 125 at particularly selected penetration depths of, in particular, 100 nm, 300 nm and 1000 nm can be considered as reliable measures for determining the static mechanical properties 145 of the stack 125 comprised by the optical sensor 110. As already indicated above, surprisingly, it has been found that the optical sensor 110 exhibits preferred static mechanical properties 145 in the case where the stack 125 comprises the following properties: In quasi-static nanoindenter measurements of the stack 125, the Young's modulus and the hardness of the stack 125 can be considered as reliable measures for determining the static mechanical properties 145 of the stack 125 comprised by the optical sensor 110. As already indicated above, surprisingly, it has been found that the optical sensor 110 exhibits preferred static mechanical properties 145 in the case where the stack 125 comprises the following properties:
[0281] - 75 GPa to 107 GPa, preferably 80 GPa to 102 GPa, more preferably 86 GPa to 96 GPa at a penetration depth of 100 nm;
[0282] - 47 to 127 GPa at a penetration depth of 300 nm, preferably 60 GPa to 114
[0283] GPa, more preferably 74 GPa to 100 GPa; and
[0284] - 49 to 119 GPa at a penetration depth of 1000 nm, preferably 61 GPa to 107
[0285] GPa, more preferably 72 GPa to 96 GPa;
[0286] The hardness
[0287] - 1.20 GPa to 4.70 GPa, preferably 1.78 GPa to 4.12 GPa, more preferably 2.37 to 3.53 GPa at a penetration depth of 100 nm;
[0288] - 1.60 GPa to 4.60 GPa, preferably 2.10 GPa to 4.10 GPa, more preferably 2.60 GPa to 3.60 GPa at a penetration depth of 300 nm; and
[0289] 1.60 GPa to 8.00 GPa at a penetration depth of 1000 nm, preferably 2.67
[0290] GPa to 6.93 GPa, more preferably 3.73 GPa to 5.87 GPa.
[0291] Further, the stack 125 as comprised by the optical sensor 110 may preferably exhibit a particularly selected dielectric property 146. In this document, the dielectric property 146 referring to the response of the stack 125 to an incident electromagnetic wave applied to the stack 125 may be referred to as follows: Figure 3D The microwave reflectometry experiment described in more detail is achieved. Therefore, the S11 reflectivity factor can be considered as a reliable measure for determining the dielectric properties 146 of the stack 125 as comprised by the optical sensor 110. As already indicated above, surprisingly, it has been found that the optical sensor 110 exhibits preferred dielectric properties 146 in the case where the stack 125 comprises the following properties: In a microwave reflectometry experiment at 75 GHz applied to the stack 125, the reflectivity factor S11 can have -6.70 dB to -1.30 dB, preferably -5.80 dB to -2.20 dB, more preferably -4.90 dB to -3.10 dB.
[0292] Further, the stack as comprised by the optical sensor 110 may preferably exhibit a particularly selected composition 148. As further described below in more detail with respect to FIG. 3 , wavelength dispersive X-ray spectroscopy (WDXS) of the stack 125 may preferably be used to determine the characteristics of the composition 148 of the stack 125. In this context, the photoconductive material 114 used in the optical sensor 110 may preferably be a lead chalcogenide compound, a solid solution and / or a doped variant thereof, wherein the lead chalcogenide compound may in particular be lead sulfide (PbS), wherein, at the same time, the cap 116 may be an amorphous cap comprising an aluminum-containing compound selected from oxides, hydroxides, or combinations thereof, also denoted as “Al2O3”. Here, the Al, K, and PbS may be present in the form of an amorphous cap, respectively. α1 Line, Pb M α1 Line and SK α1 The net counts of the WDXS measurements of stack 125 are determined from the peak maximum of the line as described below with respect to Figure 3E As already indicated above, surprisingly, it has been found that the optical sensor 110 exhibits preferred properties in the case where the stack comprises a composition 148 confirmed by WDXS measurements of the stack 125 using an electron beam microanalyser and an accelerating voltage of 20 kV, in the case of Al K α1 The net counts / s·nA measured at the peak maximum of the line are similar to those in Pb M α1The ratio of net counts / s·nA measured at the peak maximum of the line may be from 0.113 to 0.279, preferably from 0.141 to 0.251, more preferably from 0.168 to 0.224, while in the specific case of PbS used as the specific lead chalcogenide compound, at Al K α1 The net counts / s·nA measured at the peak maximum of the line are similar to those in Pb M α1 Line neutralization in SK α1 Another ratio of the sum of the net counts / s·nA measured in the line may be from 0.0841 to 0.1456, preferably from 0.0944 to 0.1354, more preferably from 0.1046 to 0.1251.
[0293] Figure 2 An exemplary embodiment of an optical detector 150 according to the invention is shown in a highly schematic manner, which may preferably be adapted for use as an infrared detector. However, other embodiments are possible. The optical detector 150 comprises at least one of the optical sensors 100 as described in more detail above, which may be arranged along an optical axis of the detector 150. In particular, the optical axis may be a symmetry and / or rotation axis of the arrangement of the optical sensor 100. The optical sensor 100 may be located within a housing of the detector 150. Further, at least one of the conveying devices may comprise a preferably refractive lens. An opening in the housing, which may in particular be positioned concentrically with respect to the optical axis, may preferably define a viewing direction of the detector 150.
[0294] Further, the optical sensor 100 is designed to generate at least one sensor signal in a manner that depends on the illumination of the sensor area 152 by the light beam 127. In this context, the detector 150 may have a straight beam path or an inclined beam path, an angular beam path, a branched beam path, a deflected or split beam path, or other types of beam paths. Further, the light beam 127 may propagate once or repeatedly, unidirectionally or bidirectionally along each beam path or a portion of the beam path.
[0295] According to the FiP effect, the optical sensor 100 can provide a sensor signal which, given the same total power of the illumination, depends on the beam profile 130 of the light beam 127 in the sensor area. However, other kinds of signals may also be feasible. As indicated above, the sensor area 152 comprises at least one of the layers 112 of a photoconductive material 114, preferably a chalcogen compound of lead, its solid solution, and / or a doped variant, wherein the chalcogen compound of lead may in particular be lead sulfide (PbS). However, other photoconductive materials 114, in particular other chalcogen compounds, may be used. As a result of the use of the photoconductive material 114 in the sensor area 152, given the total power of the illumination, the conductivity of the sensor area 152 depends on the beam profile of the light beam 127 in the sensor area 152. Therefore, the sensor signal generated as provided by the optical sensor 110 when incident by the light beam 127 may depend on the conductivity of the photoconductive material 114 in the sensor area 152 and, therefore, allow the beam profile 130 of the light beam 127 in the sensor area 152 to be determined.
[0296] Via further electrical leads 154, 154' (to which leads 138, 138' are coupled), the sensor wire signal can be sent to an evaluation device 156, which is generally designed to generate at least one information item by evaluating the sensor signal of the optical sensor 110. For this purpose, the evaluation device 156 can include one or more electronic devices and / or one or more software components in order to evaluate the sensor signal. Generally, the evaluation device 156 can be part of a data processing device 158 and / or can include one or more data processing devices 158. The evaluation device 156 can be fully or partially integrated into the housing and / or can be fully or partially implemented as a separate device, which is electrically connected to the optical sensor 100 in a wireless or wired manner. The evaluation device 156 can also include one or more additional components, such as one or more electronic hardware components and / or one or more software components, such as one or more measuring units and / or one or more evaluation units and / or one or more control units (not depicted here).
[0297] FIG. 3A to FIG. 3F An exemplary embodiment of a method for manufacturing an optical sensor 110 according to the invention is shown in a highly schematic manner.
[0298] like Figure 3AAs shown, substrate 124 is provided as a base layer on which further layers are continuously deposited. In this article, the normal vector 126 perpendicular to the extension of the surface of substrate 124 can be used as a specific direction according to which the stack 125 can be arranged. Preferably, before providing the layer 112 of photoconductive material 114, electrical contacts 136, 136' can be produced, such as in the form of an evaporated metal layer that can be provided on substrate 124 by known evaporation techniques, preferably including glass as optically transparent material 132. In particular, the evaporated metal layer may include one or more of the following: Ag, Al, Pt, Mg, Cr, Ti, or Au. Alternatively, electrical contacts 136, 136' may include a graphene layer. However, as mentioned in more detail above, other methods of producing electrical contacts 136, 136' may also be feasible.
[0299] like Figure 3A As further shown, subsequently, a layer 112 of a photoconductive material 114 is provided. For this purpose, the photoconductive material 114 can be synthesized according to the following process. Thus, 0.015 mol / L thiourea or a substitute thereof, 0.015 mol / L lead acetate, lead nitrate, or a substitute thereof, and 0.15 mol / L sodium hydroxide or a substitute thereof are dissolved in a reaction volume, wherein a transparent solution is obtained at room temperature. As is known in the prior art, when the above-mentioned solutions are mixed in any order, lead sulfide (PbS) precipitates from the solution at a temperature above 30°C, generally in such a way that a uniform and relatively smooth layer can be formed at the side walls and the bottom of the reactor containing the liquid or on the walls of any object located therein.
[0300] However, when, immediately before the actual precipitation of PbS from the mixed precipitation solution, a solution of an agent capable of releasing relatively large amounts of nascent oxygen, preferably potassium persulfate, hydrogen peroxide, or sodium perborate, is added thereto, PbS is precipitated therefrom in the usual manner but in an activated form capable of direct use in cells or of additional sensitization by aging or low-temperature drying. The precipitation solution and the activator are preferably mixed and stirred at a temperature above 35° C. for one to three hours, during which time deposition occurs. In this context, the amount of persulfate ions, perborate ions, or nascent oxygen from hydrogen peroxide, expressed in moles, added to the liquid solution for precipitation of PbS may preferably be 0.01 to 0.5 of the theoretical amount of PbS in the bath, expressed in moles, wherein the theoretical amount of PbS is the amount that would be formed if there were a total conversion of lead and sulfur precipitation compounds to lead sulfide.
[0301] After the formation of the PbS layer, an aging step in a climate chamber, preferably at a temperature of about 50° C. and a humidity above 70%, can optionally be performed, which appears to be beneficial for the photoconductive properties. Improved photoconductivity can be obtained when the deposited and aged film is further treated by annealing, i.e., by heating in vacuum or air at a temperature of about 100° C. to 150° C. for 1 to 100 hours.
[0302] However, other types of providing the layer 112 of photoconductive material 114 may also be feasible.
[0303] Figure 3B Schematically shown is the deposition of a metal-containing compound 120 as an amorphous cap 116 on a layer 112 of a photoconductive material PbS 114 and an accessible surface 118, 134 of a substrate 124 in order in particular to serve as an encapsulation layer. For this purpose, at least one precursor suitable for reacting the metal-containing compound 120 can be applied. In this preferred embodiment, an atomic layer deposition (ALD) process or a combination of ALD and sputtering has been used as a deposition method. Alternatively, however, other deposition processes, such as a chemical vapor deposition (CVD) process, can also be applied.
[0304] In a preferred embodiment of the invention, the cover 116 comprises Al2O3 that has been produced via an ALD process or a combination of an ALD process and a sputtering process. Alternatively, a laminate like Al2O3 / TiO2 / Al2O3 / … or Al2O3 / ZrO2 / Al2O3 / … can also be produced. In this particular embodiment, the ALD process has been performed applying the following process parameters:
[0305] -First precursor: H20;
[0306] - Second precursor: Al(CH3)3 (trimethylaluminum, TMA);
[0307] - Temperature about 60°C;
[0308] - About 700 cycles.
[0309] like Figure 3B As further depicted, a cap 116 comprising Al2O3 may be applied in accordance with the present invention in such a manner that it may simultaneously coat an accessible surface 118 of the photoconductive PbS layer 112, electrical contacts 136, 136' contacting the photoconductive PbS layer 112, and an accessible surface 134 of the substrate 124.
[0310] like Figure 3B As further shown, the stack 125 is now obtained by providing a substrate 124, depositing a layer 112 of a photoconductive material 114 onto the substrate 124 and subsequently depositing a cover 116 onto the layer 112 of the photoconductive material 114. Figure 3BAs schematically shown, a normal vector 126 extending perpendicularly to the surface of the substrate 124 is used herein as a specific direction for the arrangement of the stack 125 .
[0311] According to the present invention, the stack 125 exhibits a specifically selected static mechanical property 145 related to the response of the stack 125 to an incident static force applied to the stack 125. In this document, the specifically selected static mechanical property 145 of the stack 125 is determined by measuring the Young's modulus and hardness of the stack 125 in a quasi-static nanoindenter measurement. Figure 3C Schematically depicted, the quasi-static nanoindenter measurement comprises the measurement of the Young's modulus and the hardness of the body, preferably performed according to standards EN ISO 14577-1:2015 and EN ISO 14577-4:2016. For this purpose, a nanoindenter 160 is used, wherein the nanoindenter comprises a probe 162 with a tip 164, which is designed to penetrate into a very small volume 166 of the stack 125 in order to perform the quasi-static nanoindenter measurement. For this purpose, the tip 164 of the nanoindenter 160 may preferably comprise a cone geometry, wherein a Berkovich tip 168 according to standard EN ISO 14577-2:2015 may be particularly preferred. Thus, the Young's modulus and the hardness of the stack 125 are measured by using the nanoindenter 160, thereby measuring the preferred static and dynamic mechanical properties 145, 146 of the stack 125 as presented in more detail above. However, in cases where the Young's modulus and hardness of the stack 125 measured by the nanoindenter 160 may deviate from the preferred static mechanical properties 145 as indicated above, that particular sample of the optical sensor 110 may be rejected for further use in the optical detector 150 .
[0312] Quasi-static nanoindenter measurements of Young's modulus and hardness at penetration depths of 100 nm, 300 nm and 1000 nm, respectively, were performed using the Bosch tips on 30 individual optical sensors that had been selected according to the selection criteria as indicated in more detail above. Thus, the selection criteria were defined as optical sensors 110 having a relative dark resistance change of less than 0.1% and a relative detectivity change of less than 0.1% and exhibiting an absolute maximum deviation of the linear resistivity between -10V and +10V of less than 0.1% of the dark resistance. As obtained from these quasi-static nanoindenter measurement results, the following values categorized by size as presented in Table 1:
[0313]
[0314]
[0315] Based on these results, the following parameters can be determined as presented in Table 2, where the respective values after the symbol "±" indicate ±1.5σ, where σ refers to the corresponding standard deviation:
[0316]
[0317] Further in accordance with the present invention, stack 125 may exhibit a specifically selected dielectric property 146 related to the response of stack 125 to an incident electromagnetic wave applied to stack 125. In this context, specifically selected dielectric property 146 of stack 125 may be determined in a microwave reflectometry experiment. Figure 3D Schematically depicted, dielectric properties 146 of stack 125 are determined by measuring the S11 reflectivity factor using microwave device 170 in a microwave reflectometry experiment. Herein, microwave device 170 may include microwave transmitter 172, which may generate and transmit incident microwaves 174 at a frequency of 75 GHz. Incident microwaves 174 may be incident on stack 125, wherein stack 125 may then reflect a portion of incident microwaves 174 as reflected microwaves 176 that may be detected by microwave receiver 178. Microwave evaluation unit 180 may be used to determine the S11 reflectivity factor defined in dB. 10 log(P refl / P in ) of the S11 reflectivity factor, where P in is the power of the incident microwave 174 incident on the stack 125 as provided by the microwave launcher 172, and wherein P refl is the reflected microwave 176 reflected by the stack 125 as measured by the microwave receiver 178. Therefore, by measuring the S11 reflectivity factor, the dielectric properties 146 of the stack 125 can be reliably determined. However, in cases where the S11 reflectivity factor of the stack 125 measured by the microwave device 170 may deviate from the preferred dielectric properties 146 of the stack 125 as indicated above, the specific sample of optical sensors 110 may be rejected for further use in the optical detector 150. The following values, sorted by size as presented in Table 3, were obtained from microwave reflectometry experiments on 30 individual optical sensors that have been selected according to the selection criteria as indicated above:
[0318]
[0319] Based on these results, the measured value of the S11 reflectivity factor may be determined to be -4.00 dB ± 2.70 dB, where the corresponding value after the symbol "±" indicates 1.5σ, where σ refers to the corresponding standard deviation.
[0320] In a particularly preferred embodiment, the photoconductive material 114 may in particular be a lead chalcogenide, in particular PbS, a solid solution and / or a doped variant thereof, wherein, at the same time, the cover 116 may be an amorphous cover comprising Al2O3. In this context, wavelength dispersive X-ray spectroscopy (WDXS) may allow the composition 148 of the stack 125 comprising the cover 116 comprising Al2O3, which is applied onto the PbS layer 112 deposited on the glass substrate 124, to be determined. Figure 3E As shown, WDXS measurements may preferably be performed by using an electron beam microanalyzer 182. The electron beam microanalyzer 182 may include an electron source 184 for generating an incident electron beam 186, wherein the incident electron beam 186 is incident on the stack 125. As a result thereof, the stack 125 emits an X-ray beam 188, which may then be collimated in a collimator 190 so as to thereafter irradiate a known single crystal 192 at a precise angle, wherein the single crystal 192 diffracts the X-ray beam 188 into a diffracted X-ray beam 194 for collection by a detector 196.
[0321] In this context, the single crystal 192, the stack 125 and the detector 196 can be precisely mounted on a goniometer (not depicted here), wherein the distance between the stack 125 and the single crystal 192 can be equal to the distance between the single crystal 192 and the detector 196. Preferably, an accelerating voltage of 20 kV can be used for the incident electron beam 186. Further, an automatic changing unit (not depicted here) for changing the single crystal 192, in particular depending on the energy of the incident electron beam 186, can be used, thereby allowing the analysis of different compositions within the composition 148 of the stack 125.
[0322] By using the WDXS evaluation unit 200, it is possible to α1 Line, Pb M α1 Line and SK α1 The net counts of the WDXS measurement are determined from the peak maximum of the line, thereby confirming the composition 148 of the stack 125. However, in the case where the peak maximum of the indicator line measured by the electron beam microanalyzer deviates from the preferred value as indicated above, the particular sample of the optical sensor 110 can be rejected for further use in the optical detector 150.
[0323] In order to characterize the composition of the Al2O3 / PbS layer 148, WDXS measurements were performed using a commercial electron beam microanalyzer, wherein the material used for the single crystal 192 was selected from the materials used for measuring Al K α1 The thallium phthalate (TAP) and Pb M α1 Line and SK α1For WDXS measurements, an accelerating voltage of 20 kV, a beam current of 150 nA, a measurement time of 100 s at the peak maximum, a measurement time of 20 s in the background on each side of the peak, and a measurement spot diameter of 300 μm were used. α1 Line, Pb M α1 Line and SK α1 All net counts for the WDXS measurement are determined from the peak maximum of the line. In a specific electron beam microanalyzer 182 used for WDXS measurements, for Al measurements, the Al K α1 The net count of the wire is measured at 90.918 mm. For Pb measurement, Pb M α1 The net count of the wire is measured at 169.291mm, for S measurement, SK α1 The net count of was measured at 172.124 mm. The following values, sorted by size as presented in Table 4, were obtained from WDXS experiments on 30 individual optical sensors that had been selected according to the selection criteria as indicated above:
[0324]
[0325]
[0326] The total count ratio of Al / Pb was determined to be 0.196±0.83, and the net count ratio of Al / (Pb+S) was determined to be 0.1142±0.3075, wherein, in both cases, the corresponding values after the symbol “±” indicate 1.5σ, wherein σ refers to the corresponding standard deviation.
[0327] like Figure 3F As shown, the two electrical contacts 136, 136' of the layer 112 electrically contacting the photoconductive material 114 may preferably eventually be bonded to an external connection by means of conductive leads 138, 138' (such as gold wires), which are provided here by the cover 116. However, as mentioned above, other ways of providing the photoconductive PBS layer 112 with the electrical contacts 136, 136' may also be feasible, such as by providing the leads 138, 138' already before depositing the amorphous cover 116, i.e., in the case of Figure 3A and Figure 3B After production, the stack 125 as a whole can be rotated in any direction, which may however have no effect on the arrangement and composition 148 of the stack 125 .
[0328] Reference numerals list
[0329] 110 Sensors
[0330] 112 Layer of photoconductive material
[0331] 114 Photoconductive materials
[0332] 116 Cover
[0333] 118 Accessible surface of layer of photoconductive material
[0334] 120 Metal compounds
[0335] 122 Cover surface
[0336] 124 Substrate
[0337] 125 Stack
[0338] 126 Normal vector
[0339] 127 Beam
[0340] 128 beam paths
[0341] 130 beam diameter; beam profile
[0342] 132 Optically transparent materials
[0343] 134 Accessible surface of substrate
[0344] 136, 136' Electrical contact
[0345] 138, 138' Electrical connection lead
[0346] 140 Glue film
[0347] 142 Circuit carrier device
[0348] 144 Printed Circuit Board
[0349] 145 Static Mechanical Properties
[0350] 146 Dynamic Mechanical Properties
[0351] 148 Composition
[0352] 150 Optical detector
[0353] 152 sensor area
[0354] 154, 154' Further electrical leads
[0355] 156 Evaluation Device
[0356] 158 Processing Device
[0357] 160 Nanoindenter
[0358] 162 Probe
[0359] 164 Tip
[0360] 166 Volume
[0361] 168 Bosch Tip
[0362] 170 Microwave Device
[0363] 172 Microwave Transmitter
[0364] 174 Incident microwave
[0365] 176 Reflected Microwaves
[0366] 178 Microwave Receiver
[0367] 180 Microwave Evaluation Unit
[0368] 182 Electron Beam Microanalyzer
[0369] 184 Electron Source
[0370] 186 Incident electron beam
[0371] 188 Emitting X-ray Beams
[0372] 190 Collimator
[0373] 192 Single Crystal
[0374] 194 Diffracted X-ray Beam
[0375] 196 X-ray detector
[0376] 198 Spot diameter
[0377] 200 WDXS evaluation unit
Claims
1. A method of selecting an optical sensor (110) having an overall long-term quality, the method comprising the steps of: Providing an optical sensor (110) comprising a stack (125), wherein the stack (125) has: - a substrate (124), - at least one layer (112) of photoconductive material (114) applied to said substrate (124), and - a cover (116) covering the accessible surface of the photoconductive material (114), and at least two separate electrical contacts (136, 136') spaced apart from the stack (125) and contacting the layer (112) of photoconductive material (114); measuring the Young's modulus and hardness of the stack (125) in a quasi-static nanoindenter measurement; and Selecting an optical sensor (110) that exhibits such preferred static mechanical properties (145) in quasi-static nanoindenter measurements of the stack (125), Young's modulus 75 GPa to 107 GPa at a penetration depth of 100 nm, 47 GPa to 127 GPa at a penetration depth of 300 nm, 49 GPa to 119 GPa at a penetration depth of 1000 nm, and hardness 1.20 GPa to 4.70 GPa at a penetration depth of 100 nm, and 1.60 GPa to 4.60 GPa at a penetration depth of 300 nm, 1.60 GPa to 8.00 GPa at a penetration depth of 1000 nm, wherein the penetration depth is determined with respect to a surface of the stack (125), or In the event that the Young's modulus and the hardness of the stack (125) deviate from the preferred static mechanical properties (145) of the stack (125), the optical sensor (110) is rejected.
2. The method according to the preceding claim, wherein: Preferred static mechanical properties (145) of the stack (125) include, in a quasi-static nanoindentation of the stack (125), the Young's modulus 80 GPa to 102 GPa at a penetration depth of 100 nm, 60 GPa to 114 GPa at a penetration depth of 300 nm, 61 GPa to 107 GPa at a penetration depth of 1000 nm, and The hardness 1.78 GPa to 4.12 GPa at a penetration depth of 100 nm, and 2.10 GPa to 4.10 GPa at a penetration depth of 300 nm, 2.67 GPa to 6.93 GPa at a penetration depth of 1000 nm.
3. A method according to any one of the preceding claims, wherein: The layer (112) of at least one photoconductive material (114) exhibits a thickness of 10 nm to 100 μm.
4. The method according to any one of the preceding claims 1 and 2, wherein: The cap (116) exhibits a thickness of 10 nm to 600 nm.
5. The method according to any one of the preceding claims 1 and 2, wherein: The substrate (124) exhibits a thickness of 10 μm to 2000 μm.
6. The method according to any one of the preceding claims 1 and 2, wherein: Preferred static mechanical properties (145) of the stack (125) include a reflectivity factor S11 of -6.70 dB to -1.30 dB in a microwave reflectometry test of the stack (125) at 75 GHz.
7. The method according to claim 6, wherein: Preferred static mechanical properties (145) of the stack (125) include a reflectivity factor S11 of -5.80 dB to -2.20 dB in a microwave reflectometry test at 75 GHz of the stack (125).
8. The method according to any one of the preceding claims 1, 2 and 7, wherein: The cap (116) includes an aluminum-containing compound selected from oxides, hydroxides, or combinations thereof.
9. The method according to any one of the preceding claims 1, 2 and 7, wherein: The photoconductive material (114) is selected from lead chalcogenide compounds, solid solutions and / or doped modifications thereof.
10. The method according to claim 1 or 2, wherein: Preferred static mechanical properties (145) of the stack (125) include wavelength dispersive X-ray spectroscopy of the stack (125) using an electron beam microanalyzer (182) and an accelerating voltage of 20 kV. α1 The net counts / s·nA measured at the peak maximum of the line are similar to those in Pb M α1 The ratio of net counts / s·nA measured at the peak maximum of the line ranged from 0.113 to 0.
279.
11. The method according to claim 10, wherein: Preferred static mechanical properties (145) of the stack (125) include wavelength dispersive X-ray spectroscopy of the stack (125) using the electron beam microanalyzer (182) and an accelerating voltage of 20 kV. α1 The net counts / s·nA measured at the peak maximum of the line are similar to the Pb M α1 The ratio of net counts / s·nA measured at the peak maximum of the line ranged from 0.141 to 0.
251.
12. The method according to any one of the preceding claims 1, 2, 7 and 11, wherein: The photoconductive material (114) is selected from lead sulfide (PbS), its solid solution and / or doped variants.
13. The method according to claim 10, wherein: Preferred static mechanical characterization (145) of the stack (125) includes wavelength dispersive X-ray spectroscopy of the stack (125) using an electron beam microanalyzer (182) and an accelerating voltage of 20 kV. α1 The net counts / s·nA measured at the peak maximum of the line are similar to the Pb M α1 Line neutralization in SK α1 Another ratio of the sum of the net counts / s·nA measured in the lines ranged from 0.0841 to 0.1456.
14. The method according to claim 13, wherein: Preferred static mechanical properties (145) of the stack (125) include wavelength dispersive X-ray spectroscopy of the stack (125) using the electron beam microanalyzer (182) and an accelerating voltage of 20 kV. α1 The net counts / s·nA measured at the peak maximum of the line are similar to the Pb M α1 Line neutralization and in the SK α1 Another ratio of the sum of the net counts / s·nA measured in the lines ranged from 0.0944 to 0.1354.