Electrode and secondary battery including the same
By using a single-walled carbon nanotube structure dispersed in hydrogenated nitrile rubber in the electrode active material layer, a network conductive path is formed, which solves the problem of poor dispersion of the conductive agent and improves the conductivity and life characteristics of the secondary battery.
Patent Information
- Application Number
- CN202080026696.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-28
- Filing Date
- 2020-03-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-03-27
AI Technical Summary
Existing secondary battery conductive agents such as carbon black and carbon nanotubes have poor dispersion in the electrode active material layer, leading to deterioration in conductivity and processability, and production difficulties of graphene and electrolyte mobility limit battery efficiency.
A carbon nanotube structure including 2 to 5,000 single-walled carbon nanotube units is used as the conductive agent. Through the improvement of the dispersion of hydrogenated nitrile rubber, the carbon nanotubes form a network structure, improve conductivity and enhance electrode adhesion.
Significantly improves battery conductivity and life characteristics, reduces electrode resistance, and improves electrode adhesion and energy density.
Smart Images

Figure CN113661586B_ABST
Abstract
Description
Technical Field
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of priority from Korean Patent Application No. 10-2019-0035776, filed on March 28, 2019, the disclosure of which is hereby incorporated by reference in its entirety. Technical Field
[0004] The present invention relates to an electrode and a secondary battery including the electrode, and more particularly, to an electrode and a secondary battery including an electrode active material layer, wherein: the electrode active material layer includes an electrode active material, hydrogenated nitrile rubber and a conductive agent; the conductive agent includes a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are incorporated; and the carbon nanotube structure is included in the electrode active material layer in an amount of 0.01 wt % to 0.5 wt %. Background Art
[0005] A typical example of an electrochemical device that uses electrochemical energy is a secondary battery, and the trend is that its use range is becoming increasingly wider. In recent years, with the technological development and increased demand for portable devices such as portable computers, mobile phones, and cameras, the demand for secondary batteries as energy sources has greatly increased. Among these secondary batteries, lithium secondary batteries with high energy density, that is, high capacity, have been extensively studied and commercialized and widely used.
[0006] Typically, a secondary battery consists of a positive electrode, a negative electrode, an electrolyte, and a separator. The positive and negative electrodes are typically composed of an electrode current collector and an electrode active material layer formed on the electrode current collector. The electrode active material layer is prepared by coating an electrode slurry composition comprising an electrode active material, a conductive agent, a binder, etc. onto the electrode current collector, drying it, and then winding it.
[0007] Meanwhile, conventionally, point-type conductive agents such as carbon black have been mainly used as conductive agents for secondary batteries, but such point-type conductive agents have limitations because they do not have a sufficient effect of improving conductivity. In order to overcome such limitations, research has been actively conducted on methods of applying linear conductive agents such as carbon nanotubes (CNTs) and carbon nanofibers (CNFs) and planar conductive agents such as graphene.
[0008] However, linear conductive agents such as carbon nanotubes or carbon nanofibers have excellent conductivity, but due to the inherent properties of the materials, which grow in bundles or tangles, their dispersion in the slurry is poor, resulting in poor coating performance and processability. Furthermore, the linear conductive agents are not evenly distributed in the electrode active material layer, resulting in limitations. To overcome these limitations, attempts have been made to improve dispersibility by introducing functional groups into the linear conductive agents. However, this approach has been limited by the presence of functional groups, which can lead to surface side reactions and deteriorate electrochemical properties.
[0009] Meanwhile, planar conductive materials such as graphene also have excellent conductivity, but they are also limited because it is difficult to produce a thin single layer of graphene, and using thick graphene reduces battery efficiency. Furthermore, planar conductive materials have limitations because they restrict the mobility of the electrolyte in the battery due to the wide planar contact.
[0010] Therefore, there is a need to develop an electrode coated with a conductive agent that has excellent electrical conductivity and can be uniformly distributed in the electrode. Summary of the Invention
[0011] Technical issues
[0012] One aspect of the present invention provides a novel electrode that can greatly improve conductivity in a battery and improve lifespan characteristics of the battery due to excellent electrode adhesion.
[0013] Another aspect of the present invention provides a secondary battery including the electrode.
[0014] Technical Solution
[0015] According to one aspect of the present invention, there is provided an electrode including an electrode active material layer, wherein the electrode active material layer includes an electrode active material, hydrogenated nitrile rubber and a conductive agent, the conductive agent includes a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are incorporated, and the carbon nanotube structure is included in the electrode active material layer in an amount of 0.01 wt % to 0.5 wt %.
[0016] According to another embodiment of the present inventive concept, a secondary battery including the electrode is provided.
[0017] Beneficial effects
[0018] Since the electrode according to the present invention is prepared by using a conductive agent dispersion in which bundle-type single-walled carbon nanotubes are appropriately dispersed using hydrogenated nitrile rubber, the carbon nanotube structures in the shape of ropes (long fibers) can be connected to each other to form a network structure in the electrode. In particular, since a network structure can be formed so that conductive connection (relatively long distance) can be carried out between the electrode active materials in the form of secondary particles and conductive connection can be carried out between the primary materials in the electrode active materials, a conductive path (path) in the electrode can be effectively formed. Therefore, even with a small amount of conductive agent, the conductivity in the battery can be greatly improved. In addition, the electrode active material layer is firmly fixed by the carbon nanotube structure forming a network structure, thereby having an effect of improving electrode adhesion.
[0019] Furthermore, when the electrode slurry includes the carbon nanotube structure, the powder resistance of the electrode slurry is reduced compared to the prior art, thereby achieving the effect of reducing the electrode resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a TEM photograph of the electrode of Example 1.
[0021] Figure 2 The SEM images of the conductive agent dispersions of Preparation Examples 1 to 5 were taken after drying on a silicon wafer (Preparation Examples 1 to 5 correspond to Figure 2 A to 2E).
[0022] Figure 3 Preparation Example 1 ( Figure 3 A) and Preparation Example 6 ( Figure 3 B) SEM photograph of the conductive agent dispersion after drying (Preparation Examples 1 to 5 correspond to Figure 2 A to 2E).
[0023] Figure 4 is a photograph showing the process of leaving the conductive agent dispersions of Preparation Examples 1 to 5 for 2 weeks (Preparation Examples 1 to 5 correspond to Figure 4 A to 4E).
[0024] Figure 5 is a TEM photograph of each conductive agent dispersion used in Example 1 and Comparative Example 4, and Example 1 ( Figure 5 A) and Comparative Example 4 ( Figure 5 B) SEM images of each positive electrode. DETAILED DESCRIPTION
[0025] The terms or words used in the present specification and claims should not be construed as limited to ordinary meanings or dictionary meanings, but should be construed as meanings and concepts consistent with the technical spirit based on the concept that the inventor can appropriately define the terms in order to interpret the principle of the present invention in the best manner.
[0026] The terminology used herein is for the purpose of describing particular exemplary embodiments only and is not intended to be limiting of the present invention. Terms in the singular may include plural forms unless the context clearly indicates otherwise.
[0027] It should be understood that when used in this specification, the terms "comprises", "comprising" or "having" specify the presence of stated features, numbers, steps, elements or combinations thereof, but do not preclude the presence or addition of one or more other features, numbers, steps, elements or combinations thereof.
[0028] In this specification, unless otherwise specifically stated, the expression "%" means wt%.
[0029] In this specification, the expression "specific surface area" is measured by the BET method, wherein, specifically, the specific surface area can be calculated from the nitrogen adsorption amount at liquid nitrogen temperature (77K) using BELSORP-mini manufactured by Bell Japan.
[0030] Hereinafter, the present invention will be described in detail.
[0031] electrode
[0032] The electrode according to the present invention includes an electrode active material layer, wherein the electrode active material layer includes an electrode active material, hydrogenated nitrile rubber and a conductive agent, the conductive agent includes a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are incorporated, and the carbon nanotube structure can be included in the electrode active material layer in an amount of 0.01 wt % to 0.5 wt %.
[0033] The electrode may include an electrode active material layer. The electrode may further include a current collector, and in this case, the electrode active material layer may be provided on one surface or both surfaces of the current collector.
[0034] The current collector is not particularly limited as long as the material of the current collector has conductivity and does not cause adverse chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, alloys thereof, these materials surface-treated with carbon, nickel, titanium, silver, etc., calcined carbon, etc. can be used.
[0035] The current collector can generally have a thickness of 3 μm to 500 μm, and minute concavities and convexities can be formed on the surface of the current collector to improve the adhesion of the electrode active material. In addition, for example, the current collector can be used in various forms such as a film, sheet, foil, net, porous body, foam body, non-woven fabric body, etc.
[0036] The electrode active material layer can include an electrode active material, hydrogenated nitrile rubber, and a conductive agent.
[0037] The electrode active material can be a positive electrode active material or a negative electrode active material commonly used in the art, and there is no particular limitation on its type.
[0038] For example, at least one metal such as cobalt, manganese, nickel, or aluminum and a lithium-containing lithium oxide can be used as the positive electrode active material. Specifically, the lithium oxide can include lithium manganese-based oxides (e.g., LiMnO2, LiMn2O, etc.), lithium cobalt-based oxides (e.g., LiCoO2, etc.), lithium nickel-based oxides (e.g., LiNiO2, etc.), lithium nickel manganese-based oxides (e.g., LiNi R1 Mn Y1 O2 (where 0 < Y1 < 1), LiNi Z1 Mn 2-Z1 O4 (where 0 < Z1 < 2), etc.), lithium-nickel cobalt-based oxides (e.g., LiNi 1-Y2 Co Y2 O2 (where 0 < Y2 < 1), etc.), lithium manganese cobalt-based oxides (e.g., LiCo 1-Y3 Mn Y3 O2 (where 0 < Y3 < 1), LiMn 2-Z2 Co z2 O4 (where 0 < Z2 < 2, etc.), lithium nickel cobalt manganese-based oxides (e.g., Li(Ni P1 Co Q1 Mn R1 )O2 (where 0 < P1 < 1, 0 < Q1 < 1, 0 < R1 < 1, and P1 + Q1 + R1 = 1) or Li(Ni P2 Co Q2 Mn R2 )O4 (where 0 < P2 < 2, 0 < Q2 < 2, 0 < R2 < 2, and P2 + Q2 + R2 = 2), etc.), or lithium nickel cobalt manganese other metal (M) oxides (e.g., Li(Ni P3 Co Q3 Mn R3 M 1 S)O2 (where M1 is selected from the group consisting of l, Cu, Fe, V, Cr, Ti, Zr, Zn, Ta, Nb, Mg, B, W, and Mo, and P3, Q3, R3, and S are the atomic fractions of each independent element, where 0 < P3 < 1, 0 < Q3 < 1, 0 < R3 < 1, 0 < S < 1, and P3 + Q3 + R3 + S = 1), etc.), and may include any one of them or two or more of them.
[0039] Meanwhile, the negative electrode active material may include, for example: carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; and metal compounds that can alloy with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; metal oxides that may or may not be doped with lithium such as SiO v (0 < v < 2), SnO2, vanadium oxides, and lithium vanadium oxides; or composites including metal compounds and carbonaceous materials such as Si-C composites or Sn-C composites; any one of them or a mixture of two or more of them may be used. In addition, a thin film of metallic lithium may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbon material.
[0040] The electrode active material may be included in an amount of 70% to 99.5% by weight, preferably 80% to 99% by weight, based on the total weight of the electrode active material layer. When the content of the electrode active material satisfies the above range, excellent energy density, electrode adhesion, and conductivity can be achieved.
[0041] The conductive agent may include a carbon nanotube structure.
[0042] The carbon nanotube structure may include a plurality of single-walled carbon nanotube units. Specifically, the carbon nanotube structure may be a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are bonded to each other, and more specifically, the carbon nanotube structure may be a carbon nanotube structure in which 2 to 4,500 single-walled carbon nanotube units are bonded to each other. More specifically, considering the dispersibility of the carbon nanotube structure and the durability of the electrode, it is most preferable that the carbon nanotube structure is a carbon nanotube structure in which 2 to 50 single-walled carbon nanotube units are bonded to each other.
[0043] In the carbon nanotube structure, the single-walled carbon nanotube units may be arranged side by side (where the long axes of the units are bonded to each other in parallel to have a flexible cylindrical structure) to form the carbon nanotube structure, and thus, the carbon nanotube structure may exhibit a rope-like shape. In addition, the carbon nanotube structures may be connected to each other to form a network structure in the electrode.
[0044] Conventional electrodes comprising carbon nanotubes are prepared by dispersing bundle-type or entangled-type carbon nanotubes (single-walled carbon nanotube units or multi-walled carbon nanotube units attached or entangled to each other) in a dispersion medium to prepare a conductive agent dispersion, and then using the conductive agent dispersion. In this case, the carbon nanotubes are completely dispersed in the typical conductive agent dispersion, thereby existing as a conductive agent dispersion in which single-chain carbon nanotube units are dispersed. In conventional conductive agent dispersions, the carbon nanotube units are easily cut by the over-dispersion process, making the length of the carbon nanotube units less than the initial length. In addition, the carbon nanotube units are also easily cut during the rolling process of the electrode, and another limitation arises, in which the carbon nanotube units are cut due to excessive volume changes of the electrode active material during battery operation. Therefore, due to the deterioration of the conductivity of the electrode, there is a limitation in that the input characteristics, output characteristics, and life characteristics of the battery deteriorate. In addition, for the multi-walled carbon nanotube unit, the structural defects are high due to the node growth mechanism (not a smooth linear shape, but the nodes exist due to defects generated during the growth process). Therefore, during the dispersion process, the multi-walled carbon nanotube unit is more likely to be cut, and the cut multi-walled carbon nanotube unit may be cut short through the carbon of the unit. Therefore, it is difficult to make the multi-walled carbon nanotube units disperse more uniformly and exist in the electrode slurry.
[0045] Alternatively, since the carbon nanotube structure included in the electrode of the present invention has a form in which 2 to 5,000 single-walled carbon nanotube units are bonded side by side and relatively maintain high crystallinity without structural defects, their length can be well maintained without being cut even during battery operation, thereby maintaining the conductivity of the electrode. In addition, since the high conductivity of the single-walled carbon nanotube units with high crystallinity leads to increased conductivity of the electrode, the input characteristics, output characteristics, and life characteristics of the battery can be significantly improved. In addition, since the carbon nanotube structure can be connected to each other to have a network structure in the electrode, excessive volume changes of the electrode active material can be suppressed, and at the same time, a strong conductive path can be ensured, and the peeling of the electrode active material can be suppressed to significantly improve the electrode adhesion.
[0046] In the carbon nanotube structure, the average diameter of the single-walled carbon nanotube units can be 0.5 nm to 10 nm, particularly 1 nm to 9 nm. When this average diameter is met, even with a very small amount of conductive agent, the conductivity of the electrode is maximized. When the prepared electrode is observed by SEM, the average diameter corresponds to the average of the diameters of the first 100 single-walled carbon nanotubes with large diameters and the last 100 single-walled carbon nanotubes with small diameters.
[0047] In the carbon nanotube structure, the average length of the single-walled carbon nanotube unit can be 1 μm to 100 μm, particularly 5 μm to 50 μm. When the average length is satisfied, a long conductive path for conductive connection between the electrode active material particles can be formed, and a unique network structure can be formed. Therefore, even with a very small amount of conductive agent, the conductivity in the electrode can be maximized. When the prepared electrode is observed by SEM, the average length corresponds to the average of the lengths of the first 100 single-walled carbon nanotubes with long lengths and the last 100 single-walled carbon nanotubes with short lengths.
[0048] The specific surface area of a single-walled carbon nanotube unit can be 500m 2 / g to 1,000m 2 / g, especially 600m 2 / g to 800m 2 When the above range is met, the large specific surface area allows for a smooth conductive path in the electrode, maximizing the conductivity of the electrode even with a minimal amount of conductive agent. The specific surface area of a single-walled carbon nanotube unit can be calculated from the amount of nitrogen adsorbed at liquid nitrogen temperature (77K) using Bell Japan's BELSORP-mini.
[0049] The carbon nanotube structure can be included in the electrode active material layer in an amount of 0.01 wt % to 0.5 wt %, particularly 0.03 wt % to 0.3 wt %, and more particularly 0.05 wt % to 0.2 wt %. When the above range is met, since the conductive path of the electrode can be ensured, the life characteristics of the battery can be improved while keeping the electrode resistance at a low level. In contrast, when an electrode is prepared by using a conductive agent dispersion including fully dispersed conventional single-walled carbon nanotube units, the carbon nanotube structure is not included in the electrode active material layer, or even if it is included unintentionally, it will be included in a very low content that can be ignored. In other words, when an electrode is prepared by using a conductive agent dispersion including fully dispersed conventional single-walled carbon nanotube units, the content of the above-mentioned carbon nanotube structure cannot be deduced.
[0050] Regarding the prior art in which an electrode includes multi-walled carbon nanotube units, a large content (e.g., greater than 0.5 wt%) of multi-walled carbon nanotube units must be used to compensate for the low conductivity of the multi-walled carbon nanotube units. In addition, when an electrode is prepared by using a conductive agent dispersion in which single-walled carbon nanotube units are completely dispersed, the single-walled carbon nanotube units cannot be used at a low content because the single-walled carbon nanotube units may be cut.
[0051] In contrast, the carbon nanotube structure included in the electrode of the present invention has a structure in which 2 to 5,000 single-walled carbon nanotube units are bonded side by side. Therefore, even during battery operation, their length is well maintained without being cut, thereby maintaining the conductivity of the electrode. Furthermore, due to the high conductivity of the single-walled carbon nanotube units, the conductivity of the electrode can be smoothly maintained. Therefore, even if the content of the carbon nanotube structure in the electrode is very low, the input characteristics, output characteristics, and lifespan characteristics of the battery can be excellent.
[0052] Hydrogenated nitrile rubber is a material that is initially included in the electrode, as part of the conductive agent dispersion required for preparing the electrode slurry. Hydrogenated nitrile rubber helps bundled carbon nanotubes to be smoothly dispersed in the conductive agent dispersion.
[0053] The weight average molecular weight of the hydrogenated nitrile rubber may be 50,000 g / mol to 500,000 g / mol, particularly 100,000 g / mol to 300,000 g / mol. When the above range is met, the hydrogenated nitrile rubber can easily penetrate between the single-walled carbon nanotube units in the bundled carbon nanotubes, thereby obtaining a suitable dispersion of the bundled carbon nanotubes and improving the phase stability of the conductive agent dispersion.
[0054] Hydrogenated nitrile butadiene rubber can be with 0.1 weight % to 5.0 weight %, particularly 0.1 weight % to 3.0 weight %, and more particularly 0.1 weight % to 3.0 weight %, for example 0.3 weight % to 3.0 weight % amount is included in the electrode active material layer. When meeting above-mentioned scope, the diameter of carbon nanotube structure can be suitably controlled, the dispersion stability of carbon nanotube structure in electrode slurry can be improved, and gelation (gelation) can be prevented by the compatibility between adhesive (particularly PVdF) and hydrogenated nitrile butadiene rubber. Therefore, the input characteristics, output characteristics and the life characteristics of battery can be improved.
[0055] The weight ratio of the carbon nanotube structure to the hydrogenated nitrile rubber can be in the range of 1:0.1 to 1:10, particularly in the range of 1:1 to 1:5. When the above range is met, the diameter of the carbon nanotube structure can be appropriately controlled, the dispersion stability of the carbon nanotube structure in the electrode slurry can be further improved, and gelation can be further prevented due to the compatibility between the binder (particularly PVdF) and the hydrogenated nitrile rubber. Therefore, the input characteristics, output characteristics, and life characteristics of the battery can be improved.
[0056] The electrode active material layer may further include an adhesive. Adhesive is used to ensure the bonding force between the electrode active material particles or between the electrode active material and the current collector, wherein any adhesive commonly used in the art can be used, and its type is not particularly limited. Adhesive can include, for example, polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile (polyacrylonitrile), carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber or their various copolymers, and any one of them or a mixture of two or more thereof can be used.
[0057] The binder may be included in an amount of 10 wt % or less, preferably 1 wt % to 3 wt % based on the total weight of the electrode active material layer. When the binder content satisfies the above range, excellent electrode adhesion can be achieved while minimizing the increase in electrode resistance.
[0058] Method for preparing electrodes
[0059] Next, the method for producing an electrode of the present invention will be described.
[0060] The method for preparing an electrode of the present invention includes: (1) preparing a mixture comprising bundled carbon nanotubes, hydrogenated nitrile rubber, and a dispersion medium; (2) dispersing the bundled carbon nanotubes in the mixture to form a conductive agent dispersion; (3) preparing an electrode slurry comprising the conductive agent dispersion and an electrode active material; and (4) coating the electrode slurry on a current collector and then drying the coated current collector. The electrode of the above embodiment can be prepared by the above method.
[0061] (1) Steps for preparing the mixture
[0062] A mixture can be prepared by injecting bundled carbon nanotubes and hydrogenated nitrile rubber into a dispersion medium. In the bundled carbon nanotubes, the single-walled carbon nanotube units are aggregated into a bundle, wherein the bundled carbon nanotubes typically include two or more single-walled carbon nanotube units. Specifically, the number of carbon nanotube units comprising the bundled carbon nanotubes is greater than the number of carbon nanotube units comprising the carbon nanotube structure.
[0063] Since the hydrogenated nitrile rubber is the same as the above-mentioned hydrogenated nitrile rubber, description thereof will be omitted.
[0064] The weight ratio of the bundled carbon nanotubes to the hydrogenated nitrile rubber can be in the range of 1:0.1 to 1:10, particularly in the range of 1:1 to 1:5. The diameter of the carbon nanotube structure can be appropriately controlled, which can further improve the dispersion stability of the carbon nanotube structure in the electrode slurry. Furthermore, gelation can be further prevented by improving the compatibility between the binder (particularly PVdF) and the hydrogenated nitrile rubber. Consequently, the input, output, and life characteristics of the battery can be improved.
[0065] The dispersion medium may include, for example, an amide-based polar organic solvent such as dimethylformamide (DMF), diethylformamide, dimethylacetamide (DMAc) and N-methylpyrrolidone (NMP); an alcohol such as methanol, ethanol, 1-propanol, 2-propanol (isopropanol), 1-butanol (n-butanol), 2-methyl-1-propanol (isobutanol), 2-butanol (sec-butanol), 1-methyl-2-propanol (tert-butanol), pentanol, hexanol, heptanol or octanol; a diol such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propylene glycol, 1,3-butanediol, 1,5-pentanediol or hexanediol. Alcohol; Polyols such as glycerol, trimethylolpropane, pentaerythritol or sorbitol; Glycol ethers such as ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, tetraethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, tetraethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether or tetraethylene glycol monobutyl ether; Ketones such as acetone, methyl ethyl ketone, methyl acetone or cyclopentanone; Ester such as ethyl acetate, γ-butyrolactone and ε-propiolactone, any one of them or a mixture of two or more of them can be used, but are not limited thereto. Specifically, the dispersion medium can be N-methylpyrrolidone (NMP).
[0066] The solid content of the mixed solution can be in the range of 0.1% to 10% by weight, particularly 1% to 5% by weight. The diameter of the carbon nanotube structure can be appropriately controlled, and the dispersion stability of the carbon nanotube structure in the electrode slurry can be further improved. In addition, the electrode slurry can have a high solid content while maintaining appropriate viscosity and elasticity.
[0067] (2) Step of forming a conductive agent dispersion
[0068] The process of dispersing the bundle-shaped carbon nanotubes in the mixture can be carried out using a mixing device such as a homogenizer, a bead mill, a ball mill, a basket mill, an attritor, a universal stirrer, a transparent mixer, a pin mill, a TK mixer, or an ultrasonic treatment (sonification) device. Among them, the bead mill method is preferred because the diameter size of the carbon nanotube structure can be controlled, the carbon nanotube structure can be uniformly distributed, and it has cost advantages.
[0069] The bead milling method can be as follows: the mixture is added to a container containing beads, and the container is rotated to disperse the bundled carbon nanotubes.
[0070] In this case, the conditions for performing the bead milling method are as follows.
[0071] The average particle size of the beads may be 0.5 to 1.5 mm, particularly 0.5 to 1.0 mm. Within this range, the carbon nanotube structure is not broken and its diameter can be appropriately controlled during the dispersion process, and a dispersed solution having a uniform composition can be prepared.
[0072] The rotation speed of the container may be 500 to 10,000 RPM, particularly 2,000 to 6,000 RPM. Within the range, during the dispersion process, the carbon nanotube structure is not broken and its diameter can be appropriately controlled, and a dispersed solution having a uniform composition can be prepared.
[0073] The bead milling time may be 0.5 to 10 hours, particularly 1 to 5 hours, and more particularly 1 to 2 hours. When the above range is met, the carbon nanotube structure is not broken during the dispersion process, its diameter can be appropriately controlled, and a dispersed solution with a uniform composition can be prepared. The bead milling time refers to the total time the bead mill is used. For example, if the bead milling is performed several times, the bead milling time refers to the total time spent on the several bead millings.
[0074] Bead milling conditions are designed to properly disperse the bundled carbon nanotubes, particularly in situations where the bundled carbon nanotubes are completely dispersed into single-stranded single-walled carbon nanotubes. Specifically, bead milling conditions are designed to properly disperse the bundled carbon nanotubes to form a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are bound side by side in the resulting conductive agent dispersion. This can only be achieved by strictly controlling the composition of the mixture, the bead milling conditions, and other factors.
[0075] Through the above process, a conductive agent dispersion containing a carbon nanotube structure can be formed.
[0076] (3) Steps for preparing electrode slurry
[0077] When the conductive agent dispersion is prepared through the above process, the electrode active material is mixed with the conductive agent dispersion to form an electrode slurry. In this case, the above-mentioned electrode active material can be used as the electrode active material.
[0078] In addition, as needed, the electrode slurry may further include a binder and a solvent. In this case, the binder of the above embodiment may be used as a binder. The solvent may include, for example, an amide-based polar organic solvent such as dimethylformamide (DMF), diethylformamide, dimethylacetamide (DMAc) and N-methylpyrrolidone (NMP); alcohols such as methanol, ethanol, 1-propanol, 2-propanol (isopropanol), 1-butanol (n-butanol), 2-methyl-1-propanol (isobutanol), 2-butanol (sec-butanol), 1-methyl-2-propanol (tert-butanol), pentanol, hexanol, heptanol or octanol; glycols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propylene glycol, 1,3-butanediol, 1,5-pentanediol or hexanediol; polyols such as propylene glycol, diethylene glycol, triethylene glycol, propylene glycol, 1,3-propanediol ... Polyols such as glycerol, trimethylolpropane, pentaerythritol or sorbitol; glycol ethers such as ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, triethylene glycol monomethyl ether, tetraethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monoethyl ether, triethylene glycol monoethyl ether, tetraethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, triethylene glycol monobutyl ether or tetraethylene glycol monobutyl ether; ketones such as acetone, methyl ethyl ketone, methyl propyl ether or cyclopentanone; esters such as ethyl acetate, γ-butyrolactone and ε-propiolactone, any one of them or a mixture of two or more of them can be used, but the present invention is not limited thereto. The solvent may be the same as or different from the dispersion medium used in the pre-dispersion, and may preferably be N-methylpyrrolidone (NMP, N-methylpyrrolidone).
[0079] Meanwhile, in this case, the electrode active material can be included in an amount of 70 wt % to 99.5 wt %, preferably 80 wt % to 99 wt %, based on the total solid content in the electrode slurry. When the content of the electrode active material satisfies the above range, excellent energy density, electrode adhesion and conductivity can be achieved.
[0080] In addition, in the case of including a binder, the binder may be included in an amount of 10 wt % or less, specifically 0.5 wt % to 5 wt %, preferably 1 wt % to 3 wt % based on the total solid content in the electrode slurry.
[0081] The solid content in the electrode slurry can be in the range of 60% to 80% by weight, particularly 65% to 75% by weight. When the above range is met, during the drying period after the electrode slurry is applied, the migration of the conductive agent and the binder due to evaporation of the solvent can be suppressed, and an electrode with excellent electrode adhesion and conductivity can be prepared. In addition, high-quality electrodes with less deformation during rolling can be prepared.
[0082] (4) Step of forming an electrode active material layer
[0083] Next, an electrode active material layer is formed by applying and drying the electrode slurry prepared as described above. Specifically, the electrode active material layer can be formed by applying the electrode slurry to an electrode current collector and then drying the applied current collector, or the electrode active material layer can be formed by casting the electrode slurry on a separate support and then laminating the film separated from the support onto the electrode current collector. If necessary, after the electrode active material layer is formed by the above method, a rolling process can be further performed.
[0084] In this case, the drying and rolling may be performed under appropriate conditions in consideration of the physical properties of the finally produced electrode, without particular limitation.
[0085] secondary batteries
[0086] Next, a secondary battery according to the present invention will be described.
[0087] The secondary battery according to the present invention includes the electrode of the present invention as described above. In this case, the electrode may be at least one of a positive electrode and a negative electrode. Specifically, the secondary battery according to the present invention may include a positive electrode, a negative electrode, a separator arranged between the positive electrode and the negative electrode, and an electrolyte. In this case, at least one of the positive electrode and the negative electrode includes the above-mentioned electrode of the present invention, that is, the electrode active material layer, the electrode active material layer includes an electrode active material, hydrogenated nitrile rubber and a conductive agent, the conductive agent includes a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are combined, and the carbon nanotube structure can be included in the electrode active material layer in an amount of 0.01 wt % to 0.5 wt %. Preferably, the electrode of the present invention may be a positive electrode. Since the electrode according to the present invention has been described above, a detailed description will be omitted, and only other components will be described below.
[0088] The separator separates the positive electrode and the negative electrode and provides a mobile path for lithium ions, wherein any separator can be used as a separator without particular limitation, as long as it is commonly used for secondary batteries. Specifically, a porous polymer film can be used, for example, a porous polymer film prepared from a polyolefin-based polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminated structure of these polymer films with two or more layers as a separator. In addition, a typical porous non-woven fabric can be used, for example, a non-woven fabric formed of high-melting-point glass fiber or polyethylene terephthalate fiber. In addition, a coated separator including a ceramic component or a polymer component can be used to ensure heat resistance or mechanical strength, and a separator with a single layer or multilayer structure can be selectively used.
[0089] The electrolyte may include an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel-type polymer electrolyte, a solid inorganic electrolyte, or a melt-type inorganic electrolyte that can be used in the preparation of a lithium secondary battery, but is not limited thereto.
[0090] Specifically, the electrolyte may include a non-aqueous organic solvent and a metal salt.
[0091] For example, aprotic organic solvents such as N-methyl-2-pyrrolidone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran (franc), 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxymethane, dioxolane derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ether, methyl propionate, and ethyl propionate can be used as the non-aqueous organic solvent.
[0092] In particular, cyclic carbonates (ethylene carbonate and propylene carbonate) in carbonate-based organic solvents are highly viscous organic solvents that dissociate lithium salts in electrolyte solutions well due to their high dielectric constant, and therefore cyclic carbonates can be preferably used. Since, when the cyclic carbonates are mixed with low-viscosity, low-dielectric-constant linear carbonates such as dimethyl carbonate and diethyl carbonate in an appropriate ratio, highly conductive electrolyte solutions can be prepared, the cyclic carbonates can be more preferably used.
[0093] As the metal salt, a lithium salt can be used. The lithium salt is a material that is easily soluble in a non-aqueous electrolyte solution. For example, as an anion of the lithium salt, at least one selected from the group consisting of: F - 、Cl -, I - 、NO3 - 、N(CN)2 - 、BF4 - 、ClO4 - PF6 - 、(CF3)2PF4 - 、(CF3)3PF3 - 、(CF3)4PF2 - 、(CF3)5PF - 、(CF3)6P - CF3SO3 - CF3CF2SO3 - 、(CF3SO2)2N - 、(FSO2)2N - CF3CF2(CF3)2CO - 、(CF3SO2)2CH - 、(SF5)3C - 、(CF3SO2)3C - CF3(CF2)7SO3 - CF3CO2 - 、CH3CO2 - 、SCN - and (CF3CF2SO2)2N - .
[0094] In order to improve the life characteristics of the battery, prevent the reduction of the battery capacity, and improve the discharge capacity of the battery, in addition to the above-mentioned electrolyte components, at least one additive may be further included in the electrolyte, for example, a halogenated alkylene carbonate compound such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dye, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol, or aluminum chloride.
[0095] The secondary battery according to the present invention as described above has excellent electrode adhesion and excellent lifespan characteristics at high temperatures compared to typical secondary batteries.
[0096] Hereinafter, the present invention will be described in more detail based on specific examples.
[0097] Preparation Example 1: Preparation of Conductive Agent Dispersion
[0098] Bundle-type carbon nanotubes (specific surface area 650 m2) consisting of single-walled carbon nanotube units with an average diameter of 1.5 nm and an average length of 5 μm or more 2 / g) and hydrogenated nitrile rubber (weight average molecular weight: 260,000 g / mol) were mixed in N-methylpyrrolidone (NMP) as a solvent to prepare a mixture so that the solid content was 2.4% by weight.
[0099] The mixture was stirred using a bead mill method, and the bundled carbon nanotubes were dispersed in a solvent to prepare a conductive agent dispersion. In this case, the diameter of the beads was 1 mm, the rotation speed of the stirring container containing the beads was 3,000 RPM, and stirring was performed for 60 minutes. The conductive agent dispersion included a carbon nanotube structure having a form in which 2 to 5,000 single-walled carbon nanotube units were bonded side by side.
[0100] In the conductive agent dispersion, the amount of the carbon nanotube structure was 0.4% by weight, and the amount of the hydrogenated nitrile rubber was 2.0% by weight.
[0101] Preparation Example 2: Preparation of Conductive Agent Dispersion
[0102] A conductive agent dispersion was prepared in the same manner as in Preparation Example 1, except that the conductive agent dispersion was prepared so that the carbon nanotube structure was present in an amount of 0.4 wt % and the hydrogenated nitrile rubber was present in the conductive agent dispersion in an amount of 0.2 wt %.
[0103] Preparation Example 3: Preparation of Conductive Agent Dispersion
[0104] A conductive agent dispersion was prepared in the same manner as in Preparation Example 1, except that polyvinylidene fluoride (PVdF, Solef-5130) having a weight average molecular weight of 880,000 g / mol was used instead of hydrogenated nitrile rubber.
[0105] Preparation Example 4: Preparation of Conductive Agent Dispersion
[0106] A conductive agent dispersion was prepared in the same manner as in Preparation Example 1, except that polyvinylidene fluoride (PVdF, KF9700) having a weight average molecular weight of 880,000 g / mol was used instead of hydrogenated nitrile rubber.
[0107] Preparation Example 5: Preparation of Conductive Agent Dispersion
[0108] A conductive agent dispersion was prepared in the same manner as in Preparation Example 1, except that hydrogenated nitrile rubber was not used.
[0109] Preparation Example 6: Preparation of Conductive Agent Dispersion
[0110] A conductive agent dispersion was prepared in the same manner as in Preparation Example 1, except that bundle-type carbon nanotubes (specific surface area of 185 m 2 / g) instead of the bundle-type carbon nanotubes used in Preparation Example 1.
[0111] Test Example 1: Observation of the Dispersion and Formation of Carbon Nanotube Structures in Conductive Agent Dispersion
[0112] For each of Preparation Examples 1 to 6, the dispersion and formation of the carbon nanotube structure were observed by SEM, and the results are shown in FIG. Figure 2 and Figure 3 . Figure 2 A to 2E correspond to Preparation Examples 1 to 5, respectively. Figure 3 A corresponds to Preparation Example 1, Figure 3 B corresponds to Preparation 6.
[0113] Test Example 2: Evaluation of Formation of Bundled Carbon Nanotubes in Conductive Agent Dispersion
[0114] The conductive agent dispersions of Preparation Examples 1 to 5 were left at 25°C for 2 weeks. The results are shown in FIG. Figure 4 .
[0115] Reference Figure 2 In the case of Preparation Examples 1 and 2, it can be seen that there is a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are bonded side by side. In addition, it can be seen that the dispersion of Preparation Examples 1 and 2 using hydrogenated nitrile rubber as a dispersant is better than that of Preparation Examples 3 and 4 using polyvinylidene fluoride and Preparation Example 5 not using a dispersant. In addition, referring to Figure 4 , since the dispersities of Preparation Examples 1 and 2 are better than those of other Preparation Examples, it can be seen that the dispersibility remains optimal even after being placed for a long time. In addition, since 2.0 wt % of hydrogenated nitrile butadiene rubber is used in Preparation Example 1, the dispersibility of Preparation Example 1 is better than that of Preparation Example 2 which uses 0.2 wt % of hydrogenated nitrile butadiene rubber.
[0116] Reference Figure 3 , it can be seen that the single-walled carbon nanotube units in the conductive agent dispersion of Preparation Example 1 were not cut and were maintained in a long fiber length, showing high dispersibility. On the other hand, it can be seen that the multi-walled carbon nanotube units in the conductive agent dispersion of Preparation Example 6 were mostly cut and existed only in a length of 1 μm, and its dispersibility was low even when the dispersion process was applied under the same conditions.
[0117] Therefore, it can be seen that the use of hydrogenated nitrile rubber, its content, and appropriate use of bundle-type carbon nanotubes composed of single-walled carbon nanotube units can improve dispersibility and conductivity.
[0118] Examples and Comparative Examples
[0119] Example 1: Manufacturing the positive electrode
[0120] LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622) and a binder (PVDF, KF9700) were added to the conductive agent dispersion of Preparation Example 1, and N-methylpyrrolidone (NMP) was further added to prepare a positive electrode slurry having a solid content of 72.0 wt%. This positive electrode slurry was coated on a 20 μm thick Al thin film current collector, dried at 130°C, and roll-pressed to prepare a positive electrode including a positive electrode active material layer.
[0121] In the positive electrode active material layer, LiNi 0.6 Co 0.2 Mn 0.2 The content of O2 (NCM622) was 97.9 wt%, the content of the binder was 1.8 wt%, the content of the hydrogenated nitrile rubber was 0.25 wt%, and the content of the carbon nanotube structure was 0.05 wt%.
[0122] Reference Figure 1 and Figure 5 A. It can be seen that in the positive electrode of Example 1, the rope-shaped carbon nanotube structure forms a network structure and connects the NCM622 to each other.
[0123] Example 2: Manufacturing the positive electrode
[0124] LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622) and a binder (PVDF, KF9700) were added to the conductive agent dispersion of Preparation Example 1, and N-methylpyrrolidone (NMP) was further added to prepare a positive electrode slurry having a solid content of 70.1% by weight. This positive electrode slurry was coated on a 20 μm thick Al thin film current collector, dried at 130°C, and roll-pressed to prepare a positive electrode including a positive electrode active material layer.
[0125] In the positive electrode active material layer, LiNi 0.6 Co 0.2 Mn 0.2 The content of O2 (NCM622) was 97.6% by weight, the content of the binder was 1.8% by weight, the content of the hydrogenated nitrile rubber was 0.5% by weight, and the content of the carbon nanotube structure was 0.1% by weight.
[0126] Comparative Example 1: Manufacturing a positive electrode
[0127] (1) Preparation of conductive agent dispersion
[0128] The specific surface area is 240m 2 / g of carbon black and hydrogenated nitrile rubber (weight average molecular weight: 260,000 g / mol) were mixed with N-methylpyrrolidone (NMP) as a solvent to prepare a mixture having a solid content of 16.5% by weight.
[0129] The mixture was stirred by a bead mill method and the bundle-type carbon nanotubes were dispersed in the solvent to prepare a conductive agent dispersion. In this case, the diameter of the beads was 1 mm, the rotation speed of the stirring container containing the beads was 3,000 RPM, and stirring was performed for 60 minutes.
[0130] In the conductive agent dispersion, the amount of carbon black was 15% by weight, and the amount of hydrogenated nitrile rubber was 1.5% by weight.
[0131] (2) Preparation of positive electrode
[0132] LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622) and a binder (PVDF, KF9700) were added to the conductive agent dispersion, and N-methylpyrrolidone (NMP) was further added to prepare a positive electrode slurry with a solid content of 72.0 wt%. The positive electrode slurry was coated on an Al thin film current collector with a thickness of 20 μm, dried at 130°C, and roll-pressed to prepare a positive electrode including a positive electrode active material layer.
[0133] In the positive electrode active material layer, LiNi 0.6 Co 0.2 Mn 0.2 The content of O2 (NCM622) was 96.35 wt %, the content of the binder was 2.0 wt %, the content of the hydrogenated nitrile rubber was 0.15 wt %, and the content of the carbon black was 1.5 wt %.
[0134] Comparative Example 2: Manufacturing a positive electrode
[0135] LiNi 0.6 Co 0.2 Mn 0.2O2 (NCM622) and a binder (PVDF, KF9700) were added to the conductive agent dispersion of Preparation Example 6, and N-methylpyrrolidone (NMP) was further added to prepare a positive electrode slurry having a solid content of 72.1% by weight. This positive electrode slurry was coated on a 20 μm thick Al thin film current collector, dried at 130°C, and roll-pressed to prepare a positive electrode including a positive electrode active material layer.
[0136] In the positive electrode active material layer, LiNi 0.6 Co 0.2 Mn 0.2 The content of O2 (NCM622) was 97.48 wt%, the content of the binder was 1.8 wt%, the content of the hydrogenated nitrile rubber was 0.12 wt%, and the content of the multi-walled carbon nanotube was 0.6 wt%.
[0137] Comparative Example 3: Manufacturing a positive electrode
[0138] LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622) and a binder (PVDF, KF9700) were added to the conductive agent dispersion of Preparation Example 6, and N-methylpyrrolidone (NMP) was further added to prepare a positive electrode slurry having a solid content of 71.8 wt%. This positive electrode slurry was coated on a 20 μm thick Al thin film current collector, dried at 130°C, and roll-pressed to prepare a positive electrode including a positive electrode active material layer.
[0139] In the positive electrode active material layer, LiNi 0.6 Co 0.2 Mn 0.2 The content of O2 (NCM622) was 97.04 wt%, the content of the binder was 2.0 wt%, the content of the hydrogenated nitrile rubber was 0.16 wt%, and the content of the multi-walled carbon nanotube was 0.8 wt%.
[0140] Comparative Example 4: Manufacturing a positive electrode
[0141] (1) Preparation of conductive agent dispersion
[0142] Bundle-type carbon nanotubes (specific surface area 650 m2) consisting of single-walled carbon nanotube units with an average diameter of 1.5 nm and an average length of 5 μm or more 2 / g) and hydrogenated nitrile rubber (weight average molecular weight: 260,000 g / mol) were mixed in N-methylpyrrolidone (NMP) as a solvent to prepare a mixture so that the solid content was 4.4% by weight.
[0143] The mixture was stirred using a bead mill method, and the bundled carbon nanotubes were dispersed in the solvent to prepare a conductive agent dispersion. In this case, the diameter of the beads was 1 mm, the rotation speed of the stirring container containing the beads was 3,000 RPM, and when one cycle was stirred for 60 minutes, a total of four cycles were performed (natural cooling for 60 minutes between two cycles).
[0144] In the conductive material dispersion, the amount of the bundle-type carbon nanotubes was 0.4% by weight, and the amount of the hydrogenated nitrile rubber was 4.0% by weight.
[0145] (2) Preparation of positive electrode
[0146] LiNi 0.6 Co 0.2 Mn 0.2 O2 (NCM622) and a binder (PVDF, KF9700) were added to the conductive agent dispersion, and N-methylpyrrolidone (NMP) was further added to prepare a positive electrode slurry with a solid content of 72.0 wt%. The positive electrode slurry was coated on an Al thin film current collector with a thickness of 20 μm, dried at 130°C, and roll-pressed to prepare a positive electrode including a positive electrode active material layer.
[0147] In the positive electrode active material layer, LiNi 0.6 Co 0.2 Mn 0.2 The content of O2 (NCM622) is 97.65 wt %, the content of the binder is 1.8 wt %, the content of the hydrogenated nitrile rubber is 0.5 wt %, and the content of the single-walled carbon nanotube is 0.05 wt %. Figure 5 B, no carbon nanotube structure is observed in the positive electrode active material layer, and it can be seen that the single-walled carbon nanotube unit exists alone in the form of a single chain. Figure 5 In B, the single-walled carbon nanotube units are observed to partially overlap, which is not a bonded state, but only the single-walled carbon nanotube units are observed to overlap above and below the observation direction, and have different orientations.
[0148] Experimental Example 1
[0149] Each positive electrode slurry used to prepare the positive electrodes of Examples 1 and 2 and Comparative Examples 1 to 4 was dried in a vacuum at 130°C for 3 hours and then pulverized to prepare a powder. Thereafter, pellets were prepared using a Loresta GP apparatus from Mitsubishi Chemical Analytic Co., Ltd. at 25°C under a load of 9.8 MPa and in an atmosphere of 50% relative humidity. The powder resistance was then measured using a 4-probe method. The measurement results are shown in Table 1 below.
[0150] Experimental Example 2
[0151] The adhesion of each of the positive electrodes prepared in Examples 1 and 2 and Comparative Examples 1 to 4 was measured by a 90° peel test method.
[0152] Specifically, double-sided tape was attached to a glass slide, and an electrode punched out to 20 mm x 180 mm was placed on the glass slide and adhered to it by reciprocating a 2 kg roller 10 times. The electrode was then pulled out at a speed of 200 mm / min using a UTM (TA Corporation) device to measure the force required to peel it from the glass slide. In this case, the measurement angle between the glass slide and the electrode was 90°. The measurement results are shown in Table 1 below.
[0153] Experimental Example 3
[0154] A single cell was prepared by combining a positive electrode, a negative electrode, and a 15 μm thick polyethylene-based separator prepared according to Examples 1 and 2 and Comparative Examples 1 to 4. In this case, a negative electrode slurry was prepared by mixing graphite, SBR / CMC, and a conductive agent in a weight ratio of 96.5:2.5:1, coating the negative electrode slurry on a 10 μm copper foil, and drying it at 100°C to prepare the negative electrode. Then, an electrolyte solution containing 1M LiPF6 was injected into a mixed solvent of dimethyl carbonate (DEC) and ethylene carbonate (EC) (DEC:EC=1:1) to manufacture a lithium secondary battery.
[0155] The lithium secondary battery prepared as described above was charged and discharged 60 times at 0.33C / 0.33C at 45°C, and then life characteristics were measured by using the measured charge efficiency and discharge efficiency. The measurement results are shown in Table 1 below.
[0156] [Table 1]
[0157]
[0158] Referring to Table 1, it can be seen that the electrode adhesion and life characteristics of Examples 1 and 2 including the carbon nanotube structure described in this specification are high, and the powder resistance of the slurry used to manufacture the electrodes is low.
[0159] In particular, in the case of Comparative Examples 2 and 3, since the multi-walled carbon nanotube units were cut during the dispersion process, it was difficult to maintain the conductive path, so the powder resistance of the slurry was high, and it was difficult to form a conductive network structure in the electrode, so it appeared to have very low electrode adhesion and life characteristics.
[0160] In Comparative Example 4, the bundled carbon nanotubes were excessively dispersed, resulting in the single-walled carbon nanotubes being isolated and present in the electrode as single strands. Furthermore, the single-walled carbon nanotubes were cut during the battery manufacturing process, failing to form a network structure like the rope-like carbon nanotube structure, and instead existed only in close contact with the surface of the electrode active material. Consequently, the conductive network could not be smoothly maintained, resulting in high slurry powder resistance and poor electrode adhesion and lifespan.
Claims
1. An electrode comprising an electrode active material layer, in: The electrode active material layer comprises an electrode active material, hydrogenated nitrile rubber and a conductive agent; The conductive agent includes a carbon nanotube structure in which 2 to 5,000 single-walled carbon nanotube units are incorporated; and The carbon nanotube structure is included in the electrode active material layer in an amount of 0.01 wt % to 0.5 wt %, The carbon nanotube structures are connected to each other to form a network structure in the electrode, and The average diameter of the single-walled carbon nanotube unit is 0.5 nm to 9 nm, The average length of the single-walled carbon nanotube unit is 1 μm to 100 μm, The specific surface area of the single-walled carbon nanotube unit is 500 m 2 / g to 1,000 m 2 / g, The weight ratio of the carbon nanotube structure to the hydrogenated nitrile rubber is 1:0.1 to 1:
10. 2 . The electrode according to claim 1 , wherein in the carbon nanotube structure, the single-walled carbon nanotube units are arranged and combined side by side. 3 . The electrode according to claim 1 , wherein the hydrogenated nitrile rubber has a weight average molecular weight of 50,000 g / mol to 500,000 g / mol. The electrode according to claim 1 , wherein the electrode is a positive electrode. 5 . A secondary battery comprising the electrode according to claim 1 .