Semiconductor device and method for manufacturing the same

By introducing dopant substances at the Ge-Si interface and optimizing the interface structure, the problems of dark current and leakage current in semiconductor optical sensors are solved, and the performance and reliability of the device are improved.

CN113675229BActive Publication Date: 2024-10-15TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202110880144.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-06-02
Filing Date
2021-08-02
Publication Date
2024-10-15
Estimated Expiration
2041-08-02

AI Technical Summary

Technical Problem

In existing semiconductor optical image sensors, dark current problems caused by poor interface quality between semiconductor layers affect device performance and reliability. Especially in Ge-based sensors, since the energy band gap of Ge is smaller than Si, the leakage current increases. , reducing optical performance.

Method used

By performing doping treatment at the Ge-Si interface, dopants are introduced using ion implantation or dopant substances such as P-type materials (such as boron, aluminum, gallium, BF2) and Group VIIA materials (such as fluorine, chlorine, bromine) , optimizing the interface to prevent electrons in the Si layer from entering the germanium layer, thereby reducing leakage current.

Benefits of technology

It significantly reduces the dark current and leakage current problems in Ge-based sensors, improves the performance of the optical sensor, and improves the reliability of the device. The specific effect is that the leakage current/dark current is reduced by about 10%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113675229B_ABST
    Figure CN113675229B_ABST
Patent Text Reader

Abstract

Methods and structures for providing an optical sensor with an optimized Ge-Si interface include providing a substrate having a pixel region and a logic region. In some embodiments, the method further includes forming a trench in the pixel region. In various examples, and after forming the trench, the method further includes forming a doped semiconductor layer along the sidewalls and bottom surface of the trench. In some embodiments, the method further includes forming a germanium layer in the trench and above the doped semiconductor layer. In some examples, and after forming the germanium layer, the method further includes forming an optical sensor in the germanium layer. Embodiments of the present invention also relate to semiconductor devices and methods for manufacturing the same.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present invention relate to a semiconductor device and a method for manufacturing the same. Background Art

[0002] The electronics industry has experienced an ever-increasing demand for smaller and faster electronic devices that are simultaneously capable of supporting a greater number of increasingly complex and sophisticated functions. Therefore, there is a continuing trend in the semiconductor industry to manufacture low-cost, high-performance, and low-power integrated circuits (ICs). To date, these goals have been achieved to a large extent by scaling down the size of semiconductor ICs (e.g., minimum component size), thereby improving production efficiency and reducing associated costs. However, this scaling has also caused an increase in the complexity of semiconductor manufacturing processes. Therefore, achieving continued progress in semiconductor ICs and devices requires similar advances in semiconductor manufacturing processes and technologies.

[0003] As an example, semiconductor sensors are widely used in various applications to measure physical, chemical, biological, and environmental parameters. Some specific types of semiconductor sensors include gas sensors, pressure sensors, temperature sensors, and optical image sensors, among others. In optical image sensors, dark current is a major issue that affects device performance and reliability. Dark current is the current that flows in the absence of light and can be more generally described as leakage current present in optical image sensors. In at least some cases, poor interface quality between the various semiconductor layers used in optical image sensors can result in significant dark current.

[0004] Thus, the prior art has not proven to be completely satisfactory in all respects. Summary of the invention

[0005] An embodiment of the present invention provides a method for manufacturing a semiconductor device, comprising: providing a substrate including a pixel area and a logic area; forming a groove in the pixel area; after forming the groove, forming a doped semiconductor layer along the sidewall and bottom of the groove; forming a germanium layer in the groove and above the doped semiconductor layer; and after forming the germanium layer, forming an optical sensor in the germanium layer.

[0006] Another embodiment of the present invention provides a method for manufacturing a semiconductor device, comprising: providing a substrate; forming a germanium layer above the substrate; after forming the germanium layer, forming a doping layer along the bottom of the germanium layer, wherein forming the doping layer comprises performing an ion implantation process on the germanium layer; and after forming the doping layer, forming an optical sensor in the germanium layer.

[0007] Another embodiment of the present invention provides a semiconductor device, comprising: a silicon (Si) substrate, including a pixel area and a logic area adjacent to the pixel area; a germanium (Ge) layer formed in a groove, the groove being located in the silicon substrate arranged in the pixel area, wherein a Ge-Si interface is defined along the sidewall and bottom surface of the groove, and wherein a sensor is arranged in the germanium layer; and a doped region arranged near the Ge-Si interface, wherein the doped region prevents electrons in the silicon substrate from entering the germanium layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Aspects of the present invention will be best understood from the following detailed description when read in conjunction with the accompanying drawings. It should be noted that, in accordance with standard practice in the industry, the various components are not drawn to scale. In fact, the dimensions of the various components may be arbitrarily increased or decreased for clarity of discussion.

[0009] Figure 1 , Fig.10 , Fig.18 , Fig.26 , Fig.33 , Fig.42 , Fig.50 and Fig.58 Various methods of manufacturing semiconductor devices including Ge-based optical sensors according to some embodiments are shown;

[0010] Figure 2 , Figure 3 , Figure 4 , Figure 5 , Figure 6 , Figure 7 , Figure 8 and Fig. 9 is based on Figure 1 a cross-sectional view of an exemplary device manufactured by one or more steps of the method;

[0011] Fig.11 , Fig.12 , Fig.13 , Fig.14 , Fig.15 , Fig.16 and Fig.17 is based on Fig.10 a cross-sectional view of an exemplary device manufactured by one or more steps of the method;

[0012] Fig.19 , Fig. 20 , Fig.21 , Fig. 22 , Fig.23 , Fig.24 and Fig.25 is based on Fig.18 a cross-sectional view of an exemplary device manufactured by one or more steps of the method;

[0013] Fig. 27 , Fig.28 , Fig.29 , Fig.30 , Fig.31 and Fig.32 is based on Fig.26 a cross-sectional view of an exemplary device manufactured by one or more steps of the method;

[0014] Fig.34 , Fig.35 , Fig.36 , Fig.37 , Fig.38 , Fig.39 , Fig.40 and Fig.41 is based on Fig.33 a cross-sectional view of an exemplary device manufactured by one or more steps of the method;

[0015] Fig.43 , Fig.44 , Fig.45 , Fig.46 , Fig.47 , Fig.48 and Fig.49 is based on Fig.42 a cross-sectional view of an exemplary device manufactured by one or more steps of the method;

[0016] Fig.51 , Fig.52 , Fig.53 , Fig.54 , Fig.55 , Fig.56 and Fig.57 is based on Fig.50 a cross-sectional view of an exemplary device fabricated by one or more steps of the method; and

[0017] Fig.59 , Fig.60 , Fig.61 , Fig.62 , Fig.63 and Fig.64 is based on Fig.58 A cross-sectional view of an exemplary device fabricated by one or more steps of a method. DETAILED DESCRIPTION

[0018] The following disclosure provides many different embodiments or examples for realizing the different features of the provided subject matter. Specific examples of components and arrangements are described below to simplify the present invention. Of course, these are only examples and are not intended to be limiting. For example, in the following description, forming a first component above or on a second component may include an embodiment in which the first component and the second component are directly contacted, and may also include an embodiment in which an additional component may be formed between the first component and the second component so that the first component and the second component may not be in direct contact. In addition, the present invention may repeat reference numbers and / or letters in various examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the individual embodiments and / or configurations discussed.

[0019] Additionally, for ease of description, spatially relative terms such as "below," "beneath," "lower," "above," "upper," etc. may be used herein to describe the relationship of one element or component to another element or component as illustrated in the figures. The spatially relative terms are intended to encompass different orientations of the device in use or during operation in addition to the orientation depicted in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein should likewise be interpreted accordingly.

[0020] It should also be noted that the present invention provides embodiments that can be used in any of a variety of semiconductor device types. For example, embodiments of the present invention can be used in planar bulk metal oxide semiconductor field effect transistors (MOSFETs), FinFETs, all-around gate (GAA) transistors, strained semiconductor devices, silicon on insulator (SOI) devices, partially depleted SOI devices, fully depleted SOI devices, charge coupled devices, CMOS sensors, photodiodes, or other devices known in the art. In addition, the embodiments disclosed herein can be used to form P-type and / or N-type devices. Ordinary technicians can recognize other embodiments of semiconductor devices that can benefit from aspects of the present invention.

[0021] Semiconductor sensors are widely used in various applications to measure physical, chemical, biological, and environmental parameters. Some types of semiconductor sensors include gas sensors, pressure sensors, temperature sensors, and optical image sensors, among others. In optical image sensors, dark current is a major issue that affects device performance and reliability. Dark current is the current that flows in the absence of light and can be more generally described as leakage current present in optical image sensors. In at least some cases, poor interface quality between the various semiconductor layers used in optical image sensors can result in significant dark current.

[0022] The present invention generally relates to optical sensors with improved interfaces between various semiconductor layers to reduce dark current and improve device performance. More specifically, various embodiments relate to germanium (Ge) based sensors and manufacturing processes for such sensors. Although not meant to be limited to a specific application, but as an example only, some embodiments of Ge-based sensors disclosed herein may be particularly beneficial for mid-infrared (mid-IR) photonics because of Ge's wide transparent window and its strong nonlinear refractive index. Mid-infrared light, which has a wavelength longer than visible light but shorter than microwaves, has many important applications in remote sensing and communication technologies. For the avoidance of doubt, the Ge-based sensors and processes described herein may also be applicable to other types of applications. In addition, in some embodiments, the Ge-based sensors disclosed herein may include photodiodes (PDs), photodetectors, or other types of Ge-based optical sensors. However, without departing from the scope of the present invention, aspects of the present invention may be equally applicable to other types of optical sensors. As described above, poor interface quality between semiconductor layers may lead to increased dark current. For Ge-based devices, semiconductor interface quality and dark current become more critical, at least because the band gap of Ge is smaller than the band gap of silicon (Si). Therefore, increased dark current (leakage current) in Ge-based optical sensors is a significant issue as it degrades the optical performance and reliability of the device.

[0023] Embodiments of the present invention provide advantages over the prior art, but it is understood that other embodiments may provide different advantages, not all advantages must be discussed herein, and no particular advantage is required by all embodiments. For example, the embodiments discussed herein include structures and methods for passivating interfaces between various semiconductor layers to reduce dark current and improve device performance. In some embodiments, the interface includes an interface between Ge and Si. Therefore, in some examples, the structures and methods disclosed herein are used to passivate the interface between Ge and Si (or "Ge-Si interface"). According to various embodiments, the passivation of the Ge-Si interface can be achieved by doping the Ge-Si interface. For example, the phrase "doped Ge-Si interface" can include introducing a dopant substance at the Ge-Si interface (e.g., across the Ge and silicon layers), in a germanium layer adjacent to the Ge-Si interface, in a silicon layer adjacent to the Ge-Si interface, in a germanium layer spaced a certain distance from the Ge-Si interface, or in a silicon layer spaced a certain distance from the Ge-Si interface. In various embodiments, the doping of the Ge-Si interface can be performed by ion implantation and / or diffusion (e.g., using a gas, liquid or solid dopant source). In some embodiments, the dopant species used to dope the Ge-Si interface may include a P-type material (e.g., Group IIIA (e.g., boron (B), aluminum (Al), gallium (Ga), indium (In), BF2) or Group VIIA material (e.g., fluorine (F), chlorine (Cl), bromine (Br)). By introducing one or more of these dopant species into the Ge-Si interface, the Ge-Si interface can be optimized to substantially prevent electrons in the silicon layer from entering the germanium layer according to one or more methods described herein. As a result, leakage current and dark current problems in Ge-based sensors are significantly alleviated. In at least some examples, the leakage current / dark current of the Ge-based sensor is reduced / improved by about 10%. Those skilled in the art will recognize other benefits and advantages of the methods and devices described herein, and the described embodiments are not meant to be limited beyond what is specifically recited in the appended claims.

[0024] Reference now Figure 1 , a method 100 of manufacturing a semiconductor device 200 including a Ge-based optical sensor according to some embodiments is shown. Figures 2 to 9 Discussion Method 100, Figures 2 to 9A cross-sectional view of a semiconductor device 200 at various stages of fabrication according to one or more steps of method 100 is provided. It should be understood that method 100, as well as methods 1000, 2000, 3000, 4000, 5000, 6000, 7000 (discussed below), include steps that are characteristic of a complementary metal oxide semiconductor (CMOS) technology process flow and, therefore, are only briefly described herein. In addition, additional steps may be performed before, after, and / or during each of methods 100, 1000, 2000, 3000, 4000, 5000, 6000, 7000, and some process steps may be replaced or eliminated without departing from the scope of the present invention.

[0025] In addition, the semiconductor device 200 and the semiconductor devices 1100, 2100, 3100, 4100, 5100, 6100, 7100 (discussed below) may include various other devices and components, including other types of devices, such as planar MOSFETs, FinFETs, GAA transistors, strained semiconductor devices, SOI devices, charge coupled devices, CMOS sensors, photodiodes, other optical devices, bipolar junction transistors, resistors, capacitors, inductors, diodes, fuses, memory devices (such as static random access memory (SRAM) devices), I / O transistors, other logic devices and / or circuits, etc., but are simplified for a better understanding of the inventive concepts of the present invention. In some embodiments, the semiconductor device 200 and the semiconductor devices 1100, 2100, 3100, 4100, 5100, 6100, 7100 (discussed below) include multiple semiconductor devices (e.g., transistors), including P-type transistors, N-type transistors, etc., which can be interconnected. Additionally, it should be noted that the process steps of methods 100, 1000, 2000, 3000, 4000, 5000, 6000, 7000, including any description given with reference to the figures, are exemplary only and are not intended to be limiting beyond what is specifically recited in the appended claims.

[0026] The method 100 begins at block 102 where a substrate is provided. Figure 2In an example of, in an embodiment of box 102, a substrate 202 is provided. In some embodiments, substrate 202 may be a semiconductor substrate such as a silicon substrate. Substrate 202 may include various layers, including a conductive layer or an insulating layer formed on a semiconductor substrate. Depending on design requirements known in the art, substrate 202 may include various doping configurations. Substrate 202 may also include other semiconductors, such as germanium, silicon carbide (SiC), silicon germanium (SiGe), or diamond. Optionally, substrate 202 may include a compound semiconductor and / or an alloy semiconductor. In addition, substrate 202 may optionally include an epitaxial layer (epi layer), may be strained for performance enhancement, may include a silicon on insulator (SOI) structure, and / or have other suitable enhancement components.

[0027] In some embodiments, the substrate 202 also includes a photoelectric region 204 and a logic region 206 adjacent to the photoelectric region 204. For example, the photoelectric region 204 may include one or more photoelectric devices (e.g., such as photodiodes) associated with one or more imaging pixels. Therefore, in some cases, the photoelectric region 204 may be equivalently referred to as a "pixel region". In some embodiments, the logic region 206 may generally include core (logic) transistors and circuits. In at least some examples, the devices and / or circuits within the logic region 206 may include planar MOSFETs, FinFETs, GAA transistors, CMOS transistors, strained semiconductor devices, SOI devices, bipolar junction transistors, resistors, capacitors, inductors, diodes, fuses, memory devices (such as SRAM devices), I / O transistors and / or other logic devices and / or circuits. In some cases, one or more devices within the logic region 206 may be coupled to one or more devices in the photoelectric region 204, for example to jointly define a pixel circuit or other photoelectric circuit.

[0028] The method 100 then proceeds to block 104 where a trench is formed. Figure 3In the example of, in the embodiment of frame 104, a groove 302 is formed in the photovoltaic region 204. In some embodiments, and before forming the groove 302, a hard mask (HM) layer 304 is deposited over the substrate 202. In some examples, the HM layer 304 may include a silicon nitride layer (such as Si3N4), silicon oxynitride, silicon carbide, an oxide layer, or a combination thereof. The HM layer 304 may be deposited by CVD, PVD, ALD, or other suitable processes. In various examples, a photoresist (etching agent) layer may be deposited (e.g., by spin coating) over the HM layer 304. After forming the photoresist layer, the photoresist layer may be exposed and developed to pattern the photoresist layer. In some embodiments, the patterning of the photoresist layer removes portions of the photoresist layer from the photovoltaic region 204 where the grooves will be formed, while other portions of the photoresist layer remain intact. In various embodiments, after patterning the photoresist layer, an etching process (e.g., such as dry etching, wet etching, or a combination thereof) may be performed to etch the HM layer 304 within the photovoltaic region 204 using the patterned photoresist layer as a mask. After etching the HM layer 304, the patterned photoresist layer may be removed, for example, by a solvent, a photoresist stripper, ashing, or other suitable technique. Thereafter, another etching process (e.g., such as dry etching, wet etching, or a combination thereof) may be performed to etch the substrate 202 using the patterned HM layer 304 as a mask to form a trench 302 within the substrate 202. In some embodiments, the trench 302 may have a depth "D" in the range of about 0.5-2 microns, a width "W" in the range of about 0.5-2 microns, and a length "L" (into the page) in the range of about 0.5-2 microns. In some examples, after forming the trench 302, the HM layer 304 may be removed using a wet etching process, a dry etching process, or a combination thereof.

[0029] The method 100 then proceeds to block 106 where an oxide layer is deposited. Figure 4In an example of, in an embodiment of block 106, an oxide layer 402 is deposited over the substrate 202 (e.g., within the photovoltaic region 204 and the logic region 206), including within the trench 302. The oxide layer 402 may include SiO2 or other suitable oxide layers. In various examples, the oxide layer 402 may be deposited by CVD, PVD, ALD, or by other suitable processes. In some cases, the oxide layer 402 is a conformal layer having a substantially uniform thickness “T” over the substrate 202 and within the trench 302. In some optional embodiments, the oxide layer 402 may be formed in the photovoltaic region 204, but not in the logic region 206. In addition, in some cases, the oxide layer 402 may be formed within the trench 302 (e.g., including on the sidewalls and bottom surface of the trench 302), but not in other portions of the photovoltaic region 204 or the logic region 206. In various embodiments, the oxide layer 402 may be used to control the depth (e.g., projection range) of a subsequently performed ion implantation process. For example, the ion implantation depth may decrease as the thickness of the oxide layer 402 increases. In some embodiments, the thickness of the oxide layer 402 may be in the range of approximately 50-5000 angstroms.

[0030] The method 100 then proceeds to block 108 where an ion implantation process is performed. Figure 5In an embodiment of block 108, an implantation masking layer 502 may first be formed over substrate 202 (e.g., within optoelectronic region 204 and logic region 206). In some examples, implantation masking layer 502 may include a silicon nitride layer, an oxide layer, a polysilicon layer, a photoresist layer, or other suitable layer. Implantation masking layer 502 may be deposited by CVD, PVD, ALD, or by other suitable processes. After implantation masking layer 502 is formed, implantation masking layer 502 may be patterned (e.g., using a photolithography and etching process similar to the process described above for patterning HM layer 304) to form an opening in implantation masking layer 502, the opening exposing trench 302. Thereafter, in some embodiments, an ion implantation process 504 is performed in device 200. In some examples, the dopant species used for ion implantation process 504 may include a P-type material (e.g., Group IIIA (e.g., boron (B), aluminum (Al), gallium (Ga), indium (In), BF2) and / or Group VIIA material (e.g., fluorine (F), chlorine (Cl), bromine (Br)). In at least some embodiments, ion implantation process 504 includes multiple ion implantations, wherein the multiple ion implantations implant different dopant species, or wherein the multiple ion implantations implant the same dopant species using different ion implantation parameters (e.g., such as dose and energy). As a result of ion implantation process 504, an implantation region 506 is formed in and along a top surface of substrate 202 that is not covered by implantation masking layer 502 (e.g., a surface of substrate 202 proximate trench 302). In some cases, implantation region 506 is formed in a portion of substrate 202 along a sidewall and bottom surface of trench 302. In embodiments where substrate 202 includes Si, implantation region 506 defines an ion-implanted Si region.

[0031] As described in more detail below, the implanted region 506 will be located near the Ge-Si interface (e.g., after the germanium layer is formed within the trench 302). In some embodiments, the P-type material used for the ion implantation process 504 can be used to change the carrier concentration of the substrate 202 (e.g., such as a Si substrate) so that the Ge-Si interface is optimized and electrons in the Si are substantially blocked from entering the germanium layer, as described below. In some cases, the Group VIIA material used for the ion implantation process 504 can be used to neutralize trapped charge within the substrate 202 (e.g., such as a Si substrate), which may be trapped by defects (e.g., dangling bonds) along the top surface of the substrate 202 and in the area near the top surface of the substrate 202. In particular, the Group VIIIA material can be used to neutralize trapped charge along the surface area of ​​the substrate 202 (e.g., such as a Si substrate) near the germanium layer (or Ge photodiode layer) so that the Ge-Si interface is optimized and electrons in the Si are substantially blocked from entering the germanium layer.

[0032] The method 100 then proceeds to block 110 where the oxide layer is removed and a germanium layer is formed. Figure 6 , in an embodiment of block 110, after forming the implant region 506 (block 108), the oxide layer 402 may be removed from the trench 302 (e.g., from the sidewalls and bottom surface of the trench 302) using a wet etching process, a dry etching process, or a combination thereof. The removal of the oxide layer 402 thus exposes the implant region 506 along the sidewalls and bottom surface of the trench 302. After removing the oxide layer 402 from the trench 302, the implant masking layer 502 may be removed using a wet etching process, a dry etching process, or a combination thereof. It should be noted that after removing the implant masking layer 502, portions of the oxide layer 402 disposed below the implant masking layer 502 may remain on the surface of the device 200 located outside the trench 302. After removing the oxide layer 402 and the implant masking layer 502 (e.g., from the trench 302), and in a further embodiment of block 110, a germanium (Ge) layer 602 is formed within the trench 302 and above the implant region 506 (e.g., including above the implant region 506 along the sidewalls and bottom surface of the trench 302). As shown, in some cases, the germanium layer 602 may overfill the trench 302, resulting in a surface topography 604 of the germanium layer 602. In some embodiments, the germanium layer 602 is grown by ALD, CVD, molecular beam epitaxy (MBE), metal organic CVD (MOCVD), and / or other suitable growth processes. Additionally, in some examples, the germanium layer 602 includes an intrinsic germanium layer. Thus, in some embodiments, the germanium layer 602 may be substantially undoped (e.g., with trace amounts of dopant species present). It should be noted that after removing implant masking layer 502 , the portion of oxide layer 402 remaining on the surface of device 200 (eg, outside trench 302 ) may prevent germanium layer 602 from growing on the remaining oxide layer 402 (eg, outside trench 302 ).

[0033] The method 100 then proceeds to block 112 where a chemical mechanical polishing (CMP) process is performed. Figure 7 302, in an embodiment of block 112, a CMP process is performed after the germanium layer 602 is formed within the trench 302. In various embodiments, the CMP process is used to remove excess portions of the germanium layer 602 (e.g., portions of the germanium layer 602 that extend outside the trench 302 and include the surface topography 604) and planarize the top surface of the device 200. In various embodiments, the CMP process may also remove portions of the oxide layer 402 that remain on the surface of the device 200 (e.g., outside the trench 302). As a result of the CMP process, the top surface of the substrate 202 (e.g., adjacent to the trench 302), the top surface of the germanium layer 602, and the top surfaces of the portions of the implanted regions 506 along the sidewall surfaces of the trench 302 are substantially coplanar (flush) with each other.

[0034] The method 100 then proceeds to block 114 where the optical sensor and logic device are formed. Figure 8 In the example of block 114, an optical sensor 802 is formed in the optoelectronic region 204 within the germanium layer 602, and logic devices 804, 806 are formed in the logic region 206. Referring first to the optoelectronic region 204, and in some embodiments, the optical sensor 802 may include a Ge optical sensor, such as a Ge photodiode (PD). The optical sensor 802 may include an N-type region 808 and a P-type region 810 formed within the germanium layer 602. In some embodiments, the N-type region 808 and the P-type region 810 may be formed by ion implantation, as discussed further below. In various examples, the N-type region 808 may provide a cathode for the optical sensor 802, and the P-type region 810 may provide an anode for the optical sensor 802. Therefore, the P-type region 810, the region of the (intrinsic) germanium layer 602 located between the P-type region 810 and the N-type region 808, and the N-type region 808 may collectively define a PIN Ge PD (or P-NGe PD for short). In some examples, electron-hole pairs are generated when photons of sufficient energy strike the optical sensor 802. In some cases, if the photon absorption occurs in the intrinsic (or depletion) region of the optical sensor 802, the generated electrons are swept toward the cathode (N-type region 808) and the generated holes are swept toward the anode (P-type) region 810), thereby generating a photocurrent.

[0035] In various embodiments, the total current through the optical sensor 802 (Ge PD) is the sum of the dark current and the photocurrent. However, according to some embodiments, the implant region 506 disposed near the Ge-Si interface (e.g., within the substrate 202 near the germanium layer 602) is used to effectively block the current (electrons) from the substrate 202 (e.g., such as Si) from entering the germanium layer 602. As a result, the dark current component of the total current through the optical sensor 802 is reduced, and the performance of the optical sensor 802 is improved. For example, as discussed above, the P-type material within the implant region 506 can be used to change the carrier concentration of the substrate 202, and / or the Group VIIA material within the implant region 506 can be used to neutralize trapped charges within the substrate 202, thereby optimizing the Ge-Si interface.

[0036] Referring now to the logic region 206, and in some embodiments, the logic device 804 may include an N-type MOS (NMOS) transistor, and the logic device 806 may include a P-type MOS (PMOS) transistor. In addition, the logic device 804 may include a gate stack 816, and the logic device 806 may include a gate stack 818. In various examples, each of the gate stacks 816, 818 may include a gate dielectric and a gate electrode located above the gate dielectric, and sidewall spacers may be formed on the sidewalls of the gate stacks 816, 818. In addition, in various examples, the logic device 804 may include an N-type source / drain region 812 formed in the substrate 202, adjacent to the gate stack 816 and located on either side of the gate stack 816, and the logic device 806 may include a P-type source / drain region 814 formed in the substrate 202, adjacent to the gate stack 818 and on either side of the gate stack 818.

[0037] In some embodiments, the gate dielectric of the gate stacks 816, 818 may include an interfacial layer such as a silicon oxide layer (SiO2) or a silicon oxynitride (SiON). In some examples, the gate dielectric of the gate stacks 816, 818 includes a high-k dielectric layer such as hafnium oxide (HfO2). Alternatively, the high-k dielectric layer may include other high-k dielectrics such as TiO2, HfZrO, Ta2O3, HfSiO4, ZrO2, ZrSiO2, LaO, AlO, ZrO, TiO, Ta2O5, Y2O3, SrTiO3 (STO), BaTiO3 (BTO), BaZrO, HfZrO, HfLaO, HfSiO, LaSiO, AlSiO, HfTaO, HfTiO, (Ba, Sr)TiO3 (BST), Al2O3, Si3N4, oxynitride (SiON), combinations thereof, or other suitable materials. As used and described herein, a high-K gate dielectric includes a dielectric material having a high dielectric constant, such as greater than that of thermal silicon oxide (-3.9). In other embodiments, the gate dielectric of the gate stacks 816, 818 may include silicon dioxide or other suitable dielectrics.

[0038] In some embodiments, the gate electrodes of the gate stacks 816, 818 can be deposited as part of a gate-first or gate-last (e.g., replacement gate) process, and the gate electrodes can include a conductive layer such as W, Ti, TiN, TiAl, TiAlN, Ta, TaN, WN, Re, Ir, Ru, Mo, Al, Cu, Co, CoSi, Ni, NiSi, combinations thereof, and / or other suitable compositions. In some examples, the gate electrodes of the gate stacks 816, 818 can include a first metal material for an NMOS transistor (logic device 804) and a second metal material for a PMOS transistor (logic device 806). Thus, the logic devices 804, 806 can include a dual work function metal gate configuration. For example, the first metal material (e.g., for an NMOS transistor) can include a metal having a work function substantially aligned with a work function of a substrate conduction band or at least substantially aligned with a work function of a conduction band of a channel region of the logic device 804. Similarly, the second metal material (e.g., for a PMOS transistor) may include a metal having a work function substantially aligned with the work function of the substrate valence band or at least substantially aligned with the work function of the valence band of the channel region of the logic device 806. Thus, the gate electrodes of the gate stacks 816, 818 may provide gate electrodes for both NMOS transistors and PMOS transistors. In some embodiments, the gate electrodes of the gate stacks 816, 818 may alternatively or additionally include a polysilicon layer. In some embodiments, the sidewall spacers (formed on the sidewalls of the gate stacks 816, 818) may include a dielectric material such as silicon oxide, silicon nitride, silicon carbide, silicon oxynitride, or a combination thereof.

[0039] In various embodiments, the N-type source / drain regions 812 and the P-type source / drain regions 814 include diffused source / drain regions, ion-implanted source / drain regions, epitaxially grown source / drain regions, or a combination thereof. The channel region of the logic device 804 is defined as a region between the N-type source / drain regions 812 below the gate stack 816 and within the substrate 202. Similarly, the channel region of the logic device 806 is defined as a region between the P-type source / drain regions 814 below the gate stack 818 and within the substrate 202. When a voltage greater than the threshold voltage (V tWhen a bias voltage of ) (i.e., on-voltage) is applied to their respective gate electrodes and the bias voltage is simultaneously applied between their respective source and drain regions, current (e.g., transistor drive current) flows between the respective source and drain regions through the respective channel regions. The amount of drive current generated for a given bias voltage (e.g., applied to the gate electrode or between the source and drain regions) is a function of, among other things, the mobility of the material used to form the channel region in each of the logic devices 804, 806. In some examples, the channel region includes silicon (Si) that can be epitaxially grown and / or high-mobility materials such as germanium, as well as any of a variety of compound semiconductors or alloy semiconductors. High-mobility materials include those materials having electron and / or hole mobilities greater than those of silicon (Si), and their intrinsic electron mobility at room temperature (300K) is approximately 1350cm 2 / Vs, the hole mobility is about 480cm 2 / Vs.

[0040] In some embodiments, as described above, N-type region 808 and P-type region 810 may be formed within germanium layer 602 by ion implantation. Similarly, in some embodiments, N-type source / drain region 812 and P-type source / drain region 814 may be formed by ion implantation, also as described above. In particular, in some examples, the ion implantation process used to form N-type source / drain region 812 may simultaneously form N-type region 808 within germanium layer 602. Moreover, in some embodiments, the ion implantation process used to form P-type source / drain region 814 may simultaneously form P-type region 810 within germanium layer 602. In other words, source / drain implantation for logic device 804 (NMOS transistor) may be used to simultaneously form N-type region 808, and source / drain implantation for logic device 806 (PMOS transistor) may be used to simultaneously form P-type region 810. Of course, in some embodiments, separate ion implantation processes may be performed for the N-type source / drain regions 812 and the N-type regions 808, and separate ion implantation processes may be performed for the P-type source / drain regions 814 and the P-type regions 810. In various examples, the dopant material used to dope the N-type source / drain regions 812 and the N-type regions 808 may include phosphorus (P), arsenic (As), antimony (Sb), a combination thereof, or another suitable N-type dopant. In some embodiments, the dopant material used to dope the P-type source / drain regions 814 and the P-type regions 810 may include boron (B), aluminum (Al), gallium (Ga), indium (In), or another suitable P-type dopant.

[0041] It should be noted that while logic device 804 and logic device 806 have been shown and described as including MOS transistors, these examples are not meant to be limiting, and it should be understood that various other device types may likewise be fabricated within logic region 206 without departing from the scope of the present invention. For example, in other embodiments, logic region 206 may alternatively or additionally include FinFETs, GAA transistors, CMOS transistors, strained semiconductor devices, SOI devices, bipolar junction transistors, resistors, capacitors, inductors, diodes, fuses, memory devices (such as SRAM devices), I / O transistors, and / or other devices and / or circuits.

[0042] The method 100 then proceeds to block 116 where contacts are formed and back-end-of-line (BEOL) processing is performed. Fig. 9 In the example of block 116, a dielectric layer 902 is formed over the substrate 202 and over each of the optical sensor 802 in the optoelectronic region 204 and the logic devices 804, 806 in the logic region 206. In various embodiments, the dielectric layer 902 may include a plurality of dielectric layers. In some examples, the dielectric layer 902 may include an interlayer dielectric (ILD) layer, which may include materials such as tetraethyl orthosilicate (TEOS) oxide, undoped silicate glass, or doped silicon oxide (such as borophosphosilicate glass (BPSG), fluorosilicate glass (FSG), phosphosilicate glass (PSG), boron-doped silicate glass (BSG)), and / or other suitable dielectric materials.

[0043] In various examples, dielectric layer 902 may be patterned using a suitable combination of photolithography and etching (e.g., wet etching or dry etching) processes to form openings, and metal layers may be deposited within the openings to provide electrical contacts to underlying substrate components. In some embodiments, the formation of such contacts may be part of BEOL processing. For example, metal layer 904 may be formed to provide electrical contacts to N-type region 808, metal layer 906 may be formed to provide electrical contacts to P-type region 810, metal layer 908 may be formed to provide electrical contacts to N-type source / drain region 812, metal layer 910 may be formed to provide electrical contacts to the gate electrode of gate stack 816, metal layer 912 may be formed to provide electrical contacts to P-type source / drain region 814, and metal layer 914 may be formed to provide electrical contacts to the gate electrode of gate stack 818. In some examples, the metal layers 904 , 906 , 908 , 910 , 912 , 914 may include W, Cu, Co, Ru, Al, Rh, Mo, Ta, Ti, TiN, TaN, WN, silicide, combinations thereof, or another suitable conductive material.

[0044] After forming contacts to underlying substrate components (e.g., including metal layers 904, 906, 908, 910, 912, 914), further BEOL processing may be performed. For example, various vias / metal lines and multi-layer interconnect components (e.g., metal layers and interlayer dielectrics, including portions of dielectric layer 902) may be formed over substrate 202 and may be configured to connect various underlying substrate components to form functional circuits (e.g., such as optoelectronic circuits), which may include one or more optical sensors 802 from optoelectronic region 204 and one or more logic devices 804, 806 from logic region 206. Fig. 9 As shown in the example of , the multi-layer interconnect (MLI) region 915 may include vertical interconnects (such as vias or contacts) and horizontal interconnects (such as metal lines). Various interconnect components may be made of various conductive materials, including copper, tungsten and / or silicide. In one example, a damascene and / or dual damascene process is used to form a copper-related multi-layer interconnect structure. In some embodiments, portion 916 of the MLI region 915 may be formed to provide electrical contact to metal layer 904 in contact with N-type region 808, portion 918 of the MLI region 915 may be formed to provide electrical contact to metal layer 906 in contact with P-type region 810, portion 920 / 924 of the MLI region 915 may be formed to provide electrical contact to metal layer 908 in contact with N-type source / drain region 812, portion 922 of the MLI region 915 may be formed to provide electrical contact to metal layer 910 in contact with a gate electrode of gate stack 816, portion 926 / 930 of the MLI region 915 may be formed to provide electrical contact to metal layer 912 in contact with P-type source / drain region 814, and portion 928 of the MLI region 915 may be formed to provide electrical contact to metal layer 914 in contact with a gate electrode of gate stack 818.

[0045] Reference now Fig.10 , a method 1000 of manufacturing a semiconductor device 1100 including a Ge-based optical sensor according to some embodiments is shown. Figures 11 to 17 Discussion Method 1000, Figures 11 to 17 Cross-sectional views of a semiconductor device 1100 are provided at various stages of fabrication according to one or more steps of method 1000. Note that various aspects of method 1000 may be similar to method 100 discussed above. Therefore, for clarity of discussion, only certain aspects of method 1000 are briefly discussed.

[0046] Method 1000 begins at block 1002, where a substrate is provided. Fig.11In an example of block 1002, a substrate 1202 is provided. In various embodiments, substrate 1202 may be a semiconductor substrate such as a silicon substrate. More generally, substrate 1202 may be substantially the same as substrate 202 and may include one or more layers or components, as described above with reference to Figure 2 as described.

[0047] Instead of including separate optoelectronic regions and logic regions, as discussed above with reference to method 100, and in some embodiments, substrate 1202 may include a dedicated optoelectronic substrate that includes one or more optoelectronic devices (e.g., such as photodiodes) associated with one or more imaging pixels. Of course, in at least some embodiments, substrate 1202 may also include one or more logic devices and / or circuits. In some embodiments, and as described in more detail below, a separate device substrate (e.g., including core (logic) transistors and circuits and other devices) may be bonded to the optoelectronic substrate at a later stage of processing. In at least some examples, the devices and / or circuits within the separate device substrate may include planar MOSFETs, FinFETs, GAA transistors, CMOS transistors, strained semiconductor devices, SOI devices, bipolar junction transistors, resistors, capacitors, inductors, diodes, fuses, memory devices such as SRAM devices, I / O transistors, and / or other logic devices and / or circuits. In some embodiments, the separate device substrate may include an application specific integrated circuit (ASIC). In some cases, after the bonding process, one or more devices within the optoelectronic substrate may be coupled to one or more devices in the separate device substrate, for example to jointly define a pixel circuit or other optoelectronic circuit.

[0048] The method 1000 then proceeds to block 1004 where an oxide layer is deposited. Fig.12 In an example of, in an embodiment of box 1004, an oxide layer 1402 is deposited over substrate 1202. Oxide layer 1402 may include SiO2 or other suitable oxide layers. In various examples, oxide layer 1402 may be deposited by CVD, PVD, ALD, or by other suitable processes. In some cases, oxide layer 1402 is a conformal layer having a substantially uniform thickness over substrate 1202. In various embodiments, and as discussed above with respect to oxide layer 402, oxide layer 1402 may be used to control the depth (e.g., projected range) of a subsequently performed ion implantation process. For example, as the thickness of oxide layer 1402 increases, the ion implantation depth may decrease. In some embodiments, and as with oxide layer 402, oxide layer 1402 may have a thickness "T" in the range of approximately 50-5000 angstroms.

[0049] The method 1000 then proceeds to block 1006 where an ion implantation process is performed. Fig.13 In an example of, in an embodiment of block 1006, an ion implantation process 1504 is performed on the device 1100. In some examples, the dopant species used for the ion implantation process 1504 may include a P-type material (e.g., a Group IIIA material (e.g., boron (B), aluminum (Al), gallium (Ga), indium (In), BF2) and / or a Group VIIA material (e.g., fluorine (F), chlorine (Cl), bromine (Br)). In at least some embodiments, the ion implantation process 1504 includes multiple ion implantations, wherein the multiple ion implantations implant different dopant species, or wherein the multiple ion implantations implant the same dopant species using different ion implantation parameters (e.g., such as dose and energy). As a result of the ion implantation process 1504, an implantation region 1506 is formed in and along the top surface of the substrate 1202. In an embodiment where the substrate 1202 includes Si, the implantation region 1506 defines an ion implanted Si region.

[0050] After a germanium layer is subsequently formed over the implanted region 506, as described below, the implanted region 506 will be located near the Ge-Si interface. In some embodiments, the P-type material used for the ion implantation process 1504 can be used to change the carrier concentration of the substrate 1202 (e.g., such as a Si substrate) so that the Ge-Si interface is optimized and electrons in the Si are substantially blocked from entering the germanium layer. In some cases, the Group VIIA material used for the ion implantation process 1504 can be used to neutralize trapped charge within the substrate 1202 (e.g., such as a Si substrate), which may be trapped by defects (e.g., dangling bonds) in the region along the top surface of the substrate 1202 and near the top surface of the substrate 1202. In particular, the Group VIIIA material can be used to neutralize trapped charge along the surface region of the substrate 1202 (e.g., such as a Si substrate) near the germanium layer (or Ge photodiode layer) so that the Ge-Si interface is optimized and electrons in the Si are substantially blocked from entering the germanium layer.

[0051] The method 1000 then proceeds to block 1008 where the oxide layer is removed and a germanium layer is formed. Fig.14In an example of, in an embodiment of block 1008, after forming the implant region 1506, the oxide layer 1402 is removed to expose the implant region 1506. In some embodiments, the oxide layer 1402 can be removed using a wet etching process, a dry etching process, or a combination thereof. After removing the oxide layer 1402, and in a further embodiment of block 1008, a germanium (Ge) layer 1602 is formed over the substrate 1202 (e.g., including over the implant region 1506). In some embodiments, the germanium layer 1602 is formed by ALD, CVD, molecular beam epitaxy (MBE), metal organic CVD (MOCVD), and / or other suitable growth processes. In addition, in some examples, the germanium layer 1602 includes an intrinsic germanium layer. Therefore, in some embodiments, the germanium layer 1602 can be substantially undoped (e.g., there is a trace amount of dopant species). In some embodiments, a CMP process can be optionally performed to planarize and / or thin the germanium layer 1602.

[0052] Method 1000 then proceeds to block 1010 where an optical sensor is formed. Fig.15In the example of block 1010, one or more optical sensors 1802 are formed within the germanium layer 1602. In some embodiments, the one or more optical sensors 1802 may include a Ge optical sensor, such as a Ge photodiode (PD). Each of the one or more optical sensors 1802 may include an N-type region 1808 and a P-type region 1810 formed within the germanium layer 1602. In some embodiments, the N-type region 1808 and the P-type region 1810 may be formed by ion implantation. In various examples, the dopant material for doping the N-type region 1808 may include phosphorus (P), arsenic (As), antimony (Sb), a combination thereof, or another suitable N-type dopant. In some embodiments, the dopant material for doping the P-type region 1810 may include boron (B), aluminum (Al), gallium (Ga), indium (In), or another suitable P-type dopant. In various examples, the N-type region 1808 may provide a cathode for the corresponding optical sensor 1802, and the P-type region 1810 may provide an anode for the corresponding optical sensor 1802. Thus, for each optical sensor 1802, the P-type region 1810, the region of the (intrinsic) germanium layer 1602 between the P-type region 1810 and the N-type region 1808, and the N-type region 1808 may collectively define a PIN Ge PD (or PN Ge PD for short). In some examples, when photons of sufficient energy strike one or more optical sensors 1802, electron-hole pairs are generated. In some cases, if photon absorption occurs in the intrinsic (or depletion) region of one or more optical sensors 1802, the generated electrons are swept toward the cathode (N-type region 1808), and the generated holes are swept toward the anode (P-type region 1810), thereby generating a photocurrent.

[0053] As previously discussed, the total current through an optical sensor (e.g., such as one or more optical sensors 1802) is the sum of the dark current and the photocurrent. However, according to some embodiments, an implant region 1506 disposed near the Ge-Si interface (e.g., within the substrate 1202 near the germanium layer 1602) is used to effectively block current (electrons) from the substrate 1202 (e.g., such as Si) from entering the germanium layer 1602. As a result, the dark current component of the total current through the one or more optical sensors 1802 is reduced, and the performance of the one or more optical sensors 1802 is improved. For example, as discussed above, a P-type material within the implant region 1506 can be used to change the carrier concentration of the substrate 1202, and / or a Group VIIA material within the implant region 1506 can be used to neutralize trapped charges within the substrate 1202, thereby optimizing the Ge-Si interface.

[0054] The method 1000 then proceeds to block 1012 where contacts are formed and BEOL processing is performed. Fig.16In an example of a block 1012 embodiment, a dielectric layer 1902 is formed over the substrate 1202 and over the one or more optical sensors 1802. In various embodiments, the dielectric layer 1902 may include a plurality of dielectric layers. In some examples, the dielectric layer 1902 may include an ILD layer that may include a material such as TEOS oxide, undoped silicate glass, or doped silicon oxide such as BPSG, FSG, PSG, BSG, and / or other suitable dielectric materials.

[0055] In various examples, dielectric layer 1902 can be patterned using a suitable combination of photolithography and etching (e.g., wet etching or dry etching) processes to form openings, and metal layers can be deposited within the openings to provide electrical contacts to underlying substrate components. In some embodiments, the formation of such contacts can be part of BEOL processing. For example, metal layer 1904 can be formed to provide electrical contacts to N-type region 1808, and metal layer 1906 can be formed to provide electrical contacts to P-type region 1810. In some examples, metal layers 1904, 1906 can include W, Cu, Co, Ru, Al, Rh, Mo, Ta, Ti, TiN, TaN, WN, silicide, combinations thereof, or another suitable conductive material.

[0056] After contacts are formed to underlying substrate components (e.g., including metal layers 1904, 1906), further BEOL processing may be performed. For example, various vias / metal lines and multi-layer interconnect components (e.g., metal layers and interlayer dielectrics, including portions of dielectric layer 1902) may be formed over substrate 1202 and may be configured to connect various underlying substrate components (to each other and to one or more devices on a separate device substrate that is subsequently bonded to substrate 1202) to form functional circuits (e.g., such as optoelectronic circuits), which may include one or more optical sensors 1802 and, in some cases, one or more devices (e.g., such as logic devices or other devices) from a separate device substrate. Fig.16 As shown in the example of , the multi-layer interconnect (MLI) region 1915 may include vertical interconnects (such as vias or contacts) and horizontal interconnects (such as metal lines). The various interconnect components may be made of various conductive materials, including copper, tungsten and / or silicide. In one example, a copper-related multi-layer interconnect structure is formed using a damascene and / or dual damascene process. In some embodiments, a portion 1916 of the MLI region 1915 may be formed to provide electrical contact to the metal layer 1904 in contact with the N-type region 1808, and a portion 1918 of the MLI region 1915 may be formed to provide electrical contact to the metal layer 1906 in contact with the P-type region 1810.

[0057] The method 1000 then proceeds to block 1014 where the optoelectronic substrate is bonded to a separate device substrate. Fig.17 In an example of, in an embodiment of box 1014, the device 1100 (including the optoelectronic substrate) is bonded to a separate device substrate 1950. As previously described, the separate device substrate 1950 may include core (logic) transistors and circuits as well as other devices. In at least some examples, the devices and / or circuits within the separate device substrate 1950 may include planar MOSFETs, FinFETs, GAA transistors, CMOS transistors, strained semiconductor devices, SOI devices, bipolar junction transistors, resistors, capacitors, inductors, diodes, fuses, memory devices (such as SRAM devices), I / O transistors, and / or other logic devices and / or circuits. In some embodiments, the separate device substrate 1950 may include an application specific integrated circuit (ASIC). In some cases, for example, after the bonding process of box 1014, one or more devices (device 1100) within the optoelectronic substrate may be coupled to one or more devices in the separate device substrate 1950 to jointly define a pixel circuit or other optoelectronic circuit. In some examples, various structures and / or methods can be used to bond device 1100 (including optoelectronic substrates) to a separate device substrate 1950, such as copper-to-copper hybrid bonding, interposers, through silicon vias (TSVs), redistribution layers (RDLs), bond pads, copper microbumps and pillars, wire bonding, flip chips, wafer level packaging (WLP), or other suitable wafer bonding techniques, including 2.5D and 3D integrated circuit (IC) packaging techniques.

[0058] Reference now Fig.18 , a method 2000 of manufacturing a semiconductor device 2100 including a Ge-based optical sensor according to some embodiments is shown. Figures 19 to 25 Discussion Methods 2000, Figures 19 to 25 A cross-sectional view of a semiconductor device 2100 at various stages of fabrication according to one or more steps of method 2000 is provided. Note that various aspects of method 2000 may be similar to method 100 discussed above. Therefore, for clarity of discussion, only certain aspects of method 2000 are briefly discussed. Generally, as discussed below, while method 100 forms a doped silicon region in a trench using ion implantation, in some embodiments, method 2000 forms a doped silicon region in a trench by doped epitaxial growth of a silicon layer.

[0059] Method 2000 begins at block 2002, where a substrate is provided. Fig.19In an example of block 2002, a substrate 2202 is provided. In some embodiments, substrate 2202 may be a semiconductor substrate such as a silicon substrate. More generally, substrate 2202 may be substantially the same as substrate 202 and may include one or more layers or components, as described above with reference to Figure 2 as described.

[0060] As with device 200 discussed above, substrate 2202 also includes an optoelectronic region 2204 (pixel region) and a logic region 2206. In some embodiments, optoelectronic region 2204 and logic region 2206 include various components and / or devices and circuits discussed above with reference to optoelectronic region 204 and logic region 206 of device 200. Additionally, in some embodiments, one or more devices within logic region 2206 may be coupled to one or more devices in optoelectronic region 2204, for example, to collectively define a pixel circuit or other optoelectronic circuit.

[0061] The method 2000 then proceeds to block 2004 where a trench is formed. Fig. 20 In the example of the embodiment of the block 2004, a trench 2302 is formed in the photovoltaic region 2204. In some embodiments, and before forming the trench 2302, a hard mask (HM) layer 2304 is deposited over the substrate 2202. The HM layer 2304 may include a silicon nitride layer, such as Si3N4, silicon oxynitride, silicon carbide, an oxide layer, or a combination thereof. In various examples, as described above with reference to the device 200, the HM layer 2304 may first be patterned using a photolithography and etching process. Thereafter, using the patterned HM layer 2304 as a mask, an etching process (e.g., such as dry etching, wet etching, or a combination thereof) may be performed to etch the substrate 2202 to form the trench 2302 in the substrate 2202.

[0062] The method 2000 then proceeds to block 2006 where a doped silicon layer is formed. Fig.21In an example of, in an embodiment of box 2006, a doped silicon (Si) layer 2506 is formed within the trench 2302 (e.g., including along the sidewalls and bottom surface of the trench 2302). In some examples, the doped silicon layer 2506 may include an epitaxially grown silicon layer. More generally, in some embodiments, the doped silicon layer 2506 is formed by ALD, CVD, molecular beam epitaxy (MBE), metal organic CVD (MOCVD), and / or other suitable growth processes. In order to provide doping of the doped silicon layer 2506, a suitable dopant substance may be introduced into the process chamber during the growth of the silicon layer (e.g., such as in an in-situ doping process) to provide the doped silicon layer 2506. In some examples, the dopant substance may include a P-type material (e.g., a Group IIIA material (e.g., boron (B), aluminum (Al), gallium (Ga), indium (In), BF2) and / or a Group VIIA material (e.g., fluorine (F), chlorine (Cl), bromine (Br)).

[0063] As described in more detail below, the doped silicon layer 2506 will be located near the Ge-Si interface (e.g., after the germanium layer is formed within the trench 2302). In some embodiments, the P-type material used to form the doped silicon layer 2506 can be used to change the carrier concentration of the substrate 2202 (e.g., such as a Si substrate) so that the Ge-Si interface is optimized and electrons in the Si are substantially blocked from entering the germanium layer. In some cases, the Group VIIA material used to form the doped silicon layer 2506 can be used to neutralize trapped charge within the substrate 2202 (e.g., such as a Si substrate), which may be trapped by defects (e.g., dangling bonds) in the area along the top surface of the substrate 2202 and near the top surface of the substrate 2202. In particular, the Group VIIIA material can be used to neutralize trapped charge along the surface area of ​​the substrate 2202 (e.g., such as a Si substrate) near the germanium layer (or Ge photodiode layer) so that the Ge-Si interface is optimized and electrons in the Si are substantially blocked from entering the germanium layer.

[0064] The method 2000 then proceeds to block 2008 where a germanium layer is formed. Fig. 22In the example of the embodiment of box 2008, after the doped silicon layer 2506 is formed along the sidewalls and bottom surface of the groove 2302, a germanium (Ge) layer 2602 is formed in the groove 2302 and above the implanted region doped silicon layer 2506. As shown in the figure, in some cases, the germanium layer 2602 can overfill the groove 2302, resulting in a surface morphology 2604 of the germanium layer 2602. In some embodiments, the germanium layer 2602 is formed by ALD, CVD, molecular beam epitaxy (MBE), metal organic CVD (MOCVD) and / or other suitable growth processes. In addition, in some examples, the germanium layer 2602 includes an intrinsic germanium layer. Therefore, in some embodiments, the germanium layer 2602 can be substantially undoped (e.g., there is a trace amount of dopant species). It should be noted that the portion of the HM layer 2304 that remains on the surface of the device 2100 (eg, outside the trench 2302 ) may prevent the growth of the germanium layer 2602 on the HM layer 2304 (eg, outside the trench 2302 ).

[0065] The method 2000 then proceeds to block 2010 where a chemical mechanical polishing (CMP) process is performed. Fig.23 In the example of FIG. 2010, a CMP process is performed after forming the germanium layer 2602 in an embodiment of block 2010. In various embodiments, the CMP process is used to remove excess portions of the germanium layer 2602 (e.g., portions of the germanium layer 2602 that are outside the trench 2302 and include the surface topography 2604) and planarize the top surface of the device 2100. In some embodiments, the CMP process of block 2010 may also be used to remove the HM layer 2304, as shown. As a result of the CMP process, the top surface of the substrate 2202 (e.g., adjacent to the trench 2302), the top surface of the germanium layer 2602, and the top surface of the portion of the doped silicon layer 2506 along the sidewall surface of the trench 2302 are substantially coplanar (flush) with each other.

[0066] The method 2000 then proceeds to block 2012 where an optical sensor is formed. Fig.24In the example of block 2012, an optical sensor 2802 is formed in the photoelectric region 2204 within the germanium layer 2602. In some embodiments, the optical sensor 2802 may include a Ge optical sensor, such as a Ge photodiode (PD). The optical sensor 2802 may include an N-type region 2808 and a P-type region 2810 formed within the germanium layer 2602. In some embodiments, the N-type region 2808 and the P-type region 2810 may be formed by ion implantation. In various examples, the dopant material for doping the N-type region 2808 may include phosphorus (P), arsenic (As), antimony (Sb), a combination thereof, or another suitable N-type dopant. In some embodiments, the dopant material for doping the P-type region 2810 may include boron (B), aluminum (Al), gallium (Ga), indium (In), or another suitable P-type dopant. In various examples, the N-type region 2808 may provide a cathode for the optical sensor 2802, and the P-type region 2810 may provide an anode for the optical sensor 2802. Thus, the P-type region 2810, the region of the (intrinsic) germanium layer 2602 between the P-type region 2810 and the N-type region 2808, and the N-type region 2808 may collectively define a PIN Ge PD (or PN Ge PD for short). In some examples, when photons of sufficient energy strike the optical sensor 2802, electron-hole pairs are generated. In some cases, if photon absorption occurs in the intrinsic (or depletion) region of the optical sensor 2802, the generated electrons are swept toward the cathode (N-type region 2808), and the generated holes are swept toward the anode (P-type region 2810), thereby generating a photocurrent.

[0067] In various embodiments, the total current through the optical sensor 2802 (Ge PD) is the sum of the dark current and the photocurrent. However, according to some embodiments, the doped silicon layer 2506 disposed near the Ge-Si interface (e.g., near the germanium layer 2602) is used to effectively block the current (electrons) from the substrate 2202 (e.g., such as Si) from entering the germanium layer 2602. As a result, the dark current component of the total current through the optical sensor 2802 is reduced, and the performance of the optical sensor 2802 is improved. For example, as discussed above, the P-type material within the doped silicon layer 2506 can be used to change the carrier concentration of the substrate 2202, and / or the Group VIIA material within the doped silicon layer 2506 can be used to neutralize trapped charges within the substrate 2202, thereby optimizing the Ge-Si interface.

[0068] The method 2000 then proceeds to block 2014 where a logic device is formed, contacts are formed, and BEOL processing is performed. Fig.25In the example of block 2014, logic devices 2804, 2806 are formed within logic region 2206. In some embodiments, logic device 2804 may include an NMOS transistor, and logic device 2806 may include a PMOS transistor. In addition, logic device 2804 may include a gate stack 2816, and logic device 2806 may include a gate stack 2818. In various examples, each of gate stacks 2816, 2818 may include a gate dielectric and a gate electrode located above the gate dielectric, and sidewall spacers may be formed on sidewalls of gate stacks 2816, 2818. Additionally, in various examples, the logic device 2804 may include an N-type source / drain region 2812 formed within the substrate 2202, adjacent to the gate stack 2816, and located on either side of the gate stack 2816, and the logic device 2806 may include a P-type source / drain region 2814 formed within the substrate 2202, adjacent to the gate stack 2818, and located on either side of the gate stack 2818.

[0069] In various embodiments, the gate dielectrics of the gate stacks 2816, 2818 may be the same as those described above with reference to Figure 8 The gate dielectrics of the gate stacks 816, 818 described above are substantially the same. In some embodiments, the gate electrodes of the gate stacks 2816, 2818 may be the same as those described above with reference to Figure 8 The gate electrodes of the gate stacks 816, 818 described above are substantially the same. In some examples, the sidewall spacers formed on the sidewalls of the gate stacks 2816, 2818 can be the same as those described above with reference to Figure 8 The sidewall spacers formed on the sidewalls of the gate stacks 816, 818 are substantially the same as described above. In addition, in some embodiments, the N-type source / drain regions 2812 and the P-type source / drain regions 2814 may be the same as described above with reference to Figure 8 The depicted N-type source / drain regions 812 and P-type source / drain regions 814 are substantially the same. The channel region of the logic device 2804 is defined as a region between the N-type source / drain regions 2812 below the gate stack 2816 and within the substrate 2202. Similarly, the channel region of the logic device 2806 is defined as a region between the P-type source / drain regions 2814 below the gate stack 2818 and within the substrate 2202. In some examples, the channel region includes silicon (Si) and / or a high mobility material such as germanium, which can be epitaxially grown, and any of a variety of compound semiconductors or alloy semiconductors.

[0070] In at least some examples, the ion implantation process used to form the N-type source / drain region 2812 can simultaneously form the N-type region 2808 in the germanium layer 2602. Moreover, in some embodiments, the ion implantation process used to form the P-type source / drain region 2814 can simultaneously form the P-type region 2810 in the germanium layer 2602. In some instances, separate ion implantation processes can be performed for the N-type source / drain region 2812 and the N-type region 2808, and separate ion implantation processes can be performed for the P-type source / drain region 2814 and the P-type region 2810. In various examples, the dopant material used to dope the N-type source / drain region 2812 can include phosphorus (P), arsenic (As), antimony (Sb), combinations thereof, or another suitable N-type dopant. In some embodiments, the dopant material used to dope the P-type source / drain region 2814 can include boron (B), aluminum (Al), gallium (Ga), indium (In), or another suitable P-type dopant.

[0071] It should be noted that while logic device 2804 and logic device 2806 have been shown and described as including MOS transistors, these examples are not meant to be limiting, and it should be understood that various other device types may also be fabricated within logic region 2206 without departing from the scope of the present invention. For example, in other embodiments, logic region 2206 may alternatively or additionally include FinFETs, GAA transistors, CMOS transistors, strained semiconductor devices, SOI devices, bipolar junction transistors, resistors, capacitors, inductors, diodes, fuses, memory devices (such as SRAM devices), I / O transistors, and / or other devices and / or circuits.

[0072] In a further embodiment of block 2014, and still with reference to Fig.25 In the example of FIG. 2 , dielectric layer 2902 is formed over substrate 2202 and over each of optical sensor 2802 in optoelectronic region 2204 and logic devices 2804, 2806 in logic region 2206. In various embodiments, dielectric layer 2902 may be formed as described above with reference to FIG. Fig. 9 The dielectric layer 902 depicted is substantially the same.

[0073] Like dielectric layer 902, dielectric layer 2902 may be patterned to form openings within which metal layers may be deposited to provide electrical contacts to underlying substrate components. For example, metal layer 2904 may be formed to provide electrical contacts to N-type region 2808, metal layer 2906 may be formed to provide electrical contacts to P-type region 2810, metal layer 2908 may be formed to provide electrical contacts to N-type source / drain region 2812, metal layer 2910 may be formed to provide electrical contacts to the gate electrode of gate stack 2816, metal layer 2912 may be formed to provide electrical contacts to P-type source / drain region 2814, and metal layer 2914 may be formed to provide electrical contacts to the gate electrode of gate stack 2818. In some examples, the metal layers 2904, 2906, 2908, 2910, 2912, 2914 may include W, Cu, Co, Ru, Al, Rh, Mo, Ta, Ti, TiN, TaN, WN, silicide, combinations thereof, or another suitable conductive material.

[0074] After forming contacts to underlying substrate components (e.g., including metal layers 2904, 2906, 2908, 2910, 2912, 2914), further BEOL processing may be performed. For example, various vias / metal lines and multi-layer interconnect components (e.g., metal layers and interlayer dielectrics, including portions of dielectric layer 2902) may be formed over substrate 2202 and may be configured to connect various underlying substrate components to form functional circuits (e.g., such as optoelectronic circuits), which may include one or more optical sensors 2802 from optoelectronic region 2204 and one or more logic devices 2804, 2806 from logic region 2206. Fig.25As shown, a multi-layer interconnect (MLI) region 2915 may include vertical interconnects (such as vias or contacts) and horizontal interconnects (such as metal lines). Various interconnect components may be made of various conductive materials, including copper, tungsten and / or silicide. In one example, a copper-related multi-layer interconnect structure is formed using a damascene and / or dual damascene process. In some embodiments, a portion 2916 of the MLI region 2915 may be formed to provide electrical contact to a metal layer 2904 in contact with an N-type region 2808, a portion 2918 of the MLI region 2915 may be formed to provide electrical contact to a metal layer 2906 in contact with a P-type region 2810, a portion 2920 / 2924 of the MLI region 2915 may be formed to provide electrical contact to a metal layer 2908 in contact with an N-type source / drain region 2812, and a portion 2920 / 2924 of the MLI region 2915 may be formed to provide electrical contact to a metal layer 2908 in contact with an N-type source / drain region 2812. Portion 2922 of the I region 2915 may be formed to provide an electrical contact to the metal layer 2910 in contact with the gate electrode of the gate stack 2816, portion 2926 / 2930 of the MLI region 2915 may be formed to provide an electrical contact to the metal layer 2912 in contact with the P-type source / drain region 2814, and portion 2928 of the MLI region 2915 may be formed to provide an electrical contact to the metal layer 2914 in contact with the gate electrode of the gate stack 2818.

[0075] Reference now Fig.26 , a method 3000 of manufacturing a semiconductor device 3100 including a Ge-based optical sensor according to some embodiments is shown. Figures 27 to 32 Discussion Method 3000, Figures 27 to 32 A cross-sectional view of a semiconductor device 3100 at various stages of fabrication according to one or more steps of method 3000 is provided. Note that various aspects of method 3000 may be similar to methods 1000 and 2000 discussed above. Therefore, for clarity of discussion, only certain aspects of methods 1000 and 2000 are briefly discussed. Generally, in some embodiments, method 3000 forms a doped Si region by doped epitaxial growth of a silicon layer (similar to method 2000), and method 3000 provides a dedicated optoelectronic substrate bonded to a separate device substrate (similar to method 1000).

[0076] Method 3000 begins at block 3002, where a substrate is provided. Fig. 27 In the example of block 3002, a substrate 3202 is provided. In various embodiments, substrate 3202 may be a semiconductor substrate such as a silicon substrate. More generally, substrate 3202 may be substantially the same as substrate 202 and may include one or more layers or components, as described above with reference to Figure 2 As described.

[0077] As with device 1100 discussed above, substrate 3202 of device 3100 may include a dedicated optoelectronic substrate that includes one or more optoelectronic devices (e.g., such as photodiodes) associated with one or more imaging pixels. Of course, in at least some embodiments, substrate 3202 may also include one or more logic devices and / or circuits. In some embodiments, and as described in more detail below, a separate device substrate (e.g., including core (logic) transistors and circuits as well as other devices) may be bonded to the optoelectronic substrate at a later stage of processing.

[0078] The method 3000 then proceeds to block 3004 where a doped silicon layer is formed. Fig.28 In an example of, in an embodiment of box 3004, a doped silicon (Si) layer 3506 is formed over substrate 3202. In some examples, the doped silicon layer 3506 may include an epitaxially grown silicon layer. More generally, in some embodiments, the doped silicon layer 3506 is formed by ALD, CVD, MBE, MOCVD, and / or other suitable growth processes. In order to provide doping of the doped silicon layer 3506, a suitable dopant substance may be introduced into a process chamber during the growth of the silicon layer (e.g., such as in an in-situ doping process) to provide the doped silicon layer 3506. In some examples, the dopant substance may include a P-type material (e.g., Group IIIA (e.g., boron (B), aluminum (Al), gallium (Ga), indium (In), BF2) and / or Group VIIA material (e.g., fluorine (F), chlorine (Cl), bromine (Br)).

[0079] After the subsequent formation of the germanium layer, as described below, the doped silicon layer 3506 will be located near the Ge-Si interface. In some embodiments, the P-type material used to form the doped silicon layer 3506 can be used to change the carrier concentration of the substrate 3202 (e.g., such as a Si substrate) so as to optimize the Ge-Si interface and substantially prevent electrons in the Si from entering the germanium layer. In some cases, the VIIA group material used to form the doped silicon layer 3506 can be used to neutralize trapped charge within the substrate 3202 (e.g., such as a Si substrate), which can be trapped by defects (e.g., dangling bonds) in the region along the top surface of the substrate 3202 and near the top surface of the substrate 3202. In particular, the VIIIA group material can be used to neutralize trapped charge along the surface region of the substrate 3202 (e.g., such as a Si substrate) near the germanium layer (or Ge photodiode layer) so as to optimize the Ge-Si interface and substantially prevent electrons in the Si from entering the germanium layer.

[0080] The method 3000 then proceeds to block 3006 where a germanium layer is formed. Fig.29In the example of block 3006, after forming the doped silicon layer 3506 over the substrate 3202, a germanium (Ge) layer 3602 is formed over the doped silicon layer 3506. In some embodiments, the germanium layer 3602 is formed by ALD, CVD, MBE, MOCVD, and / or other suitable growth processes. In addition, in some examples, the germanium layer 3602 includes an intrinsic germanium layer. Therefore, in some embodiments, the germanium layer 3602 can be substantially undoped (e.g., there is a trace amount of dopant species). In some embodiments, a CMP process can be optionally performed to planarize and / or thin the germanium layer 3602.

[0081] The method 3000 then proceeds to block 3008 where an optical sensor is formed. Fig.30 In the example of block 3008, one or more optical sensors 3802 are formed within the germanium layer 3602. In some embodiments, the one or more optical sensors 3802 may include a Ge optical sensor, such as a Ge photodiode (PD). Each of the one or more optical sensors 3802 may include an N-type region 3808 and a P-type region 3810 formed within the germanium layer 3602. In some embodiments, the N-type region 3808 and the P-type region 3810 may be formed by ion implantation. In various examples, the dopant material for doping the N-type region 3808 may include phosphorus (P), arsenic (As), antimony (Sb), a combination thereof, or another suitable N-type dopant. In some embodiments, the dopant material for doping the P-type region 3810 may include boron (B), aluminum (Al), gallium (Ga), indium (In), or another suitable P-type dopant. In various examples, the N-type region 3808 may provide a cathode for the corresponding optical sensor 3802, and the P-type region 3810 may provide an anode for the corresponding optical sensor 3802. Thus, for each optical sensor 3802, the P-type region 3810, the region of the (intrinsic) germanium layer 3602 between the P-type region 3810 and the N-type region 3808, and the N-type region 3808 may collectively define a PIN Ge PD (or PN Ge PD for short). In some examples, when photons of sufficient energy strike one or more optical sensors 3802, electron-hole pairs are generated. In some cases, if photon absorption occurs in the intrinsic (or depletion) region of one or more optical sensors 3802, the generated electrons are swept toward the cathode (N-type region 3808) and the generated holes are swept toward the anode (P-type region 3810), thereby generating a photocurrent.

[0082] As previously discussed, the total current through an optical sensor (e.g., such as one or more optical sensors 3802) is the sum of the dark current and the photocurrent. However, according to some embodiments, the doped silicon layer 3506 disposed near the Ge-Si interface (e.g., near the germanium layer 3602) is used to effectively block current (electrons) from the substrate 3202 (e.g., such as Si) from entering the germanium layer 3602. As a result, the dark current component of the total current through the one or more optical sensors 3802 is reduced, and the performance of the one or more optical sensors 3802 is improved. For example, as discussed above, the P-type material within the doped silicon layer 3506 can be used to change the carrier concentration of the substrate 3202, and / or the Group VIIA material within the doped silicon layer 3506 can be used to neutralize trapped charges within the substrate 3202, thereby optimizing the Ge-Si interface.

[0083] The method 3000 then proceeds to block 3010 where contacts are formed and BEOL processing is performed. Fig.31 In the example of block 3010, a dielectric layer 3902 is formed over the substrate 3202 and over the one or more optical sensors 3802. In various embodiments, the dielectric layer 3902 may be formed as described above with reference to Fig. 9 The dielectric layer 902 depicted is substantially the same.

[0084] Like dielectric layer 902, dielectric layer 3902 may be patterned to form openings within which metal layers may be deposited to provide electrical contacts to underlying substrate components. For example, metal layer 3904 may be formed to provide electrical contacts to N-type region 3808, and metal layer 3906 may be formed to provide electrical contacts to P-type region 3810. In some examples, metal layers 3904, 3906 may include W, Cu, Co, Ru, Al, Rh, Mo, Ta, Ti, TiN, TaN, WN, silicide, combinations thereof, or another suitable conductive material.

[0085] After contacts are formed to underlying substrate components (e.g., including metal layers 3904, 3906), further BEOL processing may be performed. For example, various vias / metal lines and multi-layer interconnect components (e.g., metal layers and interlayer dielectrics, including portions of dielectric layer 3902) may be formed over substrate 3202 and may be configured to connect various underlying substrate components (to each other and to one or more devices on a separate device substrate that is subsequently bonded to substrate 3202) to form functional circuits (e.g., such as optoelectronic circuits), which may include one or more optical sensors 3802 and, in some cases, one or more devices (e.g., such as logic devices or other devices) from a separate device substrate. Fig.31As shown, a multi-layer interconnect (MLI) region 3915 may include vertical interconnects (such as vias or contacts) and horizontal interconnects (such as metal lines). Various interconnect components may be made of various conductive materials, including copper, tungsten and / or silicide. In one example, a copper-related multi-layer interconnect structure is formed using a damascene and / or dual damascene process. In some embodiments, a portion 3916 of the MLI region 3915 may be formed to provide an electrical contact to a metal layer 3904 in contact with an N-type region 3808, and a portion 3918 of the MLI region 3915 may be formed to provide an electrical contact to a metal layer 3906 in contact with a P-type region 3810.

[0086] The method 3000 then proceeds to block 3012 where the optoelectronic substrate is bonded to a separate device substrate. Fig.32 In the example of the embodiment of frame 3012, the device 3100 (including the optoelectronic substrate) is bonded to a separate device substrate 3950. As previously described, the separate device substrate 3950 may include core (logic) transistors and circuits and other devices. In at least some examples, the devices and / or circuits within the separate device substrate 3950 may include planar MOSFETs, FinFETs, GAA transistors, CMOS transistors, strained semiconductor devices, SOI devices, bipolar junction transistors, resistors, capacitors, inductors, diodes, fuses, memory devices (such as SRAM devices), I / O transistors and / or other logic devices and / or circuits. In some embodiments, the separate device substrate 3950 may include an application specific integrated circuit (ASIC). In some cases, after the bonding process of frame 3012, one or more devices (device 3100) within the optoelectronic substrate may be coupled to one or more devices in the separate device substrate 3950, for example, to jointly define a pixel circuit or other optoelectronic circuit. In some examples, device 3100 (including optoelectronic substrate) can be bonded to a separate device substrate 3950 using various structures and / or methods, such as copper-to-copper hybrid bonding, interposers, through silicon vias (TSVs), redistribution layers (RDLs), bond pads, copper microbumps and pillars, wire bonding, flip chips, wafer level packaging (WLP), or other suitable wafer bonding techniques, including 2.5D and 3D integrated circuit (IC) packaging techniques.

[0087] In methods 100, 1000, 2000 and 3000 discussed above, passivation of the Ge-Si interface is described as being typically accomplished by the following steps: forming an ion-implanted Si region in a trench adjacent to a germanium layer formed in the trench (as in method 100); forming an ion-implanted silicon layer in a dedicated optoelectronic substrate adjacent to a germanium layer formed above the optoelectronic substrate (as in method 1000); epitaxial growth of an doped silicon layer in the trench adjacent to the germanium layer formed in the trench (as in method 2000); or epitaxial growth of an doped silicon layer above a dedicated optoelectronic substrate adjacent to a germanium layer formed above the optoelectronic substrate (as in method 3000).

[0088] In some alternative embodiments, methods 100, 1000, 2000, 3000 may be modified so that ions are implanted into a germanium layer (instead of Si), or so that a doped epitaxial germanium layer (instead of a doped epitaxial silicon layer) is formed. These alternative embodiments are described below with reference to methods 4000, 5000, 6000, and 7000. Note that methods 4000, 5000, 6000, 7000 are substantially similar to methods 100, 1000, 2000, 3000, respectively. For example, in method 4000, which reflects method 100, passivation of the Ge-Si interface may generally be achieved by forming an ion-implanted Ge region in a germanium layer disposed in a trench and near the Ge-Si interface. In method 5000, which reflects method 1000, passivation of the Ge-Si interface may generally be achieved by forming an ion-implanted Ge region near the Ge-Si interface (in a germanium layer formed above the silicon layer). In method 6000, which reflects method 2000, passivation of the Ge-Si interface may be achieved by epitaxial growth of a doped germanium layer within the trench and near the Ge-Si interface. In method 7000, which reflects method 3000, passivation of the Ge-Si interface may be achieved by epitaxial growth of a doped germanium layer (above a dedicated optoelectronic substrate) near the Ge-Si interface.

[0089] It should also be noted that various aspects discussed above with reference to methods 100, 1000, 2000, 3000 may be equally applicable to methods 4000, 5000, 6000, 7000 discussed below. For example, various layers, components, or process steps discussed above may be equally applicable to the discussion below. In addition, the discussion of methods 4000, 5000, 6000, 7000 may repeat the reference numbers and / or letters used above in the corresponding methods 100, 1000, 2000, 3000. This repetition is for the purpose of simplicity and clarity, and does not in itself indicate the relationship between the various embodiments and / or configurations discussed. In addition, in view of the similarities between methods 4000, 5000, 6000, 7000 and methods 100, 1000, 2000, 3000, respectively, for the sake of clarity, only methods 4000, 5000, 6000, 7000 will be briefly discussed below, with particular attention to those components and / or method steps that are substantially different.

[0090] Reference now Fig.33 , a method 4000 of manufacturing a semiconductor device 4100 including a Ge-based optical sensor according to some embodiments is shown. Figures 34 to 41 Discussion Method 4000, Figures 34 to 41 A cross-sectional view of a semiconductor device 4100 at various stages of fabrication according to one or more steps of method 4000 is provided. As previously mentioned, method 4000 in some respects reflects method 100 discussed above. Therefore, for clarity of discussion, only certain aspects of method 4000 are briefly discussed. Furthermore, for clarity of discussion, various reference numbers and / or letters used above in the discussion of method 100 are repeated in the discussion of method 4000 when referring to similar components.

[0091] Method 4000 begins at block 4002, where a substrate is provided. In some embodiments, block 4002 of method 4000 is substantially the same as block 102 of method 100. Therefore, reference is made to Fig.34 In the example of FIG. 4002, a substrate 202 is provided. The substrate 202 may be a silicon substrate or other substrate as described above, and as discussed above, the substrate 202 further includes an optoelectronic region 204 and a logic region 206.

[0092] Method 4000 then proceeds to block 4004 where a trench is formed. In some embodiments, block 4004 of method 4000 is substantially the same as block 104 of method 100. Fig.35 In the example of FIG. 4004, in the embodiment of block 4004, trenches 302 are formed in the photovoltaic region 204. The HM layer 304 discussed above is also shown.

[0093] The method 4000 then proceeds to block 4006 where a germanium layer is formed. In some embodiments, block 4006 of the method 4000 is similar to block 110 of the method 100. Fig.36 In the example of block 4006, a germanium (Ge) layer 602 is formed within the trench 302. As shown, the germanium layer 602 may overfill the trench 302 in some cases, resulting in a surface topography 604 of the germanium layer 602. In some examples, the germanium layer 602 includes an intrinsic germanium layer. Therefore, in contrast to method 100, as described below, method 4000 forms the germanium layer 602 before forming an implantation region at the Ge-Si interface.

[0094] Method 4000 then proceeds to block 4008 where a CMP process is performed. In some embodiments, block 4008 of method 4000 is similar to block 112 of method 100. Fig.37 In an example of the present invention, in an embodiment of block 4008, a CMP process is performed to remove excess portions of the germanium layer 602 and planarize the top surface of the device 4100. As a result of the CMP process, the top surface of the substrate 202 (e.g., adjacent to the trench 302) and the top surface of the germanium layer 602 are substantially coplanar (level) with each other.

[0095] The method 4000 then proceeds to block 4010 where an oxide layer is deposited. In some embodiments, block 4010 of the method 4000 is similar to block 106 of the method 100. Fig.38 In the example of FIG. 4010 , an oxide layer 402 is deposited over the substrate 202 (e.g., within the optoelectronic region 204 and the logic region 206), including over the germanium layer 602 deposited within the trench 302. As described above, in various embodiments, the oxide layer 402 can be used to control the depth (e.g., projection range) of a subsequently performed ion implantation process.

[0096] Method 4000 then proceeds to block 4012 where an ion implantation process is performed. In some embodiments, block 4012 of method 4000 is similar to block 108 of method 100. Fig.39In an example of the present invention, in an embodiment of block 4012, a patterned implantation masking layer 502 is formed over the substrate 202, and an ion implantation process 504 is performed on the device 4100. In some examples, the dopant species used for the ion implantation process 504 may include a P-type material (e.g., a Group IIIA material (e.g., boron (B), aluminum (Al), gallium (Ga), indium (In), BF2) and / or a Group VIIA material (e.g., fluorine (F), chlorine (Cl), bromine (Br)). As a result of the ion implantation process 504, an implantation region 507 is formed within the germanium layer 602 near the Ge-Si interface and along the bottom of the germanium layer 602. Therefore, the implantation region 507 defines an ion-implanted Ge region. After forming the implantation region 507, the implantation masking layer 502 and the oxide layer 402 may be removed.

[0097] In some embodiments, the P-type material used to form the injection region 507 can be used to change the carrier concentration of the germanium layer 602 (e.g., at least the bottom of the germanium layer 602) so as to optimize the Ge-Si interface and substantially prevent electrons in the Si from entering the germanium layer. In some cases, the Group VIIA material used to form the injection region 507 can be used to neutralize trapped charges within the germanium layer 602, which can be trapped by defects (e.g., dangling bonds) along the bottom surface of the germanium layer 602 near the Ge-Si interface, so as to optimize the Ge-Si interface and substantially prevent electrons in the Si from entering the germanium layer.

[0098] Method 4000 then proceeds to block 4014 where an optical sensor and a logic device are formed. In some embodiments, block 4014 of method 4000 is similar to block 114 of method 100. Fig.40 / Fig.41 In the example of block 4014, the optical sensor 803 is formed in the photoelectric region 204 in the germanium layer 602, and the logic devices 804, 806 are formed in the logic region 206. The optical sensor 803 may include a Ge optical sensor (such as a Ge photodiode (PD)), and may include an N-type region 808 (cathode) and a P-type region 810 (anode) formed in the germanium layer 602. The optical sensor 803 may include a PI-NGe PD (or simply a PN Ge PD).

[0099] In various embodiments, the total current through the optical sensor 803 (Ge PD) is the sum of the dark current and the photocurrent. However, according to some embodiments, the implantation region 507 disposed near the Ge-Si interface (e.g., within the germanium layer 602) is used to effectively block the current (electrons) from the substrate 202 (e.g., such as Si) from entering the germanium layer 602. As a result, the dark current component of the total current through the optical sensor 803 is reduced, and the performance of the optical sensor 803 is improved.

[0100] As described above, logic region 206 includes logic device 804 (NMOS transistor) and logic device 806 (PMOS transistor). As described above, logic device 804 includes gate stack 816, and logic device 806 includes gate stack 818. Sidewall spacers may be formed on the sidewalls of gate stacks 816, 818. In addition, logic device 804 may include N-type source / drain regions 812 formed in substrate 202, adjacent to gate stack 816 and located on either side of gate stack 816, and logic device 806 may include P-type source / drain regions 814 formed in substrate 202, adjacent to gate stack 818 and located on either side of gate stack 818.

[0101] In some examples, the ion implantation process for forming the N-type source / drain region 812 can simultaneously form the N-type region 808 in the germanium layer 602. Moreover, in some embodiments, the ion implantation process for forming the P-type source / drain region 814 can simultaneously form the P-type region 810 in the germanium layer 602. Alternatively, in some embodiments, separate ion implantation processes can be performed for the N-type source / drain region 812 and the N-type region 808, and separate ion implantation processes can be performed for the P-type source / drain region 814 and the P-type region 810. In various examples, the dopant material for doping the N-type source / drain region 812 and the N-type region 808 can include phosphorus (P), arsenic (As), antimony (Sb), a combination thereof, or another suitable N-type dopant. In some embodiments, the dopant material for doping the P-type source / drain region 814 and the P-type region 810 can include boron (B), aluminum (Al), gallium (Ga), indium (In), or another suitable P-type dopant.

[0102] The method 4000 then proceeds to block 4016 where contacts are formed and BEOL processing is performed. In some embodiments, block 4016 of the method 4000 is similar to block 116 of the method 100. Fig.41 In the example of block 4016 , a dielectric layer 902 is formed over the substrate 202 and over each of the optical sensor 803 in the optoelectronic region 204 and the logic devices 804 , 806 in the logic region 206 .

[0103] In various examples, dielectric layer 902 may be patterned to form openings, and metal layers may be deposited within the openings to provide electrical contacts to underlying substrate components. For example, metal layer 904 may be formed to provide electrical contacts to N-type region 808, metal layer 906 may be formed to provide electrical contacts to P-type region 810, metal layer 908 may be formed to provide electrical contacts to N-type source / drain region 812, metal layer 910 may be formed to provide electrical contacts to the gate electrode of gate stack 816, metal layer 912 may be formed to provide electrical contacts to P-type source / drain region 814, and metal layer 914 may be formed to provide electrical contacts to the gate electrode of gate stack 818.

[0104] Thereafter, a multi-layer interconnect feature may be formed. As discussed above, portion 916 of MLI region 915 may be formed to provide electrical contact to metal layer 904 in contact with N-type region 808, portion 918 of MLI region 915 may be formed to provide electrical contact to metal layer 906 in contact with P-type region 810, portions 920 / 924 of MLI region 915 may be formed to provide electrical contact to metal layer 908 in contact with N-type source / drain region 812, portion 922 of MLI region 915 may be formed to provide electrical contact to metal layer 910 in contact with a gate electrode of gate stack 816, portions 926 / 930 of MLI region 915 may be formed to provide electrical contact to metal layer 912 in contact with P-type source / drain region 814, and portion 928 of MLI region 915 may be formed to provide electrical contact to metal layer 914 in contact with a gate electrode of gate stack 818.

[0105] Reference now Fig.42 , a method 5000 of manufacturing a semiconductor device 5100 including a Ge-based optical sensor according to some embodiments is shown. Figure 43 to Figure 49 Discussion Method 5000, Figure 43 to Figure 49 A cross-sectional view of a semiconductor device 5100 at various stages of fabrication according to one or more steps of method 5000 is provided. As previously mentioned, method 5000 in some respects reflects method 1000 discussed above. Therefore, for clarity of discussion, only certain aspects of method 5000 are briefly discussed. Also, for clarity of discussion, various reference numbers and / or letters used above in the discussion of method 1000 are repeated in the discussion of method 5000 when reference is made to similar components.

[0106] Method 5000 begins at block 5002, where a substrate is provided. In some embodiments, block 5002 of method 5000 is substantially the same as block 1002 of method 1000. Therefore, reference is made to Fig.43In an example of, in an embodiment of block 5002, a substrate 1202 is provided. As described above, the substrate 1202 may be a silicon substrate or other substrate. In addition, as described above, the substrate 1202 may include a dedicated optoelectronic substrate that includes one or more optoelectronic devices (e.g., such as photodiodes) associated with one or more imaging pixels. In at least some embodiments, the substrate 1202 may also include one or more logic devices and / or circuits. In some embodiments, a separate device substrate may be bonded to the optoelectronic substrate at a later stage of processing.

[0107] The method 5000 then proceeds to block 5004 where a germanium layer is formed. In some embodiments, block 5004 of the method 5000 is similar to block 1008 of the method 1000. Fig.44 In an example of the present invention, in an embodiment of block 5004, a germanium (Ge) layer 1602 is formed over the substrate 1202. In some examples, the germanium layer 1602 includes an intrinsic germanium layer. In some embodiments, a CMP process may be optionally performed to planarize and / or thin the germanium layer 1602. Thus, in contrast to method 1000, as described below, method 5000 forms the germanium layer 1602 before forming an implantation region at the Ge-Si interface.

[0108] Method 5000 then proceeds to block 5006 where an oxide layer is deposited. In some embodiments, block 5006 of method 5000 is similar to block 1004 of method 1000. Fig.45 In the example of FIG. 5006 , an oxide layer 1402 is deposited over the germanium layer 1602. The oxide layer 1402 may be used to control the depth (eg, projection range) of a subsequently performed ion implantation process.

[0109] Method 5000 then proceeds to block 5008 where an ion implantation process is performed. In some embodiments, block 5008 of method 5000 is similar to block 1006 of method 1000. Fig.46 In an example of, in an embodiment of block 5008, an ion implantation process 1504 is performed on the device 5100. In some examples, the dopant species used for the ion implantation process 1504 may include a P-type material (e.g., Group IIIA (e.g., boron (B), aluminum (Al), gallium (Ga), indium (In), BF2) and / or Group VIIA material (e.g., fluorine (F), chlorine (Cl), bromine (Br)). As a result of the ion implantation process 1504, an implantation region 1507 is formed within the germanium layer 1602 near the Ge-Si interface and along the bottom of the germanium layer 1602. Therefore, the implantation region 15070 defines an ion-implanted Ge region. After forming the implantation region 1507, the oxide layer 1402 can be removed.

[0110] In some embodiments, the P-type material used to form the injection region 1507 can be used to change the carrier concentration of the germanium layer 1602 (e.g., at least the bottom of the germanium layer 1602) so as to optimize the Ge-Si interface and substantially prevent electrons in the Si from entering the germanium layer. In some cases, the Group VIIA material used to form the injection region 1507 can be used to neutralize trapped charges within the germanium layer 1602, which can be trapped by defects (e.g., dangling bonds) along the bottom surface of the germanium layer 1602 near the Ge-Si interface, so as to optimize the Ge-Si interface and substantially prevent electrons in the Si from entering the germanium layer.

[0111] Method 5000 then proceeds to block 5010 where an optical sensor is formed. In some embodiments, block 5010 of method 5000 is similar to block 1010 of method 1000. Fig.47 In the example of the embodiment of block 5010, one or more optical sensors 1803 are formed within the germanium layer 1602. In some embodiments, the one or more optical sensors 1803 may include a Ge optical sensor, such as a Ge photodiode (PD). Each of the one or more optical sensors 1803 may include an N-type region 1808 (cathode) and a P-type region 1810 (anode) formed within the germanium layer 1602. The one or more optical sensors 1803 may include a PIN Ge PD (or simply PN Ge PD).

[0112] In various embodiments, the total current through the one or more optical sensors 1803 is the sum of the dark current and the photocurrent. However, according to some embodiments, the implant region 1507 disposed near the Ge-Si interface (e.g., within the germanium layer 1602) is used to effectively block the current (electrons) from the substrate 1202 (e.g., such as Si) from entering the germanium layer 1602. As a result, the dark current component of the total current through the one or more optical sensors 1803 is reduced, and the performance of the one or more optical sensors 1803 is improved.

[0113] The method 5000 then proceeds to block 5012 where contacts are formed and BEOL processing is performed. In some embodiments, block 5012 of the method 5000 is similar to block 1012 of the method 1000. Fig.48 In the example of block 5012 , a dielectric layer 1902 is formed over the substrate 1202 and over the one or more optical sensors 1803 .

[0114] In various examples, dielectric layer 1902 can be patterned to form an opening within which a metal layer can be deposited to provide electrical contact to underlying substrate components. For example, metal layer 1904 can be formed to provide electrical contact to N-type region 1808, and metal layer 1906 can be formed to provide electrical contact to P-type region 1810.

[0115] Thereafter, a multilayer interconnect component may be formed. As discussed above, portion 1916 of MLI region 1915 may be formed to provide electrical contact to metal layer 1904 in contact with N-type region 1808, and portion 1918 of MLI region 1915 may be formed to provide electrical contact to metal layer 1906 in contact with P-type region 1810.

[0116] Method 5000 then proceeds to block 5014 where the optoelectronic substrate is bonded to a separate device substrate. In some embodiments, block 5014 of method 5000 is similar to block 1014 of method 1000. Fig.49 In an example of a block 5014 embodiment, the device 5100 (including the optoelectronic substrate) is bonded to a separate device substrate 1950, which may include core (logic) transistors and circuits and other devices as described above. In some cases, for example, after the bonding process of block 5014, one or more devices (device 5100) within the optoelectronic substrate may be coupled to one or more devices in the separate device substrate 1950 to jointly define a pixel circuit or other optoelectronic circuit.

[0117] Reference now Fig.50 , a method 6000 of manufacturing a semiconductor device 6100 including a Ge-based optical sensor according to some embodiments is shown. Figure 51 to Figure 57 Discussion Method 6000, Figure 51 to Figure 57 A cross-sectional view of a semiconductor device 6100 at various stages of fabrication according to one or more steps of method 6000 is provided. As previously described, method 6000 reflects in some respects method 2000 discussed above. For example, in the illustrated embodiment, method 6000 is identical to method 2000, except that instead of epitaxially growing a doped silicon layer in a trench (block 2006 of method 2000), method 6000 includes epitaxially growing a doped germanium layer in a trench (block 6006 of method 6000). Therefore, for clarity of discussion, method 6000 is only discussed very briefly. Moreover, for clarity of discussion, various reference numbers and / or letters used above in the discussion of method 2000 are repeated in the discussion of method 6000 when reference is made to similar components.

[0118] The method 6000 begins at block 6002, where a substrate is provided. Fig.51In the example of FIG. 6002, a substrate 2202 is provided as described above. The substrate 2202 also includes an optoelectronic region 2204 (pixel region) and a logic region 2206.

[0119] The method 6000 then proceeds to block 6004 where a trench is formed. Fig.52 In the example of FIG. 6004, in the embodiment of block 6004, as described above, trenches 2302 are formed in the photovoltaic region 2204. A patterned HM layer 2304 is also shown.

[0120] The method 6000 then proceeds to block 6006 where a doped germanium layer is formed. Fig.53 In an example of, in an embodiment of box 6006, a doped germanium (Ge) layer 2507 is formed within the trench 2302 (e.g., including along the sidewalls and bottom surface of the trench 2302). In some examples, the doped germanium layer 2507 may include an epitaxially grown germanium layer. More generally, in some embodiments, the doped germanium layer 2507 is formed by ALD, CVD, MBE, MOCVD, and / or other suitable growth processes. In order to provide doping for the doped germanium layer 2507, a suitable dopant substance may be introduced into the process chamber during the growth of the germanium layer (e.g., in an in-situ doping process) to provide the doped germanium layer 2507. In some examples, the dopant substance may include a P-type material (e.g., Group IIIA (e.g., boron (B), aluminum (Al), gallium (Ga), indium (In), BF2) and / or Group VIIA material (e.g., fluorine (F), chlorine (Cl), bromine (Br)).

[0121] As described below, the doped germanium layer 2507 will be located near the Ge-Si interface of the subsequently formed Ge PD. In some embodiments, the P-type material used to form the doped germanium layer 2507 can be used to change the carrier concentration of the Ge PD (e.g., at least along the bottom of the Ge PD near the Ge-Si interface), so that the Ge-Si interface is optimized and electrons in Si are substantially prevented from entering the germanium layer. In some cases, the Group VIIA material used to form the doped germanium layer 2507 can be used to neutralize trapped charges within the Ge PD, which can be captured by defects (e.g., dangling bonds) along the bottom of the Ge PD near the Ge-Si interface, so that the Ge-Si interface is optimized and electrons in Si are substantially prevented from entering the germanium layer.

[0122] The method 6000 then proceeds to block 6008 where a germanium layer is formed. Fig.54 In the example of block 6008, after forming the doped germanium layer 2507 along the sidewalls and bottom of the trench 2302, a germanium layer 2602 (as described above) is formed within the trench 2302 and over the doped germanium layer 2507. In some examples, the germanium layer 2602 includes an intrinsic germanium layer.

[0123] The method 6000 then proceeds to block 6010 where a CMP process is performed. Fig.55 In the example of FIG. 6010, a CMP process is performed after forming the germanium layer 2602 in the embodiment of block 6010. The CMP process is used to remove excess portions of the germanium layer 2602 and planarize the top surface of the device 6100. In some embodiments, as shown, the CMP process of block 6010 can also be used to remove the HM layer 2304. As a result of the CMP process, the top surface of the substrate 2202 (e.g., adjacent to the trench 2302), the top surface of the germanium layer 2602, and the top surface of the portion of the doped germanium layer 2507 along the sidewall surface of the trench 2302 are substantially coplanar (flush) with each other.

[0124] The method 6000 then proceeds to block 6012 where an optical sensor is formed. Fig.56 In the example of FIG. 6012, in the embodiment of block 6012, an optical sensor 2803 is formed in the photoelectric region 2204 within the germanium layer 2602. In some embodiments, the optical sensor 2803 may include a Ge optical sensor, such as a Ge photodiode (PD). The optical sensor 2803 may include an N-type region 2808 (cathode) and a P-type region 2810 (anode) formed within the germanium layer 2602. The N-type region 2808 and the P-type region 2810 may be formed in substantially the same manner as described above. In addition, the optical sensor 2803 may include a PI-NGe PD (or simply a P-NGe PD).

[0125] In various embodiments, the total current through the optical sensor 2803 (Ge PD) is the sum of the dark current and the photocurrent. However, according to some embodiments, the doped germanium layer 2507 disposed near the Ge-Si interface is used to effectively block the current (electrons) from the substrate 2202 (e.g., such as Si) from entering the Ge PD (e.g., including the germanium layer 2602). As a result, the dark current component of the total current through the optical sensor 2803 is reduced, and the performance of the optical sensor 2803 is improved.

[0126] The method 6000 then proceeds to block 6014 where a logic device is formed, contacts are formed, and BEOL processing is performed. Fig.57 In the example of block 6014, logic devices 2804, 2806 are formed within logic region 2206 as described above.

[0127] In at least some examples, the ion implantation process used to form the N-type source / drain region 2812 can simultaneously form the N-type region 2808 within the germanium layer 2602. Moreover, in some embodiments, the ion implantation process used to form the P-type source / drain region 2814 can simultaneously form the P-type region 2810 within the germanium layer 2602. In some instances, separate ion implantation processes can be performed for the N-type source / drain region 2812 and the N-type region 2808, and separate ion implantation processes can be performed for the P-type source / drain region 2814 and the P-type region 2810.

[0128] In a further embodiment of block 6014, and still with reference to Fig.57 In the example of , dielectric layer 2902 is formed over substrate 2202 and over each of optical sensor 2803 in optoelectronic region 2204 and logic devices 2804, 2806 in logic region 2206. Dielectric layer 2902 can be patterned to form openings, within which metal layers can be deposited to provide electrical contacts to underlying substrate components, as described above. After forming contacts to underlying substrate components (e.g., including metal layers 2904, 2906, 2908, 2910, 2912, 2914), further BEOL processing can be performed. In some embodiments, further BEOL processing can include the formation of MLI region 2915, which includes portions 2916, 2918, 2920, 2922, 2924, 2926, 2928, and 2930, as described above.

[0129] Reference now Fig.58 , a method 7000 of manufacturing a semiconductor device 7100 including a Ge-based optical sensor according to some embodiments is shown. Figure 59 to Figure 64 Discussion Method 7000, Figure 59 to Figure 64 A cross-sectional view of a semiconductor device 7100 at various stages of fabrication according to one or more steps of method 7000 is provided. As previously described, method 7000 reflects in some respects method 3000 discussed above. For example, in the illustrated embodiment, method 7000 is identical to method 3000, except that instead of epitaxially growing a doped silicon layer above a substrate (block 3004 of method 3000), method 7000 includes epitaxially growing a doped germanium layer above a substrate (block 7004 of method 7000). Therefore, for clarity of discussion, method 7000 is only discussed very briefly. Moreover, for clarity of discussion, various reference numbers and / or letters used above in the discussion of method 3000 are repeated in the discussion of method 7000 when reference is made to similar components.

[0130] Method 7000 begins at block 7002, where a substrate is provided. Fig.59In the example of block 7002, a substrate 3202 is provided as described above. In some embodiments, the substrate 3202 of the device 7100 may include a dedicated optoelectronic substrate that includes one or more optoelectronic devices (e.g., such as photodiodes) associated with one or more imaging pixels. Of course, in at least some embodiments, the substrate 3202 may also include one or more logic devices and / or circuits.

[0131] The method 7000 then proceeds to block 7004 where a doped germanium layer is formed. Fig.60 In an example of, in an embodiment of block 7004, a doped germanium (Ge) layer 3507 is formed over substrate 3202. In some examples, the doped germanium layer 3507 may include an epitaxially grown germanium layer. More generally, in some embodiments, the doped germanium layer 3507 is formed by ALD, CVD, MBE, MOCVD, and / or other suitable growth processes. In order to provide doping for the doped germanium layer 3507, a suitable dopant substance may be introduced into a process chamber during the growth of the silicon layer (e.g., in an in-situ doping process) to provide the doped germanium layer 3507. In some examples, the dopant substance may include a P-type material (e.g., Group IIIA (e.g., boron (B), aluminum (Al), gallium (Ga), indium (In), BF2) and / or Group VIIA material (e.g., fluorine (F), chlorine (Cl), bromine (Br)).

[0132] The doped germanium layer 3507 will be located near the Ge-Si interface of the subsequently formed Ge PD, as described below. In some embodiments, the P-type material used to form the doped germanium layer 3507 can be used to change the carrier concentration of the Ge PD (e.g., at least along the bottom of the Ge PD near the Ge-Si interface), so that the Ge-Si interface is optimized and electrons in Si are substantially prevented from entering the germanium layer. In some cases, the Group VIIA material used to form the doped germanium layer 3507 can be used to neutralize trapped charges within the Ge PD, which can be captured by defects (e.g., dangling bonds) along the bottom of the Ge PD near the Ge-Si interface, so that the Ge-Si interface is optimized and electrons in Si are substantially prevented from entering the germanium layer.

[0133] The method 7000 then proceeds to block 7006 where a germanium layer is formed. Fig.61 In an example of the present invention, in an embodiment of block 7006, after forming the doped germanium layer 3507 over the substrate 3202, a germanium layer 3602 is formed over the doped germanium layer 3507 (as described above). In some examples, the germanium layer 3602 includes an intrinsic germanium layer. In some embodiments, a CMP process may be optionally performed to planarize and / or thin the germanium layer 3602.

[0134] Method 7000 then proceeds to block 7008 where an optical sensor is formed. Fig.62 In the example of block 7008, one or more optical sensors 3803 are formed within the germanium layer 3602. In some embodiments, the one or more optical sensors 3803 may include a Ge optical sensor, such as a Ge photodiode (PD). Each of the one or more optical sensors 3803 may include an N-type region 3808 (cathode) and a P-type region 3810 (anode) formed within the germanium layer 3602 in substantially the same manner as described above. In addition, the one or more optical sensors 3803 may include a PI-NGe PD (or simply a P-NGe PD).

[0135] In various embodiments, the total current through the one or more optical sensors 3802 (Ge PD) is the sum of the dark current and the photocurrent. However, according to some embodiments, the doped germanium layer 3507 disposed near the Ge-Si interface is used to effectively block the current (electrons) from the substrate 3202 (e.g., such as Si) from entering the Ge PD (e.g., including the germanium layer 3602). As a result, the dark current component of the total current through the one or more optical sensors 3803 is reduced, and the performance of the one or more optical sensors 3803 is improved.

[0136] The method 7000 then proceeds to block 7010 where contacts are formed and BEOL processing is performed. Fig.63 In the example of block 7010, dielectric layer 3902 is formed over substrate 3202 and over one or more optical sensors 3803. Dielectric layer 3902 may be patterned to form openings, and metal layers may be deposited within the openings to provide electrical contacts to underlying substrate components, as described above. After forming contacts to underlying substrate components (e.g., including metal layers 3904, 3906), further BEOL processing may be performed. In some embodiments, further BEOL processing may include the formation of MLI region 3915, which includes portions 3916 and 3918, as described above.

[0137] The method 7000 then proceeds to block 7012 where the optoelectronic substrate is bonded to a separate device substrate. Fig.64 In an example of a block 7012 embodiment, the device 7100 (including the optoelectronic substrate) is bonded to a separate device substrate 3950, which may include core (logic) transistors and circuits and other devices as described above. In some cases, for example, after the bonding process of block 7012, one or more devices (device 7100) within the optoelectronic substrate may be coupled to one or more devices in the separate device substrate 3950 to jointly define a pixel circuit or other optoelectronic circuit.

[0138] Although the above examples describe various methods of doping the Ge-Si interface, for example, by implanting dopant species into Si or Ge at the Ge-Si interface of the Ge PD, or by epitaxially growing a doped silicon layer or a doped germanium layer at the Ge-Si interface of the Ge PD, such examples are not meant to be limiting, and other embodiments may similarly fall within the scope of the present invention. For example, in some cases, for a given Ge PD, the Ge-Si interface may include (i) an implanted silicon layer and an implanted germanium layer, (ii) a doped epitaxial silicon layer and a doped epitaxial germanium layer, (iii) an implanted silicon layer and a doped epitaxial silicon layer, (iv) an implanted germanium layer and a doped epitaxial germanium layer, (v) an implanted silicon layer and a doped epitaxial germanium layer, (vi) an implanted germanium layer and a doped epitaxial silicon layer, or any other suitable combination of an ion-implanted layer and a doped epitaxial layer. In addition, in various embodiments, the ion-implanted silicon layer may be formed so that it is adjacent to the Ge-Si interface or spaced a certain distance from the Ge-Si interface. Similarly, in some examples, the ion-implanted germanium layer can be formed so as to be adjacent to the Ge-Si interface or spaced a distance away from the Ge-Si interface.

[0139] The various embodiments described herein provide several advantages over the prior art. It should be understood that not all advantages must be discussed herein, and no particular advantage is required by all embodiments, and other embodiments may provide different advantages. For example, the embodiments discussed herein include structures and methods for passivating interfaces between various semiconductor layers to reduce dark current and improve device performance. In some embodiments, the passivated interface includes a Ge-Si interface of a Ge PD. In various embodiments, passivation of the Ge-Si interface can be achieved by doping the Ge-Si interface, for example, by ion implanting Ge or Si at the Ge-Si interface, or by epitaxially growing a doped silicon layer or a doped germanium layer at the Ge-Si interface. In some embodiments, the dopant species used to dope the Ge-Si interface may include a P-type material (e.g., Group IIIA (e.g., boron (B), aluminum (Al), gallium (Ga), indium (In), BF2) or Group VIIA material (e.g., fluorine (F), chlorine (Cl), bromine (Br)). By introducing one or more of these dopant species into the Ge-Si interface, the Ge-Si interface can be optimized to substantially prevent electrons in the silicon layer from entering the germanium layer (including the Ge PD) according to one or more methods described herein. As a result, the leakage current and dark current problems in Ge-based sensors are significantly alleviated. In at least some examples, the leakage current / dark current of the Ge-based sensor is reduced / improved by about 10%.

[0140] Thus, one of the embodiments of the present invention describes a method including providing a substrate having a pixel region and a logic region. In some embodiments, the method further includes forming a trench in the pixel region. In various examples, and after forming the trench, the method further includes forming a doped semiconductor layer along the sidewalls and bottom surface of the trench. In some embodiments, the method further includes forming a germanium layer in the trench and above the doped semiconductor layer. In some examples, and after forming the germanium layer, the method further includes forming an optical sensor in the germanium layer.

[0141] In the above method, wherein forming the doped semiconductor layer includes performing an ion implantation process on the sidewall and the bottom surface of the trench.

[0142] In the above method, wherein forming the doped semiconductor layer includes performing an ion implantation process on the sidewalls and the bottom surface of the trench, the method further includes forming an oxide layer on the sidewalls and the bottom surface of the trench before performing the ion implantation process.

[0143] In the above method, forming the doped semiconductor layer includes performing an ion implantation process on the side walls and the bottom surface of the trench, and the method also includes forming an oxide layer above the side walls and the bottom surface of the trench before performing the ion implantation process; and removing the oxide layer before forming the germanium layer.

[0144] In the above method, forming the doped semiconductor layer includes performing an ion implantation process on the sidewalls and the bottom surface of the trench, and the ion implantation process forms a doped silicon (Si) layer along the sidewalls and the bottom surface of the trench.

[0145] In the above method, wherein forming the doped semiconductor layer includes epitaxially growing a doped silicon layer along the sidewalls and the bottom surface of the trench.

[0146] In the above method, wherein forming the doped semiconductor layer includes epitaxially growing a doped germanium (Ge) layer along the sidewalls and the bottom surface of the trench.

[0147] In the above method, the doped semiconductor layer includes at least one of a P-type material and a Group VIIA material.

[0148] In the above method, the doped semiconductor layer includes at least one of a P-type material and a Group VIIA material, and the P-type material includes boron (B), aluminum (Al), gallium (Ga), indium (In) and BF2.

[0149] In the above method, the doped semiconductor layer includes at least one of a P-type material and a Group VIIA material, and the Group VIIA material includes fluorine (F), chlorine (Cl) and bromine (Br).

[0150] In another embodiment, a method is discussed, including providing a substrate and forming a germanium layer over the substrate. In some embodiments, and after forming the germanium layer, the method further includes forming a doping layer along a bottom of the germanium layer, wherein forming the doping layer includes performing an ion implantation process on the germanium layer. In some examples, and after forming the doping layer, the method further includes forming an optical sensor within the germanium layer.

[0151] In the above method, the method further includes forming an oxide layer on the germanium layer before performing the ion implantation process.

[0152] In the above method, the method further includes forming an oxide layer on the germanium layer before performing the ion implantation process; and removing the oxide layer before forming the optical sensor.

[0153] In the above method, the method further includes forming a contact and a multi-layer interconnection component coupled to the optical sensor after forming the optical sensor.

[0154] In the above method, the method further includes forming contacts and multi-layer interconnect components coupled to the optical sensor after forming the optical sensor; and bonding the substrate including the optical sensor to a separate device substrate after forming the contacts and the multi-layer interconnect components.

[0155] In the above method, the doping layer includes at least one of a P-type material and a Group VIIA material.

[0156] In the above method, the method further includes forming a trench in a pixel region of the substrate before forming the germanium layer, and forming the germanium layer in the trench.

[0157] In yet another embodiment, a semiconductor device is discussed, including a silicon substrate having a pixel region and a logic region adjacent to the pixel region. In some embodiments, the semiconductor device also includes a germanium layer formed in a trench in the silicon substrate disposed in the pixel region, wherein a Ge-Si interface is defined along a sidewall and a bottom surface of the trench, and wherein the sensor is disposed in the germanium layer. In some cases, the semiconductor device also includes a doped region disposed proximate to the Ge-Si interface, wherein the doped region substantially blocks electrons within the Si substrate from entering the germanium layer.

[0158] In the above semiconductor device, the doped region is arranged on the germanium side of the Ge-Si interface or on the silicon side of the Ge-Si interface.

[0159] In the above-mentioned semiconductor device, wherein the doped region includes at least one of a P-type material and a Group VIIA material, wherein the P-type material includes boron (B), aluminum (Al), gallium (Ga), indium (In) and BF2, and wherein the Group VIIA material includes fluorine (F), chlorine (Cl) and bromine (Br).

[0160] The features of several embodiments are summarized above so that those skilled in the art can better understand aspects of the present invention. Those skilled in the art should understand that they can easily use the present invention as a substrate to design or modify other processes and structures for implementing the same purpose and / or achieving the same advantages as the embodiments introduced herein. Those skilled in the art should also appreciate that this equivalent configuration does not deviate from the spirit and scope of the present invention, and that they can make multiple changes, substitutions and changes herein without departing from the spirit and scope of the present invention.

Claims

1. A method for manufacturing a semiconductor device, include: providing a substrate including a pixel region and a logic region; forming a groove in the pixel region; After forming the trench, forming a doped semiconductor layer along the sidewalls and bottom surface of the trench; forming a germanium layer in the trench and over the doped semiconductor layer; as well as After forming the germanium layer, an optical sensor is formed in the germanium layer, the optical sensor including an anode and a cathode embedded in the germanium layer, the anode and the cathode being separated from the doped semiconductor layer.

2. The method according to claim 1, in, Forming the doped semiconductor layer includes performing an ion implantation process on the sidewalls and the bottom surface of the trench. 3 . The method according to claim 2 , further comprising forming an oxide layer over the sidewalls and the bottom surface of the trench before performing the ion implantation process. The method according to claim 3 , further comprising removing the oxide layer before forming the germanium layer.

5. The method according to claim 2, in, The ion implantation process forms a doped silicon (Si) layer along the sidewalls and the bottom surface of the trench.

6. The method according to claim 1, in, Forming the doped semiconductor layer includes epitaxially growing a doped silicon layer along the sidewalls and the bottom surface of the trench.

7. The method according to claim 1, in, Forming the doped semiconductor layer includes epitaxially growing a doped germanium (Ge) layer along the sidewalls and the bottom surface of the trench.

8. The method according to claim 1, in, The doped semiconductor layer includes at least one of a P-type material and a Group VIIA material.

9. The method according to claim 8, in, The P-type material includes boron (B), aluminum (Al), gallium (Ga), indium (In) and BF 2 .

10. The method according to claim 8, in, The Group VIIA materials include fluorine (F), chlorine (Cl), and bromine (Br).

11. A method of manufacturing a semiconductor device, include: providing a substrate; forming a germanium layer over the substrate; After forming the germanium layer, forming a doping layer along the bottom of the germanium layer, wherein forming the doping layer comprises performing an ion implantation process on the germanium layer; as well as After forming the doping layer, an optical sensor is formed in the germanium layer, the optical sensor including an anode and a cathode embedded in the germanium layer, the anode and the cathode being separated from the doping layer. 12 . The method of claim 11 , further comprising forming an oxide layer over the germanium layer before performing the ion implantation process.

13. The method of claim 12, further comprising removing the oxide layer before forming the optical sensor.

14. The method of claim 11, further comprising forming contacts and multi-layer interconnect components coupled to the optical sensor after forming the optical sensor. 15 . The method of claim 14 , further comprising bonding the substrate including the optical sensor to a separate device substrate after forming the contacts and the multi-layer interconnection feature.

16. The method according to claim 11, in, The doping layer includes at least one of a P-type material and a Group VIIA material. 17 . The method according to claim 11 , further comprising forming a trench in a pixel region of the substrate and forming the germanium layer in the trench before forming the germanium layer.

18. A semiconductor device, include: A silicon (Si) substrate, comprising a pixel region and a logic region adjacent to the pixel region; a germanium (Ge) layer formed in a trench in the silicon substrate disposed in the pixel region, wherein a Ge-Si interface is defined along a sidewall and a bottom surface of the trench, and wherein an optical sensor is disposed in the germanium layer, the optical sensor comprising an anode and a cathode embedded in the germanium layer; and A doped region is separated from the anode and the cathode and is disposed near the Ge-Si interface, wherein the doped region prevents electrons in the silicon substrate from entering the germanium layer.

19. The semiconductor device according to claim 18, in, The doped region is disposed on the germanium side of the Ge-Si interface or on the silicon side of the Ge-Si interface.

20. The semiconductor device according to claim 18, in, The doped region includes at least one of a P-type material and a Group VIIA material, wherein the P-type material includes boron (B), aluminum (Al), gallium (Ga), indium (In), and BF 2 , and wherein the Group VIIA material includes fluorine (F), chlorine (Cl) and bromine (Br).

Citation Information

Patent Citations

  • A CMOS imager photodiode with enhanced capacitance and method for manufacturing same

    CN101022118A

  • Complementary metal oxide semiconductor (CMOS) image sensor and manufacturing method thereof

    CN102651372A

  • Implant damage free image sensor and method of the same

    CN106206629A

  • Semiconductor Structure with Air Gap and Method Sealing the Air Gap

    CN110729233A

  • Image sensor, integrated circuit and method of forming image sensor

    CN110970451A