Semiconductor element manufacturing method and semiconductor substrate

By forming a fixed layer and an organic material layer on the semiconductor thin film layer, the semiconductor epitaxial layer is separated from the base material substrate and bonded to other substrates by using pick-up substrate technology, solving the problem of low movement and bonding efficiency of semiconductor epitaxial layer. Achieve efficient semiconductor component manufacturing.

CN113690184BActive Publication Date: 2024-11-12PHILNIX CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110993602.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-02-28
Filing Date
2018-03-27
Publication Date
2024-11-12
Estimated Expiration
2038-03-27

AI Technical Summary

Technical Problem

In the prior art, the semiconductor epitaxial layer is separated from the base material substrate after the etching of the sacrificial layer is completed, resulting in low movement and bonding efficiency of the semiconductor epitaxial layer, and it is difficult to efficiently bond it to other substrates.

Method used

By forming a fixed layer on the semiconductor film layer and combining it with the organic material layer, the semiconductor film layer is separated from the base material substrate and bonded to other substrates using a pick-up substrate, and a void is formed using an etching technique to improve separation efficiency.

Benefits of technology

提高了半导体磊晶层的移动和接合效率,实现了半导体元件的高效制造,减少了半导体磊晶层在蚀刻过程中的损伤,并提高了接合质量。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113690184B_ABST
    Figure CN113690184B_ABST
Patent Text Reader

Abstract

The object of the present invention is to improve the efficiency of the method of manufacturing semiconductor elements by bonding a semiconductor epitaxial layer to other substrates. The method of manufacturing a semiconductor element of the present invention includes: a step of forming a fixed layer as a thin film, wherein the fixed layer bonds at least a portion of the main surface of the semiconductor thin film layer opposite to the mother substrate side with at least a portion of the surface of the mother substrate on the semiconductor thin film layer side; a step of forming a gap by removing a portion of the semiconductor thin film layer or the mother substrate; a step of bonding an organic material layer formed on a pickup substrate to the fixed layer on the main surface of the semiconductor thin film layer after the gap is formed; a step of moving the pickup substrate in a direction away from the mother substrate in a state where the organic material layer is bonded to the fixed layer, thereby separating the semiconductor thin film layer from the first substrate; and a step of bonding the semiconductor thin film layer separated from the mother substrate to a second substrate. The present invention also provides a semiconductor element.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This invention is a divisional application of the invention patent application with application number 201880089952.1 filed on March 27, 2018 and invention name “Method for manufacturing semiconductor element”. Technical Field

[0002] The invention relates to a method for manufacturing a semiconductor element and the semiconductor element. Background Art

[0003] Conventionally, there is known a technique for removing a semiconductor epitaxial layer from a mother substrate and transferring the layer to another substrate (see, for example, Patent Document 1).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent No. 3813123 Summary of the invention

[0007] Problems to be solved by the invention

[0008] Fig. 22 It is a diagram used to explain the prior art. Fig. 22 The semiconductor structure includes a mother substrate 3001, a sacrificial layer 3002, a semiconductor epitaxial layer 3003, and a support 3004. The sacrificial layer 3002 is disposed between the semiconductor epitaxial layer 3003 and the mother substrate 3001, and becomes smaller than the semiconductor epitaxial layer 3003 due to etching. Reference numeral 3010 indicates an etched region of the sacrificial layer 3002.

[0009] The support body 3004 has the same shape as the semiconductor epitaxial layer 3003 in its horizontal cross section and is disposed on the semiconductor epitaxial layer 3003. The support body 3004 is a member for supporting the semiconductor epitaxial layer 3003 when the semiconductor epitaxial layer 3003 is removed from the mother substrate 3001. Fig. 22 In the conventional technology shown, the semiconductor epitaxial layer 3003 is peeled off from the mother substrate 3001 by removing the sacrificial layer 3002 by etching.

[0010] exist Fig. 22 In the prior art shown, the semiconductor epitaxial layer 3003 and the support body 3004 are peeled off from the mother substrate 3001 at the time point when the etching of the sacrificial layer 3002 is completed. Therefore, there is the following problem: at the time point when the sacrificial layer 3002 is completely etched and the mother substrate 3001 and the semiconductor epitaxial layer 3003 are separated, the semiconductor epitaxial layer 3003 needs to be moved and placed at a temporary position different from the mother substrate 3001.

[0011] Therefore, the present invention has been made in view of the above-mentioned situation, and an object of the present invention is to improve the efficiency of a method for manufacturing a semiconductor device by bonding a semiconductor epitaxial layer to another substrate.

[0012] Technical means of solving problems

[0013] A method for manufacturing a semiconductor element according to a first embodiment of the present invention is a method for manufacturing a semiconductor element in which a semiconductor thin film layer formed on top of a first substrate is separated from the first substrate and bonded to a second substrate different from the first substrate, and includes: a step of forming a fixed layer as a thin film, wherein the fixed layer bonds at least a portion of a main surface of the semiconductor thin film layer on the opposite side to a side of the first substrate to at least a portion of a surface on one side of the semiconductor thin film layer in the first substrate; a step of forming a gap by removing a portion of an area of ​​the semiconductor thin film layer or the first substrate, or a portion of an area of ​​a layer between the semiconductor thin film layer and the first substrate; a step of bonding an organic material layer formed on a third substrate to at least a portion of a bonding area of ​​the fixed layer and the semiconductor thin film layer on the main surface of the semiconductor thin film layer after forming the gap; a step of moving the third substrate in a direction away from the first substrate while the organic material layer is bonded to the bonding area, thereby separating the semiconductor thin film layer from the first substrate; and a step of bonding the semiconductor thin film layer separated from the first substrate to the second substrate.

[0014] The manufacturing method may further include, after the step of bonding the semiconductor thin film layer to the second substrate: separating the semiconductor thin film layer from the third substrate by removing the organic material layer.

[0015] In the step of separating the semiconductor thin film layer from the third substrate, the organic material layer may be removed by dissolving.

[0016] In the step of forming the fixing layer, the fixing layer may be formed to have a thickness that is thick enough to cut off the fixing layer formed on the first substrate and the fixing layer formed on the side of the semiconductor thin film layer by the force of moving the third substrate.

[0017] In the step of forming the fixed layer, the fixed layer can be formed in a manner that extends between the two ends of the semiconductor thin film layer in a first direction on the main surface of the semiconductor thin film layer, and the semiconductor thin film layer is exposed in at least a portion of the two side surfaces of the semiconductor thin film layer in a second direction orthogonal to the first direction.

[0018] In the step of forming the fixed layer, the fixed layer can be formed in a manner that the coverage of the two side surfaces in the second direction of the semiconductor thin film layer by the fixed layer extending in the second direction becomes smaller than the coverage of the two side surfaces in the first direction of the semiconductor thin film layer by the fixed layer extending in the first direction.

[0019] In the step of forming the fixing layer, the fixing layer may be formed in such a manner that the coverage of the side surfaces of the long sides of the semiconductor thin film layer becomes smaller than the coverage of the side surfaces of the short sides of the semiconductor thin film layer.

[0020] The manufacturing method may include: a step of forming a plurality of islands of the semiconductor thin film layer; and in the step of forming the fixed layer, a step of forming a plurality of the fixed layers corresponding to the plurality of islands.

[0021] The step of combining the organic material layer with the fixed layer may include: preparing the third substrate having the organic material layers formed at positions corresponding to the plurality of islands; and combining the plurality of organic material layers formed on the third substrate to the plurality of combining regions.

[0022] In the step of forming the fixed layer, an electrode may be set between the fixed layer and the semiconductor thin film layer. The manufacturing method may further include: a step of forming an opening in the fixed layer; and a step of forming a wiring layer connected to the electrode through the opening after the step of bonding the semiconductor thin film layer to the second substrate.

[0023] The method for manufacturing the semiconductor element may further include, after the step of bonding the semiconductor thin film layer to the second substrate: a step of forming an opening in the fixed layer; a step of setting an electrode in the opening; a step of forming an interlayer insulating layer including at least a portion of the fixed layer; and a step of forming a wiring layer connected to the electrode via the opening.

[0024] The invention also includes the step of forming an island of the semiconductor thin film layer that is the same size as the first substrate or smaller than the first substrate, and in the step of forming the island of the semiconductor thin film layer, the island of the semiconductor thin film layer can be formed in such a way that the angle between the direction of the side of the island of the semiconductor thin film layer and the <112> direction of the Si(111) substrate as the first substrate is within the angle range of ±45° or less. In the step of forming the island of the semiconductor thin film layer, the island of the semiconductor thin film layer can be formed in such a way that the angle between the direction of the longest side in the island of the semiconductor thin film layer and the <112> direction of the Si(111) substrate as the first substrate is within the angle range of ±45° or less.

[0025] In the step of forming the islands of the semiconductor thin film layer, the islands of the semiconductor thin film layer can be formed in such a way that the direction of the longest side in the islands of the semiconductor thin film layer composed of hexagonal crystals is within an angle range of ±45° or less relative to the <1-100> direction of the hexagonal crystals.

[0026] In the step of forming the fixed layer, an electrode may be set between the fixed layer and the semiconductor thin film layer. The method for manufacturing the semiconductor element may further include: a step of forming an opening in the fixed layer; and a step of forming a wiring layer connected to the electrode through the opening after the step of bonding the semiconductor thin film layer to the second substrate.

[0027] The manufacturing method may further include, before the step of forming the fixed layer: a step of forming a heterogeneous material layer formed of a material different from the semiconductor thin film layer on the first substrate; and a step of forming the semiconductor thin film layer on the heterogeneous material layer, wherein the difference in lattice constants between the first substrate and the semiconductor thin film layer is smaller than the difference in lattice constants between the semiconductor thin film layer and the heterogeneous material layer.

[0028] The difference in thermal expansion coefficient between the first substrate and the semiconductor thin film layer is, for example, smaller than the difference in thermal expansion coefficient between the semiconductor thin film layer and the heterogeneous material layer. In addition, the etching speed of the heterogeneous material layer relative to a predetermined etching method may be greater than the etching speed of the first substrate and the semiconductor thin film layer relative to the predetermined etching method.

[0029] The manufacturing method may further include, before the step of bonding the semiconductor thin film layer to the second substrate, the step of preparing the second substrate made of a material having a higher thermal conductivity than the first substrate. In the case, the method may include the step of forming a plurality of islands of the semiconductor thin film layer, bonding the plurality of islands of the semiconductor thin film layer to the second substrate in the step of bonding to the second substrate, and after the step of bonding to the second substrate, the method may further include the step of forming wiring for connecting at least any one of the plurality of islands of the semiconductor thin film layer bonded to the second substrate.

[0030] The manufacturing method may further include a step of forming the semiconductor thin film layer before the step of forming the fixed layer, and in the step of forming the semiconductor thin film layer, a step difference structure that is not exposed to the periphery of the semiconductor thin film layer may be formed.

[0031] A semiconductor element according to a second embodiment of the present invention includes: a second substrate different from a first substrate on which a semiconductor thin film layer is formed; the semiconductor thin film layer is bonded to the second substrate; and a fixed layer different from the semiconductor thin film layer, formed in at least a portion of a region between two ends of the semiconductor thin film layer in a first direction of the semiconductor thin film layer. The fixed layer may be formed on the upper surface of the semiconductor thin film layer and on the side surfaces of the semiconductor thin film layer on both sides in the first direction. In the fixed layer, the coverage of the two side surfaces of the semiconductor thin film layer in a second direction orthogonal to the first direction is smaller than the coverage of the two side surfaces of the semiconductor thin film layer in the first direction.

[0032] The semiconductor element may further include: an electrode provided between the fixing layer and the semiconductor thin film layer; and a wiring layer connected to the electrode via an opening formed in the fixing layer.

[0033] In the semiconductor element, the angle at which the longest side among the plurality of sides of the semiconductor thin film layer composed of hexagonal crystals in an island shape is oriented in the <1-100> direction of the hexagonal crystals may be ±45° or less.

[0034] The semiconductor thin film layer may have a step structure that is not exposed to the periphery. In addition, the semiconductor element may include: a plurality of islands of the semiconductor thin film layer bonded to the second substrate; and wiring for connecting at least any one of the plurality of islands of the semiconductor thin film layer.

[0035] Effects of the Invention

[0036] According to the present invention, there is an effect that the step of bonding the moved semiconductor epitaxial layer to another substrate can be made more efficient. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1A This is a diagram for explaining a method of removing an island of a semiconductor thin film layer from a mother substrate.

[0038] Figure 1B This is a diagram for explaining a method of removing an island of a semiconductor thin film layer from a mother substrate.

[0039] Figure 1C This is a diagram for explaining a method of removing an island of a semiconductor thin film layer from a mother substrate.

[0040] Figure 1D This is a diagram for explaining a method of removing an island of a semiconductor thin film layer from a mother substrate.

[0041] Figure 1E This is a diagram for explaining a method of removing an island of a semiconductor thin film layer from a mother substrate.

[0042] Figure 2A It is a diagram showing a pickup substrate as a third substrate.

[0043] Figure 2B yes Figure 2A AA profile.

[0044] Figure 2C It is a diagram showing a modified example of picking up the substrate.

[0045] Figure 3A This is a diagram schematically showing the step of separating islands of a semiconductor thin film layer from a mother substrate.

[0046] Figure 3B This is a diagram schematically showing the step of separating islands of a semiconductor thin film layer from a mother substrate.

[0047] Figure 3C This is a diagram schematically showing the step of separating islands of a semiconductor thin film layer from a mother substrate.

[0048] Figure 3D The figure schematically shows the steps from the separated islands of the semiconductor thin film layer to the transfer destination substrate.

[0049] Figure 3E The figure schematically shows the steps from the separated islands of the semiconductor thin film layer to the transfer destination substrate.

[0050] Figure 3F The figure schematically shows the steps from the separated islands of the semiconductor thin film layer to the transfer destination substrate.

[0051] Figure 4A The figure schematically shows the steps of moving the islands of a plurality of semiconductor thin film layers.

[0052] Figure 4B The figure schematically shows the steps of moving the islands of a plurality of semiconductor thin film layers.

[0053] Figure 4C The figure schematically shows the steps of moving the islands of a plurality of semiconductor thin film layers.

[0054] Figure 4D The figure schematically shows the steps of moving the islands of a plurality of semiconductor thin film layers.

[0055] Figure 4E The figure schematically shows the steps of moving the islands of a plurality of semiconductor thin film layers.

[0056] Figure 5A This is a diagram for explaining a method of moving islands of a plurality of semiconductor thin film layers.

[0057] Figure 5B This is a diagram for explaining a method of moving islands of a plurality of semiconductor thin film layers.

[0058] Figure 5C This is a diagram for explaining a method of moving islands of a plurality of semiconductor thin film layers.

[0059] Figure 5D This is a diagram for explaining a method of moving islands of a plurality of semiconductor thin film layers.

[0060] Figure 5E This is a diagram for explaining a method of moving islands of a plurality of semiconductor thin film layers.

[0061] Figure 6 It is a diagram showing the process flow of the method for manufacturing a semiconductor element according to the present embodiment.

[0062] Fig. 7A This is an example of a modification of the method for manufacturing a semiconductor element.

[0063] Figure 7B This is an example of a modification of the method for manufacturing a semiconductor element.

[0064] Figure 7C This is an example of a modification of the method for manufacturing a semiconductor element.

[0065] Fig.7D This is a cross-sectional view of a semiconductor device taken along line AA.

[0066] Fig. 8A It is a diagram showing the structure of a semiconductor element.

[0067] Figure 8B It is a diagram showing the structure of a semiconductor element.

[0068] Figure 8C It is a diagram showing the structure of a semiconductor element.

[0069] Fig.9A It is a diagram showing a modified example of the shape of the fixing layer.

[0070] Fig. 9B It is a diagram showing a modified example of the shape of the fixing layer.

[0071] Fig. 9C It is a diagram showing a modified example of the shape of the fixing layer.

[0072] Fig.9D It is a diagram showing a modified example of the shape of the fixing layer.

[0073] Fig.10 The figure schematically illustrates a semiconductor epitaxial wafer used as a mother substrate.

[0074] Fig.11AThis is a graph showing the relationship between the angle θ and the etching rate of the Si (111) substrate surface region in the direction perpendicular to the long sides of the islands of the semiconductor thin film layer.

[0075] Fig. 11B It is a diagram for explaining the angle θ.

[0076] Fig.12 A diagram showing hexagonal islands of a semiconductor thin film layer.

[0077] Fig.13A This is a microscopic photograph of islands of a GaN semiconductor thin film layer formed on a Si (111) substrate serving as a base substrate.

[0078] Fig. 13B The direction of the long side of the island of the semiconductor thin film layer relative to the crystal direction of the parent substrate Fig.13A Microscope images of different islands of GaN semiconductor thin film layers.

[0079] Fig.14 This is a microscope photograph showing a state where islands of a semiconductor thin film layer whose long sides are substantially parallel to the <1-100> direction are bonded to a substrate to which they are transferred.

[0080] Fig.15A This is a diagram for explaining a method for making the fixing layer easy to break.

[0081] Fig. 15B This is a diagram for explaining a method for making the fixing layer easy to break.

[0082] Fig.16 This is a microscope photograph showing the result of observing the separation state of the pinning layer in an actual experiment.

[0083] Fig.17 This is a microscope photograph showing a state in which an island of a semiconductor thin film layer separated from a mother substrate is bonded to a transfer destination substrate.

[0084] Fig.18A This is a diagram showing an example of a fixing layer having a region extending in the short-side direction.

[0085] Fig.18B This is a diagram showing an example of a fixing layer having a region extending in the short-side direction.

[0086] Fig.19A It is a diagram schematically showing a state in which a semiconductor thin film layer formed on a mother substrate is divided into islands of individual semiconductor thin film layers, and is a top view of the mother substrate and the islands of semiconductor thin film layers.

[0087] Fig.19B It is a cross-sectional view of the island of the base substrate and the semiconductor thin film layer.

[0088] Fig. 20A 1 is a top view of a semiconductor element including a semiconductor thin film layer having a step structure formed therein that is not exposed to the periphery of an island of the semiconductor thin film layer.

[0089] Fig. 20B yes Fig. 20A AA line cross-sectional view of the semiconductor device shown.

[0090] Fig. 20C yes Fig. 20A The BB line cross-sectional view of the semiconductor device shown.

[0091] Fig.21A This is a diagram for explaining a method of manufacturing a semiconductor device.

[0092] Fig. 21B This is a diagram for explaining a method of manufacturing a semiconductor device.

[0093] Fig. 21C This is a diagram for explaining a method of manufacturing a semiconductor device.

[0094] Fig.21D This is a diagram for explaining a method of manufacturing a semiconductor device.

[0095] Fig.21E This is a diagram for explaining a method of manufacturing a semiconductor device.

[0096] Fig.21F This is a diagram for explaining a method of manufacturing a semiconductor device.

[0097] Figure 21G This is a diagram for explaining a method of manufacturing a semiconductor device.

[0098] Fig.21H This is a diagram for explaining a method of manufacturing a semiconductor device.

[0099] Fig.21I This is a diagram for explaining a method of manufacturing a semiconductor device.

[0100] Fig. 22 It is a diagram used to explain the prior art.

[0101] Description of Figure Numbers

[0102] 101, 401, 501, 701, 801, 901, 1001, 3001: base material substrate

[0103] 102: Predetermined removal layer

[0104] 103, 117, 403a, 403b, 403c, 503a-503c, 703a, 703b, 703c, 703d, 803: gap

[0105] 104: Semiconductor thin film layer

[0106] 106: Area scheduled for removal

[0107] 108, 109, 408a, 408b, 408c, 508a, 508b, 508c, 708a, 708b, 708c, 708d, 718a, 718b, 808, 920: islands / islands of semiconductor thin film layers

[0108] 110, 112, 114, 410a, 410b, 410c, 414a, 414b, 414c, 416a, 416b, 416c, 510a, 510b, 510c, 514a, 514c, 516a, 516c, 705a, 705b, 705c, 705d, 714a, 714b, 814, 928: fixed layer 130, 131, 921, 922, 1002a, 1002b: region

[0109] 200, 200', 420, 520, 710, 930: Pick up substrate

[0110] 201, 421, 521, 711: Base substrate

[0111] 202, 422a, 422b, 422c, 522a, 522c: Pick up bumps

[0112] 204, 712: Pickup layer

[0113] 210, 430, 530: Structure

[0114] 301, 451, 531, 731, 831, 931: Move destination substrate

[0115] 302, 551: Surface

[0116] 308, 558a, 558c: Face

[0117] 742, 744: Component loading area

[0118] 800: Semiconductor components

[0119] 816a, 816b: opening

[0120] 822, 824, 924, 925: Electrodes

[0121] 842, 926: Interlayer insulation film

[0122] 854, 856, 927: Wiring layer

[0123] 923: Outer wall

[0124] 1003: Slot

[0125] 3002: Sacrificial Layer

[0126] 3003: Semiconductor epitaxial layer

[0127] 3004: Support

[0128] 3010: Area where the sacrificial layer is etched

[0129] a, b: side

[0130] L1, L2, L3, L4: Length

[0131] L2a, L2b: Width

[0132] θ: Angle DETAILED DESCRIPTION

[0133] [Overview of Method for Manufacturing Semiconductor Element]

[0134] In the method for manufacturing a semiconductor element of the present embodiment, an island of a semiconductor thin film layer on a mother substrate as a first substrate is moved to a destination substrate as a second substrate, thereby manufacturing a semiconductor element having a destination substrate and a semiconductor thin film layer. An "island of a semiconductor thin film layer" is a region of a semiconductor thin film layer of the same size as a mother substrate, or a region of a semiconductor thin film layer smaller than a mother substrate. An island of a semiconductor thin film layer may be formed on one mother substrate, or an island of a plurality of semiconductor thin film layers may be formed.

[0135] The manufacturing method of the semiconductor element of the present embodiment is characterized in that: a fixing layer is formed to support the island of the semiconductor thin film layer when the island of the semiconductor thin film layer is separated from the mother substrate, so that when the island of the semiconductor thin film layer is separated from the mother substrate in order to move the island of the semiconductor thin film layer from the mother substrate to the moving destination substrate, the island of the semiconductor thin film layer can maintain a stable state on the mother substrate. In this way, after the island of the semiconductor thin film layer is connected to the organic layer formed on the pickup substrate as the third substrate, the island of the semiconductor thin film layer can be separated from the mother substrate, and the separated island of the semiconductor thin film layer can be moved to the second substrate.

[0136] [Step of removing the island of semiconductor thin film layer from the mother substrate]

[0137] Figure 1A to Figure 1E This is a diagram for explaining a method of removing the island of the semiconductor thin film layer from the mother substrate. Figure 1A to Figure 1E An overview of a method for removing islands of semiconductor thin film layers from a mother substrate will be described.

[0138] First, if Figure 1A As shown, a planned removal layer 102 is formed on a mother substrate 101 as a first substrate, and a semiconductor thin film layer 104 as a semiconductor epitaxial layer is formed on the planned removal layer 102. The planned removal layer 102 is a region to be removed by etching in a subsequent step.

[0139] The planned removal layer 102 is, for example, formed of a material having an etching rate different from that of the mother substrate 101 and the semiconductor thin film layer 104 when etching is performed using a predetermined etching method (wet etching using a predetermined etching solution or dry etching using a predetermined gas). The planned removal layer 102 may also be formed of the same material as the mother substrate 101. For example, the planned removal layer 102 may be a partial region near the surface of the mother substrate 101.

[0140] The semiconductor thin film layer 104 is, for example, a semiconductor thin film layer formed by epitaxial growth or a semiconductor thin film layer formed by wafer bonding. The semiconductor thin film layer 104 may also be a semiconductor thin film layer formed by other methods.

[0141] The semiconductor thin film layer 104 is, for example, a III-V compound semiconductor material (such as GaAs, AlGaAs, InGaAs, InP, InAlGaP, etc.), a III-nitride semiconductor material (such as GaN, InN, AlGaN, InGaN, AlN, etc.), an oxide semiconductor material (such as ZnO, Ga2O3, etc.), a IV-compound semiconductor material (such as SiC, etc.), diamond, Si or SiGe, etc. The parent substrate 101 is, for example, a III-V compound semiconductor material substrate (such as a GaAs substrate, InP substrate, etc.), a III-nitride semiconductor material substrate (such as a GaN substrate), an oxide semiconductor material substrate (such as a ZnO substrate, Ga2O3 substrate, etc.), a IV-compound semiconductor substrate (such as SiC, etc.), a diamond substrate, or Si, SiGe, etc.

[0142] Then, if Figure 1B As shown, the semiconductor thin film layer 104 is divided into a plurality of island regions to form an island 108 of the semiconductor thin film layer (hereinafter, "island 108 of the semiconductor thin film layer" is sometimes referred to as "island 108"). The shape of the island 108 is not limited, and the following description exemplifies the case where the island 108 is a rectangle. The island 108 may be, for example, a square or a hexagon. Furthermore, instead of dividing the semiconductor thin film layer 104 into a plurality of island regions, a single or multiple islands 108 may be formed by selectively growing the semiconductor thin film layer 104 on the mother substrate 101.

[0143] The method of forming the island 108 is arbitrary, and the following method can be exemplified.

[0144] 1) Method for forming island 108 by processing semiconductor thin film layer 104 through photolithography / etching steps

[0145] 2) Method for selectively growing the semiconductor thin film layer 104 on the mother substrate 101

[0146] 3) A method of growing the semiconductor thin film layer 104 laterally along the lateral direction (horizontal direction) on the mother substrate 101

[0147] Hereinafter, one of the islands 108 of the plurality of semiconductor thin film layers will be described. Figure 1B As shown, the predetermined removal layer 102 may also be formed into an island 108. The region of the predetermined removal layer 102 included in the island 108 is Figure 1B A predetermined removal area 106 is shown.

[0148] Then, if Figure 1C and Figure 1D As shown, a fixing layer 110 is formed as a thin film, and the fixing layer 110 combines at least a portion of the main surface of the island 108 on the opposite side to the mother substrate 101 with at least a portion of the surface on the island 108 side of the mother substrate 101. The fixing layer 110 is, for example, in a shape extending between the upper surface of the island 108 and the mother substrate 101, but the fixing layer 110 may also be in other shapes as long as it can combine the island 108 with the mother substrate 101. For example, the fixing layer 110 may also be composed of two thin films that combine the area of ​​the island 108 including the two side surfaces in the length direction with the mother substrate 101. In addition, the fixing layer 110 may also be a thin film that extends in the short side direction of the island 108 in a manner that crosses the island 108 with the mother substrate 101 as the starting point and the end point. In addition, the fixing layer 110 may be parallel to the side of the island 108, or may be formed to extend in a direction different from the direction of the side of the island 108.

[0149] In the case of forming the fixing layer 110 extending in the length direction of the island 108, in the step of forming the fixing layer 110, the fixing layer 110 is formed in such a manner that the fixing layer 110 extends between the two ends of the semiconductor thin film layer 104 in a first direction (the direction is, for example, a direction connecting the two side surfaces with high coverage of the semiconductor thin film layer 104) on the main surface of the semiconductor thin film layer 104, and the semiconductor thin film layer 104 is exposed in at least a part of the two side surfaces of the semiconductor thin film layer 104 in a second direction orthogonal to the first direction. In the case of the island 108 being rectangular, the coverage of the side surfaces of the long sides of the island 108 by the fixing layer 110 is smaller than the coverage of the side surfaces of the short sides. In this manner, when etching described later is performed, the time until the island 108 or a part of the parent substrate 101 or a part of the layer between the island 108 and the parent substrate 101 is removed in order to separate the island 108 from the parent substrate 101 can be shortened.

[0150] Figure 1D For Figure 1C The fixing layer 110 has the function of retaining the island 108 above the mother substrate 101 in such a way that the position of the island 108 on at least the mother substrate 101 directly below remains unchanged. The fixing layer 110 is a thin film layer containing a material that has etching resistance relative to the etching means used to etch the predetermined removal area 106.

[0151] As a material of the fixing layer 110, for example, an oxide film (such as Si x O y 、Si x O y N z 、Al x O y 、Al x O y N z etc.), or nitride films (such as Si x N y 、Al x N y The inorganic insulating film may be a single layer or a stack of different materials. For example, the inorganic insulating film is formed by chemical vapor deposition (CVD) and a portion of the inorganic insulating film is removed by standard photolithography and etching processes, thereby forming the desired fixed layer 110. When forming the fixed layer 110, an organic film (such as a photosensitive coating film, a photosensitive organic sheet, etc.) may be used as the material of the fixed layer 110 if it has resistance to a predetermined etching means for etching the predetermined removal area 106.

[0152] The thickness of the fixing layer 110 can be selected to the most suitable thickness according to the size and thickness of the island 108 of the semiconductor thin film layer. The film thickness of the fixing layer 110 is, for example, a thickness thinner than the thickness of the island 108 of the semiconductor thin film layer (i.e., the thickness of the semiconductor thin film layer 104 formed on the mother substrate 101). The thickness of the fixing layer 110 is preferably a thickness that is cut between the fixing layer 110 formed on the mother substrate 101 and the fixing layer 110 formed on the side of the semiconductor thin film layer by the force of moving the pickup substrate 200 in a direction away from the mother substrate 101 while the pickup substrate 200 as the third substrate described later is bonded to at least a portion of the bonding area of ​​the fixing layer 110 and the semiconductor thin film layer 104.

[0153] Figure 1D The island 108 of the semiconductor thin film layer shown has sides of lengths L1 and L2, and L1>L2. The fixed layer 110 has a first region covering the upper surface of the island 108, a second region covering the right side of the island 108, and a third region covering the left side of the island 108. The fixed layer 110 also has a region covering the parent substrate 101 before having the second region and the third region. Figure 1D In the example shown, the fixed layer 110 does not cover the long side surfaces (i.e., the side surfaces with a length of L1) of the four side surfaces of the island 108, and covers a portion of the short side surfaces (i.e., the side surfaces with a length of L2).

[0154] Then, if Figure 1E As shown, the void 103 is formed by removing a portion of the island 108 or the mother substrate 101, or a portion of the predetermined removal region layer between the island 108 and the mother substrate 101. For example, the region of the island 108 connected to at least the mother substrate 101 directly below is etched away, thereby forming the void 103 in at least the region directly below the island 108 between the island 108 and the mother substrate 101. When forming the void 103, it is desirable to use an etching solution or etching gas whose etching rate of the island 108 relative to the etching solution or etching gas used is at least less than the etching rate of the predetermined removal region 106.

[0155] In the etching step, for example, when the etching of the predetermined removal region layer is performed isotropically and the etching speed is not affected by the direction, the etching distance in the direction perpendicular to the long side of the island 108 is short, so the etching ends earlier than the etching in the direction perpendicular to the short side. Therefore, by opening the side of the long side, or by forming the fixed layer 110 in a manner that the coverage of the fixed layer 110 on the long side becomes smaller than the coverage of the fixed layer 110 on the short side, the etching can be ended more quickly to form the gap 103. In this way, in the etching step for removing the predetermined removal region 106, the risk of etching damage in the island 108 can be reduced.

[0156] Furthermore, in the above description, the case where the void 103 is formed by removing the planned removal layer 102 by etching is exemplified, but the void may also be formed by removing the surface region of the mother substrate 101 by anisotropic etching without forming the planned removal layer 102 .

[0157] In the case where the void is formed by removing an area of ​​the surface of the mother substrate 101 by anisotropic etching, in the step of forming the fixed layer, it is preferred that the two side surfaces in the direction with a high etching speed are set to the second direction. The two side surfaces in the second direction may be completely exposed as a whole, or a part of the area may be covered by the fixed layer 110. Moreover, it is preferred to form the fixed layer 110 in such a manner that the coverage of the two side surfaces in the second direction of the semiconductor thin film layer 104 by the fixed layer 110 extending in the second direction becomes smaller than the coverage of the two side surfaces in the first direction of the semiconductor thin film layer 104 by the fixed layer 110 extending in the first direction. In this way, the void 103 can be easily formed by etching.

[0158] In the above description, the case where the island 108 of the semiconductor thin film layer is rectangular is exemplified. However, the island 108 may be square in the following case.

[0159] 1) When the semiconductor thin film layer is separated from the mother substrate by removing the planned removal layer 102 by etching

[0160] 2) When anisotropic etching is used to remove the surface region of the mother substrate 101

[0161] 3) When the size of the island 108 is very small (for example, less than 20 μm)

[0162] [Step of separating the islands 108 of the semiconductor thin film layer]

[0163] Figure 2A The figure shows a pickup substrate 200 as a third substrate for separating the islands 108 of the semiconductor thin film layer from the mother substrate 101 . Figure 2B yes Figure 2A AA section. Figure 2B As shown, the pickup substrate 200 has a base substrate 201 and a pickup bump 202 formed on the base substrate 201 and containing an organic material. As the base substrate 201, for example, a transparent substrate such as quartz, sapphire, glass, etc.; a semiconductor substrate such as Si; a ceramic substrate; or a metal substrate, etc. can be selected. The base substrate 201 can be a single material or a laminated material. In addition, the base substrate 201 can also be a substrate coated with other materials on the surface.

[0164] The pickup bump 202 is, for example, an organic material layer, and can be formed by coating a photosensitive organic material on the base substrate 201 and using a standard photolithography process. The organic material layer can be formed by coating the pickup base substrate, for example, by spin coating, dipping, etc., or by attaching an organic material film to the pickup base substrate.

[0165] The structure of the pickup substrate may be variously modified according to the shape or size of the picked-up island 108. For example, the pickup substrate may have other structures inserted between the base substrate 201 and the pickup bump 202. Figure 2C As shown in the pickup substrate 200 ′, the pickup substrate 200 ′ does not have the pickup bumps 202 corresponding to the shape of the islands 108 to be separated from the mother substrate 101 , but has a flat pickup layer 204 having a larger area than the islands 108 .

[0166] Figure 3A to Figure 3C The figure schematically shows a step of separating the island 108 from the mother substrate 101 using the pickup substrate 200 .

[0167] First, if Figure 3A As shown, the pickup bump 202 of the pickup substrate 200 is aligned with the island 108. Specifically, the pickup substrate 200 is disposed at a position where at least a portion of the fixed layer 110 and the island 108 overlaps with at least a portion of the pickup bump 202.

[0168] Then, if Figure 3B As shown, the pickup bump 202 is brought into contact with or pressed against at least a portion of the fixing layer 110 and the island 108. Thus, the pickup bump 202 is connected to at least a portion of the fixing layer 110 and the island 108. If the pickup substrate 200 is brought into contact with the fixing layer 110 and the island 108 and a downward force is applied while the gap 103 is formed between the island 108 and the mother substrate 101, the pick-up bump 202 is pressed against the fixing layer 110 and the island 108. Figure 3B As shown in the dotted line portion, cracks are generated in the fixing layer 110 or the fixing layer 110 is broken.

[0169] In a state where cracks are generated in the fixing layer 110 or the fixing layer 110 is broken, as shown in FIG. Figure 3C As shown, by lifting the pickup substrate 200 which is connected to a partial area of ​​the fixed layer 110, the fixed layer 110 is separated into a fixed layer 114 connected to the island 108 and a fixed layer 112 connected to the mother substrate 101, so that the island 108 of the semiconductor thin film layer and the fixed layer 114 which is a partial area of ​​the fixed layer 110 can be separated from the mother substrate 101.

[0170] Furthermore, the island 108 may be separated from the mother substrate 101 in a state where a semiconductor layer made of a material different from the semiconductor thin film layer 104 is present on the surface of the island 108 on the mother substrate 101 side after separation from the mother substrate 101. For example, the island 108 separated from the mother substrate 101 may be accompanied by a mask film or a dielectric layer provided on the mother substrate 101 for selectively growing or lateral growing the semiconductor thin film layer 104.

[0171] [Step of bonding the island 108 of the semiconductor thin film layer to another substrate]

[0172] Figure 3D to Figure 3F Schematically shows the steps of bonding the separated island 108 to the transfer destination substrate 301. Figure 3D As shown, the structure 210 in which the islands 108 and the fixing layer 114 are connected to the pickup substrate 200 is positioned at a predetermined position above the transfer destination substrate 301 as the second substrate.

[0173] Afterwards, if Figure 3E As shown, the surface 308 of the island 108 below the fixed layer 114 in the structure 210 is pressed against the moving destination substrate 301, thereby bonding the island 108 to the moving destination substrate 301. Before the step of pressing the island 108 against the moving destination substrate 301, the bonding surfaces (the surface 308 of the island 108 of the semiconductor thin film layer and the surface 302 of the moving destination substrate 301) may be appropriately surface treated.

[0174] Then, if Figure 3F As shown, the pickup bumps 202 and the base substrate 201 are removed from the fixing layer 114. For example, the fixing layer 114 and the base substrate 201 can be separated by dipping in a liquid such as an organic solvent that dissolves the organic material constituting the pickup bumps 202 to dissolve the pickup bumps 202.

[0175] Furthermore, in the step of pressing the island 108 onto the destination substrate 301, if the destination substrate 301 and the island 108 are firmly bonded, the pickup substrate 200 may be lifted before the pickup bumps 202 are dissolved using a chemical liquid such as an organic solvent. In such a case, after the pickup substrate 200 is lifted, a step of cleaning the destination substrate 301 bonded with the island 108 using a chemical liquid such as an organic solvent may be added.

[0176] Furthermore, in the island 108 bonded to the transfer destination substrate 301, a predetermined element structure or a part of the element structure may be formed before the step of forming the fixing layer 110. In addition, after the island 108 is bonded to the transfer destination substrate 301, the fixing layer 110 may be processed, or an interlayer insulating film may be formed on the semiconductor thin film layer, or a wiring structure electrically connected to an external structure may be formed.

[0177] In the above description, the island 108 is bonded to the surface of the destination substrate 301, but another layer (an inorganic material thin film layer or an organic material thin film layer, etc.) may be provided between the destination substrate 301 and the island 108. In addition, a heat treatment step may be provided after the bonding step.

[0178] Furthermore, when the island 108 separated from the mother substrate 101 is bonded to the destination substrate 301, the island 108 may be bonded to the destination substrate 301 in a state where a semiconductor layer of a material different from the semiconductor thin film layer 104 is present on the surface of the island 108 that is bonded to the destination substrate 301. For example, the island 108 may be bonded to the destination substrate 301 in a state where a mask film or a dielectric layer for selective growth or lateral growth of the semiconductor thin film layer 104 that is provided on the mother substrate 101 is present.

[0179] [Method of moving multiple islands 108]

[0180] In the above description, the method of moving the island 108 of a semiconductor thin film layer is described. However, in the method of manufacturing a semiconductor element of this embodiment, it is also possible to move the island 108 of a semiconductor thin film layer by moving .... Figure 4A to Figure 4E The islands 408a, 408b, 408c of the semiconductor thin film layer are moved as shown. When the plurality of islands 408a, 408b, 408c are separated from the mother substrate 401 in batches, a pickup substrate 420 including a plurality of pickup bumps 422a, 422b, 422c corresponding to the plurality of islands 408a, 408b, 408c is prepared. Then, the pickup substrate 420 is brought into contact with or pressed against the fixing layers 410a, 410b, 410c and the islands 408a, 408b, 408c by the same steps as the above steps, and the plurality of islands 408a, 408b, 408c are separated from the mother substrate 401, and the plurality of islands 408a, 408b, 408c are bonded to the moving destination substrate 451.

[0181] Figure 4A to Figure 4E Schematically shows the steps of moving the plurality of islands 408a, 408b, 408c. Figure 4A to Figure 4EIn the embodiment, a mother substrate 401, a plurality of gaps 403a, 403b, 403c, a plurality of islands 408a, 408b, 408c, a plurality of fixed layers 410a, 410b, 410c, a plurality of fixed layers 414a, 414b, 414c, a plurality of fixed layers 416a, 416b, 416c, a pickup substrate 420, a base substrate 421, a plurality of pickup bumps 422a, 422b, 422c, a structure 430, and a moving destination substrate 451 are respectively connected to Figure 3A to Figure 3F The mother substrate 101, the gap 103, the island 108, the fixing layer 110, the fixing layer 114, the fixing layer 112, the pickup substrate 200, the base substrate 201, the pickup bump 202, the structure 210 and the transfer destination substrate 301 correspond to each other. When the plurality of islands 408a, 408b, 408c are separated from the mother substrate 401, the following method can also be used: Figure 2C A pickup substrate is shown without pickup bumps and comprising a pickup layer comprising an organic material.

[0182] [Movement of multiple semiconductor thin film layers]

[0183] Figure 5A to Figure 5E This is a diagram for explaining a method of moving islands of multiple semiconductor thin film layers. Figure 5A to Figure 5E In the embodiment, a mother substrate 501, a plurality of gaps 503a, 503b, 503c, a plurality of islands 508a, 508b, 508c, a plurality of fixed layers 510a, 510b, 510c, a plurality of fixed layers 514a, 514c, a plurality of fixed layers 516a, 516c, a pickup substrate 520, a base substrate 521, a plurality of pickup bumps 522a, 522c, a structure 530, a moving destination substrate 531, and a surface 551 are respectively connected to Figure 3A to Figure 3F 1, the mother substrate 101, the gap 103, the island 108, the fixing layer 110, the fixing layer 114, the fixing layer 112, the pickup substrate 200, the base substrate 201, the pickup bump 202, the structure 210, the transfer destination substrate 301 and the surface 302 correspond to each other. Hereinafter, a method of selecting a part of the islands of a plurality of semiconductor thin film layers formed on the mother substrate and moving them to the transfer destination substrate will be described.

[0184] like Figure 5A As shown, after forming the gaps 503a to 503c at least directly below the islands of the semiconductor thin film layer, pick-up bumps 522a and 522c made of organic material are provided on the base substrate 521 of the pick-up substrate 520 only at positions corresponding to the islands 508a and 508c of the selected semiconductor thin film layer. Then, the pick-up bumps 522a and 522c are brought into contact or pressed against the islands 508a and 508c, thereby connecting the pick-up substrate 520 to the selected islands 508a and 508c. Figure 5B for Figure 5A A top view of Figure 5B The AA profile is equivalent to Figure 5A .

[0185] Then, if Figure 5C As shown, the pick-up substrate 520 connected to the selected island 508 a and the island 508 c is lifted up, so that only the selected island 508 a and the island 508 c are separated from the mother substrate 501 . Figure 5C 5 is a diagram showing a state where the selected islands 508a and 508c are lifted by picking up the substrate 520. Figure 5C As shown, unselected islands 508 b remain on the mother substrate 501 .

[0186] Then, if Figure 5D As shown, the structure of the island 508a, the island 508c, the fixed layer 514a and the fixed layer 514c is connected on the pickup substrate 520 ( Figure 5C The structure 530 shown in FIG. 1 is arranged at a predetermined position on the destination substrate 531. Then, the surfaces 558a and 558c of the islands 508a and 508c on the opposite sides to the fixing layers 514a and 514c are pressed against the surface 551 of the destination substrate 531, thereby bonding the selected islands 508a and 508c to the destination substrate 531.

[0187] Next, the pick-up bumps 522a, the pick-up bumps 522c, and the base substrate 521 are removed from the destination substrate 531, thereby manufacturing a Figure 5E As shown in the figure, semiconductor elements including islands 508a and 508c of semiconductor thin film layers are bonded to the transfer destination substrate 531.

[0188] [Process flow of semiconductor device manufacturing method]

[0189] Figure 6 1 is a diagram showing a process flow of a method for manufacturing a semiconductor device according to this embodiment. Figure 6 As shown, in the method for manufacturing a semiconductor element of the present embodiment, a pickup substrate 520 including pickup bumps 522a and 522c of an organic material corresponding to islands 508a and 508c of a predetermined selected semiconductor thin film layer on a mother substrate 501 can be used to separate the selected islands 508a and 508c from the mother substrate 501 and bond them to a transfer destination substrate 531. In this way, the desired islands 508a and 508c can be selected from a plurality of islands 508a, 508b, and 508c on the mother substrate 501 and bonded to the transfer destination substrate 531.

[0190] It is obvious that various modifications can be made to the separation pattern for separating desired islands 508a and 508c from the mother substrate 501 among the plurality of islands 508a, 508b, and 508c on the mother substrate 501.

[0191] [Effects of the method for manufacturing a semiconductor device according to the present embodiment]

[0192] According to the manufacturing method of the semiconductor element described above, the island 108 of the semiconductor thin film layer fixed to the mother substrate 101 by the fixing layer 110 is separated from the mother substrate 101 using the pickup substrate 200 including the pickup bump 202 formed by photolithography and using an organic material on the base substrate 201, and the island 108 of the semiconductor thin film layer connected to the pickup substrate 200 is pressed and bonded to the transfer destination substrate 301. In this way, the semiconductor thin film layer 104 separated from the mother substrate 101 can be easily moved to another substrate.

[0193] In addition, it is obvious to those skilled in the art that the pickup substrate 200 including the pickup bumps 202 of the most suitable shape and size can be easily manufactured corresponding to the island 108 of the semiconductor thin film layer separated from the mother substrate 101. According to the method for manufacturing a semiconductor element of this embodiment, the island 108 of the semiconductor thin film layer can be separated from the mother substrate 101 and joined to the transfer destination substrate 301 using the easily manufactured pickup substrate 200, so that the island 108 of the semiconductor thin film layer can be moved at a low cost.

[0194] Furthermore, after the island 108 of the semiconductor thin film layer is bonded to the mobile destination substrate 301, the pickup bump 202 including the organic material and the base substrate 201 of the pickup substrate 200 are removed from the mobile destination substrate 301, thereby achieving the effect of repeatedly reusing the base substrate 201.

[0195] Furthermore, as described above, when the pinned layer 110 is formed to extend in the longitudinal direction of the island 108, the following effects are produced.

[0196] (1) When an etching solution or an etching gas is used in the step of forming a gap between the island 108 of the semiconductor thin film layer and the mother substrate 101, the surface of the semiconductor thin film layer and the element structures such as electrodes and wiring formed on the island 108 of the semiconductor thin film layer can be protected.

[0197] (2) In the step of forming a gap between the island 108 of the semiconductor thin film layer and the mother substrate 101 and then bonding to the destination substrate 301, the amount of warping of the island 108 of the semiconductor thin film layer due to the stress applied to the island 108 of the semiconductor thin film layer can be reduced. If the warping of the island 108 of the semiconductor thin film layer is reduced by adjusting in a manner to reduce the stress, for example, even in a state where a gap is formed, it is easy to hold the island 108 of the semiconductor thin film layer on the mother substrate 101 by the fixing layer 110. As a result, it is easy to separate the island 108 of the semiconductor thin film layer by the pickup substrate 200, and it is easy to hold the island 108 of the semiconductor thin film layer on the destination substrate 301 in the bonding step on the destination substrate 301.

[0198] (3) In the element forming step after bonding to the transfer destination substrate 301, the fixing layer 110 can be used as an interlayer insulating film or the like between the wiring layer and the semiconductor thin film layer.

[0199] (4) When a wiring layer is formed on the fixing layer 110 in the element forming step after bonding to the transfer destination substrate 301, disconnection of the wiring layer at a step existing when the fixing layer 110 is discontinuous can be prevented.

[0200] (5) It is easy to ensure the uniformity of the characteristics of the semiconductor element formed using the island 108 of the semiconductor thin film layer bonded to the transfer destination substrate 301. When the surface of the island 108 of the semiconductor thin film layer is covered with a continuous fixing layer 110, for example, the intensity distribution of light emitted from the upper surface of the light-emitting element becomes uniform. When it is covered with a discontinuous fixing layer 110, the light intensity changes in the discontinuous region of the fixing layer 110.

[0201] Furthermore, in the above description, the shape of the semiconductor thin film layer is described as a rectangular shape, but in addition to the rectangular shape, it can also be a circular shape or a complex shape. In addition, in the above description, a simple semiconductor thin film layer without an element structure is illustrated (illustrated), but the semiconductor thin film layer can also have an element structure. In addition, the surface of the semiconductor thin film layer can also be uneven and include a thin film structure of a dielectric material or a metal material corresponding to the element structure.

[0202] [Variation of the method for manufacturing a semiconductor element]

[0203] Figure 7A to Figure 7D This is an example of a modified example of a method for manufacturing a semiconductor element. Figure 7A to Figure 7DIn the embodiment, a mother substrate 701, a plurality of gaps 703a, 703b, 703c, 703d, a plurality of islands 708a, 708b, 708c, 708d, 718a, 718b, a plurality of fixed layers 705a, 705b, 705c, 705d, a plurality of fixed layers 714a, 714b, a pickup substrate 710, a base substrate 711, a pickup layer 712, and a moving destination substrate 731 are respectively connected to Figure 2C , Figure 3A to Figure 3F The mother substrate 101, the gap 103, the island 108, the fixing layer 110, the fixing layer 114, the pickup substrate 200, the base substrate 201, the pickup layer 204 and the moving destination substrate 301 correspond to each other. Fig. 7A and Figure 7B ( Figure 7B for Fig. 7A As shown in the AA cross-sectional view of FIG. 7 , a predetermined portion of the plurality of islands (e.g., islands 708a, 708b, 708c, 708d, 718a, and 718b) of the plurality of semiconductor thin film layers on the mother substrate 701 may be separated from the mother substrate. Figure 7C and Fig.7D ( Fig.7D for Figure 7C As shown in the AA cross-sectional view of FIG. 7 , the island ( Figure 7C 708a, 708b, 718a, 718b) are well bonded to a portion of the area ( Figure 7C A predetermined position on the destination substrate 731 where other components are mounted (in the component mounting area 742, the component mounting area 744).

[0204] [Production sequence of composite material components]

[0205] Figure 8A to Figure 8C 1 is a diagram showing the structure of a semiconductor element 800 manufactured using the manufacturing method of the semiconductor element. The semiconductor element 800 is a composite material element manufactured by the manufacturing method. The semiconductor element 800 can be manufactured by separating the island 808 of the semiconductor thin film layer having the element structure formed on the mother substrate from the mother substrate 801 and bonding it to the transfer destination substrate 831, and forming wiring connected to the outside of the semiconductor thin film layer. The example shown here is only one example, and it can be applied to semiconductor elements of various types, materials, and structures.

[0206] Fig. 8A FIG. 8 shows a cross-sectional structure of a semiconductor element 800. Fig. 8A, an island 808 of a semiconductor thin film layer is shown; an electrode 822 and an electrode 824 formed on the island 808; a fixed layer 814 including openings 816a and 816b at the electrode positions; an interlayer insulating film 842, a wiring layer 854, and a wiring layer 856.

[0207] When manufacturing the semiconductor element 800, after forming a semiconductor thin film layer for forming a predetermined element on a mother substrate, electrodes 822 and 824 are formed, or the islands 808 of the semiconductor thin film layer are divided (element separation), thereby forming an element structure. Figure 8B The fixing layer 814 is formed as shown. Furthermore, a gap 803 is formed at least between the mother substrate 801 and the island 808. The gap 803 is formed by etching away the area to be removed.

[0208] Thereafter, after connecting a pickup substrate including a pickup bump or a pickup layer including an organic material to the island 808 and a portion of the fixing layer 814, the island 808 is separated from the mother substrate 801. Thereafter, it is joined to a predetermined position on the mobile destination substrate 831. The mobile destination substrate 831 may also be made of a material different from that of the mother substrate 801 or the island 808, for example. Before joining, the joined surfaces (the joining surface of the island and the surface of the mobile destination substrate) may be subjected to surface treatment for joining as needed. Although not shown in the figure, other thin film layers may also be provided between the mobile destination substrate 831 and the island 808.

[0209] After the island 808 is bonded to the destination substrate 831, as shown in FIG. Figure 8C As shown in FIG. 1 , openings are formed in the fixed layer 814 serving as an insulating film at the positions of the electrodes 822 and 824 on the island 808. Thereafter, an interlayer insulating film 842 for wiring formation is formed, and as shown in FIG. Fig. 8A Wiring layers 854 and 856 are formed as shown, and are respectively bonded to electrodes 822 and 824. In this way, the semiconductor device 800 in which the fixing layer 814 extends on the upper surface of the island 808 and on both side surfaces of the island 808 in the first direction is completed.

[0210] As described above, according to the method for manufacturing a semiconductor element of the present embodiment, the island of the semiconductor thin film layer including the element formed on the mother substrate can be well separated from the mother substrate, and can be well bonded to the mobile destination substrate, so that a composite material element with high performance and high reliability can be obtained. Various forms of the size, structure, etc. of the semiconductor thin film layer included in the semiconductor element can be applied to the manufacturing method. The pickup bumps containing organic materials included in the pickup substrate are made, for example, by standard photolithography, so the most suitable pickup substrate can be easily prepared corresponding to various changes in the element structure and the shape of the semiconductor thin film layer, as well as various changes in the shape of the mobile destination substrate. In this way, according to the method for manufacturing a semiconductor element of the present embodiment, the separation of the most suitable semiconductor thin film layer from the mother substrate and the bonding on the mobile destination substrate can be easily achieved.

[0211] [Modification of the shape of the fixing layer 110]

[0212] FIG. 9A to FIG. 9D 1 and 2 are diagrams showing modified examples of the shape of the fixing layer 110 .

[0213] like Fig.9A As shown, the width L2b of the fixing layer 110 provided on the mother substrate 101 and the width L2b of the fixing layer 110 on the side of the island 108 covering the semiconductor thin film layer can be made narrower than the width L2a of the fixing layer covering the upper surface of the island 108. In this way, when the island 108 is removed from the mother substrate 101 by picking up the substrate 200, the fixing layer 110 provided on the mother substrate 101 and the fixing layer 110 provided on the island 108 are easily separated.

[0214] In the case described, Fig. 9B As shown, in the form of the composite material element bonded to the destination substrate 301, the width L2b of the fixing layer 114 on the side of the short side of the island 108 covering the semiconductor thin film layer is also narrower than the width L2a of the fixing layer 114 covering the upper surface.

[0215] In addition, if Fig. 9C As shown, in the long side region of the fixing layer 110 of the island 108 covered with the semiconductor thin film layer, a region 130 which is a part of the side surface of the long side of the island 108 covered with the semiconductor thin film layer and extends toward the mother substrate 101 can be provided. In this case, it is preferred that the coverage rate of the side surface of the long side by the fixing layer 110 is smaller than the coverage rate of the short side. In the above case, Fig.9D As shown, in the state where the island 108 of the semiconductor thin film layer is bonded to the transfer destination substrate 301, a region 131 of the fixing layer 110 is formed to cover a part of the side surface of the long side of the island 108 of the semiconductor thin film layer. In this state, the coverage of the side surface of the long side by the fixing layer 110 is smaller than the coverage of the short side.

[0216] [Reduction of Lattice Defects in Semiconductor Thin Film Layer 104]

[0217] During the process of forming a GaN epitaxial layer on a Si wafer, crystal defects are sometimes introduced into the semiconductor thin film layer 104 due to the lattice mismatch between the material of the mother substrate 101 and the material of the semiconductor thin film layer, and the mismatch between the thermal expansion coefficients (difference in thermal expansion coefficients) between the material of the mother substrate 101 and the material of the semiconductor thin film layer.

[0218] In order to solve this problem, as the mother substrate 101, a material of the same system as the semiconductor thin film layer can be used. In the above case, it is difficult to separate the semiconductor thin film layer from the mother substrate 101 by etching. Therefore, a semiconductor wafer having a heterogeneous material layer with a large difference in etching rate between the mother substrate 101 and the semiconductor thin film layer 104 can be used as the first substrate. In addition, a semiconductor wafer having a heterogeneous material layer composed of materials with different lattice constants and thermal expansion coefficients between the mother substrate 101 and the semiconductor thin film layer 104 can also be used as the first substrate. As the material of the heterogeneous material layer, for example, Si can be used. In the above case, it is preferred to set the upper limit of the thickness of the heterogeneous material layer provided between the mother substrate 101 and the semiconductor thin film layer 104 to be the same as the thickness of the semiconductor thin film layer 104.

[0219] The difference in lattice constant between the mother substrate 101 and the semiconductor thin film layer 104 is, for example, smaller than the difference in lattice constant between the semiconductor thin film layer 104 and the heterogeneous material layer. In addition, the difference in thermal expansion coefficient between the mother substrate 101 and the semiconductor thin film layer 104 is, for example, smaller than the difference in thermal expansion coefficient between the semiconductor thin film layer 104 and the heterogeneous material layer.

[0220] When the mother substrate 101 is, for example, a GaN substrate, the heterogeneous material layer is, for example, formed of Si (111), and the semiconductor thin film layer 104 is, for example, formed of GaN, the thermal expansion coefficient of GaN, 2.59 ppm, is smaller than the thermal expansion coefficient of Si (111), 5.59 ppm, and therefore, sometimes a stress causing warping on the lower side (stress in the direction of protruding to the upper side) is generated in the mother substrate 101, and a stress causing warping on the upper side (stress in the direction of protruding to the lower side) is generated in the semiconductor thin film layer 104, in contrast to the mother substrate 101. In this way, by generating stresses in opposite directions in the mother substrate 101 and the semiconductor thin film layer 104, respectively, the mother substrate 101 and the semiconductor thin film layer 104 are less likely to warp.

[0221] Furthermore, by setting the upper limit of the thickness of the heterogeneous material layer provided between the mother substrate 101 and the semiconductor thin film layer 104 to be the same as that of the semiconductor thin film layer 104, even if the thermal expansion coefficient of the heterogeneous material layer provided between the mother substrate 101 and the semiconductor thin film layer 104 is different from that of the semiconductor thin film layer 104, the influence of the mother substrate 101 having a small difference in thermal expansion coefficient with the semiconductor thin film layer 104 is dominant in the influence of the thermal stress of the substrate (the stacked structure of the mother substrate 101 and the thin heterogeneous material layer) on the semiconductor thin film layer 104. Therefore, the influence of the thermal stress caused by the heterogeneous material layer on the semiconductor thin film layer 104 can be suppressed to be small. As a result, the lattice defects of the semiconductor thin film layer 104 can be reduced.

[0222] In addition, the etching rate of the heterogeneous material layer with respect to the predetermined etching method is greater than the etching rate of the mother substrate 101 and the semiconductor thin film layer 104 with respect to the predetermined etching method. In this way, a semiconductor thin film layer 104 with fewer lattice defects can be formed, and by using the heterogeneous material layer, Figure 1C The predetermined removal area 106 shown can effectively form the gap 103.

[0223] [Modification of the Material of the Destination Substrate 301]

[0224] When the chip size of the semiconductor element is large, the following problem occurs: due to the thermal conductivity characteristics of the substrate material as the base of the semiconductor element chip, heat distribution occurs in the chip, and when the semiconductor element chip is operated, the temperature of the chip rises greatly in the central area of ​​the chip. In particular, when the thermal conductivity of the substrate as the base of the semiconductor element chip is low, the problem of large temperature distribution occurs.

[0225] Therefore, as the material of the transfer destination substrate 301, a material having a higher thermal conductivity than the thermal conductivity of the base substrate 101 can be selected. As the transfer destination substrate 301, for example, a ceramic substrate such as SiC, AlN, SiN, etc.; a metal substrate such as Cu or Al, etc.; a composite material substrate or a laminated material substrate including a composite metal material composed of multiple metals such as W, Cr, Cu, Mo, etc., a metal material layer and a ceramic material; a substrate containing a carbon material, etc. By making the thermal conductivity of the transfer destination substrate 301 greater than that of the base substrate 101, a semiconductor element that is easy to dissipate heat can be manufactured.

[0226] By dividing the semiconductor thin film layer into a plurality of islands and connecting a plurality of element elements formed on the divided islands, the heat dissipation of the element elements can be improved, thereby suppressing the temperature rise of the semiconductor element composed of the plurality of element elements. In particular, by using a material with high thermal conductivity as the transfer destination substrate 301, the temperature rise of each element element can be suppressed even in operation with a large current flowing.

[0227] When manufacturing an aggregate semiconductor element composed of a plurality of element elements, a plurality of islands 108 of a semiconductor thin film layer formed on a mother substrate 101 can be simultaneously moved to a destination substrate 301. By forming electrodes on the plurality of islands 108 moved to the destination substrate 301, or forming a wiring pattern that connects at least any one of the plurality of islands 108, an aggregate semiconductor element in which a plurality of element elements operate in conjunction can be manufactured.

[0228] [Optimization of crystal orientation]

[0229] Fig.10 1 is a diagram schematically illustrating a semiconductor epitaxial wafer used as a mother substrate 101. Fig.10 , an island 108 of a plurality of group III nitride semiconductor thin film layers formed on a Si substrate as a mother substrate 101 is shown. In order to remove the island 108 of the group III nitride semiconductor thin film layer from the mother substrate 101 in a good state, the direction of the side of the island 108 is preferably within an angle range of ±45° or less relative to the <112> direction of the Si(111) substrate as the mother substrate 101. The direction of the long side of the island 108 is preferably in the <112> direction of the Si(111) substrate as the mother substrate 101.

[0230] Si(111) exhibits anisotropic etching properties with respect to a specific etching solution. By utilizing the anisotropic etching properties of Si(111), the semiconductor thin film layer obtained by epitaxial growth on Si(111) can be separated from Si(111) by removing the surface area of ​​Si(111) by etching without etching the entire wafer. Previously, when Si(111) was used as the mother substrate 101, the preferred direction of the island 108 of the semiconductor thin film layer formed by epitaxial growth on the mother substrate 101 was not known. In contrast, the inventors have found that it is preferred to set the direction of one side (e.g., the longer side) of the island 108 to an angle range of less than ±45° relative to the <112> direction of the Si substrate. In particular, the inventors have found that it is further preferred to set the direction of the long side of the island 108 to be approximately parallel to the <112> direction of the Si substrate.

[0231] In addition, the inventors have found that when the islands 108 of the semiconductor thin film layer are formed of hexagonal crystals, it is preferable to set the direction of the long sides of the islands 108 of the semiconductor thin film layer to an angle range of ±45° or less relative to the <1-100> direction of a hexagonal crystal material such as a group III nitride semiconductor single crystal such as GaN. In particular, the inventors have found that it is further preferable to set the direction of the long sides of the islands 108 of the semiconductor thin film layer to be approximately parallel to the <1-100> direction of the hexagonal crystal material.

[0232] like Fig.10 As shown, the island 108 has a side with a length of L3 and a side with a length of L4. In the following description, the case of a rectangle in which the length of the side L3 is longer than the length of the side L4 is exemplified, but in the case where L3 = L4 (i.e., the island 108 is a square), the present invention can be applied by setting any side as the long side.

[0233] When the island 108 is rectangular, it is preferred that the island 108 be formed so that the side having a length of L3 (the longer side) is substantially parallel to the <112> direction of the Si (111) substrate. Here, the term "substantially parallel" means parallel within a certain range of error or deviation and does not deviate extremely far from parallel (for example, not exceeding ±10° relative to parallel).

[0234] When a C-plane ((0001) plane) III-nitride semiconductor thin film layer is crystallized and grown on a Si (111) substrate, the <112> direction of Si is parallel to the <1-100> direction of the crystallization of the III-nitride semiconductor thin film layer. In this case, it is preferred that the island 108 is formed so that the side of the island 108 having a length L3 is substantially parallel to the <1-100> direction of the crystallization of the III-nitride semiconductor epitaxial layer.

[0235] As mentioned above, a variety of methods can be used as a method for forming the island 108. For example, by etching the semiconductor thin film layer obtained by crystal growth, an island 108 of the semiconductor thin film layer can be formed with one side direction roughly parallel to the <1-100> direction of the crystallization of the III-nitride semiconductor epitaxial layer.

[0236] Alternatively, the mother substrate 101 may be formed of SiO2, Si x N yAn inorganic insulating film such as Si(111) is used to form a mask layer having an opening, and a semiconductor thin film layer is selectively grown in the opening region, thereby forming an island 108 of a semiconductor thin film layer in which the longest side of the island 108 is approximately parallel to the <112> direction of Si(111) or the <1-100> direction of a hexagonal crystal. Alternatively, the semiconductor thin film layer obtained by self-selective growth can be crystallized on the mask layer in the lateral direction to form an island 108 of a semiconductor thin film layer in which the longest side of the island 108 is approximately parallel to the <112> direction of Si(111) or the <1-100> direction of a hexagonal crystal. The island 108 of a semiconductor thin film layer obtained by crystallization growth on the mask layer has fewer defects than a semiconductor thin film layer obtained by crystallization growth in a region other than the mask layer, and a high-quality crystal growth region can be obtained.

[0237] According to the verification experiment conducted by the inventors, when the long side (the side with the length of L3) of the island 108 of the semiconductor thin film layer is made substantially parallel to the <110> direction of the Si (111) substrate ( Fig.10 In the case where the rectangular island 108 shown in FIG. 1 is rotated 90°, the etching of the Si(111) substrate surface directly below the element region is not performed, and the etching removal of the Si substrate surface over the entire surface directly below the island 108 cannot be performed. As a result, the island 108 cannot be removed from the Si(111) substrate used as the mother substrate 101 in a good state.

[0238] Figure 11A to Figure 11B This is a graph obtained by the inventor through experimental investigation, which shows the relationship between the angle θ formed by the direction of the long side of the island 108 of the semiconductor thin film layer and the <112> direction of Si(111) or the <1-100> direction of the hexagonal crystal, and the etching rate of the Si(111) substrate surface area in the direction perpendicular to the long side of the island 108 of the semiconductor thin film layer. Fig.11A The vertical axis of θ shows the value obtained by dividing the etching rate when θ=0°, 45°, and 90° by the etching rate when θ=0°. Fig. 11B It is a diagram for explaining the angle θ.

[0239] like Fig.11A As shown in , if θ exceeds 45° and approaches 90°, the etching rate relative to the direction perpendicular to the long side will be greatly reduced. Figure 11A to Figure 11B As shown, in order to allow good etching between the island 108 and the Si(111) substrate and to form a gap in the entire area directly below the island 108 between the island 108 and the Si(111) substrate, it is ideal that the angle θ formed by the direction of the long side of the island 108 and the <112> direction of Si(111) or the <1-100> direction of the hexagonal crystal does not exceed 45°.

[0240] Based on the results, it can be confirmed that when the surface area of ​​the Si (111) substrate is etched away over the entire surface directly below the island 108, in order to etch away the surface of the Si substrate over the entire surface directly below the island 108 and remove the island 108 from the Si (111) substrate in a good condition, it is ideal to set the angle between the long side (side with a length of L1) of the rectangular island 108 and the <112> direction of the Si (111) substrate to an angle range of less than ±45°.

[0241] When the semiconductor thin film layer is a hexagonal crystal such as a group III nitride or SiC, it is desirable to make the long side ( Fig.10 The angle θ formed by the direction of L3) and the direction of the hexagonal crystal <1-100> is within the range of ±45°. Furthermore, the island 108 of the semiconductor thin film layer can also be a hexagonal material other than a III-nitride semiconductor or SiC, such as ZnO.

[0242] In the above description, the case where the island 108 of the semiconductor thin film layer is in a rectangular shape is used as an example. When the island 108 of the semiconductor thin film layer is in other shapes, the longest side of the island 108 of the semiconductor thin film layer can be set to a direction roughly parallel to the <112> direction of the Si (111) substrate (so that the direction of the longest side is roughly parallel to the <1-100> direction of the crystallization of the semiconductor epitaxial layer).

[0243] Fig.12 1 is a diagram showing an island 109 of a hexagonal semiconductor thin film layer provided on a mother substrate 101 of a Si (111) substrate. The island 109 has sides of lengths L1, L2, and L3, and satisfies the relationship L1>L2, L3. That is, the side of length L1 is the longest side. Fig.12 As shown, the side of the L1 length of the island 109 of the semiconductor thin film layer is made substantially parallel to the <112> direction of Si (111). In the above case, when the island 109 of the semiconductor thin film layer composed of hexagonal crystals is bonded to the transfer destination substrate 301, the side of the L1 length of the island 109 of the semiconductor thin film layer (i.e., the longest side) is substantially parallel to the <1-100> direction of the hexagonal crystals.

[0244] Furthermore, the mother substrate 101 may also be a silicon on insulator (SOI) substrate. In addition, the mother substrate 101 and the semiconductor thin film layer may be a substrate made of the same material. For example, in the case where the semiconductor thin film layer is a group III nitride semiconductor, the mother substrate 101 may be, for example, a substrate having a Si(111) layer disposed on a GaN substrate. In the case where a substrate having Si(111) disposed on a GaN substrate is set as the mother substrate 101, GaN may be an insulating substrate (a semi-insulating substrate or a high-resistance substrate) or a conductive substrate (a substrate doped with impurities).

[0245] As another example, the mother substrate 101 may be a substrate obtained by bonding a Si (111) layer wafer to a substrate including an oxide material such as a quartz substrate or a sapphire substrate, a nitride material such as SiN or AlN, or a semiconductor material.

[0246] (Experimental example)

[0247] Fig.13A This is a microscopic photograph of islands of a GaN semiconductor thin film layer formed on a Si (111) substrate serving as the mother substrate 101 . Fig.13A The present invention is a microscopic photograph of a state in which at least a surface area of ​​a Si(111) substrate directly below an island of a semiconductor thin film layer is etched away, wherein the island of the semiconductor thin film layer has a long side in a direction substantially parallel to the <112> direction of Si(111) or substantially parallel to the <1-100> direction of a GaN semiconductor thin film layer. In at least a region directly below the island of the semiconductor thin film layer, a gap is formed between the island of the semiconductor thin film layer and the Si(111) substrate.

[0248] Fig. 13B The direction of the long side of the island of the semiconductor thin film layer relative to the crystal direction of the mother substrate 101 is Fig.13A Microscope images of different islands of GaN semiconductor thin film layers. Fig. 13B The state after the step of etching the surface area of ​​the Si(111) substrate at least directly below the island of the semiconductor thin film layer is shown, wherein the island of the semiconductor thin film layer has a long side in a direction substantially perpendicular to the <112> direction of the Si(111) or substantially perpendicular to the <1-100> direction of the GaN semiconductor thin film layer. Fig. 13B As shown, in at least the region directly below the island of the semiconductor thin film layer, there remains a region where no gap is formed between the island of the semiconductor thin film layer and the Si (111) substrate.

[0249] Furthermore, Fig. 13B The etching time for the samples shown is Fig.13A The etch time for the sample shown is approximately 3 times longer. Fig. 13B The color of the area indicated by (1) appears dark, and the area that appears dark is an area where no voids are formed. Fig. 13B As shown, even for Fig. 13B The sample shown was etched for a relatively long time, and in the area directly below the island of the semiconductor thin film layer, there remained an area where no gap was formed between the island of the semiconductor thin film layer and the Si (111) substrate.

[0250] Fig. 13B The region indicated by (2) is the fixed layer. Fig. 13B The area indicated by (3) is the semiconductor thin film layer. Fig. 13B In the region indicated by (4), it can be confirmed that etching damage has occurred in the islands of the semiconductor thin film layer.

[0251] As described above, the inventors have confirmed through experiments that in order to form a hexagonal semiconductor thin film layer (such as GaN, InN, AlN, GaN / Al x Ga 1-x N / In x Ga 1-x N, etc.; SiC, ZnO, etc. semiconductor thin film layers) are separated from the first substrate (Si(111) substrate) and a gap is formed between the island of the semiconductor thin film layer and the first substrate in the entire area directly below the island of the hexagonal crystal semiconductor thin film layer. To this end, it is ideal to make the direction of the long side of the island of the semiconductor thin film layer at least roughly parallel to the direction of <112> of Si(111), or roughly parallel to the direction of <1-100> of the hexagonal crystal (GaN epitaxial layer).

[0252] Fig.14 This is a microscope photograph of a state in which an island of a semiconductor thin film layer whose long side is substantially parallel to the <1-100> direction is bonded to a transfer destination substrate 301 in an experiment conducted by the inventor. Fig.14 As shown, a portion of the fixing layer 114 remains on the island of the semiconductor thin film layer (the fixing layer covering a portion of the upper surface and the side surfaces of the short sides of the island of the semiconductor thin film layer).

[0253] exist Fig.14In the microscope photograph shown, no interference fringes or color unevenness are observed in the island of the semiconductor thin film layer bonded to the destination substrate 301, and it can be confirmed that the island of the semiconductor thin film layer can be well bonded to the destination substrate 301. The reason why the island of the semiconductor thin film layer can be well bonded to the destination substrate 301 is that the island of the semiconductor thin film layer can be formed in a <1-100> direction substantially parallel to the direction of the long side of the island of the semiconductor thin film layer, and a gap can be formed between the island of the semiconductor thin film layer and the mother substrate 101, at least in the region directly below the island of the semiconductor thin film layer, and no damage caused by the etching step occurs on the surface of the semiconductor thin film layer facing the gap. It is also believed that the reason is that by separating the island of the semiconductor thin film layer from the mother substrate 101 in a state where the gap is formed in the region directly below the island of the semiconductor thin film layer, the island of the semiconductor thin film layer can be separated from the mother substrate 101 in a good state.

[0254] [Method for making the fixing layer 110 easy to break]

[0255] Figure 15A to Figure 15B This is a diagram for explaining a method for making the fixing layer 110 easy to break. Fig.15A As shown, in the etching step of forming a gap between the island 108 of the semiconductor thin film layer and the mother substrate 101, a relatively large gap can also be formed. Figure 1E The gap 103 shown is wider than the gap 117. Fig.15A In the illustrated example, a gap 117 is formed between the fixing layer 110 and the base substrate 101 in a portion of the region where the fixing layer 110 is formed on the base substrate 101 .

[0256] If a downward force is applied to the fixing layer 110 in the above state, the corners ( Fig.15A The dotted ellipse part) adds a large stress, so Fig. 15B The portion indicated by the dotted line is susceptible to cracks or breaks.

[0257] Fig.16 This is a microscope photograph showing the result of observing the separation state of the fixing layer 110 in an actual experiment. Fig.16 This is a microscope photograph of the island 108 of the semiconductor thin film layer separated from the mother substrate 101, observed from the back side (the intended bonding surface). Fig.16 The portion indicated by A has a fixed layer 110 covering a portion of the side surface of the island 108 of the semiconductor thin film layer. Fig.16 Since the observation is made from the back side of the island of the semiconductor thin film layer, it is difficult to observe the upper surface of the fixed layer 110, but Fig.16The fixed layer 110 of width indicated by the bracket near A is formed from the side a of the island 108 of the semiconductor thin film layer through the upper surface of the island 108 of the semiconductor thin film layer (with Fig.16 The surface observed in the figure is the surface on the opposite side) and reaches the side b.

[0258] like Fig.16 As shown in FIG. 1 , no fixed layer 110 extending from the side of the island 108 of the semiconductor thin film layer to the outside of the island 108 of the semiconductor thin film layer is observed. In addition, no fixed layer 110 extending beyond the island 108 of the semiconductor thin film layer is observed. Fig.16 The pinned layer 110 is extended to the height of the back side (the side observed using a microscope) of the island 108 of the semiconductor thin film layer shown.

[0259] Fig.17 Yes Fig.16 The microscopic photograph of the state where the island 108 of the semiconductor thin film layer separated from the mother substrate is bonded to the transfer destination substrate 301 is shown. Fig.17 A portion of the fixed layer 110 remains on the upper surface and side surfaces of the island 108 of the semiconductor thin film layer shown in FIG. Fig.17 As shown, the island 108 of the semiconductor thin film layer separated from the mother substrate 101 can be well bonded to the transfer destination substrate 301 .

[0260] exist Fig.16 and Fig.17 In the microscope observation photograph shown, the position of the fixed layer provided on the island 108 of the semiconductor thin film layer is formed at a position slightly offset upward from the center position of the island 108 of the semiconductor thin film layer, but the position where the fixed layer 110 is formed relative to the island 108 of the semiconductor thin film layer may be on the center line of the island 108 of the semiconductor thin film layer, or may be formed at a position offset from the center line. In addition, the position where the fixed layer 110 is formed may also be in a direction inclined relative to the center line of the island 108.

[0261] Alternatively, the fixing layer 110 may include a region extending in the short-side direction corresponding to the second direction from at least a portion of the region extending in the longitudinal direction corresponding to the first direction. Figures 18A to 18B 1 is a diagram showing an example of the fixing layer 110 having a region extending in the short-side direction. Fig.18A The fixing layer 110 shown has regions extending toward both sides from the same position in the longitudinal direction of the fixing layer 110 . Fig.18B The fixing layer 110 shown has regions extending toward both sides from different positions in the length direction of the fixing layer 110 .

[0262] [Formation of step structure in semiconductor thin film layer]

[0263] When a device structure is formed in a semiconductor thin film layer, a step difference is formed in the semiconductor thin film layer according to the function of the device structure. Figure 19A to Figure 19B This is a diagram schematically showing a state in which a semiconductor thin film layer formed on a mother substrate 1001 is divided into islands of individual semiconductor thin film layers. Fig.19A It is a top view of the mother substrate 1001 and the island of the semiconductor thin film layer. Fig.19B The island of the semiconductor thin film layer has a plurality of regions (1002a, 1002b) of different heights.

[0264] In the step of removing the surface of the mother substrate 1001 on which the island of the semiconductor thin film layer is formed by etching away and separating the island of the semiconductor thin film layer from the mother substrate, since the thickness of the region 1002b is less than the thickness of the region 1002a, the periphery of the region 1002b in the mother substrate 1001 is also removed by etching. Since the alignment accuracy of the mask opening when the resist mask opening is formed before etching is not ±0, an offset occurs between the mask opening and the outer periphery of the island. Therefore, in order to ensure a margin, the outer periphery of the resist mask opening needs to be located outside the outer periphery of the island. As a result, as shown in 19B, a groove 1003 is formed in the area around the region 1002b.

[0265] If the groove 1003 is formed, the area of ​​the side surface of the surface area of ​​the mother substrate 1001 directly below the area 1002b exposed in the area of ​​the groove 1003 is larger than the area of ​​the side surface of the mother substrate 1001 directly below the area 1002a. As a result, the removal of a part of the mother substrate 1001 (the area directly below the area 1002b) having a large area of ​​the side surface in contact with the etching liquid is carried out more quickly by etching, thereby generating a step difference in the mother substrate 1001 directly below the area 1002b. If there is a step difference directly below the island of the semiconductor thin film layer, when the island of the semiconductor thin film layer is pressed downward (toward the mother substrate), the problem of cracking may occur in that the island of the semiconductor thin film layer is bent at an acute angle due to the step difference. Therefore, in order to solve this problem, in the method of manufacturing a semiconductor element by separating the semiconductor thin film layer from the mother substrate, it is preferred to form a step difference structure that is not exposed to the periphery of the semiconductor thin film layer in the step of forming the semiconductor thin film layer.

[0266] Figure 20A to Figure 20C The diagram shows a semiconductor device including an island 920 having a semiconductor thin film layer having a step structure that is not exposed to the periphery of the island of the semiconductor thin film layer. Fig. 20A It is a top view of a semiconductor component. Fig. 20B This is the AA line section. Fig. 20C This is a cross-sectional view of line BB. Figure 20A to Figure 20CIn the present invention, an island 920 of a semiconductor thin film layer is bonded to a mobile destination substrate 931, wherein the island 920 of the semiconductor thin film layer includes a region 921 on the surface of which a p-type semiconductor layer is exposed, a concave region 922 on the surface of which an n-type semiconductor layer is exposed, and an outer peripheral wall 923 on the surface of which the p-type semiconductor layer is exposed.

[0267] Figures 21A to 21I It is used to illustrate the manufacturing Figure 20A to Figure 20C Here, a light emitting diode (LED) structure is used as an example for explanation, but the manufacturing method is not limited to a method for manufacturing a semiconductor element having an LED structure, and can be applied to a method for manufacturing semiconductor elements including various element structures.

[0268] Fig.21A The mother substrate 901 in the figure is a mother substrate for epitaxially growing LED semiconductor layers (eg, a stacked structure of group III nitride semiconductor layers such as GaN), and is, for example, a Si substrate. Fig.21A The dotted line area in FIG. 1 is an area where a plurality of islands 920 of semiconductor thin film layers are planned to be formed.

[0269] Fig. 21B yes Fig.21A AA line profile. Fig. 21B As shown, the island 920 of the semiconductor thin film layer has a region 921 where the p-type semiconductor layer is exposed on the surface, a region 922 where the n-type semiconductor layer is exposed on the surface by etching away the p-type semiconductor layer, and an outer peripheral wall 923 where the p-type semiconductor layer is exposed on the surface.

[0270] like Fig. 21C As shown, islands 920 of individual semiconductor thin film layers are divided on a mother substrate 901. Then, a fixing layer 928 is formed by bonding a region 921 where a p-type semiconductor layer is exposed, a region 922 where an n-type semiconductor layer is exposed, and at least a portion of the surface of the peripheral wall 923 to the mother substrate 901. Fig.21D 9 is a cross-sectional view of the periphery of the island 920 formed by segmentation, and shows a state where a fixing layer 928 is formed to bond the island 920 to the mother substrate 901. Fig. 21C 6 islands 920 of semiconductor thin film layers are shown in the figure, but the number, spacing, shape, size, etc. of the islands 920 of semiconductor thin film layers can be appropriately designed. In the region 922 where the n-type semiconductor layer is exposed, the peripheral wall 923 is provided in such a manner that the step difference is not exposed to the periphery of the islands 920 of the semiconductor thin film layers, so that in the region of the mother substrate 901 around the islands 920 of the semiconductor thin film layers, the step difference reflecting the element structure included in the islands 920 of the semiconductor thin film layers is not formed.

[0271] In the step of etching the semiconductor thin film layer outside the predetermined region of the island 920 where the semiconductor thin film layer is formed to form the island 920 of the semiconductor thin film layer, a standard photolithography and etching step can be applied. Although not shown in the figure, after the step, electrode contacts can also be formed in a part of the surface of the region 921 where the p-type semiconductor layer is exposed and a part of the surface of the region 922 where the n-type semiconductor layer is exposed. In the formation of the electrode contacts, for example, a metal thin film layer that can form an ohmic contact is formed, and in order to form a low-resistance electrode contact, an electrode contact sintering step can be appropriately performed.

[0272] Then, if Fig.21E As shown, in the surface of the mother substrate 901, at least the surface area of ​​the mother substrate 901 directly below the island 920 of the semiconductor thin film layer is removed by etching. In the step of etching away the surface area of ​​the mother substrate 901 directly below the island 920 of the semiconductor thin film layer, it is desirable to use an etching liquid or etching gas whose etching speed of the surface area of ​​the mother substrate 901 is faster than that of the semiconductor thin film layer. In the etching step, a gap ( Fig.21E ).

[0273] Then, if Fig.21F As shown, the island 920 of the semiconductor thin film layer is separated from the first substrate. Although not shown in the figure, a structure (such as the pickup substrate) for temporarily adhering or adsorbing the island of the semiconductor thin film layer may be used in the step. Fig.21F In the example shown, after the island 920 is separated, a portion of the fixing layer 928 remains on the mother substrate 901.

[0274] Then, if Figure 21G As shown, the island 920 of the semiconductor thin film layer separated from the mother substrate 901 is bonded to the mobile destination substrate 931. In the step of bonding the island 920 of the semiconductor thin film layer to the mobile destination substrate 931, the island 920 of the semiconductor thin film layer is pressed onto the mobile destination substrate 931 without using an adhesive. Before the step of bonding the island 920 of the semiconductor thin film layer to the mobile destination substrate 931, a surface treatment step of the bonding surface of the island 920 of the semiconductor thin film layer and the surface of the mobile destination substrate 931 may be performed. Although not shown in the figure, other material layers may be provided between the island 920 of the semiconductor thin film layer and the mobile destination substrate 931 (at least the area directly below the semiconductor thin film layer). Furthermore, in the step of bonding the island 920 of the semiconductor thin film layer to the mobile destination substrate 931, bonding without using an adhesive is ideal, but bonding may also be performed using a paste or sheet containing an adhesive.

[0275] Then, if Fig.21H As shown, after the island 920 of the semiconductor thin film layer is bonded to the transfer destination substrate 931, structures necessary for the semiconductor element such as an interlayer insulating film and wiring are formed. For example, when sintering for reducing the contact resistance between the electrode and the surface of the island 920 of the semiconductor thin film layer is not required or when the sintering temperature is low, after the island 920 of the semiconductor thin film layer is bonded to the transfer destination substrate 931, an opening is formed in the fixing layer 928, an electrode 924 is formed in the region 921 where the p-type semiconductor layer is exposed in the opening, an electrode 925 is formed in the region 922 where the n-type semiconductor layer is exposed, and a wiring layer 927 connected to the electrode 924 and the electrode 925 is formed. Furthermore, an interlayer insulating film 926 including a portion of the fixing layer 928 may be formed. For example, the interlayer insulating film 926 may be provided on a portion of the fixing layer 928.

[0276] When the plurality of islands 920 are bonded to the destination substrate 931, the electrodes 924 and the electrodes 925 formed on the plurality of islands 920 may be connected by the wiring layer 927. The plurality of islands 920 may be formed by dividing a semiconductor element of a predetermined size into a plurality of small-sized element semiconductor elements (a plurality of small-sized islands). The plurality of small-sized element semiconductor elements may all include the same structure or may all be the same size. By the above method, it is preferable to suppress the temperature rise as described below.

[0277] In a large-sized semiconductor element, the heat generated during operation is large, and the heat generated in the central region is poorly dissipated, so the temperature rise of the element in the central region is large. In contrast, when a semiconductor element is divided into a plurality of small-sized element semiconductor elements, the divided element semiconductor elements are small-sized, and each element semiconductor element is connected by a wiring layer 927 of a metal material with high thermal conductivity, so that the heat generated in each element semiconductor element is efficiently dissipated through the transfer destination substrate 931 and the wiring layer 927. As a result, the temperature rise of each small-sized element semiconductor element is suppressed.

[0278] In addition, since a plurality of element semiconductor elements as semiconductor thin film layers are bonded to the transfer destination substrate 931, each small-sized element semiconductor element can be connected through a metal thin film wiring layer, thereby achieving high-density integration. As a result, even if a semiconductor element is divided into a plurality of element semiconductor elements, a compact semiconductor element can be obtained. This form is particularly preferred for semiconductor elements that flow large currents, such as power semiconductor elements using semiconductor materials such as Si, SiC, GaN, Ga2O3, and diamond.

[0279] Furthermore, in reference Figures 21A to 21HIn the method for manufacturing a semiconductor device described above, Fig.21D The example of forming the fixing layer 928 is shown in FIG. 1 , but the fixing layer 928 may not be formed. Fig.21E and subsequent steps. In the above case, for example, Fig.21I As shown, when the pick-up substrate 930 is fixed to the surface of the island 920 (for example, the surface where the p-type semiconductor layer region 921 and the peripheral wall 923 are exposed), a gap indicated by oblique lines is formed, and after the gap is formed, the pick-up substrate 930 is lifted up, thereby separating the island 920 from the mother substrate 901. Fig.21I In the state, the island 920 can also be fixed by an external device other than the pick-up substrate 930.

[0280] In this way, after the island 920 of the semiconductor thin film layer is bonded to the transfer destination substrate 931 without forming the fixing layer 928, the electrode 924 is formed in the region 921 where the p-type semiconductor layer is exposed, and the electrode 925 is formed in the region 922 where the n-type semiconductor layer is exposed. In addition, an interlayer insulating film 926 is formed to cover at least a portion of the region 921 where the p-type semiconductor layer is exposed and the region 922 where the n-type semiconductor layer is exposed and to have an opening portion that exposes a portion of the electrode 924 and the electrode 925, and a wiring layer 927 connected to the electrode 924 and the electrode 925 is formed.

[0281] The present invention has been described above using the embodiments, but the technical scope of the present invention is not limited to the scope described in the embodiments, and various modifications and changes can be made within the scope of its main purpose. In addition, new embodiments generated by any combination of multiple embodiments are also included in the embodiments of the present invention. The effects of the new embodiments generated by the combination have the effects of the original embodiments.

Claims

1. A method for manufacturing a semiconductor device, wherein an island of a semiconductor thin film layer of a group III nitride formed on a first substrate is separated from the first substrate and bonded to a second substrate different from the first substrate, wherein the method for manufacturing a semiconductor device is characterized by: include: A step of forming islands of the semiconductor thin film layer on the first substrate in such a manner that the angle between the long sides of the islands of the semiconductor thin film layer of group III nitride and the <112> direction of the Si (111) substrate as the first substrate is in the range of -45° to 45°; A step of forming a fixing layer as a thin film, the fixing layer bonding at least a portion of a main surface of the semiconductor thin film layer opposite to the first substrate side to at least a portion of a surface of the first substrate on the semiconductor thin film layer side; After the step of forming the fixed layer as a thin film, a step of forming a gap on the first substrate side of the island of the semiconductor thin film layer by removing the island of the semiconductor thin film layer or a part of the first substrate, or a part of the layer between the island of the semiconductor thin film layer and the first substrate; After forming the gap, a step of bonding a third substrate different from the first substrate and the second substrate to at least a portion of a bonding area of ​​the fixed layer and the island of the semiconductor thin film layer; The step of moving the third substrate in a direction away from the first substrate while the third substrate is bonded to the bonding area, thereby separating the islands of the semiconductor thin film layer from the first substrate; as well as The step of bonding the island of the semiconductor thin film layer separated from the first substrate to the second substrate, and In the step of forming the fixed layer, multiple fixed layers with the following thickness corresponding to the islands of the multiple semiconductor thin film layers are formed, that is, the thickness is such that a crack is generated between the fixed layer formed on the first substrate and the fixed layer formed on the side of the semiconductor thin film layer by moving the force of the third substrate.

2. A method for manufacturing a semiconductor element, wherein an island of a semiconductor thin film layer in which a C-plane hexagonal crystal is grown on a first substrate formed of Si (111) is separated from the first substrate and bonded to a second substrate different from the first substrate, wherein the method for manufacturing a semiconductor element is characterized by: include: The step of forming the islands of the semiconductor thin film layer on the first substrate in such a manner that the angle of the long sides of the islands of the semiconductor thin film layer of the hexagonal crystal is in the range of -45° to 45° with respect to the <1-100> direction of the hexagonal crystal; A step of forming a fixing layer as a thin film, the fixing layer bonding at least a portion of a main surface of the semiconductor thin film layer opposite to the first substrate side to at least a portion of a surface of the first substrate on the semiconductor thin film layer side; After the step of forming the fixed layer as a thin film, a step of forming a gap on the first substrate side of the island of the semiconductor thin film layer by removing the island of the semiconductor thin film layer or a part of the first substrate, or a part of the layer between the island of the semiconductor thin film layer and the first substrate; After forming the gap, a step of bonding a third substrate different from the first substrate and the second substrate to at least a portion of a bonding area of ​​the fixed layer and the island of the semiconductor thin film layer; The step of moving the third substrate in a direction away from the first substrate while the third substrate is bonded to the bonding area, thereby separating the islands of the semiconductor thin film layer from the first substrate; as well as The step of bonding the island of the semiconductor thin film layer separated from the first substrate to the second substrate, and In the step of forming the fixed layer, multiple fixed layers with the following thickness corresponding to the islands of the multiple semiconductor thin film layers are formed, that is, the thickness is such that a crack is generated between the fixed layer formed on the first substrate and the fixed layer formed on the side of the semiconductor thin film layer by moving the force of the third substrate.

3. The method for manufacturing a semiconductor element according to claim 1 or 2, It is characterized in that In the step of forming the fixing layers, the plurality of fixing layers are formed to have a thickness that allows the plurality of fixing layers to be cut by a force that moves the third substrate in a direction away from the first substrate.

4. The method for manufacturing a semiconductor element according to claim 1 or 2, It is characterized in that In the step of forming the fixing layers, a plurality of the fixing layers are formed to have a thickness that allows cracks to be generated in the fixing layers when a force is applied to the fixing layers by the third substrate in the step of bonding with the bonding region.

5. The method for manufacturing a semiconductor element according to claim 1 or 2, It is characterized in that In the step of forming the pinned layer, a plurality of the pinned layers are formed to have a thickness thinner than that of the islands of the semiconductor thin film layer.

6. The method for manufacturing a semiconductor element according to claim 1 or 2, It is characterized in that After the step of bonding the semiconductor thin film layer to the second substrate, the method further comprises: The step of separating the semiconductor thin film layer from the third substrate by removing the organic material layer possessed by the third substrate and combined with the second substrate.

7. A semiconductor substrate, It is characterized in that include: A first substrate formed of Si (111); A plurality of islands of group III nitride semiconductor thin film layers are formed on the first substrate in such a manner that the angle between the direction of the long side and the <112> direction of the Si (111) substrate as the first substrate is within a range of -45° to 45°; and As a plurality of fixed layers of thin films, at least a portion of the main surface of the plurality of islands of the semiconductor thin film layer on the side opposite to the first substrate is bonded to at least a portion of the surface of the plurality of islands of the semiconductor thin film layer in the first substrate on one side, and There are gaps between the islands of the plurality of semiconductor thin film layers and the first substrate, and at least a portion of the plurality of fixed layers is exposed in the gaps. The plurality of fixed layers have a thickness that causes cracks to form when a third substrate different from the first substrate is bonded to a bonding region with the plurality of fixed layers and at least a portion of the semiconductor thin film layer and a force is applied to move the third substrate.

8. A semiconductor substrate, It is characterized in that include: A first substrate formed of Si (111); a plurality of islands of semiconductor thin film layers, which are formed by growing C-plane hexagonal crystals on the first substrate; and As a plurality of fixed layers of thin films, at least a portion of the main surface of the plurality of islands of the semiconductor thin film layer on the side opposite to the first substrate is bonded to at least a portion of the surface of the plurality of islands of the semiconductor thin film layer in the first substrate on one side, and The angle of the long sides of the islands of the semiconductor thin film layer relative to the <1-100> direction of the hexagonal crystals of the islands of the semiconductor thin film layer is in the range of -45° to 45°; There are gaps between the islands of the plurality of semiconductor thin film layers and the first substrate, and at least a portion of the plurality of fixed layers is exposed in the gaps. The plurality of fixed layers have a thickness that causes cracks to form by applying a force to move the third substrate when a third substrate different from the first substrate is bonded to a bonding area with at least a portion of the islands of the plurality of fixed layers and the plurality of semiconductor thin film layers.

9. The semiconductor substrate according to claim 7 or 8, It is characterized in that The thickness of the fixed layer is thinner than that of the semiconductor thin film layer.