Semiconductor device and method for manufacturing the same
By using an etch stop layer made of aluminum-based insulating material in semiconductor devices, the complexity of the metal wiring layer structure and capacitance problems are solved, and more efficient process margin and performance improvements are achieved.
Patent Information
- Application Number
- CN202111011878.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2016-03-07
- Filing Date
- 2016-12-05
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2036-12-05
AI Technical Summary
In manufacturing complex and high-density semiconductor integrated circuits, the complexity of the structure and size of the metal wiring layer make it difficult for the existing damascene process to effectively reduce the capacitance of the interconnect layer, affecting circuit performance.
Using an etch stop layer made of aluminum-based insulating material, hafnium oxide, zirconium oxide or titanium oxide, openings are formed through the etching process to expose the metal wiring layer, using a high etch selective material to reduce the thickness of the etch stop layer and reduce the interconnection layer capacitor.
A wide process margin and lower interconnect layer capacitance are achieved, improving the performance and density of semiconductor devices.
Smart Images

Figure CN113725152B_ABST
Abstract
Description
[0001] This application is a divisional application of the invention patent application entitled “Semiconductor device and method for manufacturing the same” with application number 201611105455.5 filed on December 5, 2016. Technical Field
[0002] Embodiments of the present invention relate to semiconductor integrated circuits, and more particularly, to semiconductor devices having a metal layer formed by a dual damascene process. Background Art
[0003] As the semiconductor industry introduces a new generation of integrated circuits (ICs) with high performance and multifunctions, the density of the components that make up the integrated circuits is increased, while the size and spacing between the components or elements of the integrated circuits are reduced. The structure of the metal wiring layer is also becoming more and more complex and minimized. In order to manufacture the metal wiring layer, a damascene process has been used in combination with low-k (low dielectric constant, such as 3.5 or lower) materials. Summary of the invention
[0004] According to one embodiment of the present invention, a semiconductor device is provided, comprising: a first metal wiring layer; an interlayer insulating layer formed above the first metal wiring layer; a second metal wiring structure embedded in the interlayer insulating layer and connected to the first metal wiring layer; and an etch stop layer arranged between the first metal wiring layer and the first interlayer insulating layer, the etch stop layer comprising one or more sublayers, wherein the etch stop layer comprises a first sublayer made of an aluminum-based insulating material, hafnium oxide, zirconium oxide or titanium oxide.
[0005] According to another embodiment of the present invention, a method for manufacturing a semiconductor device is also provided, comprising: forming a first metal wiring layer; forming an etch stop layer above the first metal wiring layer; forming an interlayer insulating layer on the etch stop layer; forming a mask layer on the interlayer insulating layer; forming an opening by etching the interlayer insulating layer; and forming a second metal layer in the opening, wherein: the etch stop layer comprises a first sublayer made of at least one of aluminum oxide, aluminum carbon oxide and aluminum nitrogen oxide, the etching for forming the opening comprises a first etching process for etching the interlayer insulating layer and a second etching process after the first etching process to expose the first metal wiring layer, and the first sublayer is used as an etching stop layer for the first etching process.
[0006] According to another embodiment of the present invention, a method for manufacturing a semiconductor device is also provided, which includes: forming a first metal wiring layer; forming an etch stop layer above the first metal wiring layer; forming an interlayer insulating layer on the etch stop layer; forming a mask layer on the interlayer insulating layer; forming an opening by etching the interlayer insulating layer; and forming a second metal layer in the opening, wherein: the etch stop layer includes a first sublayer made of at least one of aluminum oxide, aluminum carbon oxide and aluminum nitrogen oxide and a second sublayer made of a silicon-based insulating material, the etching for forming the opening includes a first etching process for etching the interlayer insulating layer and a second etching process after the first etching process to expose the first metal wiring layer, and the second sublayer is used as an etching stop layer for the first etching process. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] The present invention can be better understood by reading the following detailed description in conjunction with the accompanying drawings. It should be emphasized that, in accordance with standard industry practice, the functional components are not drawn to scale and are only used for illustrative purposes. In fact, for the sake of clarity, the size of each functional component can be arbitrarily enlarged or reduced.
[0008] Figures 1A to 1E An exemplary sequential process for fabricating a metal wiring structure according to one embodiment of the present invention is shown.
[0009] FIG. 2A to FIG. 2H Exemplary etch stop layers according to various embodiments of the present invention are shown.
[0010] FIG. 3A to FIG. 3D and 4A to Figure 4D Shown for manufacturing Figure 2A An exemplary sequential process of a metal wiring layer structure is shown in FIG.
[0011] FIG. 5A to FIG. 5D Shown for manufacturing Figure 2B An exemplary continuous process of metal wiring structure is shown in FIG.
[0012] FIG. 6A to FIG. 6D Shown for manufacturing Figure 2C An exemplary continuous process of metal wiring structure is shown in FIG.
[0013] FIG. 7A to FIG. 7D Shown for manufacturing Figure 2D An exemplary continuous process of metal wiring structure is shown in FIG.
[0014] FIG. 8A to FIG. 8D Shown for manufacturing Figure 2E An exemplary continuous process of metal wiring structure is shown in FIG.
[0015] 9A to 9D Shown for manufacturing Figure 2F An exemplary continuous process of metal wiring structure is shown in FIG.
[0016] FIG. 10A to FIG. 10D Shown for manufacturing Figure 2G An exemplary continuous process of metal wiring structure is shown in FIG.
[0017] FIG. 11A to FIG. 11D Shown for manufacturing Figure 2H An exemplary continuous process of metal wiring structure is shown in FIG. DETAILED DESCRIPTION
[0018] The following disclosure provides many different embodiments or examples for implementing different features of the present invention. Specific examples of components and arrangements are described below to simplify the present invention. Of course, these are merely examples and are not intended to limit the present invention. For example, in the following description, forming a first component above or on a second component may include an embodiment in which the first component and the second component are directly in contact with each other, and may also include an example in which an additional component may be formed between the first component and the second component so that the first component and the second component may not be in direct contact. In addition, the present invention may repeat reference numerals and / or characters in various embodiments. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or configurations discussed.
[0019] Furthermore, for ease of description, spatially relative terms such as "under," "beneath," "lower," "above," "upper," and the like may be used herein to describe the relationship of one element or component to another (or additional) elements or components as shown in the figures. Spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation shown in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations), and the spatially relative descriptors used herein may likewise be interpreted accordingly. Additionally, the term "made of" may mean "comprising" or "consisting of."
[0020] Figures 1A to 1E An exemplary sequential process for fabricating a metal wiring structure according to an embodiment of the present invention is shown. Figures 1A to 1E An exemplary sequential process for manufacturing one of the metal wiring structures (wiring layers) is shown, which is formed above the underlying structure. The underlying structure includes the substrate, the contact to the transistor or the underlying metal wiring structure, which constitutes the semiconductor device. For simplicity of description, Figures 1A to 1E The specific structure of the lower structure can be omitted.
[0021] like Figure 1A, a lower structure 10 is formed above a substrate (not shown). In the present embodiment, the lower structure is a lower metal structure 10, which includes metal wiring extending along a first direction such as an X direction. In some embodiments, the lower metal structure 10 includes copper or a copper alloy. In some embodiments, a capping layer (not shown) is formed on the upper surface of the lower metal structure, and the capping layer serves as a copper diffusion barrier. The capping layer may include one or more of Co, Ni, Ru, Mo, CoWP, and NiMoP.
[0022] An etch stop layer (ESL) 20 is formed on the lower metal structure 10, and then an interlayer dielectric (ILD) layer 30 is formed on the ESL 20. The interlayer dielectric layer may also be referred to as an intermetallic dielectric (IMD) layer. Also, a first mask layer 40 is formed on the ILD layer 30 and a second mask layer 50 is formed on the first mask layer 40.
[0023] ESL20 is a single layer of insulating material or a multilayer of different insulating materials. In both cases, at least one layer is made of an aluminum-based insulating material, hafnium oxide, zirconium oxide or titanium oxide. The aluminum-based insulating material includes aluminum oxide, aluminum carbon oxide and aluminum oxynitride. In the present invention, aluminum oxide is referred to as AlO, aluminum carbon oxide is referred to as AlOC and aluminum oxynitride is referred to as ALON. These materials are stoichiometric or non-stoichiometric.
[0024] When the ESL 20 includes more than one layer (such as two or more sub-layers), at least one sub-layer is made of a silicon-based insulating material such as silicon nitride, silicon oxycarbide, silicon nitride, silicon oxycarbonitride, silicon carbide, or silicon oxide. The silicon nitride is referred to as SiN, the silicon oxycarbide is referred to as SiCO, the silicon carbonitride is referred to as SiCN, the silicon oxynitride is referred to as SiON, the silicon oxycarbonitride is referred to as SiCON, the silicon carbide is referred to as SiC, and silicon oxide (silicon dioxide) is referred to as SiO. These materials are stoichiometric or non-stoichiometric.
[0025] In some embodiments, the thickness of ESL 20 ranges from about 1 nm to about 10 nm, and in other embodiments, from about 2 nm to about 5 nm. When ESL 20 includes multiple sub-layers, in some embodiments, the thickness of each sub-layer ranges from about 2 nm to about 10 nm, and in other embodiments, from about 3 nm to about 6 nm.
[0026] The ILD layer 30 is made of one or more layers of a low-k dielectric material, for example. Low-k dielectric materials have a k value (dielectric constant) less than about 4.0. Some low-k dielectric materials have a k value less than about 3.5 and may have a k value less than about 2.5.
[0027] Materials for the ILD layer 30 include Si, O, C and / or H elements, such as SiCOH and SiOC. Organic materials such as polymers or porous materials can be used for the ILD layer 30. For example, the ILD layer 30 is made of one or more layers of carbon-containing materials, organic silicate glass, porogen materials and / or combinations thereof. In some embodiments, nitrogen can also be used in the ILD layer 30. In one embodiment, the density of the ILD layer 30 is less than about 3 g / cm 3 , in other embodiments may be less than 2.5 g / cm 3 The ILD layer 30 is formed by using techniques such as plasma enhanced chemical vapor deposition (PECVD), low pressure CVD (LPCVD), atomic layer CVD (ALCVD), and / or spin coating. In the case of PECVD, the film is deposited at a temperature ranging from about 25° C. to about 400° C. and a pressure less than 100 Torr.
[0028] In some embodiments, the ILD layer 30 has a thickness ranging from about 10 nm to about 200 nm.
[0029] The first mask layer 40 is made of a dielectric material such as a silicon-based insulating material. In one embodiment, SiO is used as the first mask layer 40. In some embodiments, the thickness of the first mask layer 40 ranges from about 10 nm to about 300 nm.
[0030] The second mask layer 50 is made of a metal-based material such as TiN, TaN, or TiO 2. In some embodiments, the second mask layer 50 has a thickness ranging from about 3 nm to about 100 nm.
[0031] like Figure 1B As shown, a first opening 32 corresponding to a through-hole pattern is formed by a suitable patterning operation. In one embodiment, a photoresist pattern having an opening is formed on a second mask layer 50, and the photoresist pattern is patterned on the second mask layer 50 using an etching mask. The photoresist pattern is removed after etching the second mask layer. Thereafter, the first mask layer 40 is patterned by using the second mask layer 50 as an etching mask. In some embodiments, during the patterning process of the first mask layer 40, the photoresist pattern remains on the second mask layer 50, and the photoresist pattern is removed after etching the first mask layer.
[0032] Thereafter, the ILD layer 30 is etched by using the patterned first and second mask layers as an etching mask. The patterning of the ILD layer 30 includes dry etching.
[0033] In the present embodiment, the etching selectivity of the ESL 20 with respect to the ILD layer 30 is set high. For example, in some embodiments, during the ILD etching, the etching selectivity of the ESL 20 with respect to the ILD layer 30 is about 3 or more, and in other embodiments, about 4 or more. In one embodiment, the etching selectivity of the ESL 20 with respect to the ILD layer 30 ranges from about 4 to about 6. Because the etching selectivity of the ESL 20 is very high, the thickness of the ESL 20 can be very thin, such as less than 5 nm. Therefore, in the dry etching of the ILD layer 30, the ESL 20 is substantially not etched after the surface of the ESL is exposed. In other words, the ESL 20 is used as an etching stop layer for the ILD etching process.
[0034] Next, if Figure 1C As shown, a second opening 34 corresponding to the wiring pattern is formed by a suitable patterning operation. The patterning operation is substantially similar to the patterning operation for the first opening and includes dry etching of the ILD layer 30. Similar to the etching of the ILD layer 30 for the opening 32, the ESL 20 serves as an etch stop layer with high etch selectivity.
[0035] Figure 1B Patterning operations and Figure 1C The order of patterning operations is interchangeable.
[0036] After forming the second opening 34, the second mask layer 50 is removed by a wet etching operation. Figure 1D As shown, the ESL 20 at the bottom of the opening 32 is removed by a dry etching operation. During the dry etching, the first mask layer 40 may also be etched, and the thickness of the first mask layer 40 may be reduced.
[0037] like Figure 1E As shown, after etching ESL20, a second metal layer structure is formed. For example, the second metal layer structure includes a barrier layer 60 such as made of TiN, TaN or Cu and a main layer 70, and the main layer 70 includes a through-hole layer 72 and a wiring layer 74 such as made of Cu or a Cu-based material. The main layer 70 extends along a second direction (such as, Y direction) perpendicular to the first direction. The metal wiring structure can be made by a damascene process. The second metal layer structure is formed by a damascene process, and the damascene process includes a chemical mechanical polishing (CMP) operation. By the CMP operation, the first mask layer 40 is removed. The main layer 70 is formed by physical vapor deposition (PVD) including sputtering, electrochemical plating and / or electroplating by CVD.
[0038] FIG. 2A to FIG. 2H Exemplary etch stop layers according to various embodiments of the present invention are shown.
[0039] exist Figure 2A, ESL 20 includes two sublayers: a first sublayer 20A and a second sublayer 22A. The first sublayer 20A is formed on the lower metal wiring 10, and the second sublayer 22A is formed on the first sublayer 20A. The first sublayer is made of AlO, AlOC, AlON, hafnium oxide, zirconium oxide and titanium oxide. The second sublayer is made of a silicon-based insulating material such as SiCO, SiCN, SiC, SiO, SiON, SiCON or SiN.
[0040] exist Figure 2B , ESL 20 includes two sublayers: a first sublayer 20B and a second sublayer 22B. The first sublayer 20B is formed on the lower metal wiring 10, and the second sublayer 22B is formed on the first sublayer 20B. The first sublayer is made of a silicon-based insulating material such as SiCO, SiCN, SiC, SiO, SiON, SiCON or SiN. The second sublayer is made of one of AlO, AlOC, AlON, hafnium oxide, zirconium oxide and titanium oxide.
[0041] exist Figure 2C In the embodiment, ESL 20 is a single layer 20C made of one of AlO, AlOC, AlON, hafnium oxide, zirconium oxide and titanium oxide.
[0042] exist Figure 2D , ESL20 includes three sublayers: a first sublayer 20D, a second sublayer 22D, and a third sublayer 24D. The first sublayer 20D is formed on the lower metal wiring 10, the second sublayer 22D is formed on the first sublayer 20D, and the third sublayer 24D is formed on the second sublayer 22D. The first and third sublayers are made of one of AlO, AlOC, AlON, hafnium oxide, zirconium oxide, and titanium oxide. The second sublayer is made of a silicon-based insulating material such as SiCO, SiCN, SiC, SiO, SiON, SiCON, or SiN. The first and third sublayers may be made of the same or different materials. Sublayer 20D may be two or more stacked layers each including aluminum without inserting any Si-based insulating layer.
[0043] exist Figure 2E, ESL20 includes three sublayers: a first sublayer 20E, a second sublayer 22E, and a third sublayer 24E. The first sublayer 20E is formed on the lower metal wiring 10, the second sublayer 22E is formed on the first sublayer 20E, and the third sublayer 24E is formed on the second sublayer 22E. The first sublayer is made of one of AlO, AlOC, AlON, hafnium oxide, zirconium oxide, and titanium oxide. The first and third sublayers are made of a silicon-based insulating material, and the second sublayer 22E is made of a material different from the third sublayer 24E. The second sublayer 22E is made of one of SiCN, SiON, SiCON, and SiN, and the third sublayer 24E is made of one of SiCO, SiC, and SiO.
[0044] exist Figure 2F , ESL20 includes three sublayers: a first sublayer 20F, a second sublayer 22F, and a third sublayer 24F. The first sublayer 20F is formed on the lower metal wiring 10, the second sublayer 22F is formed on the first sublayer 20F, and the third sublayer 24F is formed on the second sublayer 22F. The second sublayer is made of one of AlO, AlOC, AlON, hafnium oxide, zirconium oxide, and titanium oxide. The first and third sublayers are made of silicon-based insulating materials such as SiCO, SiCN, SiC, SiO, SiON, SiCON, or SiN. The first and third sublayers may be made of the same or different materials.
[0045] exist Figure 2G , ESL20 includes three sublayers: a first sublayer 20G, a second sublayer 22G, and a third sublayer 24G. The first sublayer 20G is formed on the lower metal wiring 10, the second sublayer 22G is formed on the first sublayer 20G, and the third sublayer 24G is formed on the second sublayer 22G. The first and third sublayers are made of silicon-based insulating materials such as SiCO, SiCN, SiC, SiO, SiON, SiCON or SiN. The first and second sublayers are made of different materials. In some embodiments, the second sublayer 22E is made of one of SiCO, SiC and SiO, and the third sublayer 24E is made of one of SiCN, SiON, SiCON and SiN. The third sublayer is made of one of AlO, AlOC, AlON, hafnium oxide, zirconium oxide and titanium oxide.
[0046] exist Figure 2HIn the embodiment, ESL20 includes four sublayers: a first sublayer 20H, a second sublayer 22H, a third sublayer 24H, and a fourth sublayer 26H. The first sublayer 20H is formed on the lower metal wiring 10, the second sublayer 22H is formed on the first sublayer 20H, the third sublayer 24H is formed on the second sublayer 22H, and the fourth sublayer 26H is formed on the third sublayer 24H. The first and third sublayers are made of one of AlO, AlOC, AlON, hafnium oxide, zirconium oxide, and titanium oxide. The second and fourth sublayers are made of silicon-based insulating materials such as SiCO, SiCN, SiC, SiO, SiON, SiCON, or SiN. The first and third sublayers may be made of the same or different materials, and the second and fourth sublayers may be made of the same or different materials.
[0047] The aluminum-based insulating material, such as AlO, AlOC and AlON, can be formed by the following operations. First, an aluminum layer is formed on a bottom layer (such as, a lower metal structure or another sublayer of ESL20). The aluminum layer is formed by metal organic CVD (MOCVD) or ALD using trimethylaluminum (TMA). Afterwards, NH3, CO2 and / or CO gas are used to perform plasma treatment above the aluminum layer to convert the aluminum layer into AlO, AlOC or AlON. The concentrations of Al, O, C and / or N in the aluminum layer treated with the plasma are inconsistent, especially the concentrations in the vertical direction are inconsistent. The AlON layer is made of two layers of AlO and AlN. In some embodiments, a thin layer of aluminum having a thickness of less than 1nm is maintained at the bottom of the layer. Chemical oxidation of the aluminum layer using an oxidizing solution can be used. In some embodiments, the AlO, AlOC or AlON layer is directly formed by CVD, PVD or ALD using a suitable source gas.
[0048] Hafnium oxide, zirconium oxide, and titanium oxide are formed by a similar method as described above or by CVD, PVD, or ALD or other suitable film forming method by using a suitable source gas.
[0049] FIG. 3A to FIG. 3D A method for manufacturing a Figure 2A An exemplary continuous process of metal wiring structure is shown in FIG.
[0050] and Figure 1A Similarly, an ESL including a first sublayer 20A and a second sublayer 22A is formed on the lower metal wiring 10. The first sublayer 20A is formed on the lower metal wiring 10, and the second sublayer 22A is formed on the first sublayer 20A. Figure 3A As shown, the ILD layer 30 is formed on the first sub-layer 22A, and the first and second mask layers 40 , 50 are formed on the ILD layer 30 .
[0051] and Figure 1B and 1C Similar, such as Figure 3B As shown, openings 32 and 34 are formed by etching the ILD layer 30. During etching of the ILD layer 30, the second sub-layer 22A is etched, while the first sub-layer 20A serves as an etch stop layer.
[0052] Afterwards, if Figure 3C As shown, the second mask layer 50 is removed by a wet etching process. In the wet etching process, the first sub-layer 20A is not substantially etched.
[0053] and Figure 1D Similar, such as Figure 3D As shown, the first mask layer 20A is removed by a dry etching process. Figure 1E Similarly, a second metal structure is formed in the opening.
[0054] FIG. 4A to FIG. 4D A method for manufacturing a Figure 2A An exemplary continuous process of metal wiring structure is shown in FIG.
[0055] and Figure 1A Similarly, an ESL including a first sublayer 20A and a second sublayer 22A is formed on the lower metal wiring 10. The first sublayer 20A is formed on the lower metal wiring 10, and the second sublayer 22A is formed on the first sublayer 20A. Figure 4A As shown, the ILD layer 30 is formed on the first sub-layer 22A, and the first and second mask layers 40 , 50 are formed on the ILD layer 30 .
[0056] and Figure 1B and 1C Similar, such as Figure 4B As shown, the openings 32 and 34 are formed by etching the ILD layer 30. During the etching of the ILD layer 30, the second sub-layer 22A serves as an etch stop layer.
[0057] Afterwards, if Figure 4C As shown, the second mask layer 50 is removed by a wet etching process. In the wet etching process, the first sub-layer 22A is not substantially etched.
[0058] and Figure 1D Similar, such as Figure 4D As shown, the second sub-layer 22A and the first sub-layer 20A are etched by a dry etching process. Figure 1E Similarly, a second metal structure is formed in the opening.
[0059] FIG. 5A to FIG. 5D The present invention is shown in one embodiment Figure 2B An exemplary continuous process for fabricating a metal wiring structure is shown in FIG.
[0060] and Figure 1A Similarly, an ESL including a first sublayer 20B and a second sublayer 22B is formed on the lower metal wiring 10. The first sublayer 20B is formed on the lower metal wiring 10, and the second sublayer 22B is formed on the first sublayer 20B. Figure 5A As shown, the ILD layer 30 is formed on the first sub-layer 22B, and the first and second mask layers 40 , 50 are formed on the ILD layer 30 .
[0061] and Figure 1B and 1C Similar, such as Figure 5B As shown, openings 32 and 34 are formed by etching the ILD layer 30. During etching of the ILD layer 30, the second sub-layer 22B serves as an etch stop layer.
[0062] Afterwards, if Figure 5C As shown, the second mask layer 50 is removed by a wet etching process. In the etching process of the second mask layer 50, the second sub-layer 22B is also removed.
[0063] and Figure 1D Similar, such as Figure 5D As shown in FIG. 1 , the first sublayer 20B is removed by a dry etching process. Figure 1E Similarly, a second metal structure is formed in the opening.
[0064] FIG. 6A to FIG. 6D A method for manufacturing a Figure 2C An exemplary continuous process of metal wiring structure is shown in FIG.
[0065] and Figure 1A Similarly, an ESL including a first sub-layer 20C is formed on the lower metal wiring 10. Also, as Fig. 6A As shown, the ILD layer 30 is formed on the first sub-layer 22B, and the first and second mask layers 40 , 50 are formed on the ILD layer 30 .
[0066] and Figure 1B and 1C Similar, such as Figure 6B As shown, openings 32 and 34 are formed by etching the ILD layer 30. During etching of the ILD layer 30, the first sub-layer 22A serves as an etch stop layer.
[0067] Afterwards, if Figure 6C As shown, the second mask layer 50 is removed by a wet etching process and / or a dry etching process. In the etching process of the second mask layer 50, the second sub-layer 22C is not substantially removed.
[0068] and Figure 1D Similar, such as Fig.6DAs shown, the first sub-layer 20C is removed by a dry etching process. Figure 1E Similarly, a second metal structure is formed in the opening.
[0069] FIG. 7A to FIG. 7D A method for manufacturing a Figure 2D An exemplary continuous process of metal wiring structure is shown in FIG.
[0070] and Figure 1A Similarly, an ESL including a first sublayer 20D, a second sublayer 22D, and a third sublayer 24D is formed on the lower metal wiring 10. The first sublayer 20D is formed on the lower metal wiring 10, the second sublayer 22D is formed on the first sublayer 20D, and the third sublayer 24D is formed on the second sublayer 22D. Fig. 7A As shown, the ILD layer 30 is formed on the third sub-layer 24D, and the first and second mask layers 40 , 50 are formed on the ILD layer 30 .
[0071] and Figure 1B and 1C Similar, such as Figure 7B As shown, the openings 32 and 34 are formed by etching the ILD layer 30. During the etching of the ILD layer 30, the third sub-layer 24D serves as an etch stop layer.
[0072] Afterwards, if Figure 7C As shown, the second mask layer 50 is removed by a wet etching process. In the etching process of the second mask layer 50, the third sub-layer 24D is also removed.
[0073] and Figure 1D Similar, such as Fig.7D As shown, the second sub-layer 22D and the first sub-layer 20D are etched by a dry etching process. Figure 1E Similarly, a second metal structure is formed in the opening.
[0074] FIG. 8A to FIG. 8D A method for manufacturing a Figure 2E An exemplary continuous process of metal wiring structure is shown in FIG.
[0075] and Figure 1A Similarly, an ESL including a first sublayer 20E, a second sublayer 22E, and a third sublayer 24E is formed on the lower metal wiring 10. The first sublayer 20E is formed on the lower metal wiring 10, the second sublayer 22E is formed on the first sublayer 20E, and the third sublayer 24E is formed on the second sublayer 22E. Fig. 8A As shown, the ILD layer 30 is formed on the third sub-layer 24E, and the first and second mask layers 40 , 50 are formed on the ILD layer 30 .
[0076] and Figure 1B and 1C Similar, such as Figure 8B As shown, the openings 32 and 34 are formed by etching the ILD layer 30. During the etching of the ILD layer 30, the third sub-layer 22E is etched, and the second sub-layer 24E serves as an etch stop layer.
[0077] Afterwards, if Figure 8C As shown, the second mask layer 50 is removed by a wet etching process and / or a dry etching process. In the etching process of the second mask layer 50, the second sub-layer 22E is not substantially removed.
[0078] and Figure 1D Similar, such as Fig.8D As shown, the second sub-layer 22E and the first sub-layer 20E are etched by a dry etching process. Figure 1E Similarly, a second metal structure is formed in the opening.
[0079] 9A to 9D A method for manufacturing a Figure 2F An exemplary continuous process of metal wiring structure is shown in FIG.
[0080] and Figure 1A Similarly, an ESL including a first sublayer 20F, a second sublayer 22F, and a third sublayer 24F is formed on the lower metal wiring 10. The first sublayer 20F is formed on the lower metal wiring 10, the second sublayer 22F is formed on the first sublayer 20F, and the third sublayer 24F is formed on the second sublayer 22F. Fig. 9A As shown, the ILD layer 30 is formed on the third sub-layer 24F, and the first and second mask layers 40 , 50 are formed on the ILD layer 30 .
[0081] and Figure 1B and 1C Similar, such as Fig. 9B As shown, the openings 32 and 34 are formed by etching the ILD layer 30. During the etching of the ILD layer 30, the third sub-layer 24F is etched, and the second sub-layer 22F serves as an etch stop layer.
[0082] Afterwards, if Fig. 9C As shown, the second mask layer 50 is removed by a wet etching process and / or a dry etching process. In the etching process of the second mask layer 50, the second sub-layer 22F is etched, but the second sub-layer 20F is not substantially removed.
[0083] and Figure 1D Similar, such as Fig.9D As shown in FIG. 1 , the first sub-layer 20F is removed by a dry etching process. Figure 1E Similarly, a second metal structure is formed in the opening.
[0084] FIG. 10A to FIG. 10D A method for manufacturing a Figure 2G An exemplary continuous process of metal wiring structure is shown in FIG.
[0085] and Figure 1A Similarly, an ESL including a first sublayer 20G, a second sublayer 22G, and a third sublayer 24G is formed on the lower metal wiring 10. The first sublayer 20G is formed on the lower metal wiring 10, the second sublayer 22G is formed on the first sublayer 20G, and the third sublayer 24G is formed on the second sublayer 22G. Fig. 10A As shown, the ILD layer 30 is formed on the third sub-layer 24 , and the first and second mask layers 40 , 50 are formed on the ILD layer 30 .
[0086] and Figure 1B and 1C Similar, such as Fig. 10B As shown, the openings 32 and 34 are formed by etching the ILD layer 30. During the etching of the ILD layer 30, the third sub-layer 24G serves as an etch stop layer.
[0087] Afterwards, if Fig. 10C As shown, the second mask layer 50 is removed by a wet etching process and / or a dry etching process. In the etching process of the second mask layer 50, the second sub-layer 24G is etched, and the second sub-layer 22G is not substantially removed.
[0088] and Figure 1D Similar, such as Fig. 10D As shown, the second sub-layer 22G and the first sub-layer 20G are etched by a dry etching process. Figure 1E Similarly, a second metal structure is formed in the opening.
[0089] FIG. 11A to FIG. 11D A method for manufacturing a Figure 2H An exemplary continuous process of metal wiring structure is shown in FIG.
[0090] and Figure 4A Similarly, an ESL including a first sublayer 20H, a second sublayer 22H, a third sublayer 24H, and a fourth sublayer 26H is formed on the lower metal wiring 10. The first sublayer 20H is formed on the lower metal wiring 10, the second sublayer 22H is formed on the first sublayer 20H, the third sublayer 24H is formed on the second sublayer 22H, and the fourth sublayer 26H is formed on the third sublayer 24H. Fig.11A As shown, the ILD layer 30 is formed on the fourth sub-layer 26H, and the first and second mask layers 40 , 50 are formed on the ILD layer 30 .
[0091] and Figure 1B and 1C Similar, such as Fig. 11B As shown, the openings 32 and 34 are formed by etching the ILD layer 30. During the etching of the ILD layer 30, the fourth sub-layer 26H is also etched, and the third sub-layer 24H serves as an etch stop layer.
[0092] Afterwards, if Fig. 11C As shown, the second mask layer 50 is removed by a wet etching process and / or a dry etching process. In the etching process of etching the second mask layer 50, the third sub-layer 24H is also etched, but the second sub-layer 22H is not substantially etched.
[0093] and Figure 1D Similar, such as Fig.11D As shown, the second sub-layer 22H and the first sub-layer 20H are etched by a dry etching process. Figure 1E Similarly, a second metal structure is formed in the opening.
[0094] Various embodiments or examples described herein provide a variety of advantages over the prior art as described above. For example, in the present invention, a wider process margin for ILD layer etching is obtained by utilizing an etch stop layer including at least one sublayer made of aluminum-based insulating materials, hafnium oxide, zirconium oxide, or titanium oxide. Also, because the etching selectivity of these materials is high, the thickness of the etch stop layer can be reduced, which can reduce the capacitance of the interconnect layer.
[0095] It will be understood that not all advantages are necessarily discussed herein, that all embodiments or examples do not require a particular advantage, and that other embodiments or examples may provide different advantages.
[0096] According to one aspect of the present invention, a semiconductor device includes a first metal wiring layer, an interlayer insulating layer formed above the first metal wiring layer, a second metal wiring structure and an etching stop layer. The second metal wiring structure is embedded in the interlayer insulating layer and connected to the first metal wiring layer. The etching stop layer is arranged between the first metal wiring layer and the first interlayer insulating layer, and includes one or more sublayers. The etching stop layer includes a first sublayer made of an aluminum-based insulating material, hafnium oxide, zirconium oxide or titanium oxide.
[0097] According to another aspect of the present invention, in a method for manufacturing a semiconductor device, a first metal wiring layer is formed. An etch stop layer is formed above the first metal wiring layer. An interlayer insulating layer is formed on the etch stop layer. A mask layer is formed on the interlayer insulating layer. An opening is formed by etching the interlayer insulating layer. A second metal layer is formed in the opening. The etch stop layer includes a first sublayer made of at least one of aluminum oxide, aluminum oxycarbon and aluminum oxynitride. The etching for forming the opening includes a first etching process for etching the interlayer dielectric layer and a second etching process performed after the first etching process to expose the first metal wiring layer. The first sublayer serves as an etching stop layer for the first etching process.
[0098] According to another aspect of the present invention, in a method for manufacturing a semiconductor device, a first metal wiring layer is formed. An etch stop layer is formed above the first metal wiring layer. An interlayer insulating layer is formed on the etch stop layer. A mask layer is formed on the interlayer insulating layer. An opening is formed by etching the interlayer insulating layer. A second metal layer is formed in the opening. The etch stop layer includes a first sublayer made of one of aluminum oxide, aluminum oxycarbon and aluminum oxynitride and a second sublayer made of a silicon-based insulating material. The etching for forming the opening includes a first etching process for etching the interlayer dielectric layer and a second etching process performed after the first etching process to expose the first metal wiring layer. The second sublayer serves as an etching stop layer for the first etching process.
[0099] According to one embodiment of the present invention, a semiconductor device is provided, comprising: a first metal wiring layer; an interlayer insulating layer formed above the first metal wiring layer; a second metal wiring structure embedded in the interlayer insulating layer and connected to the first metal wiring layer; and an etch stop layer arranged between the first metal wiring layer and the first interlayer insulating layer, the etch stop layer comprising one or more sublayers, wherein the etch stop layer comprises a first sublayer made of an aluminum-based insulating material, hafnium oxide, zirconium oxide or titanium oxide.
[0100] In the above semiconductor device, the first sub-layer is made of at least one of aluminum oxide, aluminum oxycarbide, and aluminum oxynitride.
[0101] In the above semiconductor device, the etching stop layer further includes a second sub-layer made of a silicon-based insulating material, the first sub-layer is formed on the first metal wiring layer, and the second sub-layer is formed on the first sub-layer.
[0102] In the above semiconductor device, the etching stop layer further includes a second sub-layer made of a silicon-based insulating material, the second sub-layer is formed on the first metal wiring layer, and the first sub-layer is formed on the second sub-layer.
[0103] In the above semiconductor device, the etching stop layer consists of the first sub-layer.
[0104] In the above-mentioned semiconductor device, the etching stop layer also includes: a second sublayer made of a silicon-based insulating material; and a third sublayer made of at least one of aluminum oxide, aluminum carbon oxide and aluminum nitrogen oxide, the first sublayer is formed on the first metal wiring layer, the second sublayer is formed on the first sublayer, and the third sublayer is formed on the second sublayer.
[0105] In the above semiconductor device, the first sub-layer and the third sub-layer are made of different materials.
[0106] In the above-mentioned semiconductor device, the etching stop layer also includes: a second sublayer made of a first silicon-based insulating material; and a third sublayer made of a second silicon-based insulating material different from the first silicon-based insulating material, the first sublayer is formed on the first metal wiring layer, the second sublayer is formed on the first sublayer, and the third sublayer is formed on the second sublayer.
[0107] In the above-mentioned semiconductor device, the first silicon-based insulating material is one of silicon carbonitride, silicon oxynitride, silicon carbon oxynitride and silicon nitride, and the second silicon-based insulating material is one of silicon carbide, silicon carbide and silicon oxide.
[0108] In the above semiconductor device, the etching stop layer further includes: a second sublayer made of a first silicon-based insulating material; and a third sublayer made of a second silicon-based insulating material, the second sublayer being formed on the first metal wiring layer, the first sublayer being formed on the second sublayer, and
[0109] The third sub-layer is formed on the first sub-layer.
[0110] In the above semiconductor device, the first silicon-based insulating material is different from the second silicon-based insulating material.
[0111] In the above-mentioned semiconductor device, the etching stop layer also includes: a second sublayer made of a first silicon-based insulating material; and a third sublayer made of a second silicon-based insulating material different from the first silicon-based insulating material, the second sublayer is formed on the first metal wiring layer, the third sublayer is formed on the second sublayer, and the first sublayer is formed on the third sublayer.
[0112] In the above-mentioned semiconductor device, the etching stop layer also includes: a second sublayer made of a first silicon-based insulating material; and a third sublayer made of at least one of aluminum oxide, aluminum carbon oxide and aluminum nitrogen oxide; and a fourth sublayer made of a second silicon-based insulating material; and the first sublayer is formed on the first metal wiring layer, the second sublayer is formed on the first sublayer, the third sublayer is formed on the second sublayer, and the fourth sublayer is formed on the third sublayer.
[0113] In the above semiconductor device, the first sub-layer and the third sub-layer are made of different materials.
[0114] In the above semiconductor device, the second sub-layer and the fourth sub-layer are made of different materials.
[0115] According to another embodiment of the present invention, a method for manufacturing a semiconductor device is also provided, comprising: forming a first metal wiring layer; forming an etch stop layer above the first metal wiring layer; forming an interlayer insulating layer on the etch stop layer; forming a mask layer on the interlayer insulating layer; forming an opening by etching the interlayer insulating layer; and forming a second metal layer in the opening, wherein: the etch stop layer comprises a first sublayer made of at least one of aluminum oxide, aluminum carbon oxide and aluminum nitrogen oxide, the etching for forming the opening comprises a first etching process for etching the interlayer insulating layer and a second etching process after the first etching process to expose the first metal wiring layer, and the first sublayer is used as an etching stop layer for the first etching process.
[0116] In the above method: the etching stop layer also includes a second sublayer made of a silicon-based insulating material, the first sublayer is formed on the first metal wiring layer, the second sublayer is formed on the first sublayer, and the second sublayer is etched during the first etching process.
[0117] In the above method, wherein: the etching stop layer also includes: a second sublayer made of a silicon-based insulating material; and a third sublayer made of at least one of aluminum oxide, aluminum carbon oxide and aluminum nitrogen oxide, the third sublayer is formed on the first metal wiring layer, the second sublayer is formed on the third sublayer, and the first sublayer is formed on the second sublayer.
[0118] According to another embodiment of the present invention, a method for manufacturing a semiconductor device is also provided, which includes: forming a first metal wiring layer; forming an etch stop layer above the first metal wiring layer; forming an interlayer insulating layer on the etch stop layer; forming a mask layer on the interlayer insulating layer; forming an opening by etching the interlayer insulating layer; and forming a second metal layer in the opening, wherein: the etch stop layer includes a first sublayer made of at least one of aluminum oxide, aluminum carbon oxide and aluminum nitrogen oxide and a second sublayer made of a silicon-based insulating material, the etching for forming the opening includes a first etching process for etching the interlayer insulating layer and a second etching process after the first etching process to expose the first metal wiring layer, and the second sublayer is used as an etching stop layer for the first etching process.
[0119] In the above method, the etching stop layer further includes a second sublayer made of a silicon-based insulating material, the first sublayer is formed on the first metal wiring layer, the second sublayer is formed on the first sublayer, and the first sublayer is etched during the second etching process.
[0120] The features of several embodiments are summarized above so that those skilled in the art can better understand aspects of the present invention. Those skilled in the art should understand that they can easily use the present invention as a basis to design or modify other processes and structures for implementing the same purpose and / or achieving the same advantages as the embodiments introduced by me. Those skilled in the art should also appreciate that such equivalent constructions do not deviate from the spirit and scope of the present invention, and they can make various changes, substitutions and modifications herein without departing from the spirit and scope of the present invention.
Claims
1. A method for manufacturing a semiconductor device, comprising: forming a first metal wiring layer; forming an etch stop layer over the first metal wiring layer; forming an interlayer insulating layer on the etch stop layer; forming a first mask layer and a second mask layer on the interlayer insulating layer, wherein the second mask layer is made of a metal-based material and the first mask layer is made of a dielectric material; forming an opening by etching the interlayer insulating layer; and A second metal layer is formed in the opening, wherein: The etch stop layer includes, in order of proximity to the first metal wiring layer, a first sublayer made of at least one of aluminum carbide and aluminum oxynitride, a second sublayer made of a first silicon-based insulating material, and a third sublayer made of a second silicon-based insulating material different from the first silicon-based insulating material, and the first sublayer has a non-uniform aluminum, oxygen, carbon, or nitrogen concentration in a thickness direction, The etching for forming the opening includes a first etching process for etching the interlayer insulating layer and a second etching process after the first etching process to expose the first metal wiring layer, and wherein the first etching process includes a first patterning operation of forming a first opening through the interlayer insulating layer and a second patterning operation of forming a second opening at an upper portion of the interlayer insulating layer, wherein the first opening and the second opening have different shapes, wherein, from the start of the first patterning operation to the end of the second patterning operation of forming the second opening, the bottom surface at the lower portion of the first opening remains unchanged, wherein the first etching process and the second etching process use different masks, and the first etching process and the second etching process include multiple etching stop layer etching processes for etching the etching stop layer, and wherein the multiple etching stop layer etching processes use different masks, wherein the etching for forming the opening also includes a mask removal process, the mask removal process removes the second mask layer after the first etching process and before the second etching process, and the second etching process removes a portion of the first mask layer, and the mask removal process is different from the second etching process.
2. The method according to claim 1, wherein: The mask removal process is a wet etching process.
3. The method according to claim 2, wherein: During the mask removal process, the third sublayer is etched while the second mask layer is removed, and during the second etching process, the first mask layer is thinned while the first sublayer and the second sublayer are etched, so that during the period from the start of the mask removal process to the end of the second etching process, the top surface of the opening is lowered while the bottom surface of the opening is lowered.
4. The method according to claim 1, wherein: The method for forming a first sub-layer having a non-uniform aluminum, oxygen, carbon or nitrogen concentration in a thickness direction includes: forming an aluminum layer; Plasma treatment is performed on the aluminum layer using at least one of NH3 gas, CO2 gas, and CO gas to form aluminum carbon oxide or aluminum nitrogen oxide having inconsistent aluminum, oxygen, carbon, or nitrogen concentrations in a thickness direction.
5. The method according to claim 1, wherein: The first sub-layer is made of aluminum oxycarbide and aluminum oxynitride.
6. The method according to claim 1, wherein: The first sub-layer contacts a top surface of the first metal wiring layer, and The second sub-layer contacts a top surface of the first sub-layer.
7. The method according to claim 1, wherein: The second metal layer includes a barrier layer and a bulk layer located on the barrier layer.
8. The method according to claim 7, wherein: The body layer includes a via layer and a wiring layer located above the via layer, and the wiring layer has a tapered side wall.
9. The method according to claim 3, wherein: The second sub-layer serves as an etch stop layer for the mask removal process.
10. A method for manufacturing a semiconductor device, comprising: forming a first metal wiring layer; forming an etch stop layer over the first metal wiring layer; forming an interlayer insulating layer on the etch stop layer; forming a first mask layer and a second mask layer on the interlayer insulating layer, wherein the second mask layer is made of a metal-based material and the first mask layer is made of a dielectric material; forming an opening by etching the interlayer insulating layer; and A second metal layer is formed in the opening, wherein: the etch stop layer includes, in order of proximity to the first metal wiring layer, a first sublayer made of at least one of aluminum oxycarbide and aluminum oxynitride, a second sublayer made of a first silicon-based insulating material, and a third sublayer made of a second silicon-based insulating material different from the first silicon-based insulating material, and the first sublayer has a non-uniform aluminum concentration in a thickness direction, The etching for forming the opening includes a first dry etching process for etching the interlayer insulating layer, a mask removal process to remove the second mask layer, and a second dry etching process after the first dry etching process to expose the first metal wiring layer, and The second sub-layer is used as an etching stop layer for the first dry etching process, wherein during the mask removal process, the second mask layer is removed while the second sub-layer is etched, and during the second dry etching process, the first sub-layer is etched while the first mask layer is thinned, so that during the period from the start of the mask removal process to the end of the second dry etching process, the top surface of the opening is lowered while the bottom surface of the opening is lowered, wherein, when the first metal wiring layer is exposed, the top surface of the interlayer insulating layer is covered by the remaining portion of the first mask layer in contact with the interlayer insulating layer, wherein the first dry etching process and the second dry etching process use different masks, and the first dry etching process and the second dry etching process include multiple etching stop layer etching processes for etching the etching stop layer, and wherein the multiple etching stop layer etching processes use different masks, wherein the etching for forming the opening also includes a mask removal process, the mask removal process removes the second mask layer after the first dry etching process and before the second dry etching process, and the second dry etching process removes a portion of the first mask layer, and the mask removal process is different from the second dry etching process.
11. The method according to claim 10, wherein: The first sub-layer is made of aluminum oxycarbide and aluminum oxynitride.
12. The method according to claim 10, wherein: The first sublayer contacts a top surface of the first metal wiring, and The second sub-layer contacts a top surface of the first sub-layer.
13. The method of claim 10, wherein: The method for forming a first sub-layer having a non-uniform aluminum concentration in a thickness direction includes: forming an aluminum layer; Plasma treatment is performed on the aluminum layer using at least one of NH3 gas, CO2 gas, and CO gas to form aluminum carbon oxide or aluminum nitrogen oxide having inconsistent aluminum, oxygen, carbon, or nitrogen concentrations in a thickness direction.
14. A semiconductor device comprising: a first metal wiring layer; an interlayer insulating layer formed above the first metal wiring layer; a second metal wiring structure embedded in the interlayer insulating layer and connected to the first metal wiring layer; as well as an etch stop layer, disposed between the first metal wiring layer and the interlayer insulating layer, the etch stop layer comprising one or more sublayers, wherein, in order of proximity to the first metal wiring layer, the etching stop layer includes a first sublayer made of at least one of aluminum oxynitride having inconsistent aluminum, oxygen, and nitrogen concentrations in a thickness direction, and aluminum oxycarbon having inconsistent aluminum, oxygen, and carbon concentrations in a thickness direction, a second sublayer made of a first silicon-based insulating material, and a third sublayer made of a second silicon-based insulating material different from the first silicon-based insulating material, wherein the first sublayer is made of aluminum oxycarbon and aluminum oxynitride, The etching selectivity of the etching stop layer relative to the interlayer insulating layer having a k value lower than 2.5 is in the range of 4 to 6, and the thickness of the etching stop layer is less than 5 nm. The second metal wiring structure includes a first portion and a second portion located above the first portion, an interface between the first portion and the second portion includes a horizontally extending surface above the etching stop layer and embedded in the interlayer insulating layer, and a width of the second portion gradually increases from the horizontally extending surface in a direction away from the etching stop layer, wherein the density of the interlayer insulating layer is less than 2.5 g / cm 3 .
15. The semiconductor device according to claim 14, wherein: The material for the interlayer insulating layer includes Si, O, C and / or H elements.
16. The semiconductor device according to claim 14, wherein: The first sub-layer is formed on the first metal wiring layer, The second sub-layer is formed on the first sub-layer, and The third sub-layer is formed on the second sub-layer.
17. The semiconductor device according to claim 16, wherein: The third sublayer is made of one or more of SiCO, SiCN, SiC, SiO, SiON, SiCON or SiN.
18. The semiconductor device according to claim 16, wherein: The first silicon-based insulating material is one of silicon carbonitride, silicon oxynitride, silicon carbon oxynitride and silicon nitride, and The second silicon-based insulating material is one of silicon oxycarbide, silicon carbide, and silicon oxide.
19. The semiconductor device according to claim 16, wherein: The second sub-layer contacts a top surface of the first sub-layer.
20. The semiconductor device according to claim 14, wherein The second metal wiring structure includes a barrier layer and a body layer located on the barrier layer.