Semiconductor device and method for manufacturing the same
By forming dielectric material spacers and conductive material filling methods in semiconductor device manufacturing, the size reduction and etching protection problems in wire-electrode contact and magnetic tunnel junction structure construction are solved, achieving higher precision and flexibility. .
Patent Information
- Application Number
- CN202110451919.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-11-20
- Filing Date
- 2021-04-26
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-04-26
AI Technical Summary
In the manufacturing process of semiconductor devices, as the minimum component size decreases, additional problems arise in the process. Those that need to be solved include the physical contact between the wires and the electrodes and the formation of the magnetic tunnel junction structure, especially protecting the bottom during the etching process. Risks and precision requirements for electrode through holes.
A first dielectric layer and a second dielectric layer are formed above the conductor, and a first opening is formed in the second dielectric layer, and a spacer of dielectric material is formed along the side wall of the opening, and the conductive material fills the opening and is in physical contact with the conductor, Bottom and top electrodes are formed, and a magnetic tunnel junction structure is built on them. Protecting the bottom electrode vias with spacers reduces their size and prevents etch damage while allowing for a larger process window and flexibility.
It achieves the formation of smaller-sized bottom electrode through holes and the effective construction of the magnetic tunnel junction structure, reduces the risk of damage to the bottom electrode during the etching process, expands the process window, and improves the flexibility and accuracy of the process.
Smart Images

Figure CN113725354B_ABST
Abstract
Description
Technical Field
[0001] Embodiments of the present application relate to a semiconductor device and a method for manufacturing the same. Background Art
[0002] Semiconductor devices are used in a variety of electronic applications, such as, for example, personal computers, cell phones, digital cameras, and other electronic devices. Semiconductor devices are typically manufactured by sequentially depositing insulating or dielectric layers, conductive layers, and semiconducting layers of materials over a semiconductor substrate and patterning the various material layers using photolithography and etching processes to form circuit components and elements thereon.
[0003] The semiconductor industry continues to increase the integration density of individual electronic components (e.g., transistors, diodes, resistors, capacitors, etc.) by continuously reducing the minimum feature size, which allows more components to be integrated into a given area. However, as the minimum feature size decreases, additional problems arise in each of the processes used, and these additional problems should be solved. Summary of the invention
[0004] Some embodiments of the present application provide a method for manufacturing a semiconductor device, the method comprising: forming a first dielectric layer and a second dielectric layer above a conductive line; forming a first opening at least within the second dielectric layer; forming a spacer along a sidewall of the first opening, the spacer comprising a dielectric material; filling the first opening with a conductive material, the conductive material being in physical contact with the conductive line; forming a bottom electrode above the conductive material; forming a magnetic tunnel junction structure above the bottom electrode; and forming a top electrode above the magnetic tunnel junction structure.
[0005] Other embodiments of the present application provide a method for manufacturing a semiconductor device, the method comprising: forming a first opening at least partially passing through a first dielectric layer above a conductive line; lining the first opening with a dielectric material; etching the dielectric material to form a spacer and expose the conductive line; forming a through hole in the first opening; forming a magnetic tunnel junction (MTJ) structure above the through hole; and etching the magnetic tunnel junction structure and the first dielectric layer.
[0006] Still other embodiments of the present application provide a semiconductor device, comprising: a conductive line located above a substrate; a spacer located above the conductive line and spaced apart from the conductive line, the spacer being located at least within a first dielectric layer; a through hole extending through the spacer to make physical contact with the conductive line; a bottom electrode in physical contact with the through hole; a magnetic tunnel junction structure in physical contact with the bottom electrode; and a top electrode in physical contact with the magnetic tunnel junction structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] When read in conjunction with the accompanying drawings, various aspects of the present invention can be best understood from the following detailed description. It should be noted that, in accordance with standard practice in the industry, the various components are not drawn to scale. In fact, for clarity of discussion, the size of the various components may be arbitrarily increased or reduced.
[0008] Figure 1 The formation of a dielectric layer over a substrate is shown in accordance with some embodiments.
[0009] Figure 2 The formation of a first opening in a dielectric layer is shown in accordance with some embodiments.
[0010] Figure 3 The formation of a spacer material according to some embodiments is shown.
[0011] Figure 4 The formation of spacers according to some embodiments is shown.
[0012] Figure 5 The formation of a bottom electrode via is shown in accordance with some embodiments.
[0013] Figure 6 Deposition of a bottom electrode, MTJ structure, and top electrode are shown in accordance with some embodiments.
[0014] FIG. 7A to FIG. 7B An etching process according to some embodiments is shown.
[0015] Figure 8 The formation of a dielectric material according to some embodiments is shown.
[0016] Fig. 9 The formation of a dielectric material according to some embodiments is shown.
[0017] Fig.10 The formation of contacts according to some embodiments is shown.
[0018] Fig.11 The placement of photoresist in an offset position is shown in accordance with some embodiments.
[0019] FIG. 12A to FIG. 12B An offset etch process is shown in accordance with some embodiments.
[0020] Fig.13 The formation of a first opening completely in the second dielectric layer is shown in accordance with some embodiments.
[0021] Fig.14 The formation of spacers completely within the second dielectric layer is shown in accordance with some embodiments.
[0022] FIG. 15A to FIG. 15BThe formation of a bottom electrode, an MTJ structure, and a top electrode are shown in accordance with some embodiments.
[0023] FIG. 16A to FIG. 16B An offset embodiment is shown in which the spacers are formed entirely within the second dielectric layer in accordance with some embodiments.
[0024] 17A to 17C Embodiments are shown where portions of the dielectric material remain adjacent to the spacer in accordance with some embodiments.
[0025] FIG. 18A to FIG. 18B An offset embodiment is shown where portions of the dielectric material remain adjacent to the spacer in accordance with some embodiments.
[0026] FIG. 19A to FIG. 19B Embodiments are shown where portions of the dielectric material remain adjacent to the spacers and the spacers are formed completely within the dielectric material, in accordance with some embodiments.
[0027] FIG. 20A to FIG. 20B An offset embodiment is shown where portions of the dielectric material remain adjacent to the spacers and the spacers are formed completely within the dielectric material, in accordance with some embodiments. DETAILED DESCRIPTION
[0028] The following disclosure provides many different embodiments or examples for implementing different features of the present invention. Specific examples of components and arrangements are described below to simplify the present invention. Of course, these are merely examples and are not intended to limit the present invention. For example, in the following description, forming a first component above or on a second component may include an embodiment in which the first component and the second component are directly in contact with each other, and may also include an embodiment in which an additional component may be formed between the first component and the second component so that the first component and the second component may not be in direct contact. In addition, the present invention may repeat reference numerals and / or characters in various examples. This repetition is for the purpose of simplicity and clarity, and does not itself indicate the relationship between the various embodiments and / or configurations discussed.
[0029] Furthermore, for ease of description, spatially relative terms such as "below," "beneath," "lower," "above," "upper," etc. may be used herein to describe the relationship of one element or component to another (or additional) elements or components as shown in the figures. The spatially relative terms are intended to encompass different orientations of the device in use or operation in addition to the orientation depicted in the figures. The device may be otherwise oriented (rotated 90 degrees or at other orientations) and the spatially relative descriptors used herein should likewise be interpreted accordingly.
[0030] Embodiments will now be described with respect to specific embodiments in which spacers 401 are used to protect bottom electrode vias 501 that provide electrical connections to a magnetic random access memory (MRAM) device 100. However, the embodiments discussed herein may be implemented in a variety of structures and methods, and all such embodiments are fully intended to be included within the scope of the discussion.
[0031] Reference now Figure 1 , Figure 1 An intermediate fabrication of an MRAM device 100 is shown, wherein the MRAM device 100 includes a semiconductor substrate 101 , an active device 103 within an active region of the semiconductor substrate 101 , a metallization layer 105 above the active device 103 , and a conductive line 107 within an upper layer of the metallization layer 105 .
[0032] In an embodiment, the semiconductor substrate 101 may include an active layer of a doped or undoped bulk silicon or silicon-on-insulator (SOI) substrate. Typically, an SOI substrate includes a semiconductor material layer such as silicon, germanium, silicon germanium, SOI, silicon germanium on insulator (SGOI), or a combination thereof. Other substrates that may be used include multilayer substrates, gradient substrates, or hybrid orientation substrates.
[0033] The semiconductor substrate 101 may include active devices 103. As will be appreciated by one of ordinary skill in the art, a wide variety of active and passive devices such as transistors (e.g., planar transistors, finFETs (fin field effect transistors), nanowire transistors, etc.), capacitors, resistors, combinations of these, etc. may be used to generate the desired structural and functional requirements for the design of the MRAM device 100. The active devices 103 may be formed using any suitable method.
[0034] A metallization layer 105 designed to connect each active device 103 is formed over the semiconductor substrate 101 and the active devices 103 to form a functional circuit. Figure 1 104 is shown as a single layer, but the metallization layer 105 is formed of alternating layers of dielectric and conductive materials and may be formed by any suitable process such as deposition, damascene, dual damascene, etc. In an embodiment, there may be one or more metallization layers above the semiconductor substrate 102, but the exact number of metallization layers 105 depends on the design of the semiconductor device.
[0035] Conductive wire 107 is formed as part of a conductive portion of metallization layer 105. In a specific embodiment, conductive wire 107 is formed using a damascene or dual damascene process, whereby an opening is formed in a dielectric portion of metallization layer 105 and the opening is filled with one or more conductive materials such as a barrier layer and a filling material such as copper. However, any suitable method may be utilized.
[0036] Figure 1 Also shown is the formation of a first dielectric layer 109, a second dielectric layer 111, and a third dielectric layer 113 formed over the conductive line 107. The first dielectric layer 109 formed using a deposition process such as atomic layer deposition, chemical vapor deposition, physical vapor deposition, combinations thereof, and the like may include a dielectric material such as SiCN, SiOCN, or SiOC, silicon oxide, silicon nitride, phosphosilicate glass (PSG), borosilicate glass (BSG), boron-doped phosphosilicate glass (BPSG), undoped silicate glass (USG), combinations thereof, and the like. The first dielectric layer 109 may be deposited to about Peace However, any suitable material, any suitable deposition process, and any suitable thickness may be utilized.
[0037] A second dielectric layer 111 is formed over the first dielectric layer 109. In an embodiment, the second dielectric layer 111 formed using a deposition process such as atomic layer deposition, chemical vapor deposition, physical vapor deposition, combinations thereof, etc. may be a dielectric material different from the first dielectric layer 109, such as silicon-rich oxide (SRO), silicon oxycarbide, SiCN or SiOCN, silicon oxide, silicon nitride, phosphosilicate glass (PSG), borosilicate glass (BSG), boron-doped phosphosilicate glass (BPSG), undoped silicate glass (USG), combinations thereof, etc. The second dielectric layer 111 may be deposited to about Peace However, any suitable material, any suitable deposition method, and any suitable thickness may be utilized.
[0038] A third dielectric layer 113 is formed over the second dielectric layer 111. In embodiments, the third dielectric layer 113 may be a dielectric material different from the second dielectric layer 111, such as a nitrogen-free anti-reflective layer (NFARC), a silicon-rich oxide (SRO), silicon oxycarbide, SiCN, SiOCN, silicon oxide, silicon nitride, phosphosilicate glass (PSG), borosilicate glass (BSG), boron-doped phosphosilicate glass (BPSG), undoped silicate glass (USG), combinations thereof, and the like. In some embodiments, the third dielectric layer 113 is formed by atomic layer deposition, chemical vapor deposition, physical vapor deposition, combinations thereof, and the like. The third dielectric layer 113 may be deposited to about Peace However, any suitable material, any suitable deposition method, and any suitable thickness may be utilized.
[0039] Figure 1Additionally shown is the placement of a first photoresist 115 over the third dielectric layer 113 to aid in patterning a first opening 201 ( 202 ) through the third dielectric layer 113, the second dielectric layer 111, and partially into the first dielectric layer 109. Figure 1 Not shown, but the following Figure 2 1 and 2. In an embodiment, the first photoresist 115 may be a triple layer photoresist (including, for example, a bottom anti-reflective layer, a hard mask layer, and a photosensitive layer) or even a single layer of a photosensitive layer. Any suitable number of layers may be utilized.
[0040] In an embodiment, the first photoresist 115 may be deposited or placed using one or more processes such as chemical vapor deposition, atomic layer deposition, a spin coating process, a combination of these, etc. Once the first photoresist 115 is in place, the photosensitive layer may be patterned by exposing the photosensitive layer to a patterned energy source (e.g., light). Once exposed, the photosensitive layer may be developed and then used as a mask to pattern the layers below the first photoresist 115 and to expose the third dielectric layer 113.
[0041] Figure 2 It is shown that once the first photoresist 115 has been patterned, a first opening 201 may be formed. In an embodiment, the first opening 201 may be formed using one or more dry etches (such as reactive ion etches) that utilize the first photoresist 115 as a mask to sequentially etch through the third dielectric layer 113, the second dielectric layer 111, and the first dielectric layer 109. However, any suitable etching process may be utilized.
[0042] In an embodiment, the first opening 201 may be formed to have a first width W1 between about 27 nm and about 80 nm or between about 50 nm and about 60 nm along the top of the first opening 201. In addition, in view of the directionality of the etching process, the first opening 201 may also have a second width W2 between about 50 nm and about 70 nm along the bottom of the first opening 201. However, any suitable width may be utilized.
[0043] Furthermore, although the etching process described above may form the first opening 201 completely through the third dielectric layer 113 and the second dielectric layer 111, the etching process in this embodiment may form the first opening 201 only partially through the first dielectric layer 109. Thus, the first opening 201 may extend to approximately Peace By stopping the etching process, a portion of the first dielectric layer 109 remains between the first opening 201 and the conductive line 107, wherein the portion of the first dielectric layer 109 may have a thickness of about Peace A second distance D2 between them. However, any suitable distance may be utilized.
[0044] Figure 3 Deposition of a first spacer material 301 to line the first opening 201 is shown. In an embodiment, the first spacer material 301 can be a dielectric material that has high selectivity to a subsequent etching process (e.g., a wet etching process for etching the second dielectric layer 111 described below with respect to 7A). For example, the first spacer material 301 can be a material that has good selectivity to oxide for an etchant such as dilute hydrofluoric acid (dHF). For example, when an etchant such as dilute hydrofluoric acid (dHF, having, for example, a volume ratio of H2O:HF of 100:1) and a first spacer material 301 such as silicon nitride are used, the oxide / silicon nitride etch selectivity is greater than 10. In a specific embodiment, the first spacer material 301 can be a dielectric material such as silicon nitride (SiN x ), silicon oxynitride (SiO x N y ), silicon oxide (SiO x ), Silicon Oxycarbide (SiC x O y ), silicon oxycarbon nitride (SiC x O y N z ), Silicon Carbon (SiC x ), where x, y, and z can each be any positive number, combinations of these, etc. However, any suitable material may be used.
[0045] The first spacer material 301 may be deposited using a deposition process such as plasma enhanced atomic layer deposition, atomic layer deposition, chemical vapor deposition, plasma enhanced chemical vapor deposition, physical vapor deposition, combinations thereof, and the like. In addition, the first spacer material 301 may be deposited to about Peace However, any suitable deposition process and thickness may be utilized.
[0046] Figure 4 A liner removal process is shown that additionally patterns the first spacer material 301 to form the spacer 401. In an embodiment, the liner removal process may be an anisotropic dry etching process using an etchant that is selective to the material of the first spacer material 301. Thus, the anisotropic etching process will remove horizontal portions of the first spacer material 301 (e.g., portions along the third dielectric layer 113 and along the bottom of the first opening 201) while leaving vertical portions of the first spacer material 301 (e.g., portions along the sidewalls of the first opening 201). Thus, the spacer 401 is formed along the sidewalls of the first opening 201.
[0047] Furthermore, once the horizontal portion of the first spacer material 301 has been removed from the third dielectric layer 113 (to expose the third dielectric layer 113) and the horizontal portion of the first spacer material 301 has also been removed from the bottom of the first opening 201 (to expose the first dielectric layer 109), the third dielectric layer 113 may be removed, and the first dielectric layer 109 may be penetrated to expose the conductive line 107. In an embodiment, the third dielectric layer 113 and the first dielectric layer 109 may be removed using one or more etching processes, such as a dry etching process using an etchant that is selective to the materials of the third dielectric layer 113 and the first dielectric layer 109. In some embodiments, the same etching process used to form the spacer 401 may be used to remove the third dielectric layer 113 and the first dielectric layer 109. However, any suitable number of etching processes may be used.
[0048] Figure 5 The formation of the bottom electrode via 501 within the first opening 201 is shown. In an embodiment, the bottom electrode via 501 may include a barrier layer (not shown separately for clarity) and a conductive fill material. The barrier layer formed using a deposition process such as atomic layer deposition, chemical vapor deposition, physical vapor deposition, combinations of these, etc. may be a material such as titanium, titanium nitride, tantalum, tantalum nitride, combinations of these, etc. However, any suitable material and manufacturing method may be utilized.
[0049] The conductive fill material may include copper, although other suitable materials may alternatively be utilized, such as aluminum, alloys, doped polysilicon, combinations thereof, etc. The conductive fill material may be formed by first depositing a seed layer (not shown) and then electroplating copper on the seed layer, thereby filling and overfilling the first opening 201. Once the first opening 201 has been filled, the excess barrier layer, seed layer, and conductive fill material outside of the first opening 201 may be removed by a planarization process such as chemical mechanical polishing (CMP), although any suitable removal process may be used.
[0050] like Figure 5 As shown, by forming the spacer 401 before forming the bottom electrode via 501, the spacer 401 covers the upper portion of the sidewall of the bottom electrode via 501, while the lower portion of the sidewall of the bottom electrode via 501 is not covered by the spacer 401 and is in direct physical contact with the first dielectric layer 109. In a specific embodiment, the ratio of the covered sidewall to the uncovered sidewall can be between about 6 and about 12. However, any suitable amount can be utilized.
[0051] Furthermore, by utilizing the spacers 401, the overall size of the bottom electrode via 501 can be further reduced without risk of damage or exposure during subsequent etching processes. For example, by using the spacers 401, the bottom electrode via 501 can have a reduced third width W3 between about 25 nm and about 40 nm (such as less than 40 nm). Furthermore, by protecting the bottom electrode via 501 with the spacers 401, further processes (e.g., subsequent etching processes) do not have to be strictly controlled to avoid damaging the bottom electrode via 501, thereby allowing for an increase in the overall process window and greater flexibility.
[0052] Figure 6 The formation of a bottom electrode 601, a magnetic tunnel junction (MTJ) structure 603, and a top electrode 605 is shown. The bottom electrode 601 is formed over the second dielectric layer 111 in physical contact with the bottom electrode via 501 and electrically connected to the conductive line 107. In an embodiment, the bottom electrode 601 includes a conductive material such as titanium (Ti), tantalum (Ta), platinum (Pt), ruthenium (Ru), tungsten (W), aluminum (Al), copper (Cu), titanium nitride (TiN), tantalum nitride (TaN), tungsten nitride (WN), cobalt (Co), molybdenum (Mo), alloys thereof, or combinations thereof, and can be formed using a deposition process such as atomic layer deposition, chemical vapor deposition, physical vapor deposition, combinations thereof, and the like. The bottom electrode 601 may be formed to be approximately Peace However, any suitable material and any suitable manufacturing method may be utilized.
[0053] Once the bottom electrode 601 has been formed, the MTJ structure 603 may be formed. In an embodiment, the MTJ structure 603 may be formed with an antiferromagnetic material, a ferromagnetic fixed layer, a tunneling layer, and a ferromagnetic free layer (for clarity in FIG. Figure 6 In an embodiment, an antiferromagnetic material (AFM) layer is formed above the bottom electrode 601. In the antiferromagnetic material (AFM) layer, the magnetic moments of atoms (or molecules) are aligned in a regular pattern in the opposite direction to the magnetic moments of adjacent atoms (or molecules). The net magnetic moment of the AFM layer is zero. In some embodiments, the AFM layer formed using a deposition method such as atomic layer deposition, chemical vapor deposition, physical vapor deposition, combinations of these, etc. includes platinum manganese (PtMn), iridium manganese (IrMn), rhodium manganese (RhMn), iron manganese (FeMn), combinations of these, etc. The AFM layer can be formed to be about Peace However, any suitable material, deposition process, and thickness may be utilized.
[0054] A ferromagnetic fixed layer is formed above the AFM layer. The ferromagnetic fixed layer forms a permanent magnet and exhibits a strong interaction with the magnet. The magnetic moment direction of the ferromagnetic fixed layer is fixed by the adjacent AFM layer and does not change during the operation of its associated magnetic tunnel junction (MTJ) element. In some embodiments, the ferromagnetic fixed layer formed using a deposition method such as atomic layer deposition, chemical vapor deposition, physical vapor deposition, a combination of these, etc. includes one or more layers of cobalt iron boron (CoFeB), CoFeTa, NiFe, Co, CoFe, CoPt, Ni, an alloy of Co and Fe, a combination of these, etc. However, any suitable material and manufacturing method can be used.
[0055] A tunneling layer is formed over the ferromagnetic pinned layer. The tunneling layer is thin enough to allow electrons to pass through the tunneling layer when a bias voltage is applied. In certain embodiments, the tunneling layer includes magnesium oxide (MgO), aluminum oxide (Al2O3), aluminum nitride (AlN), aluminum oxynitride (AlON), hafnium oxide (HfO2), or zirconium oxide (ZrO2), and can be deposited using a deposition process such as atomic layer deposition, chemical vapor deposition, physical vapor deposition, combinations of these, and the like. The tunneling layer can be deposited to about Peace The thickness between.
[0056] A ferromagnetic free layer is formed above the tunneling layer. The direction of the magnetic moment of the ferromagnetic free layer is not fixed because there is no antiferromagnetic material near the ferromagnetic free layer. Therefore, the magnetic orientation of the layer is adjustable, so the layer is called a free layer. In at least one embodiment, the direction of the magnetic moment of the ferromagnetic free layer is parallel or antiparallel to the fixed direction of the magnetic moment of the ferromagnetic fixed layer and rotates freely. The ferromagnetic free layer formed using a deposition process such as atomic layer deposition, chemical vapor deposition, physical vapor deposition, a combination of these, etc. may include ferromagnetic materials similar to the materials in the ferromagnetic fixed layer, and may include materials such as cobalt, nickel, iron or boron. However, any suitable material and deposition method may be utilized.
[0057] Once the MTJ structure 603 has been formed, a top electrode 605 is formed over the ferromagnetic free layer to provide electrical connections to other parts of the structure for electrical wiring. The top electrode 605 includes a conductive material. In some embodiments, the top electrode 605 is similar to the bottom electrode 601 in terms of composition. For example, in some embodiments, the top electrode 605 includes titanium (Ti), tantalum (Ta), platinum (Pt), ruthenium (Ru), tungsten (W), aluminum (Al), copper (Cu), cobalt (Co), molybdenum (Mo), their alloys, or combinations thereof. However, any suitable material may be utilized.
[0058] Figure 6Additionally shown is a second photoresist 607 placed and patterned over the top electrode 605. In an embodiment, the second photoresist 607 can be similar to the first photoresist 115, such as by being a photoresist as described above with respect to Figure 1 A three-layer photoresist having a bottom antireflective coating, a middle hard mask layer, and a top photosensitive material is placed and patterned as described. However, any suitable material or combination of materials may be utilized.
[0059] In an embodiment, the second photoresist 607 can be placed and patterned to have a fourth width W4 between about 40 nm and about 60 nm, or between about 30 nm and about 55 nm, or not greater than 50 nm. In addition, the second photoresist 607 can be placed so that the first center line 609 of the second photoresist 607 is aligned with the second center line 611 of the bottom electrode through hole 501. Therefore, the second photoresist 607 is centered directly above the bottom electrode through hole 501. However, any suitable width and any suitable alignment can be utilized.
[0060] Fig. 7A It is shown that once the second photoresist 607 has been placed, the second photoresist 607 can be used as a mask to pattern the underlying layers, where the center line 609 of the second photoresist 607 is transferred to the top electrode 605, the MTJ structure 603, and the bottom electrode 601. In an embodiment, the underlying layers can be patterned using one or more anisotropic etching processes (such as reactive ion etching). However, any suitable etching process can be utilized.
[0061] In an embodiment, one or more etching processes may continue to pattern the top electrode 605, the MTJ structure 603, and the bottom electrode 601. After the anisotropic etching process, the top electrode 605 may be formed to have a fifth width W5 between about 30 nm and about 50 nm, the MTJ structure 603 may be formed to have a sixth width W6 between about 40 nm and about 60 nm, and the bottom electrode 601 may be formed to have a seventh width W7 between about 45 nm and about 65 nm. However, any suitable width may be utilized.
[0062] Fig. 7A It is additionally shown that once one or more etching processes have been used to pattern the bottom electrode 601, one or more etching processes may be continued to etch into the second dielectric layer 111. In an embodiment, the one or more etching processes may etch into the second dielectric layer 111 to about Peace A third distance D3 between them. However, any suitable distance may be utilized.
[0063] Once one or more etching processes have been used to pattern the top electrode 605, the MTJ structure 603, the bottom electrode 601, and the second dielectric layer 111, the second photoresist 607 may be removed (if not already removed during a previous etching process). In an embodiment, the second photoresist 607 may be removed using an ashing process, whereby the temperature of the second photoresist 607 is increased until the second photoresist 607 undergoes thermal decomposition and can then be easily removed. However, any suitable removal process may be utilized.
[0064] However, by forming the spacer 401 adjacent to the bottom electrode through hole 501, the etching of the second dielectric layer 111 can be performed with a reduced risk of exposing and / or damaging the bottom electrode through hole 501. Therefore, the bottom electrode through hole 501 can have a reduced width without risk. For example, the bottom electrode through hole 501 can have a third width W3 that is smaller than the seventh width W7 of the bottom electrode 601 by at least the thickness of the spacer 401 (see FIG. Figure 5 ).
[0065] Figure 7B Shows Fig. 7A 4. A top view of the structure shown. From this view, it can be seen that the top electrode 605 completely covers the spacer 401 (not visible in the top view). In addition, the bottom electrode via 501 is centered below the top electrode 605. Therefore, the spacer 401 can help prevent undesirable etching and damage to the bottom electrode via 501 during etching of the second dielectric layer 111.
[0066] Figure 8 It is shown that once the second dielectric layer 111 has been etched and the second photoresist 607 has been removed, a capping layer 801 can be deposited over the structure. In an embodiment, the capping layer 801 can be a material such as silicon nitride, silicon carbon nitride, silicon carbon oxide, carbon nitride, etc., or a combination thereof, and can be deposited to about 1000 Å using a deposition process such as atomic layer deposition, chemical vapor deposition, physical vapor deposition, combinations of these, etc. Peace However, any suitable material, any suitable deposition process, and any suitable thickness may be utilized.
[0067] Once the capping layer 801 has been formed, a fourth dielectric layer 803 may be deposited to cover the capping layer 801. In an embodiment, the fourth dielectric layer 803 may include materials such as phosphosilicate glass (PSG), borosilicate glass (BSG), boron-doped phosphosilicate glass (BPSG), undoped silicate glass (USG), combinations of these, etc., but any suitable dielectric may be used. The fourth dielectric layer 803 may be formed using a process such as PECVD, but other processes such as LPCVD may also be used.
[0068] Fig. 9 It is shown that once the fourth dielectric layer 803 has been deposited, the fourth dielectric layer 803 and the capping layer 801 are planarized to at least partially expose the top electrode 605. In an embodiment, a chemical mechanical polishing process may be used to planarize the fourth dielectric layer 803. However, any suitable planarization process may be utilized, such as mechanical grinding, an etch-back process, etc.
[0069] Once the top electrode 605 has been exposed, a fifth dielectric layer 901 may be deposited over the fourth dielectric layer 803. In an embodiment, the fifth dielectric layer 901 may include materials such as phosphosilicate glass (PSG), borosilicate glass (BSG), boron-doped phosphosilicate glass (BPSG), undoped silicate glass (USG), combinations of these, etc., but any suitable dielectric may be used. The fifth dielectric layer 901 may be formed using a process such as PECVD, but other processes such as LPCVD may alternatively be used.
[0070] Fig.10 It is shown that once the fifth dielectric layer 901 has been deposited, a top contact 1001 is formed. In an embodiment, the top contact 1001 is formed using a damascene or dual damascene process, whereby an opening is formed within the fifth dielectric layer 901, the opening being filled with one or more conductive materials such as a barrier layer and a fill material such as copper, aluminum, tungsten, combinations of these, etc. Once the opening has been filled, excess material of the barrier layer and fill material may be removed using, for example, a chemical mechanical polishing process. However, any suitable method may be utilized.
[0071] Fig.11 Another embodiment is shown where, instead of the second photoresist 607 being positioned such that it is centered over the bottom electrode via 501, the second photoresist 607 is offset from being centered over the bottom electrode via 501. Thus, the first centerline 609 of the second photoresist 607 is offset from the second centerline 611 of the bottom electrode via 501 by a fourth distance D4 between about 3 nm and about 10 nm. However, any suitable distance may be utilized.
[0072] Fig. 12A Shows the use of Fig.11 The second photoresist 607 with an offset in the patterning of the top electrode 605, the MTJ structure 603 and the bottom electrode 601. In an embodiment, the top electrode 605, the MTJ structure 603 and the bottom electrode 601 can be patterned as described above. Fig. 7A Patterning the top electrode 605, MTJ structure 603, and bottom electrode 601 is performed as described. For example, one or more reactive ion etching processes may be used to sequentially etch through the top electrode 605, MTJ structure 603, bottom electrode 601, and second dielectric layer 111. However, any suitable process may be utilized.
[0073] However, in this embodiment, instead of the bottom electrode 601 completely covering the spacer 401, during the patterning process, the top surface of the spacer 401 along one side is uncovered or partially uncovered, while the other side of the spacer 401 remains completely covered by the bottom electrode 601. In some embodiments, the top surface of the spacer 401 may expose about Peace A fifth distance D5 between. However, any suitable distance may be utilized.
[0074] Fig. 12B Shows Fig. 12A . It can be seen in the top view that the top electrode 605 is offset from the bottom electrode via 501, and a portion of the spacer 401 is exposed by the top electrode 605 along one side while being covered by the top electrode 605 along the other side. Therefore, even though the top electrode 605 is offset from the bottom electrode via 501, the bottom electrode via 501 can still be protected.
[0075] Fig.13 1 shows another embodiment, in which the first opening 201 is formed to extend only partially through the second dielectric layer 111 and not into the first dielectric layer 109, rather than extending through the second dielectric layer 111 all the way into the first dielectric layer 109. In an embodiment, the first opening 201 may be formed as described above with respect to Figure 2 The formation of the first opening 201 is described as being performed by, for example, one or more reactive ion etching processes. However, any other suitable method may be utilized.
[0076] However, in this embodiment, the etching process is stopped before etching through the second dielectric layer 111, thereby leaving a portion of the second dielectric layer 111 between the first opening 201 and the first dielectric layer 109. In some embodiments, the first opening 201 extends to about Peace Therefore, the portion of the second dielectric layer 111 between the first opening 201 and the first dielectric layer 109 has a sixth distance D6 of about Peace A seventh distance D7 therebetween. However, any suitable dimensions may be utilized.
[0077] Fig.14 A further processing step is shown, which shows the formation of spacers 401 along the sidewalls of the first opening 201. In an embodiment, the spacers 401 may be formed as described above with respect to Figure 3 to Figure 4The spacers 401 are formed as described. For example, a material for the spacers 401 is deposited to line the sidewalls of the first opening 201, and then etched to remove portions of the material to form the spacers 401. However, any suitable method may be utilized.
[0078] However, in this embodiment, the liner removal process that penetrates the material of the spacer 401 along the bottom of the first opening 201 and the first dielectric layer 109 also etches through the second dielectric layer 111 before penetrating the first dielectric layer 109. Therefore, the spacer 401 is formed to be completely located within the second dielectric layer 111 without extending into the first dielectric layer 109. In addition, the spacer 401 can be spaced apart from the first dielectric layer 109 by a seventh distance D7. However, any suitable distance can be utilized.
[0079] Fig.15A The bottom electrode via 501, the bottom electrode 601, the MTJ structure 603 and the top electrode 605 are shown formed after the spacer 401 is formed completely within the second dielectric layer 111. In an embodiment, the top electrode 605 may be formed as described above. Figure 5 and Figure 6 The bottom electrode via 501, the bottom electrode 601, the MTJ structure 603, and the top electrode 605 are formed as described. For example, the material of the top electrode 605, the MTJ structure 603, and the bottom electrode 601 is deposited, a photoresist is placed and patterned to be centered with the bottom electrode via 501, and then the material of the top electrode 605, the MTJ structure 603, and the bottom electrode 601 is etched. However, any suitable process may be utilized.
[0080] Fig. 15B Shows Fig.15A . From this view, it can be seen that the top electrode 605 completely covers the spacer 401 (not visible in the top view). In addition, the bottom electrode via 501 is centered below the top electrode 605. Therefore, the spacer 401 can help prevent undesirable etching and damage to the bottom electrode via 501 during etching of the second dielectric layer 111.
[0081] Fig.16A Yet another embodiment is shown, in which a spacer is formed in the second dielectric layer 111, and during etching of the top electrode 605, the MTJ structure 603, and the bottom electrode 601, the top surface of the spacer 401 is also partially exposed in the second dielectric layer 111. In this embodiment, as described above with respect to Figure 13 to Figure 14 The spacers 401 are formed as described, wherein the spacers 401 are formed entirely within the second dielectric layer 111 and do not extend into the first dielectric layer 109. However, any suitable process may be used to form the spacers 401.
[0082] Furthermore, in this embodiment, a second photoresist 607 is placed and patterned as described above with respect to Figures 11 to 12A The second centerline 611 of the bottom electrode through hole 501 is offset. In addition, the top electrode 605, the MTJ structure 603, and the bottom electrode 601 are patterned using the offset second photoresist 607, resulting in a portion of the top surface of the spacer 401 being exposed (e.g., by the amount of the fifth distance D5). However, any suitable process may be utilized.
[0083] Fig. 16B Shows Fig.16A . From the top view, it can be seen that the top electrode 605 is offset from the bottom electrode through hole 501, and a portion of the spacer 401 is exposed by the top electrode 605 along one side while being covered by the top electrode 605 along the other side. Therefore, even if the top electrode 605 is offset from the bottom electrode through hole 501, the bottom electrode through hole 501 can still be protected.
[0084] Fig.17A Yet another embodiment is shown, in which the width of the second photoresist 607 is enlarged so that etching the second dielectric layer 111 leaves a layer of the second dielectric layer 111 along the spacer 401 to provide additional protection. In this embodiment, the second dielectric layer 111 can be formed as described above. Figures 1 to 6 The process begins as discussed, with the spacer 401 formed to be completely within the second dielectric layer 111 and at least partially within the first dielectric layer 109. However, when the second photoresist 607 is placed and patterned, the second photoresist 607 expands to an eighth width W8 between about 25 nm and about 80 nm. However, any suitable width may be utilized.
[0085] Once the second photoresist 607 has been placed and patterned, the second photoresist 607 is then used to pattern the top electrode 605, the MTJ structure 603, the bottom electrode 601, and the second dielectric layer 111. For example, one or more etching processes may be used to etch the materials of the top electrode 605, the MTJ structure 603, the bottom electrode 601, and the second dielectric layer 111. Thus, the top electrode 605 may be formed to have a ninth width W9 between about 25 nm and about 70 nm, the MTJ structure 603 may be formed to have a tenth width W10 between about 25 nm and about 75 nm, and the bottom electrode 601 may be formed to have an eleventh width W11 between about 25 nm and about 80 nm. However, any suitable width may be utilized.
[0086] However, in this embodiment, the expanded width of the second photoresist 607 (e.g., the eighth width W8) causes the etching process to leave a portion of the second dielectric layer 111 along the sidewalls of the spacer 401. In addition, the second dielectric layer 111 will have a width adjacent to the spacer 401 and approximately below the bottom electrode 601. Peace The width of the sixth distance D6 between them. However, any suitable size may be utilized.
[0087] Fig. 17C Shows Fig. 17B 4 is a top view of the structure of FIG. It can be seen that in this embodiment, the top electrode 605 is not only located above the bottom electrode via 501 and the spacer 401, but also located above a portion of the second dielectric layer 111. By being located above a portion of the second dielectric layer 111, the portion of the second dielectric layer 111 helps the spacer 401 to protect the bottom electrode via 501 from damage during the etching process.
[0088] Fig.18A Yet another embodiment is shown, in which a portion of the second dielectric layer 111 remains next to the top of the spacer 401 (similar to 17A to 17C For example, in this embodiment, as described above with respect to 17A to 17C The second photoresist 607 is placed and patterned as described. However, in this embodiment, as described above with respect to Figures 11 to 12B The second photoresist 607 is offset placed and patterned as described.
[0089] Given the offset placement and patterning of the second photoresist 607, while the spacer 401 will remain covered by the bottom electrode 601, portions of the second dielectric layer 111 adjacent to the first side of the spacer 401 may extend a lesser distance from the spacer 401 than portions adjacent to the second side of the spacer 401. For example, on the first side of the spacer 401, the second dielectric layer 111 may extend to about Peace The seventh distance D7 between the spacers 401 and the second dielectric layer 111 may extend to about Peace An eighth distance D8 between. However, any suitable distance may be utilized.
[0090] Fig.18B Shows Fig.18A4. It can be seen that the top electrode 605 is offset from the bottom electrode via 501, but still completely covers the spacer 401. In addition, the top electrode 605 covers a portion of the second dielectric layer 111 in addition to the spacer 401. However, in this embodiment, the top electrode 605 covers less of the second dielectric layer 111 along the first side of the spacer 401 than along the second side of the spacer 401.
[0091] Fig.19A Yet another embodiment is shown, in which the process leaves portions of the second dielectric layer 111 along the sidewalls of the spacer 401, similar to the above description of 17A to 17C However, in this embodiment, the spacer 401 is not formed to completely pass through the second dielectric layer 111 and into the first dielectric layer 109, but is formed to be completely formed in the second dielectric layer 111 without extending into the first dielectric layer 109. For example, the spacer 401 may be formed as described above with respect to Figure 13 to Figure 14 The spacers 401 are formed as described. However, any suitable process may be utilized.
[0092] Fig.19B Shows Fig.19A 4 is a top view of the structure of FIG. It can be seen that in this embodiment, the top electrode 605 is not only located above the bottom electrode via 501 and the spacer 401, but also located above a portion of the second dielectric layer 111. By being located above a portion of the second dielectric layer 111, the portion of the second dielectric layer 111 helps the spacer 401 to protect the bottom electrode via 501 from damage during the etching process.
[0093] Fig. 20A Yet another embodiment is shown, in which the process leaves portions of the second dielectric layer 111 along the sidewalls of the spacer 401, similar to the above description of FIG. 18A to FIG. 18B However, in this embodiment, the spacer 401 is not formed to completely pass through the second dielectric layer 111 and into the first dielectric layer 109, but is formed to be completely formed in the second dielectric layer 111 without extending into the first dielectric layer 109. For example, the spacer 401 may be formed as described above with respect to Figure 13 to Figure 14 The spacers 401 are formed as described. However, any suitable process may be utilized.
[0094] Fig. 20B Shows Fig. 20A FIG. 4 is a top view of a structure of FIG. 4. It can be seen that the top electrode 605 is offset from the bottom electrode via 501 and completely covers the spacer 401. In addition, the top electrode 605 covers a portion of the second dielectric layer 111 in addition to the spacer 401. However, in this embodiment, the top electrode 605 covers less of the second dielectric layer 111 along the first side of the spacer 401 than along the second side of the spacer 401.
[0095] The bottom electrode via 501 can be protected from the etching process by utilizing the spacer 401 beside the bottom electrode via 501. This protection allows the bottom electrode via 501 to be formed to a smaller size without worrying about undesired damage, thereby allowing the process window for the etching process to be expanded.
[0096] According to an embodiment, a method for manufacturing a semiconductor device includes: forming a first dielectric layer and a second dielectric layer above a conductive line; forming a first opening at least within the second dielectric layer; forming a spacer along a sidewall of the first opening, the spacer including a dielectric material; filling the first opening with a conductive material, the conductive material being in physical contact with the conductive line; forming a bottom electrode above the conductive material; forming an MTJ structure above the bottom electrode; and forming a top electrode above the MTJ structure. In an embodiment, forming the first opening forms the first opening at least within the first dielectric layer. In an embodiment, forming the first opening forms the first opening outside the first dielectric layer. In an embodiment, forming the spacer further includes: depositing material for the spacer; and removing portions of the material from the horizontal surface. In an embodiment, the top electrode has a centerline aligned with a centerline of the conductive material. In an embodiment, the top electrode has a centerline offset from a centerline of the conductive material. In an embodiment, at least a portion of the spacer is exposed by the bottom electrode.
[0097] According to another embodiment, a method of manufacturing a semiconductor device includes: forming a first opening at least partially through a first dielectric layer above a conductive line; lining the first opening with a dielectric material; etching the dielectric material to form a spacer and expose the conductive line; forming a through hole in the first opening; forming a magnetic tunnel junction (MTJ) structure above the through hole; and etching the MTJ structure and the first dielectric layer. In an embodiment, forming the first opening additionally forms a first opening through a second dielectric layer, the second dielectric layer being located between the conductive line and the first dielectric layer. In an embodiment, etching the MTJ structure and the first dielectric layer exposes a top surface of the spacer. In an embodiment, lining the first opening with a dielectric material is lining the first opening with silicon nitride. In an embodiment, after etching the dielectric material to form the spacer, the spacer is located only within the first dielectric layer. In an embodiment, etching the MTJ structure and the first dielectric layer exposes a top surface of the spacer. In an embodiment, after etching the MTJ structure and the first dielectric layer, a portion of the first dielectric layer remains adjacent to the top surface of the spacer.
[0098] According to yet another embodiment, a semiconductor device includes: a conductive line located above a substrate; a spacer located above and spaced apart from the conductive line, the spacer being located at least within a first dielectric layer; a through hole extending through the spacer so as to be in physical contact with the conductive line; a bottom electrode in physical contact with the through hole; an MTJ structure in physical contact with the bottom electrode; and a top electrode in physical contact with the MTJ structure. In an embodiment, a top surface of the spacer is covered by the bottom electrode. In an embodiment, a top surface of the spacer is at least partially exposed by the bottom electrode. In an embodiment, the spacer is completely located within the first dielectric layer. In an embodiment, the spacer is located in a second dielectric layer different from the first dielectric layer. In an embodiment, the bottom electrode has a width that is greater than a width of the through hole by a first distance, and the first distance is at least as great as a thickness of the spacer.
[0099] The features of several embodiments are summarized above so that those skilled in the art can better understand aspects of the present invention. Those skilled in the art should understand that they can easily use the present invention as a basis to design or modify other processes and structures for implementing the same purpose and / or achieving the same advantages as the embodiments introduced herein. Those skilled in the art should also appreciate that such equivalent constructions do not deviate from the spirit and scope of the present invention, and that they can make various changes, substitutions and modifications herein without departing from the spirit and scope of the present invention.
Claims
1. A method for manufacturing a semiconductor device, the method comprising: forming a first dielectric layer over the conductive line and a second dielectric layer over the first dielectric layer; forming a first opening at least within the second dielectric layer and in an upper portion of the first dielectric layer; forming a spacer along a sidewall of the first opening and spaced apart from the conductive line, the spacer comprising a dielectric material; filling the first opening with a conductive material, the conductive material being in physical contact with the conductive line, wherein the conductive material is in physical contact with the spacer and is in physical contact with a lower portion of the first dielectric layer; forming a bottom electrode over the conductive material; forming a magnetic tunnel junction structure over the bottom electrode; and A top electrode is formed over the magnetic tunnel junction structure.
2. The method according to claim 1, wherein: The first opening is formed to have a first width between 27 nm and 80 nm along a top portion of the first opening.
3. The method according to claim 1, wherein: The first opening has a second width along a bottom of the first opening between 50 nm and 70 nm.
4. The method according to claim 1, wherein: The forming of the spacer further comprises: depositing a material for the spacer; and Removing portions of the material from horizontal surfaces.
5. The method according to claim 1, wherein: The top electrode has a centerline aligned with a centerline of the conductive material.
6. The method according to claim 1, wherein: The top electrode has a centerline that is offset from a centerline of the conductive material.
7. The method according to claim 6, wherein: At least a portion of the spacer is exposed by the bottom electrode.
8. A method for manufacturing a semiconductor device, the method comprising: forming a first opening at least partially through the first dielectric layer over the conductive line, the first opening also passing through an upper portion of a second dielectric layer between the conductive line and the first dielectric layer; lining the first opening with a dielectric material; etching the dielectric material to form spacers and expose the conductive lines, wherein the spacers are separated from the conductive lines; forming a via in the first opening, wherein the via physically contacts the spacer and physically contacts a lower portion of the second dielectric layer; forming a magnetic tunnel junction structure over the through hole; and The magnetic tunnel junction structure and the first dielectric layer are etched.
9. The method according to claim 8, wherein: The through hole has a third width between 25 nm and 40 nm.
10. The method according to claim 8, wherein: The etching of the magnetic tunnel junction structure and the first dielectric layer exposes a top surface of the spacer.
11. The method according to claim 8, wherein: The lining the first opening with the dielectric material lines the first opening with silicon nitride.
12. The method according to claim 8, wherein: After the etching of the dielectric material to form the spacers, the spacers are located only within the first dielectric layer.
13. The method according to claim 10, wherein: The etching of the magnetic tunnel junction structure and the first dielectric layer exposes a top surface of the spacer.
14. The method according to claim 8, wherein: After said etching the magnetic tunnel junction structure and the first dielectric layer, a portion of the first dielectric layer remains adjacent to a top surface of the spacer.
15. A semiconductor device comprising: A wire is located above the substrate; a spacer located above the conductive line and spaced apart from the conductive line, the spacer comprising a dielectric material and located within the first dielectric layer and within an upper portion of a second dielectric layer located between the conductive line and the first dielectric layer; a via extending through the spacer to make physical contact with the conductive line, wherein the via physically contacts the spacer and physically contacts a lower portion of the second dielectric layer; a bottom electrode in physical contact with the through hole; a magnetic tunnel junction structure in physical contact with the bottom electrode; and A top electrode is in physical contact with the magnetic tunnel junction structure.
16. The semiconductor device according to claim 15, wherein: A top surface of the spacer is covered by the bottom electrode.
17. The semiconductor device according to claim 15, wherein: A top surface of the spacer is at least partially exposed by the bottom electrode.
18. The semiconductor device according to claim 15, wherein: The spacer has and The thickness between.
19. The semiconductor device according to claim 15, wherein: The bottom electrode has and The thickness between.
20. The semiconductor device according to claim 15, wherein The bottom electrode has a width greater than a width of the via by a first distance, the first distance being at least as great as a thickness of the spacer.