Process for manufacturing multilayer thin film, method for manufacturing solar cell, and method for manufacturing solar cell module

By forming a Cu2O photoelectric conversion layer on a transparent electrode and placing it in a low-oxygen atmosphere, the problem of low efficiency of cuprous oxide solar cells is solved, efficient photoelectric conversion and light transmittance improvement are achieved, and a high-quality multi-layer film is formed .

CN113728445BActive Publication Date: 2024-10-29KK TOSHIBA +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080015675.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-08-25
Publication Date
2024-10-29
Estimated Expiration
2040-08-25

Smart Images

  • Figure CN113728445B_ABST
    Figure CN113728445B_ABST
Patent Text Reader

Abstract

The present invention provides a process for manufacturing a multilayer thin film, a method for manufacturing a solar cell, a method for manufacturing a multijunction solar cell, and a method for manufacturing a solar cell module. The process for manufacturing a multilayer thin film comprises: forming a photoelectric conversion layer containing Cu2O as a main component on a first transparent electrode; and placing a member having the photoelectric conversion layer formed on the first transparent electrode in an oxygen concentration of 5.0×10 ‑8 [g / L] to 5.0×10 ‑5 [g / L] for 1 h to 1600 h.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments described herein generally relate to processes for making multilayer thin films, methods for making solar cells, and methods for making solar cell modules. Background Art

[0002] Examples of high-efficiency solar cells include multi-junction (tandem) solar cells. Tandem solar cells can utilize cells with high spectral sensitivity to each band, so that their efficiency is higher than that of single-junction solar cells. Cuprous oxide compounds are inexpensive materials with wide band gaps and are expected to be used as top cells in tandem solar cells. At the same time, although the efficiency of cuprous oxide solar cells previously produced by oxidizing copper foil has been recorded to be about 8%, the efficiency is lower than the theoretical maximum efficiency. This may be because when the copper foil is oxidized and the heterogeneous phase such as copper oxide on the top surface is removed by etching, it is impossible to completely remove the phase and the constituent elements in the etching solution still exist. Therefore, a good pn junction cannot be formed. In addition, in this process, it is necessary to first oxidize the foil with a thickness of about 0.1 mm and then polish it to about 20 μm. Therefore, it is difficult to make the area larger.

[0003] As a process for manufacturing cuprous oxide thin films, a sputtering method is known. In some reports, this process has been used to manufacture cuprous oxide thin films. However, its conversion efficiency needs to be further improved.

[0004] Prior art literature

[0005] Non-patent literature

[0006] Non-patent literature 1Sang Woon Lee, Yun Seog Lee et al., Adv. Energy Mater., 2014, 4, 1301916 Summary of the invention

[0007] Problems to be solved by the invention

[0008] Embodiments described herein provide processes for making high quality multilayer thin films, methods for making solar cells, methods for making multijunction solar cells, and methods for making solar cell modules.

[0009] Means for solving problems

[0010] The process for manufacturing a multilayer thin film of an embodiment includes: forming a photoelectric conversion layer including Cu2O as a main component on a first transparent electrode; and placing a member having the photoelectric conversion layer formed on the first transparent electrode under an oxygen concentration of 5.0×10 -8 [g / L] to 5.0×10 -5 [g / L] for 1 h to 1600 h. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 is a schematic cross-sectional view of a multilayer film in an embodiment.

[0012] Figure 2 is a flow chart illustrating a process for making a multilayer film according to an embodiment.

[0013] Figure 3 is a schematic cross-sectional view of a multilayer film in an embodiment.

[0014] Figure 4 is a schematic cross-sectional view of a solar cell in an embodiment.

[0015] Figure 5 is a schematic cross-sectional view of a multi-junction solar cell in an embodiment.

[0016] Figure 6 is a schematic diagram of a solar cell module in an embodiment.

[0017] Figure 7 is a schematic cross-sectional view of a solar cell module in an embodiment.

[0018] Figure 8 is a schematic diagram of a photovoltaic power generation system in an embodiment.

[0019] Fig. 9 It is a schematic diagram of a vehicle in an embodiment.

[0020] Fig.10 is a table of embodiments.

[0021] Fig.11 It is a table of Examples, Reference Examples and Comparative Examples.

[0022] Fig.12 It is a table of Examples, Reference Examples and Comparative Examples. DETAILED DESCRIPTION

[0023] (First Embodiment)

[0024] The first embodiment pertains to a multilayer film and a process for manufacturing the multilayer film. Figure 1 is a schematic cross-sectional view illustrating the multilayer film 100 . Figure 1 The multilayer film 100 shown includes: a first transparent electrode 1; and a photoelectric conversion layer 2 formed on the first transparent electrode 1. The surface of the photoelectric conversion layer 2 opposite to the first transparent electrode 1 has a CuO-containing region 20. Unless otherwise specified herein, values ​​at 25° C. and 1 atm are indicated.

[0025] The first transparent electrode 1 is a layer stacked on the photoelectric conversion layer 2. Figure 1In the embodiment, the first transparent electrode 1 is in direct contact with the photoelectric conversion layer 2. The main surface of the first transparent electrode 1 faces the main surface of the photoelectric conversion layer 2 and has an interface. The entire surface of the photoelectric conversion layer 2 facing the first transparent electrode 1 is preferably in direct contact with the first transparent electrode 1. The first transparent electrode 1 is a p-type electrode in direct contact with the p-type photoelectric conversion layer 2. The first transparent electrode 1 has a thickness of, for example, preferably 100 nm to 1000 nm.

[0026] The first transparent electrode 1 preferably includes a transparent conductive oxide film. Examples of transparent conductive oxide films include, but are not limited to, indium tin oxide (ITO), aluminum-doped zinc oxide (AZO), boron-doped zinc oxide (BZO), gallium-doped zinc oxide (GZO), fluorine-doped tin oxide (FTO), antimony-doped tin oxide (ATO), titanium-doped indium oxide (ITiO), indium zinc oxide (IZO), indium gallium zinc oxide (IGZO), tantalum-doped tin oxide (SnO2:Ta), niobium-doped tin oxide (SnO2:Nb), tungsten-doped tin oxide (SnO2:W), molybdenum-doped tin oxide (SnO2:Mo), fluorine-doped tin oxide (SnO2:F), or indium hydroxide-doped (IOH). The transparent conductive oxide film may be a multilayer film having a plurality of films. The multilayer film may include, for example, a tin oxide film in addition to the above-mentioned oxide film. The dopant in the tin oxide film is, for example, at least one selected from the group consisting of In, Si, Ge, Ti, Cu, Sb, Nb, F, Ta, W, Mo, Br, I and Cl, and is not particularly limited. The photoelectric conversion layer 2 is preferably in direct contact with the transparent conductive oxide film included in the first transparent electrode 1 .

[0027] Preferably, the first transparent electrode 1 includes a multilayer structure in which an indium tin oxide film is stacked on a doped tin oxide film. Specifically, the first transparent electrode 1 preferably includes at least one multilayer structure selected from the following group, the group consisting of a multilayer film having an indium tin oxide film and an antimony-doped tin oxide film, a multilayer film having an indium tin oxide film and a fluorine-doped tin oxide film, a multilayer film having an indium tin oxide film and a tantalum-doped tin oxide film, and a multilayer film having an indium tin oxide film and a niobium-doped tin oxide film. If the first transparent electrode 1 includes a doped tin oxide film, the doped tin oxide film is preferably in direct contact with the photoelectric conversion layer 2.

[0028] The first transparent electrode 1 may include a metal film having a thickness of 10 nm or less. The metal film is, for example, at least one film selected from the group consisting of Mo, Au, Cu, Ag, Al, Ta, Pt, Ru and W, and is not particularly limited. At the same time, the first transparent electrode 1 may be an electrode having a dot-shaped, linear or mesh-shaped metal on the upper or lower part of the transparent conductive oxide film. At this time, the dot-shaped, linear or mesh-shaped metal is arranged between the transparent conductive oxide film and the photoelectric conversion layer 2. The dot-shaped, linear or mesh-shaped metal preferably has an opening ratio of 50% or more relative to the transparent conductive oxide film. The dot-shaped, linear or mesh-shaped metal is, for example, Mo, Au, Cu, Ag, Al, Ta, Pt, Ru or W, and is not particularly limited. If a dot-shaped, linear or mesh-shaped metal is provided, transparency is guaranteed. Therefore, the thickness of the metal film is not limited.

[0029] From the viewpoint of improving the crystallinity of the photoelectric conversion layer 2, it is preferred that the surface of the first transparent electrode 1 on which the photoelectric conversion layer 2 is formed is a metal oxide film (transparent conductive oxide film). The metal of the metal oxide containing Sn as the main component is preferably 90atom% or more of Sn. In addition to Sn, the metal oxide film containing Sn as the main component also includes at least one metal (metal oxide) selected from the group consisting of Zn, Al, Ga, In, Si, Ge, Ti, Cu, Sb, Nb, F and Ta. When the photoelectric conversion layer 2 is directly deposited on a metal oxide (such as ITO) film containing indium as the main component, the resulting multilayer body including the ITO film and the substrate is easily deformed at high temperatures. Therefore, it is not suitable for depositing a Cu2O film on an ITO film.

[0030] The photoelectric conversion layer 2 is a p-type compound semiconductor layer mainly containing cuprous oxide. Cuprous oxide is represented by Cu2O and is an oxide semiconductor. Cuprous oxide is undoped or doped cuprous oxide. The photoelectric conversion layer 2 has a thickness of, for example, 500nm to 10μm. The thickness of the photoelectric conversion layer 2 is preferably 1000nm to 5μm, and more preferably 1500nm to 3μm. The thickness of the photoelectric conversion layer 2 can be determined by, for example, observing a cross section.

[0031] Preferably, the photoelectric conversion layer 2 is rich in large cuprous oxide crystals and is superior to the solar cell using the multilayer film 100 in terms of conversion efficiency and transmittance. If the multilayer film 100 is manufactured using the process of the present embodiment, the cuprous oxide crystals become larger, which helps to improve the conversion efficiency and transmittance. Preferably, more than 95wt% of the photoelectric conversion layer 2 includes cuprous oxide as a component. More preferably, more than 98wt% of the photoelectric conversion layer 2 includes cuprous oxide as a component. That is, preferably, the photoelectric conversion layer 2 has almost (substantially) no heterogeneous phases such as CuO and / or Cu. If the photoelectric conversion layer 2 does not include any heterogeneous phases such as CuO and / or Cu, and is substantially a Cu2O single-phase film, it is preferred because of its very high transmittance. The fact that the photoelectric conversion layer 2 is substantially a Cu2O single phase can be confirmed by measuring photoluminescence (PL method).

[0032] Preferably, the photoelectric conversion layer 2 includes Cu with a content of 60.0atom% to 67.0atom% and O (oxygen) with a content of 32.5atom% to 34.0atom%. In addition to Cu and oxygen, an element selected from the group consisting of metals, dopants and impurities other than Cu may also be included. The photoelectric conversion layer 2 may include metals other than copper in the form of oxides, and the photoelectric conversion layer 2 may be a composite oxide. The metal contained in the photoelectric conversion layer 2 is at least one metal selected from the group consisting of Sn, Sb, Ag, Li, Na, K, Cs, Rb, Al, Ga, In, Zn, Mg and Ca in addition to copper. If at least one metal selected from the group consisting of Ag, Li, Na, K, Cs, Rb, Al, Ga, In, Zn, Mg, Ta and Ca is included in addition to copper, the band gap in the photoelectric conversion layer 2 is adjustable. The first transparent electrode 1 side of the photoelectric conversion layer 2 may have a P+ type region, in which at least one P-type dopant selected from Si, Ge or N is dispersed in high concentration.

[0033] The photoelectric conversion layer 2 preferably has a band gap of 2.0 eV to 2.2 eV. A band gap within this range can effectively utilize sunlight in the top cell and the bottom cell of a multi-junction solar cell, wherein a solar cell using Si in the light absorbing layer is used as the bottom cell and a solar cell using the thin film in this embodiment is used as the top cell. The composition of the photoelectric conversion layer 2 can be made of Cu a M b O c. M is at least one element selected from the group consisting of Si, Ge, N, Sn, Sb, Ag, Li, Na, K, Cs, Rb, Al, Ga, In, Zn, Mg, Ta and Ca. Preferably, a, b and c satisfy 1.80≤a≤2.01, 0.00≤b≤0.20, and 0.98≤c≤1.02. The above composition ratio in the photoelectric conversion layer 2 is the composition ratio in the entire photoelectric conversion layer 2. In addition, for the entire photoelectric conversion layer 2, it is preferred to satisfy the above compound composition ratio in the photoelectric conversion layer 2. The photoelectric conversion layer 2 may include additional additives.

[0034] The CuO-containing region 20 exists on the side with the n-type layer. When a solar cell is manufactured using a multilayer film 100 including a photoelectric conversion layer 2 having a very thin region containing CuO on the surface, it has a higher open circuit voltage (Voc) than a solar cell manufactured using a multilayer film without the CuO region 20. The CuO-containing region 20 is a region with a depth of 5 nm in the direction inward from the surface of the photoelectric conversion layer 2 opposite to the first transparent electrode 1 side. The CuO-containing region 20 contains 1.0 mol% or more of CuO. Preferably, in the photoelectric conversion layer 2 excluding the CuO-containing region 20, the ratio of Cu2O to Cu2O, CuO and Cu ([mass of Cu2O] / ([mass of Cu2O]+[mass of CuO]+[mass of Cu])) is 99.5% to 100.0%. The CuO-containing region 20 preferably exists only as a thin surface region. Therefore, the CuO-containing region 20 is preferably a region having a depth of 3 nm from the surface of the photoelectric conversion layer 2 opposite to the first transparent electrode 1 side toward the photoelectric conversion layer 2, and more preferably a region having a depth of 1 nm from the surface of the photoelectric conversion layer 2 opposite to the first transparent electrode 1 side toward the photoelectric conversion layer 2. In the region having a depth (starting point) of 20 nm to a depth of 25 nm in the direction from the surface of the photoelectric conversion layer 2 toward the first transparent electrode 1 side, it is preferred to have a CuO concentration of 0.5 mol% or less.

[0035] Due to the presence of CuO in a very thin region, the CuO-rich ratio in the CuO-containing region 20 may be high. With regard to the ratio of CuO in the CuO-containing region 20 to Cu2O and CuO ([the number of moles of CuO in the CuO-containing region 20] / ([the number of moles of Cu2O in the CuO-containing region 20]+[the number of moles of CuO in the CuO-containing region 20])), the content of CuO is preferably 1.0 mol% to 100 mol%, and the content of CuO is more preferably 20 mol% to 100 mol%. The ratio of Cu2O in the CuO-containing region 20 to Cu2O and Cu ([the number of moles of Cu2O in the CuO-containing region 20] / ([the number of moles of Cu2O in the CuO-containing region 20]+[the number of moles of Cu in the CuO-containing region 20])) is preferably 99.5 mol% to 100.0 mol% (excluding the case where the CuO-containing region 20 includes 100 mol% CuO). The composition of the photoelectric conversion layer 2 including the CuO-containing region 20 can be confirmed by analyzing the multilayer thin film 100 by XPS (X-ray Photoelectron Spectroscopy) or RBS (Rutherford Backscattering Spectroscopy).

[0036] Next, a process of manufacturing the multilayer thin film 100 will be described. Figure 2 1 is a flow chart illustrating a process for manufacturing the multilayer thin film 100. The process for manufacturing the multilayer thin film 100 includes: a step (S01) of depositing a photoelectric conversion layer 2 including Cu2O as a main component on a first transparent electrode 1; and a step (S02) of placing a member having the photoelectric conversion layer 2 formed on the first transparent electrode 1 under an oxygen concentration of 5.0×10 -3 [Pa] to 5.0 [Pa] in a low oxygen atmosphere (first atmosphere) for 1h to 1600h. Before the step (S01) of depositing the photoelectric conversion layer 2, a decompression step (S00) may be selectively performed. In the step (S02) of placing the component having the photoelectric conversion layer 2 formed on the first transparent electrode 1 in a low oxygen atmosphere (first atmosphere), the component is, for example, maintained in a low oxygen atmosphere. For convenience, "placing the component having the photoelectric conversion layer 2 formed on the first transparent electrode 1 in a low oxygen atmosphere" is expressed as the component having the photoelectric conversion layer 2 formed on the first transparent electrode 1 being maintained in a low oxygen atmosphere. It is preferred that the component be maintained in a chamber where the oxygen concentration and water vapor concentration are controllable.

[0037] Preferably, the photoelectric conversion layer 2 containing cuprous oxide as a main component is deposited by sputtering with copper as a target in an oxidizing atmosphere. The photoelectric conversion layer 2 is preferably deposited by sputtering at a high temperature. In the multilayer thin film 100 manufactured by the process of this embodiment, the photoelectric conversion layer 2 contains Cu2O with a large grain size, which helps to improve the conversion efficiency of the solar cell.

[0038] The target material containing Cu as the main component contains Cu with a purity of 99.99%. The purity of Cu is preferably 99.995% or higher, more preferably 99.999% or higher. Using high-purity Cu as the target material, a Cu2O single-phase photoelectric conversion layer 2 can be formed substantially. If the target material contains an element (such as Si) contained in the photoelectric conversion layer 2, the purity of copper is not limited to the above.

[0039] Preferably, the atmosphere during sputtering is an oxidizing atmosphere in which an inert gas and oxygen are mixed. More preferably, the atmosphere during sputtering is an atmosphere including an inert gas and oxygen. Preferred examples of the inert gas include nitrogen, argon, or a mixed gas of nitrogen and argon.

[0040] For example, sputtering is performed on a base material in which the first transparent electrode is formed on the glass substrate 10 or the like. Figure 3 1 is a schematic cross-sectional view illustrating a multilayer thin film 100 including a substrate 10. Sputtering is performed on the surface of the first transparent electrode 1, so that the photoelectric conversion layer 2 is deposited on the first transparent electrode 1. Preferably, before sputtering, the pressure in the chamber where the first transparent electrode 1 is placed is reduced to 5.0×10 -3 [Pa] or lower step (S00). The decompression step (S00) can be performed in the chamber where sputtering is performed, or in a sub-chamber. Unlike the sputtering step, no oxygen is injected during the decompression step. The substrate 10 can be used as a substrate for a solar cell using the thin film 100. The first transparent electrode 1 is formed on the substrate 10 by, for example, sputtering. Preferred examples of the material of the substrate 10 used include glass, such as whiteboard glass, soda-lime glass, chemically strengthened glass or quartz glass. In addition, organic materials such as acrylic, polycarbonate or polyimide can also be used for the substrate 10.

[0041] The thickness of the Cu2O (photoelectric conversion layer 2) film can be set to T. In this case, preferably, the average diameter of the Cu2O crystals in the film thickness direction of the photoelectric conversion layer 2 is 0.7T to 1.0T, excluding the microscopic Cu2O phase of Cu2O crystals having a diameter of 50nm or less in the film thickness direction. When the microscopic Cu2O phase is abundant, there are many grain boundaries, which may lead to a decrease in conversion efficiency. Preferably, the cross-sectional area of ​​the microscopic Cu2O phase of Cu2O crystals having a diameter of 50nm or less in the film thickness direction accounts for 10% or less of the cross-sectional area of ​​the photoelectric conversion layer 2. The photoelectric conversion layer 2 may include Cu2O crystals of small grain size. In this case, during the following step of maintaining a low oxygen atmosphere, oxidation proceeds in the deep part of the photoelectric conversion layer 2. This produces a heterogeneous phase, resulting in a decrease in the crystallinity of the photoelectric conversion layer 2. From the viewpoint of limiting the region having the CuO-containing region 20 to a very thin surface region of the photoelectric conversion layer 2, it is preferred to include many large Cu2O crystals. Specifically, preferably, crystals having a diameter equal to or less than 50 nm account for 10% or less of the cross-sectional area of ​​the photoelectric conversion layer 2. The absorption band of CuO overlaps with the absorption band of a solar cell using Si. From the viewpoint of applying the multilayer film 100 in this embodiment to a multi-junction solar cell, the photoelectric conversion layer 2 preferably has Cu2O with a large grain size.

[0042] In addition, when the photoelectric conversion layer 2 is deposited on a metal oxide film containing Sn as a main component, Sn diffuses in the Cu2O film during the deposition of the Cu2O film. This makes the grain size larger than when sputtered on a glass substrate at the same temperature, thereby increasing the crystallinity. When heated, Cu2O is sputtered on a metal oxide film containing Sn as a main component, thereby allowing the deposition of a Cu2O film having Cu2O crystals grown to a size comparable to the film thickness. This cannot be achieved by sputtering without heating. As described above, the Cu2O film is essentially a Cu2O single phase, and is therefore ideal as a photoelectric conversion layer for a transparent solar cell because the entire film has good crystallinity.

[0043] The copper sheet is oxidized at high temperature to deposit a thick Cu2O film, in which the Cu2O grows to a size comparable to the film thickness. At the same time, in this case, after the Cu sheet is oxidized, a transparent electrode is formed on the Cu2O film. If the transparent electrode is formed directly on the Cu2O film by sputtering, the generated Cu2O crystals disintegrate. This leads to a decrease in the power generation efficiency when manufacturing solar cells. The multilayer film in this embodiment is obtained by depositing the photoelectric conversion layer 2 on the transparent electrode 1. Therefore, after the solar cell is manufactured, the high-quality photoelectric conversion layer 2 can be maintained.

[0044] In the present embodiment, the photoelectric conversion layer 2 is not deposited on a glass substrate, but the photoelectric conversion layer 2 is deposited on the first transparent electrode 1. If the photoelectric conversion layer 2 is deposited on a glass substrate, impurities present in the glass diffuse into the photoelectric conversion layer 2. Due to the formation of impurity energy levels, this may cause changes in film deposition conditions or reduce the film quality of the photoelectric conversion layer 2. In addition, if the photoelectric conversion layer 2 is deposited on a metal film that can be used as an electrode, the generated multilayer film 100 does not have light transmittance. In the present embodiment, light transmittance is a necessary feature. Therefore, the multilayer film obtained by depositing the photoelectric conversion layer 2 on the metal film is impractical from the point of view of light transmittance. If a portion of the glass appears after scribing, there is almost no problem. The case where a cuprous oxide solar cell is used alone is not applicable to the above case.

[0045] Post-sputtering heating is optional. Preferably, the heating is performed while the multilayer structure is held in the chamber from room temperature to the sputtering temperature for a desired period of time.

[0046] Next, the step of holding in a low oxygen atmosphere (S02) will be described. The member having the photoelectric conversion layer 2 formed on the first transparent electrode 1 is held in a low oxygen atmosphere. Holding in a low oxygen atmosphere enables the CuO-containing region 20 to be formed in a very thin surface region of the photoelectric conversion layer 2. The low oxygen atmosphere is preferably an atmosphere having an oxygen concentration (mass / volume) of 5.0×10 -8 [g / L] to 5.0×10 -5 [g / L], and more preferably an atmosphere with an oxygen concentration of 5.0×10 -8 [g / L] to 3.5×10 -5 [g / L] atmosphere. The member having the photoelectric conversion layer 2 formed on the first transparent electrode 1 under a low oxygen atmosphere can be maintained under a low oxygen atmosphere. This enables the formation of a CuO-containing region 20 in a very thin surface region of the photoelectric conversion layer 2. If the member is maintained for a short time in an atmosphere of high oxygen concentration, such as an air atmosphere, a very thin CuO-containing region 20 is not formed on the surface of the photoelectric conversion layer 2. On the contrary, if the member is maintained for a long time in an atmosphere of high oxygen concentration, such as an air atmosphere, CuO is present not only on the surface but also in the inner part of the photoelectric conversion layer 2. Therefore, before the step (S02) of maintaining the member having the photoelectric conversion layer 2 formed on the first transparent electrode 1 under a low oxygen atmosphere, a step (S03) of placing the member having the photoelectric conversion layer 2 formed on the first transparent electrode 1 in an air atmosphere (second atmosphere) of 0°C to 50°C for 1 hour or less is performed.

[0047] The low oxygen atmosphere selectively contains ozone. The oxygen concentration is the sum of the concentrations of oxygen molecules and ozone molecules. For example, the oxygen concentration and water vapor concentration in the air can be reduced to form a low oxygen atmosphere. If a large amount of other oxidizing gases and / or reducing gases are contained in the low oxygen atmosphere, it is not suitable for properly oxidizing a very thin surface area of ​​the Cu2O film. Therefore, in the case of obtaining a low oxygen atmosphere from the air, preferably, the inert gas accounts for 95% or more of the total pressure [Pa] of the low oxygen atmosphere; more preferably, the inert gas accounts for 99% or more of the total pressure [Pa] of the low oxygen atmosphere; further preferably, the inert gas accounts for 99.9% or more of the total pressure [Pa] of the low oxygen atmosphere. Note that carbon dioxide is acidic and does not easily oxidize Cu2O. Therefore, the carbon dioxide concentration is not particularly limited.

[0048] The total pressure of the low oxygen atmosphere is not particularly limited. When the low oxygen atmosphere is obtained by reducing the oxygen concentration in the air, it is typically preferred to set the total pressure to 8.0×10 4 [Pa] to 1.2×10 5 [Pa] If the member having the photoelectric conversion layer 2 formed on the first transparent electrode 1 is maintained under a low oxygen atmosphere in a vacuum chamber, the total pressure of the low oxygen atmosphere is preferably 100 [Pa] or less.

[0049] The member having the photoelectric conversion layer 2 formed on the first transparent electrode 1 may be collected from a film deposition chamber in which the photoelectric conversion layer 2 has been deposited on the first transparent electrode 1, and transported from an air atmosphere and then maintained in a low oxygen atmosphere. In this case, it is preferred to reduce the oxygen concentration and the water vapor concentration so that the above or following atmosphere is achieved within one hour after the member having the photoelectric conversion layer 2 formed on the first transparent electrode 1 is transported to the chamber of the low oxygen atmosphere.

[0050] At the same time, the member having the photovoltaic conversion layer 2 formed on the first transparent electrode 1 can be kept in a low oxygen atmosphere. The holding time is preferably 1h to 1600h. When the holding time is less than 1h, almost no CuO is generated. In addition, even if the holding time is extended, the further increase in open circuit voltage is also small. In addition, the extended holding time has a greater impact on productivity. Then the holding time is preferably 1h to 1600h.

[0051] During the holding step in the low oxygen atmosphere, the water vapor concentration (mass / volume) in the low oxygen atmosphere is preferably 5.0×10 -8 [g / L] to 5.0×10 -5 [g / L], and more preferably 5.0×10 -8 [g / L] to 4.0×10 -5[g / L] If the water vapor concentration in the low oxygen atmosphere is high, oxidation may proceed and the deep portion of the photoelectric conversion layer 2 may also be easily oxidized. Then, the photoelectric conversion layer 2 is preferably kept in an atmosphere in which both the water vapor concentration and the oxygen concentration are low.

[0052] In the holding step under the low oxygen atmosphere, the temperature of the low oxygen atmosphere is preferably 0°C to 100°C. If the temperature is too low when holding under the low oxygen atmosphere, it is difficult to perform Cu2O oxidation on the surface of the photoelectric conversion layer 2. On the contrary, if the temperature is too high when holding under the low oxygen atmosphere, an oxidation reaction occurs even in a deep portion of the photoelectric conversion layer 2. Therefore, a reaction similar to that during long-term holding in the air occurs. Therefore, during the holding step of the low oxygen atmosphere, the temperature of the low oxygen atmosphere is preferably 0°C to 50°C.

[0053] If the oxygen concentration, water vapor concentration and temperature are close to the lower limit of the above range, oxidation of the surface of the photoelectric conversion layer 2 is not easy to proceed. In addition, very little CuO is generated in a short time, so Voc hardly increases. Therefore, the retention time in the low oxygen atmosphere is preferably 72h to 1600h.

[0054] If the oxygen concentration, water vapor concentration and temperature are close to the upper limit of the above range, the surface of the photoelectric conversion layer 2 is excessively oxidized. Therefore, in some cases, the film quality of the photoelectric conversion layer 2 is reduced. Therefore, the retention time in the low oxygen atmosphere is preferably 1 hour to 1000 hours.

[0055] From the viewpoint of appropriately oxidizing a very thin surface region of the photoelectric conversion layer 2 , the retention time in the low-oxygen atmosphere is preferably 72 h to 1000 h, more preferably 500 h to 1000 h.

[0056] When the holding time in the low oxygen atmosphere during the holding step in the low oxygen atmosphere is defined as t[h], the oxygen concentration in the low oxygen atmosphere is defined as C o (g / L), and the water vapor concentration in the low oxygen atmosphere is defined as C w (g / L), preferably satisfying 1.0×10 -7 [h·g / L]≤t×C o [h·g / L]≤1.6×10 -3 [h·g / L] and 1.0×10 -7 [h·g / L]≤t×C w [h·g / L]≤6.5×10 -2 [h·g / L]; more preferably, 1.0×10 -6 [h·g / L]≤t×C o [h·g / L]≤2.5×10 -4 [h·g / L] and 1.0×10 -6 [h·g / L]≤t×Cw [h·g / L]≤2.0×10 -3 [h·g / L]; and more preferably, 1.0×10 -5 [h·g / L]≤t×C o [h·g / L]≤2.5×10 -4 [h·g / L] and 5.0×10 -5 [h·g / L]≤t×C w [h·g / L]≤2.5×10 -4 [h·g / L]. If the oxygen concentration and the water vapor concentration are high, even a short holding time is likely to cause CuO to form on the surface of the photoelectric conversion layer 2. If the oxygen concentration and the water vapor concentration are low, a longer holding time is likely to cause CuO to form on the surface of the photoelectric conversion layer 2, thereby increasing Voc when manufacturing a solar cell. Taking into account the oxygen concentration and the water vapor concentration, the holding time preferably satisfies the above range. The product of time and oxygen concentration or water vapor concentration refers to the product of time and average oxygen concentration or average water vapor concentration during the holding period in a low oxygen atmosphere.

[0057] The oxygen concentration in the gas (low oxygen atmosphere) can be determined from the oxygen concentration in the gas by using, for example, a galvanic oxygen sensor or a zirconium oxide sensor. In addition, the water vapor concentration in the gas (low oxygen atmosphere) can be determined from the measured dew point and temperature by using, for example, a capacitive or mirror reflection dew point meter.

[0058] Prior to the step (S02) of maintaining the member having the photoelectric conversion layer 2 formed on the first transparent electrode 1 under a low oxygen atmosphere, a step (S03) of placing the member having the photoelectric conversion layer 2 formed on the first transparent electrode 1 in an air atmosphere (second atmosphere) at 0°C to 50°C for 1 hour or less is performed.

[0059] In the multilayer film 100 manufactured by this process, the transmittance of the wavelength of 700nm to 1000nm is 50% or more. Therefore, the multilayer film 100 has excellent transmittance. The multilayer film 100 with excellent transmittance is suitable for the top cell of a light-transmitting solar cell and / or a multi-junction solar cell, wherein even the bottom cell can effectively generate electricity.

[0060] (Second Embodiment)

[0061] The second embodiment pertains to a solar cell and a method of manufacturing the solar cell. Figure 4 2 is a schematic cross-sectional view illustrating a solar cell 200. Figure 4As shown, it includes: a first transparent electrode 1; a photoelectric conversion layer 2; an n-type layer 3; and a second transparent electrode 4. The multilayer body obtained by stacking the first transparent electrode 1 and the photoelectric conversion layer 2 is the multilayer film 100 in the first embodiment. The photoelectric conversion layer 2 is arranged between the first transparent electrode 1 and the n-type layer 3. The n-type layer 3 is arranged between the photoelectric conversion layer 2 and the second transparent electrode 4. The photoelectric conversion layer 2 and the n-type layer 3 are used to form a pn junction. The first transparent electrode 1 and the photoelectric conversion layer 2 are the same as in the first embodiment, so the description is omitted. For example, an intermediate layer (not shown) may be arranged between the n-type layer 3 and the second transparent electrode 4. By stacking the solar cell 200 in the second embodiment onto a solar cell (e.g., a Si solar cell) having a photoelectric conversion layer with a narrower band gap than the photoelectric conversion layer 2, a multi-junction solar cell can be manufactured.

[0062] The n-type layer 3 is an n-type semiconductor layer. The n-type layer 3 is disposed between the photoelectric conversion layer 2 and the n-electrode 4. The n-type layer 3 is in direct contact with the surface of the p-type light absorbing layer 2, which is opposite to the surface in contact with the first transparent electrode 1. The n-type layer 3 is preferably a layer including an oxide layer and / or a sulfide layer. More specifically, the oxide layer used in the n-type layer 3 is preferably selected from Zn (1-x) A x O y (A=Si, Ge or Sn, 0≤x≤0.6, 0.9≤y≤1.1), Cu (2-x) M x O(M=Mn, Mg, Ca, Zn, Sr or Ba, 0≤x≤0.3), A (2-x-y) Al y Ga x O3 (A = Si, Ge or Sn, 1.3 ≤ x ≤ 2, 0 ≤ y ≤ 0.7, x + y ≤ 2) and Al (2-x) Ga x The sulfide layer used in the n-type layer 3 is preferably selected from Zn x In (2-2x) S (3-2x) (1≤x≤1.5), ZnS and In x Ga (1-x) At least one sulfide layer selected from the group consisting of S (0≤x≤1). The n-type layer 3 may have a multilayer structure obtained by stacking the above-mentioned oxide layers and / or sulfide layers.

[0063] The n-type layer 3 typically has a film thickness of 5nm to 100nm. If the thickness of the n-type layer 3 is equal to or less than 5nm, leakage current will be generated when the coverage of the n-type layer 3 is poor. This may result in reduced characteristics. When the coverage is good, the film thickness is not limited to the above. If the thickness of the n-type layer 3 exceeds 100nm, the characteristics may be reduced due to the excessive resistance of the n-type layer 4, or the short-circuit current may be reduced due to the reduced transmittance. Therefore, the thickness of the n-type layer 3 is preferably 10nm to 50nm. In addition, in order to achieve a film with good coverage, the surface roughness of the n-type layer 3 is preferably 5nm or less. When the quality of the n-type layer 3 is high, the solar cell can operate even when the film thickness is about 200nm.

[0064] The conduction band offset (ΔE=Ecp-Ecn) refers to the difference between the potential (Ecp (eV)) of the conduction band minimum (CBM) of the photoelectric conversion layer 2 and the potential (Ecn (eV)) of the conduction band minimum of the n-type layer 3, which is preferably -0.2eV to 0.6eV (-0.2eV≤ΔE≤+0.6eV). If the conduction band offset is greater than 0, the conduction band at the pn junction interface is discontinuous and a spike appears. When the conduction band offset is less than 0, the conduction band at the pn junction interface is discontinuous and a cliff appears. Both the spike and the cliff are barriers to photogenerated electrons. Therefore, the smaller the better. Therefore, the conduction band offset is preferably 0.0eV to 0.4eV (0.0eV≤ΔE≤+0.4eV). In this regard, the above does not apply to the case where conduction is performed using energy levels within the gap. The potential of the CBM can be estimated using the following steps. Photoelectron spectroscopy is a method for evaluating electron occupation energy levels and is used to actually measure the valence band top (VBM). Next, the band gap of the material being measured is estimated. The CBM is then calculated. However, for the actual pn junction interface, the ideal interface cannot be maintained due to the appearance of mutual diffusion and / or cation holes. This is very likely to cause a change in the band gap. For the above reasons, it is preferred to use inverse photoemission spectroscopy using the photoelectron emission reversal process to directly evaluate the CBM. Specifically, the electronic state of the pn junction interface can be evaluated by repeating photoelectron spectroscopy / inverse photoelectron spectroscopy and low-energy ion etching of the solar cell surface.

[0065] Before forming the n-type layer 3, it is preferably kept in an air atmosphere at 0°C to 50°C for less than 1 hour. If the holding time in the air atmosphere is prolonged, the inside of the photoelectric conversion layer 2 is oxidized. This is not preferred. Preferably, the n-type layer 3 is formed immediately after the multilayer thin film 100 is manufactured.

[0066] The second transparent electrode 4 is preferably a transparent conductive oxide film or a multilayer body thereof represented by the first transparent electrode 1 .

[0067] In the second embodiment, the process for manufacturing the multilayer film 100 according to the first embodiment should be adopted. This makes it possible to manufacture a solar cell with excellent light transmittance. A film with excellent light transmittance can be used for the photoelectric conversion layer 2, and a film with high light transmittance can also be deposited like other layers. This makes it possible to manufacture a solar cell with excellent light transmittance.

[0068] (Third Embodiment)

[0069] The third embodiment pertains to a multi-junction solar cell. Figure 5 is a schematic cross-sectional view illustrating a multi-junction solar cell in a third embodiment. Figure 5 The multi-junction solar cell 200 in the embodiment includes: the solar cell (first solar cell) 200 in the second embodiment arranged on the light incident side; and the second solar cell 201. The first solar cell 200 is manufactured using the multilayer thin film 100 manufactured by the process of the first embodiment. The band gap in the light absorption layer of the second solar cell 201 is smaller than the band gap in the photoelectric conversion layer 2 of the solar cell 200 in the second embodiment. Note that examples of the multi-junction solar cell in the present embodiment include solar cells in which three or more solar cells are connected.

[0070] The band gap of the photoelectric conversion layer of the multilayer thin film 100 in the first embodiment is about 2.0 eV to 2.2 eV. Therefore, the band gap in the light absorbing layer of the second solar cell 201 is preferably 1.0 eV to 1.6 eV. The light absorbing layer in the second solar cell is preferably one selected from the group consisting of at least one compound semiconductor selected from a perovskite compound, crystalline silicon, and a compound based on CIGS and CdTe having a high In content ratio.

[0071] (Fourth Embodiment)

[0072] The fourth embodiment pertains to a solar cell module. Figure 6 It is a perspective view illustrating a solar cell module 300 according to the fourth embodiment. Figure 6 In the solar cell module 300 in the embodiment, the first solar cell module 301 and the second solar cell module 302 are stacked. The first solar cell module 301 is placed on the light incident side, and the solar cell 200 made of the multilayer film 100 made by the process of the first embodiment is used. It is preferred to use the second solar cell 201 for the second solar cell module 302.

[0073] Figure 7 3 is a cross-sectional view illustrating the solar cell module 300. Figure 7In the embodiment of the present invention, the structure of the first solar cell module 301 is described in detail, but the structure of the second solar cell module 302 is not explained. In the second solar cell module 302, the selection of the structure of the solar cell module is appropriate depending on, for example, the light absorbing layer in the solar cell used. Figure 7 The solar cell assembly includes a plurality of subassemblies 303, which are framed by dotted lines and are electrically connected in series using wiring 304, so that a plurality of solar cells 200 (solar cells) are arranged horizontally. The plurality of subassemblies 303 are electrically connected in parallel or in series. Adjacent subassemblies 303 are electrically connected via busbars 305.

[0074] Adjacent solar cells 200 are configured so that the second transparent electrodes 4 on the upper side thereof are connected to the corresponding first transparent electrodes 1 on the lower side using wiring 304. Both ends of the solar cells 200 in the subassembly 303 are connected to the bus bar 305. The bus bar 305 is configured to electrically connect the plurality of subassemblies 303 in parallel or in series to adjust the voltage output to or from the second solar cell assembly 302. Note that how the solar cells 200 are connected as explained in the fourth embodiment is an example. Therefore, the solar cell assembly may be configured to use other connection methods.

[0075] (Fifth Embodiment)

[0076] The fifth embodiment belongs to a photovoltaic power generation system. The solar cell module in the fourth embodiment can be used as a generator to generate electricity in the photovoltaic power generation system in the fifth embodiment. The photovoltaic power generation system in this embodiment generates electricity using the solar cell module, and specifically includes: a solar cell module configured to generate electricity; a unit configured to convert the generated electricity; and a power storage unit configured to store the generated electricity or a load configured to consume the generated electricity. Figure 8 This is a diagram illustrating the structure of a photovoltaic power generation system 400 in this embodiment. Figure 8 The photovoltaic power generation system in includes a solar cell module 401 (300), a converter 402, a battery 403 and a load 404. Either the battery 403 or the load 404 may be omitted. The load 404 may be configured to utilize the electric energy stored in the battery 403. The converter 402 is a device having a circuit or an element configured to perform power conversion, such as voltage conversion or DC-AC conversion, including a DC-DC converter, a DC-AC converter or an AC-AC converter. As the configuration of the converter 402, a suitable configuration may be adopted according to the configuration of the generated voltage, the battery 403 and the load 404.

[0077] The solar cell included in each light receiving subassembly 301 included in the solar cell assembly 300 can generate electricity. This electric energy is converted by the converter 402 and stored in the storage battery 403 or consumed in the load 404. Preferably, the solar cell assembly 401 is equipped with a solar light tracking device, which is configured to continuously guide the solar cell assembly 401 to the sun, and is also equipped with a concentrator for concentrating sunlight, and / or is additionally provided with a device for improving power generation efficiency, for example.

[0078] Preferably, the photovoltaic power generation system 400 is used in real estate such as residences, commercial facilities, or factories, or in movable property such as vehicles, aircraft, electronic equipment, etc. In the above embodiment, the use of a photovoltaic conversion element for a solar cell module and having excellent conversion efficiency should increase the amount of power generated.

[0079] As an example of using the photovoltaic power generation system 400, a vehicle is shown. Fig. 9 2 is a schematic diagram illustrating a vehicle 500 . Fig. 9 The vehicle 500 in the embodiment includes a vehicle body 501, a solar cell module 502, a power converter 503, a battery 504, a motor 505, and a tire (wheel) 506. The power generated in the solar cell module 502 disposed on the upper portion of the vehicle body 501 is converted by the power converter 503, and the generated electric energy is charged in the battery 504 or consumed in a load such as the motor 505. When the tire (wheel) 506 is rotated by the motor 505, the power provided by the solar cell module 502 or the battery 504 can be used to drive the vehicle 500. The solar cell module 502 is not necessarily a multi-junction type, and may be composed of only a first solar cell module including, for example, the solar cell 200 in the second embodiment. If a transparent solar cell module 502 is used, it is preferred that the solar cell module 502 be used as a power generation window disposed on the side of the vehicle body 501 and on the top of the vehicle body 501.

[0080] The present invention will be described in more detail below in conjunction with the following examples. However, the present invention is not limited to the following examples.

[0081] [Example]

[0082] (Example 1)

[0083] The ITO transparent conductive film as the first transparent electrode on the back side was first deposited on the white glass substrate in the chamber, and then the Sb-doped SnO2 transparent conductive film was deposited thereon. The pressure of the chamber where the transparent member with the first transparent electrode was placed was reduced to 1×10 -3[Pa] or less. Next, a cuprous oxide compound was deposited thereon as a 2 μm photoelectric conversion layer by sputtering in an oxygen and argon atmosphere. The resulting structure was kept in an air atmosphere at 25°C for 30 minutes, and then kept in a low oxygen atmosphere created by reducing the oxygen and water vapor concentrations in the air for 1 hour (temperature 25°C, oxygen concentration 1.5×10 -7 (g / L), and the water vapor concentration is 1.2×10 -6 (g / L) atmosphere). Subsequently, n-type Zn 0.8 Ge 0.2 O is deposited on the p-type cuprous oxide layer by sputtering at room temperature. After that, an AZO transparent conductive film is deposited as the second transparent electrode on the surface side. Finally, MgF2 is deposited thereon as an anti-reflection film.

[0084] (Examples 2-41, Reference Example 1 and Comparative Examples 1-5)

[0085] Fig.10 and 11 The table in the embodiment, reference example and comparative example are provided together. As in Example 1, the solar cells in Examples 2-41, Reference Example 1 and Comparative Examples 1-5 are Fig.10 and 11 Note that in Example 41 and Comparative Example 5, In 0.7 Ga 0.3 S instead of n-type Zn 0.8 Ge 0.2 O is deposited on the p-type cuprous oxide layer.

[0086] Before the deposition of the n-type layer film, the presence of CuO is confirmed by XPS detection of the region 1 nm deep from the surface of the photoelectric conversion layer. When the CuO content of the region 1 nm deep from the surface of the photoelectric conversion layer is found to be 20 mol%-100 mol%, it is classified as A. When the CuO content of the region is found to be 1 mol% to less than 20 mol%, it is classified as B. When the CuO content of the region is found to be less than 1 mol%, it is classified as C. In addition, Voc is calculated based on the conversion efficiency of each solar cell obtained. When Voc is 0.95V or higher, it is classified as A. When Voc is 0.85V to less than 0.95V, it is classified as B. When Voc is less than 0.85V, it is classified as C. The transmittance of each solar cell obtained at a wavelength of 700nm to 1000nm is further evaluated. When the transmittance of the obtained solar cell at a wavelength of 700nm to 1000nm is 50% or more, it is classified as A. When the transmittance is 10% to less than 50%, it is classified as B. When the transmittance is less than 10%, it is classified as C. Fig.12 As shown in the table.

[0087] By keeping the sample in an atmosphere of low oxygen and water vapor concentration for a long time, CuO with a thickness of up to 1 nm can be generated in very thin areas. Similarly, if the sample is kept in an atmosphere of high oxygen and water vapor concentration for a long time, CuO is also generated. However, CuO is generated in deeper areas, which leads to a decrease in voltage. Therefore, it seems better to convert Cu2O to CuO over a considerable period of time in an atmosphere of low oxygen and water vapor concentration.

[0088] When the holding time in the low oxygen atmosphere is about 0.5h, the formation of CuO on the surface of the photoelectric conversion layer is not detected. However, when the holding time is 1h or 10h, the formation of a small amount of CuO can be detected. When the sample is kept in a low oxygen atmosphere for 72h or longer, a large amount of CuO is selectively formed in a very thin surface area of ​​the photoelectric conversion layer. At this time, before the sample is kept in a low oxygen atmosphere, the sample is exposed to air at room temperature for 0.5h. Keeping it in a low oxygen atmosphere for a long time can fully form copper oxide. However, when the sample is kept in a low oxygen atmosphere for 2000h as in the reference example, no further increase in Voc is observed. Therefore, it is not economical to keep it for 2000h for a long time. But from the point of view of increasing Voc, keeping it is a suitable treatment.

[0089] As shown in Examples 9 to 22, even when the oxygen concentration and water vapor concentration change, CuO can be formed in a very thin area and Voc increases. As shown in Examples 23 to 24, even when the product of oxygen concentration (water vapor concentration) and time is very large, CuO can be formed in a very thin surface area as in other embodiments. As shown in Comparative Example 2, when the oxygen concentration is too low, CuO cannot be formed. As shown in Comparative Examples 3 to 4, when the oxygen concentration is too high, Voc decreases due to excessive oxidation and CuO is formed at the same time.

[0090] As shown in Examples 25 to 27, CuO can be formed when the temperature changes from 0° C. to 100° C. The formation rate of CuO is slow at low temperatures, and the formation rate of CuO is fast at high temperatures. Therefore, it is preferred to adjust the oxygen concentration, water vapor concentration and time within the above range according to the temperature.

[0091] In addition, as shown in Examples 28 to 31, even if the air exposure conditions are changed, oxidation will not proceed in the deeper regions of the photoelectric conversion layer unless the treatment is performed for a long time at a higher temperature. The temperature in Example 29 is high. In addition, the time in Example 31 is long. Therefore, compared with other examples, oxidation proceeds in the deeper regions of the photoelectric conversion layer. This does not produce harmful effects such as reducing Voc.

[0092] In Examples 32 and 33, the holding time was 72 hours, a higher oxygen concentration was used, and the water vapor concentration was changed. In any of the examples, CuO was relatively abundant in a very thin surface area of ​​the photoelectric conversion layer; and copper oxide was not generated in deeper areas; this increased Voc. In Example 34, a higher oxygen concentration than that in Example 32 was used, and the holding time was 50 hours. Although the amount of copper oxide generated was smaller than that in Examples 32 and 33, the copper oxide generated was relatively abundant. Therefore, Voc increased.

[0093] In addition, even if the air exposure conditions are changed as in Examples 35 to 39, oxidation will not proceed in the deep region of the photoelectric conversion layer unless the treatment is performed for a long time at a higher temperature. The temperature is high in Example 36. In addition, the time is long in Example 39. Therefore, oxidation proceeds in a deeper region of the photoelectric conversion layer than in other Examples. This does not produce a harmful effect such as reducing Voc.

[0094] In Example 40, the total pressure is lower than the atmospheric pressure. Even if the total pressure is low, CuO is also formed in a very thin surface area of ​​the photoelectric conversion layer. In Example 41 and Comparative Example 5, the n-type layer is composed of sulfide. Even if the n-type layer is not made of oxide, good results can be obtained.

[0095] In Example 41, although the holding time is short, the oxygen concentration increases. Therefore, the CuO ratio is as high as when it is held for a long time. In addition, Voc is excellent.

[0096] In the specification, some elements are represented by only the chemical symbols of the elements.

[0097] Although certain embodiments have been described, these embodiments are presented by way of example only and are not intended to limit the scope of the invention. In fact, the novel embodiments described herein may be embodied in a variety of other forms; furthermore, various omissions, substitutions, and changes may be made in the form of the embodiments described herein without departing from the spirit of the invention. The accompanying claims and their equivalents are intended to cover forms or modifications that fall within the scope and spirit of the invention.

[0098] Explanation of symbols

[0099] 100 Multilayer Film

[0100] 1. First transparent electrode

[0101] 2 Photoelectric conversion layer

[0102] 3 N-type layer

[0103] 4 Second transparent electrode

[0104] 10 Base

[0105] 200 Solar Cells (First Solar Cells)

[0106] 201 Second Solar Cell

[0107] 300 Solar cell modules

[0108] 301 First Solar Cell Module

[0109] 302 Second solar cell module

[0110] 303 Subcomponents

[0111] 304 Busbar

[0112] 400 Photovoltaic power generation system

[0113] 401 Solar cell modules

[0114] 402 Converter

[0115] 403 Battery

[0116] 404 Payload

[0117] 500 vehicles

[0118] 501 Body

[0119] 502 Solar cell modules

[0120] 503 Power Converter

[0121] 504 Battery

[0122] 505 Motor

[0123] 506 Tire (Wheel)

Claims

1. A process for manufacturing a multilayer film, comprising: forming a photoelectric conversion layer including Cu2O as a main component on the first transparent electrode; and The member having the photoelectric conversion layer formed on the first transparent electrode was placed in an oxygen concentration of 5.0×10 -8 [g / L] to 5.0×10 -5 [g / L] for 1 h to 1600 h; During the placement under the first atmosphere, the temperature of the first atmosphere is 0° C. to 100° C.; During the period of being placed in the first atmosphere, the water vapor concentration in the first atmosphere is 5.0×10 -8 [g / L] to 5.0×10 -5 [g / L].

2. The process for manufacturing a multilayer thin film according to claim 1 further comprises the following step: before being placed in the first atmosphere, placing the component having the photoelectric conversion layer formed on the first transparent electrode in a second air atmosphere at 0°C to 50°C for 1 hour or less.

3. The process for producing a multilayer film according to claim 1 or 2, wherein: During the placement under the first atmosphere, the temperature of the first atmosphere is 0°C to 50°C.

4. The process for producing a multilayer film according to any one of claims 1 to 3, wherein: During the placement under the first atmosphere, the retention time in the first atmosphere is 72 h to 1600 h.

5. The process for producing a multilayer film according to any one of claims 1 to 4, wherein: During the period of being placed in the first atmosphere, the oxygen concentration in the low oxygen atmosphere was 5.0×10 -8 [g / L] to 3.5×10 -5 [g / L], and During the period of being placed in the first atmosphere, the water vapor concentration in the low oxygen atmosphere is 5.0×10 -8 [g / L] to 4.0×10 -5 [g / L].

6. The process for producing a multilayer film according to any one of claims 1 to 5, wherein: During the placement in the first atmosphere, when the retention time in the first atmosphere is defined as t[h], the oxygen concentration in the first atmosphere is defined as C O [g / L], and the water vapor concentration in the first atmosphere is defined as C W [g / L], Meet 1.0×10 -7 [h·g / L]≤t×C O [h·g / L]≤1.6×10 -3 [h·g / L], and Meet 1.0×10 -7 [h·g / L]≤t×C W [h·g / L]≤6.5×10 -2 [h·g / L].

7. A method for manufacturing a solar cell, comprising manufacturing a multi-layer thin film using the process for manufacturing a multi-layer thin film according to any one of claims 1 to 6.

8. A method for manufacturing a multi-junction solar cell, comprising manufacturing a multi-layer thin film using the process for manufacturing a multi-layer thin film according to any one of claims 1 to 6.

9. A method for manufacturing a solar cell module, comprising manufacturing a multilayer film using the process for manufacturing a multilayer film according to any one of claims 1 to 6.