A flexible and lightweight magnetic diaphragm material that is easy to operate after magnetization and a preparation method thereof
By inserting a flexible soft structural core layer into the magnetic diaphragm material and increasing the thickness of the non-magnetic phase, the problem of inconvenient operation caused by high magnetic attraction is solved, a balance of light weight, flexibility and high magnetic performance is achieved, improving user experience and Production convenience.
Patent Information
- Application Number
- CN202010459961.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-05-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-05-27
AI Technical Summary
When pursuing high magnetic attraction, existing magnetic diaphragm materials cause inconvenience in printing, installation, storage and other operations, and it is difficult to balance light weight and flexibility. Conventional methods such as modifying the magnetization method or adding a tissue paper layer will lead to a reduction in magnetic attraction or product Stiff.
Insert a flexible soft structural core layer between the magnetic layer and the decorative or directly printable writing layer to increase the thickness of the continuous non-magnetic phase, and use a modified polymer composite layer of non-magnetic inorganic or organic powder fillers to reduce the overall Density and weight while improving magnetic properties.
It effectively weakens the magnetic attraction between magnetic diaphragms, achieves edge alignment and automatic paper feeding, improves user experience and production convenience, and at the same time reduces the overall density and weight of the diaphragm, solving the conflicting needs of magnetic materials.
Smart Images

Figure CN113752655B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of magnetic materials, and in particular relates to a flexible and lightweight magnetic diaphragm material which is easy to operate after magnetization and a preparation method thereof. Background Art
[0002] Flexible magnetic diaphragm materials, because of their multiple properties of magnetism, flexibility, and diaphragm, can be directly printed or written on, can be installed magnetically without glue, and can be rolled up for easy storage and transportation. They are widely used in advertising consumables, teaching, projection, product display, architectural decoration and other fields.
[0003] Conventional magnetic film materials pursue "high, light, wide, and thin", with higher magnetic properties and higher magnetic attraction. The materials take up less storage space, transportation space, and use space, saving material loss and energy loss. However, high magnetic attraction also brings many unexpected troubles to our operations: adjacent printed films that have been magnetized during printing hold each other tightly due to magnetic attraction, and magnetic printing cannot be rubbed apart, so automatic paper feeding cannot be carried out; paper feeding in the printing machine is affected by magnetic attraction; magnetic film materials stacked together hold each other tightly due to magnetic attraction and cannot be aligned at the edges; these bring inconveniences to production, packaging, transportation, storage and other operations; too thin film products plus magnetic attraction, poor handling experience in taking out, installing, replacing, writing, etc., also affect the user experience.
[0004] The existing methods for solving the above problems include modifying the magnetization method between adjacent magnetic surfaces, random magnetic moments and random nonlinear multi-pole magnetization, so that the magnetic poles of adjacent diaphragms cannot be completely matched with each other, thereby weakening the magnetic attraction of adjacent surfaces. This technology can be seen in U.S. Patent US 9,455,078 B2. The defects it brings are obvious, because adjacent diaphragms cannot be completely matched, the attraction between each other becomes weak, and it is contrary to the principle of consistency in the production of products. The use effect and scope of diaphragm products are bound to be limited, and the magnetization fixture is complicated to manufacture, install and operate.
[0005] The invention patent with application number CN201710654934.0 and title "A directly printable magnetic paper product" discloses a directly printable magnetic paper product, which is characterized in that it consists of a friction covering layer, a magnetic layer and a printable layer sequentially arranged on one side of the friction covering layer, wherein the friction covering layer is cotton paper. The patent sacrifices an appropriate amount of magnetic properties through the isolation effect of the cotton paper to achieve the best match between magnetic attraction and maximum static friction, but the feel, volume and thickness of the cotton paper itself have certain limitations in terms of controllability, and the addition of the cotton paper layer increases the stiffness of the product and weakens its flexibility, so that the product becomes stiff or maintains curling after being curled and stretched out.
[0006] Despite this, the pursuit of higher and stronger magnetic properties of the diaphragm is still the primary condition for the use of diaphragm materials. Moreover, it is a contradiction to have both high magnetic attraction and light weight, because high magnetic attraction can only be achieved by a higher filling amount of magnetic powder or a thicker magnetic layer under certain conditions of material magnetic properties, which will inevitably make the diaphragm heavier.
[0007] There is no precedent in the field of magnetic diaphragm materials for inserting a flexible soft structural core layer between the magnetic layer and the decorative or directly printable writing layer, because this is contrary to the magnetic diaphragm material industry's consistent practice of pursuing "high, light, wide, and thin" and pursuing stronger magnetic properties. This will increase the thickness of the non-magnetic layer, which means increasing the overall volume and weight of the diaphragm, which will undoubtedly increase the threshold for the magnetic attraction requirements of the diaphragm material.
[0008] In the prior art, wood powder, rice husk, straw and other plant fibers are used as organic fillers to make wood-plastic composite materials: boards or profiles, which replace pure wood, but are better than pure wood, light, rigid, good processing performance, large elastic modulus, and not easy to deform. The composite material of the core layer of this technical solution is exactly the opposite of conventional technology. It is light and soft, and its hardness and elastic modulus are smaller than magnetic glue and coated paper. Its technical effect is very different from that of wood-plastic boards or profiles.
[0009] The technical solution of the present invention is to insert a flexible soft structure core layer between the magnetic layer and the decorative or directly printable writing layer, increase the proportion of the continuous non-magnetic phase thickness, and improve the application effect of the magnetic diaphragm material from the perspective of not improving the magnetic properties. Summary of the invention
[0010] A flexible and lightweight magnetic diaphragm material which is easy to operate after magnetization, characterized in that it includes a tightly connected magnetic layer, an isolation layer, and a decorative or directly printable and writable layer in sequence, the magnetic layer is a flexible modified polymer composite material layer with at least one magnetic powder selected from permanent magnetic material and soft magnetic material as a filler, the isolation layer is a modified polymer composite material layer with at least one non-magnetic inorganic powder or non-magnetic organic powder as a filler, the isolation layer has a lower density than the tightly connected magnetic layer, and a lower hardness and elastic modulus than the magnetic layer and the decorative or directly printable and writable layer, and the proportion of the continuous non-magnetic phase thickness of the diaphragm material to the total thickness of the diaphragm material exceeds 50%.
[0011] The continuous non-magnetic phase thickness refers to the sum of the thicknesses of the closely connected isolation layer, the decoration layer or the directly printable writing layer on the film material, without any interval of magnetic phase therebetween.
[0012] Furthermore, the density of the magnetic layer is [2.6, 4.0] g / cm 3 , the density of the isolation layer is [1.2, 2.3] g / cm 3, the density of the decorative or directly printable writing layer is [0.6, 1.5] g / cm 3 .
[0013] The numerical values in [ ] are a series of numerical values between the two numerical values in the brackets and including the end values.
[0014] Furthermore, the isolation layer has a Shore hardness lower than 45 degrees and an elastic modulus lower than 100 MPa.
[0015] Furthermore, the thickness of the magnetic layer is [0.10, 0.5] mm, the thickness of the isolation layer is [0.10, 0.5] mm, and the thickness of the decorative or directly printable writing layer is [0.015, 0.3] mm.
[0016] Furthermore, the isolation layer has a color of any one of red, orange, yellow, green, cyan, blue, and purple, or a combination thereof.
[0017] Furthermore, the non-magnetic inorganic powder is at least one of talc, calcium carbonate, magnesium carbonate, hollow glass beads, silicon dioxide, talc, kaolin, mica, pyrophyllite, wollastonite, tremolite, diopside, quartz, feldspar, sepiolite, attapulgite, bentonite, illite, zeolite, diatomaceous earth, silica powder, barium sulfate, calcium sulfate, alumina, magnesium oxide, aluminum hydroxide, magnesium hydroxide, graphite powder, carbon powder, and graphene powder.
[0018] Furthermore, the non-magnetic organic powder is at least one of wood powder, cotton linter, wheat straw, starch and synthetic fiber.
[0019] Furthermore, the isolation layer is a modified high molecular polymer composite material layer with non-magnetic inorganic powder and non-magnetic organic powder as fillers in a mass ratio of 5.5:4.5.
[0020] One of a UV protective layer, a silicone layer and a release film is arranged on the outer side of the magnetic layer.
[0021] The decorative or directly printable writing layer is a decorative or directly printable writing layer, or is composed of a decorative or directly printable writing substrate and a printing coating or erasable coating arranged on the decorative or directly printable writing substrate.
[0022] Furthermore, the decorative or directly printable writing layer material is selected from at least one or at least one layer of paper, organic film, canvas, fabric, non-woven fabric, and leather.
[0023] Furthermore, the paper is at least one of office paper, packaging paper, printing paper or writing paper.
[0024] Furthermore, the organic film layer is at least one or at least one layer of PE, PP, PET, TPU, CPU, WPU, PA, PVC, PVDC, EVOH, TPU, PI film, and polyimide film layer.
[0025] The high molecular polymer is at least one of rubber, thermoplastic elastomer, plastic and latex.
[0026] Further, the binder is at least one of CPE, NBR, HNBR, PVC, PE, PP, POE, EVA, EAA, EEA, TPE, TPU, SEBS, SBS, IR, IIR, CR, EPDM, NR, EVA emulsion, VAE emulsion, propylene benzene emulsion, silicone acrylic emulsion, pure acrylic emulsion, vinegar acrylic emulsion, and polyurethane emulsion.
[0027] The method for preparing a flexible and lightweight magnetic diaphragm material that is easy to operate after magnetization is characterized in that it includes the following steps: Step A, making a magnetic layer: magnetic powder, adhesive, and auxiliary agent are mixed in proportion, and then formed by calendaring, casting, and extrusion; making an isolation layer: non-magnetic material powder, adhesive, and auxiliary agent are mixed in proportion, and then formed by calendaring, casting, and extrusion; Step B, the magnetic layer and the isolation layer are bonded or pressed together; or, the magnetic layer and the isolation layer are integrally formed by co-extrusion or casting; Step C, laminating a decorative or directly printable writing layer; Step D, cutting and magnetizing.
[0028] Beneficial Effects of the Invention
[0029] 1. With the insertion of the core layer, the overall density and weight of the diaphragm material are reduced, and the requirement for the diaphragm material to rely on magnetic attraction for installation and fixation is reduced. This technical solution allows technical personnel in the industry to break away from the inertial thinking of simply improving the magnetic properties of magnetic materials to improve the quality of the diaphragm, balance the contradiction between light weight and magnetic requirements, and open up another world of design.
[0030] 2. With the insertion of the core layer, the ratio of the non-magnetic phase thickness of the diaphragm material to the total thickness of the diaphragm material is greatly increased, which effectively blocks or weakens the magnetic attraction between the overlapping magnetized flexible diaphragm materials. The edges can be aligned, and the magnetized magnetic paper on the printing press can be automatically fed, solving a major problem that has been plaguing the magnetic and printing industries. The problem of edge alignment during production, packaging, and transportation is also solved.
[0031] 3. The flexible modified polymer composite isolation layer with non-magnetic powder as filler has lower hardness and elastic modulus than the magnetic layer and the surface layer. It is soft, light and flat, has good compatibility with the magnetic layer, and provides a better hand-held feel during installation and replacement, avoiding the abrupt feeling of the material of the installation surface caused by writing on a diaphragm that is too thin, which provides a better experience for users of diaphragm materials.
[0032] 4. The non-magnetic powder filler used is abundant in nature and low in price. The product of the present invention is easy to mass produce, easy to implement, and easy to promote. While improving the quality of the flexible diaphragm product, it is also easy to be absorbed by the environment.
[0033] The present invention is further described below in conjunction with illustrations and specific embodiments, but this should not be construed as limiting the present invention, and any equivalent replacement of the present invention, addition to the prior art, or decoration will still fall within the protection scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a schematic diagram of the structure of the patent of the present invention: 2 is a magnetic layer, 1 is an isolation layer, and 3 is a decorative or directly printable writing layer.
[0035] Figure 2 This is a schematic diagram of a structure without an isolation layer in the prior art: 2 is a magnetic layer, and 3 is a decorative or directly printable writing layer.
[0036] Figure 3 This is a schematic diagram of a structure without an isolation layer in the prior art: 2 is a magnetic layer, 3 is a decorative or directly printable writing layer, and 4 is a cotton paper layer. DETAILED DESCRIPTION
[0037] As attached Figure 1 As shown: A flexible and lightweight magnetic film material which is easy to operate after magnetization, comprises in sequence a tightly connected magnetic layer 2, an isolation layer 1, and a decorative or directly printable writing layer 3, wherein the magnetic layer 2 is a modified polymer composite material layer with flexible permanent magnetic anisotropic ferrite magnetic powder as filler, the isolation layer 1 is a flexible polymer composite material layer with non-magnetic inorganic powder calcium carbonate as filler, and the decorative or directly printable writing layer 3 is an Indigo directly printable PP film (or coated paper).
[0038] The test records and analysis of the overall diaphragm material and the density and thickness of each layer are shown in Table 1.1, and the test of the physical parameters of each layer constituting the diaphragm is shown in Table 2.
[0039] The method for making the diaphragm material comprises the following steps:
[0040] Step A: Preparation of magnetic layer
[0041] Ingredients: Permanent magnetic anisotropic ferrite powder, chlorinated polyethylene, epoxy soybean oil, polyethylene wax, calcium zinc stabilizer are mixed in proportion;
[0042] Internal mixing: Use internal mixer to mix rubber, and discharge the clinker after mixing;
[0043] Open mixing: Use the open mixing mill to mix the mixed materials again;
[0044] Refining and crushing: The refined film is re-refined into small balls using an internal mixer and then crushed using a crusher;
[0045] Calendering: The crushed pellets are directly calendered using a calender;
[0046] Step B: Preparation of isolation layer
[0047] Ingredients: calcium carbonate powder (or wood powder), chlorinated polyethylene, epoxy soybean oil, polyethylene wax, calcium zinc stabilizer;
[0048] Internal mixing: Use internal mixer to mix rubber, and discharge the clinker after mixing;
[0049] Open mixing: Use the open mixing mill to mix the mixed materials again;
[0050] Refining and crushing: The refined film is re-refined into small balls using an internal mixer and then crushed using a crusher;
[0051] Calendering: The crushed pellets are directly calendered using a calender;
[0052] Step C, bonding
[0053] Magnetic layer, isolation layer, Indigo can directly print PP film layer (or coated paper) and laminate to form;
[0054] Step D, Cutting
[0055] Flexible lightweight diaphragm magnetic material samples of 460mm×320mm×0.35mm and 480mm×330mm×0.40mm were made respectively;
[0056] Magnetization
[0057] Tested on the HP Indigo 5500 / 7800 digital printing press, 100 pages of flexible lightweight magnetic material diaphragm samples prepared in the above steps can be aligned at the edges after being piled up, the magnetic printing can meet the requirements of rubbing and automatic paper feeding, the paper feed in the printing press is smooth, the magnetic printing quality is no problem, and the magnetic suction installation of the diaphragm material is stable.
[0058] The flexible and lightweight magnetic film material sample is soft, flat after being rolled up, and has a good user experience in handwriting, separation, magnetic installation, etc.
[0059] Comparative Example
[0060] As attached Figure 2 As shown: A flexible and lightweight magnetic film material which is easy to operate after magnetization, comprises in sequence a tightly connected magnetic layer 2 and a decorative or directly printable writing layer 3, wherein the magnetic layer 2 is a modified polymer composite material layer with flexible high-performance magnetic powder as filler, and the decorative or directly printable writing layer 3 is a writable PVC film.
[0061] The test records and analysis of the overall diaphragm material and the density and thickness of each layer are shown in Tables 1.1 and 1.2, and the test of the physical parameters of each layer constituting the diaphragm is shown in Table 2.
[0062] The method for making the diaphragm material comprises the following steps:
[0063] Step A: Preparation of magnetic layer
[0064] Ingredients: high-performance magnetic powder, chlorinated polyethylene, epoxy soybean oil, polyethylene wax, calcium zinc stabilizer are mixed in proportion;
[0065] Internal mixing: Use internal mixer to mix rubber, and discharge the clinker after mixing;
[0066] Open mixing: Use the open mixing mill to mix the mixed materials again;
[0067] Refining and crushing: The refined film is re-refined into small balls using an internal mixer and then crushed using a crusher;
[0068] Calendering: The crushed pellets are directly calendered using a calender;
[0069] Step B, bonding and molding
[0070] The magnetic layer and the writable PVC film layer are laminated and formed;
[0071] Or, as attached Figure 3 As shown, the cotton paper layer, the magnetic layer, and the writable PVC film layer are bonded together to form a shape;
[0072] Cut
[0073] Flexible magnetic diaphragm material samples of 460mm×320mm×0.35mm and 480mm×330mm×0.40mm were made respectively;
[0074] Magnetization
[0075] Tested on HP Indigo 5500 / 7800 digital printing press, 100 pages of flexible lightweight magnetic material film samples prepared by the above steps could not be aligned at the edges after being piled up, and the magnetic printing could not be rubbed open and automatically fed. However, the magnetic suction installation of the film material was stable.
[0076] Table 1.1 Diaphragm and each layer density, thickness test records and analysis
[0077]
[0078] Table 1.2 Density and thickness test records and analysis of membrane and each layer
[0079]
[0080] Remark:
[0081] The wood glue is a flexible modified high molecular polymer composite material with wood powder as filler;
[0082] The calcium gel is a modified polymer composite material with calcium titanate powder as filler;
[0083] The magnetic glue is a modified high molecular polymer composite material with permanent ferrite magnetic powder as filler.
[0084] Analysis 1
[0085] Comparative Example 2 is a conventional printable magnetic film material in the prior art, and its magnetic attraction is [14, 20] g / cm 2 The suction force is higher than that of the present technical solution [12, 16] g / cm 2 It is a specific example of the "high" higher magnetic properties and "smaller" volume pursued by the existing diaphragm industry. The purpose is to achieve better adsorption and reduce storage and transportation costs. It is achieved by increasing the thickness of the magnetic layer to 0.3mm and reducing the overall thickness of the diaphragm to 0.4mm.
[0086] Comparative Example 1 is also a prior art with higher adsorption capacity [42, 50] g / cm 2 The PVC film is based on Comparative Example 2, and the powder content of the magnetic layer is increased, and the density reaches 3.93 g / m 3 , and uses higher performance magnetic powder to improve the magnetic properties to achieve higher magnetic attraction, but the weight increases by 9.2%, although the overall thickness of the diaphragm is reduced to 0.4mm.
[0087] Comparative Example 3 realizes magnetic printing and automatic paper feeding by sticking another layer of cotton paper on the magnetic bottom layer to increase the maximum static friction, but it also increases the stiffness of the overall diaphragm product.
[0088] Embodiments 1, 2, and 3 of the present technical solution no longer follow the conventional approach: simply improving the magnetic properties to increase the adsorption effect and smaller volume, but take a different approach: inserting a core layer between the surface layer (decorative or directly writable and printed layer) and the bottom layer (magnetic layer). The density of the core layer is lower than that of the magnetic layer, which reduces the overall weight of the diaphragm by 14.7% to 32.7%, greatly increases the non-magnetic proportion of the diaphragm from 24%-25% in the comparative example to 53%-66%, and adopts a larger volume and a larger continuous non-magnetic proportion. In exchange for a smaller diaphragm weight, it effectively avoids the inertial method of improving the use of the diaphragm by relying on increasing the magnetic attraction and magnetic properties to improve the adsorption function of the magnetic diaphragm. The magnetic attraction is lower than that of comparison examples 1, 2, and 3, but it does not affect the normal use of the magnetic diaphragm. Because the diaphragm weight is reduced and the non-magnetic proportion is increased, the magnetic layer spacing between adjacent magnetic diaphragms stacked together is effectively isolated, and the diaphragm edge cannot be aligned due to magnetic attraction locking, and automatic paper feeding cannot be carried out when printing, and the soft magnetic attraction in the printing machine is also weakened.
[0089] Table 2 Physical parameters of each layer of the membrane
[0090]
[0091] Analysis 2
[0092] 1. Different from the conventional practice of pursuing higher hardness and elastic modulus in composite materials using inorganic material powder as fillers in the prior art, the hardness and elastic modulus of the calcium glue layer and the wood glue layer in this technical solution are lower than those of the PVC film layer, the magnetic glue layer, the PP film layer, and the coated paper layer, which improves the overall flexibility and softness of the diaphragm. Therefore, the flexible magnetic diaphragm material of the embodiment of this technical solution has a better user experience.
[0093] 2. The combination of the physical performance parameters of the three-layer diaphragm product optimizes the physical performance of the diaphragm product.
Claims
1. A flexible and lightweight magnetic diaphragm material that is easy to operate after magnetization, characterized in that: The invention comprises in sequence a tightly connected magnetic layer, an isolation layer, and a decorative or directly printable writing layer, wherein the magnetic layer is a flexible modified polymer composite material layer with at least one magnetic powder selected from permanent magnetic material and soft magnetic material as a filler, the isolation layer is a modified polymer composite material layer with at least one non-magnetic inorganic powder or non-magnetic organic powder as a filler, the density of the isolation layer is lower than the density of the tightly connected magnetic layer, and the hardness and elastic modulus are lower than those of the magnetic layer and the decorative or directly printable writing layer, the proportion of the continuous non-magnetic phase thickness of the diaphragm material to the total thickness of the diaphragm material exceeds 50%, and the continuous non-magnetic phase thickness of the diaphragm material is the total thickness of the isolation layer and the decorative or directly printable writing layer; The method for preparing a flexible and lightweight magnetic diaphragm material that is easy to operate after magnetization is characterized in that it includes the following steps: Step A, making a magnetic layer: magnetic powder, adhesive, and auxiliary agent are mixed in proportion, and then formed by calendaring, casting, and extrusion; making an isolation layer: non-magnetic material powder, adhesive, and auxiliary agent are mixed in proportion, and then formed by calendaring, casting, and extrusion; Step B, the magnetic layer and the isolation layer are bonded or pressed together; or, the magnetic layer and the isolation layer are integrally formed by co-extrusion or casting; Step C, laminating a decorative or directly printable writing layer; Step D, cutting and magnetizing.
2. According to claim 1, a flexible and lightweight magnetic diaphragm material that is easy to operate after magnetization, characterized in that: The density of the magnetic layer is 2.6-4.0 g / cm 3 , the density of the isolation layer is 1.2~2.3g / cm 3 The density of the decorative or directly printable writing layer is 0.6~1.5g / cm 3 .
3. A flexible and lightweight magnetic diaphragm material that is easy to operate after magnetization according to any one of claims 1 or 2, characterized in that: The isolation layer has a Shore hardness lower than 45 degrees and an elastic modulus lower than 100 MPa.
4. According to claim 3, a flexible and lightweight magnetic diaphragm material that is easy to operate after magnetization, characterized in that: The thickness of the magnetic layer is 0.1-0.5 mm, the thickness of the isolation layer is 0.10-0.5 mm, and the thickness of the decorative or directly printable writing layer is 0.015-0.3 mm.
5. According to claim 4, a flexible and lightweight magnetic diaphragm material that is easy to operate after magnetization, characterized in that: The color of the isolation layer is any one of red, orange, yellow, green, cyan, blue, and purple, or a combination thereof.
6. According to claim 5, a flexible and lightweight magnetic diaphragm material that is easy to operate after magnetization, characterized in that: The non-magnetic inorganic powder is at least one of talc, calcium carbonate, magnesium carbonate, hollow glass beads, silicon dioxide, talc, kaolin, mica, pyrophyllite, wollastonite, tremolite, diopside, quartz, feldspar, sepiolite, attapulgite, bentonite, illite, zeolite, diatomaceous earth, silica powder, barium sulfate, calcium sulfate, aluminum oxide, magnesium oxide, aluminum hydroxide, magnesium hydroxide, graphite powder, carbon powder, and graphene powder.
7. According to claim 5, a flexible and lightweight magnetic diaphragm material that is easy to operate after magnetization, characterized in that: The non-magnetic organic powder is at least one of wood powder, cotton linter, wheat straw, starch and synthetic fiber.
8. The flexible and lightweight magnetic diaphragm material that is easy to operate after magnetization according to claim 5, characterized in that: The isolation layer is a modified high molecular polymer composite material layer with non-magnetic inorganic powder and non-magnetic organic powder as fillers in a mass ratio of 5.5:4.
5.
9. The flexible and lightweight magnetic diaphragm material that is easy to operate after magnetization according to claim 1, characterized in that: One of a UV protective layer, a silicone layer and a release film is arranged on the outer side of the magnetic layer.
10. The flexible and lightweight magnetic diaphragm material that is easy to operate after magnetization according to claim 1, characterized in that: The high molecular polymer is at least one of rubber, thermoplastic elastomer, plastic and latex.