Composite positive electrode active material and preparation method thereof, positive electrode and lithium battery
By using a composite cathode active material of a lithium transition metal oxide core, a carbonaceous material, and a metal oxide shell in a lithium battery, the problem of battery performance degradation caused by the side reaction of the nickel-based cathode active material is solved, and the cycle life of the lithium battery is significantly improved. properties and high temperature stability.
Patent Information
- Application Number
- CN202110598158.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-31
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-05-31
AI Technical Summary
Existing nickel-based positive electrode active materials have side reactions in lithium batteries, resulting in battery performance degradation, poor life characteristics and thermal stability.
A composite cathode active material is used. This material is composed of lithium transition metal oxide as the core, and the outer layer is coated with a carbonaceous material and a metal oxide shell. A uniform shell layer is formed through mechanical grinding to block the contact between the electrolyte and the core and inhibit side reactions.
Effectively prevent battery performance degradation, improve the cycle characteristics and high temperature stability of lithium batteries, extend the life and increase the discharge capacity of nickel content.
Smart Images

Figure CN113764665B_ABST
Abstract
Description
[0001] This application is based on and claims the benefit of priority from Korean Patent Application No. 10-2020-0066016 filed on June 1, 2020, in the Korean Intellectual Property Office, the disclosure of which is incorporated herein in its entirety by reference. Technical Field
[0002] One or more embodiments relate to a composite positive electrode active material, a positive electrode including the composite positive electrode active material, a lithium battery using the positive electrode, and a method for preparing the composite positive electrode active material. Background Art
[0003] In order to meet the miniaturization and high performance of various devices, in addition to the miniaturization and weight reduction of lithium batteries, the high energy density of lithium batteries is becoming more and more important. That is, high-capacity lithium batteries are becoming more and more important.
[0004] In order to realize lithium batteries suitable for the above applications, positive electrode active materials having high capacity have been proposed.
[0005] The nickel-based positive active material in the art has poor lifespan characteristics and poor thermal stability due to side reactions.
[0006] Therefore, there is a need for a method capable of preventing battery performance degradation while including a nickel-based positive active material. Summary of the invention
[0007] One or more embodiments provide a novel composite positive active material that can prevent degradation of battery performance by suppressing side reactions of the composite positive active material.
[0008] One or more embodiments provide a positive electrode including a composite positive active material.
[0009] One or more embodiments provide a lithium battery using a positive electrode.
[0010] One or more embodiments provide a method for preparing a composite positive active material.
[0011] Additional aspects will be set forth in part in the description which follows and, in part, will be obvious from the description, or may be learned by practice of the disclosed presented embodiments.
[0012] According to one or more embodiments, the composite positive active material includes:
[0013] a core comprising a lithium transition metal oxide; and
[0014] a shell disposed on and conforming to the surface of the core,
[0015] Among them, the shell includes at least one first metal oxide represented by the formula M a O b (0 < a ≤ 3, 0 < b ≤ 4, when a is 1, 2, or 3, b is not an integer) and a carbonaceous material,
[0016] The first metal oxide is disposed in a carbonaceous material matrix, and M is at least one metal selected from Groups 2 to 13, 15, and 16 of the periodic table.
[0017] The lithium transition metal oxide contains nickel, and based on the total number of moles of transition metals, the content of nickel is 80 mol% or more.
[0018] According to one or more embodiments, the positive electrode includes a composite positive electrode active material.
[0019] According to one or more embodiments, the lithium battery includes a positive electrode.
[0020] According to one or more embodiments, a method for preparing a composite positive electrode active material includes:
[0021] Providing a lithium transition metal oxide;
[0022] Providing a composite; and
[0023] Mechanically grinding the lithium transition metal oxide and the composite,
[0024] Among them, the composite includes at least one first metal oxide represented by the formula M a O b (0 < a ≤ 3, 0 < b ≤ 4, when a is 1, 2, or 3, b is not an integer) and a carbonaceous material,
[0025] The first metal oxide is disposed in a carbonaceous material matrix, and M is at least one metal selected from Groups 2 to 13, 15, and 16 of the periodic table,
[0026] The lithium transition metal oxide contains nickel, and based on the total number of moles of transition metals, the content of nickel is 80 mol% or more. Description of the Drawings
[0027] Through the following description in conjunction with the drawings, the above and other aspects, features, and advantages of certain disclosed embodiments will become more apparent. In the drawings:
[0028] Figure 1 is a graph showing XPS images of bare NCA91, the composite prepared in Preparation Example 1, and the composite positive electrode active material prepared in Example 3;
[0029] Figure 2is a graph showing Raman spectra of the composite prepared in Preparation Example 1 and the composite positive active material prepared in Example 3; and
[0030] Figure 3 is a schematic diagram of a lithium battery according to an embodiment. DETAILED DESCRIPTION
[0031] Now will refer to embodiment in detail, the example of embodiment is shown in the accompanying drawings, wherein the same reference numerals refer to the same elements from time to time. In this regard, the current embodiment can have different forms and should not be construed as being limited to the description set forth herein. Therefore, the embodiment is described below only by reference to the drawings to illustrate the aspects of this specification. As used herein, the term "and / or" includes any combination and all combinations of one or more of the related listed items. Such as "at least one (kind / person) of ... " statement modifies the entire column of elements when it is after a column of elements, without modifying the individual elements in the column.
[0032] Since the inventive concept described below can be modified differently and can have various embodiments, specific embodiments are shown in the drawings and described in detail in the specific embodiments. However, this is not intended to limit the inventive concept to specific embodiments, and should be understood to include all modifications, equivalents or substitutes included in the technical scope of the inventive concept.
[0033] The terms used below are only used to describe specific embodiments and are not intended to limit the inventive concept. Unless the context clearly indicates otherwise, singular expressions include plural expressions. Hereinafter, it will also be understood that when the terms "comprise", "include" or "have" are used in this specification, the stated features, wholes, steps, operations, elements and / or components are indicated, but the presence or addition of one or more other features, wholes, steps, operations, elements, components and / or their groups are not excluded. Depending on the circumstances, the " / " used below can be interpreted as "and" or "or".
[0034] In the accompanying drawings, in order to clearly represent various layers and regions, the thickness is enlarged or reduced. Throughout the specification, the same reference numerals represent the same components. Throughout the specification, when referring to a component such as a layer, film, region or plate being placed "on" another component, it will be understood that the component can be directly on another component, or another component can be placed between the component and another component. Throughout the specification, although the terms "first", "second", "third" etc. can be used here to describe various elements, components, regions and / or layers, these elements, components, regions and / or layers should not be limited by these terms. These terms are only used to distinguish one component from another component.
[0035] Hereinafter, a composite cathode active material according to an embodiment, a cathode including the composite cathode active material, a lithium battery including the cathode, and a method for preparing the composite cathode active material will be described in more detail.
[0036] The composite cathode active material according to an embodiment includes: a core including a lithium transition metal oxide; and a shell disposed on the surface of the core and conformal with the surface of the core, wherein the shell includes at least one first metal oxide represented by the formula M a O b (0 < a ≤ 3, 0 < b ≤ 4, when a is 1, 2, or 3, b is not an integer), and a carbonaceous material, the first metal oxide being disposed in a carbonaceous material matrix, M being at least one metal selected from Groups 2 to 13, 15, and 16 of the periodic table, the lithium transition metal oxide containing nickel, and the content of nickel being 80 mol% or more based on the total moles of transition metals. For example, the total moles of transition metals refer to the total moles of elements other than lithium and oxygen (and F, S, Br, and Cl, if present) in the lithium transition metal oxide.
[0037] Hereinafter, the theoretical basis for providing excellent effects of the composite cathode active material according to an embodiment will be described, but this is for helping to understand the inventive concept and is not intended to limit the inventive concept in any way.
[0038] The shell including the first metal oxide and the carbonaceous material is disposed on and / or conformal with the core of the composite cathode active material. Due to aggregation, uniform coating of a conventional carbonaceous material on the core is difficult. On the other hand, the composite cathode active material uses a composite including at least one metal oxide or a plurality of first metal oxides disposed in a carbonaceous material matrix, thereby preventing aggregation of the carbonaceous material and placing a uniform shell on the core. Therefore, contact between the core and the electrolyte is effectively blocked, thereby preventing side reactions caused by contact between the core and the electrolyte. In addition, reduction of nickel ions due to the electrolyte is inhibited (Ni 3+ >Ni 2+) and cation mixing caused by the electrolyte, thereby preventing the formation of a resistive layer (such as a NiO phase). In addition, the elution of nickel ions is also suppressed. The carbonaceous material may be, for example, a crystalline carbonaceous material. The carbonaceous material may be a carbonaceous nanostructure. The carbonaceous material may be graphene. In this case, since the shell including graphene is flexible, it is easy to accept the volume change of the composite positive active material during charging and discharging, and the occurrence of cracks in the composite positive active material is suppressed. Since graphene has high electronic conductivity, the interface resistance between the composite positive active material and the electrolyte is reduced. Therefore, despite the introduction of a shell containing graphene, the internal resistance of the lithium battery is maintained or reduced. In addition, since the first metal oxide has voltage resistance, it is possible to prevent the degradation of the lithium transition metal oxide included in the core during charging and discharging at high voltage. As a result, the cycle characteristics and high temperature stability of the lithium battery including the composite positive active material are improved. The shell may include, for example, one first metal oxide or two or more different first metal oxides.
[0039] In addition, in the composite positive active material, the lithium transition metal oxide has a nickel content of 80 mol% or more based on the total molar number of the transition metal, and a shell including a first metal oxide and a carbonaceous material is disposed on the core, thereby providing high discharge capacity and cycle characteristics at the same time. Therefore, compared with a composite positive active material having a relatively low nickel content, a composite positive active material having a nickel content of 80 mol% or more can provide improved capacity and excellent life characteristics.
[0040] The metal included in the first metal oxide may be at least one selected from Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se. The first metal oxide may be, for example, Al 2 O z (0 <z<3)、NbO x (0 <x<2.5)、MgO x (0 <x<1)、Sc 2 O z (0 <z<3)、TiO y (0 <y<2)、ZrO y (0 <y<2)、V 2 O z (0 <z<3)、WO y (0 <y<2)、MnO y (0 <y<2)、Fe 2 O z (0 <z<3)、Co 3 O w (0 <w<4)、PdO x(0 < x < 1), CuO x (0 < x < 1), AgO x ((0 < x < 1), ZnO x (0 < x < 1), Sb 2 O z (0 < z < 3) and SeO y At least one selected from (0 < y < 2). Since such a first metal oxide is placed in a carbonaceous material matrix, the uniformity of the shell placed on the core is improved, and the voltage resistance of the composite cathode active material is also improved. For example, the shell includes Al 2 O x (0 < x < 3) as the first metal oxide.
[0041] The shell may further include at least one second metal oxide represented by M a O c (0 < a ≤ 3, 0 < c ≤ 4, when a is 1, 2 or 3, c is an integer). M is at least one metal selected from Groups 2 to 13, 15 and 16 of the periodic table. For example, the second metal oxide includes the same metal as the first metal oxide, and the ratio c / a of c to a in the second metal oxide is larger than the ratio b / a of b to a in the first metal oxide. For example, c / a > b / a. The second metal oxide is selected from Al 2 O 3 、NbO, NbO 2 、Nb 2 O 5 、MgO, Sc 2 O 3 、TiO 2 、ZrO 2 、V 2 O 3 、WO 2 、MnO 2 、Fe 2 O 3 、Co 3 O 4 、PdO, CuO, AgO, ZnO, Sb 2 O 3 and SeO 2 . The first metal oxide is the reduction product of the second metal oxide. The first metal oxide is obtained by reducing part or all of the second metal oxide. Therefore, compared with the second metal oxide, the first metal oxide has a lower oxygen content and a lower metal oxidation number. For example, the shell includes Al as the first metal oxide 2 O x (0 < x < 3) and Al as the second metal oxide 2 O3 .
[0042] In the composite positive electrode active material, for example, the carbonaceous material included in the shell is chemically bonded to the transition metal of the lithium transition metal oxide included in the core by a chemical bond. The carbon atoms (C) of the carbonaceous material in the shell are chemically bonded to the transition metal (Me) of the lithium transition metal oxide using oxygen atoms as intermediates through CO-Me bonding (e.g., CO-Ni bonding). The carbonaceous material included in the shell is chemically bonded to the lithium transition metal oxide included in the core so that the core and the shell can become a composite. Therefore, the composite of the core and the shell is different from a simple physical mixture of a carbonaceous material and a lithium transition metal oxide.
[0043] In addition, the first metal oxide and the carbonaceous material included in the shell are chemically bonded by a chemical bond. Here, the chemical bond is a covalent bond or an ionic bond. A covalent bond is, for example, a bond including at least one of an ester group, an ether group, a carbonyl group, an amide group, a carbonate anhydride group, and an anhydride group. An ionic bond is, for example, a bond including a carboxylic acid ion, an ammonium ion, or an acyl cation group.
[0044] The thickness of the shell is, for example, about 1 nm to about 5 μm, about 1 nm to about 1 μm, about 1 nm to about 500 nm, about 1 nm to about 200 nm, about 1 nm to about 100 nm, about 1 nm to about 90 nm, about 1 nm to about 80 nm, about 1 nm to about 70 nm, about 1 nm to about 60 nm, about 1 nm to about 50 nm, about 1 nm to about 40 nm, about 1 nm to about 30 nm, about 1 nm to about 20 nm, or about 1 nm to about 10 nm. When the thickness of the shell is within the above range, the increase in the internal resistance of the lithium battery including the composite positive active material is suppressed.
[0045] The composite positive electrode active material may further include: a third metal, doped on the core; or a third metal oxide, applied on the core. The shell may be disposed on the doped third metal or the applied third metal oxide. For example, after doping the third metal on the surface of the lithium transition metal oxide included in the core or applying the third metal oxide on the surface of the lithium transition metal oxide, the shell may be placed on the third metal and / or the third metal oxide. For example, the composite positive electrode active material may include: a core; an intermediate layer, disposed on the core; and a shell, disposed on the intermediate layer, wherein the intermediate layer may include a third metal or a third metal oxide. The third metal may be at least one metal selected from Al, Zr, W and Co, and the third metal oxide may be Al 2 O 3 , Li 2 O-ZrO 2 , WO 2 , CoO, Co 2 O 3、Co 3 O 4 wait.
[0046] The shell included in the composite positive active material includes at least one selected from a composite including a first metal oxide and a carbonaceous material (e.g., graphene) and a resultant product of grinding the composite, and the first metal oxide is placed in a carbonaceous material matrix (e.g., a graphene matrix). The shell is prepared by a composite including a first metal oxide and a carbonaceous material. In addition to the first metal oxide, the composite may also include a second metal oxide. The composite may include, for example, two or more first metal oxides. The composite may include, for example, two or more first metal oxides and two or more second metal oxides.
[0047] Based on the total weight of the composite positive active material, the content of the composite in the composite positive active material may be 3wt% or less, 2wt% or less, 1wt% or less, 0.5wt% or less, or 0.2wt% or less. Based on the total weight of the composite positive active material, the content of the composite may be about 0.01wt% to about 3wt%, about 0.01wt% to about 1wt%, about 0.01wt% to about 0.7wt%, about 0.01% to about 0.6wt%, about 0.1wt% to about 0.5wt%, about 0.01wt% to about 0.2wt%, about 0.01wt% to about 0.1wt%, or about 0.03wt% to about 0.07wt%. When the composite positive active material includes a composite within this range, the cycle characteristics of the lithium battery including the composite positive active material are further improved.
[0048] At least one selected from the first metal oxide and the second metal oxide included in the composite can have an average particle size of about 1nm to about 1μm, about 1nm to about 500nm, about 1nm to about 200nm, about 1nm to about 100nm, about 1nm to about 70nm, about 1nm to about 50nm, about 1nm to about 30nm, about 3nm to about 30nm, about 3nm to about 25nm, about 5nm to about 25nm, about 5nm to about 20nm or about 7nm to about 20nm. Because the first metal oxide and / or the second metal oxide have a particle size in the nanometer range, the first metal oxide and / or the second metal oxide can be more evenly distributed in the carbonaceous material matrix (e.g., graphene matrix) of the composite. Therefore, this composite can be uniformly applied to the core to form a shell. In addition, because the first metal oxide and / or the second metal oxide have a particle size in the nanometer range, the first metal oxide and / or the second metal oxide can be more uniformly arranged on the core. Therefore, the first metal oxide and / or the second metal oxide may be uniformly disposed on the core, thereby more effectively exhibiting the withstand voltage characteristic.
[0049] The average particle diameter of the first metal oxide and the second metal oxide is measured by a measuring device using a laser diffraction method or a dynamic light scattering method. Their average particle diameter is measured using a laser scattering particle size distribution instrument (e.g., LA-920 of Horiba Corporation), and is the value of the median diameter (D50) when the metal oxide particles accumulate from small particles to 50% in volume conversion.
[0050] The uniformity deviation of at least one selected from the first metal oxide and the second metal oxide included in the composite may be 3% or less, 2% or less, or 1% or less. For example, the uniformity may be obtained by XPS. Therefore, at least one selected from the first metal oxide and the second metal oxide included in the composite may have a uniformity deviation of 3% or less, 2% or less, or 1% or less, and may be uniformly distributed.
[0051] The carbonaceous material included in the composite has a branched structure, and at least one selected from the first metal oxide and the second metal oxide can be distributed in the branched structure of the carbonaceous material. The branched structure of the carbonaceous material includes a plurality of carbonaceous material particles in contact with each other. Since the carbonaceous material has a branched structure, various conductive paths can be provided. For example, the carbonaceous material included in the composite can be graphene or can have graphene. The branched structure of graphene includes a plurality of graphene particles in contact with each other. Since the graphene has a branched structure, various conductive paths can be provided.
[0052] The carbonaceous material included in the composite has a spherical structure, and at least one selected from the first metal oxide and the second metal oxide may be distributed in the spherical structure. The spherical structure of the carbonaceous material may have a size of about 50nm to about 300nm. A plurality of carbonaceous materials with a spherical structure may be provided. Since the carbonaceous material has a spherical structure, the composite may have a solid structure. For example, the carbonaceous material included in the composite may be graphene or may include graphene. The spherical structure of graphene may have a size of about 50nm to about 300nm. A plurality of graphenes with a spherical structure may be provided. Since the graphene has a spherical structure, the composite may have a solid structure.
[0053] The carbonaceous material included in the composite has a spiral structure in which a plurality of spherical structures are connected to each other, and at least one selected from the first metal oxide and the second metal oxide may be distributed in the spherical structure of the spiral structure. The spiral structure of the carbonaceous material may have a size of about 500nm to about 100μm. Since the carbonaceous material has a spiral structure, the composite may have a strong structure. The carbonaceous material included in the composite material may be graphene or may include graphene. The spiral structure of graphene may have a size of about 500nm to about 100μm. Since graphene has a spiral structure, the composite may have a strong structure.
[0054] The carbonaceous material included in the composite has a cluster structure in which a plurality of spherical structures are aggregated to each other, and at least one selected from the first metal oxide and the second metal oxide can be distributed in the spherical structure of the cluster structure. The cluster structure of the carbonaceous material can have a size of about 5 μm to about 1 mm or about 0.5 mm to about 10 cm. Since the carbonaceous material has a cluster structure, the composite can have a solid structure. The carbonaceous material included in the composite can be graphene or can include graphene. The cluster structure of graphene can have a size of about 5 μm to about 1 mm or about 0.5 mm to about 10 cm. Since graphene has a cluster structure, the composite can have a solid structure. The size of the spherical structure, the spiral structure or the cluster structure can be measured by a scanning electron microscope (SEM) or a transmission electron microscope (TEM). The size of the spherical structure, the spiral structure or the cluster structure can be the average particle size of the structure.
[0055] The composite may be a wrinkled polyhedral spherical structure, and at least one selected from the first metal oxide and the second metal oxide may be distributed inside the structure or on the surface of the structure. Since the composite is such a polyhedral spherical structure, the composite can be easily applied to the irregular surface of the core.
[0056] The composite may be a planar structure, and at least one selected from the first metal oxide and the second metal oxide may be distributed inside the structure or on the surface of the structure. Since the composite is such a two-dimensional planar structure, the composite can be easily applied to the irregular surface of the core.
[0057] The carbonaceous material included in the composite can extend a distance of 10 nm or less from the first metal oxide and can include at least 1 to 20 carbonaceous material layers. For example, due to stacking multiple carbonaceous material layers, a carbonaceous material with a total thickness of 12 nm or less can be placed on the first metal oxide. For example, the total thickness of the carbonaceous material can be about 0.6 nm to about 12 nm. The carbonaceous material included in the composite can be graphene or can include graphene. For example, due to stacking multiple graphene layers, graphene with a total thickness of 12 nm or less can be placed on the first metal oxide. For example, the total thickness of the graphene can be about 0.6 nm to about 12 nm.
[0058] The core included in the composite positive electrode active material includes, for example, a lithium transition metal oxide represented by the following formula 1:
[0059] <Formula 1>
[0060] Li a Ni x Co y M z O 2-b A b
[0061] In the above formula 1,
[0062] 1.0 ≤ a ≤ 1.2, 0 ≤ b ≤ 0.2, 0.8 ≤ x ≤ 1, 0 ≤ y ≤ 0.3, 0 < z ≤ 0.3, and x + y + z = 1,
[0063] M is at least one selected from manganese (Mn), niobium (Nb), vanadium (V), magnesium (Mg), gallium (Ga), silicon (Si), tungsten (W), molybdenum (Mo), iron (Fe), chromium (Cr), copper (Cu), zinc (Zn), titanium (Ti), aluminum (Al), and boron (B), and A is F, S, Cl, Br, or a combination thereof.
[0064] The core included in the composite positive electrode active material includes, for example, lithium transition metal oxides represented by the following formula 2 and formula 3:
[0065] <Formula 2>
[0066] LiNi x Co y Mn z O 2
[0067] <Formula 3>
[0068] LiNi x Co y Al z O 2
[0069] In Formulas 2 and 3, 0.8 ≤ x ≤ 0.95, 0 < y ≤ 0.2, 0 < z ≤ 0.2, and x + y + z = 1.
[0070] Based on the total molar amount of the transition metals (e.g., 100 mol% based on the total amount of Ni, Co, and M in Formula 1, 100 mol% based on the total amount of Ni, Co, and Mn in Formula 2, and 100 mol% based on the total amount of Ni, Co, and Al in Formula 3), each lithium transition metal oxide of Formulas 1 to 3 has a high nickel content of 80 mol% or more, 85 mol% or more, or 90 mol% or more, and can provide excellent initial capacity, room temperature life characteristics, and high temperature life characteristics.
[0071] The positive electrode according to another embodiment includes the above composite positive electrode active material. Since the positive electrode includes the above composite positive electrode active material, the positive electrode provides improved cycle characteristics and thermal stability.
[0072] The positive electrode is manufactured by the following exemplary method, but the manufacturing method is not necessarily limited to this method and is adjusted according to the required conditions.
[0073] First, a positive electrode active material composition is prepared by mixing the above composite positive electrode active material, a conductive agent, a binder, and a solvent. The prepared positive electrode active material composition is directly applied to an aluminum current collector and dried to form a positive electrode plate provided with a positive electrode active material layer. Alternatively, a film obtained by casting the positive electrode active material composition on a separate carrier and then separating the composition from the carrier is laminated on the aluminum current collector to form a positive electrode plate provided with a positive electrode active material layer.
[0074] As the conductive agent, carbon black, fine graphite particles, natural graphite, artificial graphite, acetylene black, Ketjen black, carbon fiber, carbon nanotube; metal powders, metal fibers, or metal tubes such as copper, nickel, aluminum, or silver; or conductive polymers such as polyphenylene derivatives can be used, but the present disclosure is not limited thereto. Any conductive agent can be used as long as it is used in the art.
[0075] As the binder, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene (PTFE), a mixture of the above polymers, or styrene-butadiene rubber polymer can be used, but the present disclosure is not limited thereto. Any binder can be used as long as it is used in the art. As the solvent, N-methylpyrrolidone (NMP), acetone, or water can be used, but the present disclosure is not limited thereto. Any solvent can be used as long as it is used in the art.
[0076] Holes can also be formed in the electrode plate by further adding a plasticizer or a pore former to the positive electrode active material composition.
[0077] The contents of the composite positive electrode active material, conductive agent, binder and solvent used in the positive electrode are at the levels commonly used in lithium batteries. Depending on the use and configuration of the lithium battery, one or more of the conductive agent, binder and solvent may be omitted.
[0078] Furthermore, the positive electrode may further include a general positive electrode active material other than the above-mentioned composite positive electrode active material.
[0079] As a general positive electrode active material, any lithium-containing metal oxide can be used without limitation as long as it is used in the art. For example, at least one of a composite oxide of lithium and a metal selected from cobalt, manganese, nickel, and a combination thereof can be used as the lithium-containing metal oxide, specifically, a compound represented by any one of the following formulae: Li a A 1-b B b D 2 (where 0.90≤a≤1, and 0≤b≤0.5); Li a E 1-b B b O 2-c D c (where 0.90≤a≤1, 0≤b≤0.5, and 0≤c≤0.05); LiE 2-b B b O 4-c D c (where 0≤b≤0.5 and 0≤c≤0.05); Li a Ni 1-b-c Co b B c D α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α≤2); Li a Ni 1-b-c Co b B c O 2-α F α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Co b B c O 2-α F 2 (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c D α(where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α≤2); Li a Ni 1-b- c Mn b B c O 2-α F α (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Mn b B c O 2-α F 2 (where 0.90≤a≤1, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni b E c G d O 2 (where 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5, and 0.001≤d≤0.1); Li a Ni b Co c Mn d GeO 2 (where 0.90≤a≤1, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, and 0.001≤e≤0.1); Li a NeG b O 2 (where 0.90≤a≤1, and 0.001≤b≤0.1); Li a CoG b O 2 (where 0.90≤a≤1, and 0.001≤b≤0.1); Li a MnG b O 2 (where 0.90≤a≤1, and 0.001≤b≤0.1); Li a Mn 2 G b O 4 (where 0.90≤a≤1, and 0.001≤b≤0.1); QO 2 ;QS 2 ;LiQS 2 ; V 2 O 5 ;LiV 2 O 5 ;LiIO 2 ;LiNiVO 4 ;Li(3-f) J 2 (PO 4 ) 3 (0≤f≤2);Li (3-f) Fe 2 (PO 4 ) 3 (0≤f≤2); and LiFePO 4 .
[0080] In the formula representing the above compounds, A is Ni, Co, Mn or a combination thereof; B is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element or a combination thereof; D is O, F, S, P or a combination thereof; E is Co, Mn or a combination thereof; F is F, S, P or a combination thereof; G is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is Ti, Mo, Mn or a combination thereof; I is Cr, V, Fe, Sc, Y or a combination thereof; and J is V, Cr, Mn, Co, Ni, Cu or a combination thereof.
[0081] A compound in which a coating is disposed on the surface of the above-mentioned compound can be used, and a mixture of the above-mentioned compound and a compound provided with a coating can also be used. The coating disposed on the surface of the above-mentioned compound may include a coating element compound, such as an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, a carbonate of a coating element, or a hydroxycarbonate of a coating element. The compound constituting the coating is amorphous or crystalline. The coating element included in the coating may be Mg, Al, Co, K, Na, Ca, Si, Ti, V, Sn, Ge, Ga, B, As, Zr, or a mixture thereof. The method for forming the coating is selected within the range that does not adversely affect the physical properties of the positive active material. The coating method is, for example, a spraying method, an immersion method, and the like. Since the coating method can be well understood by those skilled in the art, a detailed description of the coating method will be omitted.
[0082] A lithium battery according to another embodiment uses a positive electrode including the composite positive electrode active material.
[0083] Since the lithium battery employs the positive electrode including the composite positive electrode active material, improved cycle characteristics and thermal stability are provided.
[0084] The lithium battery can be manufactured, for example, by the following exemplary method, but the present disclosure is not necessarily limited to this method and is adjusted according to required conditions.
[0085] First, a positive electrode is prepared according to the above method for preparing a positive electrode.
[0086] Next, the negative electrode is prepared as follows. The negative electrode is prepared in the same manner as the positive electrode except that the negative electrode active material is used instead of the composite positive electrode active material. In addition, in the negative electrode active material composition, a conductive agent, a binder and a solvent substantially the same as those in the positive electrode can be used.
[0087] For example, a negative electrode active material, a conductive agent, a binder and a solvent are mixed to prepare a negative electrode active material composition, and the negative electrode active material composition is directly applied to a copper current collector to prepare a negative electrode plate. Alternatively, a film obtained by casting the prepared negative electrode active material composition on a separate carrier and then separating the composition from the carrier is laminated on a copper current collector to prepare a negative electrode plate.
[0088] Any negative electrode active material may be used as long as it is used in the art. For example, the negative electrode active material includes at least one selected from lithium metal, metal alloyable with lithium, transition metal oxide, non-transition metal oxide, and carbon-based material.
[0089] Examples of metals that can be alloyed with lithium include Si, Sn, Al, Ge, Pb, Bi, Sb, Si-Y alloys (Y is an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, or a combination thereof, other than Si) and Sn-Y alloys (Y is an alkali metal, an alkaline earth metal, a Group 13 element, a Group 14 element, a transition metal, a rare earth element, or a combination thereof, other than Sn). Element Y is, for example, Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, or a combination thereof.
[0090] The transition metal oxide is, for example, lithium titanium oxide, vanadium oxide or lithium vanadium oxide.
[0091] Non-transition metal oxides are, for example, SnO 2 or SiO x (0 <x<2)。
[0092] The carbon-based material is, for example, crystalline carbon, amorphous carbon or a mixture thereof. Crystalline carbon is, for example, graphite (such as plate-like, flaky, spherical or fibrous natural graphite or artificial graphite). Amorphous carbon is, for example, soft carbon (low temperature fired carbon), hard carbon, mesophase pitch carbide or fired coke.
[0093] The contents of the negative electrode active material, conductive agent, binder and solvent used in the negative electrode are at levels generally used in lithium batteries. Depending on the use and configuration of the lithium battery, one or more of the conductive agent, binder and solvent may be omitted.
[0094] Next, a separator to be inserted between the positive electrode and the negative electrode is prepared.
[0095] Any diaphragm can be used as long as it is generally used in lithium batteries. As the diaphragm, for example, a diaphragm having low resistance to ion migration of the electrolyte and having excellent electrolyte moisture retention ability is used. The diaphragm is a nonwoven fabric or a textile fabric including at least one selected from glass fiber, polyester, Teflon, polyethylene, polypropylene, polytetrafluoroethylene (PTFE) and a combination thereof. For lithium ion batteries, for example, a rollable diaphragm including polyethylene, polypropylene, etc. is used, and for lithium ion polymer batteries, a diaphragm with excellent organic electrolyte impregnation ability is used.
[0096] The separator is manufactured by the following exemplary method, but the present disclosure is not necessarily limited to this method and is adjusted according to required conditions.
[0097] First, a polymer resin, a filler and a solvent are mixed to prepare a separator composition. The separator composition is directly applied to an electrode and dried to form a separator. Alternatively, a film obtained by casting and drying the separator composition on a support and then separating the composition from the support is laminated on the electrode to form a separator.
[0098] The polymer used to make the separator is not particularly limited, and any polymer can be used as long as it is used as a binder for the electrode plate. For example, as the polymer, vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, or a mixture thereof is used.
[0099] Next, an electrolyte is prepared.
[0100] The electrolyte is, for example, an organic electrolyte. For example, the organic electrolyte is prepared by dissolving a lithium salt in an organic solvent.
[0101] As the organic solvent, any organic solvent can be used as long as it is used in the art. The organic solvent is, for example, propylene carbonate, ethylene carbonate, fluoroethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, γ-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, cyclopentane, dichloroethane, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether or a mixture thereof.
[0102] As the lithium salt, any lithium salt can be used as long as it is used in the art. The lithium salt is, for example, LiPF 6 , LiBF 4 、LiSbF 6 、LiAsF 6 、LiClO 4 、LiCF 3 SO 3 、Li(CF 3 SO 2 ) 2 N, LiC 4 F 9 SO 3 、LiAlO 2 、LiAlCl 4 、LiN(C x F 2x+1 SO 2 )(C y F 2y+1 SO 2 )(wherein x and y are natural numbers), LiCl, LiI or a mixture thereof.
[0103] Optionally, the electrolyte is a solid electrolyte. The solid electrolyte is, for example, boron oxide or lithium oxynitride, but is not limited thereto. Any solid electrolyte may be used as long as it is used in the art. The solid electrolyte is formed on the negative electrode by a method such as sputtering, or a separate solid electrolyte sheet is laminated on the negative electrode.
[0104] like Figure 3 As shown in FIG. 1 , a lithium battery 1 includes a positive electrode 3, a negative electrode 2, and a separator 4. The positive electrode 3, the negative electrode 2, and the separator 4 are wound or folded to be accommodated in a battery case 5. An organic electrolyte is injected into the battery case 5 and the battery case 5 is sealed with a cap assembly 6 to complete the lithium battery 1. The battery case 5 is cylindrical, but is not necessarily limited to this shape, for example, its shape is a square, a film, etc.
[0105] The pouch-type lithium battery includes at least one battery structure. A separator is disposed between the positive electrode and the negative electrode to form the battery structure. After stacking the battery structures into a dual-battery structure, it is impregnated with an organic electrolyte solution and accommodated and sealed in a pouch to complete the pouch-type lithium battery. A plurality of battery structures are stacked to form a battery pack, and the battery pack is used in all devices that require high capacity and high output. For example, the battery pack is used in laptop computers, smart phones, electric vehicles, etc.
[0106] Since lithium batteries have excellent life characteristics and high rate characteristics, they are used in electric vehicles (EVs). For example, lithium batteries are used in hybrid vehicles (such as plug-in hybrid electric vehicles (PHEVs)). In addition, lithium batteries are used in fields that require a large amount of power storage. For example, lithium batteries are used in electric bicycles, power tools, etc.
[0107] A method for preparing a composite positive electrode active material according to another embodiment includes: providing a lithium transition metal oxide; providing a composite; and mechanically grinding the lithium transition metal oxide and the composite, wherein the composite includes at least one first metal oxide represented by the formula M a O b (0 < a ≤ 3, 0 < b ≤ 4, when a is 1, 2, or 3, b is not an integer) and graphene, the first metal oxide is disposed within a carbonaceous material matrix, M is at least one metal selected from Groups 2 to 13, 15, and 16 of the periodic table, the transition metal oxide contains nickel, and based on the total molar amount of the transition metals, the content of nickel is 80 mol% or more.
[0108] Provide a lithium transition metal oxide. The lithium transition metal oxide is, for example, a compound represented by any one of Formulas 1 to 3 above.
[0109] The step of providing the composite includes, for example, supplying a reaction gas including a carbon source gas to a structure including a metal oxide and performing a heat treatment.
[0110] The step of providing the composite includes, for example, supplying a reaction gas including a carbon source gas to a second metal oxide represented by the formula M a O c (0 < a ≤ 3, 0 < c ≤ 4, when a is 1, 2, or 3, c is an integer) and performing a heat treatment, and M is at least one metal selected from Groups 2 to 13, 15, and 16 of the periodic table.
[0111] The carbon source gas may be a compound represented by Formula 4 below, or a mixed gas of a compound represented by Formula 4 and at least one selected from a compound represented by Formula 5 and an oxygen-containing gas represented by Formula 6.
[0112] <Formula 4>
[0113] C n H (2n+2-a) [OH] a
[0114] In Formula 4, n is from 1 to 20 and a is 0 or 1;
[0115] <Formula 5>
[0116] C n H 2n
[0117] In Formula 5, n is from 2 to 6; and
[0118] <Formula 6>
[0119] C x H y O z
[0120] In Formula 6, x is 0 or an integer from 1 to 20, y is 0 or an integer from 1 to 20, and z is 1 or 2.
[0121] The compound represented by Formula 4 and the compound represented by Formula 5 include at least one selected from methane, ethylene, propylene, methanol, ethanol, and propanol. The oxygen-containing gas represented by Formula 6 includes carbon dioxide (CO 2 ), carbon monoxide (CO), water vapor (H 2 O), or a mixture thereof.
[0122] After supplying a reaction gas including a carbon source gas to a second metal oxide represented by M a O c (0 < a ≤ 3, 0 < c ≤ 4, when a is 1, 2, or 3, c is an integer) and performing heat treatment, a cooling process using at least one inert gas selected from nitrogen, helium, and argon can be further performed. The cooling process refers to a process of adjusting the temperature to room temperature (about 20 °C to about 25 °C). The carbon source gas may include at least one inert gas selected from nitrogen, helium, and argon.
[0123] In the method for preparing a composite, a process of growing a carbonaceous material (such as graphene) can be performed according to a gas-phase reaction under various conditions.
[0124] According to the first condition, for example, first, methane is supplied to a reactor provided with M a O cA reactor for a second metal oxide represented by (0 < a ≤ 3, 0 < c ≤ 4, where c is an integer when a is 1, 2, or 3) is heated to a heat treatment temperature (T). The heating time to reach the heat treatment temperature (T) is about 10 minutes to about 4 hours, and the heat treatment temperature (T) is about 700 °C to about 1100 °C. Heat treatment is performed at the heat treatment temperature (T) for a reaction time. The reaction time is, for example, about 4 hours to about 8 hours. The obtained product after heat treatment is cooled to room temperature to prepare a composite. The time taken for the process of cooling the obtained product from the heat treatment temperature to room temperature is, for example, about 1 hour to 5 hours.
[0125] According to the second condition, for example, first, hydrogen is supplied to a reactor provided with a second metal oxide represented by M a O c (0 < a ≤ 3, 0 < c ≤ 4, where c is an integer when a is 1, 2, or 3) and heated to a heat treatment temperature (T). The heating time to reach the heat treatment temperature (T) is about 10 minutes to about 4 hours, and the heat treatment temperature (T) is about 700 °C to about 1100 °C. After heat treatment is performed at the heat treatment temperature (T) for a predetermined reaction time, methane gas is supplied, and heat treatment is performed for the remaining reaction time. The reaction time is, for example, about 4 hours to about 8 hours. The obtained product after heat treatment is cooled to room temperature to prepare a composite. Nitrogen is supplied during the process of cooling the obtained product. The time taken for the process of cooling the obtained product from the heat treatment temperature to room temperature is, for example, about 1 hour to 5 hours.
[0126] According to the third condition, for example, first, hydrogen is supplied to a reactor provided with a second metal oxide represented by M a O c (0 < a ≤ 3, 0 < c ≤ 4, where c is an integer when a is 1, 2, or 3) and heated to a heat treatment temperature (T). The heating time to reach the heat treatment temperature (T) is about 10 minutes to about 4 hours, and the heat treatment temperature (T) is about 700 °C to about 1100 °C. After heat treatment is performed at the heat treatment temperature (T) for a predetermined reaction time, a mixed gas of methane and hydrogen is supplied, and heat treatment is performed for the remaining reaction time. The reaction time is, for example, about 4 hours to about 8 hours. The obtained product after heat treatment is cooled to room temperature to prepare a composite. Nitrogen is supplied during the process of cooling the obtained product. The time taken for the process of cooling the obtained product from the heat treatment temperature to room temperature is, for example, about 1 hour to 5 hours.
[0127] In the process of preparing the composite, when the carbon source gas includes water vapor, a composite having very excellent electrical conductivity can be obtained. The content of water vapor in the gas mixture is not limited, and for example, it is about 0.01 vol% to about 10 vol% based on 100 vol% of the total carbon source gas. The carbon source gas can be, for example: methane; a mixed gas containing methane and an inert gas; or a mixed gas containing methane and an oxygen-containing gas.
[0128] The carbon source gas may be, for example, methane; a mixed gas of methane and carbon dioxide; or a mixed gas of methane, carbon dioxide and water vapor. The molar ratio of methane to carbon dioxide in the mixed gas of methane and carbon dioxide is about 1:0.20 to about 1:0.50, about 1:0.25 to about 1:0.45, or about 1:0.30 to about 1:0.40. The molar ratio of methane, carbon dioxide and water vapor in the mixed gas of methane, carbon dioxide and water vapor is about 1:0.20-0.50:0.01-1.45, about 1:0.25-0.45:0.10-1.35, or about 1:0.30-0.40:0.50-1.0.
[0129] The carbon source gas is, for example, carbon monoxide or carbon dioxide. The carbon source gas is, for example, a mixed gas of methane and nitrogen. The molar ratio of methane to nitrogen in the mixed gas of methane and nitrogen is about 1:0.20 to about 1:0.50, about 1:0.25 to about 1:0.45, or about 1:0.30 to about 1:0.40. The carbon source gas may not include an inert gas such as nitrogen.
[0130] The heat treatment pressure can be selected taking into account the heat treatment temperature, the composition of the gas mixture and the desired amount of carbon coating. The heat treatment pressure can be controlled by adjusting the amount of the inflow gas mixture and the amount of the outflow gas mixture. The heat treatment pressure is, for example, 0.5 atm or greater, 1 atm or greater, 2 atm or greater, 3 atm or greater, 4 atm or greater, or 5 atm or greater.
[0131] The composition of heat treatment temperature, heat treatment pressure, gas mixture and the coating amount of desired carbon can be considered to select heat treatment time.For example, the reaction time under heat treatment temperature is for example about 10 minutes to about 100 hours, about 30 minutes to about 90 hours or about 50 minutes to about 40 hours.For example, as the heat treatment time increases, the amount of deposited carbon (for example, Graphene) increases, so the electrical property of composite can be improved.However, this trend may not be proportional to time.For example, after a predetermined time period, the deposition of carbon (for example, Graphene) may no longer occur, or the deposition rate of carbon (for example, Graphene) may be reduced.
[0132] Even at relatively low temperatures, a O c(0 < a ≤ 3, 0 < c ≤ 4, where c is an integer when a is 1, 2, or 3) represents a second metal oxide and its reduction product selected from the first metal oxide represented by M a O b (0 < a ≤ 3, 0 < b ≤ 4, a is 1, 2, or 3, and b is not an integer) is uniformly coated with a carbonaceous material (e.g., graphene coating) through a gas-phase reaction of the above carbon source gas to obtain a composite.
[0133] The composite includes a carbonaceous material matrix (e.g., graphene matrix), and the carbonaceous material matrix has at least one structure selected from a spherical structure, a helical structure in which multiple spherical structures are connected to each other, a cluster structure in which multiple spherical structures are aggregated, and a sponge structure, and is selected from the first metal oxide represented by M a O b (0 < a ≤ 3, 0 < b ≤ 4, a is 1, 2, or 3, and b is not an integer) and at least one selected from the second metal oxide represented by M a O c (0 < a ≤ 3, 0 < c ≤ 4, where c is an integer when a is 1, 2, or 3) is placed in the carbonaceous material matrix (e.g., graphene matrix).
[0134] Next, the lithium transition metal oxide and the composite are mechanically ground. A Nobilta mixer can be used for grinding. The rotation speed of the mixer during grinding is, for example, about 1000 rpm to about 2500 rpm. When the grinding speed is less than 1000 rpm, the shear force applied to the lithium transition metal oxide and the composite is weak, so it is difficult for the lithium transition metal oxide and the composite to form chemical bonds. When the grinding speed is too high, since the formation of the composite is carried out in too short a time, the composite may not be uniformly applied to the lithium transition metal oxide, so it may be difficult to form a uniform and continuous shell. The grinding time is, for example, about 5 minutes to about 100 minutes, about 5 minutes to about 60 minutes, or about 5 minutes to about 30 minutes. When the grinding time is too short, the composite cannot be uniformly applied to the lithium transition metal oxide, so it will be difficult to form a uniform and continuous shell. When the grinding time is too long, the production efficiency will decrease. Based on the total weight of the lithium transition metal oxide and the composite, the content of the composite can be 3 wt% or less, 2 wt% or less, or 1 wt% or less. For example, based on 100 parts by weight of the mixture of the lithium transition metal oxide and the composite, the content of the composite can be about 0.01 part by weight to about 3 parts by weight, about 0.1 part by weight to about 3 parts by weight, about 0.1 part by weight to about 2 parts by weight, or about 0.1 part by weight to about 1 part by weight.
[0135] The average particle size (D50) of the composite used in the mechanical grinding of lithium transition metal oxides and composites is, for example, about 1 μm to about 20 μm, about 3 μm to about 15 μm, or about 5 μm to about 10 μm.
[0136] The present disclosure will be described in more detail by the following examples and comparative examples. However, these examples are for illustrative purposes only, and the scope of the present disclosure is not limited thereto.
[0137] (Preparation of Composite)
[0138] Preparation Example 1: Al 2 O 3 @Gr Composite
[0139] Al 2 O 3 particles (average particle size: about 15 nm) were introduced into the reactor, and then CH 4 was supplied to the reactor at about 300 sccm and about 1 atm for about 30 minutes, and the temperature in the reactor was raised to 1000 °C.
[0140] Subsequently, heat treatment was performed for 7 hours while maintaining the temperature at 1000 °C. Subsequently, the temperature in the reactor was adjusted to room temperature (about 20 °C to about 25 °C) to obtain a composite in which Al 2 O 3 particles and Al 2 O z (0 < z < 3) particles were embedded in graphene.
[0141] The content of alumina included in the composite was 60 wt%.
[0142] Comparative Preparation Example 1: SiO 2 @Gr Composite
[0143] SiO 2 particles (average particle size: about 15 nm) were introduced into the reactor, and then CH 4 was supplied to the reactor at about 300 sccm and about 1 atm for about 30 minutes, and the temperature in the reactor was raised to 1000 °C.
[0144] Subsequently, heat treatment was performed for 7 hours while maintaining the temperature at 1000 °C. Subsequently, the temperature in the reactor was adjusted to room temperature (about 20 °C to about 25 °C) to obtain a composite in which SiO 2 particles and SiO y (0 < y < 2) particles were embedded in graphene.
[0145] (Preparation of Composite Cathode Active Material)
[0146] Example 1: 0.1wt% Al 2 O 3 @Gr composite coated NCA91 (0.06wt% alumina)
[0147] LiNi was mixed using a Nobilta mixer (Hosokawa, Japan) at a speed of about 1000 rpm to about 2000 rpm. 0.91 Co 0.05 Al 0.04 O 2 (hereinafter, referred to as NCA91) and the composite prepared in Preparation Example 1 were ground for about 5 minutes to about 30 minutes to obtain a composite positive active material.
[0148] The mixing weight ratio of NCA91 to the composite prepared in Preparation Example 1 was 99.9:0.1.
[0149] Example 2: 0.25wt%Al 2 O 3 @Gr composite coated NCA91 (0.15wt% alumina)
[0150] A composite positive active material was prepared in the same manner as in Example 1, except that the mixing weight ratio of NCA91 to the composite prepared in Preparation Example 1 was changed to 99.75:0.25.
[0151] Example 3: 0.4wt%Al 2 O 3 @Gr composite coated NCA91 (0.24wt% alumina)
[0152] A composite cathode active material was prepared in the same manner as in Example 1, except that the mixing weight ratio of NCA91 to the composite prepared in Preparation Example 1 was changed to 99.6:0.4.
[0153] Example 4: 1.0wt% Al 2 O 3 @Gr composite coated NCA91 (0.6wt% alumina)
[0154] A composite positive active material was prepared in the same manner as in Example 1, except that the mixing weight ratio of NCA91 to the composite prepared in Preparation Example 1 was changed to 99.0:1.0.
[0155] Comparison example 1: Bare NCA91
[0156] NCA91 was used as the positive electrode active material.
[0157] Comparative Example 2: 0.4wt%SiO2 @Gr composite coated NCA91 (0.24wt% silica)
[0158] In addition to using the SiO prepared in Comparative Preparation Example 1 2 @Gr composite instead of Al prepared in Preparation Example 1 2 O 3 A composite positive electrode active material was prepared in the same manner as in Example 3 except for the @Gr composite.
[0159] (Manufacture of lithium batteries (half-cells))
[0160] Example 5
[0161] (Manufacturing of positive electrode)
[0162] A mixture obtained by mixing the composite cathode active material prepared in Example 1, a carbon conductive agent (Denka Black), and polyvinylidene fluoride (PVDF) at a weight ratio of 92:4:4 was mixed with N-methylpyrrolidone (NMP) in an agate mortar to prepare a slurry.
[0163] The slurry was applied on an aluminum current collector having a thickness of 15 μm by bar coating, dried at room temperature, further dried in a vacuum, and rolled and punched to obtain a positive electrode plate having a thickness of 55 μm.
[0164] (Button battery manufacturing)
[0165] Each button cell was manufactured using the obtained positive electrode plate, in which lithium metal was used as a counter electrode, and a PTFE separator and 1.3 M LiPF 6 A solution dissolved in EC (ethylene carbonate) + EMC (ethyl methyl carbonate) + DMC (dimethyl carbonate) (3:4:3 by volume) was used as an electrolyte.
[0166] Examples 6 to 8
[0167] Button cells were manufactured in the same manner as in Example 5, except that the composite positive active materials prepared in Examples 2 to 4 were used instead of the composite positive active material prepared in Example 1, respectively.
[0168] Comparative Example 3 and Comparative Example 4
[0169] Button cells were manufactured in the same manner as in Example 5, except that the composite positive active materials prepared in Comparative Examples 1 and 2 were used instead of the composite positive active material prepared in Example 1, respectively.
[0170] Evaluation Example 1: XPS Spectrum Evaluation
[0171] In the process of preparing the composite prepared in Example 1, the XPS spectrum was measured over time using Quantum 2000 (Physical Electronics). Before heating, the XPS spectra of the C1s orbital and the Al 2p orbital of the sample were measured after 1 minute, 5 minutes, 30 minutes, 1 hour and 4 hours, respectively. At the time of initial heating, only the peak of the Al 2p orbital appeared, and the peak of the C1s orbital did not appear. After 30 minutes, the peak of the C 1s orbital appeared clearly, and the size of the peak of the Al 2p orbital was significantly reduced.
[0172] After 30 minutes, at around 284.5 eV, a peak of a CC bond due to graphene growth and a peak of a C1s orbital due to a C═C bond clearly appear.
[0173] As the reaction time elapses, the oxidation number of aluminum decreases, shifting the peak position of the Al 2p orbital toward lower binding energy (eV).
[0174] Therefore, it is found that as the reaction proceeds, graphene 2 O 3 particles grow and generate Al 2 O 3 The reduction product of Al 2 O x (0 <x<3)。
[0175] The average contents of carbon and aluminum in 10 regions of the composite sample prepared in Preparation Example 1 were measured by XPS analysis results. For the measurement results, the deviation of the aluminum content in each region was calculated. The deviation of the aluminum content was expressed as a percentage of the average value, and the percentage was called uniformity. The percentage of the average value of the aluminum content deviation (i.e., the uniformity of the aluminum content) was 1%. Therefore, it was found that aluminum oxide was uniformly distributed in the composite prepared in Preparation Example 1.
[0176] Evaluation Example 2: SEM, HR-TEM, and SEM-EDAX Analysis
[0177] Scanning electron microscope (SEM) analysis, high-resolution transmission electron microscope (HR-TEM) analysis and SEM-EDAX analysis were performed on the composite prepared in Preparation Example 1, the composite positive electrode active material prepared in Example 3 and the bare NCA91 of Comparative Example 1. For SEM-EDAX analysis, FEI Titan 80-300 of Philips was used.
[0178] The composite prepared in Preparation Example 1 shows Al 2 O 3 Particles and Al as their reduction product 2 O zThe structure in which (0 < z < 3) particles are embedded in graphene. It is found that the graphene layer is disposed on the outside of one or more particles selected from Al 2 O 3 particles and Al 2 O z (0 < z < 3) particles. One or more particles selected from Al 2 O 3 particles and Al 2 O z (0 < z < 3) particles are uniformly distributed. At least one of Al 2 O 3 particles and Al 2 O z (0 < z < 3) particles has a particle size of about 15 nm. The particle size of the composite prepared in Preparation Example 1 is about 100 nm to about 200 nm.
[0179] It is found that in the composite positive electrode active material prepared in Example 3, a shell formed of a composite including graphene is disposed on the NCA91 core.
[0180] SEM-EDAX analysis was performed on the bare NCA91 of Comparative Example 1 and the composite positive electrode active material prepared in Example 3.
[0181] It is found that the concentration of aluminum (Al) distributed on the surface of the composite positive electrode active material of Example 3 is increased compared to the surface of the bare NCA91 positive electrode active material of Comparative Example 1. Therefore, it was confirmed that in the composite positive electrode active material of Example 3, the composite prepared in Preparation Example 1 was uniformly applied on the NCA91 core to form a shell.
[0182] Evaluation Example 3: XPS spectrum evaluation (graphene-NCA91 chemical bond)
[0183] For the composite prepared in Preparation Example 1, NCA91 of Comparative Example 1, and the composite positive electrode active material prepared in Example 3, the XPS spectrum of the O1s orbital was measured using Quantum 2000 (Physical Electronics), and the results are shown in Figure 1 .
[0184] As shown in Figure 1 , for the composite positive electrode active material of Example 3, a peak due to the C-O-Ni bond was observed near 530.2 eV. This peak was determined to be a peak due to the bond formed between the NiO phase existing on the surface of NCA91 and the carbon of graphene. Therefore, it was found that the graphene contained in the shell formed on the core forms a covalent bond with Ni, which is a transition metal contained in the core.
[0185] Evaluation Example 4: Raman spectroscopy evaluation (graphene-NCA91 chemical bond)
[0186] The Raman spectra of the composite prepared in Preparation Example 1 and the composite positive electrode active material prepared in Example 3 were measured, and the results are shown in Figure 2 middle.
[0187] like Figure 2 As shown in FIG. , the composite prepared in Preparation Example 1 has a high conductivity at 1338.7 cm due to graphene. -1 The D band peak is shown at 1575.0 cm -1 The G band peak is shown at .
[0188] In contrast, in the composite positive electrode active material of Example 3, the D band peak shifts by about 12 cm due to the inclusion of graphene in the shell. -1 Up to 1351.3cm -1 , and the G band peak shifts by about 18 cm -1 Up to 1593.6cm -1 .
[0189] The shift of the D-band peak was determined to be due to the strain of graphene, which is bonded to the core by milling to form the shell.
[0190] The shift of the G band peak was determined to be due to the charge transfer between the core and graphene in the composite formed through the CO-Ni bond between the core and graphene.
[0191] Therefore, it was confirmed that graphene contained in the shell formed on the core formed a covalent bond with Ni which was a transition metal contained in the core.
[0192] Evaluation Example 5: Evaluation of charge and discharge characteristics at room temperature
[0193] Each lithium battery manufactured in Examples 5 to 8 and Comparative Examples 3 to 4 was charged at a constant current of 0.1C rate at 25°C until the voltage reached 4.4V (relative to Li), and then the current was cut off at a 0.05C rate while maintaining the voltage at 4.4V in a constant voltage mode. Subsequently, each lithium battery was discharged at a constant current of 0.1C rate until the voltage reached 2.8V (relative to Li) (forming a cycle).
[0194] Each lithium battery that had undergone a formation cycle was charged at a constant current of 0.2C rate at 25°C until the voltage reached 4.4 V (relative to Li), and then the current was cut off at a 0.05C rate while maintaining the voltage at 4.4 V in a constant voltage mode. Subsequently, each lithium battery was discharged at a constant current of 0.2C rate until the voltage reached 2.8 V (relative to Li) (1st cycle).
[0195] Each lithium battery that had undergone the first cycle was charged at a constant current of 1C rate at 25°C until the voltage reached 4.4V (relative to Li), and then the current was cut off at a 0.05C rate while the voltage was maintained at 4.4V in a constant voltage mode. Subsequently, each lithium battery was discharged at a constant current of 1C rate until the voltage reached 2.8V (relative to Li) (2nd cycle). This cycle was repeated under the same conditions (50 repetitions) until the 50th cycle.
[0196] In all charge / discharge cycles, a rest time of 10 minutes was provided after one charge / discharge cycle. Some results of the charge and discharge experiments at room temperature are shown in the following Table 1. The capacity retention ratio in the 50th cycle is defined by the following Equation 1.
[0197] <Equation 1>
[0198] Capacity retention rate [%] = [50th cycle discharge capacity / 1st cycle discharge capacity] × 100 Evaluation Example 6: Evaluation of charge and discharge characteristics at high temperature (45°C)
[0199] The charge and discharge characteristics were evaluated in the same manner as in Evaluation Example 5, except that the temperature at which charge and discharge were performed was changed to 45°C.
[0200] Some results of the charge and discharge experiments at high temperature are shown in Table 1 below.
[0201] [Table 1]
[0202]
[0203] As shown in Table 1, in the lithium batteries of Examples 6 to 8, compared with the lithium batteries of Comparative Examples 3 and 4, the room temperature life characteristics and the high temperature life characteristics are improved.
[0204] Evaluation Example 7: Stability test at high temperature of 60° C. (capacity retention rate)
[0205] In the first cycle, at room temperature (25°C), each lithium battery manufactured in Examples 5 to 8 and Comparative Examples 3 and Comparative Examples 4 was charged at a constant current of 0.5C until the voltage reached 4.25V, charged at a constant voltage while maintaining the voltage at 4.25V until the current reached 0.05C, and discharged at a constant current of 0.2C until the voltage reached 2.8V.
[0206] In the second cycle, each lithium battery was charged at a constant current of 0.5C rate until the voltage reached 4.25V, charged at a constant voltage while maintaining the voltage at 4.25V until the current reached 0.05C, and discharged at a constant current of 0.2C rate until the voltage reached 2.8V.
[0207] In the 3rd cycle, each lithium battery was charged at a constant current of 0.5 C rate until the voltage reached 4.25 V, charged at a constant voltage while maintaining the voltage at 4.25 V until the current reached 0.05 C, and discharged at a constant current of 0.2 C rate until the voltage reached 2.8 V. The discharge capacity in the 3rd cycle was regarded as the standard capacity.
[0208] In the 4th cycle, each lithium battery was charged to 4.25V at a constant current of 0.5C rate, and charged at a constant voltage while maintaining the voltage at 4.25V until the current reached 0.05C. Then, each charged lithium battery was stored in an oven at 60°C for 70 days, taken out of the oven, and discharged to 2.8V at a constant current of 0.1C rate. Some charging and discharging results are shown in Table 2 below. The capacity retention rate after high temperature storage is defined by Equation 3 below.
[0209] <Equation 3>
[0210] Capacity retention rate after high temperature storage [%] = [discharge capacity after four cycles of high temperature storage / standard capacity] × 100
[0211] (Standard capacity is the discharge capacity in the 3rd cycle)
[0212] [Table 2]
[0213]
[0214] As shown in Table 2, in the lithium batteries of Examples 5 to 7, compared with the lithium battery of Comparative Example 3, the high temperature stability was significantly increased.
[0215] Evaluation Example 8: Stability test at high temperature of 60° C. (metal elution)
[0216] In the first cycle, at room temperature (25°C), each lithium battery manufactured in Examples 5 to 8 and Comparative Examples 3 and Comparative Examples 4 was charged at a constant current of 0.5C until the voltage reached 4.25V, charged at a constant voltage while maintaining the voltage at 4.25V until the current reached 0.05C, and discharged at a constant current of 0.5C until the voltage reached 2.8V.
[0217] In the second cycle, each lithium battery was charged at a constant current of 0.5C rate until the voltage reached 4.25V, charged at a constant voltage while maintaining the voltage at 4.25V until the current reached 0.05C, and discharged at a constant current of 0.2C rate until the voltage reached 2.8V.
[0218] In the 3rd cycle, each lithium battery was charged at a constant current of 0.5C rate until the voltage reached 4.25V, charged at a constant voltage while maintaining the voltage at 4.25V until the current reached 0.05C, and discharged at a constant current of 0.2C rate until the voltage reached 2.8V.
[0219] In the 4th cycle, each lithium battery was charged to 4.25V at a constant current of 0.5C rate, and charged at a constant voltage while maintaining the voltage at 4.25V until the current reached 0.05C. Then, each charged lithium battery was disassembled to separate the positive electrode, and then the positive electrode was immersed in the electrolyte used to manufacture the lithium battery and stored in an oven at 60°C for 30 days. Then, the content of the metal ions eluted in the electrolyte was measured, and the results are shown in Table 3 below.
[0220] [Table 3]
[0221]
[0222] As shown in Table 3, in the composite positive active material of Example 7, compared with the positive active material of Comparative Example 3, the elution of metal ions after high-temperature storage was reduced.
[0223] Evaluation Example 9: Evaluation of gas generation at a high temperature of 80°C
[0224] In the first cycle, at room temperature (25°C), each lithium battery manufactured in Examples 5 to 8 and Comparative Examples 3 and Comparative Examples 4 was charged at a constant current of 0.5C until the voltage reached 4.3V, charged at a constant voltage while maintaining the voltage at 4.3V until the current reached 0.05C, and discharged at a constant current of 0.5C until the voltage reached 2.8V.
[0225] In the second cycle, each lithium battery was charged at a constant current of 0.5C rate until the voltage reached 4.3V, charged at a constant voltage while maintaining the voltage at 4.3V until the current reached 0.05C, and discharged at a constant current of 0.2C rate until the voltage reached 2.8V.
[0226] In the 3rd cycle, each lithium battery was charged at a constant current of 0.5C rate until the voltage reached 4.3V, charged at a constant voltage while maintaining the voltage at 4.3V until the current reached 0.05C, and discharged at a constant current of 0.2C rate until the voltage reached 2.8V.
[0227] In the 4th cycle, each lithium battery was charged to 4.3V at a constant current of 0.5C rate, and charged at a constant voltage while keeping the voltage at 4.3V until the current reached 0.05C. Then, each charged lithium battery was stored in an oven at 60°C for 14 days, taken out of the oven and placed in a jig to burst it, and then the amount of gas generated was measured by converting the change in internal gas pressure into volume. The gas generation amount is expressed as the amount of gas generated per unit weight of the positive electrode active material contained in the lithium battery.
[0228] The evaluation results are shown in Table 4 below.
[0229] [Table 4]
[0230]
[0231] As shown in Table 4, in the lithium battery of Example 7, compared with the lithium battery of Comparative Example 3, the amount of gas generation was reduced.
[0232] According to an aspect, since the composite positive active material includes a shell including a first metal oxide and a carbonaceous material, cycle characteristics and high temperature stability of a lithium battery are improved.
[0233] It should be understood that the embodiments described herein should be considered in a descriptive sense only and not for the purpose of limitation. The description of features or aspects within each embodiment should generally be considered applicable to other similar features or aspects in other embodiments. Although one or more embodiments have been described with reference to the accompanying drawings, it will be understood by those of ordinary skill in the art that various changes in form and detail may be made therein without departing from the spirit and scope of the disclosure defined by the appended claims.
Claims
1. A composite positive electrode active material, comprising: a core comprising a lithium transition metal oxide; as well as a shell disposed on and conforming to the surface of the core, Wherein, the shell comprises at least one second metal oxide represented by M a O c , at least one first metal oxide represented by the formula M a O b , and a carbonaceous material, wherein 0 < a ≤ 3, 0 < b < 4, 0 < c ≤ 4, when a is 1, 2 or 3, b is not an integer, and c is an integer The first metal oxide and the second metal oxide are disposed in the carbonaceous material matrix, M is at least one selected from Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb and Se, The first metal oxide is a reduction product of the second metal oxide, and The lithium transition metal oxide contains nickel, and the content of nickel is 80 mol % or more based on the total moles of the transition metal.
2. The composite positive electrode active material according to claim 1, wherein The first metal oxide is at least one selected from the following substances: Al2O z , where 0 < z < 3; N b O x , where 0 < x < 2.5; MgO x , where 0 < x < 1; Sc2O z , where 0 < z < 3; TiO y , where 0 < y < 2; ZrO y , where 0 < y < 2; V2O z , where 0 < z < 3; WO y , where 0 < y < 2; MnO y , where 0 < y < 2; Fe2O z , where 0 < z < 3; Co3O w , where 0 < w < 4; PdO x , where 0 < x < 1; CuO x , where 0 < x < 1; AgO x , where 0 < x < 1; ZnO x , where 0 < x < 1; Sb2O z , where 0 < z < 3; and SeO y , where 0 < y < 2.
3. The composite positive electrode active material according to claim 1, wherein The second metal oxide is selected from Al2O3, NbO, NbO2, Nb2O5, MgO, Sc2O3, TiO2, ZrO2, V2O3, WO2, MnO2, Fe2O3, Co3O4, PdO, CuO, AgO, ZnO, Sb2O3 and SeO2.
4. The composite positive electrode active material according to claim 1, wherein The carbonaceous material included in the shell is chemically bonded to the transition metal of the lithium transition metal oxide included in the core through a chemical bond, The carbon atoms of the carbonaceous material in the shell are chemically bonded to the transition metal of the lithium transition metal oxide through CO-Me bonding using oxygen atoms as intermediates, or The first metal oxide is chemically bonded to the carbonaceous material through a chemical bond.
5. The composite positive electrode active material according to claim 1, wherein The shell has a thickness of 1 nm to 5 μm.
6. The composite positive electrode active material according to claim 1, further comprising: A third metal is doped on the core; or a third metal oxide is applied on the core, wherein the shell is disposed on a third metal oxide, and The third metal oxide is an oxide of at least one selected from Al, Zr, W, and Co.
7. The composite positive electrode active material according to claim 1, wherein The shell includes a composite including a second metal oxide, a first metal oxide, and a carbonaceous material.
8. The composite positive electrode active material according to claim 7, wherein: The content of the composite is 3 wt % or less based on the total weight of the composite positive active material.
9. The composite positive electrode active material according to claim 7, wherein: At least one selected from the first metal oxide and the second metal oxide has an average particle size of 1 nm to 1 μm, and At least one selected from the first metal oxide and the second metal oxide has a uniformity deviation of 3% or less.
10. The composite positive electrode active material according to claim 7, wherein The carbonaceous material has a branched structure, the first metal oxide is distributed in the branched structure, and The branched structure includes a plurality of carbonaceous material particles in contact with each other.
11. The composite positive electrode active material according to claim 7, wherein: The carbonaceous material has at least one structure selected from a spherical structure, a spiral structure in which spherical structures are connected to each other, and a cluster structure in which spherical structures are aggregated to each other, the first metal oxide is distributed in the spherical structure, the spherical structure has a size of 50nm to 300nm, the spiral structure has a size of 500nm to 100μm, and the cluster structure has a size of 0.5mm to 10cm, The composite is a wrinkled multifaceted spherical structure or a planar structure, at least one selected from the first metal oxide and the second metal oxide is distributed inside the structure or on the surface of the structure, and The carbonaceous material extends a distance of 10 nm or less from the first metal oxide, includes at least 1 to 20 carbonaceous material layers, and has a total thickness of 0.6 nm to 12 nm.
12. The composite positive electrode active material according to claim 1, wherein The lithium transition metal oxide is represented by one of Formula 1 to Formula 3: <Formula 1> Li a Ni x Co y M z O 2-b A b In formula 1, 1.0 ≤ a ≤ 1.2, 0 ≤ b ≤ 0.2, 0.8 ≤ x ≤ 1, 0 ≤ y ≤ 0.3, 0 < z ≤ 0.3, and x + y + z = 1, M is at least one selected from manganese, niobium, vanadium, magnesium, gallium, silicon, tungsten, molybdenum, iron, chromium, copper, zinc, titanium, aluminum, and boron, and A is F, S, Cl, Br, or a combination thereof; <Formula 2> LiNi x Co y Mr z O2 <Formula 3> LiNi x Co y Al z O2 In Formula 2 and Formula 3, 0.8 ≤ x ≤ 0.95, 0 < y ≤ 0.2, 0 < z ≤ 0.2, and x + y + z = 1.
13. A positive electrode, the positive electrode comprising the composite positive electrode active material according to any one of claims 1 to 12.
14. A lithium battery, the lithium battery comprising the positive electrode according to claim 13.
15. A method for preparing a composite positive electrode active material, the method comprising: providing a lithium transition metal oxide; A composite is provided, comprising the steps of: supplying a reaction gas including a carbon source gas to at least one a O c A second metal oxide is formed and a heat treatment is performed; and mechanically grinding the lithium transition metal oxide and the composite; wherein the composite includes the at least one second metal oxide represented by formula M a O c , at least one first metal oxide represented by formula M a O b , and a carbonaceous material, wherein 0 < a ≤ 3, 0 < b ≤ 4, 0 < c ≤ 4, when a is 1, 2, or 3, b is not an integer, and c is an integer placing a first metal oxide and a second metal oxide in a carbonaceous material matrix, M is at least one selected from Al, Nb, Mg, Sc, Ti, Zr, V, W, Mn, Fe, Co, Pd, Cu, Ag, Zn, Sb, and Se, the first metal oxide is a reduction product of the second metal oxide, and the lithium transition metal oxide contains nickel, and based on the total molar amount of the transition metals, the content of nickel is 80 mol% or more.
16. The method according to claim 15, wherein: The composite has an average particle size of 1 μm to 20 μm, and based on the total weight of the lithium transition metal oxide and the composite, the content of the composite is 3 wt% or less.
Citation Information
Patent Citations
Covering materials for wound capable of pH detection, and method for manufacturing the same
KR1020200066016A
Lithium secondary battery having improved safety and stability
CN104106161A
Protective coatings for conversion material cathodes
CN104241614A
Lithium metal oxide composites, and methods for preparing and using thereof
CN107004918A
Composite cathode active material, lithium battery including the same, and preparation method thereof