A method for forming a reducer

By adjusting the mold design and using medium frequency heating technology during the reducer forming process, the problem of inner wall thinning of the reducer is solved, accurate forming and efficient welding assembly of the reducer are achieved, and work efficiency is improved.

CN113814677BActive Publication Date: 2024-10-11WUXI HUAGUANG BOILER
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111343280.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-13
Publication Date
2024-10-11
Estimated Expiration
2041-11-13

AI Technical Summary

Technical Problem

The inner wall of the existing reducer is easily thinned during the molding process and cannot meet the size requirements, resulting in difficulty in welding and assembly and the need for rework, which reduces work efficiency.

Method used

By increasing the slope angle of the cone section of the mold and shortening the axial length of the cone section, combined with medium frequency heating and spinning technology, we ensure that the diameter of the small diameter part of the reducer remains unchanged and increase its axial length, using hot mold steel materials , ensuring that the reducer meets the size requirements during one-time molding.

Benefits of technology

It effectively avoids the thinning of the inner wall of the reducer, simplifies the welding assembly process, improves the forming efficiency, and ensures the dimensional accuracy of the reducer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113814677B_ABST
    Figure CN113814677B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of boiler pipes, and in particular to a method for forming a reducer, which can effectively ensure that the reducer meets size requirements, does not affect welding and assembly, and improves forming efficiency. The method comprises the following steps: (1) after a header is hoisted, one end is clamped and fixed by a four-claw chuck with a rotating spindle; (2) a medium frequency heating furnace is started, and the other end of the header, i.e., the reducer forming end, is sent into the medium frequency heating furnace for heating; (3) after heating to a set temperature, the header is withdrawn from the medium frequency heating furnace, and the reducer forming end is brought close to a side of a mold, wherein the mold comprises a small straight section, a conical section, and a large straight section; (4) the rotating spindle drives the header to rotate, and the reducer forming end of the header is pressed against the mold to start spinning, the inclined angle of the conical section of the mold increases, and the axial length of the conical section is shortened. After spinning is completed, the header leaves the mold, the rotating spindle stops rotating, and the four-claw chuck is released to remove the formed header, thereby completing the forming of the reducer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of boiler pipes, in particular to a method for forming a reducer pipe. Background Art

[0002] In the downcomer holes on the water-cooled wall of the boiler drum, the water inlet holes and other holes where temperature differences may occur, reasonable hole structures and water distribution methods should be adopted to reduce the temperature difference and thermal stress of the drum wall and prevent thermal fatigue cracks near the holes. In sub-high pressure and medium-high pressure boilers, some pressure gauge sockets use reducers in the pressure gauges and vent sockets in order to adopt a reinforced structure. Due to the different pipe diameters of the two connected headers, one end of the large-diameter open header is made into a reducer for easy welding. Reducers are widely used in boiler pipe components and come in a variety of sizes. During the production process, the closing size of the reducer cannot be guaranteed due to the fixed mode of the forming mold, and the inner wall will be thinned, resulting in defective products, such as Figure 1 As shown, during the welding process with the boiler pipe, assembly is difficult and rework is required later, which greatly reduces work efficiency. Summary of the invention

[0003] In order to solve the problem that the thinning of the inner wall of the closing end of the existing reducer cannot meet the size requirements, affects welding assembly, and reduces efficiency during later repair, the present invention provides a reducer forming method, which can effectively ensure that the reducer meets the size requirements, does not affect welding assembly, and improves forming efficiency.

[0004] The technical solution is as follows: a method for forming a reducer, which comprises the following steps:

[0005] (1) After the header is hoisted, one end is clamped and fixed by a four-jaw chuck with a rotating spindle;

[0006] (2) Start the medium frequency heating furnace and send the other end of the header, i.e. the reducing forming end, into the medium frequency heating furnace for heating;

[0007] (3) After heating to the set temperature, the header is withdrawn from the medium frequency heating furnace, and the different diameter forming end is brought close to the side of the mold. The mold includes a small diameter straight section, a conical section, and a large diameter straight section; (4) The rotating spindle drives the header to rotate, and the different-diameter forming end of the header presses against the mold to start spinning. After the spinning is completed, the header leaves the mold, the rotating spindle stops rotating, and the four-jaw chuck is released to remove the formed header, completing the forming of the different-diameter pipe;

[0008] The invention is characterized in that the slope angle of the conical section of the mold is increased, the axial length of the conical section is shortened, the diameter size of the small diameter part of the different diameter section on the header remains unchanged, and the axial length of the small diameter part is increased.

[0009] It is further characterized in that the mold is made of hot-type mold steel, the material of which is 3Cr2W8V;

[0010] Both ends of the mold are fixed by fixed blocks with connecting rods.

[0011] After adopting the present invention, under the condition that the total length of the reducer is ensured to remain unchanged, the bevel angle of the tapered section is increased, and the connection point between the tapered section and the small straight section is offset toward the large straight section, thereby increasing the axial length of the small straight section. Without thinning of the inner wall, the small straight section can be conveniently welded and assembled, ensuring that the size requirements of the reducer can be met by one-time molding, thereby improving the molding efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 It is the reducer structure of the original header;

[0013] Figure 2 The reducer structure of the present invention;

[0014] Figure 3 This is a schematic diagram of the mold structure used in the present invention. DETAILED DESCRIPTION

[0015] See Figure 2 , Figure 3 As shown, a method for forming a reducer comprises the following steps:

[0016] (1) After the header 1 is hoisted, one end is clamped and fixed by a four-jaw chuck with a rotating spindle;

[0017] (2) Start the medium frequency heating furnace and send the other end of the header, i.e. the reducing forming end, into the medium frequency heating furnace for heating;

[0018] (3) After being heated to the set temperature, the header 1 is withdrawn from the medium frequency heating furnace, and the different diameter forming end is brought close to the mold 2, which includes a small diameter straight section, a conical surface section, and a large diameter straight section;

[0019] (4) The rotating spindle drives the header 1 to rotate, and the different-diameter formed end of the header 1 presses against the mold 2 to start spinning. After the spinning is completed, the mold 2 withdraws, the rotating spindle stops rotating, and the four-jaw chuck is released to remove the formed header 1, completing the forming of the different-diameter pipe;

[0020] The bevel angle of the conical section of the mold 2 is increased, generally by 2-6°, so that the inclination angle reaches 14-18°, the axial length of the conical section is shortened, the diameter of the small diameter section of the reducing section on the header 1 remains unchanged, the axial length b' of the small diameter section increases, and the axial length a' of the conical section decreases, a' is less than Figure 1 The a and b' of Zhongyuan reducer are greater than Figure 1The b of Zhongyuan reducer has a longer small diameter straight section, which can be smoothly operated during subsequent assembly and welding. If it is too short, the welding operation will be very inconvenient.

[0021] Mold 2 is made of hot-type mold steel, the material is 3Cr2W8V, which has high toughness and good thermal conductivity, good hot hardness, good wear resistance and corrosion resistance.

[0022] Both ends of the mold 2 are fixed by a fixing block 4 with a connecting rod 3, and the two ends are clamped to ensure that the mold 2 will not move during the spinning process.

Claims

1. A method for forming a reducer, comprising the following steps: (1) After the header is hoisted, one end is clamped and fixed by a four-jaw chuck with a rotating spindle; (2) Start the medium frequency heating furnace and send the other end of the header, i.e. the reducing forming end, into the medium frequency heating furnace for heating; (3) After heating to the set temperature, the header is withdrawn from the medium frequency heating furnace, and the reduced diameter forming end is brought close to the side of the mold. The mold includes a small diameter straight section, a conical section, and a large diameter straight section. (4) The rotary spindle drives the header to rotate, and the reduced diameter forming end of the header presses against the mold to start spinning. After the spinning is completed, the header leaves the mold, the rotary spindle stops rotating, and the four-jaw chuck is released to remove the formed header, completing the forming of the reduced diameter tube. The characteristic is that, under the condition of ensuring that the total length of the reducer remains unchanged, the slope angle of the conical section of the mold is increased to 14-18°, the axial length of the conical section is shortened, the diameter size of the small diameter part of the reducer section on the header remains unchanged, and the axial length of the small diameter part is increased.

2. A method for forming a reducer according to claim 1, characterized in that: The mold is made of hot-dip mold steel, the material is 3Cr2W8V.

3. A method for forming a reducer according to claim 1, characterized in that: Both ends of the mold are fixed by fixed blocks with connecting rods.