Anode electrode compositions for battery applications
By using carbon nanostructures as conductive additives in the anode of lithium-ion batteries, the problems of deterioration of anode performance and short cycle life are solved, and more efficient battery performance and lower conductive additive usage are achieved, which significantly improves the circulation of the battery Lifespan and low temperature performance.
Patent Information
- Application Number
- CN202080037049.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-03-22
- Filing Date
- 2020-02-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-02-21
AI Technical Summary
The performance of existing lithium-ion battery anode compositions deteriorates under charging conditions, resulting in safety hazards and short cycle life. Commonly used conductive additives such as carbon black require a higher loading capacity to achieve benign properties, affecting the energy density of the battery.
Carbon nanostructures (CNS) are used as conductive additives to form polymerized structures through branching, interleaving and crosslinking, reducing the use of conductive additives, while improving the conductivity and connectivity of the anode and enhancing the cycle life of the battery.
Even at low loading, CNS significantly improves the cycle life and low temperature performance of lithium-ion batteries, reduces the anode lithium plating phenomenon, improves the battery capacity retention rate, and is lower than that required for traditional carbon additives.
Smart Images

Figure CN113841270B_ABST
Abstract
Description
[0001] Related Applications
[0002] This application claims the benefit of U.S. Provisional Patent Application No. 62 / 822,101, filed on March 22, 2019, with attorney case number 2018613P, and entitled Anode Electrode Compositions for Battery Applications, under 35 USC 119(e), which is incorporated herein by reference in its entirety. Background Art
[0003] Lithium-ion batteries are a common source of electrical energy for numerous applications ranging from electronic devices to electric vehicles. Lithium-ion batteries typically include a negative (electro) electrode and a positive (electro) electrode, which are arranged to allow lithium ions and electrons to move in and out of the electrodes during charge and discharge. The electrolyte solution in contact with the electrodes provides a conductive medium in which the ions can move. To prevent direct reaction between the electrodes, an ion-permeable separator is used to physically and electrically isolate the electrodes. During operation, the electrodes are electrically contacted, allowing electrons to flow through the device to provide power, and lithium ions move from one electrode to the other through the electrolyte.
[0004] The positive electrode typically includes a conductive substrate that supports a mixture (e.g., applied as a paste) of at least one electroactive material and a binder. The electroactive material (e.g., lithium transition metal oxide) is capable of receiving and releasing lithium ions. A binder such as polyvinylidene fluoride (PVDF) is used to provide mechanical integrity and stability to the electrode. In some cases, the positive electrode also includes a conductive additive.
[0005] Most commercially available lithium-ion batteries have anodes containing graphite, a material capable of incorporating lithium through an intercalation mechanism. Typically, lithium is added to the graphite anode during the charging cycle and removed as the battery is used. Possible alternatives to graphite include materials such as lithium titanate, tin oxide, SiO x (where x is typically 1.04, 1.06, etc.) and silicon.
[0006] In addition to the active anode components (graphite, silicon, SiO x In addition to the active material, the anode composition may further include a binder component and a conductive additive such as powder different from the active material. One known carbon conductive additive (CCA) is carbon black (CB). Summary of the invention
[0007] Despite the progress, existing anode compositions can present a variety of problems. For example, metallic lithium (Li) plated on the graphite negative electrode accelerates performance degradation under critical charging conditions and poses a safety hazard to LIBs. It is believed that when Li + The insertion of ions into graphite becomes sluggish, resulting in the occurrence of Li plating at the anode when the anode polarization increases. The study seems to indicate that the lithium ion insertion process involves three sequential steps: solvated Li + Diffusion of ions in the electrolyte, interfacial charge transfer processes, and diffusion of Li in the solid electrode material. Slowdowns in any of these steps can lead to lithium plating at the anode. Factors believed to affect the lithium ion insertion process, leading to lithium plating at the anode, include, for example, low temperature charging, overcharging, high rate charging, uneven current and potential distribution, and long-term cycling.
[0008] Alloy anodes often exhibit relatively poor cycle life and coulombic efficiency. It is believed that these effects may be related to the formation of two-phase regions during lithiation and delithiation. If one phase undergoes a larger volume change than the other phase, the two-phase region may cause internal stress in the anode material. This internal stress may cause the anode material to disintegrate over time. The volume change may also lead to deterioration of the electrical contact between the active anode material, the conductive particles, and the binder. In turn, the deterioration of the electrical contact may lead to a capacity that decreases with the cycle life of the anode (i.e., the amount of lithium that can be introduced per unit mass of active anode material).
[0009] In various embodiments, the anode material is silicon or SiO x The capacity of SiO2 has been associated with high irreversible capacity loss and poor discharge and recharge cycles, which are related to structural changes and abnormally large volume expansion. Structural changes and large volume changes can destroy the structural integrity of the electrode, thereby reducing the cycling efficiency. x - and silicon-graphite anodes in particular can exhibit large dimensional changes upon cycling, leading to loss of contact between the active material and the CCA.
[0010] There remains a need for improved lithium ion batteries (LIBs). For example, it is desirable to design a battery having a negative electrode configured to address one or more of the deficiencies associated with existing anodes and anode compositions. For example, there is a need for conductive additives such as CCA that can control anode deterioration associated with, for example, Li plating. Also of interest are conductive additives that can improve the cycle life of the battery and contribute to overall anode performance, especially when provided at low loading levels.
[0011] Some CCA materials that have the potential to enhance performance and avoid battery failure include conductive carbon black (CB) (eg, having a grape-like morphology), and carbon nanotubes (CNTs).
[0012] Since CCAs and binders generally do not participate in the electrochemical reactions that generate electrical energy, these materials can negatively affect certain performance characteristics of the battery (e.g., capacity and energy density) because they actually reduce the amount of active material that can be contained in a given volume. However, to achieve a certain level of performance, relatively high amounts of CCAs such as CBs (e.g., at least 1 weight percent (wt%) of the graphite anode) may be required.
[0013] For anode compositions, CNT can be considered as attractive additive materials. However, some difficulties may be encountered when utilizing CNT. These include limited dispersibility and insufficient purity in some media. It is believed that at least some of these problems are caused by the strong van der Waals forces that occur between the individual carbon nanotubes, thereby causing them to agglomerate into bundles or strings. Such performance can result in properties that are lower than expected and / or inconsistent performance. In some cases, relative to the enhancement expected in the case of using the original carbon nanotubes, the technology that can be used for debundling the carbon nanotubes into individual, well-dispersed members can adversely affect the desired property enhancement.
[0014] It was found that the use of carbon nanostructures (CNS) to prepare lithium-ion (Li + ) The anode composition of the battery has a positive impact on the anode performance and solves at least some of the problems discussed above. As used herein, the term "carbon nanostructure" or "CNS" refers to a plurality of carbon nanotubes (CNTs) that can exist as a polymeric structure by interlacing, branching, crosslinking and / or sharing a common wall with each other, in many cases multi-walled (also referred to as multi-walled) carbon nanotubes (MWCNTs). Therefore, CNS can be considered to have CNTs such as MWCNTs as the basic monomer units of its polymeric structure. Typically, CNS is grown under CNS growth conditions on a substrate (e.g., a fiber material). In such a case, at least a portion of the CNTs in the CNS can be oriented substantially parallel to each other, which is very similar to the parallel CNT orientation seen in conventional carbon nanotube clumps.
[0015] It was found that the use of CNSs, even when used at very low levels (e.g., less than 1 wt%, and often not more than about 0.5 wt%, or even not more than 0.1 wt%), reduced or eliminated Li plating on the graphite anode during heavy charging and / or significantly improved the cycle life of the battery. In some cases, the use of CNSs can also improve low temperature cycling. For graphite anode compositions, the improvements observed with the use of even small amounts of CNSs are surprising, given that graphite itself has good electrical properties. Without wishing to be bound by a particular explanation, it is believed that the effect is at least partially due to the formation of fragments that maintain branching, thereby allowing better connectivity between them and producing enhanced electrical conductivity (conductivity) connections. It is also possible that CNSs enhance electrolyte retention around graphite, which is critical for low temperature performance and long-term cycling. For batteries containing silicon or SiO x
[0013] With anode compositions having a less conductive material than graphite, at least some of the benefits associated with the use of CNS may be due to improvements in conductivity, connectivity, and silicon expansion management.
[0016] It has also been found that conductive additives, such as those described herein, bring about anode properties (e.g., capacity retention with cycling) that are typically achieved at higher loadings when conventional additives such as carbon black (CB) are used. Electrode additives according to the principles described herein typically will not need to be used in higher amounts to achieve the same or substantially the same electrical properties relative to comparative electrode compositions (containing, for example, CB as a conductive additive); in many cases, the required levels of CNS-based additives will be lower than those required when using conventional carbon additives.
[0017] In other words, the use of compositions prepared from CNS starting materials will result in electrodes that exhibit at least the same, and often improved, electrical properties relative to comparable electrode compositions formulated with conventional carbon additives such as CB at the same level of loading.
[0018] When used as CCA, CNS can present several advantages over ordinary CNTs, which may be due to the unique structure of CNS. Moreover, in contrast to CNTs, CNS can be provided in a form (e.g., powder) that is easy and safe to handle on an industrial scale. In some cases, CNS form a stable dispersion in a desired solvent.
[0019] Therefore, in some of its aspects, the present invention relates to a composition prepared by using a carbon nanostructure. In one embodiment, the composition comprises an active anode material and at least one material selected from the following: a carbon nanostructure, a fragment of a carbon nanostructure and a fractured multi-walled carbon nanotube. The carbon nanostructure or the fragment of a carbon nanostructure comprises a plurality of multi-walled carbon nanotubes cross-linked into a polymeric structure by branching, interlacing, entanglement and / or sharing a common wall. The fractured multi-walled carbon nanotubes are derived from a carbon nanostructure and are branched and share a common wall with each other. The active anode material may include graphite, silicon, SiOx, a silicon-graphite composite or lithium titanate. In a variety of specific implementations, the composition is in the form of a paste, a slurry or a solid.
[0020] Other aspects of the invention relate to electrodes and / or batteries comprising carbon nanostructures, carbon fragments and / or disrupted carbon nanotubes, such as disrupted multi-walled carbon nanotubes.
[0021] In further aspects of the invention, carbon nanostructures are employed to prepare compositions, anode electrodes and / or batteries.
[0022] In some embodiments, conductive additives including one or more of CNS, CNS fragments, and / or disrupted CNTs (e.g., MWCNTs) impart desirable electrical properties even when the additive is introduced in relatively low amounts, such as less than 1 weight percent (wt%) and often not more than 0.5 wt% or even not more than 0.1 wt%. It is believed that this effect is at least partially due to the formation of fragments that maintain branching, thereby allowing better connectivity between them and resulting in enhanced conductive connections.
[0023] Practicing aspects of the present invention can reduce the amount of conductive additives necessary to achieve certain performance, thereby allowing the manufacture of electrodes containing higher amounts of active electrode materials in a given electrode volume. In some embodiments, the CNS used produces fragments (including partially fragmented CNS) and / or broken CNTs such as MWCNTs. These structures can bring improved connectivity between each other, thereby enhancing conductivity in the electrode.
[0024] The above and other features of the present invention will now be described in more detail with reference to the accompanying drawings, including various details of the construction and combination of the parts, and other advantages, and which are pointed out in the claims. It will be understood that the specific methods and devices embodying the present invention are given as examples rather than limitations of the present invention. The principles and features of the present invention can be embodied in countless embodiments without departing from the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In the accompanying drawings, reference numerals refer to the same parts in different figures. The drawings are not necessarily to scale; instead, emphasis is placed on illustrating the principles of the invention. In the drawings:
[0026] Figure 1A and 1B Figure 1 is a diagram illustrating the difference between Y-shaped MWCNTs and branched MWCNTs. Y-shaped MWCNTs are not in or derived from carbon nanostructures ( Figure 2A ); branched MWCNT ( Figure 2B ) in carbon nanostructures.
[0027] Figure 2A and 2B TEM images showing features that characterize multi-walled carbon nanotubes found in carbon nanostructures.
[0028] Figure 2C and 2D The SEM image shows the presence of multiple branches in the carbon nanostructure.
[0029] Figure 3A is an illustrative depiction of a carbon nanostructure sheet material after separation of the carbon nanostructure from a growth substrate;
[0030] Figure 3B is a SEM image of an illustrative carbon nanostructure obtained as a thin-sheet material;
[0031] Figure 4A A series of optical and SEM images of CNS granules;
[0032] Figure 4B A series of SEM images of graphite anodes prepared using CNS at various magnifications;
[0033] Figure 5 A series of graphs showing the voltage discharge profiles of the first 100 cycles of a unit cell prepared according to Example 1 using an anode having only graphite at 2C charge and C / 2 discharge rates;
[0034] Figure 6 The voltage discharge profile of a unit cell (Example 3) including a graphite anode prepared using CNS at 2C charge and C / 2 discharge rates for 100 cycles is shown;
[0035] Figure 7 The capacity retention rate of the cells prepared according to Examples 1-3 as they cycle and their extrapolation are shown. Actual data for the first 100 cycles of each type of cell are shown with solid circles ( Figure 5 the bottom part of the );
[0036] Figure 8Compared with the use of SiO x And the capacity retention of the unit cell containing the following as conductive additives: (A) 0.55 wt% CNS; and (B) 1.5 wt% MWCNT and 1% P-Li. DETAILED DESCRIPTION
[0037] The present invention will be described more fully hereinafter with reference to the accompanying drawings in which illustrative embodiments of the present invention are shown. However, the present invention can be embodied in many different forms and should not be construed as limited to the description set forth herein; on the contrary, these embodiments are provided so that this disclosure will be thorough and complete and will fully convey the scope of the invention to those skilled in the art.
[0038] In general, the present invention relates to compositions useful for making electrodes for batteries, methods for making the compositions, and uses of the compositions in electrodes (e.g., anodes) and batteries. In many of its aspects, the present invention relates to compositions suitable for lithium ion batteries. In one example, the battery of interest is a rechargeable LIB.
[0039] Examples of various types of lithium-ion batteries (based on the acronyms of the electroactive materials (often intercalation compounds) used to form the cathode) include: LCO (lithium cobalt oxide), LMO (lithium manganese oxide), NCM (lithium nickel cobalt manganese oxide), NCA (lithium nickel cobalt aluminum oxide), LCP (lithium cobalt phosphate), LFP (lithium iron phosphate), LFSF (lithium fluoroferric sulfate), LTS (lithium titanium sulfide), and others as known in the art or as developed in the future. Materials such as these are collectively referred to herein as "lithium transition metal compounds", such as "lithium transition metal oxides".
[0040] Some embodiments relate to a composition consisting of, consisting essentially of, or comprising a conductive additive. The composition can be combined with a typical active anode material with or without a binder to form a negative electrode composition in the form of, for example, a slurry or paste, which can be applied to a current collector to form an anode. In turn, the anode can be used to make a battery.
[0041] The composition is prepared using: carbon nanostructures (multiple CNS, single CNS), which is a term used herein to refer to multiple carbon nanotubes (CNTs) that are cross-linked into a polymeric structure by branching (e.g., in dendritic form), interlacing, entanglement, and / or sharing a common wall with each other. The operations performed to prepare the compositions, electrodes, and / or batteries described herein can produce CNS fragments and / or broken CNTs. Fragments of CNS are derived from CNS and, like larger CNSs, include multiple CNTs that are cross-linked into a polymeric structure by branching, interlacing, entanglement, and / or sharing a common wall. Broken CNTs are derived from CNSs that are branched and share a common wall with each other.
[0042] Highly entangled CNS is visible to the naked eye in size and can be considered to have carbon nanotubes (CNTs) as the basic monomer units of its polymeric structure. For many CNTs in the CNS structure, at least a portion of the CNT sidewall is shared with other CNTs. Although it is generally understood that each carbon nanotube in the CNS does not necessarily need to be branched, crosslinked or share a common wall with other CNTs, at least a portion of the CNTs in the carbon nanostructure can be interlaced with each other and / or with branched, crosslinked, or co-walled carbon nanotubes in the carbon nanostructure of the remainder.
[0043] As is known in the art, a carbon nanotube (a CNT or a plurality of CNTs) is a nanotube comprising at least one sheet of sp 2 Carbonaceous material of hybridized carbon atoms: they are bonded to each other to form a honeycomb lattice that forms a cylindrical or tubular structure. Carbon nanotubes can be single-walled carbon nanotubes (SWCNTs) or multi-walled carbon nanotubes (MWCNTs). SWCNTs can be considered sp similar to fullerenes. 2 Allotropes of hybridized carbon. The structure is a cylindrical tube comprising a six-membered carbon ring. On the other hand, similar MWCNTs have several tubes in the form of concentric cylinders. The number of these concentric walls can vary, for example, from 2 to 25 or more. Typically, MWNTs can have a diameter of 10 nm or more, compared to a typical SWNT of 0.7-2.0 nm.
[0044] In many CNS used in the present invention, the CNT is a MWCNT having, for example, at least 2 coaxial carbon nanotubes. The number of walls present, as determined, for example, by transmission electron microscopy (TEM) at a magnification sufficient to analyze the number of walls in a particular case, can range from about 2-30, for example: 4-30; 6-30; 8-30; 10-30; 12-30; 14-30; 16-30; 18-30; 20-30; 22-30; 24-30; 26-30; 28-30; or 2-28; 4-28; 6-28; 8-28 ; 10-28; 12-28; 14-28; 16-28; 18-28; 20-28; 22-28; 24-28; 26-28; or 2-26; 4-26; 6-26; 8-26; 10-26; 12-26; 14-26; 16-26; 18-26; 20-26; 22-26; 24-26; or 2-24; 4-24; 6-24; 8-24; 10-24; 12-24; 14-24 ; 16-24; 18-24; 20-24; 22-24; or 2-22; 4-22; 6-22; 8-22; 10-22; 12-22; 14-22; 16-22; 18-22; 20-22; or 2-20; 4-20; 6-20; 8-20; 10-20; 12-20; 14-20; 16-20; 18-20; or 2-18; 4-18; 6-18; 8-18; 10-18; 12 -18; 14-18; 16-18; or 2-16; 4-16; 6-16; 8-16; 10-16; 12-16; 14-16; or 2-14; 4-14; 6-14; 8-14; 10-14; 12-14; or 2-12; 4-12; 6-12; 8-12; 10-12; or 2-10; 4-10; 6-10; 8-10; or 2-8; 4-8; 6-8; or 2-6; 4-6; or 2-4.
[0045] Since CNS are polymeric, highly branched and cross-linked networks of CNTs, some of the chemical properties observed for individualized CNTs can also be realized on CNS. In addition, some of the attractive properties often associated with the use of CNTs are also displayed in materials incorporating CNS. These include, for example, electrical conductivity; attractive physical properties including: good tensile strength, thermal stability (sometimes comparable to that of diamond crystals or in-plane graphene sheets) and / or chemical stability, to name a few, when incorporated into composites such as thermoplastic or thermosetting compounds (compounds).
[0046] However, as used herein, the term "CNS" is not synonymous with individualized, unentangled structures such as "monomeric" fullerenes (the term "fullerene" refers broadly to allotropes of carbon in the form of hollow spheres, tubes such as carbon nanotubes, and other shapes). In fact, many embodiments of the present invention highlight differences and advantages observed or expected when using CNS as opposed to using its CNT building blocks. Without wishing to be bound by a specific explanation, it is believed that the combination of branching, crosslinking, and common walls between carbon nanotubes in CNS reduces or minimizes van der Waals forces, which are often problematic when individual carbon nanotubes are used in a similar manner.
[0047] In addition or alternatively, with respect to performance properties, CNTs that are part of or derived from a CNS may be characterized by a number of features, at least some of which may be relied upon to distinguish them from nanomaterials such as ordinary CNTs (i.e., CNTs that are not derived from a CNS and may be provided as individualized, pristine or fresh CNTs).
[0048] In many cases, CNTs present in or derived from the CNS have a typical diameter of 100 nanometers (nm) or less, such as in the range of about 5 to about 100 nm, such as in the range of about 10 to about 75, about 10 to about 50, about 10 to about 30, about 10 to about 20 nm.
[0049] In various embodiments, at least one of the CNTs has a length equal to or greater than 2 microns, as determined by SEM. For example, at least one of the CNTs has a length in the following ranges: 2-2.25 microns; 2-2.5 microns; 2-2.75 microns; 2-3.0 microns; 2-3.5 microns; 2-4.0 microns; or 2.25-2.5 microns; 2.25-2.75 microns; 2.25-3 microns; 2.25-3.5 microns; 2.25-4 microns; or 2.5-2.75 microns; 2.5-3 microns; 2.5-3.5 microns; 2.5-4 microns; or 3-3.5 microns; 3-4 microns; 3.5-4 microns or more. In some embodiments, more than one, e.g., a portion, e.g., at least about 0.1%, at least about 1%, at least about 10%, at least about 15%, at least about 20%, at least about 25%, at least about 30%, at least about 35%, at least about 40, at least about 45%, at least about 50%, or even more than half, of the CNTs may have a length greater than 2 microns, e.g., within the above ranges, as determined by SEM.
[0050] The morphology of CNTs present in CNS, in fragments of CNS, or in ruptured CNTs derived from CNS will generally be characterized by a high aspect ratio, wherein the length is typically greater than 100 times the diameter, and in some cases even higher. For example, in CNS (or CNS fragments), the aspect ratio of the length to the diameter of the CNTs may be in the range of about 200 to about 1000, such as 200-300; 200-400; 200-500; 200-600; 200-700; 200-800; 200-900; or 300-400; 300-500; 300-600; 300-700; 300-800; 300-900; 300-1000; or 400-500 0; 400-600; 400-700; 400-800; 400-900; 400-1000; or 500-600; 500-700; 500-800; 500-900; 500-1000; or 600-700; 600-800; 600-900; 600-1000; 700-800; 700-900; 700-1000; or 800-900; 800-1000; or 900-1000.
[0051] It has been found that in CNS, and in structures derived from CNS (e.g., in fragments of CNS or in broken CNTs), at least one feature of CNTs is a certain "branch density". As used herein, the term "branch" refers to a feature in which a single carbon nanotube branches into multiple (two or more), connected multi-walled carbon nanotubes. An embodiment has the following branch density: according to the branch density, along the 2 micron length of the carbon nanostructure, there are at least two branches, as determined by SEM. Three or more branches may also occur.
[0052] Further features (detected using, for example, TEM or SEM) can be used to characterize the type of branching found in CNS relative to structures not derived from CNS, such as Y-shaped CNTs. For example, while Y-shaped CNTs have catalyst particles at or near branching regions (points), such catalyst particles are not present at or near branching regions that occur in CNSs, fragments of CNSs, or broken CNTs.
[0053] Additionally or alternatively, the number of walls observed at a branching region (point) in a CNS, a fragment of a CNS, or a ruptured CNT varies from one side of the branch (e.g., before the branching point) to the other side of the region (e.g., after or past the branching point). Such a variation in the number of walls, also referred to herein as "asymmetry" in the number of walls, is not observed for normal Y-shaped CNTs (where the same number of walls is observed in both the region before the branching point and the region after the branching point).
[0054] Figure 1A and 1B A diagram illustrating these features is provided in . Figure 1A 1 is an exemplary Y-shaped CNT 11 that is not derived from a CNS. The Y-shaped CNT 11 includes a catalyst particle 13 at or near a branch point 15. Regions 17 and 19 are located before and after the branch point 15, respectively. In the case of a Y-shaped CNT such as Y-shaped CNT 11, both regions 17 and 19 are characterized by the same number of walls, i.e., two walls in this figure.
[0055] In contrast, in CNS ( Figure 1B ), CNT building blocks 111 branching at branch point 115 do not include catalyst particles at or near that point, as seen in catalyst-free regions 113. In addition, the number of walls present in region 117 located before, in front of (or on a first side of) branch point 115 is different from the number of walls in region 119 (located past, after, or on the other side of branch point 115). More specifically, the three-wall feature found in region 117 is not carried through to region 119 (which is located in the region 117). Figure 1B ), resulting in the asymmetry mentioned above.
[0056] exist Figure 2A and 2B TEM images and Figure 2C and 2D These features are highlighted in the SEM images of the .
[0057] In more detail, Figure 2A The TEM area 40 of the CNS branching shows the absence of any catalyst particles. Figure 2B In the TEM of FIG. 1 , the first channel 50 and the second channel 52 show the asymmetry in the number of walls that is characteristic of branched CNS, while arrows 54 indicate regions showing shared walls. Figure 2C and 2D Multiple branches are seen in SEM areas 60 and 62, respectively.
[0058] One, more than one, or all of these attributes may be encountered in the compositions (eg, dispersions, slurries, pastes, solid or dried compositions, etc.), electrodes, and / or batteries described herein.
[0059] In some embodiments, a CNS exists as part of a tangle and / or interconnected network of CNSs. Such an interconnected network may contain bridges between CNSs.
[0060] Suitable techniques for preparing CNS are described, for example, in U.S. Patent Application Publication No. 2014 / 0093728A1, published on April 3, 2014; U.S. Patent Nos. 8,784,937B2; 9,005,755B2; 9,107,292B2; and 9,447,259B2. The entire contents of these documents are incorporated herein by reference.
[0061] As described in these documents, CNS can be grown on a suitable substrate, for example, on a catalyst-treated fiber material. The product can be a fiber-containing CNS material. In some cases, the CNS is separated from the substrate to form a sheet.
[0062] As seen in US2014 / 0093728A1, the carbon nanostructure obtained as a thin sheet material (that is, discrete particles with limited scale) exists as a three-dimensional microstructure due to the entanglement and crosslinking of its highly oriented carbon nanotubes. This orientation morphology reflects the formation of carbon nanotubes under fast carbon nanotube growth conditions (for example, several micrometers / second, for example, about 2 micrometers / second-about 10 micrometers / second) on the growth substrate, thereby causing substantially vertical carbon nanotube growth from the growth substrate. Not subject to any theory or mechanism constraints, it is believed that the fast carbon nanotube growth rate on the growth substrate can at least partially contribute to the complex structural morphology of the carbon nanostructure. In addition, by adjusting the carbon nanostructure growth conditions, including, for example, by changing the concentration of the transition metal nanoparticle catalyst particles arranged on the growth substrate to cause carbon nanotube growth, the packing density of CNS can be regulated to some extent.
[0063] The flakes may be further processed, for example by cutting or fluffing (operations that may involve mechanical milling, grinding, blending, etc.), chemical processing, or any combination thereof.
[0064] In some embodiments, the CNS employed is a "coated", also referred to herein as "sizing", or "encapsulated" CNS. In a typical sizing process, a coating is applied to the CNTs that form the CNS. The sizing process may form a partial or complete coating that is non-covalently bound to the CNTs and may act as a binder in some cases. In addition, or alternatively, a sizing agent may be applied to the already formed CNS in a post-coating (or encapsulation) process. In the case of using a sizing agent with adhesive properties, the CNS may be formed into larger structures, such as granules or pellets. In other embodiments, the granules or pellets are formed independently of the sizing function.
[0065] The amount of coating can vary. For example, the coating layer can be in the range of about 0.1 wt % to about 10 wt % (e.g., in the range of about 0.1% to about 0.5%; about 0.5% to about 1%; about 1% to about 1.5%; about 1.5% to about 2%; about 2% to about 2.5%; about 2.5% to about 3%; about 3% to about 3.5%; about 3.5% to about 4%; about 4% to about 4.5%; about 4.5% to about 5%; about 5% to about 5.5%; about 5.5% to about 6%; about 6% to about 6.5%; about 6.5% to about 7%; about 7% to about 7.5%; about 7.5% to about 8%; about 8% to about 8.5%; about 8.5% to about 9%; about 9% to about 9.5%; or about 9.5% to about 10% by weight, relative to the total weight of the coated CNS material.
[0066] In many cases, controlling the amount of coating (or sizing agent) reduces or minimizes the undesirable effects on the properties of the CNS material itself. Low coating levels, for example, are more likely to maintain the electrical properties brought about by introducing CNS or CNS-derived materials (e.g., CNS fragments of broken CNTs) materials into the cathode composition.
[0067] Can select various types of coating layer.In many cases, also can utilize the sizing solution commonly used when coating carbon fiber or glass fiber to coat CNS.The specific example of coating material includes but is not limited to fluorinated polymer such as poly (vinyl difluoride) (PVDF), poly (vinyl difluoride-co-hexafluoropropylene) (PVDF-HFP), poly (tetrafluoroethylene) (PTFE), polyimide, and water-soluble binder such as polyoxy (ethylene), polyvinyl alcohol (PVA), cellulose, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone (PVP), and copolymers and mixtures thereof.In many implementations, the CNS used is polyurethane (PU), thermoplastic polyurethane (TPU) or is processed with polyethylene glycol (PEG).
[0068] In some cases, polymers such as epoxy resins, polyesters, vinyl esters, polyetherimides, polyetherketoneketones, polyphthalamides, polyetherketones, polyetheretherketones, polyimides, phenol-formaldehyde, bismaleimide, acrylonitrile-butadiene styrene (ABS), polycarbonates, polyethyleneimines, polyurethanes, polyvinyl chlorides, polystyrenes, polyolefins, polypropylenes, polyethylenes, polytetrafluoroethylenes, elastomers such as polyisoprene, polybutadiene, butyl rubbers, nitrile rubbers, ethylene-vinyl acetate polymers, silicone polymers, and fluorinated silicone polymers, combinations thereof, or other polymers or polymer blends may also be used. To enhance conductivity, conductive polymers such as polyanilines, polypyrroles, and polythiophenes may also be used.
[0069] Some implementations employ coating materials that can assist in stabilizing the dispersion of CNS in a solvent. In one example, the coating layer is selected to promote and / or stabilize the dispersion of CNS in a medium comprising, consisting essentially of, or consisting of: N-methylpyrrolidone (NMP), acetone, a suitable alcohol, water, or any combination thereof.
[0070] Many embodiments described herein use CNS materials having a CNT purity of 97% or higher. Typically, anionic, cationic, or metallic impurities are very low, for example, in the range of several parts per million (ppm). Often, the CNS used herein do not require further additives to counteract van der Waals forces.
[0071] The CNS may be provided in the form of loose particulate material (as, for example, CNS flakes, granules, pellets, etc.) or in a formulation that also includes a liquid medium, such as a dispersion, slurry, paste, or in other forms. In many implementations, the CNS employed does not contain any growth substrate.
[0072] In some embodiments, the CNS is provided in the form of a flake material after removal from a growth substrate on which the carbon nanostructures are initially formed. As used herein, the term "flake material" refers to discrete particles having a finite size. Figure 3A is an illustrative depiction of a CNS flake material after separating the CNS from the growth substrate. The flake structure 100 may have a first dimension 110 in the range of about 1 nm to about 35 μm thick, particularly about 1 nm to about 500 nm thick, including any value between and any portion thereof. The flake structure 100 may have a second dimension 120 in the range of about 1 micron to about 750 microns high, including any value between and any portion thereof. The flake structure 100 may have a third dimension 130 that may be in the range of about 1 micron to about 750 microns, including any value between and any portion thereof. Two or all of the dimensions 110, 120, and 130 may be the same or different.
[0073] For example, in some embodiments, the second dimension 120 and the third dimension 130 may independently be approximately 1 micron to approximately 10 microns, or approximately 10 microns to approximately 100 microns, or approximately 100 microns to approximately 250 microns, approximately 250 to approximately 500 microns, or approximately 500 microns to approximately 750 microns.
[0074] CNTs within a CNS may vary in length from about 10 nanometers (nm) to about 750 micrometers (μm) or more. Thus, a CNT may be 10 nm-100 nm, 10 nm-500 nm; 10 nm-750 nm; 10 nm-1 micrometer; 10 nm-1.25 micrometers; 10 nm-1.5 micrometers; 10 nm-1.75 micrometers; 10 nm-2 micrometers; or 100 nm-500 nm, 100 nm-750 nm; 100 nm-1 micrometer; 100-1.25 micrometers; 100-1.5 micrometers; 100-1.75 micrometers; 100-2 micrometers; 500 nm-750 nm; 500 nm-1 micrometer; 500 nm-1 micrometer; 500 nm- 1.25 microns; 500nm-1.5 microns; 500nm-1.75 microns; 500nm-2 microns; 750nm-1 micron; 750nm-1.25 microns; 750nm-1.5 microns; 750nm-1.75 microns; 750nm-2 microns; 1 micron-1.25 microns; 1.0 micron-1.5 microns; 1 micron-1.75 microns; 1 micron-2 microns; or 1.25 microns-1.5 microns; 1.25 microns-1.75 microns; 1 micron-2 microns; or 1.5-1.75 microns; 1.5-2 microns; or 1.75-2 microns.
[0075] In various embodiments, at least one of the CNTs has a length equal to or greater than 2 microns, as determined by SEM. For example, at least one of the CNTs will have a length in the following ranges: 2-2.25 microns; 2-2.5 microns; 2-2.75 microns; 2-3.0 microns; 2-3.5 microns; 2-4.0 microns; or 2.25-2.5 microns; 2.25-2.75 microns; 2.25-3 microns; 2.25-3.5 microns; 2.25-4 microns; or 2.5-2.75 microns; 2.5-3 microns; 2.5-3.5 microns; 2.5-4 microns; or 3-3.5 microns; 3-4 microns; 3.5-4 microns or more.
[0076] Figure 3B Shown in is a SEM image of an illustrative carbon nanostructure obtained as a thin-plate material. Figure 3BThe carbon nanostructure shown in exists as three-dimensional microstructure due to the entanglement and crosslinking of its highly oriented carbon nanotube.This orientation morphology reflects that on growth substrate, under fast carbon nanotube growth conditions (for example, several micrometers / seconds, for example about 2 micrometers / second-about 10 micrometers / seconds), carbon nanotubes are formed, thereby causes vertical carbon nanotube growth basically from growth substrate.Not subject to any theory or mechanism restriction, it is believed that on growth substrate, fast carbon nanotube growth rate can at least partially contribute to the complex structure morphology of carbon nanostructure.In addition, by regulating carbon nanostructure growth conditions, comprise for example by changing the concentration of the transition metal nanoparticle catalyst particle that is arranged on growth substrate to cause carbon nanotube growth, the packing density of carbon nanostructure can be regulated to a certain extent.
[0077] The lamella structure may include a reticulated network of carbon nanotubes in the form of a carbon nanotube polymer (i.e., a "carbon nanopolymer") having a molecular weight in the following range: about 15,000 g / mol to about 150,000 g / mol, including all values therebetween and in any portion thereof. In some cases, the upper limit of the molecular weight range may be even higher, including about 200,000 g / mol, about 500,000 g / mol, or about 1,000,000 g / mol. This higher molecular weight may be associated with a carbon nanostructure that is long in scale. The molecular weight may also be a function of the dominant carbon nanotube diameter and the number of carbon nanotube walls present in the carbon nanostructure. The crosslinking density of the carbon nanostructure may range from about 2 mol / cm 3 -About 80mol / cm 3 Typically, the cross-link density is a function of the carbon nanostructure growth density, carbon nanostructure growth conditions, etc. on the growth substrate surface. It should be noted that the typical CNS structure (which contains many, many CNTs maintained in an open network arrangement) has removed the van der Waals forces or reduced their influence. The structure can be more easily peeled off, which makes them separate or destroy them into many other steps of branched structures unique and different from ordinary CNT.
[0078] In the case of a network-like morphology, the carbon nanostructure may have a relatively low packing density. The produced carbon nanostructure may have a density in the range of about 0.003 g / cm 3 -About 0.015g / cm 3 Further consolidation and / or coating to produce carbon nanostructure sheet materials or similar morphologies can increase the packing density to about 0.1 g / cm 3 -About 0.15g / cm 3In some embodiments, the optional further modification of the carbon nanostructure can be carried out to further change the packing density and / or other properties of the carbon nanostructure. In some embodiments, the packing density of the carbon nanostructure can be further changed by forming a coating on the carbon nanotubes of the carbon nanostructure and / or infiltrating the inside of the carbon nanostructure with various materials. The inside of the carbon nanotube coating and / or infiltrating the carbon nanostructure can be further designed for the properties of the carbon nanostructure in various applications. In addition, forming a coating on the carbon nanotube can desirably promote the operation (processing) of the carbon nanostructure. Further compaction can increase the packing density to about 1 g / cm 3 The upper limit of the carbon nanostructure is increased by chemical modification to increase the bulk density to about 1.2 g / cm 3 upper limit.
[0079] In addition to the above-mentioned flakes, the CNS material can be provided as granules, pellets, or other forms of loose particulate materials having a typical particle size in the range of about 1 mm to about 1 cm, for example, about 0.5 mm to about 1 mm, about 1 mm to about 2 mm, about 2 mm to about 3 mm, about 3 mm to about 4 mm, about 4 mm to about 5 mm, about 5 mm to about 6 mm, about 6 mm to about 7 mm, about 7 mm to about 8 mm, about 8 mm to about 9 mm, or about 9 mm to about 10 mm.
[0080] The bulk density of the CNS material that can be used can be about 0.005 g / cm 3 - About 0.1g / cm 3 , for example, about 0.01 g / cm 3 -About 0.05g / cm 3 within the range.
[0081] Examples of commercially available CNS materials are those developed by Applied Nanostructured Solutions, LLC (ANS) (Massachusetts, United States).
[0082] As used herein, CNS can be identified and / or characterized by a variety of techniques. For example, electron microscopy, including techniques such as transmission electron microscopy (TEM) and scanning electron microscopy (SEM), can provide information about characteristics such as the frequency of the specific number of walls present, branching, the absence of catalyst particles, etc. See, e.g. Figures 2A-2D .
[0083] Raman spectroscopy can reveal bands associated with impurities. For example, the D-band (about 1350 cm -1 ) is associated with amorphous carbon; the G band (about 1580 cm-1 ) is associated with crystalline graphite or CNTs). The G′ band (about 2700 cm -1 ) appears at about 2 times the frequency of the D band. In some cases, it may be possible to distinguish CNS and CNT structures by thermogravimetric analysis (TGA).
[0084] In some embodiments, the CNS is used with additional CCAs such as CBs and / or individualized, pristine CNTs, ie, CNTs that are not generated or derived from the CNS, such as during processing.
[0085] In many cases, the CB particles employed have a particle size of no greater than about 200, 180, 160, 140, 120, 100, 80, 60, or 50 m 2 In some embodiments, the CB particles have a BET surface area in the range of about 200 to about 180 m 2 / g; about 200-about 160m 2 / g; 200-about 140m 2 / g; about 200-120m 2 / g; about 200-about 100m 2 / g, about 200-about 80m 2 / g; about 200-about 60m 2 / g; about 200-about 50m 2 / g; or about 180-about 160m 2 / g; about 180-about 140m 2 / g; about 180-about 120m 2 / g; about 180-100m 2 / g, 180-about 80m 2 / g; about 180-about 60m 2 / g; 180-about 50m 2 / g; or about 160-about 140m 2 / g; about 160-120m 2 / g; about 160-about 100m 2 / g, 160-about 80m 2 / g; about 160-about 60m 2 / g; 160-about 50m 2 / g; or about 140-about 120m 2 / g; or about 140-about 100m 2 / g, 140-about 80m 2 / g; about 140-about 60m 2 / g; 140-about 50m 2 / g; or about 120-about 100m 2 / g, 120-about 80m 2 / g; about 120-about 60m 2 / g; 120-about 50m 2 / g; or about 100-about 80m 2 / g; about 100-about 60m 2 / g; 100-about 50m 2 / g; or about 80-about 60m 2 / g; 80-about 50m 2 / g; or about 60-about 50m 2 All BET surface area values disclosed herein refer to "BET nitrogen surface area" and are determined by ASTM D6556-10 (which is incorporated herein by reference in its entirety).
[0086] Suitable CBs may have an oil absorption number (OAN) of at least 130 mL / 100 g, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, or 250 mL / 100 g. Exemplary CBs have an OAN in the following ranges: about 130 to about 150 mL / 100 g; about 130 to about 170 mL / 100 g; about 130 to about 190 mL / 100 g; about 130 to about 210 mL / 100 g; about 130 to about 230 mL / 100 g; 130 to about 250 mL / 100 g or more; or about 150 to about 170, about 150 to about 190; about 150 to about 210; about 150 to about 230 mL / 100 g; about 150 to about 250 mL / 100 g or more. 100g or more; or 170 to about 190mL / 100g; about 170 to about 210; about 170 to about 230mL / 100g; about 170 to about 250mL / 100g or more; or about 190 to about 210mL / 100g; about 190 to about 230mL / 100g; about 190 to about 250mL / 100g or more; or about 210 to about 230mL / 100g; about 210 to about 250mL / 100g or more; or about 230 to about 250mL / 100g or more. All OAN values listed herein are determined by the method described in ASTM D 2414-16.
[0087] Carbon black particles can also be characterized by their statistical thickness surface area (STSA), which is a property that can be measured by ASTM D 6556-10. For a given carbon black, it may also be meaningful in some cases to specify the ratio of its STSA to its BET surface area (STSA:BET ratio). For the present application, the STSA:BET ratio of the carbon black particles can be in the range of about 0.3 to about 1.
[0088] The crystal domains can be determined by L as determined by Raman spectroscopy. a Crystallite size characterization. a It is defined as 43.5×(G band area / D band area). Crystallite size can give an indication of the degree of graphitization, where the higher the L a The value is associated with a higher degree of graphitization. a The Raman measurements are based on Gruber et al., "Raman studies of heat-treated carbon blacks", Carbon Vol. 32 (7), pp. 1377-1382, 1994, which is incorporated herein by reference. The Raman spectrum of carbon includes a wavelength of about 1340 cm -1 and 1580cm -1 There are two main "resonance" bands at , which are denoted as "D" and "G" bands. It is generally believed that the D band is attributed to the disordered sp 2 carbon, and the G band is attributed to graphitic or "ordered" sp 2 Carbon. Using empirical methods, the ratio of the G / D bands and the L measured by X-ray diffraction (XRD) a are highly correlated, and regression analysis gives the following empirical relationship:
[0089] L a =43.5×(G band area / D band area),
[0090] Where L a is measured in angstroms. Therefore, the higher the L a The higher the value, the more ordered the crystalline structure.
[0091] In some embodiments, the carbon black has a value less than or equal to For example L a Crystallite size. L a The crystallite size may have or include, for example, one of the following ranges: or or or or or or or or or or or or or In certain embodiments, L a The crystallite size can be less than or equal to or less than or equal to or less than or equal to or less than or equal to
[0092] The crystal domain can be c Crystallite size characterization. c Crystallite size is measured by X-ray diffraction using a copper tube, a tube voltage of 45kV, and a tube current of 40mA using an X-ray diffraction instrument (PANalyticalX'Pert Pro, PANalytical BV). The sample of carbon black particles is loaded in a sample holder (accessory of the diffractometer) and measured at a speed of 0.14° / min within an angle (2θ) range of 10°-80°. Peak position and half-peak full width are calculated by the software of the diffractometer. For measurement angle calibration, lanthanum hexaboride (LaB6) is used as an X-ray standard. From the obtained measurement results, L is determined using the Scherrer equation c Crystallite size: where K is the shape factor constant (0.9); λ is Cu K α1 The wavelength of the characteristic X-ray line β is the peak width at half-peak, in radians; and θ is determined by taking half the measured angular peak position (2θ).
[0093] In some embodiments, the carbon black has a value less than or equal to For example L c Crystallite size. L c The crystallite size may have or include, for example, one of the following ranges: or or or or or or or or or or or or or or or or or or or In certain embodiments, L c The crystallite size can be less than or equal to or less than or equal to or less than or equal to or less than or equal to or less than or equal to
[0094] The carbon black particles may have a high degree of graphitization as indicated by a high % crystallinity, which is measured by Raman as the ratio of the G band area to the G and D band areas (I G / I G+D ). In certain embodiments, the carbon black particles have a % crystallinity (I) in the range of about 25% to about 45% as determined by Raman spectroscopy. G / I G+D ). % crystallinity (I G / I G+D ) may have or include, for example, one of the following ranges: 25%-43%, 25%-41%, 25%-37%, 25%-39%, 25%-35%, 25%-30%, 25%-28%; or 30%-45%, 30%-43%, 30%-39%, 30%-35%; or 35%-45%, 35%-41%, 35%-39%; or 37%-45%, 37%-43%, 37%-41%; or 39%-45%, 39%-43%; or 41%-45%, or 41%-43%.
[0095] Some CB specifications characterized by these and / or other properties known and recognized by those skilled in the art are shown in Table 1 as Specifications AF.
[0096] Table 1
[0097]
[0098] Suitable CB particles that can be utilized are commercially available particles. Examples include those available from Cabot Corporation. 50. 66. 200, 300, HP and 500 Carbon black pellets; C-NERGY from Imerys TM C45, C-NERGY TM C65 and products; Li-400, Li-250, Li-100 and Li-435 products from Denka; and EC300 products from Ketjen.
[0099] Other materials that can be used with CNS are exemplified by the specification LN (Table 2 below) describing an exemplary CNT:
[0100] Table 2
[0101]
[0102] The values presented in Table 2 were typically determined using the techniques described above for CB.
[0103] In many cases, the CNS material (in the form of, for example, flakes, pellets, granules) is provided in combination with a liquid medium or in the presence of a liquid medium. Typically, the liquid medium may be any liquid, such as a solvent, suitable for use with the constituents of the composition described herein and capable of being used to manufacture the intended electrode. The solvent may be anhydrous, polar and / or aprotic. In some embodiments, the solvent has high volatility so that during manufacture, it can be easily removed (e.g., evaporated), thereby reducing drying time and manufacturing costs. Suitable examples include, but are not limited to, N-methylpyrrolidone (NMP), acetone, a suitable alcohol, water, or any combination thereof.
[0104] In some cases, the composition further includes one or more dispersants (eg, cellulosic dispersants), and / or one or more additives, typically non-conductive additives, such as maleic anhydride polymers.
[0105] Dispersants generally include materials that are capable of facilitating the dispersion of CNS in a solvent (e.g., via steric hindrance mechanisms and / or electrostatic charge mechanisms) while maintaining the viscosity of the composition low enough to enable practical processing of the composition, such as for use in making electrodes for batteries. In some embodiments, for compositions including CNS, the dispersant, polymer, and solvent have a viscosity at 450 s as measured by a rheometer. -1 At a shear rate of 200 cP or less, for example, at 450 s -1 At least 30 cP at a shear rate of 450 s -1The viscosity of 50cP-140cP under the shear rate of 10000 ℃. In various embodiments, the composition can be referred to as a slurry or paste that can be easily applied or coated to a conductive substrate to form an electrode, which is in contrast to a mud that is too thick or too viscous to be effectively applied during manufacturing. In addition to its ability to disperse CNS materials, the dispersant is also preferably thermally stable, electrochemically inert, and / or rarely hinders the conductivity of the CNS material. Thermally stable or non-volatile dispersants allow solvents (e.g., N-methylpyrrolidone, water, etc.) to be removed and recycled without removing and / or decomposing the dispersant during electrode manufacturing. "Electrochemically inert" means that the dispersant is stable during normal use of the battery (e.g., not decomposed or oxidized at or below the operating voltage of the battery), because such decomposition can negatively affect the performance of the battery. In addition, since the dispersant coats at least a portion of the CNS flakes, granules, granules, etc. to disperse the particles, the dispersant will hinder or reduce the conductive contact surface available for the particles. Preferably, a dispersant is selected that has little interference with the conductivity of the CNS particles. Examples of suitable dispersants include poly(vinyl pyrrolidone), poly(vinyl pyrrolidone-co-vinyl acetate), poly(vinyl butyral), poly(vinyl alcohol), poly(ethylene oxide), poly(propylene oxide), poly(propylene carbonate), cellulosic dispersants such as methylcellulose, carboxymethylcellulose, ethylcellulose, hydroxymethylcellulose and hydroxypropylcellulose; poly(carboxylic acids) such as poly(acrylic acid), polyacrylates, poly(methyl acrylate), poly(acrylamide), amide waxes, styrene maleic anhydride resins, octylphenol ethoxylates and others known in the art. The composition may include a dispersant of one composition or a plurality of dispersants of different compositions.
[0106] The concentration of the dispersant in the composition may vary depending on the composition of the dispersant used and the specific types and concentrations of the CNS, polymer, and solvent. In some embodiments, the concentration of the dispersant is best expressed as a ratio of dispersant to CNS material by weight. The weight ratio may range from 3:100-50:100 and may have or include, for example, one of the following ranges: 3:100-40:100, or 3:100-30:100, or 3:100-20:100, or 3:100-10:100, or 10:100-50:100, or 10:100-40:100, or 10:100-30:100, or 10:100-20:100, or 20:100-50:100, or 20:100-40:100, or 20:100-30:100, or 30:100-50:100, or 30:100-40:100, or 40:100-50:100.
[0107] The CNS material can be combined with a liquid, optionally in the presence of a dispersant, by suitable mixing techniques, using, for example, conventional mixing equipment. In various embodiments, the constituent components are blended to form a composition, such as a solution or dispersion. The composition can be characterized, for example, in that the concentration of the CNS in the solvent is about 0.25 to about 5% by weight, such as about 0.25 to about 2.5 wt % or greater. In illustrative examples, the concentration in wt % is in the range of about 0.25 to about 0.5, about 0.5 to about 0.75, about 0.75 to about 1.0, about 1.0 to about 1.25, about 1.25 to about 1.50, about 1.50 to about 1.75, about 1.75 to about 2.0, about 2.0 to about 2.25, about 2.25 to about 2.5, about 2.5 to about 2.75, about 2.75 to about 3.0, about 3.0 to about 3.25, about 3.25 to about 3.5, about 3.5 to about 3.75, about 3.75 to about 4.0, about 4.0 to about 4.25, about 4.25 to about 4.5, about 4.5 to about 4.75, or about 4.75 to about 5. Other concentrations of CNS in the solvent may be used.
[0108] Unlike common solutions or dispersions using common, individualized CNTs (e.g., in raw form), CNS, particularly when provided as coated CNS in the form of granules or pellets, can produce stable dispersions. In some embodiments, stable dispersions can be achieved even using water as a solvent in the absence of a stabilizing surfactant. Other embodiments use a solvent in combination with water during wet processing. Examples of usable solvents include, but are not limited to, isopropyl alcohol (IPA), ethanol, methanol, and water.
[0109] In some cases, the technology used to prepare the dispersion produces CNS-derived species such as "CNS fragments" and / or "broken CNTs" that become distributed in individualized form throughout the dispersion (e.g., uniformly). In addition to their reduced size, CNS fragments (also including the term partially fragmented CNS) generally share the properties of intact CNS and can be confirmed by electron microscopy and other techniques, as described above. Broken CNTs can be formed when the crosslinks between CNTs within the CNS are broken, for example, under applied stress. Derived (produced or prepared) from CNS, the broken CNTs are branched and share common walls with each other.
[0110] Compositions consisting of or consisting essentially of CNS materials or compositions prepared from CNS, such as dispersions (such as described above), are combined with other ingredients. They can be used, for example, to make a variety of energy storage devices such as lithium-ion batteries. As an example, the composition is used to make an electrode (e.g., anode) composition for a lithium-ion battery. For example, the composition can be combined with an electroactive material (component) for a specific type of anode.
[0111] In many embodiments, the active anode material is graphite, for example, natural graphite, artificial graphite, or a blend of the two. Commercially available types of graphite that can be used include mesophase carbon microbeads (MCMB), carbon fibers (MCF) based on mesophase pitch, vapor-grown carbon fibers (VGCF), large-scale artificial graphite (MAG), natural graphite, and others. In other embodiments, the active anode compound used comprises silicon, consists essentially of silicon, or consists of silicon. In one example, the active anode material is a silicon-graphite composite, a nano-silicon (Si) or SiO x Particles of graphite.
[0112] The principles described herein can also be applied to other active anode materials such as those known or currently explored, or those developed in the future. Examples include, but are not limited to: (a) intercalation / deintercalation materials (e.g., carbon-based materials, porous carbon, carbon nanotubes, graphene, TiO2, Li4Ti5O 12 (b) alloy / de-alloy materials (e.g., Si, SiO x , doped Si, Ge, Sn, Al, Bi, SnO2, etc.); and (c) conversion materials (e.g., transition metal oxides (Mn x O y 、NiO、Fe x O y , CuO, Cu2O, MoO2, etc.), by formula M x X y Metal sulfides, metal phosphides and metal nitrides represented by X=S, P, N)).
[0113] Active anode materials such as graphite, silicon, lithium titanate (Li4Ti5O 12 , also often referred to as "LTO"), SiO x , silicon-graphite composites, etc., may vary depending on the specific type of energy storage device. In an illustrative example, the active anode component is present in an amount of at least 80 wt %, such as at least 85, 90 or 95 wt %, relative to the total weight of the (dry) electrode composition, such as in an amount ranging from 80 wt % to 99 wt %, such as about 80 to about 85 wt %, about 85 to about 88 wt %, about 88 to about 90 wt %, about 90 to about 92 wt %, about 92 to about 95 wt %, about 95 to about 97 wt %, or about 97 to about 99 wt %, relative to the total weight of the electrode composition.
[0114] In some embodiments, the electrode composition contains one or more binders, which are used, for example, to enhance the mechanical properties of the formed electrode. Exemplary binder materials include, but are not limited to, fluorinated polymers such as poly (vinyl difluoride) (PVDF), poly (vinyl difluoride-co-hexafluoropropylene) (PVDF-HFP), poly (tetrafluoroethylene) (PTFE), polyimides, and water-soluble binders such as polyoxy (ethylene), polyvinyl alcohol (PVA), cellulose, carboxymethyl cellulose (CMC), styrene-butadiene rubber (SBR), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone (PVP), and copolymers and mixtures thereof. Other possible binders include polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, and fluororubber and copolymers and mixtures thereof. In illustrative examples, the active anode material is graphite and the binder is PVDF or CMC with SBR.
[0115] The binder can be present in the anode composition in an amount of about 1 to about 20 wt %, for example, about 1-2, 2-3, 3-4, 4-5, 5-6, 6-7, 7-8, 8-9, 9-10, 10-11, 11-12, 12-13, 13-14, 15-16, 16-17, 17-18, 18-19 or 19-20 wt %.
[0116] In some implementations, the CNS loading relative to the dry electrode composition (e.g., for use in a graphite negative electrode, for example, for LIB) is no greater than about 5 wt% and often no greater than about 2 wt%, such as less than 1.9, 1.8, 1.7, or 1.6 wt%. In other embodiments, the CNS loading relative to the dry electrode composition (e.g., for use in a graphite anode, for example, for LIB) is 1.5 wt% or less, such as at least 1.4, 1.3, 1.2, 1.2, 1.0, 0.95, 0.90, 0.85, 0.80, 0.75, 0.70, 0.65, 0.60, 0.55, 0.50, 0.45, 0.40, 0.35, 0.30, 0.25, 0.20, 0.15, or 0.10 wt%. In many implementations, the CNS loading relative to the dry electrode composition (e.g., used in a graphite anode for a lithium battery) is no greater than 0.5 wt%, for example, in the range of about 0.5 wt%-0.1 wt%, for example, in the range of about 0.1-about 0.2, about 02-about 0.3, about 0.3-about 0.4, or about 0.4-about 0.5 wt%. Other embodiments employ a loading in the range of about 2-about 5 wt%, for example, at least about 2.25, 2.5, 2.75, 3.0, 3.25, 3.5, 3.75, 4.0, 4.25, 4.5 or 4.75.
[0117] For many LIBs, the CNS loading is lower than that required when using other CCAs such as CB. In many cases, the CB particles used as CCA in the electrode and used to prepare the comparative samples have a particle size greater than 50 m 2 / g, and an oil absorption number (OAN) greater than 150 mL / 100 g. CB specifications characterized by these and other properties known and recognized by those skilled in the art are shown in Table 3 as Specifications I-IV. Another type of CCA that can be used in the anode composition is exemplified by Specification V (describing exemplary CNTs).
[0118] Table 3
[0119]
[0120] Suitable CB particles that can be used as CCA to prepare, for example, comparative samples can be commercially available particles. Examples include CCA available from Cabot Corporation. 50. 66. 200, 300 and HP carbon black pellets; C-NERGY from Imerys TM C45, C-NERGY TM C65 and products; Li-400, Li-250, Li-100 and Li-435 products from Denka; and EC300 products from Ketjen.
[0121] The electrode composition can be prepared by combining (eg, by intimately mixing) the above-mentioned constituent components, which can be added in any order to obtain a mixture, and in particular a homogeneous mixture. Suitable mixing techniques include mechanical agitation, shaking, stirring, and the like.
[0122] In one example, an electrode (e.g., anode) composition is made by uniformly dispersing (e.g., by uniformly mixing) a composition consisting of, consisting essentially of, or comprising CNS or a composition prepared using a CNS starting material with an electroactive anode component such as graphite. In another example, a binder is uniformly dispersed with the composition containing CNS and with graphite or another suitable active anode component.
[0123] When provided in some form, for example, as loose particulate material such as granules, pellets, or flakes, the CNS can be introduced directly into a substrate containing an active electrode material (e.g., graphite, silicon, SiO x etc.) in the slurry.
[0124] In other embodiments, loose CNS particles of pellets, granules, flakes or other forms are first dispersed in a liquid medium (e.g., PVDF), or an aqueous formulation of CMC and / or SBR, thereby producing CNS fragments (including partially fragmented CNS) and / or ruptured CNTs. The dispersion can be prepared from starting materials such as uncoated, PU or PEG coated CNS, or CNS with any other polymeric binder coating. In one implementation, an electroactive material such as graphite is added to a mixture of CNS pellets, pellets, flakes, etc. in the presence of a liquid binder such as an aqueous binder formulation of CMC and / or SBR, or an NMP-based formulation including PVDF.
[0125] Illustrative CNS fragment sizes present in the dispersion can be in the range of about 0.5 to about 20 μm, for example, in the following ranges: about 0.5 to about 1 μm; about 1 to about 5 μm; about 5 to about 10 μm; about 10 to about 15 μm; or about 15 to about 20 μm. In some cases, reducing the fragment size too much, for example to less than 0.5 μm, can impair electrical properties associated with utilizing CNS.
[0126] The resulting electrode composition may be in the form of a paste or slurry combining the anode electroactive material, the CNS-based conductive additive, the dispersant (one or more) (if present), the non-conductive additive (one or more) (if present), the solvent, and the binder (if present). In other embodiments, the electrode composition is a solid formed by removing the solvent from the paste or slurry. Adoptable drying techniques include air drying, heating (e.g., in a suitable oven), etc.
[0127] The battery electrode can be formed by applying an electrode composition such as the above-described anode composition (e.g., in the form of a paste) to a conductive substrate (e.g., an aluminum or copper current collector) followed by removal of the solvent. The paste can be applied by techniques such as doctor blade coating, reverse comma bar coating, or extrusion.
[0128] In some implementations, the paste has a solid loading (i.e., a high solids concentration) high enough to enable deposition onto a substrate while minimizing the formation of intrinsic defects (e.g., cracking) that can occur with less viscous pastes (e.g., with lower solid loadings). In addition, higher solid loadings reduce the amount of solvent required and its removal.
[0129] The solvent is removed by heating the paste at ambient temperature or under low heat conditions, for example, at a temperature in the range of 20° C. to 100° C. The deposited electrode / current collector may be cut to the desired dimensions, optionally followed by calendering.
[0130] An illustrative method of the preparation process may include some or all of the following steps: wetting and homogenizing the CNS; optionally pre-dispersing the wetted CNS; combining the wetted or pre-dispersed CNS with graphite and forming a dispersion; combining the CNS-graphite dispersion with a binder and preparing a final dispersion (in the form of, for example, a paste or slurry) containing the CNS, graphite and binder; casting the dispersion onto a current collector (foil) followed by drying.
[0131] In one specific example, the target was 14 mg / cm 2 Anodes containing 0.5 wt% CNS (including CNS derived components such as CNS fragments and / or broken CNTs), 95.5 wt% graphite, and 4% CMC / SBR (2:1) binder were coated with area loading. CNS was combined with an aqueous solution of carboxymethyl cellulose (CMC) and mixed (using, for example, a Thinky planetary mixer) for several (e.g., 12) minutes, followed by addition of graphite and further mixing (e.g., several (e.g., 12 minutes) using the Thinky mixer. SBR was then added, followed by further mixing in the Thinky mixer for several (e.g., 12 minutes). The composition was applied to a metal (e.g., Cu) foil and dried.
[0132] The process leading to the formation of the electrode can maintain some of the integrity of the initial CNS used, which will still be intact. However, some process operations and / or conditions can change at least some of the initial CNS used. As described above, one example involving such operations and / or conditions is the application of shear forces, such as encountered when preparing an emulsion from a CNS starting material.
[0133] In some cases, the initial CNS is disrupted into smaller CNS units or fragments. In addition to their reduced size, these fragments generally share the properties of the intact CNS and can be confirmed by electron microscopy and other techniques, as described above.
[0134] It is also possible that the initial nanostructure morphology of CNS changes. For example, the applied shear can destroy the crosslinking between the CNTs in the CNS to form CNTs that are typically dispersed in the electrode composition as separate CNTs. It is found that for many of these CNTs, even after crosslinking is removed, the structural features of branching and shared walls are also retained. CNTs derived (prepared) by CNS and retaining the structural features of CNT branching and shared walls are referred to as "broken ()" CNTs in this article. These species can impart improved interconnectivity (between CNT units), resulting in better conductivity at lower concentrations.
[0135] Thus, compared to electrodes or electrode compositions employing ordinary, individualized CNTs (e.g., in pristine form), the electrodes and electrode compositions described herein will often include broken CNTs. These broken CNTs can be easily distinguished from ordinary carbon nanotubes by standard carbon nanotube analysis techniques such as SEM. It is further noted that not every CNT encountered needs to be branched and share a common wall; rather, a plurality of broken CNTs as a whole will have these features.
[0136] The formed electrode can be introduced into a lithium ion battery according to methods known in the art, such as described in "Lithium Ion Batteries Fundamentals and Applications", Yuping Wu, CRC press, (2015). In some embodiments, the battery is a coin type, such as a 2032 coin cell, a 18650 cylindrical cell, a pouch cell, and others. In addition to an anode containing a CNS material (e.g., as described above), the battery also includes other components, such as a cathode, which is made of, for example, a cathode material based on an intercalation chemistry, such as a chemical reaction that typically involves the transfer of a single electron. Other types of cathode materials (inserting lithium ions into, for example, FeF3) can transfer multiple electrons through a more complex reaction mechanism known as a conversion reaction.
[0137] Examples of suitable cathode electroactive materials include, but are not limited to, LCO, LMO, NCM, NCA, LCP, LFP, LFSF, LTS, and others as known in the art or as developed in the future. In some embodiments, the anode composition containing CNS described above is used together with an NCM or NCA cathode composition. NCM (also referred to as "NMC") and NCA are well known to those skilled in the art of batteries.
[0138] In more detail, NCM can be represented by the formula Li 1+x (Ni y Co 1-y-z Mn z ) 1-x O2 represents, wherein x ranges from 0-1, y ranges from 0-1 (e.g., 0.3-0.8), and z ranges from 0-1 (e.g., 0.1-0.3). Examples of NCMs include Li 1+x (Ni 0.33 Co 0.33 Mn 0.33 ) 1-x O2、Li 1+x (Ni 0.4 Co 0.3 Mn 0.3 ) 1-x O2、Li1+x (Ni 0.4 Co 0.2 Mn 0.4 ) 1-x O2、Li 1+x (Ni 0.4 Co 0.1 Mn 0.5 ) 1-x O2、Li 1+x (Ni 0.5 Co 0.1 Mn 0.4 ) 1-x O2、Li 1+x (Ni 0.5 Co 0.3 Mn 0.2 ) 1-x O2、Li 1+x (Ni 0.5 Co 0.2 Mn 0.3 ) 1-x O2、Li 1+x (Ni 0.6 Co 0.2 Mn 0.2 ) 1-x O2, and Li 1+x (Ni 0.8 Co 0.1 Mn 0.1 ) 1-x O2.
[0139] NCA can be represented by the formula Li 1+x (Ni y Co 1-y-z Al z ) 1-x O2 represents, where x ranges from 0-1, y ranges from 0-1, and z ranges from 0-1. An example of NCA is Li 1+x (Ni 0.8 Co 0.15 Al 0.05 ) 1-x O2.
[0140] The concentration of NCM or NCA in the electrode composition may vary depending on the specific type of energy storage device. In some cases, NCM or NCA is present in the electrode composition in an amount of at least 90 wt %, such as greater than 95 wt %, such as in an amount ranging from 90 wt % to 99 wt % relative to the total weight of the electrode composition.
[0141] In addition to the cathode electroactive material, the cathode composition often includes a binder such as poly(vinyl difluoride) (PVDF). Other binders such as those described above may be employed to prepare the cathode composition.
[0142] In some embodiments, the cathode composition further contains a conductive additive such as CCA. Examples include CB, CNT, graphite, graphene, etc.
[0143] In one implementation, the cathode composition includes CNS, CNS fragments and / or broken CNTs. Such cathode compositions, their preparation and use are described in the following: U.S. Provisional Patent Application No. 62 / 822,097, entitled Cathode Electrode Compositions for Battery Applications, filed on March 22, 2019, and U.S. Non-Provisional Patent Application Cathode Electrode Compositions for Battery Applications, filed concurrently therewith, with agent case number No. 2018609, both of which are incorporated herein by reference in their entirety. In many cases, the CNS used to prepare the cathode composition is coated, such as PU or PEG coated. When dried, the illustrative cathode composition contains no more than about 1wt% of carbon nanostructures, fragments of carbon nanostructures and / or broken nanotubes. Therefore, in multiple embodiments of the present invention, both anodes and cathodes contain CNS, fragments of CNS and / or broken CNTs.
[0144] In addition to the two electrodes, the Li-ion battery also contains a suitable electrolyte. Examples include, for example, ethylene carbonate-dimethyl carbonate-ethyl methyl carbonate (EC-DMC-EMC), vinylene carbonate (VC), LiPF6; ethylene carbonate-diethyl carbonate (EC-DEC, LiPF6; or (EC-DMC), LiPF6. In addition, the electrolyte composition may contain known enhanced electrolytes containing SiO x Special additives for the properties of the anode of silicon or silicon, such as fluorinated carbonates, such as fluoroethylene carbonate and others. A suitable glass fiber microfilter (e.g., Whatman GF / A) or polypropylene / polyethylene membrane (e.g., Celgard 2300) is used as a separator to absorb the electrolyte and prevent electrical contact between the electrodes while allowing the diffusion of Li ions.
[0145] In other embodiments, the compositions described herein are used in (e.g., incorporated into) electrodes of other energy storage devices such as primary alkaline batteries, primary lithium batteries, nickel metal hydride batteries, sodium batteries, lithium sulfur batteries, lithium air batteries, and supercapacitors. Methods for making such devices are known in the art and are described, for example, in the following: "Battery Reference Book", TR Crompton, Newness (2000).
[0146] A variety of techniques can be used to characterize the electrode compositions, electrodes, and batteries described herein, and / or to confirm the presence of CNS. Examples include, but are not limited to, electron microscopy such as TEM, SEM, Raman spectroscopy, or other suitable qualitative or quantitative analysis methods. For example, CNS granules ( Figure 4A ) and graphite anode containing CNS ( Figure 4B ). The white arrows show the CNSs in the graphite at a lower magnification, while the lower right image shows the CNSs in the graphite anode at a higher resolution.
[0147] Electrode performance and / or properties can be evaluated by procedures known in the art, or by adapting or developing techniques. Suitable techniques include, for example, in-plane and thru plane electrode conductivity, electrochemical impedance spectroscopy (EIS), constant current charge-discharge, hybrid pulse power characterization (HPPC), cycling. Some examples are described below.
[0148] Even at relatively low levels, CNS and / or CNS-derived components such as CNS fragments and / or broken CNTs appear to be able to provide a conductive network in the electrode. Anodes prepared using CNS often perform better than anodes that do not include conductive additives. In one example, the voltage profile of a graphite-only anode during cycles (cycles 1→100) using 2C cycling and 0.5 discharges exhibited rapid capacity decay. In contrast, graphite anodes prepared using CNS as described herein showed almost no change even at CNS loadings as low as 0.1 wt% (based on the weight of the dry anode composition).
[0149] In some embodiments, electrodes containing CNSs perform as well as comparative electrodes containing CBs at higher loadings (made using the same active electrode materials, e.g., graphite, binder, and, if used, other ingredients, e.g., dispersants). For example, anodes prepared using CNSs at loadings of no greater than about 0.5 wt %, (in some cases only 0.1 wt %) of the dry anode impart performance at least as good as electrodes containing 1 or more wt % CBs. In other implementations, anodes containing certain CNS loadings, e.g., 0.5 wt % or less, exhibit performance as good as, and often significantly better than, comparative electrodes containing the same amount of CBs (expressed as capacity retention over cycling).
[0150] The present invention is further illustrated by the following non-limiting examples.
[0151] Example
[0152] Comparative Example 1 - Preparation of graphite anode and testing in full coin cell
[0153] 48 g of graphite (grade BTR-918, available from BTR, China) was measured and placed in a 150 ml container from a Thinky mixer (model ARE-310). 20 grams of a previously prepared 10 wt% Arkema based A combination of HSV 900 polyvinylidene fluoride resin (PVDF) was combined with the graphite, and then 32 g of neat NMP was added. 1 A 1 / 4 inch diameter tungsten carbide media was carefully placed in the container and sealed.
[0154] A Thinky planetary mixer (model ARE-310) was used to prepare the anode coating slurry by the following procedure. First, the mixture was run at 2000 rpm for 30 seconds and checked to determine if all the materials were introduced. Then, the container was closed and a standard program method was run including: 4 min at 2000 rpm, 3 min rest, 4 min at 2000 rpm, 4 min rest and 4 min at 2000 rpm. The composition of the slurry was 96 wt% graphite: 4 wt% PVDF binder, based on dry matter.
[0155] The resulting anode slurry was coated onto copper foil using an automated knife coater (Model MSK-AFA-III from MTI Corp.) with a target of 14.5 mg / cm 2Coating area loading. NMP was evaporated in a convection oven set at 80°C for 20 minutes. Further, the electrode was dried at 110°C under vacuum for a minimum of 4 hours. 16 mm diameter discs were punched out using an MTI Precision DiscCutter (Model MSK-T-06) and calendered to 1.35 g / cc using a manual roller press (MR-100 from MTI Corp).
[0156] The cathode used in all examples involved a cathode electrode prepared with the following composition: NCM622 active material; CB conductive additive having the properties of Sample III in Table 3; HSV 900 PVDF binder in a ratio of 96.5:2:1.5. Specifically, the cathode was prepared by mixing an appropriate amount of 10 wt% of NCM622 in NMP (Sigma Aldrich >99% HPLC grade) with 10 wt% of PVDF. HSV 900PVDF (Arkema, molecular weight 900,000), CB conductive additive and NCM 622 (available from ShanShan, China) were mixed in NMP at 75 wt% total solids. The slurry was mixed with a Thinky mixer (Model ARE-310) for 30 minutes. The electrode slurry was coated on aluminum foil using an automated knife coater (Model MSK-AFA-III from MTI Corp.) with a target of 25 mg / cm 2 Coating area loading. NMP was evaporated in a convection oven set at 80°C for 20 minutes. 16 mm diameter discs were punched out for coin cell preparation and dried under vacuum at 110°C for a minimum of 4 hours. The discs were calendered to a density of 3.5 g / cc using an MTI manual roller press (Model MR-100).
[0157] The cathode and anode disks described above were assembled into 2032 coin cells in an argon-filled glove box (M-Braun) at an anode / cathode capacity ratio of 1.25. A glass fiber microfilter (Whatman GF / A) with a diameter of 17 mm was used as a separator. The electrolyte was 200 microliters of ethylene carbonate-dimethyl carbonate-ethyl methyl carbonate (EC-DMC-EMC), vinylene carbonate (VC) 1%, LiPF6 1M (BASF). Four coin cells were assembled for each formulation tested. Using a Maccor Series 4000 battery cycler, coin cells were formed using 2xC / 10 charge-discharge formation cycles in the 2.8-4.2 voltage window, with a constant voltage charge step to C / 20, followed by a C / 2 charge with a constant voltage charge step to C / 20.
[0158] Comparative Example 2 - Preparation of a graphite anode containing carbon black
[0159] 47.5 g of graphite (grade BTR-918, available from BTR, China) and 0.5 g of conductive carbon black (having the properties of specification I in Table 3) were weighed and combined with 20 grams of 10 wt% PVDF in the form of NMP solution in a 150 mL container. 32 g of neat NMP was added. The composition of the slurry was 95 wt% graphite: 1 wt% CB; 4 wt% PVDF, on a dry basis. The rest of the preparation protocol for the anode, cathode and full coin cell assembly was the same as in Example 1.
[0160] Example 3 - Preparation of graphite anodes containing different amounts of CNS
[0161] Several anode slurries (AC) were prepared containing different amounts of CNS ranging from 0.1 wt-0.5 wt% on a dry basis. The detailed compositions and weights (on a dry basis) of the components are summarized in Table 4. The preparation protocols of anode, cathode and full coin cell assembly were the same as those in Example 1.
[0162] Table 4
[0163]
[0164] Performance characteristics
[0165] Figure 5 Shown in is the voltage discharge profile for the first 100 cycles at 2C charge and C / 2 discharge rates for the unit cell described in Example 1 (graphite only anode). The tests were conducted at 25°C.
[0166] The rather harsh conditions were chosen to intentionally promote lithium plating at the graphite anode. The charge rate was 2C and the anode thickness was 14.5 mg / cm 2 .like Figure 5 As shown in , the cell capacity drops rapidly within the first 100 cycles. The cell was fully discharged after 100 cycles, placed in an argon glove box and carefully opened. The anode had a noticeable irregular yellow color, which indicated lithium metal plating.
[0167] The voltage discharge profile of the unit cell described in Example 3 (CNS in graphite medium anode) for 100 cycles using 2C charge and C / 2 discharge rates is shown in Figure 6 The test was carried out at 25°C.
[0168] In contrast to the cycling results of the cells using graphite-only anodes, the cycling data of the cells containing CN in the anode showed stable voltages under the same conditions. Surprisingly, even very small amounts (0.1 wt%) of CNS were effective in minimizing or reducing Li plating on the anode. No obvious signs of lithium plating were observed when one of the cells containing 0.25 wt% CNS was opened.
[0169] Perhaps a better way to illustrate the effect of CNS on cycle life is to extrapolate the existing data of Examples 1-3 using a simple exponential function such as y = a + b*exp{c*cycle #}.
[0170] Figure 7 The results of applying a three-parameter exponential function to extrapolate cycle life are summarized in FIG. This figure shows the capacity retention rate of the unit cells prepared according to Examples 1-3 as they cycle and their extrapolation. The actual data for the first 100 cycles of each example are shown as solid circles ( Figure 7 The cycling conditions were 2C charge, C / 2 discharge at 25°C. A three parameter simple exponential function (% retention = a + b*exp{c*cycle #}) was used for data extrapolation for all examples.
[0171] As is clear from the results, adding conductive additives (e.g., CB) to graphite helps extend cycle life (Example 2), however even more impressive results were obtained with CNS additives (Example 3). Modeling of data based on initial capacity fade indicates that with anodes containing CNS, 1000+ cycle lives may be possible despite harsh cycling conditions.
[0172] Comparative Example 4 - Comprising MWCNT and Preparation of P-Li anode electrode
[0173] In the same manner as described above, a 5% aqueous dispersion of multi-walled carbon nanotubes (LB217 from CNT (available from Jiangsu Cnano Technology Co. Limited)) and P-Li conductive carbon powder (available from Imerys) Anode electrode for both: 94.5wt% graphite / SiO x (Graphite to SiO x Ratio = 95:5): 1.5wt% MWCNT: 1wt% P-Li: 2wt% CMC: 1wt% SBR, based on dry matter. The electrode has a 5.2mg / cm 2 Loading amount.
[0174] The anode was pre-dried in an oven at 110° C. for 120 minutes. Further, the electrode was dried overnight at 110° C. under vacuum. 16 mm diameter discs were punched out by using an MTI Precision Disc Cutter (Model MSKT-06) and calendered to 1.2 g / cc using a manual roller press (MR-100, MTI Corp).
[0175] The cathode-NCM622 active material was formulated with the following composition: HP carbon conductive additive: HSV 900 PVDF binder, ratio 96.5:2:1.5, dry basis.
[0176] Specifically, the cathode slurry was prepared by mixing appropriate amounts of 10 wt % of HSV 900PVDF (Arkema), with carbon conductive additives HP (available from Cabot Corporation) was added with NCM 622 (available from ShanShan, China) at a total solids of 75 wt % in NMP. The slurry was mixed for 30 minutes using a Thinky mixer (Model ARE-310). The electrode slurry was coated on aluminum foil using an automated knife coater (Model MSK-AFA-III from MTI Corp.) with a target of 14 mg / cm 2 Area loading. NMP was evaporated in a convection oven set at 80°C for 20 minutes. 15 mm diameter discs were punched out for coin cell preparation and dried under vacuum at 110°C for a minimum of 4 hours. The discs were calendered to a density of 3.5 g / cc using an MTI manual roller press (Model MR-100).
[0177] The cathode and anode discs described above were assembled into 2032 coin cells in an argon-filled glove box (M-Braun) with an anode / cathode capacity ratio of 1.25. A glass fiber microfilter (Whatman GF / A) with a diameter of 17 mm was used as a separator. The electrolyte composition was ethylene carbonate-dimethyl carbonate (EC:DMC, 1:1) and included 10wt% monofluoroethylene carbonate (FEC, Solvay Fluorides) with 1M LiPF6 (Sigma Aldrich). Four coin cells were assembled for each tested formulation. Using a Maccor Series 4000 battery cycler, the coin cells were formed using 2xC / 10 charge-discharge formation cycles in the 2.8-4.2 voltage window. After the c-rate performance evaluation, the coin cells were cycled at room temperature using CC-CV (1C-4.2V, C / 20) / 1D charge / discharge rates.
[0178] Example 5 - Preparation of anode slurry and anode electrode using CNS
[0179] The combination of 17.64 grams of 2wt% carboxymethyl cellulose sodium salt (CMC) water-soluble and 16.16 grams of graphite (BTR-918, available from BTR, China) is placed in a 50ml steel jacketed tungsten carbide vial (model 8004SS) and gently mixed. Then 0.1 grams of encapsulated CNS granules (Cabot Corporation) are added together with six 1 / 4 inch diameter tungsten carbide media. The vial is closed and mixed for 80 minutes by using Spex Sampe Prep Mixer (model 8000M). The mixer is stopped every 20 minutes to determine whether all materials are being introduced. After mixing for 80 minutes, 0.85 grams of SiOx / C powder (KSC-1265, available from Shin-Etsu Chemical Co., Ltd) is added to the mixture and mixed for another 3 minutes. Afterwards, 0.353 grams of styrene-butadiene rubber (TD105A, JSR) is combined with the mixture and mixed for 1 minute. Finally, 14.35 grams of deionized water was added to the slurry and the vial was mixed for an additional 10 minutes. The composition of the slurry was 96.45 wt% graphite / SiO x (Graphite to SiO x =95:5): 0.55wt% encapsulated CNS: 2wt% CMC: 1wt% SBR, based on dry matter.
[0180] The resulting anode slurry was coated onto copper foil using an automated knife coater (Model MSK-AFA-III from MTI Corp.) with a target of 5.2 mg / cm 2Area loading. The anode was pre-dried in an oven at 110°C for 120 minutes. Further, the electrode was dried overnight at 110°C under vacuum. 16 mm diameter discs were punched out using MTI Precision Disc Cutter (Model MSKT-06) and calendered to 1.2 g / cc using a manual roller press (MR-100, MTI Corp).
[0181] The cathode and coin cell assembly were prepared according to the protocol described in Comparative Example 4.
[0182] Figure 8 The results are shown in Figure 5 using an anode containing CNS prepared as described in Example 5 (labeled A), and MWCNT+ prepared as described in Comparative Example 4. Figure 2 shows the capacity retention of a full cell using 1C / 1C cycling for a combination of MWCNTs and P additives (labeled B). As is clear from the figure, the battery cell using an anode containing CNS significantly extends the cycle life performance. The P-Li combination was only effective up to ~250 cycles (~80% retention) under these cycling conditions. More importantly, such performance required only ~1 / 4 to ~1 / 5 of the total carbon additive used in the comparative examples (0.55 wt% CNS for MWCNT+ 2.5 wt% total in the case of P-Li). This example clearly highlights the importance of x -The unit cell of graphite anode realizes the unique CNS morphology characteristics for better cycling performance.
[0183] As used herein, the term "and / or" includes any and all combinations of one or more of the related enumerated items. In addition, the singular form and the articles "a, an" and "the" are also intended to include plural forms, unless otherwise expressly stated. It will be further understood that the terms: include, contain, contain and / or contain, when used in this specification, indicate that there are stated features, wholes, steps, operations, elements, and / or components, but do not exclude the presence or addition of one or more other features, wholes, steps, operations, elements, components, and / or their collections. In addition, it will be understood that when an element, including its parts or subsystems, is referred to and / or shown as being connected or coupled to another element, it may be directly connected or coupled to the other element or there may be an intermediate element.
[0184] It will be understood that although terms such as "first" and "second" are used herein to describe various elements, these elements should not be limited by these terms. These terms are only used to distinguish one element from another element. Therefore, without departing from the teachings of the present invention, the element discussed below may be referred to as a second element, and similarly, the second element may be referred to as a first element.
[0185] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present invention pertains. It will be further understood that terms, such as those defined in commonly used dictionaries, should be interpreted as having a meaning consistent with their meaning in the context of the relevant art and will not be interpreted in an idealized or overly formal sense unless clearly so defined herein.
[0186] While the present invention has been particularly shown and described with reference to preferred embodiments thereof, it will be understood by those skilled in the art that various changes in form and details may be made therein without departing from the scope of the invention as encompassed by the appended claims.
Claims
1. An electrode composition comprising: active anode material; and at least one material selected from the group consisting of a carbon nanostructure, a fragment of a carbon nanostructure, and a broken multi-walled carbon nanotube, The active anode material includes graphite, silicon, SiO x , silicon-graphite composite or lithium titanate wherein the carbon nanostructure or the fragment of the carbon nanostructure comprises a plurality of multi-walled carbon nanotubes cross-linked into a polymeric structure by branching, interlacing, entanglement and / or sharing a common wall, and wherein the broken multi-walled carbon nanotubes are derived from a carbon nanostructure and are branched and share a common wall with each other, in: At least one of the multi-walled carbon nanotubes has a length equal to or greater than 2 micrometers, as determined by SEM, at least one of the multi-walled carbon nanotubes has an aspect ratio of length to diameter in the range of 200-1000, Along a 2 micron length of at least one of the multi-walled carbon nanotubes, there are at least two branches, as determined by SEM, At least one multi-walled carbon nanotube exhibits an asymmetry with respect to the number of walls observed in the region after the branch point relative to the region before the branch point, and / or There were no catalyst particles present at or near the branching points as determined by TEM.
2. The electrode composition of claim 1, wherein the multi-walled carbon nanotubes comprise 2 to 30 coaxial nanotubes as determined by TEM at a magnification sufficient to count the number of walls.
3. The electrode composition of claim 1 or 2, wherein at least 1% of the carbon nanotubes have a length equal to or greater than 2 microns as determined by SEM, An aspect ratio of length to diameter in the range of 200-1000, and / or an asymmetry in the number of walls observed in the region after the branch point relative to the region before the branch point.
4. The electrode composition of claim 1 or 2, wherein the composition further comprises a binder.
5. The composition of claim 4, wherein the binder is polyvinylidene fluoride, or carboxymethyl cellulose and styrene butadiene rubber.
6. The electrode composition of claim 1 or 2, wherein the composition is a paste, a slurry or a solid.
7. The electrode composition of claim 6, wherein the composition further comprises a solvent.
8. The electrode composition of claim 7, wherein the solvent is N-methylpyrrolidone, acetone, alcohol, water, or any combination thereof.
9. The electrode composition of claim 1 or 2, wherein the electrode composition contains carbon nanostructures, fragments of carbon nanostructures and / or broken multi-walled carbon nanotubes in an amount of not greater than 5 wt% when dried.
10. The electrode composition of claim 1 or 2, wherein the carbon nanostructure is a coated carbon nanostructure. 11 . The electrode composition of claim 10 , wherein the coated carbon nanostructure is a polyurethane-coated nanostructure or a polyethylene glycol-coated carbon nanostructure. 12 . The electrode composition of claim 10 , wherein the weight of the coating is in the range of 0.1% to 10% relative to the weight of the coated carbon nanostructure.
13. The electrode composition of claim 10, wherein the electrode composition contains coated carbon nanostructures, fragments of coated carbon nanostructures, and / or broken multi-walled carbon nanotubes derived from coated carbon nanostructures in an amount of no greater than 5 wt% when dried.
14. The electrode composition of claim 1 or 2, comprising the active anode material in an amount of 80-99 wt%.
15. The electrode composition of claim 1 or 2, further comprising a carbon conductive additive selected from the group consisting of carbon black, individualized carbon nanotubes in pristine form, and any combination thereof.
16. The electrode composition of claim 1 or 2, further comprising carbon black, wherein the carbon black has a carbon black content of 200 m 2 / g or less and an OAN of at least 130 mL / 100 g.
17. An electrode comprising a composition according to any one of the preceding claims and a current collector in contact with the electrode composition.
18. A battery comprising a composition according to any one of claims 1 to 16 or an electrode according to claim 17.
19. The battery of claim 18, further comprising a cathode comprising a lithium transition metal compound and at least one material selected from the group consisting of a carbon nanostructure, a fragment of a carbon nanostructure, and a broken multi-walled carbon nanotube, wherein the carbon nanostructure or the fragment of the carbon nanostructure comprises a plurality of multi-walled carbon nanotubes cross-linked into a polymeric structure by branching, interlacing, entanglement and / or sharing a common wall, and The broken multi-walled carbon nanotubes are derived from a carbon nanostructure and are branched and share a common wall with each other.
20. A rechargeable lithium ion battery comprising the composition of any one of claims 1 to 16, or the electrode of claim 17.
21. A method for preparing an electrode composition, the method comprising: combining a dispersion comprising at least one material selected from the group consisting of carbon nanostructures, fragments of carbon nanostructures, and broken multi-walled carbon nanotubes with an active anode material to form the electrode composition, wherein the carbon nanostructure or the fragment of the carbon nanostructure comprises a plurality of multi-walled carbon nanotubes cross-linked into a polymeric structure by branching, interlacing, entanglement and / or sharing a common wall, wherein the broken multi-walled carbon nanotubes are derived from a carbon nanostructure and are branched and share a common wall with each other, and The active anode material includes graphite, silicon, SiO x , silicon-graphite composite or lithium titanate, in: At least one of the multi-walled carbon nanotubes has a length equal to or greater than 2 micrometers, as determined by SEM, at least one of the multi-walled carbon nanotubes has an aspect ratio of length to diameter in the range of 200-1000, Along a 2 micron length of at least one of the multi-walled carbon nanotubes, there are at least two branches, as determined by SEM, At least one multi-walled carbon nanotube exhibits an asymmetry with respect to the number of walls observed in the region after the branch point relative to the region before the branch point, and / or There were no catalyst particles present at or near the branching points as determined by TEM.
22. The method of claim 21, wherein the multi-walled carbon nanotubes comprise 2-30 coaxial nanotubes as determined by TEM at a magnification sufficient to count the number of walls.
23. The method of claim 21 or 22, wherein at least 1% of the carbon nanotubes have a length equal to or greater than 2 microns as determined by SEM, An aspect ratio of length to diameter in the range of 200-1000, and / or an asymmetry in the number of walls observed in the region after the branch point relative to the region before the branch point.
24. The method of claim 21 or 22, wherein the dispersion contains a liquid selected from the group consisting of N-methylpyrrolidone, acetone, alcohol, water, and any combination thereof.
25. The method of claim 21 or 22, wherein the electrode composition further comprises a binder.
26. The method of claim 25, wherein the binder is polyvinylidene fluoride or styrene butadiene rubber and carboxymethyl cellulose.
27. The method of claim 21 or 22, further comprising drying the electrode composition.
28. The method of claim 21 or 22, wherein the active anode material is provided in an amount of 80-99 wt%.
29. The method of claim 21 or 22, further comprising applying the electrode composition to a current collector.
30. The method of claim 21 or 22, wherein the electrode composition comprises carbon nanostructures, fragments of carbon nanostructures, and / or broken multi-walled carbon nanotubes in an amount of no greater than 5 wt% when dried.
31. The method of claim 21 or 22, wherein the carbon nanostructure is a coated carbon nanostructure.
32. The method of claim 31, wherein the carbon nanostructure is a polyurethane-coated nanostructure or a polyethylene glycol-coated carbon nanostructure.
33. The method of claim 31, wherein The weight of the coating is in the range of 0.1-10% relative to the weight of the coated carbon nanostructure.
34. The method of claim 31, wherein The capped carbon nanostructure is provided in an amount of no greater than 5 wt % based on the weight of the composition when dry.
35. The method of claim 21 or 22, wherein the dispersion further comprises a carbon conductive additive selected from the group consisting of carbon black, individualized carbon nanotubes in pristine form, and any combination thereof.
36. The method of claim 21 or 22, further comprising carbon black, wherein the carbon black has a 200 m 2 / g or less and an OAN of at least 130 mL / 100 g.
37. The method of claim 21 or 22, wherein the dispersion is prepared by combining the carbon nanostructures with a liquid.
38. The method of claim 37, wherein the carbon nanostructures are provided in the form of loose particulate material.
39. The method of claim 38, wherein the liquid is selected from the group consisting of N-methylpyrrolidone, acetone, alcohol, water, and any combination thereof.
40. A method of preparing an electrode composition, the method comprising introducing a carbon nanostructure into a slurry comprising an active anode material to form the electrode composition, The active anode material includes graphite, silicon, SiO x , silicon-graphite composite or lithium titanate, and wherein the carbon nanostructure comprises a plurality of multi-walled carbon nanotubes cross-linked into a polymeric structure by branching, interlacing, entanglement and / or sharing a common wall, in: At least one of the multi-walled carbon nanotubes has a length equal to or greater than 2 micrometers, as determined by SEM, at least one of the multi-walled carbon nanotubes has an aspect ratio of length to diameter in the range of 200-1000, Along a 2 micron length of at least one of the multi-walled carbon nanotubes, there are at least two branches, as determined by SEM, At least one multi-walled carbon nanotube exhibits an asymmetry with respect to the number of walls observed in the region after the branch point relative to the region before the branch point, and / or There were no catalyst particles present at or near the branching points as determined by TEM.
41. The method of claim 40, wherein the multi-walled carbon nanotubes comprise 2-30 coaxial nanotubes as determined by TEM at a magnification sufficient to count the number of walls.
42. The method of claim 40 or 41, wherein at least 1% of the carbon nanotubes have a length equal to or greater than 2 microns as determined by SEM, An aspect ratio of length to diameter in the range of 200-1000, and / or an asymmetry in the number of walls observed in the region after the branch point relative to the region before the branch point.
43. The method of claim 40 or 41, wherein the carbon nanostructures are provided as flakes, pellets or granules.
44. The method of claim 40 or 41, wherein the active anode material is provided in an amount of 80-99 wt%.
45. The method of claim 40 or 41, further comprising applying the electrode composition to a current collector.
46. The method of claim 40 or 41, further comprising drying the electrode composition.
47. The method of claim 40 or 41, wherein the electrode composition comprises carbon nanostructures, fragments of carbon nanostructures, and / or broken multi-walled carbon nanotubes in an amount of no greater than 5 weight percent when dried.
48. The method of claim 40 or 41, wherein the carbon nanostructure is a coated carbon nanostructure.
49. The method of claim 48, wherein the coated carbon nanostructure is a polyurethane-coated carbon nanostructure or a polyethylene glycol-coated carbon nanostructure.
50. The method of claim 48, wherein The weight of the coating is in the range of 0.1-10% relative to the weight of the coated carbon nanostructure.
51. The method of claim 48, wherein The capped carbon nanostructure is provided in an amount of no greater than 5 wt % based on the weight of the composition when dry.
52. The method of claim 40 or 41, wherein the electrode composition further comprises a binder.
53. The method of claim 52, wherein the binder is polyvinylidene fluoride or styrene butadiene rubber and carboxymethyl cellulose.
54. The method of claim 40 or 41, wherein the electrode composition further comprises a liquid.
55. The method of claim 54, wherein the liquid is selected from the group consisting of N-methylpyrrolidone, acetone, alcohol, water, and any combination thereof.
56. The method of claim 40 or 41, wherein the electrode composition further comprises a carbon conductive additive selected from the group consisting of carbon black, individualized carbon nanotubes in pristine form, and any combination thereof.
57. The method of claim 40 or 41, wherein the slurry further comprises carbon black and the carbon black has a 200 m 2 / g or less and an OAN of at least 130 mL / 100 g.
58. The method of claim 21, 22, 40 or 41, wherein the method produces fragments of carbon nanostructures and / or broken multi-walled carbon nanotubes, wherein the carbon nanostructure or the fragment of the carbon nanostructure comprises a plurality of multi-walled carbon nanotubes cross-linked into a polymeric structure by branching, interlacing, entanglement and / or sharing a common wall, and The broken multi-walled carbon nanotubes are derived from a carbon nanostructure and are branched and share a common wall with each other.
59. Lithium batteries, including: a cathode comprising a lithium transition metal compound and a material selected from the group consisting of a carbon nanostructure, a fragment of a carbon nanostructure, and a broken multi-walled carbon nanotube, and an anode comprising an active anode material and a material selected from the group consisting of carbon nanostructures, fragments of carbon nanostructures, and broken multi-walled carbon nanotubes, wherein the carbon nanostructure or the fragment of the carbon nanostructure comprises a plurality of multi-walled carbon nanotubes cross-linked into a polymeric structure by branching, interlacing, entanglement and / or sharing a common wall, and wherein the broken multi-walled carbon nanotubes are derived from a carbon nanostructure and are branched and share a common wall with each other, in: At least one of the multi-walled carbon nanotubes has a length equal to or greater than 2 micrometers, as determined by SEM, at least one of the multi-walled carbon nanotubes has an aspect ratio of length to diameter in the range of 200-1000, Along a 2 micron length of at least one of the multi-walled carbon nanotubes, there are at least two branches, as determined by SEM, At least one multi-walled carbon nanotube exhibits an asymmetry with respect to the number of walls observed in the region after the branch point relative to the region before the branch point, and / or There were no catalyst particles present at or near the branching points as determined by TEM.