A pressed cathode and a method for preparing the same

By setting a tungsten sponge and doped emitter active substance on the magnetron cathode substrate for pressing and sintering, a cermet-like surface is formed, which solves the problem of insufficient cathode resistance to electron bombardment in the prior art, and achieves high power and long life The continuous wave magnetron cathode simplifies the preparation process and improves operability.

CN113889388BActive Publication Date: 2024-12-03AEROSPACE INFORMATION RES INST CAS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202110956410.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-19
Publication Date
2024-12-03
Estimated Expiration
2041-08-19

AI Technical Summary

Technical Problem

The existing magnetron cathode has insufficient electron bombardment resistance in high power, high frequency, continuous wave working modes, resulting in a decrease in emission current density and shortened lifetime, and the preparation process is complicated and the process is difficult.

Method used

Using the pressed cathode preparation method, by setting a tungsten sponge and Y-Gd-Hf-O emission active substance doped with Sc2O3 on the surface of the cathode substrate, it is pressed and sintered to form a cermet-like surface, which enhances the bonding performance and density. , improve the resistance to electronic bombardment.

Benefits of technology

It effectively improves the cathode's electron bombardment resistance and secondary electron emission performance, reduces the working temperature, extends the service life of the magnetron, simplifies the preparation process, and improves operability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113889388B_ABST
    Figure CN113889388B_ABST
Patent Text Reader

Abstract

The present invention provides a pressed cathode and a preparation method thereof, the method comprising sequentially arranging tungsten sponge and active material on the surface of the cathode substrate, and then pressing and sintering. The pressed cathode prepared by the present invention has a metal ceramic surface, and can stably work for more than 500 hours under continuous electron bombardment of 10W, effectively improving the cathode's ability to withstand electron bombardment; at the same time, the secondary electron emission capacity of the metal ceramic pressed cathode is also improved, which can reduce the filament heating current after the magnetron is started, and correspondingly reduce the cathode's working temperature, thereby extending the cathode's service life and realizing the widespread use of high-power, long-life, continuous-wave magnetron cathodes. The method of the present invention is short in time and energy consumption, and has a simple process flow, strong operability, and broad application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electric vacuum devices, and in particular to a pressed cathode and a preparation method thereof. Background Art

[0002] Magnetron is a reentrant resonant orthogonal oscillator and a high-power microwave source in microwave technology. Its main features are high output power, high efficiency and low operating voltage; secondly, its simple structure brings small size, light weight, easy use, reliable operation and low cost. At present, the application scope of magnetron has gradually expanded from military fields such as radar and navigation to civilian fields. Since the 1960s, the wide application of microwave heating in industrial and agricultural production, physical therapy and daily life has brought broad prospects for the production of continuous wave magnetrons, and this trend has continued to increase, and it is gradually being understood and used in various fields of the national economy.

[0003] According to the working principle of the magnetron, when working, the electrons emitted from the cathode surface into the vacuum, among which the electrons in the acceleration phase in the high-frequency field, obtain energy from the microwave field and are continuously accelerated and their kinetic energy increases. These electrons do not hit the anode and form the anode current, but reach the cathode surface to stop moving, and at the same time generate a certain proportion of secondary electrons. According to analysis, when the magnetron works normally, 90% of the anode current is composed of secondary electrons. However, when the emitted electrons return to the cathode surface, they will bombard the cathode surface, which will not only sputter the active substances on the surface to a certain extent, causing the emission active substances on the cathode surface to decompose, but also a large amount of electron bombardment will cause the temperature of the cathode to rise rapidly, accelerate the evaporation of the active substances, and thus cause the emission current density of the cathode to drop rapidly and shorten the life. Therefore, for the cathode working in the orthogonal field, improving the cathode's ability to withstand electron bombardment is one of the keys to improving the performance of the magnetron.

[0004] With the development of magnetrons towards high power, high frequency, and continuous wave working modes, higher requirements are put forward for the cathode's thermal emission, secondary electron emission, and electron bombardment resistance to extend its service life. Continuous wave magnetrons generally use pure W cathodes, ThO2-W cathodes, and their alloy cathodes, but the pure W cathode has a high operating temperature, low thermal emission capacity, and high vacuum requirements; the ThO2-W cathode is radioactive and has a complex preparation process; the rare earth oxide cathode has a lower operating temperature than the pure W cathode, and has a large secondary emission coefficient and is resistant to high temperatures, but the cathodes obtained by the currently commonly used impregnation coating technology or surface spraying technology have the defects of complicated processes and high difficulty, and when the obtained cathode works at high temperature, the oxide coating in the molten state on the surface is greatly affected by electron bombardment, and the surface active material is easily lost, thereby shortening the cathode life. Therefore, in order to better apply the cathode to high-power continuous wave magnetrons and extend its service life, it is very important to improve the cathode's electron bombardment resistance. Summary of the invention

[0005] In view of the shortcomings of the prior art, one of the objectives of the present invention is to provide a method for preparing a pressed cathode.

[0006] Another object of the present invention is to provide a pressed cathode prepared by the above method.

[0007] Another object of the present invention is to provide application of the above pressed cathode in the preparation of magnetron.

[0008] To this end, the present invention provides the following technical solutions:

[0009] A method for preparing a pressed cathode comprises the following steps: arranging tungsten sponge and emitting active material on the surface of a cathode substrate in sequence, and then pressing and sintering the cathode.

[0010] The present invention finds that pressing the emission active material can enhance the bonding performance between the emission active materials and between the emission active material and the substrate, and can make the emission active material more compact and flat. Subsequent sintering further enhances the density of the cathode, making its surface present a metal ceramic state, which can prolong the retention time of the emission active material on the cathode surface. On the premise of meeting the thermal emission requirements, it can not only improve the cathode's electron bombardment resistance, but also improve the cathode's secondary electron emission performance. Correspondingly, it can reduce the filament heating current after the magnetron is started, reduce the cathode's operating temperature, and thus prolong the service life of the continuous wave magnetron, thereby realizing the promotion of cathodes for high-power continuous wave magnetrons.

[0011] The beneficial effects of the present invention are:

[0012] The surface of the pressed cathode prepared by the method of the present invention is in the shape of metal ceramics. Under the continuous bombardment of 10 W electrons, it can stably work for more than 500 hours, effectively improving the electron bombardment resistance of the cathode; at the same time, the secondary electron emission capacity of the pressed cathode in the shape of metal ceramics is also improved, which can reduce the filament heating current after the magnetron is started, and correspondingly reduce the working temperature of the cathode, thereby extending the service life of the cathode, and realizing the widespread use of high-power, long-life, continuous-wave magnetron cathodes.

[0013] The method of the invention is time-saving, energy-saving, simple in process flow, highly operable, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 The present invention provides a flow chart for preparing the pressed cathode.

[0015] Figure 2 This is a schematic diagram of the structure of a pressed cathode made by the method provided by the present invention, 1-cathode substrate; 2-tungsten sponge; 3-Y-Gd-Hf-O emission active material doped with Sc2O3.

[0016] Figure 3 The present invention provides a microscopic morphology of the surface of a pressed cathode prepared by the preparation method provided by the present invention.

[0017] Figure 4 The thermal emission volt-ampere characteristic results of the pressed cathode prepared by the preparation method provided by the present invention.

[0018] Figure 5 Schematic diagram of the cathode electron bombardment resistance test principle.

[0019] Figure 6 The graph is the cathode electron bombardment resistance test result. Among them, a is the curve of the emission current percentage of the cathode obtained by the preparation method of the present invention versus the bombardment time, and b is the curve of the emission current percentage of the cathode obtained by the common coating method versus the bombardment time.

[0020] Figure 7 The results are life test results of the pressed cathode prepared by the preparation method provided by the present invention. DETAILED DESCRIPTION

[0021] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] In an exemplary embodiment of the present invention, a method for preparing a pressed cathode is provided. The method comprises:

[0023] providing a cathode substrate;

[0024] A tungsten sponge is arranged on the surface of the cathode substrate;

[0025] Molding the emission active material on the tungsten sponge;

[0026] High temperature hydrogen furnace sintering.

[0027] The flow chart of the method for preparing a pressed cathode provided by the present invention is as follows: Figure 1 As shown, the specific steps include:

[0028] Cathode substrate preparation: The cathode substrate material can be tungsten or tungsten-rhenium alloy (W-Re), and its shape can be strip, round or other shapes. Before use, sandblasting and cleaning are carried out to thoroughly remove surface oil, sandblasting particles and other impurities, and the cleaned substrate is annealed in a hydrogen atmosphere to keep the cathode substrate surface clean and roughened.

[0029] Among them, the cathode substrate material is preferably W-Re alloy. Studies have found that the introduction of Re element can effectively improve the comprehensive performance of the cathode, not only can refine the grains, improve the thermal emission capacity of the cathode, but also improve the emission uniformity and improve the cathode's resistance to electron bombardment. The doping amount of Re in the W-Re alloy is preferably 25wt.%.

[0030] The annealing heat treatment process is: in a hydrogen atmosphere, the temperature is linearly increased from room temperature to 1300~1350 ℃, the heating rate is 40~50 ℃ / min, and the temperature is kept at this temperature for 10~15 min, and then the temperature is slowly cooled to room temperature naturally in a hydrogen atmosphere. The cathode substrate is annealed to eliminate the stress caused by sandblasting, and the cathode can be purified at the same time.

[0031] The cathode substrate of the present invention not only serves as a support for the emission active material, but also can replenish the emitted electrons in time when the cathode surface active material emits electrons, so that the cathode always maintains an electrically neutral state.

[0032] Tungsten sponge is prepared on the surface of the cathode substrate: a mixture of tungsten powder and nitrate-cotton solution mixed in a certain proportion is sprayed evenly on the roughened side of the cathode substrate by spraying, and baked under an infrared lamp. After drying, it is sintered at high temperature in a hydrogen atmosphere.

[0033] The purity of the tungsten powder used is 99.9%, the average particle size is 1-3 µm, the concentration of the saltpeter solution is 0.8-3.0 wt.%, and the tungsten powder and the saltpeter solution are evenly mixed in a volume ratio of 1:2-4. Before high-temperature sintering, the cathode substrate sprayed with tungsten sponge can be placed under an infrared lamp for drying to volatilize the organic solvent in advance, which is conducive to the smooth progress of subsequent high-temperature sintering. Preferably, the baking time is not less than 30 min.

[0034] The high temperature sintering process is: linearly increase the temperature from room temperature to 1500~1550 ℃, the heating rate is 40~50 ℃ / min, and keep it at this temperature for 10~15 min, and finally slowly cool it down to room temperature in a hydrogen atmosphere. The high temperature hydrogen atmosphere sintering of tungsten sponge can not only enhance the bonding between tungsten sponge and substrate, but also completely evaporate the organic solvent, making the tungsten sponge present a loose porous structure.

[0035] The loose porous tungsten sponge prepared by the present invention can not only enhance the bonding between the emission active material and the cathode substrate, but also the porous sponge structure is conducive to the transmission and replenishment of electrons from the substrate to the surface layer, improves the thermal emission capacity of the cathode, and can also increase the reserve of the emission active material. Studies have found that if the thickness of the tungsten sponge is too thick, it will hinder the transmission and replenishment of electrons from the cathode substrate to the emission surface layer, thereby affecting the thermal emission performance of the cathode; on the contrary, if it is thin, it will not only affect the storage of the emission active material, but also affect the bonding between the emission active material and the substrate, reducing the cathode's ability to withstand electron bombardment. Preferably, the thickness of the tungsten sponge is controlled at 0.1~0.2 mm.

[0036] Prepare the doped emission active material on the tungsten sponge and press it: mix the emission active material with the nitrate cotton solution into a viscous slurry, use a micro brush to evenly apply and impregnate it on the prepared tungsten sponge, mold the cathode impregnated with the emission active material, and demold after the pressing is completed.

[0037] Among them, the emission active material is Y-Gd-Hf-O, and Y-Gd-Hf-O is made of Y2O3, Gd2O3, and HfO2 with molar percentages of 45-50%, 5-10%, and 50-45%, respectively. Studies have shown that doping Sc2O3 into the emission active material can improve the thermal emission ability of the cathode, and the doping amount of Sc2O3 is preferably 3-5 wt.%. At the same time, controlling the thickness of the tungsten sponge and the total thickness of the tungsten sponge and the emission active material can improve the bonding strength between the emission active material and the substrate while ensuring that the cathode substrate can replenish the emitted electrons in time, so that the emission surface layer always maintains electrical neutrality, which is also conducive to the base metal. Preferably, the total thickness of the active material and the tungsten sponge is controlled within 0.3-0.4 mm.

[0038] In some preferred embodiments, the pressing pressure is 4 kN and the holding time is 30 to 60 s. The pressing can be performed on an oil press or by other methods, such as vacuum hot pressing, isostatic pressing, etc.

[0039] High-temperature hydrogen furnace sintering: The pressed cathode is placed in a hydrogen atmosphere, and the temperature is linearly increased from room temperature to 1300-1350°C at a heating rate of 40-50°C / min, and the temperature is kept at this temperature for 3-5 min, and then the temperature is slowly naturally cooled to room temperature in a hydrogen atmosphere to prepare the cathode of the present invention, and its structure is as follows: Figure 2 shown. Example

[0040] This embodiment provides a method for preparing a pressed cathode, comprising the following steps:

[0041] Preparation of cathode substrate: The cathode substrate material is W-Re alloy (Re doping amount is 25wt.%), strip-shaped, with a size of l×d×h: 10 mm×0.3 mm×0.2 mm. Before use, it is sandblasted and cleaned to thoroughly remove surface oil, sandblasting particles and other impurities, and the cleaned substrate is annealed in a hydrogen atmosphere. The annealing heat treatment process is: linearly increase the temperature from room temperature to 1300 ℃, the heating rate is 40 ℃ / min, and the temperature is kept at this temperature for 10 minutes, and then slowly and naturally cooled to room temperature in a hydrogen atmosphere.

[0042] Tungsten sponge was prepared on the surface of the cathode substrate: W powder (purity of 99.9%, average particle size of 1~3 μm) and nitrate cotton solution (concentration of 1.5 wt.%) were mixed evenly in a volume ratio of 1:2, and the resulting mixture was sprayed evenly on the roughened side of the cathode substrate by spraying, and then baked under a 100 W infrared lamp for about 60 min. After drying, high-temperature sintering was performed in a hydrogen atmosphere. The high-temperature sintering process was: linearly heating from room temperature to 1550 ℃, the heating rate was 40 ℃ / min, and the temperature was kept at this temperature for 10 min, and finally slowly cooled to room temperature in a hydrogen atmosphere. The thickness of the tungsten sponge layer was controlled at 0.09~0.11 mm.

[0043] Preparation of Y-Gd-Hf-O emission active material doped with Sc2O3 on tungsten sponge and pressing: Y-Gd-Hf-O emission active material doped with Sc2O3 is mixed with a 1.5 wt.% nitrate cotton solution to form a viscous slurry, and a micro brush is used to evenly apply and impregnate the tungsten sponge. The cathode impregnated with the active material is pressed using an oil press, with a pressure of 4 kN and a holding time of 30 s. After the pressing is completed, the mold is removed. Among them, the doping amount of Sc2O3 is 5 wt.%. Preparation of Y-Gd-Hf-O: Y2O3, Gd2O3, and HfO2 with a purity of 99.99% and molar percentages of 45%, 5%, and 50% are weighed, mixed, and placed in a ball mill, and anhydrous ethanol with a volume ratio of 2 / 3 is added as a ball milling medium. The ball mill is milled for more than 100 hours to fully mix them evenly. The obtained suspension was dried under an infrared lamp to obtain a fully mixed powder, which was pressed into a 10 mm × 2 mm cake using a hydraulic press at a pressure of 200 MPa. The obtained cake was sintered at a high temperature of 1450 ° C for 3 h in a muffle furnace and then naturally cooled to room temperature. Finally, the obtained cake was doped with 5 wt.% Sc2O3 and mechanically ground in a mortar for more than 2 h to obtain a uniformly mixed emission active material. The total thickness of the emission active material and tungsten sponge was controlled within 0.35~0.4 mm.

[0044] High-temperature hydrogen furnace sintering: The pressed cathode is placed in a hydrogen atmosphere, and the temperature is linearly increased from room temperature to 1350°C at a heating rate of 40°C / min, and maintained at this temperature for 3 min, and then slowly cooled to room temperature in a hydrogen atmosphere to prepare a pressed cathode.

[0045] The pressed cathode was subjected to SEM micromorphology analysis, such as Figure 3 As shown, the cathode surface presents a dense and flat microscopic morphology, and the surface is in a metal ceramic shape with a high degree of density, which is beneficial to improving the cathode's ability to withstand electron bombardment.

[0046] The pressed cathode prepared in the present invention was subjected to thermal emission voltammetric characteristics test. The pressed cathode prepared in Example 1 was placed in a thermal emission diode test system, and firstly vacuumed. -6 After Pa, high temperature degassing, activation, and aging were carried out in sequence, and finally the volt-ampere characteristics were tested at different temperatures. The results are as follows Figure 4 When the cathode temperature is 1350℃, 1400℃, 1450℃, 1500℃, and 1550℃, the saturated emission current density of the cathode is 0.64 A / cm 2 , 0.88 A / cm 2 , 1.2 A / cm 2 , 1.6 A / cm2 , 2.08 A / cm 2 .

[0047] The electron bombardment resistance test of the pressed cathode prepared by the present invention is carried out. The test principle is as follows: Figure 5 The prepared pressed cathode is placed in the electron bombardment resistant diode test system, and firstly evacuated until the vacuum degree is better than 10 -6 After Pa, the pressed cathode A and the bombardment source cathode B of the present invention were subjected to high temperature degassing, activation, and aging, and finally subjected to electron bombardment resistance test. During the test, by controlling the heating power supply Uf1 and the acceleration voltage Ua1, the working temperature of the pressed cathode of the present invention was kept at 1500-1550 °C, and the thermal emission current density was kept at 1 A / cm 2 At the same time, the bombardment source cathode Uf2 and Ua2 are adjusted to make the rated bombardment power reach 10 W, and the pressed cathode of the present invention is bombarded continuously, and the emission current density Ia of the pressed cathode changes with the bombardment time t to evaluate the cathode's ability to withstand electron bombardment. The test results are as follows: Figure 6 As shown in curve a.

[0048] In order to obtain obvious experimental comparison data and more fully reflect the superiority of the pressed cathode of the present invention, the same test method and the same emission active material are used to conduct an electron bombardment resistance test on the W-Re based direct heated cathode prepared by the ordinary coating method. As an example, the difference between this preparation method and Example 1 is only that the pressing step is omitted, that is, the Y-Gd-Hf-O emission active material doped with Sc2O3 is mixed with a 1.5 wt.% nitrate cotton solution to obtain a uniformly mixed viscous slurry, and the slurry is evenly coated on the prepared W-Re substrate containing W sponge using a micro brush, and then placed under an infrared lamp for drying until the nitrate cotton solvent is completely evaporated, and finally placed in a high-temperature hydrogen furnace for high-temperature sintering at 1350°C for 3 minutes to complete the preparation of the ordinary coated cathode. The test results are as follows: Figure 6 As shown in curve b.

[0049] Figure 6It is a comparative curve of the cathode emission current Ia obtained by different preparation methods with the bombardment time t. a is a curve of the emission current of the cathode obtained by the preparation method of the present invention with the bombardment time, and b is a curve of the emission current of the cathode obtained by the ordinary coating method with the bombardment time. It can be found from the figure that after 72 hours of continuous electron bombardment, the cathode thermal emission current density obtained by the ordinary coating method drops sharply to 58.8% of the initial value, and after 168 hours of continuous bombardment, the emission current remains at 51.8% of the initial value; while for the pressed cathode obtained by the preparation method of the present invention, under 10 W continuous electron bombardment, when the cathode works for 288 hours, the emission current drops to 93.75% of the initial value, and after 480 hours, the emission current can still be maintained at 87.5% of the initial value. In comparison, the electron bombardment resistance of the pressed cathode prepared by the method of the present invention has been greatly improved.

[0050] The cathode obtained by the present invention was subjected to a life test, the cathode operating temperature was 1500-1550°C, and the emission current density Ia was recorded as a function of time t to evaluate the life characteristics of the cathode. The test results are shown in FIG. Figure 7 As shown in Figure 2, during the first 400 h, the cathode emission current remained stable at the initial value of 1 A / cm 2 , indicating that the cathode has good thermal emission stability.

[0051] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a pressed cathode, characterized in that: Tungsten sponge and emission active material are sequentially arranged on the surface of the cathode substrate, and then pressed and sintered; The pressing pressure is 3-4 kN, and the holding time is 30-60 s; The sintering is carried out in a hydrogen atmosphere, and the sintering process is: linearly heating from room temperature to 1300-1350°C at a rate of 40-50°C / min, keeping the temperature for 3-5 minutes, and then slowly cooling down to room temperature in a hydrogen atmosphere; The thickness of the tungsten sponge is controlled to be 0.1-0.2 mm, and the total thickness of the tungsten sponge and the emission active material in the pressed cathode is controlled to be 0.3-0.4 mm; The cathode substrate is made of tungsten or tungsten-rhenium alloy, and the doping amount of rhenium in the tungsten-rhenium alloy is 25wt%; The preparation method further includes pre-annealing the cathode substrate in a hydrogen atmosphere, wherein the annealing is performed in a hydrogen atmosphere, and the specific process is: linearly heating from room temperature to 1300-1350°C at a rate of 40-50°C / min, keeping the temperature for 10-15min, and then slowly cooling to room temperature in a hydrogen atmosphere. The tungsten sponge is specifically provided by spraying a mixed suspension of tungsten powder and nitrate-cotton solution on the surface of the cathode substrate, and then performing heat treatment; the purity of the tungsten powder is 99.9%, the average particle size is 1-3 µm, and the concentration of the nitrate-cotton solution is 0.8-3.0 wt%; the volume ratio of the tungsten powder to the nitrate-cotton solution is 1:(2-4); the heat treatment is performed in a hydrogen atmosphere, and the specific process is: linearly heating from room temperature to 1500-1550°C at a rate of 40-50°C / min, keeping the temperature for 10-15 min, and then slowly cooling to room temperature in a hydrogen atmosphere; The method of setting up the emission active material specifically includes: uniformly applying and impregnating a mixed viscous slurry of the emission active material and the nitrate-cotton solution on the surface of the tungsten sponge, and then pressing it in a mold using a pressure device; the emission active material is Y-Gd-Hf-O, and the Y-Gd-Hf-O is made of Y2O3, Gd2O3 and HfO2 with molar percentages of 45-50%, 5-10% and 50-45% respectively; the Y-Gd-Hf-O is doped with Sc2O3, and the doping amount of Sc2O3 is 3-5 wt%.

2. A pressed cathode prepared by the preparation method according to claim 1.

3. Use of the pressed cathode according to claim 2 in the preparation of a magnetron.

Citation Information

Patent Citations

  • Directly heated cathode and preparation method thereof

    CN105304436A