Method for producing titanium-containing silicon oxide, method for producing epoxide, and titanium-containing silicon oxide
By using a titanium-containing silicon oxide catalyst with a porous structure in the reaction of olefins and hydroperoxides, the problem of low epoxide yield in the existing technology is solved, and the effect of efficiently manufacturing epoxides is achieved.
Patent Information
- Application Number
- CN202080039822.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-04-03
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-04-03
AI Technical Summary
The existing technology has a low yield in the reaction of generating epoxides from olefins and hydroperoxides, and it is difficult to achieve efficient production of epoxides.
A titanium-containing silicon oxide manufacturing method is adopted, by mixing a silicon source, a template agent and a solvent, removing the template agent, performing silylation, and introducing titanium into the system to form a porous structure of a titanium-containing silicon oxide catalyst. , used in the reaction of olefins and hydroperoxides.
A method for producing epoxides with high yield in the reaction of olefins and hydroperoxides is realized, and the production efficiency of epoxides is improved.
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing titanium-containing silicon oxide, a method for producing epoxide from olefin using the titanium-containing silicon oxide produced by the method as a catalyst, and titanium-containing silicon oxide. Background Art
[0002] The method of producing epoxide from hydroperoxide and olefin in the presence of a catalyst is well known. As a catalyst used in this method, for example, Patent Document 1 describes a titanium-containing silicon oxide obtained by the following production method, the production method comprising: a first step of obtaining a solid containing a catalyst component and a template by mixing a silicon source, a titanium source and a template in a liquid state; a second step of removing the template from the solid obtained in the first step by a solvent extraction operation; a third step of replacing the extraction solvent contained in the solid obtained in the second step after the template is removed with a solvent that is substantially inert to the silylating agent used in the fourth step described below; and a fourth step of obtaining a silylated catalyst by subjecting the solid obtained in the third step to a silylation treatment.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2004-195379 Summary of the invention
[0006] Problems to be solved by the invention
[0007] A method for producing epoxides in high yield in the reaction of olefins and hydroperoxides to form epoxides is desired.
[0008] Means used to solve problems
[0009] The present invention relates to the following, but is not limited thereto.
[0010] [Invention 1]
[0011] A method for producing titanium-containing silicon oxide, the method comprising the following steps:
[0012] A step of mixing a silicon source, a template, and a solvent to obtain a solid containing silicon oxide and the template (raw material mixing step);
[0013] a step of removing the template from the solid obtained in the raw material mixing step to obtain a solid containing silicon oxide (template removal step);
[0014] a step of obtaining a solid containing silylated silicon oxide by contacting the solid obtained in the template removal step with a silylating agent (silylation step); and
[0015] A step of introducing titanium into the system (titanium introduction step),
[0016] The template agent is a mixture of a quaternary ammonium compound having a quaternary ammonium ion represented by the following formula I and an amine compound represented by the following formula II,
[0017] [NR 1 R 2 R 3 R 4 ] + I
[0018] (In Formula 1,
[0019] R 1 Represents C 2~36 The hydrocarbon group,
[0020] R 2 , R 3 and R 4 Each independently represents C 1~6 of hydrocarbon groups)
[0021] NR 5 R 6 R 7 II
[0022] (In Formula II,
[0023] R 5 Represents C 2~36 The hydrocarbon group,
[0024] R 6 and R 7 Each independently represents a hydrogen atom or a C 1~6 of hydrocarbon groups)
[0025] The molar ratio of the amine compound to the quaternary ammonium compound is 0.005 to 0.16.
[0026] [Invention 2]
[0027] The method according to Invention 1, wherein R 1 C 10~22 of hydrocarbon groups.
[0028] [Invention 3]
[0029] The method according to claim 1 or 2, wherein R 5 C 10~22 of hydrocarbon groups.
[0030] [Invention 4]
[0031] The method according to any one of Inventions 1 to 3, wherein R 1 With R 5 same.
[0032] [Invention 5]
[0033] The method according to Invention 1, wherein the quaternary ammonium ion is hexadecyltrimethylammonium ion, and the amine compound is hexadecyldimethylamine.
[0034] [Invention 6]
[0035] The method according to any one of Inventions 1 to 5, wherein the molar ratio of the amine compound to the quaternary ammonium compound is 0.01 to 0.13.
[0036] [Invention 7]
[0037] The method according to Invention 6, wherein the molar ratio of the amine compound to the quaternary ammonium compound is 0.04 to 0.13.
[0038] [Invention 8]
[0039] The method according to any one of Inventions 1 to 7, wherein the raw material mixing step is the following step, and the titanium introducing step is carried out in the raw material mixing step:
[0040] A step of mixing a silicon source, a titanium source, a template, and a solvent to obtain a solid containing silicon oxide into which titanium is introduced and the template.
[0041] [Invention 9]
[0042] A titanium-containing silicon oxide, wherein the titanium-containing silicon oxide can be produced by the method according to any one of Inventions 1 to 8.
[0043] [Invention 10]
[0044] A method for producing an epoxide, comprising the step of reacting an olefin with a hydroperoxide in the presence of a titanium-containing silicon oxide that can be produced by the method of any one of Inventions 1 to 8 or the titanium-containing silicon oxide of Invention 9.
[0045] [Invention 11]
[0046] The method according to Invention 10, wherein the olefin is an α-olefin.
[0047] [Invention 12]
[0048] The method according to Invention 10, wherein the olefin is propylene.
[0049] [Invention 13]
[0050] The method according to any one of Inventions 10 to 12, wherein the hydroperoxide is cumene hydroperoxide.
[0051] Effects of the Invention
[0052] According to one embodiment of the present invention, there is provided a method for producing an epoxide in a high yield in a reaction of generating an epoxide from an olefin and a hydroperoxide. DETAILED DESCRIPTION
[0053] definition
[0054] In the present specification, the term "α-olefin" refers to a hydrocarbon having a carbon-carbon unsaturated double bond at the α position.
[0055] In this specification, the term "C X~Y The term "hydrocarbon group" refers to a hydrocarbon group having X to Y carbon atoms.
[0056] In the present specification, the description of “lower limit to upper limit” indicating a numerical range means “more than the lower limit and less than the upper limit.” That is, these descriptions indicate a numerical range including the lower limit and the upper limit.
[0057] A method for producing a titanium-containing silicon oxide according to one embodiment of the present invention includes a raw material mixing step, a template removing step, a silylation step, and a titanium introducing step.
[0058] Silicon oxide containing titanium refers to a compound in which a part of Si in porous silicate (SiO2) is replaced by Ti. This compound has a bond represented by -Si-O-Ti.
[0059] Raw material mixing process
[0060] The raw material mixing step is a step of mixing a silicon source, a template, and a solvent to obtain a solid containing silicon oxide and the template, and is sometimes referred to as step A.
[0061] The “silicon source” refers to silicon oxide and a silicon oxide precursor. The silicon oxide precursor refers to a compound that converts a part or all of the silicon oxide precursor into silicon oxide by reacting the silicon oxide precursor with water.
[0062] As the silicon oxide, amorphous silicon dioxide can be cited. As the silicon oxide precursor, alkoxysilane, alkyltrialkoxysilane, dialkyldialkoxysilane and 1,2-bis(trialkoxysilyl)alkane can be cited. As alkoxysilane, tetramethyl orthosilicate, tetraethyl orthosilicate and tetrapropyl orthosilicate can be cited. As alkyltrialkoxysilane, trimethoxy(methyl)silane can be cited. As dialkyldialkoxysilane, dimethoxydimethylsilane can be cited. As the silicon source, a single silicon source can be used, or a combination of multiple silicon sources can be used.
[0063] When a silicon oxide precursor is used as the silicon source, water is preferably used as part or all of the solvent in step A. When the silicon oxide precursor and water are mixed, part or all of the silicon oxide precursor is converted into silicon oxide.
[0064] The template agent refers to a substance capable of forming a pore structure in the titanium-containing silicon oxide. The template agent is a mixture of a quaternary ammonium compound having a quaternary ammonium ion represented by the following formula I and an amine compound represented by the following formula II.
[0065] [NR 1 R 2 R 3 R 4 ] + I
[0066] (In Formula I, R 1 Represents C 2~36 The hydrocarbon group, R 2 ~R 4 Each independently represents C 1~6 of hydrocarbon groups.)
[0067] NR 5 R 6 R 7 II
[0068] (In Formula II, R 5 Represents C 2~36 The hydrocarbon group, R 6 and R 7 Each independently represents a hydrogen atom or a C 1~6 of hydrocarbon groups.)
[0069] In Formula I, R 1 C 2~36 The hydrocarbon group may be straight-chain or branched, aliphatic or aromatic. 10~22 The hydrocarbon group R 2 ~R 4 Each independently is C 1~6 The hydrocarbon group may be straight chain or branched.2 ~R 4 All are methyl.
[0070] Specific examples of the quaternary ammonium ion represented by formula I include cations such as tetraethylammonium, tetrapropylammonium, tetrabutylammonium, decyltrimethylammonium, dodecyltrimethylammonium, hexadecyltrimethylammonium, octadecyltrimethylammonium, eicosyltrimethylammonium, docosyltrimethylammonium, and benzyltrimethylammonium.
[0071] As specific examples of the compound containing the quaternary ammonium ion represented by Formula I, there can be cited tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, decyltrimethylammonium hydroxide, decyltrimethylammonium chloride, decyltrimethylammonium bromide, dodecyltrimethylammonium hydroxide, dodecyltrimethylammonium chloride, dodecyltrimethylammonium bromide, hexadecyltrimethylammonium hydroxide, hexadecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium hydroxide, octadecyltrimethylammonium chloride, octadecyltrimethylammonium bromide, eicosyltrimethylammonium hydroxide, eicosyltrimethylammonium chloride, eicosyltrimethylammonium bromide, behenyltrimethylammonium hydroxide, behenyltrimethylammonium chloride, and behenyltrimethylammonium bromide.
[0072] In Formula II, R 5 C 2~36 The hydrocarbon group may be straight-chain or branched, aliphatic or aromatic. 10~22 The hydrocarbon group R 6 and R 7 are each independently a hydrogen atom or a C 1~6 The hydrocarbon group may be straight chain or branched. 6 and R 7 It is methyl.
[0073] Specific examples of the amine represented by formula II include ethylamine, propylamine, butylamine, octylamine, nonylamine, decylamine, undecylamine, dodecylamine, tridecylamine, tetradecylamine, pentadecylamine, hexadecylamine, heptadecanamine, octadecylamine, nonadecanylamine, eicosylamine, docosylamine and benzylamine, and methylalkylamines and dimethylalkylamines in which at least one hydrogen atom in these amines is substituted with a methyl group.
[0074] In the above mixture, the molar ratio of the above amine compound to the above quaternary ammonium compound is 0.005 to 0.16. In one embodiment, it may be 0.005 to 0.15, 0.005 to 0.14, 0.005 to 0.13, 0.01 to 0.16, 0.01 to 0.15, 0.01 to 0.14, 0.01 to 0.13, 0.02 to 0.15, 0.02 to 0.14, 0.02 to 0.13, 0.03 to 0.16, 0.03 to 0.15, 0.03 to 0.14, 0.03 to 0.13, 0.04 to 0.16, 0.04 to 0.15, 0.04 to 0.14, or 0.04 to 0.13.
[0075] Examples of methods for adjusting the molar ratio of the amine compound to the quaternary ammonium compound in the mixture include:
[0076] A method for adjusting the mixing ratio of a quaternary ammonium compound and an amine compound;
[0077] A method of converting a portion of the amine compound into a quaternary ammonium compound by reacting the amine compound with an alkylating agent in a mixture of a quaternary ammonium compound and then, if necessary, performing ion exchange to adjust the molar ratio of the amine compound to the quaternary ammonium compound;
[0078] A method of adjusting the molar ratio of the amine compound to the quaternary ammonium compound by subjecting the mixture of the quaternary ammonium compound and the amine compound to distillation, extraction, recrystallization, chromatography, or a combination of two or more of these methods.
[0079] Examples of the alkylating agent include methyl chloride, methyl bromide, and methyl iodide.
[0080] The silicon source and the template are mixed in the presence of a solvent. Examples of the solvent include water and alcohol. Examples of the alcohol include methanol, ethanol, 1-propanol, and 2-propanol. Two or more solvents may also be mixed and used.
[0081] By going through step A, a solid containing silicon oxide and a template can be obtained. Usually, a solvent removal step is included in step A. The obtained solid containing silicon oxide and a template can be extracted by filtration, decantation, drying, centrifugal separation, a combination thereof, and the like. The mixing in step A is preferably carried out at 0°C to 300°C for 30 minutes to 1000 hours. In one embodiment, the mixing can be carried out at 20°C to 100°C, at the boiling point of the solvent, at 20°C to 60°C, or at 20°C to 40°C. In one embodiment, the mixing can be carried out for 30 minutes to 24 hours, or for 2 hours to 24 hours. In addition, stirring can be carried out during the mixing.
[0082] Template removal process
[0083] The template removal step is a step of removing the template from the solid obtained in step A to obtain a solid containing silicon oxide, and is sometimes referred to as step B. By carrying out step B, a solid containing no template or substantially no template can be obtained.
[0084] The content of the template in the solid obtained in step B is preferably 10% by mass or less, more preferably 1% by mass or less.
[0085] The template can be removed by calcining the solid containing the template at 300° C. to 800° C. in air or by solvent extraction. The template is preferably removed by extraction.
[0086] Whitehurst et al. reported a technique for extracting a template using a solvent (see U.S. Patent No. 5143879). The solvent can be any solvent that can dissolve the compound used as the template, and C which is liquid at room temperature can be used. 1~12 or a mixture of two or more of these compounds. Suitable solvents include alcohols, ketones, non-cyclic ethers and cyclic ethers, and esters. Examples of alcohols include methanol, ethanol, ethylene glycol, propylene glycol, 1-propanol, 2-propanol, 1-butanol, and octanol. Examples of ketones include acetone, diethyl ketone, methyl ethyl ketone, and methyl isobutyl ketone. Examples of ethers include diisobutyl ether and tetrahydrofuran. Examples of esters include methyl acetate, ethyl acetate, butyl acetate, and butyl propionate.
[0087] As a solvent, from the viewpoint of the solubility of the template, for example, when the template is a compound containing a quaternary ammonium ion, alcohol is preferred, among which methanol is more preferred. The mass ratio of the solvent to the solid containing the template is generally 1 to 1000, preferably 5 to 300. In order to improve the extraction effect, acids or their salts may be added to these solvents. Examples of the acids used include inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid and hydrobromic acid; or organic acids such as formic acid, acetic acid and propionic acid. Examples of their salts include alkali metal salts, alkaline earth metal salts and ammonium salts. The concentration of the added acid or its salt in the solvent is preferably 30% by mass or less, and more preferably 15% by mass or less.
[0088] As a method for removing the template, there can be cited a method of fully mixing a solvent with a solid containing the template, and then separating the liquid phase by filtering, decantation, drying, centrifugal separation, or a combination thereof. This operation can be repeated multiple times. In addition, the template can also be extracted by filling a solid containing the template into a container such as a column and circulating an extraction solvent. The extraction temperature is preferably 0°C to 200°C, and more preferably 20°C to 100°C. When the boiling point of the extraction solvent is low, the extraction can be performed in a pressurized manner.
[0089] The template in the solution obtained by the extraction treatment can be recovered by ion exchange or the like as necessary and reused as the template in step A. Similarly, the extraction solvent can be purified by a normal distillation operation or the like and reused.
[0090] Silylation process
[0091] The silylation step is a step of obtaining a solid containing silylated silicon oxide by contacting the solid obtained in step B with a silylating agent, and is sometimes referred to as step C. By carrying out step C, the silicon oxide contained in the solid obtained in step B is silylated.
[0092] Silylation can be carried out by a gas phase method in which a gaseous silylating agent is brought into contact with the solid obtained in step B and reacted, or by a liquid phase method in which a silylating agent is brought into contact with the solid in a solvent and reacted. In one embodiment of the present invention, a liquid phase method is more preferred. Generally, when silylation is carried out by a liquid phase method, a hydrocarbon is preferably used as a solvent in step C. When silylation is carried out by a liquid phase method, drying may be performed thereafter.
[0093] The silylating agent is a silicon compound reactive with solids, and a hydrolyzable group is bonded to silicon. Examples of the hydrolyzable group bonded to silicon include hydrogen, halogen, alkoxy, acetoxy, and amino. In the silylating agent, the hydrolyzable group bonded to silicon is preferably one. In addition, at least one group selected from the group consisting of alkyl; alkenyl such as vinyl; aryl such as phenyl; halogenated alkyl and siloxy is bonded to silicon.
[0094] Examples of the silylating agent include organosilanes, organosilylamines, organosilylamides and derivatives thereof, and organosilazanes.
[0095] Examples of the organosilane include chlorotrimethylsilane, dichlorodimethylsilane, chlorobromodimethylsilane, nitrotrimethylsilane, chlorotriethylsilane, iododimethylbutylsilane, chlorodimethylphenylsilane, chlorodimethylsilane, dimethyl-n-propylchlorosilane, dimethylisopropylchlorosilane, tert-butyldimethylchlorosilane, tripropylchlorosilane, dimethyloctylchlorosilane, tributylchlorosilane, trihexylchlorosilane, dimethylethylchlorosilane, dimethyloctadecylchlorosilane, n-butyldimethylchlorosilane, bromomethyldimethylchlorosilane, chloromethyldimethylchlorosilane, 3-chloropropyldimethylchlorosilane, dimethoxymethylchlorosilane, methylphenylchlorosilane, methylphenylvinylchlorosilane, benzyldimethylchlorosilane, diphenylchlorosilane, diphenylmethylchlorosilane, dimethoxy ... Phenylvinylsilyl chloride, tribenzylsilyl chloride, methoxytrimethylsilane, dimethoxydimethylsilane, trimethoxymethylsilane, ethoxytrimethylsilane, diethoxydimethylsilane, triethoxymethylsilane, trimethoxyethylsilane, dimethoxydiethylsilane, methoxytriethylsilane, ethoxytriethylsilane, diethoxydiethylsilane, triethoxyethylsilane, methoxytriphenylsilane, dimethoxydiphenylsilane, trimethoxyphenylsilane, ethoxytriphenylsilane, diethoxydiphenylsilane, triethoxyphenylsilane, dichlorotetramethyldisiloxane, 3-cyanopropyldimethylchlorosilane, 1,3-dichloro-1,1,3,3-tetramethyldisiloxane and 1,3-dimethoxy-1,1,3,3-tetramethyldisiloxane.
[0096] Examples of the organosilylamine include N-(trimethylsilyl)imidazole, N-(tert-butyldimethylsilyl)imidazole, N-(dimethylethylsilyl)imidazole, N-(dimethyl-n-propylsilyl)imidazole, N-(dimethylisopropylsilyl)imidazole, N-(trimethylsilyl)-N,N-dimethylamine, N-(trimethylsilyl)-N,N-diethylamine, N-(trimethylsilyl)pyrrole, N-(trimethylsilyl)pyrrolidine, N-(trimethylsilyl)piperidine, 1-cyanoethyl(diethylamino)dimethylsilane, and pentafluorophenyldimethylsilylamine.
[0097] Examples of the organosilylamides and their derivatives include N,O-bis(trimethylsilyl)acetamide, N,O-bis(trimethylsilyl)trifluoroacetamide, N-(trimethylsilyl)acetamide, N-methyl-N-(trimethylsilyl)acetamide, N-methyl-N-(trimethylsilyl)trifluoroacetamide, N-methyl-N-(trimethylsilyl)heptafluorobutyramide, N-(tert-butyldimethylsilyl)-N-trifluoroacetamide and N,O-bis(diethylhydrogensilyl)trifluoroacetamide.
[0098] Examples of the organosilazane include 1,1,1,3,3,3-hexamethyldisilazane, heptamethyldisilazane, 1,1,3,3-tetramethyldisilazane, 1,3-bis(chloromethyl)-1,1,3,3-tetramethyldisilazane, 1,3-divinyl-1,1,3,3-tetramethyldisilazane, and 1,3-diphenyl-1,1,3,3-tetramethyldisilazane.
[0099] Other examples of the silylating agent include N-methoxy-N,O-bis(trimethylsilyl)trifluoroacetamide, N-methoxy-N,O-bis(trimethylsilyl)carbamate, N,O-bis(trimethylsilyl)aminosulfonate, trimethylsilyl trifluoromethanesulfonate and N,N'-bis(trimethylsilyl)urea.
[0100] The preferred silylating agent is an organosilazane, more preferably 1,1,1,3,3,3-hexamethyldisilazane.
[0101] The silicon oxide-containing solid obtained in step B is silylated by contacting the solid with a silylating agent. It is presumed that at least a portion of the silicon oxide-containing solid is hydrophobized by introducing silyl groups to surface OH groups, but the present invention is not limited to this theory.
[0102] Titanium introduction process
[0103] The titanium introduction step is a step of introducing titanium into the system. The system refers to the reaction system in the method for producing titanium-containing silicon oxide, specifically, before step A, in step A, between step A and step B, in step B, between step B and step C, in step C, and after step C.
[0104] By introducing titanium into the system, silicon oxide is mixed with a titanium source, thereby introducing a bond represented by -Si-O-Ti into silicon oxide.
[0105] Titanium can be introduced into silicon oxide by bringing silicon oxide into contact with a titanium source in a liquid phase, or can be introduced into silicon oxide by bringing a gas containing a titanium source into contact with silicon oxide.
[0106] When mixing is performed in a liquid phase, examples of the solvent include water and alcohol, and for example, the above solvents are used in step A. Examples of the mixing temperature include 0° C. to 60° C. Examples of the mixing time include 1 minute to 24 hours.
[0107] When mixing is performed in the gas phase, the titanium source can be gasified and mixed. The mixing temperature may be, for example, 100° C. to 500° C. The mixing time may be, for example, 1 minute to 24 hours. The mixing may be performed under normal pressure, for example, 10 kPa to 1000 kPa (absolute pressure).
[0108] Titanium may be introduced at any timing before step A, in step A, between step A and step B, in step B, between step B and step C, in step C, and after step C. Titanium may be introduced at two or more of the above timings.
[0109] It is preferred to introduce titanium before starting step C, more preferably at at least one timing selected from the group consisting of before step A, during step A, and between step B and step C, and even more preferably before step A or during step A.
[0110] In the case where titanium is introduced before step A, the titanium source is mixed with the silicon source, the template or the solvent before the mixing in step A.
[0111] When titanium is introduced in step A, a silicon source, a titanium source and a template are mixed in step A.
[0112] Titanium can be introduced after step A is completed and before step B is started by contacting the solid obtained in step A with a titanium source.
[0113] Titanium can be introduced after step B is completed and before step C is started by contacting the solid obtained in step B with a titanium source.
[0114] As titanium sources, there are alkoxytitanium, chelate-type titanium complexes, titanium halides and titanium-containing sulfates. As alkoxytitanium, for example, there are tetramethyl titanate, tetraethyl titanate, tetrapropyl titanate, tetraisopropyl titanate, tetrabutyl titanate, tetraisobutyl titanate, tetra(2-ethylhexyl) titanate and tetra(octadecyl) titanate. As chelate-type titanium complexes, there are acetylacetonato titanium (IV) and diisopropoxy diacetylacetonato titanium (IV). As titanium halides, for example, there are titanium tetrachloride, titanium tetrabromide and titanium tetraiodide. As titanium-containing sulfates, for example, there is titanium oxysulfate.
[0115] Uses of titanium-containing silicon oxides
[0116] The produced titanium-containing silicon oxide can be used as a catalyst for an oxidation reaction of an organic compound, for example, an epoxidation reaction of an olefin, and is particularly preferably used for reacting an olefin with a hydroperoxide to produce an epoxide.
[0117] The olefin used in the epoxidation reaction may be an acyclic olefin, a monocyclic olefin, a bicyclic olefin or a tricyclic or higher polycyclic olefin, or may be a monoolefin, a diolefin or a polyolefin. When the olefin has two or more double bonds in the molecule, these double bonds may be conjugated bonds or non-conjugated bonds. 2~60 Olefins. Olefins may have substituents. Examples of such olefins include ethylene, propylene, 1-butene, isobutylene, 1-hexene, 2-hexene, 3-hexene, 1-octene, 1-decene, styrene and cyclohexene. Olefins may contain substituents containing hydrogen atoms or carbon atoms or both and oxygen atoms, sulfur atoms or nitrogen atoms. Examples of such olefins include allyl alcohol, crotyl alcohol and allyl chloride. Examples of dienes include butadiene and isoprene. Examples of preferred olefins include α-olefins. Examples of particularly preferred olefins include propylene.
[0118] As examples of hydroperoxides, organic hydroperoxides may be mentioned. Organic hydroperoxides are compounds having the formula III.
[0119] ROOH III
[0120] (In Formula III, R is a hydrocarbon group.)
[0121] Organic hydroperoxides react with olefins to form epoxides and hydroxy compounds. R in formula III is preferably C 3~20 The hydrocarbon group is more preferably C 3~10 The organic hydroperoxide may be a straight chain or a branched chain, and may be aliphatic or aromatic. Specific examples of organic hydroperoxides include tert-butyl hydroperoxide, 1-phenylethyl hydroperoxide, and cumene hydroperoxide. Hereinafter, cumene hydroperoxide may be referred to as CMHP.
[0122] When CMHP is used as an organic hydroperoxide, the resulting hydroxy compound is 2-phenyl-2-propanol. The 2-phenyl-2-propanol undergoes a dehydration reaction and a hydrogenation reaction to generate cumene. Hereinafter, cumene is sometimes referred to as CUM. Furthermore, by oxidizing the CUM, CMHP can be obtained again. From this viewpoint, it is preferred to use CMHP as an organic hydroperoxide for epoxidation.
[0123] The epoxidation reaction can be carried out in a liquid phase using a solvent, a diluent or a mixture thereof. The solvent and the diluent must be liquid at the temperature and pressure during the reaction and must be substantially inert to the reactants and the products. When CMHP is subjected to the epoxidation reaction in the presence of CUM as its raw material, CUM may be used as a solvent without adding a solvent in particular.
[0124] The epoxidation reaction temperature is usually 0° C. to 200° C., preferably 25° C. to 200° C. The epoxidation reaction pressure may be a pressure sufficient to keep the reaction phase in a liquid state, and is usually preferably 100 kPa to 10000 kPa.
[0125] After the epoxidation reaction is completed, a liquid mixture containing the desired product can be separated from the catalyst composition. Then, the liquid mixture can be purified by an appropriate method. As the purification method, distillation, extraction, and washing can be listed. The solvent and unreacted olefin can be recycled and reused.
[0126] The reaction using the titanium-containing silicon oxide manufactured by one embodiment of the present invention as a catalyst can be carried out in the form of a slurry or a fixed bed, preferably using a fixed bed in the case of large-scale industrial operation. In the case of using the titanium-containing silicon oxide manufactured by one embodiment of the present invention as a catalyst, it can be a powder or a molded body. In the case of using a fixed bed reaction, the titanium-containing silicon oxide is preferably a molded body. This reaction can be implemented by a batch process, a semi-continuous process or a continuous process.
[0127] [Example]
[0128] Hereinafter, one embodiment of the present invention will be described in further detail by way of examples.
[0129] Example 1
[0130] Raw material mixing process and titanium introduction process
[0131] 1.0 g of hexadecyldimethylamine (CDMA) was added to hexadecyltrimethylammonium hydroxide (CTAH) (the amount of 16% by mass solution was 80.6 g) diluted to a concentration of 16% by mass using a mixed solvent having a mixing ratio (mass ratio) of water:methanol = 72:28, and stirred for 5 minutes to prepare a template solution with a CDMA / CTAH molar ratio of 0.09.
[0132] Under stirring, a mixed solution of 1.5 g of tetraisopropyl titanate and 3.5 g of 2-propanol was added dropwise at room temperature. After the addition was completed, the mixture was stirred for 30 minutes, and then 30 g of tetramethyl orthosilicate was added dropwise under stirring. Then, the mixture was stirred at 40° C. for 90 minutes, and the generated solid was filtered. The obtained solid was dried at 70° C. under reduced pressure to obtain a white solid.
[0133] Hexadecyltrimethylammonium hydroxide and hexadecyldimethylamine are templates, and tetramethyl orthosilicate and tetraisopropyl titanate are silicon sources and titanium sources, respectively.
[0134] Template removal process
[0135] 5 g of the white solid obtained in the raw material mixing step was placed in a flask, and 50 mL of methanol was added, and the mixture was heated and refluxed for 1 hour while stirring, and then naturally cooled and the solid was filtered out.
[0136] A mixed solution of 48 mL of methanol and 2.6 g of concentrated hydrochloric acid aqueous solution (content 36 wt%) was added to the obtained solid, and the mixture was heated under reflux for 1 hour while stirring, cooled naturally, and then the solid was filtered out.
[0137] The same operation was repeated again with respect to the obtained solid using a mixed solution of 49 mL of methanol and 1.3 g of a concentrated aqueous hydrochloric acid solution (content: 36% by weight).
[0138] To the obtained solid was added 50 ml of methanol, and the mixture was stirred at room temperature for 5 minutes, and then the solid was filtered out.
[0139] 50 ml of methanol was added to the obtained solid, and the mixture was heated and refluxed for 1 hour. The mixture was cooled naturally and then the solid was filtered out. The obtained white solid was dried under reduced pressure at 120° C. and 10 mmHg for 1.5 hours.
[0140] Silylation process
[0141] 2 g of the white solid obtained in the template removal step, 1.4 g of hexamethyldisilazane and 20 g of toluene were mixed and heated under reflux for 1.5 hours while stirring. The mixture was cooled naturally and then the solid was filtered out. The obtained solid was washed with 30 g of toluene and dried under reduced pressure at 120° C. and 10 mmHg for 2 hours to obtain a titanium-containing silicon oxide catalyst.
[0142] Synthesis of Propylene Oxide
[0143] 0.10 g of the titanium-containing silicon oxide catalyst prepared as described above, 60 g of a cumene solution containing 25 wt% cumene hydroperoxide (CMHP), and 33 g of propylene were placed in a 200 mL SUS autoclave, and an epoxidation reaction was carried out by a batch reaction at a reaction temperature of 100° C. and a reaction time of 90 minutes, thereby obtaining propylene oxide (PO). The reaction results are shown in Table 1.
[0144] The conversion rate of CMHP and the selectivity of PO were calculated as follows.
[0145] CMHP conversion rate = M2 / M0
[0146] M0: molar amount of raw material CMHP
[0147] M1: The molar amount of CMHP remaining after the reaction
[0148] M2: molar amount of CMHP consumed (=M0-M1)
[0149] · Molar amount of PO generated: M PO (=M2-(M ph +M ac +M pg +2×M dpg +3×M tpg ))
[0150] M ph : The molar amount of phenol produced
[0151] M ac : The molar amount of acetophenone generated
[0152] M pg : The molar amount of propylene glycol produced
[0153] M dpg : The molar amount of dipropylene glycol produced
[0154] M tpg : The molar amount of tripropylene glycol produced
[0155] PO selectivity = M PO / M2
[0156] PO yield = CMHP conversion × PO selectivity
[0157] Example 2
[0158] The same operation as in Example 1 was performed except that the amount of CDMA added in the raw material mixing step and the titanium introducing step was set to 1.5 g to prepare a template solution with a CDMA / CTAH molar ratio of 0.13, thereby obtaining a titanium-containing silicon oxide catalyst.
[0159] Using the titanium-containing silicon oxide catalyst prepared as described above, an epoxidation reaction was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.
[0160] Example 3
[0161] The same operation as in Example 1 was performed except that the amount of CDMA added in the raw material mixing step and the titanium introducing step was set to 0.5 g to prepare a template solution with a CDMA / CTAH molar ratio of 0.04, thereby obtaining a titanium-containing silicon oxide catalyst.
[0162] Using the titanium-containing silicon oxide catalyst prepared as described above, an epoxidation reaction was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.
[0163] Example 4
[0164] The same operation as in Example 1 was performed except that the amount of CDMA added in the raw material mixing step and the titanium introducing step was set to 0.1 g to prepare a template solution with a CDMA / CTAH molar ratio of 0.01, thereby obtaining a titanium-containing silicon oxide catalyst.
[0165] Using the titanium-containing silicon oxide catalyst prepared as described above, an epoxidation reaction was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.
[0166] Comparative Example 1
[0167] The same operation as in Example 1 was performed except that the amount of CDMA added was set to 0 g in the raw material mixing step and the titanium introduction step to prepare a template solution with a CDMA / CTAH molar ratio of 0, thereby obtaining a titanium-containing silicon oxide catalyst.
[0168] Using the titanium-containing silicon oxide catalyst prepared as described above, an epoxidation reaction was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.
[0169] Comparative Example 2
[0170] The same operation as in Example 1 was performed except that the amount of CDMA added in the raw material mixing step and the titanium introducing step was set to 2.1 g to prepare a template solution with a CDMA / CTAH molar ratio of 0.18, thereby obtaining a titanium-containing silicon oxide catalyst.
[0171] Using the titanium-containing silicon oxide catalyst prepared as described above, an epoxidation reaction was carried out in the same manner as in Example 1. The reaction results are shown in Table 1.
[0172] Table 1
[0173] Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 CDMA / CTAH molar ratio in template (-) 0.09 0.13 0.04 0.01 0 0.18 CMHP conversion rate (%) 83.5 76.4 85.8 70.7 63.9 65.5 PO yield (mmol) 81.5 74.8 83.9 69.0 62.7 63.7 PO selection rate (%) 99.0 99.4 99.2 99.0 99.5 98.6 PO yield (%) 82.7 75.9 85.1 70.0 63.6 64.6
[0174] Industrial Applicability
[0175] The method for producing titanium-containing silicon oxide according to one embodiment of the present invention can be applied to the production of a catalyst that can be used in a reaction of producing epoxide from olefin and hydroperoxide. The titanium-containing silicon oxide obtained by this method can be used as a catalyst for producing propylene oxide, for example.
Claims
1. A method for producing titanium-containing silicon oxide, the method comprising the following steps: A step of mixing a silicon source, a template, and a solvent to obtain a solid containing silicon oxide and the template (raw material mixing step); a step of removing the template from the solid obtained in the raw material mixing step to obtain a solid containing silicon oxide (template removal step); a step of obtaining a solid containing silylated silicon oxide by contacting the solid obtained in the template removal step with a silylating agent (silylation step); and A step of introducing titanium into the system (titanium introduction step), The template agent is a mixture of a quaternary ammonium compound having a quaternary ammonium ion and an amine compound. The molar ratio of the amine compound to the quaternary ammonium compound is 0.005 to 0.16, The quaternary ammonium ion is hexadecyltrimethylammonium ion, and the amine compound is hexadecyldimethylamine.
2. The method of claim 1, wherein: The molar ratio of the amine compound to the quaternary ammonium compound is 0.01 to 0.
13.
3. The method of claim 2, wherein: The molar ratio of the amine compound to the quaternary ammonium compound is 0.04 to 0.
13.
4. The method according to any one of claims 1 to 3, wherein: The raw material mixing step is the following step, and the titanium introduction step is implemented in the raw material mixing step: A step of mixing a silicon source, a titanium source, a template, and a solvent to obtain a solid containing silicon oxide into which titanium is introduced and the template.
5. A titanium-containing silicon oxide, wherein: The titanium-containing silicon oxide can be produced by the method according to any one of claims 1 to 4.
6. A method for producing an epoxide, wherein: The method for producing an epoxide comprises the step of reacting an olefin with a hydroperoxide in the presence of a titanium-containing silicon oxide that can be produced by the method according to any one of claims 1 to 4 or the titanium-containing silicon oxide according to claim 5.
7. The method of claim 6, wherein: The olefin is an α-olefin.
8. The method of claim 6, wherein: The olefin is propylene.
9. The method according to any one of claims 6 to 8, wherein: The hydroperoxide is cumene hydroperoxide.
Citation Information
Patent Citations
Method for manufacturing titanium-containing silicon oxide catalyst, and catalyst
JP2004195379A
Method to recover organic templates from freshly synthesized molecular sieves
US5143879A
Catalyst molding body, production method of catalyst molding body thereof, and production method of oxirane compound
JP2001286768A