A long glass fiber reinforced polypropylene composite material, its preparation method and application
By combining specially selected ultra-high strength long glass fibers and ethylene vinyl alcohol copolymers, the solvent resistance problem of long glass fiber reinforced polypropylene composites has been solved, enabling the application of the material in automotive parts.
Patent Information
- Application Number
- CN202111262428.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2041-10-28
AI Technical Summary
Long glass fiber reinforced polypropylene composites have poor solvent resistance, making them difficult to apply in the automotive parts field, especially for parts that need to be in contact with solvents for a long time.
Long glass fiber reinforced polypropylene composite material is prepared by using specially selected ultra-high strength long glass fibers and ethylene-vinyl alcohol copolymer with a specific repeating unit structure, which are mixed by a twin-screw extruder and uniformly dispersed in an impregnation die.
It significantly improves the wettability and dispersibility of long glass fibers with resin, and enhances the solvent resistance and mechanical properties of the material.
Smart Images

Figure 211026162325
Abstract
Description
Technical Field
[0001] This invention relates to the field of polymer materials technology, and in particular to a long glass fiber reinforced polypropylene composite material, its preparation method, and its application. Background Technology
[0002] Long glass fiber reinforced polypropylene (LFT-PP) possesses significant advantages such as low density, high impact resistance, low warpage, fatigue resistance, and excellent creep performance. Its high glass fiber retention length in materials and parts provides the durability and reliability required for structural and functional components, making it widely used in electronics, home appliances, and automobiles. With the increasing urgency and stringent requirements for automotive lightweighting, the performance requirements for components such as fuel tanks, expansion tanks, and water chambers are also rising, particularly regarding creep resistance, heat resistance, and chemical corrosion resistance. Parts around automotive engines, such as water chambers, thermostats, engine covers, and hoods, are in constant contact with solvents like coolant (ethylene glycol) and windshield washer fluid. Currently, glass fiber reinforced nylon is used; however, long glass fiber reinforced polypropylene, due to its superior mechanical properties, offers a promising lightweighting solution.
[0003] However, the poor solvent resistance of long glass fiber reinforced polypropylene composites has long hindered their application in automotive components. Chinese Patent 201910217593X discloses a method for preparing long glass fiber reinforced polypropylene materials, employing a traditional long glass fiber impregnation method where long glass fibers (linear density 2400-2500 tex) are impregnated with resin through an impregnation die. However, this method fails to adequately impregnate the long glass fibers with the resin, thus insufficiently improving the solvent resistance of the long glass fiber reinforced polypropylene composites. Summary of the Invention
[0004] The purpose of this invention is to overcome the above-mentioned technical defects and provide a long glass fiber reinforced polypropylene composite material with the advantages of good solvent resistance and excellent mechanical properties.
[0005] This invention is achieved through the following technical solution: A long glass fiber reinforced polypropylene composite material, comprising the following components by weight: 30-70 parts of homopolymer polypropylene; 1-8 parts of ethylene-vinyl alcohol copolymer; 1-6 parts compatibilizer; 10-70 parts long glass fiber; 0.2-2 parts of auxiliary agent; In the ethylene-vinyl alcohol copolymer segments, the ethylene unit content is 25 mol% to 45 mol%; The long glass fiber is selected from one or more of HMG long glass fiber, S-1 long glass fiber, TM long glass fiber, and S-2 long glass fiber.
[0006] Preferably, the homopolymer polypropylene comprises 40-50 parts, and the long glass fiber comprises 40-60 parts. In the prior art, generally, the higher the glass fiber content, the faster the solvent resistance decreases due to poor wettability. However, in the technical solution of this invention, the solvent resistance only decreases slowly when the long glass fiber content reaches 60 parts, indicating that the ultra-high strength long glass fiber of this invention has good wettability.
[0007] The long glass fiber has an average diameter of 12-20 micrometers, preferably 14-17 micrometers; preferably, the long glass fiber is selected from HMG long glass fiber.
[0008] The long glass fibers listed above are high-strength, alkali-free, continuous glass fibers. They have higher strength than other types of long glass fibers, but they are also more difficult to impregnate.
[0009] The homopolymer polypropylene has a melt index of 10~150g / 10min, under conditions of 230℃ and 2.16kg, and the test standard is ISO 1133.
[0010] Preferably, the ethylene unit content in the ethylene-vinyl alcohol copolymer segment is 30 mol% to 40 mol%.
[0011] The melt index of the ethylene-vinyl alcohol copolymer is 2~5 g / 10 min, the conditions are 210℃, 2.16 kg, and the test standard is ISO 1133; preferably, the melt index of the ethylene-vinyl alcohol copolymer is 3~4 g / 10 min, and the test standard is ISO 1133.
[0012] The compatibilizer is selected from at least one of maleic anhydride-grafted polypropylene, acrylic acid-grafted polypropylene, maleic acid-grafted polypropylene, and glycidyl acrylate-grafted polypropylene, wherein the grafting rate of maleic anhydride, maleic acid, acrylic acid, and glycidyl acrylate is 1-1.5 wt%, the melt index of the compatibilizer is 50-120 g / 10 min, the conditions are 190℃, and the yield is 2.16 kg. The grafting rate can be determined by acid-base titration.
[0013] Preferably, the compatibilizer is selected from maleic anhydride-grafted polypropylene.
[0014] The product also includes 0-2 parts by weight of additives, wherein the additives are selected from one or more of antioxidants, lubricants, and nucleating agents.
[0015] Antioxidants can be combinations of hindered phenolic or phosphite antioxidants.
[0016] Lubricants can be silicones, esters, amides, polyethylenes, stearic acids, fatty acids and esters, etc.
[0017] The nucleating agent is an inorganic nucleating agent with a particle size of less than 1 μm, such as talc, montmorillonite, calcium carbonate, etc.
[0018] The preparation method of the long glass fiber reinforced polypropylene composite material of the present invention involves mixing all components except long glass fibers uniformly according to the formula, performing melt mixing through a twin-screw extruder, and then passing the melt through an impregnation die. The long glass fibers are then passed through a tension dispersion system into the die pre-impregnation system, impregnated in the pre-impregnation die, and then enter the impregnation die. The resin and long glass fibers are uniformly dispersed in the impregnation die, and then extruded and granulated. The extruder temperature is 210-280℃ and the impregnation die temperature is 270-320℃ to obtain the long glass fiber reinforced polypropylene composite material.
[0019] The application of the long glass fiber reinforced polypropylene composite material of the present invention is to prepare automotive interior and exterior trim, industrial fans, and power tool structural parts.
[0020] The present invention has the following beneficial effects: In existing technologies, it is difficult to completely impregnate high-strength long glass fibers with a resin matrix.
[0021] Regarding the formulation, this invention, by specially selecting the type of ultra-high strength long glass fiber and adding ethylene-vinyl alcohol copolymer with a specific repeating unit structure, can significantly improve the wettability and dispersibility of ultra-high strength long glass fiber in homopolymer polypropylene resin matrix, thereby improving the solvent resistance and mechanical properties of long glass fiber reinforced polypropylene composites.
[0022] Regarding the preparation method, the ultra-high strength long glass fiber of the present invention can significantly improve the wettability of the long glass fiber to the resin matrix through dispersion by a tension system and a pre-impregnation system. Attached Figure Description
[0023] Figure 1 Diagram of an electrolyte resistance evaluation device. Detailed Implementation
[0024] The present invention will now be described in detail with reference to specific embodiments. These embodiments will help those skilled in the art to further understand the present invention, but do not limit the invention in any way. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention. These all fall within the scope of protection of the present invention.
[0025] The sources of raw materials used in the examples and comparative examples are as follows: Homopolymer polypropylene A: M60T, Sinopec, 60g / 10min, conditions 230℃, 2.16Kg; Homopolymer polypropylene B: Z30S, Sinopec, 25g / 10min, conditions 230℃, 2.16Kg; Copolymer polypropylene: EP548R, CNOOC Shell, 30g / 10min, conditions 230℃, 2.16Kg; Ethylene-vinyl alcohol copolymer A: ethylene unit content 29 mol%, melt index 3.0 g / 10 min, conditions 210℃, 2.16 kg, commercially available; Ethylene-vinyl alcohol copolymer B: ethylene unit content 32 mol%, melt index 3.7 g / 10 min, conditions 210℃, 2.16 kg, commercially available; Ethylene-vinyl alcohol copolymer C: ethylene unit content 38 mol%, melt index 3.7 g / 10 min, conditions 210℃, 2.16 kg, commercially available; Ethylene-vinyl alcohol copolymer D: ethylene unit content 44 mol%, melt index 4.0 g / 10 min, conditions 210℃, 2.16 kg, commercially available; Ethylene-vinyl alcohol copolymer E: ethylene unit content 35 mol%, melt index 2.3 g / 10 min, conditions 210℃, 2.16 kg, commercially available; Ethylene-vinyl alcohol copolymer F: ethylene unit content 35 mol%, melt index 4.4 g / 10 min, conditions 210℃, 2.16 kg, commercially available; Compatibilizer A: Maleic anhydride-grafted polypropylene, maleic anhydride grafting rate 1wt%, melt index 80g / 10min, conditions 230℃, 2.16Kg; Compatibilizer B: Acrylic acid grafted polypropylene, acrylic acid grafting rate 0.5wt%, melt index 50g / 10min, conditions 230℃, 2.16Kg; Compatibilizer C: Maleic acid-grafted polypropylene, maleic acid grafting rate 1.2wt%, melt index 100g / 10min, conditions 230℃, 2.16Kg; Compatibilizer D: Glycidyl acrylate grafted polypropylene, glycidyl acrylate grafting rate 1wt%, melt index 70g / 10min, conditions 230℃, 2.16Kg. Long glass fiber A-1: HMG838T, with an average diameter of 17 micrometers; Long glass fiber A-2: HMG838T, with an average diameter of 14 micrometers; Long glass fiber A-3: HMG838T, with an average diameter of 12 micrometers; Long glass fiber A-4: HMG838T, with an average diameter of 20 micrometers; Long glass fiber B: S-1 Glass, with an average diameter of 17 micrometers; Long glass fiber C: TM4305, with an average diameter of 17 micrometers; Long glass fiber D:S-2 glass with an average diameter of 14 micrometers; Long glass fiber E: EDR240-T838T, with an average diameter of 17 micrometers.
[0026] Antioxidant: Antioxidant 1010 and Antioxidant 168 are mixed in a 1:1 ratio; Lubricant: Lubricant-A-C540A.
[0027] The preparation method of the long glass fiber reinforced polypropylene composite material in the examples and comparative examples is characterized in that, according to the formula, homopolymer polypropylene, ethylene vinyl alcohol copolymer, compatibilizer and additives are mixed evenly, melt-mixed through a twin-screw extruder, and then the melt is passed through an impregnation die. Long glass fibers are passed through a tension dispersion system into the die pre-impregnation system, impregnated in the pre-impregnation die and then enter the impregnation die. In the impregnation die, the resin and long glass fibers are evenly dispersed, and then extruded and granulated. The extruder heating block has a total of 9 temperature sections, with temperatures of 50 / 180 / 210 / 280 / 280 / 280 / 280 / 280 / 280℃ and a rotation speed of 550 rpm. The impregnation die temperature is 270-320℃, thus obtaining the long glass fiber reinforced polypropylene composite material.
[0028] Various test methods (1) Notched impact strength of simply supported beam: According to ISO179 / 1eA standard, long glass fiber reinforced polypropylene composite material was molded into 4mm thick test strips using an injection molding machine. The notched impact strength of simply supported beam of the test strips was tested at 23℃. (2) Tensile strength: According to ISO527-1 / 2 standard, the long glass fiber reinforced polypropylene composite material was molded into a 4 mm thick test strip using an injection molding machine. The tensile strength of the test strip was measured under the conditions of 23℃ and 5 mm / min test speed. (3) Evaluation of ethylene glycol resistance: Ethylene glycol and deionized water were mixed evenly at a volume ratio of 1:1 and poured into a reaction vessel. The prepared tensile test specimen was placed in the reaction vessel and sealed. The reaction vessel was placed in an aging chamber at 120°C for 1000 hours and the tensile strength retention rate was tested.
[0029] (4) Evaluation of electrolyte resistance: Prepare a 35wt% sulfuric acid solution by mixing concentrated sulfuric acid with deionized water, and put the sulfuric acid solution into a container. Place the prepared tensile test specimen into the device shown in the attached figure of the instruction manual, heat it at 70°C for 24 hours, and test the retention rate of tensile strength performance.
[0030] Table 1: Examples 1-8 Long Glass Fiber Polypropylene Composite Materials (parts by weight) and Test Results Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 Example 7 Example 8 Homopolymer Polypropylene A 60 60 60 60 70 50 40 30 Ethylene-vinyl alcohol copolymer A 3 3 3 3 1 5 7 8 Compatibilizer A 3 3 3 3 1 4 5 6 Long glass fiber A-1 30 10 40 60 70 Long glass fiber A-2 30 Long glass fiber A-3 30 Long glass fiber A-4 30 antioxidants 0.8 0.8 0.8 0.8 0.8 0.8 0.8 0.8 lubricant 0.3 0.3 0.3 0.3 0.3 0.3 0.3 0.3 <![CDATA[Notched impact strength of simply supported beam, kJ / m 2 > 38 38 36 35 18 40 42 40 Tensile strength, MPa 138 138 131 130 80 150 145 142 Ethylene glycol tensile strength retention rate, % 94.3 94.8 93.6 93.5 92.8 95.7 95.6 93.8 Electrolyte resistance tensile strength retention rate, % 98.3 98.7 97.5 97.4 96.8 99.3 99.2 97.9 As can be seen from Examples 1-4, the preferred average diameter of ultra-high strength long glass fiber is 14-17 micrometers.
[0031] As can be seen from Examples 1 / 5 / 6 / 7 / 8, the optimal ratio of homopolymer polypropylene to long glass fiber results in the best mechanical properties and also good solvent resistance.
[0032] Table 2: Examples 9-11 Long Glass Fiber Polypropylene Composite Materials (parts by weight) and Test Results Example 9 Example 10 Example 11 Homopolymer Polypropylene A 60 60 60 Ethylene-vinyl alcohol copolymer A 3 3 3 Compatibilizer A 3 3 3 Long glass fiber B 30 Long glass fiber C 30 Long glass fiber D 30 antioxidants 0.8 0.8 0.8 lubricant 0.3 0.3 0.3 <![CDATA[Notched Izod impact strength, kJ / m 2 > 37 38 35 Tensile strength, MPa 135 138 139 Ethylene glycol tensile strength retention rate, % 93.5 93.2 93.9 Electrolyte resistance tensile strength retention rate, % 96.1 97.2 95.8 As can be seen from Examples 1 / 2 / 9 / 10 / 11, HMG glass fiber is preferred, as its better compatibility results in better overall mechanical properties and solvent resistance.
[0033] Table 2: Examples 12-14 Long Glass Fiber Polypropylene Composite Materials (parts by weight) and Test Results Example 12 Example 13 Example 14 Homopolymer Polypropylene A 60 60 60 Ethylene-vinyl alcohol copolymer A 3 3 3 Compatibilizer B 3 Compatibilizer C 3 Compatibilizer D 3 Long glass fiber A 30 30 30 antioxidants 0.8 0.8 0.8 lubricant 0.3 0.3 0.3 <![CDATA[Notched Izod impact strength, kJ / m 2 > 36 34 33 Tensile strength, MPa 136 136 132 Ethylene glycol tensile strength retention rate, % 93.7 93.5 93.2 Electrolyte resistance tensile strength retention rate, % 97.8 97.4 97.1 As can be seen from Examples 1 / 12 / 13 / 14, maleic anhydride-grafted polypropylene compatibilizer is preferred.
[0034] Table 3: Examples 15-21 Long Glass Fiber Polypropylene Composite Materials (parts by weight) and Test Results Example 15 Example 16 Example 17 Example 18 Example 19 Example 20 Homopolymer Polypropylene A 60 60 60 60 60 Homopolymer polypropylene B 60 Ethylene-vinyl alcohol copolymer B 3 3 Ethylene-vinyl alcohol copolymer C 3 Ethylene-vinyl alcohol copolymer D 3 Ethylene-vinyl alcohol copolymer E 3 Ethylene-vinyl alcohol copolymer F 3 Compatibilizer A 3 3 3 3 3 3 Long glass fiber A 30 30 30 30 30 30 antioxidants 0.8 0.8 0.8 0.8 0.8 0.8 lubricant 0.3 0.3 0.3 0.3 0.3 0.3 <![CDATA[Notched Izod impact strength, kJ / m 2 > 38 39 34 37 37 36 Tensile strength, MPa 139 140 134 137 136 137 Ethylene glycol tensile strength retention rate, % 95.2 94.8 94.1 94.7 95.0 95.5 Electrolyte resistance tensile strength retention rate, % 98.7 98.9 97.5 97.9 97.4 98.8 As can be seen from Examples 1 / 15-19, the preferred ethylene-vinyl alcohol copolymer has an ethylene unit content of 30mol%~40mol% and a melt index of 3-4g / 10min.
[0035] Table 4: Comparative Long Glass Fiber Polypropylene Composites (parts by weight) and Test Results Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Homopolymer Polypropylene A 60 60 60 Copolymer polypropylene 60 Ethylene-vinyl alcohol copolymer A 1 10 1 Compatibilizer A 1 1 1 1 Long glass fiber A 10 10 10 Long glass fiber E 10 antioxidants 0.8 0.8 0.8 0.8 lubricant 0.3 0.3 0.3 0.3 <![CDATA[Notched impact strength of simply supported beam, kJ / m 2 > 15 17 15 18 Tensile strength, MPa 73 79 74 76 Ethylene glycol tensile strength retention rate, % 90.5 90.0 92.4 92.0 Electrolyte resistance tensile strength retention rate, % 92.2 92.4 91.9 93.2 As can be seen from Comparative Example 1, ordinary glass fiber has low strength and insufficient resistance to ethylene glycol and electrolyte.
[0036] As can be seen from Comparative Example 2 / 3, the ethylene-vinyl alcohol copolymer is the key to this invention, and adding too much will reduce the strength and resistance to ethylene glycol and electrolyte.
[0037] As can be seen from Comparative Example 4, copolymer polypropylene cannot achieve the technical effects of the present invention.
Claims
1. A long glass fiber reinforced polypropylene composite material, characterized in that, By weight, it includes the following components: 30-60 parts of homopolymer polypropylene; 3-8 parts of ethylene-vinyl alcohol copolymer; 1-6 parts compatibilizer; 30-70 parts long glass fiber; 0.2-2 parts of auxiliary agent; The ethylene-vinyl alcohol copolymer segments contain 30 mol% to 40 mol% ethylene units. The long glass fiber is selected from one or more of HMG long glass fiber, S-1 long glass fiber, TM long glass fiber, and S-2 long glass fiber, and the average diameter of the long glass fiber is 12-20 micrometers. The ethylene-vinyl alcohol copolymer has a melt index of 2~5 g / 10 min, under the conditions of 210℃ and 2.16 kg, and the test standard is ISO 1133; The compatibilizer is selected from at least one of maleic anhydride-grafted polypropylene, acrylic acid-grafted polypropylene, maleic acid-grafted polypropylene, and glycidyl acrylate-grafted polypropylene, wherein the grafting rate of maleic anhydride, acrylic acid, maleic acid, and glycidyl acrylate is 0.5-1.5 wt%, and the melt index of the compatibilizer is 50-120 g / 10 min at 190 °C for 2.16 kg.
2. The long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that, 40-50 parts homopolymer polypropylene, 40-60 parts long glass fiber.
3. The long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that, The long glass fiber has an average diameter of 14-17 micrometers; the long glass fiber is selected from HMG long glass fiber.
4. The long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that, The homopolymer polypropylene has a melt index of 10~150g / 10min, under conditions of 230℃ and 2.16kg, and the test standard is ISO 1133.
5. The long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that, The melt index of the ethylene-vinyl alcohol copolymer is 3~4 g / 10min, the test standard is ISO 1133, and the conditions are 210℃ and 2.16 kg.
6. The long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that, The compatibilizer is selected from maleic anhydride-grafted polypropylene.
7. The long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that, The additives are selected from one or more of antioxidants, lubricants, and nucleating agents.
8. The method for preparing the long glass fiber reinforced polypropylene composite material according to any one of claims 1-7, characterized in that, According to the formula, all components except long glass fibers are mixed evenly and melt-blended using a twin-screw extruder. The melt is then passed through an impregnation die, while the long glass fibers are introduced into the die pre-impregnation system via a tension dispersion system. After being impregnated in the pre-impregnation die, the melt and long glass fibers are evenly dispersed in the impregnation die. The mixture is then extruded and granulated. The extruder temperature is 210-280℃ and the impregnation die temperature is 270-320℃ to obtain a long glass fiber reinforced polypropylene composite material.
9. The application of the long glass fiber reinforced polypropylene composite material according to any one of claims 1-7, characterized in that, Used in the manufacture of automotive interior and exterior trim, industrial fans, and power tool structural components.
Citation Information
Patent Citations
Polypropylene composite with low crystallinity
CN102329453A
Long glass fiber reinforced polypropylene material with failing ball impact resistance and good appearance as well as preparation method and application of long glass fiber reinforced polypropylene material
CN109370062A
Low-agglomeration long glass fiber reinforced polypropylene composite material for automotive trim and preparation method of low-agglomeration long glass fiber reinforced polypropylene composite material