Liquid crystal alignment agent, liquid crystal alignment film and liquid crystal element

By using polymers [A], polymers [B] and polymers [C] of specific structures, the peeling and afterimage problems of liquid crystal orientation film and substrate are solved, and high adhesion and low afterimage effects of liquid crystal components are achieved.

CN114058381BActive Publication Date: 2024-11-01JICC 02 LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110807875.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-07-29
Filing Date
2021-07-16
Publication Date
2024-11-01
Estimated Expiration
2041-07-16

AI Technical Summary

Technical Problem

When the liquid crystal element is narrowly framed, the liquid crystal alignment film is easily peeled from the substrate, and the polymer containing the interarylene structure causes the liquid crystal alignment film to become hard and fragile, making it difficult to satisfy both residual image reduction, substrate adhesion and sealing. Adhesiveness requirements.

Method used

Using a variety of polymers with different structures, including polymers [A], polymers [B] and polymers [C], a liquid crystal alignment agent is formed through specific partial structural design to improve the liquid crystal alignment film, sealant and substrate. and reduce afterimage.

Benefits of technology

The excellent adhesion between the liquid crystal alignment film and the sealant and the substrate is achieved, the afterimage of the liquid crystal element is reduced, and the reliability and performance of the liquid crystal element are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114058381B_ABST
    Figure CN114058381B_ABST
Patent Text Reader

Abstract

The present invention provides a liquid crystal alignment agent, a liquid crystal alignment film and a liquid crystal element. The liquid crystal alignment agent comprises: a polymer [A] having a partial structure represented by formula (1); a polymer [B] having a partial structure represented by formula (2); and a polymer [C] having a partial structure X in the main chain. Partial structure X: -(CH2) a ‑The structure represented by or in ‑(CH2) a Any methylene group in the structure represented by ‑NR 7 In formula (1), R 1 In formula (2), A 1 and A 4 are each independently a divalent aromatic ring group. 2 and R 3 are independently a hydrogen atom or a monovalent organic group. 1 is a single bond, ‑NR 4 ‑, ‑O‑ or a divalent aromatic heterocyclic group. #imgabs0#
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a liquid crystal alignment agent, a liquid crystal alignment film and a liquid crystal element. Background Art

[0002] As the liquid crystal material of the liquid crystal element, negative liquid crystal is used in liquid crystal elements of vertical alignment (VA) drive mode or multi-domain vertical alignment (MVA) drive mode, and positive liquid crystal is used in liquid crystal elements of twisted nematic (TN) type or in-plane switching (IPS) drive mode, fringe field switching (FFS) drive mode, etc. In addition, in recent years, in order to achieve further high-precision liquid crystal elements, it has also been proposed to use negative liquid crystal in liquid crystal elements of IPS drive mode or FFS drive mode (for example, refer to patent document 1).

[0003] In recent years, liquid crystal elements are used in a wide range of applications, from relatively large display devices such as liquid crystal televisions or information displays to small display devices such as smart phones. With the versatility of such liquid crystal elements, further high quality of liquid crystal elements is required. Therefore, it has been previously proposed that a liquid crystal alignment agent contains a polymer having a nitrogen-containing meta-arylene structure, thereby obtaining a liquid crystal alignment film with low resistance and high transparency, and obtaining a liquid crystal element with less burn marks (direct current (DC) afterimage) caused by accumulated charge (for example, refer to patent document 2).

[0004] In a touch screen display device represented by a smart phone or a tablet-type personal computer (PC), in order to further expand the operating area of ​​the touch screen and take into account the miniaturization of the display device, an attempt is made to achieve a narrow frame. As one of the methods for achieving a narrow frame, the following method is known: a liquid crystal alignment film is formed on the entire substrate surface, a sealant is applied to the liquid crystal alignment film, and the substrates are bonded to each other (for example, refer to Patent Document 3).

[0005] [Prior art literature]

[0006] [Patent Document]

[0007] [Patent Document 1] International Publication No. 2016 / 152928

[0008] [Patent Document 2] International Publication No. 2019 / 093037

[0009] [Patent Document 3] Japanese Patent Application Publication No. 2013-109154 Summary of the invention

[0010] [Problems to be solved by the invention]

[0011] When a sealant is disposed on a liquid crystal alignment film for the purpose of achieving a narrow frame of a liquid crystal element, the liquid crystal alignment film tends to be easily peeled off from the substrate at the sealant portion. This may cause a decrease in the reliability of the liquid crystal element.

[0012] In addition, when the residual image of the liquid crystal element is reduced by introducing a meta-arylene structure into a polymer as in the technology of Patent Document 2, the liquid crystal alignment film becomes hard and brittle due to the structure containing a large number of aromatic rings derived from the meta-arylene structure, and there is a concern that the adhesion between the liquid crystal alignment film and the substrate (especially the adhesion between the spacer portion and the substrate) will be reduced. On the other hand, it is difficult to simultaneously meet multiple characteristics such as the reduction of residual images, adhesion to the substrate, and adhesion to the sealant, and there is room for further improvement of the liquid crystal alignment agent.

[0013] The present invention has been made in view of the above-mentioned problems, and a main object thereof is to provide a liquid crystal aligning agent which can form a liquid crystal aligning film having excellent adhesion to a sealant and a substrate and can obtain a liquid crystal element in which an afterimage is less likely to occur.

[0014] [Technical means to solve the problem]

[0015] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that the above-mentioned problems can be solved by using a plurality of polymers having different structures, thereby completing the present invention. Specifically, the present invention provides the following means.

[0016] <1> A liquid crystal alignment agent, comprising:

[0017] The polymer [A] has a partial structure represented by the following formula (1) and does not have a partial structure represented by the following formula (2); the polymer [B] has a partial structure represented by the following formula (2); and the polymer [C] has the following partial structure X in the main chain and does not have the partial structure represented by the following formula (1) and the partial structure represented by the following formula (2).

[0018] Partial structure X: -(CH 2 ) a - (wherein a is an integer of 2 to 20), or in -(CH 2 ) a Any methylene group in the structure represented by - is selected from -NR 7 -、-O-、-COO-、-NR 7 -CO-、-NR 7-COO-, -NR 8 -CO-NR 9 - and a structure formed by substitution with at least one group selected from the group consisting of nitrogen-containing non-aromatic heterocyclic groups (wherein R 7 is a hydrogen atom or an alkyl group; R 8 and R 9 are independently a hydrogen atom or an alkyl group, or represent R 8 With R 9 Combined with R 8 The nitrogen atom to which it is bonded, R 9 The nitrogen atom and -CO- form a ring structure; -NR 7 -、-O-、-COO-、-NR 7 -CO-、-NR 7 -COO-, -NR 8 -CO-NR 9 - and nitrogen-containing non-aromatic heterocyclic groups are not adjacent to each other).

[0019] [Chemistry 1]

[0020]

[0021] (In formula (1), R 1 is a protecting group; "*" indicates a bonding bond)

[0022] [Chemistry 2]

[0023]

[0024] (In formula (2), A 1 and A 4 are independently a divalent aromatic ring group; R 2 and R 3 are independently a hydrogen atom or a monovalent organic group; 1 is a single bond, -NR 4 -, -O- or a divalent aromatic heterocyclic group; R 4 is a hydrogen atom or a monovalent organic group; in B 1 In the case of a single bond, A 2 A is a divalent aromatic ring group, 3 is a single bond or a divalent aromatic ring group; in B 1 When A is a divalent aromatic heterocyclic group, 2 and A 3 are independently a single bond or a divalent aromatic ring group; in B 1 For-NR 4 - or -O-, A 2 and A 3 are independently a divalent aromatic ring group, or represent A 2The aromatic ring and A 3 The aromatic rings are connected by single bonds or chain structures to -NR 4 - or -O- together to form a nitrogen or oxygen-containing condensed ring structure; "*" indicates a bonding bond)

[0025] <2> A liquid crystal alignment film formed from the liquid crystal alignment agent according to <1>.

[0026] <3> A liquid crystal alignment film comprising: a structural unit having a partial structure represented by the following formula (1A) in a part different from a group participating in polymerization, and a polymer having no partial structure represented by the following formula (2); a polymer having a partial structure represented by the following formula (2); and a polymer having the following partial structure X in the main chain and having no partial structure represented by the following formula (2).

[0027] [Chemistry 3]

[0028]

[0029] (In formula (1A), "*" represents a bonding bond)

[0030] <4> A liquid crystal element comprising the liquid crystal alignment film according to <2> or <3>.

[0031] [Effects of the Invention]

[0032] According to the liquid crystal alignment agent of the present invention, a liquid crystal alignment film having excellent adhesion to a sealant and a substrate can be formed and a liquid crystal element having less prone to residual images can be obtained. In particular, according to the liquid crystal alignment agent of the present invention, the adhesion between the substrate and the liquid crystal alignment film at the portion where the spacer is arranged can be improved. DETAILED DESCRIPTION

[0033] The liquid crystal aligning agent of the present disclosure contains three polymers having different monomer compositions, namely, polymer [A], polymer [B], and polymer [C]. Hereinafter, each component contained in the liquid crystal aligning agent of the present disclosure and other components arbitrarily prepared as needed will be described.

[0034] In addition, in this specification, "hydrocarbon group" means a chain hydrocarbon group, an alicyclic hydrocarbon group and an aromatic hydrocarbon group. The so-called "chain hydrocarbon group" refers to a straight-chain hydrocarbon group and a branched hydrocarbon group that does not contain a cyclic structure in the main chain and is only composed of a chain structure. Among them, it can be saturated or unsaturated. The so-called "alicyclic hydrocarbon group" refers to a hydrocarbon group that only contains an alicyclic hydrocarbon structure as a ring structure and does not contain an aromatic ring structure. Among them, it is not necessary to be composed only of an alicyclic hydrocarbon structure, and a group having a chain structure in a part thereof is also included. The so-called "aromatic hydrocarbon group" refers to a hydrocarbon group containing an aromatic ring structure as a ring structure. Among them, it is not necessary to be composed only of an aromatic ring structure, and a chain structure or an alicyclic hydrocarbon structure may also be included in a part thereof. "Aromatic ring" means an aromatic hydrocarbon ring and an aromatic heterocycle. The so-called "structural unit" refers to a unit that mainly constitutes the main chain structure, and is a unit that contains at least two or more in the main chain structure. As for each component and each compound, as long as it is not specifically mentioned, one can be used alone, or two or more can be used in combination. The term "protecting group" refers to an atomic group that temporarily replaces a highly reactive characteristic group (-NH- in the following formula (1)) with an inert functional group.

[0035] <Polymer [A]>

[0036] The polymer [A] is a polymer having a partial structure represented by the following formula (1).

[0037] [Chemistry 4]

[0038]

[0039] (In formula (1), R 1 is a protecting group; "*" indicates a bonding bond)

[0040] In the formula (1), R 1 The protecting group of is preferably a monovalent group that is detached by heat, and examples thereof include carbamate protecting groups, amide protecting groups, imide protecting groups, and sulfonamide protecting groups. Among these, R 1 Preferably, it is a carbamate-based protecting group. Specific examples of the protecting group include: tert-butoxycarbonyl (Boc group), benzyloxycarbonyl, 1,1-dimethyl-2-haloethoxycarbonyl, allyloxycarbonyl (Alloc group), 2-(trimethylsilyl)ethoxycarbonyl, 9-fluorenylmethoxycarbonyl (F-moc group), etc. Among these, tert-butoxycarbonyl is particularly preferred in terms of excellent heat-induced detachability, improved adhesion to the sealant, and reduced residual amount in the film of the deprotected portion.

[0041] In addition, in the formula (1), one of the two "*" may be bonded to a hydrogen atom. That is, one of the two "*" in the formula (1) may be bonded to a hydrogen atom and the other may be bonded to a carbon atom. Alternatively, both of the two "*" may be bonded to a carbon atom.

[0042] The polymer [A] preferably has the partial structure represented by the formula (1) and the following partial structure Y. When the polymer [A] further has the partial structure Y, in addition to the DC afterimage, the generation of the alternating current (AC) afterimage caused by the deviation of the orientation direction of the liquid crystal from the initial orientation can be suppressed, which is preferred in this respect.

[0043] Partial structure Y: -(CH 2 ) b - (wherein b is an integer of 2 to 20), or in -(CH 2 ) b Any methylene group in the structure represented by - is selected from -NR 10 -、-O-、-COO-、-NR 10 -CO-、-NR 10 -COO-, -NR 10 -CO-NR 11 - and a structure formed by substitution with at least one group selected from the group consisting of nitrogen-containing non-aromatic heterocyclic groups (wherein R 10 and R 11 are independently a hydrogen atom or a monovalent organic group; in the partial structure Y, -NR 10 -、-O-、-COO-、-NR 10 -CO-、-NR 10 -COO-, -NR 10 -CO-NR 11 - and nitrogen-containing non-aromatic heterocyclic groups are not adjacent to each other).

[0044] From the perspective of improving the effect of reducing AC afterimages in the liquid crystal element, b in the partial structure Y is preferably 2 or more, and more preferably a linear alkanediyl group having 2 or more carbon atoms is included in the partial structure Y. From the perspective of suppressing a decrease in film strength, b is preferably 12 or less, and more preferably 10 or less.

[0045] In R 10 , R 11 In the case of a monovalent organic group, the monovalent organic group is preferably a monovalent hydrocarbon group having 1 to 10 carbon atoms or a protecting group. The monovalent hydrocarbon group is preferably an alkyl group having 1 to 3 carbon atoms or a phenyl group, and more preferably an alkyl group having 1 to 3 carbon atoms. Examples and preferred examples of the protecting group include R 1 .

[0046] In the above, R 10 , R 11 It is preferably a hydrogen atom, an alkyl group having 1 to 3 carbon atoms, or a tert-butoxycarbonyl group.

[0047] Examples of the nitrogen-containing non-aromatic heterocyclic group include piperidine-1,4-diyl and piperazine-1,4-diyl.

[0048] The polymer [A] may have the partial structure represented by the formula (1) independently of the partial structure Y, or may have the partial structure represented by the formula (1) in the partial structure Y. When the partial structure Y has the partial structure represented by the formula (1), the polymer [A] has the following structure as the partial structure Y: 2 ) b Any methylene group in the structure represented by - is selected from -NR 10 -、-NR 10 -CO-、-NR 10 -COO- and -NR 10 -CO-NR 11 - a structure formed by substitution of at least one group in the group consisting of, and R 10 and R 11 In the case where the partial structure Y is a structure having a protective group, it is preferred to use a monomer having the partial structure Y when manufacturing the polymer [A], thereby improving the adhesion to the sealant and reducing the AC residual image at the same time. In terms of improving the effect of reducing the AC residual image of the liquid crystal element, the polymer [A] preferably has the partial structure Y in the main chain. The polymer [A] does not have the partial structure represented by the following formula (2) that the polymer [B] has.

[0049] In addition, in this specification, the other polymer "does not have" a partial structure possessed by at least one polymer among the multiple polymers contained in the liquid crystal alignment agent (hereinafter referred to as "specific structure") means that the other polymer is allowed to have the specific structure within the scope that does not impair the effect of the present invention. When the other polymer does not have a specific structure, the content of the specific structure in the other polymer is preferably 1 mol% or less, more preferably 0.5 mol% or less, and further preferably 0.1 mol% or less relative to all structural units possessed by the other polymer (the same applies to polymer [B] and polymer [C]).

[0050] The main chain of polymer [A] is not particularly limited. From the perspective of being able to form a liquid crystal alignment film having high affinity with liquid crystals, high mechanical strength and high reliability, and being easy to introduce the partial structure represented by formula (1) into the polymer, polymer [A] is preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide.

[0051] The method for manufacturing polymer [A] is not particularly limited and can be carried out according to conventional methods of organic chemistry. Specifically, for example, there can be cited: a method of polymerizing using a monomer having a partial structure represented by the formula (1); a method of introducing the partial structure represented by the formula (1) into the polymer terminal by reacting the polymer terminal with a compound having a partial structure represented by the formula (1), etc. Among these, in terms of further improving the adhesion between the liquid crystal alignment film and the sealant, it is preferred to manufacture polymer [A] by polymerization using a monomer having a partial structure represented by the formula (1). That is, polymer [A] is preferably a polymer having a structural unit derived from the following monomer, wherein the monomer has a partial structure represented by the formula (1).

[0052] In addition, the so-called "main chain" refers to the part of the "trunk" containing the longest atomic chain in the polymer. The part of the "trunk" is allowed to contain a ring structure. For example, the so-called "having a specific structure in the main chain" means that the specific structure constitutes a part of the main chain. The so-called "side chain" refers to the part branching from the "trunk" of the polymer.

[0053] (Polyamic acid)

[0054] When the polymer [A] is a polyamic acid, the polyamic acid (hereinafter also referred to as "polyamic acid [A]") is preferably produced by a method of reacting tetracarboxylic dianhydride with a diamine compound containing a diamine having a partial structure represented by the formula (1) (hereinafter also referred to as "specific diamine (A)") from the perspective of high freedom in monomer selection and easy introduction of the partial structure represented by the formula (1).

[0055] Tetracarboxylic dianhydride

[0056] Examples of tetracarboxylic dianhydrides used in the synthesis of polyamic acid [A] include aliphatic tetracarboxylic dianhydrides, alicyclic tetracarboxylic dianhydrides, and aromatic tetracarboxylic dianhydrides. Specific examples of these include aliphatic tetracarboxylic dianhydrides such as 1,2,3,4-butanetetracarboxylic dianhydride and ethylenediaminetetraacetic dianhydride; alicyclic tetracarboxylic dianhydrides include 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,3-dimethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 2,3,5-tricarboxycyclopentylacetic dianhydride, 5-(2,5-dioxotetrahydrofuran-3-yl)-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, 5-(2,5-dioxotetrahydrofuran-3-yl)-8-methyl-3a,4,5,9b-tetrahydronaphtho[1,2-c]furan-1,3-dione, and 1,2,3,4-cyclobutanetetracarboxylic dianhydride. 2-c] furan-1,3-dione, 2,4,6,8-tetracarboxybicyclo[3.3.0]octane-2:4,6:8-dianhydride, cyclopentanetetracarboxylic dianhydride, cyclohexanetetracarboxylic dianhydride, etc.; aromatic tetracarboxylic dianhydride includes pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, ethylene glycol ditrimellitate anhydride, 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 4,4'-carbonyldiphthalic anhydride, etc. In addition, tetracarboxylic dianhydrides described in Japanese Patent Laid-Open No. 2010-97188 can also be used.

[0057] In terms of obtaining a liquid crystal alignment film having high solubility in a solvent and exhibiting low residual image characteristics, the tetracarboxylic dianhydride used in the synthesis of the polyamic acid [A] preferably contains alicyclic tetracarboxylic dianhydride. The proportion of alicyclic tetracarboxylic dianhydride used relative to the total amount of tetracarboxylic dianhydride used in the synthesis of the polyamic acid [A] is preferably 20 mol% or more, more preferably 40 mol% or more, and further preferably 50 mol% or more.

[0058] ·Diamine compounds

[0059] The specific diamine (A) used for synthesis of the polymer [A] is preferably a compound represented by the following formula (1-1).

[0060] [Chemistry 5]

[0061]

[0062] (In formula (1-1), A 7 and A 8 are independently a divalent aromatic ring group; Y 1 is a divalent organic group; r is 0 or 1; wherein, when r is 1, A 7 , A 8 and Y 1 At least one of them has a partial structure represented by the formula (1); when r is 0, A7 having a partial structure represented by the formula (1)

[0063] In the formula (1-1), A 7 and A 8 The divalent aromatic ring group may be a divalent aromatic hydrocarbon group or a divalent aromatic heterocyclic group. 7 and A 8 The aromatic ring portion may have a substituent. Examples of the substituent include an alkyl group having 1 to 5 carbon atoms, a halogen atom, and a monovalent group having a partial structure represented by the formula (1).

[0064] As A 7 , A 8 Preferred specific examples of divalent aromatic hydrocarbon groups include groups formed by removing any two hydrogen atoms bonded to carbon atoms constituting a benzene ring, naphthalene ring or anthracene ring; and divalent aromatic heterocyclic groups include groups formed by removing any two hydrogen atoms bonded to carbon atoms constituting a pyridine ring, pyrimidine ring, pyridazine ring or pyrazine ring. Among these, A 7 , A 8 Preferred is a substituted or unsubstituted phenylene group, biphenylene group or pyridylene group.

[0065] As Y 1 The divalent organic group includes: -(CH 2 ) b -The structure represented by -(CH 2 ) b Any methylene group in the structure represented by - is selected from -NR 10 -、-O-、-COO-、-NR 10 -CO-、-NR 10 -COO-, -NR 10 -CO-NR 11 - and a structure in which at least one group selected from the group consisting of nitrogen-containing non-aromatic heterocyclic groups is substituted, -NR 10 -、-NR 10 -CO-、-NR 10 -COO-, -NR 10 -CO-NR 11 - etc. Among these, Y 1 Preferably in -(CH 2 ) b Any methylene group in the structure represented by - is selected from -NR 10 -、-NR 10 -CO-、-NR 10 -COO- and -NR 10 -CO-NR 11- a structure formed by substitution of at least one group in the group consisting of 10 and R 11 When both of them are different from the protecting group, A 7 and A 8 At least one of them preferably has a partial structure represented by the formula (1) as a substituent introduced into the aromatic ring. 1 It does not have an aromatic ring group.

[0066] r is 0 or 1, and more preferably 1.

[0067] As a specific example of a specific diamine (A), the compound etc. which are each represented by following formula (DA-1) - formula (DA-12) are mentioned.

[0068] [Chemistry 6]

[0069]

[0070] [Chemistry 7]

[0071]

[0072] (wherein, "Boc" represents tert-butoxycarbonyl; "Alloc" represents allyloxycarbonyl; and "F-moc" represents 9-fluorenylmethoxycarbonyl)

[0073] Among the above, the specific diamine (A) is preferably a compound represented by each of the above formula (DA-1) to (DA-10), and more preferably a compound represented by each of the above formula (DA-1), (DA-3) to (DA-6), and (DA-8).

[0074] The diamine compound used in the synthesis of the polyamic acid [A] may be the specific diamine (A) alone, or a diamine different from the specific diamine (A) (hereinafter also referred to as "other diamine (A)") may be used together with the specific diamine (A). Examples of the other diamine (A) include aliphatic diamines, alicyclic diamines, aromatic diamines, diaminoorganosiloxanes, and the like. Specific examples of other diamines (A) include diamine compounds having a partial structure Y in the main chain, such as 4,4'-diaminodiphenylethane, 4,4'-diaminodiphenylpropane, 1,5-bis(4-aminophenoxy)pentane, 1,2-bis(4-aminophenoxy)ethane, 1,3-bis(4-aminophenoxy)propane, 1,6-bis(4-aminophenoxy)hexane, 6,6'-(pentamethylenedioxy)bis(3-aminopyridine), 4'-(2-(4-aminophenoxy)ethoxy)-[1,1'-biphenyl]-4-amine, and 1,3-bis(3-aminopropyl)-tetramethyldisiloxane.

[0075] Diamine compounds that do not have a partial structure Y in the main chain, such as o-phenylenediamine, m-phenylenediamine, p-phenylenediamine, 4,4'-diaminodiphenylmethane, 4-aminophenyl-4-aminobenzoate, 2,5-diaminobenzoic acid, 3,5-diaminobenzoic acid, 4,4'-diaminodiphenyl ether, 2,2'-dimethyl-4,4'-diaminobiphenyl, 3,5-diamino-N,N-bis(pyridin-3-ylmethyl)benzamide, etc.

[0076] When synthesizing the polyamic acid [A], from the viewpoint of sufficiently obtaining the effect of improving the adhesion with the sealant, the amount of the specific diamine (A) used is preferably 10 mol% or more, more preferably 20 mol% or more, further preferably 25 mol% or more, and particularly preferably 35 mol% or more, relative to the total amount of the diamine compounds used in the synthesis of the polyamic acid [A].

[0077] In addition, from the viewpoint of fully obtaining the improvement effect of reducing AC afterimages, the amount of the diamine having a partial structure Y used relative to the total amount of diamine compounds used in the synthesis of the polyamic acid [A] (wherein, when the specific diamine (A) has a partial structure Y, the total amount of the specific diamine (A) and the diamine compounds having a partial structure Y in the main chain among other diamines (A)) is preferably 10 mol% or more, more preferably 20 mol% or more, further preferably 30 mol% or more, and particularly preferably 40 mol% or more.

[0078] Synthesis of polyamic acid

[0079] Polyamic acid [A] can be obtained by reacting tetracarboxylic dianhydride with a diamine compound and a molecular weight modifier as needed. In the synthesis reaction of polyamic acid, the use ratio of tetracarboxylic dianhydride and diamine compound is preferably a ratio of 0.2 equivalents to 2 equivalents of the anhydride group of tetracarboxylic dianhydride relative to 1 equivalent of the amino group of the diamine compound. As molecular weight modifiers, for example, acid monoanhydrides such as maleic anhydride, phthalic anhydride, and itaconic anhydride; monoamine compounds such as aniline, cyclohexylamine, and n-butylamine; monoisocyanate compounds such as phenyl isocyanate and naphthyl isocyanate, etc. The use ratio of the molecular weight modifier is preferably set to 20 parts by mass or less relative to a total of 100 parts by mass of the tetracarboxylic dianhydride and diamine compound used.

[0080] The synthesis reaction of polyamic acid is preferably carried out in an organic solvent. The reaction temperature at this time is preferably -20°C to 150°C, and the reaction time is preferably 0.1 hour to 24 hours. As the organic solvent used in the reaction, for example, aprotic polar solvents, phenolic solvents, alcoholic solvents, ketone solvents, ester solvents, ether solvents, halogenated hydrocarbons, hydrocarbons, etc. can be cited. As specific examples of these, it is preferred to use one or more selected from the group consisting of N-methyl-2-pyrrolidone, N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, tetramethylurea, hexamethylphosphoric triamide, meta-cresol, dimethyl phenol and halogenated phenol as a reaction solvent, or use a mixture of one or more of these and other organic solvents (such as butyl cellosolve, diethylene glycol diethyl ether, etc.). The usage-amount (a) of an organic solvent is preferably an amount in which the total amount (b) of tetracarboxylic dianhydride and diamine becomes 0.1 mass % - 50 mass % with respect to the whole amount (a+b) of a reaction solution.

[0081] In this manner, a polymer solution in which the polyamic acid [A] is dissolved is obtained. The polymer solution may be used directly for the preparation of a liquid crystal aligning agent, or may be used for the preparation of a liquid crystal aligning agent after the polyamic acid [A] contained in the polymer solution is separated.

[0082] (Polyamic acid ester)

[0083] When the polymer [A] is a polyamic acid ester, the polyamic acid ester can be obtained, for example, by the following methods, etc.: [I] a method of reacting polyamic acid [A] with an esterifying agent; [II] a method of reacting a tetracarboxylic acid diester with a diamine compound containing a specific diamine (A); [III] a method of reacting a tetracarboxylic acid diester dihalide with a diamine compound containing a specific diamine (A). Polyamic acid ester may have only an amic acid ester structure, or may be a partially esterified product in which an amic acid structure and an amic acid ester structure coexist. The reaction solution formed by dissolving the polyamic acid ester can be directly used for the preparation of a liquid crystal aligning agent, or it can be used for the preparation of a liquid crystal aligning agent after separating the polyamic acid ester contained in the reaction solution. In addition, in this specification, "tetracarboxylic acid derivative" means tetracarboxylic dianhydride, tetracarboxylic acid diester and tetracarboxylic acid diester dihalide.

[0084] (Polyimide)

[0085] When the polymer [A] is a polyimide, the polyimide can be obtained, for example, by dehydrating and ring-closing the polyamic acid [A] synthesized in the above manner and imidizing it. The polyimide can be a completely imidized product formed by dehydrating and ring-closing all the amic acid structures possessed by the polyamic acid as its precursor, or it can be a partially imidized product in which only a part of the amic acid structure is dehydrated and ring-closed so that the amic acid structure and the imide ring structure coexist. The imidization rate of the polyimide is preferably 20% to 99%, and more preferably 30% to 90%. In addition, the imidization rate is expressed as a percentage of the proportion of the number of imide ring structures relative to the total number of amic acid structures and the number of imide ring structures of the polyimide. Here, a part of the imide ring may be an isoimide ring.

[0086] The dehydration ring-closure of polyamic acid is preferably carried out by the following method: dissolving polyamic acid in an organic solvent, adding a dehydrating agent and a dehydration ring-closure catalyst to the solution, and heating as needed. In the method, as a dehydrating agent, for example, anhydrides such as acetic anhydride, propionic anhydride, and trifluoroacetic anhydride can be used. The amount of the dehydrating agent used is preferably set to 0.01 mol to 20 mol relative to 1 mol of the amic acid structure of the polyamic acid. As a dehydration ring-closure catalyst, for example, tertiary amines such as pyridine, trimethylpyridine, dimethylpyridine, and triethylamine can be used. Relative to 1 mol of the dehydrating agent used, the amount of the dehydration ring-closure catalyst used is preferably set to 0.01 mol to 10 mol. As an organic solvent used in the dehydration ring-closure reaction, an organic solvent exemplified as an organic solvent used in the synthesis of polyamic acid can be cited. The reaction temperature of the dehydration ring-closure reaction is preferably 0°C to 180°C. The reaction time is preferably 1.0 hour to 120 hours. Moreover, the reaction solution containing a polyimide may be used for preparation of a liquid crystal aligning agent as it is, and may be used for preparation of a liquid crystal aligning agent after isolating a polyimide.

[0087] <Polymer [B]>

[0088] The polymer [B] is a polymer having a partial structure represented by the following formula (2).

[0089] [Chemistry 8]

[0090]

[0091] (In formula (2), A 1 and A 4 are independently a divalent aromatic ring group; R 2 and R 3 are independently a hydrogen atom or a monovalent organic group; 1 is a single bond, -NR 4 -, -O- or a divalent aromatic heterocyclic group; R 4is a hydrogen atom or a monovalent organic group; in B 1 In the case of a single bond, A 2 A is a divalent aromatic ring group, 3 is a single bond or a divalent aromatic ring group; in B 1 When A is a divalent aromatic heterocyclic group, 2 and A 3 are independently a single bond or a divalent aromatic ring group; in B 1 For-NR 4 - or -O-, A 2 and A 3 are independently a divalent aromatic ring group, or represent A 2 The aromatic ring and A 3 The aromatic rings are connected by single bonds or chain structures to -NR 4 - or -O- together to form a nitrogen or oxygen-containing condensed ring structure; "*" indicates a bonding bond)

[0092] In the formula (2), A 1 and A 4 The divalent aromatic ring group may be a divalent aromatic hydrocarbon group or a divalent aromatic heterocyclic group. 1 and A 4 The aromatic ring portion may have a substituent. Examples of the substituent include an alkyl group having 1 to 5 carbon atoms, a halogen atom, and the like. 1 , A 4 Preferred specific examples of divalent aromatic hydrocarbon groups include groups formed by removing any two hydrogen atoms bonded to carbon atoms constituting a benzene ring, naphthalene ring or anthracene ring; and divalent aromatic heterocyclic groups include groups formed by removing any two hydrogen atoms bonded to carbon atoms constituting a pyridine ring, pyrimidine ring, pyridazine ring or pyrazine ring. Among these, A 1 and A 4 It is preferably a phenylene group, a biphenylene group or a pyridylene group, and particularly preferably a phenylene group.

[0093] About R 2 and R 3 The monovalent organic group is preferably a monovalent hydrocarbon group having 1 to 10 carbon atoms or a protecting group. The monovalent hydrocarbon group is preferably an alkyl group having 1 to 3 carbon atoms or a phenyl group, and more preferably an alkyl group having 1 to 3 carbon atoms. Examples and preferred examples of the protecting group include R 1 .

[0094] Among these, R 2 and R 3 It is preferably a hydrogen atom or a monovalent hydrocarbon group having 1 to 10 carbon atoms, and more preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.

[0095] B 1 is a single bond, -NR4 -, -O- or a divalent aromatic heterocyclic group. Examples of the divalent aromatic heterocyclic group include: a group formed by removing any two hydrogen atoms from a pyridine ring, a pyrimidine ring, a pyridazine ring or a pyrazine ring; a group formed by removing any two hydrogen atoms from a furan ring; a group formed by removing any two hydrogen atoms from a thiophene ring, etc. Among these, a group formed by removing any two hydrogen atoms from a pyrrole ring, a furan ring and a thiophene ring is preferred, and a group formed by removing two hydrogen atoms from a pyrrole ring is more preferred.

[0096] R 4 The monovalent organic group is preferably an alkyl group having 1 to 3 carbon atoms or a phenyl group, and more preferably an alkyl group having 1 to 3 carbon atoms.

[0097] In B 1 When A is a single bond or a divalent aromatic heterocyclic group, 2 , A 3 For the examples and preferred examples of the divalent aromatic ring group, A 1 and A 4 Description of the divalent aromatic ring group.

[0098] In B 1 For-NR 4 - or -O-, as A 2 and A 3 A divalent aromatic ring group may be cited 1 and A 4 Description of the divalent aromatic ring group. 2 and A 3 Indicates A 2 The aromatic ring and A 3 The aromatic rings are connected to -NR by single bonds or chain structures (such as ethylene). 4 - in the case of a nitrogen-containing fused ring structure formed together with the condensed ring structure, examples of the condensed ring structure include a carbazole structure, a 9-methylcarbazole structure, and a 9-ethylcarbazole structure. 2 and A 3 Indicates A 2 The aromatic ring and A 3 In the case where the aromatic rings are linked by a single bond or a chain structure (eg, ethylene) and together with -O- form an oxygen-containing fused ring structure, examples of the fused ring structure include a dibenzofuran structure and the like.

[0099] The partial structure represented by the formula (2) has a total of 3 or more aromatic rings (including aromatic hydrocarbon rings and aromatic heterocyclic rings), and it is particularly preferred that it has 4 or more. In the case where the partial structure represented by the formula (2) contains a total of 4 or more aromatic rings, the relaxation of the residual charge is further accelerated by lengthening the conjugated structure, and the residual image (especially DC residual image) can be sufficiently reduced, which is preferred in this respect. Among these, it is particularly preferred that the partial structure represented by the formula (2) has a biphenyl structure.

[0100] The main chain of polymer [B] is not particularly limited and can be appropriately selected according to the main chain of polymer [A], etc. When polymer [A] is at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide, polymer [B] is preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide in terms of improving affinity with polymer [A].

[0101] (Polyamic acid)

[0102] When polymer [B] is a polyamic acid, the polyamic acid (hereinafter also referred to as "polyamic acid [B]") is preferably a polymer obtained by reacting a diamine compound containing a diamine having a partial structure represented by the formula (2) with a tetracarboxylic dianhydride in terms of facilitating the introduction of the partial structure represented by the formula (2) into the polymer. As tetracarboxylic dianhydride used in the synthesis of polyamic acid [B], compounds exemplified as tetracarboxylic dianhydride used in the synthesis of polyamic acid [A] can be cited. The tetracarboxylic dianhydride used in the synthesis of polyamic acid [B] preferably contains alicyclic tetracarboxylic dianhydride. Regarding the description of the amount of alicyclic tetracarboxylic dianhydride used, the description of polyamic acid [A] can be cited.

[0103] The specific diamine (B) used for synthesis of the polymer [B] is preferably a compound represented by the following formula (2-1).

[0104] [Chemistry 9]

[0105]

[0106] (In formula (2-1), A 1 ~A 4 , B 1 , R 2 and R 3 have the same meaning as in formula (2)

[0107] As a specific example of the specific diamine (B), the compound etc. represented by each of the following formula (DA-19) - formula (DA-27), formula (DA-42), and formula (DA-43) are mentioned.

[0108] [Chemistry 10]

[0109]

[0110] [Chemistry 11]

[0111]

[0112] Among the above, the specific diamine (B) is preferably a compound represented by each of the formulas (DA-19) to (DA-25) and (DA-42), more preferably a compound represented by each of the formulas (DA-19) to (DA-23) and (DA-42), and even more preferably a compound represented by each of the formulas (DA-19) to (DA-21).

[0113] The diamine compound used in the synthesis of the polyamic acid [B] may be only the specific diamine (B), or a diamine different from the specific diamine (B) (hereinafter also referred to as "other diamine (B)") may be used together with the specific diamine (B). Examples of the other diamine (B) include aliphatic diamines, alicyclic diamines, aromatic diamines, and the like. Specific examples of the other diamine (B) include diamine compounds that do not have a partial structure Y in the main chain as exemplified in the description of the polymer [A]. The polymer [B] preferably does not have any structure that has the partial structure Y and the partial structure X described below.

[0114] When synthesizing polymer [B], in terms of being able to fully achieve the reduction of residual images (especially DC residual images), the amount of specific diamine (B) used is preferably 2 mol% or more, more preferably 5 mol% or more, and more preferably 10 mol% or more relative to the total amount of diamine compounds used in the synthesis of polymer [B]. In addition, the amount of specific diamine (B) used can be arbitrarily set within the range of 100 mol% or less relative to the total amount of diamine compounds used in the synthesis of polymer [B]. In terms of making the coating property of the liquid crystal aligning agent on the substrate better, it is preferably 95 mol% or less, more preferably 90 mol% or less, and more preferably 80 mol% or less.

[0115] In addition, polyamic acid [B], polyamic acid ester and polyimide as polymer [B] can also be produced in the same manner as polymer [A]. Regarding various conditions in the synthesis method of each polymer such as polyamic acid [B], the description of polymer [A] can be cited.

[0116] <Polymer [C]>

[0117] The polymer [C] is a polymer having the following partial structure X in the main chain. By making the liquid crystal aligning agent contain the polymer [A] and the polymer [B] and the polymer [C] having the partial structure X, it is possible to achieve improved adhesion to the sealant and reduced afterimages (AC afterimages and DC afterimages), and at the same time improve the adhesion between the liquid crystal alignment film and the substrate (particularly the adhesion between the spacer portion and the substrate), which is preferred in this respect.

[0118] Partial structure X: -(CH 2 ) a - (wherein a is an integer of 2 to 20), or in -(CH 2 ) a Any methylene group in the structure represented by - is selected from -NR 7 -、-O-、-COO-、-NR 7 -CO-、-NR 7 -COO-, -NR 8 -CO-NR 9 - and a structure formed by substitution with at least one group selected from the group consisting of nitrogen-containing non-aromatic heterocyclic groups (wherein R 7 is a hydrogen atom or an alkyl group; R 8 and R 9 are independently a hydrogen atom or an alkyl group, or represent R 8 With R 9 Combined with R 8 The nitrogen atom to which it is bonded, R 9 The nitrogen atom and -CO- form a ring structure; in the partial structure X, -NR 7 -、-O-、-COO-、-NR 7 -CO-、-NR 7 -COO-, -NR 8 -CO-NR 9 - and nitrogen-containing non-aromatic heterocyclic groups are not adjacent to each other).

[0119] In the partial structure X, from the viewpoint of high improvement effect of the adhesion between the substrate and the liquid crystal alignment film at the spacer arrangement portion, it is preferred that a linear alkanediyl group having 2 or more carbon atoms is contained in the partial structure X. In addition, from the viewpoint of suppressing a decrease in film strength, a is preferably 12 or less, and more preferably 10 or less.

[0120] R 7 , R 8 , R 9 It is preferably a hydrogen atom or a methyl group, and more preferably a hydrogen atom. 8 With R 9Examples of the ring structure formed by bonding to each other include 2-oxo-4-imidazolidinone-1,3-diyl and the like. Examples of the nitrogen-containing non-aromatic heterocyclic group include piperidine-1,4-diyl and piperazine-1,4-diyl and the like. In addition, the polymer [C] does not have the partial structure represented by the formula (1) and the partial structure represented by the formula (2).

[0121] In the above, the partial structure X preferably has a structure selected from -COO-, -NR 7 -CO-、-NR 7 -COO- and -NR 8 -CO-NR 9 - structure. Since the partial structure X has such a hydrogen bonding functional group, it tends to be easily separated from the polymer [A] layer, and it is preferred from the aspect of further improving the adhesion between the liquid crystal alignment film and the substrate. In particular, from the aspect of improving the adhesion to the substrate, it is preferred that the partial structure X includes a group selected from -COO-, -NR 7 -CO-、-NR 7 -COO- and -NR 8 -CO-NR 9 -at least one group selected from the group consisting of and a straight-chain alkanediyl group having 2 or more carbon atoms.

[0122] The main chain of polymer [C] is not particularly limited. When polymer [A] is at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide, polymer [C] is also preferably at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide in terms of improving affinity with polymer [A] and facilitating introduction of partial structure X into the main chain of the polymer.

[0123] When the polymer [C] is a polyamic acid, the polyamic acid (hereinafter also referred to as "polyamic acid [C]") is preferably a polymer obtained by reacting a tetracarboxylic dianhydride with a diamine compound containing a diamine having a partial structure X (hereinafter also referred to as "specific diamine (C)") in terms of ease of introducing the partial structure X into the main chain of the polymer. As tetracarboxylic dianhydride used in the synthesis of polyamic acid [C], compounds exemplified as tetracarboxylic dianhydride used in the synthesis of polyamic acid [A] can be cited. The tetracarboxylic dianhydride used in the synthesis of polyamic acid [C] preferably contains alicyclic tetracarboxylic dianhydride. Regarding the description of the amount of alicyclic tetracarboxylic dianhydride used, the description of polyamic acid [A] can be cited.

[0124] The specific diamine (C) is not particularly limited as long as it is a diamine compound having a partial structure X, and examples thereof include aliphatic diamines, alicyclic diamines, aromatic diamines, etc. The specific diamine (C) is preferably a compound represented by the following formula (3-1).

[0125] [Chemistry 12]

[0126]

[0127] (In formula (3-1), A 5 A is a divalent aromatic ring group; 6 is a single bond or a divalent aromatic ring group; Y 2 is a divalent group having a partial structure X; R 5 is a hydrogen atom or a monovalent organic group)

[0128] In the formula (3-1), A 5 , A 6 The divalent aromatic ring group of A includes divalent aromatic hydrocarbon groups and divalent aromatic heterocyclic groups. 5 , A 6 Specific examples and preferred examples of the divalent aromatic ring group include A in the formula (2): 1 and A 4 Description of the divalent aromatic ring group.

[0129] As R 5 The monovalent organic group R includes a monovalent hydrocarbon group having 1 to 10 carbon atoms. 5 It is preferably a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and more preferably a hydrogen atom or a methyl group.

[0130] Y 2 is a divalent group having a partial structure X, examples of which include: -(CH 2 ) a - or in - (CH 2 ) a Any methylene group in the structure represented by - is selected from -NR 7 -、-O-、-COO-、-NR 7 -CO-、-NR 7 -COO-, -NR 8 -CO-NR 9 - and a divalent group consisting of at least one of the group consisting of a nitrogen-containing non-aromatic heterocyclic group (hereinafter also referred to as "heteroatom-containing group (c)"), -(CH 2 ) a - and a divalent group formed by bonding at least one (one or more) of the heteroatom-containing groups (c) to a cycloalkylene group (preferably a cyclohexylene group). 2 It does not have an aromatic ring group.

[0131] Specific examples of the specific diamine (C) include m-xylylenediamine, pentamethylenediamine, hexamethylenediamine, etc., for aliphatic diamines; 4,4'-methylenebis(cyclohexylamine), etc. for alicyclic diamines; 4,4'-diaminodiphenylethane, 4,4'-diaminodiphenylpropane, 1,3-bis(4-aminophenethyl)urea, 1,3-bis(4-aminobenzyl)urea, 1,5-bis(4-aminophenoxy)pentane, 1, 4-bis(4-aminophenoxy)butane, 1,3-bis(4-aminophenoxy)propane, 1,6-bis(4-aminophenoxy)hexane, bis[2-(4-aminophenyl)ethyl]adipic acid, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-[4,4'-propane-1,3-diylbis(piperidin-1,4-diyl)]diphenylamine, diethylene glycol bis(4-aminophenyl) ether, compounds represented by the following formula (DA-32) to (DA-40), and the like.

[0132] [Chemistry 13]

[0133]

[0134] Among the compounds represented by Formula (DA-32) to Formula (DA-40), the specific diamine (C) is preferably a compound represented by Formula (DA-32) to Formula (DA-35), and more preferably a compound represented by Formula (DA-32) to Formula (DA-34).

[0135] The diamine compound used in the synthesis of the polyamic acid [C] may be the specific diamine (C) alone, or a diamine different from the specific diamine (C) (hereinafter also referred to as "other diamine (C)") may be used together with the specific diamine (C). Examples of the other diamine (C) include diamines different from the specific diamine (A) to the specific diamine (C), for example, diamine compounds that do not have a partial structure Y in the main chain as exemplified in the description of the polymer [A].

[0136] When synthesizing the polymer [C], from the viewpoint of sufficiently improving the adhesion to the substrate, the amount of the specific diamine (C) used is preferably 10 mol% or more, more preferably 20 mol% or more, and further preferably 30 mol% or more relative to the total amount of the diamine compounds used in the synthesis of the polymer [C]. In addition, the amount of the specific diamine (C) used relative to the total amount of the diamine compounds used in the synthesis of the polymer [C] can be arbitrarily set within the range of 100 mol% or less.

[0137] In addition, polyamic acid [C], polyamic acid ester and polyimide as polymer [C] can also be produced in the same manner as polymer [A]. Regarding various conditions in the synthesis method of each polymer such as polyamic acid [C], the description of polymer [A] can be cited.

[0138] For each polymer [A], polymer [B] and polymer [C] used in the preparation of the liquid crystal alignment agent, the solution viscosity of the polymer is preferably 10mPa·s to 800mPa·s when a solution with a concentration of 10% by mass is prepared, and more preferably 15mPa·s to 500mPa·s. In addition, the solution viscosity (mPa·s) is a value measured at 25°C using an E-type rotational viscometer for a polymer solution with a concentration of 10% by mass prepared using a good solvent for the polymer (e.g., γ-butyrolactone, N-methyl-2-pyrrolidone, etc.).

[0139] For each of polymer [A], polymer [B] and polymer [C], the weight average molecular weight (Mw) measured by gel permeation chromatography (GPC) in terms of polystyrene is preferably 1,000 to 500,000, more preferably 2,000 to 300,000. In addition, the molecular weight distribution (Mw / Mn) represented by the ratio of Mw to the number average molecular weight (Mn) in terms of polystyrene measured by GPC is preferably 7 or less, more preferably 5 or less.

[0140] In the liquid crystal aligning agent, from the viewpoint of fully obtaining the effect of improving the adhesion of the sealant, the content of polymer [A] is preferably 1% by mass or more, more preferably 2% by mass or more, more preferably 5% by mass or more, and more preferably 10% by mass or more, relative to the total amount of the polymer components contained in the liquid crystal aligning agent. In addition, the content of polymer [A] is preferably 70% by mass or less, more preferably 60% by mass or less, and more preferably 50% by mass or less, relative to the total amount of the polymer components contained in the liquid crystal aligning agent.

[0141] In terms of improving the effect of reducing residual images (especially DC residual images), the content of polymer [B] is preferably 2% by mass or more, more preferably 5% by mass or more, and more preferably 10% by mass or more relative to the total amount of polymer components contained in the liquid crystal aligning agent. In addition, from the perspective of improving the coating properties of the liquid crystal aligning agent, the content of polymer [B] is preferably 90% by mass or less, more preferably 80% by mass or less, and more preferably 70% by mass or less relative to the total amount of polymer components contained in the liquid crystal aligning agent.

[0142] In terms of the effect of improving the adhesion with the substrate, the content of polymer [C] is preferably 2% by mass or more, more preferably 5% by mass or more, and more preferably 10% by mass or more, relative to the total amount of the polymer components contained in the liquid crystal aligning agent. In addition, from the perspective of improving the coating properties of the liquid crystal aligning agent, the content of polymer [C] is preferably 80% by mass or less, more preferably 70% by mass or less, and more preferably 60% by mass or less, relative to the total amount of the polymer components contained in the liquid crystal aligning agent.

[0143] Here, the polymer [A] is hydrophobized by protecting the -NH- group, and thus it is thought that when the liquid crystal aligning agent is applied to the substrate, it is likely to be present on the film surface. 1 -, it is believed that the protective group (R 1 ) is detached and replaced by hydrogen atoms, thereby generating polar functional groups. Therefore, regarding the liquid crystal alignment agent containing polymer [A], it is believed that: when the film is formed, the solubility in the solvent is high and the polymer [A] tends to be present in the surface layer, and after the film is formed, the adhesion to the sealant becomes good due to the detachment of the protective group, and even if the sealant is formed on the surface of the liquid crystal alignment film, it is not easy to peel off, and a liquid crystal element with high reliability can be obtained.

[0144] In addition, it is believed that: in order to achieve further high performance of the liquid crystal element, the polymer [B] having a specific nitrogen-containing conjugated structure represented by the formula (2) is formulated together with the polymer [A] in the liquid crystal alignment agent, thereby showing a DC residual image reduction effect. However, it is believed that: the partial structure represented by the formula (2) has many aromatic rings, and the toughness of the formed liquid crystal alignment film (especially the lower layer part) is reduced, so that, for example, when an external force is applied, the liquid crystal alignment film is easily peeled off from the substrate, and the adhesion between the liquid crystal alignment film and the substrate, especially the adhesion between the substrate and the liquid crystal alignment film at the configuration part of the spacer, is deteriorated.

[0145] In contrast, it is speculated that by preparing a liquid crystal alignment agent containing polymer [A], polymer [B], and polymer [C], a liquid crystal alignment film can be formed that has excellent adhesion to the sealant and excellent effect of reducing DC residual images, and excellent adhesion to the substrate (especially the spacer portion).

[0146] <Other ingredients>

[0147] The liquid crystal aligning agent may contain a component different from the polymer [A], the polymer [B], and the polymer [C] (hereinafter also referred to as “other components”) as necessary, in addition to the polymer [A], the polymer [B], and the polymer [C].

[0148] (Other polymers)

[0149] The liquid crystal aligning agent of the present disclosure may also contain polymers different from polymer [A], polymer [B] and polymer [C] (hereinafter also referred to as "other polymers") as polymer components. The main skeleton of other polymers is not particularly limited. As other polymers, for example, polyamic acid, polyamic acid ester, polyimide, polysiloxane, polyester, polyamine, polyurea, polyamide, polyamide-imide, polybenzoxazole precursor, polybenzoxazole, cellulose derivatives, polyacetal, (meth) acrylic polymer, styrene polymer, maleimide polymer or styrene-maleimide polymer. From the viewpoint of high affinity with liquid crystal when used in combination with polymer [A], polymer [B] and polymer [C], and improving the reliability of liquid crystal elements, other polymers are preferably selected from at least one of the group consisting of polyamic acid, polyamic acid ester and polyimide.

[0150] When the liquid crystal aligning agent contains other polymers, the content of other polymers can be appropriately set within the range that does not damage the effect of the present invention. Specifically, relative to the total amount of polymer components contained in the liquid crystal aligning agent, the content of other polymers is more preferably 5% by mass or less, further preferably 3% by mass or less, and further more preferably 1% by mass or less.

[0151] (Solvent)

[0152] The liquid crystal aligning agent of the present disclosure is prepared as a liquid composition in which the polymer [A], the polymer [B], the polymer [C] and other components used as necessary are preferably dispersed or dissolved in an appropriate solvent.

[0153] As the solvent, an organic solvent can be preferably used. Specific examples thereof include: N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, 1,2-dimethyl-2-imidazolidinone, 1,3-dimethyl-2-imidazolidinone, phenol, γ-butyrolactone, γ-butyrolactam, N,N-dimethylformamide, N,N-dimethylacetamide, 4-hydroxy-4-methyl-2-pentanone, diacetone alcohol, 1-hexanol, 2-hexanol, propane-1,2-diol, 3-methoxy-1-butanol, ethylene glycol monomethyl ether, methyl lactate, ethyl lactate, butyl lactate, methyl acetate, ethyl acetate, butyl acetate, acetoacetic acid Methyl ester, ethyl acetoacetate, ethyl propionate, methyl methoxypropionate, ethyl ethoxypropionate, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol-n-propyl ether, ethylene glycol-isopropyl ether, ethylene glycol-n-butyl ether (butyl cellosolve), ethylene glycol dimethyl ether, ethylene glycol ethyl ether acetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, diisobutyl ketone, isoamyl propionate, isoamyl isobutyrate, diisoamyl ether, ethylene carbonate, propylene carbonate, propylene glycol monomethyl ether (Propylene Glycol Monomethyl Ether, PGME), diethylene glycol diethyl ether acetate, propylene glycol monomethyl ether acetate (Propylene Glycol Monomethyl Ether Acetate, PGMEA), propylene glycol diacetate, cyclopentanone, cyclohexanone, etc.

[0154] As other components contained in the liquid crystal alignment agent, in addition to the above, for example, antioxidants, metal chelate compounds, hardening accelerators, surfactants, fillers, dispersants, photosensitizers, etc. The proportion of other components can be appropriately selected according to each compound within the range that does not impair the effects of the present disclosure.

[0155] The solid content concentration in the liquid crystal aligning agent (the ratio of the total mass of the components other than the solvent of the liquid crystal aligning agent to the total mass of the liquid crystal aligning agent) is appropriately selected in consideration of viscosity, volatility, etc., preferably in the range of 1% to 10% by mass. If the solid content concentration is 1% by mass or more, the film thickness of the coating can be fully ensured, and it is easy to obtain a liquid crystal alignment film showing good liquid crystal orientation. On the other hand, if the solid content concentration is 10% by mass or less, the coating can be made of an appropriate thickness, and it is easy to obtain a liquid crystal alignment film showing good liquid crystal orientation. In addition, the viscosity of the liquid crystal aligning agent becomes moderate and has a tendency to make the coating property good.

[0156] 《Liquid crystal alignment film and liquid crystal element》

[0157] The liquid crystal alignment film of the present invention can be manufactured by a liquid crystal alignment agent prepared as described. In addition, the liquid crystal element of the present invention includes a liquid crystal alignment film formed using the liquid crystal alignment agent described above. The driving mode of the liquid crystal in the liquid crystal element is not particularly limited, for example, it can be applied to various modes such as TN type, Super Twisted Nematic (STN) type, VA type (including Vertical Alignment-Multi-domain Vertical Alignment (VA-MVA) type, Vertical Alignment-Patterned Vertical Alignment (VA-PVA) type, etc.), IPS type, FFS type, Optically Compensated Bend (OCB) type, Polymer Sustained Alignment (PSA) type. The liquid crystal element can be manufactured, for example, by a method including the following steps 1 to 3. In step 1, the substrate used is different depending on the desired operating mode. Steps 2 and 3 are common in each operating mode.

[0158] <Step 1: Formation of coating film>

[0159] First, a coating film is formed on the substrate by coating a liquid crystal alignment agent on the substrate, preferably by heating the coated surface. As the substrate, for example, glass such as float glass and soda glass; a transparent substrate containing plastics such as polyethylene terephthalate, polybutylene terephthalate, polyether sulfone, polycarbonate, poly (alicyclic olefin) and the like can be used. As the transparent conductive film provided on one side of the substrate, tin oxide (SnO 2 ) of NESA film (a registered trademark of PPG, USA), indium oxide-tin oxide (In 2 O 3 -SnO 2 ) Indium Tin Oxide (ITO) film, etc. In the case of manufacturing TN type, STN type or VA type liquid crystal elements, two substrates provided with patterned transparent conductive films are used. On the other hand, in the case of manufacturing IPS type or FFS type liquid crystal elements, a substrate provided with electrodes patterned into a comb shape and an opposing substrate without electrodes are used.

[0160] The method for coating the liquid crystal alignment agent on the substrate is not particularly limited, and can be carried out by, for example, spin coating, printing (for example, offset printing, flexographic printing, etc.), inkjet, slit coating, rod coater, extrusion die, direct gravure coater, chamber doctor coater, offset gravure coater, impregnation coater, MB coater, etc.

[0161] After the liquid crystal alignment agent is applied, it is preferred to perform preheating (prebaking) for the purpose of preventing the applied liquid crystal alignment agent from dripping. The prebaking temperature is preferably 30°C to 200°C, and the prebaking time is preferably 0.25 minutes to 10 minutes. Thereafter, the solvent is completely removed, and a calcination (post-baking) process is performed as needed for the purpose of thermal imidization of the amide acid structure present in the polymer. The calcination temperature (post-baking temperature) at this time is preferably 80°C to 280°C, and more preferably 80°C to 250°C. The post-baking time is preferably 5 minutes to 200 minutes. The film thickness of the formed film is preferably 0.001 μm to 1 μm. Thus, a film comprising polymer [A'], polymer [B] and polymer [C] can be formed on a substrate, wherein the polymer [A'] is formed by detaching a protective group from a partial structure represented by the formula (1) possessed by the polymer [A]. In addition, the polymer [A'] has a structural unit containing an -NH- group in a portion different from the group participating in the polymerization.

[0162] <Step 2: Orientation treatment>

[0163] In the case of manufacturing TN type, STN type, IPS type or FFS type liquid crystal elements, a process (orientation treatment) of imparting liquid crystal orientation ability to the coating formed in the process 1 is implemented. Thus, the orientation ability of the liquid crystal molecules is imparted to the coating to form a liquid crystal orientation film. As an orientation treatment, it is preferred to use a friction treatment of wiping the surface of the coating formed on the substrate using cotton or the like, or to irradiate the coating with light to impart a light orientation ability to the liquid crystal. In the case of manufacturing a vertically oriented liquid crystal element, the coating formed in the process 1 can be directly used as a liquid crystal orientation film, and in order to further improve the liquid crystal orientation ability, the coating can also be subjected to an orientation treatment.

[0164] Light irradiation for photo-orientation can be performed by the following methods, etc.: a method of irradiating the coating after the post-baking process; a method of irradiating the coating after the pre-baking process and before the post-baking process; a method of irradiating the coating during the heating of the coating in at least any one of the pre-baking process and the post-baking process. As radiation irradiated to the coating, for example, ultraviolet rays and visible light containing wavelengths of 150nm to 800nm ​​can be used. Preferably, ultraviolet rays containing wavelengths of 200nm to 400nm are used. In the case where the radiation is polarized, it can be linearly polarized or partially polarized. In the case where the radiation used is linearly polarized or partially polarized, the irradiation can be performed from a direction perpendicular to the substrate surface, from an oblique direction, or in combination of these directions. The irradiation direction for non-polarized radiation is set to an oblique direction.

[0165] Examples of the light source include a low-pressure mercury lamp, a high-pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, and an excimer laser. The radiation dose is preferably 200 J / m 2 ~30,000J / m 2 , more preferably 500 J / m 2 ~10,000J / m 2 After irradiation with light for imparting alignment ability, the following treatments may also be performed: the substrate surface may be cleaned using, for example, water, an organic solvent (such as methanol, isopropanol, 1-methoxy-2-propanol acetate, butyl cellosolve, ethyl lactate, etc.) or a mixture thereof, or the substrate may be heated.

[0166] <Step 3: Construction of liquid crystal cell>

[0167] Prepare two substrates formed with liquid crystal alignment films in the described manner, and configure liquid crystal between the two substrates arranged opposite to each other, thereby manufacturing a liquid crystal unit. When manufacturing a liquid crystal unit, for example, the following methods can be cited: two substrates are arranged opposite to each other with a gap in a manner that the liquid crystal alignment film faces each other, and the peripheral portions of the two substrates are bonded using a sealant, and the cell gap surrounded by the substrate surface and the sealant is injected with a filling liquid crystal, and then the injection hole is closed, or a method using a liquid crystal drop (One Drop Fill, ODF) method. A bead-shaped spacer or a columnar spacer is configured between the two substrates as an in-plane spacer to form a cell gap. As a sealant, for example, an epoxy resin containing a hardener and alumina balls as a spacer can be used. When the sealant is applied to the substrate, on the surface of the liquid crystal alignment film of at least one substrate of the two substrates formed with the liquid crystal alignment film, for example, it can be performed by screen printing.

[0168] As liquid crystal, any of positive type and negative type can be used, preferably negative type. As negative liquid crystal, for example, "MLC-6608", "MLC-6609", "MLC-6610", "MLC-7026-100" manufactured by Merck can be listed. In particular, when negative liquid crystal is used in IPS type and FFS type liquid crystal elements, the transmission loss of the upper part of the electrode can be reduced, and the contrast can be improved, which is preferred in this respect. In addition, as liquid crystal, nematic liquid crystal and discotic liquid crystal can be listed, among which nematic liquid crystal is preferred.

[0169] When manufacturing a liquid crystal display device, a polarizing plate is then attached to the outer surface of the liquid crystal cell to obtain a liquid crystal display element. Examples of the polarizing plate include a polarizing plate formed by sandwiching a polarizing film called "H film" between cellulose acetate protective films or a polarizing plate containing the H film itself. The "H film" is a film in which polyvinyl alcohol is stretched and oriented while absorbing iodine.

[0170] The liquid crystal element of the present invention can be effectively applied to various purposes. Specifically, for example, it can be used as various display devices or dimming devices such as clocks, portable game consoles, word processors, notebook personal computers, car navigation systems, camcorders, personal digital assistants (PDAs), digital cameras, mobile phones, smart phones, various monitors, liquid crystal televisions, information displays, etc., and phase difference films.

[0171] [Example]

[0172] Hereinafter, the embodiment will be described in more detail based on examples, but the present invention is not to be construed in a limitative manner by the following examples.

[0173] In the following examples, the weight average molecular weight (Mw) of the polymer, the imidization rate of the polyimide in the polymer solution and the solution viscosity of the polymer solution were measured by the following method. The required amount of the raw material compound and the polymer used in the following examples was ensured by repeatedly performing the synthesis under the synthesis scale shown in the following synthesis example as needed.

[0174] [Weight average molecular weight Mw of polymer]

[0175] The weight average molecular weight (Mw) is a polystyrene-equivalent value measured by GPC under the following conditions.

[0176] Column: Made by Tosoh Corporation, TSKgelGRCXLII

[0177] Solvent: N,N-dimethylformamide solution containing lithium bromide and phosphoric acid

[0178] Temperature: 40℃

[0179] Pressure: 68kgf / cm 2

[0180] [Imidization ratio of polyimide]

[0181] The polyimide solution was poured into pure water, the obtained precipitate was fully dried under reduced pressure at room temperature, and then dissolved in deuterated dimethyl sulfoxide. The reaction mixture was measured at room temperature using tetramethylsilane as the reference substance. 1 H-NMR ( 1 H-NuclearMagnetic Resonance, 1 H-NMR). According to the obtained 1 The imidization ratio [%] was determined from the H-NMR spectrum using the following formula (1).

[0182] Imidization rate [%] = (1-(β 1 / (β 2 ×α)))×100…(1)

[0183] (In formula (1), β 1 is the peak area of ​​protons originating from NH groups appearing near the chemical shift of 10 ppm, β 2 is the peak area derived from other protons, and α is the ratio of the number of other protons to one proton of the NH group in the polymer precursor (polyamic acid)

[0184] [Solution viscosity of polymer solution]

[0185] The solution viscosity (mPa·s) of the polymer solution was measured at 25° C. using an E-type rotational viscometer.

[0186] The abbreviations of the compounds used in the Examples are as follows.

[0187] (Tetracarboxylic acid derivatives)

[0188] Compound (AN-1) to Compound (AN-8): Compounds represented by the following formula (AN-1) to (AN-8)

[0189] [Chemistry 14]

[0190]

[0191] (Diamine compound)

[0192] Compound (DA-1) to Compound (DA-12): Compounds represented by Formula (DA-1) to Formula (DA-12)

[0193] Compound (DA-19) to Compound (DA-27), Compound (DA-42): Compounds represented by Formula (DA-19) to Formula (DA-27) and Formula (DA-42)

[0194] Compound (DA-32) to Compound (DA-40): Compounds represented by Formula (DA-32) to Formula (DA-40)

[0195] Compound (DA-13) to Compound (DA-18), Compound (DA-28) to Compound (DA-31), Compound (DA-41): Compounds represented by the following formula (DA-13) to Formula (DA-18), Formula (DA-28) to Formula (DA-31), and Formula (DA-41)

[0196] [Chemistry 15]

[0197]

[0198] <Polymer Synthesis>

[0199] 1. Synthesis of polyamic acid

[0200] [Synthesis example 1]

[0201] Compound (DA-1) was dissolved in N-methyl-2-pyrrolidone (NMP), 0.95 equivalents (molar ratio) of compound (AN-1) were added, and the reaction was carried out at 60°C for 6 hours to obtain a solution containing 15% by mass of polyamic acid. A small amount of the obtained polyamic acid solution was taken, and NMP was added to prepare a solution with a polyamic acid concentration of 10% by mass. The viscosity of the obtained solution was measured to be 128 mPa·s. Subsequently, the polyamic acid solution was injected into a large amount of excess methanol to precipitate the reaction product. The precipitate was washed with methanol and dried at 40°C under reduced pressure for 15 hours to obtain polyamic acid (referred to as "polymer (A-1)"). The weight average molecular weight (Mw) of the obtained polymer was 27,000.

[0202] [Synthesis Examples 2 to 8, 11 to 16, 18 to 53: Synthesis of polymers (A-2) to (A-8), (A-11) to (A-16), (A-18), (A-19), (B-1) to (B-20), (C-1) to (C-14)]

[0203] The types and molar ratios of tetracarboxylic dianhydride and diamine compound were changed as described in Tables 1 to 4 below, respectively. Polymers (A-2) to (A-8), polymers (A-11) to (A-16), polymers (A-18), polymers (A-19), polymers (B-1) to (B-20), and polymers (C-1) to (C-14) were obtained in the same manner as in Synthesis Example 1. In addition, regarding the numerical values ​​in Tables 1 to 4, for acid derivatives (tetracarboxylic dianhydride in the synthesis of polyamic acid), the ratio (molar parts) of each compound relative to 100 molar parts of the total amount of the acid derivatives used in the synthesis is indicated, and for diamine compounds, the ratio (molar parts) of each compound relative to 100 molar parts of the total amount of the diamine compounds used in the synthesis is indicated.

[0204] [Synthesis Example 17: Synthesis of polymer (A-17)]

[0205] The compound (DA-13) was dissolved in N-methyl-2-pyrrolidone (NMP), 0.95 equivalents (molar ratio) of the compound (AN-1) were added, and the reaction was carried out at 60°C for 6 hours to obtain a solution containing 15% by mass of polyamic acid. 0.05 equivalents (molar ratio) of di-tert-butyl dicarbonate were added to the polyamic acid solution, and stirred at room temperature for 15 hours. Then, the polyamic acid solution was injected into a large amount of excess methanol to precipitate the reaction product. The precipitate was washed with methanol and dried at 40°C under reduced pressure for 15 hours to obtain a polyamic acid with a Boc group introduced at the end (set as "polymer (A-17)"). The weight average molecular weight (Mw) of the obtained polymer is 25,000.

[0206] 2. Synthesis of polyimide

[0207] [Synthesis Example 9: Synthesis of polymer (A-9)]

[0208] The types and molar ratios of tetracarboxylic dianhydride and diamine compounds were changed as described in Table 1 below, and polymerization was performed in the same manner as in Synthesis Example 1 to obtain a solution containing 15% by mass of polyamic acid. Then, NMP was added to the obtained polyamic acid solution to prepare a solution having a polyamic acid concentration of 10% by mass, and pyridine and acetic anhydride were added to perform a dehydration ring-closure reaction at 60°C for 4 hours. After the dehydration ring-closure reaction, the solvent in the system was replaced with a new NMP to obtain a solution containing 15% by mass of polyimide having an imidization rate of about 85%. Then, the polyimide solution was injected into a large amount of excess methanol to precipitate the reaction product. The precipitate was washed with methanol and dried for 15 hours under reduced pressure and at 40°C to obtain a polyimide (set to "polymer (A-9)"). The weight average molecular weight (Mw) of the obtained polymer was 33,000.

[0209] 3. Synthesis of polyamic acid ester

[0210] [Synthesis Example 10: Synthesis of polymer (A-10)]

[0211] 70 parts by mole of compound (DA-5), 15 parts by mole of compound (DA-6), and 15 parts by mole of compound (DA-3) as diamine compounds, 2.5 equivalents (molar ratio) of pyridine as a base relative to the total amount of diamine compounds, and N-methyl-2-pyrrolidone (NMP) as a solvent were added and dissolved. While the solution was stirred under water cooling, 97 parts by mole of dimethyl-1,3-bis(chlorocarbonyl)cyclobutane-2,4-carboxylate as an acid derivative was added, and NMP was further added in a manner that the solid content concentration became 5% by mass, and stirred for 4 hours while cooling under water. The solution was injected into water to precipitate the polymer, and the polymer was filtered out by suction filtration, washed again with water, and then washed 3 times with methanol, and dried under reduced pressure at 40°C to obtain a polyamic acid ester (referred to as "polymer (A-10)"). The weight average molecular weight (Mw) of the polymer (A-10) is 29,000.

[0212] [Table 1]

[0213]

[0214] [Table 2]

[0215]

[0216] [Table 3]

[0217]

[0218] [Table 4]

[0219]

[0220] [Example 1]

[0221] 1. Preparation of liquid crystal alignment film

[0222] 20 parts by mass of polymer (A-1) obtained in Synthesis Example 1, 40 parts by mass of polymer (B-7) obtained in Synthesis Example 26, and 40 parts by mass of polymer (C-3) obtained in Synthesis Example 40 were diluted with NMP, γ-butyrolactone (GBL), ButylCellosolve (BC), diacetone alcohol (DAA), and diethyleneglycol diethyl ether (DEDG) to obtain a solution having a solid content concentration of 4.0% by mass and a solvent composition ratio of NMP:GBL:BC:DAA:DEDG=30:30:20:10:10 (mass ratio). The solution was filtered with a filter having a pore size of 0.2 μm to prepare a liquid crystal alignment agent (R-1).

[0223] 2. Formation of liquid crystal alignment film based on rubbing method

[0224] Prepare a glass substrate with a flat electrode (bottom electrode), an insulating layer and a comb-shaped electrode (top electrode) stacked on one side in sequence, a columnar spacer on the electrode forming surface, and an opposing glass substrate without an electrode. On each surface of the pair of substrates, use a spinner to apply the liquid crystal alignment agent (R-1) prepared in 1., heat on a hot plate at 80°C (pre-bake) for 1 minute, and then dry (post-bake) for 30 minutes in a 230°C oven in which nitrogen is replaced in the reservoir to form a coating with an average film thickness of 0.1 μm. For the surface of the coating, use a friction machine with a roller wound with nylon cloth, and perform friction treatment at a roller speed of 1000 rpm, a platform moving speed of 3 cm / second, and a hair pressing length of 0.3 mm. The coating subjected to friction orientation treatment is ultrasonically cleaned in ultrapure water for 1 minute, and then dried in a clean oven at 100°C for 10 minutes to form a liquid crystal alignment film.

[0225] 3.Manufacturing of FFS type liquid crystal display elements

[0226] In the pair of substrates with liquid crystal alignment films prepared in 2., the edge of the surface on which the liquid crystal alignment film is formed on one of the substrates has a residual liquid crystal main inlet, and an epoxy resin adhesive with alumina balls of 5.5 μm in diameter is applied by screen printing, and then the substrates are overlapped and crimped in such a way that the friction directions of each substrate become anti-parallel, and the adhesive is thermally cured at 150°C for 1 hour. Then, negative nematic liquid crystal (manufactured by Merck, MLC-6608) is filled between a pair of substrates from the liquid crystal injection port, and then the liquid crystal injection port is sealed with an epoxy adhesive. Furthermore, in order to remove the flow orientation during liquid crystal injection, it is heated at 120°C and then slowly cooled to room temperature. Secondly, polarizing plates are bonded to the outer two surfaces of the substrate to manufacture an FFS type liquid crystal display element.

[0227] 4. Evaluation of sealant adhesion (sealing tightness)

[0228] A pair of substrates having a liquid crystal orientation film are prepared using a liquid crystal orientation agent (R-1) in the same manner as in 2. Next, an epoxy resin adhesive to which alumina balls having a diameter of 5.5 μm are applied to the center portion of each of the orientation film forming surfaces of the pair of substrates, and then the orientation film forming surfaces are overlapped and crimped so as to face each other, and the adhesive is hardened to form a sealant. Using a tensile testing machine, the pressure when the sealant is peeled off is measured. The case where peeling occurs when a pressure of 2.0 Kgf or more is applied is rated as "excellent", the case where peeling occurs when a pressure of 1.0 Kgf or more and less than 2.0 Kgf is applied is rated as "good", and the case where peeling occurs at a pressure of less than 1.0 Kgf is rated as "poor". The result is rated as "excellent" in the embodiment.

[0229] 5. Evaluation of AC afterimage characteristics

[0230] The same operation as in 3. was performed to produce an FFS type liquid crystal cell, except that the polarizing plates were not attached to the outer surfaces of the substrate. The FFS type liquid crystal cell was driven at an AC voltage of 10 V for 72 hours, and then the minimum relative transmittance (%) expressed by the following formula (2) was measured using a device having a polarizer and an analyzer disposed between a light source and a light quantity detector.

[0231] Minimum relative transmittance (%) = [(β-B0) / (B100-B0)] × 100…(2)

[0232] (In formula (2), B0 is the light transmittance under blank and crossed nicols; B100 is the light transmittance under blank and parallel nicols; β is the light transmittance that is minimum under crossed nicols and when the liquid crystal cell is sandwiched between the polarizer and the analyzer)

[0233] The black level in the dark state is represented by the minimum relative transmittance of the liquid crystal unit. In the FFS type liquid crystal unit, the smaller the black level in the dark state, the better the contrast. The case where the minimum relative transmittance is less than 0.3% is set as "excellent", the case where it is greater than 0.3% and less than 2.0% is set as "good", and the case where it is greater than 2.0% is set as "poor". The result is "good" in the above embodiment.

[0234] 6. Evaluation of DC afterimage characteristics

[0235] For the liquid crystal display element manufactured in 3., it is driven with AC 2.5V and the brightness difference between any two pixels is set to 0, and then driven with AC 2.5V and DC 1V is applied to only one of the pixels for 20 minutes to accumulate charge. When the application of DC 1V is terminated and only the drive with AC 2.5V is returned, a brightness difference is generated between the two pixels by the accumulated charge. By observing the change of the brightness difference over time, the relaxation time of the residual DC value attenuation process is calculated. The relaxation time is judged as "excellent" when it is less than 10 seconds, and the relaxation time is judged as "good" when it is more than 10 seconds and less than 20 seconds, and the relaxation time is judged as "poor" when it is more than 20 seconds. As a result, it is evaluated as "excellent" in the embodiment.

[0236] 7. Evaluation of adhesion to substrate (adhesion to spacer)

[0237] For the liquid crystal display element manufactured in the above 3., observe the orientation defects after applying external stress. Specifically, a rod-shaped indenter with a diameter of 5mm is pressed for 10 minutes under a weight of 2.0Kgf and a rotation speed of 200rpm, and then the number of orientation defective parts of the light leakage in the pixel under the orthogonal Nicol is counted. In the case where the toughness of the liquid crystal alignment film is high, when the liquid crystal display element is pressed from the top to the thickness direction, the liquid crystal alignment film follows the movement of the spacer in the thickness direction and deforms and restores the original state, so the liquid crystal alignment film is not easy to peel off from the substrate. In the described case, it can be said that the liquid crystal alignment film has good adhesion to the substrate. In contrast, in the case where the toughness of the liquid crystal alignment film is not sufficient, when the liquid crystal display element is pressed from the top to the thickness direction, the liquid crystal alignment film cannot follow the movement of the spacer, and cracks are generated in the liquid crystal alignment film by pressing, and it is easy to peel off from the substrate. In the described case, it can be said that the liquid crystal alignment film has poor adhesion to the substrate. Therefore, in this embodiment, the adhesion of the liquid crystal alignment film and the substrate (particularly the adhesion of the spacer portion) is evaluated by observing the alignment defects after the liquid crystal display element is given external stress. Regarding the evaluation criteria, the case where the number of alignment defects is 0 is set as "excellent", the case where the number of alignment defects is 1 or more and less than 5 is set as "good", and the case where the number of alignment defects is 5 or more is set as "poor". As a result, the evaluation is "excellent" in the embodiment.

[0238] 8. Evaluation of inkjet coating properties

[0239] As a substrate for coating the liquid crystal alignment agent (R-1), a glass substrate with a transparent electrode containing ITO is heated on a hot plate at 200°C for 1 minute, followed by ultraviolet / ozone cleaning, so that the contact angle of water on the transparent electrode surface is less than 10°. The prepared liquid crystal alignment agent (R-1) is coated on the transparent electrode surface of the glass substrate with a transparent electrode using an inkjet coater (manufactured by Shibaura Mechatronics (stock)). The coating conditions at this time are set to coat 2,500 times / (nozzle·minute) and 250 mg / 10 seconds of discharge for 2 round trips (a total of 4 times). After coating, let it stand for 1 minute, and then heat it at 80°C to form a coating film with an average film thickness of 0.1μm. For the obtained coating film, the number of unevenness and depressions is observed with the naked eye under irradiation with an interference fringe measuring lamp (sodium lamp). The case where the total number of unevenness and concave sites was 0 was judged as "excellent", the case where the total number of unevenness and concave sites was 1 or more and less than 3 was judged as "good", and the case where the total number of unevenness and concave sites was 3 or more was judged as "poor". As a result, the inkjet coating property of the liquid crystal alignment agent of this example was evaluated as "excellent".

[0240] [Examples 2 to 9, Examples 11 to 19 and Comparative Examples 1 to 9]

[0241] The composition of the liquid crystal aligning agent was changed as shown in Table 5 below. Otherwise, the liquid crystal aligning agent was prepared in the same manner as in Example 1. In addition, the obtained liquid crystal aligning agent was used to manufacture a liquid crystal display element in the same manner as in Example 1, and various evaluations were performed. The results are shown in Table 5 below. In Table 5, the resin in the brackets of each polymer represents the blending ratio (mass parts) of each polymer in terms of solid content relative to 100 parts by mass of the total amount of the polymer components used in the preparation of the liquid crystal aligning agent.

[0242] [Example 10]

[0243] Except that the composition of the liquid crystal alignment agent was changed as shown in Table 5 below and that the liquid crystal alignment film was subjected to the photo-alignment method instead of the rubbing method, the liquid crystal alignment agent was prepared in the same manner as in Example 1, and a liquid crystal display element and a liquid crystal cell were manufactured and various evaluations were performed. The formation of the liquid crystal alignment film by the photo-alignment method was performed according to the following procedure.

[0244] (Formation of Liquid Crystal Alignment Film by Photo-Alignment Method)

[0245] On a glass substrate with a flat electrode (bottom electrode), an insulating layer and a comb-shaped electrode (top electrode) stacked in sequence on one side, a columnar spacer on the electrode forming surface, and an opposing glass substrate without an electrode, a liquid crystal alignment agent is applied using a spinner, and heated (pre-baked) on a hot plate at 80°C for 1 minute. Thereafter, it is dried (post-baked) for 30 minutes in a 230°C oven substituted with nitrogen in the chamber to form a coating with an average film thickness of 0.1 μm. The obtained coating is irradiated with 1,000 J / m ultraviolet rays containing a bright line of 254 nm with linear polarization from the normal direction of the substrate using a Hg-Xe lamp. 2 The photo-alignment treatment was performed. The irradiation amount was a value measured using a light meter based on a wavelength of 254 nm. The photo-alignment treated coating was then heated in a clean oven at 230° C. for 30 minutes to form a liquid crystal alignment film.

[0246] In addition, the UV irradiation after post-baking was set at 100 J / m 2 ~10,000J / m 2 The series of operations are performed by changing the exposure amount within a range of , thereby manufacturing more than three liquid crystal units with different ultraviolet irradiation amounts, and various evaluations are performed in the same manner as in Example 1 using a liquid crystal unit with an exposure amount (optimal exposure amount) that exhibits the best orientation characteristics.

[0247] [Table 5]

[0248]

[0249] As shown in Table 5, various properties of Examples 1 to 19, including sealing adhesion, AC afterimage characteristics, DC afterimage characteristics, spacer adhesion, and coating properties, were well balanced and improved compared to Comparative Examples 1 to 9. In contrast, Comparative Examples 1 to 9, which did not contain any of the polymer [A], the polymer [B], and the polymer [C], had any one of the sealing adhesion, the DC afterimage characteristics, and the spacer adhesion evaluated as "poor".

Claims

1. A liquid crystal alignment agent, comprising: The polymer [A] has a partial structure represented by the following formula (1) and does not have a partial structure represented by the following formula (2); The polymer [B] has a partial structure represented by the following formula (2); and The polymer [C] has the following partial structure X in the main chain and does not have the partial structure represented by the following formula (1) and the partial structure represented by the following formula (2); The weight average molecular weight of the polymer [A], the polymer [B] and the polymer [C] in terms of polystyrene measured by gel permeation chromatography is 1,000 to 500,000; The polymer [A], the polymer [B] and the polymer [C] are at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide; The polymer [A] is a polymer obtained by reacting a tetracarboxylic dianhydride containing alicyclic tetracarboxylic dianhydride with a diamine compound containing a diamine having a partial structure represented by the following formula (1); When synthesizing the polymer [A], the amount of the diamine having a partial structure represented by the following formula (1) is 10 mol% or more relative to the total amount of the diamine compound used in the synthesis of the polymer [A]; The polymer [B] is a polymer obtained by reacting tetracarboxylic dianhydride with a diamine compound containing a diamine having a partial structure represented by the following formula (2); When synthesizing the polymer [B], the amount of the diamine having a partial structure represented by the following formula (2) is 2 mol% or more relative to the total amount of the diamine compound used in the synthesis of the polymer [B]; The polymer [C] is a polymer obtained by reacting tetracarboxylic dianhydride with a diamine compound including a diamine having the following partial structure X; When synthesizing the polymer [C], the amount of the diamine having the following partial structure X used is 10 mol% or more relative to the total amount of the diamine compound used in the synthesis of the polymer [C]; The content of the polymer [A] is 1% by mass or more relative to the total amount of the polymer components; The content of the polymer [B] is 2% by mass or more relative to the total amount of the polymer components; The content of the polymer [C] is 2% by mass or more relative to the total amount of the polymer components; Partial structure X: -(CH2) a -The structure represented by -(CH2) a - Any methylene group in the structure represented is selected from -NR 7 -、-O-、-COO-、-NR 7 -CO-、-NR 7 -COO-, -NR 8 -CO-NR 9 - and a structure formed by substitution with at least one group selected from the group consisting of a nitrogen-containing non-aromatic heterocyclic group; -(CH2) a - In the structure represented by, a is an integer from 2 to 20; In-(CH2) a Any methylene group in the structure represented by - is selected from -NR 7 -、-O-、-COO-、-NR 7 -CO-、-NR 7 -COO-, -NR 8 -CO-NR 9 - and nitrogen-containing non-aromatic heterocyclic groups, wherein R 7 is a hydrogen atom or an alkyl group; R 8 and R 9 are independently a hydrogen atom or an alkyl group, or represent R 8 With R 9 Combined with R 8 The nitrogen atom to which it is bonded, R 9 The nitrogen atom and -CO- form a ring structure; in the partial structure X, -NR 7 -、-O-、-COO-、-NR 7 -CO-、-NR 7 -COO-, -NR 8 -CO-NR 9 - and the nitrogen-containing non-aromatic heterocyclic groups are not adjacent to each other; In formula (1), R 1 is a carbamate protecting group, an amide protecting group, an imide protecting group or a sulfonamide protecting group; "*" indicates a bonding bond; In formula (2), A 1 and A 4 are independently a divalent aromatic ring group; R 2 and R 3 are independently a hydrogen atom or a monovalent organic group; 1 is a single bond, -NR 4 -, -O- or a divalent aromatic heterocyclic group; R 4 is a hydrogen atom or a monovalent organic group; in B 1 In the case of a single bond, A 2 A is a divalent aromatic ring group, 3 is a single bond or a divalent aromatic ring group; in B 1 When A is a divalent aromatic heterocyclic group, 2 and A 3 are independently a single bond or a divalent aromatic ring group; in B 1 For-NR 4 - or -O-, A 2 and A 3 are independently a divalent aromatic ring group, or represent A 2 The aromatic ring and A 3 The aromatic rings are connected by single bonds or chain structures to -NR 4 -or -O-together to form a nitrogen or oxygen-containing fused ring structure; "*" represents a bonding bond.

2. The liquid crystal alignment agent according to claim 1, wherein The polymer [C] comprises a structural unit derived from a diamine represented by the following formula (3-1); In formula (3-1), A 5 A is a divalent aromatic ring group; 6 is a single bond or a divalent aromatic ring group; Y 2 is a divalent group having the partial structure X; R 5 It is a hydrogen atom or a monovalent organic group.

3. The liquid crystal aligning agent according to claim 1 or 2, wherein: The partial structure X has a structure selected from -COO-, -NR 7 -CO-、-NR 7 -COO- and -NR 8 -CO-NR 9 -At least one group consisting of.

4. The liquid crystal aligning agent according to claim 1 or 2, wherein The polymer [A] comprises a structural unit derived from a diamine represented by the following formula (1-1); In formula (1-1), A 7 and A 8 are independently a divalent aromatic ring group; Y 1 is a divalent organic group; r is 0 or 1; wherein, when r is 1, A 7 , A 8 and Y 1 At least one of them has a partial structure represented by the formula (1); when r is 0, A 7 It has a partial structure represented by the above formula (1).

5. The liquid crystal aligning agent according to claim 1 or 2, wherein The polymer [A] has the following partial structure Y in the main chain; Partial structure Y: -(CH2) b -The structure represented by -(CH2) b - Any methylene group in the structure represented is selected from -NR 10 -、-O-、-COO-、-NR 10 -CO-、-NR 10 -COO-, -NR 10 -CO-NR 11 - and a structure formed by substitution with at least one group selected from the group consisting of a nitrogen-containing non-aromatic heterocyclic group; -(CH2) b - In the structure represented by, b is an integer from 2 to 20; In-(CH2) b Any methylene group in the structure represented by - is selected from -NR 10 -、-O-、-COO-、-NR 10 -CO-、-NR 10 -COO-, -NR 10 -CO-NR 11 - and nitrogen-containing non-aromatic heterocyclic groups, wherein R 10 and R 11 are independently a hydrogen atom or a monovalent organic group; in the partial structure Y, -NR 10 -、-O-、-COO-、-NR 10 -CO-、-NR 10 -COO-, -NR 10 -CO-NR 11 - and the nitrogen-containing non-aromatic heterocyclic groups are not adjacent to each other.

6. The liquid crystal aligning agent according to claim 1 or 2, wherein: The polymer [B] comprises a structural unit derived from a diamine represented by the following formula (2-1); In formula (2-1), A 1 ~A 4 , B 1 , R 2 and R 3 They have the same meanings as in the above formula (2). 7 . A liquid crystal alignment film, formed from the liquid crystal alignment agent according to claim 1 .

8. A liquid crystal alignment film comprising: A polymer [A'] having a structural unit containing a partial structure represented by the following formula (1A) in a part different from the group participating in polymerization, and having no partial structure represented by the following formula (2); A polymer [B'] having a partial structure represented by the following formula (2); and A polymer [C'] having the following partial structure X in the main chain and not having the partial structure represented by the following formula (2); The weight average molecular weight of the polymer [A'], the polymer [B'] and the polymer [C'] in terms of polystyrene measured by gel permeation chromatography is 1,000 to 500,000; The polymer [A'], the polymer [B'] and the polymer [C'] are at least one selected from the group consisting of polyamic acid, polyamic acid ester and polyimide; The polymer [A'] is a polymer obtained by reacting a tetracarboxylic dianhydride containing alicyclic tetracarboxylic dianhydride with a diamine compound containing a diamine having a partial structure represented by formula (1) described in claim 1; When synthesizing the polymer [A'], the amount of the diamine having the partial structure represented by the formula (1) described in claim 1 is used in an amount of 10 mol% or more relative to the total amount of the diamine compound used in the synthesis of the polymer [A']; The polymer [B'] is a polymer obtained by reacting tetracarboxylic dianhydride with a diamine compound containing a diamine having a partial structure represented by the following formula (2); When synthesizing the polymer [B'], the amount of the diamine having a partial structure represented by the following formula (2) is 2 mol% or more relative to the total amount of the diamine compound used in the synthesis of the polymer [B']; The polymer [C'] is a polymer obtained by reacting tetracarboxylic dianhydride with a diamine compound including a diamine having the following partial structure X; When synthesizing the polymer [C'], the amount of the diamine having the following partial structure X used is 10 mol% or more relative to the total amount of the diamine compound used in the synthesis of the polymer [C']; The content of the polymer [A'] is 1% by mass or more relative to the total amount of the polymer components; The content of the polymer [B'] is 2% by mass or more relative to the total amount of the polymer components; The content of the polymer [C'] is 2% by mass or more relative to the total amount of the polymer components; Partial structure X: -(CH2) a -The structure represented by -(CH2) a - Any methylene group in the structure represented is selected from -NR 7 -、-O-、-COO-、-NR 7 -CO-、-NR 7 -COO-, -NR 8 -CO-NR 9 - and a structure formed by substitution with at least one group selected from the group consisting of a nitrogen-containing non-aromatic heterocyclic group; -(CH2) a - In the structure represented by, a is an integer from 2 to 20; In-(CH2) a Any methylene group in the structure represented by - is selected from -NR 7 -、-O-、-COO-、-NR 7 -CO-、-NR 7 -COO-, -NR 8 -CO-NR 9 - and nitrogen-containing non-aromatic heterocyclic groups, wherein R 7 is a hydrogen atom or an alkyl group; R 8 and R 9 are independently a hydrogen atom or an alkyl group, or represent R 8 With R 9 Combined with R 8 The nitrogen atom to which it is bonded, R 9 The nitrogen atom and -CO- form a ring structure; in the partial structure X, -NR 7 -、-O-、-COO-、-NR 7 -CO-、-NR 7 -COO-, -NR 8 -CO-NR 9 - and the nitrogen-containing non-aromatic heterocyclic groups are not adjacent to each other; In formula (1A), "*" represents a bonding bond; In formula (2), A 1 and A 4 are independently a divalent aromatic ring group; R 2 and R 3 are independently a hydrogen atom or a monovalent organic group; 1 is a single bond, -NR 4 -, -O- or a divalent aromatic heterocyclic group; R 4 is a hydrogen atom or a monovalent organic group; in B 1 In the case of a single bond, A 2 A is a divalent aromatic ring group, 3 is a single bond or a divalent aromatic ring group; in B 1 When A is a divalent aromatic heterocyclic group, 2 and A 3 are independently a single bond or a divalent aromatic ring group; in B 1 For-NR 4 - or -O-, A 2 and A 3 are independently a divalent aromatic ring group, or represent A 2 The aromatic ring and A 3 The aromatic rings are connected by single bonds or chain structures to -NR 4 -or -O-together to form a nitrogen or oxygen-containing fused ring structure; "*" represents a bonding bond. 9 . A liquid crystal element comprising the liquid crystal alignment film according to claim 7 .