Wafers, wafer manufacturing methods, and device chip manufacturing methods

By printing resistivity-related information on the wafer, the problems of low productivity and laser oscillator damage caused by measuring transmittance in the prior art are solved, enabling rapid determination of processing conditions and improved production efficiency.

CN114068301BActive Publication Date: 2026-11-17DISCO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202110834950.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-08-03
Filing Date
2021-07-23
Publication Date
2026-11-17
Estimated Expiration
2041-07-23

AI Technical Summary

Technical Problem

In existing technologies, determining the laser beam irradiation conditions for a wafer requires measuring transmittance, which leads to low productivity and easy damage to the laser oscillator, making it impossible to quickly determine the processing conditions.

Method used

Markers representing resistivity-related information are formed on the wafer. Processing conditions are determined in advance by measuring the resistivity of the ingot, and the relevant information is printed on the wafer to guide the irradiation of the laser beam.

Benefits of technology

Processing conditions can be quickly determined without measuring wafer transmittance, improving productivity, reducing damage to laser oscillators, and increasing processing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114068301B_ABST
    Figure CN114068301B_ABST
Patent Text Reader

Abstract

This invention provides a wafer, a method for manufacturing a wafer, and a method for manufacturing a device chip, rapidly determining the processing conditions for the wafer. The wafer manufacturing method manufactures a wafer from an ingot, comprising the following steps: a resistivity measurement step, measuring the resistivity of the ingot at an end face; a release layer formation step, irradiating the ingot with a first laser beam of a wavelength transparent to the ingot at a depth equivalent to the thickness of the wafer to be formed, thereby forming a release layer inside the ingot; an information printing step, irradiating the ingot with a second laser beam of a second laser beam at a region of the wafer to be formed that does not form a device, thereby forming text, numbers, or markings on the end face or inside the ingot representing information related to the resistivity measured in the resistivity measurement step; and a wafer generation step, dividing the ingot starting from the release layer, and peeling off the generated wafer to produce the wafer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a wafer in the shape of a disc, a method for manufacturing a wafer from a cylindrical ingot, and a method for manufacturing a device chip by dicing the wafer. Background Technology

[0002] When multiple devices are formed on the front side of a wafer formed of semiconductor material and the wafer is broken apart according to each device, a device chip mounted on an electronic device can be formed. Wafers incorporating devices such as ICs (Integrated Circuits), LSIs (Large Scale Integrations), and LEDs (Light Emitting Diodes) are formed by breaking apart cylindrical ingots. As a method for manufacturing wafers by breaking apart ingots, for example, a method using a laser beam is known (see Patent Document 1).

[0003] In this method, a laser beam with a wavelength that is transparent to the material constituting the ingot (the wavelength transmitted through the ingot) is focused from the front side of the ingot to a predetermined depth position and scanned along a predetermined separation surface. Thus, a release layer comprising a modified layer and cracks extending from the modified layer is formed inside the ingot along the separation surface. Furthermore, the ingot is broken apart using this release layer as the separation starting point to form a wafer.

[0004] Furthermore, laser beams can also be used when dicing a wafer containing multiple devices to manufacture a device chip. During wafer dicing, a laser beam of wavelength passing through the wafer is focused into the interior of the wafer along a predetermined dicing line set on the front side of the wafer in a manner that divides the multiple devices, forming a modifier layer along the predetermined dicing line. The wafer is then diced using this modifier layer as the starting point.

[0005] Furthermore, it has been found that the yield of device chips (semiconductor elements) formed from wafers manufactured from ingots depends on the position of the wafer within the ingot, and there is a need to determine the position of the wafer within the ingot later. Moreover, it is known that wafers have identification marks on their front or back sides, and these identification marks contain information about the position of the wafer cut from the ingot within the ingot (see Patent Document 2).

[0006] Patent Document 1: Japanese Patent Application Publication No. 2016-127186

[0007] Patent Document 2: Japanese Patent Application Publication No. 2001-76981

[0008] Patent Document 3: International Publication No. 2005 / 098915

[0009] Patent Document 4: Japanese Patent Application Publication No. 2019-33162

[0010] It is believed that the irradiation conditions, such as the energy of the laser beam, when forming the modified layer inside the wafer are used are adjusted taking into account the transmittance of the laser beam to the wafer. Furthermore, it is known that the transmittance is affected by the thickness of the wafer, the concentration of impurities, etc. (see, for example, Patent Document 3), and there are known methods for calculating the transmittance by irradiating the wafer with a laser beam before processing (see, for example, Patent Document 4).

[0011] However, determining the laser beam irradiation conditions for dicing wafers according to each device requires time and effort to measure the transmittance of the laser beam for each wafer, thus reducing the device chip productivity. Furthermore, when laser processing multiple wafers one after another, the laser oscillator must remain running until the transmittance measurement of the laser beam for the new wafer is completed, which is also a major cause of accelerated laser oscillator degradation. Summary of the Invention

[0012] The present invention was made in view of this problem, and its object is to provide a wafer, a method for manufacturing the wafer, and a method for manufacturing a device chip that can quickly determine the processing conditions of the wafer without measuring the transmittance of the laser beam on the wafer.

[0013] According to one aspect of the present invention, a wafer is provided, characterized in that text, numbers or markings representing information related to resistivity are formed on the wafer.

[0014] Preferably, text, numbers, or markings representing information related to the resistivity are formed internally.

[0015] In addition, according to another aspect of the present invention, a method for manufacturing a wafer is provided, wherein the wafer manufacturing method comprises the following steps: a slicing step, wherein the ingot is sliced ​​to generate a plurality of the wafers; a grinding step, wherein the wafers generated by the slicing step are ground to a predetermined thickness; a polishing step, wherein one or both of the front or back sides of the wafer polished by the polishing step are polished; a resistivity measurement step, wherein the resistivity of the wafer is measured; and an information printing step, wherein after the resistivity measurement step, text, numbers or markings representing information related to the resistivity are formed on one or more of the front, back or interior sides of the wafer.

[0016] Additionally, according to another aspect of the present invention, a method for manufacturing a wafer is provided, comprising the following steps: a planarization step, planarizing the end face of the ingot; a resistivity measurement step, measuring the resistivity of the ingot on the planarized end face; a release layer formation step, irradiating the ingot with a first laser beam having a wavelength transparent to the ingot at a depth equivalent to the thickness of the wafer to be generated, thereby forming a release layer inside the ingot; an information printing step, irradiating the ingot with a second laser beam having a focus point at a region of the wafer to be generated that does not form a device, thereby forming text, numbers, or markings representing information related to the resistivity measured by the resistivity measurement step on one or both of the planarized end face or inside the ingot; and a wafer generation step, dividing the ingot starting from the release layer, and peeling off the generated wafer to generate the wafer.

[0017] Preferably, the ingot is a single-crystal SiC ingot, which has: the end face; an opposing end face on the side opposite to the end face; a c-axis from the end face to the opposing end face; and a c-plane perpendicular to the c-axis, the c-axis being inclined relative to the normal of the end face, and the c-plane being inclined relative to the end face at an offset angle. In the release layer forming step, a processing feed step that moves the ingot and the focusing point of the first laser beam relative to each other in a first direction to form a linear modified layer and an indexing feed step that moves the ingot and the focusing point relative to each other in a second direction are repeated to form the release layer containing the modified layer, wherein the first direction is a direction perpendicular to the direction in which the offset angle is formed and parallel to the end face, and the second direction is the direction in which the offset angle is formed and parallel to the end face.

[0018] Alternatively, it is preferable that, in the information printing step, the number representing the resistivity is formed as information related to the resistivity.

[0019] In addition, according to another aspect of the present invention, a method for manufacturing a device chip is provided, wherein a wafer is laser-processed to divide it into multiple device chips, the wafer having multiple intersecting predetermined dividing lines on its front side, and devices are formed in each region on the front side divided by the predetermined dividing lines. The method is characterized by comprising the following steps: a loading step, loading the wafer into a laser processing apparatus; a laser processing step, positioning a focal point of a laser beam of wavelengths passing through the wafer inside the wafer, irradiating the focal point with the laser beam while moving the focal point and the wafer relative to each other in a direction parallel to the front side, and forming a modified layer along the predetermined dividing lines inside the wafer; and a dividing step, dividing the wafer starting from the modified layer to manufacture multiple device chips, wherein text, numbers, or markings indicating information related to the resistivity of the wafer are formed on the wafer, and in the laser processing step, irradiating the wafer with the laser beam according to irradiation conditions determined based on the resistivity of the wafer obtainable from the text, numbers, or markings indicating information related to the resistivity of the wafer.

[0020] It is known that the transmittance of light of a specific wavelength through a wafer is affected by factors such as the impurity concentration of the wafer. Furthermore, it is known that the resistivity of the wafer is determined by the impurity concentration. That is, the irradiation conditions of the laser beam illuminating the wafer can be determined based on the resistivity of the wafer.

[0021] Furthermore, in one embodiment of the present invention, the wafer, the wafer manufacturing method, and the device chip manufacturing method, text, numbers, or markings indicating information related to the resistivity of the wafer are formed on the wafer. For example, when cutting the wafer from the ingot, the resistivity of the ingot (wafer) is measured, and the ingot's breaking condition is determined based on the measured resistivity value. At this time, a number indicating the obtained measurement value is pre-printed inside the wafer.

[0022] In this case, when the wafer is subsequently irradiated with a laser beam to form a modified layer inside the wafer as a starting point for cleavage, the resistivity of the wafer is obtained by reading the text, numbers, or markings formed on the wafer that indicate information related to the wafer's resistivity. Therefore, when determining the irradiation conditions for the laser beam, the resistivity of the wafer can be determined quickly without having to measure it again.

[0023] Therefore, according to the present invention, a wafer, a method for manufacturing the wafer, and a method for manufacturing a device chip are provided that allow for rapid determination of the processing conditions of the wafer without measuring the transmittance of the laser beam on the wafer. Attached Figure Description

[0024] Figure 1 (A) is a schematic three-dimensional view of the chip. Figure 1 (B) is a schematic cross-sectional view of the wafer.

[0025] Figure 2 It is a schematic three-dimensional view of the ingot.

[0026] Figure 3 It is a three-dimensional diagram schematically showing the grinding process.

[0027] Figure 4 It is a three-dimensional diagram schematically showing the grinding process.

[0028] Figure 5 This is a perspective view illustrating an example of the information printing process.

[0029] Figure 6 This is a perspective view schematically showing the application of protective components to the ingot.

[0030] Figure 7 (A) is a perspective view schematically illustrating the steps of the peel layer formation process. Figure 7 (B) is a schematic cross-sectional view showing an ingot undergoing laser processing.

[0031] Figure 8 (A) is a schematic top view showing an ingot with a peeling layer formed inside. Figure 8 (B) is a schematic cross-sectional view showing an ingot with a peeling layer formed inside.

[0032] Figure 9 This is a perspective view illustrating another example of the information printing process.

[0033] Figure 10 (A) is a schematic perspective view illustrating the laser processing steps. Figure 10 (B) is a schematic cross-sectional view showing a wafer undergoing laser processing.

[0034] Figure 11 (A) is a schematic cross-sectional view showing a wafer being loaded into an expansion device. Figure 11 (B) is a cross-sectional view schematically showing the segmentation steps.

[0035] Figure 12 (A) is a flowchart illustrating the steps of an example of a wafer manufacturing method. Figure 12 (B) is a flowchart illustrating the steps of another example of a wafer manufacturing method. Figure 12 (C) is a flowchart illustrating the steps of the manufacturing method for the device chip.

[0036] Label Explanation

[0037] 1: Wafer; 1a: Front side; 1b: Back side; 3: Text, numbers, or markings; 5: Notch; 7: Ingot; 9, 9a, 9b: Protective components; 11: Ingot; 13, 15: Orientation planes; 17: Normal; 19: C-axis; 21: C-plane; 23: Release layer; 25: Modified layer; 27: Crack; 29: Pre-cut dividing line; 31: Device; 33: Strip; 35: Annular frame; 37: Frame unit; 39: Modified layer; 41: Device chip; 2: Grinding device; 4, 20, 36, 42: Chuck stage; 4a, 20a, 36a, 42a: 6: Grinding unit; 8, 24: Spindle; 10, 26: Grinding wheel mounting base; 12, 28: Fixture; 14: Grinding wheel; 16: Grinding tool; 18: Grinding device; 22: Grinding unit; 30: Grinding wheel; 32: Grinding pad; 34, 40, 46: Laser processing device; 38, 44, 48: Laser processing unit; 38a, 44a, 48a: Laser beam; 44b: Focusing point; 50: Extension device; 52: Drum; 54: Frame holding unit; 56: Fixture; 58: Frame support platform; 60: Rod; 62: Cylinder. Detailed Implementation

[0038] Embodiments of the present invention will be described with reference to the accompanying drawings. First, the chip of this embodiment will be described. Figure 1 (A) is a perspective view schematically showing the chip 1 of this embodiment. Figure 1 (B) is a schematic cross-sectional view of the wafer 1 of this embodiment.

[0039] The wafer 1 is, for example, a disc-shaped substrate formed of silicon (Si), silicon carbide (SiC), gallium nitride (GaN), or other semiconductor materials. Alternatively, the wafer 1 is formed of materials such as composite oxides of lithium tantalate (LT) and lithium niobate (LN), or sapphire (Al2O3).

[0040] Multiple intersecting dicing lines are formed on the front side 1a of wafer 1, and devices such as ICs, LSIs, and LEDs are formed in the areas divided by these dicing lines. Furthermore, when the wafer is diced along the dicing lines, individual device chips can be formed. For example, if wafer 1 is a SiC ingot, wafer 1 is used for the manufacture of power devices such as inverters and converters.

[0041] In this embodiment, text, numbers, or markings 3 representing information related to resistivity are formed on the front side 1a, back side 1b, or inside of the wafer 1. For example, when determining processing conditions such as the irradiation conditions of the laser beam when irradiating the wafer 1 to cleave the wafer 1, the text, numbers, or markings 3 representing information related to resistivity are referred to.

[0042] Even when the text, number, or mark 3 is formed inside the wafer 1, it can be read as long as the wafer 1 is transparent. Furthermore, even when the wafer 1 is opaque, it can be read using light of the wavelength that passes through the wafer 1. When the text, number, or mark 3 is formed inside the wafer 1, it is not easily removed even after processing the wafer 1.

[0043] The following describes the process of manufacturing a wafer 1 having text, numbers, or markings 3 that represent information related to resistivity, and the process of manufacturing a device chip using the wafer 1, thereby further explaining the wafer 1.

[0044] Figure 2 This is a schematic perspective view of ingot 7, which serves as the raw material for wafer 1. Ingot 7 is formed, for example, by the Czochralski method, in which a seed crystal is brought into contact with a molten component and pulled. For example, in the case of manufacturing a single crystal ingot made of semiconductor materials such as silicon, boron or phosphorus can be mixed into the molten component as a dopant. However, the manufacturing method of ingot 7 is not limited to this.

[0045] When ingot 7 is a single crystal ingot, the crystal orientation of ingot 7 is measured, and a notch 5, or a cut portion called an orientation plane, is formed in ingot 7 to indicate the crystal orientation. In this case, the notch 5 and the like also remain on the wafer 1 cut from ingot 7, so the crystal orientation of the wafer 1 can be confirmed by referring to the notch 5 and the like.

[0046] Next, the method for manufacturing wafer 1 according to this embodiment, which manufactures wafer 1 from ingot 7, will be described. Figure 12 (A) is a flowchart illustrating the process of each step in the manufacturing method of wafer 1 according to this embodiment.

[0047] In the wafer 1 manufacturing method of this embodiment, a slicing step S10 is first performed to slice the ingot 7 to generate multiple wafers 1. In the slicing step S10, the ingot 7 is cut using, for example, a wire cutter (not shown) with linear serrations. When the cylindrical ingot 7 is cut at predetermined intervals along a plane perpendicular to the extending direction of the cylindrical ingot 7 using the wire cutter, the wafer 1 is cut.

[0048] Here, a processing strain layer caused by the wire cutting process is formed on the front side 1a and back side 1b of the wafer 1, which has just been cut by the wire cutting machine. Therefore, the front side 1a and back side 1b of the wafer 1 are ground to a predetermined thickness, and then the front side 1a and back side 1b of the wafer 1 are polished to a flat surface that can be described as a mirror finish. Thus, a wafer 1 of a predetermined thickness suitable for forming a device is obtained.

[0049] That is, after the slicing step S10 is performed, a grinding step S20 is performed to grind the wafer 1 generated by the slicing step S10 to a specified thickness, and a grinding step S30 is performed to polish the ground wafer 1. Figure 3 This is a perspective view schematically illustrating grinding step S20.

[0050] In grinding step S20, a grinding apparatus 2 is used. The grinding apparatus 2 includes: a chuck stage 4, which attracts and holds the wafer 1, which is the workpiece; and a grinding unit 6, which grinds the workpiece held by the chuck stage 4. The chuck stage 4 has a porous component (not shown) on its upper surface with a diameter equal to that of the wafer 1, which serves as a holding surface 4a for placing the wafer 1. The porous component is connected to an attraction source (not shown), and the chuck stage 4 is able to attract and hold the wafer 1 placed on the holding surface 4a.

[0051] The grinding unit 6 has a spindle 8 running approximately perpendicular to the holding surface 4a and a rotary drive source (not shown) such as an electric motor connected to the upper end of the spindle 8. A circular grinding wheel mounting base 10, with a diameter similar to that of the wafer 1, is provided at the lower end of the spindle 8. An annular grinding wheel 14 is fixed to the lower surface of the grinding wheel mounting base 10 by means of bolts or other fixing devices 12. Grinding tools 16 arranged in a circular pattern are mounted on the lower surface of the grinding wheel 14. The grinding tools 16 have abrasive grains such as diamond and a bonding material that disperses and fixes these abrasive grains.

[0052] In grinding step S20, the wafer 1 is first placed on the holding surface 4a of the chuck stage 4. Then, the suction source is activated, and the chuck stage 4 uses this suction to hold the wafer 1. At this time, the surface of the wafer 1 to be ground is exposed upwards, and the side opposite to the surface to be ground faces the holding surface 4a. Additionally, to protect the un-ground surface of the wafer 1, a protective member 9 can be pre-attached to this surface.

[0053] Furthermore, the chuck stage 4 is rotated about an axis approximately perpendicular to the holding surface 4a, and the spindle 8 is rotated. Then, the chuck stage 4 and the grinding unit 6 are moved relative to each other in a manner that brings them closer together, so that the grinding wheel 16, which is moving on a circular track, comes into contact with the surface of the wafer 1 to be ground. Thus, the wafer 1 is ground and thinned.

[0054] After grinding one side of wafer 1, the other side of wafer 1 is ground in the same way, thus completing the grinding of both sides of wafer 1. As a result, the processing strain layer formed on the front side 1a and back side 1b of wafer 1 due to the cutting of spindle 11 by the wire cutting machine becomes thinner, and wafer 1 is thinned to the specified thickness.

[0055] After the grinding step S20 is performed, the polishing step S30 is performed to polish one or both of the front side 1a or the back side 1b of the wafer 1 that has been ground by the grinding step S20. Figure 4 This is a perspective view schematically showing the grinding step S30. In the grinding step S30, a grinding apparatus 18 is used. The grinding apparatus 18 is configured similarly to the grinding apparatus 2, and has a chuck stage 20 for attracting and holding the wafer 1 and a grinding unit 22 for grinding the wafer 1.

[0056] The upper surface of the chuck table 4 serves as the holding surface 20a. The grinding unit 22 has a spindle 24 and a rotary drive source (not shown) such as a motor connected to the upper end of the spindle 24. A grinding wheel mounting base 26 is provided at the lower end of the spindle 24, and a grinding wheel 30 is fixed to the lower surface of the grinding wheel mounting base 26 by means of a fixing device 28. A grinding pad 32 is fixed to the lower surface of the grinding wheel 30.

[0057] In the polishing step S30, similar to the grinding step S20, the chuck stage 20 and spindle 24 are rotated while the polishing pad 32 comes into contact with the surface of the wafer 1 to be polished. Additionally, in the polishing step S30, a protective member 9a can be pre-attached to the surface of the wafer 1 opposite to the surface to be polished.

[0058] In the polishing step S30, it is preferable to polish at least one of the front side 1a and back side 1b of the wafer 1, where the device is formed, and more preferably to polish both sides. When the polishing step S30 is performed, the processing strain layer formed on the polished surface is removed, and the wafer 1 is processed into a mirror surface.

[0059] In the wafer manufacturing method of this embodiment, a resistivity measurement step S40 is further performed to measure the resistivity of wafer 1, and an information printing step S50 is performed to form text, numbers, or markings 3 representing information related to the measured resistivity. The resistivity measurement step S40 and the information printing step S50 are performed after the slicing step S10. For example, they can be performed before the grinding step S20 or after the polishing step S30.

[0060] In resistivity measurement step S40, the resistivity of wafer 1 is measured using a known method. For example, the resistivity of wafer 1 can be measured using a resistance meter "EC-80C" manufactured by NAPSON Corporation, which uses the eddy current method to measure the resistivity of wafer 1. Alternatively, the resistivity of wafer 1 can also be measured using a contact-type resistance meter such as the four-terminal method. There is no particular limitation on the method for measuring the resistivity of wafer 1, but when using a non-contact resistance meter, it is less likely to cause damage to wafer 1, so a non-contact resistance meter is preferred.

[0061] In the information printing step S50, text, numbers, or markings 3 representing information related to the resistivity of the wafer 1 measured and obtained using the resistivity measurement step S40 are formed on the wafer 1. Figure 5 This is a perspective view schematically illustrating an example of information printing step S50. Information printing step S50 is implemented, for example, using a laser processing device 34.

[0062] The laser processing apparatus 34 includes: a chuck stage 36, the upper surface of which serves as a holding surface 36a for attracting and holding the wafer 1; and a laser processing unit 38, which performs laser processing on the wafer 1 held by the chuck stage 36 by irradiating it with a laser beam. The chuck stage 36 is configured similarly to the chuck stage 4 of the grinding apparatus 2. The laser processing unit 38 includes a laser oscillator (not shown) that emits a laser beam and a focusing lens (not shown) that converges the laser beam emitted by the laser oscillator.

[0063] The laser processing unit 38 can, for example, focus a laser beam 38a of wavelength that passes through the wafer 1 at a predetermined height position inside the wafer 1 to form a modified layer near the focusing point. For example, if the wafer 1 is a SiC wafer, the laser beam 38a is irradiated under the following conditions, focusing at a height position of about 100 μm downward from the front side 1a.

[0064] Wavelength: 1064nm

[0065] Repetition frequency: 140kHz

[0066] Average output: 1.0W

[0067] The chuck stage 36 and the laser processing unit 38 can move relative to each other in a direction parallel to the holding surface 36a. When the chuck stage 36 and the laser processing unit 38 move relative to each other while irradiating the wafer 1 with a laser beam 38a, the position of the focusing point can be controlled, and a modified layer can be formed at a desired location. Furthermore, in the information printing step S50, a modified layer with a predetermined planar shape is formed, for example, inside the wafer 1, thereby forming text, numbers, or markings 3 on the wafer 1 that represent information related to resistivity.

[0068] Alternatively, the text, numbers, or markings 3 indicating information related to the resistivity of wafer 1 may not be formed inside wafer 1, but rather on the front side 1a or the back side 1b. In this case, for example, a laser beam 38a of the wavelength absorbed by wafer 1 is focused onto the front side 1a or the back side 1b of wafer 1 using a laser processing apparatus 34, and a processing mark is formed on the front side 1a of wafer 1 by ablation. That is, a processing mark of a predetermined shape is formed, thereby engraving text, numbers, or markings 3 on the front side 1a or the back side 1b.

[0069] Here, the text, numbers, or markings representing information related to resistivity are, for example, a combination of a number representing the measured resistivity value of the wafer 1 obtained by resistivity measurement step S40 and a text representing the unit of that measured value. Alternatively, it could be text indicating the level to which the resistivity belongs when resistivity is classified into multiple prescribed levels. Or it could be a barcode or QR code, or other markings that store the measured resistivity value or the level to which the resistivity belongs.

[0070] As explained above, the wafer manufacturing method of this embodiment can manufacture a wafer 1 in which text, numbers or markings 3 representing information related to resistivity are formed at least at one of the front side 1a, the back side 1b or the interior.

[0071] Multiple devices are then formed on the front side 1a of the manufactured wafer 1. When the wafer 1 is then diced according to each device, individual device chips are obtained. The text, numbers, or markings 3 formed on the wafer 1 that represent information related to resistivity are read out when the wafer 1 is diced and are used as a reference when determining processing conditions such as laser beam irradiation conditions when dicing the wafer 1.

[0072] Alternatively, wafer 1 can also be manufactured by cutting from a moat using other methods. Next, a wafer manufacturing method according to another embodiment will be described. In this wafer manufacturing method according to another embodiment, a separation surface is set at a predetermined depth inside the cylindrical moat 11, a modified layer as a release layer is formed along the separation surface, and the moat 11 is cut using the release layer to manufacture wafer 1.

[0073] exist Figure 6 It includes a perspective view schematically showing ingot 11. Figure 8 (B) is a schematic enlarged cross-sectional view of the ingot 11 having the modified layer 25 constituting the peeling layer 23 and the crack 27. The ingot 11 has a front side 11a and a back side 11b opposite to the front side 11a. The front side 11a and the back side 11b are parallel to each other.

[0074] For example, in the case where ingot 11 is a single-crystal SiC ingot, such as Figure 6 As shown, a first orientation plane 13 and a second orientation plane 15 perpendicular to the first orientation plane 13 are formed. The length of the first orientation plane 13 is longer than the length of the second orientation plane 15.

[0075] The ingot 11, being a single-crystal SiC ingot, has a c-axis 19 inclined at an angle α relative to the normal 17 of its end face (front face 11a) toward the direction of the second orientation plane 15, and a c-plane 21 perpendicular to the c-axis 19. This c-axis 19 extends, for example, from the end face (front face 11a) to the opposite end face (back face 11b). The c-plane 21 is inclined at an angle α relative to the front face 11a of the ingot 11. Typically, in a SiC ingot, the direction perpendicular to the extension direction of the shorter second orientation plane 15 is the inclination direction of the c-axis 19.

[0076] The c-face 21 is set infinitely at the molecular level in the SiC ingot. The deviation angle α is set to, for example, 4°. However, the deviation angle α is not limited to 4°, and the SiC ingot can be manufactured freely within the range of 1° to 6°. However, the ingot 11 is not limited to a SiC ingot.

[0077] Each step of the wafer manufacturing method of this other embodiment will be described. Figure 12 (B) is a flowchart illustrating the steps of the wafer manufacturing method according to this other embodiment. In this wafer manufacturing method, a planarization step S60 is first performed to planarize the end face (front side 11a or back side 11b) of the ingot 11. Additionally, as... Figure 6 As shown, before performing the planarization step S60, a protective member 9b can be attached to the side of the spindle 11 opposite to the end face to be ground.

[0078] In the planarization step S60, the end face of the ingot 11, which serves as the irradiated surface of the laser beam, is ground and planarized as described later. When the end face is planarized, the laser beam can be neatly incident from the end face into the interior of the ingot 11, thereby appropriately focusing the laser beam to a predetermined position. In the planarization step S60, for example, using… Figure 4 The grinding apparatus 18 described herein grinds the end face of the ingot 11.

[0079] Furthermore, after performing the planarization step S60, a resistivity measurement step S70 is performed to measure the resistivity of the ingot 11 on the planarized end face. The resistivity measurement step S70 is performed in the same manner as the resistivity measurement step S40 described above.

[0080] Next, the peeling layer formation step S80 is performed. Figure 7 (A) is a perspective view schematically illustrating step S80 of the peel layer formation. Figure 7 (B) is a schematic cross-sectional view of the ingot 11 during the formation of the modified layer 25 constituting the peeling layer 23 in the peeling layer formation step S80. Furthermore, Figure 8 (A) is a schematic top view showing an ingot 11 with a modified layer 25 formed thereon. Figure 8(B) is a schematic enlarged cross-sectional view of the ingot 11, showing the modified layer 25 constituting the peeling layer 23 and the crack 27. Additionally, in Figure 8 In the sectional view shown in (B), the shading lines that should have been added are omitted.

[0081] The peel layer formation step S80 is performed using a laser processing apparatus 40, which is compatible with laser processing equipment. Figure 5 The laser processing apparatus 34 described herein is similarly configured. The laser processing apparatus 40 includes: a chuck stage 42, the upper surface of which serves as a holding surface 42a; and a laser processing unit 44, which is capable of performing laser processing on the wafer 1 held by the chuck stage 42.

[0082] In the stripping layer formation step S80, the spindle 11 is first placed on the chuck table 42 of the laser processing apparatus 40, and the attraction and holding mechanism of the chuck table 42 is activated to attract and hold the spindle 11 on the chuck table 42. Next, the laser processing unit 44 is moved above the spindle 11, and the optical system of the laser processing unit 44 or the height of the laser processing unit 44 is adjusted, thereby positioning the focusing point 44b of the first laser beam 44a emitted from the laser processing unit 44 at a predetermined height.

[0083] Here, the predetermined height at which the focusing point 44b of the first laser beam 44a is positioned is a pre-set height position at a predetermined depth from the front surface 11a of the ingot 11 of the spindle. The spindle surface is a surface set parallel to the front surface 11a inside the ingot 11, and is the surface from which the ingot 11 is to be broken. The spindle surface is a surface that leaves the front surface 11a of the ingot 11 at a depth equivalent to the thickness of the wafer 1 manufactured from the ingot 11.

[0084] In the stripping layer formation step S80, a focusing point 44b of a first laser beam 44a with a wavelength that is transparent to the ingot 11 is positioned on the separation surface. Meanwhile, the focusing point 44b and the chuck stage 42 are moved relative to each other along the separation surface, while the first laser beam 44a is irradiated onto the ingot 11 from the front side 11a.

[0085] More specifically, in the stripping layer forming step S80, the processing feed step S81, which moves the ingot 11 and the focusing point 44b relative to each other in the first direction to form a linear modified layer 25, and the indexing feed step S82, which moves the ingot 11 and the focusing point 44b relative to each other in the second direction, are repeated.

[0086] Here, the first direction is a direction perpendicular to the direction in which the deviation angle α is formed and parallel to the end face (front 11a), and is parallel to the orientation plane 15. Furthermore, the second direction is a direction in which the deviation angle α is formed and parallel to the end face (front 11a), and is parallel to the orientation plane 13.

[0087] When the laser beam 44a is focused into the interior of the ingot 11, a modified layer 25 is formed near the focusing point 44b. Furthermore, cracks 27 extend from the formed modified layer 25. For example, in the case where the ingot 11 is a SiC ingot, when the modified layer 25 is formed along the second orientation plane 15, cracks 27 readily extend along the c-plane 21 of the ingot 11 (see reference). Figure 8 The trend of (B) etc. extending.

[0088] Furthermore, when multiple linear modified layers 25 are formed along the separation surface and cracks 27 extend from each modified layer 25, a state is achieved where modified layers 25 or cracks 27 are formed throughout the entire region of the separation surface. Additionally, in Figure 7 (A) Figure 7 (B) and Figure 8 In (A), for ease of explanation, the modified layer 25 formed inside the ingot 11 is shown in dashed lines, and the crack 27 is omitted.

[0089] When the modified layer 25 and crack 27 are formed along the separation surface, the ingot 11 can easily separate from the modified layer 25 and crack 27. That is, the modified layer 25 and crack 27 function as the peeling layer 23. In the peeling layer forming step S80, the peeling layer 23 is formed inside the ingot 11 along the separation surface. The peeling layer 23 includes the modified layer 25 and the crack 27 extending from the modified layer 25.

[0090] Here, the irradiation conditions of the first laser beam 44a will be explained. When irradiating the ingot 11 with the first laser beam 44a of a wavelength that transmits through the ingot 11, in order for the first laser beam 44a to reach the focusing point 44b under appropriate conditions, the irradiation conditions need to be adjusted according to the transmittance of light of that wavelength in the ingot 11.

[0091] Furthermore, the light transmittance of ingot 11 depends on the concentration of impurities contained in ingot 11. Additionally, the resistivity of ingot 11 changes depending on the concentration of impurities contained in it. Therefore, by measuring the resistivity of ingot 11, the irradiation conditions of the first laser beam 44a can be determined. Thus, in the stripping layer formation step S80, the irradiation conditions of the first laser beam 44a can be determined based on the resistivity of ingot 11 measured in the resistivity measurement step S70.

[0092] For example, if ingot 11 is a SiC ingot, and the resistivity of ingot 11 measured by resistivity measurement step S70 is 100 mΩ·cm or less, then ingot 11 can be considered a low-resistivity product. In particular, if ingot 11 is a low-resistivity product with a resistivity of 16 mΩ·cm or more and 22 mΩ·cm or less, the first laser beam 44a can be irradiated onto ingot 11 under the following irradiation conditions.

[0093] Wavelength: 1064nm

[0094] Repetition frequency: 30kHz

[0095] Average output: 5.4W

[0096] Concentration depth: 300μm

[0097] Additionally, for example, if the result measured by resistivity measurement step S70 is that the SiC ingot, i.e., ingot 11, cannot be considered a low-resistivity product, the ingot 11 can be irradiated with the first laser beam 44a under the following irradiation conditions.

[0098] Wavelength: 1064nm

[0099] Repetition frequency: 80kHz

[0100] Average output: 3.2W

[0101] Concentration depth: 300μm

[0102] Thus, in the stripping layer formation step S80, the irradiation conditions of the first laser beam 44a are adjusted according to the resistivity of the ingot 11, thereby enabling the stripping layer 23 to be appropriately formed inside the ingot 11. Furthermore, the conditions adjusted according to the resistivity of the ingot 11 are not limited to those described above; other conditions may also be adjusted.

[0103] Next, the information printing step S90 will be explained. The information printing step S90 can be implemented in the same way as the information printing step S50 described above, so the explanation of the information printing step S50 can be referred to as appropriate. Figure 9 This is a perspective view schematically illustrating the information printing step S90. The information printing step S50 can be performed, for example, using the laser processing apparatus 40 that has performed the peel layer forming step S80, after the peel layer forming step S80.

[0104] In the information printing step S90, on the wafer 1 formed by peeling it from the ingot 11 using the release layer 23, text, numbers, or markings 3 representing information related to the resistivity of the ingot 11 measured in the resistivity measurement step S70 are formed in an area where no devices will be formed thereafter. These text, numbers, or markings 3 are formed, for example, at the end of the ingot 11.

[0105] Here, in the information printing step S90, the text, numbers or markings 3 are formed on one or both of the planarized end face (front face 11a) or interior of the ingot 11 by the second laser beam 44c emitted from the laser processing unit 44.

[0106] For example, a second laser beam 44c, the wavelength of which passes through the ingot 11, can be focused to a height position inside the ingot 11 that is shallower than the stripping layer 23 to form a modified layer, thereby forming text, numbers, or markings 3 composed of the modified layer. In this case, the wavelength of the second laser beam 44c can be the wavelength that passes through the ingot 11, and the ingot 11 can be irradiated according to the following irradiation conditions.

[0107] Wavelength: 1064nm

[0108] Repetition frequency: 140kHz

[0109] Average output: 1.0W

[0110] Concentration depth: 100μm

[0111] In addition, when the text, number or mark 3 is formed on the front side 11a of the ingot 11, the second laser beam 44c of the wavelength absorbed by the ingot 11 can be focused onto the front side 11a of the ingot 11, and the text, number or mark 3 can be formed by ablation.

[0112] Furthermore, the information printing step S90 can be performed before or after the peeling layer forming step S80. However, when the information printing step S90 is performed after the peeling layer forming step S80, the text, numbers, or marks 3 formed on the ingot 11 will not hinder the formation of the peeling layer 23.

[0113] After the information printing step S90 is performed, the wafer generation step S100 is performed, in which the ingot 11 is divided starting from the release layer 23, and the generated wafer 1 is peeled off to generate the wafer 1. In the wafer generation step S100, the ingot 11, which has the release layer 23 formed inside, is divided, for example, by subjecting the ingot 11 to ultrasonic vibration. However, the method of peeling off the wafer 1 is not limited to this.

[0114] When ingot 11 is divided, a wafer 1 is obtained with text, numbers, or markings 3 indicating information related to resistivity formed on its interior or front side. As explained above, based on the utilization Figure 12 The manufacturing method of wafer 1, which is illustrated by the flowchart of (B), manufactures wafer 1 having text, numbers or markings 3 forming on the inside or front side that represent information related to resistivity.

[0115] Next, a method for manufacturing device chips will be described. This method involves laser processing a wafer 1 with text, numbers, or markings 3 that represent information related to resistivity and with multiple devices formed on the front side 1a to divide the wafer into multiple device chips. Figure 12 (C) is a flowchart illustrating the steps of the manufacturing method for the chip of this device.

[0116] exist Figure 10 (A) includes a perspective view schematically showing a wafer 1 undergoing laser processing. First, wafer 1 will be described. In the manufacturing method of this device chip, wafer 1 manufactured by the wafer manufacturing method described above is used, for example.

[0117] For wafer 1, multiple intersecting pre-defined dividing lines 29 are set on the front side 1a. Photolithography and other processes are pre-implemented in each area divided by the pre-defined dividing lines 29 on the front side 1a of wafer 1 to form devices 31 such as ICs, LSIs or LEDs.

[0118] Furthermore, the wafer 1, which undergoes laser processing, is pre-integrated with an annular frame 35 made of a material such as metal via a dicing tape 33, and is operated as part of a frame unit 37. When the frame unit 37 containing the wafer 1 is formed, the operation of the wafer 1 and the manufactured device chip becomes easier, and damage to the wafer 1 and the like can be prevented.

[0119] Laser processing of wafer 1 Figure 10 The laser processing apparatus 46 shown in (A) is configured similarly to the laser processing apparatuses 34 and 40 described above. Figure 10 In (A), the chuck table that holds the frame unit 37 is omitted.

[0120] In the manufacturing method of this device chip, the first step is the loading step S110, in which the wafer 1 in the frame unit 37 state is loaded into the laser processing apparatus 46. In the loading step S110, the wafer 1 in the frame unit 37 state is placed on a chuck stage (not shown), and the wafer 1 is attracted and held by the chuck stage through the belt 33. Furthermore, the wafer 1 is positioned below the laser processing unit 48.

[0121] Next, laser processing step S120 is performed, in which the wafer 1 is laser-processed using laser processing unit 48. Figure 10 (A) is a perspective view schematically showing laser processing step S120. Figure 10 (B) is a schematic cross-sectional view showing the wafer 1 undergoing laser processing.

[0122] In the laser processing step S120, a focal point 48b of a laser beam 48a of wavelength that passes through the wafer 1 is positioned inside the wafer 1. While moving the focal point 48b and the wafer 1 relative to each other in a direction parallel to the front surface 1a, the laser beam 48a is irradiated onto the focal point 48b. As a result, a modified layer 39 along the predetermined dividing line 29 is formed inside the wafer 1.

[0123] To explain in more detail: First, the chuck stage is rotated to align the predetermined dividing line 29 of the wafer 1 with the processing feed direction of the laser processing apparatus 46. Then, the relative positions of the chuck stage and the laser processing unit 48 are adjusted such that the laser processing unit 48 is positioned above the extension line of the predetermined dividing line 29. Finally, the focusing point 48b of the laser beam 48a is positioned at a predetermined height.

[0124] Next, while irradiating the interior of the wafer 1 with a laser beam 48a from the laser processing unit 48, the chuck stage and the laser processing unit 48 are moved relative to each other along a processing feed direction parallel to the upper surface of the chuck stage. That is, the focal point 48b of the laser beam 48a is positioned inside the wafer 1, and the laser beam 48a is irradiated into the wafer 1 along the predetermined dividing line 29. Thus, a modified layer 39 is formed inside the wafer 1. Furthermore, in Figure 10 In (A), the modified layer 39 formed inside the wafer 1 is shown by dashed lines.

[0125] After forming a modified layer 39 inside the wafer 1 along one predetermined dividing line 29, the chuck stage and the laser processing unit 48 are moved relative to each other in an indexing feed direction perpendicular to the processing feed direction, and the wafer 1 is laser-processed in the same way along the other predetermined dividing lines 29. After forming a modified layer 39 along all predetermined dividing lines 29 in one direction, the chuck stage is rotated about an axis perpendicular to the holding surface, and the wafer 1 is laser-processed in the same way along the predetermined dividing lines 29 in other directions.

[0126] Here, in the laser processing step S120, text, numbers, or markings 3 representing information related to the resistivity of wafer 1 are read, and the irradiation conditions of the laser beam 48a are determined based on the resistivity of wafer 1. For example, if wafer 1 is a low-resistivity SiC wafer, the irradiation conditions of the laser beam 48a in the laser processing step S120 are set as follows.

[0127] Wavelength: 1342nm

[0128] Repetition frequency: 90kHz

[0129] Average output: 2.2W

[0130] Machining feed rate: 700 mm / s

[0131] In addition, when wafer 1 is a high-resistivity SiC wafer, the irradiation conditions of the laser beam 48a in the laser processing step S120 are set as follows, for example.

[0132] Wavelength: 1342nm

[0133] Repetition frequency: 90kHz

[0134] Average output: 1.7W

[0135] Machining feed rate: 700 mm / s

[0136] Furthermore, in the laser processing step S120, the laser beam 48a can be irradiated onto the wafer 1 according to the irradiation conditions based on the properties of the wafer 1 as conceived from its resistivity. For example, in the case of dividing multiple wafers 1 of the same type by laser processing one after another, it is not necessary to read the text, numbers, or markings 3 for all wafers 1 and change the irradiation conditions each time.

[0137] That is, the laser beam 48a can be irradiated onto the wafer according to the irradiation conditions determined based on the resistivity of the wafer 1, which can be obtained from the text, numbers, or markings 3 that indicate information related to the resistivity of the wafer 1. When laser processing is performed on multiple wafers 1 with the same resistivity, the irradiation conditions for irradiating a particular wafer 1 with the laser beam 48a can be determined based on the resistivity that can be obtained from the text, numbers, or markings 3 formed on other wafers 1.

[0138] Furthermore, if the text, number, or mark 3 is formed inside the chip 1, light of a wavelength that passes through the chip 1 can be irradiated and the text, number, or mark 3 can be photographed using a light-receiving element capable of detecting the light. For example, if the chip 1 transmits infrared light, the text, number, or mark 3 can be photographed using infrared light, and a photographing unit having an infrared light source and an infrared light-receiving element can be used to photograph the text, number, or mark 3.

[0139] After performing the laser processing step S120, a slicing step S130 is performed to slice the wafer 1, starting from the modified layer 39, thereby manufacturing multiple device chips. In the slicing step S130, the strip 33 attached to the wafer 1 is extended radially outward, thereby applying force to the wafer 1 and slicing it. In the slicing step S130, a method can be used... Figure 11 (A) and Figure 11 The extension device 50 shown in (B)

[0140] The expansion device 50 includes: a cylindrical drum 52 having a diameter larger than that of the wafer 1; and a frame holding unit 54 including a frame support 58. The frame support 58 of the frame holding unit 54 has an opening with a diameter larger than that of the drum 52 and is disposed at the same height as the upper end of the drum 52, surrounding the upper end of the drum 52 from the outer periphery.

[0141] A clamp 56 is provided on the outer periphery of the frame support platform 58. When the frame unit 37 is placed on the frame support platform 58 and the frame 35 of the frame unit 37 is held by the clamp 56, the frame unit 37 is fixed to the frame support platform 58.

[0142] The frame support platform 58 is supported by a plurality of rods 60 extending in the vertical direction, and a cylinder 62 is provided at the lower end of each rod 60 to raise and lower the rod 60. When the cylinders 62 are actuated, the frame support platform 58 descends relative to the drum 52.

[0143] When extending the belt 33, the height of the frame support 58 is first adjusted by actuating the cylinder 62 so that the height of the upper end of the drum 52 of the extension device 50 is consistent with the height of the upper surface of the frame support 58. Then, the frame unit 37, which is removed from the laser processing device 46, is placed on the drum 52 and the frame support 58 of the extension device 50.

[0144] Then, the frame 35 of the frame unit 37 is fixed to the frame support platform 58 by the clamp 56. Figure 11 (A) is a schematic cross-sectional view showing the frame unit 37 fixed on the frame support 58. A modified layer 39 is formed inside the wafer 1 along the predetermined dividing line 29.

[0145] Next, the cylinder 62 is actuated, causing the frame support 58 of the frame holding unit 54 to descend relative to the drum 52. Thus, as... Figure 11 As shown in (B), band 33 extends radially outward. Figure 11 (B) is a schematic cross-sectional view showing the frame unit 37 with 33 extended.

[0146] As the strip 33 expands, a radially outward force is applied to the wafer 1, dividing the wafer 1 from the modified layer 39 to form individual device chips 41. When the strip 33 is further expanded, the spacing between the individual device chips 41 supported by the strip 33 increases, making it easier to pick up each individual device chip 41.

[0147] As shown above, in the wafer, wafer manufacturing method, and device chip manufacturing method of this embodiment, text, numbers, or markings 3 representing information related to the resistivity of the wafer 1 are formed on the wafer 1. Therefore, when laser processing is performed on the wafer 1 to form a modified layer 39 inside, the irradiation conditions of the laser beam 48a can be determined based on the resistivity of the wafer 1 that can be obtained from the text, numbers, or markings 3.

[0148] When manufacturing device chip 41 by laser processing of wafer 1, it is not necessary to measure the resistivity of wafer 1, which is important to consider during the formation of device 31 on the front side 1a. Therefore, the wafer 1 can be easily and quickly laser processed by irradiating the laser beam 48a under the most suitable irradiation conditions for various wafers 1, thereby improving the processing efficiency of wafer 1 and the manufacturing efficiency of device chip 41.

[0149] Furthermore, the present invention is not limited to the embodiments described above, and various modifications and implementations are possible. For example, in the above embodiments, the irradiation conditions for irradiating the wafer 1 with the laser beam 48a were adjusted and determined based on the resistivity of the wafer 1, but one aspect of the present invention is not limited to this. That is, the irradiation conditions can be determined by considering various factors such as the material or shape of the wafer 1, the focusing depth of the laser beam 48a, in addition to the resistivity of the wafer 1.

[0150] The structure and method of the above embodiments can be appropriately modified and implemented as long as they do not depart from the scope of the purpose of the present invention.

Claims

1. A method for manufacturing a device chip, comprising laser processing a wafer to divide it into multiple device chips, wherein multiple intersecting predetermined dividing lines are formed on the front side of the wafer, and devices are formed in the areas divided by the predetermined dividing lines on the front side, characterized in that... The manufacturing method of this device chip includes the following steps: The loading step involves loading the wafer into the laser processing device; In the laser processing step, the focal point of a laser beam of wavelength that passes through the wafer is positioned inside the wafer. While moving the focal point and the wafer relative to each other in a direction parallel to the front surface, the laser beam is irradiated onto the focal point to form a modified layer along the predetermined dividing line inside the wafer. as well as The dicing step involves dividing the wafer, starting with the modified layer, to manufacture multiple chips of the device. The wafer has text, numbers, or markings formed on it to indicate information related to the resistivity of the wafer. In this laser processing step, the laser beam is irradiated onto the wafer according to irradiation conditions determined based on the resistivity of the wafer, which can be obtained from text, numbers, or markings that indicate information related to the resistivity of the wafer.

Citation Information

Patent Citations

  • Semiconductor wafer and its manufacture

    JP2001076981A

  • Production method of wafer

    JP2016127186A

  • Laser processing method

    JP2019033162A

  • Laser processing method and semiconductor chip

    WO2005098915A1

  • Manufacture of semiconductor device, its manufacture device and semiconductor wafer

    JP1995050328A