Metal polyols for polyurethane polymers

By using metal chelated polyols in polyurethane materials to react with isocyanate to form polyurethane polymers, the smoke opacity and toxic emissions of polyurethane materials under fire conditions are solved, and its antifungal, antimicrobial and odor resistance is improved, achieving Improved fire performance and material properties.

CN114096576BActive Publication Date: 2024-11-29DOW GLOBAL TECHNOLOGIES LLC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202080050073.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-07
Publication Date
2024-11-29
Estimated Expiration
2040-07-07

AI Technical Summary

Technical Problem

The smoke opacity and toxic emissions generated by existing polyurethane materials when burned under fire conditions still need to be improved, and their antifungal, antimicrobial, odor resistance, hardness and friction resistance are insufficient.

Method used

Using metal chelated polyester polyols and metal chelated polyether polyols in isocyanate reactive compositions to form polyurethane polymers by reacting with isocyanate, improving hydrogen cyanide and carbon monoxide emissions during pyrolysis events and enhancing the material's Antifungal, antimicrobial and odor-proof.

Benefits of technology

It significantly improves the smog behavior of polyurethane materials under fire conditions, reduces the emission of hydrogen cyanide and carbon monoxide, and improves the antifungal, antimicrobial and odor resistance of the material, enhancing its overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004897598050000101
    Figure GDA0004897598050000101
  • Figure GDA0004897598050000311
    Figure GDA0004897598050000311
  • Figure GDA0004897598050000312
    Figure GDA0004897598050000312
Patent Text Reader

Abstract

The present disclosure provides a metal chelate polyol liquid and / or a metal chelate polyether polyol liquid, which can be used in an isocyanate reactive composition and a reaction mixture for forming a polyurethane polymer. The metal chelate polyester polyol liquid is a reaction product of a chelate polyester polyol having a chelating portion and a metal compound having a metal ion. The metal chelate polyether polyol liquid is a reaction product of a chelate polyether polyol having a chelating portion and a metal compound having a metal ion. The chelate portion of the chelate polyester polyol or the chelate polyether polyol chelates the metal ion to form the metal chelate polyester polyol liquid or the metal chelate polyether polyol liquid, respectively, having a molar ratio of the metal ion to the chelate portion of 0.05:1 to 2:1.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates generally to polyurethane polymers, and more particularly to polyurethane polymers having improved combustion / smoke behavior. Background Art

[0002] Since the 1960s, polyurethane rigid (PUR) foam has been used in construction as a high-performance thermal insulation material. Continuous technological development in Europe and the U.S. has spawned a next-generation product called polyisocyanurate rigid (PIR) foam. Both PUR and PIR are polyurethane-based foams made from two reactants, i.e., isocyanates (e.g., methyl diphenyl diisocyanate, MDI) and polyols. Although for PUR, isocyanates and polyols are implemented in a ratio close to equilibrium compared to equivalent weight, isocyanates are used in excess during the production of PIR. Isocyanates partially react with themselves, and the resulting PIR is a highly cross-linked synthetic material with a cyclic isocyanurate structure. The high degree of cross-linking and annular structure ensures the high thermal stability of rigid PIR foams. PIR also has excellent thermal stability and dimensional stability.

[0003] PIR foams are also characterized by very good fire behavior due to the inherent charring behavior, which in turn is related to the outstanding thermal stability of the isocyanurate chemical structure. In order to further enhance the formation of char, phosphorus-based flame retardants are usually added. When building products (such as insulating metal panels or insulation boards) are exposed to fire, the insulating PIR core quickly forms a coherent char that helps to protect the underlying materials. This means that only a limited part of the available combustible insulation material is exposed to the fire, and this part actually contributes to the heat release and smoke.

[0004] The combustion behavior of combustible thermoset materials is a complex issue. For example, halogenated flame retardants are very effective in reducing heat release, but may increase smoke opacity. Dow patent publication US 2014 / 0206786A1 describes the use of triethyl phosphate (TEP) as a smoke suppression additive compared to traditional halogenated flame retardants such as tris(2-chloroisopropyl) phosphate (TCPP). In addition, it is well known that the composition of combustion emissions (further than the material itself) depends strongly on the combustion conditions, particularly temperature, geometry and ventilation, including the availability of oxygen. Even though, as described above, the inherent charring behavior of polyisocyanurates limits and / or delays the amount of polymer combustion (thereby limiting and / or delaying the release of heat and smoke), there is still a need to further improve the combustion (combustion / burning) behavior so as to minimize smoke opacity and smoke toxicity.

[0005] Polyurethanes are also widely used in many coatings, adhesives, sealants and elastomers ("CASE") applications and flexible foams. There is a need to further improve combustion / burning behavior, thereby minimizing smoke opacity and smoke toxicity, and optionally improve other properties such as fungal resistance, antimicrobial resistance, odor resistance, hardness, sound insulation and friction resistance of polyurethanes used as coatings, adhesives, sealants and elastomers and foams. Summary of the invention

[0006] The present disclosure provides a metal chelated polyester polyol liquid and / or a metal chelated polyether polyol liquid, either or both of which can be used in an isocyanate reactive composition used in a reaction mixture for forming a polyurethane polymer. During a pyrolysis event (such as a fire), the polyurethane polymer of the present disclosure can have improved smoke behavior in terms of the emission of hydrogen cyanide (HCN) and carbon monoxide (CO).

[0007] For various embodiments, the metal chelated polyester polyol liquid is a reaction product of a chelated polyester polyol having a chelating portion and a metal compound having a metal ion. The chelated polyester polyol is formed by a chemical reaction of a monomer of a liquid polyester polyol or a liquid polyester polyol formed by the monomer of the liquid polyester polyol with a chelating agent having the chelating portion. In other embodiments, the metal chelated polyether polyol liquid is a reaction product of a chelated polyether polyol having a chelating portion and a metal compound having a metal ion. The chelated polyether polyol is formed by a chemical reaction of a monomer of a liquid polyether polyol or a liquid polyether polyol formed by the monomer of the liquid polyether polyol with a chelating agent having the chelating portion.

[0008] The chelating moiety is selected from a dianhydride moiety, an amino-based chelating moiety, and a combination thereof. For these embodiments, the chelating agent having the dianhydride moiety chemically reacts with the monomer of the liquid polyester polyol or the liquid polyester polyol formed by the monomer of the liquid polyester polyol to form the chelated polyester polyol having an aminopolycarboxylic acid moiety. Alternatively, the chelating agent having the amino-based chelating moiety chemically reacts with the monomer of the liquid polyester polyol or the liquid polyester polyol formed by the monomer of the liquid polyester polyol to form a polyester amino polyol as the chelated polyester polyol. The chelating moiety of the chelated polyester polyol chelates the metal ions to form the metal chelated polyester polyol liquid having a molar ratio of the metal ions to the chelating moiety of 0.05:1 to 2:1.

[0009] For these embodiments, the chelating agent with the dianhydride part can react chemically with the liquid polyester polyol at a molar ratio of 1:1.5 to 1:100 (chelating agent mole number: polyester polyol mole number) to form the chelated polyester polyol with amino polycarboxylic acid part. For these embodiments, the chelating agent with the dianhydride part is selected from the group consisting of ethylenediaminetetraacetic acid dianhydride, diethylenetriaminepentaacetic acid dianhydride and combinations thereof. For these embodiments, the chelating agent with the amino-based chelating part is selected from the group consisting of alkoxylated diamines, alkoxylated triamines, alkoxylated tetramines and combinations thereof. For these embodiments, the metal compound is selected from the group consisting of hydroxides, carbonates, carboxylates, alkaline carbonates, metal salts and combinations thereof, and the metal ions are selected from the group consisting of copper, zinc, silver, iron, manganese, cobalt, nickel, zirconium, calcium, aluminum, barium, cadmium, gallium, indium, lead, magnesium, mercury, palladium, scandium, strontium, thorium, titanium, vanadium and combinations thereof. Preferably, the metal compound is a transition metal compound, wherein the transition metal ion is selected from the group consisting of copper, zinc, silver, iron, manganese, cobalt, nickel, titanium, vanadium, cadmium and zirconium. Preferably, the transition metal compound is selected from the group consisting of copper (II) hydroxide, copper (II) carbonate, basic copper (II) carbonate, copper (II) acetate, cobalt (II) acetate, nickel (II) acetate, silver (I) acetate, zinc (II) acetate and combinations thereof.

[0010] In other embodiments, the chelating agent having the dianhydride moiety chemically reacts with the monomer of the liquid polyether polyol or the liquid polyether polyol formed from the monomer of the liquid polyether polyol to form the chelated polyether polyol having an aminopolycarboxylic acid moiety. Alternatively, the chelating agent having the amino-based chelating moiety chemically reacts with the monomer of the liquid polyether polyol or the liquid polyether polyol formed from the monomer of the liquid polyether polyol to form a polyetheramino polyol as the chelated polyether polyol. The chelating moiety of the chelated polyether polyol chelates the metal ions to form the metal chelated polyether polyol liquid having a molar ratio of the metal ions to the chelating moiety of 0.05:1 to 2:1. For these embodiments, the chelating agent with the dianhydride portion can react chemically with the liquid polyether polyol at a molar ratio of 1:1.5 to 1:100 (moles of chelating agent: moles of polyether polyol) to form the chelated polyether polyol with amino polycarboxylic acid portion. For these embodiments, the chelating agent with the dianhydride portion is selected from the group consisting of ethylenediaminetetraacetic acid dianhydride, diethylenetriaminepentaacetic acid dianhydride and combinations thereof. For these embodiments, the chelating agent with the amino-based chelating portion in the polyether polyol is selected from the group consisting of diamines, triamines, tetramines and combinations thereof. For these embodiments, the metal compound is selected from the group consisting of hydroxides, carbonates, carboxylates, alkaline carbonates, metal salts and combinations thereof, and the metal ions are selected from the group consisting of copper, zinc, silver, iron, manganese, cobalt, nickel, zirconium, calcium, aluminum, barium, cadmium, gallium, indium, lead, magnesium, mercury, palladium, scandium, strontium, thorium, titanium, vanadium and combinations thereof. Preferably, the metal compound is a transition metal compound, wherein the transition metal ion is selected from the group consisting of copper, zinc, silver, iron, manganese, cobalt, nickel, titanium, vanadium, cadmium and zirconium. Preferably, the transition metal compound is selected from the group consisting of copper (II) hydroxide, copper (II) carbonate, basic copper (II) carbonate, copper (II) acetate, cobalt (II) acetate, nickel (II) acetate, silver (I) acetate, zinc (II) acetate and combinations thereof.

[0011] The present disclosure also provides an isocyanate reactive composition having a hydroxyl moiety for forming a polyurethane polymer. For these embodiments, the isocyanate reactive composition comprises 0.1 to 100 weight % of the metal chelated polyester polyol liquid, the metal chelated polyether polyol liquid, or a combination of the metal chelated polyester polyol liquid and the metal chelated polyether polyol liquid, each as provided herein, and optionally up to 99.9 weight percent of polyols to form the isocyanate reactive composition, the weight percent being based on the total weight of the isocyanate reactive composition. For these embodiments, the isocyanate reactive composition further comprises a compound selected from the following: 0.1 weight % to 1.5 weight % of phosphorus from a flame retardant compound, preferably a halogen-free flame retardant compound, the weight % of phosphorus being based on the total weight of the isocyanate reactive composition; 0.05 weight % to 3.0 weight % of metals from the metal chelated polyester polyol liquid and / or the metal chelated polyether polyol liquid and a combination thereof, wherein the weight % of metals is based on the total weight of the isocyanate reactive composition. For these embodiments, the isocyanate reactive composition has a molar ratio of the metal to phosphorus (moles of metal:moles of phosphorus) of 0.05: 1 to 5: 1. For these embodiments, the flame retardant compound or halogen-free flame retardant compound is selected from the group consisting of phosphates, phosphonates, phosphinates, phosphites, and combinations thereof.

[0012] The present disclosure also provides a reaction mixture for forming a polyurethane polymer. The reaction mixture comprises an isocyanate compound with an isocyanate moiety and an isocyanate-reactive composition as provided herein, wherein the reaction mixture has a molar ratio of the isocyanate moiety to the hydroxyl moiety of 0.90:1 to 7:1. For these embodiments, the reaction mixture may include a compound selected from the group consisting of water, a catalyst, a surfactant, a blowing agent, or a combination thereof. For these embodiments, the reaction mixture provided herein can be used to form a polyurethane-based polymer, including a polyurethane-based foam.

[0013] The present disclosure also provides a method for preparing a metal chelated polyester polyol liquid. The method includes reacting a monomer of a liquid polyester polyol or a liquid polyester polyol formed by the monomer of the liquid polyester polyol with a chelating agent having a chelating moiety to form a chelated polyester polyol. For these embodiments, the chelating moiety is selected from a dianhydride moiety, an amino-based chelating moiety, and a combination thereof. For these embodiments, the chelating agent having the dianhydride moiety chemically reacts with the monomer of the liquid polyester polyol or the liquid polyester polyol formed by the monomer of the liquid polyester polyol to form the chelated polyester polyol having an aminopolycarboxylic acid moiety. For these embodiments, the chelating agent having the amino-based chelating moiety chemically reacts with the monomer of the liquid polyester polyol or the liquid polyester polyol formed by the monomer of the liquid polyester polyol to form a polyester amino polyol as the chelated polyester polyol. For these embodiments, the method further comprises reacting the chelated polyester polyol having the chelating moiety with a metal compound having a metal ion, wherein the chelating moiety of the chelated polyester polyol chelates the metal ion to form the metal chelated polyester polyol liquid, the reaction having a molar ratio of the metal ion to the chelating moiety of 0.05:1 to 2:1. For these embodiments, the chelating agent having the dianhydride moiety chemically reacts with the liquid polyester polyol formed from the monomer of the liquid polyester polyol at a molar ratio of 1:1.5 to 1:100 (moles of chelating agent: moles of polyester polyol) to form the chelated polyester polyol having an aminopolycarboxylic acid moiety.

[0014] The present disclosure also provides a method for preparing a metal chelated polyether polyol liquid. The method includes reacting a monomer of a liquid polyether polyol or a liquid polyether polyol formed by the monomer of the liquid polyether polyol with a chelating agent having a chelating moiety to form a chelated polyether polyol. For these embodiments, the chelating moiety is selected from a dianhydride moiety, an amino-based chelating moiety, and a combination thereof. For these embodiments, the chelating agent having the dianhydride moiety chemically reacts with the monomer of the liquid polyether polyol or the liquid polyether polyol formed by the monomer of the liquid polyether polyol to form the chelated polyether polyol having an aminopolycarboxylic acid moiety. For these embodiments, the chelating agent having the amino-based chelating moiety chemically reacts with the monomer of the liquid polyether polyol or the liquid polyether polyol formed by the monomer of the liquid polyether polyol to form a polyether amino polyol as the chelated polyether polyol. For these embodiments, the method further comprises reacting the chelated polyether polyol having the chelating moiety with a metal compound having a metal ion, wherein the chelating moiety of the chelated polyether polyol chelates the metal ion to form the metal chelated polyether polyol liquid, the reaction having a molar ratio of the metal ion to the chelating moiety of 0.05: 1 to 2: 1. For these embodiments, the chelating agent having the dianhydride moiety chemically reacts with the liquid polyether polyol formed from the monomer of the liquid polyether polyol at a molar ratio of 1: 1.5 to 1: 100 (moles of chelating agent: moles of polyester polyol) to form the chelated polyether polyol having an aminopolycarboxylic acid moiety. DETAILED DESCRIPTION

[0015] The present disclosure provides a metal chelated polyester polyol liquid and / or a metal chelated polyether polyol liquid, either or both of which can be used in isocyanate reactive compositions and reaction mixtures for forming polyurethane polymers. During a pyrolysis event (such as a fire), the polyurethane polymers of the present disclosure can have improved smoke behavior in terms of the emission of hydrogen cyanide (HCN) and carbon monoxide (CO).

[0016] For these embodiments, the metal chelate polyester polyol liquid is the reaction product of a chelate polyester polyol having a chelate moiety and a metal compound having a metal ion. The chelate polyester polyol is formed by a chemical reaction of a monomer used to form a liquid polyester polyol or a liquid polyester polyol formed by a monomer and a chelating agent having a chelate moiety. In other embodiments, the metal chelate polyether polyol liquid is the reaction product of a chelate polyether polyol having a chelate moiety and a metal compound having a metal ion. The chelate polyether polyol is formed by a chemical reaction of a monomer used to form a liquid polyether polyol or a liquid polyether polyol formed by a monomer and a chelating agent having a chelate moiety.

[0017] The chelating part of the present disclosure is selected from dianhydride part, amino-based chelating part and combination thereof. For these embodiments, the chelating agent with dianhydride part reacts chemically with the monomer for forming liquid polyester polyol or the liquid polyester polyol formed by the monomer to form the chelated polyester polyol with amino polycarboxylic acid part. Alternatively, the chelating agent with amino-based chelating part reacts chemically with the monomer for forming liquid polyester polyol or the liquid polyester polyol formed by the monomer to form the polyester amino polyol as chelated polyester polyol. The chelating part of chelated polyester polyol chelates the metal ions from the metal compound to form the metal chelated polyester polyol liquid. Preferably, the metal chelated polyester polyol liquid has a molar ratio of metal ions to the chelating part of 0.05:1 to 2:1. For these embodiments, the chelating agent with dianhydride part can also react chemically with the liquid polyether polyol to form the chelated polyether polyol with amino polycarboxylic acid part. Alternatively, a chelating agent having an amino-based chelating moiety reacts chemically with a monomer for forming a liquid polyether polyol to form a polyether amino polyol as a chelated polyether polyol. The chelating moiety of the chelated polyether polyol chelates metal ions from a metal compound to form a metal chelated polyether polyol liquid. Preferably, the metal chelated polyether polyol liquid has a molar ratio of metal ions to the chelating moiety of 0.05:1 to 2:1.

[0018] As used herein, the metal chelate polyester polyol liquid and / or the metal chelate polyether polyol liquid is liquid at a pressure of 80 to 25,000 KPa, and is liquid at a temperature above -10°C and below 80°C, preferably below 60°C, more preferably below 40°C, and most preferably below 25°C. As used herein, the metal chelate polyester polyol liquid and / or the metal chelate polyether polyol liquid contains no metal compound particles / solids to a nominal amount of metal compound particles / solids, such that the nominal amount of metal compound particles / solids is less than 0.10 weight percent (wt%), preferably less than 0.01 wt%, and more preferably less than 0.001 wt%, based on the weight of the metal chelate polyester polyol liquid and / or the metal chelate polyether polyol liquid.

[0019] The chelated polyester polyol of the present disclosure is formed by the chemical reaction of the monomer for forming the liquid polyester polyol or the liquid polyester polyol formed by the monomer and the chelating agent with the chelating part. The liquid polyester polyol can be a homopolymer, a random copolymer, a block copolymer, a multi-block copolymer and the end-capped product that can contain the initiator residue in the case of the ring-opening polyester polyol. The liquid polyester polyol can have a low to medium number average molecular weight ranging from 100 to 5,000, preferably 200 to 2,500, more preferably 300 to 1,000 and most preferably 350 to 750. The number average molecular weight can be measured using end group analysis or gel permeation chromatography (GPC) as known in the art. The liquid polyester polyol can also have 1.8 to 4, such as 2 to 3 number average isocyanate reactive group functionality (e.g., hydroxyl) per molecule, wherein each value is an average. A variety of chemical structures can constitute the liquid polyester polyol, at least one of which requires the presence of at least two hydroxyl groups (ie, diol) and is liquid at a pressure of 80 to 25,000 KPa and at a temperature below 80° C. to provide the liquid polyester polyol of the present disclosure.

[0020] For these embodiments, the monomers used to form the liquid polyester polyols may include polyols, such as diols, triols and / or higher hydroxy alcohols, and polyacids, such as dibasic acids and / or tribasic acids, such as carboxylic acids and / or polycarboxylic anhydrides or corresponding polycarboxylic acid esters of lower alcohols, cyclic esters or mixtures thereof, wherein these compounds react as known in the art to form a reaction product of the liquid polyester polyol. Exemplary polyols include, but are not limited to, ethylene glycol, propylene glycol-(1,2) and -(1,3), butanediol-(1,4) and -(2,3), hexanediol-(1,6), octanediol-(1,8), neopentyl glycol, cyclohexanedimethanol (1,4-bis-hydroxy-methylcyclohexane and other isomers), 2-methyl-1,3-propanediol, glycerol, trimethylolpropane, hexanetriol-(1,2,6), butanetriol-(1,2,4), trimethylolethane, pentaerythritol, quinitol, mannitol and sorbitol, methyl glycosides, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, polypropylene glycol, dibutylene glycol, and polybutylene glycol. The polyols may also include polycarbonate polyols such as the reaction products of diols, for example propylene glycol-(1,3), butanediol-(1,4) and / or hexanediol-(1,6), diethylene glycol, triethylene glycol or tetraethylene glycol with diaryl carbonates, for example diphenyl carbonate, dialiphatic carbonates, for example dimethyl carbonate or phosgene, or from the reaction of epoxides and carbon dioxide.

[0021] Polyacid can be aliphatic, alicyclic, aromatic and / or heterocyclic, and they can for example be substituted by halogen atoms, and / or can be undersaturated. Suitable polyacid, acid anhydride and the polycarboxylic acid ester of lower alcohol include but not limited to succinic acid, adipic acid, suberic acid, azelaic acid, sebacic acid, phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, phthalic anhydride, trimellitic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, tetrachlorophthalic anhydride, endomethylenetetrahydrophthalic anhydride, glutaric anhydride, maleic acid, maleic anhydride, fumaric acid, dimerization and trimerization fatty acid (such as oleic acid) optionally mixed with monomer fatty acid, dimethyl terephthalate and terephthalic acid-bis-ethylene glycol ester.

[0022] The cyclic esters may be aliphatic and may be substituted, for example, by alkyl groups, and / or may be unsaturated. Suitable cyclic esters include, but are not limited to, ε-caprolactone, d,l-lactide, glycolide, δ-valerolactone, pivolactone, and the like.

[0023] The liquid polyester polyols may be aromatic, aliphatic or cycloaliphatic, and may include hydrogenated products thereof.

[0024] Preferred examples of liquid polyester polyols include, but are not limited to, polycaprolactone polyols, polypropiolactone polyols, polyglycolide polyols, polypivolylactone polyols, polyvalerolactone polyols, polyethylene adipate polyols, polypropylene adipate polyols, polybutylene adipate polyols, polyhexylene adipate polyols, polyneopentyl adipate polyols, polycyclohexanedimethylene adipate polyols, polyethylene succinate polyols, polypropylene succinate polyols, polybutylene succinate polyols, polyhexylene succinate polyols, polyneopentyl succinate polyols, polycyclohexanedimethyl succinate polyols. succinate) polyol, polyethylene azelate polyol, polypropylene azelate polyol, polybutylene azelate polyol, polyhexanediol azelate polyol, polyneopentyl azelate polyol, polycyclohexanedimethyleneazelate polyol, polyethylene sebacate polyol, polypropylene sebacate polyol, polybutylene sebacate polyol, polyhexanediol sebacate polyol, polyneopentyl sebacate polyol, polycyclohexanedimethylene sebacate (polycyclohexanedimethylene sebacate) polyols, diethylene glycol / terephthalic acid polyols, polyethylene glycol / terephthalic acid polyols, diethylene glycol / phthalic acid or phthalic anhydride polyols, polyethylene glycol / phthalic acid or phthalic anhydride polyols, diethylene glycol / isophthalic acid polyols, polyethylene glycol / isophthalic acid polyols and copolyester polyols thereof.

[0025] More preferred examples of the liquid polyester polyol include polycaprolactone polyol, polyethylene adipate polyol, polypropylene adipate polyol, polybutylene adipate polyol, polyhexylene adipate polyol, polycyclohexanedimethylene adipate polyol, polyethylene succinate polyol, polybutylene succinate polyol, diethylene glycol / terephthalate polyol, polyethylene glycol / terephthalate polyol, diethylene glycol / terephthalate polyol, Polyols of terephthalate, isophthalate and / or phthalate of diethylene glycol and / or polyethylene glycol, and when the average hydroxyl functionality is greater than 2.0, copolyesters of terephthalate, isophthalate and / or phthalate of diethylene glycol and / or polyethylene glycol with optional use of glycerol and / or trimethylolpropane. For various embodiments, the polyester polyols may also be uncapped or capped with ethylene oxide (EO) and / or propylene oxide (PO) as known in the art to provide a hydrophilic or hydrophobic structure. Examples of other liquid polyester polyols include modified aromatic polyester polyols such as those provided under the trade name STEPANPOL PS-2352 (acid value 0.6-1.0 mg KOH / g, hydroxyl value 230-250 mg KOH / g, hydroxyl functionality 2.0, Stepan Company). The liquid polyester polyols may also contain a certain proportion of carboxyl end groups. Liquid polyester polyols formed with lactones such as ε-caprolactone or hydroxycarboxylic acids such as 6-hydroxycaproic acid may also be used.

[0026] Liquid polyether polyols may include those having at least 2, such as 2 or 3, hydroxyl groups per molecule and may be prepared, for example, by polymerization of epoxides / cyclic ethers such as ethylene oxide, propylene oxide, butylene oxide, styrene oxide or epichlorohydrin, either on their own or in the presence of BF3, or by chemical addition of these epoxides, optionally in the form of a mixture (such as a mixture of ethylene oxide and propylene oxide) or in sequence, to starting components having reactive hydrogen atoms such as water, ammonia, ethanol or amines. Examples of suitable starting components include ethylene glycol, propylene glycol-(1,3) or -(1,2), glycerol, trimethylolpropane, 4,4'-dihydroxy-diphenylpropane, aniline, ethanolamine or ethylenediamine. Sucrose-based polyether polyols may also be used. In many cases it is preferred to use polyethers containing a predominant amount of primary OH groups (up to 100% of the OH groups present in the polyether). The nominal functionality of the polyether polyol or copolyether polyol should be at least 2.0. The nominal functionality is preferably 2.5 to 8, more preferably 2.5 to 7 or 2.5 to 6. The hydroxyl equivalent of the polyether polyol or copolyether polyol is at least 85, preferably at least 100, more preferably 150 to 3,200, in some embodiments 250 to 3,000, and in a specific embodiment 300 to 2,500. The polyol can also be formed from a blend, wherein the blend includes a blend of a diol and a triol. The diol can have a number average molecular weight (Mn) of 200 to 8,000 g / mole and the triol has a number average molecular weight (Mn) of 250 to 6,500 g / mole. Other examples of suitable polyether polyols include those polymers or copolymers having a hydroxyl equivalent of at least 75 formed with propylene oxide. The propylene oxide can be 1,3-propylene oxide, but is more typically 1,2-propylene oxide. If it is a copolymer, the comonomer is another copolymerizable alkylene oxide, such as ethylene oxide, 2,3-butylene oxide, tetrahydrofuran, 1,2-hexylene oxide, etc. The copolymer may contain 25% by weight or more, 50% by weight or more, and preferably 75% or more of polymerized propylene oxide, based on the total weight of the polymerized alkylene oxide. The copolymer preferably contains no more than 75% by weight, especially no more than 50% by weight, of polymerized ethylene oxide.

[0027] The chelating agent with chelating moiety is selected from dianhydride moiety, amino-based chelating moiety and combination thereof. The chelating agent with dianhydride moiety can be an aminopolycarboxylic acid dianhydride compound. For example, the aminopolycarboxylic acid dianhydride compound used as the chelating agent with dianhydride moiety is selected from the group consisting of ethylenediaminetetraacetic acid dianhydride, diethylenetriaminepentaacetic acid dianhydride and combination thereof. Other aminopolycarboxylic acid dianhydride compounds used as the chelating agent with dianhydride moiety can include 4,4'-(propane-1,2-diyl)bis(morpholine-2,6-dione), 4,4'-(propane-1,3-diyl)bis(morpholine-2,6-dione), 4,4'-(oxybis(ethane-2,1-diyl))bis(morpholine-2,6-dione) and combination thereof. The chelating agent with an amino-based chelating moiety can be an aminopolycarboxylic acid containing one or more nitrogen atoms connected to two or more carboxyl groups through a carbon atom, and a tertiary polyamino compound having at least two tertiary nitrogens connected through carbon atoms and at least one alcohol group and up to five alcohol groups, which allow the alcohol groups to be connected or incorporated as part of a polyester polyol. For various embodiments, the chelating agent with an amino-based chelating moiety is selected from the group consisting of diamines, triamines, tetramines and combinations thereof. In other embodiments, the chelating agent with an amino-based chelating moiety is selected from the group consisting of alkoxylated diamines, alkoxylated triamines, alkoxylated tetramines and combinations thereof. These alkoxylated amines preferably conform to formula I

[0028]

[0029] wherein R1, R2, R3, R4 and R5 are each independently C1 to C8 alkyl, alkoxylate / polyalkoxylate (i.e. –(CH2CHRO) n-H, wherein R is H or C1 to C3 alkyl and n is an integer from 1 to 10) and equivalents thereof, provided that at least one of R1, R2, R3, R4 and R5 is an alkoxylate / polyalkoxylate as provided above, x and x' are each independently an integer of 2 or 3, and y is an integer of 0, 1 or 2. More preferably, for Formula I, R1, R2, R3, R4 and R5 are each independently C1 to C3 alkyl, an alkoxylate / polyalkoxylate as provided above, wherein the alkyl group is C1 to C2, provided that at least one of R1, R2, R3, R4 and R5 is an alkoxylate / polyalkoxylate as provided above, x and x' are each an integer of 2, and y is an integer of 0 or 1. Specific examples of chelating agents having an amino-based chelating moiety include N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine, N,N,N',N'-tetrakis(2-hydroxyethyl)ethylenediamine, 2-[[2-(dimethylamino)ethyl]methylamino]ethanol, 1-[bis[3-(dimethylamino)propyl]amino-2-propanol], 1,1',1",1"'-((((2-hydroxypropyl)azanediyl)bis(ethane-2,1-diyl))bis(1-[1-hydroxypropyl)-2-ol], 1,1',1",1"'-((((2-hydroxypropyl)azanediyl)bis(ethane-2,1-diyl))bis(1-[1-hydroxypropyl)-2-ol], 1,1',1",1"'-(((2-hydroxypropyl)azanediyl)bis(1-hydroxyethyl)-2-ol) (Azanediyl))tetra(propan-2-ol), 2,2',2",2"'-((((2-hydroxyethyl)azanediyl)bis(ethane-2,1-diyl))bis(azanediyl))tetra(ethane-1-ol), 2,2'-azanediyldiacetic acid, 2,2',2"-nitrilotriacetic acid, ethylenediaminetetraacetic acid, 2-[bis[2-bis(carboxymethyl)amino]ethyl]amino]acetic acid, ethylene glycol-bis(2-aminoethyl ether)-N,N,N',N' -tetraacetic acid, 1,2-bis(o-aminophenoxy)ethane-N,N,N′,N′-tetraacetic acid, 2,2′,2″-(1,4,7-triazanonane-1,4,7-triyl)triacetic acid (NOTA), 1,4,7,10-tetraazacyclododecane-1,4,7,10-tetraacetic acid, N-(N-(3-amino-3-carboxypropyl)-3-amino-3-carboxypropyl)azetidine-2-carboxylic acid, and 2-[2-[[2- Hydroxy-1-(2-hydroxyphenyl)-2-oxoethyl]amino]ethylamino]-2-(2-hydroxyphenyl)acetic acid, N,N-dimethyl-N',N'-2-hydroxy(propyl)-1,3-propylenediamine, N,N,N'-trimethyl-N'-hydroxyethyl-bis(aminoethyl) ether, N,N-bis(3-dimethylaminopropyl)-N-isopropanolamine, bis(dimethylaminopropyl)amino-2-propanol, N,N,N'-trimethylaminopropylethanolamine.

[0030] Chelated polyester polyol is formed by the chemical reaction of the monomer for forming liquid polyester polyol or the liquid polyester polyol formed by the monomer and the chelating agent with chelating part. For this chemical reaction, the monomer for forming liquid polyester polyol or the liquid polyester polyol formed by the monomer can exist with molar excess relative to the chelating agent. The example of the molar ratio for forming chelated polyester polyol includes the ratio in the range of 3:1 to 200:1 (the mole number of the monomer for forming liquid polyester polyol: the mole number of the chelating agent). Preferably, the range is 5:1 to 100:1 (the mole number of the monomer for forming liquid polyester polyol: the mole number of the chelating agent). For the chemical reaction of liquid polyester polyol and the chelating agent with chelating part, the molar ratio for forming chelated polyester polyol includes the ratio in the range of 1.5:1 to 100:1 (the mole number of liquid polyester polyol: the mole number of the chelating agent). Preferably, the range is 3:1 to 50:1 (the mole number of liquid polyester polyol: the mole number of the chelating agent).

[0031] For these embodiments, the chelating agent with dianhydride moiety reacts chemically with the monomer for forming the liquid polyester polyol or the liquid polyester polyol formed by the monomer to form the chelated polyester polyol with amino polycarboxylic acid moiety (acting as the chelating moiety of the chelated polyester polyol). For various embodiments, the acyl group of the dianhydride moiety reacts chemically (e.g., acetylation reaction) with any hydroxyl and / or amine (primary amine and / or secondary amine) of the monomer for forming the liquid polyester polyol or the liquid polyester polyol formed by the monomer. Such reactions can occur with optional alkaline catalysts (e.g., potassium hydroxide, potassium hydride, sodium hydroxide, sodium hydride) at atmospheric pressure (e.g., 101.23KPa) and in a temperature range of 20 to 150°C. The reaction time can vary from 5 minutes to 24 hours. An aliquot of the chelating agent with dianhydride moiety can be added to the monomer for forming the liquid polyester polyol or the liquid polyester polyol formed by the reacted monomer.

[0032] For these embodiments, the chelating agent with dianhydride moiety can react chemically with liquid polyester polyol at a molar ratio of 1:1.5 to 1:100 (molar number of chelating agent: molar number of polyester polyol) to form a chelated polyester polyol with amino polycarboxylic acid moiety, which serves as the chelating moiety of the chelated polyester polyol. Preferably, the chelating agent with dianhydride moiety can react chemically with liquid polyester polyol at a molar ratio of 1:3 to 1:50 (molar number of chelating agent: molar number of polyester polyol) to form a chelated polyester polyol with amino polycarboxylic acid moiety. Most preferably, the chelating agent with dianhydride moiety can react chemically with liquid polyester polyol at a molar ratio of 1:5 to 1:20 (molar number of chelating agent: molar number of polyester polyol) to form a chelated polyester polyol with amino polycarboxylic acid moiety.

[0033] Chelated polyether polyol is formed by the chemical reaction of liquid polyether polyol or monomer for forming liquid polyether polyol and chelating agent with chelating moiety.For this chemical reaction, liquid polyether polyol or monomer for forming liquid polyether polyol exists with molar excess relative to chelating agent.The example of the molar ratio for forming chelated polyether polyol includes the ratio (the mole number of monomer for forming liquid polyether polyol: the mole number of chelating agent) in the range of 2:1 to 200:1.Preferably, the range is 4:1 to 100:1 (the mole number of monomer for forming liquid polyether polyol: the mole number of chelating agent).For the chemical reaction of liquid polyether polyol and chelating agent with chelating moiety, the molar ratio for forming chelated polyether polyol includes the ratio (the mole number of liquid polyether polyol: the mole number of chelating agent) in the range of 2:1 to 100:1.Preferably, the range is 3:1 to 50:1 (the mole number of liquid polyether polyol: the mole number of chelating agent).

[0034] For these embodiments, the chelating agent with the dianhydride moiety reacts chemically with the liquid polyether polyol to form a chelated polyether polyol with an aminopolycarboxylic acid moiety, which acts as a chelating moiety of the chelated polyether polyol. For various embodiments, the acyl group of the dianhydride moiety reacts chemically (e.g., acetylation) with any hydroxyl and / or amine (primary and / or secondary amine) of the liquid polyether polyol. Such reactions can occur with an optional alkaline catalyst (e.g., potassium hydroxide, potassium hydride, sodium hydroxide, sodium hydride) at atmospheric pressure (e.g., 101.23 KPa) and in a temperature range of 20 to 150° C. The reaction time can vary from 5 minutes to 24 hours.

[0035] For these embodiments, the chelating agent with dianhydride moiety can react chemically with liquid polyether polyol at a molar ratio of 1:1.5 to 1:100 (chelating agent mole number: polyether polyol mole number) to form a chelated polyether polyol with amino polycarboxylic acid moiety, and the amino polycarboxylic acid moiety serves as the chelating moiety of the chelated polyether polyol. Preferably, the chelating agent with dianhydride moiety can react chemically with liquid polyether polyol at a molar ratio of 1:3 to 1:50 (chelating agent mole number: polyether polyol mole number) to form a chelated polyether polyol with amino polycarboxylic acid moiety. Most preferably, the chelating agent with dianhydride moiety can react chemically with liquid polyether polyol at a molar ratio of 1:5 to 1:20 (chelating agent mole number: polyether polyol mole number) to form a chelated polyether polyol with amino polycarboxylic acid moiety.

[0036] In other embodiments, the chelating agent having an amino-based chelating moiety reacts chemically with a monomer used to form a liquid polyester polyol or a liquid polyester polyol formed from the monomer to form a polyester amino polyol as a chelated polyester polyol. For various embodiments, the acid or alcohol group of the amino-based chelating moiety (e.g., an aminopolycarboxylic acid containing one or more nitrogen atoms connected to two or more carboxyl groups through a carbon atom or a polyamino alcohol having at least two nitrogen atoms connected to at least one alcohol group and up to five alcohol groups through a carbon atom) can be esterified with the hydroxyl group of the acid of the monomer used to form a liquid polyester polyol or a liquid polyester polyol formed from the monomer, or esterified / esterified with the carboxylic acid of the alcohol (including its derivatives) to form a polyester amino polyol as a chelated polyester polyol. Such reactions can be carried out at atmospheric pressure (e.g., 101.23 KPa), pressures below atmospheric pressure (e.g., 1 KPa), or pressures above atmospheric pressure (e.g., 200 KPa), and at a temperature range of 50 to 150° C. for aminopolycarboxylic acids and 100 to 300° C. for polyamino alcohols. The reaction time can vary from 0.5 hours up to 24 hours.

[0037] For these embodiments, the metal compound is selected from the group consisting of hydroxides, carbonates, carboxylates, alkaline carbonates, nitrates, chlorides, metal salts, and combinations thereof, and the metal ion is selected from the group consisting of metals of Groups 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13 and Periods 3, 4, 5 of the Periodic Table and combinations thereof (IUPAC Periodic Table of Elements, November 28, 2016) and barium, mercury, lead, and thorium. Preferably, the metal ion is selected from the group consisting of copper, zinc, silver, iron, manganese, cobalt, nickel, zirconium, calcium, aluminum, barium, cadmium, gallium, indium, lead, magnesium, mercury, palladium, scandium, strontium, thorium, titanium, vanadium, and combinations thereof. Preferably, the metal compound is a transition metal compound, and the transition metal ion is selected from the group consisting of copper, zinc, silver, iron, manganese, cobalt, nickel, zirconium, cadmium, mercury, palladium, titanium, vanadium, and combinations thereof. More preferably, the transition metal is selected from the group consisting of copper, zinc, silver, iron, manganese, cobalt, nickel, zirconium and combinations thereof. Most preferably, the transition metal is selected from the group consisting of copper, zinc, iron, manganese, cobalt, nickel and combinations thereof. In another most preferred embodiment, the metal compound is selected from the group consisting of hydroxides, carbonates, carboxylates, metal salts and combinations thereof, and the metal ion is selected from the group consisting of copper, zinc, silver, iron, manganese, cobalt, nickel, zirconium, calcium, aluminum, barium, cadmium, gallium, indium, lead, magnesium, mercury, palladium, scandium, strontium, thorium, titanium, vanadium and combinations thereof.

[0038] Examples of metal compound salts and calcium salts include copper (II) 2-ethylhexanoate, copper (II) hydroxide, copper (II) carbonate, copper (II) acetate, copper (I) acetate, copper butyrate, di-μ-hydroxybis [(N, N, N', N'-tetramethylethylenediamine) copper (II)] chloride, basic copper (II) carbonate, basic copper carbonate, calcium acetate, zinc stannate, zinc hydroxystannate, zinc (II) acetate, zinc (II) nitrate, zirconium (IV) hydroxide, cobalt (II) acetate, cobalt (II) chloride, cobalt (II) nitrate, nickel (II) acetate, nickel (II) chloride, nickel (II) nitrate, silver (I) acetate, silver (I) nitrate, manganese (II) 2-ethylhexanoate, and combinations thereof. Preferably, the metal compound is selected from the group consisting of copper (II) hydroxide, copper (II) carbonate, copper (II) acetate, copper (II) acetate monohydrate, and combinations thereof. Preferably, the metal compound is selected from the group consisting of copper (II) hydroxide, copper (II) carbonate, basic copper (II) carbonate, copper (II) acetate, cobalt (II) acetate, nickel (II) acetate, silver (I) acetate, zinc (II) acetate, calcium (II) acetate and combinations thereof.

[0039] The chelating part of the chelating polyester polyol and / or the chelating part of the chelating polyether polyol chelates the metal ions from the metal compound to form a metal chelating polyester polyol liquid or a metal chelating polyether polyol liquid, respectively. Preferably, the metal chelating polyester polyol liquid or the metal chelating polyether polyol liquid has a molar ratio of metal ions to the chelating part of 0.05:1 to 2:1. More preferably, the metal chelating polyester polyol liquid or the metal chelating polyether polyol liquid has a molar ratio of metal ions to the chelating part of 0.2:1 to 1.5:1. Most preferably, the metal chelating polyester polyol liquid or the metal chelating polyether polyol liquid has a molar ratio of metal ions to the chelating part of 0.4:1 to 1:1. Such reactions can occur at atmospheric pressure (e.g., 101.23KPa) and in a temperature range of 50 to 150°C. The reaction time varies from 0.5 minutes to 48 hours.

[0040] The present disclosure also provides an isocyanate-reactive composition with a hydroxyl moiety for forming a polyurethane polymer. For these embodiments, the isocyanate-reactive composition comprises a combination of 0.1 to 100% by weight of a metal-chelated polyester polyol liquid, a metal-chelated polyether polyol liquid or a metal-chelated polyester polyol liquid and a metal-chelated polyether polyol liquid, each as provided herein, and optionally up to 99.9% by weight of a polyol to form an isocyanate-reactive composition, the weight percentage being based on the gross weight of the isocyanate-reactive composition. For various embodiments, the polyol used together with a metal-chelated polyester polyol liquid and / or a metal-chelated polyether polyol liquid to form an isocyanate-reactive composition can be selected from the group consisting of polyether polyols, polyester polyols, polycarbonate polyols, polyether carbonate polyols and combinations thereof. Polyols can have a number average molecular weight of 100 g / mol to 10,000 g / mol. Other number average molecular weight values ​​are also possible. For example, the number average molecular weight of the polyol can be a low value of 100, 200, 300, 350 or 400 g / mol to a high value of 500, 750, 1,000, 2,000 or 10,000 g / mol. The number average molecular weight values ​​reported herein are determined by end group analysis, gel permeation chromatography and other methods known in the art. The polyol used together with the metal chelated polyester polyol liquid and / or the metal chelated polyether polyol liquid to form the isocyanate reactive composition can also include an aromatic moiety. As used herein, an "aromatic moiety" is at least one cyclic conjugated molecular moiety in the form of a planar unsaturated ring of carbon atoms that is covalently attached to a polyol compound. The planar unsaturated ring of carbon atoms can have at least six (6) carbon atoms.

[0041] For these embodiments, liquid polyether polyols may include those having at least 2, such as 2 or 3, hydroxyl groups per molecule and may be prepared, for example, by polymerization of epoxides / cyclic ethers such as ethylene oxide, propylene oxide, butylene oxide, styrene oxide or epichlorohydrin, either by themselves or in the presence of BF3, or by chemical addition of these epoxides, optionally in the form of a mixture (such as a mixture of ethylene oxide and propylene oxide) or in sequence, to starting components having reactive hydrogen atoms such as water, ammonia, ethanol or amines. Examples of suitable starting components include ethylene glycol, propylene glycol-(1,3) or -(1,2), glycerol, trimethylolpropane, 4,4'-dihydroxydiphenylpropane, aniline, diethanolamine, triethanolamine or ethylenediamine. Sucrose-based polyether polyols may also be used. In many cases it is preferred to use polyethers containing a dominant amount of primary OH groups (up to 100% by weight based on all OH groups present in the polyether).

[0042] For some embodiments, polyester polyol can include those having at least 1.8,2 or 3 hydroxyls (average) at the most per molecule.The example of this type of polyester polyol can include those formed as the reaction product of polyol (such as diol and / or triol) and polycarboxylic acid (such as dicarboxylic acid and / or tricarboxylic acid).Instead of free polycarboxylic acid, corresponding polycarboxylic acid esters or mixtures thereof of corresponding polycarboxylic anhydride or lower alcohol and mixtures thereof and free polycarboxylic acid can be used.Polycarboxylic acid can be aliphatic, alicyclic, aromatic and / or heterocyclic, and it can be substituted by, for example, halogen atoms, and / or can be undersaturated. Suitable exemplary polycarboxylic acids include, but are not limited to, succinic acid, adipic acid, suberic acid, azelaic acid, sebacic acid, phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, phthalic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, tetrachlorophthalic anhydride, endomethylenetetrahydrophthalic anhydride, glutaric anhydride, maleic acid, maleic anhydride, fumaric acid, dimerization and trimerization fatty acids optionally mixed with monomer fatty acids, dimethyl terephthalate and terephthalic acid-bis-ethylene glycol ester. The example of other suitable polyester polyols comprises modified aromatic polyester polyols, such as those (acid value 0.6-1.0mg KOH / g, hydroxyl value 230-250mg KOH / g, hydroxyl functionality 2.0, Stepan Company) provided with trade name STEPANPOL PS-2352.

[0043] Exemplary suitable polyols include, but are not limited to, ethylene glycol, propylene glycol-(1,2) and -(1,3), butanediol-(1,4) and -(2,3), hexanediol-(1,6), octanediol-(1,8), neopentyl glycol, cyclohexanedimethanol (1,4-bis-hydroxy-methylcyclohexane and other isomers), 2-methyl-1,3-propanediol, glycerol, trimethylolpropane, hexanetriol-(1,2,6), butanetriol-(1,2,4), trimethylolethane, pentaerythritol, quinitol, mannitol and sorbitol, methyl glycosides, diethylene glycol, triethylene glycol, tetraethylene glycol, polyethylene glycol, dipropylene glycol, polypropylene glycol, dibutylene glycol and polybutylene glycol. The polyesters may also contain a certain proportion of carboxyl end groups. Polyesters of lactones such as ε-caprolactone or hydroxycarboxylic acids such as 6-hydroxycaproic acid may also be used.

[0044] Such polyol components may also include polycarbonate polyols such as reaction products of diols, e.g., propylene glycol-(1,3), butanediol-(1,4) and / or hexanediol-(1,6), diethylene glycol, triethylene glycol or tetraethylene glycol with diaryl carbonates, e.g., diphenyl carbonate, dialiphatic carbonates, e.g., dimethyl carbonate or phosgene, or from the reaction of epoxides and carbon dioxide.

[0045] Other examples of suitable polyols include those polymers or copolymers having a hydroxyl equivalent of at least 75 formed with propylene oxide. The propylene oxide may be 1,3-propylene oxide, but is more typically 1,2-propylene oxide. If it is a copolymer, the comonomer is another copolymerizable alkylene oxide, such as ethylene oxide, 2,3-butylene oxide, tetrahydrofuran, 1,2-hexylene oxide, etc. The copolymer may contain 25% by weight or more, 50% by weight or more, preferably 75% or more of polymerized propylene oxide, based on the total weight of the polymerized alkylene oxide. The copolymer preferably contains no more than 75% by weight, especially no more than 50% by weight, of polymerized ethylene oxide. The nominal functionality of the polymer or copolymer of propylene oxide should be at least 2.0. The nominal functionality is preferably 2.5 to 8, more preferably 2.5 to 7 or 2.5 to 6. The hydroxyl equivalent weight of the polymer or copolymer of propylene oxide is at least 85, preferably at least 100, more preferably 150 to 3,200, in some embodiments 250 to 3,000 and in specific embodiments 300 to 2,500. The polyol can also be formed from a blend, wherein the blend includes a blend of a diol and a triol. The diol can have an average molecular weight (Mw) of 200 to 8,000 grams per mole, and the triol has an average molecular weight (Mw) of 250 to 6,500 grams per mole.

[0046] In various embodiments, the hydroxyl value of the polyol can be 10 mg KOH / g to 700 mg KOH / g. In other embodiments, the hydroxyl value of the polyol is 20 mg KOH / g to 500 mg KOH / g, or 30 mg KOH / g to 350 mg KOH / g. As used herein, the hydroxyl value is the milligrams of potassium hydroxide equivalent to the hydroxyl content in one gram of polyol or other hydroxy compound. The polyol can also have a number average isocyanate reactive group functionality of 1.8 to 6, such as 2 to 4 or 2.2 to 3.0.

[0047] For the various embodiments, the polyether polyols and / or polyester polyols may also be uncapped or capped with ethylene oxide (EO) and / or propylene oxide (PO) as known in the art to provide a hydrophilic or hydrophobic structure.

[0048] For these embodiments, the isocyanate-reactive composition may further comprise a compound selected from the group consisting of: 0.1 wt % to 1.5 wt % phosphorus from a flame retardant compound, preferably a halogen-free flame retardant compound (the wt % phosphorus is based on the total weight of the isocyanate-reactive composition); 0.05 wt % to 3.0 wt % metal, and combinations thereof, wherein the metal is from a metal-chelated polyester polyol liquid and / or a metal-chelated polyether polyol liquid, and the wt % metal is based on the total weight of the isocyanate-reactive composition. Preferably, the isocyanate-reactive composition comprises 0.5 wt % to 1.0 wt % phosphorus from a halogen-free flame retardant compound (the wt % phosphorus is based on the total weight of the isocyanate-reactive composition) and / or 0.15 wt % to 2.0 wt % metal from a metal-chelated polyester polyol liquid and / or a metal-chelated polyether polyol liquid (the wt % metal is based on the total weight of the isocyanate-reactive composition). More preferably, the isocyanate-reactive composition comprises 0.75 wt % to 0.90 wt % of phosphorus from the halogen-free flame retardant compound (the wt % of phosphorus is based on the total weight of the isocyanate-reactive composition) and / or 0.5 wt % to 1.0 wt % of metal from a metal-chelated polyester polyol liquid and / or a metal-chelated polyether polyol liquid (the wt % of metal is based on the total weight of the isocyanate-reactive composition). For a given weight percentage value, the isocyanate-reactive composition may have a molar ratio of metal ions to phosphorus (moles of metal ions: moles of phosphorus) of 0.05:1 to 5:1. Preferably, the molar ratio of metal ions to phosphorus (moles of metal: moles of phosphorus) is 0.10:1 to 3:1. More preferably, the molar ratio of metal ions to phosphorus (moles of metal: moles of phosphorus) is 0.15:1 to 1:1.

[0049] For the embodiments provided herein, flame retardant compounds, preferably halogen-free flame retardant compounds are selected from the group consisting of phosphoric acid esters, phosphonic acid esters, phosphinates and combinations thereof. The example of phosphoric acid esters includes trialkyl phosphates, triaryl phosphates, phosphoric acid esters and resorcinol bis (diphenyl phosphate). As used herein, trialkyl phosphates have at least one alkyl group with 2 to 12 carbon atoms and optional halogen atoms. The other two alkyl groups of trialkyl phosphates can be independently identical or different from the first alkyl group, containing 1 to 8 carbon atoms, including straight or branched alkyl groups, cyclic alkyl groups, alkoxyethyl groups, hydroxyalkyl groups, hydroxyalkoxyalkyl groups and straight or branched alkylene groups. The examples of other two alkyls of trialkyl phosphate include, for example, methyl, ethyl, propyl, butyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, butoxyethyl, isopentyl, neopentyl, isohexyl, isoheptyl, cyclohexyl, propylene, 2-methylpropylene, neopentyl, hydroxymethyl, hydroxyethyl, hydroxypropyl or hydroxybutyl. Blends of different trialkyl phosphates can also be used. The three alkyls of trialkyl phosphate can be the same. Trialkyl phosphate can be tris (2-chloro-1-methylethyl) phosphate (TCPP), tris [2-chloro-1-(chloromethyl) ethyl] phosphate (TDCP), tris (p-tert-butylphenyl) phosphate (TBPP) and tris (2-chloroethyl) phosphate (TCEP). Trialkyl phosphate is ideally triethyl phosphate (TEP).

[0050] Examples of phosphonates include diethyl (hydroxymethyl) phosphonate, dimethyl methylphosphonate and diethyl ethylphosphonate. Examples of phosphinates include metal salts of organic phosphinates, such as aluminum methylethylphosphinate, aluminum diethylphosphinate, zinc methylethylphosphinate and zinc diethylphosphinate. Examples of additional halogen-free flame retardant compounds include resorcinol diphosphoric acid, 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, ammonium polyphosphate and combinations thereof.

[0051] The present disclosure also provides a method for preparing a metal chelated polyester polyol liquid and / or a metal chelated polyether polyol liquid. The method includes reacting a monomer of a liquid polyester polyol or a liquid polyester polyol formed by the monomer of a liquid polyester polyol with a chelating agent having a chelating moiety to form a chelated polyester polyol, as discussed herein. For these embodiments, the chelating moiety is selected from a dianhydride moiety, an amino-based chelating moiety, and a combination thereof, as provided herein. For these embodiments, a chelating agent having a dianhydride moiety chemically reacts with a monomer of a liquid polyester polyol or a liquid polyester polyol formed by the monomer of a liquid polyester polyol to form a chelated polyester polyol with an aminopolycarboxylic acid moiety, as provided herein. For these embodiments, the chelating agent having the amino-based chelating moiety chemically reacts with the monomer of the liquid polyester polyol or the liquid polyester polyol formed by the monomer of the liquid polyester polyol to form a polyester amino polyol as the chelated polyester polyol. For these embodiments, the method further comprises reacting the chelated polyester polyol having the chelating moiety with a metal compound having a metal ion, wherein the chelating moiety of the chelated polyester polyol chelates the metal ion to form the metal chelated polyester polyol liquid, the reaction having a molar ratio of the metal ion to the chelating moiety of 0.05:1 to 2:1. For these embodiments, the chelating agent having the dianhydride moiety chemically reacts with the liquid polyester polyol formed from the monomer of the liquid polyester polyol at a molar ratio of 1:1.5 to 1:100 (moles of chelating agent: moles of polyester polyol) to form the chelated polyester polyol having an aminopolycarboxylic acid moiety.

[0052] The method can also include reacting the monomers of a liquid polyether polyol or a liquid polyether polyol formed by the monomers of a liquid polyether polyol with a chelating agent having a chelating moiety to form a chelated polyether polyol, as discussed herein. For these embodiments, the chelating moiety is selected from a dianhydride moiety, an amino-based chelating moiety, and a combination thereof, as provided herein. For these embodiments, a chelating agent with a dianhydride moiety chemically reacts with a monomer of a liquid polyether polyol or a liquid polyether polyol formed by the monomers of a liquid polyether polyol to form a chelated polyether polyol with an aminopolycarboxylic acid moiety, as provided herein. For these embodiments, a chelating agent with an amino-based chelating moiety chemically reacts with a monomer of a liquid polyether polyol or a liquid polyether polyol formed by the monomers of a liquid polyether polyol to form a polyetheramino polyol as a chelated polyether polyol. For these embodiments, the method further comprises reacting a chelated polyether polyol having a chelating moiety with a metal compound having a metal ion, wherein the chelating moiety of the chelated polyether polyol chelates the metal ion to form a metal chelated polyether polyol liquid, the reaction having a molar ratio of metal ion to chelating moiety of 0.05: 1 to 2: 1. For these embodiments, the chelating agent having the dianhydride moiety chemically reacts with the liquid polyether polyol formed from the monomer of the liquid polyether polyol at a molar ratio of 1: 1.5 to 1: 100 (moles of chelating agent: moles of polyether polyol) to form the chelated polyether polyol having an aminopolycarboxylic acid moiety.

[0053] The present disclosure also provides a reaction mixture for forming a polyurethane polymer. The reaction mixture comprises an isocyanate compound with an isocyanate moiety and an isocyanate-reactive composition as provided herein, wherein the reaction mixture has a mol ratio of 0.90:1 to 7:1 of an isocyanate moiety to a hydroxyl moiety. For rigid polyurethane (PUR) and rigid polyisocyanurate (PIR) foams, preferably, the mol ratio of the isocyanate moiety to the hydroxyl moiety is 1.2:1 to 7:1, more preferably, the mol ratio of the isocyanate moiety to the hydroxyl moiety is 1.5:1 to 5:1, and most preferably, the mol ratio of the isocyanate moiety to the hydroxyl moiety is 2:1 to 4:1. For flexible polyurethane foams, preferably, the mol ratio of the isocyanate moiety to the hydroxyl moiety is 0.95:1 to 1.20:1, more preferably, the mol ratio of the isocyanate moiety to the hydroxyl moiety is 0.98:1 to 1.10:1, and most preferably, the mol ratio of the isocyanate moiety to the hydroxyl moiety is 1:1 to 1.08:1. For two-component polyurethane adhesives, sealants, coatings and elastomers, preferably, the molar ratio of isocyanate moieties to hydroxyl moieties is from 0.95:1 to 1.35:1, more preferably, the molar ratio of isocyanate moieties to hydroxyl moieties is from 0.98:1 to 1.10:1, and most preferably, the molar ratio of isocyanate moieties to hydroxyl moieties is from 1:1 to 1.05:1.

[0054] For various embodiments, the isocyanate compound has a number average molecular weight of 150g / mol to 750g / mol. Other number average molecular weight values ​​are also possible. For example, the isocyanate reactive compound may have a number average molecular weight from a low value of 150, 200, 250 or 300g / mol to a high value of 350, 400, 450 or 500g / mol. In some embodiments, when the isocyanate compound is an isocyanate prepolymer obtained by reacting an isocyanate reactive compound with a molar excess of polyisocyanate compounds or polymerized isocyanate compounds without causing gelation or curing, the isocyanate prepolymer may have a number average molecular weight higher than 750g / mol, and may be calculated by the number average molecular weight of each component used to prepare the prepolymer and their relative mass. The number average molecular weight values ​​reported herein are determined by end group analysis, gel permeation chromatography and other methods known in the art. The isocyanate compound may be monomeric and / or polymeric, as known in the art. In addition, the isocyanate compound may have an isocyanate equivalent weight of 80 to 1750. In certain embodiments, the viscosity of the isocyanate at 25°C is 5 to 50,000 mPa s when measured using a Brookfield DVE viscometer. Other viscosity values ​​are also possible. For example, the isocyanate reactive compound may have a viscosity value ranging from a low value of 5, 10, 30, 60, or 150 mPa s to a high value of 500, 2500, 10,000, or 50,000 mPa s, each measured at 25°C using a Brookfield DVE viscometer.

[0055] As used herein, the polymeric isocyanate compound contains two or more than two -NCO groups per molecule. For various embodiments, the polymeric isocyanate compound is selected from aliphatic diisocyanates, alicyclic diisocyanates, aromatic diisocyanates, polyisocyanates, isocyanate prepolymers, and combinations thereof. For various embodiments, the polymeric isocyanate compound has a number average molecular weight of 150 g / mol to 500 g / mol. In addition, the polymeric isocyanate compound may have an isocyanate equivalent weight of 70 to 150, as well as a so-called MDI product, i.e., a mixture of isomers of diphenylmethane diisocyanate in the form of monomeric MDI, or a so-called polymeric MDI product, i.e., a mixture of polymethylene polyphenylene polyisocyanates in the form of monomeric MDI.

[0056] Examples of polymeric isocyanate compounds of the present disclosure may include, but are not limited to, methylene diphenyl diisocyanate (MDI), polymethylene polyphenyl isocyanates including MDI, polymeric MDI (PMDI), 1,6-hexamethylene diisocyanate (HDI), 2,4- and / or 2,6-toluene diisocyanate (TDI), 1,5-naphthalene diisocyanate (NDI), tetramethylene-1,4-diisocyanate, cyclohexane-1,4-diisocyanate, hexahydrotoluene diisocyanate, hydrogenated MDI (HDI), and the like. MDI), methoxyphenyl-2,4-diisocyanate, 4,4'-biphenylene diisocyanate, 3,3'-dimethoxy-4,4'-biphenylene diisocyanate, 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4',4"-triphenylmethane diisocyanate, polymethylene polyphenyl isocyanate, hydrogenated polymethylene polyphenyl isocyanate, toluene-2,4,6-triisocyanate and 4,4'-dimethyldiphenylmethane-2,2',5,5'-tetraisocyanate Ester, methylene biscyclohexyl isocyanate (HMDI), isophorone diisocyanate (IPDI) and combinations thereof. Suitable isocyanates may also include other aromatic and / or aliphatic polyfunctional isocyanates. Aromatic diisocyanates include those containing phenyl, tolyl, xylyl, naphthyl or diphenyl moieties or combinations thereof, such as trimethylolpropane adducts of xylylenediisocyanate, trimethylolpropane adducts of toluene diisocyanate, 4,4'-diphenylmethane diisocyanate (MDI), xylylenediisocyanate, and the like. diisocyanate (XDI), 4,4'-diphenyldimethylmethane diisocyanate, di- and tetraalkyl diphenylmethane diisocyanates, 4,4'-dibenzyl diisocyanate, 1,3-phenylene diisocyanate, 1,4-phenylene diisocyanate, and combinations thereof. Suitable aliphatic polymeric isocyanate compounds include trimers of hexamethylene diisocyanate, trimers of isophorone diisocyanate, biuret of hexamethylene diisocyanate, hydrogenated polymeric methylene diphenyl diisocyanate, hydrogenated methylene diphenyl diisocyanate, hydrogenated MDI, tetramethylxylene diisocyanate (TMXDI), 1-methyl-2,4-diisocyanato-cyclohexane, 1,6-diisocyanato-2,2,4-trimethylhexane, 1-isocyanatomethyl-3-isocyanato-1,5,5-trimethylcyclohexane, tetramethoxybutane 1,4-diisocyanate, butane 1,4-diisocyanate, hexane 1,6-diisocyanate, dicyclohexylmethane diisocyanate, cyclohexane 1,4-diisocyanate, and combinations thereof.Examples of other polymeric isocyanate compounds include other aliphatic, alicyclic, polycyclic or aromatic compounds, such as hydrogenated xylene diisocyanate (HXDI), p-phenylene diisocyanate (PPDI), 3,3'-dimethyldiphenyl-4,4'-diisocyanate (DDDI), 2,2,4-trimethylhexamethylene diisocyanate (TMDI), isophorone diisocyanate (IPDI), 4,4'-dicyclohexylmethane diisocyanate (H12MDI) and norbornane diisocyanate (NDI). In addition to the isocyanates mentioned above, partially modified polyisocyanates can be used, including uretdione, isocyanurate, carbodiimide, uretonimine, allophanate or biuret structure and combinations thereof. As provided herein, polyols can be pre-reacted with organic polyisocyanates to form prepolymers or quasi-prepolymers containing isocyanate groups. The isocyanate content of the prepolymer or quasi-prepolymer may be, for example, 1 to 20 weight percent. In some embodiments, the isocyanate content of the prepolymer or quasi-prepolymer is at least 2.5% or at least 4% and at most 15%, at most 12%, or at most 10%.

[0057] For these embodiments, the reaction mixture may further include a compound selected from the group consisting of water, a catalyst, a surfactant, a blowing agent or a combination thereof. The reaction mixture may also include other components known in the art. Based on the gross weight of the reaction mixture, the catalyst may be present in an amount of 0.01 wt % to 1.5 wt %. The catalyst may be selected from organic tertiary amines, tertiary phosphines, potassium acetate, carbamate-based catalysts and combinations thereof. The catalyst may also include organotin compounds as known in the art.

[0058] The catalyst can be a foaming catalyst, a gelling catalyst, a trimerization catalyst or a combination thereof. As used herein, a foaming catalyst and a gelling catalyst can be distinguished by the tendency to favor urea (foaming) reaction in the case of a foaming catalyst or to favor urethane (gelling) reaction in the case of a gelling catalyst. A trimerization catalyst can be used to promote the isocyanate reaction in the composition. Both a foaming catalyst and a gelling catalyst are used to prepare rigid and flexible polyurethane foams. Polyurethanes that are not foam or microporous, such as many coatings, adhesives, sealants and elastomers utilize gelling catalysts.

[0059] Examples of blowing catalysts (e.g., catalysts that may tend to favor the blowing reaction) include, but are not limited to, short chain tertiary amines or oxygen-containing tertiary amines. Amine-based catalysts may not be sterically hindered. For example, blowing catalysts include bis-(2-dimethylaminoethyl) ether, pentamethyldiethylenetriamine, triethylamine, tributylamine, N,N-dimethylaminopropylamine, dimethylethanolamine, N,N,N',N'-tetramethylethylenediamine, and combinations thereof, and the like. An example of a commercially available blowing catalyst is POLYCAT from Evonik. TM5, and other commercially available blowing catalysts.

[0060] Examples of gelling catalysts (e.g., catalysts that may tend to favor the gelling reaction) include, but are not limited to, organometallic compounds, cyclic tertiary amines and / or long chain amines (e.g., containing several nitrogen atoms), and combinations thereof. Organometallic compounds include organotin compounds, such as tin(II) salts of organic carboxylic acids, for example, tin(II) diacetate, tin(II) dioctoate, tin(II) diethylhexanoate, and tin(II) dilaurate, and dialkyltin(IV) salts of organic carboxylic acids, for example, dibutyltin diacetate, dibutyltin dilaurate, dibutyltin maleate, and dioctyltin diacetate. Bismuth salts of organic carboxylic acids may also be used as gelling catalysts, such as bismuth octoate. Cyclic tertiary amines and / or long chain amines include dimethylbenzylamine, triethylenediamine, 4,4'(oxydi-2,1-ethanediyl)bismorpholine, and combinations thereof. An example of a commercially available gelling catalyst is POLYCAT from Evonik. TM 8 and T-12, and other commercially available gelling catalysts.

[0061] Examples of trimerization catalysts include N,N,N′,N″,N″-pentamethyldiethylenetriamine (PMDETA); N,N′,N″-tris(3-dimethylaminopropyl)hexahydro-S-triazine; N,N-dimethylcyclohexylamine; 1,3,5-tris(N,N-dimethylaminopropyl)-s-hexahydrotriazine; [2,4,6-tris(dimethylaminomethyl)phenol]; potassium acetate, potassium octoate; tetraalkylammonium hydroxides such as tetramethylammonium hydroxide; alkali metal hydroxides such as sodium hydroxide; alkali metal alkoxides such as sodium methoxide and potassium isopropoxide; and alkali metal salts of long-chain fatty acids having 10 to 20 carbon atoms and combinations thereof, etc. Some commercially available trimerization catalysts include both from Evonik TMR-2, TMR-7, K 2097, K15, POLYCAT TM 41 and POLYCAT TM 46, and other commercially available trimerization catalysts.

[0062] For various embodiments, the blowing agent can be present in an amount of 1.0 wt % to 15 wt % based on the total weight of the reaction mixture. In addition to other blowing agents provided herein, blowing agents as known in the art can be selected from the group consisting of water, volatile organic substances, dissolved inert gases, and combinations thereof. Examples of blowing agents include hydrocarbons such as butane, isobutane, 2,3-dimethylbutane, n-pentane and isopentane isomers, hexane isomers, heptane isomers, and cycloalkanes, including cyclopentane, cyclohexane, cycloheptane; hydrofluorocarbons such as HCFC-142b (1-chloro-1,1-difluoroethane), HCFC-141b (1,1-dichloro-1-fluoroethane), HCFC-22 (chlorodifluoromethane), HFC-245fa (1,1,1,3,3-pentafluoropropane), HFC-365mfc (1,1,1,3,3-pentafluorobutane), HFC HFC-227ea (1,1,1,2,3,3,3-heptafluoropropane), HFC-134a (1,1,1,2-tetrafluoroethane), HFC-125 (1,1,1,2,2-pentafluoroethane), HFC-143 (1,1,2-trifluoroethane), HFC 143A (1,1,1-trifluoroethane), HFC-152 (1,1-difluoroethane), HFC-227ea (1,1,1,2,3,3,3-heptafluoropropane), HFC-236ca (1,1,2,2,3,3-hexafluoropropane), HFC 236fa (1,1,1,3,3,3-hexafluoroethane), HFC 245ca (1,1,2,2,3-pentafluoropentane), HFC356mff (1,1,1,4,4,4-hexafluorobutane), HFC 365mfc (1,1,1,3,3-pentafluorobutane); hydrofluoroolefins such as cis-1,1,1,4,4,4-hexafluoro-2-butene, 1,3,3,3-tetrafluoropropene, trans-1-chloro-3,3,3-trifluoropropene; chemical blowing agents such as formic acid and water. The blowing agent may be other volatile organic compounds such as ethyl acetate; methanol; ethanol; halogenated alkanes such as dichloromethane, chloroform, dichloroethane, dichloroethylene, trichlorofluoromethane, chlorodifluoromethane or dichlorodifluoromethane; butane; hexane; heptane; ether; as well as nitrogen, air and carbon dioxide gas.

[0063] For various embodiments, based on the total weight of the reaction mixture, the surfactant may be present in an amount of 0.1 wt % to 10 wt %. Examples of suitable surfactants include silicone-based surfactants and organic-based surfactants. Some representative materials are typically polysiloxane polyoxyalkylene block copolymers, such as those disclosed in U.S. Patent Nos. 2,834,748, 2,917,480, and 2,846,458; the disclosures of these patents are incorporated herein by reference as a whole. Also included are organic surfactants containing polyoxyethylene-polyoxybutylene block copolymers, as described in U.S. Patent No. 5,600,019, the disclosures of which are incorporated herein by reference as a whole. Other surfactants include polyethylene glycol ethers of long-chain alcohols, tertiary amines or alkanolamine salts of long-chain allyl acid sulfates, alkyl sulfonates, alkyl aryl sulfonic acids, and combinations thereof.

[0064] Water may be present in the reaction mixture in an amount of 0.1 wt % to 1.5 wt % based on the total weight of the reaction mixture.

[0065] In addition to water, catalysts, blowing agents, surfactants and combinations thereof, the reaction mixture may also include fillers and other additives. The total amount of such other additives may be from 0.01 wt % to 30.0 wt %. The use of other additives for polyurethane polymer compositions is also known and may be used with the present disclosure.

[0066] For these embodiments, the reaction mixture provided herein can be used to form a polyurethane-based polymer, including a polyurethane-based polymer foam. The method for preparing a reaction mixture for producing a polyurethane-based foam can be achieved by any process technology known in the art. Generally, the polyurethane-based foam of the present disclosure can be produced by a discontinuous or continuous process, including a process commonly referred to as a discontinuous platemaking process (DCP) and a continuous lamination process, wherein the foaming reaction and subsequent curing are carried out in a mold or on a conveyor. The method as provided herein can be carried out at a temperature of 15°C to 80°C. The mixing pressure for the method can include a value of 80kPa to 25,000kPa. The compounding of the components for the polyurethane-based foam can be carried out using a mixing device known in the art. The density of the resulting polyurethane foam can be 10kg / m 3 or greater, preferably 15 kg / m 3 or greater, more preferably 25 kg / m 3 or greater, most preferably 35 kg / m 3 or greater, and typically 200 kg / m 3 or less, preferably 100 kg / m 3 or less, more preferably 70kg / m 3 or less, and most preferably 50 kg / m3 or smaller.

[0067] The polyurethane-based foams of the present disclosure provide low smoke generation and high thermal stability as measured according to ASTM E662 "Test Method for Specific Optical Density of Smoke Generated by Solid Materials". Lower maximum specific optical density (Max Ds) values ​​mean lower smoke generation. Lower mass loss % values ​​mean higher thermal stability. Max Ds may be 400 or less, preferably 200 or less, more preferably 100 or less, and also most preferably 50 or less. Mass loss % may be 50% or less, preferably 45% or less, more preferably 40% or less, and also most preferably 30% or less.

[0068] The polyurethane-based foams of the present disclosure may have low thermal conductivity in applications such as building insulation. The thermal conductivity of rigid foams is represented by the K factor. The K factor is a measure of thermal insulation. The K factor of the prepared foam may be 30.0 mW / m·K or less, preferably 27.0 mW / m·K or less, more preferably 24.0 mW / m·K or less, and most preferably 22.0 mW / m·K or less. Thermal conductivity (K factor) F is measured using ASTM C-518-17 at an average temperature of 75°F.

[0069] Applications of the polyurethane-based foam produced by the present disclosure are those known in the industry. For example, polyurethane-based foams can be used for insulation in building walls and roofs, garage doors, transport trucks and rail cars, and cold storage facilities. The polyurethane-based foam disclosed herein can have a combination of properties required for these applications. For example, the polyurethane-based foam disclosed herein can advantageously provide desired low thermal conductivity, smoke density, thermal stability, and improved combustion characteristics while reducing HCN and CO emissions.

[0070] The metal chelate polyols and polyurethane polymers of the present disclosure may also be used, for example, as flexible foams, coatings, elastomers, sealants, binders or adhesives. For use as coatings, elastomers, sealants, binders or adhesives, the reactants are preferably formulated into a two-component system (2K), one component containing a polyisocyanate (more preferably an isocyanate-terminated prepolymer or quasi-prepolymer) and the other component containing at least one of a metal chelate polyester polyol liquid and / or a metal chelate polyether polyol liquid, wherein the metal chelate polyol imparts antifungal, antimicrobial, deodorizing, hardness, friction resistance, etc. to the cured polyurethane product. For use as coatings, elastomers, sealants, binders or adhesives, the metal chelate polyol and other optional polyols may be pre-reacted with an organic polyisocyanate to form a prepolymer or quasi-prepolymer containing isocyanate groups and used as a one-component (1K) curing system.

[0071] Some embodiments of the present disclosure will now be described in detail in the following examples.

[0072] Example

[0073] Some embodiments of the present disclosure will now be described in detail in the following examples, wherein all parts and percentages are by weight unless otherwise indicated. In these examples, the following materials and tests were used.

[0074] Material

[0075] Materials used in Examples and / or Comparative Examples include the following.

[0076] Polyol A is a polyester polyol having a hydroxyl value of 220 mg KOH / g and a functionality of 2 (an aromatic polyester polyol derived from terephthalic acid, polyethylene glycol 200, and diethylene glycol).

[0077] Polyol B is a polyester polyol having a hydroxyl value of 315 mg KOH / g and a functionality of 2.4 (an aromatic polyester polyol derived from terephthalic acid, polyethylene glycol 200, glycerol, and diethylene glycol).

[0078] Polyethylene glycol 200 (PEG 200), available from TCI America.

[0079] Polyethylene glycol 400 (PEG 400), available from TCI America.

[0080] N,N,N',N'-Tetrakis-(2-hydroxypropyl)ethylenediamine, available from TCI America.

[0081] 2-[[2-(Dimethylamino)ethyl]methylamino]ethanol, available from TCI America.

[0082] 1-[Bis[3-(dimethylamino)propyl]amino-2-propanol], available from Sigma-Aldrich.

[0083] Glycerin, available from Acros Organics.

[0084] AA105 (catalyst), available from Dorf Ketal Chemicals.

[0085] 2,2'-Bipyridine (BIPY), available from Sigma-Aldrich.

[0086] N,N,N',N'-Tetramethylethylenediamine (TMEDA), available from TCI America.

[0087] Triethyl phosphate (TEP) is a flame retardant available from LANXESS.

[0088] Meso-butane-1,2,3,4-tetracarboxylic dianhydride from TCI America.

[0089] POLYCAT TM 5 is a catalyst available from Evonik Industries AG.

[0090] POLYCAT TM 46 is a catalyst available from Evonik Industries AG.

[0091] Ethylenediaminetetraacetic dianhydride, available from TCI America.

[0092] Diethylenetriaminepentaacetic dianhydride, available from TCI America.

[0093] The surfactant was a silicone rigid foam surfactant from Evonik Industries AG.

[0094] The water is deionized water having a specific resistance of 10 MΩ×cm (million ohms) at 25°C.

[0095] Cyclopentane (c-Pentane) is a blowing agent obtained from Sigma-Aldrich.

[0096] Diethyl (hydroxymethyl) phosphonate (DEHMP) is a flame retardant available from Tokyo Chemical Industry Co., Ltd.

[0097] PAPI TM580N is a polymethylene polyphenyl isocyanate (MDI) containing methylene diphenyl diisocyanate (MDI) with 30.8% isocyanate from Dow Inc.

[0098] Copper (II) hydroxide (Cu(OH)2), technical grade, available from Sigma Aldrich.

[0099] Cuprous (I) oxide (Cu2O), technical grade, available from Sigma Aldrich.

[0100] Basic copper carbonate, available from Sigma Aldrich.

[0101] Copper(II) ethylhexanoate (CuEH), available from Sigma Aldrich.

[0102] Copper(II) acetate monohydrate (Cu(OAc)2H2O), available from Acros Organics.

[0103] Cobalt(II) acetate tetrahydrate (Co(OAc)2 4H2O), available from Acros Organics.

[0104] Nickel(II) acetate tetrahydrate (Ni(OAc)2 4H2O), available from Acros Organics.

[0105] Silver(I) acetate (Ag(OAc)), available from Fisher Scientific.

[0106] Zinc(II) acetate dihydrate (Zn(OAc)2 2H2O), available from Fisher Scientific.

[0107] Calcium (II) acetate monohydrate (Ca(OAc)2H2O), available from Acros Organics.

[0108] Preparation of non-chelated polyester polyols

[0109] Polyester polyol containing succinic anhydride and copper (II) hydroxide (for comparative example)

[0110] Polyester polyol A (85.0 grams, OH#220mg KOH / g) was charged into a dry 3-neck 250mL round-bottom flask in a heating mantle and placed under an initial nitrogen (N2, gas) purge with overhead stirring. The flask was warmed to 100°C. Meso-butane-1,2,3,4-tetracarboxylic dianhydride was added in two portions, 3.07g (first portion) and 2.99g (second portion), respectively, with a retention time of 30 minutes after the first addition and 1.75 hours after the second addition. Copper (II) hydroxide was added in two portions, 1.44g (first portion) and 1.33g (second portion), respectively, with a retention time of 60 minutes after the first addition and 2.0 hours after the second addition. Solid particles of copper (II) hydroxide were observed in the reactor product. The temperature was raised to 120°C for a total of 8 hours, and solid particles of copper (II) hydroxide were observed in the reactor product. The temperature was raised to 140°C for a total of 2 hours, and solid particles of copper (II) hydroxide were observed in the reactor product. The temperature was raised to 160°C for 3 hours, and gel-like particles were observed in the reactor product.

[0111] Preparation of Liquid Chelated Metal Polyols

[0112] Liquid Chelated Metal Polyol C

[0113] Polyester polyol A (85.99 grams, OH#220mg KOH / g) was loaded into a dry 3-neck 250 mL round bottom flask in a heating mantle and placed under an initial nitrogen (N2, gas) purge with overhead stirring. The flask was warmed to 100°C. Ethylenediaminetetraacetic acid dianhydride was added in two portions, 4.096 g (first portion) and 3.839 g (second portion), with a holding time of 30 minutes after the first addition and 60 minutes after the second addition. The contents of the flask were cooled to 60°C. Basic copper (II) carbonate was added in two portions, 1.713 g and 1.712 g, with a holding time of 60 minutes after the first addition and 6 hours after the second addition. Next, the contents of the flask were heated to 80°C and maintained at this temperature for 2 hours, then the contents of the flask were heated to 100°C and maintained at this temperature for 16 hours, and then the contents of the flask were heated to 120°C and maintained at this temperature for 6 hours. The product was a blue viscous liquid. The product was cooled to 60°C and diluted with polyester polyol B (28.63 grams, OH#315 mg KOH / gram) and triethyl phosphate (20.25 grams) under stirring, maintained at 60°C for 16 hours under stirring, and then cooled to room temperature (23°C).

[0114] Liquid Chelated Metal Polyol D

[0115] Polyester polyol A (170.49 g, OH#220 mg KOH / g) was charged to a dry 3-neck 500 mL round bottom flask in a heating mantle and placed under an initial nitrogen (N2, gas) purge with overhead stirring. The flask was warmed to 100°C. Ethylenediaminetetraacetic acid dianhydride was added in three portions, 5.047 g (first portion), 5.233 g (second portion), and 5.450 g (third portion), with a hold time of 30 minutes after the first and second additions and 60 minutes after the third addition. 4.26 g aliquots were removed. Copper (II) hydroxide was added in three portions, 2.078 g (first portion), 1.918 g (second portion), and 1.858 g (third portion), with a hold time of 30 minutes after the first and second additions and a hold time of 5.75 hours after the third addition. 7.44 g aliquots were removed and cooled to room temperature. The product has an acid value of 2.05 mg KOH / g and is a clear blue viscous liquid. The product is warmed to 60°C and diluted with polyester polyol B (53.3 grams, OH# 315 mg KOH / gram) and triethyl phosphate (37.6 grams) under stirring, kept at 40°C under stirring for 2.5 hours, and then cooled to room temperature.

[0116] Liquid Chelated Metal Polyol E

[0117] Polyethylene glycol 200 (100 grams, Mn 201) was loaded into a dry 3-neck 250 mL round bottom flask in a heating mantle and placed under an initial nitrogen (N2, gas) purge with overhead stirring. The flask was warmed to 100°C. Ethylenediaminetetraacetic acid dianhydride was added in three portions, 3.105 g (first portion), 3.095 g (second portion) and 3.026 g (third portion), with a retention time of about 25 minutes after the first and second additions and about 75 minutes after the third addition. Copper (II) hydroxide was added in three portions, 1.086 g (first portion), 1.105 g (second portion) and 1.243 g (third portion), with a retention time of 30 minutes after the first and second additions and 3.25 hours after the third addition. The product was cooled to room temperature. The product was a clear blue viscous liquid.

[0118] Liquid Chelated Metal Polyol F

[0119] N,N,N',N'-Tetra-(2-hydroxypropyl)ethylenediamine (8.85 g) and Polyol A (120.00 g) were placed in a dry 3-neck 250 mL round bottom flask in a heating mantle and placed under an initial nitrogen (N2, gas) purge with overhead stirring. The flask was warmed to 180°C and at near temperature AA105 (0.0430 g) was added and stirred for 2 hours. The contents of the flask were cooled to 100°C. Copper (II) acetate monohydrate was added in two portions, 2.779 g and 2.961 g, respectively, with a holding time of 1 hour after the first addition and 2 hours after the second addition. The product was cooled to room temperature. The product was a clear blue viscous liquid.

[0120] Liquid Chelated Metal Polyol G

[0121] Polyethylene glycol 200 (348.33 g, Mn 200), terephthalic acid (199.33 g) and TYZOR AA 105 (0.1374 g) were charged to an insulated 4-neck 1000 mL round bottom flask with N2 inlet adapter and thermocouple, with overhead stirring, and the flask was placed in a heating mantle. After degassing by cycling between vacuum (100 Torr) and N2, the reactor was completed with a heated and insulated Dean-stark type water separator and a condenser connected to the outlet adapter, wherein the N2 purge left through an oil bubbler. The reaction profile for collecting distillate was 4.5 hours at 220°C, 4 hours at 230°C, 3 hours at 240°C, and 4.5 hours at 250°C, wherein polyethylene glycol 200 (28 g, Mn 200) was added as the polyester polyol cooled.

[0122] N,N,N',N'-tetrakis-(2-hydroxypropyl)ethylenediamine (20.61 g) and the polyester polyol described in this example (122.0 g) were placed in a dry 3-neck 250 mL round bottom flask in a heating mantle and placed under an initial nitrogen (N2, gas) purge with overhead stirring, then switched to positive nitrogen (N2, gas). The flask was warmed to 180°C and at near temperature, AA105 (0.0472 g) was injected and stirred for 4 hours. The hydroxyl number of this material was 214 mg KOH / g. The contents of the flask were cooled to 100°C. Copper (II) acetate monohydrate was added in two portions, 3.505 g and 3.384 g, with a hold time of 1 hour after the first addition and 1 hour after the second addition. The product was cooled to room temperature. The product was a clear blue viscous liquid.

[0123] Liquid Chelated Metal Polyol H

[0124] 1-[Bis[3-(dimethylamino)propyl]amino-2-propanol] (8.64 g), glycerol (3.24 g) and polyol A (131.08 g) were charged into a dry 3-neck 250 mL round bottom flask placed in a heating mantle and placed under an initial nitrogen (N2, gas) purge with overhead stirring, then switched to positive nitrogen (N2, gas). The flask was warmed to 180°C and at near temperature, AA105 (0.0467 g) was injected and stirred for 4 hours. The hydroxyl number was 282 mg KOH / g. The contents of the flask were cooled to 100°C. Copper (II) acetate monohydrate was added in two portions, 3.521 g and 3.312 g, respectively, with a holding time of 1 hour after the first addition and 1 hour after the second addition. The product was cooled to room temperature. The product was a clear blue viscous liquid.

[0125] Liquid Chelated Metal Polyol I

[0126] 2-[[2-(Dimethylamino)ethyl]methylamino]ethanol (5.14 g), glycerol (3.24 g) and polyol A (134.60 g) were placed in a dry 3-neck 250 mL round bottom flask in a heating mantle and placed under an initial nitrogen (N2, gas) purge with overhead stirring, then switched to positive nitrogen (N2, gas). The flask was warmed to 165°C and at near temperature, AA105 (0.0431 g) was injected and stirred for 3 hours. The hydroxyl number was 287 mg KOH / g. The contents of the flask were cooled to 100°C. Copper (II) acetate monohydrate was added in two portions, 3.45 g and 3.45 g, respectively, with a holding time of 1 hour after the first addition and 1.75 hours after the second addition. The product was cooled to room temperature. The product was a clear blue-green viscous liquid.

[0127] Liquid Chelated Metal Polyol J

[0128] Polyethylene glycol 400 (45.0 grams, Mn 407) was charged to a dry 3-neck 100 mL round bottom flask placed in a heating mantle and placed under an initial nitrogen (N2, gas) purge with overhead stirring. The flask was warmed to 75°C. Diethylenetriaminepentaacetic dianhydride was added in three portions, 1.451 g (first portion), 1.379 g (second portion), and 1.120 g (third portion); the first portion was mixed at 75°C for 1 hour, then at 100°C for 1 hour, and the second and third portions were added at 100°C, with a holding time of about 1 hour after the second and third additions. Copper (II) hydroxide was added in two portions, 0.243 g (first portion) and 0.225 g (second portion), with a holding time of 1 hour after the first and second additions. The product was cooled to room temperature. The product was a clear blue viscous liquid.

[0129] Liquid Chelated Metal Polyol K

[0130] Polyethylene glycol 200 (348.33 g, Mn 200), terephthalic acid (199.33 g) and AA 105 (0.1374 g) was loaded into an insulated 4-neck 1000 mL round-bottom flask with N2 inlet adapter and thermocouple, with overhead stirring, and the flask was placed in a heating mantle. After degassing by circulating between vacuum (100 Torr) and N2, the reactor was completed with a heated and insulated Dean-stark type water separator and a condenser connected to an outlet adapter, wherein the N2 purge was left through an oil bubbler. The reaction profile for collecting distillate was 4.5 hours at 220°C, 4 hours at 230°C, 3 hours at 240°C, and 4.5 hours at 250°C, wherein polyethylene glycol 200 (28 g, Mn 200) was added as the polyester polyol cooled.

[0131] N,N,N',N'-tetrakis-(2-hydroxypropyl)ethylenediamine (42.24 g) and the polyester polyol described in this example (250.0 g) were placed in a dry 3-neck 500 mL round-bottom flask in a heating mantle and placed under an initial nitrogen (N2, gas) purge with overhead stirring, then degassed with a 50 torr / atmosphere N2 vacuum (cycled 3 times), and then switched to positive nitrogen (N2, gas). The flask was warmed to 180°C and at a temperature close to AA105 (0.1007 g) was added and stirred for 4 hours. The hydroxyl value of this material was 220 mg KOH / g. The contents of the flask were cooled to 80°C and transferred to a bottle.

[0132] The polyester amino polyol (previous paragraph, 60.0 grams) was charged into a 3-neck 100 mL round bottom flask placed in a heating mantle and placed under nitrogen (N2, gas) purge with overhead stirring. The flask was warmed to 100°C. Cobalt (II) acetate tetrahydrate was added in three portions, 2.51 g, 2.30 g and 2.21 g, respectively, with a holding time of 1 hour after the first and second additions and a holding time of 1.25 hours after the third addition. The product was cooled to room temperature. The product was a clear dark purple viscous liquid.

[0133] Liquid Chelated Metal Polyol L

[0134] Polyethylene glycol 200 (348.33 g, Mn 200), terephthalic acid (199.33 g) and AA 105 (0.1374 g) was loaded into an insulated 4-neck 1000 mL round-bottom flask with N2 inlet adapter and thermocouple, with overhead stirring, and the flask was placed in a heating mantle. After degassing by circulating between vacuum (100 Torr) and N2, the reactor was completed with a heated and insulated Dean-stark type water separator and a condenser connected to an outlet adapter, wherein the N2 purge was left through an oil bubbler. The reaction profile for collecting distillate was 4.5 hours at 220°C, 4 hours at 230°C, 3 hours at 240°C, and 4.5 hours at 250°C, wherein polyethylene glycol 200 (28 g, Mn 200) was added as the polyester polyol cooled.

[0135] N,N,N',N'-tetrakis-(2-hydroxypropyl)ethylenediamine (42.24 g) and the polyester polyol described in this example (250.0 g) were placed in a dry 3-neck 500 mL round-bottom flask in a heating mantle and placed under an initial nitrogen (N2, gas) purge with overhead stirring, then degassed with a 50 torr / atmosphere N2 vacuum (cycled 3 times), and then switched to positive nitrogen (N2, gas). The flask was warmed to 180°C and at a temperature close to AA105 (0.1007 g) was added and stirred for 4 hours. The hydroxyl value of this material was 220 mg KOH / g. The contents of the flask were cooled to 80°C and transferred to a bottle.

[0136] The polyester amino polyol (previous paragraph, 60.0 grams) was charged into a 3-neck 100 mL round bottom flask placed in a heating mantle and placed under a nitrogen (N2, gas) purge with overhead stirring. The flask was warmed to 100°C. Nickel (II) acetate tetrahydrate was added in three portions, 2.568 g, 2.244 g, and 2.208 g, respectively, with a holding time of 1 hour after the first, second, and third additions. The product was cooled to room temperature. The product was a clear dark blue-green viscous liquid.

[0137] Liquid Chelated Metal Polyol M

[0138] Polyethylene glycol 200 (348.33 g, Mn 200), terephthalic acid (199.33 g) and AA 105 (0.1374 g) was loaded into an insulated 4-neck 1000 mL round-bottom flask with N2 inlet adapter and thermocouple, with overhead stirring, and the flask was placed in a heating mantle. After degassing by circulating between vacuum (100 Torr) and N2, the reactor was completed with a heated and insulated Dean-stark type water separator and a condenser connected to an outlet adapter, wherein the N2 purge was left through an oil bubbler. The reaction profile for collecting distillate was 4.5 hours at 220°C, 4 hours at 230°C, 3 hours at 240°C, and 4.5 hours at 250°C, wherein polyethylene glycol 200 (28 g, Mn 200) was added as the polyester polyol cooled.

[0139] N,N,N',N'-tetrakis-(2-hydroxypropyl)ethylenediamine (42.24 g) and the polyester polyol described in this example (250.0 g) were placed in a dry 3-neck 500 mL round-bottom flask in a heating mantle and placed under an initial nitrogen (N2, gas) purge with overhead stirring, then degassed with a 50 torr / atmosphere N2 vacuum (cycled 3 times), and then switched to positive nitrogen (N2, gas). The flask was warmed to 180°C and at a temperature close to AA105 (0.1007 g) was added and stirred for 4 hours. The hydroxyl value of this material was 220 mg KOH / g. The contents of the flask were cooled to 80°C and transferred to a bottle.

[0140] Polyester amino polyol (previous paragraph, 60.0 g) was charged to a 3-neck 100 mL round bottom flask placed in a heating mantle and placed under a nitrogen (N2, gas) purge with overhead stirring. The flask was warmed to 100° C. Silver (I) acetate (1.680 g) was added to give a clear brown viscous stirrable liquid after a hold time of 1 hour.

[0141] Liquid Chelated Metal Polyol N

[0142] Polyester polyol A (250.0 g, OH#220 mg KOH / g) was loaded into a dry 3-neck 500 mL round bottom flask in a heating mantle and placed under an initial nitrogen (N2, gas) purge with overhead stirring. The flask was warmed to 100°C. Ethylenediaminetetraacetic acid dianhydride was added in four portions, 5.122 g (first portion), 4.842 g (second portion), 4.739 g (third portion) and 4.617 g (fourth portion), respectively, with a retention time of 30 minutes after the first, second and third additions, and a retention time of 60 minutes after the fourth addition. The product was cooled and transferred to a bottle.

[0143] The chelated polyester polyol with amino polycarboxylic acid moiety (previous paragraph, 55.0 g) was loaded into a 3-neck 100 mL round bottom flask placed in a heating mantle and placed under nitrogen (N2, gas) purge while stirring overhead. The flask was warmed to 100°C. Calcium acetate (II) monohydrate was added in two portions, 0.457 g (first portion) and 0.448 (second portion), respectively, with a holding time of 1 hour after each addition. The product was cooled to room temperature. The product was a golden viscous liquid.

[0144] Liquid Chelated Metal Polyol O

[0145] Polyester polyol A (250.0 g, OH#220 mg KOH / g) was loaded into a dry 3-neck 500 mL round bottom flask in a heating mantle and placed under an initial nitrogen (N2, gas) purge with overhead stirring. The flask was warmed to 100°C. Ethylenediaminetetraacetic acid dianhydride was added in four portions, 5.122 g (first portion), 4.842 g (second portion), 4.739 g (third portion) and 4.617 g (fourth portion), respectively, with a retention time of 30 minutes after the first, second and third additions, and a retention time of 60 minutes after the fourth addition. The product was cooled and transferred to a bottle.

[0146] The chelated polyester polyol with amino polycarboxylic acid part (previous paragraph, 55.0 grams) is loaded into a 3-neck 100mL round-bottom flask placed in a heating mantle and placed under nitrogen (N2, gas) purge while stirring overhead. The flask is warmed to 100°C. Zinc acetate (II) dihydrate is added in three portions, 1.187 grams (first portion), 1.169 grams (second portion) and 0.856 grams (third portion), respectively, with a retention time of 1 hour after each addition, and after the third addition at 120°C for another 1.5 hours. The product is cooled to room temperature. The product is a golden viscous liquid.

[0147] Liquid Chelated Metal Polyol P

[0148] Polyester polyol A (250.0 g, OH#220 mg KOH / g) was loaded into a dry 3-neck 500 mL round bottom flask in a heating mantle and placed under an initial nitrogen (N2, gas) purge with overhead stirring. The flask was warmed to 100°C. Ethylenediaminetetraacetic acid dianhydride was added in four portions, 5.122 g (first portion), 4.842 g (second portion), 4.739 g (third portion) and 4.617 g (fourth portion), respectively, with a retention time of 30 minutes after the first, second and third additions, and a retention time of 60 minutes after the fourth addition. The product was cooled and transferred to a bottle.

[0149] The chelated polyester polyol with amino polycarboxylic acid part (previous paragraph, 55.0 grams) is loaded into a 3-neck 100mL round-bottom flask placed in a heating mantle and placed under nitrogen (N2, gas) purge while stirring overhead. The flask is warmed to 75°C. Silver (I) acetate is added in two portions, 0.684 grams (first portion) and 0.602 grams (second portion), respectively, with a retention time of 20 hours after the first addition and 1 hour after the second addition. The product is cooled to room temperature. The product is an amber viscous liquid.

[0150] Table 1 - Polyisocyanuric Acids for Polyurethane-Based Molded Foams Using Liquid Chelated Transition Metal Polyols Reaction mixtures of ester examples and comparative examples

[0151]

[0152] Table 2 - Polyisocyanuric Acids for Polyurethane-Based Cup Foams Using Liquid Chelated Transition Metal Polyols Reaction mixtures of ester examples and comparative examples

[0153]

[0154]

[0155] Polyurethane-based molded foams were prepared as follows. For each example (EX) and comparative example (CEx), the components of the isocyanate-reactive composition provided in Table 1 were mixed in a beaker at 2,000 rpm with a rotary mixer for 10 seconds (s). Next, the isocyanate-reactive composition and the isocyanate were mixed again in a beaker at 3,000 rpm for 4 s. After mixing, the contents of the beaker were immediately poured into a mold (300 millimeters (mm) × 200 mm × 50 mm) preheated to 60°C. After curing at 60°C for 15 minutes, the foam was removed from the mold. The core density of the molded foam was about 40 kg / m 3 .

[0156] A cup-shaped foam based on polyurethane was prepared as follows. A total weight of 80 grams (g) of reaction mixture was prepared for each example and comparative example provided in Table 2 in a 500 mL beaker. The components of the isocyanate reactive composition provided in Table 2 were mixed with a rotary mixer at 2000 rpm for 10 seconds (s). Next, the isocyanate reactive composition and the isocyanate were mixed again in a beaker at 3000 rpm for 5 seconds at room temperature (23° C., 50% relative humidity). After 24 hours (h), the foam portion that had risen above the top plane of the beaker was removed, and then a 2.54 cm×2.54 cm×2.54 cm center core was cut.

[0157] Flue gas composition analysis

[0158] Pyrolysis tests were performed using a Frontier Labs 2020D pyrolyzer mounted on an Agilent 6890GC with an FID detector. Approximately 200-250 μg of sample was weighed into a Frontier labs silicon-lined stainless steel cup. The sample cup was placed in an oven for pyrolysis in single-gun mode, analyzed at 600°C in air for 2 minutes, and then analyzed for another 2 minutes under helium conditions. A micro-cryogenic trap (MCT) was used to capture volatile products emitted from the sample at the head of the separation column. A 10m×0.32mm ID×5μm PoraBond Q column from Agilent was used, and separation was achieved using HP-1 (10m×0.53mm×2.65μm) as a guard column. The rear inlet pressure was used for backflush purposes (0.5m×0.53mm guard column, using the rear inlet as the head pressure tee for the PoraBond Q and HP-1 columns). HCN was detected on the back FID detector. HCN concentration comparisons were made using HCN peak areas normalized to sample weight. The relative HCN content of a transition metal-containing sample was defined as the ratio of its normalized HCN peak area divided by the normalized HCN peak area of ​​the corresponding comparative control sample without transition metal.

[0159] GC conditions: front inlet: 300°C; 1:1 split injector; ramp pressure: 4.9 psi for 1.5 min, then increased to 3.1 psi at 50 psi / min; back inlet: 4 psi; GC column oven: 40°C for 3 min, then increased to 240°C at 30°C / min; FID: 250°C, H2 flow: 40 mL / min, air flow: 450 mL / min, tail gas (N2): 30 mL / min, 50 Hz.

[0160] result

[0161] As seen in Tables 3 and 4, a significant reduction in HCN generation was achieved using molded foams containing liquid chelated transition metal polyols.

[0162] Table 3

[0163] Comparative Example A Example 1 Example 2 Example 3 Metal ion weight% 0 0.50 0.37 0.22 Relative HCN content 1.00 0.89 0.12 0.27

[0164] Table 4

[0165] Comparative Example B Example 4 Metal ion weight% 0 0.22 Relative HCN content 1.00 0.67

[0166] As seen in Table 5, a significant reduction in HCN generation was achieved using cup-shaped foams containing a liquid chelated transition metal polyol.

[0167] Table 5

[0168] Comparative Example C Example 5 Metal ion weight% 0 0.22 Relative HCN content 1.00 0.69

Claims

1. A metal chelated polyester polyol liquid, comprising: The reaction products of: A chelated polyester polyol having a chelating portion and a metal compound having a metal ion, wherein the chelated polyester polyol is formed by: A chemical reaction of a monomer of a liquid polyester polyol or the liquid polyester polyol formed from the monomer of the liquid polyester polyol and a chelating agent having the chelating moiety, wherein the chelating moiety is selected from a dianhydride moiety, an amino-based chelating moiety and a combination thereof, wherein: The chelating agent having the dianhydride portion chemically reacts with the monomer of the liquid polyester polyol or the liquid polyester polyol formed from the monomer of the liquid polyester polyol to form the chelated polyester polyol having the aminopolycarboxylic acid portion; and The chelating agent having the amino-based chelating moiety chemically reacts with a monomer of the liquid polyester polyol or one of the liquid polyester polyols formed from the monomer of the liquid polyester polyol to form a polyester amino polyol as the chelated polyester polyol; and wherein the chelating portion of the chelated polyester polyol chelates the metal ion to form the metal chelated polyester polyol liquid having a molar ratio of the metal ion to the chelating portion of 0.05:1 to 2:1, The metal ions are selected from the group consisting of copper, zinc, silver, iron, manganese, cobalt, nickel, zirconium, calcium, aluminum, barium, cadmium, gallium, indium, lead, magnesium, mercury, palladium, scandium, strontium, thorium, titanium, vanadium and combinations thereof, The chelating agent having the dianhydride portion is an aminopolycarboxylic acid dianhydride compound, The chelating agent having the amino-based chelating moiety is selected from alkoxylated diamines, alkoxylated triamines, alkoxylated tetraamines and combinations thereof, aminopolycarboxylic acids containing one or more nitrogen atoms connected to two or more carboxyl groups via carbon atoms, tertiary polyamino compounds having at least two tertiary nitrogens connected via carbon atoms and at least one alcohol group and up to five alcohol groups, and The ratio of the moles of the monomers used to form the liquid polyester polyol to the moles of the chelating agent ranges from 3:1 to 200:

1.

2. A metal chelated polyether polyol liquid, comprising: The reaction products of: A chelated polyether polyol having a chelating portion and a metal compound having a metal ion, wherein the chelated polyether polyol is formed by: A chemical reaction of a monomer of a liquid polyether polyol or the liquid polyether polyol formed from the monomer of the liquid polyether polyol and a chelating agent having the chelating moiety, wherein the chelating moiety is selected from a dianhydride moiety, an amino-based chelating moiety and a combination thereof, wherein: The chelating agent having the dianhydride portion chemically reacts with the monomer of the liquid polyether polyol or the liquid polyether polyol formed from the monomer of the liquid polyether polyol to form the chelated polyether polyol having the aminopolycarboxylic acid portion; and The chelating agent having the amino-based chelating moiety chemically reacts with a monomer of the liquid polyether polyol or one of the liquid polyether polyols formed from the monomer of the liquid polyether polyol to form a polyether amino polyol as the chelated polyether polyol; and wherein the chelating portion of the chelated polyether polyol chelates the metal ion to form the metal chelated polyether polyol liquid having a molar ratio of the metal ion to the chelating portion of 0.05:1 to 2:1, The metal ions are selected from the group consisting of copper, zinc, silver, iron, manganese, cobalt, nickel, zirconium, calcium, aluminum, barium, cadmium, gallium, indium, lead, magnesium, mercury, palladium, scandium, strontium, thorium, titanium, vanadium and combinations thereof, The chelating agent having the dianhydride portion is an aminopolycarboxylic acid dianhydride compound, The chelating agent having the amino-based chelating moiety is selected from alkoxylated diamines, alkoxylated triamines, alkoxylated tetraamines and combinations thereof, aminopolycarboxylic acids containing one or more nitrogen atoms connected to two or more carboxyl groups via carbon atoms, tertiary polyamino compounds having at least two tertiary nitrogens connected via carbon atoms and at least one alcohol group and up to five alcohol groups, and The ratio of the number of moles of the monomers used to form the liquid polyether polyol to the number of moles of the chelating agent ranges from 2:1 to 200:

1.

3. The metal chelated polyester polyol liquid according to claim 1 or the metal chelated polyether polyol liquid according to claim 2, wherein: The chelating agent having the dianhydride portion chemically reacts with the liquid polyester polyol at a molar ratio of 1:1.5 to 1:100 to form the chelated polyester polyol having the aminopolycarboxylic acid portion; or The chelating agent having the dianhydride portion chemically reacts with the liquid polyether polyol at a molar ratio of 1:1.5 to 1:100 to form the chelated polyether polyol having the aminopolycarboxylic acid portion; or The chelating agent having the dianhydride moiety is selected from the group consisting of ethylenediaminetetraacetic dianhydride, diethylenetriaminepentaacetic dianhydride, and combinations thereof.

4. The metal chelated polyester polyol liquid according to claim 1 or the metal chelated polyether polyol liquid according to claim 2, The metal compound is selected from the group consisting of hydroxides, carbonates, carboxylates and combinations thereof.

5. The metal chelated polyester polyol liquid according to claim 1 or the metal chelated polyether polyol liquid according to claim 2, The metal compound is a metal salt.

6. The metal chelated polyester polyol liquid according to claim 1 or the metal chelated polyether polyol liquid according to claim 2, The metal compound is selected from the group consisting of copper (II) hydroxide, copper (II) carbonate, basic copper (II) carbonate, copper (II) acetate, cobalt (II) acetate, nickel (II) acetate, silver (I) acetate, zinc (II) acetate, calcium (II) acetate and combinations thereof.

7. An isocyanate-reactive composition having hydroxyl moieties for forming a polyurethane polymer, comprising: 0.1 to 100 weight percent of the metal chelated polyester polyol liquid according to any one of claims 1 and 3-6; and Optionally up to 99.9 weight percent of a polyol is used to form the isocyanate-reactive composition, the weight percent being based on the total weight of the isocyanate-reactive composition.

8. The isocyanate reactive composition according to claim 7, further comprising a compound selected from the following for the metal chelated polyester polyol liquid according to any one of claims 1 and 3-6: 0.1 wt % to 7.0 wt % phosphorus from a flame retardant compound, the wt % phosphorus based on the total weight of the isocyanate-reactive composition; 0.05 wt % to 14.0 wt % of the metal from the metal chelated polyester polyol liquid, the wt % of metal based on the total weight of the isocyanate reactive composition; and combinations thereof.

9. An isocyanate-reactive composition having hydroxyl moieties for forming a polyurethane polymer, comprising: 0.1 to 100 weight percent of the metal chelate polyether polyol liquid according to any one of claims 2 to 6; and Optionally up to 99.9 weight percent of a polyol is used to form the isocyanate-reactive composition, the weight percent being based on the total weight of the isocyanate-reactive composition.

10. The isocyanate reactive composition according to claim 9, further comprising a compound selected from the following for the metal chelate polyether polyol liquid according to any one of claims 2 to 6: 0.1 wt % to 1.5 wt % phosphorus from a flame retardant compound, the wt % phosphorus based on the total weight of the isocyanate-reactive composition; 0.05 wt % to 3.0 wt % of metal from the metal chelated polyether polyol liquid, the wt % of metal being based on the total weight of the isocyanate reactive composition; and combinations thereof.

11. A reaction mixture for forming a polyurethane polymer, comprising: an isocyanate compound having an isocyanate moiety; and The isocyanate-reactive composition of any one of claims 7 to 10, wherein the reaction mixture has a molar ratio of the isocyanate moieties to the hydroxyl moieties of 0.90:1 to 7:

1.

12. The reaction mixture of claim 11, wherein the reaction mixture comprises a compound selected from the group consisting of water, a catalyst, a surfactant, a blowing agent, or a combination thereof.

13. A polyurethane-based polymer formed from the reaction mixture of claim 11 or 12.

14. A method for preparing a metal chelated polyester polyol liquid according to any one of claims 1 and 3-6 or a metal chelated polyether polyol liquid according to any one of claims 2-6, the method for preparing the metal chelated polyester polyol liquid comprising: reacting a monomer of a liquid polyester polyol or the liquid polyester polyol formed from the monomer of the liquid polyester polyol with a chelating agent having a chelating moiety to form a chelated polyester polyol, wherein the chelating moiety is selected from a dianhydride moiety, an amino-based chelating moiety, and combinations thereof, wherein: The chelating agent having the dianhydride portion chemically reacts with the monomer of the liquid polyester polyol or the liquid polyester polyol formed from the monomer of the liquid polyester polyol to form the chelated polyester polyol having the aminopolycarboxylic acid portion; and the chelating agent having the amino-based chelating moiety chemically reacts with the monomer of the liquid polyester polyol or the liquid polyester polyol formed from the monomer of the liquid polyester polyol to form a polyester amino polyol as the chelated polyester polyol; and reacting the chelated polyester polyol having the chelating moiety with a metal compound having a metal ion, wherein the chelating moiety of the chelated polyester polyol chelates the metal ion to form the metal chelated polyester polyol liquid, the reaction having a molar ratio of the metal ion to the chelating moiety of 0.05:1 to 2:1; or The method for preparing the metal chelate polyether polyol liquid comprises: reacting a monomer of a liquid polyether polyol or the liquid polyether polyol formed from the monomer of the liquid polyether polyol with a chelating agent having a chelating moiety to form a chelated polyether polyol, wherein the chelating moiety is selected from a dianhydride moiety, an amino-based chelating moiety, and combinations thereof, wherein: The chelating agent having the dianhydride portion chemically reacts with the monomer of the liquid polyether polyol or the liquid polyether polyol formed from the monomer of the liquid polyether polyol to form the chelated polyether polyol having the aminopolycarboxylic acid portion; and the chelating agent having the amino-based chelating moiety chemically reacts with the monomer of the liquid polyether polyol or the liquid polyether polyol formed from the monomer of the liquid polyether polyol to form a polyether amino polyol as the chelating polyether polyol; and The chelated polyether polyol having the chelating moiety is reacted with a metal compound having a metal ion, wherein the chelating moiety of the chelated polyether polyol chelates the metal ion to form the metal chelated polyether polyol liquid, the reaction having a molar ratio of the metal ion to the chelating moiety of 0.05:1 to 2:1.

Citation Information

Patent Citations

  • Use of trialkyl phosphate as a smoke suppressant in polyurethane foam

    US20140206786A1

  • Siloxane-oxyalkylene block copolymers

    US2834748A

  • Organosiloxane ethers

    US2846458A

  • Siloxane oxyalkylene block copolymers

    US2917480A

  • Polyisocyanate based polymers perpared from formulations including non-silicone surfactants and method for the preparation thereof

    US5600019A