Alkaline earth aluminate phosphor, light emitting device, and method for producing alkaline earth aluminate phosphor

By adjusting the molar ratio of elements and heat treatment conditions in the alkaline earth aluminate phosphor, the problem of insufficient luminous intensity is solved and the effect of increasing luminous intensity within a specific wavelength range is achieved. It is suitable for light-emitting devices in the medical and plant growth fields.

CN114106818BActive Publication Date: 2024-10-18NICHIA CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202110879533.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-02
Publication Date
2024-10-18
Estimated Expiration
2041-08-02

AI Technical Summary

Technical Problem

Existing alkaline earth aluminate phosphors have insufficient luminous intensity in light-emitting devices, making it difficult to meet the needs of specific applications such as medical treatment and plant growth.

Method used

By rationally adjusting the molar ratio of elements in the alkaline earth aluminate phosphor, especially the proportions of Al, Cr, Mn, Eu and other elements, it has a luminescence peak wavelength in the range of 720nm and above and 900nm and below, and has a luminescence peak wavelength in the range of 1000nm. Heat treatment in a reducing atmosphere is performed at a temperature between 1500°C and 1500°C to form a phosphor with increased luminous intensity.

Benefits of technology

The alkaline earth aluminate phosphor that increases the luminous intensity in a specific wavelength range is suitable for light-emitting devices in the fields of medical treatment and plant growth, and can more effectively transmit into living organisms or promote plant growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114106818B_ABST
    Figure CN114106818B_ABST
Patent Text Reader

Abstract

The present invention provides an alkaline earth aluminate phosphor having improved luminous intensity, a light emitting device, and a method for producing the alkaline earth aluminate phosphor. The present invention provides an alkaline earth aluminate phosphor comprising at least one element A selected from alkaline earth metal elements, Al, and Cr, and optionally at least one element M selected from Group 13 elements other than Al. 1 , and at least one element M selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm 2 The alkaline earth aluminate phosphor has the following composition: the molar ratio of element A is within the range of 1.0 to 4.0, Al and element M 1 The total molar ratio of is within the range of 4.0 to 14.0, the molar ratio of Cr is within the range of 0.004 to 0.8, and the element M 2 The molar ratio of Cr to element M is within the range of 0 to 0.4. 2 The total molar ratio of Al and element M is within the range of 0.004 to 0.8. 1 When the total molar ratio of the above elements M is set to 1, 1 The molar ratio of is 0.7 or less, and the alkaline earth aluminate phosphor has a light emission peak wavelength in the range of 720 nm to 900 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to an alkaline earth aluminate phosphor, a light-emitting device and a method for manufacturing the alkaline earth aluminate phosphor. Background Art

[0002] By combining excitation light sources such as light emitting diodes (LEDs) and laser diodes (LDs) with phosphors, various light emitting devices that emit white light, bulb-colored light, etc. have been developed based on the principle of light color mixing. These light emitting devices are used in a wide range of fields, such as lighting, automotive, medical, and backlights for liquid crystal displays.

[0003] In such a light emitting device, various types of phosphors are used depending on the application. For example, Non-Patent Document 1 (Ruixia Zhong et al. "Red phosphrescence in Sr4Al 14 O 25 :Cr 3+ ,Eu 3+ ,Dy 3+ "Through persistent energy transfer" APPLIED PHYSICS LETTERS 88.201916 (2006)) records that Sr4Al has a peak emission wavelength of 693nm 14 O 25 :Cr 3+ ,Eu 3+ ,Dy 3+ Represents an alkaline earth aluminate phosphor.

[0004] Prior art literature

[0005] Non-patent literature

[0006] Non-patent literature 1: Ruixia Zhong et al. "Red phosphrescence in Sr4Al 14 O 25 :Cr 3+ ,Eu 3+ ,Dy 3+ through persistent energy transfer”APPLIED PHYSICS LETTERS 88.201916(2006) Summary of the invention

[0007] Problems to be solved by the invention

[0008] An object of the present application is to provide an alkaline earth aluminate phosphor having improved luminous intensity, a light-emitting device, and a method for producing the alkaline earth aluminate phosphor.

[0009] Solutions to the problem

[0010] The first aspect relates to an alkaline earth aluminate phosphor comprising at least one element A selected from alkaline earth metal elements, Al, and Cr, and optionally comprising an element M as required. 1 and the element M contained as required 2 , the above element M 1 is at least one selected from Group 13 elements other than Al, wherein the element M 2 is at least one selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm, and the alkaline earth aluminate phosphor has the following composition: the molar ratio of the element A is within a range of 1.0 to 4.0, and the Al and the element M are 1 The total molar ratio of is within the range of 4.0 to 14.0, the molar ratio of Cr is within the range of 0.004 to 0.8, and the element M 2 The molar ratio of Cr to the element M is within the range of 0 to 0.4. 2 The total molar ratio of Al and the element M is within the range of 0.004 to 0.8. 1 When the total molar ratio of the above elements M is set to 1, 1 The molar ratio of is 0.7 or less, and the alkaline earth aluminate phosphor has a light emission peak wavelength in the range of 720 nm to 900 nm.

[0011] A second aspect relates to a light emitting device including: the alkaline earth aluminate phosphor described above; and a light source for irradiating the alkaline earth aluminate phosphor.

[0012] A third aspect relates to a method for producing an alkaline earth aluminate phosphor, wherein the alkaline earth aluminate phosphor comprises a first compound containing at least one element A selected from alkaline earth metal elements, a second compound containing Al, and a third compound containing Cr, and optionally comprises a fourth compound contained as required, and a fifth compound contained as required, wherein the fourth compound is at least one element M selected from Group 13 elements other than Al. 1 The fifth compound is at least one element M selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm. 2, at least one compound selected from the first compound, the second compound, and the third compound is an oxide, the method comprising: a step of preparing a raw material mixture, the raw material mixture comprising the first compound, the second compound, and the third compound, and optionally comprising a fourth compound as required, and a fifth compound as required, so that the molar ratio of the element A relative to 1 mol of the composition is within a range of 1.0 to 4.0, and the molar ratio of the Al to the element M is within a range of 1.0 to 4.0. 1 The total molar ratio of is within the range of 4.0 to 14.0, the molar ratio of Cr is within the range of 0.004 to 0.8, and the element M 2 The molar ratio of Al to the element M is within the range of 0 to 0.4, and the Al and the element M 1 When the total molar ratio of the above elements M is set to 1, 1 The molar ratio of is 0.7 or less; and the step of heat treating the raw material mixture in a reducing atmosphere at a temperature in the range of 1000°C to 1500°C to obtain an alkaline earth aluminate phosphor.

[0013] Effects of the Invention

[0014] According to the present application, it is possible to provide an alkaline earth aluminate phosphor having improved emission intensity, a light-emitting device using the alkaline earth aluminate phosphor, and a method for producing the alkaline earth aluminate phosphor. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a graph showing the emission spectrum of the alkaline earth aluminate phosphor of Example 1 and the emission spectrum of the compound having the composition of the alkaline earth aluminate of Comparative Example 1.

[0016] Figure 2 This is a diagram showing the excitation spectrum of the alkaline earth aluminate phosphor of Example 1.

[0017] Figure 3 This is a graph showing the emission spectra of the alkaline earth aluminate phosphors of Examples 4, 5, and 6 and the emission spectrum of the compound having the composition of an alkaline earth aluminate of Comparative Example 2. DETAILED DESCRIPTION

[0018] Hereinafter, the alkaline earth aluminate phosphor, the light-emitting device and the method for producing the alkaline earth aluminate phosphor of the present invention will be described. However, the embodiments shown below are only examples for specifying the technical idea of ​​the present invention, and the present invention is not limited to the following alkaline earth aluminate phosphor, the light-emitting device and the method for producing the alkaline earth aluminate phosphor. It should be noted that the relationship between the color name and the chromaticity coordinates, the relationship between the wavelength range of light and the color name of monochromatic light, etc. are in accordance with JIS Z8110. It should be noted that in this specification, in the formula representing the composition of the phosphor, the multiple elements recorded by dividing with commas (,) indicate that at least one element of these multiple elements is contained in the composition, and two or more elements are optionally contained in combination. In addition, in this specification, in the formula representing the composition of the phosphor, the elements and their molar ratios constituting the mother crystal are indicated before the colon (:), and the activation element is indicated after the colon (:). In this specification, unless otherwise specified, the "molar ratio" indicates the ratio of each element in 1 mole of the chemical composition of the compound or phosphor.

[0019] Depending on the visual recognition object, the light-emitting device using a fluorescent body is required to emit the most suitable light. For example, in medical sites, it is sometimes required to easily obtain information in the body. As a light absorber, the body contains water, hemoglobin, melanin, etc. For example, hemoglobin has a high absorption rate of light in the visible light region with a wavelength less than 650nm. For a light-emitting device that emits light in the visible light region, the light in the visible light region is difficult to transmit in the body, and it is difficult to obtain information in the body. Therefore, there is a situation of seeking a light-emitting device that emits light in the near-infrared wavelength range of more than 650nm and less than 1000nm, which is called the "biological window" and is easy to transmit in the body. For example, if the increase or decrease in the oxygen concentration in the blood in the body can be measured by the increase or decrease in the absorption of light by hemoglobin bound to oxygen, the information in the body can be easily obtained by irradiating light from the light-emitting device.

[0020] In addition, when environmental changes such as climate change occur, it is expected to stably supply plants such as vegetables and improve the production efficiency of plants. Plant factories that can be artificially managed can stably supply safe vegetables to the market and are expected to be the next generation of industries. In such plant factories, it is required to irradiate light that can promote the growth of plants. The reaction of plants to light is divided into photosynthesis and photomorphogenesis. Photosynthesis is a reaction that uses light energy to decompose water, produce oxygen, and fix carbon dioxide to organic matter. It is a necessary reaction for the growth of plants. Photomorphogenesis is a morphological reaction that uses light as a signal to perform seed germination, differentiation (germination formation, leaf formation, etc.), movement (stomatal opening and closing, chloroplast movement), light refraction, etc. It is known that in the photomorphogenesis reaction, light in the wavelength region above 690nm and below 800nm ​​will affect the photoreceptors of plants. Therefore, there is a demand for light-emitting devices used in plant factories, etc. to be able to irradiate light in a wavelength region that affects plant photoreceptors (chlorophyll a, chlorophyll b, carotenoids, phytochromes, cryptochromes, phototropins) and promotes plant growth.

[0021] The same is true for the alkaline earth aluminate phosphors mentioned above. When they are combined with excitation light sources such as light emitting diodes (LEDs) and laser diodes (LDs) to form light-emitting devices, there is room for improving the light emission characteristics of the phosphors to make them suitable light sources for these applications.

[0022] Alkaline earth aluminate phosphor

[0023] The alkaline earth aluminate phosphor of the first embodiment contains at least one element A, Al, and Cr selected from alkaline earth metal elements, and optionally contains an element M as required. 1 and the element M contained as required 2 , the above element M 1 is at least one selected from Group 13 elements other than Al, wherein the element M 1 is at least one selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm, and the alkaline earth aluminate phosphor has the following composition: the molar ratio of the element A is within a range of 1.0 to 4.0, and the Al and the element M are 1 The total molar ratio of is within the range of 4.0 to 14.0, the molar ratio of Cr is within the range of 0.004 to 0.8, and the element M 2 The molar ratio of Cr to the element M is within the range of 0 to 0.4. 2 The total molar ratio of Al and the element M is within the range of 0.004 to 0.8. 1 When the total molar ratio of the above elements M is set to 1,1 The molar ratio of is 0.70 or less, and the alkaline earth aluminate phosphor has a luminescence peak wavelength in the range of 720 nm to 900 nm. The alkaline earth aluminate phosphor absorbs the excitation light and can emit light with a luminescence peak wavelength in the range of 720 nm to 900 nm, can emit light with a luminescence peak wavelength in the near-infrared wavelength range known as the "biological window", and can emit light that affects the photoreceptors of plants. In this specification, the near-infrared wavelength range refers to a wavelength range of 700 nm to 2500 nm.

[0024] For alkaline earth aluminate phosphors, preferably the elements A, Al, Cr, and the element M contained as required are 1 and the element M contained as required 2 It has a composition represented by the following formula (I).

[0025] A x (Al 1-y M 1 y ) z O x+3 / 2z :Cr v ,M 2 w (I)

[0026] (In formula (I), A is at least one element selected from alkaline earth metal elements, M 1 is at least one element selected from Group 13 elements other than Al, M 2 is at least one element selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm, and v, w, x, y and z satisfy 0.004≤v≤0.8, 0≤w≤0.4, 0.004≤v+w≤0.8, 1.0≤4.0, 0≤y≤0.7, and 4.0≤z≤14.0. )

[0027] For the alkaline earth aluminate phosphor having the above-mentioned composition, by sintering in a reducing atmosphere, Cr as an activator becomes easy to enter the matrix crystal of the alkaline earth aluminate phosphor in a state with a valence of trivalent, and thus can absorb the excitation light and emit light with a luminescence peak wavelength in the range of above 720nm and below 900nm.

[0028] Element A is at least one element selected from alkaline earth metal elements, and may also contain two or more elements. Element A may be at least one selected from Ca, Sr and Ba. Element A may also contain two or more elements selected from alkaline earth metal elements. Element A may be Sr, or Sr and Ca. When Element A contains two or more elements selected from alkaline earth metal elements,a and element A b In the case of a With element A b In terms of the molar ratio of element A a With element A b When the total molar ratio of element A is set to 10, a With element A b The molar ratio (A a / A b ) can be 1 / 9 or more, or 9 / 1 or less. The molar ratio x of the element A in the composition of the alkaline earth aluminate phosphor is within the range of 1.0 or more and 4.0 or less, and the molar ratio x of Al and the element M in 1 mol of the composition of the alkaline earth aluminate phosphor is 1 / 9 or more and 9 / 1 or less. 1 When the total molar ratio of is 14, the molar ratio x is preferably 4.

[0029] When the element A contains two or more elements selected from alkaline earth metal elements, the alkaline earth aluminate phosphor can have a composition represented by the following formula (I-1).

[0030] (A a 1-u A b u ) x (Al 1-y M 1 y ) z O x+3 / 2z :Cr v , M 2 w (I-1)

[0031] (In formula (I-1), A a is an element selected from alkaline earth metal elements, A b To remove A a An element other than one selected from the group consisting of alkaline earth metal elements, M 1 is at least one element selected from Group 13 elements other than Al, M 2 is at least one element selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm, and u, v, w, x, y and z satisfy 0.1≤u≤0.9, 0.004≤v≤0.8, 0≤w≤0.4, 0.004≤v+w≤0.8, 1.0≤4.0, 0≤y≤0.7, 4.0≤z≤14.0. )

[0032] The Al contained in the composition of the alkaline earth aluminate phosphor constitutes a crystal framework of a parent crystal of the alkaline earth aluminate phosphor together with the element A and oxygen (O). The composition of the alkaline earth aluminate phosphor contains at least one element M selected from the group 13 elements other than Al in addition to Al. 1 In the case of Al and element M 1 When the total molar ratio z of is within the range of 4.0 or more and 14.0 or less (4.0≤z≤14.0), the crystal skeleton of the parent crystal of the alkaline earth aluminate phosphor can also be formed. 1 In the case of Al and element M 1 When the total molar ratio of Al is set to 1, it is preferred to contain 0.3 mol or more of Al. 1 When the total molar ratio of Al is set to 1, if Al is contained in an amount of 0.3 mol or more, a stable crystal structure can be maintained.

[0033] The composition of the alkaline earth aluminate phosphor contains the element M 1 In the case of 1 It is preferably at least one element selected from the elements of Group 13 except Al. Element M 1 It is preferably at least one selected from B, Ga, In, and Tl, more preferably at least one selected from B, Ga, and In, and may be at least one selected from B and Ga, or may be Ga. The element M contained in the composition of the alkaline earth aluminate phosphor 1 For example, Al and element M in the composition 1 When the sum of is set to 1, the element M 1 The molar ratio y is preferably in the range of 0 to 0.7 (0≤y≤0.7). It may be in the range of 0.1 to 0.7 (0.1≤y≤0.7), or in the range of 0.2 to 0.6 (0.2≤y≤0.6).

[0034] The composition of the alkaline earth aluminate phosphor contains the element M 1 , and Al and element M in the composition 1 When the sum of is set to 1, the element M 1 When the molar ratio y is within the range of 0.1 to 0.7 (0.1≤y≤0.7), the emission wavelength and shape can be changed without significantly reducing the emission efficiency.

[0035] In the composition of the alkaline earth aluminate phosphor, the element A may be at least one element selected from Ca, Sr and Ba, and the element M may be at least one element selected from Ca, Sr and Ba. 1It can be at least one element selected from Ba, Ga and In. In the composition of the alkaline earth aluminate phosphor, element A can be Sr, element M can be 1 It can be Ga.

[0036] The alkaline earth aluminate phosphor contains Cr, which is an activation element. The molar ratio v of Cr relative to 1 mol of the alkaline earth aluminate phosphor is preferably in the range of 0.004 to 0.8 (0.004≤v≤0.8), and may be in the range of 0.005 to 0.7 (0.005≤v≤0.7), in the range of 0.008 to 0.6 (0.008≤v≤0.6), or in the range of 0.010 to 0.5 (0.010≤v≤0.5). The alkaline earth aluminate phosphor contains Cr as an activation element. When the molar ratio of Cr relative to 1 mol of the alkaline earth aluminate phosphor is in the range of 0.004 to 0.8, a phosphor emitting light having a peak emission wavelength in the range of 720 nm to 900 nm can be obtained.

[0037] The alkaline earth aluminate phosphor may contain at least one element M selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm as a co-activating element in addition to Cr. 2 The alkaline earth aluminate phosphor contains element M 2 In the case of 2 The characteristic luminescence brought by the element M 2 In the case of Cr, the phosphor may have a light emission peak wavelength in a wavelength range different from that of an alkaline earth metal aluminate phosphor containing only Cr. The alkaline earth metal aluminate phosphor may contain an element M serving as a co-activating element in its composition. 2 , element M 2 The molar ratio of Cr to M is within the range of 0 to 0.4 (0≤w≤0.4), and may be within the range of 0.1 to 0.3 (0.1≤w≤0.3). 2 The total molar ratio of is in the range of 0.004 to 0.8.

[0038] In the luminescence spectrum of the alkaline earth aluminate phosphor, the half-width value of the luminescence peak wavelength in the range of 720 nm to 900 nm is preferably 80 nm or more, and may be 90 nm or more, 150 nm or less, or 120 nm or less. If light having a luminescence peak wavelength in the range of 720 nm to 900 nm is emitted from the alkaline earth aluminate phosphor, information on the increase or decrease of the oxygen concentration in the blood in the organism can be obtained by, for example, the increase or decrease of the absorption of light by hemoglobin bound to oxygen. In the organism, light absorption and scattering occur. In order to measure the subtle changes in the light propagation behavior in the blood in the organism, it is preferred that the half-width value of the luminescence peak in the range of 720 nm to 900 nm emitted from the light emitting device is wide. In addition, it is expected that when irradiated with light, the color (hereinafter also referred to as "color rendering") presented by the object has a luminescence spectrum in a wide area. When the half-width value is wide, light with excellent color rendering can be emitted. For example, in a plant factory, even when emitting light in a wavelength region that affects the growth of plants, it is sometimes required to emit light that does not destroy the spectral balance of the light, so that the operator can operate easily. In the luminescence spectrum of alkaline earth aluminate phosphors, the half-width value of the luminescence peak in the range of 720nm to 900nm is 80nm or more, and if it is 150nm or less, the color rendering can be improved. The half-width value refers to the half-value full width (Full Width at HalfMaximum) of the luminescence peak in the luminescence spectrum, which refers to the wavelength width of the luminescence peak that shows 50% of the maximum value of the luminescence peak in the luminescence spectrum.

[0039] Light-emitting device

[0040] The light emitting device includes an alkaline earth aluminate phosphor and a light source for irradiating the alkaline earth aluminate phosphor. The aluminate phosphor according to one embodiment of the present invention can be used as a member constituting a wavelength conversion member together with a light-transmitting material.

[0041] Preferably, the light emitting device includes a light emitting element such as an LED or LD as a light source, and a wavelength converting member including an alkaline earth aluminate phosphor that emits light when irradiated with light from the light emitting element.

[0042] As the light emitting element, for example, an LED chip or an LD chip can be used. The LED chip or the LD chip is a semiconductor light emitting element using a nitride-based semiconductor.

[0043] The light-emitting element preferably has a peak emission wavelength in the range of greater than 380 nm and less than 500 nm, more preferably has a peak emission wavelength in the range of greater than 390 nm and less than 495 nm, further preferably has a peak emission wavelength in the range of greater than 400 nm and less than 490 nm, and particularly preferably has a peak emission wavelength in the range of greater than 420 nm and less than 490 nm.

[0044] The wavelength conversion member includes an alkaline earth aluminate phosphor and a light-transmitting material.

[0045] Both the alkaline earth aluminate phosphor and the light-transmitting material may contain other phosphors besides the alkaline earth aluminate phosphor.

[0046] The alkaline earth aluminate phosphor may be used as the first phosphor, and a second phosphor having a different emission peak wavelength from the first phosphor may be included. The second phosphor may be a single phosphor or a combination of two or more phosphors. As the second phosphor, for example, a phosphor having a composition represented by the following formula may be cited.

[0047] M 1 10 (PO4)6Cl2:Eu(i)

[0048] (In formula (i), M 1 is at least one element selected from Ca, Sr and Ba. )

[0049] M 2 MgAl 10 O 17 :Mn,Eu(ii)

[0050] (In formula (ii), M 2 is at least one element selected from Ba and Sr. )

[0051] M 3 8MgSi4O 16 Cl2:Eu(iii)

[0052] (In formula (iii), M 3 is at least one element selected from Ca, Sr and Ba. )

[0053] S4A 14 O 25 :Eu(iv)

[0054] M 4 3M 5 5O 12 :Ce(v)

[0055] (In formula (v), M 4is at least one element selected from Y and Gd, M 5 At least one element selected from Al and Ga.

[0056] 3M 6 5O 12 :Ce(vi)

[0057] (In formula (vi), M 6 is at least one element selected from Al and Ga. )

[0058] Si 6-z Al z O z N 8-z :Eu(vii)

[0059] (In formula (vii), z satisfies 0<z≤4.2.)

[0060] M 7 AlSiN3:Eu(viii)

[0061] (In formula (viii), M 7 is at least one element selected from Sr and Ca. )

[0062] The light-transmitting material may be at least one selected from resin, glass and inorganic substances. The resin is preferably at least one selected from epoxy resin, silicone resin, phenolic resin and polyimide resin. The inorganic substance may be at least one selected from aluminum oxide and aluminum nitride. In addition to the phosphor and the light-transmitting material, the wavelength conversion component may also contain fillers, colorants and light diffusion materials as needed. As fillers, for example, silicon oxide, barium titanate, titanium oxide, aluminum oxide, etc. may be listed.

[0063] Method for producing alkaline earth aluminate

[0064] In the method for producing an alkaline earth aluminate phosphor according to the third embodiment, the alkaline earth aluminate phosphor includes a first compound containing at least one element A selected from alkaline earth metals, a second compound containing Al, and a third compound containing Cr, and may also include a fourth compound and a fifth compound as required, wherein the fourth compound contains at least one element M selected from Group 13 elements other than Al. 1 The fifth compound comprises at least one element M selected from the group consisting of Mn, Eu, Ce, Tb, Pr, Nd, Sm, Yb, Ho, Er and Tm. 2, at least one compound selected from the first compound, the second compound, and the third compound is an oxide, the method comprising: preparing a raw material mixture, the raw material mixture comprising the first compound, the second compound, and the third compound, and optionally comprising the fourth compound as required and the fifth compound as required, so that the molar ratio of the element A relative to 1 mol of the composition is within a range of 1.0 to 4.0, and the molar ratio of the Al to the element M is within a range of 1.0 to 4.0. 1 The total molar ratio of is within the range of 4.0 to 14.0, the molar ratio of Cr is within the range of 0.004 to 0.8, and the element M 2 The molar ratio of Cr to the element M is within the range of 0 to 0.4. 2 The total molar ratio of Al and the element M is within the range of 0.004 to 0.8. 1 When the total molar ratio of the above elements M is set to 1, 1 The molar ratio of is 0.7 or less; and the step of heat treating the raw material mixture in a reducing atmosphere at a temperature in the range of 1000°C to 1500°C to obtain an alkaline earth aluminate phosphor.

[0065] Raw material mixture preparation process

[0066] raw material

[0067] The raw materials for manufacturing alkaline earth aluminate phosphors include a first compound containing element A, a second compound containing Al, and a third compound containing Cr. As the first compound, the second compound and the third compound, nitrides, hydrides, fluorides, oxides, carbonates, chlorides and their hydrates can be listed respectively. At least one compound selected from the first compound, the second compound and the third compound is an oxide, or two or more compounds can be oxides. The second compound and the third compound can be oxides. The first compound can specifically include Ca3N2, CaH2, CaF2, CaO, CaCO3, CaCl2, SrH2, Sr3N2, Sr2N, SrN, SrF2, SrO, SrCO3, SrCl2, Ba3N2, BaF2, BaO, BaCO3, BaCl2, etc. The second compound can specifically include AlN, AlF3, Al2O3, AlCl3, etc. The third compound can specifically include CrN, CrF3, Cr2O3, Cr2(CO3)3, CrCl3·6H2O. When the element A is at least one element selected from Ca, Sr and Ba, the first compound is preferably at least one compound selected from a compound containing Ca, a compound containing Sr and a compound containing Ba. When the element A is Sr, the first compound is preferably a compound containing Sr.

[0068] Contains element M 1 The fourth compound may include an element M 1 The fourth compound may be an oxide. The fourth compound is preferably a solid, and specific examples thereof include BN, B2O3, BCl3, GaN, GaBr3, Ga2O3, InBr3, In2O3, InCl3, Tl2O3, and TlF3. 1 When the fourth compound is at least one selected from B, Ga and In, it is preferred that the fourth compound is at least one compound selected from a compound containing B, a compound containing Ga and a compound containing In. 1 In the case of Ga, the fourth compound is preferably a compound containing Ga.

[0069] Contains element M 2 The fifth compound may include an element M 2 The fifth compound may be an oxide. The fifth compound is preferably a solid, and specific examples thereof include MnO2, Eu2O3, EuCl3·6H2O, CeCl3·7H2O, CeO2, TbCl3·6H2O, Tb4O7, PrCl3·7H2O, PrF3, Pr6O11 , NdCl3·6H2O, Nd2O3, SmCl3·6H2O, SmF3, Sm2O3, YbF3, Yb2O3, Ho2O3, ErCl3·6H2O, Er2O3, ErF3, TmCl3·6H2O, TmF3, Tm2O3.

[0070] Raw material mixture

[0071] The raw material compounds are weighed so that the molar ratio of each element in 1 mol becomes a specific value, and then the weighed raw material compounds are mixed by a mixer by a wet method or a dry method to obtain a raw material mixture. The mixer can be a vibration mill, a roller mill, a jet mill, etc. in addition to the ball mill commonly used in industry.

[0072] It is preferred to prepare a raw material mixture containing each compound in a measured amount so that each compound as a raw material has the following composition: the elements A, Al and Cr contained in each compound, and the element M optionally contained as required 1 and element M 2 It has a composition represented by the above formula (I). In element A, two or more elements A a and element A b In the case of a Compounds containing element A b and a raw material mixture of a compound and other compounds so that it has a composition represented by the above formula (I-1).

[0073] Flux

[0074] The raw material mixture may contain a flux. By making the raw material mixture contain a flux, the reaction between the raw materials can be further promoted, and the solid phase reaction can be carried out more uniformly, so that a phosphor with a large particle size and better luminescent properties can be obtained. The temperature of the heat treatment for obtaining the phosphor is a temperature of the same degree as the generation temperature of the liquid phase of the compound used as the flux, and the reaction between the raw materials is promoted by the flux. As a flux, a halide containing at least one element selected from rare earth metal elements, alkaline earth metal elements, and alkali metal elements can be used. As a flux, among the halides, fluorides can be used. In the case where the elements contained in the flux are the same as at least a part of the elements constituting the alkaline earth aluminate phosphor, as part of the raw materials of the alkaline earth aluminate phosphor having the target composition, the flux can be added in a manner that the composition of the alkaline earth aluminate phosphor becomes the target composition, or the flux can be added in a manner that is further added after the raw materials are mixed in a manner that becomes the target composition.

[0075] Process of obtaining alkaline earth aluminate phosphor by heat treatment

[0076] The raw material mixture can be placed in a crucible or boat made of carbon such as graphite, boron nitride (BN), alumina (Al2O3), tungsten (W), molybdenum (Mo), etc., and heat treated in a furnace.

[0077] Heat treatment atmosphere

[0078] The heat treatment is carried out in a reducing atmosphere. The reducing atmosphere may be a hydrogen-nitrogen atmosphere containing reducing hydrogen and nitrogen. The hydrogen-nitrogen atmosphere may contain preferably 70% by volume or more of nitrogen, or 80% by volume or more, or 90% by volume or more. In addition, the hydrogen-nitrogen atmosphere may contain 1% by volume or more of hydrogen, or 2% by volume or more, or 3% by volume or more, or less than 10% by volume of hydrogen.

[0079] Heat treatment temperature

[0080] The heat treatment temperature is in the range of 1000° C. to 1500° C., preferably in the range of 1100° C. to 1450° C., and more preferably in the range of 1200° C. to 1400° C. When the heat treatment temperature is 1000° C. to 1500° C., decomposition due to heat can be suppressed, and a phosphor having a target composition and a stable crystal structure can be obtained.

[0081] The heat treatment may be performed multiple times in two or more stages. For example, in the case of a two-stage heat treatment, the heat treatment may be performed at a temperature of 1000°C to 1500°C, and the second heat treatment may be performed at a temperature of 1200°C to 1400°C. When the first heat treatment temperature is 1000°C to 1500°C, it is easy to obtain a heat-treated product having a target composition. When the second heat treatment temperature is 1200°C to 1400°C, a phosphor having a stable crystal structure may be obtained.

[0082] In the heat treatment, the holding time can be set at a given temperature. For example, the holding time can be set at a temperature of about room temperature between 20°C or more and 28°C or less between the first heat treatment and the second heat treatment. The holding time can be, for example, more than 0.5 hours and less than 48 hours, or more than 1 hour and less than 40 hours, or more than 2 hours and less than 30 hours. By setting the holding time within 0.5 hours and less than 48 hours, crystal growth can be promoted.

[0083] The pressure of the heat treatment atmosphere can be standard atmospheric pressure (0.101MPa), or can be more than 0.101MPa, preferably in a pressurized atmosphere of more than 0.11MPa and less than 200MPa. The more the heat treatment temperature of the heat-treated object obtained by heat treatment becomes high temperature, the crystal structure is also easily decomposed, and by being set to pressurized atmosphere, the decomposition of the crystal structure can be suppressed, and the reduction of luminous intensity can be suppressed. The pressure of the heat treatment atmosphere is more preferably more than 0.11MPa and less than 100MPa in gauge pressure, more preferably more than 0.5MPa and less than 10MPa, and from the aspect of ease of manufacture, more preferably less than 1.0MPa.

[0084] The heat treatment time can be suitably selected according to the pressure of the atmosphere during the heat treatment temperature and the heat treatment, and is preferably more than 0.5 hour and within 20 hours. In the case of carrying out the heat treatment more than two stages, the heat treatment time is also preferably more than 0.5 hour and within 20 hours. When the heat treatment time is more than 0.5 hour and within 20 hours, the decomposition of the heat-treated object obtained can be suppressed, and the fluor with stable crystal structure and desired luminous intensity can be obtained. In addition, it is also possible to reduce production costs and make the manufacturing time shorter. The heat treatment time is more preferably more than 1 hour and within 10 hours, and more preferably more than 1.5 hours and within 9 hours.

[0085] The heat-treated product obtained by heat treatment can be subjected to post-treatment such as pulverization, dispersion, solid-liquid separation, and drying. Solid-liquid separation can be performed by methods commonly used in industry such as filtration, suction filtration, pressure filtration, centrifugal separation, and decantation. Drying can be performed by devices commonly used in industry such as a vacuum dryer, a hot air heating dryer, a conical dryer, and a rotary evaporator.

[0086] Example

[0087] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to these examples.

[0088] Example 1

[0089] As raw materials, SrCO3 was weighed to 8.86 g, Al2O3 to 10.71 g, and Cr2O3 to 0.14 g. 14 O 25 :Cr 0.12The raw materials were weighed in a manner. Using an agate mortar and an agate pestle, the raw materials were mixed for 10 minutes to obtain a raw material mixture. The obtained raw material mixture was heat-treated for 8 hours at 1300°C and standard pressure (0.101 MPa) in a hydrogen-nitrogen atmosphere containing hydrogen and nitrogen (hydrogen: 3 volume %, nitrogen: 97 volume %). After the heat treatment, the obtained heat-treated product was crushed to obtain the alkaline earth aluminate phosphor of Example 1.

[0090] Example 2

[0091] As raw materials, CaCO3 was weighed to 6.01 g, Al2O3 to 10.71 g, and Cr2O3 to 0.15 g. 14 O 25 :Cr 0.12 The alkaline earth aluminate phosphor of Example 2 was obtained in the same manner as in Example 1 except that the respective raw materials were used in the manner of .

[0092] Example 3

[0093] As raw materials, SrCO3 was measured to be 4.43 g, CaCO3 was measured to be 3.01 g, Al2O3 was measured to be 10.71 g, and Cr2O3 was measured to be 0.14 g. 0.5 Ca 0.5 )4Al 14 O 25 :Cr 0.12 The alkaline earth aluminate phosphor of Example 3 was obtained in the same manner as in Example 1, except that the raw materials were measured in a manner of and the heat treatment temperature was set to 1250°C.

[0094] Example 4

[0095] As raw materials, SrCO3 was weighed to 8.86 g, Al2O3 to 7.66 g, Ga2O3 to 5.64 g, and Cr2O3 to 0.14 g. 10 Ga4O 25 :Cr 0.12 The alkaline earth aluminate phosphor of Example 4 was obtained in the same manner as in Example 1 except that the raw materials were weighed in the manner of , and the heat treatment temperature was set to 1250°C. Table 1 shows the composition of the raw materials charged with Al and the element M. 1 When the total molar ratio of (Ga) is 1, the element M 1Table 1 also shows the molar ratio of Al and element M in Examples 1 to 3, Examples 5 and 6 described later, and Comparative Examples 1 and 2. 1 When the total molar ratio of (Ga) is 1, the element M 1 (Ga) molar ratio.

[0096] Example 5

[0097] As raw materials, SrCO3 was weighed to 8.86 g, Al2O3 to 5.36 g, Ga2O3 to 9.86 g, and Cr2O3 to 0.14 g. The raw materials were used in a charge composition of Sr4Al7Ga7O 25 :Cr 0.12 The alkaline earth aluminate phosphor of Example 5 was obtained in the same manner as in Example 1, except that the raw materials were measured in the manner of and the heat treatment temperature was set to 1200°C.

[0098] Example 6

[0099] As raw materials, SrCO3 was weighed to 8.86 g, Al2O3 to 4.60 g, Ga2O3 to 11.27 g, and Cr2O3 to 0.14 g. The raw materials were used in a charge composition of Sr4Al6Ga8O 25 :Cr 0.12 The alkaline earth aluminate phosphor of Example 6 was obtained in the same manner as in Example 1, except that the raw materials were measured in the manner of and the heat treatment temperature was set to 1200°C.

[0100] Comparative Example 1

[0101] A compound having a composition of an alkaline earth aluminate of Comparative Example 1 was obtained in the same manner as in Example 1 except that the heat treatment was performed in an air atmosphere (oxygen: about 20 volume % and nitrogen: about 78 volume %).

[0102] Comparative Example 2

[0103] As raw materials, SrCO3 was weighed to 8.86 g, Al2O3 to 3.07 g, Ga2O3 to 14.09 g, and Cr2O3 to 0.14 g. The raw materials were used in a charge composition of Sr4Al4Ga 10 O 25 :Cr 0.12 A compound having the composition of an alkaline earth aluminate of Comparative Example 2 was obtained in the same manner as in Example 1, except that the raw materials were weighed in the manner of and the heat treatment temperature was 1200°C.

[0104] Determination of luminescence spectrum

[0105] For each alkaline earth aluminate phosphor of the example and each compound having an alkaline earth aluminate composition of the comparative example, the emission spectrum was measured using a quantum efficiency measurement system (QE-2000, manufactured by Otsuka Electronics Co., Ltd.). The emission peak wavelength of the excitation light used in the quantum efficiency measurement system is 450nm. Based on each obtained emission spectrum, the emission peak wavelength (nm) and half-width (nm) in the emission peak within the range of 720nm to 900nm were calculated. The results are shown in Table 1. In addition, the emission intensity at the emission peak wavelength of Example 2 was set to 100%, and the relative emission intensity (%) at the emission peak wavelength of the alkaline earth aluminate phosphor of the example and each compound having an alkaline earth aluminate composition of the comparative example was measured. The results are shown in Table 1. Figure 1 The emission spectrum of the alkaline earth aluminate phosphor of Example 1 and the emission spectrum of the compound having the composition of the alkaline earth aluminate of Comparative Example 1 are shown in FIG. Figure 3 The emission spectra of the alkaline earth aluminate phosphors of Examples 4, 5 and 6 and the emission spectrum of the compound having the composition of the alkaline earth aluminate of Comparative Example 2 are shown in FIG.

[0106] Determination of excitation spectrum

[0107] The alkaline earth aluminate phosphor of Example 1 was measured for its excitation spectrum in the range of 350 nm to 700 nm at 25°C ± 5°C (room temperature) with an emission wavelength of 791 nm using a spectrofluorophotometer (F-4500, manufactured by Hitachi High-Technologies Corporation). Figure 2 The excitation spectrum of the alkaline earth aluminate phosphor of Example 1 is shown in FIG.

[0108] [Table 1]

[0109]

[0110]

[0111] The alkaline earth aluminate phosphors of Examples 1 to 6 have a luminescence peak wavelength in the range of 720 nm to 900 nm in the luminescence spectrum, and show a broad luminescence peak with a half-width of 80 nm or more. Based on this result, the alkaline earth aluminate phosphors of Examples 1 to 6 can emit light having a luminescence peak wavelength in the near-infrared wavelength range known as the "biological window", and can emit light that affects the photoreceptors of plants.

[0112] like Figure 1 and Figure 3As shown, each of the alkaline earth aluminate phosphors of Example 1 and Examples 4 to 6 has a light emission peak wavelength in the range of 720 nm to 900 nm, and has a wide half-value width of 80 nm or more.

[0113] like Figure 2 As shown in the figure, for the alkaline earth aluminate phosphor of Example 1, in the excitation spectrum of the wavelength range of 350 nm to 700 nm, the relative intensity of the wavelength range of 400 nm to 450 nm and the wavelength range of 550 nm to 580 nm becomes high. According to this result, by selecting the emission peak wavelength of the excitation light source, the alkaline earth aluminate phosphor can efficiently emit light having an emission peak wavelength in the range of 720 nm to 900 nm.

[0114] The compounds having the composition of alkaline earth aluminate of Comparative Examples 1 and 2 hardly emit light even when irradiated with light having a peak emission wavelength of 450 nm.

[0115] Industrial Applicability

[0116] The alkaline earth aluminate phosphor of the present application can be used in a light-emitting device used in a lighting device, a backlight of a liquid crystal display device, etc. In addition, the alkaline earth aluminate phosphor of one embodiment of the present invention can also be used in a light-emitting device for medical lighting for obtaining information in a living body, and a light-emitting device for plant cultivation that affects the photoreceptors of plants.

Claims

1. An alkaline earth aluminate phosphor comprising at least one element selected from alkaline earth metal elements A, Al and Cr, The alkaline earth aluminate phosphor optionally contains the element M 1 , The alkaline earth aluminate phosphor has a light emission peak wavelength in the range of 720 nm to 900 nm. The element A, the Al, the Cr, the element M 1 Satisfying the composition represented by the following formula (I), A4(Al 1-y M 1 y ) 14 The 25 :Cr v (I) In the formula (I), 0.004≤v≤0.8, 0≤y≤0.7, The element A is at least one element selected from Ca, Sr and Ba, and the element M 1 For Ga.

2. The alkaline earth aluminate phosphor according to claim 1, wherein The element A is Sr. 3 . The alkaline earth aluminate phosphor according to claim 1 , which has a light emission spectrum having a light emission peak wavelength in the range of 720 nm to 900 nm, and a half-value width of 80 nm or more. 4 . The alkaline earth aluminate phosphor according to claim 2 , which has a light emission spectrum having a light emission peak wavelength in the range of 720 nm to 900 nm inclusive and a half width of 90 nm to 150 nm inclusive. 5 . A light emitting device comprising: the alkaline earth aluminate phosphor according to claim 1 , and a light source for irradiating the alkaline earth aluminate phosphor.

6. A method for producing an alkaline earth aluminate phosphor, The method for producing the alkaline earth aluminate phosphor comprises: A step of preparing a raw material mixture, wherein the raw material mixture comprises: a first compound containing at least one element A selected from alkaline earth metals, a second compound containing Al, and a third compound containing Cr, and optionally comprising an element M 1 The fourth compound, at least one of the first compound, the second compound, and the third compound is an oxide, so that the element A, the Al, the Cr, the element M 1 It is a composition represented by the following formula (I), A4(Al 1-y M 1 y ) 14 The 25 :Cr v In the formula (I), 0.004≤v≤0.8, 0≤y≤0.7, The element A is at least one element selected from Ca, Sr and Ba, and the element M 1 is Ga; and A step of heat-treating the raw material mixture at a temperature in a range of 1000° C. to 1500° C. in a reducing atmosphere to obtain an alkaline earth aluminate phosphor.

7. The method for producing an alkaline earth aluminate phosphor according to claim 6, wherein: The element A is Sr.

8. The method for producing an alkaline earth aluminate phosphor according to claim 6 or 7, wherein: The fourth compound is an oxide.

9. The method for producing an alkaline earth aluminate phosphor according to claim 6 or 7, wherein: The temperature of the heat treatment is in the range of 1100° C. or higher and 1450° C. or lower.

10. The method for producing an alkaline earth aluminate phosphor according to claim 6 or 7, wherein: The reducing atmosphere contains nitrogen and hydrogen, and contains 1 volume % or more of hydrogen.

Citation Information

Patent Citations

  • remote phosphor light emitting device

    DE102014117440B3