A metal gate structure and a method for forming the same

By forming a polysilicon gate and sidewall structure in semiconductor manufacturing, and filling the gaps with metal silicide, the problem of height loss and gate oxide layer contamination caused by excessive metal gate area in high-voltage devices is solved, and the device yield is improved.

CN114121632BActive Publication Date: 2024-10-25SHANGHAI HUALI INTEGRATED CIRCUIT CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111376136.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-19
Publication Date
2024-10-25
Estimated Expiration
2041-11-19

AI Technical Summary

Technical Problem

In semiconductor manufacturing, the metal gate area of ​​high-voltage devices is too large, resulting in serious height loss and poor controllability of the CMP process. Moreover, the way of grooving the gate exposes the gate oxide layer, making it susceptible to contamination in subsequent processes.

Method used

A method of forming a metal gate structure is adopted, which includes forming a polysilicon gate and a gap on a substrate, covering the silicon oxide and silicon nitride layers, forming a sidewall structure through a photolithography etching process, depositing a metal silicide barrier layer, and filling the gap to protect the gate oxide layer from contamination.

Benefits of technology

It effectively solves the problems of metal gate height loss and gate oxide layer contamination, improves device yield, and makes mass production of high-voltage device products using the 28nm HKMG process possible.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114121632B_ABST
    Figure CN114121632B_ABST
Patent Text Reader

Abstract

The present invention provides a metal gate structure and a method for forming the same, providing a substrate, a gate oxide layer formed in the substrate, a polysilicon gate with a plurality of gaps formed on the gate oxide layer; depositing a silicon oxide layer; performing a first photolithography etching process so that the silicon oxide layer covering the gap surface and the side of the polysilicon gate is retained; depositing a silicon nitride layer; performing a second photolithography etching process so that the silicon nitride layer covering the gap surface and the side of the polysilicon gate is retained; forming a metal silicide barrier layer; performing a third photolithography etching process so that the metal silicide barrier layer covering the substrate surface is removed; forming metal silicide on the substrate; removing the metal silicide barrier layer covering the polysilicon gate by a wet etching process, and retaining the metal silicide barrier layer covering the gap. The present invention solves the problem that the gate oxide layer is easily contaminated by subsequent processes due to grooving on the gate in the high-voltage device process, and improves the device performance and yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of semiconductor manufacturing, and in particular to a metal gate structure and a method for forming the same. Background Art

[0002] With the development of semiconductor technology, advanced logic chip technology has reached a process node below 28nm. When preparing high-voltage (HV) devices, in order to solve the problem of poor controllability of the metal gate CMP process due to the large metal gate area, which in turn causes serious loss of metal gate height, MV devices usually need to slot on the gate.

[0003] However, this method of making grooves on the gate exposes the gate oxide layer below the gate, making the gate oxide layer very susceptible to contamination in subsequent processes. Therefore, how to use the method of making grooves on the gate while ensuring that the gate oxide layer is not damaged is a problem that needs to be solved urgently. Summary of the invention

[0004] In order to solve the above problems in the prior art, the present invention provides a metal gate structure and a method for forming the same, so as to solve the problem that the gate oxide layer is easily contaminated by subsequent processes due to the grooves formed on the gate.

[0005] The present invention provides a method for forming a metal gate structure, comprising the following steps:

[0006] Step 1, providing a substrate, wherein a gate oxide layer is formed in the substrate, and a polysilicon gate with a plurality of gaps is formed on the gate oxide layer;

[0007] Step 2: depositing a silicon oxide layer, wherein the silicon oxide layer covers the surfaces of the substrate, the polysilicon gate and the gap;

[0008] Step 3, performing a first photolithography and etching process, so that the silicon oxide layer covering the surface of the gap and the side of the polysilicon gate is retained, a first sidewall is formed on the side of the polysilicon gate, and a silicon oxide layer is formed on the surface of the gap;

[0009] Step 4: depositing a silicon nitride layer, wherein the silicon nitride layer covers the surfaces of the substrate, the polysilicon gate and the gap;

[0010] Step 5: performing a second photolithography and etching process, so that the silicon nitride layer covering the surface of the gap and the side of the polysilicon gate is retained, a second sidewall is formed on the side of the polysilicon gate, and a silicon nitride layer is formed on the surface of the gap; the first sidewall and the second sidewall together constitute the sidewall structure of the polysilicon gate;

[0011] Step 6: forming a metal silicide barrier layer covering the polysilicon gate, the gap and the substrate;

[0012] Step 7: performing a third photolithography and etching process to remove the metal silicide barrier layer covering the surface of the substrate;

[0013] Step eight, forming a metal silicide on the substrate;

[0014] Step nine: using a wet etching process to remove the metal silicide barrier layer covering the polysilicon gate, retaining the metal silicide barrier layer covering the gap, and forming a metal silicide barrier layer covering the gap.

[0015] Preferably, in step one, a gap is formed in the polysilicon gate by patterning the polysilicon gate.

[0016] Preferably, step three comprises the following steps:

[0017] Step a, forming a photoresist layer having the gap pattern;

[0018] Step b, using the photoresist layer as a mask, and etching away the silicon oxide layer not blocked by the photoresist by dry etching;

[0019] Step c: removing the photoresist layer.

[0020] Preferably, step five comprises the following steps:

[0021] Step d, forming a photoresist layer having the gap pattern;

[0022] Step e, using the photoresist layer as a mask, and etching away the silicon nitride layer not blocked by the photoresist by dry etching;

[0023] Step f, removing the photoresist layer.

[0024] Preferably, the metal silicide barrier layer in step six is ​​an oxide layer deposited by chemical vapor deposition.

[0025] Preferably, step seven comprises the following steps:

[0026] Step g, forming a photoresist layer having the polysilicon gate and the gap pattern on the metal silicide barrier layer;

[0027] Step h, using the photoresist layer as a mask, and etching the metal silicide barrier layer by a dry etching process;

[0028] Step i: removing the photoresist layer.

[0029] Preferably, step eight comprises the following steps:

[0030] Step j, depositing NiPt and TiN by physical vapor deposition sputtering process;

[0031] Step k, performing a first annealing process to generate high-resistance metal silicide Ni2PtSi;

[0032] Step 1, removing TiN and NiPt that does not react with silicon by wet etching;

[0033] Step m: performing a second annealing treatment to convert the high-resistance Ni2PtSi into low-resistance NiPtSi2.

[0034] Preferably, the gap in step nine is composed of a silicon oxide layer, a silicon nitride layer and a metal silicide barrier layer;

[0035] Furthermore, the gap is integrated with the side wall structure and no gap exists.

[0036] Preferably, the method further comprises removing the polysilicon gate and depositing a metal gate.

[0037] The present invention also provides a metal gate structure, comprising:

[0038] substrate;

[0039] a gate oxide layer formed in the substrate;

[0040] a metal gate formed on the gate oxide layer;

[0041] a plurality of gaps formed in the metal gate and located above the gate oxide layer;

[0042] A sidewall structure formed on a side of the metal gate; and

[0043] a metal silicide formed on the substrate;

[0044] The gap is composed of a silicon oxide layer, a silicon nitride layer located above the silicon oxide layer, and a metal silicide barrier layer located above the silicon nitride layer; the gap is integrated with the sidewall structure without any gap.

[0045] The present invention effectively solves the problem of uneven metal grinding caused by excessive metal gate area in high-voltage devices, while avoiding the side effect of gate oxide contamination caused by gate oxide exposure, thereby improving device yield and making mass production of high-voltage device products using the 28nm HKMG process possible. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] The above and other objects, features and advantages of the present invention will become more apparent through the following description of the embodiments of the present invention with reference to the accompanying drawings, in which:

[0047] Figure 1 Shown is a schematic diagram of a large-size metal gate after CMP;

[0048] Figure 2 A schematic diagram showing a groove cut in the gate is shown;

[0049] Figure 3 Schematic diagram showing gate oxide being damaged in an exposed state;

[0050] Figure 4 Schematic diagram of an electron lens showing damage to the gate oxide in an exposed state;

[0051] Figure 5 Schematic diagram of an electron lens showing an undamaged gate oxide layer;

[0052] Figure 6 A flowchart showing a method for forming a metal gate structure according to an embodiment of the present invention;

[0053] Figure 7-Figure 15 Shown are structural schematic diagrams of various steps in a method for forming a metal gate structure according to an embodiment of the present invention;

[0054] Fig.16 Shown is a schematic diagram of a metal gate structure according to an embodiment of the present invention. DETAILED DESCRIPTION

[0055] The present invention is described below based on embodiments, but the present invention is not limited to these embodiments. In the detailed description of the present invention below, some specific details are described in detail. It is possible for a person skilled in the art to fully understand the present invention without the description of these details. In order to avoid confusing the essence of the present invention, known methods, processes, flows, components and circuits are not described in detail.

[0056] In addition, persons of ordinary skill in the art will appreciate that the drawings provided herein are for illustration purposes and are not necessarily drawn to scale.

[0057] Unless the context clearly requires otherwise, the words "include", "comprising" and similar words throughout the application should be interpreted as including rather than exclusive or exhaustive; that is, the meaning is "including but not limited to".

[0058] In the description of the present invention, it should be understood that the terms "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance. In addition, in the description of the present invention, unless otherwise specified, "plurality" means two or more.

[0059] As the size of transistors continues to shrink, HKMG (high-k insulation layer + metal gate) gradually replaces the original silicon dioxide insulation layer + polysilicon gate configuration and becomes an indispensable part of the process below 28nm. The metal gate process usually uses PVD or CVD to deposit metal, and then uses chemical mechanical polishing (CMP) to grind away excess metal and retain the required metal gate part. The chemical mechanical polishing process will produce different grinding effects for metal gates of different sizes. Metal gates that are too large will be polished too much, such as Figure 1 As shown, the bowl-shaped thickness will be low (Dishing), and the metal gate height loss will be serious. Therefore, in the HKMG process, there will be certain restrictions on the metal gate size to avoid an excessively large metal gate area.

[0060] In the high-voltage device manufacturing process, due to the special requirements of high voltage, the metal gate will inevitably have a problem of being too large, and the size cannot be limited by design rules. In order to solve the problem of serious loss of metal gate height and poor controllability of metal gate CMP process due to the large area of ​​metal gate of high-voltage devices, such as Figure 2 As shown, a gap (Slot) 21 is usually inserted on the gate, and an insulating layer is subsequently filled in the gap to serve as a support for metal gate polishing, thereby improving the controllability of the metal gate CMP process. This approach can effectively reduce the height loss of the metal gate, but it also has disadvantages, such as Figure 3 Middle coil 31 and Figure 4 As shown in the middle coil 41, inserting a slot on the gate will expose the gate oxide layer under the gate. The gate oxide layer will be affected by the subsequent IMP / WET / NiSi process in an exposed state, and will have obvious deformation and contamination marks, resulting in device malfunction. Figure 5 The middle coil 51 is an uncontaminated gate oxide layer, and the purpose of the present invention is to achieve this effect.

[0061] In summary, in order to simultaneously solve the problem of serious metal gate height loss caused by excessive metal gate area in high-voltage devices and the problem that the gate oxide layer is easily contaminated by subsequent processes due to grooving on the gate, the present invention proposes a metal gate structure and a method for forming the same. The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods.

[0062] Figure 6 The flowchart of the method for forming a metal gate structure according to an embodiment of the present invention is shown. Figure 6 As shown, the following steps are included:

[0063] Step 1: Figure 7 As shown, a substrate 101 is provided, a gate oxide layer 102 is formed in the substrate 101 , and a polysilicon gate 104 with a plurality of gaps 103 is formed on the gate oxide layer 102 .

[0064] In an embodiment of the present invention, the substrate 101 is a silicon substrate, and a shallow trench isolation structure (not shown in the figure) is also formed in the substrate 101. The shallow trench isolation structure is used to isolate different transistors and prevent electrical connection between different transistors. The material of the shallow trench isolation structure can be one or more of silicon oxide, silicon nitride, and silicon oxynitride.

[0065] In the embodiment of the present invention, a gap 103 is formed in the polysilicon gate by patterning the polysilicon gate. The number of the gaps 103 can be one or more according to actual needs. Figure 7 As shown, there are two.

[0066] Step 2: Figure 8 As shown, a silicon oxide layer 105 is deposited, and the silicon oxide layer 105 covers the surfaces of the substrate 101 , the polysilicon gate 104 and the gap 103 .

[0067] Step 3: Figure 8 and Fig. 9 As shown, a first photolithography and etching process is performed, so that the silicon oxide layer 105 covering the surface of the gap 103 and the side of the polysilicon gate 104 is retained.

[0068] Specifically, step three includes the following steps:

[0069] Step a, forming a photoresist layer having the gap pattern;

[0070] Among them, the photoresist layer is Figure 8 As shown in 106.

[0071] Step b, using the photoresist layer as a mask, and etching away the silicon oxide layer not blocked by the photoresist by dry etching;

[0072] Step c: removing the photoresist layer.

[0073] After etching, a first spacer 107 is formed on the side of the polysilicon gate 104 , and a silicon oxide layer 108 is formed on the surface of the gap 103 .

[0074] Step 4: Fig.10 As shown, a silicon nitride layer 109 is deposited, and the silicon nitride layer 109 covers the surfaces of the substrate 101 , the polysilicon gate 10 and the gap 106 .

[0075] Step 5: Fig.10 and Fig.11As shown, a second photolithography and etching process is performed, so that the silicon nitride layer 109 covering the surface of the gap 103 and the side of the polysilicon gate 104 is retained, a second sidewall 111 is formed on the side of the polysilicon gate 104, and a silicon nitride layer 112 is formed on the surface of the gap 103; the first sidewall 107 and the second sidewall 111 together constitute the sidewall structure of the polysilicon gate 104.

[0076] Specifically, step five includes the following steps:

[0077] Step d, forming a photoresist layer having the gap pattern;

[0078] Among them, the photoresist layer is Fig.10 As shown in 110.

[0079] Step e, using the photoresist layer as a mask, and etching away the silicon nitride layer not blocked by the photoresist by dry etching;

[0080] Step f, removing the photoresist layer.

[0081] After etching, a second spacer 111 is formed on the side of the polysilicon gate 104 , and a silicon nitride layer 112 is formed on the surface of the gap 103 .

[0082] In the embodiment of the present invention, the first sidewall 107 and the second sidewall 111 together form the sidewall structure of the polysilicon gate 104. Of course, in other embodiments, the sidewall structure may also be a multi-layer (greater than or equal to two layers) stacked structure, such as a nitride layer / oxide layer / nitride layer structure.

[0083] Step 6: Fig.12 As shown, a metal silicide barrier layer 113 is formed to cover the polysilicon gate 104 , the spacer structure and the gap 103 .

[0084] In the embodiment of the present invention, the metal silicide blocking layer 113 (Silicide Area Block, SAB) is an oxide layer deposited by chemical vapor deposition, preferably a SiO2 film, the purpose of which is to form SiO2 to cover the surface of the polysilicon gate, sidewall structure and gap where metal silicide (Salicide) does not need to be formed, to prevent them from forming metal silicide.

[0085] Between step 5 and step 6, a step of implanting impurity ions into the substrate 101 using the polysilicon gate 104 and the sidewall structure as a mask to form source and drain electrodes 113 may be included. In this step, the source and drain electrodes are formed by ion implantation, and the implanted impurity ions may be P-type impurity ions or N-type impurity ions.

[0086] Step 7: Fig.13As shown, a third photolithography and etching process is performed to remove the metal silicide barrier layer 113 covering the surface of the substrate 101 .

[0087] Specifically, step seven includes the following steps:

[0088] Step g, forming a photoresist layer having a polysilicon gate and a gap pattern on the metal silicide barrier layer;

[0089] Step h, using the photoresist layer as a mask, and etching the metal silicide barrier layer by a dry etching process;

[0090] Step i: removing the photoresist layer.

[0091] In step seven, the metal silicide barrier layer 113 covering the surface of the substrate 101 is removed to expose the substrate surface where the metal silicide is to be formed, in preparation for the next step of forming the metal silicide.

[0092] Step 8: Fig.14 As shown, metal silicide is formed on the substrate 101 .

[0093] Specifically, step eight includes the following steps:

[0094] Step g, depositing NiPt and TiN by physical vapor deposition sputtering process;

[0095] NiPt and thick TiN are deposited by PVD sputtering process. The function of TiN is to prevent NiPt from flowing during the RTA stage, which results in uneven thickness of metal silicide and local uneven resistance value.

[0096] Step h, performing a first annealing treatment to generate high-resistance metal silicide Ni2PtSi;

[0097] In a high temperature environment of about 200-300°C, N2 is introduced to cause NiPt to react with the active area and polysilicon to generate high-resistance metal silicide Ni2PtSi.

[0098] Step i, removing TiN and NiPt that does not react with silicon by wet etching;

[0099] In the embodiment of the present invention, wet etching is used to remove TiN and NiPt that does not react with silicon to prevent them from bridging and causing a circuit short circuit.

[0100] Step j: Perform a second annealing treatment to convert the high-resistance Ni2PtSi into low-resistance NiPtSi2.

[0101] In a high temperature environment of about 400-450℃, N2 is introduced to convert the high-resistance Ni2PtSi into the low-resistance NiPtSi2.

[0102] Step 9: Fig.15 As shown, the metal silicide barrier layer 113 covering the surface of the polysilicon gate 104 is removed by a wet etching process, and the metal silicide barrier layer covering the gap 103 is retained to form a metal silicide barrier layer 115 covering the gap 103 .

[0103] like Fig.15 As shown, a metal silicide barrier layer 115 is formed in the gap 103. In the embodiment of the present invention, the gap 103 is filled with the silicon oxide layer 108, the silicon nitride layer 112 and the metal silicide barrier layer 115, and is integrated with the sidewall structure without any gap.

[0104] The present invention utilizes the sidewall structure forming process to deposit a silicon oxide layer 108 and a silicon nitride layer 112, which are the same as the sidewall structure material, on the exposed gate oxide layer 102, and utilizes the metal silicide forming process to deposit a metal silicide barrier layer 115 on the exposed gate oxide layer, thereby filling the gap above the gate oxide layer exposed due to the grooves in the polysilicon gate, avoiding the gate oxide from being contaminated by subsequent processes, and solving the problem that the gate oxide layer is easily contaminated by subsequent processes due to the grooves on the gate.

[0105] Fig.16 It is a schematic diagram of a metal gate structure according to an embodiment of the present invention. Fig.16 As shown, it includes a substrate 101, a gate oxide layer 102 formed in the substrate, a metal gate 116 formed on the gate oxide layer with a gap 103, a sidewall structure formed on both sides of the metal gate 116, and a metal silicide 114 formed on the substrate 101. Among them, the gap 103 is filled with a silicon oxide layer 108, a silicon nitride layer 112 and a metal silicide barrier layer 115, and is integrated with the sidewall structure without any gap. In addition, the metal gate structure of the embodiment of the present invention also includes a shallow trench isolation structure 117 formed in the substrate 101.

[0106] The present invention not only effectively solves the problem of serious metal gate height loss caused by excessive metal gate area in high-voltage devices, but also solves the problem that the gate oxide layer is easily contaminated by subsequent processes due to grooving, thereby improving the yield of the prepared high-voltage devices.

[0107] It should be understood that many other layers may also be present, such as spacer elements and / or other suitable components, which are omitted from the illustration for simplicity.

[0108] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for forming a metal gate structure, characterized in that: The following steps are involved: Step 1, providing a substrate, wherein a gate oxide layer is formed in the substrate, and a polysilicon gate with a plurality of gaps is formed on the gate oxide layer; Step 2: depositing a silicon oxide layer, wherein the silicon oxide layer covers the surfaces of the substrate, the polysilicon gate and the gap; Step 3, performing a first photolithography and etching process, so that the silicon oxide layer covering the surface of the gap and the side of the polysilicon gate is retained, a first sidewall is formed on the side of the polysilicon gate, and a silicon oxide layer is formed on the surface of the gap; Step 4: depositing a silicon nitride layer, wherein the silicon nitride layer covers the surfaces of the substrate, the polysilicon gate and the gap; Step 5: performing a second photolithography and etching process, so that the silicon nitride layer covering the surface of the gap and the side of the polysilicon gate is retained, a second sidewall is formed on the side of the polysilicon gate, and a silicon nitride layer is formed on the surface of the gap; the first sidewall and the second sidewall together constitute the sidewall structure of the polysilicon gate; Step 6: forming a metal silicide barrier layer covering the polysilicon gate, the gap and the substrate; Step 7: performing a third photolithography and etching process to remove the metal silicide barrier layer covering the surface of the substrate; Step eight, forming a metal silicide on the substrate; Step nine: using a wet etching process to remove the metal silicide barrier layer covering the polysilicon gate, retaining the metal silicide barrier layer covering the gap, and forming a metal silicide barrier layer covering the gap.

2. The method for forming a metal gate structure according to claim 1, wherein: In step 1, a gap is formed in the polysilicon gate by patterning the polysilicon gate.

3. The method for forming a metal gate structure according to claim 1, wherein: Step three includes the following steps: Step a, forming a photoresist layer having the gap pattern; Step b, using the photoresist layer as a mask, and etching away the silicon oxide layer not blocked by the photoresist by dry etching; Step c: removing the photoresist layer.

4. The method for forming a metal gate structure according to claim 1, wherein: Step five includes the following steps: Step d, forming a photoresist layer having the gap pattern; Step e, using the photoresist layer as a mask, and etching away the silicon nitride layer not blocked by the photoresist by dry etching; Step f, removing the photoresist layer.

5. The method for forming a metal gate structure according to claim 1, wherein: The metal silicide barrier layer in step six is ​​an oxide layer deposited by chemical vapor deposition.

6. The method for forming a metal gate structure according to claim 1, characterized in that: Step seven includes the following steps: Step g, forming a photoresist layer having the polysilicon gate and the gap pattern on the metal silicide barrier layer; Step h, using the photoresist layer as a mask, and etching the metal silicide barrier layer by a dry etching process; Step i: removing the photoresist layer.

7. The method for forming a metal gate structure according to claim 1, wherein: Step eight includes the following steps: Step j, depositing NiPt and TiN by physical vapor deposition sputtering process; Step k, performing a first annealing process to generate high-resistance metal silicide Ni2PtSi; Step 1, removing TiN and NiPt that does not react with silicon by wet etching; Step m: performing a second annealing treatment to convert the high-resistance Ni2PtSi into low-resistance NiPtSi2.

8. The method for forming a metal gate structure according to claim 1, wherein: The gap in step nine is composed of a silicon oxide layer, a silicon nitride layer and a metal silicide barrier layer.

9. The method for forming a metal gate structure according to claim 8, characterized in that: The gap is integrated with the side wall structure and no gap exists.

10. The method for forming a metal gate structure according to claim 1, wherein: The method further includes removing the polysilicon gate and depositing a metal gate.

11. A metal gate structure formed by the method for forming a metal gate structure according to any one of claims 1 to 10, characterized in that: include: substrate; a gate oxide layer formed in the substrate; a metal gate formed on the gate oxide layer; a plurality of gaps formed in the metal gate and located above the gate oxide layer; A sidewall structure formed on the side of the metal grid; as well as a metal silicide formed on the substrate; The gap is composed of a silicon oxide layer, a silicon nitride layer located above the silicon oxide layer, and a metal silicide barrier layer located above the silicon nitride layer; the gap is integrated with the sidewall structure without any gap.