Ultra-fast flash memory floating gate TiN film manufacturing method
By using hafnium dioxide to wrap the TiN film and leverage its thermal stability, the problem of TiN film being easily agglomerated in ultra-flash memory is solved, the continuity and uniformity of the floating gate TiN film is improved, and the device performance is improved.
Patent Information
- Application Number
- CN202111399283.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-24
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-11-24
AI Technical Summary
During the production process of floating gate TiN film of ultra-flash memory, the TiN film is prone to agglomeration due to heat treatment, which affects its continuity and uniformity, and thus affects product performance.
Using hafnium dioxide as the oxide layer, TiN film is wrapped through deposition, etching and other steps, and its thermal stability is used to improve sidewall continuity, and it is also used to open wafer conveying boxes and processes such as low-temperature atomic layers with different pollution risk levels. Measures such as deposition and dry etching control the process and form a stable side wall of the oxide layer.
Improves the continuity and uniformity of the ultra-flash memory floating gate TiN film, thereby improving device performance.
Smart Images

Figure CN114121633B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of integrated circuit manufacturing, and in particular to a method for manufacturing an ultra-fast flash memory floating gate TiN film. Background Art
[0002] Compared with the third generation Nor flash in the industry, 38SF (ultra-fast flash memory at 38nm technology node) has higher erase efficiency, higher erase and write durability, higher write efficiency, faster write speed, lower erase and write voltage, lower power consumption, no read and write interference, the storage unit size is only half of SF1.0, the process is simple, the test time is short, and the cost is greatly reduced. High speed, low power consumption and low voltage are the highlights of 38SF technology. The new ultra-fast flash memory 2.0 is a new generation of Nor flash that uses horizontal electric field write operation and cutting-edge TiN voltage-free coupling erase operation, which can greatly improve erase efficiency and reduce operating voltage. The growth and etching of each subsidiary layer in the ALD TiN floating gate process has extremely high requirements for uniformity and stability. In the process, multiple heat treatments are used to make TiN easily agglomerated, resulting in discontinuous TiN film, which seriously affects product performance. Summary of the invention
[0003] A series of simplified concepts are introduced in the Summary of the Invention, which are all simplifications of the prior art in the field, and will be further described in detail in the Detailed Description of the Invention. The Summary of the Invention of the present invention does not mean to attempt to define the key features and essential technical features of the claimed technical solution, nor does it mean to attempt to determine the scope of protection of the claimed technical solution.
[0004] The technical problem to be solved by the present invention is to provide a method for manufacturing a TiN film for a floating gate of an ultra-fast flash memory, which can improve the continuity of the TiN film on the side wall of the ultra-fast flash memory and enhance the device performance and uniformity.
[0005] In order to solve the above technical problems, the present invention provides a method for manufacturing a floating gate TiN film of an ultra-fast flash memory, comprising the following steps:
[0006] S1, completing the previous process according to the prior art until the trench etching is completed;
[0007] S2, TiN deposition;
[0008] S3, depositing an oxide layer to encapsulate TiN;
[0009] S4, wafer back cleaning;
[0010] S5, photolithography defines the protection area and the non-protection area, and forms a protection layer to protect the protection area and expose the non-protection area;
[0011] S6, etching to remove the oxide layer in the non-protected area, exposing the TiN in the non-protected area;
[0012] S7, removing the protective layer of the protected area;
[0013] S8, etching to remove TiN in non-protected areas;
[0014] S9, depositing an oxide layer to encapsulate the TiN in the protection zone;
[0015] S10, etching and removing the oxide layer at the top of the protection zone and the bottom of the trench to form an oxide layer sidewall;
[0016] S11, etching and removing the TiN on the top of the protection zone and the bottom of the trench and the sidewall of the oxide layer, and retaining the TiN on the sidewall of the trench.
[0017] Optionally, the method for manufacturing the ultra-fast flash memory floating gate TiN film is further improved, and when implementing step S2, it is switched to a front-opening wafer transfer box with a high contamination risk level; when implementing step S4, it is switched to a front-opening wafer transfer box with a low contamination risk level; when implementing step S6, it is switched to a front-opening wafer transfer box with a high contamination risk level.
[0018] Optionally, the ultra-fast flash memory floating gate TiN film manufacturing method is further improved, and the oxide layer is hafnium dioxide.
[0019] Optionally, the method for manufacturing the ultra-fast flash memory floating gate TiN film is further improved, and the oxide layer is formed by a low-temperature atomic layer deposition process.
[0020] Optionally, the ultra-fast flash memory floating gate TiN film manufacturing method is further improved, wherein the protection area is an active area, and the non-protection area is an isolation area.
[0021] Optionally, the ultra-fast flash memory floating gate TiN film manufacturing method is further improved, and the protective layer is a photoresist.
[0022] Optionally, the method for manufacturing the ultra-fast flash memory floating gate TiN thin film is further improved by performing step S6 to remove the oxide layer by dry isotropic etching.
[0023] Optionally, the method for manufacturing the ultra-fast flash memory floating gate TiN film is further improved, and step S8 is performed to remove the TiN in the non-protected area by using dry and wet etching.
[0024] Optionally, the method for manufacturing the ultra-fast flash memory floating gate TiN thin film is further improved, and step S10 is implemented to remove the oxide layer at the top of the active area and the bottom of the trench by dry anisotropic etching.
[0025] Optionally, the method for manufacturing the ultra-fast flash memory floating gate TiN film is further improved by performing step S11 to remove the TiN at the top of the protection zone and the bottom of the trench as well as the sidewall of the oxide layer by dry and wet etching.
[0026] Hafnium dioxide is a ceramic material with a wide bandgap and high dielectric constant. It is also one of the few binary oxides that can maintain thermodynamic stability with silicon, so it can be naturally integrated into logic elements and memory devices. After the present invention completes the pre-sequence process and completes the groove according to the prior art, it is transferred to HK FOUP (to avoid metal contamination). Hafnium dioxide is deposited to wrap TiN to avoid exposure of TiN on the wafer surface to generate contamination, and then the wafer back is cleaned and transferred to HL FOUP to avoid residual contamination. The photolithography defines the protection area and the non-protection area, forms a protection layer to protect the protection area, and exposes the non-protection area; transfers to HK FOUP to avoid metal contamination, etches away the hafnium dioxide in the non-protection area, and exposes the TiN in the non-protection area; removes the protection layer in the protection area; etches away the TiN in the non-protection area; deposits hafnium dioxide to wrap the TiN in the protection area to avoid exposure of TiN on the wafer surface to produce contamination; etches away the hafnium dioxide at the top of the protection area and the bottom of the groove to form the hafnium dioxide side wall; etches away the TiN at the top of the protection area and the bottom of the groove and the hafnium dioxide side wall, and retains the TiN on the groove side wall. The present invention utilizes the thermal stability of hafnium dioxide to improve the continuity of the TiN film on the side wall of the ultra-fast flash memory, and can improve the device performance and uniformity. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The drawings of the present invention are intended to illustrate the general characteristics of the methods, structures and / or materials used in specific exemplary embodiments of the present invention, and to supplement the description in the specification. However, the drawings of the present invention are schematic diagrams not drawn to scale, and thus may not accurately reflect the precise structure or performance characteristics of any given embodiment, and the drawings of the present invention should not be interpreted as limiting or restricting the range of values or properties covered by the exemplary embodiments of the present invention. The present invention is further described in detail below in conjunction with the drawings and specific embodiments:
[0028] Figure 1 It is a schematic diagram comparing the processes of the prior art and the present invention. DETAILED DESCRIPTION
[0029] The following describes the implementation methods of the present invention through specific specific embodiments, and those skilled in the art can fully understand other advantages and technical effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through different specific implementation methods, and the details in this specification can also be applied based on different viewpoints, and various modifications or changes can be made without deviating from the overall design concept of the invention. It should be noted that the following embodiments and the features in the embodiments can be combined with each other in the absence of conflict. The following exemplary embodiments of the present invention can be implemented in a variety of different forms and should not be interpreted as being limited to the specific embodiments described herein. It should be understood that these embodiments are provided to make the disclosure of the present invention thorough and complete, and to fully convey the technical solutions of these exemplary specific embodiments to those skilled in the art.
[0030] First embodiment;
[0031] The present invention provides a method for manufacturing an ultra-fast flash memory floating gate TiN film, comprising the following steps:
[0032] S1, completing the previous process according to the prior art until the trench etching is completed;
[0033] S2, TiN deposition;
[0034] S3, depositing an oxide layer to encapsulate TiN;
[0035] S4, wafer back cleaning;
[0036] S5, photolithography defines the protection area and the non-protection area, and forms a protection layer to protect the protection area and expose the non-protection area;
[0037] S6, etching to remove the oxide layer in the non-protected area, exposing the TiN in the non-protected area;
[0038] S7, removing the protective layer of the protected area;
[0039] S8, etching to remove TiN in non-protected areas;
[0040] S9, depositing an oxide layer to encapsulate the TiN in the protection zone;
[0041] S10, etching and removing the oxide layer at the top of the protection zone and the bottom of the trench to form an oxide layer sidewall;
[0042] S11, etching and removing the TiN on the top of the protection zone and the bottom of the trench and the sidewall of the oxide layer, and retaining the TiN on the sidewall of the trench.
[0043] Second embodiment;
[0044] The present invention provides a method for manufacturing an ultra-fast flash memory floating gate TiN film, comprising the following steps:
[0045] S1, completing the previous process according to the prior art until the trench etching is completed;
[0046] S2, transfer to HK FOUP and deposit TiN;
[0047] S3, using low-temperature atomic layer deposition process to deposit hafnium dioxide and encapsulate TiN;
[0048] S4, wafer back cleaning and transfer to HL FOUP;
[0049] S5, photolithography defines the active area and the isolation area, and the photoresist shields and protects the active area, exposing the isolation area;
[0050] S6, transfer to HK FOUP, etch and remove the hafnium dioxide in the isolation area to expose the TiN in the isolation area;
[0051] S7, removing the photoresist in the active area;
[0052] S8, etching and removing TiN in the isolation area;
[0053] S9, using low temperature atomic layer deposition process to deposit hafnium dioxide to encapsulate the TiN in the active area;
[0054] S10, etching and removing the hafnium dioxide on the top of the active area and the bottom of the trench to form a hafnium dioxide sidewall;
[0055] S11, etching and removing TiN at the top of the protection zone and the bottom of the trench and the sidewall of hafnium dioxide, and retaining TiN on the sidewall of the trench;
[0056] HK FOUP is a front-opening wafer transfer box with a high contamination risk level, and HL FOUP is a front-opening wafer transfer box with a low contamination risk level.
[0057] In all the accompanying drawings, the same reference numerals represent the same elements all the time. In addition, it should also be understood that, although the terms "first", "second" etc. can be used here to describe different elements, parameters, components, regions, layers and / or parts, these elements, parameters, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish an element, parameter, component, region, layer or part from another element, parameter, component, region, layer or part. Therefore, without departing from the teaching according to exemplary embodiments of the present invention, the first element, parameter, component, region, layer or part discussed below may also be referred to as the second element, parameter, component, region, layer or part.
[0058] Third embodiment;
[0059] The present invention provides a method for manufacturing an ultra-fast flash memory floating gate TiN film, comprising the following steps:
[0060] S1, completing the previous process according to the prior art until the trench etching is completed;
[0061] S2, transfer to HK FOUP and deposit TiN;
[0062] S3, using low-temperature atomic layer deposition process to deposit hafnium dioxide and encapsulate TiN;
[0063] S4, wafer back cleaning and transfer to HL FOUP;
[0064] S5, photolithography defines the active area and the isolation area, and the photoresist shields and protects the active area, exposing the isolation area;
[0065] S6, transfer to HK FOUP, use dry isotropic etching to remove the hafnium dioxide in the isolation area, exposing the TiN in the isolation area;
[0066] S7, removing the photoresist in the active area;
[0067] S8, etching and removing TiN in the isolation area;
[0068] S9, using low temperature atomic layer deposition process to deposit hafnium dioxide to encapsulate the TiN in the active area;
[0069] S10, removing the hafnium dioxide on the top of the active area and the bottom of the trench by dry anisotropic etching to form a hafnium dioxide sidewall;
[0070] S11, using dry and wet etching to remove TiN at the top of the protection zone and the bottom of the trench and the sidewall of hafnium dioxide, and retaining TiN on the sidewall of the trench;
[0071] HK FOUP is a front-opening wafer transfer box with a high contamination risk level, and HL FOUP is a front-opening wafer transfer box with a low contamination risk level.
[0072] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. It will also be understood that, unless expressly defined herein, terms such as those defined in general dictionaries should be interpreted as having a meaning consistent with their meaning in the context of the relevant art, and not interpreted in an ideal or overly formal sense.
[0073] The present invention has been described in detail above through specific implementation modes and embodiments, but these do not constitute limitations of the present invention. Without departing from the principles of the present invention, those skilled in the art may also make many variations and improvements, which should also be regarded as the protection scope of the present invention.
Claims
1. A method for manufacturing a floating gate TiN thin film for an ultra-fast flash memory, characterized in that: The following steps are involved: S1, completing the previous process according to the prior art until the trench etching is completed; S2, TiN deposition; S3, depositing an oxide layer to encapsulate TiN; S4, wafer back cleaning; S5, photolithography defines the protection area and the non-protection area, and forms a protection layer to protect the protection area and expose the non-protection area; S6, etching to remove the oxide layer in the non-protected area, exposing the TiN in the non-protected area; S7, removing the protective layer of the protected area; S8, etching to remove TiN in non-protected areas; S9, depositing an oxide layer to encapsulate the TiN in the protection zone; S10, etching and removing the oxide layer at the top of the protection zone and the bottom of the trench to form an oxide layer sidewall; S11, etching and removing the TiN on the top of the protection zone and the bottom of the trench and the side wall of the oxide layer, and retaining the TiN on the side wall of the trench; Among them, when implementing step S2, it is transferred to a front-opening wafer transfer box with a high contamination risk level, when implementing step S4, it is transferred to a front-opening wafer transfer box with a low contamination risk level, and when implementing step S6, it is transferred to a front-opening wafer transfer box with a high contamination risk level; the oxide layer is hafnium dioxide.
2. The method for manufacturing a floating gate TiN thin film for an ultra-fast flash memory according to claim 1, wherein: The oxide layer is formed by a low-temperature atomic layer deposition process.
3. The method for manufacturing a floating gate TiN thin film for an ultra-fast flash memory as claimed in claim 1, characterized in that: The protection area is an active area, and the non-protection area is an isolation area.
4. The method for manufacturing a floating gate TiN thin film for an ultra-fast flash memory as claimed in claim 1, characterized in that: The protective layer is photoresist.
5. The method for manufacturing a floating gate TiN thin film for an ultra-fast flash memory as claimed in claim 1, characterized in that: In step S6, dry isotropic etching is used to remove the oxide layer.
6. The method for manufacturing a floating gate TiN thin film for an ultra-fast flash memory as claimed in claim 1, characterized in that: In step S8, dry and wet etching are used to remove TiN in the non-protected area.
7. The method for manufacturing a floating gate TiN thin film for an ultra-fast flash memory as claimed in claim 1, characterized in that: Step S10 is implemented to remove the oxide layer on the top of the active area and the bottom of the trench by dry anisotropic etching.
8. The method for manufacturing a floating gate TiN thin film for an ultra-fast flash memory as claimed in claim 1, characterized in that: Step S11 is implemented to remove the TiN on the top of the protection area and the bottom of the trench as well as the sidewall of the oxide layer by dry and wet etching.
Citation Information
Cited By
Efficient and uniform TiN film layer cleaning process and device
CN121295197A