Binder, slurry for solid-state battery, electrode for solid-state battery and solid-state secondary battery

By using specific fluoroelastomers as binders, the problem of insufficient solubility of binders in low-polarity solvents in sulfide-based solid-state batteries is solved, and efficient electrode preparation and performance improvement are achieved.

CN114175314BActive Publication Date: 2024-10-22DAIKIN INDUSTRIES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080052589.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-25
Filing Date
2020-07-22
Publication Date
2024-10-22
Estimated Expiration
2040-07-22

AI Technical Summary

Technical Problem

In the existing technology, the binder in sulfide-based solid-state batteries has insufficient solubility in low-polarity solvents, resulting in the inability to fully exert the function of the binder, and the types of solvents are limited, affecting the preparation effect of the electrode.

Method used

A specific fluoroelastomer is used as the binder. The fluoroelastomer whose resin terminal functional groups meet a specific ratio has excellent solubility and adhesion. It includes copolymerized units such as vinylidene fluoride and hexafluoropropylene. A slurry for a sulfide-based solid-state battery is prepared to ensure that the sulfide-based solid electrolyte particles do not react.

Benefits of technology

It achieves high solubility and softness in low-polarity solvents, expands the range of available solvents, and improves the preparation quality and performance of the electrode, especially in terms of softness and adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0003475439800000061
    Figure GDA0003475439800000061
  • Figure GDA0003475439800000241
    Figure GDA0003475439800000241
  • Figure GDA0003475439800000261
    Figure GDA0003475439800000261
Patent Text Reader

Abstract

Provided are a binder and a slurry that can be suitably used to manufacture electrodes in sulfide-based solid-state batteries. A binder is a binder used in a slurry for a solid-state battery containing sulfide-based solid electrolyte particles, wherein the binder is a fluorine-containing elastomer whose resin terminal functional groups satisfy 0.01≤([‑CH2OH]+[‑COOH]) / ([‑CH3]+[‑CF2H]+[‑CH2OH]+[‑CH2I]+[‑OC(O)RH]+[‑COOH])≤0.25 (wherein R represents an alkyl group having 1 to 20 carbon atoms).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a binder, a slurry for a solid-state battery, an electrode for a solid-state battery and a solid-state secondary battery. Background Art

[0002] Solid-state batteries have been studied as batteries with excellent safety. Sulfide-based and oxide-based solid conductors are known as solid-state batteries, and solid-state batteries using these have been studied. Among these, in sulfide-based solid-state batteries, research has been conducted on preparing a slurry containing an electrolyte and a binder, applying it, and drying it to form an electrode.

[0003] Patent Document 1 discloses that, in a method for producing a positive electrode for a solid-state battery, butyl butyrate is used as a solvent and a copolymer of vinylidene fluoride and hexafluoropropylene is used as a binder.

[0004] Patent Document 2 discloses that, in a method for producing a negative electrode for a solid-state battery, butyl butyrate is used as a solvent and a copolymer of vinylidene fluoride and hexafluoropropylene is used as a binder.

[0005] Patent Document 3 discloses a slurry for a positive electrode for a sulfide-based solid-state battery containing a fluorine-based polymer containing a vinylidene fluoride monomer component.

[0006] Patent Document 4 discloses a sulfide electrode slurry containing a fluorine-based polymer and a nitrile solvent, wherein the fluorine-based polymer contains a vinylidene fluoride monomer component.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2016-25027

[0010] Patent Document 2: Japanese Patent Application Publication No. 2016-25025

[0011] Patent Document 3: Japanese Patent Application Publication No. 2014-07138

[0012] Patent Document 4: Japanese Patent Application Publication No. 2012-204114 Summary of the invention

[0013] Technical problem to be solved by the invention

[0014] An object of the present invention is to provide a binder and a slurry that can be suitably used for producing electrodes in sulfide-based solid-state batteries.

[0015] Solutions to technical problems

[0016] The present invention relates to a binder used in a slurry for a solid-state battery containing sulfide-based solid electrolyte particles, wherein the binder is a fluorine-containing elastomer whose resin terminal functional groups satisfy the following formula.

[0017] 0.01≤([-CH2OH]+[-COOH]) / ([-CH3]+[-CF2H]+[-CH2OH]+[-CH2I]+[-OC(O)RH]+[-COOH])≤0.25

[0018] (In the formula, R represents an alkyl group having 1 to 20 carbon atoms.)

[0019] The fluorine-containing elastomer is preferably composed of vinylidene fluoride (VdF) monomer units and copolymer units.

[0020] The fluorinated elastomer preferably has at least one copolymerized unit selected from the group consisting of hexafluoropropylene (HFP), 2,3,3,3-tetrafluoropropylene, 1,3,3,3-tetrafluoropropylene, perfluoroalkyl vinyl ether (PAVE) and tetrafluoroethylene (TFE).

[0021] The fluorinated elastomer preferably has at least a portion of copolymerized units of hexafluoropropylene (HFP), perfluoroalkyl vinyl ether (PAVE) or tetrafluoroethylene (TFE). The fluorinated elastomer preferably has a fluorine content of 60 to 71% by mass.

[0022] The above-mentioned fluorine-containing elastomer preferably has a glass transition temperature of 25° C. or lower.

[0023] The above-mentioned fluorine-containing elastomer is preferably amorphous.

[0024] The present invention relates to a slurry for solid-state batteries comprising sulfide-based solid electrolyte particles, a binder and a solvent, wherein:

[0025] The binder is preferably any of the binders described above.

[0026] The above solvent is preferably a low-polarity solvent.

[0027] The solvent preferably contains at least one compound selected from the group consisting of aromatic compounds and ester compounds.

[0028] The solid-state battery slurry preferably further contains active material particles.

[0029] The active material particles are preferably negative electrode active materials.

[0030] The present invention also relates to a solid-state battery electrode comprising an electrode active material layer formed from a slurry containing the active material particles, and a current collector.

[0031] The solid-state battery electrode is preferably a negative electrode.

[0032] It is preferred that at least a part of the electrode active material contains a carbonaceous material.

[0033] It is preferred that at least a part of the electrode active material contains a silicon-containing compound.

[0034] The present invention also relates to a solid-state lithium-ion secondary battery, characterized in that it comprises the above-mentioned solid-state battery electrode.

[0035] Effects of the Invention

[0036] The binder of the present invention has excellent solubility in low-polarity solvents, excellent adhesion and flexibility, and can be suitably used when producing electrodes in sulfide-based solid-state batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] Figure 1 This is a diagram showing an example of the layered structure of the sulfide-based solid-state battery of the present invention. DETAILED DESCRIPTION

[0038] Hereinafter, the present invention will be described in detail.

[0039] The present invention relates to binders primarily for forming electrodes for solid-state batteries.

[0040] In the formation of electrodes for sulfide-based solid-state batteries, it is known that a slurry containing sulfide-based solid electrolyte particles, a binder and a solvent is applied, dried, and then pressed. In the case of forming a good electrode using such a method, it is important to select a binder and a solvent used in combination with the sulfide-based solid electrolyte particles. In particular, when using sulfide-based solid electrolyte particles, it is necessary to select a substance that does not react with the sulfide-based solid electrolyte particles, and the types of solvents that can be used are limited. In addition, in order to prepare a slurry using such a solvent, it is necessary to select a substance that dissolves in the solvent as a binder.

[0041] Therefore, as a binder, it is preferred to use a binder having a suitable solubility in a solvent. However, most of the known binders have a low solubility in a solvent. Therefore, it cannot be fully dissolved in the slurry containing sulfide-based solid electrolyte particles, and the function as a binder cannot be fully exerted. In the present invention, by using a polymer having the above-mentioned specific composition, a binder with good solubility can be obtained. Thus, a good slurry suitable for manufacturing a battery can be obtained.

[0042] In the present invention, a fluorine-containing elastomer having a resin terminal functional group satisfying the following formula is used.

[0043] 0.01≤([-CH2OH]+[-COOH]) / ([-CH3]+[-CF2H]+[-CH2OH]+[-CH2I]+[-OC(O)RH]+[-COOH]≤0.25

[0044] (In the formula, R represents an alkyl group having 1 to 20 carbon atoms.)

[0045] Preferably, 0.03≤([-CH2OH]+[-COOH]) / ([-CH3]+[-CF2H]+[-CH2OH]+[-CH2I]+[-OC(O)RH]+[-COOH]≤0.20.

[0046] The polymer has excellent properties such as heat resistance and flexibility, and is also excellent in terms of high solubility in low-polarity solvents. As a result, it is also possible to obtain a slurry in which the sulfide-based solid electrolyte particles do not react. In addition, the range of solvents that can be used is also widened, so solvents can be used differently according to the purpose. In particular, it is particularly preferred that the amount of the resin terminal functional group satisfies the above-mentioned flexibility.

[0047] The polymer of the present invention is a fluorine-containing elastomer. The fluorine-containing elastomer is an amorphous or low-crystalline fluorine-based polymer having a low glass transition temperature.

[0048] The fluorinated elastomer preferably has a glass transition temperature of 25°C or less. More preferably, the glass transition temperature is 0°C or less. Further preferably, the glass transition temperature is -5°C or less, and most preferably -10°C or less. Further, it may be -20°C or less. Here, regarding the glass transition temperature, a differential scanning calorimeter (manufactured by Hitachi Technosense Co., Ltd., X-DSC823e) is used. After cooling to -75°C, 10 mg of the sample is heated at 20°C / min to obtain a DSC curve. The temperature of the intersection of the extended line of the baseline before and after the secondary phase transition of the DSC curve and the tangent line at the inflection point of the DSC curve is taken as the glass transition temperature.

[0049] The fluorine-containing elastomer is preferably amorphous. Being amorphous means that there is no melting point peak in the DSC curve.

[0050] Such a low Tg, amorphous fluorinated elastomer is easily soluble in a solvent, and when used as a binder, it is particularly preferred in terms of imparting flexibility and easy processability to an electrode.

[0051] The preferred terminal structure of the polymer satisfies the following inequality: 0.01≤([-CH2OH]+[-COOH]) / ([-CH3]+[-CF2H]+[-CH2OH]+[-CH2I]+[-OC(O)RH]+[-COOH])≤0.25

[0052] (In the formula, R represents an alkyl group having 1 to 20 carbon atoms).

[0053] When the terminal functional group satisfies the above formula, the adhesiveness is good and the compound has an excellent function as a binder.

[0054] That is, [-CH2OH] and [-COOH] have functional groups with high affinity such as hydroxyl and carboxyl. Therefore, the resin with these functional groups has excellent affinity for the hydrophilic solvent used to prepare the slurry. Further, when the amount of these functional groups is excessive or too small, it becomes a resin with low flexibility, and therefore it is impossible to ensure the sufficient physical properties required as a binder. Further, when these functional groups are contained in a certain ratio or more, it will become a binder with excellent adhesion, which is preferred in this respect. Considering from such an aspect, [-CH2OH] and [-COOH] are preferably within the above range.

[0055] It should be noted that satisfying the above general formula does not mean that all functional groups such as [-CH3], [-CF2H], [-CH2OH], [-CH2I], [-OC(O)RH], and [-COOH] are present at the resin ends, but rather means that the number ratio of the terminal groups present therein is within the above range.

[0056] In addition, the amount of each terminal group of the resin can be analyzed by NMR. In addition, there is no particular limitation on the method of setting [-CH2OH] and [-COOH] within the above-defined range, and it can be controlled by known methods (for example, the selection and dosage of the initiator used).

[0057] It should be noted that the terminal group analysis by NMR is measured by a solution NMR method using protons. The analysis sample is adjusted to a 20 wt % solution using deuterated acetone (Acetone-d6) as a solvent and then measured.

[0058] Regarding the reference peak, the peak value of acetone was set to 2.05 ppm.

[0059] Measurement device: Varian VNMRS400

[0060] Resonance frequency: 399.74 (Sfrq)

[0061] Pulse width: 45°

[0062] Each end was made to correspond to the following peak position.

[0063] [-CH3]: 1.72~1.86ppm

[0064] [-CF2H]: 6.1~6.8ppm

[0065] [-CH2OH]: 3.74~3.80ppm

[0066] [-CH2I]: 3.87~3.92ppm

[0067] [-OC(O)RH]: 1.09~1.16ppm

[0068] [-COOH]: 10~15ppm

[0069] Based on the integrated value of each peak determined by the above measurement, the amount of functional groups was calculated from the intensity of each peak, and the amount was calculated by the following formula based on the result.

[0070] ([-CH2OH]+[-COOH]) / ([-CH3]+[-CF2H]+[-CH2OH]+[-CH2I]+[-OC(O)RH]+[-COOH])

[0071] The amount of terminal groups in the fluorinated elastomer can be controlled by a known general method. Specifically, the amount can be set to the above-specified range by adjusting the selection and amount of the initiator, the selection and amount of the chain transfer agent, etc.

[0072] The composition of the fluorine-containing elastomer of the present invention is not particularly limited as long as it has the above-mentioned terminal group amount, and a fluorine-containing polymer may be used.

[0073] It should be noted that the fluorine-containing elastomer of the present invention may be a substance other than the following polymer, which is a polymer having a vinylidene fluoride unit and at least one copolymerization unit (A) selected from the group consisting of a monomer unit having a structure represented by the following general formula (1) and a monomer unit having a structure represented by the following general formula (2).

[0074] [Chemistry 1]

[0075]

[0076] In the formula, Rf1 and Rf2 are linear or branched fluoroalkyl or fluoroalkoxy groups having 1 to 12 carbon atoms. When the number of carbon atoms is 2 or more, an oxygen atom may be contained between carbon atoms.

[0077] As the above-mentioned fluorine-containing elastomer, specifically, for example, vinylidene fluoride (VdF)-based fluorine-containing elastomer, TFE / propylene (Pr)-based fluorine-containing elastomer, TFE / Pr / VdF-based fluorine-containing elastomer, ethylene (Et) / HFP-based fluorine-containing elastomer, Et / HFP / VdF-based fluorine-containing elastomer, Et / HFP / TFE-based fluorine-containing elastomer, fluorosilicone-based fluorine-containing elastomer, or fluorophosphazene-based fluorine-containing elastomer, etc., can be mentioned, and they can be used alone or in any combination within the range that does not impair the effect of the present invention. Among these, VdF-based fluorine-containing elastomer is preferably used.

[0078] The above-mentioned VdF-based fluorinated elastomer is a fluorinated elastomer having a VdF repeating unit. The VdF repeating unit of the VdF-based fluorinated elastomer is preferably 20 mol% or more and 90 mol% or less of the total molar number of the VdF repeating unit and the repeating unit derived from other comonomers, more preferably 40 mol% or more and 85 mol% or less. A further preferred lower limit is 45 mol%, and a particularly preferred lower limit is 50 mol%. A further preferred upper limit is 80 mol%.

[0079] The comonomer in the VdF-based elastomer is not particularly limited as long as it is copolymerizable with VdF, and examples thereof include tetrafluoroethylene (TFE), hexafluoropropylene (HFP), perfluoroalkyl vinyl ether (PAVE), chlorotrifluoroethylene (CTFE), trifluoroethylene, trifluoropropylene, tetrafluoropropylene, pentafluoropropylene, trifluorobutylene, tetrafluoroisobutylene, hexafluoroisobutylene, vinyl fluoride, iodine-containing fluorovinyl ether, and the like represented by the general formula (1-1):

[0080] CH2=CFRf1 (1-1)

[0081] (wherein Rf1 is a linear or branched fluoroalkyl or fluoroalkoxy group having 1 to 12 carbon atoms, and when the number of carbon atoms is 2 or more, an oxygen atom may be contained between carbon atoms.) The fluorine-containing monomer represented by the general formula (2-1)

[0082] CHF=CHRf2 (2-1)

[0083] (wherein Rf2 is a straight-chain or branched fluorinated alkyl or fluorinated alkoxy group having 1 to 12 carbon atoms. When the number of carbon atoms is 2 or more, oxygen atoms may be contained between carbon-carbon atoms.) Fluorine-containing monomers such as fluorine-containing monomers represented by; non-fluorine-containing monomers such as ethylene (Et), propylene (Pr), alkyl vinyl ether, monomers providing crosslinking groups (vulcanization points), and reactive emulsifiers, etc., and one of these monomers or compounds can be used or a combination of two or more of them can be used.

[0084] In the compound represented by the general formula (1-1), Rf1 is a linear or branched fluoroalkyl group having 1 to 12 carbon atoms, or a linear or branched fluoroalkoxy group having 1 to 12 carbon atoms. When the number of carbon atoms of the fluoroalkyl group and the fluoroalkoxy group are both 2 or more, an oxygen atom (—O—) may be contained between carbon atoms.

[0085] The fluoroalkyl group of Rf1 may be a partial fluoroalkyl group in which a part of the hydrogen atoms bonded to the carbon atom is replaced by a fluorine atom, or a perfluoroalkyl group in which all the hydrogen atoms bonded to the carbon atom are replaced by fluorine atoms. In addition, the fluoroalkyl group of Rf1 may be a hydrogen atom replaced by a substituent other than a fluorine atom, but preferably does not contain a substituent other than a fluorine atom.

[0086] In addition, the fluoroalkoxy group of Rf1 may be a partial fluoroalkoxy group in which a part of the hydrogen atoms bonded to the carbon atom is replaced by a fluorine atom, or may be a perfluoroalkoxy group in which all the hydrogen atoms bonded to the carbon atom are replaced by fluorine atoms. In addition, the fluoroalkoxy group of Rf1 may be a hydrogen atom replaced by a substituent other than a fluorine atom, but preferably does not contain a substituent other than a fluorine atom.

[0087] The number of carbon atoms in Rf1 is preferably 1 to 10, more preferably 1 to 6, further preferably 1 to 4, and particularly preferably 1.

[0088] As Rf1, the general formula is preferred:

[0089] -(Rf 11 )m-(O)p-(Rf 12 -O)n-Rf 13

[0090] (Where Rf 11 and Rf 12 is independently a linear or branched fluoroalkylene group having 1 to 4 carbon atoms, Rf 13 A group represented by a linear or branched fluoroalkyl group having 1 to 4 carbon atoms, wherein p is 0 or 1, m is an integer of 0 to 4, and n is an integer of 0 to 4).

[0091] R 11 and Rf 12 The fluorinated alkylene group may be a partially fluorinated alkylene group in which a part of the hydrogen atoms bonded to the carbon atoms are replaced by fluorine atoms, or a perfluorinated alkylene group in which all the hydrogen atoms bonded to the carbon atoms are replaced by fluorine atoms. 11 and Rf 12 The fluorinated alkylene group may have a hydrogen atom substituted by a substituent other than a fluorine atom, but preferably does not contain a substituent other than a fluorine atom. 11 and Rf 12 It may be the same or different in each occurrence.

[0092] As Rf 11 The fluorinated alkylene group may include -CHF-, -CF2-, -CH2-CF2-, -CHF-CF2-, -CF2-CF2-, -CF(CF3)-, -CH2-CF2-CF2-, -CHF-CF2-CF2-, -CF2-CF2-CF2-, -CF(CF3)-CF2-, -CF2–CF(CF3)-, -C(CF3)2-, -CH2-CF2-CF2-CF2-, -CHF-CF2-CF2-CF2-, -CF2-CF2-CF2-CF2-, -CH(CF3)-CF2-CF2-, -CF(CF3)-CF2-CF2-, -C(CF3)2-, etc. Among them, a perfluoroalkylene group having 1 or 2 carbon atoms is preferred, and -CF2- is more preferred.

[0093] As Rf 12 The fluoroalkylene group includes -CHF-, -CF2-, -CH2-CF2-, -CHF-CF2-, -CF2-CF2-, -CF(CF3)-, -CH2-CF2-CF2-, -CHF-CF2-CF2-, -CF2-CF2-CF2-, -CF(CF3)-CF2-, -CF2-CF(CF3)-, -C(CF3)2-, -CH2-CF2-CF2-CF2-, -C HF-CF2-CF2-CF2-, -CF2-CF2-CF2-CF2-, -CH(CF3)-CF2-CF2-, -CF(CF3)-CF2-CF2-, -C(CF3)2-CF2-, etc., among which perfluoroalkylene having 1 to 3 carbon atoms is preferred, and -CF2-, -CF2CF2-, -CF2-CF2-CF2-, -CF(CF3)-CF2- or -CF2-CF(CF3) is more preferred.

[0094] As Rf 13 The fluorinated alkyl group may be a partially fluorinated alkyl group in which a part of the hydrogen atoms bonded to the carbon atoms are replaced by fluorine atoms, or a perfluorinated alkyl group in which all the hydrogen atoms bonded to the carbon atoms are replaced by fluorine atoms. 13 The fluorinated alkyl group may have a hydrogen atom substituted by a substituent other than a fluorine atom, but preferably does not contain a substituent other than a fluorine atom (for example, -CN, -CH2I, -CH2Br, etc.).

[0095] As Rf 13The fluoroalkyl group includes -CH2F, -CHF2, -CF3, -CH2-CH2F, -CH2-CHF2, -CH2-CF3, -CHF-CH2F, -CHF-CHF2, -CHF-CF3, -CF2-CH2F, -CF2-CHF2, -CF2-CF3, -CH2-CF2-CH2F, -CHF-CF2-CH2F, -CF2-CF2-CH2F, -CF(CF3)-CH2F, -CH2-CF2-CHF2, -CHF-CF2-CHF2, -CF2-CF2-CHF2, -CF(CF3)-CHF2, -CH2-CF2-CF3, -CHF-CF 2-CF3, -CF2-CF2-CF3, -CF(CF3)-CF3, -CH2-CF2-CF2-CF3, -CHF-CF2-CF2-CF3, -CF2-CF2-CF2-CF3, -CH(CF3)-CF2-CF3, -CF(CF3)-CF2-CF3, -C(CF3 )2-CF3, etc., among which -CF3, -CHF-CF3, -CF2-CHF2, -CF2-CF3, -CF2-CF2-CF3, -CF(CF3)-CF3, -CF2-CF2-CF2-CF3, -CH(CF3)-CF2-CF3 or -CF(CF3)-CF2-CF3 are preferred.

[0096] As p, 0 is preferred.

[0097] m is preferably an integer of 0 to 2, more preferably 0 or 1, and further preferably 0. When p is 0, m is preferably 0 as well.

[0098] n is preferably an integer of 0 to 2, more preferably 0 or 1, and even more preferably 0.

[0099] As the repeating unit, preferably

[0100] -CH2-CF[-CF3]-,

[0101] -CH2-CF[-CF2CF3]-,

[0102] -CH2-CF[-CF2CF2CF3]-,

[0103] -CH2-CF[-CF2CF2CF2CF3]-,

[0104] -CH2-CF[-CF2-O-CF(CF3)-CF2-O-CHF-CF3]-,

[0105] -CH2-CF[-CF2-O-CF(CF3)-CF2-O-CF2-CF3]-,

[0106] -CH2-CF[-CF2-O-CF(CF3)-CF2-O-CF(CF3)-CF3]-,

[0107] -CH2-CF[-CF2-O-CF(CF3)-CF2-O-CH(CF3)-CF2-CF3]-,

[0108] -CH2-CF[-CF2-O-CF(CF3)-CF2-O-CF(CF3)-CF2-CF3]-,

[0109] -CH2-CF[-OCF2OCF3]-,

[0110] -CH2-CF[-OCF2CF2CF2OCF3]-,

[0111] -CH2-CF[-CF2OCFOCF3]-,

[0112] -CH2-CF[-CF2OCF2CF2CF2OCF3]-, or

[0113] -CH2-CF[-O-CF2-CF3]-,

[0114] More preferred is -CH2-CF[-CF3]-.

[0115] As the compound represented by the above formula (2-1), Rf2 is a linear or branched fluoroalkyl group having 1 to 12 carbon atoms, or a linear or branched fluoroalkoxy group having 1 to 12 carbon atoms. When the fluoroalkyl group and the fluoroalkoxy group have 2 or more carbon atoms, an oxygen atom (-O-) may be contained between carbon atoms.

[0116] The fluoroalkyl group of Rf2 can be a partial fluoroalkyl group substituted by a fluorine atom as a part of the hydrogen atom bonded to the carbon atom, or a perfluoroalkyl group in which the hydrogen atom bonded to the carbon atom is all substituted by a fluorine atom. In addition, the fluoroalkyl group of Rf2 can also be a hydrogen atom substituted by a substituent other than a fluorine atom, but preferably does not contain a substituent other than a fluorine atom.

[0117] In addition, the fluoroalkoxy group of Rf2 can be a partial fluoroalkoxy group in which a part of the hydrogen atom bonded to the carbon atom is replaced by a fluorine atom, or can be a perfluoroalkoxy group in which the hydrogen atom bonded to the carbon atom is all replaced by a fluorine atom. In addition, the fluoroalkoxy group of Rf2 can also be a hydrogen atom replaced by a substituent other than a fluorine atom, but preferably does not contain a substituent other than a fluorine atom.

[0118] The number of carbon atoms in Rf2 is preferably 1 to 10, more preferably 1 to 6, further preferably 1 to 4, and particularly preferably 1.

[0119] As Rf2, the general formula is preferred:

[0120] -(Rf 21 )m-(O)p-(Rf 22 -O)n-Rf 23

[0121] (Where Rf 21 and Rf 22 is independently a linear or branched fluoroalkylene group having 1 to 4 carbon atoms, Rf 23 It is a linear or branched fluorinated alkyl group having 1 to 4 carbon atoms, p is 0 or 1, m is an integer of 0 to 4, and n is an integer of 0 to 4. )

[0122] R 21 and Rf 22 The fluorinated alkylene group may be a partially fluorinated alkylene group in which a part of the hydrogen atoms bonded to the carbon atoms are replaced by fluorine atoms, or a perfluorinated alkylene group in which all the hydrogen atoms bonded to the carbon atoms are replaced by fluorine atoms. 21 and Rf 22 The fluorinated alkylene group may have a hydrogen atom substituted by a substituent other than a fluorine atom, but preferably does not contain a substituent other than a fluorine atom. 21 and Rf 22 It may be the same or different in each occurrence.

[0123] As Rf 21 The fluorinated alkylene group may include -CHF-, -CF2-, -CH2-CF2-, -CHF-CF2-, -CF2-CF2-, -CF(CF3)-, -CH2-CF2-CF2-, -CHF-CF2-CF2-, -CF2-CF2-CF2-, -CF(CF3)-CF2-, -CF2-CF(CF3)-, -C(CF3)2-, -CH2-CF2-CF2-CF2-, -CHF-CF2-CF2-CF2-, -CF2-CF2-CF2-CF2-, -CH(CF3)-CF2-CF2-, -CF(CF3)-CF2-CF2-, -C(CF3)2-, etc. Among them, perfluoroalkylene group having 1 or 2 carbon atoms is preferred, and -CF2 is more preferred.

[0124] As Rf 22The fluoroalkylene group includes -CHF-, -CF2-, -CH2-CF2-, -CHF-CF2-, -CF2-CF2-, -CF(CF3)-, -CH2-CF2-CF2-, -CHF-CF2-CF2-, -CF2-CF2-CF2-, -CF(CF3)-CF2-, -CF 2- CF(CF3)-, -C(CF3)2-, -CH2-CF2-CF2-CF2-, -CHF-CF2-CF2-CF2-, -CF2-CF2-CF2-CF2-, -CH(CF3)-CF2-CF2-, -CF(CF3)-CF2-CF2-, -C(CF3)2-CF2-, etc., among which perfluoroalkylene having 1 to 3 carbon atoms is preferred, and -CF2-, -CF2CF2-, -CF2-CF2-CF2-, -CF(CF3)-CF2- or -CF2-CF(CF3) is more preferred.

[0125] As Rf 23 The fluorinated alkyl group may be a partially fluorinated alkyl group in which a part of the hydrogen atoms bonded to the carbon atoms are replaced by fluorine atoms, or a perfluorinated alkyl group in which all the hydrogen atoms bonded to the carbon atoms are replaced by fluorine atoms. 23 The fluorinated alkyl group may have a hydrogen atom substituted by a substituent other than a fluorine atom, but preferably contains no substituent other than a fluorine atom (for example, -CN, -CH2I, -CH2Br, etc.).

[0126] As Rf 23The fluoroalkyl group includes -CH2F, -CHF2, -CF3, -CH2-CH2F, -CH2-CHF2, -CH2-CF3, -CHF-CH2F, -CHF-CHF2, -CHF-CF3, -CF2-CH2F, -CF2-CHF2, -CF2-CF3, -CH2-CF2-CH2F, -CHF-CF2-CH2F, -CF2-CF2-CH2F, -CF(CF3)-CH2F, -CH2-CF2-CHF2, -CHF-CF2-CHF2, -CF2-CF2-CHF2, -CF(CF3)-CHF2, -CH2-CF2-CF3, -CHF-CF 2-CF3, -CF2-CF2-CF3, -CF(CF3)-CF3, -CH2-CF2-CF2-CF3, -CHF-CF2-CF2-CF3, -CF2-CF2-CF2-CF3, -CH(CF3)-CF2-CF3, -CF(CF3)-CF2-CF3, -C(CF3 )2-CF3, etc., among which -CF3, -CHF-CF3, -CF2-CHF2, -CF2-CF3, -CF2-CF2-CF3, -CF(CF3)-CF3, -CF2-CF2-CF2-CF3, -CH(CF3)-CF2-CF3 or -CF(CF3)-CF2-CF3 are preferred.

[0127] As p, 0 is preferred.

[0128] m is preferably an integer of 0 to 2, more preferably 0 or 1, and further preferably 0. When p is 0, m is preferably 0 as well.

[0129] n is preferably an integer of 0 to 2, more preferably 0 or 1, and even more preferably 0.

[0130] As the repeating unit, preferably

[0131] -CHF-CH[-CF3]-,

[0132] -CHF-CH[-CF2CF3]-,

[0133] -CHF-CH[-CF2CF2CF3]-, or

[0134] -CHF-CH[-CF2CF2CF2CF3]-,

[0135] More preferred is -CHF-CH[-CF3]-.

[0136] Among them, the copolymerization unit is preferably composed of hexafluoropropylene (HFP), tetrafluoroethylene (TFE), 2,3,3,3-tetrafluoropropylene, 1,3,3,3-tetrafluoropropylene, and perfluoroalkyl vinyl ether (PAVE). Further, it is most preferred that at least a portion of the copolymerization unit is hexafluoropropylene (HFP). As a vinylidene fluoride elastomer in which at least a portion of the copolymerization unit is hexafluoropropylene (HFP), a binary elastomer composed of vinylidene fluoride and hexafluoropropylene, a ternary elastomer composed of vinylidene fluoride, tetrafluoroethylene and hexafluoropropylene, etc. can be cited.

[0137] As the PAVE, perfluoro(methyl vinyl ether) (PMVE) and perfluoro(propyl vinyl ether) (PPVE) are more preferred, and PMVE is particularly preferred.

[0138] Alternatively, as the above PAVE, the formula: CF2=CFOCF2ORf c

[0139] (Where Rf c The perfluorovinyl ether is a straight or branched perfluoroalkyl group having 1 to 6 carbon atoms, a cyclic perfluoroalkyl group having 5 to 6 carbon atoms, or a straight or branched perfluorooxyalkyl group having 2 to 6 carbon atoms and containing 1 to 3 oxygen atoms. For example, CF2=CFOCF2OCF3, CF2=CFOCF2OCF2CF3, or CF2=CFOCF2OCF2CF2OCF3 is preferably used.

[0140] As the above-mentioned VdF-based fluorine-containing elastomer, at least one copolymer selected from the group consisting of a copolymer of VdF / HFP copolymer, VdF / TFE / HFP copolymer, VdF / CTFE copolymer, VdF / CTFE / TFE copolymer, VdF / PAVE copolymer, VdF / TFE / PAVE copolymer, VdF / HFP / PAVE copolymer, VdF / HFP / TFE / PAVE copolymer, VdF / TFE / Pr copolymer, VdF / Et / HFP copolymer and VdF / a fluorine-containing monomer represented by formula (1-1) or formula (2-1) is preferred. In addition, as other comonomers other than VdF, at least one comonomer selected from the group consisting of TFE, HFP and PAVE is more preferred.

[0141] Among these, at least one copolymer selected from the group consisting of VdF / HFP copolymers, VdF / TFE / HFP copolymers, VdF / copolymers of fluorinated monomers represented by formula (1-1) or formula (2-1), VdF / PAVE copolymers, VdF / TFE / PAVE copolymers, VdF / HFP / PAVE copolymers and VdF / HFP / TFE / PAVE copolymers is preferred; at least one copolymer selected from the group consisting of VdF / HFP copolymers, VdF / TFE / HFP copolymers, VdF / copolymers of fluorinated monomers represented by formula (1-1) or formula (2-1) and VdF / PAVE copolymers is more preferred; and at least one copolymer selected from the group consisting of VdF / HFP copolymers, VdF / TFE / HFP copolymers and VdF / PAVE copolymers is particularly preferred.

[0142] The VdF / HFP copolymer preferably has a VdF / HFP composition of (45-85) / (55-15) (mol%), more preferably (50-80) / (50-20) (mol%), and even more preferably (60-80) / (40-20) (mol%). The VdF / HFP composition is also preferably (50-78) / (50-22) (mol%).

[0143] The VdF / TFE / HFP copolymer preferably has a composition of VdF / TFE / HFP of (30 to 80) / (4 to 35) / (10 to 35) (mol %).

[0144] As the VdF / PAVE copolymer, the composition of VdF / PAVE is preferably (65 to 90) / (35 to 10) (mol %). In addition, the composition of VdF / PAVE is (50 to 78) / (50 to 22) (mol %), which is also one of the preferred embodiments.

[0145] As the VdF / TFE / PAVE copolymer, the composition of VdF / TFE / PAVE is preferably (40 to 80) / (3 to 40) / (15 to 35) (mol %).

[0146] As the VdF / HFP / PAVE copolymer, it is preferable that the composition of VdF / HFP / PAVE is (65 to 90) / (3 to 25) / (3 to 25) (mol %).

[0147] The VdF / HFP / TFE / PAVE copolymer preferably has a composition of (40-90) / (0-25) / (0-40) / (3-35) (mol %), and more preferably (40-80) / (3-25) / (3-40) / (3-25) (mol %).

[0148] As a copolymer of VdF / fluorinated monomer (1-1) or (2-1) represented by formula (1-1) or (2-1), it is preferred that the VdF / fluorinated monomer (1-1) or (2-1) unit is 87 / 13 to 20 / 80 (mol %), and the other monomer units other than VdF and fluorinated monomer (1-1) or (2-1) account for 0 to 50 mol % of all monomer units, and more preferably the mol % ratio of VdF / fluorinated monomer (1-1) or (2-1) unit is 80 / 20 to 20 / 80. In addition, it is also one of the preferred embodiments that the composition of VdF / fluorinated monomer (1-1) or (2-1) unit is 78 / 22 to 50 / 50 (mol %). It is also preferred that the VdF / fluorinated monomer (1-1) or (2-1) unit is 87 / 13 to 50 / 50 (mol%), and the monomer units other than VdF and the fluorinated monomer (1-1) or (2-1) account for 1 to 50 mol% of the total monomer units. As the monomers other than VdF and the fluorinated monomer (1-1) or (2-1), TFE, HFP, PMVE, perfluoroethyl vinyl ether (PEVE), PPVE, CTFE, trifluoroethylene, hexafluoroisobutylene, vinyl fluoride, Et, Pr, alkyl vinyl ether, monomers providing crosslinking groups, and reactive emulsifiers are preferred as the monomers exemplified as the comonomers of VdF, and PMVE, CTFE, HFP, and TFE are more preferred.

[0149] The TFE / Pr-based fluorinated elastomer is a fluorinated copolymer composed of 45 to 70 mol% TFE and 55 to 30 mol% Pr, and may contain 0 to 40 mol% of a specific third component (eg, PAVE) in addition to these two components.

[0150] As the Et / HFP copolymer, the composition of Et / HFP is preferably (35 to 80) / (65 to 20) (mol %), and more preferably (40 to 75) / (60 to 25) (mol %).

[0151] The Et / HFP / TFE copolymer preferably has a composition of Et / HFP / TFE of (35 to 75) / (25 to 50) / (0 to 15) (mol %), and more preferably (45 to 75) / (25 to 45) / (0 to 10) (mol %).

[0152] Perfluoroelastomers include those composed of TFE / PAVE, etc. The composition of TFE / PAVE is preferably (50-90) / (50-10) (mol %), more preferably (50-80) / (50-20) (mol %), and further preferably (55-75) / (45-25) (mol %).

[0153] Examples of PAVE in this case include PMVE and PPVE, and these can be used alone or in any combination.

[0154] The fluorine content of the fluorine-containing elastomer is preferably 50% by mass or more, more preferably 55% by mass or more, and further preferably 60% by mass or more. The upper limit of the fluorine content is not particularly limited, but is preferably 71% by mass or less.

[0155] The fluorine content is a value obtained by calculation from the composition of the fluorinated elastomer measured by 19F-NMR.

[0156] The molecular weight was calculated from the composition ratio, and the mass of fluorine atoms contained therein was found to calculate the fluorine content.

[0157] In the present invention, the composition ratio of each repeating unit of the fluorinated elastomer is a value measured by an NMR method. Specifically, it is a value measured by the following solution NMR method.

[0158] Measurement device: Varian VNMRS400

[0159] Resonance frequency: 376.04 (Sfrq)

[0160] Pulse width: 30° (pw=6.8)

[0161] The non-perfluorinated fluoroelastomer and perfluorinated fluoroelastomer described above can be produced by conventional methods such as emulsion polymerization, suspension polymerization, solution polymerization, etc. In particular, a fluoroelastomer having a narrow molecular weight distribution can be produced by a polymerization method using an iodine (bromine) compound which is well known as iodine (bromine) transfer polymerization.

[0162] The above polymer may have structural units other than vinylidene fluoride units and copolymerization units (A). In this case, the content of other structural units is preferably less than 50 mol%. It should be noted that it may also be composed only of vinylidene fluoride units and copolymerization units (A). The content of other structural units is more preferably less than 30 mol%, and further preferably less than 15 mol%.

[0163] The polymer may use a monomer that provides a crosslinking site as the other monomer.

[0164] The monomer providing the crosslinking site is not particularly limited, and for example, the monomer of the general formula:

[0165] CX 1 2=CX 1 -Rf 1 CHR 1 X 2

[0166] (Where X 1 is a hydrogen atom, a fluorine atom or -CH3, Rf 1 is a fluoroalkylene group, a perfluoroalkylene group, a fluoro(poly)oxyalkylene group or a perfluoro(poly)oxyalkylene group, R 1 is a hydrogen atom or -CH3, X 2 is an iodine atom or a bromine atom. ) The iodine-containing or bromine-containing monomer represented by the general formula:

[0167] CF2=CFO(CF2CF(CF3)O) m (CF2) n -X 3 (wherein, m is an integer from 0 to 5, n is an integer from 1 to 3, and X 3 is a cyano group, a carboxyl group, an alkoxycarbonyl group, an iodine atom or a bromine atom. ) The monomer represented by the general formula:

[0168] CH2=CFCF2O(CF(CF3)CF2O) m (CF(CF3)) n -X 4

[0169] (wherein, m is an integer from 0 to 5, n is an integer from 1 to 3, and X 4 is a cyano group, a carboxyl group, an alkoxycarbonyl group, an iodine atom, a bromine atom or -CH2OH. ) as other monomers.

[0170] Among them, at least one of the group consisting of CF2=CFOCF2CF(CF3)OCF2CF2CN, CF2=CFOCF2CF(CF3)OCF2CF2COOH, CF2=CFOCF2CF2CH2I, CF2=CFOCF2CF(CF3)OCF2CF2CH2I, CH2=CFCF2OCF(CF3)CF2OCF(CF3)CN, CH2=CFCF2OCF(CF3)CF2OCF(CF3)COOH, and CH2=CFCF2OCF(CF3)CF2OCF(CF3)CH2OH is preferred. In addition, repeating units based on monomers providing crosslinking sites may be contained, but in one embodiment of the present invention, a crosslinking agent is not contained.

[0171] In order to make the above-mentioned fluorine-containing elastomer have good adhesion and flexibility and good solubility in solvents, the number average molecular weight (Mn) is preferably 7000 to 5000000, the mass average molecular weight (Mw) is preferably 10000 to 10000000, and Mw / Mn is preferably 1.0 to 30.0, more preferably 1.5 to 25.0. The above-mentioned number average molecular weight (Mn), mass average molecular weight (Mw) and Mw / Mn are values ​​measured by GPC method.

[0172] The fluorinated elastomer preferably has a Mooney viscosity at 121°C (ML1+10(121°C)) of 2 or more, more preferably 5 or more, further preferably 10 or more, particularly preferably 30 or more. The Mooney viscosity is a value measured in accordance with ASTM-D1646-15 and JIS K6300-1:2013.

[0173] The fluorine-containing polymer can be produced by a general free radical polymerization method. The polymerization method may be any of bulk polymerization, solution polymerization, suspension polymerization and emulsion polymerization, but emulsion polymerization is preferred because it is easy to implement industrially.

[0174] In the polymerization, a polymerization initiator, a chain transfer agent, a surfactant, and a solvent may be used, and any conventionally known one may be used. In the polymerization of the copolymer, an oil-soluble radical polymerization initiator or a water-soluble radical initiator may be used as the polymerization initiator.

[0175] The oil-soluble free radical polymerization initiator may be a known oil-soluble peroxide. Representative examples include dialkyl peroxycarbonates such as diisopropyl peroxydicarbonate and di-sec-butyl peroxydicarbonate, peroxyesters such as tert-butyl peroxyisobutyrate and tert-butyl peroxypivalate, dialkyl peroxides such as di-tert-butyl peroxide, and di(ω-hydro-dodecafluoroheptanoyl)peroxide, di(ω-hydro-tetradecafluoroheptanoyl)peroxide, di(ω-hydro-hexadecanoyl)peroxide, di(perfluorobutyryl)peroxide, di(perfluorovaleryl)peroxide, di(perfluorohexanoyl)peroxide, di(perfluoroheptanoyl)peroxide, and di(perfluorooctanoyl)peroxide. peroxide, bis(perfluorononanoyl) peroxide, bis(ω-chloro-hexafluorobutyryl) peroxide, bis(ω-chloro-decafluorohexanoyl) peroxide, bis(ω-chloro-tetrafluorooctanoyl) peroxide, ω-hydro-dodecafluoroheptanoyl-ω-hydrohexafluorononanoyl-peroxide, ω-chloro-hexafluorobutyryl-ω-chloro-decafluorohexanoyl-peroxide, ω-hydro-dodecafluoroheptanoyl-perfluorobutyryl-peroxide, bis(dichloropentafluorobutyryl) peroxide, bis(trichlorooctafluorohexanoyl) peroxide, bis(tetrachloroundecanoyl) peroxide, bis(pentachlorotetrafluorodecanoyl) peroxide, bis(undecachlorotriadecanoyl) peroxide and the like.

[0176] As the water-soluble free radical polymerization initiator, it can be a known water-soluble peroxide, for example, ammonium salts, potassium salts, sodium salts of persulfuric acid, perboric acid, perchloric acid, perphosphoric acid, percarbonic acid, etc., tert-butyl peroxymaleate, tert-butyl hydroperoxide, etc. It can also contain a reducing agent such as sulfite esters and sulfites, and the amount used can be 0.1 to 20 times that of the peroxide.

[0177] The amount of the free radical polymerization initiator added is not particularly limited, and can be added all at once, sequentially, or continuously at the initial stage of polymerization in an amount that does not significantly reduce the polymerization rate (for example, a concentration of several ppm relative to water). The upper limit is the range in which the polymerization reaction heat can be removed from the device surface.

[0178] As a surfactant, a nonionic surfactant, an anionic surfactant, a cationic surfactant, etc. can be used, preferably a linear or branched fluorinated anionic surfactant having 4 to 20 carbon atoms such as ammonium perfluorooctanoate and ammonium perfluorohexanoate. The addition amount (relative to polymerization water) is preferably 10 to 5000 ppm. More preferably, it is 50 to 5000 ppm. In addition, as a surfactant, a reactive emulsifier can be used. As long as the reactive emulsifier is a compound having one or more unsaturated bonds and one or more hydrophilic groups, there is no particular limitation, and examples thereof include CH2=CFCF2OCF(CF3)CF2OCF(CF3)COONH4, CH2=CFCF2CF(CF3)OCF2CF2COONH4, and CF2=CFOCF2CF(CF3)OCF(CF3)COONH4. The addition amount (relative to polymerization water) is preferably 10 to 5000 ppm. More preferably, it is 50 to 5000 ppm.

[0179] The solvent is preferably a solvent without chain transfer properties. In the case of solution polymerization, dichloropentafluoropropane (R-225) can be used, and in the case of emulsion polymerization and suspension polymerization, water, a mixture of water and a water-soluble organic solvent, or a mixture of water and a water-insoluble organic solvent can be used.

[0180] In the above polymerization, examples of chain transfer agents include esters such as dimethyl malonate, diethyl malonate, methyl acetate, ethyl acetate, butyl acetate, dimethyl succinate, and isopentane, methane, ethane, propane, isopropanol, acetone, various mercaptans, carbon tetrachloride, cyclohexane, and the like.

[0181] As the chain transfer agent, a bromine compound or an iodine compound can be used. As a polymerization method using a bromine compound or an iodine compound, for example, a method of performing emulsion polymerization in an aqueous medium under pressure in the presence of a bromine compound or an iodine compound in a substantially oxygen-free state (iodine transfer polymerization method) can be cited. As a representative example of the bromine compound or iodine compound used, for example, the general formula:

[0182] A compound represented by R2IxBry (wherein x and y are integers of 0 to 2 respectively and satisfy 1≤x+y≤2, and R2 is a saturated or unsaturated fluorocarbon or chlorofluorocarbon group having 1 to 16 carbon atoms, or a hydrocarbon group having 1 to 3 carbon atoms, which may contain oxygen atoms).

[0183] Examples of the iodine compound include 1,3-diiodoperfluoropropane, 2-iodoperfluoropropane, 1,3-diiodoperfluoropropane-2-chloroperfluoropropane, 1,4-diiodoperfluorobutane, 1,5-diiodoperfluoropentane-2,4-dichloroperfluoropentane, 1,6-diiodoperfluorohexane, 1,8-diiodoperfluorooctane, 1,12-diiodoperfluorododecane, 1,16-diiodoperfluorohexadecane, diiodomethane, 1,2-diiodoethane, 1,3-diiodoperfluoropropane, CF2Br2, BrCF2CF2Br, CF3CFBrCF2Br, CFClBr2, BrC F2CFClBr, CFBrClCFClBr, BrCF2CF2CF2Br, BrCF2CFBrOCF3, 1-bromo-2-iodoperfluoroethane, 1-bromo-3-iodoperfluoropropane, 1-bromo-4-iodoperfluorobutane, 2-bromo-3-iodoperfluorobutane, 3-bromo-4-iodoperfluoro-1-butene, 2-bromo-4-iodoperfluoro-1-butene, mono-iodine and mono-bromine substitutes of benzene, di-iodine and mono-bromine substitutes, and (2-iodoethyl) and (2-bromoethyl) substitutes, etc. These compounds can be used alone or in combination with each other.

[0184] Among these, 1,4-diiodoperfluorobutane, 1,6-diiodoperfluorohexane, and 2-iodoperfluoropropane are preferably used in view of polymerization reactivity, crosslinking reactivity, and availability.

[0185] The above-mentioned copolymer can be any form such as aqueous dispersion, powder. About the powder of copolymer, in the case of emulsion polymerization, can be by making the dispersion liquid of finishing polymerization precipitate, and wash, dehydrate, dry and obtain. Precipitation can be carried out by adding inorganic salts or inorganic acids such as aluminum sulfate or imparting mechanical shear force or freezing dispersion liquid. In the case of suspension polymerization, can be by reclaiming and drying from the dispersion liquid of finishing polymerization. In the case of solution polymerization, the solution containing fluoropolymer can be dried as it is and obtained, and can also be obtained by dripping poor solvent and refining.

[0186] As the polymer, one kind may be used, or two or more kinds may be used. In particular, a mode in which two copolymers having different molecular structures are used in combination is also possible.

[0187] The binder of the present invention is used in a slurry for a solid-state battery containing sulfide-based solid electrolyte particles. Specifically, it is used in a slurry for forming a layer constituting a solid-state battery. More specifically, it is used in a slurry for a solid-state battery containing sulfide-based solid electrolyte particles, a binder, and a solvent.

[0188] The preferred solvent of the slurry of the present invention is a low polarity solvent. By using a low polarity solvent, it is difficult to react with the sulfide solid electrolyte particles, which is preferred in this respect. Regarding the low polarity solvent, in the present invention, the low polarity solvent is defined as a substance having a relative dielectric constant of less than 20 at a frequency of 100kHz. It is further preferably less than 10. The solvent preferably contains at least one compound selected from the group consisting of an aromatic compound, an ester compound, an aliphatic hydrocarbon compound, an ether compound and a carbonate compound. Preferably, it is an aromatic compound, an ester compound, and most preferably, an ester compound.

[0189] The low polarity solvent is not particularly limited, and examples thereof include n-octane, n-nonane, n-decane, n-butyl ether, diisoamyl ether, ethylbenzene, ethyl acetate, ethyl butyrate, butyl butyrate, propyl propionate, butyl methacrylate, dimethyl carbonate, diethyl carbonate, methyl phenyl ether, cyclopentyl methyl ether, ethylene carbonate, diphenyl ether, fluorobenzene, trifluoromethylbenzene, bistrifluoromethylbenzene, benzene, mercaptan, and the like.

[0190] Among these, at least one solvent selected from the group consisting of propyl propionate, butyl methacrylate, ethyl acetate, ethyl butyrate, and butyl butyrate can be more preferably used. A mixed solvent of two or more of these solvents may be used in combination.

[0191] The slurry of the present invention contains a sulfide-based solid electrolyte. As the sulfide-based solid electrolyte, there is no particular limitation, and a sulfide-based solid electrolyte selected from Li2S-P2S5, Li2S-P2S3, Li2S-P2S3-P2S5, Li2S-SiS2, LiI-Li2S-SiS2, LiI-Li2S-P2S5, LiI-Li2S-P2O5, LiI-Li3PO4-P2S5, LiI-Li2S-SiS2-P2S5, Li2S-SiS2-Li4SiO4, Li2S-SiS2-Li3PO4, Li3PS4-Li4GeS4, Li 3.4 P 0.6 Si 0.4 S4, Li 3.25 P 0.25 Ge 0.76 S4, Li4-xGe 1-x P x Any one of S4, etc., or a mixture of two or more thereof.

[0192] The slurry of the present invention preferably has a low water content. Specifically, it is preferably 1000 ppm or less, more preferably 500 ppm or less, and most preferably 100 ppm or less.

[0193] The slurry of the present invention can be used as a slurry for a positive electrode or a slurry for a negative electrode. It can also be used as a slurry for forming a solid electrolyte. Among these, when used as an electrode slurry, active material particles are also contained. The active material particles can be used as a positive electrode active material or a negative electrode active material. The slurry of the present invention can be more appropriately used as a slurry for a negative electrode using a negative electrode active material.

[0194] When the slurry of the present invention is used as a positive electrode slurry, a positive electrode active material is mixed into the slurry. Regarding the above-mentioned positive electrode active material, a positive electrode active material known as a positive electrode active material for a solid-state battery can be applied. It is particularly preferred to use a positive electrode active material that can absorb and release lithium ions.

[0195] Specific examples of the positive electrode active material include LiCoO2, Li(Ni,Co,Al)O2, Li 1+x Ni 1 / 3Mn 1 / 3 Co 1 / 3 O2 (x is a real number greater than 0), LiNiO2, LiMn2O4, LiCoMnO4, Li2NiMn3O8, Li3Fe2(PO4)3, Li3V2(PO4)3, 1+x Mn 2-x-y M y O4 (M is at least one metal selected from the group consisting of Al, Mg, Co, Fe, Ni, and Zn, and y is a real number greater than 0) is substituted with a heterogeneous element in the composition represented by Li-Mn spinel, lithium titanate (Li x TiO y ), lithium metal phosphate having a composition represented by LiMPO4 (M is Fe, Mn, Co or Ni), etc.

[0196] Among these, LiCoO2, Li(Ni,Co,Al)O2, LiNi 1 / 3 Mn 1 / 3 Co 1 / 3 O2 is used as the positive electrode active material. In addition, the present invention can also use the positive electrode active material coated on the surface of these materials. The coating material that can be used in the present invention is any material that has lithium ion conductivity and can maintain the form of a coating layer on the surface of the active material. Examples of the coating material include LiNbO3, Li4Ti5O 12 , Li3PO4, etc. The shape of the positive electrode active material is not particularly limited, but is preferably in powder form.

[0197] The average particle size of the positive electrode active material is preferably, for example, 1 to 50 μm, preferably 1 to 20 μm, and particularly preferably 3 to 7 μm. This is because if the average particle size of the positive electrode active material is too small, the handling property may deteriorate, and if the average particle size of the positive electrode active material is too large, it is sometimes difficult to obtain a flat positive electrode active material layer. It should be noted that the average particle size of the positive electrode active material can be obtained by measuring the particle size of the observed active material carrier using, for example, a scanning electron microscope (SEM) and averaging it.

[0198] The negative electrode active material is not particularly limited, and examples thereof include materials selected from carbonaceous materials such as artificial graphite, graphite carbon fiber, resin-fired carbon, pyrolytic vapor-grown carbon, coke, mesocarbon microbeads (MCMB), furfuryl alcohol resin-fired carbon, polyacene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, and non-graphitizable carbon, silicon-containing compounds such as silicon and silicon alloys, Li4Ti5O 12 Among them, a substance containing at least a part of a carbonaceous material or a silicon-containing compound can be particularly suitably used.

[0199] The slurry for sulfide-based solid-state batteries of the present invention may further contain a conductive aid as needed. The conductive aid used in the present invention is not particularly limited as long as it can improve the conductivity of the target sulfide-based solid-state battery positive electrode, and examples thereof include carbon black such as acetylene black and Ketjen black; carbon fibers such as multilayer carbon nanotubes, single-layer carbon nanotubes, carbon nanofibers, and vapor-grown carbon fibers (VGCF); metal powders such as SUS powder and aluminum powder, etc.

[0200] The slurry may contain materials other than the above-mentioned materials. However, when the volume of the entire slurry is taken as 100% by mass, the content of the above-mentioned materials is preferably 8% by mass or less, and more preferably 4% by mass or less.

[0201] In the process of making the slurry of the present invention, the above-mentioned components are mixed to form a slurry. The mixing order of the components is not particularly limited, and the components can be added to a solvent and mixed. However, from the perspective of obtaining a slurry in which the binder is dissolved, it is preferred to mix by the following method.

[0202] In the step of preparing the slurry, it is preferred that a binder solution is prepared by dissolving the binder in the solvent in advance, and then mixed with other materials.

[0203] In the present invention, the slurry is preferably prepared according to the following steps.

[0204] (1) The above-mentioned binder is dissolved in a solvent to obtain a "binder solution".

[0205] (2) By adding the binder solution obtained by (1) and a separately prepared sulfide-based solid electrolyte or a positive electrode active material or a negative electrode active material used as needed to a solvent and subjecting the mixture to a dispersion treatment (e.g., ultrasonic treatment), a "solid electrolyte-binder slurry" in which the sulfide-based solid electrolyte is highly dispersed in the solvent or an "active material-binder slurry" in which the active material is highly dispersed in the solvent is obtained.

[0206] (3) In the case of electrode slurry, a sulfide-based solid electrolyte or an electrode active material is added to the "active material-binder slurry" or "solid electrolyte-binder slurry" obtained by (2), and a dispersion treatment (e.g., ultrasonic treatment) is applied to obtain an "electrode slurry" in which the electrode active material and the sulfide-based solid electrolyte are highly dispersed in a solvent.

[0207] In this way, it is possible to add a binder, a sulfide-based solid electrolyte and an electrode active material used as needed in stages, and apply a successive dispersion process, and easily obtain a slurry in which each component is highly dispersed in a solvent. The addition of any component other than these (conductive aid, etc.) is also preferably added while applying a successive dispersion process.

[0208] However, a slurry can also be obtained by adding a binder, a sulfide-based solid electrolyte, an electrode active material used as required, and optional components to a solvent at once and performing a dispersion treatment at once.

[0209] It should be noted that as a method of dispersion treatment, the above-mentioned ultrasonic treatment can be cited as an example. In addition, other dispersion using a high-speed disk can also be considered.

[0210] It should be noted that the "solution" in the present invention refers to a "binder solution" in which the binder obtained in the above step (1) is dissolved in a solvent.

[0211] In the step of preparing the slurry, the mixing ratio of the binder, the sulfide-based solid electrolyte, and the electrode active material used as required may be any mixing ratio that allows the respective layers to function appropriately, and a known mixing ratio may be adopted.

[0212] It should be noted that, relative to 100 parts by mass of the total mass of the solid component in the slurry, it is particularly preferred to contain more than 0.5 parts by mass and less than 4.5 parts by mass of the above-mentioned binder. When the binder is too little, in the case of making an electrode, the adhesion between particles such as electrolytes and the adhesion between particles such as collectors and electrolytes is poor, and it is sometimes difficult to handle the electrode. On the other hand, when the binder is too much, the resistance of the electrode becomes large, and sometimes it is impossible to obtain a solid-state battery with sufficient performance.

[0213] In the process of making the slurry of the present invention, the amount of solid components (electrode active material, sulfide-based solid electrolyte and binder) relative to the solvent is not particularly limited, but it is preferred that the solid components in the slurry be 30% by mass or more and 75% by mass or less. If it is such a solid component ratio, it is easier to manufacture electrodes and solid electrolyte layers. The lower limit of the solid component ratio is more preferably 50% by mass or more, and the upper limit is more preferably 70% by mass or less.

[0214] The slurry of the present invention can be used to form a solid-state battery electrode and / or a sulfide-based solid-state battery electrolyte layer. The method for producing such a solid-state battery electrode is not particularly limited, and can be carried out by (1) preparing a substrate, (2) preparing a slurry, and (3) applying the slurry to form a sulfide-based solid-state battery electrode.

[0215] Hereinafter, the above steps (1) to (3) will be described in order.

[0216] Step (1) Step of preparing a substrate

[0217] The substrate used in the present invention is not particularly limited as long as it has a flat surface to which the slurry can be applied. The substrate may be in the form of a plate or a sheet. In addition, the substrate may be prefabricated or a commercially available product.

[0218] The substrate used in the present invention can be used in a sulfide-based solid-state battery after forming an electrode for a sulfide-based solid-state battery and / or an electrolyte layer for a sulfide-based solid-state battery, or it may not be a material for a sulfide-based solid-state battery. Examples of substrates for sulfide-based solid-state batteries include electrode materials such as current collectors, sulfide-based solid electrolyte layer materials such as sulfide-based solid electrolyte membranes, and the like. The sulfide-based solid-state battery electrode and / or the sulfide-based solid-state battery electrolyte layer obtained by using the slurry of the present invention is used as a substrate, and a sulfide-based solid-state battery electrode and / or a sulfide-based solid-state battery electrolyte layer can also be further formed here.

[0219] As a substrate that does not become a material of the sulfide-based solid-state battery, there can be mentioned, for example, a transfer substrate such as a transfer sheet and a transfer substrate. The sulfide-based solid-state battery electrode and / or the sulfide-based solid-state battery electrolyte layer formed on the transfer substrate can be formed on the sulfide-based solid-state battery electrode by bonding with the sulfide-based solid-state battery electrode and / or the sulfide-based solid-state battery electrolyte layer by thermal compression bonding or the like, and then peeling off the transfer substrate.

[0220] In addition, after the sulfide-based solid-state battery electrode active material layer formed on the transfer substrate is bonded to the current collector by thermocompression bonding or the like, the transfer substrate is peeled off to obtain a sulfide-based solid-state battery electrode having an electrode active material layer formed on the electrode current collector.

[0221] Step (2) Step of preparing slurry

[0222] This step can be carried out according to the above-mentioned method for preparing the slurry.

[0223] Step (3) Step of applying slurry to form an electrode for a sulfide-based solid-state battery

[0224] This step is a step of applying the slurry to at least one surface of the substrate to form a sulfide-based solid-state battery electrode.

[0225] The sulfide-based solid-state battery electrode may be formed on only one surface of the substrate or may be formed on both surfaces of the substrate.

[0226] The coating method and drying method of the slurry can be appropriately selected. For example, as the coating method, spraying, screen printing, scraper method, rod coating, roller coating, gravure printing, die coating, etc. can be cited. In addition, as the drying method, for example, reduced pressure drying, heating drying, reduced pressure heating drying, etc. can be cited. The specific conditions in reduced pressure drying and heating drying are not limited and can be appropriately set.

[0227] The amount of slurry applied varies depending on the composition of the slurry, the intended use of the sulfide-based solid-state battery electrode, etc., but is 5 to 30 mg / cm in a dry state. 2 The thickness of the sulfide-based solid-state battery electrode is not particularly limited, but may be about 10 to 250 μm.

[0228] The sulfide-based solid-state battery electrode of the present invention may further include a current collector and a lead wire connected to the current collector in addition to the above-mentioned active material layer.

[0229] The thickness of the active material layer used in the present invention varies depending on the intended use of the sulfide-based solid-state battery, but is preferably 10 to 250 μm, particularly preferably 20 to 200 μm, and most preferably 30 to 150 μm.

[0230] The current collector used in the present invention is not particularly limited as long as it has the function of collecting current from the active material layer.

[0231] As the material of the positive electrode collector, for example, aluminum, SUS, nickel, iron, titanium, chromium, gold, platinum, zinc, etc. can be cited, among which aluminum and SUS are preferred. In addition, as the shape of the positive electrode collector, for example, foil, plate, mesh, etc. can be cited, among which foil is preferred.

[0232] Regarding the positive electrode for a sulfide-based solid-state battery of the present invention, by setting the content ratio of the above-mentioned binder to 0.5 to 10 mass % of the positive electrode for a sulfide-based solid-state battery (preferably the electrode active material layer), excellent bonding strength is exerted, and the sulfide-based solid-state battery using the positive electrode exerts high output power.

[0233] The present invention also relates to a solid-state secondary battery, characterized in that the solid-state secondary battery comprises the above-mentioned solid-state battery electrode. The solid-state secondary battery is preferably a lithium-ion battery. The sulfide-based solid-state battery of the present invention comprises a positive electrode, a negative electrode, and a sulfide-based solid electrolyte layer between the positive electrode and the negative electrode, and the positive electrode and / or the negative electrode contain the above-mentioned binder of the present invention.

[0234] Figure 1 This is a diagram showing an example of a layered structure of the sulfide-based solid-state battery of the present invention, and schematically shows a cross section cut along the layered direction. It should be noted that the sulfide-based solid-state battery of the present invention is not necessarily limited to this example.

[0235] The sulfide-based solid-state battery includes a positive electrode 6 including a positive electrode active material layer 2 and a positive electrode current collector 4 , a negative electrode 7 including a negative electrode active material layer 3 and a negative electrode current collector 5 , and a sulfide-based solid electrolyte layer 1 sandwiched between the positive electrode 6 and the negative electrode 7 .

[0236] The positive electrode and negative electrode used in the present invention are the same as the electrodes for the sulfide-based solid-state battery described above. Hereinafter, the negative electrode and sulfide-based solid electrolyte layer used in the sulfide-based solid-state battery of the present invention, and the separator and battery case suitably used in the sulfide-based solid-state battery of the present invention are described in detail.

[0237] The negative electrode current collector used in the present invention is not particularly limited as long as it has the function of collecting current from the negative electrode active material layer.

[0238] As the material of the negative electrode current collector, for example, chromium, SUS, nickel, iron, titanium, copper, cobalt and zinc can be cited, among which copper, iron and SUS are preferred. In addition, as the shape of the negative electrode current collector, for example, foil, plate, mesh, etc. can be cited, among which foil is preferred.

[0239] Regarding the negative electrode for a sulfide-based solid-state battery of the present invention, by setting the content ratio of the above-mentioned binder to 0.5 to 10 mass % of the negative electrode for a sulfide-based solid-state battery (preferably the electrode active material layer), excellent bonding strength is exerted, and the sulfide-based solid-state battery using the negative electrode exerts high output power.

[0240] The sulfide-based solid electrolyte layer used in the present invention is not particularly limited as long as it is a layer containing the above-mentioned sulfide-based solid electrolyte. The sulfide-based solid electrolyte layer used in the present invention is preferably a layer composed of the above-mentioned sulfide-based solid electrolyte.

[0241] The sulfide-based solid-state battery of the present invention may include a separator between the positive electrode and the negative electrode. Examples of the separator include porous films such as polyethylene and polypropylene, and nonwoven fabrics such as nonwoven fabrics made of resins such as polypropylene and nonwoven fabrics made of glass fiber.

[0242] The sulfide-based solid-state battery of the present invention may further include a battery case. The shape of the battery case used in the present invention is not particularly limited as long as it can accommodate the positive electrode, negative electrode, sulfide-based solid-state battery electrolyte layer, etc., and specific examples include cylindrical, square, button-shaped, laminated, and the like.

[0243] The method for producing a sulfide-based solid-state battery of the present invention is a method for producing a sulfide-based solid-state battery having a positive electrode, a negative electrode, and an electrolyte layer for a sulfide-based solid-state battery between the positive electrode and the negative electrode, characterized in that the method comprises: a step of preparing the above-mentioned electrolyte layer for a sulfide-based solid-state battery, a step of kneading the above-mentioned positive electrode or negative electrode active material, a sulfide-based solid electrolyte, a binder, and a solvent or a dispersion medium to prepare a slurry, and a step of coating the above-mentioned slurry on one side of the above-mentioned electrolyte layer for a sulfide-based solid-state battery to form a positive electrode, and forming the above-mentioned negative electrode on the other side of the above-mentioned electrolyte layer for a sulfide-based solid-state battery, thereby producing a sulfide-based solid-state battery.

[0244] Example

[0245] Hereinafter, the present invention will be specifically described based on Examples. Unless otherwise specified in the following Examples, "part" and "%" respectively represent "part by mass" and "mass %".

[0246] (Method for producing adhesive)

[0247] (Binder 2; for example)

[0248] 1650 ml of pure water was added to a 3L stainless steel autoclave, and nitrogen was substituted. The autoclave was slightly pressurized with hexafluoropropylene (HFP), and the temperature was adjusted to 80°C while stirring at 380 rpm. HFP was pressed in until 0.23 MPa, and a mixed liquid monomer of vinylidene fluoride (VdF) and HFP with a molar ratio of 78.2 / 21.8 was further pressed in until 1.472 MPa. 2-Methylbutane was pressed in with 0.097 cc of nitrogen, and a solution of 36.4 g of ammonium persulfate dissolved in 80 ml of pure water was pressed in with nitrogen to start polymerization. When the pressure dropped to 1.44 MPa, the pressure was increased to 1.50 MPa with continuous monomer. This was repeated for about 9.3 hours, and when 607 g of continuous monomer was added, the gas in the autoclave was released, cooled, and 2299 g of dispersion was recovered. The solid content of the dispersion was 26.9 wt%. By adding magnesium chloride to the dispersion and precipitating and drying, 610 g of polymer was obtained. The obtained polymer contained HFP and VdF in a molar ratio of 22.1 / 77.9. The Mooney viscosity (ML1+10 (121°C)) of the obtained polymer was 140, and Tg was determined by DSC to be -18°C. In addition, no heat of fusion was confirmed in the second temperature increase.

[0249] (Binders 1, 3 to 6; for use in embodiments)

[0250] This substance was obtained by adjusting the polymer composition to the compositions of Binders 1 and 3 to 6 shown in Table 1 in the same manner.

[0251] (Binder 7; for comparative example)

[0252] As the adhesive 7, KF7200 (manufactured by KUREHA) was used.

[0253] (Binder 10; for comparative example)

[0254] Into a 3 L stainless steel autoclave were added 1716 ml of pure water, 0.3432 g of a 50% aqueous solution of CH2=CFCF2OCF(CF3)CF2OCF(CF3)COONH4, and C5F 113.421g of 50% aqueous solution of COONH4 was replaced with nitrogen, slightly pressurized with HFP, and the temperature was adjusted to 80°C while stirring at 560rpm. HFP was pressed in until 0.56MPa, VdF was pressed in until 0.69MPa, and a mixed liquid monomer of VdF, TFE and HFP with a molar ratio of 70.2 / 11.3 / 18.5 was further pressed in until 2.000MPa. A solution of 0.0218g of ammonium persulfate dissolved in 4ml of pure water was pressed in with nitrogen and polymerization was started. When the continuous monomer reached 12g, 2.5022g of 1,4-diiodoperfluorobutane was added. When the pressure dropped to 1.97MPa, the pressure was increased to 2.03MPa with continuous monomer. After repeating this process for about 5.0 hours, when 572g of continuous monomer was added, the gas in the autoclave was released, cooled and 2302g of dispersion was recovered. The solid content of the dispersion was 23.5 wt %. Aluminum sulfate was added to the dispersion and precipitated and dried to obtain 571 g of a polymer. The obtained polymer contained VdF, TFE and HFP in a molar ratio of 69.9 / 11.2 / 18.9. The Mooney viscosity (ML1+10 (121° C.)) of the obtained polymer was 48, and Tg was determined to be -20° C. by DSC. In addition, no heat of fusion was confirmed in the second temperature rise.

[0255] (Binder 8; for comparative example)

[0256] This material was obtained by adjusting the polymer composition in the same manner so as to have the composition of the binder 8 shown in Table 1.

[0257] (Binder 9; for comparative example)

[0258] Into a 3L stainless steel autoclave, add 1.7L of pure water, 0.17g of a 50% aqueous solution of CH2=CFCF2OCF(CF3)CF2OCF(CF3)COONH4, and 6.8g of a 50% aqueous solution of F(CF2)5COONH4, and fully replace the reaction system with nitrogen. After heating to 80°C while stirring at 600rpm, the monomers are pressed in such a way that the initial monomer composition in the tank is VdF / HFP=45 / 55 (molar ratio) and 1.52MPa. Then, a polymerization initiator solution prepared by dissolving 60mg of ammonium persulfate (APS) in 5ml of pure water is pressed in with nitrogen to start the reaction. As the polymerization proceeds, when the internal pressure drops to 1.42MPa, additional mixed monomers with VdF / HFP=78 / 22 (molar ratio) are pressed in until the internal pressure reaches 1.52MPa. At this time, 2.15g of the diiodide compound I(CF2)4I are pressed in. The pressure was repeatedly increased and decreased, and at the same time, a polymerization initiator solution prepared by dissolving 60 mg of APS in 5 ml of pure water was injected with nitrogen every 3 hours to continue the polymerization reaction. When 600 g of mixed monomers were added, the unreacted monomers were discharged, and the autoclave was cooled to obtain 2364 g of a fluororubber dispersion with a solid content concentration of 25.8% by mass. The polymerization time was 7.1 hours. The copolymer composition of the fluororubber was investigated by NMR analysis, and it was found that VdF / HFP=78 / 22 (molar ratio) and the Mooney viscosity (ML1+10 (121°C)) was 35.

[0259] Table 1 shows the binders used in Examples and Comparative Examples.

[0260] [Table 1]

[0261]

[0262] (Preparation of Binder Solution)

[0263] The binder was placed in a vacuum dryer and vacuum dried at 50°C for 12 hours. The binder was then added to the solvent, stirred overnight, and then ultrasonically treated 3 times (90 seconds) with an ultrasonic homogenizer to prepare a binder solution. Here, when the binder solution as a whole is set to 100% by mass, the binder is contained at 5% by mass. The composition of the binder used in the examples is shown in Table 1. In addition, the combination of the binder and the solvent is shown in Tables 2 and 3.

[0264] (Examples 1 to 8, Comparative Examples 1 to 5)

[0265] In the present invention, the positive electrode, negative electrode slurry and solid electrolyte layer are prepared according to the following steps.

[0266] (Preparation of negative electrode slurry)

[0267] The prepared binder solution was used to prepare negative electrode slurries of Examples and Comparative Examples. The details are as follows.

[0268] The above-mentioned binder solution, graphite as a negative electrode active material, and the solvent contained in the binder solution are added to a PET container, and ultrasonic treatment (50 seconds) is performed once with an ultrasonic homogenizer to prepare a "negative electrode active material-binder slurry". The binder solution, solvent and sulfide-based solid electrolyte (30LiI·70 (0.75Li2S·0.25P2S5)) are further added to the obtained negative electrode active material-binder slurry, and ultrasonic treatment (30 seconds) is performed 3 times with an ultrasonic homogenizer to obtain a "negative electrode slurry" in which the negative electrode active material, sulfide-based solid electrolyte and binder are highly dispersed. The concentration of the binder solid component in the final slurry is 3.0% by mass.

[0269] (Production of negative electrode)

[0270] Each negative electrode slurry was applied onto a copper foil as a negative electrode current collector using a doctor blade and dried to obtain a negative electrode having a negative electrode layer having a thickness of 110 μm formed on the surface of the negative electrode current collector.

[0271] Table 2 shows the evaluation results of the negative electrode.

[0272] (Production of positive electrode)

[0273] Butyl butyrate was used as a solvent and Li(NiMnCo) was used as a ternary active material for the positive electrode. 1 / 3O2, the above-mentioned sulfide-based solid electrolyte as a solid electrolyte, and the above-mentioned binder solution as a binder, and the binder solid content concentration in the slurry is adjusted to 5% by mass to obtain a positive electrode slurry. The prepared positive electrode slurry is applied to an aluminum foil as a positive electrode collector with a scraper and dried to obtain a positive electrode having a positive electrode layer with a thickness of 85 μm formed on the surface of the positive electrode collector.

[0274] Table 3 shows the evaluation results of the positive electrode.

[0275] (Fabrication of Solid Electrolyte Sheet)

[0276] An electrolyte slurry is prepared using butyl butyrate as a solvent, the above-mentioned sulfide-based solid electrolyte as a solid electrolyte, and a binder solution containing a binder (3) or a binder (9) as a binder. The prepared electrolyte slurry is applied to a peelable substrate (PTFE sheet) with a scraper and dried to form a solid electrolyte sheet with a thickness of 45 μm on the substrate. The mass ratio of the solid electrolyte to the binder in the solid electrolyte sheet is solid electrolyte: binder = 100 parts by mass: 1 part by mass.

[0277] The preparation of the solid electrolyte slurry is as follows. That is, the solid electrolyte and the binder solution are added to butyl butyrate as a solvent, and ultrasonic treatment (30 seconds) is performed once with an ultrasonic homogenizer to obtain an electrolyte slurry in which the solid electrolyte and the binder are highly dissolved or dispersed. It should be noted that the solid content at this time is 49%.

[0278] [Table 2]

[0279]

[0280] [Table 3]

[0281]

[0282] The obtained slurry was evaluated based on the following criteria. The results are shown in Tables 1 to 3.

[0283] The evaluation method is as follows.

[0284] (Polar terminal group amount)

[0285] By performing composition analysis using NMR using the above method, the ratio of ([-CH2OH]+[-COOH]) / ([-CH3]+[-CF2H]+[-CH2OH]+[-CH2I]+[-OC(O)RH]+[-COOH]) was calculated.

[0286] (Glass transition temperature)

[0287] According to ASTM E1356-98, a DSC measuring device manufactured by METLER TOLEDO was used to determine the glass transition temperature from the heat absorption in the second heating by the midpoint method. The results are shown in Table 1. In addition, the presence or absence of a crystalline melting point in the second heating was confirmed. Those without a crystalline melting point in the second heating were judged to be "amorphous".

[0288] Measurement conditions

[0289] Heating rate: 20℃ / min

[0290] Sample volume: 10mg

[0291] Thermal cycle: -100℃~220℃, heating, cooling, heating

[0292] <Evaluation Results of Solvent and Electrolyte Solubility>

[0293] As shown in Table 2, when propyl propionate or butyl butyrate was used as the solvent, the binder was dissolved while suppressing the reaction between the solvent and the sulfide-based solid electrolyte. On the other hand, in Comparative Examples 1 and 2, the binder was not dissolved, and a uniform slurry could not be prepared.

[0294] <Flexibility (Electrode Bending Test)>

[0295] The prepared electrode was cut into pieces of 3 cm in length and 6 cm in width, and then rolled using a roller press at 10 tons. After folding 180 degrees, it was unfolded and visually checked for cracks. The case where no cracks were found was evaluated as ○, and the case where cracks were found was evaluated as ×.

[0296] (Long-term reliability)

[0297] The prepared electrolyte sheet was placed in a sample bottle and sealed. The sample was opened in a chamber pre-adjusted to 50% RH, and deterioration was promoted by exposure to moisture in the air in the chamber. After 1 hour, the sample was taken out and the state was observed. In addition, for the solid electrolyte, the AC impedance was measured at a frequency of 10 MHz to 0.01 Hz using an impedance analyzer (manufactured by Solartron: SI-1260), and the conductivity was calculated based on the measurement results. The conductivity of the sample using the binder (3) before exposure was 4×10 -4 S / cm.

[0298] <Adhesion strength (90 degree peel test of electrode / current collector interface)>

[0299] The electrode side of the positive or negative electrode cut into 1.2×8.0cm is fixed to a movable clamp, and a tape is attached to the collector side. The stress (N / mm) of the tape side when the tape is stretched 90 degrees at a speed of 100mm / min is measured by Autograph. The force sensor of Autograph uses 1N. The result of Comparative Example 4 is taken as 100 for relative comparison. In Example 8 using the positive electrode active material, relative evaluation is performed with Comparative Example 5 as 100. In Comparative Examples 1 and 2, the binder is insoluble in butyl butyrate, and it is difficult to make electrodes, so the adhesion and flexibility cannot be evaluated.

[0300] From the results in Tables 2 and 3, it can be seen that the adhesives of the examples all have superior adhesion than conventional adhesives.

[0301] In addition, the results of long-term reliability showed that the sample using adhesive (3) also maintained its shape after exposure, while the sample using adhesive (9) became brittle and difficult to remove with tweezers. In addition, the conductivity of the sample using adhesive (3) after exposure was 4×10 -5 S / cm.

[0302] In addition, the case of using a binder satisfying 0.01≤([-CH2OH]+[-COOH]) / ([-CH3]+[-CF2H]+[-CH2OH]+[-CH2I]+[-OC(O)RH]+[-COOH])≤0.25 is a binder with excellent flexibility compared to the case of a binder outside the range. It can be seen from this that in the case of an application that particularly requires flexibility, it is preferable to use a binder that satisfies the above parameters.

[0303] Industrial Applicability

[0304] The binder of the present invention can be used as a binder for a slurry for a solid-state battery.

[0305] Explanation of symbols

[0306] 1 Sulfide-based solid electrolyte layer

[0307] 2 Positive electrode active material layer

[0308] 3 Negative electrode active material layer

[0309] 4. Positive electrode collector

[0310] 5 Negative electrode collector

[0311] 6 Positive electrode

[0312] 7 Negative electrode

Claims

1. A binder used in a slurry for a solid-state battery containing sulfide-based solid electrolyte particles, characterized in that: The binder contains a fluorinated elastomer whose resin terminal functional groups satisfy the following formula: 0.01≤([-CH2OH]+[-COOH]) / ([-CH3]+[-CF2H]+[-CH2OH]+[-CH2I]+[-OC(O)RH]+[-COOH])≤0.25 In the formula, R represents an alkyl group having 1 to 20 carbon atoms, [] represents the amount of the functional group, Fluoroelastomers are composed of vinylidene fluoride (VdF) monomer units and copolymer units. The copolymerized unit of the fluorine-containing elastomer is at least one copolymerized unit selected from the group consisting of hexafluoropropylene (HFP), tetrafluoroethylene (TFE), 2,3,3,3-tetrafluoropropylene, 1,3,3,3-tetrafluoropropylene, and perfluoroalkyl vinyl ether (PAVE).

2. The adhesive according to claim 1, wherein At least a portion of the copolymerized units of the fluorine-containing elastomer is hexafluoropropylene (HFP).

3. The adhesive according to claim 1 or 2, wherein The fluorine content is 60% to 71% by mass.

4. The adhesive according to claim 1 or 2, wherein The glass transition temperature is 25°C or lower.

5. A solution used in a slurry for a solid-state battery containing sulfide-based solid electrolyte particles, characterized in that: The solution contains a binder and a solvent, and the binder is the binder according to any one of claims 1 to 4.

6. A slurry for a solid-state battery, comprising sulfide-based solid electrolyte particles, a binder and a solvent, characterized in that: The binder is the binder according to any one of claims 1 to 4.

7. The slurry for solid-state battery according to claim 6, wherein: The solvent is a low polarity solvent.

8. The slurry for solid-state battery according to claim 6 or 7, wherein: The solvent contains at least one compound selected from the group consisting of aromatic compounds and ester compounds.

9. The slurry for solid-state battery according to claim 6 or 7, wherein: The solid-state battery slurry further contains active material particles.

10. The slurry for solid-state battery according to claim 9, wherein: The active material particles are negative electrode active materials. 11 . An electrode for a solid-state battery, comprising an electrode active material layer formed from the slurry according to claim 9 or 10, and a current collector.

12. The solid-state battery electrode according to claim 11, wherein: The electrode for the solid-state battery is the negative electrode.

13. The solid-state battery electrode according to claim 12, wherein: At least a part of the electrode active material includes a carbonaceous material.

14. The solid-state battery electrode according to claim 12, wherein: At least a portion of the electrode active material contains a silicon-containing compound.