Semiconductor equipment sealing component and manufacturing method thereof

By adopting physical bonding methods in semiconductor equipment sealing components and utilizing the recessed structure to fill the elastomer and the base material, the problem of sealing failure caused by the decomposition of the adhesive is solved and the sealing performance and cost-effectiveness are improved.

CN114274624BActive Publication Date: 2024-10-22IC SEAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111613819.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-27
Publication Date
2024-10-22
Estimated Expiration
2041-12-27

AI Technical Summary

Technical Problem

Existing semiconductor equipment sealing components fail due to high-temperature decomposition of the adhesive in harsh environments, resulting in delamination of the elastomer and the base material, which increases the development cycle and cost.

Method used

The elastomer and the base material are physically bonded, and multiple recesses are formed on the surface of the base material and filled with the elastomer, and vulcanized to form a sealed component, thereby reducing delamination and cost.

Benefits of technology

The mechanical strength and performance of the sealing component are improved, the process is simplified, the production cycle is shortened, the cost is reduced, and the sealing effect is maintained in harsh environments such as high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114274624B_ABST
    Figure CN114274624B_ABST
Patent Text Reader

Abstract

The present invention discloses a semiconductor device sealing component and a manufacturing method thereof, wherein the manufacturing method comprises: providing a substrate; forming a plurality of recesses on the surface of the substrate, wherein the plurality of recesses are mutually interlocked; arranging an elastomer in the recesses, wherein the elastomer fills and covers the recesses; and vulcanizing the elastomer to form a semiconductor device sealing component. The semiconductor device sealing component and the manufacturing method thereof provided by the present invention can improve the performance of the semiconductor device sealing component and reduce the manufacturing cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor equipment, and in particular to a semiconductor equipment sealing component and a manufacturing method thereof. Background Art

[0002] The sealing performance of semiconductor equipment directly affects the yield rate of semiconductor device manufacturing. Semiconductor equipment includes sealing components that use adhesives to composite elastomers and substrates, but the adhesive components will decompose at high temperatures in harsh operating environments, causing the elastomer and substrate to be stratified or even completely separated, causing the sealing components to fail, affecting the sealing performance of the equipment, and causing the semiconductor device to be scrapped. On the other hand, each elastomer is chemically bonded to different substrates, and it is necessary to develop an appropriate adhesive, which increases the project development cycle and experimental costs.

[0003] Therefore, how to obtain a sealing component with good sealing performance and low cost has become an urgent problem to be solved. Summary of the invention

[0004] In view of the above-mentioned shortcomings of the prior art, the purpose of the present invention is to provide a semiconductor device sealing component and a manufacturing method thereof, which adopts a physical method to bond the elastomer and the substrate, improves the delamination phenomenon, shortens the manufacturing cycle, and saves costs.

[0005] To achieve the above-mentioned purpose and other related purposes, the present invention adopts the following technical solutions:

[0006] A method for manufacturing a semiconductor device sealing component is provided, comprising:

[0007] providing a substrate;

[0008] A plurality of recesses are formed on the surface of the substrate, and the plurality of recesses are interlocked with each other;

[0009] An elastomer is arranged in the recess, and the elastomer fills and covers the recess; and the elastomer is vulcanized to form a semiconductor device sealing component.

[0010] In some embodiments of the present invention, the recess is at least one of circular, rectangular, elliptical, polygonal or linear.

[0011] In some embodiments of the present invention, the depth of the recess is 0.2 to 3 mm.

[0012] In some embodiments of the present invention, the substrate comprises a metal substrate, and the metal substrate comprises at least one of a magnesium substrate, a titanium substrate, an aluminum substrate, a copper substrate, a chromium substrate, an alloy substrate or a stainless steel substrate.

[0013] In some embodiments of the present invention, after the recess is formed, the metal substrate is subjected to anodization to form a porous anodic oxide on the surface of the metal substrate.

[0014] In some embodiments of the present invention, the substrate includes a polymer substrate, and the polymer substrate includes at least one of a polyetheretherketone substrate, a polytetrafluoroethylene substrate, a polyphenylene ether substrate, a polyimide substrate, a poly-4-methylpentene substrate, a polyetherketone substrate, a polyamide substrate or a composite material substrate.

[0015] In some embodiments of the present invention, after the recess is formed, the polymer substrate is subjected to a corona surface treatment.

[0016] In some embodiments of the present invention, the surface roughness of the polymer substrate is 5 to 100 μm.

[0017] In some embodiments of the present invention, after the elastomer is vulcanized once, it is physically bonded to the recess to form the semiconductor device sealing component.

[0018] Another object of the present invention is to provide a semiconductor device sealing assembly, comprising:

[0019] A substrate, wherein a surface of the substrate is provided with a plurality of recesses that fit into each other; and

[0020] An elastic body fills and covers the recess.

[0021] The present invention provides a semiconductor device sealing component and a manufacturing method thereof. The elastomer and the substrate are firmly bonded, the prepared semiconductor device sealing component has high mechanical strength, reduces delamination, and does not use chemical adhesives. The bonding method is simple, the process is less, the cycle is short, energy consumption is saved, and the cost is reduced. In summary, the semiconductor device sealing component and the manufacturing method thereof provided by the present invention can improve the performance of the sealing component and reduce the cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 Schematic diagram of the structure of a semiconductor device sealing component in one embodiment.

[0023] Figure 2 FIG. 1 is a schematic diagram of a substrate and a recessed portion structure in one embodiment.

[0024] Figure 3 FIG. 1 is a schematic diagram of a substrate and a recessed portion structure in one embodiment.

[0025] Figure 4 FIG. 1 is a schematic diagram of a substrate and a recessed portion structure in one embodiment.

[0026] Figure 5 FIG. 1 is a schematic diagram of a substrate and a recessed portion structure in one embodiment.

[0027] Figure 6 FIG. 1 is a schematic diagram of a substrate and a recessed portion structure in one embodiment.

[0028] Figure 7 FIG. 1 is a schematic diagram of a substrate and a recessed portion structure in one embodiment.

[0029] Figure 8 Schematic diagram of the internal failure of an elastic body in one embodiment.

[0030] Fig. 9 This is a schematic diagram of testing the delamination after the elastomer and the substrate are directly pressed together in one embodiment.

[0031] Fig.10 This is a schematic diagram of testing the delamination of an elastomer and a substrate after compounding them with an adhesive in one embodiment.

[0032] Description of labels:

[0033] 1 substrate; 2 elastomer; 3 recess; 4 adhesive. DETAILED DESCRIPTION

[0034] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0035] It should be understood that the present invention can be implemented in different forms and should not be construed as being limited to the embodiments set forth herein. On the contrary, providing these embodiments will make the disclosure thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. Unless otherwise specified, the "%" and "parts" shown in the following examples refer to "mass %" and "parts" respectively.

[0036] The present invention provides a semiconductor sealing component and a method for manufacturing the same. The substrate is processed to obtain a roughened surface including a plurality of recesses. An elastomer is filled into the recesses and covers the surface of the substrate through an external force to form a sealing component. In the formed sealing component, the substrate and the elastomer are physically bonded and firmly combined. The elastomer is not easy to delaminate and fall off, and has good mechanical and chemical properties. The sealing component does not contain adhesives, and the seal will not fail due to the failure of the adhesive. It can be widely used in semiconductor sealing components in semiconductor equipment, such as etching, cleaning and coating processes, and can also be used in transportation, metallurgy, electricity, electronic instruments and parts sealing and other industries.

[0037] See also Figure 1 As shown, in one embodiment of the present invention, the surface of the substrate 1 is roughened to form a plurality of recesses 3. The present invention does not limit the material of the substrate 1, and it can be selected according to the usage scenario. For example, the substrate 1 can be a metal substrate or a polymer substrate, wherein the metal substrate includes but is not limited to at least one of a magnesium substrate, a titanium substrate, an aluminum substrate, a copper substrate, a chromium substrate, an alloy substrate or a stainless steel substrate, and the polymer substrate includes but is not limited to at least one of a polyetheretherketone (PEEK) substrate, a polytetrafluoroethylene (PTFE) substrate, a polyphenylene ether (PPO) substrate, a polyimide (PI) substrate, a poly-4-methylpentene (TPX) substrate, a polyetherketone (PEK) substrate, a polyamide (PA) substrate or a composite material.

[0038] See also Figure 1 As shown, in one embodiment of the present invention, the recess 3 on the surface of the substrate 1 is a plurality of three-dimensional hollow lines formed on the surface of the substrate 1, and the recess 3 is prepared by an integrated molding process, wherein the metal substrate is prepared by, for example, Computer Numerical Control (CNC) integrated molding, and the polymer substrate is prepared by, for example, 3D printing integrated molding. The recess 3 is prepared by an integrated molding process, which is beneficial for the substrate 1 to maintain high strength. The multiple recesses 3 on the substrate 1, that is, the multiple three-dimensional hollow lines are interlocked with each other, which can improve the bonding force between the substrate 1 and the elastomer 2. The present invention does not limit the shape of the recess 3, for example, it can be at least one of a circle, a square, a polygon or a curve, that is, the morphology of the three-dimensional hollow lines can be flexibly selected. In other embodiments, other molding methods can be selected according to the production requirements to form recesses 3 of other shapes.

[0039] See also Figure 1 As shown, in one embodiment of the present invention, the depth of the recess 3, i.e., the hollowed-out portion, on the surface of the substrate 1 is, for example, 0.2 to 3.0 mm, and the thickness of the untreated bottom of the substrate 1 is determined according to the size of the sealing component, for example, greater than 0.5 mm. After the recess 3 is formed, the substrate 1 is further treated to increase the roughness of the surface of the substrate 1, wherein the metal substrate is, for example, anodized to form a porous anodic oxide on its surface, and the polymer substrate is, for example, corona surface treated to increase its roughness. In this embodiment, the average roughness of the surface of the polymer substrate is, for example, 5 to 100 μm, and for example, 10 to 100 μm, wherein the average roughness is measured using a laser microscope. In other embodiments, the depth of the recess 3 and the thickness of the untreated substrate 1 can be changed according to the usage scenario of the sealing component.

[0040] See also Figure 1As shown, in one embodiment of the present invention, elastomer 2 is selected from fluorine-containing elastomers, and the fluorine-containing elastomer composition is selected from unvulcanized elastomers, including but not limited to perfluoroether elastomers, tetrafluoropropylene elastomers, tetrafluoroethylene / propylene / vinylidene fluoride type fluorine-containing elastomers, ethylene / hexafluoropropylene type fluorine-containing elastomers, ethylene / hexafluoropropylene / vinylidene fluoride type fluorine-containing elastomers, ethylene / hexafluoropropylene / tetrafluoroethylene type fluorine-containing elastomers, fluoropolysilicone type fluorine-containing elastomers, fluoroaphosphazene type fluorine-containing elastomers, etc. One or a combination thereof. In other embodiments, elastomer 2 can also be selected according to the usage scenario. A cross-linking agent is added to elastomer 2, and the cross-linking agent content is at least 1 part, and the cross-linking agent includes but is not limited to one or a combination of peroxide cross-linking agents, polyol cross-linking agents, polyamine cross-linking agents, triazine cross-linking agents, oxazole cross-linking agents, imidazole cross-linking agents or thiazole cross-linking agents, etc. By adding a crosslinking agent, the functional groups in the crosslinking agent and the crosslinking points in the elastomer 2 undergo addition, cyclization and other reactions under certain temperature and pressure, thereby causing the molecular chains in the elastomer 2 to crosslink from a linear structure to a network structure, giving the sealing component product high elasticity.

[0041] See also Figure 1 As shown, in one embodiment of the present invention, a variety of additives are added to the elastomer 2, such as anti-aging agents, antioxidants, vulcanization accelerators, tackifiers, silane coupling agents, plasticizers and flame retardants. The addition of various additives helps to improve the performance of the sealing component. In this embodiment, a release agent is also added to the elastomer 2, such as octadecylamine. By adding a release agent, when the elastomer 2 is combined with the substrate 1, it is beneficial to demold the elastomer 2 and the metal mold, prevent the part of the elastomer 2 in contact with the mold from adhering to the mold, causing defects such as the breakage of the preformed seal at the moment of the press vulcanization mold opening process, and at the same time, it is beneficial to regulate the processing performance of the elastomer 2.

[0042] See also Figure 1 As shown, in one embodiment of the present invention, the elastomer 2 is arranged on one side of the concave portion 3 of the substrate 1. By physical methods, the elastomer 2 is filled in the concave portion 3, which can improve the mechanical strength of the sealing component and increase the physical adhesion between the elastomer 2 and the substrate 1. In this embodiment, the elastomer 2 and the substrate 1 are molded to prepare the sealing component, and before the molding, the elastomer 2 passes through a plunger extruder to remove the gas in the rubber material. At the same time, the molecular segments in the rubber strip are arranged in a long-range order along the flow field direction, which is beneficial to improve the dimensional stability of the molding stage and the mechanical properties of the rubber material along the flow field direction. The extrusion temperature of the elastomer 2 is, for example, 60 to 100°C, and the speed of rubber extrusion is, for example, 10 to 70 mm / s. At this temperature and extrusion speed, the gas in the rubber material can be completely removed. The surface of the extruded rubber material is smooth, which is beneficial to the size control of the cross section of the product during the molding process.

[0043] See also Figure 1 As shown, in one embodiment of the present invention, the elastomer 2 is vulcanized once in a press, and a sealing component product is prepared by lamination. In this embodiment, the vulcanization is performed once in a press, and the temperature of the vulcanization is, for example, 150 to 200°C, the pressure of the vulcanization is, for example, 5 to 20 MPa, and the vulcanization time is, for example, 3 to 20 minutes. After the vulcanization is performed once at this temperature, time and pressure, the preformed product maintains a high degree of crosslinking, which can improve the mechanical properties of the product while taking into account the production efficiency.

[0044] See also Figure 1 As shown, in one embodiment of the present invention, during the molding process of the sealing component, the substrate 1 is placed between the upper and lower molds, and the bottom of the substrate 1 is fixed to prevent the substrate 1 from shaking between the upper and lower molds during the molding process. The fixing method of the substrate 1 includes providing a positioning pin at the bottom of the substrate 1 or designing a mold cavity for placing the substrate 1 in the lower mold. By fixing the substrate 1, it is beneficial to the close adhesion of the elastomer 2 and the substrate 1 during the molding process, and the yield rate of the sealing component is improved. Among them, when the substrate 1 is a metal material, the substrate 1 is placed between the upper and lower molds and can be preheated, and the preheating time is, for example, greater than 30s, to ensure that the temperature of the metal substrate and the upper and lower molds is consistent, to ensure that the elastomer 2 reaches 90% of the crosslinking degree during the primary vulcanization process, and to improve the physical and mechanical properties of the elastomer 2. When the substrate 1 is a polymer substrate, during the lamination process of the polymer substrate, since the thermal expansion coefficient of plastics such as polyetheretherketone, polytetrafluoroethylene or poly-4-methylpentene is greater than that of the mold metal, no preheating treatment is performed. Since most plastic substrates are thermoplastic, when the mold temperature is close to the melting point, the polymer substrate will soften. Therefore, during the compression molding process, the primary vulcanization temperature is lower than the melting point of the polymer substrate, and the primary vulcanization temperature is at least 30°C lower than the melting point of the polymer substrate. By setting the primary vulcanization temperature lower than the melting point of the polymer substrate, the strength of the substrate 1 is ensured.

[0045] See also Figure 1As shown, in one embodiment of the present invention, the total thickness of the elastomer 2 is greater than the maximum thickness of the recess 3, that is, the elastomer 2 completely fills the three-dimensional hollow substrate part and covers the surface of the substrate 1, and the total thickness of the elastomer 2 after compression molding is, for example, greater than 30% or more of the maximum thickness of the recess 3. In other embodiments, the thickness of the elastomer 2 can be flexibly selected according to the manufacturing requirements. After the sealing component is compression molded, the elastomer 2 is subjected to secondary vulcanization, and the temperature of the secondary vulcanization is, for example, 210 to 280°C, and the time of the secondary vulcanization is, for example, 4 to 30 hours. After the vulcanization is completed, the mechanical properties of the sealing component are tested, and the mechanical properties test of the sealing component is carried out in accordance with the test standard of the rubber performance test standard test method-bonding strength test with a rigid substrate (ASTM D429-14). In the present invention, the bonding of the elastomer 2 and the substrate 1 is completely physical cross-linked, which is environmentally friendly and safe, with fewer processes, and can improve production efficiency. In addition, during the use of the sealing component, there is no stratification between the elastomer 2 and the metal or polymer substrate, and it can be suitable for sealing high temperature, corrosive, ultraviolet, plasma or vacuum chambers.

[0046] See also Figure 2 As shown, in one embodiment of the present invention, the substrate 1 is a polytetramethylpentene substrate, and the concave portion 3 is processed by 3D printing. The total thickness of the substrate 1 is, for example, 5 mm, the minimum depth of the three-dimensional hollow pattern is, for example, 0.3 mm, the maximum depth is, for example, 2 mm, and the total thickness of the elastomer is, for example, 3 mm. After the processing of the concave portion 3 of the substrate 1 is completed, the processed substrate 1 is subjected to corona treatment to ensure that the average roughness of the surface of the polytetramethylpentene substrate is, for example, 15 um. Add, for example, 2 parts of a cross-linking agent of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and, for example, 0.3 parts of an antioxidant GA550 to the elastomer raw rubber, mix well, and extrude into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 70°C, and the extrusion rate is, for example, 50 mm / s. The extruded rubber strip is vulcanized once in a press at, for example, a temperature of 150°C, a pressure of 10 MPa, and a time of 15 min, and then laminated to prepare a sealing component product. The sealing component is then subjected to secondary curing at a temperature of, for example, 210°C for a time of, for example, 24 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, for example, a 180° peel test of the elastomer at 150°C is performed. In the sealing component, the elastomer is internally damaged but no delamination occurs. Figure 8 As shown, it indicates that the bonding between the elastomer and the substrate 1 is good, the elastomer is embedded in the recess 3 on the substrate 1, and the mechanical properties of the prepared sealing component are good.

[0047] See also Fig. 9As shown, in one embodiment of the present invention, the substrate 1 is a polytetramethylpentene substrate, and the polytetramethylpentene substrate is not surface treated. A cross-linking agent such as 2 parts of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane and an antioxidant such as 0.3 parts of GA550 are added to the elastomer raw rubber, mixed evenly, and then extruded into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 70°C, and the extrusion rate is, for example, 50mm / s. The extruded rubber strip is vulcanized in a press at a temperature of 150°C, a pressure of 10MPa, and a time of 15min, and then laminated to prepare a sealing component product. The sealing component product is then subjected to a secondary vulcanization time of, for example, 24h at a temperature of, for example, 210°C, and the sealing component is prepared. The mechanical properties of the sealing assembly were tested, for example, a 180° peel test was performed on the elastomer 2 at 150°C. In the sealing assembly, the elastomer 2 and the substrate 1 were delaminated, indicating that the adhesion between the elastomer 2 and the substrate 1 was poor, and further indicating that the adhesion between the elastomer and the substrate can be increased by the recess.

[0048] See also Figure 2 As shown, in one embodiment of the present invention, the substrate 1 is a metal aluminum-chromium alloy substrate, and the concave portion 3 is processed by CNC, wherein the total thickness of the substrate 1 is, for example, 8 mm, the minimum depth of the three-dimensional hollow pattern is, for example, 0.7 mm, the maximum depth is, for example, 3 mm, and the total thickness of the elastomer is, for example, 4.5 mm. After the processing of the concave portion 3 of the substrate 1 is completed, the processed substrate 1 is anodized. For example, 1.5 parts of diisopropylbenzene hydroperoxide crosslinking agent and 0.3 parts of silane coupling agent vinyl tris (2-methoxyethoxy) silane are added to the elastomer raw rubber, mixed evenly, and then extruded into a specific shape of rubber strip in a plunger extruder. Among them, the extrusion temperature is, for example, 80°C, the extrusion rate is, for example, 35 mm / s, and before extruding the rubber strip, the substrate 1 is preheated for, for example, 60 seconds. The extruded rubber strip is vulcanized in a press at, for example, a temperature of 170°C, a pressure of 20 MPa, and a time of 20 minutes, and then laminated to prepare a sealing component product. The sealing component is then subjected to secondary curing at a temperature of, for example, 230°C for a time of, for example, 28 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, for example, a 180° peeling test of the elastomer at 150°C is performed. In the sealing component, the elastomer is internally damaged and no delamination occurs, indicating that the elastomer and the substrate 1 are well bonded, the elastomer is embedded in the recess 3 on the substrate 1, and different substrates and recesses can be well physically bonded to the elastomer.

[0049] See also Figure 2As shown, in one embodiment of the present invention, the substrate 1 is a metal aluminum substrate, and the concave portion 3 is processed by CNC, wherein the total thickness of the substrate 1 is, for example, 8 mm, the minimum depth of the three-dimensional hollow pattern is, for example, 1.5 mm, the maximum depth is, for example, 3 mm, and the total thickness of the elastomer is, for example, 5 mm. After the processing of the concave portion 3 of the substrate 1 is completed, the processed substrate 1 is anodized. For example, 1.5 parts of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane crosslinking agent and, for example, 0.2 parts of antioxidant 3,5-di-tert-butyl-4-hydroxyphenylpropionic acid isooctyl ester are added to the elastomer raw rubber, mixed evenly, and extruded into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 80°C, the extrusion rate is, for example, 60 mm / s, and before extruding the rubber strip, the substrate 1 is preheated for, for example, 45 seconds. The extruded rubber strip is vulcanized once in a press at a temperature of 170°C, a pressure of 15 MPa and a time of 15 minutes, and then laminated to prepare a sealing component product. The sealing component product is then subjected to a secondary vulcanization at a temperature of, for example, 250°C for a time of, for example, 15 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, such as a 180° peel test of the elastomer at 150°C. In the sealing component, the elastomer has internal damage and no delamination, indicating that the adhesion between the elastomer and the substrate 1 is good, the elastomer is embedded in the recess 3 on the substrate 1, and the type of the elastomer and the substrate 1 and the depth of the recess 3 do not affect the embedding of the elastomer and the substrate 1.

[0050] See also Figure 3As shown, in one embodiment of the present invention, the substrate 1 is a polyetheretherketone substrate, and the concave portion 3 is processed by 3D printing, wherein the total thickness of the substrate 1 is, for example, 3mm, the minimum depth of the three-dimensional hollow pattern is, for example, 0.2mm, the maximum depth is, for example, 1mm, and the total thickness of the elastomer is, for example, 4mm. After the processing of the concave portion 3 of the substrate 1 is completed, the processed substrate 1 is subjected to corona treatment to ensure that the average roughness of the surface of the polyetheretherketone substrate is, for example, 10um. For example, 1 part of methyltrimethoxysilane and, for example, 0.5 parts of N,N-methylenebisacrylamide as a crosslinking agent, and, for example, 0.2 parts of a plasticizer phthalate are added to the elastomer raw rubber, mixed evenly, and extruded into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 75°C, and the extrusion rate is, for example, 60mm / s. The extruded rubber strip is vulcanized once in a press at, for example, a temperature of 160°C, a pressure of 15MPa, and a time of 15min, and then laminated to prepare a sealing component product. The sealing component is then subjected to secondary vulcanization at a temperature of, for example, 230°C for a time of, for example, 20 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, and a 180° peeling test is performed on the elastomer at 150°C. In the sealing component, the elastomer is internally damaged and does not delaminate, indicating that the elastomer and the substrate 1 are well bonded, and the elastomer is embedded in the recess 3 on the substrate 1, and the morphology of the recess does not affect the physical bonding between the elastomer and the substrate.

[0051] See also Fig. 9 As shown, in one embodiment of the present invention, the substrate 1 is a polyetheretherketone substrate, and the polyetheretherketone substrate is not surface treated. For example, 1 part of methyltrimethoxysilane and 0.5 parts of N,N-methylenebisacrylamide are added to the elastomer rubber as a crosslinking agent, and 0.2 parts of a plasticizer phthalate are mixed evenly, and then extruded into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 75°C, and the extrusion rate is, for example, 60mm / s. The extruded rubber strip is vulcanized in a press at a temperature of 160°C, a pressure of 15MPa, and a time of 15min, and then laminated to prepare a sealing component product. Then, the sealing component product is subjected to a secondary vulcanization time of, for example, 20h at a temperature of, for example, 230°C, and the sealing component is prepared. The mechanical properties of the sealing component were tested, for example, a 180° peel test was performed on the elastomer 2 at 150°C. In the sealing component, the elastomer 2 and the substrate 1 were delaminated, indicating that the adhesion between the elastomer 2 and the substrate 1 was poor. Furthermore, the elastomer was directly bonded to the polymer substrate, and the adhesion between the elastomer and the polymer substrate was poor.

[0052] See also Figure 3As shown, in one embodiment of the present invention, the substrate 1 is a metal stainless steel substrate, and the concave portion 3 is processed by CNC processing, wherein the total thickness of the substrate 1 is, for example, 7 mm, the minimum depth of the three-dimensional hollow pattern is, for example, 0.3 mm, the maximum depth is, for example, 2.5 mm, and the total thickness of the elastomer is, for example, 5 mm. After the processing of the concave portion 3 of the substrate 1 is completed, the processed substrate 1 is anodized. For example, 5 parts of a bis[2-(perfluorohexyl)ethyl]phosphate crosslinker and, for example, 0.1 parts of a plasticizer dioctyl phthalate are added to the elastomer raw rubber, mixed evenly, and then extruded into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 100°C, the extrusion rate is, for example, 25 mm / s, and before extruding the rubber strip, the substrate 1 is preheated for, for example, 40 seconds. The extruded rubber strip is vulcanized in a press, for example, at a temperature of 180°C, a pressure of 12 MPa, and a time of 20 minutes, and then laminated to prepare a sealing component product. The sealing component is then subjected to secondary vulcanization at a temperature of, for example, 270°C for a time of, for example, 12 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, for example, a 180° peeling test of the elastomer at 150°C is performed. In the sealing component, the elastomer is internally damaged and does not delaminate, indicating that the elastomer and the substrate 1 are well bonded, and the elastomer is embedded in the recess 3 on the metal substrate on the substrate 1.

[0053] See also Figure 3As shown, in one embodiment of the present invention, the substrate 1 is a metal copper substrate, and the concave portion 3 is processed by CNC machining, wherein the total thickness of the substrate 1 is, for example, 4.5 mm, the minimum depth of the three-dimensional hollow pattern is, for example, 0.3 mm, the maximum depth is, for example, 1.5 mm, and the total thickness of the elastomer is, for example, 3 mm. After the concave portion 3 of the substrate 1 is processed, the processed substrate 1 is anodized. For example, 1.5 parts of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane crosslinking agent and, for example, 0.3 parts of silane coupling agent triethoxyfluorosilane are added to the elastomer raw rubber, mixed evenly, and extruded into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 80°C, the extrusion rate is, for example, 35 mm / s, and before extruding the rubber strip, the substrate 1 is preheated for, for example, 55 seconds. The extruded rubber strip is vulcanized once in a press at a temperature of 190°C, a pressure of 15 MPa and a time of 8 minutes, and then laminated to prepare a sealing component product. The sealing component product is then subjected to a secondary vulcanization at a temperature of, for example, 220°C and a time of, for example, 28 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, such as a 180° peel test of the elastomer at 150°C. In the sealing component, the elastomer has internal damage and no delamination, indicating that the bonding between the elastomer and the substrate 1 is good, the elastomer is embedded in the recess 3 on the substrate 1, and the shape of the recess 3 does not affect the bonding between the elastomer and the substrate 1.

[0054] See also Figure 4As shown, in one embodiment of the present invention, the substrate 1 is a metal titanium substrate, and the concave portion 3 is processed by CNC machining, wherein the total thickness of the substrate 1 is, for example, 5 mm, the minimum depth of the three-dimensional hollow pattern is, for example, 0.5 mm, the maximum depth is, for example, 1.5 mm, and the total thickness of the elastomer is, for example, 3 mm. After the processing of the concave portion 3 of the substrate 1 is completed, the processed substrate 1 is anodized. For example, 1.0 parts of sodium dibutyl dithiocarbamate crosslinking agent and, for example, 0.3 parts of plasticizer phthalate are added to the elastomer raw rubber, mixed evenly, and then extruded into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 95°C, the extrusion rate is, for example, 40 mm / s, and before extruding the rubber strip, the substrate 1 is preheated for, for example, 50 seconds. The extruded rubber strip is vulcanized once in a press at, for example, a temperature of 150°C, a pressure of 8 MPa, and a time of 20 minutes, and then laminated to prepare a sealing component product. The sealing component is then subjected to secondary curing at a temperature of, for example, 210°C for a time of, for example, 30 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, for example, a 180° peeling test of the elastomer at 150°C is performed. In the sealing component, the elastomer is internally damaged and no delamination occurs, indicating that the elastomer and the substrate 1 are well bonded, the elastomer is embedded in the recess 3 on the substrate 1, and the material of the substrate 1 does not affect the physical bonding between the elastomer 2 and the substrate 1.

[0055] See also Fig. 9 As shown, in one embodiment of the present invention, the substrate 1 is a metal titanium substrate, and the metal titanium substrate is not surface treated. For example, 1.0 parts of sodium dibutyl dithiocarbamate crosslinking agent and 0.3 parts of plasticizer phthalate are added to the elastomer raw rubber, mixed evenly, and then extruded into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 95°C, and the extrusion rate is, for example, 40mm / s. The extruded rubber strip is vulcanized in a press, for example, at a temperature of 150°C, a pressure of 8MPa, and a time of 20min, and then laminated to prepare a sealing component product. Then, the sealing component product is subjected to a secondary vulcanization time of, for example, 30h at a temperature of, for example, 210°C, and the sealing component is prepared. The mechanical properties of the sealing component are tested, for example, a 180° peel test of the elastomer is performed at 150°C. In the sealing component, the elastomer and the substrate 1 are layered, indicating that the adhesion between the elastomer 2 and the substrate 1 is poor.

[0056] See also Figure 4As shown, in one embodiment of the present invention, the substrate 1 is a metal magnesium substrate, and the concave portion 3 is processed by CNC machining, wherein the total thickness of the substrate 1 is, for example, 2.9 mm, the minimum depth of the three-dimensional hollow pattern is, for example, 0.4 mm, the maximum depth is, for example, 0.9 mm, and the total thickness of the elastomer is, for example, 3.5 mm. After the concave portion 3 of the substrate 1 is processed, the processed substrate 1 is anodized. For example, 1 part of perfluoro-1,3-dimethylcyclohexane and 1 part of benzoyl peroxide crosslinking agent, for example, 0.3 parts of silane coupling agent (3-mercaptopropyl) trimethoxysilane are added to the elastomer raw rubber, mixed evenly, and extruded into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 85°C, the extrusion rate is, for example, 20 mm / s, and before extruding the rubber strip, the substrate 1 is preheated for, for example, 40 seconds. The extruded rubber strip is vulcanized once in a press at a temperature of 190°C, a pressure of 15 MPa and a time of 15 minutes, and then laminated to prepare a sealing component product. The sealing component product is then subjected to a secondary vulcanization at a temperature of, for example, 280°C for a time of, for example, 6 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, such as a 180° peel test of the elastomer at 150°C. In the sealing component, the elastomer has internal damage and no delamination, indicating that the bonding between the elastomer and the substrate 1 is good, the elastomer is embedded in the recess 3 on the substrate 1, and the depth of the recess has little effect on the bonding between the elastomer 2 and the substrate 1.

[0057] See also Figure 4As shown, in one embodiment of the present invention, the substrate 1 is a polyamide substrate, and the concave portion 3 is processed by 3D printing, wherein the total thickness of the substrate 1 is, for example, 7.5 mm, the minimum depth of the three-dimensional hollow pattern is, for example, 0.5 mm, the maximum depth is, for example, 3 mm, and the total thickness of the elastomer is, for example, 4.5 mm. After the processing of the concave portion 3 of the substrate 1 is completed, the processed substrate 1 is subjected to corona treatment to ensure that the roughness of the surface of the polyamide substrate is, for example, 55 um. For example, 3 parts of di-tert-butyl peroxide crosslinking agent and, for example, 0.3 parts of silane coupling agent tributyl silane are added to the elastomer raw rubber, mixed evenly, and then extruded into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 95°C, and the extrusion rate is, for example, 70 mm / s. The extruded rubber strip is vulcanized once in a press at, for example, a temperature of 185°C, a pressure of 15 MPa, and a time of 5 min, and then laminated to prepare a sealing component product. The sealing component is then subjected to secondary curing at a temperature of, for example, 270°C for a time of, for example, 20 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, for example, a 180° peeling test of the elastomer at 150°C is performed. In the sealing component, the elastomer is internally damaged and does not delaminate, indicating that the elastomer and the substrate 1 are well bonded, the elastomer is embedded in the recess 3 on the substrate 1, and the type of crosslinking agent does not affect the performance of the sealing component.

[0058] See also Figure 5 As shown, in one embodiment of the present invention, the substrate 1 is a metal aluminum substrate, and the concave portion 3 is processed by CNC, wherein the total thickness of the substrate 1 is, for example, 3 mm, the minimum depth of the three-dimensional hollow pattern is, for example, 0.4 mm, the maximum depth is, for example, 1 mm, and the total thickness of the elastomer is, for example, 3.5 mm. After the processing of the concave portion 3 of the substrate 1 is completed, the processed substrate 1 is anodized. For example, 1.2 parts of a bis[2-(perfluorohexyl)ethyl]phosphate crosslinker and, for example, 0.5 parts of a plasticizer terephthalate are added to the elastomer raw rubber, mixed evenly, and then extruded into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 90°C, the extrusion rate is, for example, 30 mm / s, and before extruding the rubber strip, the substrate 1 is preheated for, for example, 30 seconds. The extruded rubber strip is vulcanized once in a press at, for example, a temperature of 190°C, a pressure of 8 MPa, and a time of 3 minutes, and then laminated to prepare a sealing component product. The sealing component is then subjected to secondary vulcanization at a temperature of, for example, 280°C for a time of, for example, 8 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, for example, a 180° peeling test of the elastomer at 150°C is performed. In the sealing component, the elastomer is internally damaged but not delaminated, indicating that the elastomer and the substrate 1 are well bonded and the elastomer is embedded in the recess 3 on the substrate 1.

[0059] See also Fig. 9 As shown, in one embodiment of the present invention, the substrate 1 is a metal aluminum substrate, and the metal aluminum substrate is not surface treated. For example, 1.2 parts of bis[2-(perfluorohexyl)ethyl]phosphate crosslinking agent and 0.5 parts of plasticizer terephthalate are added to the elastomer raw rubber, mixed evenly, and then extruded into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 90°C, and the extrusion rate is, for example, 30mm / s. The extruded rubber strip is vulcanized in a press at a temperature of 190°C, a pressure of 8MPa, and a time of 3min, and then laminated to prepare a sealing component product. The sealing component product is then subjected to a secondary vulcanization at a temperature of, for example, 280°C, and a time of, for example, 8h, and the sealing component is prepared. The mechanical properties of the sealing component were tested, for example, a 180° peel test was performed on the elastomer at 150°C. In the sealing component, the elastomer 2 and the substrate 1 were delaminated, indicating that the adhesion between the elastomer 2 and the substrate 1 was poor, which further indicated that the elastomer and the substrate were tightly bonded through the recess. If there were no recess, the adhesion between the elastomer and the substrate would also be small through the cross-linking agent and other additives.

[0060] See also Figure 5 As shown, in one embodiment of the present invention, the substrate 1 is a metal aluminum substrate, and the concave portion 3 is processed by CNC, wherein the total thickness of the substrate 1 is, for example, 7.7 mm, the minimum depth of the three-dimensional hollow pattern is, for example, 0.4 mm, the maximum depth is, for example, 2.7 mm, and the total thickness of the elastomer is, for example, 3 mm. After the concave portion 3 of the substrate 1 is processed, the processed substrate 1 is anodized. For example, 2 parts of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane crosslinking agent and, for example, 0.3 parts of silane coupling agent 3-glycidyl trimethoxysilane are added to the elastomer raw rubber, mixed evenly, and extruded into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 90°C, the extrusion rate is, for example, 55 mm / s, and before extruding the rubber strip, the substrate 1 is preheated for, for example, 45 seconds. The extruded rubber strip is vulcanized in a press at a temperature of 175°C, a pressure of 18 MPa and a time of 5 minutes, and then laminated to prepare a sealing component product. The sealing component product is then subjected to a secondary vulcanization at a temperature of, for example, 260°C and a time of, for example, 15 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, such as a 180° peel test of the elastomer at 150°C. In the sealing component, the elastomer has internal damage and no delamination occurs, and the extrusion speed of the rubber strip has little effect on the mechanical properties of the sealing component.

[0061] See also Figure 5As shown, in one embodiment of the present invention, the substrate 1 is a polyphenylene ether substrate, and the concave portion 3 is processed by 3D printing, wherein the total thickness of the substrate 1 is, for example, 7 mm, the minimum depth of the three-dimensional hollow pattern is, for example, 0.5 mm, the maximum depth is, for example, 2.5 mm, and the total thickness of the elastomer is, for example, 4.5 mm. After the processing of the concave portion 3 of the substrate 1 is completed, the processed substrate 1 is subjected to corona treatment to ensure that the roughness of the surface of the polyphenylene ether substrate is, for example, 10 um. For example, 1 part of 2-ethyl-4-methylimidazole and 1 part of phthalic anhydride crosslinking agent, for example, 0.3 parts of silane coupling agent dimethylphenylsilane are added to the elastomer raw rubber, mixed evenly, and extruded into a specific shape of rubber strip in a plunger extruder. Among them, the extrusion temperature is, for example, 75 ° C, and the extrusion rate is, for example, 10 mm / s. The extruded rubber strip is vulcanized once in a press at a temperature of 185 ° C, a pressure of 18 MPa, and a time of 18 min, and then laminated to prepare a sealing component product. The sealing component is then subjected to secondary curing at a temperature of, for example, 250°C for a time of, for example, 24 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, for example, a 180° peeling test of the elastomer at 150°C is performed. In the sealing component, the elastomer is internally damaged but not delaminated, indicating that the elastomer and the substrate 1 are well bonded and the elastomer is embedded in the recess 3 on the substrate 1.

[0062] See also Figure 6 As shown, in one embodiment of the present invention, the substrate 1 is a polyimide substrate, and the concave portion 3 is processed by 3D printing, wherein the total thickness of the substrate 1 is, for example, 3 mm, the minimum depth of the three-dimensional hollow pattern is, for example, 0.7 mm, the maximum depth is, for example, 1 mm, and the total thickness of the elastomer is, for example, 4 mm. After the concave portion 3 of the substrate 1 is processed, the processed substrate 1 is subjected to corona treatment to ensure that the roughness of the surface of the polyimide substrate is, for example, 3 um. For example, 3 parts of 2,2-bis(trifluoromethanesulfonyloxy)-1,1-biphenyl (1,1-bisphenol bisphenolate) crosslinking agent and, for example, 0.2 parts of plasticizer diisononyl phthalate are added to the elastomer raw rubber, mixed evenly, and extruded into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 70°C, and the extrusion rate is, for example, 10 mm / s. The extruded rubber strip is vulcanized in a press at a temperature of 160°C, a pressure of 20 MPa and a time of 10 minutes, and then laminated to prepare a sealing component product. The sealing component product is then subjected to a secondary vulcanization at a temperature of, for example, 280°C and a time of, for example, 15 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, for example, a 180° peel test of the elastomer at 150°C is performed. In the sealing component, the elastomer is internally damaged and no delamination occurs, indicating that the bonding between the elastomer and the substrate 1 is good, and the elastomer is embedded in the recess 3 on the substrate 1.

[0063] See also Figure 6 As shown, in one embodiment of the present invention, the substrate 1 is a polyetherketone substrate, and the concave portion 3 is processed by 3D printing, wherein the total thickness of the substrate 1 is, for example, 8 mm, the minimum depth of the three-dimensional hollow pattern is, for example, 0.5 mm, the maximum depth is, for example, 3 mm, and the total thickness of the elastomer is, for example, 5 mm. After the processing of the concave portion 3 of the substrate 1 is completed, the processed substrate 1 is subjected to corona treatment to ensure that the roughness of the surface of the polyetherketone substrate is, for example, 70 um. For example, 2 parts of 2-ethyl-4-methylimidazole crosslinking agent and, for example, 0.2 parts of antioxidant 3,6-dihydroxybenzonorbornane are added to the elastomer raw rubber, mixed evenly, and extruded into a rubber strip of a specific shape in a plunger extruder. Among them, the extrusion temperature is, for example, 100°C, and the extrusion rate is, for example, 40 mm / s. The extruded rubber strip is vulcanized once in a press at, for example, a temperature of 180°C, a pressure of 13 MPa, and a time of 17 min, and then laminated to prepare a sealing component product. The sealing component is then subjected to secondary curing at a temperature of, for example, 280°C for a time of, for example, 16 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, for example, a 180° peeling test of the elastomer at 150°C is performed. In the sealing component, the elastomer is internally damaged but not delaminated, indicating that the elastomer and the substrate 1 are well bonded and the elastomer is embedded in the recess 3 on the substrate 1.

[0064] See also Figure 7As shown, in one embodiment of the present invention, the substrate 1 is a composite substrate of polyetheretherketone and polytetrafluoroethylene, and the concave portion 3 is processed by 3D printing, wherein the total thickness of the substrate 1 is, for example, 5.5 mm, the minimum depth of the three-dimensional hollow pattern is, for example, 1 mm, the maximum depth is, for example, 2 mm, and the total thickness of the elastomer is, for example, 3.5 mm. After the concave portion 3 of the substrate 1 is processed, the processed substrate 1 is subjected to corona treatment to ensure that the roughness of the composite substrate of polyetheretherketone and polytetrafluoroethylene is, for example, 35 um. For example, 1 part of 2-ethyl-4-methylimidazole and 1 part of phthalic anhydride crosslinking agent, for example, 0.3 parts of silane coupling agent dimethylphenylsilane are added to the elastomer raw rubber, and after mixing evenly, a rubber strip of a specific shape is extruded in a plunger extruder. Among them, the extrusion temperature is, for example, 70°C, and the extrusion rate is, for example, 35 mm / s. The extruded rubber strip is vulcanized in a press at a temperature of 150°C, a pressure of 20 MPa and a time of 17 minutes, and then laminated to prepare a sealing component product. The sealing component product is then subjected to a secondary vulcanization at a temperature of, for example, 260°C and a time of, for example, 18 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, for example, a 180° peel test of the elastomer at 150°C is performed. In the sealing component, the elastomer is internally damaged and no delamination occurs, indicating that the bonding between the elastomer and the substrate 1 is good, and the elastomer is embedded in the recess 3 on the substrate 1.

[0065] See also Fig.10 As shown, in one embodiment of the present invention, the substrate 1 is a metal aluminum substrate, a layer of adhesive 4 is coated on the substrate 1, and the adhesive 4 is, for example, polydimethylsiloxane (PDMS), and the uncross-linked elastomer fragments are directly placed on the substrate 1 in a swinging manner. The elastomer rubber is vulcanized at a temperature of, for example, 145°C, a pressure of, for example, 5MPa, and a time of, for example, 40min, and then laminated to prepare a sealing component product. The sealing component product is then subjected to a secondary vulcanization at a temperature of, for example, 200°C for a time of, for example, 10h, and the sealing component is completed. The mechanical properties of the sealing component are tested, for example, a 180° peeling test of the elastomer 2 at 150°C is performed. In the sealing component, the elastomer 2 is delaminated from the substrate 1, indicating that the sealing component compounded by the adhesive 4 has poor adhesion between the elastomer 2 and the substrate 1, and is not suitable for equipment with higher requirements.

[0066] See also Fig.10As shown, in one embodiment of the present invention, the substrate 1 is a PTFE substrate, a layer of adhesive 4 is coated on the substrate 1, and the adhesive 4 is, for example, Chemlok 607, and the uncrosslinked elastomer fragments are directly placed on the substrate 1 in a swinging manner. The elastomer rubber is vulcanized at a temperature of, for example, 200°C, a pressure of, for example, 25MPa, and a time of, for example, 3min, and then laminated to prepare a sealing component product. The sealing component product is then subjected to a secondary vulcanization at a temperature of, for example, 295°C for a time of, for example, 18h, and the sealing component is completed. The mechanical properties of the sealing component are tested, for example, a 180° peel test of the elastomer 2 at 150°C is performed. In the sealing component, the elastomer 3 is layered from the substrate 1, indicating that the sealing component compounded by the adhesive 4 has poor adhesion between the elastomer 2 and the substrate 1.

[0067] See also Fig.10 As shown, in one embodiment of the present invention, the substrate 1 is a metal aluminum-magnesium alloy substrate, a layer of adhesive 4 is coated on the substrate 1, and the adhesive 4 is, for example, an epoxy resin adhesive, and the uncross-linked elastomer fragments are directly placed on the substrate 1 in a swinging manner. The elastomer rubber is vulcanized at a temperature of, for example, 160°C, a pressure of, for example, 10MPa, and a time of, for example, 5min, and then laminated to prepare a sealing component product. The sealing component product is then subjected to a secondary vulcanization at a temperature of, for example, 220°C for a time of, for example, 16h, and the sealing component is completed. The mechanical properties of the sealing component are tested, for example, a 180° peeling test of the elastomer 2 at 150°C is performed. In the sealing component, the elastomer 2 is delaminated from the substrate 1, indicating that the sealing component compounded by the adhesive 4 has poor adhesion between the elastomer 2 and the substrate 1, and is not suitable for sealing conditions in relatively harsh environments.

[0068] See also Fig.10 As shown, in one embodiment of the present invention, the substrate 1 is a metal aluminum-magnesium alloy substrate, a layer of adhesive 4 is coated on the substrate 1, and the adhesive 4 is, for example, an epoxy resin adhesive, and the uncrosslinked elastomer fragments are directly placed on the substrate 1 in a swinging manner. The elastomer rubber is vulcanized at a temperature of, for example, 170°C, a pressure of, for example, 15 MPa, and a time of, for example, 15 min, and then laminated to prepare a sealing component product. The sealing component product is then subjected to a secondary vulcanization at a temperature of, for example, 260°C for, for example, 18 hours, and the sealing component is completed. The mechanical properties of the sealing component are tested, for example, a 180° peeling test of the elastomer 2 at 150°C is performed. In the sealing component, the elastomer 2 is delaminated from the substrate 1, indicating that the sealing component compounded by the adhesive 4 has different types of adhesive 4, but the bonding between the elastomer 2 and the substrate 1 is not improved, and is not suitable for sealing conditions with relatively harsh environments.

[0069] In summary, the present invention provides a semiconductor device sealing component and a manufacturing method thereof, wherein the elastomer and the substrate are physically bonded through the three-dimensional hollow lines of the concave portion, thereby improving the mechanical and chemical properties of the sealing component and having a low manufacturing cost. When the sealing component is applied to a semiconductor sealing device, the sealing component will not fail due to the delamination of the elastomer and the substrate, thereby improving the reliability of the semiconductor process.

[0070] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for manufacturing a sealing component of a semiconductor device, characterized in that: include: providing a substrate; A plurality of recesses are formed on the surface of the substrate, wherein the recesses are three-dimensional hollow patterns, and the plurality of recesses are interlocked with each other; An elastomer is arranged in the concave portion, wherein the elastomer is a fluorine-containing elastomer, and the fluorine-containing elastomer is an elastomer that has not been vulcanized, and the elastomer fills and covers the concave portion; and The elastomer is vulcanized, and after the elastomer is vulcanized once, a sealing component preform is prepared by lamination, and then the sealing component preform is subjected to secondary vulcanization to form a semiconductor device sealing component; the temperature of the primary vulcanization is 150~200°C, the pressure of the primary vulcanization is 5~20MPa, and the vulcanization time of the primary vulcanization is 3~20min; the temperature of the secondary vulcanization is 210~280°C, and the time of the secondary vulcanization is 4~30h.

2. The method for manufacturing a semiconductor device sealing component according to claim 1, characterized in that: The concave portion is at least one of a circle, an ellipse, a polygon or a curve.

3. The method for manufacturing a semiconductor device sealing component according to claim 2, characterized in that: The depth of the recess is 0.2-3 mm.

4. The method for manufacturing a semiconductor device sealing component according to claim 1, characterized in that: The substrate includes a metal substrate, and the metal substrate includes at least one of a magnesium substrate, a titanium substrate, an aluminum substrate, a copper substrate, a chromium substrate or an alloy substrate.

5. The method for manufacturing a semiconductor device sealing component according to claim 4, characterized in that: After the recessed portion is formed, the metal substrate is subjected to anodizing treatment to form porous anodic oxide on the surface of the metal substrate.

6. The method for manufacturing a semiconductor device sealing component according to claim 1, characterized in that: The substrate includes a high molecular polymer substrate, and the high molecular polymer substrate includes at least one of a polyetheretherketone substrate, a polytetrafluoroethylene substrate, a polyphenylene ether substrate, a polyimide substrate, a poly-4-methylpentene substrate, a polyetherketone substrate, a polyamide substrate or a composite material substrate.

7. The method for manufacturing a semiconductor device sealing component according to claim 6, characterized in that: After the recessed portion is formed, the high molecular polymer substrate is subjected to a corona surface treatment.

8. The method for manufacturing a semiconductor device sealing component according to claim 6, characterized in that: The surface roughness of the high molecular polymer substrate is 5-100 μm.

9. A semiconductor device sealing component, obtained by the manufacturing method according to any one of claims 1 to 8, characterized in that: include: A substrate, wherein a plurality of mutually engaging recesses are provided on a surface of the substrate; as well as An elastic body fills and covers the recess.