Oxygen absorption and desorption material and preparation method thereof and fully enclosed lithium-air battery

By using oxygen adsorption and desorption materials as oxygen storage layers in lithium-air batteries, the problems of large size and influence of external gases in lithium-air batteries are solved, efficient capture and storage of oxygen is achieved, and the stability and energy density of the battery are improved.

CN114307952BActive Publication Date: 2024-10-08HARBIN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111602275.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-24
Publication Date
2024-10-08
Estimated Expiration
2041-12-24

AI Technical Summary

Technical Problem

Lithium-air batteries are large and inflexible due to the storage space of O2 in the cathode, and gases in the air affect battery stability, limiting their large-scale application.

Method used

Oxygen adsorption and desorption materials are used as oxygen storage layers with pores and/or channel structures for fully enclosed lithium-air batteries to ensure reversible adsorption and desorption of oxygen and avoid the entry of external gases. The material is prepared by mixing an oxygen storage material and a binder in an organic solvent, stirring and drying, and is used in a laminated structure of lithium anodes, separators, cathodes and isolation layers.

Benefits of technology

It solves the problem of large size and flexibility of lithium-air batteries, while avoiding the adverse effects of external gases on the battery, improving the stability and energy density of the battery, and achieving efficient capture and storage of oxygen.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114307952B_ABST
    Figure CN114307952B_ABST
Patent Text Reader

Abstract

Oxygen adsorption and desorption materials, preparation methods thereof and fully enclosed lithium-air batteries relate to the technical field of lithium-air batteries. The present invention aims to solve the problem that the storage space for oxygen in the cathode of a lithium-air battery will cause adverse effects such as large volume and lack of flexibility on the battery. The present invention describes a reversible oxygen adsorption and desorption material and applies it to a fully enclosed lithium-air battery. The oxygen storage layer of the fully enclosed lithium-air battery is an oxygen adsorption and desorption material with pores and channel structures, and has a reversible adsorption and desorption capability for oxygen. When the battery is discharged, oxygen is released from the oxygen storage layer and enters the cathode through the isolation layer to react; when the battery is charged, the oxygen generated by the reaction will be absorbed by the oxygen storage layer again through the isolation layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium-air batteries. Background Art

[0002] The global energy depletion and environmental pollution problems have become increasingly serious, so the demand for a variety of clean and cheap new energy systems is particularly urgent. Currently, lithium-ion battery technology has been widely used in various industries, but the low theoretical specific energy of lithium-ion batteries can no longer meet the increasingly high demand.

[0003] As a new energy system, lithium-air battery is expected to become a substitute for lithium-ion battery. Lithium-air battery is a typical metal-air battery, which uses metallic lithium as the negative electrode reaction substance, oxygen in the air as the positive electrode reaction substance, and water, organic electrolyte or solid electrolyte as the electrolyte, forming a complete ion transmission channel inside the battery. Without calculating the mass of oxygen in the positive electrode reaction substance, lithium-air battery has an extremely high theoretical energy density of 11140Wh / kg, which is much higher than the theoretical energy density of other metal batteries and close to that of petroleum. Even when calculating the mass of the positive electrode reaction substance, the energy density of lithium-air battery is as high as 5200Wh / kg. It is much higher than other current rechargeable battery systems.

[0004] There are still many unsolved problems in lithium-air batteries that limit their large-scale use, which can be divided into the following four points:

[0005] (1) Slow OER and ORR reaction kinetics at the cathode:

[0006] Carbon materials are the most widely used cathode materials in lithium-air batteries at this stage, but the slow OER and ORR reactions of carbon materials themselves will reduce the performance of the battery. Secondly, the deposition of discharge products on the cathode is also one of the main factors limiting its energy release. Therefore, reasonable cathode material and structural design is also a major direction of cathode research.

[0007] (2) Stability and safety of electrolyte:

[0008] Because of the main problem that aqueous electrolytes react violently with lithium metal, a lot of research has focused on organic electrolytes. However, organic electrolytes have disadvantages such as volatility, poor stability and poor safety, which affect the practical application of batteries. In addition, the insolubility of discharge products in organic electrolytes can easily lead to blockage of cathode pores. Currently, a large number of researchers are focusing on the development of solid electrolytes. Although they can overcome many problems of organic electrolytes, they also have disadvantages such as poor conductivity and poor interface impedance. Therefore, finding a suitable and stable electrolyte system is the main purpose of the research.

[0009] (3) Corrosion of lithium metal anode and lithium dendrites:

[0010] On the lithium negative electrode side, the corrosion of lithium metal by oxygen or other gases that penetrate through the electrolyte is one of the main problems that prevent lithium-air batteries from long-term circulation. At the same time, the growth of lithium dendrites can easily penetrate the diaphragm and cause internal short circuits, which can cause safety hazards. This is also a problem that lithium negative electrodes need to face. Currently, a large number of studies focus on the growth mechanism of lithium dendrites and how to inhibit and completely solve the problems caused by the growth of lithium dendrites. An equally dense electrolyte membrane may become another measure to protect lithium metal.

[0011] (4) Influence of gas components in the air:

[0012] The ultimate goal of lithium-oxygen batteries is to be converted into lithium-air batteries for practical use, but N2, CO2, H2O and other gases in the air will have an adverse effect on the inside of the battery. Therefore, the main purpose of the research is to capture only O2 from the air and block other gases from entering the battery while maintaining sufficient oxygen pressure inside the battery for discharge.

[0013] In summary, lithium-air batteries are subject to many restrictions in their application. In particular, the capture and storage of the cathode reactant O2 in lithium-air batteries seriously affects the battery's supply and discharge requirements. In order to ensure that the battery only captures O2 in the air, most use a closed structure to seal O2 inside the battery. However, the storage space for O2 in the cathode of lithium-air batteries will bring adverse effects to the battery, such as large volume and lack of flexibility. Summary of the invention

[0014] The present invention aims to solve the problem that the storage space of O2 in the cathode of a lithium-air battery will bring adverse effects such as large volume and lack of flexibility to the battery. An oxygen absorption and desorption material and a preparation method thereof and a fully enclosed lithium-air battery are provided.

[0015] Oxygen absorption and desorption materials have pores and / or channel structures inside for storing oxygen.

[0016] Furthermore, the inner diameter of the pores and / or channels is 0.1 nm to 100 nm.

[0017] The preparation method of the above oxygen absorption and desorption material is as follows:

[0018] First, the oxygen storage material and the binder are mixed in an organic solvent in proportion.

[0019] Then, the uniformly stirred mixture is scraped onto the substrate until the mixture is completely dry to obtain an oxygen adsorption and desorption material.

[0020] The mass ratio between the oxygen storage material and the binder is 9:1, 6:1, 5:1, 4:1 or 3:1.

[0021] Furthermore, the oxygen storage material is one or more of A-type zeolite molecular sieve, X-type zeolite molecular sieve, Y-type zeolite molecular sieve, carbon molecular sieve and mesoporous carbon.

[0022] The above-mentioned binder is polyvinylidene fluoride or polytetrafluoroethylene,

[0023] The organic solvent is N-methylpyrrolidone, dimethylacetamide, dimethylformamide or ethylene glycol dimethyl ether.

[0024] Furthermore, the oxygen storage material and the binder are stirred in an organic solvent at 25° C. to 50° C. for 10 h to 20 h.

[0025] A fully enclosed lithium-air battery comprises: a lithium anode 1, a diaphragm 2, a cathode 3, a separation layer 4 and an oxygen storage layer 5 which are stacked in sequence.

[0026] The oxygen storage layer 5 is an oxygen absorption and desorption material.

[0027] The lithium anode 1, the separator 2, the cathode 3, the isolation layer 4 and the oxygen storage layer 5 are all located inside the sealed battery shell.

[0028] Furthermore, the lithium anode 1 is a lithium sheet having a purity of 99.99% and a thickness of 100 μm to 200 μm.

[0029] Furthermore, the material of the above-mentioned separator 2 is polypropylene, and the thickness is 20 μm to 50 μm.

[0030] Furthermore, the cathode 3 is carbon nanotube, BP2000, graphene or commercial carbon.

[0031] Furthermore, the isolation layer 4 is one or more of carbon paper, carbon felt and nickel foam.

[0032] The present invention provides a reversible oxygen absorption and desorption material and applies it to a fully enclosed lithium-air battery. The oxygen storage layer of the fully enclosed lithium-air battery is an oxygen absorption and desorption material with pores and channel structures, and has the ability to reversibly absorb and desorb oxygen. When the battery is discharged, oxygen is released from the oxygen storage layer and enters the cathode through the isolation layer to react; when the battery is charged, the oxygen generated by the reaction will be absorbed by the oxygen storage layer again through the isolation layer. The present invention solves the long-standing problems of lithium-air batteries such as large size and bulkiness caused by the storage of oxygen, and also avoids the instability problem caused to the battery by external gases (such as H2O, CO2 and N2 in the air) in an open battery system. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 A schematic diagram of a novel battery structure of the present invention;

[0034] Figure 2Schematic diagram of oxygen transport during battery charging and discharging, where (a) represents discharging and (b) represents charging;

[0035] Figure 3 This is a diagram of the charge and discharge test results in Example 1;

[0036] Figure 4 This is a diagram of the charge and discharge test results in Example 2;

[0037] Figure 5 This is a graph showing the cycle test results in Example 2. DETAILED DESCRIPTION

[0038] The following will be combined with the accompanying drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict. Specific implementation method one:

[0040] The oxygen absorption and desorption material described in this embodiment has pores and / or channel structures for storing oxygen inside, and the inner diameter of the pores and / or channels is 0.1 nm to 100 nm.

[0041] The oxygen absorption and desorption material described in this embodiment is used in lithium batteries. When the lithium battery is charged and discharged, oxygen can be reversibly adsorbed and desorbed inside the material. Specific implementation method 2:

[0043] The oxygen absorption and desorption material described in this embodiment is prepared by a casting method:

[0044] First, the oxygen storage material and the binder are mixed in an organic solvent in a mass ratio of 9:1, 6:1, 5:1, 4:1 or 3:1; then, the oxygen storage material and the binder are stirred in the organic solvent for 10 hours to 20 hours at 25°C to 50°C; finally, the stirred mixture is applied on a substrate with a scraper, and dried in an oven at 60-100°C for 10 hours to 20 hours until the mixture is completely dry, thereby obtaining an oxygen adsorption and desorption material.

[0045] The oxygen storage material is one or more of A-type zeolite molecular sieve, X-type zeolite molecular sieve, Y-type zeolite molecular sieve, carbon molecular sieve and mesoporous carbon.

[0046] The above-mentioned binder is polyvinylidene fluoride or polytetrafluoroethylene,

[0047] The organic solvent is N-methylpyrrolidone, dimethylacetamide, dimethylformamide or ethylene glycol dimethyl ether.

[0048] The thickness of the scraper is 100 μm, 150 μm, 200 μm, 250 μm, 500 μm, 750 μm or 1000 μm.

[0049] The substrate is aluminum foil, copper foil, carbon paper, carbon-coated aluminum foil or carbon-coated copper foil.

[0050] The oxygen adsorption and desorption material prepared by the above method needs to be stored in a drying oven at a temperature of 50-70°C. Specific implementation method three:

[0052] Reference Figure 1 and Figure 2 Specifically describing the present embodiment, the fully enclosed lithium-air battery described in the present embodiment comprises: a lithium anode 1, a diaphragm 2, a cathode 3, an isolation layer 4 and an oxygen storage layer 5 which are stacked in sequence. Among them, the oxygen storage layer 5 is an oxygen absorption and desorption material. The lithium anode 1, the diaphragm 2, the cathode 3, the isolation layer 4 and the oxygen storage layer 5 are all located inside a sealed battery shell. The oxygen storage layer of the fully enclosed lithium-air battery is an oxygen absorption and desorption material having a pore and channel structure, and has a reversible absorption and desorption capacity for oxygen. When the battery is discharged, oxygen is released from the oxygen storage layer, enters the cathode through the isolation layer to react; when the battery is charged, the oxygen generated by the reaction will be absorbed by the oxygen storage layer again through the isolation layer.

[0053] The lithium anode 1 is a lithium sheet having a purity of 99.99% and a thickness of 100 μm to 200 μm.

[0054] The material of the separator 2 is polypropylene, and the thickness is 20 μm to 50 μm.

[0055] The cathode 3 is carbon nanotube, BP2000, graphene or commercial carbon.

[0056] The isolation layer 4 is one or more of carbon paper, carbon felt and nickel foam.

[0057] The above battery case model is 2032.

[0058] The above-mentioned spring pieces and gaskets are all made of stainless steel.

[0059] In the above electrolyte, the solvent is dimethyl sulfoxide or ethylene glycol dimethyl ether, the lithium salt is lithium bis(trifluoromethanesulfonyl)imide, and the concentration of the lithium salt is mol / L.

[0060] When assembling the fully enclosed lithium-air battery described in this embodiment, in an argon environment (the bias voltages of oxygen and water are both less than 0.5ppm), the spring, gasket, lithium anode 1 and diaphragm 2 are placed in the battery shell in sequence, 10μL~50μL of electrolyte is added, and then the cathode active material is placed on the diaphragm 2. After infiltration, the isolation layer 4 and the oxygen storage layer 5 are added in sequence, and finally the battery shell back cover is covered and sealed to obtain a lithium-air battery with a sealed structure.

[0061] The preparation method of cathode 3 is as follows: active electrode material (commercial carbon, BP2000, graphene or carbon nanotube) and polytetrafluoroethylene are mixed in a mass ratio of 9:1, 6:1, 5:1, 4:1 or 3:1, anhydrous ethanol is added and dispersed by ultrasonic for 30 to 90 minutes, then the mixture is evenly drop-coated on a polypropylene diaphragm at 60 to 100 degrees Celsius, and finally dried in an oven at 60 to 100 degrees Celsius for 10 to 20 hours to obtain a cathode active material. In this method, the mass surface density of the active material can be controlled by controlling the mass of the active material in the drop-coating slurry and the area of ​​the drop-coating substrate.

[0062] The following examples are used to illustrate the effect of the present invention in practical applications:

[0063] Embodiment 1:

[0064] Weigh 240 mg of polyvinylidene fluoride, dissolve it in 8 mL of N,N-methylpyrrolidone, and stir magnetically for 12 hours. After the polyvinylidene fluoride is completely dissolved in N,N-methylpyrrolidone, add 1200 mg of mesoporous carbon and continue to stir magnetically for 12 hours. The obtained slurry is evenly scraped on the carbon-coated aluminum foil using a 150 μm thick scraper, and placed in an oven at 80 ° C for 12 hours to obtain an oxygen storage layer. Finally, place it in a drying oven at 60 ° C to dry for use. After weighing, the mass density of the oxygen storage layer is 1.5 mg / cm 2 The oxygen storage layer was punched into a circular shape with a diameter of 15 mm (mass of 2.65 mg) for later use.

[0065] Weigh 36 mg of carbon nanotubes, mix them with 200 mg of 2% polytetrafluoroethylene aqueous solution, add 30 mL of anhydrous ethanol, crush and ultrasonicate for 30 min, and use a rubber dropper to evenly apply it on an area of ​​40 cm 2 The cathode was finally placed in an oven at 80°C and dried for 12 hours to obtain a cathode. The obtained cathode was punched into a circular electrode with a diameter of 15 mm (active material loading of 1.77 mg) for later use.

[0066] The obtained oxygen storage layer and cathode were assembled with lithium metal anode, separator and electrolyte into sealed button cells and then tested. The charge, discharge and cycle tests were performed using Neware instruments at a test temperature of 25°C and a relative humidity of 50%. The charge and discharge test results are shown in Figure 2. Figure 3 As shown, the solid line represents the current density of 0.01 mA / cm 2 The constant current discharge test is performed under the condition of constant current discharge, and the dotted line is the charging test curve.

[0067] Embodiment 2:

[0068] Weigh 240 mg of polyvinylidene fluoride and dissolve it in 8 mL of N,N-methylpyrrolidone. Stir magnetically for 12 hours. After the polyvinylidene fluoride is completely dissolved in N,N-methylpyrrolidone, add 1200 mg of mesoporous carbon and continue to stir magnetically for 12 hours. Use a 500 μm scraper to evenly apply the obtained slurry on the carbon-coated aluminum foil, place it in an oven at 80 ° C and dry it for 12 hours to obtain the oxygen storage layer, and finally place it in a drying oven at 60 ° C to dry for use. After weighing, the mass surface density of the oxygen storage layer is 4.0 mg / cm 2 The oxygen storage layer was punched into a circular shape with a diameter of 15 mm (mass of 7.08 mg) for later use.

[0069] Weigh 72 mg of carbon nanotubes, mix them with 400 mg of 2% polytetrafluoroethylene aqueous solution, add 70 mL of anhydrous ethanol, crush and ultrasonicate for 30 min, and use a rubber dropper to evenly apply it on an area of ​​40 cm 2 The cathode was finally placed in an oven at 80°C and dried for 12 hours to obtain a cathode. The obtained cathode was punched into a circular electrode with a diameter of 15 mm (active material loading of 3.55 mg) for later use.

[0070] The obtained oxygen storage layer and cathode were assembled with lithium metal anode, separator and electrolyte into sealed button cells and then tested. The charge, discharge and cycle tests were performed using Neware instruments at a test temperature of 25°C and a relative humidity of 50%. The charge and discharge test results are shown in Figure 2. Figure 4 As shown, the solid line represents the current density of 0.01 mA / cm 2 The constant current discharge test is performed under the condition of constant current discharge, and the dotted line is the charging test curve.

[0071] Cycle test: Figure 5 The battery is shown at 0.01 mA / cm 2 The cyclic test under current density demonstrated the reversible oxygen adsorption and desorption ability of the oxygen storage layer inside the battery.

[0072] Although the present invention is described herein with reference to specific embodiments, it should be understood that these embodiments are merely examples of the principles and applications of the present invention. It should therefore be understood that many modifications may be made to the exemplary embodiments and that other arrangements may be devised without departing from the spirit and scope of the present invention as defined by the appended claims. It should be understood that the various dependent claims and features described herein may be combined in a manner different from that described in the original claims. It should also be understood that the features described in conjunction with a single embodiment may be used in other described embodiments.

Claims

1. Fully enclosed lithium-air battery, It is characterized in that include: A lithium anode (1), a separator (2), a cathode (3), a separation layer (4) and an oxygen storage layer (5) are stacked in sequence. The oxygen storage layer (5) is an oxygen absorbing and desorbing material, and the oxygen absorbing and desorbing material has a pore and / or channel structure for storing oxygen; the inner diameter of the pore and / or channel is 0.1nm to 100nm; The preparation method of oxygen absorption and desorption material is as follows: First, the oxygen storage material and the binder are mixed in an organic solvent in proportion. Then, the uniformly stirred mixture is scraped onto the substrate until the mixture is completely dry to obtain an oxygen adsorption and desorption material. The mass ratio between the oxygen storage material and the binder is 9:1, 6:1, 5:1, 4:1 or 3:1; The oxygen storage material is one or more of A-type zeolite molecular sieve, X-type zeolite molecular sieve, Y-type zeolite molecular sieve, carbon molecular sieve and mesoporous carbon, The binder is polyvinylidene fluoride or polytetrafluoroethylene, The organic solvent is N-methylpyrrolidone, dimethylacetamide, dimethylformamide or ethylene glycol dimethyl ether; Stirring the oxygen storage material and the binder in an organic solvent for 10 h to 20 h at a temperature of 25 to 50 °C; When the battery is discharged, oxygen is released from the oxygen storage layer (5) and enters the cathode (3) through the isolation layer to react; when the battery is charged, the oxygen generated by the reaction is absorbed by the oxygen storage layer (5) again through the isolation layer (4); The lithium anode (1), the separator (2), the cathode (3), the isolation layer (4) and the oxygen storage layer (5) are all located inside the sealed battery case.

2. The fully enclosed lithium-air battery according to claim 1, It is characterized in that The lithium anode (1) is a lithium sheet with a purity of 99.99% and a thickness of 100 μm to 200 μm.

3. The fully enclosed lithium-air battery according to claim 1, It is characterized in that The material of the diaphragm (2) is polypropylene and has a thickness of 20 μm to 50 μm.

4. The fully enclosed lithium-air battery according to claim 1, It is characterized in that The cathode (3) is carbon nanotubes, BP2000, graphene or commercial carbon.

5. The fully enclosed lithium-air battery according to claim 1, It is characterized in that The isolation layer (4) is one or more of carbon paper, carbon felt and nickel foam.