A solid electrolyte material and solid-state lithium battery

By adjusting the chemical composition and structure of the solid electrolyte material in the solid-state lithium battery, the deficiencies in ionic conductivity and air stability of the solid-state lithium battery electrolyte material in the existing technology are solved, and a balance between high ionic conductivity and air stability is achieved. Lithium The ionic conductivity retention rate reaches more than 94%, and the lithium ion conduction efficiency is improved.

CN114335703BActive Publication Date: 2024-10-08GUOLIAN CORE MATERIALS (BEIJING) TECHNOLOGY CO LTD +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202111564528.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-20
Publication Date
2024-10-08
Estimated Expiration
2041-12-20

AI Technical Summary

Technical Problem

The solid electrolyte material of existing solid-state lithium batteries has poor ionic conductivity and insufficient stability in humid air, and easily reacts with moisture in the air, resulting in performance degradation.

Method used

By adjusting the composition and structure of the solid electrolyte material, the chemical composition of LixZryM1-yXaOb is adopted, where M is selected from Fe, Mo, and X is selected from F, Cl, Br, I, and the ratio of each element is controlled to ensure the molar ratio of Zr to M When the ratio is 1

Benefits of technology

The ion conductivity retention rate after air exposure is achieved to be higher than 94%, and on the basis of ensuring high ion conductivity, the air stability is further improved, and the lithium ion conductivity reaches >7.5*10-4S/cm, which reduces Lithium ion migration barrier improves lithium ion conduction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003421404330000061
    Figure BDA0003421404330000061
  • Figure BDA0003421404330000071
    Figure BDA0003421404330000071
  • Figure BDA0003421404330000081
    Figure BDA0003421404330000081
Patent Text Reader

Abstract

The present invention provides a solid electrolyte material and a solid lithium battery, wherein the solid electrolyte material has Li x Zr y M 1‑y X a O b wherein 1≤x≤2.5, 0.5<y≤1, 5≤a≤6.5, 0.01<b / a<0.1, M is selected from at least one of Fe and Mo, and X is selected from at least one of F, Cl, Br, and I and contains Cl. The present invention can further achieve good air stability on the basis of ensuring high ionic conductivity by adjusting the composition and structure of the solid electrolyte material, thereby ultimately achieving a balance of excellent properties such as low cost, high ionic conductivity, and high air stability. Under preferred conditions, the ionic conductivity of the obtained solid electrolyte material reaches more than 1.2 mS / cm, and the ionic conductivity retention rate after air exposure reaches more than 94%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of secondary batteries, and in particular to a solid electrolyte material and a solid-state lithium battery. Background Art

[0002] With the accelerated development of the new energy vehicle market and industry, automobile safety accidents caused by thermal runaway of power batteries have occurred frequently. Due to the use of non-flammable inorganic electrolyte materials, solid-state lithium batteries with high safety characteristics are considered to be the next generation of advanced energy storage and conversion devices.

[0003] Solid electrolyte material is the core of solid-state batteries and the focus of research and development in the industry. CN112204675A discloses a solid electrolyte material Li 6-4a M a X6, M is at least one element selected from Zr, Hf and Ti, X is a halogen element, wherein Li 2.4 Zr 0.9 Cl6 exhibits an ionic conductivity of 4.9*10 -4 S / cm, this material avoids the defect of sulfide electrolytes that they easily release toxic gas H2S, and because its main components are cheap Zr and Cl, it has great advantages in manufacturing costs. However, the solid electrolyte materials under the existing technology still have poor ion conductivity and poor stability with humid air. They are easy to react with moisture in the air, causing performance degradation.

[0004] CN112838264A discloses a halide solid electrolyte material Li a MeX b O c , oxygen is introduced into the existing halide solid electrolyte material, and the ratio between the elements is controlled at the same time, so as to obtain a halide solid electrolyte material with higher ionic conductivity and higher air stability. However, the ionic conductivity retention rate of the solid electrolyte material after air exposure is only 87.4% at most, which still needs to be improved. That is, it is still necessary to obtain a solid electrolyte material with higher air stability while ensuring high ionic conductivity. Summary of the invention

[0005] In view of the problems existing in the prior art, the present invention provides a solid electrolyte material and a solid-state lithium battery, which achieve excellent performance such as low cost, high ion conductivity, and high air stability by adjusting the composition and structure of the solid electrolyte material.

[0006] The present invention provides a solid electrolyte material having Li x Zr y M 1-y X a O bThe composition of , wherein 1≤x≤2.5, 0.5<y≤1, 5≤a≤6.5, 0.01<b / a<0.1,

[0007] M is selected from at least one of Fe and Mo,

[0008] X is selected from at least one of F, Cl, Br, and I, and includes Cl.

[0009] The present invention has found that when the solid electrolyte material has the above composition, it can achieve good air stability while ensuring high ionic conductivity, and the ionic conductivity retention rate of the solid electrolyte material after being exposed to air is higher than 94%. In the prior art, solid electrolyte materials are generally prepared by randomly selecting metals such as Zr, Y, Yb, In, Hf, and Ti and combining them with metal Li. However, the present invention has found that by fixing Zr, combining metals Fe and Mo, and adjusting the ratio of O element to X element, a solid electrolyte material with better performance and more comprehensive can be obtained.

[0010] Furthermore, the molar ratio of Zr to M satisfies 1<y / (1-y)<5. The present invention has found that when the molar ratio of Zr to M is greater than 5, a solid electrolyte material with a crystal structure belonging to the cubic system can be realized, which has a molecular weight of >7.5*10 -4 When the molar ratio of Zr to M is greater than 1 and less than 5, a solid electrolyte material with a crystal structure belonging to the orthorhombic system can be realized, which has a conductivity of >10 -3 S / cm. When the molar ratio of Zr to M is less than 1, its crystal structure belongs to the hexagonal system and the ionic conductivity is less than 5*10 -4 S / cm. It is speculated that the reason for this phenomenon is that the activation energy of lithium ion migration in the crystal structure of the first two crystal systems is lower and the ion diffusion kinetic conditions are better.

[0011] Therefore, it is further preferred that the crystal structure of the solid electrolyte material of the present invention belongs to the cubic system or the orthorhombic system.

[0012] Furthermore, in the above solid electrolyte material composition, 1.5<x / y<3.5, 3.0<a / y<9.0. Furthermore, 1.8<x / y<3.0, 5.0<a / y<7.0.

[0013] By adopting the above chemical components and adjusting the content of each element, the lithium ion carrier concentration and the lithium vacancy concentration can work synergistically, optimize the lithium ion diffusion path, and reduce the lithium ion migration barrier, so that lithium ions become easier to conduct and higher ionic conductivity can be achieved.

[0014] Furthermore, in the element X, the molar fraction of Cl is greater than 50%.

[0015] The study found that higher ionic conductivity can be achieved under the above conditions. Specifically, it is due to Cl - Compared with F - Br - with I - , can better communicate with Li + and Zr 4+ The ions form a crystal structure that can be transported by lithium ions, resulting in higher ionic conductivity.

[0016] Furthermore, in X-ray diffraction measurement using CuKα rays, there are diffraction peaks in a first range of diffraction angle 2θ values ​​of 14.5° to 15.4°, a second range of diffraction angle 2θ values ​​of 29.9° to 30.8°, and a third range of diffraction angle 2θ values ​​of 62.6° to 63.4°.

[0017] Furthermore, in X-ray diffraction measurement using CuKα rays, there are diffraction peaks in a first range of diffraction angle 2θ values ​​of 16.0° to 16.9°, a second range of diffraction angle 2θ values ​​of 31.3° to 32.4°, and a third range of diffraction angle 2θ values ​​of 35.5° to 36.8°.

[0018] Even if the chemical formula composition of the solid electrolyte material is the same, its crystal structure may be different due to the different preparation environment (temperature T, pressure P, etc.), so their physical and chemical properties are also different (isomeric phenomenon). The present invention has found that according to the above crystal structure, a solid electrolyte material with higher lithium ion conductivity can be achieved. Specifically, by adjusting the diffraction peak to a crystal structure within the above range, the bond energy between the halogen anion and the intermediate ion is stronger, and the Bragg equation is quoted to adjust the interplanar spacing through different XRD peak positions, thereby optimizing the lithium ion diffusion channel, making lithium ions easier to conduct, and further improving the lithium ion conductivity of the solid electrolyte.

[0019] The present invention also provides a method for preparing the solid electrolyte material, which can adopt a high-energy ball milling method or a high-temperature melting method.

[0020] Specifically, in one embodiment of the present invention, the preparation method comprises: mixing ZrCl4, LiCl and Li2O raw materials, heating to above 300°C under vacuum or inert gas conditions for sintering. The proportion of each raw material is determined according to the composition of the solid electrolyte material. For example, the solid electrolyte material composition is Li2ZrCl 5.4 O 0.3 The raw materials are ZrCl4, LiCl and Li2O in a molar ratio of 1:1.4:0.3.

[0021] When the solid electrolyte material also includes metal M, the raw material also includes a halide of metal M. For example, the solid electrolyte material composition is Li2Zr 0.7 Fe 0.3 Cl 5.1 O 0.3 , the raw materials are ZrCl4, FeCl3, LiCl and Li2O in a molar ratio of 0.7:0.3:1.4:0.3.

[0022] The present invention also provides a solid-state lithium battery, comprising a positive electrode layer, a negative electrode layer and a solid electrolyte layer formed between the positive electrode layer and the negative electrode layer, wherein at least one of the positive electrode layer, the negative electrode layer and the solid electrolyte layer contains any of the above-mentioned solid electrolyte materials.

[0023] The present invention provides a solid electrolyte material and a solid lithium battery. By adjusting the composition and structure of the solid electrolyte material, it is possible to further achieve good air stability on the basis of ensuring high ionic conductivity, thereby ultimately achieving a balance of excellent performances such as low cost, high ionic conductivity, and high air stability. Under preferred conditions, the ionic conductivity of the obtained solid electrolyte material reaches more than 1.2 mS / cm, and the ionic conductivity retention rate after air exposure reaches more than 94%. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Unless otherwise stated, the raw materials and auxiliary materials involved in the following examples can be purchased from the market.

[0026] Example 1

[0027] This embodiment provides a solid electrolyte material composed of Li2ZrCl 5.4 O 0.3 , and its preparation method is as follows:

[0028] In an Ar-filled glove box, ZrCl4, LiCl and Li2O were weighed in a molar ratio of 1:1.4:0.3, mixed evenly, heated to 400°C under vacuum conditions for 12 hours, and ground and crushed after cooling. The obtained product is the target solid electrolyte material.

[0029] Characterization and analysis of crystal structure:

[0030] X-ray diffraction was used to measure the CuKα radiation with a wavelength of The step size was 0.02° and the scanning speed was 10° / min.

[0031] Evaluation of ionic conductivity:

[0032] The ionic conductivity of the material was tested by the AC impedance method based on ion blocking electrode (BE / SSE / BE). The test method was as follows: 150 mg of electrolyte material was weighed in a glove box, and then the tablets were pressed in a mold battery at a pressure of 300 MPa. The thickness of the electrolyte layer was measured and recorded as L. Subsequently, a carbon / electrolyte / carbon symmetrical blocking electrode battery was assembled in the mold battery, and the AC impedance of the battery under open circuit conditions was measured. The impedance value was recorded as R and calculated using the formula σ=L / (R·A), where σ is the ionic conductivity, L is the thickness of the electrolyte layer, R is the impedance value, and A is the electrode area of ​​the electrolyte sheet.

[0033] Production and electrochemical performance testing of lithium secondary batteries:

[0034] The solid electrolyte material in the embodiment is matched with LiNi 0.6 Co 0.2 Mn 0.2 O2 positive electrode material and assembled battery for charge and discharge test. The specific test method is: weigh 70 mg of electrolyte material in the glove box, and then press it into tablets in the mold battery at a pressure of 300 MPa. Add 10 mg of a mixture of electrolyte material and positive electrode material to one end of the electrolyte with a mass ratio of 3:7, and press it for the second time at a pressure of 300 MPa. Add sulfide ion conductor and metal indium sheet to the other end of the electrolyte in turn, and press it for the third time at a pressure of 50 MPa, and perform constant current charge and discharge test at a rate of 0.1C.

[0035] Example 2-18

[0036] The composition of the solid electrolyte material provided in each embodiment is shown in Table 1. The raw materials are weighed according to the element ratio shown, and the preparation is carried out by the same preparation method as in Example 1. For example, the preparation method of the electrolyte material in Example 6 is to weigh ZrCl4, FeCl3, LiCl and Li2O in a molar ratio of 0.7:0.3:1.4:0.3 in an Ar-filled glove box, mix them evenly, heat them to 400°C under vacuum conditions for 12 hours, grind and crush them after cooling, and the obtained product is Li2Zr 0.7 Fe 0.3 Cl 5.1 O 0.3 Solid electrolyte materials.

[0037] After each solid electrolyte material was prepared, various tests were performed according to the same test methods as in Example 1. The results are shown in Table 1.

[0038] Table 1 Performance test results of solid electrolyte materials in various embodiments

[0039]

[0040]

[0041] When the molar ratio of O to halogen X in the solid electrolyte material is above 0.01 and below 0.1, better air stability and interfacial chemical stability with the positive electrode oxide material can be achieved. For example, in Example 6, the molar ratio of O to halogen X is above 0.01 and below 0.1, and at this time, very good ionic conductivity after air exposure is exhibited, while for Examples 11 to 18, the molar ratio of O to halogen X is above 0.1. Although the air exposure ion conductivity retention rate increases, due to its low initial ion conductivity, its ion conductivity after air exposure is low, and thus the battery capacity is correspondingly reduced. Wherein, ion conductivity retention rate = ion conductivity after exposure / ion conductivity before exposure.

[0042] The present invention also provides a solid electrolyte material having the following composition, and the same determination method is used to perform performance tests, and the results are shown in Table 2.

[0043] Table 2 Performance test results of solid electrolyte materials in various comparative examples

[0044]

[0045] It can be seen from the above results that since the compositions of Comparative Examples 1-4 are different from those of the present invention, their ion conductivity retention rates and battery specific capacities are relatively low.

[0046] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A solid electrolyte material, characterized in that: With Li x Zr y M 1-y X a O b The composition of , wherein 1≤x≤2.5, 0.5<y<1, 5≤a≤6.5, 0.01<b / a<0.1, M is selected from at least one of Fe and Mo, and the molar ratio of Zr to M satisfies 1<y / (1-y)<5; X is selected from at least one of F, Cl, Br, and I and contains Cl, and the molar fraction of Cl in element X is greater than 50%; The crystal structure of the solid electrolyte material belongs to a cubic system or an orthorhombic system.

2. The solid electrolyte material according to claim 1, characterized in that 1.5<x / y<3.5, 3.0<a / y<9.

0.

3. The solid electrolyte material according to claim 2, characterized in that 1.8<x / y<3.0, 5.0<a / y<7.

0.

4. The solid electrolyte material according to claim 1, characterized in that In X-ray diffraction measurement using CuKα rays, there are diffraction peaks in a first range of diffraction angle 2θ values ​​of 14.5° to 15.4°, a second range of diffraction angle 2θ values ​​of 29.9° to 30.8°, and a third range of diffraction angle 2θ values ​​of 62.6° to 63.4°.

5. The solid electrolyte material according to claim 1, characterized in that In X-ray diffraction measurement using CuKα rays, diffraction angles 2θ have diffraction peaks in a first range of 16.0° to 16.9°, a second range of 31.3° to 32.4°, and a third range of 35.5° to 36.8°.

6. A solid-state lithium battery, characterized in that: The invention comprises a positive electrode layer, a negative electrode layer and a solid electrolyte layer formed between the positive electrode layer and the negative electrode layer, wherein at least one of the positive electrode layer, the negative electrode layer and the solid electrolyte layer contains the solid electrolyte material according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Halide solid electrolyte material and battery using same

    CN112204675A

  • Solid electrolyte material, preparation method thereof and solid-state lithium battery

    CN112838264A

  • Battery arrays, constructions and method

    CN102823021A

  • Ceramic garnet based ionically conducting material

    US20180013171A1

  • Mixed ionic and electronic conductor for solid state battery

    US20200259211A1