Polyamide-imide polymers, polymer compositions and articles containing the same, and methods for preparing the same

By using melt polymerization method and specific components in the preparation process of PAI polymer, the problem of low fluidity and solubility of the polymer is solved, and the preparation of PAI polymer with high glass transition temperature and good mechanical properties is achieved, which is suitable for Various applications.

CN114364719BActive Publication Date: 2024-10-01SOLVAY SPECIALTY POLYMERS USA LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080062915.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-09
Filing Date
2020-09-08
Publication Date
2024-10-01
Estimated Expiration
2040-09-08

AI Technical Summary

Technical Problem

Existing polyamide-imide (PAI) polymers suffer from high-temperature cross-linking side reactions, low fluidity and solubility problems during the preparation process, which limit their processability and application potential.

Method used

Using a melt polymerization method, a reaction mixture containing an alicyclic acid component and a diamine component containing three carboxyl moieties is used to maintain a uniform liquid state at a temperature of at least 200°C, avoiding the use of organic solvents and achieving colorless results. Preparation of transparent PAI polymers.

Benefits of technology

A PAI polymer with low branching and good mechanical properties was obtained, which improved its solubility and melt processability. It can be processed into films and other products through conventional polymer processing technology, while maintaining excellent thermal and mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FDF0000030458580000011
    Figure FDF0000030458580000011
  • Figure FDF0000030458580000021
    Figure FDF0000030458580000021
  • Figure FDF0000030458580000022
    Figure FDF0000030458580000022
Patent Text Reader

Abstract

A method for preparing a polyamide-imide (PAI) polymer is provided. The method comprises melt polymerizing a reaction mixture comprising: at least one alicyclic acid component comprising three carboxyl moieties selected from the group consisting of carboxylic acid, anhydride and ester functional groups; and at least one diamine component. The method comprises maintaining the reaction mixture in a liquid state during polymerization at a temperature of at least 200°C.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application is international application No. PCT / EP2020 / 074992 filed on September 8, 2020, which has entered the national phase, and claims priority to U.S. Provisional Application No. 62 / 897,473 filed on September 9, 2019, and the entire contents of each of the applications are incorporated into this application by reference. Technical Field

[0003] Provided are polyamide-imide (PAI) polymers, polymer compositions comprising the same, methods for preparing the same, and articles comprising the same. Background Art

[0004] Polyamide-imides (PAI) are high-performance polymers with excellent thermal, chemical and mechanical properties and are therefore suitable for demanding applications requiring high mechanical strength, stiffness and low friction combined with high temperature resistance, corrosion resistance and wear resistance. For these reasons, they are widely used in the aerospace and automotive industries and as insulating materials, coatings, solvent-resistant films, and in electronic devices.

[0005] PAI polymers contain both amide and imide functional groups in the backbone. Therefore, PAI polymers tend to exhibit a hybrid nature of polyamides and polyimides. The increased rigidity of the imide group imparts better hydrolysis, chemical and thermal stability and excellent mechanical properties to polymers, especially those based on aromatic monomers. Most commercial PAI polymers are indeed aromatic, typically based on trimellitic acid, trimellitic anhydride or trimellitic acid halides.

[0006] In the preparation of PAI, imide is formed by the reaction between two adjacent carboxylic acid groups (or their derivatives, such as acyl halides, anhydrides and esters) and a primary amine-containing molecule. Initially, an amic acid is formed, which closes into an imide ring after further removal of a water molecule.

[0007] Imidization reactions generally require high temperatures, especially for PAI polymers based on aromatic monomers. However, the use of high temperatures results in crosslinking side reactions, resulting in PAI polymers with limited processability or even a thermoset-like structure. Although the PAI polymers are chemically stable, their use in certain applications is limited due to their low flow during melt processing, their thermal intractability (i.e., their low melt processability) in conventional processing methods, and their low solubility.

[0008] Several attempts have been made to improve these properties while maintaining the good thermal and mechanical properties of the PAI polymers, notably by grafting these polymers, blending them with other types of polymers and / or forming composites with additives and inorganic fibers.

[0009] Other attempts to improve the solubility and processability of the PAI polymer involve incorporating flexible bonds and alicyclic units into the PAI polymer chain. For example, JP 2017-186560 discloses PAI based on cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (CTA) (instead of trimellitic anhydride) and meta-xylylenediamine (MXD). The method described in this document is carried out in a solution of an organic solvent. The use of organic solvents exhibits great disadvantages. First, additional stages are required to recover the polymer after synthesis, such as precipitating the polymer from a non-solvent and washing and drying the polymer. Second, some solvents are toxic. Third, the polymer typically contains a residual amount of solvent, which may affect the mechanical properties of the polymer or its use in certain applications. In other cases, the solvent may cause color problems.

[0010] US2011 / 160407 relates to a method for preparing PAI polymers by melt polymerization of at least one aromatic organic compound having a carboxyl group, at least one diamine compound and optionally at least one dibasic acid compound. This document more precisely describes the use of trimellitic acid, pyromellitic acid, or anhydrides, esters or amides of these as aromatic organic compounds. However, the aromaticity of these reaction materials imparts color (yellow to orange to red) to the polymer.

[0011] None of the above listed references describe an organic solvent-free polymerization process for preparing PAI polymers and the art would greatly benefit from such. Summary of the invention

[0012] In a first aspect, a method for preparing a polyamide-imide (PAI) polymer is provided. The method comprises a reaction mixture in which the molten polymer comprises:

[0013] a) at least one cycloaliphatic acid component comprising three carboxyl moieties selected from the group consisting of carboxylic acid, anhydride and ester functional groups; and

[0014] b) at least one diamine component.

[0015] The reaction mixture is maintained in a homogeneous liquid state during the polymerization and at a temperature of at least 200°C.

[0016] In a second aspect, a polyamide-imide (PAI) polymer obtained by the method is provided.

[0017] In a third aspect, a polymer composition comprising the PAI polymer is provided.

[0018] In a fourth aspect, an article comprising the PAI polymer or the polymer composition is provided. DETAILED DESCRIPTION

[0019] A method for preparing a polyamide-imide (PAI) polymer is provided. The method includes melt polymerization of at least one alicyclic acid component and at least one diamine component. The alicyclic acid component contains three carboxyl moieties selected from the group consisting of carboxylic acid, anhydride and ester functional groups. The method further includes maintaining the reaction mixture in a homogeneous liquid state at a temperature of at least 200° C. during polymerization.

[0020] A colorless, transparent PAI polymer with low branching and good mechanical properties is also provided. Thus, this PAI polymer can be processed into films and other articles using standard polymer processing techniques such as extrusion and injection molding.

[0021] PAI polymers show low and controlled branching, which contributes to the optimized properties (e.g., improved solubility, melt processability and moldability) shown by PAI polymers combined with good thermal and mechanical properties such as high glass transition temperature (Tg). Specifically, PAI polymers can be easily processed using conventional polymer processing techniques such as extrusion and injection molding. In addition, PAI polymers can be easily converted into films and other articles. Articles comprising PAI polymers or polymer compositions comprising PAI polymers are transparent and colorless with a low yellowness index.

[0022] In this specification, unless otherwise specified, the following terms are interpreted as follows.

[0023] "Alicyclic moiety" means an organic group containing at least one aliphatic ring and no aromatic ring. The alicyclic moiety may be substituted by one or more linear or branched alkyl or alkoxy groups and / or halogen atoms and / or may contain one or more heteroatoms in the ring, such as nitrogen, oxygen and sulfur.

[0024] The term "alkyl" and derivative terms such as "alkoxy" include within their scope straight chain, branched chain and cyclic moieties. Examples of alkyl groups are methyl, ethyl, 1-methylethyl, propyl, 1,1-dimethylethyl and cyclopropyl. Unless otherwise expressly indicated, each alkyl group may be unsubstituted or substituted with one or more substituents including, but not limited to, hydroxy, sulfo, C 1 -C 6 Alkoxy and C 1 -C 6Alkylthio groups, provided that the substituents are sterically compatible and satisfy the rules of chemical bonding and strain energy.

[0025] The term "halogen" or "halo" includes fluorine, chlorine, bromine and iodine, with fluorine being preferred.

[0026] Alicyclic acid component

[0027] The PAI polymer is prepared from a reaction mixture comprising an alicyclic acid component, a diamine component and optionally a dibasic acid component. In a preferred embodiment, the alicyclic acid component is according to any one of formulas (I) and (II):

[0028]

[0029] in:

[0030] -Z is an alicyclic moiety selected from the group consisting of a substituted or unsubstituted monocyclic or polycyclic group having 5 to 50 carbon atoms, preferably 6 to 18 carbon atoms;

[0031] -Y is OR a , where R a is H or an alkyl group, preferably an alkyl group having 1 to 5 carbon atoms, and

[0032] - In formula (II), at least two Y(C=O) are attached to 2 adjacent carbon atoms of Z, meaning that at least two carboxyl moieties are in ortho position relative to each other.

[0033] Preferably, Z is an alicyclic moiety containing from one to four aliphatic rings. If Z contains more than one aliphatic ring, i.e. two aliphatic rings or more, the aliphatic rings may be condensed or bridged together directly or via the following bridges: -O-, -CH 2 -、-C(CH 3 ) 2 -、-C(CF 3 ) 2 -, or-(CF 2 ) q -, wherein q is an integer from 1 to 5. The term "directly" means that the aliphatic rings are linked together through a bond.

[0034] Preferably, Z is a trivalent alicyclic moiety selected from the group consisting of moieties having formula (III-A), (III-B), (III-C) and (III-D):

[0035]

[0036] and the corresponding substituted structures,

[0037] Where X is -O-, -CH2 -、-C(CH 3 ) 2 -、-C(CF 3 ) 2 -, or-(CF 2 ) q -, and q is an integer from 1 to 5.

[0038] In a preferred embodiment, the alicyclic acid component is according to any one of formulas (Ia) and (IIa):

[0039]

[0040] According to this embodiment, the method comprises:

[0041] - melt polymerizing an alicyclic acid component according to formula (Ia) and at least one diamine component,

[0042] - melt polymerizing an alicyclic acid component according to formula (IIa) and at least one diamine component, or

[0043] - melt polymerizing a mixture of cycloaliphatic acid components according to formula (Ia) and (IIa) and at least one diamine component.

[0044] Diamine component

[0045] The reaction mixture subjected to melt polymerization further comprises at least one diamine component. The diamine component used in the method can be aliphatic, alicyclic or aromatic. The diamine component comprises at least two amine moieties (-NH 2 ) and optionally at least one heteroatom, which is preferably selected from the group consisting of N, S and O.

[0046] The diamine component is preferably represented by the formula:

[0047] H 2 NR-NH 2 (IV)

[0048] wherein R is a C4 to C50 divalent hydrocarbon group, specifically a divalent aliphatic, alicyclic or aromatic hydrocarbon group.

[0049] The diamine component is preferably selected from the group consisting of putrescine, cadaverine, hexamethylenediamine, 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 1,9-diaminononane, 2-methyl-1,8-diaminooctane, dodecamethylenediamine, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, isophoronediamine, 1,4-diaminocyclohexane, 1,3-diaminocyclohexane, 4,4′-methylenebis(cyclohexylamine), 4,4′-methylenebis(2-methylcyclohexylamine), p-xylylenediamine, m-xylylenediamine, and mixtures thereof.

[0050] The diamine component may comprise different diamines, for example a mixture of two or three different diamines.

[0051] Preferably, at least 50 mol.%, more preferably at least 65 mol.%, even more preferably at least 80 mol.%, most preferably at least 95 mol.% of the diamine component is cycloaliphatic, based on the total moles of diamines in the diamine component.

[0052] According to an embodiment, the diamine component comprises a cycloaliphatic diamine, such as a mixture of two or three different cycloaliphatic diamines.

[0053] According to another embodiment, the diamine component comprises only one cycloaliphatic diamine. In such embodiments, the diamine is preferably 1,3-bis(aminomethyl)cyclohexane.

[0054] Dibasic acid components

[0055] The reaction mixture subjected to melt polymerization optionally further comprises at least one dibasic acid component or a derivative thereof.

[0056] The expression "derivatives thereof" indicates derivatives that can react under polycondensation conditions to produce amide bonds. Examples of dibasic acid derivatives that form amide bonds include substituted or unsubstituted acyl groups, such as aliphatic acyl groups and aromatic acyl groups. Examples of acyl groups include, but are not limited to, formyl, acetyl, propionyl, butyryl, isobutyryl, valeryl, isovaleryl, pivaloyl, benzoyl, toluoyl, and xylol.

[0057] The dibasic acid component may be aliphatic, alicyclic or aromatic, and optionally contains at least one heteroatom selected from the group consisting of N, S and O.

[0058] The dibasic acid component is preferably represented by the formula:

[0059] HOOC-R'-COOH (V)

[0060] wherein R' is a C4 to C18 divalent hydrocarbon group, specifically a divalent aliphatic, alicyclic or aromatic hydrocarbon group.

[0061] The dibasic acid component is preferably selected from the group consisting of adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, isophthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenylcarboxylic acid, 5-hydroxyisophthalic acid, 5-sulfophthalic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, and mixtures thereof.

[0062] Melt Polymerization

[0063] The PAI polymer is provided by a process comprising melt polymerization of the above components. More specifically, the process comprises combining an alicyclic acid component, a diamine component, and an optional dibasic acid component to provide a reaction mixture, and maintaining the reaction mixture in a homogeneous liquid state during polymerization at a temperature of at least 200°C.

[0064] The term "melt polymerization" means maintaining the reaction mixture in a homogeneous liquid state during polymerization at a temperature of at least 200°C.

[0065] In the context of the present invention, the phrase "maintained in a homogeneous liquid state" means that the reaction mixture remains in a liquid state without any solidification and / or precipitation of the resulting PAI polymer.

[0066] During polymerization, the reaction mixture is continuously heated to an elevated temperature so that the PAI polymer being prepared is in a molten state. The minimum temperature to which the reaction mixture should be heated can generally be determined based on the melting point or softening point of the PAI polymer being prepared. The melting point or softening point of the PAI polymer being prepared can vary with polymerization time, based on the amount of reactants involved in the reaction, notably the amount of the limiting reactant, if, for example, one of the reactants is gradually added to the reaction mixture. In this case, the melting point or softening point of the PAI polymer being prepared can be determined based on the complete conversion of the limiting reactant monomer. Since the limiting reactant can be sequentially added to the reaction mixture, multiple temperature increases / heating may be required to prepare the PAI polymer of the present invention. Each step of the polymerization process is then performed at a temperature not lower than the melting point or softening point of the PAI polymer being produced.

[0067] The process is carried out in the absence of an organic solvent. In other words, the process is free of organic solvent, which means that the reaction mixture does not contain an organic solvent, or contains an amount of organic solvent of less than 1 wt.%, less than 0.5 wt.%, or even less than 0.2 wt.%, based on the total weight of the reaction mixture. The process may include water as a solvent.

[0068] In some embodiments, the method is carried out in the absence of added water, or in the presence of less than 50 wt.%, preferably less than 40 wt.%, more preferably less than 30 wt.%, even more preferably less than 15 wt.%, and most preferably less than 5 wt.% of added water based on the total weight of the reaction mixture.

[0069] Thus, the reaction mixture may be an aqueous solution comprising the above components (i.e., at least one alicyclic acid component, at least one diamine component and optionally at least one dibasic acid component). Preferably, the reaction mixture comprises water as a solvent, since this facilitates stirring of the reaction mixture and thus facilitates its homogeneity.

[0070] According to various embodiments, the cycloaliphatic acid component or the diamine component is added to the reaction mixture sequentially, gradually, or continuously.

[0071] Preferably, the reaction mixture contains the aliphatic acid component and the diamine component in a ratio (CAC:DC) ranging from 0.8 to 1.2, preferably from 0.9 to 1.1, more preferably from 0.95 to 1.05, even more preferably from 0.97 to 1.03.

[0072] When the method of the present invention uses a dibasic acid component, the dibasic acid component and the diamine component may be introduced at least partially in the form of a salt of the dibasic acid and the diamine component.

[0073] PAI polymers are generally obtained by polycondensation between one or more cycloaliphatic acid components, one or more diamine components and optionally one or more dibasic acid components to form polyamide-imide chains, forming elimination products, especially water. Preferably, the water produced in the process is evaporated, for example by fractional distillation using a condenser at a pressure between 1 mbar and 30 bar.

[0074] The reaction mixture is maintained in a homogeneous liquid state during the polymerization at a temperature of at least 200° C., preferably from 215° C. to 300° C., in order to evaporate water (initially present in the reaction mixture and / or formed during the polycondensation) while preventing the formation of any solid phase in order to prevent the mixture from solidifying.

[0075] For at least a portion of the method, the method can be carried out under pressure. In these cases, a maximum pressure of 20 bar, preferably a maximum pressure of 10 bar, more preferably a maximum pressure of 3 bar is used. The end of the process is preferably carried out under low pressure (vacuum or atmospheric pressure) to drive the reaction to completion and more easily remove the water produced in the process.

[0076] The method can be carried out in an apparatus made of a material that is inert to the above-mentioned components (i.e., the alicyclic acid component, the diamine component and the optional dibasic acid component). In this case, the apparatus is selected to provide sufficient contact between the components and to make it feasible to remove volatile reaction products, notably water. Suitable apparatus include stirred reactors, extruders and kneaders. The reaction vessel is preferably equipped with a stirring device, such as a rotating shaft.

[0077] Chain limiters or end-cappers can be added to the reaction mixture to control the molecular weight of the resulting PAI polymer. Chain limiters or end-cappers are molecules that have only one reactive site with amines and / or carboxylic acids. Examples of end-cappers are monoamines, such as benzylamine and 1-hexylamine, and monocarboxylic acids, such as acetic acid, propionic acid, benzoic acid, phthalic acid or anhydrides.

[0078] Preferably, the order in which the components are introduced into the reaction vessel in this process is as follows: water is added first, then the diamine component is charged and finally the cycloaliphatic acid component and optionally the dibasic acid component are added.

[0079] Preferably, an inert gas such as nitrogen is introduced into the reaction vessel to replace the atmosphere in the vessel. Preferably, the reaction vessel is purged with the inert gas before and after all the above components are loaded. Preferably, the flow of the inert gas is maintained during this process.

[0080] Polyamide-imide polymer

[0081] There is also provided a polyamide-imide (PAI) polymer obtainable by the process defined above.

[0082] Preferably, the PAI polymer has a Tg of at least 100°C, more preferably at least 120°C, even more preferably at least 140°C, most preferably at least 150°C, as determined by DSC according to ASTM D3418.

[0083] Preferably, the PAI polymer has a Tg of at most 250°C, more preferably at most 240°C, even more preferably at most 230°C, most preferably at most 220°C, as determined by DSC according to ASTM D3418.

[0084] Preferably, the PAI polymer has a number average molecular weight (Mn) of at least 5,000 g / mol, more preferably at least 10,000 g / mol, even more preferably at least 15,000 g / mol, as determined by gel permeation chromatography (GPC) using a fluorinated solvent, a 2HFIP gel column, and a UV-vis / refractive index detector.

[0085] Preferably, the PAI polymer has an Mn of at most 50,000 g / mol, more preferably at most 45,000 g / mol, even more preferably at most 40,000 g / mol, as determined by gel permeation chromatography (GPC) using a fluorinated solvent, a 2HFIP gel column and a UV-vis / refractive index detector.

[0086] Advantageously, the PAI polymer is soluble in a variety of solvents, notably hexafluoro-2-propanol, o-cresol, 98% sulfuric acid, and dimethylformamide.

[0087] The PAI polymer obtained by this method is in molten form and can therefore be formed directly or can be processed using conventional polymer processing techniques such as extrusion and injection molding for subsequent shaping after melting.

[0088] In addition, the PAI polymers according to the present invention can be easily converted into films and other articles. Because the PAI polymers of the present invention are soluble in a variety of organic solvents, films can be advantageously made by casting a solution containing the PAI polymer and then evaporating the solvent according to standard methods known to those skilled in the art. Specifically, the film can be made by dissolving the PAI polymer in a solvent to obtain a solution, casting the solution on a substrate and finally evaporating the solvent.

[0089] The PAI polymer can be used in a large number of applications, in particular for making yarns, fibers or filaments, or films, or for shaping articles by injection molding, extrusion or extrusion / blow molding. It can be used in particular in engineering plastic compositions.

[0090] Polymer composition

[0091] Also provided are polymer compositions comprising the PAI polymers.

[0092] Preferably, the PAI polymer is present in the polymer composition in an amount of at least 10 wt.%, more preferably at least 15 wt.%, even more preferably at least 20 wt.%, most preferably at least 25 wt.%, based on the total weight of the polymer composition.

[0093] Preferably, the PAI polymer is present in the polymer composition in an amount of at most 99 wt.%, more preferably at most 95 wt.%, even more preferably at most 80 wt.%, most preferably at most 60 wt.%, based on the total weight of the polymer composition.

[0094] According to an embodiment, the PAI polymer is present in the polymer composition in an amount ranging from 10 to 70 wt. %, preferably from 20 to 60 wt. %, based on the total weight of the polymer composition.

[0095] According to an embodiment, the polymer composition comprises at least one additional additive selected from the group consisting of reinforcing agents, colorants, dyes, pigments, lubricants, plasticizers, flame retardants, nucleating agents, heat stabilizers, light stabilizers, antioxidants, processing aids, fluxes, electromagnetic absorbers and combinations thereof.

[0096] Reinforcement agent is also called reinforcing filler or fiber, can be selected from the group consisting of fiber reinforced filler, particle reinforced filler and mixture thereof. Fiber reinforced filler is considered herein as having length, width and thickness of the material, wherein the average length is significantly greater than both width and thickness. In general, fiber reinforced filler has an aspect ratio (defined as the average ratio between the largest of length and width and thickness) of at least 5, at least 10, at least 20 or at least 50.

[0097] Fiber-reinforced fillers include glass fibers, carbon fibers or graphite fibers, and fibers formed from silicon carbide, aluminum oxide, titanium dioxide, boron, etc., and may include mixtures containing two or more such fibers. According to an embodiment, the fibers are flat fibers. Non-fiber-reinforced fillers notably include talc, mica, titanium dioxide, potassium titanate, silica, kaolin, chalk, aluminum oxide, mineral fillers, etc.

[0098] Also provided are methods of providing these polymer compositions, and the methods include mixing the PAI polymer with the at least one additional additive. Preferably, the mixing of the PAI polymer and the at least one additional additive is performed by dry blending and / or melt compounding. More preferably, the mixing of the PAI polymer and the at least one additional additive is performed by melt compounding, notably in a continuous or batch device. Such devices are well known to those skilled in the art. An example of a suitable continuous device is a screw extruder. Preferably, melt compounding is performed in a twin screw extruder.

[0099] Products

[0100] Also provided is an article comprising the PAI polymer or the polymer composition.

[0101] The article is preferably a molded article. Preferably, the article is molded from the PAI polymer or a polymer composition comprising the PAI polymer using methods well known in the art, such as by methods including but not limited to injection molding, blow molding, rotational molding, compression molding or extrusion molding.

[0102] Should the disclosure of any patents, patent applications, and publications incorporated herein by reference conflict with the description of the present application to the extent that it renders a term unclear, the present description shall take precedence.

[0103] The present invention will now be described with reference to the following examples, which are intended to be illustrative only and are not intended to limit the scope of the claims.

[0104] Experimental Section

[0105] Material

[0106] Cyclohexane-1,2,4-tricarboxylic acid-1,2-anhydride (CTA), available from Mitsubishi Gas Chemicals.

[0107] 1,3-Bis(aminomethyl)cyclohexane (1,3-BAC), available from Mitsubishi Gas Chemical Co.

[0108] Hexamethylenediamine (HMDA), available from Ascend Performance Materials.

[0109] 4,4'-Methylenebis(cyclohexylamine) (PACM), available from Sigma-Aldrich.

[0110] Phosphoric acid, available from Sigma-Aldrich.

[0111] method

[0112] Thermal Analysis

[0113] Thermal properties were determined using differential scanning calorimetry (DSC). DSC analysis was performed on a DSC Q200-5293 TA instrument according to ASTM D3418. Three scans were used for each DSC test: the first heating cycle, at 20.00°C / min to 300°C; the first cooling cycle, at 20.00°C / min to 30.00°C; the second heating cycle, at 20.00°C / min to 300.00°C. During the second heating cycle, Tg was determined from the midpoint of the transition.

[0114] GPC

[0115] Mn was measured by gel permeation chromatography (GPC) using a fluorinated solvent, a 2HFIP gel column and a UV-vis / refractive index detector.

[0116] Solubility

[0117] 5mg of PAI polymer sample was added to 5ml of solvent. The resulting mixture was stirred at room temperature for 24 to 48 hours, and any dissolution or softening of the sample was recorded. If the sample is completely dissolved, it is considered to be soluble. If the sample does not show any changes in appearance after 48 hours, it is considered to be insoluble. Solubility in hexafluoro-2-propanol (HFIP), o-cresol, 98% sulfuric acid and dimethylformamide (DMF) was tested.

[0118] Yellowness test

[0119] Films with a thickness of 0.1-0.2 mm were prepared in a hot press (280° C., 2000 lb-f). The yellowness index of the films was measured using an X-Rite Ci7800 spectrophotometer.

[0120] Mechanical Testing

[0121] As described below, the synthesized PAI 1 polymer was ground in a grinder and dried overnight at 120° C. under vacuum. The resulting material was injection molded into V-type tensile bars according to ASTM D3641 using a molding temperature of 140° C., a melt temperature of 290° C., and an injection molding pressure of 6 bar. Mechanical testing of injection molded test specimens with a gauge length of 0.3 inches was performed using an Instron 5569 machine and according to ASTM D638 at 23.2° C. and 54.7% humidity. Notched Izod impact strength was determined using the injection molded test specimens by ASTM D256.

[0122] Synthesis method

[0123] Polyamide-imide 1 (PAI 1)

[0124] CTA (53.9 g), 1,3-BAC (39.1 g), phosphoric acid (0.032 g) and deionized water (42 g) were loaded into a 300 ml reactor. The reactor was then purged with nitrogen for 5 minutes and stirred, and the polymerization reaction was carried out by heating to 280° C. within 2 hours. After reaching the target temperature, the generated steam was released. A vacuum was then applied to the reactor, and the molten polymer thus obtained was then kept under this condition for another hour. After cooling, the polymer was taken out of the reactor and used for analysis.

[0125] Polyamide-imide 2 (PAI 2)

[0126] CTA (55.6 g), 1,3-BAC (25.9 g), HMDA (11.7 g), phosphoric acid (0.032 g) and deionized water (42 g) were loaded into a 300 ml reactor. The reactor was then purged with nitrogen for 5 minutes and stirred, and polymerization was carried out by heating to 280° C. within 2 hours. After reaching the target temperature, the generated steam was released. A vacuum was then applied to the reactor, and the molten polymer thus obtained was then kept under this condition for another hour. After cooling, the polymer was taken out of the reactor and used for analysis.

[0127] Polyamide-imide 3 (PAI 3)

[0128] CTA (50.7 g), PACM (27.1 g), HMDA (15.0 g), phosphoric acid (0.032 g) and deionized water (42 g) were loaded into a 300 ml reactor. The reactor was then purged with nitrogen for 5 minutes and stirred, and the polymerization reaction was carried out by heating to 280° C. within 2 hours. After reaching the target temperature, the generated steam was released. A vacuum was then applied to the reactor, and the molten polymer thus obtained was then kept under this condition for another hour. After cooling, the polymer was taken out from the reactor and used for analysis.

[0129] result

[0130] Table 1 shows the Tg, Mn, yellowness index and solubility results of the prepared PAI 1, PAI 2 and PAI 3 polymers.

[0131] Table 2 shows the mechanical properties of PAI 1.

[0132] Table 1

[0133]

[0134]

[0135] Table 2

[0136]

[0137] As demonstrated in Table 1 above, PAI polymers based on CTA and different diamines (1,3-BAC, HMDA and PACM) were successfully prepared. The PAI polymers had a number average molecular weight greater than 19000 g / mol and showed a Tg ranging between 150° C. and 176° C. The Tg can be easily adjusted by varying the nature and amount of the diamine component.

[0138] The PAI polymers also show a very low yellowness index.

[0139] However, these PAI polymers were shown to be soluble in several organic solvents, indicating that they have low and controlled branching.

[0140] As demonstrated in Table 2, PAI 1 was melt processed and made into parts by injection molding, indicating that PAI 1 also exhibits melt processability and moldability. PAI 1 also shows excellent mechanical properties, combining high tensile modulus and strength.

Claims

1. A method for preparing a polyamide-imide (PAI) polymer by melt polymerizing a reaction mixture comprising: at least one alicyclic acid component comprising three carboxyl moieties selected from the group consisting of carboxylic acid, anhydride, and ester functional groups; and at least one diamine component, The process comprises maintaining the reaction mixture in a homogeneous liquid state during polymerization at a temperature of at least 200° C., in, The at least one alicyclic acid component is according to any one of formulas (I) and (II): in: Y is OR a , where R a is H or alkyl, and In formula II, at least two Y(C=O) moieties are in ortho positions relative to each other, Z is a trivalent alicyclic moiety selected from the group consisting of moieties having formula (III-A), (III-B), (III-C) and (III-D): Where X is -O-, -CH 2 -、-C(CH 3 ) 2 -、-C(CF 3 ) 2 -, or-(CF 2 ) q -,and q is an integer from 1 to 5.

2. The method according to claim 1, in, The alkyl group is an alkyl group having 1 to 5 carbon atoms.

3. The method according to claim 1, in, The at least one alicyclic acid component is according to any one of formulas (Ia) and (IIa):

4. The method according to any one of claims 1 to 3, in, The diamine component is aliphatic, cycloaliphatic or aromatic and comprises at least two amine moieties and optionally at least one heteroatom selected from the group consisting of N, S and O.

5. The method of claim 4, wherein the diamine component is selected from the group consisting of putrescine, cadaverine, hexamethylenediamine, 2,2,4-trimethylhexamethylenediamine, 2,4,4-trimethylhexamethylenediamine, 1,9-diaminononane, 2-methyl-1,8-diaminooctane, dodecamethylenediamine, 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, isophoronediamine, 1,4-diaminocyclohexane, 1,3-diaminocyclohexane, 4,4'-methylenebis(cyclohexylamine), 4,4'-methylenebis(2-methylcyclohexylamine), p-xylylenediamine, m-xylylenediamine, and mixtures thereof.

6. The method according to any one of claims 1 to 3, in, The reaction mixture further comprises at least one aliphatic, alicyclic or aromatic dibasic acid component or a derivative thereof, the dibasic acid component or a derivative thereof optionally comprising at least one heteroatom selected from the group consisting of N, S and O.

7. The method of claim 6, wherein the dibasic acid component is selected from the group consisting of adipic acid, azelaic acid, sebacic acid, dodecanedicarboxylic acid, isophthalic acid, terephthalic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenylcarboxylic acid, 5-hydroxyisophthalic acid, 5-sulfophthalic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, and mixtures thereof.

8. The method according to any one of claims 1 to 3, in, The process is carried out in the absence of organic solvents and in the presence of added water in an amount of less than 50 wt. %, based on the total weight of the reaction mixture.

9. The method according to any one of claims 1 to 3, in, The alicyclic acid component or the diamine component is added to the reaction mixture sequentially, gradually or continuously.

10. The method according to any one of claims 1 to 3, in, The water produced during the polymerization is evaporated by fractional distillation using a condenser at a pressure between 1 mbar and 30 bar.

11. The method according to any one of claims 1 to 3, in, The reaction mixture was maintained in a homogeneous liquid state during the polymerization at a temperature ranging from 215°C to 300°C.

12. The method according to any one of claims 1 to 3, in, At least 50 mol. % of the diamine component is alicyclic, based on the total moles of diamines in the diamine component.

13. The method according to any one of claims 1 to 3, in, At least 65 mol % of the diamine component is alicyclic, based on the total moles of diamines in the diamine component.

14. The method according to any one of claims 1 to 3, in, At least 80 mol. % of the diamine component is alicyclic, based on the total moles of diamines in the diamine component.

15. The method according to any one of claims 1 to 3, in, At least 95 mol. % of the diamine component is alicyclic, based on the total moles of diamines in the diamine component.

16. The method according to any one of claims 1 to 3, in, The reaction mixture contains no organic solvent or contains an amount of organic solvent less than 1 wt. % based on the total weight of the reaction mixture.

17. The method according to any one of claims 1 to 3, in, The PAI polymer has the following glass transition temperature: At least 100°C and / or Up to 250°C, As determined by DSC according to ASTM D3418.

18. The method according to any one of claims 1 to 3, in, The PAI polymer has the following glass transition temperature: At least 120°C and / or Up to 240°C, As determined by DSC according to ASTM D3418.

19. The method according to any one of claims 1 to 3, in, The PAI polymer has the following glass transition temperature: At least 140°C and / or Up to 230°C, As determined by DSC according to ASTM D3418.

20. The method according to any one of claims 1 to 3, in, The PAI polymer has the following glass transition temperature: at least 150°C, and / or Up to 220°C, As determined by DSC according to ASTM D3418.

21. The method according to any one of claims 1 to 3, in, The PAI polymer has the following number average molecular weight (Mn): At least 5,000 g / mol and / or Up to 50,000 g / mol, As determined by gel permeation chromatography using a fluorinated solvent, a 2HFIP gel column and a UV-vis / refractive index detector.

22. The method according to any one of claims 1 to 3, in, The PAI polymer has the following number average molecular weight (Mn): At least 10,000 g / mol and / or Up to 45,000 g / mol, As determined by gel permeation chromatography using a fluorinated solvent, a 2HFIP gel column and a UV-vis / refractive index detector.

23. The method according to any one of claims 1 to 3, in, The PAI polymer has the following number average molecular weight (Mn): at least 15,000 g / mol, and / or Up to 40,000 g / mol, As determined by gel permeation chromatography using a fluorinated solvent, a 2HFIP gel column and a UV-vis / refractive index detector.

24. The method according to any one of claims 1 to 3, in, The PAI polymer is soluble in hexafluoro-2-propanol, o-cresol, 98% sulfuric acid, and / or dimethylformamide.

25. A polyamide-imide (PAI) polymer obtained by the process of any one of claims 1 to 24.

26. A polymer composition comprising the PAI polymer of claim 25.

27. An article comprising the PAI polymer of claim 25 or the polymer composition of claim 26.