A cuprous oxide composite material and its preparation method and application
Cuprous oxide composite materials are prepared through the reaction method of cuprous oxide, urea and alkali, which solves the synthesis difficulties and the hazards of ammonia in the existing technology, achieves a safe and simple preparation process and improves the catalytic activity of lithium-air batteries, significantly Improved material properties.
Patent Information
- Application Number
- CN202210042688.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-01-14
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-01-14
AI Technical Summary
It is difficult to synthesize cuprous oxide and copper nitride composite materials with the existing technology, and the use of ammonia is hazardous, which limits its application.
The reaction method of cuprous oxide with urea and alkali is used to prepare cuprous oxide composite materials through heating and washing steps, avoiding the use of ammonia gas, and forming a core-shell structure material with a spherical interior and a cubic exterior.
It achieves safe and simple preparation of composite materials, improves the catalytic activity and material stability of lithium-air batteries, reduces experimental condition requirements, and significantly improves catalytic activity and performance stability.
Smart Images

Figure CN114373950B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of nano compound composite materials, and in particular to a cuprous oxide composite material and a preparation method and application thereof. Background Art
[0002] Composite materials are new materials composed of two or more materials of different properties through physical or chemical methods at the macro or micro level. They are widely used in chemistry, life, materials, physics, electronics and other fields. Composite materials grown in situ often have better catalytic activity. However, the realization of in situ growth is very difficult and they are often thin film materials, which limits their application. Therefore, it is necessary to develop new methods to construct composite materials in situ.
[0003] Copper oxides have the advantages of low price, simple preparation method, rich redox properties and good chemical stability. Recently, great progress has been made in the research on copper oxides, including the design and synthesis of copper oxides with different morphologies and structures. In addition, copper, as a 3d transition metal, has a rich electronic state structure. The combination of copper oxides with other materials can construct a special electronic state structure, and the resulting composite material is of great research significance. Copper nitride has a special electronic structure, high chemical stability and good conductivity, and has therefore received widespread attention in the field of renewable energy. However, the synthesis of copper nitride often involves the use of ammonia cylinders, and ammonia has a pungent odor and is very harmful to the human body. Long-term use of ammonia also has certain risks. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present invention is that it is difficult to synthesize cuprous oxide and copper nitride composite materials, thereby providing a cuprous oxide composite material and a preparation method and application thereof.
[0005] To this end, the present invention adopts the following technical solutions:
[0006] The present invention provides a method for preparing a cuprous oxide composite material, comprising the following steps:
[0007] S1: fully mix cuprous oxide, urea and alkali, and heat to react;
[0008] S2: washing and drying the product after the reaction to obtain the cuprous oxide composite material.
[0009] Furthermore, the molar ratio of cuprous oxide to urea and alkali is 1:5-25:5-25.
[0010] In step S1, the heating reaction temperature is 180-200°C and the reaction time is 4-10h;
[0011] In step S2, the drying temperature is 70-90°C and the drying time is 8-16h.
[0012] Preferably, the cuprous oxide is prepared by the following process:
[0013] Dissolve cupric sulfate pentahydrate in ultrapure water, add hexadecyltrimethylammonium bromide and ascorbic acid, mix, heat and stir to react; then add sodium hydroxide solution until the solution turns bright yellow, heat and stir and stand to obtain a yellow suspension; alternately use ultrapure water and anhydrous ethanol to centrifuge the suspension to obtain a dark orange solid; dry the dark orange solid to obtain a brown-yellow solid cuprous oxide.
[0014] Furthermore, the molar ratio of the copper sulfate pentahydrate, hexadecyltrimethylammonium bromide and ascorbic acid is 1:5:5.
[0015] Preferably, the base is at least one of sodium hydroxide and potassium hydroxide.
[0016] The invention also provides a cuprous oxide composite material, which is prepared by the above preparation method.
[0017] The present invention also provides an application of the cuprous oxide composite material, specifically an application in a positive electrode catalyst of a lithium-air battery.
[0018] The technical solution of the present invention has the following advantages:
[0019] (1) The present invention provides a convenient and feasible new method for in-situ synthesis of copper nitride from cuprous oxide to obtain a composite material by controlling the raw materials and reaction time; since the amount of urea used is limited, the amount of ammonia produced is small and controllable, and no ammonia cylinder is used, the experimental conditions are lower, the operation is simple and convenient, and the safety factor is high.
[0020] (2) The cuprous oxide composite material obtained by the present invention is a core-shell structure material with a spherical interior and a cubic exterior, and has a stable structure and broad application prospects.
[0021] (3) The cuprous oxide composite material obtained by the present invention is applied to lithium-air battery reaction. The nitridation of cuprous oxide plays an important role in improving the catalytic activity of lithium-air battery. The construction of the composite material can not only further improve its catalytic activity, but also improve the stability of material performance. Due to the interface effect of the composite material formed in situ, the catalytic activity is more significantly improved compared with the mechanically compounded composite material. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1 The scanning electron microscope energy dispersive spectrometer test results of the cuprous oxide composite material obtained in Example 1 of the present invention;
[0024] Figure 2 The X-ray diffraction patterns of the powders obtained in Example 1 and Comparative Examples 1-3 in Test Example 1 of the present invention;
[0025] Figure 3 The scanning electron microscope images of the powders obtained in Example 1 and Comparative Examples 1-3 in Test Example 1 of the present invention are shown;
[0026] Figure 4 TEM images of the powders obtained in Example 1 and Comparative Examples 1-3 in Test Example 1 of the present invention;
[0027] Figure 5 The discharge-charge curve of the lithium-air battery in which the powders obtained in Example 1 and Comparative Examples 1-3 are positive electrode catalysts in Test Example 2 of the present invention at a current density of 100 mA / g and a voltage range of 2.5-4.4 V;
[0028] Figure 6 The discharge-charge curve of the lithium-air battery in which the powders obtained in Example 1 and Comparative Examples 1-3 are positive electrode catalysts at a current density of 200 mA / g and a voltage range of 2.5-4.4 V in Test Example 2 of the present invention;
[0029] Figure 7 The discharge-charge curve of the lithium-air battery in which the powders obtained in Example 1 and Comparative Examples 1-3 are positive electrode catalysts at a current density of 500 mA / g and a voltage range of 2.5-4.4 V in Test Example 2 of the present invention;
[0030] Figure 8 The capacity retention rate of the lithium-air battery in which the powders obtained in Example 1 and Comparative Examples 1-3 are positive electrode catalysts in Test Example 2 of the present invention;
[0031] Fig. 9 The cycle stability of the lithium-air battery in which the powders obtained in Example 1 and Comparative Examples 1-3 are positive electrode catalysts in Test Example 2 of the present invention. DETAILED DESCRIPTION
[0032] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0033] If no specific experimental steps or conditions are specified in the examples, the experiments can be carried out according to the conventional experimental steps or conditions described in the literature in the art.
[0034] Example 1
[0035] This embodiment provides a cuprous oxide composite material, and the preparation method thereof is as follows:
[0036] (1) Synthesis of cuprous oxide
[0037] 0.16g sodium hydroxide solid is dissolved in 20mL ultrapure water, stirred and dissolved, and a transparent clear solution is formed for standby use. 0.1g copper sulfate pentahydrate is added to a beaker containing 200mL ultrapure water, stirred and dissolved, and then 7.33g hexadecyl trimethyl ammonium bromide and 0.36g ascorbic acid are added, warmed to 60°C, and stirred for 30 minutes. Subsequently, the prepared sodium hydroxide solution is added to the beaker, and the solution gradually turns bright yellow. After heating and stirring for ten minutes, it is allowed to stand to obtain a yellow suspension. The cooled suspension is alternately centrifuged and washed three times at 8000rpm with ultrapure water and anhydrous ethanol, each time for 5 minutes. The obtained dark orange solid is placed in a vacuum drying oven and dried at 60°C for 12 hours to obtain a brown solid, i.e. cuprous oxide.
[0038] (2) Nitriding of cuprous oxide
[0039] Weigh 0.1431 g of the cuprous oxide obtained in step (1), mix it evenly with 0.3003 g of urea and 0.2 g of sodium hydroxide, put it into a 25 mL reactor, place it in an oven at 200°C, and react for 6 hours. Wash the obtained solid with ultrapure water three times, place it in an oven at 80°C and dry it for 12 hours to obtain a dark brown solid, i.e., the cuprous oxide composite material. Figure 1 As shown, the obtained cuprous oxide composite material is tested by a scanning electron microscope energy dispersive spectrometer, and it can be seen that the molar ratio of the O element to the N element is 1:2. Therefore, it can be known that the molar ratio of cuprous oxide to copper nitride in the above cuprous oxide composite material is 1:2.
[0040] Example 2
[0041] This embodiment provides a cuprous oxide composite material, and the preparation method thereof is as follows:
[0042] 0.1431 g of the cuprous oxide obtained in step (1) of Example 1 was weighed, mixed evenly with 0.6006 g of urea and 0.4 g of sodium hydroxide, placed in a 25 mL reactor, and placed in an oven at 180° C. for 7 hours. The obtained solid was washed with ultrapure water three times, and then placed in an oven at 80° C. for 12 hours to obtain a dark brown solid, i.e., the cuprous oxide composite material.
[0043] Example 3
[0044] This embodiment provides a cuprous oxide composite material, and the preparation method thereof is as follows:
[0045] 0.1431 g of the cuprous oxide obtained in step (1) of Example 1 was weighed, mixed evenly with 0.3003 g of urea and 0.28 g of potassium hydroxide, placed in a 25 mL reactor, and placed in an oven at 190° C. for 4 hours. The obtained solid was washed three times with ultrapure water, and then placed in an oven at 90° C. for 16 hours to obtain a dark brown solid, i.e., the cuprous oxide composite material.
[0046] Example 4
[0047] This embodiment provides a cuprous oxide composite material, and the preparation method thereof is as follows:
[0048] 0.1431 g of the cuprous oxide obtained in step (1) of Example 1 was weighed, mixed evenly with 1.5015 g of urea and 1 g of sodium hydroxide, placed in a 25 mL reactor, and placed in an oven at 200° C. for reaction for 9 hours. The obtained solid was washed three times with ultrapure water, and then placed in an oven at 80° C. for drying for 8 hours to obtain a dark brown solid, i.e., the cuprous oxide composite material.
[0049] Example 5
[0050] This embodiment provides a cuprous oxide composite material, and the preparation method thereof is as follows:
[0051] 0.1431 g of the cuprous oxide obtained in step (1) of Example 1 was weighed, mixed evenly with 0.3003 g of urea, 0.14 g of potassium hydroxide, and 0.1 g of sodium hydroxide, and placed in a 25 mL reactor, placed in an oven at 180° C., and reacted for 10 hours. The obtained solid was washed three times with ultrapure water, and then placed in an oven at 70° C. and dried for 10 hours to obtain a dark brown solid, i.e., the cuprous oxide composite material.
[0052] Comparative Example 1
[0053] This comparative example uses the cuprous oxide prepared in step (1) of Example 1.
[0054] Comparative Example 2
[0055] The difference between this comparative example and Example 1 is that step (2) is changed to: 0.1431 g of cuprous oxide obtained in step (1) is weighed, mixed evenly with 0.3003 g of urea and 0.2 g of sodium hydroxide, put into a 25 mL reaction kettle, placed in an oven at 200° C., and reacted for 12 hours. The obtained solid is washed three times with ultrapure water, and then placed in an oven at 80° C. for 12 hours to obtain a dark brown solid.
[0056] Comparative Example 3
[0057] In this comparative example, the powders obtained in comparative example 1 and comparative example 2 were mixed thoroughly at a molar ratio of 1:2.
[0058] Test Example 1
[0059] The powder obtained in Comparative Example 1 was recorded as C-1, the powder obtained in Comparative Example 2 was recorded as C-2, the powder obtained in Example 1 was recorded as C-3, and the powder obtained in Comparative Example 3 was recorded as C-4. C-1, C-2, C-3 and C-4 were tested. Figure 2-4 .
[0060] from Figure 2 It can be seen that C-1 and C-2 have only one set of diffraction peaks, corresponding to cuprous oxide and copper nitride, respectively, indicating that they are pure phases of cuprous oxide and copper nitride, respectively; while C-3 and C-4 have two sets of diffraction peaks of cuprous oxide and copper nitride, indicating that C-3 and C-4 are composed of a combination of the two and are composite materials of cuprous oxide and copper nitride.
[0061] Figure 3 In the figure, (a), (b), (c) and (d) correspond to the scanning electron microscope images of C-1, C-2, C-3 and C-4 respectively. It can be seen that (a) shows that C-1 is spherical; (b) shows that C-2 is nearly cubic; and in (c), the morphology of C-3 is between C-1 and C-2, which is a transitional morphology from sphere to cube; (d) shows that C-4 is a mixture of sphere and cube, indicating that it is a mixture of C-1 and C-2.
[0062] Figure 4In the figure, (a), (b), (c) and (d) correspond to the transmission electron micrographs of C-1, C-2, C-3 and C-4, respectively. It can be seen that (a) shows that C-1 is spherical with a core-shell structure; (b) shows that C-2 is cubic with a core-shell structure, indicating that after a long period of urea treatment, cuprous oxide has been completely transformed into copper nitride; and in (c), C-3 is a core-shell structure with a spherical interior and a cubic exterior, which indicates that a short period of urea treatment only causes the cuprous oxide on the exterior to be nitrided and transformed into copper nitride, while the interior still maintains a cuprous oxide structure, which proves that C-3 is a composite of cuprous oxide and copper nitride; (d) shows that C-4 has both spherical and cubic core-shell structures, which once again confirms that it is a mixture of C-1 and C-2.
[0063] Test Example 2
[0064] The C-1, C-2, C-3 and C-4 powders in Test Example 1 were used as positive electrode catalysts for lithium-air batteries. The specific method was as follows: the obtained powder was weighed and mixed with carbon black and lithium naphthol in a mass ratio of 3:6:1, NMP was added as a solvent and mixed evenly, coated on carbon paper, and placed in a vacuum drying oven at 120°C for 12 hours. The dried carbon paper was cut into discs with a diameter of 12 mm, and the lithium sheet was used as the negative electrode. It was assembled with a traditional CR2032 button-type lithium-air battery module to obtain the lithium-air battery required for subsequent tests.
[0065] The obtained lithium-air battery was subjected to performance tests, such as Figure 5-9 shown.
[0066] Figure 5 The discharge-charge curves of lithium-air batteries with C-1, C-2, C-3 and C-4 as cathode catalysts were tested at a current density of 100 mA / g and a voltage range of 2.5-4.4 V. Their discharge specific capacities were 5794.9, 6529.2, 10845.8 and 7131.6 mAh / g, respectively. When the current density was increased to 200 mA / g, the Figure 6 As shown, the discharge specific capacities of lithium-air batteries with C-1, C-2, C-3 and C-4 as cathode catalysts are 4521.6, 5044.7, 8867.6 and 5617.8 mAh / g, respectively. Figure 7 In the test, the current density was further increased to 500mA / g, and the discharge specific capacities of the four lithium-air batteries were 2753.7, 4057.8, 7288.0, and 4574.2mAh / g. Figure 5-7Comparing C-1 and C-2, the catalytic activity of the material for lithium-air batteries is improved after nitridation, but the degree of improvement is not obvious; comparing C-3, C-4 with C-1 and C-2, it can be found that their catalytic activity for lithium-air batteries is greatly improved, which shows that material composite has a promoting effect on their performance; comparing C-3 and C-4, it is found that the catalytic activity of C-3 is more significantly improved, which shows that in-situ composite is more advantageous than ordinary composite.
[0067] exist Figure 8 The capacity retention rate of lithium-air batteries of materials in the figure. When the current density increases to 200mA / g, the capacity retention rates of C-1, C-2, C-3, and C-4 are 78%, 78%, 82%, and 79%, respectively; when the current density further increases to 500mA / g, the capacity retention rate of C-1 is only 48%, C-2 drops to 62%, C-3 maintains at 67%, and C-4 is 64%. Comparing C-1 with C-2, C-3, and C-4, it can be found that copper nitride plays a role in improving the capacity retention rate. The capacity retention rates of C-3 and C-4 are better than those of C-2, which shows the important role of composite materials, and C-3 is better than C-4, which shows the important role of in-situ composites.
[0068] Fig. 9 The test results of the cycle stability of lithium-air batteries with C-1, C-2, C-3 and C-4 as positive electrode catalysts are as follows: the current density of 100mA / g is used for the cut-off capacity test, and the capacity limit is 500mAh / g. It can be seen that C-1 and C-2 can be stably cycled for 94 and 100 cycles respectively, and C-4 can be stably cycled for 105 cycles, which is a slight improvement; while C-3 can maintain a stable cycle of 154 cycles, and its cycle stability has increased by 50%.
[0069] Depend on Figure 5-9 It can be seen that the nitridation of cuprous oxide plays an important role in improving the catalytic activity of its lithium-air battery, and the construction of the composite material can not only further improve its catalytic activity, but also improve the stability of the material performance. Due to the interface effect of the composite material, C-3 exhibits excellent lithium-air battery performance, and its catalytic activity is significantly improved compared to the mechanically composited C-4.
[0070] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A method for preparing a cuprous oxide composite material for a cathode catalyst of a lithium-air battery, characterized in that: The steps include: S1: fully mix cuprous oxide, urea and alkali, and heat to react, wherein the heating reaction temperature is 180-200° C., the reaction time is 4-10 hours, and the molar ratio of cuprous oxide, urea and alkali is 1: 5-25: 5-25; S2: washing and drying the product after the reaction to obtain the cuprous oxide composite material.
2. The preparation method according to claim 1, characterized in that: In step S2, the drying temperature is 70-90°C and the drying time is 8-16h.
3. The preparation method according to any one of claims 1 to 2, characterized in that: The cuprous oxide is prepared by the following process: Dissolve cupric sulfate pentahydrate in ultrapure water, add hexadecyltrimethylammonium bromide and ascorbic acid, mix, heat and stir to react; then add sodium hydroxide solution until the solution turns bright yellow, heat and stir and stand to obtain a yellow suspension; alternately use ultrapure water and anhydrous ethanol to centrifuge the suspension to obtain a dark orange solid; dry the dark orange solid to obtain a brown-yellow solid cuprous oxide.
4. The preparation method according to claim 3, characterized in that: The molar ratio of the copper sulfate pentahydrate, hexadecyltrimethylammonium bromide and ascorbic acid is 1:5:
5.
5. The preparation method according to claim 4, characterized in that: The alkali is at least one of sodium hydroxide and potassium hydroxide.
6. A cuprous oxide composite material, characterized in that: Prepared by the preparation method according to any one of claims 1 to 5.
7. The use of the cuprous oxide composite material according to claim 6, characterized in that: Cathode catalyst for lithium-air batteries.