Liquid hydrocarbon adsorption dearsenication catalyst and preparation method thereof

Through the composite carrier of activated carbon and pseudo-boehmite powder and the low-temperature-medium-high-temperature step-by-step roasting process, an efficient adsorption arsenic removal catalyst is prepared, which solves the problems of low removal efficiency, short life and complex process in the existing technology. problem, achieving efficient and stable arsenide removal and cost reduction.

CN114377667BActive Publication Date: 2024-10-01PETROCHINA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011108577.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-16
Publication Date
2024-10-01
Estimated Expiration
2040-10-16

AI Technical Summary

Technical Problem

Existing adsorption dearsenic catalysts are not efficient in removing arsenic compounds from liquid hydrocarbons, have short service life, complex preparation processes and high costs, making it difficult to meet long-term operation requirements.

Method used

Activated carbon is mixed with pseudo-boehmite powder, additives and acidic solutions are added, extruded and dried, then roasted anaerobically, the pH value of the active metal precursor solution is adjusted, and the loaded active metal is impregnated using an equal volume saturated impregnation method, and low-temperature - The carbon-alumina composite carrier catalyst with a composite pore structure is prepared by stepwise and continuous roasting at medium to high temperatures.

Benefits of technology

The arsenic removal efficiency and arsenic capacity of the catalyst are improved, the service life is extended, the preparation cost is reduced, and the efficient deep removal and stability of arsenic compounds are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114377667B_ABST
    Figure CN114377667B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a liquid hydrocarbon adsorption dearsenication catalyst with a large specific surface area, a multi-level pore distribution and a high dearsenication performance and an aerobic roasting method thereof, the method comprising: 1) mixing activated carbon and pseudo-boehmite in proportion, kneading, rolling, adding a pore-expanding agent and an acidic solution, extruding strips, and roasting at high temperature in a nitrogen atmosphere to obtain a carbon-alumina composite carrier; 2) adjusting the pH value of the main metal precursor solution to be higher than the isoelectric point of the active metal oxide used; 3) impregnating the composite carrier, and roasting in an aerobic environment at low temperature, medium temperature and high temperature in steps to obtain a finished catalyst. Aerobic step-by-step continuous roasting not only overcomes the flammable defect of activated carbon, but also reduces the cost of catalyst preparation. Low temperature ensures deep drying of the catalyst, slow decomposition of the medium temperature metal precursor, and high temperature roasting ensures that the active metal precursor is completely converted into an oxidized state, giving full play to the dearsenication activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing an adsorption arsenic removal catalyst in the field of petrochemical industry, and is particularly suitable for the field of low-temperature adsorption removal of arsenide in liquid petroleum hydrocarbons. Background Art

[0002] As oil resources become increasingly depleted, crude oil composition becomes more complex, and the arsenic content in crude oil produced by some oil fields increases year by year. Hydrogenation catalysts all contain Group VIII elements. Organic arsenic and inorganic arsenic in oil products will be reduced to AsH3 under high temperature hydrogen conditions. Trivalent As has active reducing properties and can easily combine with the d orbital electrons of Group VIII elements to form coordination bonds that poison and inactivate the catalyst. This poisoning is difficult to eliminate through activation or regeneration methods, so a very small amount of arsenic in the crude oil will cause the catalyst to be permanently poisoned and inactivated. Therefore, in order to maintain the activity of hydrogenation catalysts and extend their service life, removing arsenic from liquid hydrocarbons has important practical value.

[0003] At present, there are two main methods for dearsenification of hydrocarbon compounds: adsorption dearsenification technology and hydroarsenification technology. Hydroarsenification technology is that under certain reaction conditions (usually 1.5-3.0Mpa, 180-300℃), arsenide reacts with alkyl arsenide or phenyl arsenide under the catalytic action of dearsenification agent to generate AsH3, and AsH3 decomposes into As and adsorbs on the active metal. Because the reaction temperature of hydroarsenification is high, the reaction can enter the bulk phase of the active group, and the active metal can fully play its role, with a large arsenic capacity and good dearsenification effect. The disadvantage is that the application process of hydroarsenification agent is complicated and inconvenient to operate, and it will cause partial olefin saturation during the dearsenification process, causing octane loss. Adsorption dearsenification technology refers to the combination of arsenide and the active metal of the dearsenification agent in the form of chemical adsorption at a lower temperature (<100℃), and arsenic and the active metal undergo partial electron cloud transfer and adsorb on the surface of the active group of the metal, thereby achieving the purpose of dearsenification. Adsorption arsenic removal technology has a simple process, is easy to operate, has a low reaction temperature, and is not likely to affect the properties of oil products. It can be used as a "pre-arsenic removal" unit placed before a complete set of hydrogenation units to treat raw materials with complex components, a wide range, and high arsenic content. It is mainly used for the removal of arsenides from naphtha and gasoline. The main problem facing adsorption arsenic removal technology is that the adsorption arsenic removal agent, which is the core of its technology, has not made a major breakthrough, the arsenic removal efficiency is not high, and the adsorption capacity is small, the service life is short, the amount of waste residue is large, and it is difficult to handle. It is easy to cause environmental pollution, especially in the treatment of liquid hydrocarbons. Therefore, low-temperature adsorption arsenic removal agents with large arsenic capacity, high arsenic removal efficiency, long service life, and easy waste residue treatment have always been a research hotspot for liquid hydrocarbon arsenide removal catalysts.

[0004] Arsenides in petroleum hydrocarbons are mainly trivalent organic arsenic complexes, which exist in the form of R3As, where R is a hydrogen atom or a hydrocarbon group such as methyl, ethyl, propyl or phenyl. Organic arsenic complexes with different boiling points enter into various fractions after crude oil distillation. Arsenides with low boiling points in liquid petroleum hydrocarbons include AsH3, CH3AsH2, etc., and arsenides with high boiling points include As(CH3)3, As(C2H5)3, etc. Arsenides with higher boiling points and containing one or more hydrocarbon groups have lower affinity for transition metal oxides and are difficult to be removed by adsorption. The higher the boiling point of the arsenide or the longer the alkyl chain length, the more difficult it is to be removed, and the higher the requirements for arsenic removal agents.

[0005] Adsorption arsenic removal generally uses the combined action of physical adsorption and chemical adsorption at room temperature and pressure to achieve the purpose of arsenic removal. The arsenic removal agent used for adsorption arsenic removal is mainly composed of two parts: a carrier and an active component, and also includes other small amounts of auxiliary agents. The carrier used as the adsorption arsenic removal agent is more suitable for a mixture of one or more of alumina, silica, manganese oxide, titanium dioxide, activated carbon, molecular sieves, and silicon aluminum oxide. The main active component is selected from one or more of transition metals such as copper, zinc, and manganese or their oxides. Some arsenic removal agents also add rare earth elements such as lanthanum, cerium, and samarium, as well as precious metals such as gold, silver, rhodium, and palladium as auxiliary active components. By summarizing the liquid adsorption arsenic removal agents at room temperature and pressure in the literature, it is found that the commonly used adsorption arsenic removal agents that are studied more include two categories. One category is a arsenic removal agent that uses silicon aluminum oxide as a carrier and loads metals such as copper, zinc, and their metal oxides as active components; the other category is a arsenic removal agent that uses activated carbon as a carrier and loads active metals and their active metal oxides as an active component.

[0006] For adsorption arsenic removal agents, the specific surface area, effective pore volume and pore structure of the formed carrier have a direct impact on the performance of the arsenic removal agent, especially for adsorption arsenic removal of liquid petroleum hydrocarbons at room temperature and pressure. Increasing the proportion of mesopores or macropores is conducive to the transmission of liquid petroleum hydrocarbons, and a higher specific surface area ensures a relatively large number of dearsenication active points. The pore structure of the arsenic removal agent carrier prepared with silicon aluminum oxide or aluminum oxide as a carrier is uncontrollable and has a small specific surface area. Activated carbon is used as a arsenic removal agent carrier because of its excellent properties of developed pore structure, high specific surface area, high surface activity and diverse surface chemical properties. It can be used as a arsenic removal agent carrier to obtain an oil product arsenic removal agent with excellent performance. At the same time, its pore structure can be adjusted to adapt to changes in dearsenication conditions. Small molecule arsenides have strong reducibility and are easily subjected to redox reactions with active metals such as copper oxide, nickel oxide, and zinc oxide to generate arsenides of the corresponding metals. The reaction equation is:

[0007] 3CuO+2R3As→Cu3As+As+3R2O

[0008] 3CuO+2R3As→3Cu+As+3R2O

[0009] Therefore, when activated carbon is used as a carrier to prepare the dearsenication catalyst, and the active metal is in an oxidized state, its adsorption dearsenication activity is higher. In the existing dearsenication catalyst patents, in order to ensure that the adsorption dearsenication catalyst with activated carbon as a carrier can be successfully prepared, an oxygen-free roasting method is usually used. This method is firstly complicated in process, harsh in conditions, and relatively expensive. In addition, its oxygen-free environment also makes it difficult to ensure that the active metal of the catalyst is converted into an oxidized state, and the dearsenication activity of the active metal cannot be fully exerted. There are very few patents for preparing activated carbon-based adsorption dearsenication catalysts by aerobic methods, and there are very few other related patents that clearly specify the aerobic roasting process method.

[0010] By loading certain active components on a shaped carrier, a more excellent arsenic removal effect can be obtained. Patent CN101591556B introduces a dearsenicating agent that is suitable for deep removal of arsenides from various oil products, using copper oxide, zinc oxide, and oxides of one or more metals in Group VIII as active components and aluminum oxide as a carrier. This invention reduces the amount of expensive metallic copper and correspondingly increases the content of other low-priced highly active metals, thereby reducing the cost of the dearsenicating agent, while achieving a dearsenication rate of more than 99.0%, ensuring the arsenic removal efficiency. However, the investigation used a high-concentration arsine hydrogen gas, supplemented with a certain amount of nitrogen, which cannot represent the dearsenication effect in oil products. At the same time, the invention did not evaluate the arsenic capacity of the dearsenicating agent, and it was impossible to evaluate its dearsenication performance from a long-term perspective.

[0011] The dearsenicating agent introduced in patent CN102553517A has copper oxide and zinc oxide as active components, but uses silicon aluminum oxide as a carrier, and can be used as an adsorption dearsenicating agent for light oil. The waste silicon aluminum catalyst with no recycling value in the fluidized catalytic cracking unit is carbonized, ground, and sieved to obtain waste catalyst powder, and the powder is kneaded, extruded, dried, and roasted with aluminum oxide to obtain a carrier, and then impregnated with active components containing copper oxide and zinc oxide to finally obtain a dearsenicating agent. The dearsenicating agent is heated at 60°C and the air velocity is 2h -1 Under the conditions of , the arsenic removal rate reaches more than 94%, and the arsenic capacity can reach 0.12%, which is 1.3 times higher than the arsenic capacity of the industrial comparison agent of 0.09%. The arsenic removal agent not only has good arsenic removal performance, but also simply treats the waste silicon aluminum catalyst, turning waste into treasure, which not only reduces pollution to the environment, but also reduces the production cost of the arsenic removal agent. However, the arsenic capacity of the catalyst is 0.12%, which is relatively low and cannot meet the needs of long-term operation of the catalyst.

[0012] Patent CN101591556A introduces a dearsenicating agent that is suitable for deep removal of arsenides from various oil products, using copper oxide, zinc oxide, and oxides of one or more metals in Group VIII as active components and aluminum oxide as a carrier. This invention reduces the amount of copper metal, which is more expensive, and correspondingly increases the content of other low-priced highly active metals, thereby reducing the cost of the dearsenicating agent, while achieving a dearsenicating rate of more than 99.0%, ensuring the arsenic removal efficiency. However, the dearsenicating effect of the gas prepared to contain arsine was investigated by using a high-concentration arsine gas supplemented with a certain amount of nitrogen, which cannot represent the dearsenicating effect in oil products. At the same time, the invention does not evaluate the arsenic capacity of the dearsenicating agent, and cannot evaluate its dearsenicating performance from a long-term perspective.

[0013] Patent CN201310342825.7 relates to a supported arsenic removal agent, wherein the carrier is activated carbon and the active component is a metal oxide. When preparing the supported arsenic removal agent, first, the activated carbon carrier is pre-treated, and then a semi-finished product of the supported arsenic removal agent impregnated with the active component is prepared, and then the semi-finished product is subjected to alkali treatment, so that the active metal salt component supported on the activated carbon carrier can be decomposed to generate an active oxide component at a lower temperature. This preparation method is cumbersome and difficult to promote and apply on a large scale.

[0014] Patent CN201310279739.6 relates to a liquid hydrocarbon dearsenicating agent and its preparation method. The dearsenicating agent is prepared by one carrier pretreatment and three impregnations, and is composed of active components CuO, transition metals La2O3 and CeO2, and precious metals PdO, AgO additives and activated carbon carriers. The preparation process is complicated and not conducive to large-scale industrial production.

[0015] Patent CN201811162149.4 uses a certain proportion of activated carbon and alumina as carriers, prepares nickel, copper, molybdenum and cobalt active metal precursors into solutions, impregnates them onto the carriers in steps and roasts them to prepare Ni-Cu-Mo-Co system adsorption dearsenic catalysts for adsorption dearsenication of gasoline. The preparation process of this patent is cumbersome and does not mention the roasting method for obtaining oxidized active metals.

[0016] Patent CN201511020498.9 adopts a one-step preparation method, mixing the precursor for preparing the carrier, the extrusion aid, the nitric acid solution and the prepared active component precursor solution, wet mixing, extrusion and molding in one step, and calcining in a nitrogen atmosphere to obtain the FCC gasoline adsorption arsenic removal catalyst. The catalyst of this patent is calcined in an oxygen-free manner.

[0017] Patent CN201310342825.7 relates to a supported dearsenication catalyst, the carrier of which is activated carbon. The preparation process requires first pre-treating the activated carbon carrier, and then alkali-treating the catalyst after loading the metal to ensure that the active metal salt component decomposes to generate oxide components under aerobic conditions at a lower temperature. However, the preparation process is complicated, and the alkali treatment will enrich a large amount of sodium or potassium ions on the catalyst, affecting the activity of the dearsenication catalyst.

[0018] In summary, some of the technologies currently reported in patents or literature are limited to written reports and theoretical discussions but have not been put into practical use. Although some technologies have been applied in industry, their processes are relatively complex and their preparation costs are high, which is not conducive to large-scale industrial production and promotion and application. At the same time, most of the roasting methods for activated carbon catalysts use oxygen-free roasting, which has the advantages of being safe and non-flammable, but also has the defect that some active metals on the catalyst cannot be completely converted into oxidized metals. After the activated carbon-alumina-based carrier is prepared in this patent, the pH value of the metal precursor solution is increased to be higher than the isoelectric point of the metal oxide or hydroxide during the impregnation process, which can increase the dispersion of the metal loaded thereon and avoid metal agglomeration. At the same time, the catalyst adopts a low-temperature-medium-temperature-high-temperature step-by-step continuous roasting method in an aerobic environment to reduce the cost of catalyst preparation, overcome the defect of activated carbon being flammable, and ensure that the active metal precursor is completely converted into an oxidized state, thereby giving full play to the dearsenicization activity. Summary of the invention

[0019] The main purpose of the present invention is to provide a liquid hydrocarbon adsorption dearsenication catalyst and a preparation method thereof, so as to overcome the defects of the existing preparation methods, such as complex process operation, low dearsenication efficiency of the prepared catalyst, small adsorption capacity and short service life.

[0020] A preparation method for an adsorption dearsenicizing catalyst is characterized in that it comprises the following steps: adding an auxiliary agent and an acidic solution to a powder containing activated carbon and pseudo-boehmite, extruding strips, drying, and roasting under anaerobic conditions to obtain a composite carrier mainly composed of carbon-alumina; adjusting the pH value of an active metal precursor solution to be higher than the isoelectric point of the active metal oxide to prepare an impregnation solution, impregnating the composite carrier with an equal volume saturation impregnation method, and then drying and roasting continuously in steps of low temperature, medium temperature, and high temperature under aerobic conditions to obtain a shaped catalyst.

[0021] The activated carbon of the present invention can be one or a mixture of wood activated carbon, coal activated carbon, coconut shell activated carbon and the like.

[0022] The alumina in the composite carrier obtained by calcination in the present invention can be one or a mixture of γ-Al2O3, γ-Al2O3 containing B, γ-Al2O3 containing F, γ-Al2O3 containing Si, and γ-Al2O3 containing P.

[0023] The auxiliary agent of the present invention can be an extrusion aid, a pore expander, etc., and the preferred addition amount accounts for 1-10% of the weight ratio of the carrier; the preferred auxiliary agent is one or a mixture of sesbania powder, methyl cellulose, and ethyl cellulose.

[0024] In the present invention, the mixture of powders containing activated carbon and pseudo-boehmite is preferably rolled and fully stirred. The activated carbon usually has a large pore diameter, a particle size of about 3 to 6 mm, and a high specific surface area, usually ≥500m 2 / g, in order to fully mix with pseudo-boehmite, it is best to roll it, the rolling time is preferably 10-60min, and the stirring time is preferably 10-80min.

[0025] In the present invention, the acidic solution is an organic acid and / or an inorganic acid, preferably one or a mixture of nitric acid, citric acid, phosphoric acid, ethylenediaminetetraacetic acid and oxalic acid.

[0026] In the present invention, the carrier is dried at a temperature of 80-150°C, dried for 2-6 hours, calcined in an oxygen-free atmosphere at a temperature of 400-750°C, and calcined for 1-6 hours. The more preferred conditions are a drying temperature of 100-140°C, a drying time of 2-4 hours, a calcined in an oxygen-free atmosphere at a temperature of 450-600°C, and calcined for 2-4 hours. The catalyst is calcined at a low temperature of 80-170°C, and calcined for 2-6 hours. The more preferred conditions are a drying temperature of 100-140°C, a drying time of 2-4 hours, a calcined in an oxygen-free atmosphere at a temperature of 450-600°C, and calcined for 2-4 hours. The calcination temperature is 130-170°C, and the calcination time is 2-4h; the medium-temperature calcination temperature is the decomposition temperature of the active metal precursor ±40°C, and the calcination time is 1-6h. The more preferred first step aerobic calcination temperature is the decomposition temperature of the active metal precursor ±20°C, and the calcination time is 2-4h; the high-temperature calcination temperature is 300-500°C, and the calcination time is 1-6h. The more preferred high-temperature calcination temperature is 350-450°C, and the calcination time is 2-4h.

[0027] In the present invention, there is no particular limitation on which active metals are used. Any metal that can be commonly used for arsenic removal in the prior art can be used, such as one or more of the Group VIII elements in the periodic table, one or more of the transition metal elements, one or more of the alkali metal or alkaline earth metal elements, etc. The present invention also particularly recommends selecting a metal with a partially filled d orbital as the active metal, which can increase the active interaction between the arsenide and the metal, thereby forming a strong metal-arsenic chemical bond and efficiently removing the arsenide in depth. The active metal is preferably one or more of Ni, Cu, Co, Zn, Mo, Fe, Pb, V, Ag, and Mn; the active metal precursor is one or more of the corresponding nitrates, acetates, sulfates, and basic carbonates.

[0028] The isoelectric point of the present invention refers to the pH value when a molecule or surface is not charged. In the present invention, it is required to increase the pH value of the metal precursor solution to be higher than the isoelectric point of the oxide or hydroxide of the main metal element, so as to weaken the interaction between the main metal and the carrier, improve the dispersion of the metal loaded thereon, and make it reflect a higher arsenic removal efficiency. Table 1 shows the isoelectric point data of the metals used.

[0029] Table 1 Isoelectric points of oxides or hydroxides of common metal elements

[0030]

[0031]

[0032] The catalyst in the present invention is prepared in the form of impregnation loading, and it is particularly recommended to prepare the catalyst by an equal volume saturated impregnation method, which is very different from the co-precipitation method. The powders of activated carbon and pseudo-boehmite are co-precipitated, formed, dried, and calcined together with the active metal precursor solution. Too high a calcination temperature is not conducive to the dispersion of the active metal, and too low a calcination temperature affects the morphology of alumina. In addition, since it is a dearsenication catalyst obtained by the co-precipitation process, most of the metal components are not highly dispersed in the carrier pores and the outer surface, resulting in low metal utilization. At the same time, the prepared active component precursor solution is mixed with alumina / activated carbon in an acidic environment and extruded. Under strong acid conditions, the interaction between the carrier and the metal is strong, and the metal is more likely to agglomerate, resulting in a further reduction in utilization efficiency. The catalyst thus obtained still cannot meet the long-term dearsenication requirements of liquid hydrocarbons with high arsenic content.

[0033] Using activated carbon or pseudo-boehmite alone to prepare a carrier cannot achieve a good arsenic removal effect. In the present invention, activated carbon and pseudo-boehmite are used in combination, the carrier structure characteristics are optimized, the pore volume and specific surface area of ​​the composite carrier are improved, and the dispersion of its pores and pore sizes is made more uniform, multi-level and orderly. By adjusting the addition ratio of activated carbon, a carbon-alumina composite carrier with a suitable specific surface area and multi-level pore distribution can be obtained, which is beneficial to the diffusion, reaction and escape of reactant molecules in the pores.

[0034] The present invention also provides an adsorption dearsenication catalyst obtained by the above preparation method, wherein the ratio of activated carbon to alumina in the composite carrier is preferably 0.5-2:1. The preferred adsorption dearsenication catalyst, based on 100% by mass of the catalyst, accounts for 15-25% by mass of the active metal oxide.

[0035] The present invention also provides a more specific adsorption dearsenicization catalyst, based on 100% by mass of the catalyst, and calculated on the basis of the oxides of the respective metals, the content of Cu or Mo is 5 to 30% by mass, the content of Co or Ni is 1 to 11% by mass, the content of Zn or Mn is 0 to 10% by mass, and the total loading amount of Zn, Fe, Pb, V, and Ag is 1 to 5% by mass.

[0036] The specific surface area of ​​the catalyst recommended by the present invention is 350 to 550 m 2 / g, pore volume is 0.55~0.75mL / g, bulk density is 0.48~0.58g / cm 3 The most probable pore size is 7 to 11 nm; the more preferred specific surface area is 400 to 500 m 2 / g, pore volume is 0.60~0.70mL / g, bulk density is 0.50~0.55g / cm 3 , the most probable pore size is 8 to 9 nm.

[0037] The present invention particularly provides a more preferred method for preparing an adsorption arsenic removal catalyst, the specific preparation steps mainly comprising:

[0038] (1) Mix activated carbon and pseudo-boehmite in a mass ratio of 0.5-2:1, add an auxiliary agent accounting for 1-10% of the carrier mass content, such as one or a mixture of sesbania powder, methyl cellulose, and ethyl cellulose, add acid after mixing, such as one or a mixed solution of nitric acid, citric acid, phosphoric acid, ethylenediaminetetraacetic acid and oxalic acid, roll for 10-60 minutes, stir for 10-60 minutes, shape, such as a Φ3.0 clover shape, 80-150°C, and dry for 2-6 hours. The calcination temperature in an oxygen-free atmosphere is 400-750°C, and the calcination time is 1-6 hours. A composite carrier is obtained.

[0039] (2) Place one or more mixed metal salts of Cu, Zn, and Co in a solution of water or ammonia, adjust the pH of the solution to a value higher than the isoelectric point of the metal used, and then heat and stir until the metal salt is dissolved;

[0040] (3) adding one or more mixed salts of Ni, Fe, Mo, Pb, V, Ag or Mn to the solution in (2), and continuing to adjust the pH value of the solution to be higher than the isoelectric point of the metal precursor salt used, so that all the metal salts are dissolved;

[0041] (4) The impregnation solution prepared in (3) is loaded on the composite support prepared in (1) by an equal volume saturation impregnation method, and the mixture is allowed to stand for 12-24 hours to obtain a catalyst;

[0042] (5) The low-temperature calcination temperature is 130-170°C, and the calcination time is 2-4h; the medium-temperature calcination temperature is the decomposition temperature of the active metal precursor ± 20°C, and the calcination time is 2-4h; the high-temperature calcination temperature is 350-450°C, and the calcination time is 2-4h.

[0043] The advantages of the present invention are:

[0044] (1) The preparation method first obtains a carrier with a composite pore structure distribution, which is conducive to the high dispersion of metal components on the carrier, improves the utilization rate of the metal, and can also improve the diffusion, reaction and escape of reactant molecules in the pores, thereby improving the reaction efficiency;

[0045] (2) Selecting a metal with partially filled d orbitals as the active metal can increase the active interaction between the arsenide and the metal, thereby forming a strong metal-arsenic chemical bond and efficiently removing the arsenide in depth;

[0046] (3) Increasing the pH value of the metal precursor solution to make it higher than the isoelectric point of the metal oxide or hydroxide can weaken the interaction between the metal and the carrier, improve the dispersion of the metal loaded thereon, avoid metal agglomeration, and ultimately improve the arsenic removal efficiency of the catalyst.

[0047] (4) The catalyst calcination temperature and calcination steps are adjusted in an aerobic environment, and a low-temperature-medium-temperature-high-temperature step-by-step continuous calcination method is adopted to reduce the catalyst preparation cost, overcome the defect of activated carbon being flammable, and ensure that the active metal precursor is completely converted into an oxidized state, thereby giving full play to the arsenic removal activity. The catalyst prepared by this method exhibits excellent arsenic removal performance, high arsenic tolerance performance and high arsenic removal stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 These are XRD characterization spectra of the adsorption dearsenicization catalysts of Example 2, Example 7, Comparative Example 1 and Comparative Example 2. DETAILED DESCRIPTION

[0049] The following examples are intended to further illustrate the method of the present invention but should not be construed as limiting.

[0050] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0051] Example 1

[0052] 500g of activated carbon, 1000g of pseudo-boehmite, 30g of sesbania powder and 20g of methyl cellulose were mixed for 5 minutes, and 1600g of aqueous solution containing 5% nitric acid was added. After rolling for 30 minutes, the mixture was kneaded for 30 minutes, extruded through a Φ3.0 hole plate, dried at 120℃ for 2 hours, and calcined at 450℃ in an oxygen-free atmosphere for 4 hours to obtain carrier Z-1. 10g of the carrier was taken, 5.5g of copper nitrate was dissolved in deionized water, and the impregnation solution was loaded onto carrier Z-1 by an equal volume saturation impregnation method, and allowed to stand and dry for 12 hours, and then calcined at 130℃ in an oxygen-free atmosphere for 4 hours, and then heated at a volume space velocity of 200m / s. 3 .h -1 , after purging with nitrogen with an oxygen content of 2% for 30 minutes, calcining at 240°C for 4 hours and calcining at 350°C in the presence of oxygen for 2 hours, catalyst C1 was obtained.

[0053] Example 2

[0054] Mix 500g of activated carbon, 500g of pseudo-boehmite, 50g of sesbania powder and 50g of methyl cellulose for 5 minutes, add 1000g of aqueous solution containing 5% nitric acid, roll for 30 minutes and then knead for 30 minutes, squeeze into strips with a Φ3.0 hole plate, dry at 120℃ for 2 hours, and roast at 450℃ in an oxygen-free atmosphere for 4 hours to obtain carrier Z-2. Take 10g of the carrier, dissolve 7.2g of copper nitrate in deionized water, use an equal volume saturation impregnation method to load the above impregnation solution onto carrier Z-2, let it stand and dry for 12 hours, then roast at 130℃ in an aerobic environment for 4 hours, and then heat at a volume space velocity of 200m / s. 3 .h -1 , after purging with nitrogen with an oxygen content of 2% for 30 minutes, calcining at 240°C for 4 hours and calcining at 350°C in the presence of oxygen for 2 hours, catalyst C2 was obtained.

[0055] Example 3

[0056] 1000g activated carbon, 500g pseudo-boehmite, 80g sesbania powder and 80g ethyl cellulose were mixed for 5min, 1600g aqueous solution containing 5% nitric acid was added, and the mixture was rolled for 30min and then kneaded for 30min, and then extruded through a Φ3.0 hole plate, dried at 120℃ for 2h, and calcined at 450℃ in an oxygen-free atmosphere for 4h to obtain carrier Z-3. 10g of the carrier was taken, 9.5g of copper nitrate was dissolved in deionized water, and the impregnation solution was loaded onto carrier Z-3 by an equal volume saturation impregnation method, and then allowed to stand and dry for 12h, and then calcined at 150℃ in an oxygen-free atmosphere for 3h, and then heated at a volume space velocity of 300m / s. 3 .h -1 , after purging with nitrogen with an oxygen content of 2% for 30 minutes, calcining at 260°C for 4 hours and calcining at 400°C in the presence of oxygen for 2 hours, catalyst C3 was obtained.

[0057] Example 4

[0058] Take 10g of carrier Z-1, dissolve 6.0g of copper nitrate and 1.0g of nickel nitrate in deionized water, use equal volume saturation impregnation method to load the above impregnation solution onto the carrier, let it stand and dry for 12h, then dry at 120℃ for 2h, calcine at 130℃ for 4h, and then calcine at a volume space velocity of 300m / s. 3 .h -1 , after purging with nitrogen with an oxygen content of 2% for 50 minutes, calcining at 260°C for 4 hours and calcining at 400°C in the presence of oxygen for 2 hours, finally obtaining catalyst C4.

[0059] Example 5

[0060] Take 10g of carrier Z-1, dissolve 6.0g of copper nitrate and 1.0g of nickel nitrate in deionized water, adjust the pH value of the solution to 11.0 with ammonia water, load the above impregnation solution onto carrier Z-1 by equal volume saturation impregnation method, let it stand and dry for 12h, calcine at 170℃ for 2h, and then calcine at a volume space velocity of 300m / s. 3 .h -1 , calcined at 260°C for 4 h in a nitrogen atmosphere with an oxygen content of 2%, and calcined at 350°C in an oxygen atmosphere for 2 h to finally obtain catalyst C5.

[0061] Example 6

[0062] Take 10g of carrier Z-2, dissolve 6.0g of copper nitrate and 1.0g of nickel nitrate in deionized water, adjust the pH value of the solution to 12.0 with ammonia water, load the above impregnation solution onto carrier Z-2 by equal volume saturation impregnation method, let it stand and dry for 12h, calcine at 170℃ for 2h, and then calcine at a volume space velocity of 300m / s. 3 .h -1 , calcined at 260°C for 4 h in a nitrogen atmosphere with an oxygen content of 2%, and calcined at 350°C in an oxygen atmosphere for 2 h to finally obtain catalyst C6.

[0063] Example 7

[0064] Take 10g of carrier Z-3, dissolve 8.0g of copper nitrate, 0.6g of nickel nitrate and 1.2g of zinc nitrate in deionized water, adjust the pH value of the solution to 11.0 with ammonia water, load the above impregnation solution onto carrier Z-3 by equal volume saturation impregnation method, let it stand and dry for 12h, calcine at 150℃ for 3h, and then calcine at a volume space velocity of 300m / s. 3 .h -1 , calcined at 280°C for 4 h in a nitrogen atmosphere with an oxygen content of 2%, and calcined at 400°C in an oxygen atmosphere for 2 h to finally obtain catalyst C7.

[0065] Example 8

[0066] Take 10g of carrier Z-3, dissolve 10.0g of copper nitrate, 1.2g of nickel nitrate and 1.0g of ferric nitrate in deionized water, adjust the pH value of the solution to 11.0 with ammonia water, load the above impregnation solution onto carrier Z-3 by equal volume saturation impregnation method, let it stand and dry for 12h, calcine at 150℃ for 3h, and then calcine at a volume space velocity of 300m / s. 3 .h -1 , calcined at 280°C for 4 h in a nitrogen atmosphere with an oxygen content of 2%, and calcined at 400°C in an oxygen atmosphere for 2 h to finally obtain catalyst C8.

[0067] Example 9

[0068] Take 10g of carrier Z-3, dissolve 8.0g of copper nitrate, 2.5g of nickel nitrate and 1.0g of cobalt nitrate in deionized water, adjust the pH value of the solution to 13.0 with ammonia water, load the impregnation solution onto carrier Z-3 by equal volume saturation impregnation method, let it stand and dry for 12h, calcine at 130℃ for 4h, and then calcine at a volume space velocity of 300m / s. 3 .h -1 , after purging with nitrogen with an oxygen content of 2% for 40 minutes, calcining at 260°C for 4 hours, and calcining at 450°C in the presence of oxygen for 2 hours, finally obtaining catalyst C9.

[0069] Example 10

[0070] Take 10g of carrier Z-3, dissolve 12.0g of copper nitrate, 3.0g of nickel nitrate and 4.5g of ammonium molybdate in deionized water, adjust the pH value of the solution to 11.0 with ammonia water, load the above impregnation solution onto carrier Z-3 by equal volume saturation impregnation method, let it stand and dry for 12h, calcine at 130℃ for 4h, and then calcine at a volume space velocity of 300m / s. 3 .h -1 , after purging with nitrogen with an oxygen content of 2% for 40 minutes, calcining at 260°C for 4 hours, and calcining at 450°C in the presence of oxygen for 2 hours, finally obtaining catalyst C10.

[0071] Embodiment 11

[0072] Take 10g of carrier Z-3, dissolve 5.0g of copper nitrate, 3.0g of nickel nitrate and 8.0g of lead nitrate in deionized water, adjust the pH value of the solution to 12.0 with ammonia water, load the impregnation solution onto carrier Z-3 by equal volume saturation impregnation method, let it stand and dry for 12h, calcine at 170℃ for 2h, and then calcine at a volume space velocity of 300m / s. 3 .h -1 , after purging with nitrogen with an oxygen content of 2% for 20 minutes, calcining at 260°C for 4 hours and calcining at 350°C in the presence of oxygen for 2 hours, finally obtaining catalyst C11.

[0073] Example 12

[0074] Take 10g of carrier Z-3, dissolve 8.0g of copper nitrate, 1.5g of nickel nitrate and 6.0g of ammonium metavanadate in deionized water, adjust the pH value of the solution to 10.0 with ammonia water, load the impregnation solution onto carrier Z-3 by equal volume saturation impregnation method, let it stand and dry for 12h, calcine at 170℃ for 2h, and then calcine at a volume space velocity of 300m / s. 3 .h -1 , after purging with nitrogen with an oxygen content of 2% for 20 minutes, calcining at 260°C for 4 hours and calcining at 350°C in the presence of oxygen for 2 hours, finally obtaining catalyst C12.

[0075] Embodiment 13

[0076] Take 10g of carrier Z-3, dissolve 9.0g of copper nitrate, 1.5g of nickel nitrate and 2.5g of silver nitrate in deionized water, adjust the pH value of the solution to 12.0 with ammonia water, load the impregnation solution onto carrier Z-3 by equal volume saturation impregnation method, let it stand and dry for 12h, calcine at 130℃ for 4h, and then precipitate at a volume space velocity of 400m / s. 3 .h -1 , after purging with nitrogen with an oxygen content of 2% for 40 minutes, calcining at 240°C for 4 hours and calcining at 350°C in the presence of oxygen for 2 hours, finally obtaining catalyst C13.

[0077] Embodiment 14

[0078] Take 10g of carrier Z-3, dissolve 5.0g of copper acetate, 1.0g of nickel acetate and 4.0g of ferric nitrate in deionized water, adjust the pH value of the solution to 12.0 with ammonia water, load the above impregnation solution onto carrier Z-3 by equal volume saturation impregnation method, let it stand and dry for 12h, calcine at 130℃ for 4h, and then calcine at a volume space velocity of 400m / s. 3 .h -1 , after purging with nitrogen with an oxygen content of 2% for 40 minutes, calcining at 240°C for 4 hours and calcining at 350°C in the presence of oxygen for 2 hours, finally obtaining catalyst C14.

[0079] Embodiment 15

[0080] Take 10g of carrier Z-3, dissolve 3.0g of copper acetate, 5.0g of nickel acetate and 6.0g of silver nitrate in deionized water, adjust the pH value of the solution to 11.0 with ammonia water, load the impregnation solution onto carrier Z-3 by equal volume saturation impregnation method, let it stand and dry for 12h, calcine at 150℃ for 3h, and then calcine at a volume space velocity of 400m / s. 3 .h -1 , after purging with nitrogen with an oxygen content of 2% for 20 minutes, calcining at 240°C for 4 hours and calcining at 450°C in the presence of oxygen for 2 hours, finally obtaining catalyst C15.

[0081] Example 16

[0082] Take 10g of carrier Z-3, dissolve 3.0g of copper sulfate, 8.0g of nickel acetate and 6.0g of silver nitrate in deionized water, adjust the pH value of the solution to 12.0 with ammonia water, load the above impregnation solution onto carrier Z-3 by equal volume saturation impregnation method, let it stand and dry for 12h, calcine at 150℃ for 3h, and then precipitate at a volume space velocity of 400m / s. 3 .h -1 , after purging with nitrogen with an oxygen content of 2% for 20 minutes, calcining at 240°C for 4 hours and calcining at 450°C in the presence of oxygen for 2 hours, finally obtaining catalyst C16.

[0083] Comparative Example 1

[0084] 50g of activated carbon forming composite binder was added to 300g of activated carbon, and Φ3.0 pure carbon carrier strip AC1 was squeezed. 10g of AC1 was taken, 10.0g of copper nitrate, 1.0g of nickel nitrate and 2.0g of zinc nitrate were dissolved in deionized water, and the impregnation solution was loaded onto the carrier by equal volume saturation impregnation method, and then allowed to stand and dry for 12h, dried at 120℃ for 2h, and calcined at 500℃ for 4h without oxygen to finally obtain catalyst D1.

[0085] Comparative Example 2

[0086] Add 10g of sesbania powder to 300g of pseudo-boehmite, mix well, then add 200g of an aqueous solution containing 3% nitric acid solution, roll and stir, squeeze Φ3.0 strips, dry at 120°C for 2h, and roast at 550°C for 4h to obtain an alumina carrier strip. Take 10g of the alumina carrier strip, dissolve 5.0g of copper nitrate, 2.0g of nickel nitrate and 6.0g of zinc nitrate in deionized water, use an equal volume saturation impregnation method to load the above impregnation solution onto the alumina carrier, let it stand and dry for 12h, then dry at 120°C for 2h, and roast at 500°C for 4h without oxygen to finally obtain catalyst D2.

[0087] Comparative Example 3

[0088] Add 10g of sesbania powder to 300g of pseudo-boehmite, mix well, then add 200g of an aqueous solution containing 3% nitric acid solution, roll and stir, squeeze Φ3.0 strips, dry at 120℃ for 2h, and roast at 550℃ for 4h to obtain an alumina carrier strip. Take 10g of the alumina carrier strip, dissolve 7.0g of copper nitrate, 3.0g of nickel nitrate and 3.0g of zinc nitrate in deionized water, use an equal volume saturation impregnation method to load the above impregnation solution onto the alumina carrier, let it stand and dry for 12h, and roast at 350℃ for 3h to obtain catalyst D3. Due to the lack of step-by-step roasting, part of the catalyst was oxidized by oxygen and the surface turned gray.

[0089] Catalytic performance evaluation:

[0090] In this test example, the arsenic removal activities of the adsorptive arsenic removal catalyst prepared by the method provided by the present invention and the adsorptive arsenic removal catalyst provided by the comparative example were evaluated according to the following method, and the results are listed.

[0091] Adsorption arsenic removal: The adsorption arsenic removal activity of the catalyst was evaluated on a continuous high-pressure reaction device using a full-fraction FCC gasoline with an arsenic content of 125 ppb as the raw material. The raw oil was fed in from the bottom and discharged from the top. The reaction conditions were: weight hourly space velocity 3.0 h-1, temperature 20°C, pressure 0.5 MPa. Samples were taken after the reaction was stable for 24 hours, and the arsenic content of the samples was analyzed by graphite furnace atomic absorption spectrometry. The results are shown in Table 1. The arsenic capacity was determined by adding triphenylarsenic to FCC gasoline to prepare an arsenic standard gasoline A with an arsenic content of 2000 ppm. 10 g of the catalyst was placed in 100 g of the arsenic standard gasoline. After shaking for 24 hours, the dearsenicized standard gasoline B was obtained. After measuring the arsenic content in B, the catalyst arsenic capacity was calculated, as shown in Table 2.

[0092] The arsenic removal rate is calculated according to formula 1:

[0093]

[0094] Arsenic capacity is calculated according to formula 2:

[0095]

[0096] Table 2 Evaluation results of the adsorption and arsenic removal activity of the catalyst

[0097]

[0098]

[0099] The results in Table 1 indicate that the present invention has successfully prepared an adsorptive arsenic removal catalyst with high arsenic removal efficiency and high arsenic capacity by adjusting the carrier composition and the loading method of the active metal component. Compared with the comparison agent made from pure activated carbon and alumina, it exhibits more excellent adsorptive arsenic removal activity.

[0100] Catalyst structure characterization

[0101] This test example compares the XRD characterization results of the catalysts C2, C7, D-1 and D-2 provided by the present invention. Figure 1It can be found that under the condition of equivalent metal loading, the D1 and D2 catalysts prepared with conventional activated carbon and alumina as carriers show obvious characteristic diffraction peaks belonging to crystalline CuO, indicating that the dispersion of CuO on the catalyst is poor. On the C2 catalyst prepared by mixing activated carbon and alumina in a mass ratio of 1:1, the characteristic diffraction peak intensity of CuO is greatly reduced compared with D1 and D2, indicating that the addition of activated carbon greatly improves the dispersion of metal on the catalyst. The substantial addition of activated carbon in the C7 catalyst greatly improves the specific surface area and pore structure of the catalyst, and at the same time adjusts the solution pH to 11, which is higher than the isoelectric point of the three metal oxides of CuNiZn. At this time, the metal components can be better dispersed without agglomeration, greatly improving the metal dispersion. This fully demonstrates that the preparation technology provided by the present invention is conducive to maintaining a high dispersion of active components while achieving a high loading of active components.

[0102] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the present invention.

Claims

1. A method for preparing a liquid hydrocarbon adsorption arsenic removal catalyst, characterized in that: The following steps are involved: Step 1: Mix the activated carbon and pseudo-boehmite powder, add an additive and an acid solution, and extrude into strips to obtain a shaped carrier; Step 2: drying the formed carrier and calcining it under oxygen-free conditions to obtain a composite carrier whose main component is carbon-alumina; Step 3: adjusting the pH value of the active metal precursor solution to be higher than the isoelectric point of the active metal oxide used to prepare an impregnation solution; Step 4: impregnating the composite support by an equal volume saturation impregnation method, and then drying to obtain a dried catalyst precursor; Step 5: calcining the dried catalyst precursor in a low temperature, medium temperature and high temperature step by step under aerobic conditions to completely convert the active metal precursor into an oxidized state to obtain a finished catalyst; In step 5, the low temperature roasting temperature is 80-170°C and the roasting time is 2-6 h; The medium temperature calcination temperature is the decomposition temperature of the active metal precursor -40 °C to the decomposition temperature of the active metal precursor +40 °C, and the calcination time is 1-6 h; The high temperature calcination temperature is 300-500°C and the calcination time is 1-6 h; Wherein, after low-temperature calcination and before medium-temperature calcination, the catalyst precursor is purged with gas, and the purging gas is nitrogen with an oxygen content of 2%; The isoelectric point of the active metal oxide refers to the pH value when the surface of the active metal oxide is uncharged; The activated carbon is one or both of coal-based activated carbon and coconut shell activated carbon; The active metal is at least one selected from Ni, Cu, Co, Zn, Mo, Fe, Pb, V, Ag and Mn.

2. The method for preparing a liquid hydrocarbon adsorption arsenic removal catalyst according to claim 1, characterized in that: The auxiliary agent is at least one of sesbania powder, methyl cellulose and ethyl cellulose, and the amount of the auxiliary agent added accounts for 1-10% of the total weight of the composite carrier.

3. The method for preparing a liquid hydrocarbon adsorption arsenic removal catalyst according to claim 1, characterized in that: The acidic solution is an organic acid and / or an inorganic acid.

4. The method for preparing a liquid hydrocarbon adsorption arsenic removal catalyst according to claim 3, characterized in that: The acidic solution is at least one of nitric acid, citric acid, phosphoric acid, ethylenediaminetetraacetic acid and oxalic acid.

5. The method for preparing a liquid hydrocarbon adsorption arsenic removal catalyst according to claim 1, characterized in that: In the step 2, the drying temperature is 80-150°C, the drying time is 2-6h, the calcination temperature under anaerobic conditions is 400-750°C, the calcination time is 1-6h, and the anaerobic conditions are an inert gas or nitrogen atmosphere; in the step 5, the low-temperature calcination temperature is 130-170°C, and the calcination time is 2-4h; the medium-temperature calcination temperature is the decomposition temperature of the active metal precursor -20°C to the decomposition temperature of the active metal precursor +20°C, and the calcination time is 2-4h; the high-temperature calcination temperature is 350-450°C, and the calcination time is 2-4h.

6. The method for preparing a liquid hydrocarbon adsorption arsenic removal catalyst according to claim 5, characterized in that: In step 2, the drying temperature is 100-140°C, the drying time is 2-4 hours, and the calcination temperature is 450-600°C under oxygen-free conditions, and the calcination time is 2-4 hours.

7. The method for preparing a liquid hydrocarbon adsorption arsenic removal catalyst according to claim 1, characterized in that: The mass ratio of the activated carbon to pseudo-boehmite is 0.5-2:1; the molding conditions are rolling for 10-60 min and stirring for 10-80 min; the molded shape is at least one of a clover, a four-leaf clover, a sphere and a toothed sphere.

8. A liquid hydrocarbon adsorption dearsenication catalyst obtained according to the preparation method according to any one of claims 1 to 7, characterized in that: The active metal in the catalyst is 15-25wt% in terms of oxide.

9. The liquid hydrocarbon adsorption arsenic removal catalyst according to claim 8, characterized in that: The active metals are based on 100% by mass of the catalyst, and calculated as oxides of the respective metals, with a Cu or Mo content of 5-30wt%, a Co or Ni content of 1-11wt%, a Zn or Mn content of 0-10wt%, and a total loading of Zn, Fe, Pb, V, and Ag of 0-5wt%.

10. The liquid hydrocarbon adsorption arsenic removal catalyst according to claim 8, characterized in that: The specific surface area of ​​the adsorption dearsenicization catalyst is 350 to 550 m 2 / g, pore volume is 0.55~0.75 mL / g, and bulk density is 0.48~0.58 g / cm 3 , the most probable pore diameter is 7 to 11 nm.

11. The liquid hydrocarbon adsorption arsenic removal catalyst according to claim 10, characterized in that: The specific surface area of ​​the adsorption dearsenicization catalyst is 400 to 500 m 2 / g, pore volume is 0.60~0.70 mL / g, bulk density is 0.50~0.55 g / cm 3 , the most probable pore diameter is 8 to 9 nm.