Multi-layer coating

By adopting a repeat-start process in the PVD method and using ion etching to interrupt the coating process, coating roughness and residual stress issues are solved, coating durability and adhesion are improved, and more efficient coating production is achieved .

CN114423882BActive Publication Date: 2024-10-11CEMECON AG
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202080064726.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-09-12
Filing Date
2020-09-08
Publication Date
2024-10-11
Estimated Expiration
2040-09-08

AI Technical Summary

Technical Problem

When applying hard material coatings using the existing PVD method, longer coating duration and larger coating thickness will lead to increased coating roughness and residual stress, affecting the durability and adhesion of the coating.

Method used

A repeat-start process is adopted, that is, the coating process is interrupted by ion etching, and coating is restarted to form a multi-layer coating. The parameters of the etching and coating steps are controlled to reduce residual stress and microscopic defects, and improve the density and smoothness of the coating. Spend.

Benefits of technology

This reduces residual stress, improves the ductility and adhesion of the coating, and produces a denser, smoother and chemically resistant coating with longer coating duration and larger coating thickness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114423882B_ABST
    Figure CN114423882B_ABST
Patent Text Reader

Abstract

The invention relates to a method for coating a substrate (40), a coating system for carrying out the method and a coated body. In a first method step (62), the substrate (40) is pretreated in an ion etching process. In a second method step (64), a first coating layer (56a) with a thickness of 0.1 μm to 6 μm is deposited on the substrate (40) by a PVD process. In order to achieve a particularly high-quality and durable coating (50), in a third method step (66), the surface of the first coating layer (56a) is treated by an ion etching process, and in a fourth method step (68), a further coating layer (56b) with a thickness of 0.1 μm to 6 μm is deposited on the first coating layer (56a) by a PVD process. The coated body comprises at least two coating layers (56a, 56b, 56c, 56d) with a thickness of 0.1 μm to 6 μm on a substrate (40), wherein an interface region formed by ion etching is arranged between the coating layers (56a, 56b, 56c, 56d).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention relates to a method for coating a substrate, a coating system for carrying out the method and a coated body.

[0002] It is known to provide an object or a part of an object with a surface coating in order to improve its properties. In particular for cutting tools it is known to provide a functional surface with a hard material coating.

[0003] One class of known methods for applying hard material coatings is the known methods of PVD (physical vapor deposition) methods, which include, for example, cathode sputtering and arc sputtering. In these methods, a coating comprising a sputtered target material is deposited on a substrate.

[0004] In this respect, in particular, it is known to pretreat the substrate before applying the coating in order to achieve good coating adhesion. In addition to chemical and mechanical pretreatment steps, an ion etching step, in which ions are accelerated towards the substrate by an accelerating voltage, thereby producing an etching effect on the substrate surface, is suitable for pretreating substrates such as hard metal substrates or steel substrates.

[0005] WO 2009 / 132822 A2 describes a device and method for pre-treating and coating an object by magnetron sputtering. The device comprises a vacuum chamber with a metal chamber wall and a magnetron in which a sputtering target is arranged. At least one of the magnetrons is provided for operation according to high power pulsed magnetron sputtering (HPPMS, also referred to as HIPIMS). An electric pulse is fed to the HPPMS magnetron, wherein a capacitive element is connected to the sputtering target by a switching element. In the method, the object to be coated is arranged in the vacuum chamber of the device, and plasma is generated during the operation of the HPPMS magnetron. In the etching step, a negative bias is applied to the object and the object is etched by bombarding with metal ions. Subsequently, the bias is continuously reduced so that the material sputtered by the sputtering target produces a layer accumulation on the object.

[0006] DE 10 2006 019 000 A1 describes an apparatus and a method for plasma-enhanced deposition of hard material coatings, in particular an apparatus and a method for producing titanium-aluminum-nitride layers. A substrate support that can rotate around a central axis is arranged in a vacuum chamber. At least one vaporization source and at least one hollow cathode are arranged radially outside the substrate support. In a plane at right angles to the axis, the line between the hollow cathode and the associated anode is offset by 15° to 70° relative to the line between the target of the vaporization source and the axis. The arc discharge of the hollow cathode is maintained parallel to the axis and the vaporization of the target material from the vaporization source. A target with a Ti:Al ratio of 1:1 is used to produce titanium-aluminum-nitride coatings with a Ti:Al ratio of 50:50 to 40:60 in a reactive nitrogen atmosphere.

[0007] EP 2 042 261 A2 describes a method for producing a coated cutting tool, the method comprising: providing a substrate, depositing a cathodic arc evaporation PVD coating of a nitride, oxide, boride, carbide, carbonitride, carbonoxynitride or a combination thereof on the substrate. During deposition, the coating is subjected to more than one ion etching step. The cutting tool exhibits an increased life due to the increased smoothness of the PVD coating due to a reduced number of surface defects.

[0008] It can be considered an object to specify a coated body and a method for coating a substrate and a coating system for carrying out the method, in which a particularly high-quality and durable coating can be achieved.

[0009] This object is achieved by a method according to claim 1, a coating system according to claim 12 and a coated body according to claim 13. The dependent claims relate to advantageous embodiments of the invention.

[0010] It has been shown that coatings applied in PVD methods can have different properties depending on the coating thickness. In particular, it has been shown, for example, that longer coating durations and greater coating thicknesses generally increase roughness and residual stresses in the coating. Therefore, the basic idea of ​​the invention is not to produce the coating in a continuous manner, but to interrupt the growth of the coating once or several times in a targeted manner and then restart the growth of the coating.

[0011] The method according to the invention initially provides a pretreatment of the substrate by an ion etching process in a first method step. Here, ions such as gas ions or preferably metal ions are generated and the ions are accelerated toward the substrate surface by a bias voltage. Due to the impact ions, an etching effect that may include activation of the substrate surface, removal of surface material and ion implantation occurs over the entire exposure time.

[0012] In the second step of the method according to the invention, a first coating layer with a thickness of 0.1 μm to 6 μm is deposited on the substrate by a PVD process. Magnetron sputtering is used as the coating method. The coating process is performed for a selected coating duration so that the first coating layer is deposited on the substrate surface.

[0013] According to the invention, the application of the coating in the second step is interrupted by a third method step as a further etching step. In the third method step, according to the invention, the surface of the previously produced first coating layer is treated by an ion etching process. The ion etching process of the third method step can preferably be a process of the same type as in the first method step; the method parameters used, in particular the etching duration and the bias voltage, can be selected so as to be identical or different from one another.

[0014] By using an etching process in the third method step, the layer growth is initially interrupted. Depending on the intensity of the etching step, a more or less substantial amount of layer material can be removed. In addition, the etching process leads to nucleation of the surface due to the introduction of microscopic defects.

[0015] In a fourth method step according to the invention, following the third method step, a further coating layer with a thickness of 0.1 μm to 6 μm is deposited on the first coating layer or on the surface of the first coating layer prepared by a previous etching step by a PVD cathode sputtering process. Preferably, in the fourth method step, a coating method of the same type as in the second method step is used. In both steps, individual or all method parameters can be selected to be identical or different from each other.

[0016] The method according to the invention thus comprises a sequence of steps - coating, etching, coating - which can also be referred to as a "repeat-start" procedure.

[0017] Surprisingly, it has been found that a repetitive-start procedure (i.e., interrupting the coating process with ion etching and subsequently continuing the coating) produces structural changes in the multilayer coating compared to a single-layer coating applied once and without interruption of the coating formation by an intermediate etching step. For example, the microstructure produced during the formation of the coating can be at least partially interrupted by an intermediate etching step, so that in the subsequent coating step there is no seamless continuation of the previous growth, but rather the formation of new growth nuclei. While in some cases the continuous coating process may make the coating morphology rougher in the direction of growth, this effect can be reduced or even completely reversed by the intermediate etching step. Thus, a coating morphology can be achieved in which the layer structure of the additional coating layer applied after the intermediate etching step is finer than the layer structure of the previous coating layer at least at the surface at the beginning (i.e., adjacent to the interface region relative to the previous coating layer).

[0018] In particular, the residual stress in the produced coating can be influenced. The residual stress in the coating can increase with increasing coating duration and thickness. It has been shown that the residual stress in the multilayer coating does not increase to the same extent as in the case of a single-layer coating when the coating is interrupted and restarted within the scope of a repeat-start process. Therefore, a coating with an overall lower residual stress is obtained by using a repeat-start method at longer coating durations and greater coating thicknesses. A coating with lower residual stress has more favorable ductility properties and better adhesion to the substrate.

[0019] It has been shown that by interrupting the growth one or more times, it is possible overall to produce layers which have a lower number of defects and are therefore denser and less porous. On the one hand, this can result in a smoother layer surface. On the other hand, a denser layer has significant advantages in terms of chemical resistance, since a denser structure means that there are fewer diffusion paths, for example, for atmospheric oxygen which diffuses in undesirably during use, which can lead to failure of the coating.

[0020] As will be apparent to a person skilled in the art, the sequence of the first to fourth steps described above can be modified, for example, by subdividing the coating step or etching step into a plurality of sub-steps with different coating parameters or etching parameters or by temporally inserted method steps involving other treatment measures, such as heat treatment (annealing) or chemical treatment (e.g. oxidation, carburizing), etc. However, the basic pattern (i.e. the sequence of the first to fourth steps) always remains the same.

[0021] Although the advantages of the repeat-start process have become apparent after a single application, multiple applications can show particular advantages. For example, following the fourth method step, the surface of the topmost coating layer can be treated by an ion etching process, and subsequently, additional coating layers can be deposited on the coating layer below by a PVD cathode sputtering process. This can be repeated once or multiple times, thereby producing, for example, at least three or four coating layers. The total number of repetitions of the repeat-start sequence can be selected, for example, according to the type and desired thickness, so that 2 to 50 coating layers are formed, preferably 3 to 20, more preferably 3 to 10 or 3 to 5.

[0022] In principle, the advantage of interrupting and subsequently continuing the growth of the coating can also be harnessed if individual method steps or even all method steps are carried out so that they are separated from one another in space and / or time, for example at separate locations or in separate processing or coating systems, if applicable after intermediate storage, etc. However, it is particularly effective to carry out the method steps in the same coating system, in particular in the same vacuum chamber. Preferably, the implementation of two or more of the above-mentioned method steps is carried out without interrupting the vacuum, for example, the repetition-starting steps (second method step—coating, third method step—ion etching, fourth method step—coating), particularly preferably the implementation of the first to fourth steps.

[0023] Preferably, more than one method step or all method steps can be performed in the same vacuum chamber of the coating system and / or using the same electrode (e.g., cathode and / or electrically connected to the substrate or holder), wherein only the power supply and / or the device for changing the pressure or atmosphere are switched to perform different method steps without equipping the instrument with new mechanical tools. However, for example, various magnetron cathodes (e.g., HIPIMS cathodes and DC cathodes) can also be arranged in the same vacuum chamber, which can then be started differently in the method steps or even disconnected in a single method step. Similarly, cathodes equipped with different palladium can be used. In this way, in continuous method steps, different process parameters can be achieved only by external control without equipping the system instrument with new mechanical tools or without interrupting the vacuum between method steps.

[0024] Like the temporally interleaved etching steps, the coating steps can also be identical or different from one another, for example with respect to the duration of application and / or process parameters such as pressure, atmosphere composition, target material, voltage / electric power etc.

[0025] Preferably, a negative bias is applied to the substrate during both the coating step (i.e., the second method step and the fourth method step, and (if applicable) the further method step in which the coating layer is produced by PVD magnetron sputtering) and the one or more etching steps. In this respect, the bias in the third method step is preferably higher than in the second method step and the fourth method step. By means of a higher bias, the ions of the plasma are accelerated more strongly onto the substrate, and therefore ion etching is performed at a higher bias. Therefore, it is possible to switch between the operating modes of coating and etching by changing the bias.

[0026] According to a preferred embodiment of the invention, in addition to the second method step and the fourth method step, a further coating step may optionally be carried out to produce a corresponding coating layer with a thickness of 0.1 μm to 6 μm, preferably 0.5 μm to 5 μm, more preferably 1 μm to 4 μm, particularly preferably, the thickness of at least two consecutive coating layers differs from each other by less than + / -50%, more preferably less than + / -25%, particularly preferably less than + / -15% (in each case, relative to the thinner coating layer). More preferably, this applies to all coating layers produced in the repeat-start process.

[0027] By means of the method according to the invention, coatings having a total thickness of 12 μm or more are produced.

[0028] For such thick coatings, particular advantages of the method according to the invention are present. The total thickness can be up to 30 μm. The continuous production of single-layer coatings with such thicknesses by PVD coating methods usually leads to such rough structures and / or high residual stresses that the coatings are no longer usable for many applications, for example due to insufficient coating adhesion and / or excessive roughness. Surprisingly, these disadvantages can be prevented by subdividing the thick coating into, for example, two or more, preferably three or more coating layers.

[0029] For at least one, preferably all, of the method steps of applying the coating (ie the second method step, the fourth method step and / or one or more further method steps), a cathode sputtering method is used in which at least one target of at least one magnetron cathode is sputtered.

[0030] Although in this method, for example, a DC voltage, an AC voltage or a pulsed voltage can be applied to the cathode, the HIPIMS method is particularly preferred. The HIPIMS method is a class of methods that can also be referred to as "high power pulsed magnetron sputtering" and in which the magnetron cathode is supplied with electrical power in the form of very short but extremely high energy pulses, as a result of which a high ion density can be achieved in the coating particles in front of the magnetron cathode. During the pulse, for example 60 W / cm 2 or greater, preferably 100 W / cm 2 or greater, particularly preferably 200 W / cm 2 Up to 2,300W / cm 2 A high peak power (per cathode, related to the target surface area of ​​the corresponding cathode) is a characteristic of the HIPIMS method. In addition, the duty cycle (i.e., the ratio of the pulse duration to the pulse interval) is typically less than 0.5, i.e., the pulse interval is longer than the pulse duration. The applicant discloses, for example, in WO 2009 / 132822 A2, an apparatus and a method for operating a magnetron cathode by HIPIMS. The HIPIMS coating method is preferably understood to mean that according to the HIPIMS method, one, more or all cathodes in the vacuum chamber of the coating system are operated under high power pulses, wherein, if necessary, other cathodes can be operated simultaneously in DC mode.

[0031] The pulse duration preferably used in the HIPIMS method can be, for example, 5 μs to 200 μs. The HIPIMS pulses can preferably be generated at a frequency of, for example, 100 Hz to 10,000 Hz, particularly preferably 2,000 Hz to 6,000 Hz.

[0032] In one or more coating steps, a bias, in particular a negative bias, is preferably applied to the substrate so that the positively charged ions are accelerated toward the substrate surface. In particular, when magnetron sputtering is used, for example, at at least one magnetron cathode under a DC voltage, a pulsed DC voltage or a HIPIMS pulse, the bias may be a constant DC voltage or a pulsed DC voltage. The pulsed DC voltage is preferably pulsed in a unipolar manner. The pulse frequency may be in the MF (medium frequency) range, for example 50kHz to 3MHz, preferably 100kHz to 1MHz, particularly preferably 150kHz to 500kHz.

[0033] However, according to a preferred embodiment, the HIPIMS coating method is performed with a pulse bias applied to the substrate. Preferably, in this case, the bias pulse can be synchronized in time with the HIPIMS pulse applied to the cathode. "Synchronization" is understood to mean a pulse (bias pulse) that applies a bias at the same frequency as the HIPIMS pulse at one or more cathodes, or means that the frequencies are integer multiples of each other. In the case of a plurality of HIPIMS cathodes that are controlled so that the HIPIMS pulses are not applied simultaneously but sequentially, the pulse frequency of the bias pulse preferably corresponds at least to the HIPIMS pulse frequency multiplied by the number of HIPIMS cathodes.

[0034] In this aspect, the HIPIMS pulse and the bias pulse can be synchronized in time so that they have the same duration and start at the same time. However, preferably, the duration can also be different and / or an advance or delay time (offset) of the bias pulse relative to the associated HIPIMS pulse can be specified. Particularly preferably, the synchronization is such that the bias pulse appears with a delay (offset) of, for example, 5 microseconds or more, preferably 20 microseconds to 50 microseconds or more, relative to the specified HIPIMS pulse. In addition, the synchronization is preferably such that the bias pulse in each case has a lag time of, for example, 5 microseconds or more, preferably 10 microseconds or more, after the specified HIPIMS pulse.

[0035] It has been shown that when applying HIPIMS pulses, different types of ions, particularly metal ions and gas ions, occur at different times. A large amount of gas ions are usually observed in the early stages of the HIPIMS pulse, and the appearance of higher density metal ions can be observed as time delays. By delaying the bias pulse relative to the HIPIMS pulse in a targeted manner, metal ions and less gas ions can be preferably accelerated toward the substrate by the bias voltage applied. It has been shown that injecting gas ions significantly contributes to the increase of residual stress in the coating when forming a coating. A coating with low residual stress can be obtained by: synchronizing the bias pulse with the cathode pulse in time so that the voltage of the bias pulse is applied during the time interval rich in metal ions.

[0036] For the composition of the coating or each coating layer, various ingredients can be considered. On the one hand, these ingredients include one or more target materials released by sputtering. On the other hand, the ingredients can be supplied in gaseous form. In particular, the coating can be carried out in a reactive coating process, for example, by supplying a reactive gas containing nitrogen, oxygen and / or carbon.

[0037] Preferably, the coating is a hard material coating. Each coating layer can, for example, be composed of such a material system: the material system contains one or more metal elements, or preferably, contains at least one metal element and at least one non-metallic element. In particular, the material system can be composed of one or more metal elements and one or more non-metallic elements. Binary hard materials, ternary hard materials and quaternary hard materials, that is, hard materials with two, three or four different metal elements are preferred. In this regard, such a composition is preferred: wherein one or more metal elements are selected from the group of elements of Groups 4 to 6 of the IUPAC Periodic Table (1988). (For simplicity, in this context, semi-metallic Si and B are considered to be metal elements). Particularly preferably, Ti is included in the composition as one of the metal elements. The non-metallic element can, for example, be selected from the group including C, N and O, preferably from the group including C and N, and particularly preferably, N is provided as the only non-metallic element.

[0038] In the following examples, the composition of the coating is directly referred to as a chemical compound or phase or as a material system. In this aspect, the material system is specified by a list of elements contained therein, each separated from each other by a dash, wherein the metal elements are indicated first, followed by the non-metal elements. In each case, the metal elements and the non-metal elements are preferably named in the order of their proportions (in atomic percentages). The name of the material system may correspond to a chemical compound, but this is not always the case. For example, the material system Ti-C will contain the hard material compound TiC or be completely composed of the hard material compound TiC, while the material system Ti-B contains the hard material compound TiB2 or is composed of the hard material compound TiB2. Preferred material systems include, for example, Al-Ti-N, Ti-B, Ti-Si-N, Al-Ti-Si-N, Ti-CN, Al-Ti-Cr-Si-N or Ti-Al-CN. Metals such as Al, Ti, Si and / or Cr are preferably provided as components of one or more cathode targets in solid form.

[0039] In a preferred embodiment, at least one coating layer, preferably a plurality of coating layers or all coating layers are made of Al x -Ti 1-x-N formation, further preferably, wherein x≥0.4 or x≥0.5, particularly preferably 0.55≤x≤0.65. The x of the Al portion is preferably at most 70%.

[0040] At least two coating layers, preferably more or all coating layers, of the coating formed during the coating step may have the same elements, i.e. the same material system and, if applicable, the same relative proportions of the elements contained. Alternatively, different compositions for the coating layers may also be provided.

[0041] The ion etching process in the first method step, the third method step and / or the other method step can preferably be performed by igniting the plasma by means of a cathode and applying a relatively high accelerating voltage (bias) to the substrate. For example, the plasma can be mainly composed of gas ions. Alternatively, the cathode can be operated with a HIPIMS pulse to produce a plasma with a large amount of metal ions. The bias voltage can preferably be a constant DC voltage or a unipolar or bipolar (MF-) pulsed DC voltage in a unipolar or bipolar manner.

[0042] As described below based on an exemplary embodiment, the ion etching process may include multiple sub-steps, such as an etching sub-step and another etching sub-step, in which a plasma is generated and a bias voltage in the form of a DC voltage pulsed in a bipolar manner at an intermediate frequency of, for example, 50kHz to 1MHz and at a pulse height of, for example, 100V to 1,000V, preferably 300V to 800V is applied for a first time period, and in the other etching sub-step, after the plasma is generated, a bias voltage in the form of a DC voltage in the range of, for example, -50V to -400V, preferably -100V to -300V is applied for a second time period. The second time period is preferably longer than the first time period, further preferably at least twice as long. As an example, the first time period can be 5 minutes to 30 minutes, and the second time period can be 30 minutes to 200 minutes, preferably 40 minutes to 150 minutes.

[0043] The two etching sub-steps differ in their effect on the substrate, in particular due to the use of electrical edge effects in the presence of a DC bias. Etching with an MF pulse bias has a substantially uniform effect on all surfaces of the substrate. In the case of etching with a DC bias, mainly the edges, i.e., in particular the cutting edges, are etched.

[0044] The parameters of the ion etching process in the first method step in which the substrate is etched can be consistent with the parameters of the etching process in the third method step (and (if applicable) the other method steps in which other intermediate etchings are performed). Alternatively, different parameters can also be used. For example, the substrate can be etched for a longer time in the first method step than in the subsequent intermediate etching step in which the relevant surface of the coating is etched. Further preferably, a lower bias voltage can be applied in the first method step, for example, compared with other etching steps. The total amount of material removed in the intermediate etching step preferably corresponds to less than 20% of the thickness of the relevant coating, more preferably less than 10%, more preferably less than 5% or less, particularly preferably 2% or less.

[0045] The method according to the invention is particularly suitable for producing tools, in particular tools having at least one cutting edge. In particular, for example, drills, milling cutters or indexable inserts are preferred.

[0046] The coated substrate can be composed of various materials such as steel (HSS). Preferably, the coated substrate is a hard metal, in particular a WC / Co sintered material. Likewise, the method according to the invention can also be applied to other types of substrate materials, such as cBN substrates or ceramic substrates.

[0047] According to a second aspect, the present invention also relates to a coating system for performing the method according to the present invention. The system comprises a vacuum chamber and a device such as a substrate holder for arranging the substrate in the vacuum chamber, preferably a substrate holder for rotating the substrate, and particularly preferably a substrate holder for planetary rotation. A device for generating plasma is provided in the vacuum chamber, preferably a magnetron cathode connected to a suitable power supply. In addition, a device for generating a bias voltage on the substrate is provided, preferably a power supply attached to the substrate. Two power supplies can be attached to a counter electrode such as a chamber wall or a separate anode.

[0048] According to the invention, the coating system comprises a control device for controlling the coating system to automatically perform the method according to the invention. The control device may, for example, comprise a programmable computer having an operating program that specifies the method steps according to the invention. In particular, the device for generating plasma and / or the device for generating a bias voltage may preferably be controlled by the control device. The programming preferably comprises at least one cycle for repeating the method steps of the programming to implement the above-mentioned repeat-start method.

[0049] According to a third aspect, in addition to the method according to the invention, the present invention also relates to a coated body preferably produced by the method according to the invention. The coated body according to the invention comprises a substrate and at least one coating applied to the substrate. The coating comprises at least two coating layers each having a thickness of 0.1 μm to 6 μm. The interface region formed by ion etching is arranged at least between the two coating layers. At the interface region, due to the above-mentioned interruption of the growth of the layer, the coating layer has a visible structural change, i.e. different layer morphologies directly adjacent to each other.

[0050] The coating can preferably comprise more than two coating layers each of 0.1 μm to 6 μm, with an interface region formed by ion etching being arranged in each case between the coating layers.

[0051] According to claim 13, the morphology of the coating is such that if - viewed in the direction of increasing distance from the substrate - a first coating layer and a subsequent second coating layer are separated from each other by an interface region, the structure of the adjoining interface region of the second coating layer is finer than the structure of the adjoining interface region of the first coating layer. Thus, the interface region is preferably characterized by a change in the coating morphology from a coarser morphology to a finer morphology.

[0052] The morphology can be assessed in a manner known to the person skilled in the art, for example based on a structural domain model, for example according to Thornton (Thornton, J., 1974. Influence of apparatus geometry and deposition conditions in the structure and topography of thick sputtered coatings. Journal of Vacuum Science & Technology, Vol. 11, pp. 666-670).

[0053] Preferably, the coating generally has lower residual stress than a coating of equal thickness deposited continuously under otherwise identical conditions (ie, without interruption and without forming an interface region by ion etching).

[0054] Hereinafter, exemplary embodiments will be described in more detail with reference to the accompanying drawings, in which:

[0055] Figure 1 is a schematic diagram of a coating system in a top view;

[0056] Figure 2 For Figure 1 A schematic diagram in perspective view of a portion of a coating system;

[0057] Figure 3 One embodiment of a coated body in the form of an indexable insert is shown;

[0058] Figure 4 For Figure 3 A schematic cross-sectional view of a coating having multiple coating layers of a coated body;

[0059] Figure 5 is a flow chart of an exemplary embodiment of a coating process;

[0060] Figure 6 is a graph showing the history of various electrical variables over time during a coating step;

[0061] Figure 7a is a photograph of calotte grinding of a coating according to an exemplary embodiment;

[0062] Figure 7b is a photograph of dome grinding of a coating according to the reference method;

[0063] Figure 7c is the SEM image of the coating on the substrate;

[0064] Figure 7d For Figure 7c An enlarged view of a portion of the SEM photograph.

[0065] Figure 1 and Figure 2 A PVD coating system 10 is shown, which includes a vacuum chamber 12. The interior 20 of the vacuum chamber 12 can be evacuated to create a vacuum through an exhaust port 14. A process gas, preferably a noble gas or a mixture of various noble gases such as argon and / or krypton, can be fed via an inlet 16. A reactive gas such as nitrogen can be fed via an inlet 18. In an alternative embodiment, the inlets 16, 18 can be replaced by a common inlet for the process gas and the non-flammable reactive gas.

[0066] Four magnetron cathodes 22a, 22b, 22c, 22d each having a plate-shaped sputtering target 24a, 24b, 24c, 24d are arranged in the interior 20 of the vacuum chamber 12. For better viewing, Figure 2 Only two magnetron cathodes 22a, 22b are shown.

[0067] The magnetron cathodes 22a, 22b, 22c, 22d and their sputtering targets 24a, 24b, 24c, 24d are oriented toward the center of the vacuum chamber 12. There is a rotatable substrate stage 30 on which a number of rotatable substrate plates 32 are arranged, the rotatable substrate plates 32 having substrate holders 34. In the example shown, indexable inserts 40 are loaded as substrates. The substrate holder 34 is a vertical rod-shaped holder on which the indexable inserts 40 are placed. The indexable inserts 40 are electrically connected to the substrate stage 30 via the substrate holders 34 and the substrate plates 32. For better viewing, Figure 2 Only the substrate holder 34 of one substrate plate 32 is shown.

[0068] Figure 3 The indexable insert 40 is shown in FIG. The indexable insert 40 includes a rake face 42 and a side face 44. Figure 2 In the arrangement shown in , the side faces 44 are arranged parallel to the sputtering targets 24a, 24b, 24c, 24d of the magnetron cathodes 22a, 22b, 22c, 22d. The edge between the faces 42, 44 is intended to be used as a cutting edge during machining. The indexable insert 40 comprises a WC / Co sintered hard metal.

[0069] The indexable insert 40 is only one example of a substrate to be coated. Alternatively, differently shaped components or tools can be loaded on a suitably shaped substrate holder 34 in each case.

[0070] The magnetron cathodes 24a, 24b, 24c, 24d are connected to corresponding controllable power supplies 26a, 26b, 26c, 26d, through which a voltage can be applied to the conductive wall of the vacuum chamber 12.

[0071] Attached to the substrate stage 30 is a controllable bias power supply 36 , by which a voltage directed to the walls of the vacuum chamber 12 can be applied to the substrate stage 30 , the substrate holder 34 , and the substrate 40 .

[0072] In this case, power supplies 26a, 26b, 26c, 26d, 36 are each only schematically shown as a controllable voltage power supply. It can be a conventional DC power supply, a pulse power supply and / or a HIPIMS power supply. In the example shown, power supplies 26a, 26b, 26c, 26d are controlled so that they can switch between a DC operating mode and a HIPIMS operating mode. In an alternative embodiment, corresponding dedicated DC cathodes and HIPIMS cathodes can be arranged inside the vacuum chamber 12 and connected with dedicated DC power supplies and HIPIMS power supplies, and then can be activated or deactivated as needed when started by a central control unit 36.

[0073] The power supplies 26a, 26b, 26c, 26d, 36 and the pumps (not shown) at the inlets 16, 18 and outlet 14 are each attached to a central control unit 36 ​​of the system 10. The central control unit 36 ​​can be programmed so that all parameters of the pretreatment and coating methods performed in the interior 20 of the vacuum chamber 12 are controlled by the control unit 36.

[0074] In the following, the sequence of the coating process programmed in the central control unit 36 ​​will be explained by way of example:

[0075] Example: PVD hard material coating with great thickness

[0076] A hard material coating having a particularly large thickness of more than 10 μm is applied to coat a substrate, such as an indexable insert 40. Coatings of this thickness generally cannot be applied with sufficient coating adhesion for machining applications.

[0077] Figure 5 Schematically shown is the sequence of the coating process which is automatically prescribed by programming of the central control unit 36. Titanium plates, each provided with an aluminum plug, serve as sputtering targets 24a, 24b, 24c, 24d inside the system 10. In a preparatory step 60, the substrate 40 is charged inside the system 10, the vacuum chamber 12 is evacuated to a pressure of 350 mPa and heated.

[0078] Subsequently, the surface 54 of the hard metal material 52 of the substrate 40 is etched in a first etching step 62. In the illustrated embodiment, the first etching step 62 is a combined etching step having a first etching substep and a second etching substep, by which the substrate surface is cleaned and etched by gas ions.

[0079] In the first etching sub-step, ion etching is performed, wherein plasma is initially ignited by the magnetron cathodes 22a, 22b, 22c, 22d.

[0080] The bias power supply 36 is thus activated so that a bias voltage of -650 V against the chamber wall and pulsed in a bipolar manner at a medium frequency (240 kHz) is applied to the substrate 40. In this way, the gas ions of the plasma are accelerated onto the surface 54 of the substrate 40.

[0081] The first etching sub-step was applied for a period of about 15 minutes. This resulted in a low etching removal rate of 0.1 μm / hour.

[0082] In the second etching sub-step, ion etching is performed again, wherein the plasma is initially ignited again by the magnetron cathodes 22a, 22b, 22c, 22d.

[0083] With an argon / krypton gas mixture supplied as the process gas, the bias power supply 36 was activated for a processing time of 60 minutes so that the substrate 40 was subjected to a constant DC bias of -200 V having a negative potential.

[0084] The etching removal in the second etching sub-step was about 0.5 μm / hour.

[0085] Since a part of the central control unit 36 ​​is switched on and without interrupting the vacuum, the etching step 62 is followed by a coating step 64 in which the power supplies 26a, 26b, 26c, 26d of the magnetron cathodes 22a, 22b, 22c, 22d are activated so that they operate under short high voltage pulses in HIPIMS mode. During the coating step 64, each of the four magnetron cathodes 22a, 22b, 22c, 22d is supplied with a peak power of about 100kW.

[0086] The bias power supply 36 is activated so that a pulsed bias of, for example, -50 V to -150 V is applied, wherein the bias pulse is synchronized with the power pulse of the magnetron cathodes 22a, 22b, 22c, 22d. In this aspect, the bias voltage is provided with an offset so that the bias pulse starts with a slight time delay relative to the HIPIMS pulse.

[0087] During the coating time of about 100 minutes, nitrogen was fed as reactive gas in addition to argon / krypton as process gas.

[0088] Figure 6 An example of a time profile of various electrical variables, namely, voltage 80 (solid line), cathode current 82 (dashed line), cathode peak power 84 (dotted line), bias voltage 86 (dotted line), and bias current 88 (dashed line) at the magnetron cathodes 24a, 24b, 24c, 24d during the coating step 64 is shown. As can be clearly seen, the voltage 80 is applied to the magnetron cathodes 24a, 24b, 24c, 24d in pulses 90, while the bias voltage 86 is applied in bias pulses 92 that trail in time.

[0089] Figure 4 The structure of a coating 50 on a hard metal substrate material 52 is schematically shown. A first coating layer 56a is produced there in a coating step 64. The coating rate is about 2 μm / hour, so that at the end of the coating step 64 a first coating layer 56a thickness of about 3 μm is produced.

[0090] The material system of the first coating layer 56a is Al—Ti—N, with an Al content x (in the metal element) of approximately 60%.

[0091] By delaying the bias pulse 92 relative to the HIPIMS pulse 90 , relatively few gas ions are implanted into the coating layer 56 a , and thus the coating layer 56 a has a relatively low residual stress.

[0092] The coating step 64 is followed by an intermediate etching step 66. In the embodiment shown, the intermediate etching step 66 is carried out using the same parameters as in the first etching step 62, i.e. with two consecutive etching sub-steps. As already mentioned, alternatively, the etching steps 62, 66 may be carried out using different parameters, in particular wherein the duration of the intermediate etching step is shorter than the first etching step 62.

[0093] Since the etched coating layer 56 a is harder than the substrate surface etched in the first etching step 62 , the amount of material removed in the intermediate etching step 66 is significantly less than the above-indicated value for the first etching step 62 .

[0094] Subsequently, a further coating step 68 follows. In the present embodiment, the coating step 68 corresponds to the previous coating step 64 with respect to all parameters used. In the embodiment shown, the coating step 68 is also carried out for the same duration as the previous coating step 64. Alternatively, different coating steps can be carried out using different parameters, so that coating layers that differ, for example, in thickness, structure and / or composition are produced.

[0095] In the present exemplary embodiment, the coating / intermediate etching / coating cycle controlled in cyclic form by the programming of the central control unit 36 ​​is repeated until a total of four coating layers 56a, 56b, 56c, 56d are deposited one on top of the other in each case with intermediate etching of the underlying surface ( Figure 4 ). Thereafter, the substrate 40 is cooled in a subsequent step 70 .

[0096] By interrupting the layer growth at various points by means of the intermediate etching step 66, there is no further growth of crystals after the subsequent coating step 68 is started again, but new crystallization nuclei are formed. Although the coating steps 64, 68 are each carried out using the same parameters as in the example given above, the resulting coating 50 has a structure with identifiable separate coating layers 56a, 56b, 56c, 56d.

[0097] Figure 7a The case of dome grinding on the surface 44 of the coated body 40 is shown. The interface region between the coating layers 56a, 56b, 56c, 56d and formed as a ring by the intermediate etching step can be seen. In contrast, Figure 7b A continuously produced coating without such rings after dome grinding is shown.

[0098] Figure 7cSEM photograph of substrate material 52 with coating layers 56a, 56b, 56c, 56d formed thereon. The interface region is indicated by the white frame. The corresponding changes in the coating morphology are difficult to discern in situ at the magnification shown, but are more clearly seen at higher magnifications ( Figure 7d ). Figure 7c and Figure 7d (The latter is clearer) shows that at least for the first interface region, the coating morphology changes from a coarser structure to a substantially finer structure - as viewed from the substrate surface. In the structural domain model according to Thornton, this corresponds to a change from structural domain 1 to structural domain T.

[0099] The surface of the coating 50 proves to be smooth, dense and substantially free of pores. Thus, the tool 40 coated with the coating 50 has a high resistance for different applications, in particular for machining purposes.

[0100] The total thickness of coating 50 is about 12 μm. Whereas the reference coating using the same parameters but applied continuously exhibits very high coating residual stress and poor adhesion to substrate material 52, coating 50 having the same thickness has only a compressive stress of about -1.4 GPa and good coating adhesion.

[0101] Further possible embodiments can be taken from the following table, which specifies the coating material, total coating thickness and number of coating layers for various examples as well as the type of coated tool, its application and the workpiece material machined with the tool.

[0102] In the exemplary embodiment, for the sake of simplicity, it is assumed that the coating layers each have at least substantially the same thickness, ie, for example, a coating layer with a total coating thickness of 12 μm and 4 coating layers each being 3 μm thick.

[0103]

[0104]

[0105]

[0106]

[0107]

[0108]

[0109]

[0110] Although exemplary embodiments of the method are given above by way of example only, a person skilled in the art will recognize that the principles can be applied to various material systems, layer structures, coating types and coating parameters and to a variety of applications. Although the advantages of particularly thick coatings 50 are presented above, advantages may also be present for thin coatings, such as coatings with a total thickness of less than 1 μm on very fine drills (micro drills) and formed, for example, of three coating layers each measuring 0.2 μm.

[0111] The components of the PVD coating system 10 and in particular the magnetron cathodes 22a, 22b, 22c, 22d therein and their circuits should be considered as examples only. Alternatively, different numbers of magnetron cathodes can be provided inside the vacuum chamber 12. Different cathodes can be connected to different types of power supplies, for example, different cathodes can also be connected to a pure DC power supply. As shown, the power supply can be connected to the chamber wall or alternatively, a separate anode electrically separated from the chamber wall can be provided. For DC for magnetron cathode operation, in particular, it is preferred that the magnetron cathode is connected to an anode of this type.

Claims

1. A method for coating a substrate (40), wherein - in a first method step (62), the substrate is pretreated in an ion etching process, - in a second method step (64), depositing a first coating layer (56a) having a thickness of 0.1 μm to 6 μm on the substrate (40) by a HIPIMS PVD cathode sputtering process using HIPIMS pulses applied to cathodes (24a, 24b, 24c, 24d), the HIPIMS PVD cathode sputtering process being carried out while applying a DC bias to the substrate with bias pulses, the bias pulses being synchronized in time with the HIPIMS pulses, - in a third method step (66), the surface of the first coating layer (56a) is treated by an ion etching process, - in a fourth method step (68), a second coating layer (56b) having a thickness of 0.1 μm to 6 μm is deposited on the first coating layer (56a) by means of the HIPIMS PVD cathode sputtering process, so that an interface region is formed between the first coating layer (56a) below and the second coating layer (56b) on the first coating layer (56a), - wherein the structure of the second coating layer (56b) adjoining the interface region from above is finer than the structure of the first coating layer (56a) adjoining the interface region from below, - optionally, repeating the third method step (66) and the fourth method step (68) one or more times, depositing one or more further coating layers (56c, 56d) with a thickness of 0.1 μm to 6 μm by means of the HIPIMS PVD cathode sputtering process, - wherein the thickness of the coating layers deposited on top of one another amounts to 12 μm to 30 μm, - In the first method step (62), the ion etching pretreatment process is carried out as a first etching sub-step with an mf pulse bias and a second etching sub-step with a constant DC bias.

2. The method according to claim 1, characterized in that - Following said fourth method step (68), one or more times -First, the surface of the topmost coating layer is processed by an ion etching process, - Subsequently, a further coating layer is deposited on the underlying coating layer by means of the HIPIMS PVD cathode sputtering process.

3. The method according to claim 2, characterized in that For each further coating layer, an interface region is formed between the lower coating layer and the further coating layer thereon, wherein in each case the structure of the upper coating layer adjoining the interface region from above is finer than the structure of the lower coating layer adjoining the interface region from below.

4. The method according to claim 1, characterized in that At least the second method step (64), the third method step (66) and the fourth method step (68) are carried out without interrupting the vacuum.

5. The method according to any one of claims 1 to 3, characterized in that - in each of the second method step, the third method step and the fourth method step, applying a bias voltage to the substrate, - wherein the bias voltage is higher in the third method step than in the second method step and in the fourth method step.

6. The method according to any one of claims 1 to 3, characterized in that - Metal ions are generated during the ion etching process and are accelerated towards the substrate surface by a bias voltage.

7. The method according to any one of claims 1 to 3, characterized in that - One or more of the coating layers comprises at least a composition selected from the group consisting of: Al-Ti-N, Ti-B, Ti-Si-N, Al-Ti-Si-N, Ti-CN, Ti-Al-CN, Al-Ti-Cr-Si-N.

8. The method according to any one of claims 1 to 3, characterized in that - Multiple coating layers are produced from the same element.

9. The method according to any one of claims 1 to 3, characterized in that The substrate (40) is a cutting tool having at least one cutting edge.

10. A coating system for performing the method according to any one of claims 1 to 9, comprising: - a vacuum chamber (12), - means for arranging a substrate (40) in said vacuum chamber (12), - means for generating a plasma in said vacuum chamber (12), - means for generating a pulsed DC bias on said substrate (40), - and control means for controlling the coating system to automatically perform the method.

11. A coated body produced by the method according to any one of claims 1 to 9, comprising: - a substrate (40), - and a coating (50) with a thickness of 12 μm to 30 μm, the coating (50) being applied to the substrate by a HIPIMS PVD cathode sputtering process and comprising at least two coating layers each with a thickness of 0.1 μm to 6 μm, - wherein an interface region formed by ion etching is arranged between said coating layers, - wherein the coating layer comprises a first coating layer (56a) and a second coating layer (56b) on the first coating layer (56a), and the interface region is arranged between the first coating layer (56a) and the second coating layer (56b), - wherein the structure of the second coating layer (56b) adjoining the interface region from above is finer than the structure of the first coating layer (56a) adjoining the interface region from below.

12. The coated body according to claim 11, wherein - the coating (50) comprises three or more coating layers each having a thickness of 0.1 μm to 6 μm, - wherein an interface region formed by ion etching is arranged between each of said coating layers.

13. The coated body according to claim 11 or 12, wherein - The coating (50) has lower residual stress than a continuous coating of the same thickness formed without an interface region.

Citation Information

Patent Citations

  • Equipment and method for plasma-assisted deposition of hard material layers

    DE102006019000A1

  • Method of making a coated cutting tool

    EP2042261A2

  • Device and method for pretreating and coating bodies

    WO2009132822A2

  • Coated body

    CN101426947A

  • Method of making a coated cutting tool

    CN101691654A