Solid electrolytic capacitors with barrier coating
By using barrier coatings, particularly hydrophobic olefin polymers, on the terminals of solid electrolytic capacitors, the problems of shell material delamination and oxygen diffusion at high temperatures are solved, ensuring the stable electrical performance of the capacitors in high-temperature and high-humidity environments.
Patent Information
- Application Number
- CN202080065912.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-18
- Filing Date
- 2020-09-18
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-09-18
AI Technical Summary
Existing solid electrolytic capacitors are prone to microcracks in the casing material and oxygen diffusion at high temperatures, which leads to deterioration of electrical performance. Therefore, it is necessary to improve the mechanical stability and electrical performance of capacitors.
A barrier coating is used to cover the anode and/or cathode terminals, using hydrophobic resinous materials such as olefin polymers, with a glass transition temperature between 20°C and 160°C, to reduce delamination and oxygen diffusion.
The capacitor maintains stable electrical performance at high temperatures, with capacitance and ESR remaining within the expected range, low leakage current, and adaptability to high temperature and high humidity environments.
Smart Images

Figure CN114424307B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of U.S. Provisional Patent Application Serial No. 62 / 901,922, filed September 18, 2019, the entire contents of which are incorporated herein by reference. Technical Field
[0003] The present invention relates to the field of solid electrolytic capacitors, and more particularly, to solid electrolytic capacitors containing barrier coatings. Background Art
[0004] Due to the volumetric efficiency, reliability and process compatibility of electrolytic capacitors, electrolytic capacitors (e.g., tantalum capacitors) are increasingly used in circuit design. For example, a capacitor that has been developed is a solid electrolytic capacitor, which includes a tantalum anode, a dielectric layer and a conductive polymer solid electrolyte. In order to help protect the capacitor from the external environment and provide good mechanical stability for the capacitor, the capacitor element is also encapsulated with a housing material (e.g., epoxy resin) so that parts of the anode terminal and the cathode terminal are still exposed for mounting to the surface. Unfortunately, it has been found that the high temperatures often used in capacitor manufacturing (e.g., reflow soldering) may cause residual moisture to evaporate into steam, which may leave the housing with considerable force and cause microcracks to form in the housing material. These microcracks can cause the housing material to delaminate from the capacitor element and can also cause rapid deterioration of electrical performance. Further, oxygen may also diffuse into the cathode, further exacerbating the degradation of electrical performance at high temperatures, especially when the capacitor is exposed to high temperatures. Therefore, there is a need for an improved solid electrolytic capacitor that can exhibit better electrical performance, especially at high temperatures. Summary of the invention
[0005] According to one embodiment of the present invention, a solid electrolytic capacitor is disclosed, the solid electrolytic capacitor comprising: a capacitor element, the capacitor element comprising a sintered porous anode body, a dielectric overlying the anode body, and a solid electrolyte overlying the dielectric; an anode lead extending from a surface of the capacitor element; an anode terminal electrically connected to the anode lead; a cathode terminal electrically connected to the solid electrolyte; and a shell material encapsulating the capacitor element and the anode lead. A barrier coating is disposed on at least a portion of the anode terminal and / or at least a portion of the cathode terminal and in contact with the shell material. The coating comprises a hydrophobic resinous material comprising an olefin polymer having a glass transition temperature of about 20°C to about 160°C.
[0006] Other features and aspects of the present invention are described in more detail below. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] In the remainder of this specification, a full and enabling disclosure of the present invention, including the best mode thereof, is more particularly set forth to one of ordinary skill in the art with reference to the accompanying drawings, in which:
[0008] Figure 1 is a schematic diagram of one embodiment of a solid electrolytic capacitor that can be formed according to the present invention.
[0009] Repeat use of reference characters in the present specification and drawings is intended to represent the same or analogous features or elements of the invention. DETAILED DESCRIPTION
[0010] Those skilled in the art will appreciate that the present discussion is merely a description of exemplary embodiments and is not intended to limit the broader aspects of the invention, which are embodied in the exemplary constructions.
[0011] In general, the present invention relates to a solid electrolytic capacitor comprising a capacitor element, the capacitor element comprising a porous anode body, a dielectric overlying the anode body, and a solid electrolyte overlying the dielectric. An anode lead extends from the anode body and is in electrical contact with an anode terminal. A cathode terminal is also in electrical contact with the solid electrolyte. Further, a casing material encapsulates the capacitor element and the anode lead and exposes at least a portion of the anode terminal and at least a portion of the cathode terminal for external contact. To help minimize the possibility of delamination and oxygen diffusion, a barrier coating is also employed in the capacitor, the barrier coating covering at least a portion of the anode terminal and / or at least a portion of the cathode terminal and in contact with the casing material. The barrier coating comprises a hydrophobic resinous material including an olefin polymer having a glass transition temperature of from about 20°C to about 160°C, in some embodiments from about 40°C to about 150°C, and in some embodiments from about 60°C to about 120°C, as measured according to JIS K 7121:2012 (e.g., at a temperature ramp rate of 10°C / min). Without intending to be limited by theory, it is believed that these materials may not only function as a barrier to moisture and oxygen, but they may also contribute to an increased degree of adhesion of the resulting coating to the housing material, which makes such materials less likely to delaminate from the capacitor element when exposed to high temperatures often experienced during capacitor manufacturing (e.g., reflow soldering).
[0012] In the resinous material, any of a variety of olefin polymers with a desired glass transition temperature can be used. For example, in a specific embodiment, the olefin polymer can be a cycloolefin polymer. Cycloolefin resins are polymer compounds with a main chain consisting of a carbon-carbon bond, wherein at least a portion of the main chain has a cyclic hydrocarbon structure. The cyclic hydrocarbon structure is introduced by using a monomer that has at least one alkene double bond ("cycloolefin") in the cyclic hydrocarbon structure, such as norbornene or tetracyclododecene. For example, specific examples of suitable cycloolefin monomers for forming the polymer may include: monocyclic cycloolefins such as cyclopentene, cyclohexene, cyclooctene, cyclopentadiene, and 1,3-cyclohexadiene; bicyclic cycloolefins such as bicyclo[2.2.1]hept-2-ene ("norbornene"), 5-methyl-bicyclo[2.2.1]hept-2-ene, 5,5-dimethyl-bicyclo[2.2.1]hept-2-ene, 5-ethyl-bicyclo[2.2.1]hept-2-ene, 5-butyl ... ]hept-2-ene, 5-ethylidene-bicyclo[2.2.1]hept-2-ene, 5-hexyl-bicyclo[2.2.1]hept-2-ene, 5-octyl-bicyclo[2.2.1]hept-2-ene, 5-octadecyl-bicyclo[2.2.1]hept-2-ene, 5-methylene-bicyclo[2.2.1]hept-2-ene, 5-vinyl-bicyclo[2.2.1]hept-2-ene and 5-propenyl-bicyclo[2.2.1]hept-2-ene; tricyclic cycloolefins such as tricyclo[4.3.0.1 2,5 ]Decyl-3,7-diene (tricyclo[4.3.0.1 2,5 ]deca-3,7-diene)("dicyclopentadiene"), tricyclo[4.3.0.1 2,5 ]Deca-3-ene (tricyclo[4.3.0.1 2,5 ]dec-3-ene), tricyclic [4.4.0.1 2,5 ]Undec-3,7-diene (tricyclo[4.4.0.1 2,5 ]undeca-3,7-diene), or tricyclic [4.4.0.1 2,5 ] undec-3,8-diene, or a partially hydrogenated product thereof (or an adduct of cyclopentadiene and cyclohexene) tricyclic [4.4.0.1 2,5 ] undec-3-ene, 5-cyclopentyl-bicyclo[2.2.1]hept-2-ene, 5-cyclohexyl-bicyclo[2.2.1]hept-2-ene, 5-cyclohexenyl-bicyclo[2.2.1]hept-2-ene, and 5-phenyl-bicyclo[2.2.1]hept-2-ene; tetracyclic cycloalkenes such as tetracyclo[4.4.0.1 2,5 .1 7,10 ]Dodec-3-ene (tetracyclo[4.4.0.12,5 .1 7,10 ]dodec-3-ene)("tetracyclododecene"), 8-methyltetracyclo[4.4.0.1 2, 5 .1 7,10 ] dodec-3-ene, 8-ethyltetracyclo[4.4.0.1 2,5 .1 7,10 ]Dodec-3-ene, 8-methylenetetracyclo[4.4.0.1 2 ,5 .1 7,10 ] dodec-3-ene, 8-ethylenetetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, 8-vinyltetracyclo[4,4,0.1 2 ,5.1 7,10 ] dodec-3-ene, and 8-propenyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ] dodeca-3-ene; polycyclic cycloolefins, such as 8-cyclopentyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, 8-cyclohexyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, 8-cyclohexenyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, 8-phenyl-cyclopentyl-tetracyclo[4.4.0.1 2,5 .1 7,10 ] dodec-3-ene, tetracyclo[7.4.1 3,6。 0 1,9 .0. 2,7 ]tetradecane-4,9,11,13-tetraene ("1,4-methano-1,4,4a,9a-tetrahydrofluorene"), tetracyclo[8.4.1 4 ,7 .0. 1,10 .0. 3,8 ] pentadeca-5,10,12,14-tetraene ("1,4-methano-1,4,4a,5,10,10a-hexahydroanthracene"), pentacyclic [6.6.1.1 3,6 .0. 2,7 .0. 9,14 ]-4-hexadecene, pentacyclic [6.5.1.1. 3,6.0. 2,7 .0. 9,13 ]-4-pentadecene, pentacyclo[7.4.0.0. 2,7 .1. 3,6 .1. 10,13 ]-4-pentadecene, heptacyclo[8.7.0.1. 2,9 .1. 4,7 .1. 11,17 .0. 3,8 .0. 12,16 ]-5-eicosene, heptacyclic [8.7.0.1. 2 ,9 .0. 3,8 .1. 4,7 .0. 12,17 .1. 13,16 ]-14-eicosene; and tetramer of cyclopentadiene, etc.
[0013] Cycloolefin monomer can be unsubstituted or substituted with functional group.An embodiment of this functional group is alkyl, such as alkyl (for example, methyl, ethyl, n-propyl, isopropyl, n-butyl, 2-methylpropyl, n-heptyl, n-hexyl) modified with at least one halogen atom (for example, chlorine or fluorine).Suitable halogenated hydrocarbon group can include for example trifluoromethyl or trichloromethyl.Also cycloolefin monomer can be used alone to form homopolymer, or cycloolefin monomer (for example, two or more) is used in combination to form multipolymer.For example, cycloolefin polymer can be the multipolymer of cycloolefin monomer and one or more additional comonomers (such as, alpha-olefin comonomer, halogenated hydrocarbon comonomer etc.). Specific examples of suitable α-olefin comonomer monomers copolymerized with cycloolefin monomers can include, for example, α-olefins having 2 to 20 carbon atoms, and in some embodiments, α-olefins having 2 to 8 carbon atoms, such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, etc. These α-olefins can be used alone or in combination of two or more α-olefins. Ethylene may be particularly suitable for use as a comonomer in combination with cycloolefin monomers (e.g., norbornene or tetracyclododecene).
[0014] Any known technique known in the art can be used to produce cycloolefin polymers. For example, the polymer can be obtained by ring-opening the polymerized cycloolefin monomer using a metathesis polymerization catalyst containing a transition metal halide and an organometallic compound. The mixed solution can be obtained by hydrogenation by contacting with hydrogen in the presence of a hydrogenation catalyst. Alternatively, a well-known catalyst (such as a Ziegler-Natta catalyst) can be used to form the polymer.
[0015] To aid in its application, the barrier coating may be initially provided in a coating formulation comprising a hydrophobic resinous material (e.g., a cyclic olefin polymer) and an organic solvent, which is generally liquid at room temperature. When used, such solvents generally constitute from about 70 wt.% to about 99.9 wt.%, in some embodiments from about 80 wt.% to about 99.8 wt.%, and in some embodiments from about 90 wt.% to about 99.5 wt.%, of the formulation, while the hydrophobic resinous material may constitute from about 0.1 wt.% to about 30 wt.%, in some embodiments from about 0.2 wt.% to about 20 wt.%, and in some embodiments from about 0.5 wt.% to about 10 wt.% of the solution. The solvent employed depends in part on the nature of the resinous material, but generally includes organic alcohols, hydrocarbon solvents, fluorinated hydrocarbon solvents, and the like. For example, particularly suitable solvents for use with cycloolefin polymers can be hydrocarbon solvents, such as aromatic hydrocarbons (e.g., xylene, toluene, and ethylbenzene); cyclic hydrocarbons, such as alicyclic hydrocarbons (e.g., cyclohexane, cyclohexene, and methylcyclohexane); aliphatic hydrocarbons (e.g., hexane, heptane, octane, and decane); and the like, and combinations thereof. Alicyclic hydrocarbons are particularly suitable for coating formulations.
[0016] The coating formulation can be applied using various known techniques, such as by spin coating, impregnation, pouring, dropwise application, injection, spraying, blade application, brushing, printing (e.g., inkjet printing, screen printing, or pad printing), or dipping. In any case, upon application, the coating formulation can be dried, heated, and / or cured to remove any residual solvent and leave a coating of resinous material in the desired location.
[0017] By selectively controlling the specific properties of the barrier coating, the resulting capacitor can resist delamination during the manufacturing process and can therefore exhibit excellent electrical performance. For example, the capacitor can exhibit a dry capacitance of about 20 microfarads (μF) or greater, in some embodiments about 25 μF or greater, in some embodiments about 30 μF to about 100 μF, and in some embodiments about 40 μF to about 80 μF measured at a temperature of about 23°C and a frequency of 120 Hz. Notably, the capacitance value can remain stable even at high temperatures. For example, even if the capacitor is exposed to a "high temperature storage" test at a temperature of about 80°C or higher, in some embodiments, about 100°C to about 180°C, and in some embodiments, about 105°C to about 150°C (e.g., about 105°C, 125°C, or 150°C) for a considerable period of time (such as about 100 hours or more, and in some embodiments, about 150 hours to about 3,000 hours (e.g., 500, 1,000, 1,500, 2,000, 2,500, or 3,000 hours)), and then allowed to recover for about 1 to 2 hours, the capacitor can still exhibit an aged capacitance value within the above range at a temperature of about 23°C. For example, in one embodiment, after the capacitor is exposed to a high temperature storage test at a temperature of 150°C for 3,000 hours (with a recovery time of 1 to 2 hours), the capacitor can still exhibit an aged capacitance value within the above range (at 23°C). In this regard, the ratio of the aged capacitance at 23°C after undergoing the “high temperature storage test” to the initial capacitance at 23°C before the “high temperature storage test” can be about 0.6 to 1, in some embodiments, about 0.7 to 1, in some embodiments, about 0.8 to 1, and in some embodiments, about 0.9 to 1.
[0018] The capacitor can exhibit other good electrical properties. For example, the capacitor can exhibit a relatively low equivalent series resistance (equivalence series resistance, "ESR") measured at an operating frequency of 100kHz and a temperature of about 23°C, such as about 200 milliohms or less, in some embodiments about 150 milliohms or less, in some embodiments about 0.01 milliohms to about 100 milliohms, and in some embodiments about 0.1 milliohms to about 60 milliohms. Similar to the capacitance value, the aging ESR after the above-mentioned "high temperature storage" test can also remain stable and within the above range. For example, in one embodiment, the ratio of the aging ESR at 23°C after undergoing the "high temperature storage test" to the initial ESR at 23°C before the "high temperature storage test" can be about 10 or less, in some embodiments about 8 or less, in some embodiments about 5 or less, in some embodiments about 0.7 to 4, in some embodiments about 0.8 to 3, and in some embodiments 1 to about 2.
[0019] The capacitor may also exhibit a DCL of only about 50 microamperes ("μA") or less, in some embodiments about 40 μA or less, in some embodiments about 30 μA or less, in some embodiments about 20 μA or less, in some embodiments about 10 μA or less, in some embodiments about 9 μA or less, and in some embodiments about 0.01 μA to about 8 μA at a temperature of 23° C. after being subjected to an applied voltage (e.g., the rated voltage or a multiple of the rated voltage, such as 1.1X the rated voltage) for a period of about 60 seconds. Notably, the low DCL value remains stable even at high temperatures. For example, the capacitor can exhibit a low DCL within the above range after being exposed to an elevated temperature (such as about 80°C to about 150°C (e.g., about 85°C)) for a substantial period of time (such as about 100 hours or longer, and in some embodiments, about 120 hours to about 1,500 hours (e.g., 120, 250, 500, 1,000, or 1,500 hours)) and then allowed to recover for 1 to 2 hours. For example, in one embodiment, after being tested at a temperature of 85°C for 1,500 hours (with a recovery time of 1 to 2 hours), the capacitor can exhibit an aged DCL value (at 23°C) within the above range. In this regard, the ratio of the aged DCL at 23°C after undergoing the "high temperature test" to the initial DCL at 23°C before the "high temperature test" can be about 10 or less, in some embodiments, about 5 or less, in some embodiments, about 2 or less, in some embodiments, about 1 or less, in some embodiments, from about 0.05 to about 0.8, and in some embodiments, from about 0.1 to about 0.5.
[0020] The DCL may also remain stable after exposure to the "High Humidity Test" for a considerable period of time at high relative humidity levels (without or without the above-mentioned elevated temperatures) as described above, such as about 40% or more, in some embodiments about 45% or more, in some embodiments about 50% or more, and in some embodiments about 70% or more (e.g., about 85% to 100%). For example, relative humidity may be determined according to ASTM E337-02, Method A (2007). For example, after being exposed to a humidity level of 85% and a temperature of 85°C for a substantial period of time (such as about 100 hours or more, and in some embodiments, about 120 hours to about 1,500 hours (e.g., 120, 250, 500, 1,000, or 1,500 hours), and then allowed to recover for about 1 to 2 hours, the capacitor can exhibit an aged DCL value (at 23°C) within the above range. For example, the ratio of the aged DCL (23°C) of the capacitor after exposure to high humidity levels (e.g., about 85%) and high temperatures (e.g., about 85°C) for 1,500 hours (with a recovery time of 1 to 2 hours) to the initial DCL prior to such testing can be about 10 or less, in some embodiments, about 5 or less, in some embodiments, about 2 or less, in some embodiments, about 1 or less, in some embodiments, about 0.05 about 0.8 to about 0.8, and in some embodiments, about 0.1 to about 0.5.
[0021] Various embodiments of the capacitor will now be described in more detail.
[0022] I. Capacitor Components
[0023] A. Anode
[0024] The capacitor element includes an anode containing a dielectric formed on a sintered porous body. The porous anode body can be formed from a powder containing a valve metal (i.e., a metal that can be oxidized) or a valve metal compound (such as tantalum, niobium, aluminum, hafnium, titanium, their alloys, their oxides, their nitrides, etc.). The powder is typically formed by a reduction process in which a tantalum salt (e.g., potassium fluorotantalate (K 2 Tf 7 ), sodium fluorotantalate (Na 2 Tf 7 ), tantalum pentachloride (TaCl 5) etc.) with a reducing agent. The reducing agent may be provided in the form of a liquid, a gas (e.g., hydrogen), or a solid (such as a metal (e.g., sodium), a metal alloy, or a metal salt). In one embodiment, for example, a tantalum salt (e.g., TaCl) may be heated at a temperature of about 900° C. to about 2,000° C., in some embodiments, about 1,000° C. to about 1,800° C., and in some embodiments, about 1,100° C. to about 1,600° C. 5 ) to form a vapor that can be reduced in the presence of a gaseous reducing agent (e.g., hydrogen). Additional details of such a reduction reaction can be described in WO2014 / 199480 by Maeshima et al. After reduction, the product can be cooled, crushed and washed to form a powder.
[0025] The specific charge of the powder generally varies from about 2,000 to about 600,000 microfarads*volts / gram ("μF*V / g"), depending on the desired application. For example, in certain embodiments, a high charge powder may be employed having a specific charge of about 100,000 μF*V / g to about 550,000 μF*V / g, in some embodiments about 120,000 μF*V / g to about 500,000 μF*V / g, and in some embodiments about 150,000 μF*V / g to about 400,000 μF*V / g. In other embodiments, a low charge powder may be employed having a specific charge of about 2,000 μF*V / g to about 100,000 μF*V / g, in some embodiments about 5,000 μF*V / g to about 80,000 μF*V / g, and in some embodiments about 10,000 μF*V / g to about 70,000 μF*V / g. As is known in the art, the specific charge can be determined by multiplying the capacitance by the anode voltage employed and then dividing the product by the weight of the anodized electrode body.
[0026] The powder may be a free-flowing, finely divided powder containing primary particles. The median size (D 50) is typically from about 5 nanometers to about 500 nanometers, in some embodiments, from about 10 nanometers to about 400 nanometers, and in some embodiments, from about 20 nanometers to about 250 nanometers, such as measured using a laser particle size distribution analyzer (e.g., LS-230) manufactured by BECKMAN COULTER, optionally after subjecting the particles to 70 seconds of ultrasonic vibration. The primary particles typically have a three-dimensional granular shape (e.g., nodular or angular). Such particles typically have a relatively low "aspect ratio", which is the average diameter or width of the particles divided by the average thickness ("D / T") . For example, the aspect ratio of the particles can be about 4 or less, in some embodiments, about 3 or less, and in some embodiments, from about 1 to about 2. In addition to primary particles, the powder may also contain other types of particles, such as secondary particles formed by aggregating (or agglomerating) primary particles. The median size (D / T) of such secondary particles is about 1.5 to about 2. 50 ) can be from about 1 micron to about 500 microns, and in some embodiments, from about 10 microns to about 250 microns.
[0027] Agglomeration of the particles can occur by heating the particles and / or by using a binder. For example, agglomeration can occur at a temperature of about 0°C to about 40°C, in some embodiments about 5°C to about 35°C, and in some embodiments about 15°C to about 30°C. Suitable binders may likewise include, for example, poly(vinyl butyral); poly(vinyl acetate); poly(vinyl alcohol); poly(vinyl pyrrolidone); cellulosic polymers such as carboxymethyl cellulose, methyl cellulose, ethyl cellulose, hydroxyethyl cellulose and methyl hydroxyethyl cellulose; random polypropylene, polyethylene; polyethylene glycol (e.g., Carbowax from Dow Chemical Co.); polystyrene, poly(butadiene / styrene); polyamides, polyimides and polyacrylamides, high molecular weight polyethers; copolymers of ethylene oxide and propylene oxide; fluoropolymers such as polytetrafluoroethylene, polyvinylidene fluoride and fluoroolefin copolymers; acrylic polymers such as sodium polyacrylate, poly(lower alkyl acrylates), poly(lower alkyl methacrylates) and copolymers of lower alkyl acrylates and methacrylates; and fatty acids and waxes such as stearic acid and other soapy fatty acids, vegetable waxes, microcrystalline waxes (purified paraffin waxes), and the like.
[0028] The resulting powder can be compacted to form pellets using any conventional powder compacting equipment. For example, a press mold can be used, which is a single-station compaction press containing a die and one or more punches. Alternatively, an anvil-type compaction press mold using only a die and a single lower punch can be used. The single-station compaction press mold can use several basic types with multiple functions (such as single-action, double-action, floating die, movable platen, opposed ram, screw, impact, hot pressing, stamping or sizing), such as cam, toggle / knuckle and eccentric / crank presses. The powder can be compacted around an anode lead, which can be in the form of a wire, sheet, etc. The lead can extend longitudinally from the anode body and can be formed of any conductive material (e.g., tantalum, niobium, aluminum, hafnium, titanium, etc., and their conductive oxides and / or nitrides). Connection of the lead wire may also be accomplished using other known techniques, such as by welding the lead wire to the anode body, or embedding the lead wire within the anode body during the formation process (eg, prior to compaction and / or sintering).
[0029] After pressing, the pellets can be heated for several minutes under vacuum at certain temperatures (e.g., about 150°C to about 500°C) to remove any binder. Alternatively, the binder can also be removed by contacting the pellets with an aqueous solution, such as described in U.S. Patent No. 6,197,252 by Bishop et al. Afterwards, the pellets are sintered to form a porous integral mass. The pellets are typically sintered at a temperature of about 700°C to about 1800°C, about 800°C to about 1700°C in some embodiments, and about 900°C to about 1400°C for about 5 minutes to about 100 minutes, and about 8 minutes to about 15 minutes in some embodiments. This can be carried out in one or more steps. If desired, sintering can be carried out in an atmosphere that limits the transfer of oxygen atoms to the anode. For example, sintering can be carried out in a reducing atmosphere, such as in a vacuum, an inert gas, hydrogen, etc. The pressure of the reducing atmosphere may be from about 10 Torr to about 2000 Torr, in some embodiments from about 100 Torr to about 1000 Torr, and in some embodiments from about 100 Torr to about 930 Torr. Mixtures of hydrogen and other gases (eg, argon or nitrogen) may also be employed.
[0030] B. Dielectric
[0031] The anode is also coated with a dielectric. The dielectric is formed by anodic oxidation ("anodization") through a sintered anode so that a dielectric layer is formed above the anode and / or in the anode. For example, a tantalum (Ta) anode can be anodized to tantalum pentoxide (Ta2O5). Typically, anodization is implemented by initially applying a solution to the anode, such as by dipping the anode into an electrolyte. Typically a solvent, such as water (e.g., deionized water) is used. In order to enhance ionic conductivity, a compound that can dissociate in a solvent to form ions is typically used. Examples of these compounds include, for example, acids, such as the acids described below about electrolytes. For example, an acid (e.g., phosphoric acid) can constitute about 0.01wt.% to about 5wt.% of anodizing solution, about 0.05wt.% to about 0.8wt.% in some embodiments, and about 0.1wt.% to about 0.5wt.% in some embodiments. If desired, a mixture of acids can also be used.
[0032] The current is passed through the anodizing solution to form a dielectric layer. The value of the formation voltage controls the thickness of the dielectric layer. For example, the power supply can be initially set to a constant current mode until the desired voltage is reached. Afterwards, the power supply can be switched to a constant potential mode to ensure that the desired dielectric thickness is formed over the entire surface of the anode. Of course, other known methods, such as a pulsed constant potential method or a step-by-step constant potential method, can also be used. The voltage range for anodization is generally about 4V to about 250V, and in some embodiments about 5V to about 200V, and in some embodiments about 10V to about 150V. During the oxidation process, the anodizing solution can be maintained at an elevated temperature, such as about 30°C or higher, in some embodiments about 40°C to about 200°C, and in some embodiments about 50°C to about 100°C. Anodization can also be performed at ambient temperature or a lower temperature. The resulting dielectric layer can be formed on the surface of the anode and in the pores of the anode.
[0033] Although not necessary, in certain embodiments, the dielectric layer can have different thicknesses over the entire anode, because the dielectric layer has a first portion covering the outer surface of the anode and a second portion covering the inner surface of the anode. In such an embodiment, the first portion is selectively formed so that the thickness of the first portion is greater than the thickness of the second portion. However, it should be understood that the thickness of the dielectric layer in a specific area does not need to be uniform. For example, some portions of the dielectric layer adjacent to the outer surface can actually be thinner than some portions of the layer at the inner surface, and vice versa. Nevertheless, the dielectric layer can be formed so that at least a portion of the layer at the outer surface has a greater thickness than at least a portion at the inner surface. Although the exact difference in these thicknesses can vary depending on the specific application, the ratio of the thickness of the first portion to the thickness of the second portion is generally about 1.2 to about 40, about 1.5 to about 25 in some embodiments, and about 2 to about 20 in some embodiments.
[0034] In order to form a dielectric layer with different thicknesses, a multi-stage process is generally used. In each stage of the process, the sintered anode is anodized ("anodized") to form a dielectric layer (e.g., tantalum pentoxide). During the first stage of anodization, a relatively small formation voltage is generally used to ensure that the desired dielectric thickness for the inner region is obtained, such as a formation voltage ranging from about 1 volt to about 90 volts, in some embodiments, about 2 volts to about 50 volts, and in some embodiments, about 5 volts to about 20 volts. Afterwards, the sintered body can be anodized in the second stage of the process to increase the thickness of the dielectric to a desired level. This is generally achieved by anodizing in an electrolyte at a voltage higher than the voltage used during the first stage, such as a formation voltage ranging from about 50 volts to about 350 volts, in some embodiments, about 60 volts to about 300 volts, and in some embodiments, about 70 volts to about 200 volts. During the first stage and / or the second stage, the electrolyte may be maintained at a temperature ranging from about 15°C to about 95°C, in some embodiments, from about 20°C to about 90°C, and in some embodiments, from about 25°C to about 85°C.
[0035] The electrolyte used during the first and second stages of the anodizing process may be the same or different. However, in general, it is desirable to use different solutions to help better facilitate obtaining a greater thickness at the outer portion of the dielectric layer. For example, it may be desirable that the electrolyte used in the second stage has a lower ionic conductivity than the electrolyte used in the first stage to prevent the formation of a large amount of oxide film on the inner surface of the anode. In this regard, the electrolyte used during the first stage may contain an acidic compound such as nitric acid, sulfuric acid, phosphoric acid, polyphosphoric acid, boric acid, boric acid, etc. Such an electrolyte may have a conductivity of about 0.1 mS / cm to about 100 mS / cm measured at a temperature of 25°C, about 0.2 mS / cm to about 20 mS / cm in some embodiments, and about 1 mS / cm to about 10 mS / cm in some embodiments. The electrolyte used during the second stage generally contains a salt of a weak acid so that the concentration of hydronium ions in the pores increases due to the charge passage in the pores. Ion transport or diffusion allows weak acid anions to move into the pores when necessary to balance the charge. As a result, when equilibrium is established between hydronium ions, acid anions and undissociated acid, the concentration of the main conductive species (hydronium ions) is reduced, thus forming a poorly conductive species. The reduction in the concentration of the conductive species results in a relatively high voltage drop in the electrolyte, which hinders further anodization of the interior, and in areas of sustained high conductivity, a thicker oxide layer is deposited on the exterior to achieve a higher formation voltage. Suitable weak acid salts may include, for example, ammonium or alkali metal salts (e.g., sodium, potassium, etc.) of boric acid, borous acid, acetic acid, oxalic acid, lactic acid, adipic acid, etc. Particularly suitable salts include sodium tetraborate and ammonium pentaborate. Such electrolytes typically have a conductivity of about 0.1 mS / cm to about 20 mS / cm measured at a temperature of 25 ° C, in some embodiments about 0.5 mS / cm to about 10 mS / cm, and in some embodiments about 1 mS / cm to about 5 mS / cm.
[0036] If desired, each stage of anodization can be repeated for one or more cycles to obtain the desired dielectric thickness. In addition, after the first stage and / or the second stage, the anode can also be cleaned or washed with another solvent (eg, water) to remove the electrolyte.
[0037] C. Solid Electrolyte
[0038] The solid electrolyte is coated on the dielectric and is generally used as the cathode of the capacitor. The solid electrolyte may include materials such as conductive polymers (e.g., polypyrrole, polythiophene, polyaniline, etc.), manganese dioxide, etc., as known in the art. For example, in one embodiment, the solid electrolyte comprises one or more layers containing non-intrinsic electrical polymer particles and / or intrinsic conductive polymer particles. One benefit of using such particles is that they can make ionic species (e.g., Fe, Fe, etc.) generated during conventional in situ polymerization processes 2+ or Fe 3+ ) is minimized, and the ionic species can cause dielectric breakdown under high voltage electric fields due to ion migration. Therefore, by applying the conductive polymer as pre-polymerized particles rather than by in-situ polymerization, the resulting capacitor can exhibit a relatively high "breakdown voltage". If desired, the solid electrolyte can be formed by one or more layers. When multiple layers are used, one or more of the layers may include a conductive polymer formed by in-situ polymerization. However, when it is desired to achieve a very high breakdown voltage, the solid electrolyte can be desirably formed primarily by the above-mentioned conductive particles, so that the solid electrolyte is generally free of conductive polymers formed by in-situ polymerization. Regardless of how many layers are used, the resulting solid electrolyte generally has a total thickness of about 1 micrometer (μm) to about 200 μm, in some embodiments about 2 μm to about 50 μm, and in some embodiments about 5 μm to about 30 μm.
[0039] Thiophene polymers are particularly suitable for use in solid electrolytes. For example, in certain embodiments, a "non-intrinsic" conductive thiophene polymer may be used in a solid electrolyte, wherein the "non-intrinsic" conductive thiophene polymer has a repeating unit of the following formula (I):
[0040]
[0041] in,
[0042] R 7 Straight chain or branched C 1 To C 18 Alkyl groups (e.g., methyl, ethyl, n-propyl or isopropyl, n-butyl, isobutyl, sec-butyl or tert-butyl, n-pentyl, 1-methylbutyl, 2-methylbutyl, 3-methylbutyl, 1-ethylpropyl, 1,1-dimethylpropyl, 1,2-dimethylpropyl, 2,2-dimethylpropyl, n-hexyl, n-heptyl, n-octyl, 2-ethylhexyl, n-nonyl, n-decyl, n-undecyl, n-dodecyl, n-tridecyl, n-tetradecyl, n-hexadecyl, n-octadecyl, etc.); C 5 To C 12 Cycloalkyl groups (e.g., cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, cyclononyl, cyclodecyl, etc.); C6 To C 14 Aryl group (eg, phenyl, naphthyl, etc.); C 7 To C 18 an aralkyl group (e.g., benzyl, o-tolyl, m-tolyl, p-tolyl, 2,3-xylyl, 2,4-xylyl, 2,5-xylyl, 2-6-xylyl, 3-4-xylyl, 3,5-xylyl, mesityl, etc.); and
[0043] q is an integer from 0 to 8, in some embodiments from 0 to 2, and in one embodiment is 0. In a specific embodiment, "q" is 0 and the polymer is poly(3,4-ethylenedioxythiophene). A commercially available example of a monomer suitable for forming such a polymer is 3,4-ethylenedioxythiophene, which can be purchased from Heraeus as Clevios TM M (trade name).
[0044] The polymers of formula (I) are generally considered to be "non-intrinsically" conductive, and the degree of conductivity generally requires the presence of a separate counterion that is not covalently bound to the polymer. The counterion can be a monomeric anion or a polymeric anion that offsets the charge of the conductive polymer. The polymeric anion can be, for example, an anion of a polymeric carboxylic acid (e.g., polyacrylic acid, polymethacrylic acid, polymaleic acid, etc.); a polymeric sulfonic acid (e.g., polystyrene sulfonic acid ("polystyrene sulfonic acid, PSS"), polyvinyl sulfonic acid, etc.); and the like. The acid can also be a copolymer, such as a copolymer of vinyl carboxylic acid and vinyl sulfonic acid, with other polymerizable monomers (such as acrylates and styrene). Likewise, suitable monomeric anions include, for example, anions of: C 1 To C 20 Alkane sulfonic acid (e.g., dodecane sulfonic acid); aliphatic perfluorosulfonic acid (e.g., trifluoromethane sulfonic acid, perfluorobutane sulfonic acid, or perfluorooctane sulfonic acid); aliphatic C 1 To C 20 carboxylic acid (e.g., 2-ethyl-hexyl carboxylic acid); aliphatic perfluorocarboxylic acid (e.g., trifluoroacetic acid or perfluorooctanoic acid); optionally C 1 To C 20Alkyl substituted aromatic sulfonic acids (e.g., benzenesulfonic acid, o-toluenesulfonic acid, p-toluenesulfonic acid, or dodecylbenzenesulfonic acid); cycloalkanesulfonic acids (e.g., camphorsulfonic acid or tetrafluoroborate, hexafluorophosphate, perchlorate, hexafluoroantimonate, hexafluoroarsenate, or hexachloroantimonate); and the like. Particularly suitable counter anions are polymeric anions, such as polymeric carboxylic acids or sulfonic acids (e.g., polystyrenesulfonic acid ("PSS")). The molecular weight of such polymeric anions is typically in the range of about 1,000 to about 2,000,000, and in some embodiments, from about 2,000 to about 500,000.
[0045] Intrinsically conductive polymers may also be used, which have positive charges located on the backbone that are at least partially offset by anions covalently bonded to the polymer. For example, one embodiment of a suitable intrinsically conductive thiophene polymer may have repeating units of the following formula (II):
[0046]
[0047] in,
[0048] R is (CH 2 ) a -O-(CH 2 ) b -L, where L is a bond or HC([CH 2 ] C H);
[0049] a is 0 to 10, in some embodiments 0 to 6, and in some embodiments 1 to 4 (e.g., 1);
[0050] b is 1 to 18, in some embodiments 1 to 10, and in some embodiments 2 to 6 (e.g., 2, 3, 4, or 5);
[0051] c is 0 to 10, in some embodiments 0 to 6, and in some embodiments 1 to 4 (e.g., 1);
[0052] Z is an anion, such as SO 3 - 、C(O)O - , BF 4 - CF 3 SO 3 - , SbF 6 - 、N(SO 2 CF 3 ) 2 - , C 4 H3 O 4 - , ClO 4 - ,etc;
[0053] X is a cation such as hydrogen, an alkali metal (eg, lithium, sodium, rubidium, cesium, or potassium), ammonium, or the like.
[0054] In a specific embodiment, Z in formula (II) is a sulfonate ion, so that the intrinsically conductive polymer comprises a repeating unit of the following formula (III):
[0055]
[0056] wherein R and X are as defined above. In formula (II) or (III), a is preferably 1 and b is preferably 3 or 4. Likewise, X is preferably sodium or potassium.
[0057] If desired, the polymer can be a copolymer comprising other types of repeating units. In such embodiments, the repeating unit of formula (II) generally constitutes about 50 mol.% or higher of the total amount of repeating units in the copolymer, in some embodiments about 75 mol.% to about 99 mol.%, and in some embodiments about 85 mol.% to about 95 mol.%. Of course, the polymer can also be a homopolymer comprising 100 mol.% of the repeating unit of formula (II). Specific examples of such homopolymers include poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-ylmethoxy)-1-butane-sulfonic acid salt) and poly(4-(2,3-dihydrothieno[3,4-b][1,4]dioxin-2-ylmethoxy)-1-butane-sulfonic acid salt).
[0058] Regardless of the specific properties of the polymer, the resulting conductive polymer particles typically have an average size (e.g., diameter) of about 1 nanometer to about 80 nanometers, in some embodiments about 2 nanometers to about 70 nanometers, and in some embodiments about 3 nanometers to about 60 nanometers. The diameter of the particles can be determined using known techniques, such as by ultracentrifugation, laser diffraction, etc. The shape of the particles can also vary. For example, in a specific embodiment, the particles are spherical. However, it should be understood that the present invention also contemplates other shapes, such as plates, rods, disks, rods, tubes, irregular shapes, etc.
[0059] Although not required, the conductive polymer particles can be applied in the form of a dispersion. The concentration of the conductive polymer in the dispersion can vary according to the desired dispersion viscosity and the specific manner in which the dispersion is applied to the capacitor element. However, generally, the polymer constitutes about 0.1 to about 10wt.%, in some embodiments about 0.4 to about 5wt.%, and in some embodiments about 0.5 to about 4wt.%. The dispersion can also include one or more components to enhance the overall performance of the resulting solid electrolyte. For example, the dispersion can include an adhesive to further enhance the adhesive properties of the polymer layer and also increase the stability of the particles in the dispersion. The binder can be of organic nature, such as polyvinyl alcohol, polyvinyl pyrrolidone, polyvinyl chloride, polyvinyl acetate, polyvinyl butyrate, polyacrylate, polyacrylamide, polymethacrylate, polymethacrylamide, polyacrylonitrile, styrene / acrylate, vinyl acetate / acrylate and ethylene / vinyl acetate copolymers, polybutadiene, polyisoprene, polystyrene, polyether, polyester, polycarbonate, polyurethane, polyamide, polyimide, polysulfone, melamine formaldehyde resin, epoxy resin, silicone resin or cellulose. Crosslinking agents can also be used to enhance the adhesion of the binder. Such crosslinking agents can include, for example, melamine compounds, blocked (masked) isocyanates or crosslinking polymers (such as polyurethane, polyacrylate or polyolefin), and subsequent crosslinking. Dispersants can also be used to promote the ability of the layer to be applied to the anode. Suitable dispersants include solvents such as aliphatic alcohols (e.g., methanol, ethanol, isopropanol, and butanol), aliphatic ketones (e.g., acetone and methyl ethyl ketone), aliphatic carboxylates (e.g., ethyl acetate and butyl acetate), aromatic hydrocarbons (e.g., toluene and xylene), aliphatic hydrocarbons (e.g., hexane, heptane, and cyclohexane), chlorinated hydrocarbons (e.g., methylene chloride and ethylene dichloride), aliphatic nitriles (e.g., acetonitrile), aliphatic sulfoxides and sulfones (e.g., dimethyl sulfoxide and sulfolane), aliphatic carboxylic acid amides (e.g., methylacetamide, dimethylacetamide, and dimethylformamide), aliphatic and araliphatic ethers (e.g., diethyl ether and anisole), water, and mixtures of any of the foregoing solvents. A particularly suitable dispersant is water.
[0060] In addition to those mentioned above, other ingredients can also be used in the dispersion. For example, conventional fillers can be used, the size of which is from about 10 nanometers to about 100 microns, from about 50 nanometers to about 50 microns in some embodiments and from about 100 nanometers to about 30 microns in some embodiments. Examples of such fillers include calcium carbonate, silicates, silicon oxide, calcium sulfate or barium sulfate, aluminum hydroxide, glass fibers or glass bulbs, wood powder, cellulose powder carbon black, conductive polymers, etc. The filler can be introduced into the dispersion in powder form, but can also exist in other forms (such as fibers).
[0061] Surface active substances such as ionic or nonionic surfactants may also be used in the dispersion. In addition, adhesives such as organofunctional silanes or their hydrolysis products, such as 3-glycidoxypropyltrialkoxysilane, 3-aminopropyl-triethoxysilane, 3-mercaptopropyl-trimethoxysilane, 3-methacryloxypropyltrimethoxysilane, vinyltrimethoxysilane or octyltriethoxysilane may be used. The dispersion may also contain additives to increase conductivity, such as compounds containing ether groups (e.g., tetrahydrofuran), compounds containing lactone groups (e.g., γ-butyrolactone or γ-valerolactone), compounds containing amide groups or lactam groups (e.g., caprolactam, N-methylcaprolactam, N,N-dimethylacetamide, N-methylacetamide, N,N-dimethylformamide (DMF), N-methylformamide, N-methylformanilide, N-methylpyrrolidone (N -methylpyrrolidone, NMP), N-octylpyrrolidone or pyrrolidone), sulfones and sulfoxides (e.g., sulfolane (tetramethylene sulfone) or dimethylsulfoxide (DMSO)), sugars or sugar derivatives (e.g., sucrose, glucose, fructose or lactose), sugar alcohols (e.g., sorbitol or mannitol), furan derivatives (e.g., 2-furancarboxylic acid or 3-furancarboxylic acid), alcohols (e.g., ethylene glycol, glycerol, diethylene glycol or triethylene glycol).
[0062] The dispersion can be applied using various known techniques, for example by spin coating, dipping, pouring, dropwise application, injection, spraying, doctor blade coating, brushing, printing (e.g., inkjet printing, screen printing or pad printing) or immersion. The viscosity of the dispersion is generally from about 0.1 mPas to about 100,000 mPas (at 100 s -1 ), in some embodiments, from about 1 mPas to about 10,000 mPas, in some embodiments, from about 10 mPas to about 1,500 mPas, and in some embodiments, from about 100 mPas to about 1000 mPas.
[0063] i. Inner Layer
[0064] Solid electrolytes are generally formed by one or more "inner" conductive polymer layers. In this article, the term "inner" refers to one or more layers coated on the dielectric, whether directly or via another layer (e.g., pre-coating). One or more inner layers can be used. For example, the solid electrolyte generally comprises 2 to 30 inner layers, in some embodiments 4 to 20 inner layers, and in some embodiments about 5 to 15 inner layers (e.g., 10 layers). For example, the inner layer may include intrinsic polymer particles and / or non-intrinsic polymer particles as described above. For example, such particles may constitute about 50wt.% or more of the inner layer, about 70wt.% or more in some embodiments, and about 90wt.% or more (e.g., 100wt.%) in some embodiments. In alternative embodiments, the inner layer may include an in-situ polymerized conductive polymer. In such an embodiment, such an in-situ polymerized polymer may constitute about 50wt.% or more of the inner layer, about 70wt.% or more in some embodiments, and about 90wt.% or more (e.g., 100wt.%) in some embodiments.
[0065] i. Outer Layer
[0066] The solid electrolyte may also include one or more optional "outer" conductive polymer layers that are coated on top of the inner layer and are formed of different materials. For example, the outer layer may include non-intrinsic conductive polymer particles. In a specific embodiment, the outer layer is mainly formed by such non-intrinsic conductive polymer particles, because the non-intrinsic conductive polymer particles constitute about 50wt.% or more of each outer layer, about 70wt.% or more in some embodiments, and about 90wt.% or more (e.g., 100wt.%). One or more outer layers may be used. For example, the solid electrolyte may include 2 to 30 outer layers, 4 to 20 outer layers in some embodiments, and about 5 to 15 outer layers in some embodiments, each outer layer may be optionally formed by a dispersion of non-intrinsic conductive polymer particles.
[0067] D. External polymer coating
[0068] The external polymer coating can also be coated on the solid electrolyte. The external polymer coating can include one or more layers formed by prepolymerized conductive polymer particles (e.g., dispersions of non-intrinsic conductive polymer particles) as described above. The external coating may be able to further penetrate into the edge region of the capacitor body to increase the adhesion to the dielectric and produce a more mechanically stable (robust) component, which can reduce equivalent series resistance and leakage current. Because it is generally intended to improve the edge coverage rather than to immerse the inside of the anode body, the particles used in the external coating generally have a larger size than the particles used in the solid electrolyte. For example, the average size of the particles used in the external polymer coating is generally about 1.5 to about 30, about 2 to about 20 in some embodiments, and about 5 to about 15 in some embodiments. For example, the average size of the particles used in the dispersion of the external coating can be about 80 nanometers to about 500 nanometers, about 90 nanometers to about 250 nanometers in some embodiments, and about 100 nanometers to about 200 nanometers in some embodiments.
[0069] If desired, a crosslinking agent may also be employed in the outer polymer coating to improve adhesion to the solid electrolyte. Typically, the crosslinking agent is applied prior to application of the dispersion used in the outer coating. Suitable crosslinking agents are described, for example, in Merker et al. and include, for example, amines (e.g., diamines, triamines, oligoamines, polyamines, etc.); polyvalent metal cations, such as salts or compounds of Mg, Al, Ca, Fe, Cr, Mn, Ba, Ti, Co, Ni, Cu, Ru, Ce, or Zn, phosphonium compounds, sulfonium compounds, etc. Particularly suitable examples include, for example, 1,4-diaminocyclohexane, 1,4-bis(amino-methyl)cyclohexane, ethylenediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,12-dodecanediamine, N,N-dimethylethylenediamine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethyl-1,4-butanediamine, etc., and mixtures thereof.
[0070] The crosslinking agent is typically applied by a solution or dispersion having a pH of 1 to 10, in some embodiments 2 to 7, and in some embodiments 3 to 6, measured at 25°C. Acidic compounds may be used to help achieve the desired pH level. Examples of solvents or dispersants for the crosslinking agent include water or organic solvents, such as alcohols, ketones, carboxylates, and the like. The crosslinking agent may be applied to the capacitor body by any known process, such as spin coating, dipping, pouring, dropwise application, spray application, vapor deposition, sputtering, sublimation, scraping, painting, or printing (e.g., inkjet printing, screen printing, or pad printing). When applied, the crosslinking agent may be dried before applying the polymer dispersion. The process may then be repeated until the desired thickness is obtained. For example, the total thickness of the entire outer polymer coating (including the crosslinking agent and the dispersion layer) may be from about 1 μm to about 50 μm, from about 2 μm to about 40 μm in some embodiments, and from about 5 μm to about 20 μm in some embodiments.
[0071] E. Cathodic coating
[0072] If desired, the capacitor element may also employ a cathode coating and other optional layers (e.g., an outer polymer coating) overlying the solid electrolyte. The cathode coating may contain a metal particle layer comprising a plurality of conductive metal particles dispersed in a polymer matrix. The particles typically constitute about 50 wt.% to about 99 wt.%, in some embodiments about 60 wt.% to about 98 wt.%, and in some embodiments about 70 wt.% to about 95 wt.%, of the layer, while the polymer matrix typically constitutes about 1 wt.% to about 50 wt.%, in some embodiments about 2 wt.% to about 40 wt.%, and in some embodiments about 5 wt.% to about 30 wt.%.
[0073] Conductive metal particles can be formed from a variety of different metals (e.g., copper, nickel, silver, nickel, zinc, tin, lead, copper, aluminum, molybdenum, titanium, iron, zirconium, magnesium, etc., and their alloys). Silver is a particularly suitable conductive metal for this layer. The metal particles are generally of relatively small size, such as an average size of about 0.01 micron to about 50 microns, in some embodiments about 0.1 micron to about 40 microns, and in some embodiments about 1 micron to about 30 microns. Typically, only one metal particle layer is used, but it should be understood that multiple layers can be used if desired. The total thickness of such a layer is generally in the range of about 1 μm to about 500 μm, in some embodiments about 5 μm to about 200 μm, and in some embodiments about 10 μm to about 100 μm.
[0074] The polymer matrix generally includes a polymer, which can be a thermoplastic or thermosetting property. However, generally, the polymer is selected so that the polymer can be used as a barrier for the electromigration of silver ions, and the polymer is also made to contain a relatively small amount of polar groups to minimize the water adsorption degree in the cathode coating. In this regard, the inventors have found that vinyl acetal polymers (such as polyvinyl butyral, polyvinyl formal, etc.) are particularly suitable for this purpose. For example, polyvinyl butyral can be formed by reacting polyvinyl alcohol with an aldehyde (for example, butyraldehyde). Because this reaction is generally incomplete, polyvinyl butyral generally has a residual hydroxyl content. However, by minimizing this content, the polymer can have a small degree of strong polar groups, which can cause a high degree of moisture adsorption and cause silver ion migration. For example, the residual hydroxyl content in the polyvinyl acetal can be about 35mol.% or less, about 30mol.% or less in some embodiments, and about 10mol.% to about 25mol.% in some embodiments. One commercially available example of such a polymer is available from Sekisui Chemical Co., Ltd as "BH-S" (polyvinyl butyral, trade name).
[0075] To form the cathode coating, a conductive slurry is typically applied to the capacitor overlying the solid electrolyte. One or more organic solvents are typically employed in the slurry. Generally, various organic solvents can be used, such as glycols (e.g., propylene glycol, butylene glycol, triethylene glycol, hexylene glycol, polyethylene glycol, ethoxydiethylene glycol and dipropylene glycol), glycol ethers (e.g., methyl glycol ether, ethyl glycol ether and isopropyl glycol ether), ethers (e.g., diethyl ether and tetrahydrofuran), alcohols (e.g., benzyl alcohol, methanol, ethanol, n-propanol, isopropanol and butanol), triglycerides, ketones (e.g., acetone, methyl ethyl ketone and methyl isobutyl ketone), esters (e.g., ethyl acetate, butyl acetate, diethylene glycol ether acetate and methoxypropyl acetate); amides (e.g., dimethylformamide, dimethylacetamide, dimethyl octanyl / decyl fatty acid amide and N-alkylpyrrolidone), nitriles (e.g., acetonitrile, propionitrile, butyronitrile and benzonitrile); sulfoxides or sulfones (e.g., dimethyl sulfoxide (DMSO) and sulfolane), etc., and mixtures thereof. The organic solvent typically constitutes about 10 wt.% to about 70 wt.% of the slurry, in some embodiments, about 20 wt.% to about 65 wt.%, and in some embodiments, about 30 wt.% to about 60 wt.%. Typically, the metal particles constitute about 10 wt.% to about 60 wt.% of the slurry, in some embodiments, about 20 wt.% to about 45 wt.%, and in some embodiments, about 25 wt.% to about 40 wt.%, and the resinous matrix constitutes about 0.1 wt.% to about 20 wt.%, in some embodiments, about 0.2 wt.% to about 10 wt.%, and in some embodiments, about 0.5 wt.% to about 8 wt.%.
[0076] The slurry can have a relatively low viscosity, making it easy to handle and apply to capacitor elements. For example, the viscosity can be from about 50 centipoise to about 3,000 centipoise, from about 100 to about 2,000 centipoise in some embodiments, and from about 200 to about 1,000 centipoise in some embodiments, such as measured by operating a Brookfield Dv-1 viscometer (cone and plate) at a speed of 10 rpm and a temperature of 25°C. If desired, a thickener or other viscosity modifier can be used in the slurry to increase or reduce the viscosity. In addition, the thickness of the applied slurry can also be relatively thin and still achieve the desired properties. For example, the thickness of the slurry can be from about 0.01 microns to about 50 microns, from about 0.5 microns to about 30 microns in some embodiments, and from about 1 micron to about 25 microns in some embodiments. When applied, the metal slurry can be optionally dried to remove certain components, such as organic solvents. For example, drying may occur at a temperature of from about 20°C to about 150°C, in some embodiments, from about 50°C to about 140°C, and in some embodiments, from about 80°C to about 130°C.
[0077] F. Other Components
[0078] If desired, the capacitor may also include other layers known in the art. In certain embodiments, for example, a carbon layer (e.g., graphite) may be positioned between the solid electrolyte and the silver layer, which may help further limit the contact of the silver layer with the solid electrolyte. In addition, a pre-coating layer may be used that is above the dielectric and includes an organometallic compound, such as described in detail below.
[0079] II. terminal
[0080] When forming the desired layer, the capacitor can be provided with the terminal as described above. More specifically, the capacitor contains an anode terminal and a cathode terminal, the anode terminal is electrically connected to the anode lead of the capacitor element, and the cathode terminal is electrically connected to the solid electrolyte of the capacitor element. Any conductive material can be used to form the terminal, such as conductive metal (for example, copper, nickel, silver, nickel, zinc, tin, palladium, lead, copper, aluminum, molybdenum, titanium, iron, zirconium, magnesium and their alloys). Particularly suitable conductive metals include, for example, copper, copper alloys (for example, copper-zirconium, copper-magnesium, copper-zinc or copper-iron), nickel and nickel alloys (for example, nickel-iron). The thickness of the terminal is generally selected to minimize the thickness of the capacitor. For example, the thickness of the terminal can be in the range of about 0.05 mm to about 1 mm, in some embodiments about 0.05 mm to about 0.5 mm, and about 0.07 mm to about 0.2 mm. An exemplary conductive material is a copper-iron alloy metal plate that can be purchased from Wieland Electric (Wieland, Germany). If desired, the surface of the terminal can be plated with nickel, silver, gold, tin, etc. as known in the art to ensure that the final component can be mounted to the circuit board. In a specific embodiment, the two surfaces of the terminal are plated with a nickel color band and a silver band (flash) respectively, and the mounting surface is also plated with a tin solder layer.
[0081] The terminals can be connected to the capacitor element using any technique known in the art. For example, in one embodiment, a lead frame defining a cathode terminal and an anode terminal can be provided. In order to attach the capacitor element to the lead frame, a conductive adhesive can first be applied to the surface of the cathode terminal. The conductive adhesive can include, for example, conductive metal particles containing a resin composition. The metal particles can be silver, copper, gold, platinum, nickel, zinc, bismuth, etc. The resin composition can include a thermosetting resin (e.g., an epoxy resin), a curing agent (e.g., anhydride), and a coupling agent (e.g., a silane coupling agent). Suitable conductive adhesives can be used in Osako et al.Any of a variety of techniques may be used to apply the conductive adhesive to the cathode terminal. For example, printing techniques may be used due to their practical and cost-effective advantages. The anode lead may also be electrically connected to the anode terminal using any technique known in the art (e.g., mechanical welding, laser welding, conductive adhesive, etc.). When the anode lead is electrically connected to the anode terminal, the conductive adhesive may be cured to ensure that the electrolytic capacitor is adequately adhered to the cathode terminal.
[0082] For example, refer to Figure 1 , a capacitor 30 is shown, which includes an anode terminal 62 and a cathode terminal 72, which are electrically connected to a capacitor element 33, and the capacitor element 33 has an upper surface 37, a lower surface 39, a front surface 36, a rear surface 38, a first side surface 35, and an opposite side surface (not shown). The cathode terminal 72 can be arranged to be in electrical contact with any surface of the capacitor element, such as by a conductive adhesive. For example, in the embodiment shown, the cathode terminal 72 includes a first component 73 and a second component 75, the first component 73 is generally parallel to and adjacent to the upper surface 37, and the second component 75 is generally parallel to and adjacent to the lower surface 39. The first component 73 is also in electrical contact with the upper surface 37. The cathode terminal 72 can also include a third component 77, which is generally extended in a direction perpendicular to the first component 73 and the second component 75. If desired, the third component 77 can also be arranged to be in electrical contact with the rear surface 38 of the capacitor element 33. The anode termination 62 likewise includes a first component 63 that is generally parallel to the lower surface 39 of the capacitor element 33 and a second component 67 that is generally parallel to the anode lead 16. Further, the anode termination 62 may include a third component 64 that is generally perpendicular to the first component 63 and a fourth component 69 that is generally perpendicular to the second component 67 and is located near the anode lead 16. In the illustrated embodiment, the second component 67 and the fourth component 69 define the area 51 for connection to the anode lead 16. Although Figure 1 Not depicted, but region 51 may have a “U-shape” to further enhance surface contact and mechanical stability of lead 16 .
[0083] The terminals may be connected to the capacitor element using any technique known in the art. For example, in one embodiment, a lead frame may be provided that defines the cathode terminal 72 and the anode terminal 62. To attach the capacitor element 33 to the lead frame, a conductive adhesive 49 may first be applied to the surface of the cathode terminal 72. In one embodiment, the anode terminal 62 and the cathode terminal 72 are folded to Figure 1in the position shown. Thereafter, the capacitor element 33 is positioned on the cathode terminal 72 so that the lower surface 39 of the capacitor element contacts the adhesive 49 and the anode lead 16 contacts the area 51. The anode lead 16 is then electrically connected to the area 51 using any technique known in the art (e.g., mechanical welding, laser welding, conductive adhesive, etc.). For example, the anode lead 16 can be welded to the anode terminal 62 using a laser. A laser typically includes a resonator that includes a laser medium capable of releasing photons by stimulated emission and an energy source that excites the laser medium elements. A suitable laser is one in which the laser medium is composed of aluminum and yttrium garnet (YAG) doped with neodymium (Nd). The excited particles are neodymium ions Nd 3+ The energy source may provide continuous energy to the laser medium to emit a continuous laser beam or energy release to emit a pulsed laser beam. The conductive adhesive may then be cured when the anode lead 16 is electrically connected to the anode terminal 62. For example, a heat press may be used to apply heat and pressure to ensure that the electrolytic capacitor element 33 is adequately adhered to the cathode terminal 72 via the adhesive 49.
[0084] III. Barrier coating
[0085] As described above, the barrier coating is disposed proximate the anode terminal and / or the cathode terminal such that the barrier coating contacts the housing material. One or more coatings may be employed. For example, in one embodiment, a barrier coating may be employed that covers at least a portion of the anode terminal. In such an embodiment, the coating may also contact at least a portion of a surface of the capacitor element, such as the front surface, bottom surface, and / or top surface of the capacitor element. Similarly, the coating may also contact at least a portion of the anode lead. In another embodiment, a barrier coating may be employed that covers at least a portion of the cathode terminal. In such an embodiment, the coating may also contact at least a portion of a surface of the capacitor element, such as the rear surface, top surface, and / or bottom surface. Again, refer to Figure 1 , for example, a capacitor 30 is shown having a barrier coating 90 located on the anode terminal 62. More specifically, in the illustrated embodiment, the coating 90 contacts the second component 67 and the fourth component 69 of the anode terminal 62 so that the region 51 is generally covered. The coating 90 also contacts at least a portion of the anode lead 16, particularly at those locations around the region 51 where the lead 16 is connected to the anode terminal 62. Of course, it should be understood that the coating may also be provided in other configurations and disposed on any desired surface. For example, in one embodiment, the coating may only contact the second component 67 of the anode terminal 62.
[0086] IV. Shell material
[0087] As described above, the capacitor element and the anode lead are typically encapsulated with a casing material such that at least a portion of the anode termination and at least a portion of the cathode termination are exposed for mounting to a circuit board. Figure 1 For example, capacitor element 33 and anode lead 16 may be encapsulated within casing material 28 such that at least a portion of anode termination 62 and at least a portion of cathode termination 72 remain exposed. Further, as indicated above, at least a portion of casing material 28 is also in contact with barrier coating 90.
[0088] The shell material can be formed by a variety of materials. For example, in one embodiment, the shell material can be formed by a curable resinous matrix, and the resinous matrix can be hydrophobic. For example, in certain embodiments, the resinous matrix can include polycyanate, which contains at least two cyanate groups. For example, when solidified, polycyanate can form a polycyanurate with a triazine ring. Due to the high symmetry in the triazine ring, when the dipole associated with the carbon-nitrogen bond and the carbon-oxygen bond is offset, the resulting polycyanurate can have a relatively high degree of moisture resistance. For example, suitable polycyanates may include: bisphenol A dicyanate; 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, resorcinol, hydroquinone, 4,4'-thiodiphenol, 4,4'-sulfonylbiphenyl, 3,3',5,5'-tetrabromobisphenol A, 2,2',6,6'-tetrabromobisphenol A, 2,2'-dihydroxybiphenyl, 3,3'-dimethoxybisphenol A, 4,4'-dihydroxydi phenyl bicarbonate (ester), dicyclopentadiene bisphenol, 4,4'-dihydroxybenzophenone, 4,4'-dihydroxydiphenylmethane, tricyclopentadiene bisphenol and the like dicyanate; tri(hydroxyphenyl)methane tricyanate, 2,2',4,4'-tetrahydroxydiphenylmethane tetracyanate, phenol formaldehyde condensation product (novolac) polycyanate; dicyclopentadiene and phenol condensation product polycyanate; etc. If desired, the polycyanate may also contain one or more polycyclic aliphatic groups containing two or more cyclic rings, such as C 7 -C 20Polycyclic aliphatic groups include cyclopentadiene, norbornane, bornane, norbornadiene, tetrahydroindene, methyltetrahydroindene, dicyclopentadiene, dicyclo-(2,2,1)-hept-2,5-diene, 5-methylene-2-norbornene, 5-ethylidene-2-norbornene, 5-propenyl-2-norbornene, 5-(4-cyclopentenyl)-2-norbornene, 5-cyclohexylidene-2-norbornene, 5-vinyl-2-norbornene, etc. In a specific embodiment, for example, the polycyanate can be dicyclopentadiene bisphenol cyanate. Without intending to be limited by theory, it is believed that this polycyclic group can be used as a non-polar bridging group for polycyanate, which helps improve moisture resistance.
[0089] The resinous matrix may also contain only epoxy resin, or epoxy resin and polycyanate are combined. When used in combination, epoxy resin can react with polycyanate to form a copolymer and / or crosslink with polycyanate resin when cured. Examples of suitable epoxy resins include, for example, bisphenol A type epoxy resin, bisphenol F type epoxy resin, phenol novolac type epoxy resin, o-cresol novolac type epoxy resin, brominated epoxy resin and biphenyl type epoxy resin, cycloaliphatic epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, cresol novolac type epoxy resin, naphthalene type epoxy resin, phenol aralkyl type epoxy resin, cyclopentadiene type epoxy resin, heterocyclic epoxy resin, etc. However, in order to help provide the desired humidity resistance, it is particularly desirable to use epoxy phenol novolac ("EPN") resin, which is a glycidyl ether of phenol novolac resin. For example, these resins can be prepared by the reaction of phenol and excess formaldehyde in the presence of an acidic catalyst to produce phenolic novolac resins. Then, by reacting phenolic novolac resins with epichlorihydrin in the presence of sodium hydroxide, novolac epoxy resins are prepared. Specific embodiments of novolac epoxy resins include phenol-novolac epoxy resins, cresol-novolac epoxy resins, naphthol-novolac epoxy resins, naphthol-phenol co-condensation novolac epoxy resins, naphthol-cresol co-condensation novolac epoxy resins, brominated phenol-novolac epoxy resins, etc. No matter which resin is selected, the resulting phenolic novolac epoxy resins usually have more than two oxirane groups, and can be used to produce a cured coating composition with a high crosslinking density, which is particularly suitable for enhancing moisture resistance. One such phenolic novolac epoxy resin is poly[(phenyl glycidyl ether)-copolymer-formaldehyde]. Other suitable resins may be ARALDITE commercially available from Huntsman (trade names such as GY289, EPN 1183, EP 1179, EPN 1139 and EPN 1138).
[0090] The polycyanate and / or epoxy resin can be cross-linked with a co-reactant (hardener) to further improve the mechanical properties of the composition and also improve the overall moisture resistance of the composition as described above. Examples of these co-reactants may include, for example, polyamides, amidoamines (e.g., aromatic amidoamines such as aminobenzamide, aminobenzanilide, and aminobenzenesulfonamide), aromatic diamines (e.g., diaminodiphenylmethane, diaminodiphenylsulfone, etc.), aminobenzoates (e.g., propylene glycol diparaaminobenzoate and neopentyl glycol diparaaminobenzoate), fatty amines (e.g., triethylenetetramine, isophoronediamine), alicyclic amines (e.g., isophoronediamine), imidazole derivatives, guanidines (e.g., tetramethylguanidine), carboxylic anhydrides (e.g., methylhexahydrophthalic anhydride), carboxylic acid hydrazides (e.g., adipic acid hydrazides), phenolic novolac resins (e.g., phenol novolac, cresol novolac, etc.), carboxylic acid amides, etc., and combinations thereof. Phenolic novolac resins may be particularly suitable for use in the present invention.
[0091] The shell material may also include an inorganic oxide filler. Such fillers are typically maintained at high levels of the shell material, for example, from about 75 wt.% to about 99.5 wt.%, in some embodiments from about 76 wt.% to about 99 wt.%, and in some embodiments from about 77 wt.% to about 90 wt.%, while the resinous matrix typically constitutes from about 0.5 wt.% to about 25 wt.%, in some embodiments from about 1 wt.% to about 24 wt.%, and in some embodiments from about 10 wt.% to about 23 wt.% of the shell material. The nature of the inorganic oxide filler may vary, such as silica, alumina, zirconium oxide, magnesium oxide, iron oxide (e.g., iron hydroxide oxide yellow), titanium oxide (e.g., titanium dioxide), zinc oxide (e.g., boron zinc hydroxide), copper oxide, zeolites, silicates, clays (e.g., montmorillonite clay), etc., as well as composite materials (e.g., alumina-coated silica particles), and mixtures thereof. However, regardless of the specific filler employed, most, if not all, of the inorganic oxide fillers are typically in the form of glassy silica, which is believed to further improve the thermal expansion resistance of the shell material due to the high purity and relatively simple chemical form of glassy silica. For example, glassy silica can constitute about 30 wt.% or more of the total weight of fillers employed in the composition, in some embodiments, about 35 wt.% to about 90 wt.%, and in some embodiments, about 40 wt.% to about 80 wt.%, and glassy silica is about 20 wt.% to about 70 wt.%, in some embodiments, about 25 wt.% to about 65 wt.%, and in some embodiments, about 30 wt.% to about 60 wt.% of the entire composition. Of course, other forms of silica may also be used in combination with glassy silica, such as quartz, fumed silica, cristobalite, and the like.
[0092] In addition to the components mentioned above, it should be understood that other additives may be employed in the shell material, such as photoinitiators, viscosity modifiers, suspension aids, pigments, stress reducers, coupling agents (e.g., silane coupling agents), stabilizers, etc. When employed, these additives typically constitute from about 0.1 to about 20 wt. % of the total composition.
[0093] The specific manner in which the shell material is applied to the capacitor element can be varied as desired. In a specific embodiment, the capacitor element is placed in a mold and the shell material is applied to the capacitor element so that the shell material occupies the space defined by the mold and exposes at least a portion of the anode terminal and at least a portion of the cathode terminal. The shell material may initially be provided in the form of a single or multiple compositions. For example, the first composition may include a resinous matrix and a filler, and the second composition may include a co-reactant. In any case, after application, the shell material may be heated or allowed to stand at ambient temperature so that the resinous matrix is cross-linked with the co-reactant, thereby curing and hardening the shell material into a desired shell shape. For example, the shell material may be heated to about 15°C to about 150°C, in some embodiments about 20°C to about 120°C, and in some embodiments about 25°C to about 100°C.
[0094] The present invention may be better understood with reference to the following examples.
[0095] Testing Procedure
[0096] capacitance
[0097] Capacitance is measured using a Keithley 3330 Precision LCZ meter with Kelvin Leads, at a 2.2 volt DC bias and a 0.5 volt peak to peak sinusoidal signal. The operating frequency may be 120 Hz and the temperature may be 23°C ± 2°C. In some cases, "wet-dry" capacitance may be determined. "Dry capacitance" refers to the capacitance of the part before the solid electrolyte, graphite, and silver layers are applied, while "wet capacitance" refers to the capacitance of the part after the dielectric is formed, measured in 14% nitric acid, with a 1 mF tantalum cathode as reference with a 10 volt DC bias and a 0.5 volt peak to peak sinusoidal signal, after immersion in the electrolyte for 30 seconds.
[0098] Equivalent Series Resistance (ESR)
[0099] The equivalent series resistance can be measured using a Keithley 3330 precision LCZ meter with Kelvin leads, with a 2.2 volt DC bias and a 0.5 volt peak-to-peak sinusoidal signal. The operating frequency is 100 kHz and the temperature is 23°C ± 2°C.
[0100] Dissipation Factor
[0101] The dissipation factor may be measured using a Keithley 3330 precision LCZ meter with Kelvin leads, with a 2.2 volt DC bias and a 0.5 volt peak-to-peak sinusoidal signal. The operating frequency may be 120 Hz and the temperature may be 23°C ± 2°C.
[0102] Leakage Current
[0103] The leakage current may be measured using a leakage tester at a temperature of 23°C ± 2°C and at the rated voltage after at least 60 seconds.
[0104] Load humidity test
[0105] The humidity test can be performed based on standard IEC 68-2-67:1995 (85°C / 85% relative humidity). 25 test components (mounted on a printed circuit board substrate) can be loaded with the rated voltage under the above humidity test conditions. After recovering from the humidity test conditions for 2 to 24 hours, the capacitance and ESR can be measured at 0, 120, 250, 500, 1000 and 1500 hours at a temperature of 23°C ± 2°C.
[0106] High temperature storage test
[0107] High temperature storage testing can be performed based on IEC 60068-2-2:2007 (Condition Bb, temperature 150°C). 25 test components (not mounted on a printed circuit board substrate) can be tested under the above temperature conditions. All measurements of capacitance and ESR can be performed at a temperature of 23°C ± 2°C after 1 to 2 hours of recovery from the temperature test conditions.
[0108] Example 1
[0109] Anode samples were formed using 50,000 μFV / g tantalum powder. Each anode sample was embedded with tantalum wire, sintered at 1380°C, and pressed to 5.8 g / cm 3 The pellets were anodized to 24.5 volts at 85°C in a water / phosphoric acid electrolyte with a conductivity of 8.6 mS to form a dielectric layer. The pellets were anodized again to 80 volts at 30°C for 25 seconds in a water / boric acid / disodium tetraborate electrolyte with a conductivity of 2.0 mS to form a thicker oxide layer built on the exterior. The anode was then immersed in iron (III) toluenesulfonate (Clevios TM C, Heraeus) in butanol and then immersed in 3,4-ethylenedioxythiophene (Clevios TM M, Heraeus) and polymerized to form a conductive polymer coating. After 45 minutes of polymerization, a thin layer of poly(3,4-ethylenedioxythiophene) was formed on the dielectric surface. The anode was washed in methanol to remove reaction byproducts, anodized in a liquid electrolyte, and washed again in methanol. This process was repeated 6 times. Afterwards, the component was immersed in a dispersed poly(3,4-ethylenedioxythiophene) (Clevios) with a solid content of 2.0% and a viscosity of 20mPa.s.TM K, Heraeus). After coating, the parts were dried at 125° C. for 20 minutes. This process was repeated 3 times. Afterwards, the parts were immersed in a dispersed poly(3,4-ethylenedioxythiophene) (Clevios TM K, Heraeus). After coating, the parts were dried at 125°C for 20 minutes. This process was repeated 12 times. The parts were then dipped into a graphite dispersion and dried. The parts were dipped into a silver dispersion and dried. Finally, the parts were mounted with metal terminals formed from a copper-based material. Multiple parts (500) of 47μF / 10V capacitors were made in this way and will be encapsulated in standard silica resin.
[0110] Example 2
[0111] Capacitors were formed in the manner described in Example 1, except that the resulting parts were dip coated with a hydrophobic resinous material (glass transition temperature of about 100° C.) described herein after the silver dispersion was applied and dried. Multiple parts (500) of 47 μF / 10V capacitors were made in this manner and encapsulated in standard silica resin.
[0112] Example 3
[0113] Capacitors were formed in the manner described in Example 1 except that the hydrophobic resinous material was applied to the anode lead and anode termination connection sites and dried. Multiple components (500) of 47 μF / 10V capacitors were made in this manner and potted in standard silica resin.
[0114] The component samples of Examples 1 and 2 were subjected to a high temperature storage test. The results of ESR and capacitance in the high temperature storage test are listed in Tables 1 and 2 below.
[0115] Table 1: High temperature storage test - capacitance
[0116]
[0117] Table 2: High temperature storage test-ESR
[0118]
[0119] The component samples of Examples 1 and 3 were also subjected to a load humidity test. The leakage current results of the load humidity test are listed in Table 3 below.
[0120] Table 3: Load humidity test - leakage current
[0121]
[0122] Without departing from the spirit and scope of the present invention, those of ordinary skill in the art may implement these and other modifications and variations of the present invention. In addition, it should be understood that the various aspects of the various embodiments may be interchangeable in whole or in part. In addition, those of ordinary skill in the art will appreciate that the foregoing description is exemplary only and is not intended to limit the present invention further described in these appended claims.
Claims
1. A solid electrolytic capacitor, comprising: A capacitor element comprising a sintered porous anode body, a dielectric overlying the anode body, and a solid electrolyte overlying the dielectric; an anode lead extending from a surface of the capacitor element; an anode terminal electrically connected to the anode lead; and a cathode terminal electrically connected to the solid electrolyte, a casing material encapsulating the capacitor element and anode lead; as well as, A barrier coating disposed on at least a portion of the anode terminal and / or at least a portion of the cathode terminal and in contact with the shell material, wherein the coating comprises a hydrophobic resinous material, wherein the resinous material comprises an olefin polymer having a glass transition temperature of 20°C to 160°C.
2. The solid electrolytic capacitor according to claim 1, wherein: The olefin polymer includes a cycloolefin polymer.
3. The solid electrolytic capacitor according to claim 2, wherein: The cycloolefin polymer is formed from cycloolefin monomers.
4. The solid electrolytic capacitor according to claim 3, wherein: The monomers include bicyclic cycloolefins.
5. The solid electrolytic capacitor according to claim 4, wherein: The bicyclic cycloolefins include norbornene.
6. The solid electrolytic capacitor according to claim 3, wherein: The cycloolefin polymers are formed from tetracyclic cycloolefins.
7. The solid electrolytic capacitor according to claim 6, wherein: The tetracyclic cycloolefins include tetracyclododecene.
8. The solid electrolytic capacitor according to claim 3, wherein: The cycloolefin monomer is copolymerized with an α-olefin monomer.
9. The solid electrolytic capacitor according to claim 3, wherein: The cycloolefin monomer is substituted with a halocarbon functional group.
10. The solid electrolytic capacitor according to claim 1, wherein: The barrier coating covers at least a portion of the anode terminal.
11. The solid electrolytic capacitor according to claim 10, wherein: The barrier coating also covers at least a portion of the anode lead.
12. The solid electrolytic capacitor according to claim 10, wherein: The barrier coating also covers at least a portion of the surface of the capacitor element from which the anode lead extends.
13. The solid electrolytic capacitor according to claim 1, wherein: The shell material is formed of a resinous matrix.
14. The solid electrolytic capacitor according to claim 13, wherein: The resinous matrix comprises an epoxy resin.
15. The solid electrolytic capacitor according to claim 13, wherein: The resinous matrix further comprises silicon dioxide in an amount of 75 wt. % to 99.5 wt. % of the matrix.
16. The solid electrolytic capacitor according to claim 1, wherein: The capacitor element further includes a cathode coating comprising a metal particle layer overlying the solid electrolyte, wherein the metal particle layer includes a plurality of conductive metal particles.
17. The solid electrolytic capacitor according to claim 16, wherein: The metal particles include silver.
18. The solid electrolytic capacitor according to claim 1, wherein: The anode body includes tantalum.
19. The solid electrolytic capacitor according to claim 1, wherein: The solid electrolyte includes a conductive polymer.
20. The solid electrolytic capacitor according to claim 19, wherein: The conductive polymer has a repeating unit of the formula: in R7 is a linear or branched C1 to C 18 Alkyl, C5 to C 12 Cycloalkyl, C6 to C 14 Aryl, C7 to C 18 Aralkyl, or a combination thereof; and q is an integer from 0 to 8.
21. The solid electrolytic capacitor according to claim 20, wherein: The conductive polymer is poly(3,4-ethylenedioxythiophene).
22. The solid electrolytic capacitor according to claim 20, wherein: The solid electrolyte also includes a polymer counter ion.
23. The solid electrolytic capacitor of claim 1, further comprising an outer polymer coating overlying the solid electrolyte and comprising prepolymerized conductive polymer particles and a crosslinking agent.
24. The solid electrolytic capacitor according to claim 1, wherein: The capacitor exhibits an aged capacitance measured at 23°C after being exposed to the high temperature storage test at a temperature of 150°C for 3000 hours and then allowed to recover for 1 to 2 hours, and exhibits an initial capacitance measured at 23°C before being exposed to the high temperature storage test, wherein the ratio of the aged capacitance to the initial capacitance is 0.6 to 1.
25. The solid electrolytic capacitor according to claim 1, wherein: The capacitor exhibits an aged ESR measured at 23°C after being exposed to a high temperature storage test at a temperature of 150°C for 3000 hours and then allowed to recover for 1 to 2 hours, and exhibits an initial ESR measured at 23°C before being exposed to the high temperature storage test, wherein the ratio of the aged ESR to the initial ESR is 10 or less.
26. The solid electrolytic capacitor according to claim 1, wherein: The capacitor has an ESR of 0.1 milliohm to 60 milliohm measured at a temperature of 23°C.
27. The solid electrolytic capacitor according to claim 1, wherein: The capacitor exhibits an aged DCL measured at 23°C after being exposed to a high humidity test at a relative humidity level of 85% and a temperature of 85°C for 1500 hours and then allowed to recover for 1 to 2 hours, and exhibits an initial DCL measured at 23°C before being exposed to the high humidity test, wherein a ratio of the aged DCL to the initial DCL is 10 or less.
28. A method of forming a solid electrolytic capacitor as claimed in any one of the preceding claims, the method comprising: disposing a coating formulation on at least a portion of the anode terminal, the coating formulation comprising a hydrophobic resinous material and a solvent; as well as, The solvent is removed from the coating formulation to form the barrier coating.
29. The method according to claim 28, wherein: The solvent includes a hydrocarbon solvent.