Nickel-based active material, positive electrode including the same, and lithium secondary battery

By using a mixture of large-diameter and small-diameter nickel-based active materials in lithium secondary batteries, the electrochemical reaction is homogenized, solving the problem of deterioration in the cycle characteristics of nickel-based active materials in lithium secondary batteries, and improving the high-temperature stability and lifespan of the battery.

CN114430036BActive Publication Date: 2024-11-15SAMSUNG SDI CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111234675.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-10-29
Filing Date
2021-10-22
Publication Date
2024-11-15
Estimated Expiration
2041-10-22

AI Technical Summary

Technical Problem

Existing nickel-based active materials suffer from deterioration in cycle characteristics in lithium secondary batteries, especially under high temperature and high pressure conditions, which affects the stability and lifespan of the battery.

Method used

By using a mixture of positive electrode active materials, including large-diameter and small-diameter nickel-based active materials, and controlling the particle size and type, the electrochemical reaction is homogenized, gas generation is reduced, and structural stability is improved.

Benefits of technology

This study achieved improved cycle life characteristics of lithium secondary batteries at both room temperature and high temperature, suppressed gas generation, and improved the high-temperature stability and safety of the batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114430036B_ABST
    Figure CN114430036B_ABST
Patent Text Reader

Abstract

A nickel-based active material, a positive electrode including the same, and a lithium secondary battery are provided, the lithium secondary battery including a positive electrode, a negative electrode, and an electrolyte between the positive electrode and the negative electrode. The nickel-based active material includes 80 mol% or more of nickel relative to metal elements other than lithium, and the nickel-based active material includes: i) large secondary particles having a size in the range of 10 μm to 20 μm and including aggregates of primary particles having a size of 1 μm or less; ii) large crystalline particles including primary particles having a size in the range of 1 μm to 5 μm; and iii) small secondary particles having a size in the range of 1 μm to 7 μm and including aggregates of primary particles having a size of 1 μm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One or more aspects of embodiments of the present disclosure relate to a nickel-based active material, a positive electrode including the same, and a lithium secondary battery using the positive electrode. Background Art

[0002] In order to meet the development trend for compact, high-performance devices, it is becoming increasingly important to manufacture small, lightweight, and high-energy-density lithium secondary batteries. In addition, the stability of lithium secondary batteries under high-capacity, high-temperature, and high-voltage conditions has become an important factor for their application in electric vehicles and the like.

[0003] Various positive electrode active materials are currently being studied to realize lithium secondary batteries suitable for the above-mentioned purpose. The positive electrode active material plays an important role in the capacity and cycle characteristics of lithium secondary batteries.

[0004] A nickel-based active material including a large amount (eg, ratio) of nickel is used as a positive electrode active material having excellent capacity characteristics. However, a large amount of nickel may be associated with deteriorated cycle characteristics, and thus improvement in this regard is desired. Summary of the invention

[0005] One or more aspects of the disclosed embodiments are directed to nickel-based active materials that provide reduced cell resistance while having excellent or desirable capacity characteristics.

[0006] One or more aspects of embodiments of the present disclosure relate to a positive electrode including a nickel-based active material.

[0007] One or more aspects of embodiments of the present disclosure are directed to a positive electrode having improved cycle characteristics by employing a positive electrode.

[0008] Additional aspects will be set forth in part in the description which follows and, in part, will be obvious from the description, or may be learned by practice of the embodiments presented in the disclosure.

[0009] One or more embodiments of the present disclosure provide a nickel-based active material, the nickel-based active material comprising 80 mol % or more of nickel relative to metal elements other than lithium, wherein:

[0010] The nickel-based active material includes: i) large secondary particles having a size in the range of 10 μm to 20 μm, each of which includes aggregates of primary particles having a size of 1 μm or less; ii) large crystalline particles, which include primary particles having a size in the range of 1 μm to 5 μm; and iii) small secondary particles having a size in the range of 1 μm to 7 μm, each of which includes aggregates of primary particles having a size of 1 μm or less.

[0011] One or more embodiments of the present disclosure provide a positive electrode including a nickel-based active material.

[0012] One or more embodiments of the present disclosure provide a lithium secondary battery including a positive electrode, a negative electrode, and an electrolyte between the positive electrode and the negative electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] The above and other aspects, features and advantages of the embodiments of the present disclosure will become more apparent from the following description taken in conjunction with the accompanying drawings, in which:

[0014] Figure 1 is a scanning electron microscope (SEM) image of the positive electrode active material prepared in Example 1;

[0015] Figure 2 and Figure 3 They are Figure 1 SEM images of large crystalline particles and small secondary particles in the positive electrode active material;

[0016] FIG. 4A to FIG. 4C is a SEM image of the large secondary particles prepared in Preparation Example 1;

[0017] Figure 5A and 5B is a SEM image of the large crystal particles prepared in Preparation Example 2;

[0018] Fig. 6A and Figure 6B is a SEM image of the small secondary particles prepared in Preparation Example 3;

[0019] Figure 7 Showing the room temperature life characteristics of the lithium secondary batteries according to Example 1 and Comparative Example 1;

[0020] Figure 8 The high temperature life characteristics of the lithium secondary batteries according to Example 1 and Comparative Example 1 are shown; and

[0021] Fig. 9 is a schematic diagram of a lithium secondary battery according to an embodiment. DETAILED DESCRIPTION

[0022] Now will refer to the embodiment in more detail, its example is explained in the attached drawings, wherein the same reference numerals refer to the same elements throughout, and its repeated description may not be provided. In this regard, the present embodiment may have different forms, and should not be interpreted as being limited to the description set forth herein. Therefore, the embodiment is only described by reference to the accompanying drawings to explain the aspects of this description. As used herein, the term "and / or" includes any and all combinations of one or more related enumerated items. Expressions such as "at least one of ...", "one of ..." and "selected from ..." before / after the list of elements modify the entire list of elements, without modifying the individual elements of the list.

[0023] As used herein, the singular forms "a", "an", and "the" are intended to include the plural forms as well, unless the context clearly indicates otherwise. It will be further understood that the terms "includes", "including", "comprises", and / or "comprising", when used in this specification, indicate the presence of stated features, steps, operations, elements, and / or components, but do not preclude the presence or addition of one or more other features, steps, operations, elements, components, and / or groups thereof. In addition, when describing embodiments of the present disclosure, the use of "may" refers to "one or more embodiments of the present disclosure."

[0024] It will be understood that when an element is referred to as being "on," "connected to," or "coupled to" another element, it may be directly on, directly connected to, or directly coupled to the other element, or one or more intervening elements may also be present. When an element is referred to as being "directly on," "directly connected to," or "directly coupled to" another element, there are no intervening elements.

[0025] Hereinafter, a nickel-based active material, a method of preparing the same, a positive electrode including the same, and a lithium secondary battery including the positive electrode according to one or more embodiments will now be described in more detail.

[0026] Among metal elements other than lithium, the nickel-based active material includes 80 mol% or more of nickel, wherein the nickel-based active material includes: i) large secondary particles having a size in the range of 10 μm to 20 μm and each including aggregates of primary particles having a size of 1 μm or less; ii) large crystalline particles, the large crystalline particles including primary particles having a size in the range of 1 μm to 5 μm; and iii) small secondary particles, the small secondary particles having a size in the range of 1 μm to 7 μm and each including aggregates of primary particles having a size of 1 μm or less.

[0027] According to an embodiment, the large crystal particle may be a one-piece particle or a monolithic particle (e.g., it does not aggregate to form a secondary particle). According to another embodiment, the large crystal particle may be an aggregate of primary particles (e.g., it may be a secondary particle). In some embodiments, the term "large crystal particle" may indicate a primary particle having a crystal size larger than the crystal size of each primary particle included in the small secondary particle.

[0028] In this specification, the term "integral particles" refers to a particle structure in which each particle exists as an independent phase and is not a morphologically aggregated particle. Alternative particle structures of integral particles may include structures in which small particles (primary particles) are physically and / or chemically aggregated to form large particles (secondary particles). In this specification, the term "integral" may refer to a morphology in which particles are separated and / or dispersed from each other so that each particle has an independent and / or discrete (e.g., one) phase, as opposed to a morphology in which multiple crystalline particles are aggregated. In some embodiments, the particle structure may have a morphology in which no more than 10 particles are aggregated together.

[0029] In the nickel-based active material, the amount of nickel may be 80 mol% or more, 80 mol% to 95 mol%, 85 mol% to 92 mol% or 88 mol% to 90 mol%, relative to 100 mol% of the total amount of non-lithium metal in the positive electrode active material (e.g., metal other than lithium in the metal-oxide layer).

[0030] A nickel-based active material containing a large amount of nickel can be used as a positive electrode active material with improved capacity characteristics. A nickel-based active material containing a large amount of nickel may have excellent capacity characteristics but deteriorated cycle characteristics, and, in this regard, improvement is desired.

[0031] To overcome the above problems, attempts have been made to utilize a mixture of nickel-based active materials having different sizes, but the cycle life improvement has not been sufficient.

[0032] In the present disclosure, in order to obtain a lithium secondary battery with improved cycle life, a mixture of a large-diameter nickel-type particle active material and a small-diameter nickel-type particle active material is used as a positive electrode active material, and the small-diameter nickel-type particle active material is diversified (e.g., a nickel-type active material having particles with relatively smaller diameters is provided as a mixture and / or provided in one or more forms). By changing the particle type (e.g., morphology and / or size) and nickel content of the small-diameter nickel-type particle active material, the non-uniform electrochemical reaction between the large-diameter nickel-type particle active material and the small-diameter nickel-type particle active material can become substantially uniform, thereby achieving structural stability while suppressing or reducing gas generation. By adopting such a positive electrode including such a nickel-type active material, a lithium secondary battery with improved cycle life characteristics at room temperature and high temperature can be achieved.

[0033] According to the embodiment, the nickel-based active material includes large secondary particles, large crystal particles and small diameter secondary particles (small secondary particles), and by controlling or selecting the particle size and the type (e.g., morphology) of the three types (kinds) of particles, the non-uniformity of the electrochemical reaction between the large diameter particle nickel-based active material and the small diameter particle nickel-based active material can be alleviated, thereby preventing or reducing the increase in resistance caused by the non-uniformity.

[0034] In this specification, the term "size" refers to, for example, a diameter when the particles of the lithium-based active material are spherical. In some embodiments, when the particles of the lithium-based active material are not spherical, the term "size" may indicate the major axis length. The particle diameter may be an average particle diameter, and the major axis length may be an average major axis length. For example, the particle diameter may be a median particle size or a D50 particle size.

[0035] The average particle diameter can be measured using a particle size distribution (PSD) meter or by a scanning electron microscope (SEM). The major axis length can be measured by SEM.

[0036] The D50 particle size indicates that 50% of the particles in the volume distribution of the particle size have a larger particle size, while 50% of the particles in the volume distribution of the particle size have a smaller particle size. When the particles are spherical, the term "average particle diameter" of the particles may be the median diameter (D50). In this specification, "D50" refers to the particle diameter corresponding to 50% of the volume relative to the cumulative particle distribution in the order of the smallest size to the largest size. The distribution may be accumulated in the order of the smallest particle size to the largest particle size. In the curve, when the total number of particles is 100%, it means the value corresponding to 50% of the particle diameter from the smallest particle.

[0037] By aggregating primary particles with an average particle size of 1 μm or less, large secondary particles can be formed into secondary particles with an average particle size of 10 μm to 20 μm, and by aggregating primary particles with a size of 1 μm or less, small secondary particles can be formed into secondary particles with an average particle size of 1 μm to 7 μm. In some embodiments, unlike large secondary particles, large crystalline particles can have an integral (e.g., integral) shape or form, for example, by increasing the size of primary particles. In some embodiments, large crystalline particles can have a secondary particle form, that is, can be an aggregate of primary particles.

[0038] In the nickel-based active material according to the embodiment, the large crystal particles may each have an integral particle shape obtained by, for example, increasing the size of the primary particles (e.g., forming primary particles with relatively large or increased sizes). Because the large crystal particles have an integral particle structure, the moving path length of the lithium ions to the surface of the nickel-based active material (e.g., when diffusing from the inside of the particles) increases. Therefore, surface impurities can be reduced or minimized, and the surface impurities are formed due to the adsorption of Li2CO3 or LiOH, which can be generated on the surface of the nickel-based active material by the reaction between the lithium ions migrating to the surface of the nickel-based active material and CO2 or moisture in the air. In some embodiments, possible problems caused by such surface impurities (e.g., reducing the risk or occurrence of problems) can be avoided, such as a reduction in battery capacity, an increased interface resistance due to the suppression of the movement of lithium ions, gas generation due to the decomposition of impurities, and causing battery expansion. Therefore, when the nickel-based active material is applied to a battery, the battery may have improved capacity characteristics, high temperature stability, and charge / discharge characteristics.

[0039] According to an embodiment, the large secondary particles may have the highest amount (eg, concentration or ratio) of nickel compared to the large crystalline particles and the small secondary particles. For example, the amount of nickel may decrease in the order of large secondary particles, large crystalline particles, and small secondary particles.

[0040] According to another embodiment, the amount of nickel contained in the large crystalline particles may be equal to or less than the amount of nickel contained in the small secondary particles. According to yet another embodiment, the amount of nickel contained in the large crystalline particles may be greater than the amount of nickel contained in the small secondary particles. The amount of nickel contained in the large secondary particles as described above may be greater than the amount of nickel contained in the small secondary particles and / or may be greater than the amount of nickel contained in the large crystalline particles. Based on 100 mol% of the total amount of metal elements other than lithium in the nickel-based active material, the amount of nickel contained in the large secondary particles may be 90 mol% to 99 mol%, and based on 100 mol% of the total amount of metal elements other than lithium in the nickel-based active material, the amount of nickel contained in the small secondary particles may be 80 mol% to 95 mol%.

[0041] Based on 100 mol% of the total amount of metal elements other than lithium of the nickel-based active material, the amount of nickel contained in the large crystal particles may be 80 mol% to 95 mol%. By controlling or selecting the amount of nickel contained in the large crystal particles to be greater than the amount of nickel contained in the small secondary particles, the nickel-based active material may have enhanced life characteristics and increased mixture density and / or high output performance.

[0042] The difference in nickel amount between the large secondary particles and the large crystalline particles and / or the difference in nickel amount between the large secondary particles and the small secondary particles may be, for example, 19 mol% or less, 15 mol% or less, 10 mol% or less, 1 mol% to 10 mol%, 1 mol% to 5 mol% or 1 mol% to 4 mol%.

[0043] According to still another embodiment, primary particles included in the large crystal particles may have a larger average particle diameter than primary particles included in the small secondary particles.

[0044] The average particle diameter of the primary particles contained in the large secondary particles, large crystal particles and / or small secondary particles constituting the nickel-based active material can be identified by SEM, respectively. For example, the average particle diameter of the primary particles can be obtained from the average value of the particle diameters of 10 to 30 primary particles.

[0045] In the nickel-based active material according to the embodiment, the primary particles in the large secondary particles may have a size of 0.01 to 1 μm, 0.02 to 0.8 μm, 0.03 to 0.5 μm, 0.04 to 0.1 μm, or 0.05 to 0.07 μm (50 to 70 nm).

[0046] In the nickel-based active material according to an embodiment, the large crystal particles may be integral particles or secondary particles as aggregates of primary particles. According to an embodiment, the secondary particles may have a size of 1 μm to 9 μm, for example, 3 μm to 9 μm. According to another embodiment, the secondary particles may have a size of 1 μm to 5 μm.

[0047] In the nickel-based active material according to the embodiment, the small secondary particles may have a size of 1 μm to 7 μm, 3 μm to 7 μm, or 3 μm to 6 μm.

[0048] A lithium secondary battery can be manufactured by utilizing a positive electrode including a nickel-based active material, wherein the nickel-based active material comprises large crystalline particles having a particle size within the above-mentioned range and small secondary particles, and the lithium secondary battery has stable electrochemical reactivity, suppressed gas generation under high voltage, improved reliability and / or safety, and / or high output and / or long cycle life characteristics.

[0049] Based on 100 wt% of the total amount of large secondary particles, large crystalline particles and small secondary particles, the amount of large crystalline particles may be 5 wt% to 25 wt%, 5 wt% to 15 wt% or 5 wt% to 10 wt%, and based on 100 wt% of the total amount of large secondary particles, large crystalline particles and small secondary particles, the amount of small secondary particles may be 5 wt% to 25 wt%, 5 wt% to 15 wt% or 10 wt% to 15 wt%. When the amount of large crystalline particles and small secondary particles is within the above range, a positive electrode having improved life characteristics while having excellent capacity characteristics per volume without (e.g., with reduced) deterioration of expansion characteristics (e.g., due to gas generation at high pressure and / or high temperature) can be manufactured.

[0050] The nickel-based active material according to the embodiment may have an average particle diameter of 10 μm to 20 μm. In some embodiments, the nickel-based active material may have a basic plate form or structure, and may have various suitable shapes, including, for example, a polygonal nanoplate shape (e.g., a hexagonal shape), a spherical shape, an elliptical shape, a nanodisk shape, or a rectangular parallelepiped shape. When the nickel-based active material does not have a spherical shape, its particle size may refer to the major axis length.

[0051] The density of the mixture of the positive electrode including the nickel-based active material may be, for example, 4.0 g / cm 3 or greater, 4.1g / cm 3 or larger, 4.15g / cm 3 or greater or 4.15g / cm 3 Up to 4.20g / cm 3 The mixture density of the positive electrode was obtained by rolling the positive electrode active material layer, cutting it into a size of 30 mm x 30 mm, and measuring the thickness and weight to obtain the mixture density.

[0052] The porosity of the positive electrode according to the embodiment may be 15% or less.

[0053] The porosity of the solid-state ion conductor can be determined by scanning electron microscopy, and the details can be determined by those skilled in the art without undue experimentation. Alternatively, the porosity can be determined using nitrogen isotherms as disclosed in E.P. Barrett, L.G. Joyner, P.P. Halenda, “The determination of pore volume and area distributions in porous substances. I. Computations from nitrogen isotherms,” J. Am. Chem. Soc. (1951), 73, 373–380, and the details can be determined by those skilled in the art without undue experimentation.

[0054] In addition to the above methods, the porosity can also be measured by analysis (such as mercury intrusion porosimetry, transmission electron microscopy (TEM), or cross-sectional analysis of particles using a focused ion beam (FIB)). According to one embodiment, it can be confirmed by scanning electron microscopy and / or transmission electron microscopy analysis. The porosity can be expressed by examining the total volume of the pores in the volume occupied by each layer.

[0055] The nickel-based active material can be, for example, a compound represented by Formula 1, a compound represented by Formula 2, or a combination thereof:

[0056] Formula 1

[0057] Li x Ni 1-y Co y O 2-z X z ,

[0058] wherein, in Formula 1, 0.9 ≤ x ≤ 1.2, 0 < y ≤ 0.2, 0 ≤ z ≤ 0.5, and 0.8 ≤ 1 - y < 1, and

[0059] X is fluorine (F), sulfur (S), phosphorus (P), or a combination thereof,

[0060] Formula 2

[0061] Li x Ni 1-y-z Co y M z O 2-a X a ,

[0062] Among them, in Formula 2, 0.9 ≤ x ≤ 1.2, 0 < y < 0.5 (for example, 0 < y < 0.2), 0.8 ≤ 1 - y - z < 1, 0 ≤ z ≤ 0.5 (for example, 0 < z < 0.2), 0 < y + z ≤ 0.2, and 0 ≤ a < 2.

[0063] M is nickel (Ni), cobalt (Co), manganese (Mn), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), titanium (Ti), zirconium (Zr), niobium (Nb), molybdenum (Mo), tungsten (W), zinc (Zn), aluminum (Al), silicon (Si), chromium (Cr), iron (Fe), vanadium (V), rare earth elements or a combination thereof, and X is F, S, P or a combination thereof.

[0064] In Formulas 1 and 2, the amount of nickel can be 80 mol% or more, for example, 80 mol% to 95 mol% or 85 mol% to 92 mol%; x can be 1 to 1.05; and y can be 0.01 to 0.19. In some embodiments, in Formula 2, M can be Al, and z can be, for example, 0.01 to 0.05.

[0065] The nickel-based active material can be a compound represented by Formula 3, a compound represented by Formula 4 or a combination thereof:

[0066] Formula 3

[0067] Li x Co a Ni b Mn c O2,

[0068] Among them, in Formula 3, 0.9 < x < 1.2, 0 < a < 0.5 (for example, 0 < a < 0.2), 0.8 ≤ b < 1, 0 < c < 0.5, and a + b + c = 1, and

[0069] Formula 4

[0070] Li x Co a Ni b Al c O2,

[0071] Among them, in Formula 4, 0.9 < x < 1.2, 0 < a < 0.5 (for example, 0 < a < 0.2), 0.8 ≤ b < 1, 0 < c < 0.5, and a + b + c = 1.

[0072] In Formula 3 and Formula 4, x may be in the range of 1.0 to 1.1, 1.0 to 1.1, or 1.0 to 1.05; a may be in the range of, for example, 0.001 to 0.45, 0.01 to 0.4, 0.01 to 0.3, 0.01 to 0.2, 0.01 to 0.1, 0.02 to 0.09, or 0.04 to 0.08; b may be in the range of, for example, 0.8 to 0.99, 0.8 to 0.98, or 0.85 to 0.95; and c may be in the range of, for example, 0.001 to 0.19, 0.001 to 0.1, 0.005 to 0.02, or 0.005 to 0.01.

[0073] Non-limiting examples of nickel-based active materials may include LiNi 0.9 Co 0.09 Al 0.01 O2、LiNi 0.9 Co 0.09 Mn 0.01 O2、Li 1.05 Ni 0.9 Co 0.09 Al 0.01 O2、Li 1.05 Ni 0.9 Co 0.09 Mn 0.01 O2、LiNi 0.9 Co 0.09 Al 0.005 Mn 0.005 O、LiNi 0.94 Co 0.04 Al 0.02 O2、LiNi 0.95 Co 0.04 Al 0.01 O2、LiNi 0.85 Co 0.14 Al 0.01 O2、LiNi 0.8 Co 0.19 Al 0.01 O2 and LiNi 0.94 Co 0.04 Al 0.01 Mn 0.01 O2.

[0074] According to an embodiment, when a lithium secondary battery is implemented by using a nickel-based active material with a controlled particle size, high temperature characteristics and rate performance of the lithium secondary battery can be improved, the amount of gas generated under high pressure can be reduced, and / or reliability and / or safety can be ensured.

[0075] During the positive electrode active material manufacturing process, by adjusting the size of the primary particles and secondary particles contained therein, for example, by controlling the conditions of the heat treatment (ie, heat treatment temperature, atmosphere and / or time), the nickel-based active material according to the embodiment may have a reduced specific surface area. As a result, by reducing the residual lithium as much as possible, the nickel-based active material can inhibit the surface side reaction between the residual lithium and the electrolyte solution. In some embodiments, by controlling the manufacturing process in this manner as described above, a positive electrode active material having guaranteed stability under high pressure while having improved crystallinity can be obtained.

[0076] According to an embodiment, in an X-ray diffraction spectrum (XRD) analysis of a nickel-based active material,

[0077] The full width at half maximum (FWHM) of the (003) plane peak may be 0.120 degrees (°) to 0.270°, for example, 0.120° to 0.150°. In some embodiments, the full width at half maximum of the (104) plane peak may be 0.120° to 0.270°, for example, 0.13° to 0.23°, and the interval between the (108) plane peak and the (110) plane peak may be 0.1° to 0.5°. The full width at half maximum value and the peak interval value indicate the crystallinity of the nickel-based active material. From these results, it can be confirmed that the nickel-based active material has a layered crystal structure.

[0078] In the X-ray diffraction spectrum analysis for general nickel-based active materials, the lower half-maximum full width value of the (003) plane peak means the increased crystallinity of the nickel-based active material. Therefore, the crystallinity of the nickel-based active material according to the embodiment can be higher than the crystallinity of the general nickel-based active material. When using a nickel-based active material with increased crystallinity, a lithium secondary battery with good safety under high pressure can be manufactured.

[0079] By X-ray diffraction (XRD) spectral analysis, it was confirmed that the nickel-based active material can have a hexagonal crystal structure. Here, the length of the a-axis can be to The length of the c-axis can be within the range of to The unit cell volume can be within the range of to In XRD spectrum analysis, there is about CuK-α characteristic X-rays of a wavelength of 200 Å can be used as a radiation source.

[0080] In the nickel-based active material according to the embodiment, the amount of residual lithium may be 3,000 ppm or less, for example, 2,000 ppm to 3,000 ppm. The amount of residual lithium can be measured by a titration method. When the amount of residual lithium is within the above range, the side reaction of the residual lithium with the electrolyte solution can be suppressed to suppress gas generation at high pressure and high temperature, and thus the positive electrode active material can have increased stability. In some embodiments, when the amount of residual lithium is within the above range, the pH value of the positive electrode slurry can be reduced in the positive electrode slurry preparation process, so that the positive electrode slurry is stable, and a substantially uniform plate coating process may be possible.

[0081] The nickel-based active material according to the embodiment may be prepared using a general nickel-based active material precursor.

[0082] A method of preparing a nickel-based active material according to an embodiment will now be described in more detail.

[0083] The nickel-based active material may be prepared by, for example, mixing a lithium precursor and a nickel-based active material precursor at a set or predetermined molar ratio, followed by performing a first heat treatment.

[0084] The lithium precursor may be or include, for example, lithium hydroxide, lithium fluoride, lithium carbonate or a mixture thereof. The mixing ratio of the lithium precursor and the nickel-based active material precursor may be stoichiometrically controlled or selected to obtain the nickel-based active material of Formula 2, Formula 3 or Formula 4.

[0085] The mixing of the lithium precursor and the nickel-based active material precursor may be a dry mixing process and may be performed using a mixer or the like. The dry mixing process may be performed by grinding. The grinding conditions are not particularly limited, and grinding may be performed under any conditions as long as the deformation of the precursor used as the starting material (e.g., crushed into fine powder) is minimized or reduced. The size of the lithium precursor mixed with the nickel-based active material precursor may be controlled in advance. The size (average particle diameter) of the lithium precursor may be in the range of 5 μm to 15 μm, for example, about 10 μm. By grinding the lithium precursor (to a size within the above range) and the nickel-based active material precursor at 300 rpm to 3,000 rpm, a desired or appropriate mixture may be obtained. During grinding, when the internal temperature of the mixer rises to 30° C. or higher, a cooling process may be performed to keep the internal temperature of the mixer near room temperature (25° C.).

[0086] The first heat treatment may be performed in an air or oxygen atmosphere.The first heat treatment may be performed at a temperature in the range of, for example, 600°C to 800°C, for example, 650°C to 800°C.

[0087] The method for preparing the nickel-based active material may further include a second heat treatment performed in an air or oxygen atmosphere after the first heat treatment. The second heat treatment may be performed at a temperature in the range of, for example, 700 °C to 900 °C.

[0088] The nickel-based active material precursor may be prepared by co-precipitation of a nickel precursor and other transition metal precursors. For example, the nickel-based active material precursor may be a hydroxide or oxide including nickel, cobalt, and other metals.

[0089] The nickel-based active material precursor may be prepared by mixing a nickel precursor, a cobalt precursor, and a manganese precursor with a first solvent. The nickel precursor, the cobalt precursor, and the manganese precursor may include any materials available in the art, and the amounts of the nickel precursor, the cobalt precursor, and the manganese precursor may be stoichiometrically controlled or selected to obtain a compound of Formula 3.

[0090] The first solvent may be water, ethanol, propanol, or butanol. In some embodiments, based on the total weight of 100 parts by weight of the nickel precursor, the cobalt precursor, and the manganese precursor, the amount of the first solvent may be in the range of 100 parts by weight to 2,000 parts by weight.

[0091] When the nickel-based active material precursor is mixed with a lithium precursor, a second solvent may be used. Similar to the first solvent, the second solvent may be water, ethanol, propanol, or butanol, and based on 100 parts by weight of the lithium precursor, the amount of the second solvent used may be 100 parts by weight to 2,000 parts by weight.

[0092] A complexing agent and a pH regulator may be added and mixed with the mixture of the nickel-based active material precursor and the lithium precursor.

[0093] The nickel-based active material precursor may be, for example, a compound represented by Formula 3-1:

[0094] Formula 3-1

[0095] Ni 1-y-z Co y M z (OH)2,

[0096] wherein in Formula 3-1, 0 < y < 0.5 (for example, 0 < y < 0.2), 0.8 ≤ 1 - y - z < 1, and 0 ≤ z ≤ 0.5, and

[0097] M is Ni, Co, Mn, Mg, Ca, Sr, Ba, Ti, Zr, Nb, Mo, W, Zn, Al, Si, Cr, Fe, V, rare earth elements, or a combination thereof.

[0098] The lithium precursor may include one or more selected from lithium hydroxide, lithium carbonate, lithium sulfate and lithium nitrate. A non-limiting example of the complexing agent may be an ammonia solution as an ammonium ion provider, and a non-limiting example of the pH adjuster may be a sodium hydroxide aqueous solution.

[0099] The pH of the obtained product may be controlled within a range of about 11 to about 13 by adjusting the amount of the pH adjuster. In some embodiments, a precipitate may be obtained from the obtained product and may be washed with pure water and then subjected to a second heat treatment to obtain a nickel-based active material.

[0100] According to another aspect, a positive electrode includes a nickel-based active material as an active material. The positive electrode includes: a current collector; and a nickel-based positive electrode active material layer according to an embodiment provided on the current collector.

[0101] The positive electrode may be prepared by, for example, molding a positive electrode active material composition including a positive electrode active material and a binder in a set or predetermined shape or coating the positive electrode active material composition on a current collector made of, for example, aluminum foil.

[0102] For example, in some embodiments, a positive electrode active material composition can be prepared by mixing a positive electrode active material, a conductive agent, a binder, and a solvent. The positive electrode active material composition can be directly coated on a metal current collector to manufacture a positive electrode plate. In some embodiments, a positive electrode plate can be manufactured by casting the positive electrode active material composition on a separate support and laminating a film separated from the support on a metal current collector. The type (e.g., form) of the positive electrode is not limited to those listed above, and the positive electrode can be formed to have any appropriate type (form).

[0103] The positive electrode may further include any suitable positive electrode active material suitable in the art (eg, mixed or combined with the nickel-based active material according to an embodiment of the present disclosure).

[0104] Non-limiting examples of general positive electrode active materials may include, but are not limited to, one or more selected from the group consisting of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium iron phosphorus oxide, and lithium manganese oxide, and any positive electrode active material available in the art may also be utilized.

[0105] Non-limiting examples of the positive electrode active material may include compounds represented by one or more of the following formulae: Li a A 1-b B' b D2 (where 0.90≤a≤1.8 and 0≤b≤0.5); Li a E 1-b B' b O 2-cD c (where 0.90≤a≤1.8, 0≤b≤0.5, and 0≤c≤0.05); LiE 2-b B'bO 4-c D c (where 0≤b≤0.5 and 0≤c≤0.05); Li a Ni 1-b-c Co b B' c D α (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α≤2); Li a Ni 1-b-c Co b B' c O 2-α F' α (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Co b B' c O 2-α F'2 (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Mn b B' c D α (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α≤2); Li a Ni 1-b-c Mn b B' c O 2-α F' α (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni 1-b-c Mn b B' c O 2-α F'2 (where 0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.05, and 0<α<2); Li a Ni b E c G' d O2 (where 0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, and 0.001≤d≤0.1); Li a Ni b Co c Mn d G'e O2 (where 0.90≤a≤1.8, 0≤b≤0.9, 0≤c≤0.5, 0≤d≤0.5, and 0.001≤e≤0.1); Li a NiG' b O2 (where 0.90≤a≤1.8 and 0.001≤b≤0.1); Li a CoG' b O2 (where 0.90≤a≤1.8 and 0.001≤b≤0.1); Li a MnG' b O2 (where 0.90≤a≤1.8 and 0.001≤b≤0.1); Li a Mn2G' b O4 (where 0.90≤a≤1.8 and 0.001≤b≤0.1); QO2; QS2; LiQS2; V2O5; LiV2O5; LiI'O2; LiNiVO4; Li (3-f) J2(PO4)3(0≤f≤2);Li (3-f) Fe2(PO4)3 (wherein 0≤f≤2); and / or LiFePO4.

[0106] In the above formula: A is Ni, Co, Mn or a combination thereof; B' is Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V, a rare earth element or a combination thereof; D is O, F, S, P or a combination thereof; E is Co, Mn or a combination thereof; F' is F, S, P or a combination thereof; G' is Al, Cr, Mn, Fe, Mg, La, Ce, Sr, V or a combination thereof; Q is Ti, Mo, Mn or a combination thereof; I' is Cr, V, Fe, Sc, Y or a combination thereof; and J is V, Cr, Mn, Co, Ni, Cu or a combination thereof.

[0107] In some embodiments, the above compounds, compounds including a coating on its surface, or a mixture of compounds and compounds including a coating can be used. The coating may include a coating element compound in the form of an oxide of a coating element, a hydroxide of a coating element, an oxyhydroxide of a coating element, an oxycarbonate of a coating element, or a hydroxycarbonate of a coating element. The compounds forming these coatings may be amorphous or crystalline. The coating element included in the coating may be magnesium (Mg), aluminum (Al), cobalt (Co), potassium (K), sodium (Na), calcium (Ca), silicon (Si), titanium (Ti), vanadium (V), tin (Sn), germanium (Ge), gallium (Ga), boron (B), arsenic (As), zirconium (Zr), or a combination thereof. Any suitable method (e.g., spray coating, dip coating, etc.) may be used as a coating formation method, as long as these coating elements do not adversely affect the physical properties of the positive electrode active material when used for the compound. Any suitable coating formation method may be used, and further description thereof will not be provided.

[0108] For example, LiNiO2, LiCoO2, LiMn x O 2x (x=1 or 2), LiNi 1-x Mn x O2(0 <x<1)、LiNi 1-x-y Co x Mn y O2 (0≤x≤0.5 and 0≤y≤0.5), LiFeO2, V2O5, TiS and / or MoS may be used as the positive electrode active material.

[0109] The conductive agent may be or include carbon black and / or graphite particles, but the embodiments are not limited thereto. Any suitable material that can be used as a conductive agent in the art can be used. Non-limiting examples of conductive agents may include: graphite (such as natural graphite and / or artificial graphite); carbon-containing materials (such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black and / or thermal black); conductive fibers (such as carbon fibers and / or metal fibers); metal powders (such as fluorocarbons, aluminum and / or nickel powders); conductive whiskers (such as zinc oxide and / or potassium titanate); conductive metal oxides (such as titanium oxide); and / or conductive materials (such as polyphenylene derivatives).

[0110] Non-limiting examples of the binder include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, polytetrafluoroethylene, mixtures thereof, and / or styrene butadiene rubber polymers, but embodiments are not limited thereto. Any suitable material available in the art as a binder may be utilized.

[0111] Non-limiting examples of the solvent include N-methylpyrrolidone, acetone and / or water, but are not limited thereto. Any material that can be used as a solvent in the art can be utilized.

[0112] The amount of the positive electrode active material, the conductive agent, the binder and the solvent may be within the range generally used in the manufacture of lithium secondary batteries in the relevant field. In some embodiments, one or more of the conductive agent, the binder and the solvent may be omitted according to the intended use and / or structure of the lithium secondary battery.

[0113] The term "true density" of the positive electrode according to the embodiment may refer to the intrinsic density of the positive electrode active material without pores. The true density of the positive electrode may be 4.76 g / cc to 5.10 g / cc.

[0114] A lithium secondary battery according to another embodiment may include a positive electrode including a positive electrode active material, a negative electrode, and an electrolyte disposed therebetween. The lithium secondary battery may be manufactured in the following manner.

[0115] First, a positive electrode may be prepared according to the above-mentioned positive electrode preparation method.

[0116] Next, the negative electrode active material, the conductive agent, the binder and the solvent may be mixed to prepare a negative electrode active material composition. The negative electrode active material composition may be directly coated on a metal current collector and dried to prepare a negative electrode plate. In another embodiment, the negative electrode active material composition may be cast on a separate support, and the film peeled off from the support may then be laminated on a metal current collector to prepare a negative electrode plate.

[0117] Any suitable negative electrode active material generally available in the art may be used as the negative electrode active material without particular limitation, and non-limiting examples of the negative electrode active material may include lithium metal, a metal that can form an alloy with lithium, a transition metal oxide, a transition metal sulfide, a material capable of doping or dedoping lithium, a material capable of reversibly inserting and deinserting lithium ions, and / or a conductive polymer.

[0118] The transition metal oxide may be, for example, tungsten oxide, molybdenum oxide, titanium oxide, lithium titanium oxide, vanadium oxide, or lithium vanadium oxide. Non-limiting examples of transition metal oxides and transition metal sulfides may include: Group I metal oxides or sulfides (such as CuO, Cu2O, Ag2O, CuS, and / or CuSO4); Group IV metal oxides or sulfides (such as TiS2 and / or SnO); Group V metal oxides or sulfides (such as V2O5, V6O5); 12 , VO x(0 < x < 6), Nb2O5, Bi2O3 or Sb2O3); Group VI metal oxides or sulfides (such as, CrO3, Cr2O3, MoO3, MoS2, WO3 or SeO2); Group VII metal oxides or sulfides (such as MnO2 or Mn2O3); Group VIII metal oxides or sulfides (such as, Fe2O3, FeO, Fe3O4, Ni2O3, NiO, CoO3 or CoO); and / or metal oxides or sulfides represented by the general formula Li x MN y X2 (wherein M and N are each a Group I metal to a Group VIII metal, X is oxygen or sulfur, 0.1 ≤ x ≤ 2, and 0 ≤ y ≤ 1), for example, lithium titanate represented by Li y TiO2 (0 ≤ y ≤ 1), Li 4+y Ti5O 12 (0 ≤ y ≤ 1) or Li 4+y Ti 11 O 20 (0 ≤ y ≤ 1).

[0119] Non-limiting examples of materials capable of doping or undoping lithium may include Si, SiO x (0 < x ≤ 2), Si-Y' alloys (wherein Y' may be an alkali metal, an alkaline earth metal, an element of Group 13, an element of Group 14 other than Si, a transition metal, a rare earth element or a combination thereof), Sn, SnO2, Sn-Y' alloys (wherein Y' may be an alkali metal, an alkaline earth metal, an element of Group 13, an element of Group 14 other than Sn, a transition metal, a rare earth element or a combination thereof) and / or a mixture of at least one of them with SiO2. The element Y' may be magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), scandium (Sc), yttrium (Y), titanium (Ti), zirconium (Zr), hafnium (Hf), (Rf), vanadium (V), niobium (Nb), tantalum (Ta), thorium (Db), chromium (Cr), molybdenum (Mo), tungsten (W), (Sg), technetium (Tc), rhenium (Re), (Bh), iron (Fe), lead (Pb), ruthenium (Ru), osmium (Os), (Hs), rhodium (Rh), iridium (Ir), palladium (Pd), platinum (Pt), copper (Cu), silver (Ag), gold (Au), zinc (Zn), cadmium (Cd), boron (B), aluminum (Al), gallium (Ga), tin (Sn), indium (In), titanium (Ti), germanium (Ge), phosphorus (P), arsenic (As), antimony (Sb), bismuth (Bi), sulfur (S), selenium (Se), tellurium (Te), polonium (Po) or a combination thereof.

[0120] The material capable of reversibly inserting and extracting lithium ions may be a carbonaceous material, and any carbonaceous negative electrode active material generally used in the manufacture of lithium secondary batteries may be used. The carbonaceous material may be, for example, crystalline carbon, amorphous carbon, and mixtures thereof. Non-limiting examples of crystalline carbon may include natural graphite, which is shapeless, plate-shaped, flaky, spherical and / or fibrous; and / or artificial graphite, and non-limiting examples of amorphous carbon may include soft carbon (carbon calcined at low temperature), hard carbon, mesophase pitch carbide, and / or calcined coke.

[0121] Non-limiting examples of the conductive polymer may include disulfide materials, polypyrrole, polyaniline, polyparaphenylene, polyacetylene, and / or polyacene materials.

[0122] The same conductive agent, binder, and solvent as those in the above-mentioned positive electrode active material composition can be used for the negative electrode active material composition.

[0123] The amount of the negative electrode active material, the conductive agent, the binder and the solvent may be within the range generally used in the manufacture of lithium secondary batteries in the relevant field. In some embodiments, according to the intended use and / or structure of the lithium secondary battery, one or more of the conductive agent, the binder and the solvent may be omitted (e.g., not included).

[0124] The negative electrode active material may further include a thickener. The thickener may include one or more of carboxymethyl cellulose (CMC), carboxyethyl cellulose, starch, regenerated cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, styrene butadiene rubber (SBR) and polyvinyl alcohol. For example, CMC may be used as a thickener.

[0125] If necessary, the negative electrode active material may further include a conductive agent. The conductive agent is not particularly limited, and may be any material that can be used as a material having conductivity without causing chemical changes in the art, and non-limiting examples thereof may include: carbonaceous materials (such as carbon black, acetylene black, Ketjen black, channel carbon black, furnace carbon black, lamp carbon black, graphite (such as natural graphite and / or artificial graphite) and / or thermal carbon black); conductive fibers (such as carbon fibers and / or metal fibers); metal powders (such as carbon fluoride powders, aluminum powders and / or nickel powders); conductive whiskers (such as zinc oxide and / or potassium titanate); conductive metal oxides (such as titanium oxide); and / or any other conductive material (such as polyphenylene derivatives). The conductive agent may be carbon black, for example, carbon black having an average particle diameter of tens of nanometers.

[0126] Next, prepare a separator inserted between the positive electrode and the negative electrode. The separator may be any suitable separator generally used in lithium secondary batteries. A separator having low resistance and / or excellent electrolyte retention capacity for the migration of ions in the electrolyte (e.g., lithium ion diffusion) may be used. Non-limiting examples of separators include glass fiber, polyester, polyethylene, polypropylene, polytetrafluoroethylene (PTFE) and / or combinations thereof, each of which may be in the form of a nonwoven or textile fabric. For example, a rollable separator including polyethylene and / or polypropylene may be used for lithium ion batteries, and a separator having good organic electrolyte solution retention capacity may be used for lithium ion polymer batteries. For example, a separator may be manufactured in the following manner:

[0127] The polymer resin, filler and solvent may be mixed together to prepare a separator composition. The separator composition may be directly coated on the electrode and then dried to form a separator. In some embodiments, the separator composition may be cast on a support and then dried to form a separator film, which may then be separated from the support and laminated on the electrode to form a separator.

[0128] The polymer resin used in the preparation of the separator is not particularly limited, and any suitable material used as a binder for the electrode plate can be used. Non-limiting examples of the polymer resin used in the preparation of the separator may include vinylidene fluoride / hexafluoropropylene copolymer, polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate and / or one or more mixtures thereof, and / or styrene butadiene rubber polymer, but embodiments are not limited thereto.

[0129] Next, an electrolyte is prepared.

[0130] For example, the electrolyte may be an organic electrolyte. The organic electrolyte solution may be prepared by dissolving a lithium salt in an organic solvent.

[0131] As organic solvent, any suitable material that can be used as organic solvent in the art can be utilized. Non-limiting examples of organic solvent can include propylene carbonate, ethylene carbonate, ethylene fluorocarbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, methyl isopropyl carbonate, dipropyl carbonate, dibutyl carbonate, benzonitrile, acetonitrile, tetrahydrofuran, 2-methyltetrahydrofuran, gamma-butyrolactone, dioxolane, 4-methyldioxolane, N,N-dimethylformamide, dimethylacetamide, dimethyl sulfoxide, dioxane, 1,2-dimethoxyethane, cyclopentane, ethylene dichloride, chlorobenzene, nitrobenzene, diethylene glycol, dimethyl ether and / or its mixture.

[0132] The lithium salt may also be any suitable material that can be used as a lithium salt in the art. Non-limiting examples of lithium salts may include LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiCF3SO3, Li(CF3SO2)2N, Li(FSO2)2N, LiC4F9SO3, LiAlO2, LiAlCl4, LiN(C x F 2x+1 SO2)(C y F 2y+1 SO2) (wherein x and y are each independently a natural number), LiCl, LiI and / or a mixture thereof.

[0133] In some embodiments, the electrolyte may be a solid electrolyte (such as an organic solid electrolyte and / or an inorganic solid electrolyte). When a solid electrolyte is utilized, the solid electrolyte may also serve as a separator.

[0134] Non-limiting examples of the organic solid electrolyte may include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyalginate lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and / or polymers including an ion dissociative group.

[0135] Non-limiting examples of inorganic solid electrolytes may include boron oxide and / or lithium oxynitride, and may be any inorganic solid electrolyte that can be suitably used as a solid electrolyte. The solid electrolyte may be formed on the negative electrode by, for example, sputtering. Non-limiting examples of lithium salts may include Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH and / or Li3PO4-Li2S-SiS2.

[0136] like Fig. 9 , an example lithium secondary battery 1 includes a positive electrode 3, a negative electrode 2, and a separator 4. The positive electrode 3, the negative electrode 2, and the separator 4 may be wound or folded and then placed in a battery case 5. Next, an organic electrolyte solution is injected into the battery case 5 and a cap assembly 6 may seal the battery case 5, thereby completing the lithium secondary battery 1. The battery case 5 may be cylindrical or in the form, rectangular or in the form, or thin film or in the form. For example, the lithium secondary battery 1 may be a thin film type or in the form of a battery. The lithium secondary battery 1 may be a lithium ion secondary battery.

[0137] The separator 4 may be placed between the positive electrode 3 and the negative electrode 2 to form a battery structure. In some embodiments, the battery structure may be stacked in a bi-cell structure and immersed in an organic electrolyte solution, and the resulting product may be placed in a bag and hermetically sealed, thereby completing the manufacture of a lithium ion polymer battery.

[0138] In some embodiments, multiple battery structures can be stacked to form a series battery pack, which can be used in any device requiring high capacity and high output. For example, the battery pack can be used in laptop computers, smart phones and / or electric vehicles.

[0139] Lithium secondary batteries can have excellent or appropriate high temperature cycle characteristics and / or high temperature stability, and therefore can be suitable for medium and large energy storage devices. Lithium secondary batteries can be used as, for example, the power supply of electric vehicles (EVs). Lithium secondary batteries can be suitably used as, for example, the power supply of hybrid electric vehicles (such as, plug-in hybrid electric vehicles (PHEVs)).

[0140] The present disclosure will now be described in more detail through the following examples and comparative examples. However, the examples are provided only as examples, and embodiments of the present disclosure are not limited thereto.

[0141] Preparation of large secondary particles, large crystal particles and small secondary particles

[0142] Preparation Example 1: LiNi with an average particle diameter of 18 μm 0.95 Co 0.04 Al 0.01 Preparation of large secondary particles (particle A) of O2(NCA)

[0143] Al2(SO4)3(H2O) as an aluminum precursor 18 It was mixed with NaOH, NH4OH and water in a reactor to prepare an aluminum precursor aqueous solution.

[0144] NiSO4(H2O)6 as a nickel precursor and CoSO4(H2O)7 as a cobalt precursor were mixed with water to obtain a nickel precursor aqueous solution and a cobalt precursor aqueous solution, respectively.

[0145] The aluminum precursor is added to the reactor, and the nickel precursor aqueous solution and the cobalt precursor aqueous solution are added dropwise thereto to produce a reaction mixture, which is then stirred for 15 hours. The amounts of the nickel precursor, the cobalt precursor and the aluminum precursor are stoichiometrically controlled to have a mixed molar ratio of 95:4:1 in the reaction mixture of nickel, cobalt and aluminum.

[0146] A sodium hydroxide aqueous solution was added dropwise to the reaction mixture to adjust the pH to be within the range of 10 to 12. The obtained precipitate was filtered and then washed to obtain the resulting product, which was then dried at a temperature of 100° C. in a vacuum to prepare Ni as nickel cobalt aluminum hydroxide. 0.95 Co 0.04 Al 0.01 (OH)2 powder.

[0147] Nickel cobalt aluminum hydroxide and a lithium precursor were mixed together in a mortar, and the mixture was put into a furnace, followed by heat treatment at 720° C. for 20 hours using a flow of O 2 , thereby preparing a nickel-based active material. The amounts of nickel cobalt aluminum hydroxide and the lithium precursor were controlled to have a mixing ratio of transition metal to lithium of 1:1.02.

[0148] The nickel active material prepared according to the method is LiNi 0.95 Co 0.04 Al 0.01 O2(NCA), which includes large secondary particles, and the average particle diameter of the large secondary particles is 18 μm.

[0149] Preparation Example 2: Monolithic LiNi with an average particle diameter of 4 μm 0.85 Co 0.14 Al 0.01 Preparation of large O2(NCA) crystal particles (particles B)

[0150] The integrated LiNi 0.85 Co 0.14 Al 0.01 O2(NCA) large crystalline particles, except that the precursor size is controlled by changing the stirring time of the reaction mixture for obtaining nickel cobalt aluminum hydroxide to 30 hours, heat treating at 900°C instead of 720°C, followed by a pulverizing process and then heat treating at 750°C.

[0151] In the large crystalline particles prepared according to this method, the average particle diameter of the integral type or kind of primary particles was about 4 μm. The average particle diameter of the primary particles was measured using a scanning electron microscope (SEM) [FEI Sirion].

[0152] Preparation Example 3: LiNi with an average particle diameter of 4 μm 0.8 Co 0.19 Al 0.01 Preparation of small secondary particles (particles C) of O2(NCA)

[0153] Small secondary LiNi having an average particle diameter of about 4 μm was prepared in substantially the same manner as in Preparation Example 1. 0.8 Co 0.19 Al 0.01 O2(NCA) particles (particles C), except that the heat treatment temperature is controlled to 800°C.

[0154] Preparation Example 4: Preparation of one-piece NCA large crystal particles (particles B) having an average particle diameter of 5 μm

[0155] In substantially the same manner as in Preparation Example 2, a monolithic LiNi nanostructured carbon nanotube having an average particle diameter (D50) of about 5 μm was prepared. 0.85 Co 0.14 Al 0.01 O2(NCA) particles, the difference is that the stirring time is changed to obtain an integrated LiNi 0.85 Co 0.14 Al 0.01 O2(NCA) particles, and the average particle diameter of primary particles in the obtained positive electrode active material was about 5 μm.

[0156] Preparation Example 5: Preparation of one-piece NCA large crystal particles (particles B) having an average particle diameter of 1 μm

[0157] In substantially the same manner as in Preparation Example 2, a monolithic LiNi nanostructured carbon nanotube having an average particle diameter (D50) of about 1 μm was prepared. 0.85 Co 0.14 Al 0.01 O2(NCA) particles, the difference is that the stirring time is changed to obtain an integrated LiNi 0.85 Co 0.14 Al 0.01 O2(NCA) particles, and the average particle diameter of primary particles in the obtained positive electrode active material was about 1 μm.

[0158] Comparative Preparation Example 1: Preparation of one-piece large crystal particles (particles B) having an average particle diameter of 6.4 μm

[0159] One-piece large crystal particles having an average particle diameter of about 6.4 μm were prepared in substantially the same manner as in Preparation Example 4, except that the stirring time was changed so as to obtain one-piece large crystal particles having an average particle diameter of about 6.4 μm.

[0160] Comparative Preparation Example 2: Preparation of one-piece large crystal particles (particles B) having an average particle diameter of 0.5 μm

[0161] One-piece large crystal particles having an average particle diameter of about 0.5 μm were prepared in substantially the same manner as in Preparation Example 4, except that the stirring time was changed so as to obtain one-piece large crystal particles having an average particle diameter of about 0.5 μm.

[0162] Preparation of nickel active materials and lithium secondary batteries

[0163] Example 1

[0164] The LiNi prepared according to Preparation Example 1 and having an average particle diameter of about 18 μm was 0.95 Co 0.04 Al0.01 O2 (NCA) large secondary particles (particles A), one-piece LiNi prepared according to Preparation Example 2 with an average particle diameter of about 4 μm 0.85 Co 0.14 Al 0.01 O2(NCA) large crystal particles (particles B) and LiNi prepared according to Preparation Example 3 with an average particle diameter of about 4 μm 0.8 Co 0.19 Al 0.01 The nickel-based active material was prepared as a positive electrode active material. The mixing weight ratio of particles A, B and C was 80:10:10.

[0165] The positive electrode active material, carbon conductive agent (Super P) and polyvinylidene fluoride (PVDF) binder solution were mixed to prepare active material slurry. In the active material slurry, the mixing weight ratio of the positive electrode active material, conductive agent and binder was 98:1:1. The slurry was coated on a 12 μm thick aluminum current collector using a thick film coating device to have a 36 mg / cm 2 The loading level of , and the resulting product was dried at a temperature of 120° C. for about 1 hour or more, followed by a roll-pressing process to prepare a positive electrode.

[0166] The negative electrode active material slurry was prepared by mixing graphite powder (Nippon Carbon) as a negative electrode active material at a weight ratio of 98:2, and a mixture of styrene butadiene rubber (SBR) and carboxymethyl cellulose (CMC) at a weight ratio of 1:1.

[0167] The prepared negative electrode active material slurry was coated on a 8 μm thick copper foil collector to a density of 19.5 mg / cm 2 The electrode plate in which the coating is completed is dried at a temperature of 100° C. for 1 hour or more, and then subjected to a roll pressing process to produce an electrode having a coating thickness of 1.66 g / cm 3 The density of the mixture is the negative electrode.

[0168] A lithium secondary battery with a capacity of 2,000 mAh was fabricated using a positive electrode, a negative electrode, a polyethylene separator (STAR ​​20, Asahi) and an electrolyte solution in which 1.15 M LiPF6 was dissolved in a mixed solvent of EC (ethylene carbonate), EMC (ethyl methyl carbonate) and DMC (dimethyl carbonate) (volume ratio of 3:3:4).

[0169] Example 2

[0170] A lithium secondary battery was manufactured in substantially the same manner as in Example 1, except that when preparing the nickel-based active material, the mixing weight ratio of the particles A, B, and C was changed to 80:5:15.

[0171] Examples 3 and 4

[0172] Another lithium secondary battery was manufactured in substantially the same manner as in Example 1, except that the large secondary particles LiNi having an average particle diameter of about 18 μm were not used in the preparation of the nickel-based active material. 0.95 Co 0.04 Al 0.01 O2(NCA) (particle A), but rather large secondary particles LiNi with an average particle diameter of about 10 μm were used. 0.95 Co 0.04 Al 0.01 O2(NCA) (particle A) and large secondary particles LiNi with an average particle diameter of about 14 μm 0.95 Co 0.04 Al 0.01 O2(NCA)(Particle A).

[0173] Examples 5 and 6

[0174] Another lithium secondary battery was manufactured in substantially the same manner as in Example 1, except that the integrated LiNi prepared according to Preparation Example 2 and having an average particle diameter of about 4 μm was not used in preparing the nickel-based active material. 0.85 Co 0.14 Al 0.01 O2 (NCA) large crystal particles (particles B), but the one-piece particles LiNi prepared according to Preparation Example 5 with an average particle diameter of about 1 μm 0.85 Co 0.14 Al 0.01 O2 (NCA) large crystal particles (particles B) and the integral particle LiNi having an average particle diameter of about 5 μm prepared according to Preparation Example 4 0.85 Co 0.14 Al 0.01 O2(NCA) large crystal particles (particle B).

[0175] Examples 7 and 8

[0176] Another lithium secondary battery was manufactured in substantially the same manner as in Example 1, except that LiNi having an average particle diameter of about 4 μm was not used in preparing the nickel-based active material. 0.8 Co 0.19 Al 0.01O2(NCA) small secondary particles (particles C), but LiNi with an average particle diameter of about 1 μm 0.8 Co 0.19 Al 0.01 O2(NCA) small secondary particles (particles C) and LiNi with an average particle diameter of about 5 μm 0.8 Co 0.19 Al 0.01 O2(NCA) small secondary particles (particles C).

[0177] Examples 9 to 11

[0178] Another lithium secondary battery was manufactured in substantially the same manner as in Example 1, except that a mixture of large secondary particles (particles A), large crystalline particles (particles B), and small secondary particles (particles C) having the compositions listed in Table 1 were used as positive electrode active materials, respectively.

[0179] Table 1

[0180] data Granule A Granule B Granule C Example 1 <![CDATA[LiNi 0.95 Yes 0.04 Al 0.01 O2]]> <![CDATA[LiNi 0.85 Yes 0.14 Al 0.01 O2]]> <![CDATA[LiNi 0.8 Yes 0.19 Al 0.01 O2]]> Example 9 <![CDATA[LiNi 0.95 Yes 0.04 Al 0.01 O2]]> <![CDATA[LiNi 0.9 Yes 0.085 Al 0.015 O2]]> <![CDATA[LiNi 0.8 Yes 0.19 Al 0.01 O2]]> Example 10 <![CDATA[LiNi 0.95 Yes 0.04 Al 0.01 O2]]> <![CDATA[LiNi 0.9 Yes 0.085 Al 0.015 O2]]> <![CDATA[LiNi 0.95 Yes 0.04 Al 0.01 O2]]> Embodiment 11 <![CDATA[LiNi 0.95 Yes 0.04 Al 0.01 O2]]> <![CDATA[LiNi 0.8 Yes 0.15 Al 0.05 O2]]> <![CDATA[LiNi 0.8 Yes 0.15 Al 0.05 O2]]>

[0181] Comparative Example 1

[0182] A lithium secondary battery was manufactured in substantially the same manner as in Example 1, except that large crystalline particles (integrated particles) including primary particles having an average particle diameter of about 6.4 μm prepared according to Comparative Preparation Example 1 were used as particles B when preparing the nickel-based active material.

[0183] Comparative Example 2

[0184] A lithium secondary battery was manufactured in substantially the same manner as in Example 1, except that the small secondary particles LiNi having an average particle diameter of about 4 μm were not used (included) when preparing the nickel-based active material. 0.8 Co 0.19 Al 0.01 O2(NCA)(Particle C).

[0185] Comparative Example 3

[0186] A lithium secondary battery was manufactured in substantially the same manner as in Example 1, except that large crystalline particles (integrated particles) including primary particles having an average particle diameter of about 0.5 μm prepared according to Comparative Preparation Example 2 were used as particles B when preparing the nickel-based active material.

[0187] Evaluation Example 1: Size Analysis of Primary Particles and Secondary Particles Using a Scanning Electron Microscope (SEM)

[0188] Analysis of SEM images of the nickel-based active material prepared according to Example 1. The equipment used for SEM analysis is commercially available under the model name of Sirion (FEI, USA).

[0189] The results of SEM analysis of Example 1 are shown in Figure 1 middle.

[0190] refer to Figure 1 It was confirmed that the nickel-based active material of Example 1 contained large secondary particles (particles A), large integrated crystal particles (particles B) and small secondary particles (particles C).

[0191] exist Figure 1 In the nickel-based active material shown in FIG. , a SEM image of large crystal particles (eg, having a relatively small diameter) is shown in FIG. Figure 2 The SEM images of the small secondary particles are shown in Figure 3 middle.

[0192] The SEM analysis results of the large secondary particles prepared according to Preparation Example 1 are shown in FIG. 4A to FIG. 4C The SEM analysis results of the large crystal particles prepared according to Preparation Example 2 are shown in Figure 5A and Figure 5B and the SEM analysis results of the small secondary particles prepared according to Preparation Example 3 are shown in Fig. 6A and Figure 6B middle.

[0193] Evaluation Example 2: X-ray diffraction analysis

[0194] XRD analysis was performed on the nickel-based active material prepared according to Example 1. In the XRD analysis, an analysis device Xpert PRO (Philips / Power 3kW) was used.

[0195] The average particle diameter of the primary particles in the nickel-based active material obtained from the XRD analysis results can be calculated by the Scherrer equation using the half-maximum full width of the peak associated with the (003) crystal plane. In the nickel-based active material of Example 1, the average particle diameter of the primary particles constituting the large secondary particles, the large crystal particles, and the small secondary particles is in the range of 50 nm to 70 nm, as derived from the Scherrer equation.

[0196] Evaluation Example 3: Room Temperature Life and Rate Performance

[0197] The lithium secondary batteries manufactured in Examples 1 to 4, 7 and 8 and Comparative Example 1 were charged and discharged under the following conditions.

[0198] The first cycle of charging and discharging was performed as follows: the current was 0.1C until the voltage reached 3.0V to 4.25V, and then the battery was discharged at 0.1C, 0.2C, 0.5C, 1.0C, 2.0C or 3.0C to evaluate the high rate discharge characteristics by the discharge capacity ratio. After a total of 50 additional charge and discharge cycles were performed at 1.0C, the life characteristics were evaluated by the capacity retention rate, and the evaluation results are shown in Table 2.

[0199] During the first cycle, constant current charging was performed with a current of 0.1 C until the voltage reached 4.25 V, and then constant voltage charging was performed until the current reached 0.05 C. The charged single cell was left to rest for about 10 minutes and then constant current discharged with a current of 0.1 C until the voltage reached 3.0 V.

[0200] During the second cycle, constant current charging was performed with a current of 0.2 C until the voltage reached 4.25 V, and then constant voltage charging was performed until the current reached 0.05 C. The charged single cell was left to rest for about 10 minutes and then constant current discharged with a current of 0.2 C until the voltage reached 3.0 V.

[0201] During the third cycle, constant current charging was performed with a current of 0.5 C until the voltage reached 4.25 V, and then constant voltage charging was performed until the current reached 0.05 C. The charged single cell was left to rest for about 10 minutes and then constant current discharged with a current of 0.5 C until the voltage reached 3.0 V.

[0202] During the fourth cycle, constant current charging was performed with a current of 0.5 C until the voltage reached 4.25 V, and then constant voltage charging was performed until the current reached 0.05 C. The charged single cell was left to rest for about 10 minutes and then constant current discharged with a current of 1.0 C until the voltage reached 3.0 V.

[0203] During the fifth cycle, constant current charging was performed with a current of 2.0 C until the voltage reached 4.25 V, and then constant voltage charging was performed until the current reached 0.05 C. The charged single cell was left to rest for about 10 minutes and then constant current discharged with a current of 2.0 C until the voltage reached 3.0 V.

[0204] During the sixth cycle, constant current charging was performed with a current of 3.0 C until the voltage reached 4.25 V, and then constant voltage charging was performed until the current reached 0.05 C. The charged single cell was left to rest for about 10 minutes and then constant current discharged with a current of 3.0 C until the voltage reached 3.0 V.

[0205] After the sixth cycle, in order to evaluate the single cell under 0.5C, 1.0C, 2.0C or 3.0C conditions, constant current charging was performed on each sample single cell with a current corresponding to the above conditions until the voltage reached 4.25V, and then constant voltage charging was performed until the current reached 0.05C. The charged single cell was left to stand for about 10 minutes and then constant current discharged with the corresponding current until the voltage reached 3.0V, and this procedure was repeated 50 times to evaluate the cycle characteristics of the single cell. The cycle characteristics evaluation results are shown in Figure 7 and Table 2.

[0206] Table 2

[0207]

[0208] As indicated in Table 2, the lithium secondary batteries of Examples 1 to 4, 7 and 8 have improved room temperature life characteristics and rate performance compared to the lithium secondary battery of Comparative Example 1. Figure 7 As shown in , the lithium secondary battery of Example 1 has an improved room temperature life compared to the lithium secondary battery of Comparative Example 1. Figure 7 As shown in , the lithium secondary battery of Example 1 has an improved room temperature lifespan compared to the lithium secondary battery of Comparative Example 1.

[0209] Evaluation Example 4: High Temperature Cycle Characteristics

[0210] The lithium secondary batteries prepared in Examples 1 to 4, 7 and 8 and Comparative Examples 1 to 3 were each subjected to constant current charging at 45°C with a current of 0.2C until the voltage reached 4.35V, and then subjected to constant voltage charging until the current reached 0.05C while maintaining a voltage of 4.35V. Subsequently, during the discharge period, the single cell was discharged with a constant current of 0.2C until the voltage reached 3.0V. (Formation Step)

[0211] Next, constant current charging was performed with a current of 0.7 C until the voltage reached 4.35 V, and then constant voltage charging was performed until the current reached 0.05 C while maintaining a voltage of 4.35 V. Subsequently, during discharge, the single cell was discharged with a constant current of 0.5 C until the voltage reached 3.0 V (standard procedure).

[0212] The lithium secondary batteries each having undergone the formation step and the standard step were subjected to constant current charging at 25° C. and 45° C. with a current of 0.5 C until the voltage reached 4.35 V, and then subjected to constant voltage charging until the current reached 0.05 C while maintaining a voltage of 4.35 V. Subsequently, a cycle of discharging with a constant current of 0.5 C during discharge until the voltage reached 3.0 V was repeated 50 times.

[0213] The high temperature cycle characteristics obtained from the results of the charge / discharge cycle test are shown in Figure 8 and Table 3.

[0214] Table 3

[0215] data High temperature cycle life (%) Example 1 91.6 Example 2 90.8 Example 3 93.5 Example 4 91.8 Example 7 90.5 Example 8 91.2 Comparative Example 1 82.3

[0216] like Figure 8 As shown in Table 3, the lithium secondary battery of Example 1 has an improved high temperature life compared to the lithium secondary battery of Comparative Example 1. As confirmed from Table 3, the lithium secondary batteries of Examples 2 to 4, 7 and 8 each have an improved high temperature life compared to the lithium secondary battery of Comparative Example 1.

[0217] Evaluation Example 5: Residual Lithium

[0218] The amount of residual lithium in the nickel-based active materials prepared in Preparation Example 1 and Comparative Preparation Examples 1 and 2 was measured, and the results are shown in Table 4. The residual lithium was measured by a titration method. For example, the positive electrode active material powder was dissolved in water and then titrated with hydrochloric acid to obtain the amount of LiOH and Li2CO3 contained in the nickel-based active material powder. Based on the obtained amount, the amount of LiOH and Li2CO3 remaining on the surface of the positive electrode active material was calculated.

[0219] Table 4

[0220]

[0221] Referring to Table 4, it is confirmed that the nickel-based active material of Preparation Example 1 has a reduced amount of LiOH compared to the nickel-based active material of Comparative Preparation Example 1.

[0222] Evaluation Example 6: Ball Density

[0223] The pellet density (PD) of each of the positive electrode active materials of Examples 1 to 4, 7 and 8 and the positive electrode active material of Comparative Example 1 was analyzed and the results are shown in Table 5.

[0224] Table 5

[0225] data Pellet Density (PD) (g / cc) Example 1 3.55 Example 2 3.52 Example 3 3.17 Example 4 3.34 Example 7 3.63 Example 8 3.48 Comparative Example 1 3.28

[0226] As confirmed from Table 5, the positive electrode active materials of Examples 1, 2, 4, 7, and 8 demonstrated increased pellet density compared to the positive electrode active material of Comparative Example 1. Although the positive electrode active material of Example 3 had a smaller pellet density than the positive electrode active material of Comparative Example 1, the lithium secondary battery including the positive electrode using the positive electrode active material of Example 3 had considerably improved room temperature and high temperature lifespans compared to the lithium secondary battery including the positive electrode using the positive electrode active material of Comparative Example 1.

[0227] The nickel-based active material according to the present disclosure allows electrochemical reactions to become substantially uniform while having excellent capacity characteristics, and thus gas generation can be suppressed by using the nickel-based active material. A lithium secondary battery including a positive electrode containing the nickel-based active material can have improved cycle life characteristics.

[0228] As used herein, the terms "substantially," "about," and similar terms are used as terms of approximation rather than as terms of degree, and are intended to account for the inherent deviations in measured or calculated values ​​that one of ordinary skill in the art will recognize. As used herein, "about" or "approximately" includes the stated value and means within the range of acceptable deviations of the particular value as determined by one of ordinary skill in the art taking into account the measurement in question and the errors associated with the measurement of the particular quantity (i.e., the limitations of the measurement system). For example, "about" may mean within one or more standard deviations of the stated value, or within ±30%, ±20%, ±10%, or ±5% of the stated value.

[0229] Any numerical range described herein is intended to include all subranges of the same numerical precision contained within the described range. For example, the range of "1.0 to 10.0" is intended to include between the described minimum value 1.0 and the described maximum value 10.0 (and including 1.0 and 10.0), that is, all subranges with a minimum value equal to or greater than 1.0 and a maximum value equal to or less than 10.0, such as, for example, 2.4 to 7.6. Any maximum numerical limit described herein is intended to include all lower numerical limits contained therein, and any minimum numerical limit described in this specification is intended to include all higher numerical limits contained therein. Therefore, the applicant reserves the right to amend this specification (including claims) to explicitly describe any subranges contained within the range explicitly described herein.

[0230] It should be understood that the embodiments described herein should be considered in a descriptive sense only and not for limiting purposes. The description of features or aspects in each embodiment should generally be considered to be applicable to other similar features or aspects in other embodiments. Although one or more embodiments have been described with reference to the accompanying drawings, it will be understood by those of ordinary skill in the art that various changes in form and detail may be made therein without departing from the spirit and scope of the present disclosure as defined by the appended claims and their equivalents.

Claims

1. A nickel-based active material having 80 mol % or more of nickel relative to a metal element other than lithium, The nickel active material comprises: i) large secondary particles, the large secondary particles having a size in the range of 10 μm to 20 μm and each comprising an aggregate of primary particles having a size of 1 μm or less; ii) large crystalline particles, the large crystalline particles comprising primary particles having a size in the range of 1 μm to 5 μm, wherein the large crystalline particles are each an integral particle or each have an integral structure; and iii) small secondary particles, the small secondary particles having a size in the range of 1 μm to 7 μm and each comprising an aggregate of primary particles having a size of 1 μm or less, wherein based on the total amount of metal elements other than lithium in the nickel-based active material of 100 mol%, the amount of nickel in the large secondary particles is 90 mol% to 99 mol%, the amount of nickel in the large crystalline particles is 80 mol% to 95 mol%, and the amount of nickel in the small secondary particles is 80 mol% to 95 mol%, and the large secondary particles have the highest amount of nickel compared to the large crystalline particles and the small secondary particles. 2 . The nickel-based active material according to claim 1 , wherein a larger amount of nickel is contained in the large secondary particles than in the large crystal particles or in the small secondary particles. 3 . The nickel-based active material according to claim 2 , wherein the amount of nickel in the large crystal particles is greater than the amount of nickel in the small secondary particles.

4. The nickel-based active material according to claim 1, based on the total amount of 100wt% of the large secondary particles, the large crystal particles and the small secondary particles, the amount of the large crystal particles is 5wt% to 25wt%, and based on the total amount of 100wt% of the large secondary particles, the large crystal particles and the small secondary particles, the amount of the small secondary particles is 5wt% to 25wt%.

5. The nickel-based active material according to claim 1, wherein: The nickel-based active material is a compound represented by Formula 1, a compound represented by Formula 2, or a combination thereof: Formula 1 Li x Ni 1-y Co y O 2-z X z , wherein, in Formula 1, 0.9 ≤ x ≤ 1.2, 0 < y ≤ 0.2, 0 ≤ z ≤ 0.5, and 0.8 ≤ 1 - y < 1, and X is F, S, P, or a combination thereof, and Formula 2 Li x Ni 1-y-z Co y M z O 2-a X a , wherein, in Formula 2, 0.9 ≤ x ≤ 1.2, 0 < y < 0.5, 0.8 ≤ 1 - y - z < 1, 0 ≤ z ≤ 0.5, 0 < y + z ≤ 0.2, and 0 ≤ a < 2, M is Ni, Co, Mn, Mg, Ca, Sr, Ba, Ti, Zr, Nb, Mo, W, Zn, Al, Si, Cr, Fe, V, a rare earth element, or a combination thereof, and X is F, S, P, or a combination thereof.

6. The nickel-based active material according to claim 1, wherein: The nickel-based active material is a compound represented by Formula 3, a compound represented by Formula 4, or a combination thereof: Formula 3 Li x Co a Ni b Mr c O2, wherein, in Formula 3, 0.9 < x < 1.2, 0 < a < 0.5, 0.8 ≤ b < 1, 0 < c < 0.5, and a + b + c = 1, and Formula 4 Li x Co a Ni b Al c O2, wherein, in Formula 4, 0.9 < x < 1.2, 0 < a < 0.5, 0.8 ≤ b < 1, 0 < c < 0.5, and a + b + c = 1.

7. The nickel-based active material according to claim 1, wherein: In the X-ray diffraction analysis of the nickel-based active material, the full width at half maximum of the (003) plane peak is 0.120° to 0.270°, the full width at half maximum of the (104) plane peak is 0.120° to 0.270°, and the interval between the (108) plane peak and the (110) plane peak is 0.1° to 0.5°. 8 . A positive electrode comprising the nickel-based active material according to claim 1 . 9 . A lithium secondary battery comprising the positive electrode according to claim 8 , a negative electrode, and an electrolyte between the positive electrode and the negative electrode.