Preparation method of unipolar resistive random access memory based on one-dimensional zinc selenide nanostructure

By using zinc selenide one-dimensional nanostructure and weak acidic solution processing technology in resistive switching memory, the problems of high voltage and poor stability in the existing technology are solved, and a unipolar resistive switching memory with low operating voltage and high stability is realized. , with fast resistive switching speed and unipolar conductive characteristics.

CN114447218BInactive Publication Date: 2024-10-15WENZHENG COLLEGE OF SOOCHOW UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011231818.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-11-06
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing resistive switching memories require a large voltage when working for the first time, making the voltage incompatible with the semiconductor industry, and the formation process of conductive filaments is uncontrollable, resulting in poor device stability.

Method used

A unipolar resistive switching memory based on the one-dimensional zinc selenide nanostructure is used. The zinc selenide one-dimensional nanostructure is formed on the substrate, and a double electrode layer and a single electrode layer are formed at both ends, and placed in a weakly acidic solution. Clean and dry at a preset time, or form a modified material film containing active metal elements on the surface, and then place it in a weak acidic solution again to reduce the operating voltage and improve stability.

Benefits of technology

It achieves low operating voltage, fast resistive switching speed and unipolar conductive characteristics, reduces the electroforming voltage during first operation, improves the stability of the memory, and simplifies the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114447218B_ABST
    Figure CN114447218B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a unipolar resistive random access memory based on a one-dimensional zinc selenide nanostructure. The preparation method comprises the following steps: providing a substrate; forming a one-dimensional zinc selenide nanostructure on the substrate; forming a double electrode layer and a single electrode layer at both ends of the one-dimensional zinc selenide nanostructure to obtain a unipolar resistive random access memory blank, wherein the double electrode layer comprises an active metal electrode layer in contact with the one-dimensional zinc selenide nanostructure; placing the unipolar resistive random access memory blank in a weak acid solution for a preset time, washing and drying to obtain a unipolar resistive random access memory. The preparation method of the present invention is used to obtain a unipolar resistive random access memory based on a one-dimensional zinc selenide nanostructure having the characteristics of low operating voltage, fast resistive random access speed, and unipolar conductivity. In addition, by selecting a weak acid solution and controlling the treatment time of the weak acid solution, the electric forming voltage required for the first operation of the resistive random access memory is further reduced, and the stability of the resistive random access memory is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of unipolar resistive random access memory, and in particular to a method for preparing a unipolar resistive random access memory based on a zinc selenide one-dimensional nanostructure. Background Art

[0002] Resistive random access memory has a simple structure and excellent storage performance, and is an ideal candidate for the next generation of high-density memory devices. At present, there are still many key issues in resistive random access memory that need to be solved in terms of power consumption control, integrated assembly, and flexible anti-bending.

[0003] The current commercial memory is a three-terminal floating gate non-volatile memory based on field effect transistors (FETs). In comparison, resistive random access memory has a two-terminal structure, lower operating voltage, fast read and write speed, lower manufacturing cost, lower power consumption and higher storage density. In resistive random access memory, the most common structure is the metal-insulator-metal structure, in which the three materials serve as active electrodes, solid dielectrics and counter electrodes respectively. By controlling the bias applied to the device, the formation and breaking of the conductive filaments in the resistive random access memory can be controlled, thereby controlling the "on" and "off" of the conductive state of the device. During the operation of the device, the conductive filaments are always in a critical state on the verge of formation and breaking, and only a small bias voltage needs to be applied to control the device switch.

[0004] However, when the device is first operated, the formation of the conductive filaments in the device is a process from scratch, which requires a large positive bias to be applied to the active metal electrode for a long time to oxidize the active electrode and make the active metal cations migrate to the cathode, and then reduce them to metal atoms near the counter electrode, finally forming conductive filaments. However, large bias is incompatible with the semiconductor industry, and the formation process of conductive filaments is uncontrollable, which will lead to large differences between individual devices. Summary of the invention

[0005] The inventors of the present invention have found that semiconductor materials can be used to replace insulator materials in resistive random access memory. Semiconductor-based resistive random access memory has unipolar conductivity, which is beneficial to avoid the generation of sneak current, and is thus used for the integration of resistive random access memory. In addition, by utilizing the photoelectric properties of semiconductor materials, the photoelectric response function and the electronic storage function can be integrated into one device at the same time to construct a non-volatile photoelectric random access memory. The one-dimensional nanostructure of zinc selenide has excellent photoelectric properties and anti-bending ability. Active metal ions (copper ions or silver ions) have a faster migration speed in zinc selenide. Therefore, if a resistive random access memory is constructed based on a one-dimensional nanostructure of zinc selenide, it is expected to obtain characteristics such as low operating voltage, fast resistive switching speed, and unipolar conductivity. However, there is currently no report on a unipolar resistive random access memory based on a one-dimensional nanostructure of zinc selenide.

[0006] An object of the present invention is to provide a method for preparing a unipolar resistive random access memory based on a one-dimensional zinc selenide nanostructure, thereby preparing a new resistive random access memory having the characteristics of low operating voltage, fast resistive random access speed, unipolar conductivity, etc.

[0007] A further object of the present invention is to solve the technical problem in the prior art that when the resistive memory works for the first time, a large voltage (i.e., an electroforming voltage) needs to be applied to the active metal electrode for a long time, which causes the large voltage to be incompatible with the semiconductor industry and the poor stability of the resistive memory.

[0008] In particular, the present invention provides a method for preparing a unipolar resistive random access memory based on a one-dimensional zinc selenide nanostructure, comprising the following steps:

[0009] providing a substrate;

[0010] forming a zinc selenide one-dimensional nanostructure on the substrate;

[0011] Forming a double electrode layer and a single electrode layer at both ends of the zinc selenide one-dimensional nanostructure respectively to obtain a unipolar resistive random access memory blank, wherein the double electrode layer includes an active metal electrode layer in contact with the zinc selenide one-dimensional nanostructure;

[0012] The unipolar resistive random access memory blank is placed in a weakly acidic solution for a preset time, cleaned and dried to obtain a unipolar resistive random access memory.

[0013] Optionally, the pH value of the weakly acidic solution is any value in the range of 4-6.5, and the preset time is any value in the range of 1s-60s.

[0014] Optionally, the weak acid is selected from a combination of one or more of hydrochloric acid, sulfuric acid, nitric acid, acetic acid and molybdic acid.

[0015] Optionally, the thickness of the active metal electrode layer is 2nm-6nm;

[0016] The material of the active metal electrode layer is copper or silver.

[0017] Optionally, another electrode layer of the double electrode layer is formed on another surface of the active metal electrode layer opposite to the surface in contact with the zinc selenide one-dimensional nanostructure, and has a thickness in the range of 30-200 nm;

[0018] Optionally, the thickness of the single electrode layer is any value in the range of 30-200 nm.

[0019] In particular, the present invention also provides a method for preparing a unipolar resistive random access memory based on a one-dimensional zinc selenide nanostructure, comprising the following steps:

[0020] providing a substrate;

[0021] forming a zinc selenide one-dimensional nanostructure on the substrate;

[0022] Forming a first electrode layer and a second electrode layer at two ends of the zinc selenide one-dimensional nanostructure respectively to obtain a unipolar resistive random access memory blank;

[0023] forming a modification material film containing active metal elements on the surface of the unipolar resistive random access memory blank;

[0024] The unipolar resistive memory blank formed with the modification material film is placed in a weak acid solution for a preset time, cleaned and dried to obtain a unipolar resistive memory.

[0025] Optionally, the pH value of the weakly acidic solution is any value in the range of 4-6.5, and the preset time is any value in the range of 1s-60s.

[0026] Optionally, the weak acid is selected from a combination of one or more of hydrochloric acid, sulfuric acid, nitric acid, acetic acid and molybdic acid.

[0027] Optionally, the active metal element is selected to be copper or silver;

[0028] Optionally, the modification material film is a copper film or a cuprous oxide film.

[0029] Optionally, the thickness of the modification material film is 2nm-6nm.

[0030] According to the solution of the present invention, a one-dimensional zinc selenide nanostructure is formed on a substrate, and a double electrode layer and a single electrode layer are formed at both ends of the one-dimensional zinc selenide nanostructure, and the nanostructure is immersed in a weak acid solution for a preset time, thereby obtaining a unipolar resistive random access memory based on a one-dimensional zinc selenide nanostructure with characteristics such as low operating voltage, fast resistive random access speed, and unipolar conductivity. Prior to the present application, those skilled in the art did not propose or realize that a resistive random access memory with characteristics such as low operating voltage, fast resistive random access speed, strong stability, and unipolar conductivity can be made based on a one-dimensional zinc selenide nanostructure. Moreover, the resistive random access memory can have the characteristics of low operating voltage and high stability, thanks to the important step of processing the unipolar resistive random access memory blank by a weak acid solution. In addition, the preparation method is simple in process and has high reliability.

[0031] Furthermore, by selecting a weak acid solution and controlling the time of treatment with the weak acid solution, the electric forming voltage required for the first operation of the resistive random access memory is further reduced, and the stability of the resistive random access memory is further improved.

[0032] Similarly, by forming a zinc selenide one-dimensional nanostructure on a substrate, and forming a first electrode layer and a second electrode layer at both ends of the zinc selenide one-dimensional nanostructure, a modified material film containing active metal elements is formed on the device surface, and then the device is placed in a weakly acidic solution and soaked for a preset time, thereby obtaining a unipolar resistive random access memory based on a zinc selenide one-dimensional nanostructure with characteristics such as low operating voltage, fast resistive random access speed, and unipolar conductivity. Prior to the present application, those skilled in the art did not propose or realize that a resistive random access memory with characteristics such as low operating voltage, fast resistive random access speed, strong stability, and unipolar conductivity can be made based on a zinc selenide one-dimensional nanostructure. Moreover, the resistive random access memory can have the characteristics of low operating voltage and high stability, thanks to the important step of processing the unipolar resistive random access memory blank by a weakly acidic solution. In addition, the preparation method is simple in process and has high reliability.

[0033] Based on the following detailed description of specific embodiments of the present invention in conjunction with the accompanying drawings, those skilled in the art will become more aware of the above and other objects, advantages and features of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Hereinafter, some specific embodiments of the present invention will be described in detail in an exemplary and non-limiting manner with reference to the accompanying drawings. The same reference numerals in the accompanying drawings indicate the same or similar components or parts. It should be understood by those skilled in the art that these drawings are not necessarily drawn to scale. In the accompanying drawings:

[0035] Figure 1 A schematic flow chart of a method for preparing a unipolar resistive random access memory based on a zinc selenide one-dimensional nanostructure according to an embodiment of the present invention is shown;

[0036] Figure 2 A schematic flow chart of a method for preparing a unipolar resistive random access memory based on a zinc selenide one-dimensional nanostructure according to another embodiment of the present invention is shown;

[0037] Figure 3 A scanning electron microscope image of a unipolar resistive random access memory according to an embodiment of the present invention is shown;

[0038] Figure 4 An IV curve diagram of a unipolar resistive random access memory according to an embodiment of the present invention is shown;

[0039] Figure 5 A retention characteristic curve diagram of a unipolar resistive memory according to an embodiment of the present invention is shown, wherein data points represent current, data lines represent voltage, and the time of each data point is less than 0.3 s. DETAILED DESCRIPTION

[0040] Figure 1FIG. 1 is a schematic flow chart showing a method for preparing a unipolar resistive random access memory based on a one-dimensional zinc selenide nanostructure according to an embodiment of the present invention. Figure 1 As shown, the preparation method comprises:

[0041] Step S110, providing a substrate;

[0042] Step S120, forming a zinc selenide one-dimensional nanostructure on the substrate;

[0043] Step S130, forming a double electrode layer and a single electrode layer at both ends of the zinc selenide one-dimensional nanostructure respectively to obtain a unipolar resistive random access memory blank, wherein the double electrode layer includes an active metal electrode layer in contact with the zinc selenide one-dimensional nanostructure;

[0044] Step S140 , placing the unipolar resistive random access memory blank in a weak acid solution for a preset time, cleaning and drying to obtain the unipolar resistive random access memory.

[0045] In step S110 , the substrate may be, for example, a silicon oxide substrate.

[0046] In step S120, the one-dimensional zinc selenide nanostructure prepared by the prior art may be transferred to the substrate, wherein the transfer may be performed in a variety of ways, such as contact printing method, solution dispersion method or using a translation stage for transfer.

[0047] In step S130, the double electrode layer refers to two electrode layers stacked up and down. Among them, the double electrode layer includes an active metal electrode layer or other metal electrode layers. The other metal electrode layer refers to the metal material of the electrode layer being different from the metal material of the active metal electrode layer. In one embodiment, the metal material of the active electrode layer is copper or silver. Preferably, the material of the active electrode layer is selected as copper. The thickness of the active metal electrode layer can be, for example, 2nm, 3nm, 4nm, 5nm or 6nm, or any other thickness value in the range of 2-6nm. Among them, the other metal electrode layer can be, for example, a gold, platinum, or palladium electrode layer. The thickness of the other metal electrode layer can be, for example, 30nm, 50nm, 80nm, 100nm, 150nm, 180nm or 200nm, or any other value in the range of 30-200nm.

[0048] The single electrode layer may be, for example, a silver electrode layer. The thickness of the single electrode layer may be, for example, 30 nm, 50 nm, 80 nm, 100 nm, 150 nm, 180 nm or 200 nm, or any other value between 30 and 200 nm. It is worth noting that the single electrode layer material can only be selected as silver material. If it is replaced with other materials, it will affect the unipolar resistive switching characteristics. For example, if the single electrode layer material is gold, the device will always be in a high conductivity state, showing a single resistance characteristic. If the single electrode material is indium, the device will show a bipolar resistive switching characteristic, and neither has the characteristics of unipolar conductivity.

[0049] The method of obtaining the double electrode layer and the single electrode layer comprises the following steps:

[0050] 1) Defining corresponding electrode patterns at both ends of the zinc selenide one-dimensional nanostructure by two photolithography steps;

[0051] 2) A double electrode layer is prepared at the electrode pattern at one end of the zinc selenide one-dimensional nanostructure by physical deposition, and a single electrode layer is prepared at the electrode pattern at the other end of the zinc selenide one-dimensional nanostructure by physical deposition.

[0052] The photolithography method in step 1) can be a method in the prior art, as long as the corresponding electrode pattern can be prepared. The physical deposition method in step 2) can be, for example, an evaporation method. The evaporation method can be thin film evaporation using thermal evaporation, electron beam evaporation or magnetron sputtering evaporation.

[0053] In step S140, the weak acid solution may be, for example, a weak acid solution having a pH value of 4, 5, 6 or 6.5, or any other value between 4 and 6.5. In one embodiment, the weak acid solution may be, for example, a combination of one or more of hydrochloric acid, sulfuric acid, nitric acid, acetic acid and molybdic acid. The preset time may be, for example, 1s, 5s, 10s, 20s, 30s, 40s, 50s or 60s, or any other value between 1s and 60s.

[0054] According to the solution of the present invention, a one-dimensional zinc selenide nanostructure is formed on a substrate, and a double electrode layer and a single electrode layer are formed at both ends of the one-dimensional zinc selenide nanostructure, and the nanostructure is immersed in a weak acid solution for a preset time, thereby obtaining a unipolar resistive random access memory based on a one-dimensional zinc selenide nanostructure with characteristics such as low operating voltage, fast resistive random access speed, and unipolar conductivity. Prior to the present application, those skilled in the art did not propose or realize that a resistive random access memory with characteristics such as low operating voltage, fast resistive random access speed, strong stability, and unipolar conductivity can be made based on a one-dimensional zinc selenide nanostructure. Moreover, the resistive random access memory can have the characteristics of low operating voltage and high stability, thanks to the important step of processing the unipolar resistive random access memory blank by a weak acid solution. In addition, the preparation method is simple in process and has high reliability.

[0055] In addition, by selecting a weak acid solution and controlling the time of treatment with the weak acid solution, the electric forming voltage required for the first operation of the resistive memory can be further reduced, and the stability of the resistive memory can be further improved. In addition, the parameters involved in the embodiments of the present invention need to be combined with the specific processes and materials corresponding to each step, and a single material layer and the corresponding parameters should not be separated from other steps. Each step and the corresponding parameters are closely related and jointly determine whether a unipolar resistive memory with the aforementioned performance can be finally obtained.

[0056] Figure 2 FIG. 2 is a schematic flow chart showing a method for preparing a unipolar resistive random access memory based on a one-dimensional zinc selenide nanostructure according to another embodiment of the present invention. Figure 2 As shown, the preparation method comprises:

[0057] Step S210, providing a substrate;

[0058] Step S220, forming a zinc selenide one-dimensional nanostructure on the substrate;

[0059] Step S230, forming a first electrode layer and a second electrode layer at two ends of the zinc selenide one-dimensional nanostructure respectively to obtain a unipolar resistive random access memory blank;

[0060] Step S240, forming a modification material film containing active metal elements on the surface of the unipolar resistive random access memory blank;

[0061] Step S250 , placing the unipolar resistive memory blank with the modified material film formed thereon into a weakly acidic solution for a preset time, cleaning and drying to obtain the unipolar resistive memory.

[0062] In step S210 , the substrate may be, for example, a silicon oxide substrate.

[0063] In step S220, the one-dimensional zinc selenide nanostructure prepared by the prior art may be transferred to the substrate, wherein the transfer may be performed in a variety of ways, such as a sliding method, a solution dispersion method, or a transfer stage.

[0064] In step S230, the first electrode layer may be, for example, a gold electrode layer, and the material of the second electrode layer may be, for example, a silver electrode layer. The thickness of the first electrode layer and the second electrode layer may be, for example, 30 nm, 50 nm, 80 nm, 100 nm, 150 nm, 180 nm or 200 nm, or any other value between 30 and 200 nm.

[0065] The method of obtaining the first electrode layer and the second electrode layer comprises the following steps:

[0066] 1) Defining corresponding electrode patterns at both ends of the zinc selenide one-dimensional nanostructure by two photolithography steps;

[0067] 2) A first electrode layer is prepared at the electrode pattern at one end of the zinc selenide one-dimensional nanostructure by physical deposition, and a second electrode layer is prepared at the electrode pattern at the other end of the zinc selenide one-dimensional nanostructure by physical deposition.

[0068] The photolithography method in step 1) can be a method in the prior art, as long as the corresponding electrode pattern can be prepared. The physical deposition method in step 2) can be, for example, an evaporation method. The evaporation method can be thin film evaporation using thermal evaporation, electron beam evaporation or magnetron sputtering evaporation.

[0069] In step S240, the active metal element is selected as copper or silver. Preferably, the modification material film may be, for example, a copper film or a cuprous oxide film. The thickness of the modification material film may be 2 nm, 3 nm, 4 nm, 5 nm or 6 nm, or any other thickness value between 2 and 6 nm.

[0070] Similarly, by forming a zinc selenide one-dimensional nanostructure on a substrate, and forming a first electrode layer and a second electrode layer at both ends of the zinc selenide one-dimensional nanostructure, a modified material film containing active metal elements is formed on the device surface, and then the device is placed in a weakly acidic solution and soaked for a preset time, thereby obtaining a unipolar resistive random access memory based on a zinc selenide one-dimensional nanostructure with characteristics such as low operating voltage, fast resistive random access speed, and unipolar conductivity. Prior to the present application, those skilled in the art did not propose or realize that a resistive random access memory with characteristics such as low operating voltage, fast resistive random access speed, strong stability, and unipolar conductivity can be made based on a zinc selenide one-dimensional nanostructure. Moreover, the resistive random access memory can have the characteristics of low operating voltage and high stability, thanks to the important step of processing the unipolar resistive random access memory blank by a weakly acidic solution. In addition, the preparation method is simple in process and has high reliability.

[0071] Furthermore, by selecting a weak acid solution and controlling the time of treatment with the weak acid solution, the electric forming voltage required for the first operation of the resistive memory is further reduced, and the stability of the resistive memory is further improved. In addition, the parameters involved in the embodiments of the present invention need to be combined with the specific processes and materials corresponding to each step, and a single material layer and the corresponding parameters should not be separated from other steps. Each step and the corresponding parameters are closely related and jointly determine whether a unipolar resistive memory with the aforementioned performance can be finally obtained.

[0072] The following is described in conjunction with specific embodiments:

[0073] Embodiment 1:

[0074] The method for preparing the unipolar resistive random access memory comprises:

[0075] Step S111, transferring the zinc selenide nanoribbons to the silicon oxide substrate by using a sliding method;

[0076] Step S112: define an electrode pattern at one end of the nanobelt by photolithography, and evaporate a 4nm copper electrode and a 50nm gold electrode in sequence. Define an electrode pattern at the other end of the nanobelt by photolithography again, and evaporate a 50nm silver electrode.

[0077] Step S113, immersing the substrate carrying the device in dilute molybdic acid with a pH of 6 for 10 seconds, taking out the device, cleaning it and drying it, thereby obtaining a unipolar resistive random access memory.

[0078] It can be understood that, in this embodiment, the vapor deposition thickness of the copper electrode is not limited to 4 nm, and can be any value within the range of 2-6 nm.

[0079] Figure 3 A scanning electron microscope image of a unipolar resistive random access memory according to an embodiment of the present invention is shown. Figure 4The IV curve of the unipolar resistive memory according to the embodiment of the present invention is shown. The voltage linear scanning mode is adopted during the test. The voltage scanning range is -1V to 2V and then to -1V. The scanning speed is 0.05V / step. The IV curves of the unipolar resistive memory after the first, fifth, tenth and thirtieth cycles are shown. Figure 4 It can be seen that the device exhibits unipolar storage characteristics with an on / off ratio of 10 4 , and the electric forming voltage value is 1V. In the prior art, for example, the electric forming voltage value of the Ag / a-Si / Au NPs / Au bipolar resistive memory is 5-11V when the device is first turned on, and the turn-on voltage during normal operation is 0.5-1V. Therefore, the electric forming voltage value of the device when it is first turned on is obviously greater than the turn-on voltage value during normal operation, and the electric forming voltage value of the device when it is first turned on is relatively high. In the present application, the voltage value after normal operation is equal to or substantially equal to the turn-on voltage value, and the turn-on voltage value is lower.

[0080] Figure 5 FIG. 4 shows a retention characteristic curve diagram of a unipolar resistive memory according to an embodiment of the present invention. Figure 5 It can be seen that the unipolar resistive memory has strong stability, and by checking the time of applying the write and erase voltages, it can be seen that the time for each voltage data point is <0.3s, which shows that the device has the characteristic of fast resistive switching speed.

[0081] Embodiment 2:

[0082] The method for preparing the unipolar resistive random access memory comprises:

[0083] Step S211, transferring the zinc selenide nanoribbons to the silicon oxide substrate by using a sliding method;

[0084] Step S212: Define the electrode pattern at one end of the nanobelt by photolithography, and evaporate a 50nm gold electrode. Define the electrode pattern at the other end of the nanobelt by photolithography again, and evaporate a 50nm silver electrode.

[0085] Step S213, evaporating a 4 nm copper film on the surface of the nanobelt;

[0086] Step S214, immerse the substrate carrying the device in dilute molybdic acid with a pH of 6 for 10 seconds, take out, clean and dry the device.

[0087] It can be understood that, in this embodiment, the evaporation thickness of the copper film is not limited to 4 nm, and can be any value within the range of 2-6 nm.

[0088] Embodiment 3:

[0089] The method for preparing the unipolar resistive random access memory comprises:

[0090] Step S311, transferring the zinc selenide nanoribbons to the silicon oxide substrate by using a sliding method;

[0091] Step S312: Define the electrode pattern at one end of the nanobelt by photolithography, and evaporate a 50nm gold electrode. Define the electrode pattern at the other end of the nanobelt by photolithography again, and evaporate a 50nm silver electrode.

[0092] Step S313, evaporating a 4 nm thick cuprous oxide film on the surface of the nanobelt;

[0093] Step S314, immerse the substrate carrying the device in dilute molybdic acid with a pH of 6 for 10 seconds, take out, clean and dry the device.

[0094] It can be understood that, in this embodiment, the vapor-deposited thickness of the cuprous oxide film is not limited to 4 nm, and can be any value within the range of 2-6 nm.

[0095] In the above embodiments, it is not limited to the values ​​defined in Examples 1 to 3. For example, the one-dimensional nanostructure of zinc selenide can be a zinc selenide nanowire, a zinc selenide nanobelt or a zinc selenide nanotube. The method for transferring the one-dimensional nanostructure of zinc selenide can be a sliding method, a solution dispersion method or a displacement stage. The thickness of the evaporated gold electrode and the silver electrode can be any value in the range of 30-200nm. The evaporation method of the electrode material and the surface modification material can be thermal evaporation, electron beam evaporation or magnetron sputtering evaporation. The weak acid solution used can be hydrochloric acid, sulfuric acid, nitric acid, acetic acid or molybdic acid, etc. The pH value of the weakly acidic solution can be any value in the range of 4-6.5. The immersion time can be any value in the range of 1-60s.

[0096] At this point, those skilled in the art should recognize that, although multiple exemplary embodiments of the present invention have been shown and described in detail herein, many other variations or modifications that conform to the principles of the present invention can still be directly determined or derived based on the content disclosed in the present invention without departing from the spirit and scope of the present invention. Therefore, the scope of the present invention should be understood and recognized as covering all these other variations or modifications.

Claims

1. A method for preparing a unipolar resistive random access memory based on a one-dimensional zinc selenide nanostructure, characterized in that: The steps include: providing a substrate; forming a zinc selenide one-dimensional nanostructure on the substrate; Forming a double electrode layer and a single electrode layer at both ends of the zinc selenide one-dimensional nanostructure respectively to obtain a unipolar resistive random access memory blank, wherein the double electrode layer includes an active metal electrode layer in contact with the zinc selenide one-dimensional nanostructure; Placing the unipolar resistive random access memory blank in a weakly acidic solution for a preset time, washing and drying to obtain a unipolar resistive random access memory; The material of the active electrode layer is copper or silver, and the material of the single electrode layer is silver.

2. The method for preparing a unipolar resistive random access memory according to claim 1, characterized in that: The pH value of the weakly acidic solution is any value in the range of 4-6.5, and the preset time is any value in the range of 1s-60s.

3. The method for preparing a unipolar resistive random access memory according to claim 2, characterized in that: The weak acid is selected from one or more of hydrochloric acid, sulfuric acid, nitric acid, acetic acid and molybdic acid.

4. The method for preparing a unipolar resistive random access memory according to claim 2, characterized in that: The thickness of the active metal electrode layer is 2nm-6nm.

5. The method for preparing a unipolar resistive random access memory according to any one of claims 1 to 4, characterized in that: The other electrode layer of the double electrode layer is formed on the other surface of the active metal electrode layer opposite to the surface in contact with the zinc selenide one-dimensional nanostructure, and has a thickness in the range of 30-200 nm.

6. The method for preparing a unipolar resistive random access memory according to claim 5, characterized in that: The thickness of the single electrode layer is any value in the range of 30-200 nm.

7. A method for preparing a unipolar resistive random access memory based on a one-dimensional zinc selenide nanostructure, characterized in that: The steps include: providing a substrate; forming a zinc selenide one-dimensional nanostructure on the substrate; Forming a first electrode layer at one end of the zinc selenide one-dimensional nanostructure and a second electrode layer at the other end to obtain a unipolar resistive random access memory blank; forming a modification material film containing active metal elements on the surface of the unipolar resistive random access memory blank; Placing the unipolar resistive memory blank formed with the modification material film in a weak acid solution for a preset time, washing and drying to obtain a unipolar resistive memory; The first electrode layer is a gold electrode layer, and the second electrode layer is a silver electrode layer.

8. The preparation method according to claim 7, characterized in that: The pH value of the weakly acidic solution is any value in the range of 4-6.5, and the preset time is any value in the range of 1s-60s.

9. The preparation method according to claim 8, characterized in that: The weak acid is selected from one or more of hydrochloric acid, sulfuric acid, nitric acid, acetic acid and molybdic acid.

10. The method for preparing a unipolar resistive random access memory according to any one of claims 7 to 9, characterized in that: The active metal element is selected from copper or silver.

11. The method for preparing a unipolar resistive random access memory according to claim 10, characterized in that: The modification material film is a copper film or a cuprous oxide film.

12. The method for preparing a unipolar resistive random access memory according to claim 10, characterized in that: The thickness of the modified material film is 2nm-6nm.