Electrochemical devices and electronic devices

By combining a first particle with a porous structure and a second particle with no or small pores, the structure and composition of the positive electrode active material are optimized, which solves the shortcomings of lithium-ion batteries in high-temperature cycling and rate performance, and achieves an overall performance improvement of the battery.

CN114497512BActive Publication Date: 2024-11-01NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210140842.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-12-14
Publication Date
2024-11-01
Estimated Expiration
2040-12-14

AI Technical Summary

Technical Problem

In the existing technology, using primary or secondary particles alone as positive electrode active materials cannot meet the comprehensive performance requirements of lithium-ion batteries, especially in terms of high-temperature cycle performance, high-temperature storage performance and rate performance.

Method used

A combination of a first particle with a porous structure and a second particle with no pores or extremely small pores is used as the positive electrode active material. The area ratio and particle size range are controlled, and the electrolyte composition is optimized by adjusting the element coating on the particle surface to form a layered positive electrode material.

Benefits of technology

It achieves a balance between impedance in the initial discharge stage, cathode specific capacity, high-temperature cycle performance, low-temperature discharge capability and rate performance of lithium-ion batteries, thereby improving the overall performance of the batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114497512B_ABST
    Figure CN114497512B_ABST
Patent Text Reader

Abstract

The present application relates to an electrochemical device and an electronic device. Specifically, the present application provides an electrochemical device, which includes: a positive electrode and an electrolyte, the positive electrode includes a positive electrode current collector and a positive electrode active material layer, the positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes a first particle and a second particle, wherein the first particle has a pore of a specific size, the pore size of the second particle is less than 1 μm, and the first particle and the second particle have a specific area ratio. The electrochemical device of the present application has good initial discharge impedance, positive electrode gram capacity, high temperature cycle performance, high temperature storage performance, low temperature discharge capacity and rate performance, and can achieve balanced comprehensive performance.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an application with an application date of December 14, 2020, application number 202011478731.9, and invention name “Electrochemical Device and Electronic Device”. Technical Field

[0002] The present application relates to the field of energy storage, and in particular to an electrochemical device and an electronic device. Background Art

[0003] Electrochemical devices (e.g., lithium-ion batteries) are widely used in wearable devices, smart phones, drones, electric vehicles, large-scale energy storage devices, etc. due to their advantages such as high energy density, long cycle life and no memory effect. They have become the most promising new green chemical power source in the world today.

[0004] The performance of electrochemical devices mainly depends on the characteristics of the positive electrode, negative electrode, electrolyte and separator. The active material in the electrode is one of the important factors affecting the electrode performance. Using primary particles alone as positive electrode active materials cannot meet the rate performance required by electrochemical devices. Using secondary particles alone as positive electrode active materials cannot meet the high temperature cycle performance and high temperature storage performance of electrochemical devices. How to combine primary and secondary particles to balance the comprehensive performance of electrochemical devices has become one of the research and development directions.

[0005] In view of the above, there is a real need to provide electrochemical devices and electronic devices with improved performance balance. Summary of the invention

[0006] The present application attempts to solve at least one problem existing in the related art to at least some extent by providing a positive electrode material having a layered structure.

[0007] According to one aspect of the present application, the present application provides an electrochemical device, which includes: a positive electrode and an electrolyte, the positive electrode includes a positive electrode current collector and a positive electrode active material layer, the positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes a first particle and a second particle, wherein: the first particle has a pore, the size of the pore is 1μm to 8μm; the pore size of the second particle is less than 1μm; the ratio a of the area of ​​the first particle to the area of ​​the second particle is not greater than 9.

[0008] According to an embodiment of the present application, the average particle size of the first particles is 7 μm to 15 μm; the average particle size of the second particles is 1 μm to 7 μm, excluding 7 μm.

[0009] According to an embodiment of the present application, the first particles include primary particles, and an average particle size of the primary particles is no greater than 3 μm.

[0010] According to an embodiment of the present application, the first particles include at least 5 primary particles having a particle size of 0.5 μm or more.

[0011] According to an embodiment of the present application, the first particle and the second particle each independently contain formula Li b Ni x Co y M1 1-x-y-z M2 z O 2 A compound, wherein: M1 includes at least one of Mn or Al; M2 includes at least one of Mg, Al, Ti, Zr, La, Y, Sr or Ce; 0.1≤b≤1.1; 0.5≤x<1; 0≤y<0.5; and 0≤z≤0.01.

[0012] According to an embodiment of the present application, the first particle contains boron element. The boron content in the surface area of ​​the first particle is higher than that in the central area.

[0013] According to an embodiment of the present application, the first particles and the second particles contain boron, and the boron content of the first particles is greater than the boron content of the second particles.

[0014] According to an embodiment of the present application, based on the total weight of the positive electrode active material layer, the weight percentage c of the positive electrode active material and the ratio a satisfy the following relationship: c≤0.02×a / (a+1)+0.97.

[0015] According to an embodiment of the present application, the positive electrode active material layer has a porosity of 10% to 50%.

[0016] According to an embodiment of the present application, the compaction density of the positive electrode active material layer is 3.1 g / cm 3 Up to 4.2g / cm 3 .

[0017] According to an embodiment of the present application, the electrochemical device has a DC resistance R1 during the first 1 second of discharge time when it reaches a 100% state of charge at 25°C, and the electrochemical device has a DC resistance R2 during the first 1 second of discharge time when it reaches a 50% state of charge at 25°C, 1<R1 / R2≤1.4.

[0018] According to an embodiment of the present application, the electrolyte includes a polynitrile compound, and the content of the polynitrile compound is 0.0003 g to 0.005 g per 1 g of the positive electrode active material.

[0019] According to an embodiment of the present application, the polynitrile compound includes at least one of 1,3,6-hexanetricarboxylic acid nitrile, 1,2,6-hexanetricarboxylic acid nitrile, 1,3,5-pentanetricarboxylic acid nitrile, 1,2,3-tris(2-cyanoxy)propane, succinonitrile or adiponitrile.

[0020] According to yet another aspect of the present application, the present application provides an electronic device, which includes the electrochemical device according to the embodiment of the present application.

[0021] Additional aspects and advantages of the present application will be described, shown, or explained in part in the subsequent description through implementation of the embodiments of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The following will briefly describe the drawings necessary for describing the embodiments of the present application or the prior art to facilitate the description of the embodiments of the present application. Obviously, the drawings described below are only some of the embodiments in the present application. For those skilled in the art, without the need for creative work, drawings of other embodiments can still be obtained based on the structures illustrated in these drawings.

[0023] Figure 1 A scanning electron microscope (SEM) photograph of a cross section of the positive electrode active material layer used in Example 1 of the present application is shown.

[0024] Figure 2 Shown Figure 1 Magnified image of the middle square area.

[0025] Figure 3 A time-of-flight secondary ion mass spectrometry (TOF-SIMS) photograph of the first particles in the positive electrode active material layer used in Example 27 of the present application is shown.

[0026] Figure 4 A time-of-flight secondary ion mass spectrometry (TOF-SIMS) photograph of the second particles in the positive electrode active material layer used in Example 28 of the present application is shown. DETAILED DESCRIPTION

[0027] The embodiments of the present application will be described in detail below. The embodiments of the present application should not be interpreted as limiting the present application.

[0028] In the detailed description and claims, a list of items connected by the term "at least one of" may mean any combination of the listed items. For example, if items A and B are listed, the phrase "at least one of A and B" means only A; only B; or A and B. In another example, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements. The term "at least one of" has the same meaning as the term "at least one of."

[0029] positive electrode

[0030] When primary particles are used alone as positive electrode active materials, the primary particles usually have a larger particle size, which is not conducive to the transmission of lithium ions, so that the lithium-ion battery has a lower discharge capacity retention rate, poor high-temperature cycle performance and a higher temperature rise under high-rate conditions. It is also difficult to improve the rate performance of lithium-ion batteries by adjusting the particle size of the primary particles. When secondary particles formed by the agglomeration of primary particles are used alone as positive electrode active materials, during the charge and discharge process of lithium-ion batteries, the expansion and contraction of the lattice cause the existence of interactive stresses between the primary particles, which will cause the secondary particles to break, thereby producing primary particles with a smaller particle size and no surface coating, thereby causing the side reactions between the positive electrode active material and the electrolyte to intensify, which has an adverse effect on the high-temperature cycle performance of lithium-ion batteries. It is still difficult to take into account the high-temperature cycle performance, high-temperature storage performance and rate performance of lithium-ion batteries by simply combining primary particles and secondary particles.

[0031] The present application solves the above problems by combining primary particles and secondary particles with specific structures and adjusting their ratio. Specifically, the present application provides an electrochemical device, which includes: a positive electrode and an electrolyte, the positive electrode includes a positive electrode current collector and a positive electrode active material layer, the positive electrode active material layer includes a positive electrode active material, and the positive electrode active material includes a first particle and a second particle, wherein: the first particle has a hole, the size of the hole is 1μm to 8μm; the hole size of the second particle is less than 1μm; the ratio a of the area of ​​the first particle to the area of ​​the second particle is not greater than 9.

[0032] The first particle (i.e., secondary particle) has a pore structure, wherein the presence of the pore structure is conducive to the transmission of lithium ions, and can relieve the inter-particle stress caused by lattice expansion and contraction during the charge and discharge process of the lithium-ion battery, reduce the probability of secondary particle breakage, and thus provide excellent rate performance for the lithium-ion battery. The second particle (i.e., primary particle) has no holes or has extremely small holes, which can provide excellent high-temperature cycle performance for the lithium-ion battery. Mixing the two types of particles in a certain proportion can achieve the matching of particles of different particle sizes, relieve the pressure on the positive electrode active material at a certain compaction density, thereby reducing the probability of secondary particle breakage. In the cross section in the thickness direction of the positive electrode active material layer, the ratio a of the area of ​​the first particle to the area of ​​the second particle can reflect the weight ratio of the two particles, which plays an important role in improving the performance of the lithium-ion battery. Taking the above factors into consideration, the electrochemical device of the present application has good initial discharge impedance, positive electrode gram capacity, high temperature cycle performance, high temperature storage performance, low temperature discharge capacity and rate performance at the same time, and can achieve balanced comprehensive performance.

[0033] The pores of the first or second particles of the positive active material may be formed inside the particles, on the surface of the particles, or through the particles. "The size of the pores" is intended to illustrate the size of the pores of the positive active material particles. When the cross section of the pores of the positive active material particles is circular, the size of the pores refers to the average diameter of the pores. When the cross section of the pores of the positive active material particles is non-circular, the size of the pores refers to the longest straight-line distance between any two points on the circumference of the pores. When the pores are formed on the surface of the positive active material particles or through the positive active material particles, the size of the pores refers to the longest straight-line distance between any two points on the circumference of the pores at the surface of the positive active material particles. The size of the pores of the positive active material particles can be measured by scanning electron microscopy. Specifically, the positive electrode is immersed in dimethyl carbonate (DMC) for 24 hours, sliced ​​along the thickness direction of the positive active material layer, and then ion polished to obtain a positive cross section. The positive active material in the positive cross section is observed by scanning electron microscopy, and the area containing at least 20 first particles in the field of view is photographed, and the size of the pores of the corresponding particles in the photographed area is calculated, and the average value is taken.

[0034] In some embodiments, the size of the pores of the first particles is 2 μm to 6 μm. In some embodiments, the size of the pores of the first particles is 3 μm to 5 μm. In some embodiments, the size of the pores of the first particles is 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, or within a range consisting of any two of the above values.

[0035] In some embodiments, the pore size of the second particles is less than 0.8 μm. In some embodiments, the pore size of the second particles is less than 0.5 μm. In some embodiments, the pore size of the second particles is less than 0.3 μm. In some embodiments, the second particles have no pores.

[0036] In some embodiments, on a cross section along the thickness direction of the positive electrode active material layer, the ratio a of the area of ​​the first particle to the area of ​​the second particle is not greater than 8. In some embodiments, on a cross section along the thickness direction of the positive electrode active material layer, the ratio a of the area of ​​the first particle to the area of ​​the second particle is not greater than 7. In some embodiments, on a cross section along the thickness direction of the positive electrode active material layer, the ratio a of the area of ​​the first particle to the area of ​​the second particle is not greater than 6.5. In some embodiments, on a cross section along the thickness direction of the positive electrode active material layer, the ratio a of the area of ​​the first particle to the area of ​​the second particle is not greater than 6. When the ratio a of the area of ​​the first particle to the area of ​​the second particle is within the above range, it helps to improve the positive electrode gram capacity while enabling the electrochemical device to have good initial discharge impedance, high temperature cycle performance, good high temperature storage performance, good low temperature discharge capability and high rate performance, achieving balanced comprehensive performance.

[0037] The ratio a of the cross-sectional area of ​​the first particle to the cross-sectional area of ​​the second particle can be obtained by scanning electron microscopy and Image J image processing software. Specifically, the positive electrode is immersed in dimethyl carbonate (DMC) for 24 hours, sliced ​​along the thickness direction of the positive electrode active material layer, and then ion polished to obtain a positive electrode cross section. The positive electrode active material in the positive electrode cross section is observed by scanning electron microscopy, and the area containing at least 50 particles in the field of view is photographed, and then the total area of ​​the first particle and the total area of ​​the second particle in the photographed area are calculated using Image J image processing software, and 10 pictures are randomly selected, and the total area of ​​the first particle and the total area of ​​the second particle are calculated respectively. The average value and the ratio a are calculated.

[0038] In some embodiments, the average particle size of the first particles is 7 μm to 15 μm. In some embodiments, the average particle size of the first particles is 8 μm to 12 μm. In some embodiments, the average particle size of the first particles is 9 μm to 10 μm. In some embodiments, the average particle size of the first particles is 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm or within a range consisting of any two of the above values. When the average particle size of the first particles is within the above range, it helps the electrochemical device to achieve good initial discharge impedance, positive electrode gram capacity, good low temperature discharge capability, good high temperature cycle performance and storage performance, and high rate performance, that is, to achieve balanced comprehensive performance.

[0039] In some embodiments, the average particle size of the second particles is 1 μm to 7 μm, and 7 μm is not included. In some embodiments, the average particle size of the second particles is 2 μm to 6 μm. In some embodiments, the average particle size of the second particles is 3 μm to 5 μm. In some embodiments, the average particle size of the second particles is 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, or within a range consisting of any two of the above values. When the average particle size of the second particles is within the above range, it helps the electrochemical device to achieve good initial discharge impedance, positive electrode gram capacity, good low temperature discharge capability, good high temperature cycle performance and storage performance, and high rate performance, that is, to achieve balanced comprehensive performance.

[0040] When the particles in the positive electrode active material are spherical, the average particle size refers to the average diameter of the particles. When the particles in the positive electrode active material are non-spherical, the particle size refers to the length of the longest axis of the particles. The average particle size of the particles in the positive electrode active material can be measured by a scanning electron microscope. Specifically, the positive electrode active material is observed by a scanning electron microscope, and an area containing at least 50 particles in the field of view is photographed, and the particle sizes of the corresponding particles in the photographed area are counted and averaged.

[0041] In some embodiments, the first particles include primary particles, and the average particle size of the primary particles is no greater than 3 μm. In some embodiments, the average particle size of the primary particles in the first particles is no greater than 2 μm. In some embodiments, the average particle size of the primary particles in the first particles is no greater than 1.5 μm. In some embodiments, the average particle size of the primary particles in the first particles is no greater than 1 μm.

[0042] In some embodiments, the first particles include at least 5 primary particles having a particle size of 0.5 μm or more. In some embodiments, the first particles include at least 8 primary particles having a particle size of 0.5 μm or more. In some embodiments, the first particles include at least 10 primary particles having a particle size of 0.5 μm or more. In some embodiments, the first particles include at least 15 primary particles having a particle size of 0.5 μm or more. When the first particles have a certain number of primary particles of a certain particle size, it helps the electrochemical device to achieve good initial discharge impedance, positive electrode gram capacity, good low temperature discharge capability, good high temperature cycle performance and storage performance, and high rate performance, that is, to achieve balanced comprehensive performance.

[0043] In some embodiments, the first particle and the second particle each independently comprise a Li b Ni x Co y M1 1-x-y-z M2z O 2 Compound, wherein: M1 includes at least one of Mn or Al; M2 includes at least one of Mg, Al, Ti, Zr, La, Y, Sr or Ce; 0.1≤b≤1.1; 0.5≤x<1; 0≤y<0.5; and 0≤z≤0.01. In some implementations, the first particle and the second particle each independently include at least one of the following compounds: LiNi 0.83 Co 0.12 Mn 0.05 O 2 、LiNi 0.83 Co 0.12 Al 0.05 O 2 、LiNi 0.88 Co 0.07 Mn 0.05 O 2 、LiNi 0.83 Co 0.12 Mn 0.047 Zr 0.003 O 2 、LiNi 0.83 Co 0.12 Mn 0.047 Mg 0.003 O 2 、LiNi 0.83 Co 0.12 Mn 0.047 Al 0.003 O 2 、LiNi 0.83 Co 0.12 Mn 0.047 Y 0.003 O 2 、LiNi 0.80 Co 0.10 Mn 0.10 O 2 , or LiNi 0.60 Co 0.20 Mn 0.197 Mg 0.003 O 2 The different chemical compositions of the first particles and / or the second particles will change the initial discharge impedance, gram capacity of the positive electrode, high temperature cycle performance, high temperature storage performance, low temperature discharge capacity and rate performance of the lithium-ion battery to a certain extent. x Co y M1 1-x-y-z M2 z O 2 Compounds used as positive electrode active materials can achieve balanced comprehensive performance of electrochemical devices.

[0044] In some embodiments, the first particle contains boron. In some embodiments, the boron content of the surface region of the first particle is higher than that of the central region, that is, the surface of the first particle is coated with boron. A lower sintering temperature is required during the preparation of the first particle in the positive electrode active material, and more lithium elements usually remain on the surface of the first particle. Coating the surface of the first particle with boron can reduce the amount of residual lithium on the surface of the first particle, thereby helping to improve the positive electrode gram capacity and high temperature storage expansion rate of the electrochemical device, so that it can achieve balanced comprehensive performance.

[0045] In some embodiments, the second particle contains aluminum. In some embodiments, the aluminum content of the surface region of the second particle is higher than that of the central region, that is, the surface of the second particle is coated with aluminum. A higher sintering temperature is required during the preparation of the second particle in the positive electrode active material, so that there is almost no residual lithium on the surface of the second particle, thereby eliminating the need for boron coating. Coating the surface of the second particle with an element other than boron (e.g., aluminum coating) helps to further improve the rate performance of the electrochemical device, so that it can achieve balanced comprehensive performance.

[0046] The surface area of ​​a particle refers to the area 50 nm from the outermost surface of the particle to the center of the particle. The center area of ​​a particle refers to the area of ​​the particle other than the surface area, where the center of the particle refers to the midpoint of the longest straight line between any two points on the perimeter of the particle. The element content of the surface area and the center area of ​​the particle can be obtained by combining a scanning electron microscope (SEM) with an X-ray energy dispersive spectrometer.

[0047] In some embodiments, the first particle and the second particle contain boron. In some embodiments, the boron content of the first particle is greater than the boron content of the second particle. The boron in the first particle or the second particle may come from the chemical composition of the particle itself or its surface coating. When the boron content of the first particle is greater than the boron content of the second particle, it helps to reduce the impedance of the electrochemical device at the initial stage of discharge and improve the low-temperature discharge capability and rate performance, so that it can achieve balanced comprehensive performance.

[0048] In some embodiments, based on the total weight of the positive electrode active material layer, the weight percentage c of the positive electrode active material and the ratio a satisfy the following relationship: c≤0.02×a / (a+1)+0.97. When a and c satisfy the above relationship, it helps the electrochemical device to achieve good initial discharge impedance, good positive electrode gram capacity, good low-temperature discharge capability, good high-temperature cycle performance and storage performance, and high-rate performance, that is, to achieve balanced comprehensive performance.

[0049] In some embodiments, the positive electrode active material layer has a porosity of 10% to 50%. In some embodiments, the positive electrode active material layer has a porosity of 15% to 40%. In some embodiments, the positive electrode active material layer has a porosity of 20% to 30%. In some embodiments, the porosity of the positive electrode active material layer is 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or in a range consisting of any two of the above values. When the porosity of the positive electrode active material layer is within the above range, it helps the electrochemical device to achieve good initial discharge impedance, good positive electrode gram capacity, good low temperature discharge capability, good high temperature cycle performance and storage performance and high rate performance, that is, to achieve balanced comprehensive performance.

[0050] The "porosity" of the positive electrode active material layer refers to the percentage of the sum of the pores and gaps between the particles of the positive electrode active material in the cross-section of the positive electrode active material layer in the thickness direction of the positive electrode active material layer under an electron microscope. The porosity of the positive electrode active material layer can be obtained by scanning electron microscopy and Image J image processing software. Specifically, the positive electrode is immersed in dimethyl carbonate (DMC) for 24 hours, and then ion polished to obtain a positive electrode cross-section. The positive electrode active material in the positive electrode cross-section is observed by scanning electron microscopy, and the area containing at least 50 particles in the field of view is photographed, and then the Image J image processing software is used to adjust the grayscale value between the positive electrode active material particles and the pores and the gaps between the particles and other materials (for example, binders and conductive agents, etc.), thereby measuring the cross-sectional area S of all particles in the photographed area; at the same time, the area S of the entire photographed area is measured. 总 ; The porosity P of the positive electrode active material layer is calculated by the following formula:

[0051] P=(S 总 -S) / S 总 ×100%.

[0052] In some embodiments, the compaction density of the positive electrode active material layer is 3.1 g / cm 3 Up to 4.2g / cm 3 .

[0053] In some embodiments, the positive electrode active material further includes a binder, and optionally also includes a positive electrode conductive material.

[0054] The binder improves the bonding of the positive electrode active material particles to each other and also improves the bonding of the positive electrode active material to the current collector. Non-limiting examples of binders include polyvinyl alcohol, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin, nylon, etc.

[0055] In some embodiments, the positive electrode active material also includes a positive electrode conductive material, thereby imparting conductivity to the electrode. The positive electrode conductive material may include any conductive material as long as it does not cause chemical changes. Non-limiting examples of positive electrode conductive materials include carbon-based materials (e.g., natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.), metal-based materials (e.g., metal powder, metal fiber, etc., including, for example, copper, nickel, aluminum, silver, etc.), conductive polymers (e.g., polyphenylene derivatives) and mixtures thereof.

[0056] In some embodiments, the positive electrode current collector may be aluminum (Al), but is not limited thereto.

[0057] negative electrode

[0058] The negative electrode includes a current collector and a negative electrode active material layer disposed on the current collector. The specific types of the negative electrode active materials are not subject to specific restrictions and can be selected according to needs.

[0059] In some embodiments, the negative electrode active material is selected from natural graphite, artificial graphite, mesophase microcarbon beads (MCMB), hard carbon, soft carbon, silicon, silicon-carbon composite, Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO 2 , spinel-structured lithiated TiO 2 -Li 4 Ti 5 O 12 , one or more of Li-Al alloys.

[0060] Non-limiting examples of carbon materials include crystalline carbon, amorphous carbon and mixtures thereof. Crystalline carbon can be amorphous or flake, flake, spherical or fibrous natural graphite or artificial graphite. Amorphous carbon can be soft carbon, hard carbon, mesophase pitch carbide, calcined coke, etc.

[0061] In some embodiments, the negative active material layer may include a binder and optionally further include a conductive material.

[0062] The binder improves the bonding between the negative electrode active material particles and the bonding between the negative electrode active material and the current collector. Non-limiting examples of binders include polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene butadiene rubber, acrylated styrene butadiene rubber, epoxy resin, nylon, etc.

[0063] The negative electrode active material layer includes a conductive material to impart conductivity to the electrode. The conductive material may include any conductive material as long as it does not cause chemical changes. Non-limiting examples of conductive materials include carbon-based materials (e.g., natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, carbon fiber, etc.), metal-based materials (e.g., metal powder, metal fiber, etc., such as copper, nickel, aluminum, silver, etc.), conductive polymers (e.g., polyphenylene derivatives) and mixtures thereof.

[0064] The current collector for the negative electrode described in the present application may be selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and combinations thereof.

[0065] Electrolyte

[0066] In some embodiments, the electrolyte includes a polynitrile compound. The polynitrile compound can act as a positive electrode protective agent, which helps the electrochemical device achieve balanced comprehensive performance.

[0067] In some embodiments, based on 1g of the positive electrode active material, the content of the polynitrile compound is 0.0003g to 0.005g. In some embodiments, based on 1g of the positive electrode active material, the content of the polynitrile compound is 0.0005g to 0.003g. In some embodiments, based on 1g of the positive electrode active material, the content of the polynitrile compound is 0.001g to 0.002g. When the electrolyte contains the above-mentioned content of the polynitrile compound, the low-temperature discharge capability and high-rate performance of the lithium-ion battery can be further improved, that is, a balanced comprehensive performance is achieved.

[0068] In some embodiments, the polynitrile compound includes at least one of 1,3,6-hexanetricarboxylic acid nitrile, 1,2,6-hexanetricarboxylic acid nitrile, 1,3,5-pentanetricarboxylic acid nitrile, 1,2,3-tris(2-cyano)propane, succinonitrile, or adiponitrile.

[0069] In some embodiments, based on the total weight of the electrolyte, the content of the polynitrile compound is 0.1wt% to 10wt%. In some embodiments, based on the total weight of the electrolyte, the content of the polynitrile compound is 0.2wt% to 8wt%. In some embodiments, based on the total weight of the electrolyte, the content of the polynitrile compound is 0.5wt% to 5wt%. In some embodiments, based on the total weight of the electrolyte, the content of the polynitrile compound is 1wt% to 3wt%. In some embodiments, based on the total weight of the electrolyte, the content of the polynitrile compound is 0.1wt%, 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt%, 6wt%, 6.5wt%, 7wt%, 7.5wt%, 8wt%, 8.5wt%, 9wt%, 9.5wt%, 10wt% or in the range consisting of any two of the above values.

[0070] The lithium salts that can be used in the electrolyte of the present application include, but are not limited to: inorganic lithium salts, such as LiPF 6 , LiBF 4 、LiSbF 6 、LiSO 3 F、LiN(FSO 2 ) 2 etc.; Fluorinated organic lithium salts, such as LiCF 3 SO 3 、LiN(FSO 2 )(CF 3 SO 2 )、LiN(CF 3 SO 2 ) 2 、LiN(C 2 F 5 SO 2 ) 2 , cyclic 1,3-hexafluoropropane disulfonyl imide lithium, cyclic 1,2-tetrafluoroethane disulfonyl imide lithium, LiN(CF 3 SO 2 )(C 4 F 9 SO 2 )、LiC(CF 3 SO 2 ) 3 、LiPF 4 (CF 3 ) 2 、LiPF 4 (C 2 F 5 ) 2 、LiPF4 (CF 3 SO 2 ) 2 、LiPF 4 (C 2 F 5 SO 2 ) 2 , LiBF 2 (CF 3 ) 2 、LiBF2(C2F5)2、LiBF 2 (CF 3 SO 2 ) 2 , LiBF 2 (C 2 F 5 SO 2 ) 2 ; lithium salts containing dicarboxylic acid complexes, such as lithium bis(oxalato)borate, lithium difluorooxalatoborate, lithium tri(oxalato)phosphate, lithium difluorobis(oxalato)phosphate, lithium tetrafluoro(oxalato)phosphate, etc. In addition, the above lithium salts can be used alone or in combination of two or more. In some embodiments, the lithium salt includes LiPF 6 and LiBF 4 In some embodiments, the lithium salt includes LiPF 6 or LiBF 4 Inorganic lithium salts and LiCF 3 SO 3 、LiN(CF 3 SO 2 ) 2 、LiN(C 2 F 5 SO 2 ) 2 In some embodiments, the concentration of the lithium salt is in the range of 0.8 mol / L to 3 mol / L, in the range of 0.8 mol / L to 2.5 mol / L, in the range of 0.8 mol / L to 2 mol / L, or in the range of 1 mol / L to 2 mol / L. In some embodiments, the concentration of the lithium salt is about 1 mol / L, about 1.15 mol / L, about 1.2 mol / L, about 1.5 mol / L, about 2 mol / L, or about 2.5 mol / L.

[0071] The solvents that can be used in the electrolyte of the embodiment of the present application include, but are not limited to: cyclic carbonates, chain carbonates, cyclic carboxylates, and chain carboxylates.

[0072] In some embodiments, the cyclic carbonate includes, but is not limited to, ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate. In some embodiments, the cyclic carbonate has 3-6 carbon atoms.

[0073] In some embodiments, the linear carbonates include, but are not limited to: dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate (DEC), methyl n-propyl carbonate, ethyl n-propyl carbonate, di-n-propyl carbonate and the like; as fluorine-substituted linear carbonates, for example, bis(fluoromethyl) carbonate, bis(difluoromethyl) carbonate, bis(trifluoromethyl) carbonate, bis(2-fluoroethyl) carbonate, bis(2,2-difluoroethyl) carbonate, bis(2,2,2-trifluoroethyl) carbonate, 2-fluoroethyl methyl carbonate, 2,2-difluoroethyl methyl carbonate and 2,2,2-trifluoroethyl methyl carbonate.

[0074] In some embodiments, the cyclic carboxylic acid ester includes, but is not limited to, γ-butyrolactone and γ-valerolactone. In some embodiments, part of the hydrogen atoms of the cyclic carboxylic acid ester may be substituted with fluorine.

[0075] In some embodiments, the chain carboxylic acid ester includes, but is not limited to: ethyl acetate, propyl acetate, isopropyl acetate, butyl acetate, sec-butyl acetate, isobutyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, isopropyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, methyl isobutyrate, ethyl isobutyrate, methyl valerate, ethyl valerate, methyl pivalate and ethyl pivalate. In some embodiments, part of the hydrogen atoms of the chain carboxylic acid ester can be substituted by fluorine. In some embodiments, the chain carboxylic acid ester substituted with fluorine includes, but is not limited to: methyl trifluoroacetate, ethyl trifluoroacetate, propyl trifluoroacetate, butyl trifluoroacetate and 2,2,2-trifluoroethyl trifluoroacetate.

[0076] In some embodiments, the solvent used in the electrolyte of the present application includes one or more of the above. In some embodiments, the solvent used in the electrolyte of the present application includes cyclic carbonates, chain carbonates, cyclic carboxylates, chain carboxylates and combinations thereof. In some embodiments, the electrolyte of the present application includes at least one of ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl propionate, propyl propionate, propyl acetate or ethyl acetate. In some embodiments, the electrolyte of the present application includes at least one of ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl propionate, propyl propionate or γ-butyrolactone.

[0077] Additives that can be used in the electrolyte of the embodiment of the present application include, but are not limited to: cyclic carbonates containing carbon-carbon double bonds, and compounds containing sulfur-oxygen double bonds.

[0078] In some embodiments, the cyclic carbonate having a carbon-carbon double bond specifically includes, but is not limited to, at least one of vinylene carbonate, methyl vinylene carbonate, ethyl vinylene carbonate, vinyl vinyl ethylene carbonate, or 1,2-dimethyl vinylene carbonate.

[0079] In some embodiments, the compound containing a sulfur-oxygen double bond includes, but is not limited to, at least one of vinyl sulfate, 1,2-propylene glycol sulfate, 1,3-propane sultone, 1-fluoro-1,3-propane sultone, 2-fluoro-1,3-propane sultone or 3-fluoro-1,3-propane sultone.

[0080] Isolation film

[0081] A separator may be provided between the positive electrode and the negative electrode to prevent short circuit. The material and shape of the separator used in the embodiments of the present application are not particularly limited, and it may be any technology disclosed in the prior art. In some embodiments, the separator includes a polymer or an inorganic substance formed of a material that is stable to the electrolyte of the present application.

[0082] For example, the isolation film may include a substrate layer and a surface treatment layer. The substrate layer is a non-woven fabric, a film or a composite film having a porous structure, and the material of the substrate layer includes at least one of polyethylene, polypropylene, polyethylene terephthalate and polyimide. Specifically, a polypropylene porous film, a polyethylene porous film, a polypropylene non-woven fabric, a polyethylene non-woven fabric or a polypropylene-polyethylene-polypropylene porous composite film may be selected.

[0083] A surface treatment layer is disposed on at least one surface of the substrate layer. The surface treatment layer may be a polymer layer or an inorganic layer, or a layer formed by mixing a polymer and an inorganic layer.

[0084] The inorganic layer includes inorganic particles and a binder, wherein the inorganic particles are selected from one or a combination of aluminum oxide, silicon oxide, magnesium oxide, titanium oxide, hafnium dioxide, tin oxide, cerium dioxide, nickel oxide, zinc oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, boehmite, aluminum hydroxide, magnesium hydroxide, calcium hydroxide and barium sulfate. The binder includes at least one of polyvinylidene fluoride, a copolymer of vinylidene fluoride and hexafluoropropylene, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinylpyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene or polyhexafluoropropylene.

[0085] The polymer layer contains polymers, and the polymer material contains at least one of polyamide, polyacrylonitrile, acrylate polymer, polyacrylic acid, polyacrylic acid salt, polyvinylpyrrolidone, polyvinyl ether, polyvinylidene fluoride, and poly(vinylidene fluoride-hexafluoropropylene).

[0086] Electrochemical Devices

[0087] In some embodiments, the electrochemical device of the present application has a DC resistance R1 in the first 1 second of discharge time when it reaches 100% state of charge at 25°C, and the electrochemical device has a DC resistance R2 in the first 1 second of discharge time when it reaches 50% state of charge at 25°C, 1<R1 / R2≤1.4. In some embodiments, 1<R1 / R2≤1.3. In some embodiments, 1<R1 / R2≤1.2. In some embodiments, 1<R1 / R2≤1.1. When the R1 / R2 ratio is within the above range, the impedance of the electrochemical device is small at the beginning of discharge, which is conducive to achieving superior low-temperature discharge performance and reducing the temperature rise under high-rate discharge.

[0088] The electrochemical device of the present application includes any device that generates an electrochemical reaction, and its specific examples include all kinds of primary batteries and secondary batteries. In particular, the electrochemical device is a lithium secondary battery. The lithium secondary battery may include a lithium metal secondary battery, a lithium ion secondary battery, a lithium polymer secondary battery or a lithium ion polymer secondary battery.

[0089] Electronic Devices

[0090] The present application further provides an electronic device, which includes an electrochemical device according to the present application. The purpose of the electrochemical device of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. In some embodiments, the electrochemical device of the present application can be used for, but not limited to, mobile phones, laptops, pen-input computers, mobile computers, e-book players, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries, etc.

[0091] The preparation of lithium-ion batteries is described below by taking lithium-ion batteries as an example and combining specific embodiments. Those skilled in the art will understand that the preparation method described in this application is only an example, and any other suitable preparation method is within the scope of this application.

[0092] Example

[0093] The following describes the performance evaluation of the examples and comparative examples of the lithium-ion battery according to the present application.

[0094] 1. Preparation of lithium-ion batteries

[0095] 1. Preparation of positive electrode

[0096] For Example 1-42, the first particles, the second particles, acetylene black and polyvinylidene fluoride prepared according to the following method are mixed uniformly in a certain proportion, and an appropriate amount of N-methylpyrrolidone is added and stirred fully to prepare a uniform positive electrode active material slurry. The positive electrode active material slurry is coated on the positive electrode current collector aluminum foil and dried. Then, the edges are trimmed, cut into pieces, divided into strips, and dried to obtain a positive electrode active material layer, and then the pieces are cut and the pole ears are welded to obtain a positive electrode.

[0097] The ratio of the cross-sectional area of ​​the first particles to the cross-sectional area of ​​the second particles can be adjusted by the addition ratio.

[0098] Example 1

[0099] According to LiNi 0.83 Co 0.12 Mn 0.05 O 2 Prepare nickel sulfate (NiSO) containing a nickel source in a stoichiometric ratio 4 ), cobalt sulfate (CoSO 4 ) and manganese source manganese sulfate (MnSO 4 ) solution, and mix it with sodium hydroxide (NaOH) solution and ammonia (NH 3 ·H 2 O) and LiOH solution are mixed uniformly in an atomized form, and dried at 200° C. to control the particle size of the particles to be 10 μm, and then calcined at 800° C. for 16 hours to obtain first particles.

[0100] According to LiNi 0.83 Co 0.12 Mn 0.05 O 2 The stoichiometric ratio of Ni, Co, Mn and NCM precursors was prepared. 0.83 Co 0.12 Mn 0.05 (OH) 2 The precursor particles have a particle size of 3 μm, are uniformly mixed with lithium hydroxide (LiOH) and dried, and then calcined at 840° C. for 15 hours to obtain second particles.

[0101] The first particles, the second particles, acetylene black, and polyvinylidene fluoride were mixed in a weight ratio of 73.1:24.4:1.3:1.2 so that the weight ratio of the positive electrode active material including the first particles and the second particles was 97.5%.

[0102] Example 2

[0103] According to LiNi 0.83 Co 0.12Al 0.05 O 2 Prepare a nickel (Ni) source containing nickel sulfate (NiSO 4 ), cobalt (Co) source cobalt sulfate (CoSO 4 ) and aluminum (Al) source aluminum sulfate (Al 2 (SO 4 ) 3 ) solution, and mix it with sodium hydroxide (NaOH) solution and ammonia (NH 3 ·H 2 O) and LiOH solution are mixed uniformly in an atomized form, and dried at 200° C. to control the particle size of the particles to be 10 μm, and then calcined at 800° C. for 16 hours to obtain first particles.

[0104] According to LiNi 0.83 Co 0.12 Al 0.05 O 2 The stoichiometric ratio of Ni / Co / Al ternary material precursor Ni 0.83 Co 0.12 Al 0.05 (OH) 2 The precursor particles have a particle size of 3 μm, are uniformly mixed with lithium hydroxide (LiOH) and dried, and then calcined at 840° C. for 15 hours to obtain second particles.

[0105] The first particles, the second particles, acetylene black and polyvinylidene fluoride were mixed in the same proportion as in Example 1.

[0106] Example 3

[0107] According to LiNi 0.88 Co 0.07 Mn 0.05 O 2 Prepare nickel sulfate (NiSO) containing a nickel source in a stoichiometric ratio 4 ), cobalt sulfate (CoSO 4 ) and manganese source manganese sulfate (MnSO 4 ) solution, and mix it with sodium hydroxide (NaOH) solution, ammonia (NH 3 ·H 2 O) and LiOH solution are mixed uniformly in an atomized form, dried at 200°C, the particle size is controlled to be 10 μm, and then calcined at 780°C for 16 hours to obtain first particles.

[0108] According to LiNi 0.88 Co 0.07 Mn 0.05 O 2The stoichiometric ratio of Ni, Co, Mn and NCM precursors was prepared. 0.88 Co 0.07 Mn 0.05 (OH) 2 The precursor particles have a particle size of 3 μm, are uniformly mixed with lithium hydroxide (LiOH) and dried, and then calcined at 820° C. for 15 hours to obtain second particles.

[0109] The first particles, the second particles, acetylene black and polyvinylidene fluoride were mixed in the same proportion as in Example 1.

[0110] Example 4

[0111] The first particles and the second particles were prepared by a method similar to that of Example 1. The difference was that the calcination temperature and calcination time of the first particles were controlled so that the pore size of the first particles was 5 μm.

[0112] Example 5

[0113] The first and second particles were prepared in the same manner as in Example 1. The first and second particles, acetylene black and polyvinylidene fluoride were mixed in a weight ratio of 72.0:24.0:2.5:1.5, so that the weight ratio of the positive electrode active material including the first and second particles was 96.0%.

[0114] Example 6

[0115] The first and second particles were prepared in the same manner as in Example 1. The first and second particles, acetylene black and polyvinylidene fluoride were mixed in a weight ratio of 48.0:48.0:2.5:1.5, so that the weight ratio of the positive electrode active material including the first and second particles was 96.0%.

[0116] Example 7

[0117] The first and second particles were prepared in the same manner as in Example 1. The first and second particles, acetylene black and polyvinylidene fluoride were mixed in a weight ratio of 24.0:72.0:2.5:1.5, so that the weight ratio of the positive electrode active material including the first and second particles was 96.0%.

[0118] Example 8

[0119] The first and second particles were prepared in the same manner as in Example 1. The first and second particles, acetylene black and polyvinylidene fluoride were mixed in a weight ratio of 4.6:91.4:2.5:1.5, so that the weight ratio of the positive electrode active material including the first and second particles was 96.0%.

[0120] Example 9

[0121] The first particles were obtained by a preparation method similar to that of Example 1, and the particle size was controlled to be 10 μm and the particle pore size was 1 μm by adjusting the sintering temperature and time. The second particles were obtained by the same preparation method as that of Example 1, and then the first particles, the second particles, acetylene black and polyvinylidene fluoride were mixed in a weight ratio of 4.6:91.4:2.5:1.5, so that the weight ratio of the positive electrode active material containing the first particles and the second particles was 96.0%.

[0122] Example 10

[0123] The first particles were obtained by a preparation method similar to that of Example 5, and the particle pore size was controlled to be 7 μm by adjusting the sintering temperature and time. The second particles were obtained by the same preparation method as that of Example 5. The first particles, the second particles, acetylene black and polyvinylidene fluoride were then mixed in a weight ratio of 72.0:24.0:2.5:1.5, so that the weight ratio of the positive electrode active material containing the first particles and the second particles was 96.0%.

[0124] Embodiment 11

[0125] The first particles were obtained by the same preparation method as in Example 5, and the second particles were obtained by a similar preparation method as in Example 5. The pore size of the particles was controlled to be 0.5 μm by adjusting the sintering temperature and time. The first particles, the second particles, acetylene black and polyvinylidene fluoride were then mixed in a weight ratio of 72.0:24.0:2.5:1.5, so that the weight ratio of the positive electrode active material containing the first particles and the second particles was 96.0%.

[0126] Example 12

[0127] According to LiNi 0.83 Co 0.12 Mn 0.047 Zr 0.003 O 2 Prepare nickel sulfate (NiSO) containing a nickel source in a stoichiometric ratio 4 ), cobalt sulfate (CoSO 4 ), manganese source manganese sulfate (MnSO 4 ) and zirconium source zirconium sulfate (Zr(SO 4 ) 2 ) solution, and mix it with sodium hydroxide (NaOH) solution and ammonia (NH 3 ·H 2O) and LiOH solution were mixed in an atomized form and dried at 200 °C to control the particle size to 10 μm. The product was then calcined at 815 °C for 24 h and mixed with boric acid (H 3 BO 3 ) are mixed evenly and sintered at 400° C. for 4 hours, wherein the weight percentage of boron element is 0.1%, to obtain first particles.

[0128] According to LiNi 0.83 Co 0.12 Mn 0.047 Zr 0.003 O 2 The stoichiometric ratio of Ni, Co, Mn and NCM precursors was prepared. 0.83 Co 0.12 Mn 0.05 (OH) 2 The precursor particles have a particle size of 3 μm and are mixed with lithium hydroxide (LiOH) and nano zirconium oxide (ZrO 2 ) were uniformly mixed and dried, and then calcined at 840°C for 15 hours. 2 O 3 ) are mixed evenly, and sintered at 600° C. for 4 hours, wherein the weight percentage of aluminum element is 0.15%, to obtain second particles.

[0129] The first particles, the second particles, acetylene black and polyvinylidene fluoride were mixed in the same proportion as in Example 7.

[0130] Embodiment 13

[0131] The preparation method is basically the same as that of Example 12, except that the particle size is controlled to be 7 μm when preparing the first particles.

[0132] Embodiment 14

[0133] The preparation method is basically the same as that of Example 12, except that the particle size is controlled to be 5 μm when preparing the first particles.

[0134] Embodiment 15

[0135] The preparation method is basically the same as that of Example 12, except that the particle size is controlled to be 15 μm when preparing the first particles.

[0136] Example 16

[0137] The preparation method is basically the same as that of Example 12, except that the particle size is controlled to be 17 μm when preparing the first particles.

[0138] Embodiment 17

[0139] The preparation method is basically the same as that of Example 12, except that the particle size is controlled to be 5 μm when preparing the second particles.

[0140] Embodiment 18

[0141] The preparation method is basically the same as that of Example 12, except that the particle size is controlled to be 7 μm when preparing the second particles.

[0142] Embodiment 19

[0143] The preparation method is basically the same as that of Example 12, except that the particle size is controlled to be 0.5 μm when preparing the second particles.

[0144] Embodiment 20

[0145] The preparation method is basically the same as that of Example 12, except that the particle size is controlled to be 1 μm when preparing the second particles.

[0146] Embodiment 21

[0147] The preparation method is basically the same as that of Example 12, except that the particle size is controlled to be 8 μm when preparing the second particles.

[0148] Embodiment 22

[0149] According to LiNi 0.83 Co 0.12 Mn 0.047 Zr 0.003 O 2 Prepare nickel sulfate (NiSO) containing a nickel source in a stoichiometric ratio 4 ), cobalt sulfate (CoSO 4 ), manganese source manganese sulfate (MnSO 4 ) and zirconium source zirconium sulfate (Zr(SO 4 ) 2 ) solution, and mix it with sodium hydroxide (NaOH) solution and ammonia (NH 3 ·H 2 O) and LiOH solution were mixed in an atomized form and dried at 200 °C to control the particle size to 10 μm. The product was then calcined at 800 °C for 16 h and mixed with boric acid (H 3 BO 3 ) are mixed evenly, and sintered at 400° C. for 4 hours, wherein the weight percentage of boron element is 0.1%, to obtain first particles. In the first particles, the particle size of the primary particles is 0.2 μm.

[0150] According to LiNi 0.83 Co0.12 Mn 0.047 Zr 0.003 O 2 The stoichiometric ratio of Ni, Co, Mn and NCM precursors was prepared. 0.83 Co 0.12 Mn 0.047 Zr 0.003 (OH) 2 The precursor particles have a particle size of 3 μm and are mixed with lithium hydroxide (LiOH) and nano zirconium oxide (ZrO 2 ) were uniformly mixed and dried, and then calcined at 840°C for 15 hours. 2 O 3 ) are mixed evenly, and sintered at 600° C. for 4 hours, wherein the weight percentage of aluminum element is 0.15%, to obtain second particles.

[0151] The first particles, the second particles, acetylene black and polyvinylidene fluoride were mixed in the same proportion as in Example 7.

[0152] Embodiment 23

[0153] According to LiNi 0.83 Co 0.12 Mn 0.047 Zr 0.003 O 2 Prepare nickel sulfate (NiSO) containing a nickel source in a stoichiometric ratio 4 ), cobalt sulfate (CoSO 4 ), manganese source manganese sulfate (MnSO 4 ) and zirconium source zirconium sulfate (Zr(SO 4 ) 2 ) solution, and mix it with sodium hydroxide (NaOH) solution and ammonia (NH 3 ·H 2 O) and LiOH solution were mixed in an atomized form and dried at 200 °C to control the particle size to 10 μm. The product was then calcined at 815 °C for 24 h and mixed with boric acid (H 3 BO 3 ) are mixed evenly, and sintered at 400° C. for 4 hours, wherein the weight percentage of boron element is 0.1%, to obtain first particles. Among the first particles, the number of primary particles with a particle size of more than 0.5 μm is 8.

[0154] The same method as in Example 22 was used to prepare the second particles.

[0155] The first particles, the second particles, acetylene black and polyvinylidene fluoride were mixed in the same proportion as in Example 22.

[0156] Embodiment 24

[0157] The preparation method is basically the same as that of Example 23, except that when preparing the first particles, the primary particle size is controlled to be 3 μm, and the number of primary particles with a particle size of more than 0.5 μm is 6.

[0158] Embodiment 25

[0159] The preparation method is basically the same as that of Example 23, except that when preparing the first particles, the primary particle size is controlled to be 4 μm, and the number of primary particles with a particle size of more than 0.5 μm is 4.

[0160] Embodiment 26

[0161] According to LiNi 0.83 Co 0.12 Mn 0.047 Zr 0.003 O 2 Prepare nickel sulfate (NiSO) containing a nickel source in a stoichiometric ratio 4 ), cobalt sulfate (CoSO 4 ), manganese source manganese sulfate (MnSO 4 ) and zirconium source zirconium sulfate (Zr(SO 4 ) 2 ) solution, and mix it with sodium hydroxide (NaOH) solution and ammonia (NH 3 ·H 2 O) and LiOH solution are mixed evenly in an atomized form, and dried at 200° C., the particle size Dv50 is controlled to be 10 μm, and then calcined at 800° C. for 16 hours to obtain first particles.

[0162] According to LiNi 0.83 Co 0.12 Mn 0.047 Zr 0.003 O 2 The precursor of nickel-cobalt-manganese ternary material (NCM) was prepared in a stoichiometric ratio, wherein the precursor particle size was 3 μm, and lithium hydroxide (LiOH) and nano zirconium oxide (ZrO 2 ) are uniformly mixed and dried, and then calcined at 840° C. for 15 hours to obtain second particles.

[0163] The first particles, the second particles, acetylene black and polyvinylidene fluoride were mixed in the same proportion as in Example 7.

[0164] Embodiment 27

[0165] According to LiNi 0.83 Co 0.12 Mn 0.047 Zr0.003 O 2 Prepare nickel sulfate (NiSO) containing a nickel source in a stoichiometric ratio 4 ), cobalt sulfate (CoSO 4 ), manganese source manganese sulfate (MnSO 4 ) and zirconium source zirconium sulfate (Zr(SO 4 ) 2 ) solution, and mix it with sodium hydroxide (NaOH) solution and ammonia (NH 3 ·H 2 O) and LiOH solution were mixed in an atomized form and dried at 200 °C to control the particle size to 10 μm. The product was then calcined at 800 °C for 16 h and mixed with boric acid (H 3 BO 3 ) are mixed evenly, and sintered at 400° C. for 4 hours, wherein the weight percentage of boron element is 0.1%, to obtain first particles.

[0166] The same method as in Example 26 was used to prepare the second particles.

[0167] The first particles, the second particles, acetylene black and polyvinylidene fluoride were mixed in the same proportion as in Example 26.

[0168] Embodiment 28

[0169] The first particles were prepared in the same manner as in Example 27.

[0170] According to LiNi 0.83 Co 0.12 Mn 0.047 Zr 0.003 O 2 The stoichiometric ratio of Ni, Co, Mn and NCM precursors was prepared. 0.83 Co 0.12 Mn 0.047 Zr 0.003 (OH) 2 The precursor particles have a particle size of 3 μm and are mixed with lithium hydroxide (LiOH) and nano zirconium oxide (ZrO 2 ) were uniformly mixed and dried, and then calcined at 840°C for 15 hours. 3 BO 3 ) are mixed evenly, and sintered at 400° C. for 4 hours for boron coating, wherein the weight percentage of boron element is 0.1%, to obtain second particles.

[0171] The first particles, the second particles, acetylene black and polyvinylidene fluoride were mixed in the same proportion as in Example 26.

[0172] Embodiment 29

[0173] The preparation method is basically the same as that of Example 28, except that the weight percentage of boron element is controlled to be 400 ppm when preparing the second particles.

[0174] Embodiment 30

[0175] The same method as in Example 26 was used to prepare the first particles.

[0176] The same method as in Example 28 was used to prepare the second particles.

[0177] The first particles, the second particles, acetylene black and polyvinylidene fluoride were mixed in the same proportion as in Example 26.

[0178] Embodiment 31

[0179] The first and second particles were prepared in the same manner as in Example 1. The first and second particles, acetylene black and polyvinylidene fluoride were mixed in a weight ratio of 72.75:24.25:1.7:1.3, so that the weight ratio of the positive electrode active material including the first and second particles was 97.0%.

[0180] Embodiment 32

[0181] The first particles and the second particles were prepared in the same manner as in Example 1. The first particles, the second particles, acetylene black and polyvinylidene fluoride were mixed in a weight ratio of 73.95:24.65:0.6:0.8, so that the weight ratio of the positive electrode active material including the first particles and the second particles was 98.6%.

[0182] Embodiment 33

[0183] The preparation method is substantially the same as that of Example 26, the only difference being that a magnesium (Mg) source is used to replace a zirconium (Zr) source when preparing the first particles.

[0184] Embodiment 34

[0185] The preparation method is basically the same as that of Example 26, the only difference being that an aluminum (Al) source is used to replace a zirconium (Zr) source when preparing the first particles.

[0186] Embodiment 35

[0187] The preparation method is basically the same as that of Example 26, the only difference being that an yttrium (Y) source is used to replace a zirconium (Zr) source when preparing the first particles.

[0188] Embodiment 36

[0189] The preparation method is basically the same as that of Example 23, except that the compaction density of the positive electrode active material layer is increased from 3.5 g / cm 3 Adjusted to 3.3g / cm 3 , the porosity of the positive electrode active material layer is 50%

[0190] Embodiment 37

[0191] The preparation method is basically the same as that of Example 23, except that the compaction density of the positive electrode active material layer is increased from 3.5 g / cm 3 Adjusted to 3.55g / cm 3 , the porosity of the positive electrode active material layer is 5%.

[0192] Embodiment 38

[0193] The preparation method is basically the same as that of Example 23, except that the compaction density of the positive electrode active material layer is increased from 3.5 g / cm 3 Adjusted to 3.40g / cm 3 , the porosity of the positive electrode active material layer is 25%.

[0194] Embodiment 39

[0195] The method for preparing the positive electrode material is the same as that in Example 23, except that the electrolyte used in Example 30 contains 0.0003 (g) of 1,3,6-hexanetricarboxylate per 1g of positive electrode active material.

[0196] Embodiment 40

[0197] The method for preparing the positive electrode material is the same as that in Example 23, except that the electrolyte used in Example 31 contains 0.002 (g) of 1,3,6-hexanetricarboxylate per 1g of positive electrode active material.

[0198] Embodiment 41

[0199] The method for preparing the positive electrode material is the same as that in Example 23, except that the electrolyte used in Example 32 contains 0.005 (g) of 1,3,6-hexanetricarboxylate per 1g of positive electrode active material.

[0200] Embodiment 42

[0201] The method for preparing the positive electrode material is the same as that in Example 23, except that the electrolyte used contains 0.008 (g) of 1,3,6-hexanetricarboxylate per 1g of positive electrode active material.

[0202] Comparative Example 1

[0203] According to LiNi 0.83Co 0.12 Mn 0.05 O 2 Prepare nickel sulfate (NiSO) containing a nickel source in a stoichiometric ratio 4 ), cobalt sulfate (CoSO 4 ) and manganese source manganese sulfate (MnSO 4 ) solution, and mix it with sodium hydroxide (NaOH) solution and ammonia (NH 3 ·H 2 O) and LiOH solution are mixed uniformly in an atomized form, and dried at 200° C. to control the particle size of the particles to be 10 μm, and then calcined at 800° C. for 16 hours to obtain first particles.

[0204] The first particles, acetylene black and polyvinylidene fluoride are mixed uniformly in a weight ratio of 97.5:1.3:1.2, and an appropriate amount of N-methylpyrrolidone is added and stirred to prepare a uniform positive electrode active material slurry. The positive electrode active material slurry is coated on the positive electrode current collector aluminum foil and dried. Then the edges are trimmed, cut into pieces, divided into strips, and dried to obtain a positive electrode active material layer, and then the pieces are cut and the pole ears are welded to obtain a positive electrode.

[0205] Comparative Example 2

[0206] According to LiNi 0.83 Co 0.12 Mn 0.05 O 2 The stoichiometric ratio of Ni, Co, Mn and NCM precursors was prepared. 0.83 Co 0.12 Mn 0.05 (OH) 2 The precursor particles have a particle size of 3 μm, are uniformly mixed with lithium hydroxide (LiOH) and dried, and then calcined at 840° C. for 15 hours to obtain second particles.

[0207] The second particles, acetylene black and polyvinylidene fluoride are mixed uniformly in a weight ratio of 97.5:1.3:1.2, and an appropriate amount of N-methylpyrrolidone is added and stirred to prepare a uniform positive electrode active material slurry. The positive electrode active material slurry is coated on the positive electrode current collector aluminum foil and dried. Then the edges are trimmed, cut into pieces, divided into strips, and dried to obtain a positive electrode active material layer, and then the pieces are cut and the pole ears are welded to obtain a positive electrode.

[0208] Comparative Example 3

[0209] According to LiNi 0.83 Co 0.12 Mn 0.05 O 2 Prepare nickel sulfate (NiSO) containing a nickel source in a stoichiometric ratio 4), cobalt sulfate (CoSO 4 ) and manganese source manganese sulfate (MnSO 4 ) solution, and mix it with sodium hydroxide (NaOH) solution and ammonia (NH 3 ·H 2 O) and LiOH solution are mixed uniformly in an atomized form, and dried at 200° C. to control the particle size of the particles to be 10 μm, and then calcined at 800° C. for 16 hours to obtain first particles.

[0210] According to LiNi 0.83 Co 0.12 Mn 0.05 O 2 Prepare nickel sulfate (NiSO) containing a nickel source in a stoichiometric ratio 4 ), cobalt sulfate (CoSO 4 ) and manganese source manganese sulfate (MnSO 4 ) solution, and mix it with sodium hydroxide (NaOH) solution and ammonia (NH 3 ·H 2 O) and LiOH solution are mixed evenly in an atomized form, and dried at 200° C. to control the particle size of the particles to be 3 μm, and then calcined at 800° C. for 16 hours to obtain second particles.

[0211] The first particles, the second particles, acetylene black, and polyvinylidene fluoride were mixed in a weight ratio of 72.0:24.0:2.5:1.5 so that the weight ratio of the positive electrode active material including the first particles and the second particles was 96.0%.

[0212] Comparative Example 4

[0213] The first and second particles were prepared in the same manner as in Example 1. The first and second particles, acetylene black and polyvinylidene fluoride were mixed in a weight ratio of 86.4:9.6:2.5:1.5, so that the weight ratio of the positive electrode active material including the first and second particles was 96.0%.

[0214] Comparative Example 5

[0215] The first particles were obtained by a similar preparation method as in Example 5, and the particle pore size was controlled to be 0.5 μm by adjusting the sintering temperature and time. The second particles were obtained by the same preparation method as in Example 5, and then the first particles, the second particles, acetylene black and polyvinylidene fluoride were mixed in a weight ratio of 72.0:24.0:2.5:1.5, so that the weight ratio of the positive electrode active material containing the first particles and the second particles was 96.0%.

[0216] Comparative Example 6

[0217] The first particles were obtained by a similar preparation method as in Example 5, and the particle pore size was controlled to be 9 μm by adjusting the sintering temperature and time. The second particles were obtained by the same preparation method as in Example 5, and then the first particles, the second particles, acetylene black and polyvinylidene fluoride were mixed in a weight ratio of 72.0:24.0:2.5:1.5, so that the weight ratio of the positive electrode active material containing the first particles and the second particles was 96.0%.

[0218] 2. Preparation of negative electrode

[0219] Artificial graphite, acetylene black, styrene butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC) are fully stirred and mixed in a proper amount of deionized water solvent according to a weight ratio of 95:2:2:1 to form a uniform negative electrode active material slurry. The negative electrode active material slurry is coated on the negative electrode current collector copper foil and dried. Then, the negative electrode active material layer is obtained by trimming, cutting, stripping and drying, and then the negative electrode is obtained by cutting and welding the pole ears.

[0220] 3. Preparation of electrolyte

[0221] In a dry argon atmosphere, LiPF was added to a solvent consisting of propylene carbonate (PC), ethylene carbonate (EC), and diethyl carbonate (DEC) (weight ratio 1:1:1). 6 Mix well, LiPF 6 The concentration is 1.15 mol / L to obtain a basic electrolyte.

[0222] 4. Preparation of isolation membrane

[0223] A polyethylene (PE) porous polymer film was used as the separator.

[0224] 5. Preparation of lithium-ion batteries

[0225] The positive electrode, separator and negative electrode are stacked in order, wound, placed in an outer package, injected with electrolyte, and packaged. After the process of formation, degassing, trimming and other processes, a lithium-ion battery is obtained.

[0226] 2. Test Method

[0227] 1. Test method for element content in positive electrode active materials

[0228] The lithium-ion battery was fully discharged to 2.8V, the positive electrode was disassembled, and immersed in a DMC solution for 24 hours and dried. The obtained positive electrode was cut along the thickness direction of the positive electrode active material layer (perpendicular to the direction of the positive electrode current collector) using a cross-section polisher, and the cross section was observed under a scanning electron microscope (model JEOL 6390LV) and an X-ray energy dispersive spectrometer (model Oxford Link-7584EDS) to analyze the content of each element in the positive electrode active material and the element content in different regions.

[0229] 2. Test method for positive electrode gram capacity

[0230] In an environment of about 25°C, the lithium-ion battery is charged at a constant current and constant voltage at a charging current of 0.5C (i.e., the current value of the theoretical capacity is completely discharged within 2 hours) until the upper limit voltage is about 4.2V, and then discharged at a constant current at a discharge current of 0.2C until the final voltage is about 2.8V, and the first discharge capacity is calculated. The ratio of the first discharge capacity to the weight of the positive electrode is recorded as the positive electrode gram capacity. Four samples are tested for each embodiment or comparative example, and the average value is taken.

[0231] 3. Test method for high temperature cycle performance of lithium-ion batteries

[0232] Test the thickness of the lithium-ion battery to be tested, and record it as the initial thickness. In an environment of about 45°C, charge the lithium-ion battery at a constant current and constant voltage at a charging current of 2C until the upper limit voltage is about 4.2V, and then discharge it at a constant current at a discharge current of 6C until the final voltage is about 2.8V, and record the discharge capacity of the first cycle. Then, perform 500 charge and discharge cycles in the same steps, record the discharge capacity of the lithium-ion battery after 500 cycles, and test the thickness of the lithium-ion battery after 500 cycles.

[0233] The cycle capacity retention rate of lithium-ion batteries is calculated by the following formula:

[0234] Cycle capacity retention rate=(discharge capacity at the 500th cycle / discharge capacity at the first cycle)×100%.

[0235] The cycle expansion rate of lithium-ion batteries is calculated by the following formula:

[0236] Cycle expansion rate = (thickness after 500th cycle - initial thickness) / initial thickness × 100%

[0237] Four samples were tested for each embodiment or comparative example, and the average value was taken.

[0238] 4. Test method for high temperature storage performance of lithium-ion batteries

[0239] In an environment of about 25°C, the lithium-ion battery is charged at a constant current of 0.5C to a voltage higher than about 4.2V, and charged at a constant voltage of about 4.2V to a current lower than 0.05C, so that the battery is in a fully charged state of 4.2V. The thickness of the lithium-ion battery is tested. The fully charged battery is then placed in an oven at about 85°C for about 24 hours, and its thickness after storage is tested. The high-temperature storage expansion rate of the lithium-ion battery is calculated by the following formula:

[0240] High temperature storage expansion ratio = (thickness after storage - thickness before storage) / thickness before storage) × 100%.

[0241] Four samples were tested for each embodiment or comparative example, and the average value was taken.

[0242] 5. Test method for DC resistance of lithium-ion batteries

[0243] The lithium-ion battery was placed in an environment of 25°C for 5 minutes, then charged to 4.2V at a constant current of 2C, charged to 0.025C at a constant voltage of 4.2V, placed for 5 minutes, and then discharged to 2.8V at a rate of 0.2C. The discharge capacity at this time was recorded as the actual capacity of the lithium-ion battery. The following test uses this actual capacity to calculate the rate.

[0244] Then let the lithium-ion battery stand for 5 minutes in an environment of 25℃, charge to 4.2V at 2C constant current, charge to 0.025C at 4.2V constant voltage, and let stand for 120 minutes. The battery state of charge is 100%. Then discharge at 0.1C rate for 10 seconds, record the discharge current I1 and the voltage V1 after discharge, and the sampling interval of voltage, current and time during this period is 100 milliseconds; then discharge the lithium-ion battery at 1C rate for 360 seconds, record the discharge current 12 and the voltage V2 at 1 second of discharge, and the sampling interval of voltage, current and time during this period is 100 milliseconds. Calculate the DC positive voltage R of the lithium-ion battery by the following formula:

[0245] R = (V1-V2) / (I2-I1).

[0246] The DC resistance R measured when the battery state of charge is 100% is recorded as R1. Repeat the above steps 5 times, and the DC resistance R measured when the battery state of charge is 50% is recorded as R2.

[0247] 6. Test method for 10C discharge capacity retention rate of lithium-ion batteries

[0248] The lithium-ion battery was placed in a 25°C environment for 30 minutes, then charged to 4.2V at a constant current rate of 0.5C, charged to 0.05C at a constant voltage of 4.2V, and placed for 30 minutes, and then discharged to 2.8V at a rate of 0.2C. The discharge capacity at this time was recorded as the actual capacity C1 of the lithium-ion battery; after standing for 30 minutes, it was charged to 4.2V at a constant current rate of 0.5C, charged to 0.05C at a constant voltage of 4.2V, and placed for 30 minutes, and then discharged to 2.8V at a rate of 10C. The discharge capacity at this time was recorded as the actual capacity C2 of the lithium-ion battery. The 10C discharge capacity retention rate is calculated by the following formula:

[0249] 10C discharge capacity retention rate = C1 / C1.

[0250] 7. Test method for low temperature valley voltage of lithium-ion batteries

[0251] The lithium-ion battery was placed in a -20°C environment for 120 minutes, then charged to 4.2V at a constant current rate of 0.5C, charged to 0.05C at a constant voltage of 4.2V, placed for 30 minutes, and then discharged to 2.8V at a rate of 10C. The discharge voltage curve was recorded, and the low-temperature valley voltage was the minimum value in the voltage curve of the 100%-50% state of charge (SOC) interval at the beginning of discharge.

[0252] 3. Test Results

[0253] Table 1 shows the effects of different types of particles in the positive electrode active material on the initial discharge impedance, positive electrode gram capacity, high temperature cycle performance, high temperature storage performance, low temperature discharge capacity and rate performance of lithium-ion batteries.

[0254] The positive active material used in Comparative Example 1 only includes the first particles, which have a higher 10C discharge capacity retention rate (i.e., high rate performance), a higher low-temperature valley voltage (i.e., good low-temperature discharge capability) and a positive electrode gram capacity, but its initial discharge impedance is high and the cycle capacity retention rate under high temperature conditions is low and the cycle expansion rate and storage expansion rate are high (i.e., high-temperature cycle performance and high-temperature storage performance are poor), and the overall performance is poor. The positive active material used in Comparative Example 2 only includes the second particles, which have a higher positive electrode gram capacity and a higher cycle capacity retention rate and a lower cycle expansion rate and high-temperature storage expansion rate under high temperature conditions (i.e., good high-temperature cycle performance and high-temperature storage performance), but its initial discharge impedance is high and the 10C discharge capacity retention rate and low-temperature valley voltage are low (i.e., rate performance and low-temperature discharge capability are poor), and the overall performance is poor. The positive active material used in Comparative Example 3 includes the first particle and the second particle, but the second particle has a hole with a size greater than 1 μm, which causes the positive active material to be easily broken during the cycle and has poor overall performance.

[0255] The positive electrode active material used in Example 1 includes a combination of first particles and second particles, such as Figure 1 shown. Figure 2 Shown Figure 1 The enlarged view of the square area in the middle, where the first particle is shown by the circular dotted line, which has a pore structure, and the second particle is shown by the circular solid line, which does not have a pore structure. The combination of the first particle and the second particle can enable the lithium-ion battery to simultaneously achieve lower initial discharge impedance, higher cycle capacity retention rate, low temperature valley voltage and 10C discharge capacity retention rate, as well as lower cycle expansion rate and high temperature storage expansion rate, that is, it has good initial discharge kinetics, high temperature cycle performance, good high temperature storage performance, good low temperature discharge capacity and high rate performance, and has balanced comprehensive performance. The positive electrode active material used in Examples 2 and 3 also includes a combination of the first particle and the second particle, wherein the difference between Example 2 and Example 1 is only that the aluminum element is used to replace the manganese element, and the difference between Example 3 and Example 1 is only that the stoichiometric ratio of each element is different. The results show that changing the element types of the first particles and the second particles and the stoichiometric ratio of the elements will change the gram capacity, high temperature cycle performance, high temperature storage performance, low temperature discharge capacity and rate performance of the positive electrode of the lithium-ion battery to a certain extent, but overall, Examples 2 and 3 can achieve effects basically equivalent to Example 1, that is, they have lower initial discharge impedance, higher positive electrode gram capacity, good high temperature cycle performance, good high temperature storage performance, good low temperature discharge capacity and high rate performance at the same time, and have balanced comprehensive performance.

[0256] Table 2 shows the ratio a of the area of ​​the first particle to the area of ​​the second particle in the positive active material in the cross section in the thickness direction of the positive active material layer (or perpendicular to the direction of the positive current collector) and the effect of the pore size of the particles on the initial discharge impedance, positive electrode gram capacity, high temperature cycle performance, high temperature storage performance, low temperature discharge capacity and rate performance of the lithium ion battery. The results show that when the ratio a of the area of ​​the first particle to the area of ​​the second particle is greater than 9 (Comparative Example 4), the first particle content is too much, resulting in the positive active material being prone to breakage during the cycle, making the high temperature storage expansion rate and high temperature cycle expansion rate of the lithium ion battery high and the high temperature cycle capacity retention rate low, and the overall performance is poor. When the ratio a of the area of ​​the first particle to the area of ​​the second particle is not greater than 9, the lithium ion battery has a low initial discharge impedance, a high positive electrode gram capacity, good high temperature cycle performance, good high temperature storage performance, good low temperature discharge capacity and high rate performance, and has a balanced overall performance. As the area ratio a decreases, the high temperature cycle capacity retention rate of the lithium ion battery gradually increases, which can further balance the overall performance of the lithium ion battery.

[0257] When the pore size of the first particle is less than 1 μm (Comparative Example 5), the low-temperature valley voltage and 10C discharge capacity retention rate of the lithium-ion battery are low, and the overall performance is poor. When the pore size of the first particle is greater than 8 μm (Comparative Example 6), the high-temperature storage expansion rate and high-temperature cycle expansion rate of the lithium-ion battery are high and the high-temperature cycle capacity retention rate is low, and the overall performance is poor. When the pore size of the first particle is in the range of 1 μm to 8 μm and the pore size of the second particle is below 1 μm (Examples 5-11), it helps to further balance the initial discharge impedance, positive electrode gram capacity, high-temperature cycle performance, high-temperature storage performance, low-temperature discharge capacity and rate performance of the lithium-ion battery.

[0258] Table 3-9 further shows the effect of the positive electrode and the electrolyte on the performance of the lithium-ion battery. In each embodiment shown in Table 3-9, the pore size of the first particle is 3 μm, the second particle has no pores (i.e., the pore size is 0 μm), and the ratio a of the area of ​​the first particle to the area of ​​the second particle is 3.

[0259] Table 3 shows the effect of the average particle size of the first particle and the second particle in the positive electrode active material on the initial discharge impedance, positive electrode gram capacity, high temperature cycle performance, high temperature storage performance, low temperature discharge capacity and rate performance of the lithium ion battery. The results show that when the particle size of the first particle is 7μm to 15μm and the average particle size of the second particle is 1μm to 7μm and does not include 7μm, the lithium ion battery has low initial discharge impedance, high positive electrode gram capacity, good high temperature cycle performance, good high temperature storage performance, good low temperature discharge capacity and high rate performance, and has balanced comprehensive performance.

[0260] Table 4 shows the effect of the particle size of the primary particles in the first particles of the positive electrode active material on the initial discharge impedance, positive electrode gram capacity, high temperature cycle performance, high temperature storage performance, low temperature discharge capacity and rate performance of the lithium ion battery. The results show that when the average particle size of the primary particles in the first particles in the positive electrode active material is not more than 3μm, it helps to further reduce the storage expansion rate and cycle expansion rate of the lithium ion battery under high temperature conditions and further improve the cycle capacity retention rate of the lithium ion battery under high temperature conditions, and achieve balanced comprehensive performance. When the first particle in the positive electrode active material includes at least 5 primary particles with a particle size of 0.5μm or more (particle size is not more than 3μm), the side reactions on the surface of the first particles are reduced, and the stress between the first particles during the cycle process is reduced, thereby further improving the high temperature storage performance and high temperature cycle performance of the lithium ion battery, so that the lithium ion battery has a more superior comprehensive performance.

[0261] Table 5 shows the effects of the surface coating of the first and second particles in the positive electrode active material on the initial discharge impedance, positive electrode gram capacity, high temperature cycle performance, high temperature storage performance, low temperature discharge capacity and rate performance of lithium-ion batteries. Figure 3 As shown, the surface of the first particle in the positive electrode active material layer in Example 27 is coated with boron, so that the boron content of the surface area of ​​the first particle is higher than that of the central area. Compared with Example 26, it has a higher positive electrode gram capacity and a lower high-temperature storage expansion rate, thereby further balancing the comprehensive performance of the lithium-ion battery. Figure 4 As shown, the surface of the second particle may also be coated with boron (Example 28). When the boron content of the first particle is greater than the boron content of the second particle, the initial discharge impedance (R1 / R2) of the lithium ion battery can be significantly reduced, and the 10C discharge capacity retention rate and low temperature valley voltage of the lithium ion battery can be improved, thereby further balancing the comprehensive performance of the lithium ion battery.

[0262] Table 6 shows the relationship between the weight percentage c of the positive electrode active material and the ratio a of the cross-sectional area of ​​the first particle to the cross-sectional area of ​​the second particle on the positive electrode gram capacity, high temperature cycle performance, high temperature storage performance, low temperature discharge capacity and rate performance of the lithium-ion battery. The results show that when a and c meet c≤0.02×a / (a+1)+0.97, the lithium-ion battery has low initial discharge impedance, high positive electrode gram capacity, good high temperature cycle performance, good high temperature storage performance, good low temperature discharge capacity and high rate performance, and has balanced comprehensive performance. As the weight percentage c of the positive electrode active material decreases, the 10C discharge capacity retention rate and high temperature cycle capacity retention rate of the lithium-ion battery gradually increase, and the high temperature cycle expansion rate gradually decreases, which can further balance the comprehensive performance of the lithium-ion battery.

[0263] Table 7 shows the effects of different doping elements in the first particle and the second particle in the positive electrode active material on the initial discharge impedance, positive electrode gram capacity, high temperature cycle performance, high temperature storage performance, low temperature discharge capacity and rate performance of the lithium ion battery. The results show that when the first particle or the second particle is doped with zirconium (Zr), aluminum (Al), magnesium (Mg) or yttrium (Y) elements, the positive electrode active material has a more stable structure, which helps to further improve the cycle expansion rate, cycle capacity retention rate and storage expansion rate of the lithium ion battery under high temperature conditions, thereby further balancing the comprehensive performance of the lithium ion battery.

[0264] Table 8 shows the effect of the porosity of the positive electrode active material layer on the initial discharge impedance, positive electrode gram capacity, high temperature cycle performance, high temperature storage performance, low temperature discharge capacity and rate performance of the lithium-ion battery. The results show that when the porosity of the positive electrode active material layer is 10% to 50%, the storage expansion rate and cycle expansion rate of the lithium-ion battery under high temperature conditions can be further reduced, and the cycle capacity retention rate, 10C discharge capacity retention rate and low temperature valley voltage of the lithium-ion battery under high temperature conditions can be further improved, so that the lithium-ion battery has low initial discharge impedance, high positive electrode gram capacity, good high temperature cycle performance, good high temperature storage performance, good low temperature discharge capacity and high rate performance, and has balanced comprehensive performance.

[0265] Table 9 shows the influence of the content of polynitrile compound in electrolyte relative to positive electrode active material on positive electrode gram capacity, high temperature cycle performance, high temperature storage performance, low temperature discharge capacity and rate performance of lithium ion battery. The results show that when the electrolyte contains 0.0003g to 0.005g polynitrile compound based on 1g of the positive electrode active material, the 10C discharge capacity retention rate and low temperature valley voltage of the lithium ion battery can be further improved, thereby further balancing the comprehensive performance of the lithium ion battery.

[0266]

[0267]

[0268]

[0269]

[0270] References to "embodiments", "partial embodiments", "one embodiment", "another example", "example", "specific example" or "partial example" throughout the specification mean that at least one embodiment or example in the present application includes the specific features, structures, materials or characteristics described in the embodiment or example. Therefore, descriptions appearing in various places throughout the specification, such as: "in some embodiments", "in an embodiment", "in one embodiment", "in another example", "in an example", "in a specific example" or "example", do not necessarily refer to the same embodiment or example in the present application. In addition, the specific features, structures, materials or characteristics herein may be combined in one or more embodiments or examples in any suitable manner.

[0271] Although illustrative embodiments have been demonstrated and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the spirit, principles and scope of the present application.

Claims

1. An electrochemical device comprising: A positive electrode and an electrolyte, wherein the positive electrode comprises a positive electrode current collector and a positive electrode active material layer, wherein the positive electrode active material layer comprises a positive electrode active material, wherein the positive electrode active material comprises a first particle and a second particle, wherein the first particle is a secondary particle, and the second particle is a primary particle, wherein: The first particles have pores, and the size of the pores is 1 μm to 8 μm; The pore size of the second particles is less than 1 μm; In a cross section in the thickness direction of the positive electrode active material layer, a ratio a of an area of ​​the first particle to an area of ​​the second particle is not greater than 9; Wherein, the electrochemical device has a DC resistance R1 for the first 1 second of discharge time when it reaches 100% state of charge at 25°C, and the electrochemical device has a DC resistance R2 for the first 1 second of discharge time when it reaches 50% state of charge at 25°C, 1<R1 / R2≤1.4; The first particle and the second particle each independently contain the formula Li b Ni x Co y M1 1-x-y-z M2 z O2 compounds, wherein: M1 includes at least one of Mn or Al; M2 includes at least one of Mg, Al, Ti, Zr, La, Y, Sr or Ce; 0.1≤b≤1.1; 0.5≤x<1; 0≤y<0.5; and 0≤z≤0.01。 2 . The electrochemical device according to claim 1 , wherein the average particle size of the first particles is 7 μm to 15 μm; and the average particle size of the second particles is 1 μm to 7 μm, excluding 7 μm. 3 . The electrochemical device according to claim 2 , wherein the first particles include primary particles, and an average particle size of the primary particles is not greater than 3 μm. The electrochemical device according to claim 3 , wherein the first particles include at least five primary particles having a particle size of 0.5 μm or more. 5 . The electrochemical device according to claim 1 , wherein the first particles contain boron, and a boron content in a surface region of the first particles is higher than a boron content in a central region. 6 . The electrochemical device according to claim 1 , wherein the first particles and the second particles contain boron, and a boron content of the first particles is greater than a boron content of the second particles. 7 . The electrochemical device according to claim 1 , wherein based on the total weight of the positive electrode active material layer, the weight percentage c of the positive electrode active material and the ratio a satisfy the following relationship: c≤0.02×a / (a+1)+0.

97. 8 . The electrochemical device according to claim 1 , wherein the positive electrode active material layer has a porosity of 10% to 50%. 9 . The electrochemical device according to claim 1 , wherein the electrolyte comprises a polynitrile compound, and the content of the polynitrile compound is 0.0003 g to 0.005 g per 1 g of the positive electrode active material.

10. The electrochemical device according to claim 9, wherein the polynitrile compound comprises at least one of 1,3,6-hexanetricarboxylic acid nitrile, 1,2,6-hexanetricarboxylic acid nitrile, 1,3,5-pentanetricarboxylic acid nitrile, 1,2,3-tris(2-cyanato)propane, succinonitrile or adiponitrile.

11. An electronic device comprising the electrochemical device according to any one of claims 1 to 10.