A composite electrode material and preparation method thereof and potassium ion battery
By using carbon-based nanocage-filled copper oxide composite electrode materials in potassium-ion batteries, the problem of copper oxide volume expansion is solved, high-rate performance and cycle stability are achieved, and the electrochemical performance and Coulombic efficiency of potassium-ion batteries are improved.
Patent Information
- Application Number
- CN202210218017.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-03-08
AI Technical Summary
In potassium-ion batteries, the volume expansion of copper oxide in conventional lithium-ion battery materials causes material structural distortion, resulting in lower capacity, rate performance and cycle performance, which limits the development of potassium-ion batteries.
Composite electrode materials using carbon-based nanocages filled with copper oxide provide ion transmission channels through the three-dimensional hierarchical structure and high specific surface area of the carbon-based nanocages, inhibit the volume expansion of copper oxide, and improve conductivity and cycle stability.
The composite electrode material has achieved excellent electrochemical performance and high cycle stability at high rates. The discharge specific capacity reaches 409~475mAh·g-1 in the range of 0.2~1A·g-1, and the Coulombic efficiency is as high as 99.5~99.6%. Significantly improved potassium-ion battery performance.
Smart Images

Figure CN114566635B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrode materials, and in particular to a composite electrode material and a preparation method thereof, and a potassium ion battery. Background Art
[0002] Secondary batteries - lithium-ion batteries have the advantages of high energy density, high output power, low self-discharge, no memory effect, wide operating temperature range, long cycle life and relatively "friendly" to the environment. The working principle of potassium-ion batteries is very similar to that of lithium-ion batteries. During the battery charging process, potassium ions migrate from the positive electrode to the negative electrode through the electrolyte, and electrons with equal charge in the external circuit also migrate from the positive electrode to the negative electrode. During discharge, potassium-ion batteries migrate in the opposite working mode. However, potassium ions The size is significantly larger than that of lithium-ion If conventional lithium-ion battery materials are directly used in potassium-ion batteries, the process of potassium ions being extracted / embedded into the battery materials will often cause the material structure to distort or even collapse, ultimately leading to lower capacity, extremely poor rate performance and cycle performance, and even some materials that do not have potassium storage properties at all, thus limiting the development of potassium-ion batteries. Therefore, research on potassium-ion battery electrode materials is very important. In the field of energy storage, copper oxide, as a conversion negative electrode material, has a high theoretical specific capacity (675mAh g -1 ), but it faces problems such as large volume expansion during charge and discharge, poor conductivity, and easy loss of active materials during long cycles.
[0003] At present, researchers mainly use morphology control, composition regulation, and hybridization with conductive carbon to improve the electrochemical performance of electrode materials. By loading nanoparticles on carbon, the conductivity can be effectively improved, but the open structure cannot effectively prevent the loss of active components, and the electrode structure is prone to collapse during repeated charging and discharging, which ultimately leads to rapid capacity decay. By using carbon-wrapped nanoparticles, the active components can be retained to a certain content, but in the case of K + There are not enough cavities to accommodate the large volume changes during the deposition / stripping process, which usually leads to the rupture of the carbon coating and the rapid degradation of electrochemical performance. For example, Cao et al. reported "CuO nanoplates for high-performance potassium-ion batteries". They prepared CuO nanoplates by hydrothermal method and -1 After 100 cycles, the battery capacity is only 206 mAh g -1Specific capacity, which seriously limits the development of CuO negative electrode materials. The invention patent with publication number CN110311109B reports "a preparation method for negative electrode materials of copper oxide composite lithium batteries". The patent stirs and ball-mills copper oxide powder and graphite powder, and performs drying treatment, carbonizes the mixture, adds a conductive agent and a binder to mix; adds the relevant raw materials to the thickener solution, mixes to obtain a mixture, and then mixes and stirs it with the weighed polyvinylidene fluoride to obtain a negative electrode gel mixture. Although the process of this patent is simple, the volume expansion problem of CuO particles is still difficult to solve, which limits the improvement of the electrochemical performance of the electrode material.
[0004] Therefore, there is an urgent need to provide a composite electrode material that can inhibit the volume expansion of copper oxide so that it has excellent rate performance and high cycle stability after being prepared into a battery. Summary of the invention
[0005] The object of the present invention is to provide a composite electrode material and a preparation method thereof and a potassium ion battery. The composite electrode material provided by the present invention has excellent rate performance and high cycle stability after being prepared into a battery and can inhibit the volume expansion of copper oxide. After being prepared into a battery, the composite electrode material has excellent rate performance and high cycle stability.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The invention provides a composite electrode material, comprising a carbon-based nanocage and copper oxide filled in the carbon-based nanocage; the mass of the copper oxide is 10% to 70% of the total mass of the composite electrode material.
[0008] Preferably, the carbon-based nanocage includes one of a carbon nanocage, a nitrogen-doped carbon nanocage, a sulfur-doped carbon nanocage and a phosphorus-doped carbon nanocage.
[0009] Preferably, the specific surface area of the carbon-based nanocage is 600 to 2000 m 2 / g.
[0010] The present invention also provides a method for preparing the composite electrode material described in the above technical solution, comprising the following steps:
[0011] The present invention also provides a method for preparing the composite electrode material, comprising the following steps:
[0012] (1) Under vacuum conditions, the carbon-based nanocage is sequentially immersed in a copper oxide precursor solution and post-treated to obtain a composite electrode precursor;
[0013] (2) thermally decomposing the composite electrode precursor obtained in step (1) to obtain a composite electrode material; the thermal decomposition atmosphere is argon or nitrogen.
[0014] Preferably, the post-treatment in step (1) comprises filtering and drying performed sequentially.
[0015] Preferably, the impregnation and post-treatment in step (1) are repeated 2 to 5 times.
[0016] Preferably, the copper oxide precursor solution in step (1) comprises one or more of copper nitrate solution, copper acetate solution, cupric chloride solution, cuprous acetate solution, and cuprous chloride solution.
[0017] Preferably, the concentration of copper ions in the copper oxide precursor solution in step (1) is 0.05 to 2.0 mol / L.
[0018] Preferably, the heating rate of the thermal decomposition in step (2) is 5 to 20°C / min, the final temperature of the thermal decomposition is 180 to 400°C, and the total time of the thermal decomposition from the start of heating to the end of the thermal decomposition is 20 to 360 minutes.
[0019] The present invention also provides a potassium ion battery, comprising the composite electrode material described in the above technical solution or the composite electrode material prepared by the preparation method described in the above technical solution.
[0020] The technical solution of the present invention provides a composite electrode material, including a carbon-based nanocage and copper oxide filled inside the carbon-based nanocage; the mass of the copper oxide is 10% to 70% of the total mass of the composite electrode material. The present invention fills the copper oxide into the internal cavity of the carbon-based nanocage, and utilizes the three-dimensional hierarchical structure and high specific surface area of the carbon-based nanocage to provide a channel for ion transmission for the composite electrode material. At the same time, the high conductivity of the carbon-based nanocage is utilized to improve the conductivity of the copper oxide. In addition, the carbon-based nanocage has a cavity confinement effect, which inhibits the volume expansion of the copper oxide, thereby greatly improving the rate performance and cycle stability of the composite electrode material. The results of the embodiment show that the battery assembled from the composite electrode material provided by the present invention is subjected to electrochemical performance testing on a battery testing system. The battery has a high conductivity of 0.2 to 1 A·g -1 The following has 409~475mAh·g -1 The specific capacity is even higher at high rates of 2 to 5 A g -1 At a current density of 2.5 %, its discharge capacity can reach 218 mAh g -1 The specific capacity shows excellent rate performance; at 1A·g -1 At a current density of 1.5 mAh g / cm2, the material can still maintain a charge capacity of 238 to 288 mAh g / cm2 after 500 cycles. -1 The discharge specific capacity and coulombic efficiency are as high as 99.5-99.6%, which shows that the material has extremely high cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a low-magnification transmission image of CuO@hNCNCs prepared in Example 1 of the present invention;
[0022] Figure 2 This is a high-magnification transmission image of CuO@hNCNCs prepared in Example 1 of the present invention;
[0023] Figure 3 This is a rate performance test diagram of a potassium ion battery assembled in Application Example 1 of the present invention;
[0024] Figure 4 This is a test diagram of the cycle stability performance of the potassium ion battery assembled in Application Example 1 of the present invention;
[0025] Figure 5 This is a rate performance test diagram of a potassium ion battery assembled in Application Example 2 of the present invention;
[0026] Figure 6 This is a test chart of the cycle stability performance of the assembled potassium ion battery assembled according to Application Example 2 of the present invention. DETAILED DESCRIPTION
[0027] The invention provides a composite electrode material, comprising a carbon-based nanocage and copper oxide filled in the carbon-based nanocage; the mass of the copper oxide is 10% to 70% of the total mass of the composite electrode material.
[0028] The composite electrode material provided by the present invention includes a carbon-based nanocage. The present invention uses the carbon-based nanocage as a confined component of copper oxide to inhibit the volume expansion of copper oxide, thereby greatly improving the rate performance and cycle stability of the composite electrode material, and the three-dimensional hierarchical structure and high specific surface area of the carbon-based nanocage can provide a channel for ion transmission for the composite electrode material, and the high conductivity of the carbon-based nanocage can also improve the conductivity of copper oxide.
[0029] In the present invention, the carbon-based nanocage preferably includes one of carbon nanocage, nitrogen-doped carbon nanocage, sulfur-doped carbon nanocage and phosphorus-doped carbon nanocage. The present invention is more conducive to improving the rate performance and cycle stability of the composite electrode material by selecting the above-mentioned types of carbon-based nanocages.
[0030] The present invention has no particular limitation on the source of the carbon-based nanocages, and any carbon-based nanocages prepared by a preparation method well known to those skilled in the art or commercially available carbon-based nanocages may be used.
[0031] In the present invention, the carbon nanocage is preferably prepared by the method disclosed in Chinese patent CN101284663A; the nitrogen-doped carbon nanocage is preferably prepared by the method disclosed in Chinese patent CN102530922A; the sulfur-doped carbon nanocage is preferably prepared by co-impregnation and pyrolysis of a metal complex and thiocyanate, or prepared by chemical vapor deposition using thiophene sulfur; the phosphorus-doped carbon nanocage is preferably prepared by chemical vapor deposition using hexamethylphosphoric triamide.
[0032] In the present invention, when the carbon-based nanocage is preferably a sulfur-doped carbon nanocage, the doping amount of sulfur in the sulfur-doped carbon nanocage is preferably 0.2-4.0% of the total mass of the composite electrode material, and more preferably 2-3%. By selecting the sulfur-doped carbon nanocage, the present invention can utilize sulfur doping to contribute a part of the capacity, can fill more copper oxide, and can also expand the interlayer spacing of the carbon layer to a certain extent, which is more conducive to the transmission of ions.
[0033] In the present invention, when the carbon-based nanocage is preferably a phosphorus-doped carbon nanocage, the doping amount of the phosphorus element in the phosphorus-doped carbon nanocage is preferably 0.2 to 5.0% of the total mass of the composite electrode material, and more preferably 1 to 2.5%. By selecting the phosphorus-doped carbon nanocage, the present invention can utilize phosphorus doping to contribute a part of the capacity, and can fill more copper oxide, thereby effectively improving the electrochemical performance of the composite electrode material.
[0034] In the present invention, the specific surface area of the carbon-based nanocage is preferably 600 to 2000 m 2 / g, more preferably 800 to 1300 m 2 / g. By controlling the specific surface area of the carbon-based nanocage within the above range, the present invention can provide more ion transmission channels for the composite electrode material, thereby effectively improving the rate performance and cycle stability of the composite electrode material.
[0035] The composite electrode material provided by the present invention comprises copper oxide filled in the carbon-based nano cage. The present invention adopts copper oxide as the active component of the composite material, has good electrochemical performance, and is more suitable for the negative electrode material of potassium ion battery.
[0036] In the present invention, the mass of the copper oxide is 10% to 70% of the total mass of the composite electrode material, preferably 20% to 60%, more preferably 30% to 50%, and most preferably 40%. By controlling the filling mass of copper oxide in the composite electrode material within the above range, the present invention can effectively ensure that the copper oxide avoids volume expansion under the confinement of the carbon-based nanocage, greatly improves the potassium storage performance of the copper oxide, and thus better exerts its excellent electrochemical performance.
[0037] The composite electrode material provided by the present invention can avoid the volume expansion problem of copper oxide, has higher rate performance and cycle stability, and is more suitable as a negative electrode material for potassium ion batteries. Compared with conventional carbon-coated materials, the copper oxide active substance has more space for buffering volume expansion in the carbon-based nanocage. Even if the copper oxide active substance is pulverized, it can remain in the carbon-based nanocage without being lost, and the material continues to play its role.
[0038] The present invention also provides a method for preparing the composite electrode material described in the above technical solution, comprising the following steps:
[0039] (1) Under vacuum conditions, the carbon-based nanocage is sequentially immersed in a copper oxide precursor solution and post-treated to obtain a composite electrode precursor;
[0040] (2) thermally decomposing the composite electrode precursor obtained in step (1) to obtain a composite electrode material; the thermal decomposition atmosphere is argon or nitrogen.
[0041] The present invention sequentially immerses and post-treats the carbon-based nano cage in a copper oxide precursor solution under vacuum conditions to obtain a composite electrode precursor.
[0042] In the present invention, the copper oxide precursor solution preferably includes one or more of a copper nitrate solution, a copper acetate solution, a cupric chloride solution, a cuprous acetate solution, and a cuprous chloride solution. In the present invention, the solvent in the copper oxide precursor solution is preferably water or ethanol. The present invention is more conducive to filling the copper oxide precursor solution into the carbon-based nano cage by selecting the above-mentioned types of copper oxide precursor solution.
[0043] In the present invention, the concentration of copper ions in the copper oxide precursor solution is preferably 0.05 to 2.0 mol / L, more preferably 0.1 to 1.0 mol / L. By controlling the concentration of copper ions within the above range, the present invention is more conducive to quickly filling the carbon-based nanocages and regulating their filling amount.
[0044] In the present invention, the method for preparing the copper oxide precursor solution is preferably: mixing one or more of copper nitrate, copper acetate, copper chloride, cuprous acetate, and cuprous chloride with water or ethanol and then performing ultrasonic treatment. The present invention has no special requirements on the parameters of the ultrasonic treatment, as long as the prepared copper oxide precursor solution can be ensured to be uniform.
[0045] In the present invention, the vacuum degree of the vacuum condition is preferably 0.1 to 100 Pa, more preferably 1 to 10 Pa. By controlling the conditions for preparing the composite electrode precursor to be vacuum conditions and controlling the vacuum degree to be within the above range, the copper oxide precursor solution can be better filled into the cavity of the carbon-based nanocage, and the copper oxide precursor solution can be prevented from being oxidized prematurely to form precipitation.
[0046] In the present invention, the impregnation process is preferably stirred at the same time; the stirring time is preferably 60 to 360 minutes, more preferably 120 to 180 minutes. The present invention is more conducive to the copper oxide precursor solution being fully and evenly filled into the cavity of the carbon-based nanocage by stirring at the same time during the impregnation process.
[0047] In the present invention, the post-treatment preferably includes filtration and drying performed in sequence.
[0048] In the present invention, the drying is preferably freeze drying; the freeze drying temperature is preferably -60 to -30°C, more preferably -45°C; the freeze drying time is preferably 24 to 48 hours, more preferably 30 to 40 hours.
[0049] In the present invention, the impregnation and post-treatment are preferably repeated 2 to 5 times, more preferably 3 times. The present invention is more conducive to regulating the filling amount of copper oxide and making the filling effect more uniform by sequentially performing impregnation and post-treatment and repeating them multiple times.
[0050] After the post-treatment is completed, the present invention preferably sequentially washes and dries the post-treatment product to obtain a composite electrode precursor. The present invention can effectively remove the copper oxide precursor solution remaining on the surface through washing and drying.
[0051] In the present invention, the drying is preferably freeze drying; the freeze drying temperature is preferably -60 to -30°C, more preferably -45°C; the freeze drying time is preferably 24 to 48 hours, more preferably 30 to 40 hours.
[0052] After obtaining the composite electrode precursor, the composite electrode precursor is thermally decomposed to obtain the composite electrode material. The present invention can decompose the precursor in the carbon-based nano cage to form copper oxide by thermally decomposing the composite electrode precursor.
[0053] In the present invention, the atmosphere of the thermal decomposition is argon or nitrogen. In the present invention, the flow rate of the argon or nitrogen is preferably 50 to 400 mL / min, more preferably 100 to 200 mL / min. The present invention can effectively prevent the carbon-based nanocages from being oxidized and burned by adopting an argon or nitrogen atmosphere for thermal decomposition and controlling its flow rate within the above range, thereby ensuring that the structure of the carbon-based nanocages is more complete, thereby better confining copper oxide and preventing its volume expansion.
[0054] In the present invention, the heating rate of the thermal decomposition is preferably 5-20°C / min, more preferably 10-15°C / min; the final temperature of the thermal decomposition is preferably 180-400°C, more preferably 200-280°C; the total time of thermal decomposition required from the start of heating to the end of thermal decomposition is preferably 20-360min, more preferably 30-120min. The present invention can effectively ensure that the copper oxide precursor is fully oxidized to copper oxide while avoiding damage to the structure of the carbon-based nanocage by controlling the heating rate, final temperature and total time of thermal decomposition within the above range, which is more conducive to improving the electrochemical properties of copper oxide and avoiding its volume expansion under the action of carbon-based nanocages, so that the composite electrode material has excellent rate performance and cycle stability.
[0055] The preparation method of the composite electrode material provided by the present invention can effectively control the filling amount of copper oxide to ensure that the copper oxide is filled sufficiently and evenly; moreover, the parameters are easy to control, the material is safe and environmentally friendly, the cost is low, and the material is more suitable for large-scale production.
[0056] The present invention also provides a potassium ion battery, comprising the composite electrode material described in the above technical solution or the composite electrode material prepared by the preparation method described in the above technical solution.
[0057] In the present invention, the potassium ion battery preferably further comprises conductive carbon black and a binder; the conductive carbon black is preferably SuperP carbon black; the binder preferably comprises one or both of polyvinylidene fluoride (PVDF) and sodium carboxymethyl cellulose (CMC). In the present invention, the mass ratio of the composite electrode material to the conductive carbon black and the binder is preferably (6-10):1:1; more preferably 8:1:1. The present invention is more conducive to improving the conductivity of the potassium ion battery by controlling the mass ratio of the composite electrode material to the conductive carbon black and the binder within the above range.
[0058] The potassium ion battery provided by the present invention can avoid the volume expansion problem of copper oxide by using the composite electrode material provided by the present invention, and has higher rate performance and cycle stability, and has better application prospects.
[0059] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0060] Example 1
[0061] The composite electrode material provided in this embodiment is composed of a carbon-based nanocage and copper oxide filled in the carbon-based nanocage; the mass of the copper oxide is 59% of the total mass of the composite electrode material; the carbon-based nanocage is a nitrogen-doped carbon nanocage (hNCNCs), and the specific surface area of the carbon-based nanocage is 1150 m 2 / g.
[0062] The preparation method of the composite electrode material is specifically the following steps:
[0063] (1) Under vacuum conditions, the carbon-based nanocage is sequentially immersed and post-treated in a copper oxide precursor solution to obtain a composite electrode precursor; more specifically: 1.208 g of copper nitrate is weighed and added to 50 mL of deionized water for dissolution, stirred for 30 min, and ultrasonicated for 20 min for standby use; 100 mg of carbon-based nanocage is weighed and added to a two-necked flask, and a vacuum pump is used to evacuate the flask to below 2 Pa; the copper nitrate aqueous solution prepared above is added to the above vacuum pump, stirred for 2 h, filtered, freeze-dried, and the above steps are repeated 3 times to prepare a composite material precursor (copper nitrate@carbon-based nanocage); the composite material precursor is washed and dried before use, and the process is repeated 3 times;
[0064] (2) thermally decomposing the composite electrode precursor obtained in step (1) to obtain a composite electrode material; the thermal decomposition atmosphere is argon. More specifically, the composite electrode precursor is thermally decomposed at a heating rate of 5°C / min to 250°C in an Ar environment for 1 hour to obtain a composite electrode material, which is recorded as CuO@hNCNCs.
[0065] The CuO@hNCNCs prepared in Example 1 were observed for microstructure using a low-magnification transmission electron microscope. Figure 1 As shown. Figure 1 It can be seen that the CuO nanoparticles are located inside the hNCNCs cavity and are wrapped by hNCNCs. Such a structure is more conducive to inhibiting the volume expansion of CuO particles during the cycle. At the same time, the carbon layer can greatly improve the conductivity of the material and further increase the electrochemical properties of the material.
[0066] The microstructure of the CuO@hNCNCs prepared in Example 1 was observed using a high-magnification transmission electron microscope. Figure 2 As shown. Figure 2 It can be seen that the interplanar spacing of the particles inside the hNCNCs cavity is 0.252 nm, which is the (-111) crystal plane of CuO, indicating that the particle is CuO.
[0067] Application Example 1
[0068] Take 80 mg of the CuO@hNCNCs prepared in Example 1, mix them evenly with 10 mg of SuperP carbon black and 10 mg of PVDF, add 0.5 mL of NMP (N-methylpyrrolidone) as a solvent, mix them evenly again and coat them on copper foil, dry them in a vacuum oven at 80°C for 24 hours, and then punch them into 10 mm small discs for button cell assembly. Using 1M KFSI (EC:DEC=1:1, V:V) as the electrolyte, the counter electrode as the metal potassium sheet, and the glass fiber as the separator, the assembled battery was tested for electrochemical performance on the battery test system.
[0069] The rate performance test results of the potassium ion battery assembled using the CuO@hNCNCs prepared in Example 1 are as follows: Figure 3 shown. Figure 3 The horizontal axis is the number of cycles, and the vertical axis is the specific capacity. Figure 3 It can be seen that the battery assembled in Application Example 1 has a -1 475mAh·g -1 The specific capacity is even higher at a high rate of 5A·g -1 At a current density of 2.5 %, its discharge capacity can reach 218 mAh g -1 The specific capacity shows excellent rate performance. -1 At a current density of 1.5 %, the material can still maintain 288 mAh g after 500 cycles. -1 The discharge specific capacity is as high as 99.5%, and the coulombic efficiency is as high as 99.5%, with extremely high cycle stability.
[0070] The test results of the cycle stability performance of the potassium ion battery assembled using the CuO@hNCNCs prepared in Example 1 are as follows: Figure 4 shown. Figure 4 The horizontal axis in the middle is the number of cycles, the vertical axis on the left is the specific capacity, and the vertical axis on the right is the coulombic efficiency. Figure 4 It can be seen that at 1A·g -1 At a current density of 1.5 %, the material can still maintain 288 mAh g after 500 cycles. -1 The discharge specific capacity and coulombic efficiency are as high as 99.5%, which shows that the material has extremely high cycle stability.
[0071] Example 2
[0072] The composite electrode material provided in this embodiment is composed of a carbon-based nanocage and copper oxide filled in the carbon-based nanocage; the mass of the copper oxide is 62% of the total mass of the composite electrode material; the carbon-based nanocage is a carbon nanocage (hCNCs), and the specific surface area of the carbon-based nanocage is 1260 m 2 / g.
[0073] The preparation method of the composite electrode material is specifically the following steps:
[0074] (1) Under vacuum conditions, the carbon-based nanocages are sequentially impregnated and post-treated in a copper oxide precursor solution to obtain a composite electrode precursor; more specifically: 2.416 g of copper nitrate is weighed and added to 50 mL of deionized water for dissolution, stirred for 30 min, and ultrasonicated for 20 min for standby use. 100 mg of hCNCs is weighed and added to a two-necked flask, and a vacuum pump is used to evacuate the flask to below 5 Pa; the copper nitrate aqueous solution prepared above is added to the above vacuum pump, stirred for 2 h, filtered, freeze-dried, and the above steps are repeated twice to prepare a composite material precursor (copper nitrate @ carbon-based nanocage); the composite material precursor is washed and dried before use, and the process is repeated three times.
[0075] (2) thermally decomposing the composite electrode precursor obtained in step (1) to obtain a composite electrode material; the thermal decomposition atmosphere is argon. More specifically, the composite electrode precursor obtained in step (1) is thermally decomposed at a heating rate of 5°C / min to 250°C in an Ar environment for 1 hour to obtain a composite electrode material, which is recorded as CuO@hCNCs.
[0076] Application Example 2
[0077] Take 80mg of CuO@hCNCs prepared in Example 2, mix with 10mg SuperP carbon black and 10mg PVDF, add 0.5mL NMP (N-methylpyrrolidone) as solvent, mix again and coat on copper foil, dry in a vacuum oven at 80℃ for 24h, and then punch into 10mm small discs for button cell assembly. Using 1M KFSI (EC:DEC=1:1, V:V) as electrolyte, metal potassium sheet as counter electrode, glass fiber as separator, the assembled battery is tested for electrochemical performance on the battery test system.
[0078] The rate performance test results of the potassium ion battery assembled using the CuO@hCNCs prepared in Example 2 are as follows: Figure 5 shown. Figure 5 The horizontal axis is the number of cycles, and the vertical axis is the specific capacity. Figure 5 It can be seen that the negative electrode material has a -1 With 409mAh g -1 The specific capacity, even at a high rate of 2A·g -1 At a current density of 2.5 %, its discharge capacity can reach 218 mAh g -1 The specific capacity shows excellent rate performance.
[0079] The test results of the cycle stability performance of the potassium ion battery assembled with CuO@hCNCs prepared in Example 2 are as follows: Figure 6 shown. Figure 6 The horizontal axis in the middle is the number of cycles, the vertical axis on the left is the specific capacity, and the vertical axis on the right is the coulombic efficiency. Figure 6 It can be seen that at 1A·g -1 At a current density of 1.5 %, the material can still maintain 238 mAh g after 500 cycles. -1 The discharge specific capacity and coulombic efficiency are as high as 99.6%, which shows that the material has extremely high cycle stability.
[0080] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A composite electrode material, comprising a carbon-based nanocage and copper oxide filled in the carbon-based nanocage; the mass of the copper oxide is 10% to 70% of the total mass of the composite electrode material; The method for preparing the composite electrode material comprises the following steps: (1) Under vacuum conditions, the carbon-based nanocage is sequentially immersed in a copper oxide precursor solution and post-treated to obtain a composite electrode precursor; (2) thermally decomposing the composite electrode precursor obtained in step (1) to obtain a composite electrode material; the thermal decomposition atmosphere is argon or nitrogen; the heating rate of the thermal decomposition is 5 to 20°C / min, the final temperature of the thermal decomposition is 180 to 400°C, and the total thermal decomposition time required from the start of heating to the end of thermal decomposition is 20 to 360 minutes.
2. The composite electrode material according to claim 1, characterized in that The carbon-based nanocage includes one of a carbon nanocage, a nitrogen-doped carbon nanocage, a sulfur-doped carbon nanocage and a phosphorus-doped carbon nanocage.
3. The composite electrode material according to claim 1 or 2, characterized in that: The specific surface area of the carbon-based nanocage is 600 to 2000 m 2 / g.
4. The composite electrode material according to claim 1, characterized in that The post-treatment in step (1) comprises filtering and drying performed in sequence.
5. The composite electrode material according to claim 1, characterized in that: The impregnation and post-treatment in the step (1) are repeated 2 to 5 times.
6. The composite electrode material according to claim 1, characterized in that: The copper oxide precursor solution in step (1) includes one or more of copper nitrate solution, copper acetate solution, cupric chloride solution, cuprous acetate solution, and cuprous chloride solution.
7. The composite electrode material according to claim 1, characterized in that: The concentration of copper ions in the copper oxide precursor solution in step (1) is 0.05 to 2.0 mol / L.
8. A potassium ion battery comprising the composite electrode material according to any one of claims 1 to 7.
Citation Information
Patent Citations
Method for mass preparing hollow nano cages in high quality
CN101284663A
Method for preparing nitrogen doping hollow carbon nanocages
CN102530922A
A method for preparing copper oxide composite lithium battery anode material
CN110311109B
Graphene-coated copper oxide composite cathode material and method for manufacturing same
CN102916195A
Preparation method and application of CuO / Cu N-doped carbon nanofiber material
CN110331469A