Quantum dot light-emitting diodes, display devices and light sources
By incorporating electron-withdrawing groups-substituted 9-phenylanthracene electron-blocking and hole-blocking layers into quantum dot light-emitting diodes, the problem of electron and hole injection imbalance is solved, thereby improving the device's luminous efficiency and lifetime.
Patent Information
- Application Number
- CN202011295669.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-11-18
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2040-11-18
AI Technical Summary
In existing quantum dot light-emitting diodes, the imbalance between electron and hole injection leads to problems such as low efficiency, short lifespan, and poor color purity.
An electron blocking layer containing 9-phenylanthracene substituted with electron-withdrawing groups is placed between the quantum dot layer and the electron transport layer, combined with a hole blocking layer, to adjust the mobility of electrons and holes to achieve injection balance.
By combining electron blocking layers and hole blocking layers, a balance between electron and hole injection is achieved, improving luminous efficiency and lifespan, and enhancing the performance of display devices and light sources.
Smart Images

Figure CN114583067B_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of display device technology, and particularly relates to a quantum dot light-emitting diode, a display device, and a light source. Background Technology
[0002] As is well known, in quantum dot light-emitting diode (QLED) devices, the balance between electron and hole injection is crucial for achieving high efficiency and long lifetime. In common QLED device structures, the electron transport material is generally well-matched with the valence band of the quantum dot, resulting in an electron injection intensity that is much higher than the hole injection intensity. This imbalance in electron and hole injection leads to overcharging of the quantum dot, causing nonradiative Auger recombination and inducing exciton separation, and may even cause parasitic emission, which is highly detrimental to the device's efficiency, lifetime, and color purity.
[0003] Currently, the band structure of electron transport materials such as zinc oxide can be tuned by ion doping or interface modification, thereby achieving balanced hole and electron injection in QLED devices. For example, zinc-magnesium oxide nanoparticles doped with magnesium oxide and zinc-aluminum oxide nanoparticles doped with aluminum oxide can be used as electron transport materials. However, the doped zinc oxide obtained by using these doping methods may have performance that is better or worse than that of the original zinc oxide, resulting in performance instability, which in turn affects the stability of QLED device products.
[0004] Therefore, existing technologies need to be improved. Summary of the Invention
[0005] The purpose of this application is to provide a quantum dot light-emitting diode, a display device, and a light source, aiming to solve the technical problem of the imbalance between hole and electron injection in existing quantum dot light-emitting diode devices.
[0006] To achieve the above-mentioned objectives, the technical solution adopted in this application is as follows:
[0007] In a first aspect, this application provides a quantum dot light-emitting diode, comprising an electron transport layer, a quantum dot layer, and an electron blocking layer located between the electron transport layer and the quantum dot layer, wherein the electron blocking layer contains 9-phenylanthracene substituted with electron-withdrawing groups.
[0008] The quantum dot light-emitting diode provided in this application has an electron blocking layer containing 9-phenylanthracene substituted with electron-withdrawing groups between the quantum dot layer and the electron transport layer. The 9-phenylanthracene substituted with electron-withdrawing groups has excellent electron mobility and can have good energy level matching with the electron transport layer, thereby reducing the interface barrier between the two and facilitating electron injection and storage. This allows a large number of electrons to be accumulated in the electron blocking layer, and the electron mobility rate can be flexibly adjusted through the electron-withdrawing groups to match the electron mobility with the hole mobility, thereby making the injection of holes and electrons in the device more balanced and ultimately improving the light-emitting performance of the device.
[0009] Secondly, this application provides a display device, which includes the quantum dot light-emitting diode described above.
[0010] The display device provided in this application includes a quantum dot light-emitting diode (LED) unique to this application. Because the quantum dot LED has an electron blocking layer containing 9-phenylanthracene substituted with electron-withdrawing groups between the quantum dot layer and the electron transport layer, the electron and hole injection of the quantum dot LED is better balanced, and the display device with the quantum dot LED has better display performance.
[0011] Thirdly, this application provides a light source, which includes the quantum dot light-emitting diode described above.
[0012] The light source provided in this application includes a quantum dot light-emitting diode (LED) unique to this application. Because the quantum dot LED has an electron blocking layer containing 9-phenylanthracene substituted with electron-withdrawing groups between the quantum dot layer and the electron transport layer, the electron and hole injection of the quantum dot LED is better balanced, and the light source with the quantum dot LED has better light-emitting performance. Attached Figure Description
[0013] To more clearly illustrate the technical solutions in the embodiments of this application, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0014] Figure 1 This is a schematic diagram of the structure of a quantum dot light-emitting diode provided in one embodiment of this application;
[0015] Figure 2 This is a schematic diagram of the structure of a quantum dot light-emitting diode provided in one embodiment of this application;
[0016] Figure 3This is a schematic diagram of the structure of a quantum dot light-emitting diode provided in one embodiment of this application;
[0017] Figure 4 This is a schematic diagram of the hole-electron injection balance principle of a quantum dot light-emitting diode provided in one embodiment of this application. Detailed Implementation
[0018] To make the technical problems, technical solutions, and beneficial effects of this application clearer, the following detailed description is provided in conjunction with embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.
[0019] The first aspect of this application provides a quantum dot light-emitting diode, such as... Figure 1 As shown, it includes an electron transport layer, a quantum dot layer, and an electron blocking layer located between the electron transport layer and the quantum dot layer, wherein the electron blocking layer contains 9-phenylanthracene substituted with electron-withdrawing groups.
[0020] The quantum dot light-emitting diode provided in this application has an electron blocking layer containing 9-phenylanthracene substituted with electron-withdrawing groups between the quantum dot layer and the electron transport layer. The 9-phenylanthracene substituted with electron-withdrawing groups has excellent electron mobility and can have good energy level matching with the electron transport layer, thereby reducing the interface barrier between the two and facilitating electron injection and storage. This allows a large number of electrons to be accumulated in the electron blocking layer, and the electron mobility rate can be flexibly adjusted through the electron-withdrawing groups to match the electron mobility with the hole mobility, thereby making the injection of holes and electrons in the device more balanced and ultimately improving the light-emitting performance of the device.
[0021] In some embodiments, the HOMO level of 9-phenylanthracene substituted with electron-withdrawing groups in the electron-blocking layer is -7.0 to -7.2 eV. 9-phenylanthracene exhibits good electron mobility; after substitution with electron-withdrawing groups, its HOMO level can reach -7.0 to -7.2 eV, which can maximally match the energy levels of various electron transport layers, thereby reducing the potential barrier at the interface.
[0022] In some embodiments, the electron-withdrawing group-substituted 9-phenylanthracene is selected from at least one of the following formulas IV:
[0023]
[0024] Wherein, X1, X2, X3, X4 and X5 are the same or different electron-withdrawing groups, preferably, the electron-withdrawing groups are selected from at least one of nitro, chloro, fluorine, bromine and iodine.
[0025] An electron-blocking layer containing 9-phenylanthracene substituted with the aforementioned electron-withdrawing groups can store a large number of electrons in the electron-blocking layer, and the electron migration rate can be adjusted according to the number of electron-withdrawing groups and their electron-withdrawing ability.
[0026] In some embodiments, the electron blocking layer may comprise 9-phenylanthracene substituted with electron-withdrawing groups, or may comprise other materials with electron-blocking functionality. In a preferred embodiment, the electron blocking layer is composed of the 9-phenylanthracene substituted with electron-withdrawing groups. More preferably, the thickness of the electron blocking layer is 20-60 nm.
[0027] In some embodiments, the electron transport layer material includes, but is not limited to, at least one of zinc oxide, zirconium dioxide, titanium dioxide, and tin dioxide, with zinc oxide being preferred. Zinc oxide nanoparticles have high electron mobility, μ... e ≈1.8×10 -3 cm 2 The mobility of 9-phenylanthracene, with a velocity of / (V·s), is 1-3 orders of magnitude greater than that of commonly used hole transport materials, and it has a good valence band match with quantum dots. At the same time, the 9-phenylanthracene substituted with electron-withdrawing groups is also more compatible with the energy levels of zinc oxide, which can effectively avoid the defect of the zinc oxide electron transport layer where the electron injection intensity is much higher than the hole injection intensity, thus making the hole and electron injection of the device more balanced.
[0028] In some embodiments, such as Figure 2 As shown, the quantum dot light-emitting diode includes an electron transport layer, a quantum dot layer, and the aforementioned electron blocking layer located between the electron transport layer and the quantum dot layer. A hole blocking layer is also disposed between the quantum dot light-emitting layer and the electron blocking layer, and the hole blocking layer contains a pyrimidine-substituted 1,3,5-triphenylbenzene.
[0029] The hole-blocking layer described in this application is a "passive" or "protective" barrier, designed to retain holes within the quantum dot layer to maximize the formation of more excitons, unlike existing active hole-blocking methods (which actively reduce or slow down the number or rate of hole injection). This application places the hole-blocking layer and the electron-blocking layer on the same side of the quantum dot layer, allowing holes to migrate to the luminescent layer at the maximum rate and in the largest quantity, ensuring luminescence efficiency. Then, the hole-blocking layer separates the quantum dot layer and the electron-blocking layer, preventing holes or excitons from migrating to the electron transport layer and causing it to emit light, further improving the color gamut purity of the quantum dot emission.
[0030] The pyrimidine-substituted derivatives of 1,3,5-triphenylbenzene have a unique star-shaped molecular structure and pyrimidine modification units. By adjusting the substitution position of nitrogen atoms in the pyrimidine, the HOMO and LUMO energy levels of the compound can be effectively tuned, so that the overall energy level of the compound covers the electron blocking layer energy level. This effectively restricts holes or excitons in the quantum dot layer from diffusing into the electron transport layer, thereby increasing the exciton luminescence efficiency.
[0031] In some embodiments, the triplet energy level of the pyrimidine-substituted 1,3,5-triphenylbenzene in the hole-blocking layer is greater than 2.8 eV. For a 1,3,5-triphenylbenzene-centered compound with pyrimidine as the peripheral electron-withdrawing group, its LUMO energy level is mainly concentrated on the peripheral pyrimidine group, while the HOMO energy level is mainly concentrated on the central triphenylbenzene. As the electron-withdrawing ability of the peripheral groups increases, the HOMO energy level of the molecule gradually decreases to below -6.5 eV. Therefore, this hole-blocking material has excellent hole-blocking capability.
[0032] More preferably, the pyrimidine-substituted derivative of the 1,3,5-triphenylbenzene is selected from at least one of 1,3,5-tris(2-pyrimidinylphenyl)benzene, 1,3,5-tris(4-pyrimidinylphenyl)benzene, and 1,3,5-tris(5-pyrimidinylphenyl)benzene, and has the following structure:
[0033]
[0034] In some embodiments, the hole-blocking layer contains the pyrimidine-substituted 1,3,5-triphenylbenzene, and may also contain other materials with hole-blocking functionality. In a preferred embodiment, the hole-blocking layer is composed of the pyrimidine-substituted 1,3,5-triphenylbenzene, and preferably, the thickness of the hole-blocking layer is 5-30 nm.
[0035] Furthermore, this application combines an electron blocking layer and a hole blocking layer with a high-mobility zinc oxide electron transport layer. The electron blocking layer regulates the electron migration rate of zinc oxide, and the hole blocking layer prevents hole cross-layer diffusion, thereby achieving a balance between electron and hole injection, improving device performance and lifespan, and ultimately increasing the luminous efficiency and lifespan of QLED devices.
[0036] Furthermore, a hole transport layer, or a stacked hole injection layer and hole transport layer, are disposed between the quantum dot layer and the anode. For example... Figure 3 As shown, the quantum dot light-emitting diode includes an anode, a hole injection layer, a hole transport layer, a quantum dot layer, a hole blocking layer, an electron blocking layer, an electron transport layer, and a cathode, which are stacked sequentially.
[0037] Taking ITO as the anode, PEDOT:PSS as the hole injection layer material, zinc oxide as the electron transport layer, and Al as the cathode as an example, Figure 4As shown, the hole blocking layer retains holes up to the quantum dot layer, while the electron-withdrawing functional groups on the electron blocking layer slow down the electron injection rate, achieving a hole-electron injection balance. Placing the hole blocking layer and electron blocking layer on the same side of the quantum dot layer avoids dissolving the hole transport layer during the fabrication of the hole blocking layer (the solvents used for the hole blocking layer and hole transport layer are polar solvents with similar polarities, easily causing miscibility, but their polarity differs from that of the quantum dot layer solvent, thus isolating and protecting the quantum dot layer). Furthermore, both the hole blocking layer and the electron blocking layer are made of benzene compounds, resulting in a smaller potential barrier difference between the layer boundaries, which is beneficial for electron transport.
[0038] Specifically, the fabrication method of this quantum dot light-emitting diode includes the following steps:
[0039] 1. Prepare the anode: Taking indium tin oxide (ITO) as the anode, the cleaned indium tin oxide substrate is treated with ultraviolet ozone for a period of time to improve the surface work function and hydrophilicity of the ITO substrate.
[0040] 2. Preparation of the hole injection layer: Taking poly(3,4-ethylenedioxythiophene):poly(styrene sulfonic acid) (PEDOT:PSS) as an example, a certain amount of PEDOT:PSS solution is dropped onto an ITO substrate, spin-coated at 4000 r / min, and then annealed to obtain a PEDOT:PSS film as the hole injection layer. The thickness of the PEDOT:PSS film ranges from 20-50 nm, preferably 30 nm. The mass of PEDOT:PSS ranges from 1-5 g, preferably 2 g.
[0041] 3. Preparation of the hole transport layer: The ITO substrate coated with a PEDOT:PSS film is transferred to a glove box under nitrogen atmosphere protection, and the hole transport layer material is spin-coated at 3000 rpm. The hole transport layer material includes, but is not limited to: poly[bis(4-phenyl)(4-butylphenyl)amine] solution (poly-TPD), N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine solution (NPB), N,N,N',N'-tetraphenyl-2,6-naphthyldiamine (NDDP), and 4-[1-[4-[di(4-methylphenyl)amino]phenyl]cyclohexyl]-N-(3-methylphenyl)-N-(4-methylphenyl)aniline (TAPC), preferably NPB solution. The hole transport layer film thickness ranges from 40-60 nm, preferably 45 nm. The mass of the hole transport material ranges from 0.5-2 g, preferably 1.5 g.
[0042] 4. Preparation of the quantum dot layer: The quantum dot materials for the quantum dot layer include, but are not limited to: group II-VI, group III-V, group IV-VI quantum dots, all-inorganic perovskite quantum dots, organic-inorganic perovskite quantum dots, copper-sulfur-indium ternary quantum dots, and silicon quantum dots; the quantum dot system architecture includes, but is not limited to: a uniform binary component mononuclear structure, a uniform multi-component alloy component mononuclear structure, a multi-component alloy component graded mononuclear structure, a binary component discrete core-shell structure, and a multi-component alloy component structure. Discrete core-shell structure or quantum dot multi-element alloy composition gradient core-shell structure; the core and shell compounds of the quantum dots are, but are not limited to, group II-VI CdSe, CdS, ZnSe, ZnS, CdTe, ZnTe, CdZnS, ZnSeS, CdSeS, CdSeSTe, or CdZnSeSTe, group III-V InP, InAs, or InAsP, and group IV-VI PbS, PbSe, PbSeS, PbSeTe, or PbSTe. The thickness of the quantum dot layer ranges from 5-20 nm, preferably 10 nm. The mass of the quantum dots is 0.1-0.5 g, preferably 0.4 g.
[0043] 5. Preparation of the hole-blocking layer: A star-shaped pyrimidine-substituted derivative of 1,3,5-triphenylbenzene is used as the hole-blocking layer. The star-shaped pyrimidine-substituted derivatives of 1,3,5-triphenylbenzene include, but are not limited to: 1,3,5-tris(2-pyrimidinephenyl)benzene, 1,3,5-tris(4-pyrimidinephenyl)benzene, and 1,3,5-tris(5-pyrimidinephenyl)benzene. Solvents used include, but are not limited to: chlorobenzene, chloroform, and o-dichlorobenzene, preferably chlorobenzene. The hole-blocking layer thickness ranges from 5 to 30 nm, preferably 15 nm. The mass of the star-shaped pyrimidine-substituted derivative of 1,3,5-triphenylbenzene ranges from 0.1 to 0.8 g, preferably 0.4 g.
[0044] 6. Preparation of the electron blocking layer: 9-Phenylanthracene substituted with electron-withdrawing functional groups is used as the electron blocking layer. The 9-Phenylanthracene substituted with electron-withdrawing functional groups includes, but is not limited to, at least one of Formula IV above; wherein X1, X2, X3, X4, and X5 are the same or different electron-withdrawing groups, specifically selected from at least one of nitro, chloro, fluorine, bromine, and iodo groups. The thickness of the electron blocking layer ranges from 20 to 60 nm, preferably 50 nm. The mass ranges from 1.5 to 5 g, preferably 2.2 g. The electron blocking layer can store a large number of electrons, and the electron migration rate can be adjusted according to the number and electron-withdrawing functional groups.
[0045] 7. Preparation of the electron transport layer: The thickness of the electron transport layer ranges from 20-40 nm, preferably 25 nm. The mass of the electron transport layer ranges from 0.1-1.5 g, preferably 1.1 g. The electron transport layer material includes, but is not limited to, at least one of zinc oxide, zirconium dioxide, titanium dioxide, and tin dioxide, with zinc oxide being preferred.
[0046] 8. Preparation of cathode: Taking aluminum as an example, aluminum electrode is deposited by vapor deposition and then encapsulated.
[0047] A second aspect of this application provides a display device, which includes the quantum dot light-emitting diode described above.
[0048] The display device provided in this application includes a quantum dot light-emitting diode (LED) unique to this application. Because the quantum dot LED has an electron blocking layer containing 9-phenylanthracene substituted with electron-withdrawing groups between the quantum dot layer and the electron transport layer, the electron and hole injection of the quantum dot LED is better balanced, and the display device with the quantum dot LED has better display performance.
[0049] Furthermore, the display device is a flat panel display.
[0050] A third aspect of this application provides a light source, which includes the quantum dot light-emitting diode described above.
[0051] The light source provided in this application includes a quantum dot light-emitting diode (LED) unique to this application. Because the quantum dot LED has an electron blocking layer containing 9-phenylanthracene substituted with electron-withdrawing groups between the quantum dot layer and the electron transport layer, the electron and hole injection of the quantum dot LED is better balanced, and the light source with the quantum dot LED has better light-emitting performance.
[0052] The following description is based on specific embodiments.
[0053] Example 1
[0054] A quantum dot light-emitting diode, such as Figure 3 As shown, from bottom to top, the structure includes: an anode, a hole injection layer, a hole transport layer, a quantum dot layer, a hole blocking layer, an electron blocking layer, an electron transport layer, and a cathode. The fabrication method of this quantum dot light-emitting diode includes the following steps:
[0055] (1) Anode pretreatment of indium tin oxide (ITO) substrate: The cleaned indium tin oxide substrate is treated with ultraviolet ozone for 10 minutes to improve the surface work function and hydrophilicity of the ITO substrate.
[0056] (2) Hole injection layer preparation: 1.2g of PEDOT:PSS solution was spin-coated onto an ITO substrate at 4000r / min and then annealed to obtain a 20nm thick PEDOT:PSS film as a hole injection layer.
[0057] (3) Hole transport layer preparation: The ITO substrate coated with PEDOT:PSS film was transferred to a glove box under nitrogen atmosphere protection. 0.5g of poly[bis(4-phenyl)(4-butylphenyl)amine] (Poly-TPD) dissolved in chloroform was spin-coated onto the hole injection layer at 3000r / min to obtain a hole transport layer with a film thickness of 40nm.
[0058] (4) Quantum dot layer preparation: 0.1g of CdSe quantum dots were spin-coated onto the hole transport layer at a speed of 3000r / min to obtain a quantum dot light-emitting layer with a film thickness of 5nm.
[0059] (5) Hole blocking layer preparation: 0.15g of 1,3,5-tris(2-pyrimidinylphenyl)benzene was spin-coated onto the quantum dot layer at a speed of 3000r / min to obtain a hole blocking layer with a film thickness of 5nm.
[0060] (6) Electron blocking layer preparation: 1.5g of 1-nitrophenyl-9-anthracene was spin-coated onto the hole blocking layer at a speed of 3000r / min to obtain an electron blocking layer with a film thickness of 20nm.
[0061] (7) Electron transport layer preparation: 0.2 g zinc oxide solution was spin-coated onto the electron blocking layer at a speed of 3000 r / min to obtain a zinc oxide layer with a thickness of 20 nm as the electron transport layer.
[0062] (8) Cathode preparation: An aluminum electrode is deposited on the electron transport layer and then encapsulated.
[0063] Example 2
[0064] A quantum dot light-emitting diode, such as Figure 3 As shown, from bottom to top, the structure includes: an anode, a hole injection layer, a hole transport layer, a quantum dot layer, a hole blocking layer, an electron blocking layer, an electron transport layer, and a cathode. The fabrication method of this quantum dot light-emitting diode includes the following steps:
[0065] (1) Anode pretreatment of indium tin oxide (ITO) substrate: The cleaned indium tin oxide substrate is treated with ultraviolet ozone for 20 minutes to improve the surface work function and hydrophilicity of the ITO substrate.
[0066] (2) Hole injection layer preparation: 5g of PEDOT:PSS solution was spin-coated onto an ITO substrate at 4000r / min and then annealed to obtain a 50nm thick PEDOT:PSS film as a hole injection layer.
[0067] (3) Hole transport layer preparation: The ITO substrate coated with PEDOT:PSS film was transferred to a glove box filled with nitrogen atmosphere. 1.8g of 4-[1-[4-[di(4-methylphenyl)amino]phenyl]cyclohexyl]-N-(3-methylphenyl)-N-(4-methylphenyl)aniline was dissolved in chlorobenzene and spin-coated onto the hole injection layer at 3000r / min to obtain a hole transport layer with a film thickness of 60nm.
[0068] (4) Quantum dot layer preparation: 0.5g of PbSeS quantum dots were spin-coated onto the hole transport layer at a speed of 3000r / min to obtain a quantum dot light-emitting layer with a film thickness of 20nm.
[0069] (5) Hole blocking layer preparation: 0.8 g of 1,3,5-tris(5-pyrimidinylphenyl)benzene was spin-coated onto the quantum dot layer at a speed of 3000 r / min to obtain a hole blocking layer with a film thickness of 30 nm.
[0070] (6) Electron blocking layer preparation: 4.8 g of 1,2,3-trichlorophenyl-9-anthracene was spin-coated onto the hole blocking layer at a speed of 3000 r / min to obtain an electron blocking layer with a film thickness of 60 nm.
[0071] (7) Electron transport layer preparation: 1.5g of zirconium dioxide solution was spin-coated onto the electron blocking layer at a speed of 3000r / min to obtain a potassium silicate layer with a thickness of 40nm as the electron transport layer.
[0072] (8) Cathode preparation: An aluminum electrode is deposited on the electron transport layer and then encapsulated.
[0073] Example 3
[0074] A quantum dot light-emitting diode, such as Figure 3 As shown, from bottom to top, the structure includes: an anode, a hole injection layer, a hole transport layer, a quantum dot layer, a hole blocking layer, an electron blocking layer, an electron transport layer, and a cathode. The fabrication method of this quantum dot light-emitting diode includes the following steps:
[0075] (1) Anode pretreatment of indium tin oxide (ITO) substrate: The cleaned indium tin oxide substrate is treated with ultraviolet ozone for 30 minutes to improve the surface work function and hydrophilicity of the ITO substrate.
[0076] (2) Hole injection layer preparation: 2g of PEDOT:PSS solution was spin-coated onto an ITO substrate at 3000r / min and then annealed to obtain a 30nm thick PEDOT:PSS film as a hole injection layer.
[0077] (3) Hole transport layer preparation: The ITO substrate coated with PEDOT:PSS film was transferred to a glove box filled with nitrogen atmosphere. 0.8g of N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine solution (NPB) and N,N,N',N'-tetraphenyl-2,6-naphthyldiamine were dissolved in o-dichlorobenzene and spin-coated on the hole injection layer at 3000r / min to obtain a hole transport layer with a film thickness of 45nm.
[0078] (4) Quantum dot layer preparation: 0.4g of silicon quantum dots were spin-coated onto the hole transport layer at a speed of 3000r / min to obtain a quantum dot light-emitting layer with a film thickness of 10nm.
[0079] (5) Hole blocking layer preparation: 0.4 g of 1,3,5-tris(4-pyrimidinylphenyl)benzene was spin-coated onto the quantum dot layer at a speed of 3000 r / min to obtain a hole blocking layer with a film thickness of 15 nm.
[0080] (6) Electron blocking layer preparation: 2.2g of 1,2,3,4,5-pentaiodophenyl-9-anthracene was spin-coated onto the hole blocking layer at a speed of 3000r / min to obtain an electron blocking layer with a film thickness of 50nm.
[0081] (7) Electron transport layer preparation: 1.1g of titanium dioxide solution was spin-coated onto the electron blocking layer at a speed of 3000r / min to obtain a lithium fluoride layer with a thickness of 25nm as the electron transport layer.
[0082] (8) Cathode preparation: Aluminum electrode is deposited by vapor deposition and then encapsulated.
[0083] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of this application should be included within the protection scope of this application.
Claims
1. A quantum dot light-emitting diode, characterized in that, It includes an electron transport layer, a quantum dot layer, and an electron blocking layer located between the electron transport layer and the quantum dot layer. The electron blocking layer is composed of 9-phenylanthracene substituted with electron-withdrawing groups, wherein the 9-phenylanthracene substituted with electron-withdrawing groups is selected from at least one of the following formulas IV: Wherein, X1, X2, X3, X4 and X5 are the same or different electron-withdrawing groups, and the electron-withdrawing groups are selected from at least one of nitro, chloro, fluorine, bromine and iodine.
2. The quantum dot light-emitting diode as described in claim 1, characterized in that, The HOMO energy level of the 9-phenylanthracene substituted with electron-withdrawing groups is -7.0 to -7.2 eV.
3. The quantum dot light-emitting diode as described in claim 1, characterized in that, The thickness of the electron blocking layer is 20-60 nm.
4. The quantum dot light-emitting diode as described in any one of claims 1-3, characterized in that, A hole blocking layer is further disposed between the quantum dot luminescent layer and the electron blocking layer, the hole blocking layer containing a pyrimidine-substituted 1,3,5-triphenylbenzene.
5. The quantum dot light-emitting diode as described in claim 4, characterized in that, The triplet energy level of the pyrimidine-substituted 1,3,5-triphenylbenzene is greater than 2.8 eV.
6. The quantum dot light-emitting diode as described in claim 5, characterized in that, The HOMO energy level of the pyrimidine-substituted 1,3,5-triphenylbenzene is below -6.5 eV.
7. The quantum dot light-emitting diode as described in claim 6, characterized in that, The pyrimidine-substituted derivatives of the 1,3,5-triphenylbenzene are selected from at least one of 1,3,5-tris(2-pyrimidinephenyl)benzene, 1,3,5-tris(4-pyrimidinephenyl)benzene and 1,3,5-tris(5-pyrimidinephenyl)benzene.
8. The quantum dot light-emitting diode as described in claim 4, characterized in that, The hole-blocking layer is composed of the pyrimidine-substituted derivative of 1,3,5-triphenylbenzene.
9. The quantum dot light-emitting diode as described in claim 8, characterized in that, The thickness of the hole blocking layer is 5-30 nm.
10. A display device, characterized in that, The display device includes a quantum dot light-emitting diode as described in any one of claims 1 to 9.
11. The display device as claimed in claim 10, characterized in that, The display device is a flat panel display.
12. A light source, characterized in that, The light source includes a quantum dot light-emitting diode as described in any one of claims 1 to 9.
Citation Information
Patent Citations
Quantum dot light-emitting diode and preparation method thereof, and display panel
CN109509842A
Organic light-emitting device including organic layer including anthracene derivative compound
US20090233125A1