Composite current collector and preparation method and application thereof
By introducing flame retardant layer and conductive layer into the composite fluid, combined with the design of the base film layer and metal layer, the problems of high internal resistance and welding difficulties in lithium batteries are solved, and efficient ion transmission and safety performance improvement of lithium batteries are achieved. .
Patent Information
- Application Number
- CN202210346374.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-31
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2042-03-31
AI Technical Summary
In lithium batteries, the existing composite liquid collectors have high internal resistance, difficulty in welding and insufficient current output due to polymers, which affects the battery's magnification and safety performance.
Using a composite fluid design including a flame retardant layer, a base film layer and a metal layer, the through-hole conductive layer is formed by doping ionic conductors and flame retardant particles in the flame retardant layer to increase conductivity and reduce the ohmic impedance of the welding point. Improve the conductivity and arrange a spaced metal layer between the base film layer and the metal layer to improve welding yield.
It realizes efficient transmission of ions inside lithium batteries, reduces internal resistance, significantly improves rate performance and safety performance, and avoids the problems of welding dummy welding and insufficient current output.
Smart Images

Figure CN114597338B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium batteries, and in particular relates to a composite current collector and a preparation method and application thereof. Background Art
[0002] Lithium batteries have been widely used due to their high energy density, excellent cycle performance, high discharge rate and many other advantages. However, the current collector of conventional lithium-ion batteries usually uses metal aluminum foil for the positive electrode and metal copper foil for the negative electrode. Once a short circuit occurs inside the battery, the current cannot be cut off, which will eventually lead to heat accumulation and thermal runaway. The safety problems caused by thermal runaway are very obvious.
[0003] In recent years, some researchers have used a new type of current collector to replace conventional metal current collectors. This type of composite current collector usually uses a non-conductive polymer film as a substrate, and a layer of metal is plated on both sides of the substrate by vacuum evaporation, electroplating, etc. For example, metal aluminum is plated on both sides of a PET (polyethylene terephthalate) film as a positive electrode current collector, and metal copper is plated on both sides of a PP (polypropylene) film as a negative electrode current collector. These composite current collectors have improved the safety performance of the battery to a certain extent, while also reducing the weight of the current collector, further improving the weight energy density of the battery.
[0004] The composite current collector uses polymer materials to replace the thickness of part of the metal material, thereby reducing the weight of the current collector and improving the weight energy density of the battery cell. At the same time, since the middle of the current collector is a high molecular polymer, which is an insulating layer, when the temperature inside the battery cell is too high, the metal layer on the surface of the polymer will melt, realizing the electronic circuit breakage and preventing the thermal runaway of the battery cell. However, due to the high molecular polymer in the middle layer of the composite current collector, the electrons inside the current collector cannot be conducted, making the internal resistance of the pole piece made of this material 10 to 15 times that of the conventional pole piece, and the internal resistance of the processed and manufactured battery cell is 20 to 30 times that of the conventional battery cell, resulting in the battery cell being unable to discharge normally or releasing a small amount of electricity. At the same time, during the processing and production of this material, the high molecular polymer in the middle layer absorbs the welding energy and cannot be directly welded to the external pole ear. Multiple welding methods are required. Even so, the phenomenon of welding cold welding will still occur, and it also leads to a large AC internal resistance of the battery cell and a low battery cell rate requirement. In summary, if a composite current collector having an insulating middle layer but an outer surface that can conduct electrons can be invented, the above problems can be solved to a large extent, and the material can also be widely used in the lithium battery industry. Summary of the invention
[0005] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, one object of the present invention is to provide a composite current collector and a preparation method and application thereof, which reduces the ohmic impedance of the welding point and is applied to a lithium battery to achieve efficient transmission of ions inside the lithium battery, while ensuring that the internal resistance of the lithium battery is low, and the rate performance and safety performance of the lithium battery are significantly improved.
[0006] In one aspect of the present invention, the present invention provides a composite current collector. According to an embodiment of the present invention, the composite current collector includes a first region and a second region, wherein the first region includes:
[0007] Flame retardant layer;
[0008] A base film layer, the base film layer comprising a first base film layer and a second base film layer, the first base film layer being arranged on the flame retardant layer, and the second base film layer being arranged on a side of the flame retardant layer away from the first base film layer;
[0009] A metal layer, the metal layer comprising a first metal layer and a second metal layer, the first metal layer being disposed on the first base film layer, and the second metal layer being disposed on a side of the second base film layer away from the first metal layer;
[0010] Wherein, the flame retardant layer comprises an adhesive, an ion conductor and flame retardant particles.
[0011] According to the composite current collector of the embodiment of the present invention, by doping ion conductors and flame retardant particles in the flame retardant layer, on the one hand, the flame retardant effect of the composite current collector is improved, and on the other hand, the conductivity of the composite current collector is increased, thereby reducing the ohmic impedance of the welding points in the composite current collector; the composite current collector including the flame retardant layer is applied in a lithium-ion battery, so that efficient transmission of ions inside the lithium battery can be achieved, while ensuring that the internal resistance of the lithium battery is low, and the rate performance and safety performance of the lithium battery are improved.
[0012] In addition, the composite current collector according to the above embodiment of the present invention may also have the following additional technical features:
[0013] In some embodiments of the present invention, through holes are formed on the flame retardant layer and the base film layer along the thickness direction thereof, and a first conductive layer is provided on the hole wall of the through hole, thereby further improving the conductive performance of the composite current collector.
[0014] In some embodiments of the present invention, the thickness of the first conductive layer is 0.01-2 μm.
[0015] In some embodiments of the present invention, the first conductive layer includes at least one of graphite, graphene, acetylene black and carbon nanotubes.
[0016] In some embodiments of the present invention, the thickness of the flame retardant layer is 0.5-3 μm.
[0017] In some embodiments of the present invention, there are multiple through holes.
[0018] In some embodiments of the present invention, the diameter of the through hole is 0.02-1 mm.
[0019] In some embodiments of the present invention, the edge distance between any two adjacent through holes is 0.1 mm to 5 mm.
[0020] In some embodiments of the present invention, the second region is arranged on the first region along a first direction, and the first direction is a length direction along the first region and / or the second region.
[0021] In some embodiments of the present invention, the length of the first region is greater than or equal to the length of the second region.
[0022] In some embodiments of the present invention, the second region includes a third metal layer and a fourth metal layer, and the third metal layer and the fourth metal layer are arranged at intervals. Thus, the welding yield of the composite current collector can be improved and the phenomenon of increased impedance of the welding point can be avoided.
[0023] In some embodiments of the present invention, the thickness of the first base film layer and the second base film layer is 0.5 to 5 μm.
[0024] In some embodiments of the present invention, the thickness of the first metal layer, the second metal layer, the third metal layer and the fourth metal layer are independently 0.01-2 μm.
[0025] In some embodiments of the present invention, it is characterized in that the material of the base film layer includes at least one of polyester terephthalate, polyamide, polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyethylene terephthalate, polybutylene terephthalate, poly(p-phenylene terephthalamide), polypropylene, acrylonitrile-butadiene-styrene copolymer, polyvinyl formal, polyvinyl butyral, polyurethane, polyurethane, polyacrylonitrile, polyvinyl acetate, polyformaldehyde, phenolic resin, epoxy resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber, polycarbonate, polysulfone, polyethersulfone and polyphenylene ether.
[0026] In some embodiments of the present invention, the first metal layer, the second metal layer, the third metal layer and the fourth metal layer independently include at least one of aluminum, copper, nickel, titanium, silver, stainless steel, nickel-copper alloy and aluminum-zirconium alloy.
[0027] In some embodiments of the present invention, a second conductive layer and a third conductive layer are further included, wherein the second conductive layer is disposed on the first metal layer, and the third conductive layer is disposed on a side of the second metal layer away from the second conductive layer, thereby facilitating the improvement of the rate performance of the battery cell.
[0028] In some embodiments of the present invention, the thickness of the second conductive layer and the third conductive layer are independently 0.01-2 μm.
[0029] In some embodiments of the present invention, the second conductive layer and the third conductive layer independently include at least one of graphite, acetylene black, graphene and carbon nanotubes.
[0030] In some embodiments of the present invention, the mass ratio of the adhesive, the ion conductor and the flame retardant particles is (1-28): (1-35): (50-70). Thus, the composite current collector can have a good flame retardant effect and good conductivity.
[0031] In some embodiments of the present invention, the adhesive includes at least one of ethylene copolymers, polyolefins, polyesters, and polyamides.
[0032] In some embodiments of the present invention, the ion conductor includes at least one of LATP, LAGP, LLZO, LiTi2(PO4)3, LiCF3SO3, LiBF4, LiPF6 and LiODFB.
[0033] In some embodiments of the present invention, the flame retardant particles include at least one of magnesium hydroxide, aluminum hydroxide, ammonium polyphosphate, zinc borate, antimony trioxide and layered silicate.
[0034] In a second aspect of the present invention, the present invention provides a method for preparing the above-mentioned composite current collector. According to an embodiment of the present invention, the method comprises:
[0035] (1) mixing an adhesive, an ion conductor and flame retardant particles, and then thermoplastic extruding to obtain a flame retardant layer;
[0036] (2) forming a first base film layer and a second base film layer on both sides of the flame retardant layer, respectively, so as to obtain a composite current collector skeleton;
[0037] (3) A first metal layer and a second metal layer are respectively formed on both sides of the composite current collector skeleton.
[0038] According to the method for preparing the composite current collector according to the embodiment of the present invention, a flame retardant layer is obtained by mixing an adhesive, an ion conductor and flame retardant particles, and then thermoplastic extrusion molding is performed; the ion conductor in the flame retardant layer can improve the conductivity of the composite current collector, and the flame retardant ions can improve the flame retardant effect of the composite current collector, and then the first base film layer and the second base film layer are respectively formed on both sides of the flame retardant layer to obtain a composite current collector skeleton; since the first base film layer and the second base film layer are non-conductive and light in weight, the weight of the composite current collector can be reduced, and the weight energy density of the battery cell can be increased; then the first metal layer and the second metal layer are respectively formed on both sides of the skeleton of the composite current collector to avoid the phenomenon of poor welding caused by the base film layer absorbing welding energy during the preparation of the battery cell. As a result, the composite current collector reduces the ohmic impedance of the welding point, and when applied to a lithium battery, it can realize the efficient transmission of ions inside the lithium battery, while ensuring that the internal resistance of the lithium battery is low, and the rate performance and safety performance of the lithium battery are significantly improved.
[0039] In addition, the method for preparing a composite current collector according to the above embodiment of the present invention may also have the following additional technical features:
[0040] In some embodiments of the present invention, before the first metal layer and the second metal layer are formed on both sides of the composite current collector skeleton, the composite current collector skeleton is pre-perforated, and then the first conductive layer is formed on the hole wall, thereby facilitating the improvement of the conductivity of the composite current collector.
[0041] In some embodiments of the present invention, the method further comprises: (4) forming a third metal layer and a fourth metal layer arranged at intervals in the thickness direction of one side of the composite current collector skeleton; (5) forming a second conductive layer on the surface of the first metal layer, and forming a third conductive layer on the surface of the second metal layer. In this way, the welding yield of the composite current collector can be improved, and the phenomenon of increased impedance of the welding point can be avoided.
[0042] In the third aspect of the present invention, the present invention proposes an electrode sheet. According to an embodiment of the present invention, the electrode sheet includes the composite current collector described above or the composite current collector prepared by the method described above. As a result, the electrode sheet has a lower internal resistance, thereby enabling high-strength welding of the tabs; applying the electrode sheet in a lithium-ion battery can ensure the normal output of the lithium-ion battery current and achieve efficient transmission of ions inside the lithium-ion battery.
[0043] In a fourth aspect of the present invention, the present invention provides a lithium ion battery. According to an embodiment of the present invention, the lithium ion battery comprises the above-mentioned electrode sheet. Thus, the rate performance and safety performance of the lithium ion battery are significantly improved.
[0044] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0046] Figure 1 is a schematic structural diagram of a first region of a composite current collector according to an embodiment of the present invention;
[0047] Figure 2 is a schematic structural diagram of a composite current collector according to another embodiment of the present invention;
[0048] Figure 3 is a schematic structural diagram of a composite current collector according to another embodiment of the present invention;
[0049] Figure 4 is a schematic structural diagram of a composite current collector skeleton according to an embodiment of the present invention;
[0050] Figure 5 is a top view of a composite current collector skeleton according to an embodiment of the present invention;
[0051] Figure 6 is a schematic flow chart of a method for preparing the composite current collector according to an embodiment of the present invention;
[0052] Figure 7 It is a schematic flow chart of a method for preparing the composite current collector according to another embodiment of the present invention. DETAILED DESCRIPTION
[0053] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0054] In one aspect of the present invention, the present invention provides a composite current collector. According to an embodiment of the present invention, the composite current collector includes a first region 10 and a second region 20, Figure 1 The first region 10 in the composite current collector includes: a flame retardant layer 100 , a base film layer 200 and a metal layer 300 .
[0055] According to an embodiment of the present invention, the flame retardant layer 100 includes an adhesive, an ion conductor and flame retardant particles, wherein the ion conductor can make the flame retardant layer 100 conductive, and the flame retardant particles can make the flame retardant layer 100 flame retardant, so that the flame retardant layer 100 has both flame retardancy and conductivity.
[0056] Furthermore, the mass ratio of the above-mentioned adhesive, ion conductor and flame retardant particles is (1-28): (1-35): (50-70). The inventors found that if the amount of ion conductor added is too much, it will affect the overall conductivity and flame retardant properties of the flame retardant layer 100, thereby affecting the electrical properties of the battery. If the amount of ion conductor added is too little, the performance of the flame retardant layer 100 in conducting electrons will be seriously reduced, and the impedance of the battery made of this material will be too large. If the amount of flame retardant particles added is too much, the conductive performance in the flame retardant layer 100 will be greatly reduced, thereby changing the performance of the main body. If the amount of flame retardant particles added is too little, the flame retardant layer 100 of the battery prepared by the current collector will not achieve a good flame retardant effect when the battery has thermal runaway. At the same time, the thickness of the above-mentioned flame retardant layer 100 is 0.5-3μm. The inventors found that if the thickness of the flame retardant layer 100 is too thick, the thickness of the overall composite current collector will increase, and then the amount of active material applied in the same shell size will decrease, affecting the energy of the battery. If the thickness of the flame retardant layer 100 is too thin, the effect of the flame retardant layer 100 will be affected, and thus when the battery cell has thermal runaway, etc., an effective flame retardant effect cannot be achieved.
[0057] It should be noted that the specific materials of the above-mentioned adhesive, ion conductor and flame retardant particles are not particularly limited, and those skilled in the art can select them as needed. For example, the adhesive includes at least one of ethylene copolymer, polyolefin, polyester and polyamide, wherein the polyolefin can be polyethylene and the polyester can be polyurethane; the ion conductor includes at least one of LATP, LAGP, LLZO, LiTi2(PO4)3, LiCF3SO3, LiBF4, LiPF6 and LiODFB; the flame retardant particles include at least one of magnesium hydroxide, aluminum hydroxide, ammonium polyphosphate, zinc borate, antimony trioxide and layered silicate.
[0058] According to an embodiment of the present invention, referring to Figure 1, the base film layer 200 includes a first base film layer 21 and a second base film layer 22, the first base film layer 21 is arranged on the flame retardant layer 100, and the second base film layer 22 is arranged on the side of the flame retardant layer 100 away from the first base film layer 21. Furthermore, the thickness of the first base film layer 21 is 0.5-5 μm, and the thickness of the second base film layer 22 is 0.5-5 μm. The inventors found that if the thickness of the first base film layer 21 and the second base film layer 22 is too thick, the mass of the active material coated on the battery cell under the premise of the same shell size is reduced, thereby reducing the capacity of the battery cell. If the thickness of the first base film layer 21 and the second base film layer 22 is too thin, the intrinsic tensile strength performance of the composite current collector is reduced, which leads to the rupture of the composite current collector during the later cycle of the battery cell.
[0059] It should be noted that those skilled in the art can select specific materials for the first base film layer 21 and the second base film layer 22 as needed. For example, the first base film layer 21 and the second base film layer 22 can independently use at least one of polyester terephthalate, polyamide, polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyethylene terephthalate, polybutylene terephthalate, poly(p-phenylene terephthalamide), polypropylene, acrylonitrile-butadiene-styrene copolymer, polyvinyl formal, polyvinyl butyral, polyurethane, polyurethane, polyacrylonitrile, polyvinyl acetate, polyformaldehyde, phenolic resin, epoxy resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber, polycarbonate, polysulfone, polyethersulfone and polyphenylene ether.
[0060] Further, refer to Figure 4-5 The flame retardant layer 100 and the first base film layer 21 and the second base film layer 22 form a composite current collector skeleton, on which a through hole 11 is formed along its thickness direction, referring to Figure 5 , there are multiple through holes 11, and a first conductive layer (not shown) is provided on the hole wall of the through hole 11. The inventors found that by forming the first conductive layer on the hole wall of the through hole 11, the conductive performance of the composite current collector can be improved as a whole, and the thickness of the first conductive layer is 0.01 to 2 μm. The inventors found that if the thickness of the first conductive layer is too thick, the aperture of the through hole 11 becomes smaller, so that the channel may be blocked, thereby affecting the transmission speed of ions in the composite current collector, and if the thickness of the first conductive layer is too thin, there is no effective conductive network in the hole wall of the through hole 11, which leads to the phenomenon of increased impedance of the battery cell during the charging and discharging process.
[0061] Further, refer to Figure 5, the diameter D of the through hole 11 is 0.02 to 1 mm. The inventors found that if the diameter of the through hole 11 is too large, the intrinsic strength of the composite current collector will be greatly reduced, thereby affecting its subsequent safe use. If the diameter of the through hole 11 is too small, the aperture of the through hole 11 becomes smaller, so that the channel may be blocked, thereby affecting the transmission speed of ions in the composite current collector. In addition, the edge distance L of any two adjacent through holes 11 is 0.1 mm to 5 mm. The inventors found that if the edge distance between two adjacent through holes 11 is too large, the conductivity of the upper and lower surfaces of the composite current collector will be reduced, thereby affecting the performance of the battery cell. If the edge distance between two adjacent through holes 11 is too small, the intrinsic tensile strength of the composite current collector will be greatly reduced.
[0062] According to an embodiment of the present invention, referring to Figure 1 , the metal layer 300 includes a first metal layer 31 and a second metal layer 32, the first metal layer 31 is arranged on the first base film layer 21, and the second metal layer 32 is arranged on the side of the second base film layer 22 away from the first metal layer 31, so as to avoid the phenomenon of poor welding caused by the base film layer 200 absorbing welding energy during the preparation of the battery cell. Furthermore, the thickness of the first metal layer 31 and the second metal layer 32 are independently 0.01 to 2 μm. The inventors found that if the thickness of the first metal layer 31 and the second metal layer 32 is too thick, the mass of the active material coated on the battery cell is reduced under the premise of the same shell size, thereby reducing the capacity of the battery cell. If the thickness of the first metal layer 31 and the second metal layer 32 is too thin, the intrinsic tensile strength performance of the composite current collector is reduced, which leads to the breakage of the composite current collector during the later cycle of the battery cell.
[0063] It should be noted that those skilled in the art can select specific types of the first metal layer 31 and the second metal layer 32 as needed. For example, the first metal layer 31 and the second metal layer 32 independently include at least one of aluminum, copper, nickel, titanium, silver, stainless steel, nickel-copper alloy and aluminum-zirconium alloy.
[0064] Further, refer to Figure 2, the second region 20 is arranged on the first region 10 along the first direction, the first direction is the length direction along the first region 10 and / or the second region 20, and the length of the first region 10 is greater than or equal to the length of the second region 20, wherein the second region 20 includes a third metal layer 33 and a fourth metal layer 34, and the third metal layer 33 and the fourth metal layer 34 are arranged at intervals. The inventors found that by providing the second region 20, and the second region 20 includes the third metal layer 33 and the fourth metal layer 34 arranged at intervals, the phenomenon of poor welding due to the base film layer 200 absorbing welding energy during the preparation of the battery cell can be avoided. At the same time, since the third metal layer 33 and the fourth metal layer 34 are arranged at intervals, there is no base film layer 200 between the two, so that the welding operability is high when the tab and the current collector are welded, and the phenomenon of increased impedance of the welding point due to the insulation of the base film layer 200 can also be avoided.
[0065] Furthermore, the thickness of the third metal layer 33 and the fourth metal layer 34 are independently 0.01 to 2 μm. The inventors found that if the thickness of the third metal layer 33 and the fourth metal layer 34 is too thick, the process cost of the entire composite current collector will be greatly increased under the premise of ensuring normal charging and discharging of the battery cell. If the thickness of the third metal layer 33 and the fourth metal layer 34 is too thin, it may cause the composite current collector to be over-welded when welding the external pole ears of the battery cell. At the same time, those skilled in the art can select the specific types of the third metal layer 33 and the fourth metal layer 34 as needed, such as the third metal layer 33 and the fourth metal layer 34 independently include at least one of aluminum, copper, nickel, titanium, silver, stainless steel, nickel-copper alloy and aluminum-zirconium alloy.
[0066] According to an embodiment of the present invention, referring to Figure 3 The composite current collector also includes a second conductive layer 400 and a third conductive layer 500. The second conductive layer 400 is arranged on the first metal layer 31, and the third conductive layer 500 is arranged on the second metal layer 32 away from the second conductive layer 400, thereby significantly improving the rate performance of the battery cell.
[0067] Further, the thickness of the second conductive layer 400 and the third conductive layer 500 are independently 0.01 to 2 μm. The inventors found that if the thickness of the second conductive layer 400 and the third conductive layer 500 is too thick, the mass of the active material coated on the battery cell under the premise of the same shell size is reduced, thereby reducing the capacity of the battery cell. If the thickness of the second conductive layer 400 and the third conductive layer 500 is too thin, the metal layer 300 and the coating layer cannot form an effective conductive network, thereby causing the battery cell to have an impedance increase during the charging and discharging process. It should also be noted that those skilled in the art can select the specific types of the first conductive layer (not shown), the second conductive layer 400 and the third conductive layer 500 as needed. For example, the first conductive layer, the second conductive layer 400 and the third conductive layer 500 can independently include at least one of graphite, acetylene black, graphene and carbon nanotubes.
[0068] In the second aspect of the present invention, the present invention provides a method for preparing the above composite current collector. Figure 6 , the method comprising:
[0069] S100: Mixing adhesive, ion conductor and flame retardant particles, then thermoplastic extrusion molding
[0070] In this step, the adhesive, ion conductor and flame retardant ions are mixed and then thermoplastic extruded to obtain a flame retardant layer, wherein the ion conductor can make the flame retardant layer conductive, and the flame retardant particles can make the flame retardant layer flame retardant, so that the flame retardant layer has both flame retardancy and conductivity.
[0071] It should be noted that the specific types and mixing ratios of the adhesive, ion conductor and flame retardant ions used in this step are the same as described above, and the thickness of the flame retardant layer obtained is also the same as described above, which will not be repeated here.
[0072] S200: Forming the first base film layer and the second base film layer on both sides of the flame retardant layer respectively
[0073] In this step, refer to Figure 4 The first base film layer and the second base film layer are formed on both sides of the flame retardant layer to obtain a composite current collector skeleton. Specifically, the first base film layer and the second base film layer can be formed on both sides of the flame retardant layer by magnetron sputtering or coating to form an integrated structure.
[0074] It should be noted that the specific types of the first base membrane layer and the second base membrane layer used in this step and their formation thicknesses are the same as described above and will not be repeated here.
[0075] S300: Forming a first metal layer and a second metal layer on both sides of the composite current collector skeleton
[0076] In this step, a first metal layer and a second metal layer are formed on both sides of the composite current collector skeleton to obtain a composite current collector. Specifically, the first metal layer is arranged on the first base film layer, and the second metal layer is arranged on the side of the second base film layer away from the first metal layer. The first metal layer and the second metal layer are formed on both sides of the composite current collector skeleton by magnetron sputtering or coating, and the composite current collector and the first metal layer and the second metal layer form an integrated structure with each other.
[0077] It should be noted that the specific types and formation thicknesses of the first metal layer and the second metal layer are the same as described above and will not be repeated here.
[0078] Furthermore, before forming the first metal layer and the second metal layer on both sides of the obtained composite current collector skeleton, the composite current collector skeleton is pre-punched, and then the first conductive layer is formed on the hole wall. Specifically, through holes are formed on the composite current collector by laser punching, chemical etching process or mechanical punching, so as to increase the conductivity of the composite current collector.
[0079] It should be noted that the diameter and number of the through holes and the edge distance between any two adjacent through holes are the same as described above, and the thickness and specific type of the first conductive layer are also the same as described above, which will not be repeated here.
[0080] Therefore, the composite current collector obtained by this method reduces the ohmic impedance of the welding point. Applying it to a lithium battery can achieve efficient transmission of ions inside the lithium battery, while ensuring that the internal resistance of the lithium battery is low, and the rate performance and safety performance of the lithium battery are significantly improved.
[0081] According to an embodiment of the present invention, referring to Figure 7 , the above method further comprises:
[0082] S400: forming a third metal layer and a fourth metal layer arranged at intervals in the thickness direction of one side of the composite current collector skeleton
[0083] In this step, a third metal layer and a fourth metal layer are formed in a spaced arrangement in the thickness direction of one side of the composite current collector skeleton. Specifically, the third metal layer and the fourth metal layer are formed in the thickness direction of one side of the composite current collector skeleton by magnetron sputtering or coating. Since there is no insulating base film layer between the third metal layer and the fourth metal layer, when the surfaces of the third metal layer and the fourth metal layer are welded to the tab or other current collector, the operability is improved and the welding yield is high.
[0084] It should be noted that the specific types and formation thicknesses of the third metal layer and the fourth metal layer are the same as described above and will not be repeated here.
[0085] S500: forming a second conductive layer on the surface of the first metal layer, and forming a third conductive layer on the surface of the second metal layer
[0086] In this step, a second conductive layer is formed on the surface of the first metal layer by magnetron sputtering or coating, and a third conductive layer is formed on the surface of the second metal layer by magnetron sputtering or coating, and the first metal layer and the second conductive layer form an integrated structure, and the second metal layer and the third conductive layer also form an integrated structure. Specifically, the second conductive layer is arranged on the first metal layer, and the third conductive layer is arranged on a side of the second metal layer away from the second conductive layer, thereby significantly improving the rate performance of the battery cell.
[0087] It should be noted that the specific types and formation thicknesses of the second conductive layer and the third conductive layer are the same as described above and will not be repeated here.
[0088] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0089] Example 1
[0090] The adhesive polyethylene, ion conductor LLZO and nano flame retardant inorganic particles aluminum hydroxide are mixed (the mass ratio of polyethylene, LLZO and aluminum hydroxide is 15:23:62) and copolymerized, and then processed into a sheet roll state with a thickness of 4μm by a thermoplastic extrusion molding process. The first base film layer and the second base film layer are extruded from polyethylene terephthalate and are both in a roll state with a thickness of 1μm. Then the flame retardant layer, the first base film layer and the second base film layer are processed into a 6μm thick composite current collector skeleton by a lamination molding process, and then the composite current collector skeleton is unwound by an unwinding mechanism, and a through hole is formed on the composite current collector skeleton by a laser punching process, and a first metal aluminum conductive layer with a thickness of 2μm is formed on the hole wall of the through hole, the aperture D of the through hole is 30μm, and the distance L between any adjacent through hole edges is 175um. Then, a first metal aluminum layer and a second metal aluminum layer with a thickness of 2 μm are formed on the upper and lower surfaces of the composite current collector skeleton by a high-temperature vacuum vapor coating process, wherein the first metal aluminum layer is formed on the first base film layer, and the second metal aluminum layer is formed on the second base film layer. At the same time, a third metal aluminum layer and a fourth metal aluminum layer with a thickness of 2 μm are formed on the right side of the composite current collector skeleton by a high-temperature vacuum vapor coating process. Finally, the third metal aluminum layer and the fourth metal aluminum layer are shielded, and a conductive layer of acetylene black with a thickness of 1 μm is formed on the surface of the first metal aluminum layer and the second metal aluminum layer by a magnetron sputtering process, and finally a composite aluminum foil current collector is obtained.
[0091] The preparation method of the positive electrode sheet used in the laminated lithium-ion battery A1 includes the following steps: adding 96g of active material NMC811, 2g of conductive agent carbon black and 2g of binder PVDF to 80g of NMP, mixing them evenly to obtain a ternary positive electrode slurry, and evenly coating the ternary positive electrode slurry on the surface of the composite aluminum foil current collector obtained above, and drying to obtain a positive electrode sheet.
[0092] The preparation method of the negative electrode sheet used in the laminated lithium-ion battery A1 includes the following steps: adding 95.4g of negative electrode active material graphite powder, 2.6g of conductive agent carbon black, 1g of thickener CMC (sodium carboxymethyl cellulose) and 1g of binder SBR (styrene-butadiene rubber) to 90g of deionized water, mixing them evenly to obtain a negative electrode slurry, and evenly coating the negative electrode slurry on the surface of the negative electrode sheet collector copper foil with a thickness of 10μm, and drying to obtain a negative electrode sheet.
[0093] When preparing the above-mentioned laminated lithium-ion battery A1, the positive electrode sheet, the negative electrode sheet and the separator are laminated to obtain a laminated battery cell, and then the tabs of all the positive electrode sheets of the laminated battery cell are ultrasonically welded, and the tabs of all the negative electrode sheets are ultrasonically welded, and then placed in a shell, and electrolyte (dimethyl carbonate DMC / ethylene carbonate EC / ethyl methyl carbonate EMC, the concentration of lithium hexafluorophosphate LiPF6 is 1M) is injected, and sealed to obtain the laminated lithium-ion battery A1.
[0094] Example 2
[0095] The adhesive polyamide, the ion conductor LATP and the nano flame retardant inorganic particle antimony trioxide are mixed (the mass ratio of polyamide, LATP and antimony trioxide is 17:25:58) and copolymerized, and then processed into a sheet roll state with a thickness of 2μm by a thermoplastic extrusion molding process. The first base film layer and the second base film layer are extruded from polyethylene terephthalate and are both in a roll state with a thickness of 0.5μm. Then the flame retardant layer, the first base film layer and the second base film layer are processed into a 3μm thick composite current collector skeleton by a lamination molding process, and then the composite current collector skeleton is unwound by an unwinding mechanism, and a through hole is formed on the composite current collector skeleton by a laser punching process, and a first metal aluminum conductive layer with a thickness of 2μm is formed on the hole wall of the through hole, the aperture D of the through hole is 25μm, and the distance L between any adjacent through hole edges is 165μm. Then, a first metal copper layer and a second metal copper layer with a thickness of 1.5 μm are formed on both sides of the composite current collector skeleton by a high-temperature vacuum vapor coating process, and a third metal copper layer and a fourth metal copper layer with a thickness of 1.5 μm are formed on the right side of the composite current collector skeleton by a high-temperature vacuum vapor coating process. Finally, the third metal copper layer and the fourth metal copper layer are shielded, and a conductive layer of acetylene black with a thickness of 1 μm is formed on the surface of the first metal copper layer and the second metal copper layer by a magnetron sputtering process, and finally a composite aluminum foil current collector is obtained.
[0096] In this embodiment 2 of the present invention, the electrochemical energy storage device is a laminated lithium-ion battery A2, which differs from the laminated lithium-ion battery A1 only in that the composite current collector in the positive electrode sheet adopts the composite aluminum foil current collector obtained in embodiment 2, and the remaining steps are the same as the laminated lithium-ion battery A1.
[0097] Comparative Example
[0098] The first base film layer and the second base film layer of polyethylene terephthalate are extruded into a roll state with a thickness of 4μm. Then the first base film layer and the second base film layer are processed into a 6μm thick composite current collector skeleton by a lamination molding process. Then, a first metal aluminum layer and a second metal aluminum layer with a thickness of 2μm are formed on the upper and lower surfaces of the composite current collector skeleton by a high-temperature vacuum vapor coating process, and at the same time, a third metal aluminum layer and a fourth metal aluminum layer with a thickness of 1μm are formed on the right side of the composite current collector skeleton in the thickness direction by a high-temperature vacuum vapor coating process. Finally, the third metal aluminum layer and the fourth metal aluminum layer are shielded, and a conductive layer of acetylene black with a thickness of 1μm is formed on the surface of the first metal aluminum layer and the second metal aluminum layer by a magnetron sputtering process, and finally a composite aluminum foil current collector is obtained.
[0099] In this comparative example of the present invention, the electrochemical energy storage device is a laminated lithium-ion battery A3, which differs from the laminated lithium-ion battery A1 only in that the composite current collector in the positive electrode sheet adopts the composite aluminum foil current collector obtained in the comparative example, and the remaining steps are the same as the laminated lithium-ion battery A1.
[0100] Experimental Example 1
[0101] During the preparation process of laminated lithium-ion batteries A1~A3, tensile strength tests were performed on different composite current collectors and statistics were obtained. The test method was as follows: a 15mm wide composite current collector sample was prepared using a Ligao CD-500g tensile testing machine, the substrate was clamped by the upper and lower jaws of the tensile testing machine, and stretching was started until the material was broken.
[0102] Experimental Example 2
[0103] During the preparation of laminated lithium-ion batteries A1 to A3, the surface resistance of different positive plates was tested using an AT526SE resistance tester. One end of the resistance tester was connected to the pole ear of the pole piece, and the other end was connected to the pole piece with a contact area of Copper conductor weight 500g.
[0104] Experimental Example 3
[0105] During the preparation of laminated lithium-ion batteries A1 to A3, the same welding process was used to weld the tabs of different positive electrode sheets in the laminated battery cells, and the welding pass rate was statistically analyzed. The statistical results are shown in the table.
[0106] Experimental Example 4
[0107] During the preparation process of stacked lithium-ion batteries A1~A3, the cell capacity of different composite current collector processes was tested and counted. The test method is: the sample battery 1C battery is charged to 4.2V at a constant current, and then the cell is discharged to 0% SOC at 1C, and it is left to stand for 3 minutes. The capacity data C1 is recorded, and the cell weight W1 is weighed. The voltage platform is calculated as 3.67V, and the energy density = C1*3.67 / W1 is obtained.
[0108] The results of the composite current collector, positive electrode sheet surface resistance, positive electrode sheet welding pass rate and battery cell energy density in the laminated lithium-ion batteries A1 to A3 obtained by testing in Experimental Examples 1-4 are shown in Table 1.
[0109] Table 1
[0110]
[0111] It can be seen from Table 1 that the tensile strength of the composite current collector in the laminated lithium-ion battery A1 is higher than the tensile strength of the composite current collector in the laminated lithium-ion battery A3, while the tensile strength of the composite current collector in the laminated lithium-ion battery A2 is lower than the tensile strength of the composite current collector in the laminated lithium-ion battery A3. This is because the thickness of the composite current collector in the laminated lithium-ion battery A2 (9 μm) is lower than the thickness of the composite current collector in the laminated lithium-ion battery A3 (12 μm). At the same time, the cell energy density of the laminated lithium-ion battery A1 is slightly lower than the cell energy density in the laminated lithium-ion battery A3, while the cell energy density of the laminated lithium-ion battery A2 is slightly lower than the cell energy density in the laminated lithium-ion battery A3. This is because the thickness of the composite current collector in the laminated lithium-ion battery A2 (9 μm) is higher than the thickness of the composite current collector in the laminated lithium-ion battery A3 (12 μm). This is because the positive energy density of the laminated lithium-ion battery A1 The composite current collector of the pole piece has a flame retardant layer, and the weight of the composite current collector is higher than the composite and three-dimensional weight in the laminated lithium-ion battery A3. Under the premise of the same cell capacity and voltage, the cell energy density of the laminated lithium-ion battery A1 is lower, while the composite current collector in the positive pole piece of the laminated lithium-ion battery A2 is thin and light. Under the premise of the same capacity and voltage, the cell energy density of the laminated lithium-ion battery A2 is higher. In addition, the surface resistance of the positive pole piece in the laminated lithium-ion batteries A1 and A2 is significantly lower than that of the laminated lithium-ion battery A3, and the welding pass rate of the positive pole piece in the laminated lithium-ion batteries A1 and A2 is significantly higher than that of the laminated lithium-ion battery A3. This shows that the flame retardant layer including an adhesive, an ion conductor and flame retardant particles is provided between the base film layer and the metal layer of the present application can significantly reduce the resistance of the composite current collector, thereby reducing the internal resistance of the battery, and at the same time improving the welding pass rate of the positive pole piece using the composite current collector.
[0112] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0113] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A composite current collector, comprising a first region and a second region, characterized in that: The first area includes: Flame retardant layer; A base film layer, the base film layer comprising a first base film layer and a second base film layer, the first base film layer is arranged on the flame retardant layer, the second base film layer is arranged on a side of the flame retardant layer away from the first base film layer, the first base film layer has a thickness of 0.5 to 5 μm, and the second base film layer has a thickness of 0.5 to 5 μm; A metal layer, the metal layer comprising a first metal layer and a second metal layer, the first metal layer being disposed on the first base film layer, and the second metal layer being disposed on a side of the second base film layer away from the first metal layer; Wherein, the flame retardant layer comprises an adhesive, an ion conductor and flame retardant particles, and the mass ratio of the adhesive, the ion conductor and the flame retardant particles is (1-28):(1-35):(50-70); The second region is arranged on the first region along a first direction, the first direction is a length direction along the first region and / or the second region, and the length of the first region is greater than or equal to the length of the second region, wherein the second region includes a third metal layer and a fourth metal layer, and the third metal layer is arranged at intervals from the fourth metal layer.
2. The composite current collector according to claim 1, characterized in that: The flame retardant layer and the base film layer are provided with through holes along the thickness direction thereof, and the hole walls of the through holes are provided with a first conductive layer; The thickness of the first conductive layer is 0.01-2 μm; The first conductive layer includes at least one of graphite, acetylene black, graphene and carbon nanotubes; The thickness of the flame retardant layer is 0.5-3 μm; There are multiple through holes; The diameter of the through hole is 0.02-1 mm; The edge distance between any two adjacent through holes is 0.1 mm to 5 mm.
3. The composite current collector according to claim 1, It is characterized by: The thickness of the first base film layer and the second base film layer is 0.5-5 μm; The thickness of the first metal layer, the second metal layer, the third metal layer and the fourth metal layer are independently 0.01-2 μm.
4. The composite current collector according to claim 3, characterized in that: The material of the base film layer includes at least one of polyethylene terephthalate, polyamide, polyimide, polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyethylene terephthalate, polybutylene terephthalate, poly(p-phenylene terephthalamide), polypropylene, acrylonitrile-butadiene-styrene copolymer, polyvinyl formal, polyvinyl butyral, polyurethane, polyurethane, polyacrylonitrile, polyvinyl acetate, polyoxymethylene, phenolic resin, epoxy resin, polytetrafluoroethylene, polyvinylidene fluoride, silicone rubber, polycarbonate, polysulfone, polyethersulfone and polyphenylene ether; The first metal layer, the second metal layer, the third metal layer and the fourth metal layer independently include at least one of aluminum, copper, nickel, titanium, silver, stainless steel, nickel-copper alloy and aluminum-zirconium alloy.
5. The composite current collector according to claim 1, characterized in that: It also includes a second conductive layer and a third conductive layer, wherein the second conductive layer is disposed on the first metal layer, and the third conductive layer is disposed on a side of the second metal layer away from the second conductive layer; The thickness of the second conductive layer and the third conductive layer are independently 0.01-2 μm; The second conductive layer and the third conductive layer each independently include at least one of graphite, graphene, acetylene black and carbon nanotubes.
6. The composite current collector according to claim 1, characterized in that: The mass ratio of the adhesive, the ion conductor and the flame retardant particles is (1-28):(1-35):(50-70); The adhesive comprises at least one of ethylene copolymer, polyolefin, polyester and polyamide; The ion conductor includes at least one of LATP, LAGP, LLZO, LiTi2(PO4)3, LiCF3SO3, LiBF4, LiPF6 and LiODFB; The flame retardant particles include at least one of magnesium hydroxide, aluminum hydroxide, ammonium polyphosphate, zinc borate, antimony trioxide and layered silicate.
7. A method for preparing the composite current collector according to any one of claims 1 to 6, characterized in that: include: (1) mixing an adhesive, an ion conductor and flame retardant particles, and then thermoplastic extruding to obtain a flame retardant layer; (2) forming a first base film layer and a second base film layer on both sides of the flame retardant layer respectively to obtain a composite current collector skeleton; (3) forming a first metal layer and a second metal layer on both sides of the composite current collector skeleton, respectively; Before the first metal layer and the second metal layer are respectively formed on both sides of the composite current collector skeleton, the composite current collector skeleton is pre-punched, and then the first conductive layer is formed on the hole wall.
8. The method according to claim 7, characterized in that Further including: (4) forming a third metal layer and a fourth metal layer arranged at intervals in the thickness direction of one side of the composite current collector skeleton; (5) A second conductive layer is formed on a surface of the first metal layer, and a third conductive layer is formed on a surface of the second metal layer.
9. An electrode sheet, characterized in that: The composite current collector comprises the composite current collector described in any one of claims 1 to 6 or the composite current collector prepared by the method described in claim 7 or 8.
10. A lithium ion battery, characterized in that: Comprising the electrode sheet as claimed in claim 9.