A short-wave near-infrared broadband antireflection film and preparation method thereof

Through the Al2O3-ZrO2-Al2O3-ZrO2-MgF2 five-layer film structure, the problem of the limited band range of the existing short-wave near-infrared anti-reflection film and the easy crystallization of ZrO2 is solved, achieving high transmittance and broadband anti-reflection effect, and improving Improves the mechanical strength and damage resistance of the membrane.

CN114609702BActive Publication Date: 2024-10-15BEIJING JUNTONG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210274504.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-03-21
Publication Date
2024-10-15
Estimated Expiration
2042-03-21

AI Technical Summary

Technical Problem

The existing short-wave near-infrared anti-reflection coating has a limited range of wavelengths and high reflectivity, which affects the imaging effect and detection accuracy. Moreover, the ZrO2 material is easy to crystallize, resulting in an increase in the roughness of the film layer and a decrease in the refractive index.

Method used

Adopting a five-layer film structure of Al2O3-ZrO2-Al2O3-ZrO2-MgF2, deposited by electron beam evaporation method, using Al2O3 as the bottom material to prevent ZrO2 crystallization, and using MgF2 as the outer coating layer to improve moisture resistance and hardness, and design non-uniform film thickness to improve transmittance.

Benefits of technology

It achieves high transmittance and broadband in the range of 0.65~1.05μm, reduces light energy reflection loss, avoids the formation of fog spots under the film, and improves mechanical strength and damage resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114609702B_ABST
    Figure CN114609702B_ABST
Patent Text Reader

Abstract

A short-wave near-infrared broadband anti-reflection film and a preparation method thereof, wherein the anti-reflection film is a double-sided deposited anti-reflection film deposited on an optical glass substrate, and is composed of five thin film layers of unequal thickness, which are Al2O3 thin film layer, ZrO2 thin film layer, Al2O3 thin film layer, ZrO2 thin film layer, and MgF2 thin film layer from the surface of the optical glass substrate outward in sequence. The short-wave near-infrared broadband anti-reflection film prepared by the method of the present invention overcomes the deficiency of optical glass in anti-reflection ability, reduces the reflection loss of light energy, and improves the anti-reflection broadband. The average transmittance between 0.65-1.05μm is 99.12%, and the minimum transmittance is 98.47%, which spans the visible light band and the near-infrared band; at the same time, the problem that the film layer is easy to crystallize when it encounters moisture is further solved, and it has good moisture resistance and is not easy to have fog spots under the film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of optical thin films and evaporation thereof, and in particular to a short-wave near-infrared broadband antireflection film and a preparation method thereof. Background Art

[0002] Short-wave near-infrared broadband anti-reflection film is a necessary film layer in instruments that share visual information and lasers. Its main function is to reduce the reflected light on the surface of optical components, thereby increasing the light transmittance, reducing energy loss, improving detection accuracy, and achieving a clearer observation effect. Anti-reflection film is also called anti-reflection film. In a multi-element optical system, there are many lenses. If the anti-reflection film is not coated on the surface of the lens, it will cause light energy loss, reduce the imaging effect, and increase the component load. In addition, the stray light formed by the reflection on the surface of each lens reaches the image plane, affecting the imaging effect and the detection accuracy of the sensor. As the engineering needs continue to increase, the requirements for anti-reflection films increase accordingly. For example, in laser measuring instruments, in order to avoid laser energy damaging optical components, the reflectivity of the surface is required to be reduced; at the same time, because there is still a need for visual inspection, in order to improve image balance, imaging quality and other requirements, wide-band anti-reflection films are widely needed.

[0003] The anti-reflection band range of a single-layer anti-reflection film is limited, and the residual reflection is still high, the color balance is destroyed, and the imaging effect is poor. Multi-layer films can improve the anti-reflection band, and the geometric thickness between the film layers is non-uniformly arranged, which can effectively improve the transmittance and imaging effect.

[0004] ZrO2 is a thin film material with a relatively high refractive index, good mechanical properties and resistance to strong alkali corrosion. However, during the deposition process, due to its large particles and easy crystallization when exposed to moisture, the film roughness will increase, the refractive index will decrease, and the light dissipation loss will increase.

[0005] Al2O3 has good optical properties in the visible, near and mid-infrared bands, and its transparent area is 0.3 to 9μm. The film is hard, tough, and has good moisture resistance. As the first coating, it can effectively solve the problem of ZrO2 crystallizing easily when exposed to moisture. MgF2 material is hard and non-hygroscopic. As an outer coating layer, it effectively improves the hardness of the coating and improves moisture resistance. Summary of the invention

[0006] The object of the present invention is to provide a short-wave near-infrared broadband antireflection film, which has excellent transmittance and passband half width in the mission band.

[0007] Another object of the present invention is a method for preparing the above-mentioned short-wave near-infrared broadband antireflection film.

[0008] The purpose of the present invention is achieved through the following technical solutions:

[0009] A short-wave near-infrared broadband anti-reflection film, characterized in that: the anti-reflection film is a double-sided deposited anti-reflection film deposited on an optical glass substrate, and is composed of five non-uniform thin film layers, which are Al2O3 thin film layer, ZrO2 thin film layer, Al2O3 thin film layer, ZrO2 thin film layer, and MgF2 thin film layer from the surface of the optical glass substrate to the outside.

[0010] The present invention uses Al2O3 as a medium refractive index material, ZrO2 as a high refractive index material, and MgF2 as a low refractive index material to form a multilayer film with five layers of Al2O3-ZrO2-Al2O3-ZrO2-MgF2. -6 / K's Al2O3 is used as the bottom material to adjust the overall stress, and its good moisture resistance is used as the bottom material to effectively prevent the occurrence of fog spots after evaporation.

[0011] Furthermore, the Al2O3 thin film layer, the ZrO2 thin film layer and the MgF2 thin film layer are all prepared by electron beam evaporation, and the process is simple.

[0012] The method for preparing the above-mentioned short-wave near-infrared broadband anti-reflection film is characterized in that: after the glass substrate is cleaned, it is preheated, and Al2O3, ZrO2 and MgF2 film materials are pre-melted at the same time, and Al2O3 thin film layer, ZrO2 thin film layer, Al2O3 thin film layer, ZrO2 thin film layer, and MgF2 thin film layer are prepared on the surface of the substrate in sequence by electron beam evaporation. The thickness of each film layer is designed to be non-uniform, and is 125nm, 81nm, 23nm, 79nm, and 147nm, respectively.

[0013] The above five layers of thin film deposition are further performed when the glass substrate temperature reaches 260°C and the vacuum degree reaches 4×10 -3 When ΔP·m2 / s is 0.0447 W·m2, the electron gun is turned on and evaporation deposition is carried out in sequence. The deposition rates are as follows: Al2O3 thin film layer: 0.3~0.4nm / s, ZrO2 thin film layer: 0.28~0.30nm / s, MgF2 thin film layer: 0.36~0.40nm / s.

[0014] The selection range of the bottom low refractive index material combined with the glass substrate is very wide, and the film combination obtained under different preparation process conditions is very different. The Al2O3 film layer is used as the bottom material, and its good density is used to effectively isolate the contact between the ZrO2 film layer and the glass substrate, preventing the formation of fog spots under the film due to the reaction and crystallization of impurities existing in the glass smelting with ZrO2, thereby improving the light stability.

[0015] The most specific method is a method for preparing a short-wave near-infrared broadband, characterized in that the method is carried out according to the following steps:

[0016] S1. Evaporation pre-treatment

[0017] Optical glass with a refractive index of 1.49-1.58 was selected as the substrate. It was ultrasonically cleaned with ethanol, ether mixture and deionized water in sequence. After drying, it was placed in a vacuum chamber chuck for baking and preheating. When the temperature of the glass substrate reached 260°C, it was kept warm and the vacuum degree was drawn to 4×10 -3 Pa, pre-melting Al2O3, ZrO2, and MgF2 film materials;

[0018] S2. Preparation of Al2O3 and ZrO2 thin films by electron beam evaporation

[0019] Keep the vacuum chamber environment at 4×10 -3 Pa, and the glass substrate temperature is 260 ° C, Al2O3 material is evaporated, and the deposition rate is 0.3~0.4nm / s, and then ZrO2 material is evaporated, and the deposition rate is 0.28~0.30nm / s, and then the environmental parameters in the vacuum chamber are kept unchanged, and the above process is repeated once, and the four film layers are evaporated from the surface of the glass substrate to the outside in sequence, and the thicknesses are 125nm, 81nm, 23nm, and 79nm respectively;

[0020] S3. Preparation of MgF2 thin film by electron beam evaporation

[0021] Under the same parameter environment as in S2, MgF2 thin film layer deposition was carried out, with a deposition rate of 0.36~0.40nm / s and a film thickness of 147nm.

[0022] In the process of preparing multi-layer composite antireflection film, it is found that if the deposition rate of the film material is too fast, the edge of the film is prone to curling and shrinking. The deposition stability during the deposition process is the main reason for the uneven surface of the film and thus peeling. The present invention uses a low deposition rate to make each layer of the film material deposit more evenly, so that the adhesion between the film layers is good and it is not easy to fall off.

[0023] It was further found in the above preparation process that if the Al2O3 film layer is replaced with other low refractive index materials, it is easy to cause the ZrO2 film layer to react with the glass substrate surface, produce crystals, and form fog spots under the film. By taking advantage of the good density of Al2O3 after deposition, the reaction between the ZrO2 film layer and impurities carried in the glass smelting is effectively isolated, thereby improving the quality of the film.

[0024] The present invention has the following technical effects:

[0025] The multi-layer composite anti-reflection film prepared by the method of the present invention overcomes the deficiency of optical glass in anti-reflection ability, reduces the reflection loss of light energy, and improves the anti-reflection broadband. The average transmittance between 0.65 and 1.05 μm is 99.12%, and the minimum transmittance is 98.47%. The problem of easy crystallization of ZrO2 material is solved, and the film is not easy to produce under-film fog spots. At the same time, the stress of the film is reduced, and the residual stress is as low as 0.53 GPa. The film has excellent mechanical strength and anti-destruction quality. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 : Comparison of transmittance curves of the antireflection film prepared by the present invention and the glass substrate before coating. DETAILED DESCRIPTION

[0027] The present invention is described in detail below through examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Those skilled in the art can make some non-essential improvements and adjustments to the present invention based on the above content of the present invention.

[0028] Example 1

[0029] A method for preparing a short-wave near-infrared broadband antireflection film is carried out according to the following steps:

[0030] S1. Evaporation pre-treatment

[0031] K9 optical glass with a refractive index of 1.52 was selected as the substrate. It was ultrasonically cleaned with ethanol, ether mixture and deionized water in sequence. After drying, it was placed in a vacuum chamber chuck for baking and preheating. When the temperature of the glass substrate reached 260°C, it was kept warm for 10 minutes and the vacuum degree was drawn to 4×10 -3 Pa, pre-melting Al2O3, ZrO2, and MgF2 film materials;

[0032] S2. Preparation of Al2O3 and ZrO2 thin films by electron beam evaporation

[0033] Keep the vacuum chamber environment at 4×10 -3 Pa, and the glass substrate temperature is 260 ° C, Al2O3 material is evaporated, and the deposition rate is 0.3nm / s, and then ZrO2 material is evaporated, and the deposition rate is 0.28nm / s, and then the environmental parameters in the vacuum chamber are kept unchanged, and the above process is repeated once, and the four film layers are evaporated from the surface of the glass substrate to the outside in sequence, and the thicknesses are 125nm, 81nm, 23nm, and 79nm respectively;

[0034] S3. Preparation of MgF2 thin film by electron beam evaporation

[0035] Under the same parameter environment as in S2, MgF2 thin film layer deposition was carried out with a deposition rate of 0.38 nm / s and a film thickness of 147 nm.

[0036] After the film was placed in a humid environment for one week, no fogging was observed under the film.

[0037] Al2O3-ZrO2-MgF2 multilayer film has excellent transmittance and large bandwidth. The average transmittance between 0.65~1.05μm is 99.11%, and the minimum transmittance is 98.73%.

[0038] The mechanical properties of the prepared film layer were tested by wrapping two layers of dry degreased gauze around the rubber friction head and rubbing the film layer along the same track under a pressure of 4.9N for 25 times. The film layer had no scratches or other damage. The width was 2cm, and the peel strength was ≥2.94N / cm 2 The tape paper is firmly adhered to the surface of the film layer. After the tape paper is quickly pulled up from the edge of the part toward the surface in a direction perpendicular to the surface, the film layer does not fall off or get damaged, which proves that the thin film layer prepared above has good mechanical strength.

[0039] The antireflection film prepared by the present invention has excellent transmittance and passband width, with an average transmittance of 99.12% between 0.65 and 1.05 μm, a minimum transmittance of 98.47%, and an effective bandwidth of 400 nm. Before the glass substrate is not evaporated with the film prepared by the present invention, the average transmittance between 0.65 and 1.05 μm is only 92.17%.

Claims

1. A method for preparing a short-wave near-infrared broadband antireflection film, characterized in that: The antireflection film is a double-sided deposited antireflection film deposited on an optical glass substrate, and is composed of five non-uniform thin film layers with unequal geometric thicknesses, which are Al2O3 thin film layer, ZrO2 thin film layer, Al2O3 thin film layer, ZrO2 thin film layer, and MgF2 thin film layer in order from the surface of the optical glass substrate to the outside; The preparation method is carried out according to the following steps: S1. Pre-treatment before evaporation Optical glass with a refractive index of 1.49-1.58 was selected as the substrate. It was ultrasonically cleaned with ethanol, ether mixture and deionized water in sequence. After drying, it was placed in a vacuum chamber chuck for baking and preheating. When the temperature of the glass substrate reached 260°C, it was kept warm and the vacuum degree was drawn to 4×10 -3 Pa, pre-melting Al2O3, ZrO2, and MgF2 film materials; S2. Preparation of Al2O3 and ZrO2 thin films by electron beam evaporation Keep the vacuum environment still at 4×10 -3 Pa, and the glass substrate temperature is 260 ° C, Al2O3 material is evaporated, and the deposition rate is 0.3-0.4nm / s, and then ZrO2 material is evaporated, and the deposition rate is 0.28-0.30nm / s, and then the environmental parameters in the vacuum chamber are kept unchanged, and the above S2 process is repeated once, and the four film layers are evaporated from the surface of the glass substrate to the outside in sequence, and the thicknesses are 125nm, 81nm, 23nm, and 79nm respectively; S3. Preparation of MgF2 thin film layer by electron beam evaporation Under the same parameter environment as in S2, a MgF2 thin film layer was deposited at a deposition rate of 0.36-0.40 nm / s and a film thickness of 147 nm.