Improvement of the billet continuous casting process for aluminum-containing steel nodules
By filling the tundish with argon, adding covering agent, controlling superheat and drawing speed, and optimizing the design of the nozzle and stopper rod in the billet continuous casting process, the problem of nodulation of aluminum-containing steel was solved and the inclusion reduction was achieved. and improve the stability of the casting stream.
Patent Information
- Application Number
- CN202210306178.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-25
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-03-25
AI Technical Summary
During the continuous casting process of billet, aluminum-containing steel is easy to form nodules, resulting in nozzle blockage and production interruption. This is mainly due to the accumulation of alumina inclusions and the involvement of foreign slag inclusions, and it is difficult to effectively solve it with the existing technology.
An improved billet continuous casting process is adopted, including filling the ladle with argon before pouring, adding covering agent after pouring, controlling superheat and pulling speed, and using optimized integral immersed nozzles and stoppers to ensure protection of the casing The argon seal and liquid level are stabilized, the ladle is lifted to remove slag inclusions, and the design of the nozzle and plug rod is adjusted to reduce adhesion.
Effectively reduce the involvement of foreign inclusions, optimize the nozzle structure and plug rod design, reduce the accumulation of alumina inclusions, improve the stability of the casting flow, slow down the impact of nodulation on the plug rod head, and improve production efficiency.
Smart Images

Figure CN114619003B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron and steel metallurgy, and more specifically to a small square billet continuous casting process for improving aluminum-containing steel nodules. Background Art
[0002] The deoxidation product of aluminum-containing steel is Al2O3, whose melting point reaches 2050℃. The interfacial tension between molten steel and Al2O3 is large, and Al2O3 has a tendency to cluster with each other. It only takes 0.03s for two 10um Al2O3 inclusions to bond, and the bonding force is very large and has sufficient strength after bonding. Therefore, alumina inclusions are easily accumulated through collision to form large particle inclusions, which precipitate during the casting process and adhere to the nozzle, causing nozzle nodules.
[0003] Since the inner diameter of the continuous casting nozzle of small square billets (casting machine cross-section less than 200 square meters) is smaller, Al2O3 inclusions and adhesion are more likely to cause the nozzle to be blocked and not flow down, resulting in production interruption. Therefore, the difficulty of producing aluminum-containing steel from small square billets is much greater than that from large square billets and slabs.
[0004] In addition to the cleanliness and composition of molten steel, the inclusion of foreign slag caused by the non-steady-state casting of the continuous casting process is also an important factor affecting the nodule formation, which is often easily overlooked on site. In addition, the stopper rods and nozzles used in the production of aluminum steel and non-aluminum steel on each site are basically the same, but the two types of steel have completely different erosion effects on refractory materials. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a small square billet continuous casting process for improving the nodules of aluminum-containing steel.
[0006] The technical solution adopted by the present invention to solve the technical problem is: construct a small square billet continuous casting process for improving aluminum-containing steel nodules, comprising the following steps:
[0007] 1) Fill the middle bag with argon before pouring;
[0008] 2) When the net weight of the tundish is greater than 1 / 2 of the tundish capacity after the ladle is poured, add covering agent;
[0009] 3) Superheat and drawing speed control: The superheat control target of molten steel in the pouring furnace is 30-50℃, and the superheat control target of molten steel in the continuous pouring furnace is 25-40℃. The superheat of molten steel is not less than 20℃; after the pouring is completed and the crystallizer liquid level is stable, the steel casting operation is carried out at a constant drawing speed;
[0010] 4) The argon seal of the protective sleeve, the tundish and the liquid surface of the crystallizer are not exposed;
[0011] 5) Normally, the insertion depth of the ladle protection sleeve in the molten steel is about 250mm. When the net weight of the molten steel in the ladle is about 10 tons, the ladle is lifted about 100mm to pour steel until the molten steel in the furnace is poured. At this time, the insertion depth of the ladle protection sleeve in the molten steel is about 150mm;
[0012] 6) When the molten steel in the ladle is poured out, the ladle replacement time should not exceed 150s;
[0013] 7) Adopt optimized integral immersion nozzle suitable for aluminum-steel casting;
[0014] 8) Use optimized stopper rod suitable for aluminum-steel casting.
[0015] According to the above scheme, in step 3), the pulling speed is controlled according to the actual production rhythm on site, the pulling speed of the 150-160 square section casting machine is not less than 2.6m / min, and the pulling speed of the 200 square section casting machine is not less than 1.6m / min.
[0016] According to the above scheme, in step 7), the diameter of the inner hole of the submerged nozzle is 35-40 mm, and the inner hole of the nozzle has a 0 taper or a negative taper.
[0017] According to the above scheme, in step 8), the arc radius of the plug head is 25-30mm.
[0018] The implementation of the small square billet continuous casting process for improving aluminum-containing steel nodules of the present invention has the following beneficial effects:
[0019] 1. On the basis of controlling the protective casting, reduce the involvement of foreign inclusions. Control the time of adding covering agent in the pouring furnace to minimize the involvement of covering agent caused by the punching process.
[0020] 2. Carry out ladle lifting operation at the end of ladle casting to facilitate the floating and removal of foreign slag.
[0021] 3. In view of the characteristics of aluminum-steel nodules, the overall immersed nozzle is optimized, the inner diameter of the nozzle is enlarged, and the positive taper of the inner hole of the nozzle is adjusted to 0 taper or negative taper, so that the alumina inclusions are not easy to gather and bond on the inner wall of the nozzle.
[0022] 4. Adjusting the arc radius of the stopper rod head from the conventional 30-40mm to between 25-30mm can reduce the impact of the stopper rod head on the flow control of the casting machine caused by the enlargement of the nodule. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The present invention will be further described below with reference to the accompanying drawings and embodiments, in which:
[0024] Figure 1 This is the structural diagram of the integral submerged nozzle of a conventional small square billet;
[0025] Figure 2 The structure diagram of the stopper rod used in the conventional billet tundish;
[0026] Figure 3 This is the optimized structure diagram of the overall submerged nozzle for small square billets;
[0027] Figure 4 This is the optimized stopper rod structure for the billet tundish. DETAILED DESCRIPTION
[0028] In order to have a clearer understanding of the technical features, purposes and effects of the present invention, specific embodiments of the present invention are now described in detail with reference to the accompanying drawings.
[0029] like Figure 3-4 As shown, the small square billet continuous casting process for improving aluminum-containing steel nodules of the present invention comprises the following steps:
[0030] 1) Before pouring, fill the tundish with argon (if there is an argon blowing device on the tundish cover, turn on the argon; if there is no argon blowing device on the tundish cover, connect one end of the hose to the argon pipe and the other end to the steel pipe, and insert the steel pipe into the tundish for artificial argon blowing).
[0031] 2) After the ladle is poured, the covering agent can only be added when the net weight of the middle ladle is greater than 1 / 2 of the middle ladle capacity (for example, if the middle ladle capacity is 40t, the covering agent can be added only when the net weight of the molten steel in the middle ladle is greater than 20t). If the covering agent is added too early, the ladle flushing process will easily cause the covering agent to be drawn into the molten steel, and its impact on the steel quality is far greater than the oxidation of the molten steel caused by the lack of covering agent.
[0032] 3) Superheat and drawing speed control: The superheat control target of the molten steel in the pouring furnace is 30-50℃, and the superheat control target of the molten steel in the continuous pouring furnace is 25-40℃. The superheat of the molten steel should not be lower than 20℃, otherwise it will reduce the fluidity of the molten steel and aggravate the occurrence of nodules. After the pouring is completed and the crystallizer liquid level is stable, the steel casting operation is carried out at a constant drawing speed (the drawing speed is controlled according to the actual production rhythm on site, but it should not be too low, such as the drawing speed of the 150-160 square section casting machine should not be lower than 2.6m / min, and the drawing speed of the 200 square section casting machine should not be lower than 1.6m / min).
[0033] 4) Carry out conventional protective casting, such as argon sealing of protective sleeve, and no exposed liquid surface of tundish and crystallizer;
[0034] 5) Normally, the insertion depth of the ladle protection sleeve in the molten steel is about 250mm. When the net weight of the molten steel in the ladle is about 10 tons, the ladle is lifted about 100mm to pour the steel until the molten steel in the furnace is poured (that is, the insertion depth of the ladle protection sleeve in the molten steel is about 150mm at this time).
[0035] At the end of each casting, the molten steel is mixed with slag and flows into the tundish, which seriously affects the quality of the molten steel, unless the steel is shut off before slag is discharged. However, this operation is extremely costly and is rarely used by steel mills. At present, even if domestic steel mills perform the steel shut-off operation, they only shut off the steel after the slag reaches a certain level (using slag detection), rather than shutting off the steel before slag is discharged, which has already caused pollution to the molten steel in the tundish. Lifting the ladle 100mm to pour steel at the end of the casting will help the large particles flowing into the tundish to float up, and at the same time help to judge the slag.
[0036] 6) When the molten steel in the ladle is poured out, the ladle changing time must be strictly controlled and must not exceed 150s. During the ladle changing operation, the molten steel level in the middle ladle continues to drop. If the ladle changing time is too long and the liquid level drops too much, the ladle flushing process after the molten steel in the lower ladle is connected will easily cause slag rolling and contaminate the molten steel.
[0037] 7) The inner hole of the conventional integral immersion nozzle has a certain taper, that is, the upper size of the inner hole of the nozzle is larger than the lower size. Since aluminum steel does not corrode the nozzle strongly, the main problem of aluminum steel production from small square billets is nodules, and the number of single-drum continuous casting furnaces for aluminum steel production by domestic small square billet casting machines is generally low (generally within 10 furnaces), so the diameter of the inner hole of the conventional immersion nozzle can be expanded from the conventional 28mm to 35-40mm, and the positive taper of the inner hole of the nozzle can be adjusted to 0 taper (the upper size of the inner hole of the nozzle is consistent with the lower size) or negative taper (the upper size of the inner hole of the nozzle is smaller than the lower size).
[0038] Using the optimized nozzle can prevent alumina inclusions from gathering and sticking to the inner wall of the nozzle, and allow them to flow into the crystallizer along with the steel flow. In addition, due to the enlarged diameter of the inner hole of the nozzle, even if there is a small amount of sticking, it will not affect the normal control of the casting stream.
[0039] 8) Conventional stopper rods are used to solve the problem of molten steel corrosion. The arc radius of the stopper rod head is usually between 30-40mm. If the arc radius is designed to be too small, it will not be resistant to corrosion, making the liquid level control of the crystallizer unstable in the later stage of casting. When casting aluminum steel, the stopper rod head will become larger due to nodules. Therefore, the arc radius of the stopper rod head can be adjusted to between 25-30mm, which can reduce the impact of the nodule enlargement on the flow control of the casting machine caused by the enlargement of the stopper rod head.
[0040] The embodiments of the present invention are described above in conjunction with the accompanying drawings, but the present invention is not limited to the above-mentioned specific implementation modes, which are merely illustrative rather than restrictive. Under the guidance of the present invention, ordinary technicians in this field can also make many forms without departing from the scope of protection of the present invention and the claims, all of which are within the protection of the present invention.
Claims
1. A billet continuous casting process for improving aluminum-containing steel nodules. It is characterized in that The following steps are involved: 1) Fill the middle bag with argon before pouring; 2) When the net weight of the tundish is greater than 1 / 2 of the tundish capacity after the ladle is poured, add covering agent; 3) Superheat and drawing speed control: The superheat control target of molten steel in the pouring furnace is 30-50℃, and the superheat control target of molten steel in the continuous pouring furnace is 25-40℃. The superheat of molten steel shall not be less than 20℃; after the pouring is completed and the liquid level of the crystallizer is stable, the steel casting operation shall be carried out at a constant drawing speed; 4) The argon seal of the protective sleeve, the tundish and the liquid surface of the crystallizer are not exposed; 5) Normally, the insertion depth of the ladle protection sleeve in the molten steel is 250mm. When the net weight of the molten steel in the ladle is 10 tons, the ladle is lifted 100mm to pour steel until the molten steel in the furnace is poured. At this time, the insertion depth of the ladle protection sleeve in the molten steel is 150mm; 6) When the molten steel in the ladle is poured out, the ladle replacement time should not exceed 150s; 7) Use an integral submerged nozzle suitable for aluminum-steel casting. The diameter of the inner hole of the submerged nozzle is 35-40mm, and the inner hole of the nozzle is 0 taper or negative taper; 8) Use a stopper rod suitable for aluminum-steel casting, and the arc radius of the stopper rod head is 25-30mm.
2. The process for continuous casting of small square billets for improving nodules in aluminum-containing steel according to claim 1, It is characterized in that In step 3), the pulling speed is controlled according to the actual production rhythm on site. The pulling speed of the 150-160 square section casting machine is not less than 2.6m / min, and the pulling speed of the 200 square section casting machine is not less than 1.6m / min.
Citation Information
Patent Citations
Titanium-containing solder wire steel production method capable of alleviating continuous casting nozzle clogging
CN104259414A
Efficient production process of high aluminum-alloy-content structure round steel
CN105177215A
Casting method for overcoming blockage of stopper rod flow control Al deoxidized molten steel opening
CN109332625A
Single-point unbalanced protection casting method for producing ultrathin large-specification aluminum-containing steel special-shaped blank
CN109396409A
Process for improving IF steel continuous casting heats
CN109880970A