Foldable device, strip and method of manufacturing the same

By introducing a central tensile stress zone and a compressive stress zone into the substrate of a foldable device, combining chemical reinforcement and refractive index matching of the adhesive, the impact resistance and spin resistance of the equipment with the smallest bending radius in the prior art is solved. The problem of insufficient penetration achieves efficient impact and puncture resistance.

CN114631136BActive Publication Date: 2024-11-26CORNING INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080076312.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-14
Filing Date
2020-08-28
Publication Date
2024-11-26
Estimated Expiration
2040-08-28

AI Technical Summary

Technical Problem

When pursuing a small minimum bending radius, existing foldable equipment and strips often find it difficult to take into account excellent impact resistance and puncture resistance, especially plastic displays and cover plates with small minimum bending radius and ultra-thin glass substrates. Poor performance in impact resistance and puncture resistance.

Method used

Designed with foldable equipment including glass substrates or ceramic substrates, wherein the thickness and stress distribution of the substrate are optimized by introducing a central tensile stress zone and compressive stress zone into the substrate to achieve a low minimum bending radius and excellent impact resistance and puncture resistance. Specific methods include introducing high compression stress zones into the central portion of the substrate and reducing bending induced stresses through chemical reinforcement or matching refractive index of the adhesive, reducing the risk of fracture.

Benefits of technology

It is achieved while maintaining a small minimum bending radius, providing excellent impact resistance and puncture resistance, reducing the risk of damage caused by bending and simplifying the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114631136B_ABST
    Figure CN114631136B_ABST
Patent Text Reader

Abstract

A foldable device may include a foldable substrate including a substrate thickness and a center portion between a first portion and a second portion. The center portion may include a center thickness that is less than the substrate thickness. A first maximum tensile stress of a first tensile stress zone in the first portion and a second maximum tensile stress of a second tensile stress zone in the second portion may be less than a third maximum tensile stress of a center tensile stress zone in the center portion. A strip may include a strip thickness and a center portion between the first portion and the second portion. The center portion may include a first center compressive stress zone and a second center compressive stress zone. In some embodiments, a method of processing a strip may include masking the first portion, masking the second portion, and chemically strengthening the center portion.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of priority under 35 U.S.C. §119 to U.S. Provisional Application Serial No. 62 / 914,720, filed on October 14, 2019, and U.S. Provisional Application Serial No. 62 / 893,306, filed on August 29, 2019, the contents of each of which are based upon and incorporated herein by reference in their entirety. Technical Field

[0003] The present disclosure relates generally to foldable devices, foldable strips and methods of making the same, and more particularly to foldable devices and strips comprising a foldable substrate and the foldable substrate comprising a compressive stress region, and methods of making the foldable devices and strips. Background Art

[0004] Glass-based substrates (eg, tapes) are commonly used, for example, in display devices such as liquid crystal displays (LCDs), electrophoretic displays (EPDs), organic light emitting diode displays (OLEDs), plasma display panels (PDPs), and the like.

[0005] It is desirable to develop a display in a foldable form and a foldable protective cover mounted on the foldable display. The foldable display and the cover should have excellent impact resistance and puncture resistance. At the same time, the foldable display and the cover should have a small minimum bending radius [e.g., about 10 millimeters (mm) or less]. However, plastic displays and covers with a small minimum bending radius often have poor impact resistance and / or puncture resistance.

[0006] In addition, conventional wisdom suggests that ultra-thin glass-based sheets with a small minimum bending radius [e.g., having a thickness of less than or equal to about 75 micrometers (μm or micron)] tend to have poor impact resistance and / or puncture resistance. Furthermore, thicker glass-based sheets with excellent impact resistance and / or puncture resistance (e.g., greater than 125 microns) tend to have a relatively large minimum bending radius (e.g., greater than or equal to about 30 mm). As a result, there is a need to develop foldable substrates for foldable devices that have a low minimum bending radius and excellent impact resistance and puncture resistance.

[0007] In addition, strengthened (e.g., chemically strengthened, thermally strengthened) ribbons (e.g., glass-based ribbons, ceramic-based ribbons) with small minimum bending radii tend to have poor impact resistance and / or puncture resistance. Moreover, unstrengthened ribbons with excellent impact resistance and / or puncture resistance tend to have relatively large minimum bending radii (e.g., greater than or equal to about 30 mm). Therefore, there is a need to develop ribbons for foldable devices with low minimum bending radii and excellent impact resistance and puncture resistance. Summary of the invention

[0008] Foldable devices and methods of making foldable devices are described herein, the foldable devices including foldable substrates or strips, the strips including glass-based substrates and / or ceramic-based substrates. The foldable substrates and strips can provide a small effective minimum bending radius while providing excellent impact resistance and puncture resistance, as well as low energy fracture. The device of the present disclosure can include a first portion and a second portion and have a substrate thickness. The substrate thickness can be sufficiently large [e.g., about 80 microns (micron or μm) to about 2 millimeters] to provide excellent impact resistance and excellent puncture resistance.

[0009] The apparatus of the present disclosure may include attaching the first portion to the central portion of the second portion. In particular, embodiments of the present disclosure may provide a central portion including a central tensile stress region, which may be located between a first central compressive stress region and a second central compressive stress region. In some embodiments, the maximum tensile stress of the central tensile stress region may be greater than the maximum tensile stress of the first tensile stress region in the first portion and / or the maximum tensile stress of the second tensile stress region in the second portion. In some embodiments, the first portion and / or the second portion may be substantially unstrengthened (e.g., stress-free, chemically unstrengthened, thermally unstrengthened), and substantially have no tensile stress region or have a small value of maximum tensile stress. The central maximum tensile stress provided is greater than the first maximum tensile stress of the first tensile stress region (if provided), and / or the second maximum tensile stress of the second tensile stress region (if provided), thereby making the fracture caused by impact in the first portion and / or the second portion a low-energy fracture, while providing excellent folding performance. In some embodiments, the low-energy fracture may be the result of a reduced thickness of the central portion, and for a given maximum tensile stress, the reduced-thickness central portion stores less energy than the thicker glass portion. In some embodiments, the low energy fracture can be the result of fracture of the first portion and / or the second portion away from the central portion undergoing bending, wherein the first portion and / or the second portion comprises a lower maximum tensile stress than the central portion. The central maximum tensile stress provided is greater than the first maximum tensile stress of the first tensile stress region (if provided), and / or the second maximum tensile stress of the second tensile stress region (if provided), thereby providing excellent impact resistance and / or fracture resistance in the first portion and / or the second portion, which is indicated by excellent pen drop performance.

[0010] The device of the present disclosure may include a central portion attaching the first portion to the second portion. The central portion may include a central thickness that is less than the thickness of the substrate. The central thickness may be sufficiently small (e.g., from about 10 microns to about 125 microns) to be in the bending region of the foldable device and to provide a low effective bending radius (e.g., less than or equal to about 10 mm, or less than or equal to about 9 mm, or less than or equal to about 8 mm, or less than or equal to about 7 mm, or less than or equal to about 6 mm, or less than or equal to about 5 mm, or less than or equal to about 4 mm, or less than or equal to about 3 mm, less than or equal to about 2 mm, about 1 mm). As shown by Fig.14 As indicated by the surprising results of the presented pen drop test, glass-based substrates comprising a thickness of less than or equal to about 50 μm provide excellent pen drop performance, while a thickness of about 50 μm to about 80 μm provides poor pen drop performance. Further, in some embodiments, providing a substantially uniform compression depth associated with a compressive stress region of a foldable substrate can simplify the manufacture of the article by avoiding the use of masking or other non-uniform ion exchange methods.

[0011] The strip according to the disclosed embodiments includes a center portion including a first center compressive stress zone extending to a first center compression depth, and a second center compressive stress zone extending to a second compression depth, the strip can achieve a small minimum bend radius (e.g., less than or equal to about 10 mm) because the compressive stress zone (e.g., from chemical strengthening) can counteract the bending-induced tensile forces. Further, providing a first center compression depth and / or a second center compression depth in the range of about 10% to about 30% of the thickness of the strip can achieve a small minimum bend radius. Similarly, a center portion including a first center layer depth and / or a second center layer depth greater than or equal to about 10% can achieve a small minimum bend radius. Providing a first edge portion of the center region having a compressive stress zone, compression depth, and / or layer depth and / or a second edge portion of the center region can further achieve a small minimum bend radius by reducing damage (e.g., fracture and / or cracking) due to bending-induced stresses. In some embodiments, the maximum compressive stress of the first central compressive stress region can be substantially equal to the maximum compressive stress of the second central compressive stress region, which can provide a ribbon with low warpage (e.g., less than or equal to about 2 nm, less than or equal to about 1 nm). In some embodiments, providing a central portion having a width of about 5 times the minimum bending radius (e.g., a width of about 5 mm to about 55 mm) can reduce (e.g., avoid) stress concentration and damage along the bending length of the ribbon when it is at or near the minimum bending radius, thereby enabling a small minimum bending radius. At the same time, the first portion and / or the second portion can achieve excellent impact resistance and / or puncture resistance. In some embodiments, the first portion and / or the second portion may include a surface roughness of less than or equal to about 0.3 nanometers at the first major surface and / or the second major surface. The smoothness of the surface in the first portion and / or the second portion (e.g., low surface roughness) can minimize defects in the surface, which can reduce the incidence of ribbon damage (e.g., fracture and / or cracking). In some embodiments, the first portion and / or the second portion may include a layer depth from the first major surface and / or the second major surface that is in the range of 0% to about 5% of the tape thickness of the tape. In some embodiments, the first portion and / or the second portion may include a stress-free area at the first major surface and / or the second major surface. The lack of significant chemical strengthening and / or compressive stress at the surface of the first portion and / or the second portion can minimize the occurrence of defects in the surface, which can reduce the incidence of tape damage (e.g., fractures and / or cracks). When the tape is part of a foldable device that includes an adhesive (e.g., an optically clear adhesive), matching the refractive index of the adhesive to the refractive index of the tape (e.g., within about 0.1) can minimize optical distortion in the foldable device.

[0012] Some exemplary embodiments of the present disclosure are described below, while it should be understood that any features of the various embodiments may be used alone or in combination with each other.

[0013] Embodiment 1: A strip comprising a strip thickness defined between a first major surface and a second major surface opposite the first major surface. The strip comprises a first portion comprising a first stress-free region at the first major surface and a second stress-free region at the second major surface. The strip comprises a second portion comprising a third stress-free region at the first major surface and a fourth stress-free region at the second major surface. The strip further comprises a central portion comprising a first central compressive stress zone and a second central compressive stress zone, the first central compressive stress zone extending from the first major surface to a first central compression depth, the second central compressive stress zone extending from the second major surface to a second central compression depth. The central portion is located between the first portion and the second portion in the direction of the strip length.

[0014] Embodiment 2: A strip comprising a strip thickness defined between a first major surface and a second major surface opposite the first major surface. The strip comprises a first portion comprising a first layer depth from 0% to about 5% of the strip thickness from the first major surface and a second layer depth from 0% to about 5% of the strip thickness from the second major surface. The strip comprises a second portion comprising a third layer depth from 0% to about 5% of the strip thickness from the first major surface and a fourth layer depth from 0% to about 5% of the strip thickness from the second major surface. The strip comprises a central portion comprising a first central layer depth of about 10% or more of the strip thickness from the first major surface. The central portion comprises a first central compressive stress zone extending from the first major surface to the first central compressive depth. The central portion includes a second central layer depth that is about 10% or more of the strip thickness from the second major surface, and the central portion includes a second central compressive stress zone that extends from the second major surface to the second central compressive depth. The central portion is located between the first portion and the second portion in the direction of the strip length.

[0015] Embodiment 3: The strip of any of Embodiments 1-2, wherein the first central compression depth is about 10% to about 30% of the strip thickness.

[0016] Embodiment 4: The strip of any of Embodiments 1-3, wherein the second central compression depth is about 10% to about 30% of the strip thickness.

[0017] Embodiment 5: The ribbon includes a ribbon thickness defined between a first major surface and a second major surface opposite the first major surface. The ribbon includes a first portion including a first surface roughness of the first major surface less than or equal to about 0.3 nanometers. The first portion includes a second surface roughness of the second major surface less than or equal to about 0.3 nanometers. The ribbon includes a second portion including a third surface roughness at the first major surface less than or equal to about 0.3 nanometers. The second portion includes a fourth surface roughness of the second major surface less than or equal to about 0.3 nanometers. The ribbon includes a central portion including a first central compressive stress zone extending from the first major surface to a first central compression depth. The central portion includes a second central compressive stress zone extending from the second major surface to a second central compression depth. The first central compression depth is about 10% to about 30% of the ribbon thickness. The second central compression depth is about 10% to about 30% of the ribbon thickness. The central portion is located between the first portion and the second portion in the direction of the ribbon length.

[0018] Embodiment 6: The strip of any one of embodiments 1-5, further comprising a width defined between a first edge of the strip and a second edge of the strip opposite the first edge. The first edge extends between the first major surface and the second major surface. The second edge extends between the first major surface and the second major surface. The first central compressive stress region and the second central compressive stress region each extend from the first edge to the second edge.

[0019] Embodiment 7: The strip of any of Embodiments 2-4, further comprising a first tensile stress zone located between the first compressive stress zone and the second compressive stress zone. The first tensile stress zone comprises a first maximum tensile stress. The strip further comprises a second tensile stress zone located between the third compressive stress zone and the fourth compressive stress zone. The second tensile stress zone comprises a second maximum tensile stress. The strip further comprises a central tensile stress zone located between the first central compressive stress zone and the second central compressive stress zone. The central tensile stress zone comprises a central maximum tensile stress. The central maximum tensile stress is greater than the first maximum tensile stress. The central maximum tensile stress is greater than the second maximum tensile stress.

[0020] Embodiment 8: The strip of any of Embodiments 1-6, further comprising a central tensile stress region located between the first central compressive stress region and the second central compressive stress region. The central tensile stress comprises a central maximum tensile stress in a range of about 10 MPa to about 375 MPa.

[0021] Embodiment 9: The strip of any of Embodiments 1-8, wherein the strip comprises a minimum bend radius of less than 10 millimeters.

[0022] Embodiment 10: The strip of embodiment 9, wherein the minimum bending radius is 5 mm.

[0023] Embodiment 11: The strip of embodiment 9, wherein the minimum bending radius is 3 mm.

[0024] Embodiment 12: The strip of any of Embodiments 9-11, wherein the length of the center portion in the length direction of the strip is about 5 times or more the minimum bend radius.

[0025] Embodiment 13: The tape of any of Embodiments 1-11, wherein the length of the center portion in the length direction of the tape is in a range from about 5 mm to about 55 mm.

[0026] Embodiment 14: The tape of any of Embodiments 1-13, wherein the tape has a length in a range from about 20 mm to about 500 mm.

[0027] Embodiment 15: The tape of any of Embodiments 1-14, wherein the tape thickness is in a range from about 25 microns to about 150 microns.

[0028] Embodiment 16: The tape of any of Embodiments 1-15, wherein the tape exhibits a warp of about 10 nanometers to about 2 micrometers relative to a first plane defined by the first major surface.

[0029] As in embodiment 17: the tape of embodiment 16, wherein the warpage is in a range of about 100 nanometers to about 1 micron.

[0030] Embodiment 18: The strip of any of Embodiments 1-17, wherein the first central compressive stress region and the second central compressive stress region are enriched in sodium and / or potassium.

[0031] Embodiment 19: The tape of any of Embodiments 1-18, wherein the maximum compressive stress of the first central compressive stress zone is in a range from about 10 megapascals to about 1,500 megapascals. The maximum compressive stress of the second central compressive stress zone is in a range from about 10 megapascals to about 1,500 megapascals.

[0032] Embodiment 20: The strip of Embodiment 19, wherein the maximum compressive stress of the first central compressive stress region is substantially equal to the maximum compressive stress of the second central compressive stress region.

[0033] Embodiment 21: The ribbon of any of Embodiments 1-20, wherein the ribbon comprises a glass-based material.

[0034] Embodiment 22: The tape of any of Embodiments 1-20, wherein the tape comprises a ceramic-based substrate.

[0035] Embodiment 23: A foldable device comprising the tape of any one of embodiments 1-22. The foldable device comprises an optically clear adhesive. The foldable device comprises a release liner. The optically clear adhesive is located between the tape and the release liner.

[0036] Embodiment 24: A foldable device comprising the tape of any one of embodiments 1-22. The foldable device comprises an optically clear adhesive. The foldable device comprises a display device. The optically clear adhesive is located between the tape and the display device.

[0037] Embodiment 25: A consumer electronic product comprising a housing, the housing comprising a front surface, a rear surface, and a side surface. The consumer electronic product comprises electrical components at least partially located within the housing, the electrical components comprising a controller, a memory, and a display, the display being located at or near the front surface of the housing. The consumer electronic product comprises a cover substrate disposed above the display. At least one of a portion of the housing or the cover substrate comprises the foldable device of any one of Embodiments 1-24.

[0038] Embodiment 26: A foldable substrate that can be folded around an axis extending along the width direction of the foldable substrate. The foldable substrate also includes a substrate thickness, which is defined between a first major surface and a second major surface opposite the first major surface. The foldable substrate also includes a first portion, the first portion including the substrate thickness and a first tensile stress region, the first tensile stress region including a first maximum tensile stress. The foldable substrate also includes a second portion, the second portion including the substrate thickness and a second tensile stress region, the second tensile stress region including a second maximum tensile stress. The foldable substrate also includes a central portion, the central portion including a first central surface area opposite the second major surface, and a central tensile region, the central tensile region including a central maximum tensile stress. The central portion is located between the first portion and the second portion in the length direction of the foldable substrate, the length direction being perpendicular to the width direction of the foldable substrate. The central portion includes a central thickness defined between the first central surface area and the second major surface. The central thickness is less than the substrate thickness. The first maximum tensile stress is less than the central maximum tensile stress. The second maximum tensile stress is less than the third maximum tensile stress.

[0039] Embodiment 27: The foldable substrate of embodiment 26, wherein the first maximum tensile stress is less than or equal to about 100 megapascals (MPa). The second maximum tensile stress is less than or equal to about 100 MPa. The center maximum tensile stress is in a range from about 125 MPa to about 375 MPa.

[0040] Embodiment 28: The foldable substrate of any of Embodiments 26-27, wherein the first maximum tensile stress is in a range from about 10 megapascals (MPa) to about 100 MPa. The second maximum tensile stress is in a range from about 10 MPa to about 100 MPa.

[0041] Embodiment 29: The foldable substrate of any of Embodiments 26-28, wherein the substrate thickness is in a range from about 100 microns to about 2 millimeters.

[0042] Embodiment 30: The foldable substrate of Embodiment 29, wherein the substrate thickness is in a range from about 125 microns to about 200 microns.

[0043] Embodiment 31: The foldable substrate of any of Embodiments 26-30, wherein the center thickness is in a range from about 25 microns to about 80 microns.

[0044] Embodiment 32: The foldable substrate of Embodiment 31, wherein the center thickness is in a range from about 25 microns to about 50 microns.

[0045] Embodiment 33: The foldable substrate of any of Embodiments 26-32, wherein the center thickness is from about 0.5% to about 13% of the thickness of the substrate.

[0046] Embodiment 34: The foldable substrate of any of Embodiments 26-33, wherein the foldable substrate comprises an effective minimum bend radius in a range from about 1 mm to about 10 mm.

[0047] Embodiment 35: The foldable substrate of embodiment 34, wherein the foldable substrate achieves an effective bending radius of 10 mm.

[0048] Embodiment 36: The foldable substrate of embodiment 35, wherein the foldable substrate achieves an effective bending radius of 5 mm.

[0049] Embodiment 37: The foldable substrate of any of Embodiments 344-36, wherein the width of the central portion is in a range from about 2.8 times the effective minimum bend radius to about 6 times the effective minimum bend radius.

[0050] Embodiment 38: The foldable substrate of any of Embodiments 26-36, wherein the width of the central portion is in a range from about 2.8 mm to about 40 mm.

[0051] Embodiment 39: The foldable substrate of any of Embodiments 26-38, wherein the first portion further comprises a first compressive stress region at the first major surface and a second compressive stress region at the second major surface. The first tensile stress region is located between the first compressive stress region and the second compressive stress region. Further, the second portion comprises a third compressive stress region at the first major surface and a fourth compressive stress region at the second major surface. The second tensile stress region is located between the third compressive stress region and the fourth compressive stress region. Further, the central portion comprises a first central compressive stress region at the first central surface area and a second central compressive stress region at the second major surface. The third tensile stress region is located between the first central compressive stress region and the second central compressive stress region.

[0052] Embodiment 40: The foldable substrate of embodiment 39, wherein the first compression depth of the first compressive stress region is about 1% to about 10% of the thickness of the substrate. The second compression depth of the second compressive stress region is about 1% to about 10% of the thickness of the substrate.

[0053] Embodiment 41: The foldable substrate of any of Embodiments 39-40, wherein the third compression depth of the third compressive stress zone is about 1% to about 10% of the substrate thickness. The fourth compression depth of the fourth compressive stress zone is about 1% to about 10% of the substrate thickness.

[0054] Embodiment 42: The foldable substrate of any of Embodiments 39-41, wherein the first central compression depth of the first central compressive stress region is about 10% to about 30% of the central thickness. The second central compression depth of the second central compressive stress region is about 10% to about 30% of the central thickness.

[0055] Embodiment 43: The foldable substrate of Embodiment 42, wherein the first compression depth is substantially equal to the first central compression depth, and the third compression depth is substantially equal to the first central compression depth.

[0056] Embodiment 44: The foldable substrate of any of Embodiments 42-43, wherein the second compression depth is substantially equal to the second central compression depth, and the fourth compression depth is substantially equal to the second central compression depth.

[0057] Embodiment 45: The foldable substrate of any of Embodiments 39-44, wherein the first compressive stress region comprises a first maximum compressive stress greater than or equal to about 700 megapascals. The second compressive stress region comprises a second maximum compressive stress. The third compressive stress region comprises a third maximum compressive stress greater than or equal to about 700 megapascals. The fourth compressive stress region comprises a fourth maximum compressive stress. The first central compressive stress region comprises a first central maximum compressive stress greater than or equal to about 700 megapascals. The second central compressive stress region comprises a second central maximum compressive stress.

[0058] Embodiment 46: The foldable substrate of Embodiment 45, wherein the second maximum compressive stress is greater than or equal to about 700 megapascals. The fourth maximum compressive stress is greater than or equal to about 700 megapascals. The second center maximum compressive stress is greater than or equal to about 700 megapascals.

[0059] Embodiment 47: The foldable substrate of any one of Embodiments 26-46, wherein the foldable substrate is a glass-based material.

[0060] Embodiment 48: The foldable substrate of any of Embodiments 26-46, wherein the foldable substrate is a ceramic-based material.

[0061] Embodiment 49: A foldable device comprising the foldable substrate of any one of Embodiments 26-48, wherein a recess defined between a first central surface area of ​​the central portion and a first plane defined by the first major surface is filled with an adhesive.

[0062] Embodiment 50: The foldable device of embodiment 49, wherein the magnitude of the difference between the refractive index of the foldable substrate and the refractive index of the adhesive is about 0.1 or less.

[0063] Embodiment 51: The foldable device of any of Embodiments 49-50, wherein the adhesive comprises a first contact surface that contacts the first central surface area.

[0064] Embodiment 52: The foldable device of embodiment 51, wherein the first contact surface of the adhesive contacts the first major surface.

[0065] Embodiment 53: The foldable device of any one of Embodiments 51-52, further comprising a display device attached to the second contact surface of the adhesive.

[0066] Embodiment 54: The foldable device of any of Embodiments 51-52, further comprising a release liner attached to the second contact surface of the adhesive.

[0067] Embodiment 55: A consumer electronic product comprising a housing, the housing comprising a front surface, a rear surface, and a side surface. The consumer electronic product comprises electrical components at least partially located within the housing, the electrical components comprising a controller, a memory, and a display, the display being located at or near the front surface of the housing. The consumer electronic product comprises a cover substrate disposed above the display. At least one of a portion of the housing or the cover substrate comprises the foldable substrate of any one of Embodiments 26-48.

[0068] Embodiment 56: A method of processing a strip, the method comprising masking a first portion of the strip, the first portion comprising a first surface region of a first major surface of the strip and a second surface region of the first major surface of the strip. The method comprises masking a second portion of the strip, the second portion comprising a third surface region of the first major surface and a fourth surface region of the second major surface. The method comprises chemically strengthening a central portion of the strip to achieve a first central compressive stress region and a second central compressive stress region, the first central compressive stress region extending from a central portion of the first major surface to a first central compression depth and the second central compressive stress region extending from a central portion of the second major surface to a second central compression depth. The central portion of the strip is located between the first portion and the second portion.

[0069] Embodiment 57: The method of Embodiment 56, wherein chemical strengthening comprises immersing the strip in a bath comprising sodium and / or potassium.

[0070] Embodiment 58: The method of any of Embodiments 56-57, further comprising: demasking each of the first portion and the second portion after chemical strengthening.

[0071] Embodiment 59: The method of Embodiment 56, wherein chemical strengthening comprises placing a salt solution on a central portion of the first major surface. Chemical strengthening comprises placing a salt solution on a central portion of the second major surface. Chemical strengthening comprises heating the strip at a temperature of about 300° C. to about 500° C. for a time of about 15 minutes to about 12 hours.

[0072] Embodiment 60: The method of Embodiment 59, wherein each of the first portion and the second portion is demasked prior to heating the strip.

[0073] Embodiment 61: The method of any of Embodiments 59-60, wherein the salt solution comprises an organic binder.

[0074] Embodiment 62: The method of any of Embodiments 59-61, wherein the salt solution comprises potassium nitrate and potassium phosphate.

[0075] Embodiment 63: The method of any of Embodiments 56-62, wherein masking the first portion and masking the second portion each include placing one or more of silicon dioxide, aluminum oxide, titanium dioxide, aluminum nitride, silicon oxynitride, magnesium oxide, and / or zirconium oxide.

[0076] Embodiment 64: The method of any of Embodiments 56-63, wherein the first central compression depth is about 10% to about 30% of the strip thickness.

[0077] Embodiment 65: The method of any of Embodiments 56-64, wherein the second central compression depth is about 10% to about 30% of the strip thickness.

[0078] Embodiment 66: The method of any of Embodiments 56-65, wherein the first central compressive stress region and the second central compressive stress region are enriched in sodium and / or potassium.

[0079] Embodiment 67: The method of any of Embodiments 56-66, wherein the maximum compressive stress of the first central compressive stress region is in a range from about 10 megapascals to about 1,500 megapascals. The maximum compressive stress of the second central compressive stress region is in a range from about 10 megapascals to about 1,500 megapascals.

[0080] Embodiment 68: The method of Embodiment 67, wherein the maximum compressive stress of the first compressive stress region is substantially equal to the maximum compressive stress of the second compressive stress region.

[0081] Embodiment 69: The method of any of Embodiments 56-68, wherein the length of the center portion of the ribbon in the length direction of the ribbon is in a range from about 5 mm to about 55 mm.

[0082] Embodiment 70: The method of any of Embodiments 56-69, wherein the ribbon comprises a glass-based material.

[0083] Embodiment 71: The method of any of Embodiments 56-69, wherein the tape comprises a ceramic-based material. BRIEF DESCRIPTION OF THE DRAWINGS

[0084] The above features and advantages and other features and advantages of the embodiments of the present disclosure may be better understood by reading the following detailed description with reference to the accompanying drawings, in which:

[0085] Figure 1 is a schematic diagram of an exemplary foldable device in a flat configuration according to some embodiments;

[0086] Figure 2-3 According to some embodiments, the foldable device is Figure 1 A cross-sectional view along line 2-2 of ;

[0087] Figure 4 is a top plan view of an exemplary strip in a flat configuration according to some embodiments;

[0088] Figure 5 According to some embodiments, the strip is along Figure 4 A side view of line 5-5;

[0089] Figure 6-7Yes Figure 4-5 A cross-sectional view of an exemplary foldable device of a strip of material;

[0090] Figure 8 is in a folded configuration according to some embodiments Figure 3 A schematic diagram of an exemplary foldable device;

[0091] Fig. 9 is an exemplary foldable device in a folded configuration according to some embodiments along Figure 8 A cross-sectional view taken along line 9-9;

[0092] Fig.10 is in a folded configuration according to some embodiments Figure 4-5 A schematic diagram of an exemplary foldable device;

[0093] Fig.11 is an exemplary foldable device in a folded configuration according to some embodiments along Fig.10 A cross-sectional view taken along line 11-11;

[0094] Fig.12 is a cross-sectional view of the impact device used to measure the failure mode;

[0095] Fig.13 Another exemplary foldable device in a folded configuration according to some embodiments is shown along Figure 8 A cross-sectional view taken along line 9-9;

[0096] Fig.14 Experimental results of a pen drop test of a glass-based substrate (e.g., a ribbon) are shown, which shows the maximum principal stress on a major surface of the glass-based substrate as a function of the thickness of the glass-based substrate;

[0097] Fig.15 is a perspective schematic diagram of a pen-drop device;

[0098] Figure 16-29 Schematically illustrating steps in a method of making a foldable device (e.g., foldable substrate, tape);

[0099] Fig.30 is a flow chart illustrating an exemplary method of manufacturing a foldable device (e.g., a strip) according to an embodiment of the present disclosure;

[0100] Fig.31 is a schematic top plan view of an exemplary consumer electronic device according to some embodiments; and

[0101] Fig.32 yes Fig.31 A perspective schematic diagram of an exemplary consumer electronic device.

[0102] In the present disclosure, the drawings are used to emphasize certain aspects. Therefore, unless otherwise explicitly stated, the relative sizes of different regions, parts and substrates shown in the drawings should not be considered to be proportional to their actual relative sizes. DETAILED DESCRIPTION

[0103] The embodiments will be described more fully herein with reference to the accompanying drawings, in which exemplary embodiments are shown. Whenever possible, the same reference numerals are used throughout the drawings to represent the same or similar parts. However, the claims may include many different aspects of the embodiments and should not be construed as being limited to the embodiments set forth herein.

[0104] Figure 1-3 , 9 and 13 illustrate views of foldable devices 101, 301, 801 and 1301 including a foldable substrate 201 according to an embodiment of the present disclosure, and Figure 4-7 11 illustrate views of foldable devices 401, 601, and 701 including strip 501 according to embodiments of the present disclosure. Unless otherwise noted, a discussion of features of an embodiment of a foldable device may be equally applicable to corresponding features of any embodiment of the present disclosure. For example, throughout the present disclosure, the same part number may indicate that the identified features are identical to one another in some embodiments, and a discussion of an identified feature of one embodiment may be equally applicable to an identified feature of any other embodiment of the present disclosure, unless otherwise noted.

[0105] Figure 1-3 Schematically illustrates exemplary embodiments of foldable devices 101 and 301 in an unfolded (eg, flat) configuration according to embodiments of the present disclosure. Figure 2-3 As shown, the foldable device 101 and 301 may include a foldable substrate 201 and an adhesive 207 [e.g., an optically clear adhesive (OCA)]. In some embodiments, as Figure 2 As shown, the foldable device 101 may include a release liner 213. In some embodiments, such as Figure 3 As shown, the foldable device 301 may include a display device 303 .

[0106] Figure 4-7 Schematically illustrates exemplary embodiments of foldable devices 401, 601, and 701 in an unfolded configuration (eg, a flat configuration) according to embodiments of the present disclosure. Figure 6-7 As shown, the foldable devices 601 and 701 may include a tape 501 and an adhesive 207 [e.g., an optically clear adhesive (OCA)]. In some embodiments, as shown in FIG. Figure 6 As shown, the foldable device 601 may include a release liner 213. In some embodiments, such as Figure 7As shown, the foldable device 701 may include a display device 303 .

[0107] Foldable substrate 201 and / or 1601 and / or ribbon 501 may include a glass-based material and / or a ceramic-based material and a pencil hardness greater than or equal to 8H, such as greater than or equal to 9H.

[0108] As used herein, "glass-based" includes both glass and glass-ceramics, wherein the glass-ceramics have one or more crystalline phases and an amorphous residual glass phase. Glass-based materials (e.g., glass-based foldable substrates) may include amorphous materials (e.g., glass) and optionally one or more crystalline materials (e.g., ceramics). Amorphous materials and glass-based materials may be strengthened. As used herein, the term "strengthened" may refer to materials that have been chemically strengthened, for example, by exchanging smaller ions in the substrate surface with larger ions, as described below. However, other strengthening methods known in the art may also be used to form a strengthened substrate, such as thermal tempering, or to generate a compressive stress zone and a central tension zone using a mismatch in the thermal expansion coefficient between the various parts of the substrate. Exemplary glass substrates that do not contain or contain lithium oxide include soda-lime glass, alkali aluminosilicate glass, alkali-containing borosilicate glass, alkali-containing aluminoborosilicate glass, alkali-containing phosphosilicate glass, and alkali-containing aluminophosphosilicate glass. In one or more embodiments, the glass-based material may include, by mole percentage (mol%), about 40 mol% to about 80 mol% SiO2, about 10 mol% to about 30 mol% Al2O3, 0 mol% to about 10 mol% B2O3, 0 mol% to about 5 mol% ZrO2, 0 mol% to about 15 mol% P2O5, 0 mol% to about 2 mol% TiO2, 0 mol% to about 20 mol% R2O, and 0 mol% to about 15 mol% RO. As used herein, R2O may refer to alkali metal oxides, for example, Li2O, Na2O, K2O, Rb2O, and Cs2O. As used herein, RO may refer to MgO, CaO, SrO, BaO, and ZnO. In some embodiments, the glass-based substrate may optionally further include 0 mol % to about 2 mol % of each of the following: Na2SO4, NaCl, NaF, NaBr, K2SO4, KCl, KF, KBr, As2O3, Sb2O3, SnO2, Fe2O3, MnO, MnO2, MnO3, Mn2O3, Mn3O4, Mn2O7. "Glass-ceramics" include materials produced by controlled crystallization of glass. In some embodiments, the glass-ceramics have a crystallinity of about 1% to about 99%. Examples of suitable glass ceramics may include Li2O-Al2O3-SiO2 system (ie, LAS system) glass ceramics, MgO-Al2O3-SiO2 system (ie, MAS system) glass ceramics, ZnO×Al2O3×nSiO2 (ie, ZAS system) and / or glass ceramics containing a main crystalline phase, wherein the main crystalline phase includes β-quartz solid solution, β-spodumene, cordierite, petalite and / or lithium disilicate. The glass ceramic substrate can be strengthened using a chemical strengthening process. In one or more embodiments, the glass ceramic substrate of the MAS system can be strengthened in a Li2SO4 molten salt, thereby generating 2Li+ Mg 2+ exchange.

[0109] Throughout this disclosure, "ceramic-based" materials (e.g., ceramic-based foldable substrates) include both ceramics and glass-ceramics, wherein the glass-ceramics have one or more crystalline phases and an amorphous residual glass phase. The ceramic-based materials can be reinforced as described herein. In some embodiments, the ceramic-based materials can be formed by heating the glass-based materials to form a ceramic (e.g., crystalline) portion. In other embodiments, the ceramic-based materials may include one or more nucleating agents that may promote the formation of a crystalline phase. In some embodiments, the ceramic-based materials may include one or more oxides, nitrides, oxynitrides, carbides, borides, and / or silicides. Exemplary embodiments of ceramic oxides include zirconium oxide (ZrO2), zircon zirconium oxide (ZrSiO4), alkali metal oxides (e.g., sodium oxide (Na2O)), alkaline earth metal oxides (e.g., magnesium oxide (MgO)), titanium dioxide (TiO2), hafnium oxide (Hf2O), yttrium oxide (Y2O3), iron oxide, beryllium oxide, vanadium oxide (VO2), fused quartz, mullite (a mineral containing a combination of aluminum oxide and silicon dioxide), and spinel (MgAl2O4). Exemplary embodiments of ceramic nitrides include silicon nitride (Si3N4), aluminum nitride (AlN), gallium nitride (GaN), beryllium nitride (Be3N2), boron nitride (BN), tungsten nitride (WN), vanadium nitride, alkaline earth metal nitrides (e.g., magnesium nitride (Mg3N2)), nickel nitride, and tantalum nitride. Exemplary embodiments of oxynitride ceramics include silicon oxynitride, aluminum oxynitride, and SiAlON (eg, a combination of aluminum oxide and silicon nitride, and which may have the following chemical formula, for example, Si 12-m-n Al m+n O n N 16-n 、Si 6-n Al n O n N 8-n or Si 2-n Al n O 1+n N 2-n, wherein m, n and resulting subscripts are all non-negative integers). Exemplary embodiments of carbides and carbon-containing ceramics include silicon carbide (SiC), tungsten carbide (WC), iron carbide, boron carbide (B4C), alkali metal carbides (e.g., lithium carbide (Li4C3)), alkaline earth metal carbides (e.g., magnesium carbide (Mg2C3)), and graphite. Exemplary embodiments of borides include chromium boride (CrB2), molybdenum boride (Mo2B5), tungsten boride (W2B5), iron boride, titanium boride, zirconium boride (ZrB2), hafnium boride (HfB2), vanadium boride (VB2), niobium boride (NbB2), and lanthanum boride (LaB6). Exemplary embodiments of silicides include molybdenum disilicide (MoSi2), tungsten disilicide (WSi2), titanium disilicide (TiSi2), nickel silicide (NiSi), alkaline earth metal silicides (e.g., sodium silicide (NaSi)), alkali metal silicides (e.g., magnesium silicide (Mg2Si), hafnium disilicide (HfSi2), and platinum silicide (PtSi).

[0110] like Figure 2-3 As shown, the foldable substrate 201 may include a first major surface 203 and a second major surface 205 opposite to the first major surface 203. As shown, the first major surface 203 may extend along a first plane 204a. The second major surface 205 may extend along a second plane 204b. In some embodiments, as shown, the second plane 204b may be parallel to the first plane 204a. A substrate thickness 222 may be defined between the first plane 204a and the second plane 204b. Based on the pen drop test (hereinafter referred to as Fig.14 As a result of the above (discussed above), increased puncture resistance can be achieved by selecting a glass-based substrate thickness greater than about 80 micrometers (μm). In some embodiments, the puncture resistance of the foldable substrate can be increased when the substrate thickness 222 is greater than or equal to about 100 μm, greater than or equal to about 125 μm, greater than or equal to about 150 μm, greater than or equal to about 200 μm, greater than or equal to about 500 μm, less than or equal to about 2 millimeters (mm), less than or equal to about 1 mm, less than or equal to about 500 μm, or less than or equal to about 200 μm. In some embodiments, the substrate thickness 222 can be in the range of about 100 μm to about 2 mm, about 100 μm to about 1 mm, about 100 μm to about 500 μm, about 125 μm to about 500 μm, about 125 μm to about 200 μm, or any range or sub-range therebetween.

[0111] The foldable substrate 201 may include a first portion 221 that includes a first surface area 237 of the first major surface 203 of the foldable substrate 201. As shown, the first portion 221 of the foldable substrate 201 may also include a second surface area 247 of the second major surface 205 of the foldable substrate 201. In some embodiments, the first portion 221 may include a thickness substantially equal to the substrate thickness 222. In some embodiments, the thickness of the first portion 221 is greater than or equal to the thickness of the substrate 222 over the corresponding length 105 of the foldable substrate 201 (see Figure 1 ) and / or the corresponding width 103 of the foldable substrate 201 (see Figure 1 ) can be substantially uniform. Throughout this disclosure, the width 103 of the foldable substrate 201 is considered to be the dimension of the foldable substrate 201 obtained between opposite edges of the foldable substrate in the direction 104 of the folding axis 102 of the foldable device. Additionally, throughout this disclosure, the length 105 of the foldable substrate 201 is considered to be the dimension of the foldable substrate 201 obtained between opposite edges of the foldable substrate in the direction 106 perpendicular to the folding axis 102 of the foldable device.

[0112] like Figure 2-3 As further shown, the foldable substrate 201 may also include a second portion 223 that includes a third surface area 239 of the first major surface 203 of the foldable substrate 201. As shown, the second portion 223 of the foldable substrate 201 may also include a fourth surface area 249 of the second major surface 205 of the foldable substrate 201. The second portion 223 may include a thickness substantially equal to the substrate thickness 222. In some embodiments, the thickness of the first portion 221 may be substantially equal to the thickness of the second portion 223. For example, the thickness of the first portion 221 and the thickness of the second portion 223 may be substantially equal to the substrate thickness 222. In some embodiments, the thickness of the second portion 223 may be substantially uniform over the corresponding length 105 of the foldable substrate 201 and / or the corresponding width 103 of the foldable substrate 201.

[0113] Likewise Figure 2-3As shown, the foldable substrate may include a central portion 225. As shown, the central portion 225 may be located between the first portion 221 of the foldable substrate 201 and the second portion 223 of the foldable substrate 201. In some embodiments, the central portion 225 may be located between the first portion 221 and the second portion 223 in the direction 106 of the length 105 of the foldable substrate 201, wherein the direction 106 of the length 105 is perpendicular to the direction 104 of the folding axis 102 of the foldable substrate 201. The central portion 225 may include a first central surface area 233 located between the first surface area 237 of the first major surface 203 and the third surface area 239 of the first major surface 203. Figure 2-3 As shown, a recess 234 may be defined between the first central surface area 233 and the first plane 204a. The central portion 225 may include a second central surface area 245 of the second major surface 205, the second central surface area 245 being located between a second surface area 247 of the second major surface 205 in the first portion 221 and a fourth surface area 249 of the second major surface 205 in the second portion 223. Although not shown, in some embodiments, the recess may not be completely filled, for example, leaving space for electronic devices and / or mechanical devices.

[0114] like Figure 2-3 As shown, the central portion 225 may include a central major surface 235 of the first central surface area 233. In other embodiments, the central major surface 235 may extend along the third plane 204c. In other embodiments, the third plane 204c may be parallel to the first plane 204a. In other embodiments, the third plane 204c may be parallel to the second plane 204b.

[0115] The central portion 225 may include a central thickness 226 of the foldable substrate 201 defined between the second plane 204b and the first central surface area 233. By providing a central major surface 235 of the central portion 225 extending along a third plane 204c parallel to the second plane 204b, a uniform central thickness 226 may be provided over a portion of the central portion 225 to provide enhanced folding performance at a predetermined thickness of the central thickness 226. The uniform central thickness 226 over the central portion 225 may improve folding performance by preventing stress concentration, which would occur if a portion of the central portion 225 was thinner than the remaining central portion 231. Furthermore, based on the following reference to Fig.14The results of the pen drop test described above indicate that increased puncture resistance can be achieved by selecting a glass-based substrate thickness of less than about 50 micrometers (μm) or greater than about 80 μm. In some embodiments, the center thickness 226 can be greater than or equal to about 10 μm, greater than or equal to about 25 μm, greater than or equal to about 40 μm, greater than or equal to about 80 μm, less than or equal to about 220 μm, less than or equal to about 125 μm, less than or equal to about 80 μm, less than or equal to about 60 μm, or less than or equal to about 50 μm. In some embodiments, the center thickness 226 can be in the range of about 10 μm to about 220 μm, 25 μm to about 220 μm, about 50 μm to about 220 μm, about 80 μm to about 220 μm, about 100 μm to about 220 μm, about 125 μm to about 220 μm, about 150 μm to about 220 μm, or any range or sub-range therebetween. In other embodiments, the center thickness 226 can be greater than about 80 μm, for example, greater than or equal to about 80 μm, greater than or equal to about 100 μm, greater than or equal to about 125 μm, less than or equal to about 220 μm, less than or equal to about 175 μm, or less than or equal to about 150 μm. In other embodiments, the center thickness 226 can be in the range of about 80 μm to about 220 μm, about 80 μm to about 175 μm, about 100 μm to about 175 μm, about 100 μm to about 150 μm, about 125 μm to about 150 μm, or any range or sub-range therebetween. In some embodiments, the center thickness 226 may be less than about 80 μm, for example, in the range of about 10 μm to about 80 μm, about 25 μm to about 80 μm, about 25 μm to about 60 μm, about 25 μm to about 50 μm, about 40 μm to about 50 μm, or any range or sub-range therebetween. In other embodiments, the center thickness 226 may be less than about 50 μm, for example, greater than or equal to about 10 μm, greater than or equal to about 25 μm, greater than or equal to about 30 μm, less than or equal to about 50 μm, less than or equal to about 45 μm, or about 40 μm. In other embodiments, the center thickness 226 may be in the range of about 10 μm to about 50 μm, about 10 μm to about 45 μm, about 25 μm to about 45 μm, about 30 μm to about 45 μm, about 30 μm to about 40 μm, or any range or sub-range therebetween. It should be understood that in some embodiments, the central major surface 235 extending along a third plane 204c parallel to the second plane 204b can include a width of approximately 2.8 times or greater (e.g., approximately 3.2 times or greater, approximately 4.4 times or greater, approximately 6 times) the effective minimum bending radius (e.g., bending length) to provide reduced stress concentration and damage in the folding region of the foldable device.

[0116] In some embodiments, Figure 2-3As shown, the center thickness 226 can be less than the substrate thickness 222. In some embodiments, the center thickness 226 can be about 0.5% or more, about 1% or more, about 2% or more, about 5% or more, about 13% or less, about 10% or less, or about 5% or less of the substrate thickness 222. In some embodiments, as a percentage of the substrate thickness 222, the center thickness 226 can be in the following ranges: about 0.5% to about 13%, about 0.5% to about 10%, about 1% to about 10%, about 1% to about 5%, about 2% to about 5%, about 5% to about 13%, about 5% to about 10%, or any range or sub-range therebetween.

[0117] In some embodiments, the central portion 225 may include a first transition portion 227. Figure 2-3 As shown, the first transition portion 227 can attach the first portion 221 to the central major surface 235. The thickness of the first transition portion 227 can be defined between the second plane 204b and the first central surface area 233. Figure 2-3 As shown, the thickness of the first transition portion 227 can increase continuously from the central major surface 235 (e.g., from the central thickness 226) to the first portion 221 (e.g., to the substrate thickness 222). In some embodiments, as shown, the thickness of the first transition portion 227 can increase at a constant rate from the central major surface 235 to the first portion 221. Although not shown, in some embodiments, the thickness of the first transition portion 227 can increase more slowly at the location where the central major surface 235 meets the first transition portion 227 than at the middle of the first transition portion 227. Although not shown, in some embodiments, the thickness of the first transition portion 227 can increase more slowly at the location where the first portion 221 meets the first transition portion 227 than at the middle of the first transition portion 227.

[0118] In some embodiments, the central portion 225 may include a second transition portion 229. Figure 2-3 As shown, the second transition portion 229 can attach the second portion 223 to the central major surface 235. The thickness of the second transition portion 229 can be defined between the second plane 204b and the first central surface area 233. Figure 2-3As shown, the thickness of the second transition portion 229 can increase continuously from the central major surface 235 (e.g., from the central thickness 226) to the second portion 223 (e.g., to the substrate thickness 222). In some embodiments, as shown, the thickness of the second transition portion 229 can increase at a constant rate from the central major surface 235 to the second portion 223. Although not shown, in some embodiments, the thickness of the second transition portion 229 can increase more slowly at the location where the central major surface 235 meets the second transition portion 229 than at the middle of the second transition portion 229. Although not shown, in some embodiments, the thickness of the second transition portion 229 can increase more slowly at the location where the second portion 223 meets the second transition portion 229 than at the middle of the second transition portion 229.

[0119] In the direction 106 of the length 105 of the foldable substrate 201, a width 230a of the first transition portion 227 may be defined between the central major surface 235 and the first portion 221. In the direction 106 of the length 105 of the foldable substrate 201, a width 230b of the second transition portion 229 may be defined between the central major surface 235 and the second portion 223. Fig.14 According to the results of the following pen drop test, by selecting a glass-based substrate thickness greater than about 80 μm or less than 50 microns (μm), increased puncture resistance can be achieved. In other embodiments, the center thickness 226 can be greater than about 80 microns (μm) to achieve increased puncture resistance. The combination of a center thickness less than about 50 μm and a substrate thickness greater than about 80 μm can provide a low effective minimum bending radius while providing excellent impact resistance and / or puncture resistance. In other embodiments, the substrate thickness 222 can be in a range of greater than 80 μm, while the center thickness 226 can be greater than about 80 μm. In other embodiments, the center thickness 226 can be less than about 50 μm to achieve increased puncture resistance. In other embodiments, the substrate thickness 222 can be in a range of greater than 80 μm, while the center thickness 226 can be less than about 50 μm. The combination of a center thickness greater than about 80 μm and a substrate thickness greater than about 80 μm can provide a low effective minimum bending radius while providing excellent impact resistance and / or puncture resistance.

[0120] In some embodiments, the width 230a of the first transition portion 227 and / or the width 230b of the second transition portion 229 can be reduced (e.g., 5 mm or less) to minimize the extent of the transition portion having a thickness close to 65 μm (e.g., in the range of about 50 μm to about 80 μm), thereby enhancing the puncture resistance of a larger area of ​​the foldable substrate. In addition, at the same time, the width 230a of the first transition portion 227 and / or the width 230b of the second transition portion 229 can be sufficiently large (e.g., greater than or equal to 1 mm) to avoid optical distortion that may otherwise occur with a stepped transition width or a small transition width (e.g., less than 1 mm) between the first thickness and the center thickness. In some embodiments, to enhance the puncture resistance of the foldable substrate while avoiding optical distortion, the width 230a of the first transition portion 227 and / or the width 230b of the second transition portion 229 may be greater than or equal to about 1 mm, greater than or equal to about 2 mm, greater than or equal to about 3 mm, less than or equal to about 5 mm, less than or equal to about 4 mm, or less than or equal to about 3 mm. In some embodiments, the width 230a of the first transition portion 227 and / or the width 230b of the second transition portion 229 may be in the range of about 1 mm to about 5 mm, about 1 mm to about 4 mm, about 1 mm to about 3 mm, about 2 mm to about 5 mm, about 2 mm to about 4 mm, about 2 mm to about 3 mm, about 3 mm to about 5 mm, about 3 mm to about 4 mm, or any range or sub-range therebetween.

[0121] The second major surface 205 of the foldable substrate 201, the first major surface 403 of the strip 501, and / or the second major surface 405 of the strip 501 may include an optional coating. In some embodiments, if provided, the coating may include one or more of an easy-to-clean coating, a low-friction coating, an oleophobic coating, a diamond-like coating, a scratch-resistant coating, or a wear-resistant coating. The scratch-resistant coating may include a nitride oxide, such as aluminum oxynitride or silicon oxynitride, and have a thickness of about 500 microns or more. In such an embodiment, the wear-resistant layer may include the same material as the scratch-resistant layer. In some embodiments, the low-friction coating may include a highly fluorinated silane coupling agent, such as an alkylfluorosilane, in which an oxymethyl group is attached to the silicon atom. In such an embodiment, the easy-to-clean coating may include the same material as the low-friction coating. In other embodiments, the easy-to-clean coating may include a protonatable group, such as an amine, such as an alkylaminosilane, in which an oxymethyl group is attached to the silicon atom. In such an embodiment, the oleophobic coating may include the same material as the easy-to-clean coating. In some embodiments, the diamond-like coating comprises carbon and may be produced by applying a high voltage potential in the presence of a hydrocarbon plasma.

[0122] In some embodiments, an optically transparent polymer hard coating may be provided above the second major surface 205 of the foldable substrate 201 and / or the coating may be bonded to the second major surface 205. Materials suitable for optically transparent polymer hard coatings include, but are not limited to, cured acrylate resin materials, inorganic-organic hybrid polymer materials, aliphatic or aromatic hexafunctional urethane acrylates, siloxane-based hybrid materials, and nanocomposites, such as epoxy materials and urethane materials with nanosilicates. In some embodiments, the optically transparent polymer hard coating may be mainly composed of one or more of these materials. In some embodiments, the optically transparent polymer hard coating may be composed of one or more of these materials. As used herein, "inorganic-organic hybrid polymer material" means a polymer material comprising a monomer and the monomer having an inorganic and organic component. Inorganic-organic hybrid polymers are obtained by polymerization reactions between monomers having an inorganic group and an organic group. Inorganic-organic hybrid polymers are not nanocomposites (e.g., inorganic particles are dispersed in an organic matrix) comprising separated inorganic and organic components or phases. More specifically, materials suitable for optically transparent polymer (OTP) hard coatings include, but are not limited to, polyimide, polyethylene terephthalate (PET), polycarbonate (PC), polymethyl methacrylate (PMMA), organic polymer materials, inorganic-organic hybrid polymer materials, and aliphatic or aromatic hexafunctional urethane acrylates. In some embodiments, the OTP hard coating may be substantially composed of organic polymer materials, inorganic-organic hybrid polymer materials, or aliphatic or aromatic hexafunctional urethane acrylates. In some embodiments, the OTP hard coating may be composed of polyimide, organic polymer materials, inorganic-organic hybrid polymer materials, or aliphatic or aromatic hexafunctional urethane acrylates. In some embodiments, the OTP hard coating may include a nanocomposite material. In some embodiments, the OTP hard coating may include at least one of nano-silicates, epoxy materials, and urethane materials. Suitable compositions for such OTP hard coatings are described in U.S. Patent Publication No. 2015 / 0110990, which is incorporated herein by reference in its entirety. As used herein, "organic polymer material" means a polymer material comprising monomers and the monomers have only organic components. In some embodiments, the OTP hard coating may include an organic polymer material manufactured by Gunze Co., Ltd. and having a hardness of 9H, for example, Gunze's "High Durability Transparent Film". As used herein, "inorganic-organic hybrid polymer material" means a polymer material comprising monomers and the monomers have inorganic and organic components. Inorganic-organic hybrid polymers are obtained by polymerization reactions between monomers having inorganic groups and organic groups. Inorganic-organic hybrid polymers are not nanocomposites comprising separated inorganic and organic components or phases (e.g., inorganic particles are dispersed in an organic matrix).In some embodiments, the inorganic-organic hybrid polymer material may include a polymerized monomer containing a silicon-based inorganic group, for example, a silsesquioxane polymer. The silsesquioxane polymer may be, for example, an alkyl-silsesquioxane, an aryl-silsesquioxane, or an arylalkyl-silsesquioxane having the following chemical structure: (RSiO. 1.5)n, wherein R is an organic group, such as but not limited to methyl or phenyl. In some embodiments, the OTP hard coating may include a silsesquioxane polymer combined with an organic matrix, such as SILPLUS manufactured by Nippon Steel Chemical Co., Ltd. In some embodiments, the OTP hard coating may include 90 wt % to 95 wt % of an aromatic hexafunctional urethane acrylate [e.g., PU662NT (aromatic hexafunctional urethane acrylate) manufactured by Miwon Specialty Chemical Co.] and 10 wt % to 5 wt % of a photoinitiator [e.g., Darocur 1173 manufactured by Ciba Specialty Chemicals Corporation], and a hardness of 8H or greater. In some embodiments, an OTP hard coating layer composed of an aliphatic or aromatic hexafunctional urethane acrylate can be formed as a separate layer by spin coating the layer on a polyethylene terephthalate (PET) substrate, curing the urethane acrylate, and removing the urethane acrylate layer from the PET substrate. The thickness of the OTP hard coating layer can be in the range of 1 μm to 150 μm, including sub-ranges. For example, the OTP hard coating thickness can be in the following range: 10 μm to 140 μm, 20 μm to 130 μm, 30 μm to 120 μm, 40 μm to 110 μm, 50 μm to 100 μm, 60 μm to 90 μm, 70 μm, 80 μm, 2 μm to 140 μm, 4 μm to 130 μm, 6 μm to 120 μm, 8 μm to 110 μm, 10 μm to 100 μm, 10 μm to 90 μm, 10 μm, 80 μm, 10 μm, 70 μm, 10 μm, 60 μm, 10 μm, 50 μm, or in the range of any two of these values ​​as endpoints. In some embodiments, the OTP hard coating can be a single integral layer. In some embodiments, the OTP hard coating layer may be an inorganic-organic hybrid polymer material layer or an organic polymer material layer having a thickness in the range of 80 μm to 120 μm (including sub-ranges). For example, the thickness of the OTP hard coating layer comprising an inorganic-organic hybrid polymer material or an organic polymer material may be 80 μm to 110 μm, 90 μm to 100 μm, or in a range with any two of these values ​​as endpoints. In some embodiments, the OTP hard coating layer may be an aliphatic or aromatic hexafunctional urethane acrylate material layer having a thickness in the range of 10 μm to 60 μm (including sub-ranges).For example, the thickness of the OTP hard coating layer comprising an aliphatic or aromatic hexafunctional urethane acrylate material can be 10 μm to 55 μm, 10 μm to 50 μm, 10 μm to 45 μm, 10 μm to 40 μm, 10 μm to 35 μm, 10 μm to 30 μm, 10 μm to 25 μm, 10 μm to 20 μm, or in any range with any two of these values ​​as endpoints.

[0123] Foldable devices may have failure modes that can be described as low energy failure or high energy failure. Fig.12 The impact device 1201 shown is used to measure the failure mode of the foldable device. The impact device 1201 is similar to Fig. 9 and 11 However, the foldable substrate 201 or strip 501 is tested in the impact device 1201 without the adhesive 207 (e.g., optically clear adhesive), release liner 213, and / or display device 303 disposed on the foldable substrate 201 or strip 501. For example, Fig.12 As shown, the foldable substrate 201 is tested without an adhesive, a release liner, and / or a display device disposed above the foldable substrate 201. Fig.12 As shown, the first major surface 203 of the foldable substrate 201 is attached to the parallel plates 903, 905. The parallel plates 903, 905 are moved together at a rate of 5 mm / second until a target parallel plate distance 1211 is achieved. The target parallel plate distance 1211 is the greater of two times the effective minimum bending radius of the foldable substrate 201 or 4 mm. Next, a tungsten carbide sharp contact probe impacts the foldable substrate 201 at an impact location 1215 of the second major surface 205, the impact location 1215 being a predetermined distance 1213 from the outermost periphery of the first major surface 203 of the central portion 225 of the foldable substrate 201. The predetermined distance 1213 is 30 mm. As used herein, a fracture is high energy if during fracture, particles are ejected from the foldable substrate at an average velocity greater than or equal to 1 meter / second (m / s), and the fracture results in more than 2 crack branches. As used herein, a fracture is low energy if the fracture results in less than or equal to 2 crack branches and / or does not cause particles to be ejected from the foldable substrate at an average velocity greater than or equal to 1 m / s during the fracture. The average velocity of the ejected particles can be measured by capturing a high-speed video of the foldable substrate 201 from the time the sharp contact probe contacts the impact location 1215 to 5,000 microseconds thereafter.

[0124] Providing a foldable substrate with low energy failure (e.g., low fracture energy, low energy fracture) can avoid average particle velocities exceeding 1 m / s at failure. In some embodiments, the low energy fracture can be the result of a reduced thickness of the central portion, where the reduced thickness central portion stores less energy for a given maximum tensile stress than a thicker glass portion (e.g., glass-based portion). In some embodiments, the low energy fracture can be the result of a fracture of a first portion and / or a second portion away from the central portion that undergoes bending, wherein the first portion and / or the second portion comprises a lower maximum tensile stress than the central portion.

[0125] In some embodiments, one or more portions of the foldable substrate 201 and / or the strip 501 can include a compressive stress region. In some embodiments, the compressive stress region can be established by chemical strengthening. Chemical strengthening can include an ion exchange process in which ions in the surface layer are replaced with (or exchanged with) larger ions having the same valence or oxidation state. Methods of chemical strengthening are discussed below. Without wishing to be bound by theory, chemical strengthening of the foldable substrate 201 can achieve a small (e.g., less than about 10 mm or less) bending radius because the compressive stress from chemical strengthening can offset the compressive stress on the outermost surface of the foldable substrate (e.g., Figure 2 The first main surface 203, Figure 2 The second major surface 205 in the strip) and / or the outermost surface of the strip (e.g. Figure 5 The first main surface 403, Figure 5The bending-induced tensile stress on the second main surface 405 in the foldable substrate 201. The compressive stress zone can extend into a portion of the foldable substrate 201, extending to a certain depth, which is called the compression depth. As used herein, the compression depth means the depth at which the stress in the chemically strengthened substrate described herein changes from compressive stress to tensile stress. Depending on the ion exchange treatment and the thickness of the product being measured, the compression depth can be measured by a surface stress meter or a scattered light polarizer (SCALP, wherein the values ​​reported herein are carried out using SCALP-5 manufactured by Glasstress, Estonia). If the stress in the substrate is generated by exchanging potassium ions into the substrate, the compression depth is measured using, for example, FSM-6000 [Orihara Industrial Co., Ltd., Japan (Orihara Industrial Co., Ltd.)]. Unless otherwise specified, the compressive stress (including surface CS) is measured by a surface stress meter (FSM) using a commercially available instrument, such as FSM-6000 manufactured by Orihara. Surface stress measurement relies on the accurate measurement of the stress optical coefficient (SOC), which is related to the birefringence of the glass. Unless otherwise specified, SOC is measured according to Protocol C (Glass Disk Method) described in ASTM Standard C770-16, entitled "Standard Test Method for Measurement of Glass Stress-Optical Coefficient", which is incorporated herein by reference in its entirety. If the stress is generated by exchanging sodium ions into the substrate or strip, and the thickness of the article being measured exceeds about 75 μm, the depth of compression and central tension (CT) are measured using SCALP. If the stress in the substrate is generated by exchanging both potassium and sodium ions into the substrate or strip, and the thickness of the article being measured exceeds about 75 μm, the depth of compression and CT are measured by SCALP. Without wishing to be bound by theory, the depth of exchange of sodium can indicate the depth of compression, while the depth of exchange of potassium ions can indicate a change in the magnitude of the compressive stress (but not a change in stress from compressive stress to tensile stress). A refracted near field (RNF; the RNF method is described in U.S. Pat. No. 8,854,623, entitled “Systems and methods for measuring a profile characteristic of a glass sample,” which is incorporated herein by reference in its entirety) method can also be used to obtain a graphical representation of the stress distribution. When the RNF method is used to obtain a graphical representation of the stress distribution, the maximum central tension value provided by the SCALP is used in the RNF method.The graphical representation of the stress distribution obtained by RNF is force balanced and calibrated to the maximum central tension value provided by the SCALP measurement. As used herein, "depth of layer" (DOL) means the depth of ions (e.g., sodium, potassium) exchanged into the substrate or strip. In the present disclosure, when the central tension cannot be measured directly by SCALP (such as when the measured article is thinner than about 75 μm), the maximum central tension can be approximated by the product of the maximum compressive stress and the compression depth divided by the difference between the substrate thickness and twice the compression depth, where the compressive stress and the compression depth are measured by FSM.

[0126] In some embodiments, the first portion 221 may include a first compressive stress zone at the first surface region 203, which may extend from the first major surface 203 to a first compression depth. In other embodiments, the first compressive stress zone may include a first surface region 237, and the first compressive stress zone extends from the first surface region 237 to a first compression depth. In some embodiments, the first portion 221 may include a second compressive stress zone at the second major surface 205, which may extend from the second major surface 205 to a second compression depth. In other embodiments, the second compressive stress zone may include a second surface region 247, and the second compressive stress zone extends from the second surface region 247 to a second compression depth. In some embodiments, as a percentage of the substrate thickness 222, the first compression depth and / or the second compression depth may be greater than or equal to about 1%, greater than or equal to about 2%, greater than or equal to about 5%, less than or equal to about 10%, less than or equal to about 8%, or less than or equal to about 5%. In some embodiments, as a percentage of the substrate thickness 222, the first compression depth and / or the second compression depth may be in the range of about 1% to about 10%, about 1% to about 8%, about 1% to about 5%, about 2% to about 10%, about 2% to about 8%, about 2% to about 5%, about 5% to about 10%, about 5% to about 8%, or any range or sub-range therebetween. In other embodiments, the first compression depth may be substantially equal to the second compression depth. In some embodiments, the first compression depth and / or the second compression depth may be greater than or equal to about 1 μm, greater than or equal to about 5 μm, greater than or equal to about 10 μm, less than or equal to about 20 μm, less than or equal to about 15 μm, or less than or equal to about 10 μm. In some embodiments, the first compression depth and / or the second compression depth can be in the range of about 1 μm to about 20 μm, about 1 μm to about 15 μm, about 1 μm to about 10 μm, about 5 μm to about 10 μm, about 5 μm to about 20 μm, about 10 μm to about 20 μm, about 10 μm to about 15 μm, about 15 μm to about 20 μm, or any range or sub-range therebetween. Providing a first portion comprising a first compression depth and / or a second compression depth, and the first compression depth and / or the second compression depth being in the range of about 1% to about 10% of the thickness of the substrate, can achieve excellent impact resistance and / or puncture resistance while providing low energy fracture, as described below.

[0127] In some embodiments, the first compressive stress region may include a first maximum compressive stress. In some embodiments, the second compressive stress region may include a second maximum compressive stress. In other embodiments, the first maximum compressive stress and / or the second maximum compressive stress may be greater than or equal to about 100 megapascals (MPa), greater than or equal to about 200 MPa, greater than or equal to about 300 MPa, greater than or equal to about 400 MPa, greater than or equal to about 500 MPa, greater than or equal to about 600 MPa, greater than or equal to about 700 MPa, less than or equal to about 1,500 MPa, less than or equal to about 1,200 MPa, less than or equal to about 1,000 MPa, less than or equal to about 600 MPa, or less than or equal to about 400 MPa. In other embodiments, the first maximum compressive stress and / or the second maximum compressive stress may be in the range of about 100 MPa to about 1,500 MPa, about 200 MPa to about 1,500 MPa, about 200 MPa to about 1,200 MPa, about 300 MPa to about 1,200 MPa, about 300 MPa to about 1,000 MPa, about 300 MPa to about 600 MPa, about 300 MPa to about 400 MPa, 700 MPa to about 1,500 MPa, about 700 MPa to about 1,200 MPa, about 700 MPa to about 1,000 MPa, about 700 MPa to about 900 MPa, or any range or sub-range therebetween. By providing a first maximum compressive stress and / or a second maximum compressive stress of about 100 MPa to about 1,500 MPa, excellent impact resistance and / or puncture resistance may be achieved.

[0128] In some embodiments, the first portion 221 may include a first tensile stress region. In some embodiments, the first tensile stress region may be located between the first compressive stress region and the second compressive stress region. In some embodiments, the first tensile stress region may include a first maximum tensile stress. In other embodiments, the first maximum tensile stress may be greater than or equal to about 10 MPa, greater than or equal to about 20 MPa, greater than or equal to about 30 MPa, less than or equal to about 100 MPa, less than or equal to about 80 MPa, or less than or equal to about 60 MPa. In other embodiments, the first maximum tensile stress may be in the range of about 10 MPa to about 100 MPa, about 10 MPa to about 80 MPa, about 20 MPa to about 80 MPa, about 20 MPa to about 60 MPa, about 30 MPa to about 60 MPa, or any range or sub-range therebetween. By providing a first maximum tensile stress of about 10 MPa to about 100 MPa, excellent impact resistance and / or puncture resistance can be achieved while providing low energy fracture, as described below.

[0129] In some embodiments, the second portion 223 may include a third compressive stress zone at the first major surface 203, which may extend from the first major surface 203 to a third compression depth. In other embodiments, the third compressive stress zone may include a third surface area 239, and the third compressive stress zone may extend from the third surface area 239 to a third compression depth. In some embodiments, the second portion 223 may include a fourth compressive stress zone at the second major surface 205, which may extend from the second major surface 205 to a fourth compression depth. In other embodiments, the fourth compressive stress zone may include a fourth surface area 249, and the fourth compressive stress zone may extend from the fourth surface area 249 to a fourth compression depth. In some embodiments, as a percentage of the substrate thickness 222, the third compression depth and / or the fourth compression depth may be greater than or equal to about 1%, greater than or equal to about 2%, greater than or equal to about 5%, less than or equal to about 10%, less than or equal to about 8%, or less than or equal to about 5%. In some embodiments, the third compression depth and / or the fourth compression depth may be in the range of about 1% to about 10%, about 1% to about 8%, about 1% to about 5%, about 2% to about 10%, about 2% to about 8%, about 2% to about 5%, about 5% to about 10%, about 5% to about 8%, or any range or sub-range therebetween as a percentage of the substrate thickness 222. In other embodiments, the third compression depth may be substantially equal to the fourth compression depth. In some embodiments, the third compression depth and / or the fourth compression depth may be greater than or equal to about 1 μm, greater than or equal to about 5 μm, greater than or equal to about 10 μm, less than or equal to about 20 μm, less than or equal to about 15 μm, or less than or equal to about 10 μm. In some embodiments, the third compression depth and / or the fourth compression depth can be in the range of about 1 μm to about 20 μm, about 1 μm to about 15 μm, about 1 μm to about 10 μm, about 5 μm to about 10 μm, about 5 μm to about 20 μm, about 10 μm to about 20 μm, about 10 μm to about 15 μm, about 15 μm to about 20 μm, or any range or sub-range therebetween. Providing a second portion comprising a third compression depth and / or a fourth compression depth, and the third compression depth and / or the fourth compression depth being in the range of about 1% to about 10% of the thickness of the substrate, can achieve excellent impact resistance and / or puncture resistance while providing a small energy to fracture, as described below.

[0130] In some embodiments, the third compressive stress region may include a third maximum compressive stress. In some embodiments, the fourth compressive stress region may include a fourth maximum compressive stress. In other embodiments, the third maximum compressive stress and / or the fourth maximum compressive stress may be greater than or equal to about 100 megapascals (MPa), greater than or equal to about 200 MPa, greater than or equal to about 300 MPa, greater than or equal to about 400 MPa, greater than or equal to about 500 MPa, greater than or equal to about 600 MPa, greater than or equal to about 700 MPa, less than or equal to about 1,500 MPa, less than or equal to about 1,200 MPa, less than or equal to about 1,000 MPa, less than or equal to about 600 MPa, or less than or equal to about 400 MPa. In other embodiments, the third maximum compressive stress and / or the fourth maximum compressive stress may be in the range of about 100 MPa to about 1,500 MPa, about 200 MPa to about 1,500 MPa, about 200 MPa to about 1,200 MPa, about 300 MPa to about 1,200 MPa, about 300 MPa to about 1,000 MPa, about 300 MPa to about 600 MPa, about 300 MPa to about 400 MPa, 700 MPa to about 1,500 MPa, about 700 MPa to about 1,200 MPa, about 700 MPa to about 1,000 MPa, about 700 MPa to about 900 MPa, or any range or sub-range therebetween. By providing a third maximum compressive stress and / or a fourth maximum compressive stress of about 100 MPa to about 1,500 MPa, excellent impact resistance and / or puncture resistance may be achieved.

[0131] In some embodiments, the second portion 223 may include a second tensile stress zone. In some embodiments, the second tensile stress zone may be located between the third compressive stress zone and the fourth compressive stress zone. In some embodiments, the second compressive stress zone may include a second maximum tensile stress. In other embodiments, the second maximum tensile stress may be greater than or equal to about 10 MPa, greater than or equal to about 20 MPa, greater than or equal to about 30 MPa, less than or equal to about 100 MPa, less than or equal to about 80 MPa, or less than or equal to about 60 MPa. In other embodiments, the second maximum tensile stress may be in the range of about 10 MPa to about 100 MPa, about 10 MPa to about 80 MPa, about 20 MPa to about 80 MPa, about 20 MPa to about 60 MPa, about 30 MPa to about 60 MPa, or any range or sub-range therebetween. By providing a second maximum tensile stress of about 10 MPa to about 100 MPa, excellent impact resistance and / or puncture resistance can be achieved while providing low energy fracture, as described below.

[0132] In some embodiments, the central portion 225 may include a first central compressive stress zone from the first central surface region 233. In other embodiments, the first central compressive stress zone may include the first central surface region 233, and the first central compressive stress zone extends from the first central surface region 233 to the first central compression depth. In some embodiments, the central portion 225 may include a second central compressive stress zone at the second major surface 205, and the second central compressive stress zone may extend from the second major surface 205 to the second central compression depth. In other embodiments, the second central compressive stress zone may include the second central surface region 245, and the second central compressive stress zone extends from the second central surface region 245 to the second central compression depth. In some embodiments, as a percentage of the central thickness 226, the first central compression depth and / or the second central compression depth may be greater than or equal to about 10%, greater than or equal to about 15%, greater than or equal to about 20%, less than or equal to about 30%, less than or equal to about 25%, or less than or equal to about 20%. In some embodiments, as a percentage of the center thickness 226, the first center compression depth and / or the second center compression depth may be in the range of about 10% to about 30%, about 10% to about 25%, about 15% to about 25%, about 15% to about 20%, about 20% to about 25%, or any range or sub-range therebetween. In other embodiments, the first center compression depth may be substantially equal to the second center compression depth. In some embodiments, the first compression depth and / or the second compression depth may be greater than or equal to about 1 μm, greater than or equal to about 5 μm, greater than or equal to about 10 μm, less than or equal to about 20 μm, less than or equal to about 15 μm, or less than or equal to about 10 μm. In some embodiments, the first compression depth and / or the second compression depth may be in the range of about 1 μm to about 20 μm, about 1 μm to about 15 μm, about 5 μm to about 15 μm, about 5 μm to about 10 μm, about 10 μm to about 15 μm, or any range or sub-range therebetween. By providing a center portion including a first center compression depth and / or a second center compression depth in a range of about 10% to about 30% of the center thickness, a low minimum bend radius can be achieved.

[0133] In some embodiments, the first central compressive stress region may include a first central maximum compressive stress. In some embodiments, the second central compressive stress region may include a second central maximum compressive stress. In other embodiments, the first central maximum compressive stress and / or the second central maximum compressive stress may be greater than or equal to about 100 megapascals (MPa), greater than or equal to about 200 MPa, greater than or equal to about 300 MPa, greater than or equal to about 400 MPa, greater than or equal to about 500 MPa, greater than or equal to about 600 MPa, greater than or equal to about 700 MPa, less than or equal to about 1,500 MPa, less than or equal to about 1,200 MPa, less than or equal to about 1,000 MPa, less than or equal to about 600 MPa, or less than or equal to about 400 MPa. In other embodiments, the first center maximum compressive stress and / or the second center maximum compressive stress can be in the range of about 100 MPa to about 1,500 MPa, about 200 MPa to about 1,500 MPa, about 200 MPa to about 1,200 MPa, about 300 MPa to about 1,200 MPa, about 300 MPa to about 1,000 MPa, about 300 MPa to about 600 MPa, about 300 MPa to about 400 MPa, 700 MPa to about 1,500 MPa, about 700 MPa to about 1,200 MPa, about 700 MPa to about 1,000 MPa, about 700 MPa to about 900 MPa, or any range or sub-range therebetween. By providing a first center maximum compressive stress and / or a second center maximum compressive stress of about 100 MPa to about 1,500 MPa, a low minimum bend radius can be achieved.

[0134] In some embodiments, the central portion 225 may include a central tensile stress zone. In some embodiments, the central tensile stress zone may be located between the first central compressive stress zone and the second central compressive stress zone. In some embodiments, the central tensile stress zone may include a central maximum tensile stress. In other embodiments, the central maximum tensile stress may be greater than or equal to about 125 MPa, greater than or equal to about 150 MPa, greater than or equal to about 200 MPa, less than or equal to about 375 MPa, less than or equal to about 300 MPa, or less than or equal to about 250 MPa. In other embodiments, the central maximum tensile stress may be in the range of about 125 MPa to about 375 MPa, about 125 MPa to about 300 MPa, about 150 MPa to about 300 MPa, about 150 MPa to about 250 MPa, about 200 MPa to about 250 MPa, or any range or sub-range therebetween. Providing a central maximum tensile stress of about 125 MPa to about 375 MPa enables a low minimum bending radius.

[0135] In some embodiments, the first compressive stress region, the second compressive stress region, the third compressive stress region, the fourth compressive stress region, the first central compressive stress region, and / or the second central compressive stress region may be produced by chemical strengthening. In some embodiments, the first maximum tensile stress and the second maximum tensile stress may be less than the central maximum tensile stress. Providing a first maximum tensile stress and a second maximum tensile stress that are less than the central maximum tensile stress in the central portion can achieve low energy fracture while achieving a lower minimum bending radius. In other embodiments, the first compression depth may be substantially equal to the first central compression depth. In other embodiments, the third compression depth may be substantially equal to the first central compression depth. Providing substantially equal first compression depth, third compression depth, and first central compression depth can simplify manufacturing because no masking or other processes are required to selectively chemically strengthen the foldable substrate. In other embodiments, the second compression depth may be substantially equal to the second central compression depth. In other embodiments, the fourth compression depth may be substantially equal to the second central compression depth. Providing substantially equal second compression depth, fourth compression depth, and second central compression depth can simplify manufacturing because no masking or other processes are required to selectively chemically strengthen the foldable substrate. As described above, the center thickness can be less than the substrate thickness (e.g., in the range of about 0.5% to about 13%), which can enable the third maximum center tension to be greater than the first maximum center tension and the second maximum center tension, even when the compression depths of the first portion, the second portion, and the second portion are substantially the same.

[0136] like Figure 2-3As shown, adhesive 207 [e.g., an optically clear adhesive (OCA)] may include a first contact surface 209. In some embodiments, as shown, adhesive 207 may be disposed over a first surface region 237 of the first major surface in the first portion of foldable substrate 201. In other embodiments, as shown, first contact surface 209 of adhesive 207 may contact first surface region 237 of first major surface 203 in first portion 221 of foldable substrate 201, and adhesive 207 may be bonded to first surface region 237. In some embodiments, as shown, first contact surface 209 of adhesive 207 may be disposed over a third surface region 239 of first major surface 203 in second portion 223 of foldable substrate 201. In other embodiments, as shown, first contact surface 209 of adhesive 207 may contact third surface region 239 of first major surface 203 in second portion 223 of foldable substrate 201, and adhesive 207 may be bonded to third surface region 239. In some embodiments, a first contact surface 209 of adhesive 207 may be disposed above a first central surface area 233 of foldable substrate 201. In other embodiments, as shown, first contact surface 209 of adhesive 207 may contact first central surface area 233 of foldable substrate 201, and adhesive 207 may be bonded to first central surface area 233. As shown, adhesive 207 may fill a recess 234 defined between first plane 204a and first central surface area 233 of central portion 225. If a first layer and / or component is described as being "disposed above" a second layer and / or component, other layers may or may not exist between the first layer and / or component and the second layer and / or component. As used herein, a first layer and / or component described as being "bonded to" a second layer and / or component means that the layers and / or components are bonded to each other, either by direct contact and / or bonding between the two layers and / or components or by a layer of adhesive.

[0137] The adhesive 207 may include a second contact surface 211, which may be opposite to the first contact surface 209 and spaced apart from the first contact surface 209. In some embodiments, as shown in FIG. Figure 2-3 As shown, the second contact surface 211 of the adhesive 207 may include a planar surface. In other embodiments, as shown, the planar surface of the second contact surface 211 of the adhesive 207 may be parallel to the first plane 204a.

[0138] In some embodiments, the adhesive 207 can be optically transparent and can be referred to as an "optically clear adhesive". As used herein, "optically transparent" means that the average transmittance through a 1.0 mm thick sheet of material is 70% or greater in the wavelength range of 400 nm to 700 nm. In some embodiments, the average transmittance of the optically transparent material through a 1.0 mm thick sheet of material in the wavelength range of 400 nm to 700 nm can be 75% or greater, 80% or greater, 85% or greater, or 90% or greater, 92% or greater, 94% or greater, 96% or greater. The average transmittance in the wavelength range of 400 nm to 700 nm is calculated by measuring the transmittance of all integer wavelengths from about 400 nm to about 700 nm and averaging the measured values. In some embodiments, the foldable substrate 201 and / or the strip 501 can be optically transparent.

[0139] In some embodiments, adhesive 207 may include an optically clear adhesive. The optically clear adhesive may include a first refractive index. The first refractive index may be a function of the wavelength of light passing through the optically clear adhesive. For light of a first wavelength, the refractive index of a material is defined as the ratio between the speed of light in a vacuum and the speed of light in a corresponding material. Without being limited by theory, the refractive index of an optically clear adhesive may be determined using the ratio of the sine of a first angle to the sine of a second angle, wherein light of a first wavelength is incident on the surface of the optically clear adhesive from air at a first angle and is refracted at the surface of the optically clear adhesive, thereby causing the light to propagate within the optically clear adhesive at a second angle. Both the first angle and the second angle are measured relative to the normal to the surface of the optically clear adhesive. As used herein, the refractive index is measured according to ASTM E1967-19, wherein the first wavelength includes 589nm. In some embodiments, the first refractive index of the optically clear adhesive can be greater than or equal to about 1, greater than or equal to about 1.3, greater than or equal to about 1.4, greater than or equal to about 1.45, less than or equal to about 3, less than or equal to about 2, less than or equal to about 1.7, less than or equal to about 1.6, or less than or equal to about 1.55. In some embodiments, the first refractive index of the optically clear adhesive can be in the following ranges: from about 1 to about 3, from about 1 to about 2, from about 1.3 to about 2, from about 1.3 to about 1.7, from about 1.4 to about 1.7, from about 1.4 to about 1.6, from about 1.45 to about 1.6, from about 1.45 to about 1.55, or any range or sub-range therebetween.

[0140] The foldable substrate 201 and / or the tape 501 can be optically transparent and can include a second refractive index. The second refractive index can be within any range of the first refractive index described above. The difference equal to the absolute value of the difference between the second refractive index of the foldable substrate 201 and the first refractive index of the adhesive 207 can be less than or equal to about 0.1, less than or equal to about 0.07, less than or equal to about 0.05, greater than or equal to about 0.001, greater than or equal to about 0.01, or greater than or equal to about 0.02. In some embodiments, the difference is within the following ranges: about 0.001 to about 0.1, about 0.001 to about 0.07, about 0.01 to about 0.07, about 0.01 to about 0.05, about 0.02 to about 0.05, or any range or sub-range therebetween. In some embodiments, the second refractive index of the foldable substrate 201 can be greater than the first refractive index of the adhesive 207. In some embodiments, the second refractive index of the foldable substrate 201 can be less than the first refractive index of the adhesive 207.

[0141] In some embodiments, the adhesive 207 may include one or more of the following: polyolefins, polyamides, halogenide-containing polymers (e.g., polyvinyl chloride or fluoropolymers), elastomers, urethanes, phenolic resins, polyparaxylene, polyethylene terephthalate (PET), and polyetheretherketone (PEEK). Exemplary embodiments of polyolefins include low molecular weight polyethylene (LDPE), high molecular weight polyethylene (HDPE), ultra-high molecular weight polyethylene (UHMWPE), and polypropylene (PP). Exemplary embodiments of fluoropolymers include polytetrafluoroethylene (PTFE), polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), perfluoropolyether (PFPE), perfluorosulfonic acid (PFSA), perfluoroalkoxy polymer (PFA), fluorinated ethylene propylene (FEP) polymer, and ethylene tetrafluoroethylene (ETFE) polymer. Exemplary embodiments of elastomers include rubbers (e.g., polybutadiene, polyisoprene, chloroprene, butyl rubber, nitrile rubber) and block copolymers (e.g., styrene-butadiene, high impact polystyrene, poly(dichlorophosphazene)). In further embodiments, adhesive 207 may include an optically clear adhesive. In further embodiments, the optically clear adhesive may include one or more optically clear polymers: acrylics (e.g., polymethyl methacrylate (PMMA)), epoxies, silicones, and / or polyurethanes. Examples of epoxy materials include: bisphenol-based epoxies, novolac-based epoxies, cycloaliphatic-based epoxies, and glycidylamine-based epoxies. In further embodiments, the optically clear adhesive may include, but is not limited to, acrylic adhesives, e.g., 3M 8212 adhesive, or optically clear liquid adhesives, e.g., LOCTITE optically clear liquid adhesives. Exemplary embodiments of optically clear adhesives include transparent acrylics, epoxies, silicones, and polyurethanes.

[0142] The adhesive thickness 208 of the adhesive 207 measured from the first surface area 237 or 537 and / or the third surface area 239 or 539 of the first major surface 203 or 403 of the foldable substrate 201 or strip 501 and the second contact surface 211 of the adhesive 207 can be about 1 μm or more, about 5 μm or more, about 10 μm or more, about 20 μm or more, about 100 μm or less, about 50 μm or less, or about 30 μm or less. In some embodiments, the adhesive thickness 208 of the adhesive 207 can be in the range of about 1 μm to about 100 μm, about 5 μm to about 100 μm, about 5 μm to about 50 μm, about 10 μm to about 50 μm, about 10 μm to about 30 μm, about 20 μm to about 30 μm, or any range or sub-range therebetween.

[0143] In some embodiments, Figure 2As shown, the foldable device 101 may include a release liner 213. In other embodiments, as shown, the release liner 213 may be disposed above the adhesive 207. In other embodiments, as shown, the release liner 213 may directly contact (e.g., bond to) the second contact surface 211 of the adhesive 207. The release liner 213 may include a first major surface 215 and a second major surface 217 opposite the first major surface 215. As shown, the release liner 213 may be disposed on the adhesive 207 by attaching the second contact surface 211 of the adhesive layer 207 to the second major surface 217 of the release liner 213. In some embodiments, as shown, the first major surface 215 of the release liner 213 may include a planar surface. In some embodiments, as shown, the second major surface 217 of the release liner 213 may include a planar surface. The release liner 213 may include paper and / or a polymer. Exemplary embodiments of paper include kraft paper, machine-made paper, polymer-coated paper (e.g., polymer-coated glassine paper, siliconized paper), or clay-coated paper. Exemplary embodiments of polymers include polyesters (e.g., polyethylene terephthalate (PET)) and polyolefins (e.g., low-density polyethylene (LDPE), high-density polyethylene (HDPE), polypropylene (PP)).

[0144] In some embodiments, Figure 3 As shown, the foldable device 301 may include a display device 303. In other embodiments, as shown, the display device 303 may be disposed above the adhesive 207. In other embodiments, as shown, the display device 303 may directly contact (e.g., bond to) the second contact surface 211 of the adhesive 207. In some embodiments, by removing Figure 2The foldable device 301 can be produced by removing the release liner 213 of the foldable device 101 and attaching the display device 303 to the second contact surface 211 of the adhesive 207. Alternatively, the foldable device 301 can be produced without the step of removing the release liner 213 before attaching the display device 303 to the second contact surface 211 of the adhesive 207, for example, when the release liner 213 is not applied to the second contact surface 211 of the adhesive 207. The display device 303 may include a first major surface 309 and a second major surface 311 opposite to the first major surface 309. As shown in the figure, the display device 303 can be set on the adhesive 207 by attaching the second contact surface 211 of the adhesive 207 to the second major surface 311 of the display device 303. In some embodiments, as shown in the figure, the first major surface 309 of the display device 303 may include a planar surface. In some embodiments, as shown in the figure, the second major surface 311 of the display device 303 may include a planar surface. Display device 303 may include a liquid crystal display (LCD), an electrophoretic display (EPD), an organic light emitting diode display (OLED), or a plasma display panel (PDP). In some embodiments, display device 303 may be part of a portable electronic device such as a consumer electronic product, a smartphone, a tablet computer, a wearable device, or a laptop computer.

[0145] Embodiments of the present disclosure may include a consumer electronic product. The consumer electronic product may include a front surface, a rear surface, and a side surface. The consumer electronic product may also include an electrical component at least partially within a housing. The electrical component may include a controller, a memory, and a display. The display may be at the front surface of the housing or adjacent to the front surface of the housing. The consumer electronic product may include a cover substrate disposed above the display. In some embodiments, at least one of a portion of the housing or the cover substrate includes a foldable device or strip as described in embodiments of the present disclosure.

[0146] The foldable device disclosed herein can be incorporated into another article, such as an article with a display (or display article) [e.g., consumer electronic devices, including mobile phones, tablets, computers, navigation systems, wearable devices (such as watches), etc.]; architectural articles; transportation articles (such as cars, trains, aircraft, ships, etc.), appliance articles, or any article that can benefit from a certain degree of transparency, scratch resistance, wear resistance, or a combination of the above properties. Figure 31-32 An exemplary article of manufacture comprising any of the foldable devices disclosed herein is shown. Specifically, Figure 31-32A consumer electronic device 3100 is shown, which includes a housing 3102 having a front surface 3104, a rear surface 3106, and side surfaces 3108; electrical components (not shown) at least partially or completely located within the housing and including at least a controller, a memory, and a display 3110, the display 3110 being at or adjacent to the front surface of the housing; and a cover substrate 3112 at or above the front surface of the housing such that the cover substrate 3112 is above the display. In some embodiments, at least one of the cover substrate 3112 or a portion of the housing 3102 can include any of the foldable devices disclosed herein, for example, a foldable substrate.

[0147] In some embodiments, the foldable device 101, 301, and 601 can be arranged around a plane (e.g., see Figure 1-3 In some embodiments, plane 109 may include a central axis 107 of the foldable device, which may be located at the second major surface 205 of the foldable substrate 201. As further illustrated, in some embodiments, plane 109 may include a folding axis 102 of the foldable device. In some embodiments, the foldable device may be folded about a folding axis 102 extending in a direction 104 of a width 103, along a direction 111 (e.g., see Figure 1 ) to form a folded structure (see, for example, Figure 8-9 and 13). As shown, the foldable device may include a single folding axis to allow the foldable device to include a bifold, wherein, for example, the foldable device can be folded in half. In other embodiments, the foldable device may include two or more pivot axes, wherein each folding axis includes a corresponding central portion that is the same or similar to the central portion 225 described above. For example, providing two pivot axes may allow the foldable device to include a trifold, wherein, for example, the foldable device can be folded to have three portions, including a first portion 221, a second portion 223, and a third portion that is similar or the same as the first portion or the second portion.

[0148] According to an embodiment of the present disclosure, Figure 8-9 An embodiment of a foldable device 801 is schematically illustrated, and Fig.13 Schematically illustrates an embodiment of a foldable device 1301 in a folded configuration (e.g., similar to Figure 3 The foldable device 301 is shown in a flat configuration. Fig.13As shown, the folded foldable device 1301 is similar to the folded foldable device 301, and the display device 303 is on the inner side of the folded foldable device 1301 after folding, and the second main surface 205 of the foldable substrate 201 is on the outer side of the folded foldable device 1301. The user will view the display device 303 through the foldable substrate 201, so the user will be on the side of the second main surface 205. Fig. 9 As shown, the folded foldable device 801 is folded so that the second major surface 205 of the foldable substrate 201 is on the inner side of the folded foldable device 801, and the PET sheet 909 (eg, Figure 3 The display device 303 of the foldable device 301 in the embodiment of the present invention is an alternative to the display device 303 of the foldable device 301 in the embodiment of the present invention) is on the outside of the folded foldable device 801. However, again, the user will be on the side of the second major surface 205 to view the display device 303 through the foldable substrate 201.

[0149] As defined herein, "foldable" includes full folding, partial folding, bending, flexing, and multiple folding capabilities. As used herein, the terms "failure," "failed," and the like refer to breakage, destruction, delamination, or crack propagation. If the glass-based article resists failure when it is maintained at a radius of "X" for 24 hours at about 85° C. and a relative humidity of about 85%, the foldable substrate achieves a bending radius of "X," or has a bending radius of "X," or includes a bending radius of "X."

[0150] As used herein, the "effective minimum bending radius" of a foldable substrate (e.g., a glass-based and / or ceramic-based foldable substrate 201) is measured using a parallel plate device 901 (see Fig. 9 ) is measured by the following test configuration and process, wherein the parallel plate device 901 includes a pair of parallel rigid stainless steel plates 903, 905, the pair of parallel rigid stainless steel plates 903, 905 including a first rigid stainless steel plate 903 and a second rigid stainless steel plate 905. When measuring the "effective minimum bend radius", the optically clear adhesive 907 (e.g., replacing the adhesive 207, if present) includes a thickness of 50 μm between the second contact surface 913 of the adhesive 207 and the first surface area 237 and the third surface area 239 of the first major surface 203 of the foldable substrate 201. When measuring the "effective minimum bend radius", as Fig. 9 The results show that a 100 μm thick polyethylene terephthalate (PET) sheet is used instead of Figure 3The display device 303 is used for measurement. Therefore, during the test to determine the "effective minimum bending radius", the display device 303 is not used. In the same manner, a 100 μm thick sheet of polyethylene terephthalate (PET) 909 is attached to the second contact surface 913 of the optically clear adhesive 907 instead of the display device 303, so that the release liner 213 is attached to the second contact surface 211, as shown in FIG. Figure 2 As shown. If the foldable device 101, 301, 801 or 1301 includes an adhesive 207, and the adhesive 207 includes an optically clear adhesive, the adhesive may be adjusted to include a thickness of 50 μm. If the foldable device including the foldable substrate does not include an adhesive (e.g., the foldable device 301), an optically clear adhesive 907 including a thickness of 50 μm may be disposed above the first major surface (e.g., 203 or 403) of the foldable substrate. The assembled foldable substrate 201, the 50 μm thick optically clear adhesive 907, and the 100 μm thick PET sheet are placed between the pair of parallel rigid stainless steel plates 903, 905 so that similar to Fig. 9 In the configuration shown, the foldable substrate 201 will be on the inside of the bend. The distance between the parallel plates is reduced at a rate of 50 μm / second until the parallel plate distance 911 is equal to twice the "effective minimum bend radius" to be tested. Next, the parallel plates are maintained at twice the effective minimum bend radius to be tested at about 85°C and about 85% relative humidity for 24 hours. As used herein, the "effective minimum bend radius" is the minimum effective bend radius that the foldable substrate 201 can withstand testing without failure under the above conditions and configurations.

[0151] In some embodiments, the foldable substrate 201 of the foldable device 101 or 301 can achieve an effective minimum bending radius of less than or equal to 100 mm, less than or equal to 50 mm, less than or equal to 20 mm, or less than or equal to 10 mm. In other embodiments, the foldable substrate 201 of the foldable device 101 or 301 can achieve an effective bending radius of 10 mm, or 7 mm, or 5 mm, 3 mm, or 1 mm. In some embodiments, the foldable substrate 201 of the foldable device 101 or 303 may include an effective minimum bending radius of less than or equal to about 10 mm, less than or equal to about 7 mm, less than or equal to about 5 mm, greater than or equal to about 1 mm, greater than or equal to about 2 mm, or greater than or equal to about 5 mm. In some embodiments, the foldable substrate 201 of the foldable device 101 or 301 may include an effective minimum bending radius in the following range: about 1 mm to about 10 mm, about 1 mm to about 7 mm, about 1 mm to about 5 mm, about 2 mm to about 10 mm, about 2 mm to about 7 mm, about 2 mm to about 5 mm, about 5 mm to about 10 mm, about 5 mm to about 7 mm, about 7 mm to about 10 mm, or any range or sub-range therebetween.

[0152] In some embodiments, a width 232 of a central portion 225 of the foldable substrate 201 is defined between the first portion 221 and the second portion 223 in the direction 106 of the length 105. In some embodiments, the width 232 of the central portion 225 can be about 2.8 times or more, about 3 times or more, about 4 times or more, about 6 times or less, about 5 times or less, or about 4 times or less of the effective minimum bend radius. In some embodiments, the width 232 of the central portion 225 can be in the range of about 2.8 times to about 6 times, about 2.8 times to about 5 times, about 3 times to about 5 times, about 3 times to about 4 times, about 4 times to about 6 times, about 4 times to about 5 times, or any range or sub-range therebetween as a multiple of the effective minimum bend radius. Without wishing to be bound by theory, the length of the curved portion in the circular configuration between the parallel plates can be about 1.6 times the parallel plate distance 911 (e.g., about 3 times the effective minimum bend radius, about 3.2 times the effective minimum bend radius). In some embodiments, the width 232 of the central portion 225 of the foldable substrate 201. In some embodiments, the width 232 of the central portion 225 of the foldable substrate 201 can be greater than or equal to about 2.8 mm, greater than or equal to about 6 mm, greater than or equal to about 9 mm, less than or equal to about 60 mm, less than or equal to about 40 mm, or less than or equal to about 24 mm. In some embodiments, the width 232 of the central portion 231 of the foldable substrate 201 can be in the range of about 2.8 mm to about 60 mm, about 2.8 mm to about 40 mm, about 6 mm to about 40 mm, about 6 mm to about 24 mm, about 9 mm to about 24 mm, or any range or sub-range therebetween.

[0153] Compared to foldable substrates of uniform thickness, the foldable substrates of embodiments of the present disclosure include a central portion that includes a central thickness that is less than the thickness of the substrate, which has an advantage. One advantage can come from the difference in the maximum central tension (CT) of the central portion relative to the maximum CT of the thicker first and / or second portions. For example, when the central portion (including a central thickness that is less than the substrate thickness of the first portion and / or the second portion) is subjected to the same ion exchange conditions from the same bath as a component with the first portion and / or the second portion, the thinner central portion winds up and has a higher maximum central tension (CT) than the first portion and / or the second portion of the substrate containing the substrate thickness. Therefore, when a break occurs in the first portion and / or the second portion (including a lower maximum CT relative to the maximum CT of the central portion, and within the scope of the present disclosure), the substrate breaks into a low number of pieces and breaks in a non-violent manner. On the other hand, when fracture occurs in the central portion (having a higher maximum CT relative to the first portion and / or the second portion, and within the range of the maximum CT of the central portion proposed in the present disclosure), the fracture is constrained within the central portion and does not extend to the first portion and / or the second portion, thereby keeping a large area of ​​the substrate unfractured and still visually pleasing. In other words, the low maximum tensile stress in the first portion and / or the second portion of the foldable substrate (within the range proposed in the present disclosure) can store relatively little energy in the first portion and / or the second portion of the foldable substrate, thereby promoting low-energy failure.

[0154] The foldable device can have impact resistance defined by the ability of the first portion 221 and / or the second portion 223 of the foldable substrate 201 of the foldable device to avoid failure at a pen drop height (e.g., greater than or equal to 8 centimeters (cm)) when measured according to a "pen drop test." As used herein, the "pen drop test" is conducted such that a sample of the foldable substrate is tested under a load imparted to the second major surface of a glass-based article (i.e., from a pen dropped from a certain height), the glass-based article being constructed as in a parallel plate test and having a 100 μm thick PET layer attached with a 50 μm thick optically clear adhesive deposited on the first major surface and the central surface area of ​​the foldable substrate. It should be understood that in the pen drop test, a 100 μm thick PET layer attached by a 50 μm thick optically clear adhesive is used to replace the optically clear adhesive and optional release liner or display device, which can be used in combination with a foldable substrate as a component of a foldable device of an embodiment of the present disclosure. Therefore, the PET layer in the pen drop test is intended to simulate a foldable electronic display device (e.g., an OLED device). During the test, the cover glass substrate bonded to the PET layer was placed on an aluminum plate (6063 aluminum alloy, which was polished to a certain surface roughness with 400 paper), and the PET layer was in contact with the aluminum plate. No tape was used on the side of the sample that rested on the aluminum plate.

[0155] like Fig.15As shown, the pen drop device 1501 includes a ballpoint pen 1503. The pen used for the pen drop test is a BIC Easy Glide Pen, a fine pen, which includes a tungsten carbide bead point tip 1505 with a diameter of 0.7 mm (0.68 mm) and a weight of 5.73 grams (g) including the pen cap (the weight without the pen cap is 4.68 g). The ballpoint pen 1503 is held at a predetermined height 1509 from the first major surface 203 or 403 of the foldable substrate 201 or the strip 501. In the pen drop test, a tube (not shown for clarity) is used to guide the ballpoint pen 1503 to the first major surface 203 or 403 of the foldable substrate 201 or strip 501, and the tube is placed in contact with the first major surface 203 or 403 of the foldable substrate 201 or strip 501 so that the longitudinal axis of the tube is substantially perpendicular to the first major surface 203 or 403 of the foldable substrate 201 or strip 501. The tube has an outer diameter of 1 inch (2.54 cm), an inner diameter of nine-sixteenths of an inch (1.4 cm), and a length of 90 cm. For each test, the ballpoint pen 1503 is held at a predetermined height 1509 using an acrylonitrile butadiene ("ABS") pad. After each drop, the tube is repositioned relative to the foldable substrate 201 or strip 501 to guide the ballpoint pen 1503 to a different impact location on the foldable substrate 201 or strip 501.

[0156] For the pen drop test, a ballpoint pen 1503 is dropped with the cap attached to the top end (i.e., the end opposite the tip) so that the ballpoint tip 1505 can interact with the first major surface 203 or 403 of the foldable substrate 201 or ribbon 501. In the drop procedure according to the pen drop test, a pen drop is performed at an initial height of 1 cm, followed by sequential drops in 0.5 cm increments up to 20 cm, and then, after 20 cm, drops are performed in 2 cm increments until the foldable substrate 201 or ribbon 501 fails. After each drop is performed, the presence of any observed fracture, failure, or other evidence of damage to the foldable substrate 201 or ribbon 501 is recorded as well as the specific predetermined height 1509 of the pen drop. When using the pen drop test, multiple glass-based ribbons (e.g., samples) can be tested according to the same drop procedure to produce a population with improved statistical accuracy. For the pen drop test, the ballpoint pen 1503 was replaced with a new pen after every 5 drops, and for each new foldable substrate 201 or strip 501 tested. In addition, all pen drops were performed at or near the center of the foldable substrate 201 or strip 501, at random locations on the foldable substrate 201 or strip 501, and the pen was not dropped near or on the edge of the foldable substrate 201 or strip 501. For the purpose of the pen drop test, "failure" means the formation of a visible mechanical defect in the glass-based strip. The mechanical defect can be a crack or plastic deformation (e.g., a surface dent). The crack can be a surface crack or a through crack. The crack can be formed on the interior or exterior surface of the glass-based strip. The crack can extend through all or a portion of the foldable substrate 201 or strip layer 501. The minimum size of a visible mechanical defect is 0.2 mm or larger.

[0157] Fig.14 A curve 1401 is shown of the maximum principal stress 1405 in megapascals (MPa) on the first major surface of the foldable substrate as a function of the thickness 1403 of the glass-based substrate in micrometers based on a pen drop height of 2 cm on the second major surface of the glass-based substrate. Fig.14 As shown, the maximum principal stress on the first major surface of the glass-based sheet is greatest at a thickness 222, 503 of about 65 μm. This suggests that pen-down performance can be improved by avoiding thicknesses 222, 503 greater than or less than about 65 μm, for example, by using thicknesses 222, 503 greater than about 80 μm or less than about 50 μm.

[0158] Figure 4-7 Schematically illustrates exemplary embodiments of foldable devices 401, 601, and 701 in an unfolded configuration (e.g., a flat configuration) according to embodiments of the present disclosure. The strip 501 may include a first major surface 403 and a second major surface 405 (see Figure 5). As shown, a ribbon thickness 503 of the ribbon 501 may be defined between the first major surface 403 and the second major surface 405. In some embodiments, the ribbon thickness 503 may be greater than or equal to about 25 μm, greater than or equal to about 50 μm, greater than or equal to about 80 μm, greater than or equal to about 100 μm, greater than or equal to about 125 μm, less than or equal to about 150 μm, less than or equal to about 125 μm, less than or equal to about 100 μm, less than or equal to about 50 μm, or less than or equal to about 40 μm. In some embodiments, the ribbon thickness 503 may be in the range of about 25 μm to about 150 μm, about 25 μm to about 125 μm, about 25 μm to about 100 μm, about 25 μm to about 50 μm, about 25 μm to about 40 μm, or any range or sub-range therebetween. In some embodiments, the ribbon thickness 503 may be in the range of about 50 μm to about 150 μm, about 100 μm to about 150 μm, about 100 μm to about 125 μm, about 125 μm to about 150 μm, or any range or sub-range therebetween. In some embodiments, the ribbon thickness 503 may be in the range of about 80 μm to about 150 μm, about 80 μm to about 125 μm, or about 80 μm to about 100 μm, or any range or sub-range therebetween.

[0159] In some embodiments, Figure 5-7 As shown, the first major surface 403 of the strip 501 can extend along a first plane. In other embodiments, as shown, the second major surface 405 can extend along a second plane, which can be parallel to the first plane. In other embodiments, the strip thickness 503 can be substantially uniform along the length and / or width of the strip.

[0160] As used herein, warp is defined relative to a reference plane in accordance with ASTM F1390. In some embodiments, the warp is measured in the direction of the strip thickness 503 relative to a reference plane defined by a first plane defined by the first major surface 403 of the strip 501. In other embodiments, the warp may be greater than or equal to about 10 nanometers (nm), greater than or equal to about 50 nm, greater than or equal to about 100 nm, greater than or equal to about 200 nm, less than or equal to about 2 μm, less than or equal to about 1.5 μm, less than or equal to about 1 μm, or less than or equal to about 500 nm. In other embodiments, the warp may be in the range of about 10 nm to about 2 μm, about 50 nm to about 2 μm, about 50 nm to about 1.5 μm, about 100 nm to about 1.5 μm, about 100 nm to about 1 μm, about 200 nm to about 1 μm, about 200 nm to about 500, or any range or sub-range therebetween.

[0161] The foldable device 401 including the strip 501 may include a first edge 411 and a second edge 413 opposite the first edge, such as Figure 4 The first edge 411 may extend between the first major surface 403 and the second major surface 405. Figure 5 As shown, the second edge 413 may extend between the first major surface 403 and the second major surface 405. The width 103 of the strip 501 may be defined between the first edge 411 of the strip 501 and the second edge 413 of the strip 501. Figure 4 As shown, width 103 may extend in direction 104 of fold axis 102 of strip 501 .

[0162] The length 105 of the strip 501 may be defined in a direction 106 perpendicular to the direction 104 of the width 103 of the strip 501. Figure 4 As shown, the length 105 can extend in a direction 106 that is perpendicular to the direction 104 of the fold axis 102. In some embodiments, the direction 104 of the width 103 and the direction 106 of the length 105 can define a plane that is parallel to the plane defined by the first major surface 403. In some embodiments, as Figure 4 As shown, the strip 501 may include a third edge 415 and a fourth edge 417 opposite the third edge 415. The third edge 415 may extend between the first major surface 403 and the second major surface 405. The fourth edge 417 may extend between the first major surface 403 and the second major surface 405. In other embodiments, the length 105 may be defined between the third edge 415 and the fourth edge 417. In some embodiments, the strip 501 may include a polygon having four or more sides [e.g., a quadrilateral (rectangle), a pentagon, a hexagon], a curved shape (e.g., an ellipse), or a shape including a combination of a polygon and a curved shape (e.g., having a rounded end between a flat first edge and a flat second edge).

[0163] In some embodiments, the width 103 of the strip 501 and / or the length 105 of the strip 501 may be greater than or equal to about 10 mm, greater than or equal to about 20 mm, greater than or equal to about 50 mm, less than or equal to about 1,000 mm, less than or equal to about 500 mm, less than or equal to about 200 mm, or less than or equal to about 100 mm. In some embodiments, the width 103 of the strip 501 and / or the length 105 of the strip 501 may be in the range of about 10 mm to about 1,000 mm, about 20 mm to about 1,000 mm, about 20 mm to about 500 mm, about 50 mm to about 500 mm, about 50 mm to about 200 mm, about 50 mm to about 100 mm, or any range or sub-range therebetween.

[0164] In some embodiments, one or more portions (as described below) may be characterized by the surface roughness of one or more of their corresponding surfaces. As used herein, "surface roughness" means Ra surface roughness, which is the arithmetic mean of the absolute deviations of the surface profile from the average position in a direction perpendicular to the surface of the test area. Unless otherwise indicated, all surface roughness values ​​are average roughness (Ra) measured for an 80 μm × 80 μm test area using atomic force microscopy (AFM).

[0165] The strip 501 may include a first portion 521. Figure 5 As shown, first portion 521 of strip 501 may include first surface region 537 of first major surface 403 of strip 501. As shown, first portion 521 of strip 501 may include second surface region 527 of second major surface 405 of strip 501. Figure 5 As shown, the first portion 521 may include a thickness substantially equal to the strip thickness 503. In some embodiments, the thickness of the first portion 521 is approximately equal to the strip thickness 503. Figure 4 ) can be substantially uniform over the entire surface. In some embodiments, first portion 521 can extend from first edge 411 to second edge 413. In other embodiments, first surface area 537 of first major surface 403 can extend from first edge 411 to second edge 413, and second surface area 527 of second major surface 405 can extend from first edge 411 to second edge 413. In some embodiments, first portion 521 can include first edge portion 511 of second edge 413 and first edge portion (not shown) of first edge 411.

[0166] In some embodiments, the first portion 521 may include a first stress-free area at the first major surface 403 of the strip 501. In further embodiments, the first stress-free area may include a first surface area 537 of the first major surface 403 in the first portion 521 of the strip 501. In further embodiments, the first stress-free area may include a first edge portion 511 of the second edge 413 and / or a first edge portion of the first edge 411. In some embodiments, the first portion 521 may include a second stress-free area at the second major surface 405 of the strip 501. In further embodiments, the second stress-free area may include a second surface area 527 of the second major surface 405 in the first portion 521 of the strip 501. In further embodiments, the second stress-free area may include a first edge portion 511 of the second edge 413 and / or a first edge portion of the first edge 411. By providing a first portion including a first stress-free area and / or a second stress-free area, excellent impact resistance and / or puncture resistance can be achieved, as demonstrated by the following examples.

[0167] In some embodiments, first portion 521 can include a first layer depth from first major surface 403. In some embodiments, first portion 521 can include a second layer depth from second major surface 405. In some embodiments, first layer depth and / or second layer depth can be greater than or equal to about 0%, greater than or equal to about 1%, greater than or equal to about 2%, less than or equal to about 5%, less than or equal to about 3%, or less than or equal to about 1% as a percentage of tape thickness 503. In some embodiments, first layer depth and / or second layer depth can be in the following ranges as a percentage of tape thickness 503: 0% to about 5%, 0% to about 2%, 0% to about 1%, about 1% to about 5%, about 2% to about 5%, or any range or sub-range therebetween. In other embodiments, first layer depth can be measured from first surface area 537 of first major surface 403 in first portion 521 of tape 501. In other embodiments, first edge portion 511 of second edge 413 and / or first edge portion of first edge 411 can include first layer depth. In some embodiments, first portion 521 can include a second layer depth from second major surface 405. In other embodiments, second layer depth can be measured from second surface region 527 of second major surface 405 in first portion 521 of strip 501. In other embodiments, first edge portion 511 of second edge 413 and / or first edge portion of first edge 411 can include a second layer depth. By providing a first portion including a first layer depth and / or a second layer depth of 0% to about 5%, excellent impact resistance and / or puncture resistance can be achieved, as demonstrated by the following examples.

[0168] In some embodiments, the first portion 521 can include a first surface roughness of the first major surface 403. In some embodiments, the first portion 521 can include a second surface roughness of the second major surface 405. In some embodiments, the first surface roughness and / or the second surface roughness can be greater than or equal to about 0.01 nm, greater than or equal to about 0.1 nm, greater than or equal to about 0.2 nm, less than or equal to about 0.3 nm, less than or equal to about 0.25 nm, or less than or equal to about 0.2 nm. In some embodiments, the first surface roughness and / or the second surface roughness can be in the following ranges: about 0.01 nm to about 0.3 nm, about 0.01 nm to about 0.25 nm, about 0.1 nm to about 0.25 nm, about 0.1 nm to about 0.2 nm, about 0.2 nm to about 0.3 nm, about 0.25 nm to about 0.3 nm, or any range or sub-range therebetween. In further embodiments, the first surface roughness may be measured at a first surface region 537 of the first major surface 403 in the first portion 521 of the strip 501. In further embodiments, the first edge portion 511 of the second edge 413 and / or the first edge portion of the first edge 411 may include the first surface roughness. In further embodiments, the first surface roughness may correspond to the surface roughness of an original surface (e.g., non-etched, non-ion exchanged) of the strip 501. In further embodiments, the second surface roughness may be measured at a second surface region 527 of the second major surface 405 in the first portion 521 of the strip 501. In further embodiments, the first edge portion 511 of the second edge 413 and / or the first edge portion of the first edge 411 may include the second surface roughness. In further embodiments, the second surface roughness may correspond to the surface roughness of an original surface (e.g., non-etched, non-ion exchanged) of the strip 501. Without wishing to be bound by theory, providing a first portion comprising a low first surface roughness and / or second surface roughness (e.g., the surface roughness of the original surface) can reduce the incidence of surface defects and enable excellent impact resistance and / or puncture resistance, as demonstrated by the following examples.

[0169] The strip 501 may include a second portion 523. Figure 5 As shown, the second portion 523 of the strip 501 may include the third surface region 539 of the first major surface 403 of the strip 501. As shown, the second portion 523 of the strip 501 may include the fourth surface region 529 of the second major surface 405 of the strip 501. Figure 2As shown, second portion 523 may include a thickness substantially equal to strip thickness 503. In some embodiments, second portion 523 may include a thickness substantially equal to the thickness of first portion 521. In some embodiments, the thickness of second portion 523 may be substantially uniform over its length and / or width. In further embodiments, third surface area 539 of first major surface 403 may extend from first edge 411 to second edge 413, and fourth surface area 529 of second major surface 405 may extend from first edge 411 to second edge 413. In some embodiments, second portion 523 may include second edge portion 513 of second edge 413 and second edge portion (not shown) of first edge 411.

[0170] In some embodiments, the second portion 523 may include a third stress-free area at the first major surface 403 of the strip 501. In further embodiments, the third stress-free area may include a third surface area 539 of the first major surface 403 in the second portion 523 of the strip 501. In further embodiments, the third stress-free area may include a second edge portion 513 of the second edge 413 and / or a first edge portion of the first edge 411. In some embodiments, the second portion 523 may include a fourth stress-free area at the second major surface 405 of the strip 501. In further embodiments, the fourth stress-free area may include a fourth surface area 529 of the second major surface 405 in the second portion 523 of the strip 501. In further embodiments, the fourth stress-free area may include a second edge portion 513 of the second edge 413 and / or a first edge portion of the first edge 411. By providing a second portion including a third stress-free area and / or a fourth stress-free area, excellent impact resistance and / or puncture resistance can be achieved, as demonstrated by the following examples.

[0171] In some embodiments, the second portion 523 can include a third layer depth from the first major surface 403. In some embodiments, the second portion 523 can include a fourth layer depth from the second major surface 405. In some embodiments, the third layer depth and / or the fourth layer depth can be greater than or equal to 0%, greater than or equal to about 1%, greater than or equal to about 2%, less than or equal to about 5%, less than or equal to about 3%, or less than or equal to about 1% as a percentage of the thickness 503 of the strip. In some embodiments, the third layer depth and / or the fourth layer depth can be in the following ranges as a percentage of the thickness 503 of the strip: 0% to about 5%, 0% to about 2%, 0% to about 1%, about 1% to about 5%, about 2% to about 5%, or any range or sub-range therebetween. In other embodiments, the third layer depth can be measured from the third surface area 539 of the first major surface 403 in the second portion 523 of the strip 501. In other embodiments, the second edge portion 513 of the second edge 413 and / or the second edge portion of the first edge 411 can include the third layer depth. In further embodiments, the fourth layer depth can be measured from the fourth surface area 529 of the second major surface 405 in the second portion 523 of the strip 501. In further embodiments, the second edge portion 513 of the second edge 413 and / or the second edge portion of the first edge 411 can include the fourth layer depth. By providing a second portion including the third layer depth and / or the fourth layer depth of 0% to about 5%, excellent impact resistance and / or puncture resistance can be achieved, as demonstrated by the following examples.

[0172] In some embodiments, the first portion 521 may include a first tensile stress region including a first maximum tensile stress. In other embodiments, the first tensile stress region may be located between the first compressive stress region and the second compressive stress region. In some embodiments, the second portion 523 may include a second compressive stress region including a second maximum tensile stress. In other embodiments, the second tensile stress region may be located between the third compressive stress region and the fourth compressive stress region and include a second maximum tensile stress. In some embodiments, the first maximum tensile stress and / or the second maximum tensile stress may be greater than or equal to 0 MPa, greater than or equal to about 1 MPa, greater than or equal to about 5 MPa, greater than or equal to about 10 MPa, less than or equal to about 100 MPa, less than or equal to about 50 MPa, less than or equal to about 20 MPa, or less than or equal to about 10 MPa. In some embodiments, the first maximum tensile stress and / or the second maximum tensile stress can be in the range of 0 MPa to about 100 MPa, 0 MPa to about 50 MPa, about 1 MPa to about 50 MPa, about 1 MPa to about 20 MPa, 5 MPa to about 20 MPa, about 5 MPa to about 10 MPa, or any range or sub-range therebetween. In some embodiments, the first portion 521 can include no first tensile stress region, and / or the second portion 523 can include no second tensile stress region, for example, when the first portion 521 and / or the second portion 523 are substantially unreinforced (e.g., stress-free).

[0173] In some embodiments, the second portion 523 may include a third surface roughness of the first major surface 403. In some embodiments, the second portion 523 may include a fourth surface roughness of the second major surface 405. In some embodiments, the third surface roughness and / or the fourth surface roughness may be greater than or equal to about 0.01 nm, greater than or equal to about 0.1 nm, greater than or equal to about 0.2 nm, less than or equal to about 0.3 nm, less than or equal to about 0.25 nm, or less than or equal to about 0.2 nm. In some embodiments, the third surface roughness and / or the fourth surface roughness may be in the following ranges: about 0.01 nm to about 0.3 nm, about 0.01 nm to about 0.25 nm, about 0.1 nm to about 0.25 nm, about 0.1 nm to about 0.2 nm, about 0.2 nm to about 0.3 nm, about 0.25 nm to about 0.3 nm, or any range or sub-range therebetween. In further embodiments, the third surface roughness may be measured from a third surface area 539 of the first major surface 403 in the second portion 523 of the strip 501. In further embodiments, the second edge portion 513 of the second edge 413 and / or the second edge portion of the first edge 411 may include a third surface roughness. In further embodiments, the third surface roughness may correspond to the surface roughness of an original surface (e.g., unetched, non-ion exchanged) of the strip 501. In further embodiments, the fourth surface roughness may be measured from a fourth surface area 529 of the second major surface 405 in the second portion 523 of the strip 501. In further embodiments, the second edge portion 513 of the second edge 413 and / or the first edge portion of the first edge 411 may include a fourth surface roughness. In further embodiments, the fourth surface roughness may correspond to the surface roughness of an original surface (e.g., unetched, non-ion exchanged) of the strip 501. Without wishing to be bound by theory, providing a second portion comprising a low third surface roughness and / or fourth surface roughness (e.g., the surface roughness of the original surface) can reduce the incidence of surface defects and enable excellent impact resistance and / or puncture resistance, as demonstrated by the following examples.

[0174] The strip 501 may include a central portion 541. Figure 5 As shown, the central portion 541 of the strip 501 may include the first central surface region 535 of the first major surface 403 of the strip 501. As shown, the central portion 541 of the strip 501 may include the second central surface region 525 of the second major surface 405 of the strip 501. Figure 5As shown, the central portion 541 may include a thickness substantially equal to the strip thickness 503. In some embodiments, the central portion 541 may include a thickness substantially equal to the thickness of the first portion 521. In some embodiments, the central portion 541 may include a thickness substantially equal to the thickness of the second portion 523. In some embodiments, as shown, the first portion 521, the second portion 523, and the central portion 541 may have substantially equal thicknesses (i.e., strip thickness 522) that are substantially uniform along the length 105 and width 103 of the strip 501. In some embodiments, the thickness of the central portion 541 may be substantially uniform over its length and / or width. In further embodiments, the first central surface region 535 of the first major surface 403 may extend from the first edge 411 to the second edge 413, and the second central surface region 525 of the second major surface 405 may extend from the first edge 411 to the second edge 413. Folding performance can be improved by providing a substantially uniform thickness throughout the center portion to prevent stress concentration, which would occur if a portion of the center portion was thinner than the remaining center portion. In some embodiments, the center portion 541 may include a third edge portion 515 of the second edge 413 and a second edge portion (not shown) of the first edge 411.

[0175] like Figure 4-7 As shown, in the direction 106 of the length 105 of the strip 501, the central portion 541 can be located between the first portion 521 and the second portion 523. In some embodiments, in the direction 106 of the length 105 of the strip 501, the first portion 521, the central portion 541, and the second portion 523 can be arranged in sequence. In some embodiments, the central portion 541 can attach the first portion 521 to the second portion 523. In some embodiments, the first central surface area 535 of the first major surface 403 can be located between the first surface area 537 of the first major surface 403 and the third surface area 539 of the first major surface 403. In some embodiments, the second central surface area 525 of the second major surface 405 can be located between the second surface area 527 of the second major surface 405 and the fourth surface area 529 of the second major surface 405. In some embodiments, the third edge portion 515 of the second edge 413 can be located between the first edge portion 513 of the second edge 413 and the second edge portion 513 of the second edge 413.

[0176] In some embodiments, the central portion 541 may include a first central compressive stress zone. The first central compressive stress zone may extend from the first major surface 403 of the strip 501 to a first central compressive depth. In some embodiments, the first central compressive stress zone may include a first central surface area 535 of the first major surface 403 of the strip 501. In other embodiments, the first central compressive depth may be measured from the first central surface area 535 of the first major surface 403. In some embodiments, the first central compressive stress zone may extend from the first edge 411 to the second edge 413. In other embodiments, the first central compressive stress zone may include a third edge portion 515 of the second edge 413 and / or a third edge surface of the first edge 411. In some embodiments, the first central compressive stress zone may be enriched with sodium and / or potassium ions. In other embodiments, the first central compressive stress region can be enriched in sodium and / or potassium ions relative to first surface region 537 of first major surface 403, third surface region 539 of first major surface 403, second surface region 527 of second major surface 405, and / or third surface region 539 of second major surface 405, and / or relative to the glass body (e.g., the glass composition at a mid-plane at depth).

[0177] In some embodiments, the central portion 541 may include a second central compressive stress zone. The second central compressive stress zone may extend from the second major surface 405 of the strip 501 to a second central compressive depth. In some embodiments, the second central compressive stress zone may include a second central surface area 525 of the second major surface 405 of the strip 501. In other embodiments, the second central compressive depth may be measured from the second central surface area 525 of the second major surface 405. In some embodiments, the second central compressive stress zone may extend from the first edge 411 to the second edge 413. In other embodiments, the second central compressive stress zone may include a third edge portion 515 of the second edge 413 and / or a third edge surface of the first edge 411. In some embodiments, the second central compressive stress zone may be enriched with sodium and / or potassium ions. In other embodiments, the first central compressive stress region can be enriched with sodium and / or potassium ions relative to first surface region 537 of first major surface 403, third surface region 539 of first major surface 403, second surface region 527 of second major surface 405, and / or third surface region 539 of second major surface 405.

[0178] In some embodiments, as a percentage of the strip thickness 503, the first central compression depth and / or the second central compression depth may be greater than or equal to about 10%, greater than or equal to about 15%, greater than or equal to about 20%, less than or equal to about 30%, less than or equal to about 25%, or less than or equal to about 20%. In some embodiments, as a percentage of the strip thickness 503, the first compression depth and / or the second central compression depth may be in the range of about 10% to about 30%, about 10% to about 25%, about 15% to about 25%, about 15% to about 20%, about 20% to about 25%, or any range or sub-range therebetween. In some embodiments, the first central compression depth may be greater than, less than, or substantially equal to the second central compression depth. In some embodiments, the maximum compressive stress of the second central compressive stress region may be greater than, less than, or substantially equal to the maximum compressive stress of the first central compressive stress region.

[0179] In some embodiments, the maximum compressive stress of the first central compressive stress region and / or the maximum compressive stress of the second central compressive stress region can be greater than or equal to about 10 megapascals (MPa), greater than or equal to 50 MPa, greater than or equal to about 100 MPa, greater than or equal to about 200 MPa, greater than or equal to about 300 MPa, greater than or equal to about 400 MPa, greater than or equal to about 500 MPa, greater than or equal to about 600 MPa, greater than or equal to about 700 MPa, less than or equal to about 1,500 MPa, less than or equal to about 1,200 MPa, less than or equal to about 1,000 MPa, less than or equal to about 600 MPa, or less than or equal to about 400 MPa. In some embodiments, the maximum compressive stress of the first central compressive stress zone and / or the maximum compressive stress of the second central compressive stress zone may be in the range of about 10 MPa to about 1,500 MPa, about 10 MPa to about 1,200 MPa, about 50 MPa to about 1,200 MPa, about 50 MPa to about 1,000 MPa, about 100 MPa to about 1,000 MPa, about 100 MPa to about 700 MPa, about 100 MPa to about 600 MPa, about 300 MPa to about 600 MPa, about 300 MPa to about 400 MPa, 700 MPa to about 1,500 MPa, about 700 MPa to about 1,200 MPa, about 700 MPa to about 1,000 MPa, or any range or sub-range therebetween.

[0180] In some embodiments, the center portion 541 can include a first center layer depth from the first major surface 403 of the strip 501. In some embodiments, the first center layer depth can be measured from the first center surface region 535 of the first major surface 403 in the center portion 541 of the strip 501. In some embodiments, the first center layer depth can extend from the third edge portion 515 of the second edge 413 and / or from the third edge portion of the first edge 411.

[0181] In some embodiments, the center portion 541 can include a second center layer depth from the second major surface 405 of the strip 501. In some embodiments, the second center layer depth can be measured from the second center surface region 525 of the second major surface 405 in the center portion 541 of the strip 501. In some embodiments, the second center layer depth can extend from the third edge portion 515 of the second edge 413 and / or from the third edge portion of the first edge 411.

[0182] In some embodiments, as a percentage of the strip thickness 503, the first center layer depth and / or the second center layer depth may be greater than or equal to about 10%, greater than or equal to about 15%, greater than or equal to about 20%, less than or equal to about 40%, less than or equal to about 30%, or less than or equal to about 25%. In some embodiments, as a percentage of the substrate thickness 503, the first layer depth and / or the second layer depth may be in the following ranges: about 10% to about 40%, about 15% to about 40%, about 15% to about 30%, about 20% to about 30%, about 20% to about 25%, about 10% to about 25%, about 15% to about 25%, or any range or sub-range therebetween. In some embodiments, the area between the first major surface 403 and the first center layer depth may include a first center compressive stress zone. In some embodiments, the area between the second major surface 405 and the second center layer depth may include a second center compressive stress zone. In some embodiments, the first center layer depth may be substantially equal to the second center layer depth. In some embodiments, the first center layer depth may be greater than the second center layer depth. In some embodiments, the first center layer depth may be less than the second center layer depth.

[0183] In some embodiments, the central portion 541 may include a central tensile stress region. In some embodiments, the central tensile stress region may be located between the first central compressive stress region and the second central compressive stress region. In some embodiments, the central maximum compressive stress may be greater than or equal to about 10 MPa, greater than or equal to about 20 MPa, greater than or equal to about 50 MPa, greater than or equal to about 100 MPa, less than or equal to about 375 MPa, less than or equal to about 300 MPa, less than or equal to about 200 MPa, or less than or equal to about 150 MPa. In some embodiments, the central maximum compressive stress may be in the range of about 10 MPa to about 375 MPa, about 10 MPa to about 300 MPa, about 20 MPa to about 300 MPa, about 20 MPa to about 200 MPa, about 50 MPa to about 200 MPa, about 50 MPa to about 150 MPa, about 100 MPa to about 150 MPa, or any range or sub-range therebetween. The central maximum compressive stress may be greater than the first maximum compressive stress (if provided) and / or the second maximum compressive stress (if provided). One advantage may come from the difference in the maximum central tension (CT) of the central portion relative to the maximum CT (if provided) of the first and / or second portions. For example, when a break occurs in the first portion and / or the second portion (including a maximum CT that is substantially zero or a lower maximum CT relative to the maximum CT of the central portion), the substrate breaks into a low number of pieces and breaks in a non-violent manner. On the other hand, when a break occurs in the central portion (having a higher maximum CT relative to the maximum CT (if provided) of the first portion and / or the second portion), the break is constrained within the central portion and does not extend to the first portion and / or the second portion, thereby maintaining a large area of ​​the substrate unbroken and still visually pleasing. In other words, the low maximum tensile stress in the first portion and / or the second portion of the foldable substrate (within the scope of the present disclosure) can store relatively less energy in the first portion and / or the second portion of the foldable substrate, thereby promoting low energy failure.

[0184] Without wishing to be bound by theory, chemically strengthening the central portion 541 to establish the first central compressive stress region and / or the second central compressive stress region can achieve a small bending radius (e.g., a small, about 10 mm or less, or about 9 mm or less, or about 8 mm or less, or about 7 mm or less, or about 6 mm or less, or about 5 mm or less, or about 4 mm or less, or about 3 mm or less, or about 2 mm or less, or about 1 mm) because the compressive stress generated by the chemical strengthening can offset the outermost surface of the strip in the bent state (e.g., Fig.10In addition, including the first edge and / or the second edge in the first central compressive stress region and / or the second central compressive stress region can further achieve a small minimum bending radius by reducing damage (e.g., fracture and / or cracking) caused by folding stress.

[0185] In some embodiments, the strip 501 may be arranged around the pivot axis 102 along the Figure 4 The direction 111 shown is folded to form a folded structure, such as Figure 10-11 shown. Fig.10 According to an embodiment of the present disclosure, one exemplary embodiment of a strip 501 in a folded configuration is schematically illustrated. Fig.10 The strip 501 is shown folded such that the first major surface 403 is on the inside of the folded strip 501 and the second major surface 405 is on the outside of the folded strip 501. Although not shown, in some embodiments, the strip 501 can be folded such that the second major surface 405 is on the inside of the fold.

[0186] As shown, the ribbon can include a single center portion configured to allow the ribbon to include a bifold, where, for example, the ribbon can be folded in half. In other embodiments, the ribbon can include two or more center portions, where each center region includes corresponding first and second compressive stress regions similar or identical to those described above for center portion 541. For example, providing two center portions can allow the ribbon to include a trifold.

[0187] As used herein, the "minimum bend radius" of a strip is measured using the following test configuration and procedure using a parallel plate apparatus 1101, as follows: Fig.11 The parallel plate device 1101 includes a pair of parallel rigid stainless steel plates 903, 905, which include a first rigid stainless steel plate 903 and a second rigid stainless steel plate 905. When measuring the minimum bending radius, the strip 501 is placed between the pair of parallel rigid stainless steel plates 903, 905 so that the strip 501 will be similar to Fig.11The structure shown is folded. The distance between the parallel plates is reduced at a rate of 5 mm / second until the parallel plate distance 1111 corresponds to the bending radius (R) to be tested. As used herein, the corresponding bending radius is equal to 2.396 times the difference between the parallel plate distance 1111 and the tape thickness 503. Then, the parallel plates are kept at a parallel plate distance 1111 corresponding to the bending radius to be tested for 24 hours at about 85°C and a relative humidity of about 85%. As used herein, the "minimum bending radius" is the minimum bending radius that the tape 501 can withstand under the above conditions and construction without failure. When the difference between the parallel plate distance 1111 and the tape thickness 503 is equivalent to 2.396 times the "minimum bending radius" of the tape 501, the parallel plate distance 911 corresponds to 2 times the "effective minimum bending radius" of the foldable devices 101, 301, 801 and 1301 including the foldable substrate 201.

[0188] In some embodiments, the strip 501 can achieve a minimum bend radius of 10 mm, or 7 mm, or 5 mm, 3 mm, or 1 mm. In some embodiments, the strip 501 can include a minimum bend radius of less than 10 mm, less than 7 mm, less than 5 mm, or less than 3 mm. In some embodiments, the strip 501 can include a minimum bend radius in the range of about 1 mm to about 10 mm, about 1 mm to about 7 mm, about 2 mm to about 7 mm, about 2 mm to about 5 mm, about 5 mm to about 10 mm, about 5 mm to about 7 mm, about 7 mm to about 10 mm, or any range or sub-range therebetween.

[0189] like Figure 4 As shown, the central portion 541 may include a width 432 in the direction 106 of the length 105 of the strip 501. In some embodiments, the width 432 of the central portion 541 of the strip 501 is defined between the first portion 521 and the second portion 523, and it can be 3 times or more of the minimum bend radius. Without wishing to be bound by theory, the length of the curved portion in the circular configuration between the parallel plates can be about 3 times the corresponding minimum bend radius. In some embodiments, the width 432 of the central portion 541 of the strip 501 can be substantially equal to or greater than the curved length of the strip at the minimum bend radius. In some embodiments, the width 432 of the central portion 541 of the strip 501 can be greater than or equal to about 3 mm, greater than or equal to about 6 mm, greater than or equal to about 9 mm, less than or equal to about 55 mm, less than or equal to about 40 mm, or less than or equal to about 30 mm. In some embodiments, the width 432 of the central portion 541 of the strip 501 can be in the range of about 3 mm to about 55 mm, about 3 mm to about 40 mm, about 6 mm to about 40 mm, about 6 mm to about 30 mm, about 9 mm to about 30 mm, or any range or sub-range therebetween.

[0190] In some embodiments, the width 432 of the central portion 541 of the strip 501 defined between the first portion 521 and the second portion 523 can be 5 times or more of the minimum bend radius. Without wishing to be bound by theory, the length of the bend in the elliptical configuration between the parallel plates can be about 2.2 times the parallel plate distance 1111 corresponding to the minimum bend radius. In some embodiments, the width 432 of the central portion 541 of the strip 501 can be substantially equal to or greater than the bend length of the strip at the minimum bend radius. Without wishing to be bound by theory, by providing a width 432 of the central portion 541 that is substantially equal to or greater than the bend area, the incidence of damage (e.g., fracture and / or cracking) can be reduced because the compressive stress region in the central portion can counteract the bend-induced tensile stress compared to the unreinforced (e.g., unstressed) portion of the strip. In some embodiments, the width 432 of the central portion 541 of the strip 501 can be greater than or equal to about 5 mm, greater than or equal to about 10 mm, greater than or equal to about 20 mm, less than or equal to about 55 mm, less than or equal to about 40 mm, or less than or equal to about 30 mm. In some embodiments, the width 432 of the central portion 541 of the strip 501 can be in the range of about 5 mm to about 55 mm, about 5 mm to about 40 mm, about 5 mm to about 30 mm, about 10 mm to about 55 mm, about 10 mm to about 40 mm, about 10 mm to about 30 mm, about 20 mm to about 55 mm, about 20 mm to about 40 mm, about 20 mm to about 30 mm, or any range or sub-range therebetween.

[0191] like Figure 6-7 As shown, the strip 501 can be installed in the foldable device 601 or 701. In some embodiments, as Figure 6-7 As shown, adhesive 207 can be disposed above tape 501. In other embodiments, first contact surface 209 of adhesive layer 207 can directly contact (e.g., bond) first major surface 403 of tape 501. In other embodiments, adhesive 207 can include one or more of the materials and / or adhesive thicknesses described above. In other embodiments, as Figure 6 As shown, the foldable device 601 may include a release liner 213 disposed above the second contact surface 211 of the adhesive 207. In another embodiment, as shown in FIG. Figure 7 As shown, the foldable device 701 may include a display device 303 disposed over the second contact surface 211 of the adhesive 207. In further embodiments, the release liner 213 and / or the display device 303 may include the properties described above.

[0192] Will refer to Fig.30 Flowchart and Figure 8-14 Implementations of methods for manufacturing a foldable device of an embodiment of the present disclosure are discussed with reference to the exemplary method steps illustrated in FIG.

[0193] Now refer to Figure 16-19 and 27-29 and Fig.30 A flowchart to illustrate the manufacturing Figure 1-6 The exemplary embodiment of the method of the foldable device 101, 301 and 601 shown in FIG. In the first step 3001 of the method disclosed herein, as shown in FIG. Fig.16 As shown, the method starts with providing a foldable substrate 1601 (e.g., a glass-based foldable substrate and / or a ceramic-based foldable substrate). In some embodiments, the foldable substrate 1601 can be obtained by purchase, or otherwise obtain the foldable substrate, or provided by forming the foldable substrate. In other embodiments, the foldable substrate can be provided by forming them using various strip forming processes, such as slot drawing, down drawing, fusion down drawing, up drawing, roller pressing, redrawing or float. The foldable substrate 1601 may include a first major surface 1603, which may extend along a first plane 1604. The first major surface 1603 may be opposite to the second major surface 1605.

[0194] After step 3001, if Fig.30 As shown, the method can optionally proceed to step 3003, which includes: forming a depression 1634 in the first major surface 1603 of the foldable substrate 1601. Fig.16 As shown, the depressions 1634 can be formed by etching, laser ablation, or machining the first major surface 1603. For example, the first major surface 1603 can be machined by diamond engraving, thereby producing a very precise pattern in the foldable substrate. Fig.16As shown, a depression 1634 can be produced in the first major surface 1603 of the foldable substrate 1601 using diamond engraving, wherein a diamond tip probe 1639 can be controlled using a computer numerical control (CNC) machine 1637. Materials other than diamond can also be used for engraving using a CNC machine. In addition, other methods of forming the depression include photolithography, etching, and laser ablation. Forming the depression 1634 in the first major surface 1603 can provide a central portion 1625 between the first portion 1621 and the second portion 1623 of the foldable substrate 1601. The central portion 1625 can include a first central surface area 1633, wherein the depression 1634 can be defined between the first central surface area 1633 and the first plane 1604, and the first major surface 1603 extends along the first plane 1604. Central portion 1625 may also include a first transition portion 1627 attaching first portion 1621 to central major surface 1635 and a second transition portion 1629 attaching second portion 1623 to central major surface 1635. In some embodiments, the thickness of first transition portion 1627 may increase continuously from central major surface 1635 to first portion 1621. In other embodiments, the thickness of second transition portion 1629 may increase continuously from central major surface 1635 to second portion 1623. Fig.16 As shown, in some embodiments, the first central surface region 1633 may include a central major surface 1635 of the central portion 1625, which may be planar as shown, but in other embodiments, a non-planar configuration may be provided. In addition, the central major surface 1635 may be planar relative to the first plane 1604 and / or the second major surface 1605, such as Fig.16 shown.

[0195] After step 3003, if Fig.30 As further shown, the method may optionally proceed to step 3005, which includes: reducing the thickness of the foldable substrate 1601, such as Fig.17 Although not shown, in some embodiments, the thickness of the foldable substrate 1601 can be reduced by mechanical processing (e.g., grinding). In other embodiments, Fig.17 As shown, chemical etching can be used to reduce the thickness of the foldable substrate 1601. In some embodiments, as shown, chemical etching can include: contacting the foldable substrate 1601 with an etching solution 1703 contained in an etching bath 1701. In other embodiments, the etching solution 1703 can include one or more inorganic acids (e.g., HCl, HF, H2SO4, HNO3).

[0196] In some embodiments, the thickness of foldable substrate 1601 can be reduced by removing layers from first major surface 1603 of foldable substrate 1601 to expose a new first major surface, which can constitute Figure 1-3 In addition or alternatively, the thickness of foldable substrate 1601 may be reduced by removing a layer from second major surface 1605 of foldable substrate 1601 to expose a new second major surface, which may constitute Figure 1-3 The second major surface 205 is shown.

[0197] In some embodiments, removing a layer from the first major surface 1603 can be beneficial in removing surface defects created during the formation of the recess 1634. For example, mechanical processing (e.g., with a diamond tip probe) of the first major surface 1603 to create the recess 1634 may create cracks or other defects, which may present a weak point at which catastrophic failure of the foldable substrate 1601 may occur when folded. Therefore, by removing a layer from the first major surface 1603, surface defects created in the layer during the formation of the recess 1634 can be removed, wherein a new first major surface 203 with fewer surface defects can be presented. Because there are fewer surface defects, a smaller bending radius can be achieved without the foldable substrate failing. In addition, certain processing of the foldable substrate may present different material properties at the first and second major surfaces of the foldable substrate than at the central portion of the foldable substrate. For example, during the draw-down process, the properties of the glass-based substrate at the major surfaces of the glass-based substrate may be different from the central portion of the glass-based substrate. Thus, by removing layers from first major surface 1603 at first portion 1621 and second portion 1623, the new first major surface 203 of these portions can have the same properties as the glass-based material forming first central surface region 1633 to provide consistent optical properties over the length of the foldable substrate.

[0198] In some embodiments, the second major surface 1605 (eg, the entire second major surface 1605) can be covered with an optional mask 1705 so that the second major surface 1605 is not etched and can be used as described above with respect to Figure 1-3The second major surface 205 is used to provide the second major surface 1605. Preventing the second major surface 1605 from being etched can be beneficial in preserving the original properties of the second major surface 1605, which may exist with some processing techniques (e.g., pull-up or pull-down). Maintaining the original surface can allow the second major surface 1605 to present a particularly smooth surface, which second major surface 1605 can form the outermost surface of the foldable device, and the outermost surface can be viewed and / or touched by a user of the foldable device. Alternatively, the thickness of the foldable substrate 1601 can be reduced by removing layers from the second major surface 1605, for example, removing a surface layer to expose a center layer with more consistent optical properties over the length of the foldable substrate, as described above. Therefore, in some embodiments, layers can be removed from the second major surface 1605 to expose a new second major surface, which can be configured as follows: Figure 1-3 The second major surface 205 is shown.

[0199] In some embodiments, a layer can be removed from the first major surface 1603 to expose a new first major surface, which can constitute Figure 1-3 The first major surface 203 shown, and the layer can be removed from the second major surface 1605 to expose a new second major surface, which can constitute Figure 1-3 The second major surface 205 is shown. Removing layers from the first major surface and the second major surface can remove an outer layer of the foldable substrate that may have inconsistent optical properties compared to the inner portion of the foldable substrate below. As a result, the entire thickness of the foldable substrate across the entire length and width can have more consistent optical properties to provide consistent optical performance with little distortion across the entire foldable substrate.

[0200] like Fig.17 As shown, step 3005 may generate Figure 1-3 The foldable substrate 201 shown, wherein Fig.16 The depression 1634 of the foldable substrate 1601 develops into the depression 234 of the foldable substrate 201. In addition, the central portion 1625 of the foldable substrate 1601 may develop into Figure 1-3 The central portion 225 may include the central major surface 235, the first transition portion 227 and the second transition portion 229 described above. Still further, the first portion 1621 and the second portion 1623 of the foldable substrate 1601 may develop into the corresponding first portion 221 and the second portion 223 of the foldable substrate 201 described above.

[0201] After step 3005, if Fig.17 As further shown, the method may proceed to step 3007, which includes chemically strengthening the foldable substrate 201, such as Fig.18As shown. When a first cation within a certain depth in the surface of the foldable substrate 201 is exchanged with a second cation (which has a larger radius than the first cation) in the salt solution 1803, chemical strengthening of the foldable substrate 201 may occur through ion exchange. For example, lithium cations within the depth in the surface of the foldable substrate 201 may be exchanged with sodium cations or potassium cations in the salt solution 1803. As a result, since the radius of the lithium cation is smaller than the radius of the sodium cation or potassium cation exchanged in the salt solution 1803, the surface of the foldable substrate is in a compressed state, and thus chemically strengthened through the ion exchange process. Chemical strengthening of the foldable substrate 201 may include: contacting at least a portion of the foldable substrate 201 containing lithium cations and / or sodium cations with a salt bath 1801 containing a salt solution 1803, wherein the salt solution 1803 contains potassium nitrate, potassium phosphate, potassium chloride, potassium sulfate, sodium chloride, sodium sulfate and / or sodium nitrate, whereby the lithium cations and / or sodium cations diffuse from the foldable substrate 201 into the salt solution 1803 contained in the salt bath 1801. In some embodiments, the temperature of the salt solution 1803 can be greater than or equal to about 300° C., greater than or equal to about 360° C., greater than or equal to about 400° C., less than or equal to about 500° C., less than or equal to about 460° C., or less than or equal to about 400° C. In some embodiments, the temperature of the salt solution 1803 can be in the range of about 300° C. to about 500° C., about 360° C. to about 500° C., about 400° C. to about 500° C., about 300° C. to about 460° C., about 360° C. to about 460° C., about 400° C. to about 460° C., about 300° C. to about 400° C., about 360° C. to about 400° C., or any range or sub-range therebetween. In some embodiments, the foldable substrate 201 can be in contact with the salt solution 1803 for greater than or equal to about 15 minutes, greater than or equal to about 1 hour, greater than or equal to about 3 hours, less than or equal to about 48 hours, less than or equal to about 24 hours, or less than or equal to about 8 hours. In some embodiments, the foldable substrate 201 is contacted with the saline solution 1803 for a time in the range of about 15 minutes to about 48 hours, about 1 hour to about 48 hours, about 3 hours to about 48 hours, about 15 minutes to about 24 hours, about 1 hour to about 24 hours, about 3 hours to about 48 hours, about 3 hours to about 24 hours, about 3 hours to about 8 hours, or any range or sub-range therebetween.

[0202] Chemically strengthening foldable substrate 201 may include chemically strengthening first central surface region 233, chemically strengthening first surface region 237 of first portion 221 of first major surface 203, chemically strengthening third surface region 239 of second portion 223 of first major surface 203, and chemically strengthening second major surface 205 of foldable substrate 201. In some embodiments, chemical strengthening includes chemically strengthening first portion 221 to a first depth (e.g., a compression depth) from first surface region 237 of first major surface 203, chemically strengthening second portion 223 to a fourth depth (e.g., a compression depth) from third surface region 239 of first major surface 203, and chemically strengthening central portion 225 to a first central depth (e.g., a compression depth) from first central surface region 233.

[0203] In some embodiments, chemically strengthening second major surface 205 of foldable substrate 201 may include chemically strengthening second surface region 247 of first portion 221 of second major surface 205, chemically strengthening fourth surface region 249 of second portion 223 of second major surface 205, and chemically strengthening second central surface region 245 of central portion 225 of second major surface 205. In some embodiments, chemically strengthening second major surface 205 may include chemically strengthening first portion 221 to a second depth (e.g., a compression depth) from second surface region 247 of second major surface 205, chemically strengthening second portion 223 to a fourth depth (e.g., a compression depth) from fourth surface region 249 of second major surface 205, and chemically strengthening central portion 225 to a second central depth (e.g., a compression depth) from second central surface region 245 of second major surface 205.

[0204] After step 3007, if Fig.30 As further shown, the method may optionally proceed to step 3009, which includes chemically etching the foldable substrate, such as Fig.19 As shown above, regarding step 3003 and Fig.17As described, etching may include contacting the foldable substrate 201 with an etching solution 1903 contained in an etching bath 1901. The etching solution 1903 may include any of the compounds described above with respect to the etching solution 1703. In some embodiments, the first major surface 203 and the first central surface region 233 are etched. In some embodiments, the second major surface 205 is etched. In other embodiments, the first major surface 203, the first central surface region 1633, and the second major surface 205 are etched. The chemical etching of step 3009 may be designed to remove surface defects that may remain from step 3007 (if performed) due to chemical strengthening of the foldable substrate 201. In fact, the step 3007 of chemical strengthening may result in surface defects that may affect the strength and / or optical quality of the foldable substrate. By etching during step 3009, surface defects generated during the chemical strengthening of step 3007 may be removed. This etching during step 3009 can be designed to remove layers less than 5-10 nanometers, thereby not significantly changing the thickness of the foldable substrate or the surface compression achieved during the chemical strengthening of step 3007.

[0205] After step 3009, if Figure 27-29 As shown, the method of the present disclosure may proceed to step 3011, which includes applying adhesive layer 207 so that first surface area 237 of first major surface 203, third surface area 239 of first major surface 203, and first central surface area 233 of central portion 225 are in contact with adhesive 207 filling recess 234. Although not shown, in some embodiments, the recess may not be completely filled, for example, leaving space for an electronic device and / or a mechanical device.

[0206] In some embodiments, Fig. 27 As shown, one or more layers 2701 of adhesive may be deposited in recess 234 to fill recess 234. A central portion of first contact surface 2705 of adhesive 207 may contact first central surface region 233 of central portion 225. Fig.12As shown, a second layer 2703 of adhesive 207 may be disposed on foldable substrate 201. A first surface region of second layer 2703 may contact first surface region 237 of first major surface 203, and a second surface region of second layer 2703 may contact third surface region 239 of first major surface 203. In addition, a third surface region of second layer 2703 may contact an outer surface of the one or more layers 2701 filling recess 234 to provide an integral interface between the third surface region and the outer surface. Due to the integral interface between the one or more layers 2701 and the second layer 2703, optical refraction may be avoided when light is transmitted between sheets because the one or more layers 2701 and the second layer 2703 may include substantially the same refractive index in some embodiments. Providing the one or more layers 2701 and the second layer 2703 with substantially the same refractive index may avoid optical discontinuities that may otherwise exist near the interface between the one or more layers 2701 and the second layer 2703 of the foldable device. Thus, first contact area 2705 of adhesive 207 may contact first central surface area 233 while also contacting first surface area 237 of first major surface 203 and third surface area 239 of first major surface 203. In other embodiments, as Fig. 27 As shown, the second layer 2703 of adhesive can include a second contact surface 2707, which can be planar and, in some embodiments, can be parallel to the first surface region 237 and / or the third surface region 239. In other embodiments, the entire adhesive layer can be formed by applying (by any suitable method known in the art) a liquid material followed by optional curing.

[0207] In some embodiments, Figure 28-29 As shown, adhesive liquid 2803 can be placed into recess 234. In other embodiments, adhesive liquid 2803 can be placed into recess 234 using a conduit (e.g., a flexible tube, a micropipette, or a syringe). Fig.28As shown, adhesive liquid 2803 can be placed in recess 234 by pouring adhesive liquid 2803 from container 2801 into recess 234. In some embodiments, placing adhesive liquid 2803 in recess 234 can at least partially (e.g., substantially completely) fill recess 234. In some embodiments, adhesive liquid 2803 may include an adhesive precursor and a solvent. In some embodiments, the adhesive precursor may include, but is not limited to, one or more of a monomer, a accelerator, a curing agent, an epoxy material, and / or an acrylate. In some embodiments, the solvent of the adhesive precursor may include a polar solvent (e.g., water, alcohol, acetate, acetone, formic acid, dimethylformamide, acetonitrile, dimethyl sulfoxide, nitromethane, propylene carbonate, poly(ether ether ketone)) and / or a non-polar solvent (e.g., pentane, 1,4-dioxane, chloroform, dichloromethane, ethyl ether, hexane, heptane, benzene, toluene, xylene). The adhesive liquid 2803 may be cured to form a Fig.29 A first layer 2701 of adhesive 207 is shown. In other embodiments, curing the adhesive liquid 2803 may include heating the adhesive liquid 2803. In other embodiments, curing the adhesive liquid 2803 may include irradiating the adhesive liquid 2803 with ultraviolet (UV) radiation.

[0208] like Fig.29 As shown, a second layer 2703 of adhesive 207 can be disposed on foldable substrate 201 and first layer 2701. In some embodiments, a first surface region of second layer 2703 can contact first surface region 237 of first major surface 203, and a second surface region of second layer 2703 can contact third surface region 239 of first major surface 203. Additionally, a third surface region of second layer 2703 can contact an outer surface of first layer 2701 to provide an integral interface between the third surface region and the outer surface. Due to the integral interface between first layer 2701 and second layer 2703, optical refraction can be avoided when light is transmitted between sheets because first layer 2701 and second layer 2703 can include substantially the same refractive index in some embodiments. Providing first layer 2701 and second layer 2703 with substantially the same refractive index can optically avoid optical discontinuities that may otherwise exist near the interface between first layer 2701 and second layer 2703 of a foldable device. Thus, first contact region 209 of adhesive 207 (e.g., first contact surface 2705 of second layer 2703) can contact first central surface region 233 while also contacting first surface region 237 of first major surface 203 and third surface region 239 of first major surface 203. In other embodiments, as Fig.29As shown, the second layer 2703 of adhesive can include a second contact surface 2707 , which can be planar and, in some embodiments, can be parallel to the first surface region 237 and / or the third surface region 239 .

[0209] In some embodiments, a release liner (eg, see Figure 2 Release liner 271) or display device (see, for example, Figure 3 display device 303). Fig.30 At the end point 3013 of the flowchart, the foldable device is completed.

[0210] In some embodiments, the method of manufacturing a foldable device may include the steps disclosed above (e.g., 3001, 3003, 3005, 3007, 3009, 3011, 3013) performed in the order disclosed above. Fig.30 As shown, arrows 3002, 3004, and 3006 may be followed in sequence, wherein the provided foldable substrate 201 (step 3003) is etched to reduce the thickness of the foldable substrate 201 (step 3005) before forming the recess 1634 in the first major surface 203 of the foldable substrate 201 (step 3003) and chemically strengthening the foldable substrate 201 (e.g., ion exchange, step 3007). In some embodiments, the step of etching the foldable substrate 201 to reduce the thickness of the foldable substrate may be skipped by following arrow 3006, for example, when the provided foldable substrate 201 includes a thickness substantially equal to the substrate thickness 222. In some embodiments, the step of etching the foldable substrate 201 after chemically strengthening the foldable substrate 201 may be skipped by following arrow 3008. In some embodiments, the method may include purchasing or otherwise obtaining a foldable substrate 201 including a depression 234 and then proceeding from step 3007, which includes chemically strengthening the foldable substrate 201. Any of the above options may be combined to manufacture a foldable device according to embodiments of the present disclosure.

[0211] Will refer to Figure 20-26 illustrative method steps are used to discuss embodiments of methods of processing ribbons of embodiments of the present disclosure. In some embodiments, the ribbons can be provided by purchasing ribbons (e.g., glass-based ribbons, ceramic-based ribbons). In some embodiments, the ribbons can be provided by forming them using various ribbon forming processes, such as slot drawing, down drawing, fusion down drawing, up drawing, or float. In some embodiments, the ribbons can include the ribbons described above with respect to Figure 1 and 4-5. Two exemplary methods of processing the strip are discussed below. The first exemplary method includes immersing the strip in a bath containing sodium and / or potassium. The second exemplary method includes placing a salt solution on a central portion of the first major surface and the second major surface before heating the strip.

[0212] The method of processing a strip may include masking a first portion of the strip and masking a second portion of the strip, such as Fig. 20 As shown. A first mask 2003 may be disposed on a first portion 521 of the strip 501 to establish a first masked portion. The first masked portion may include a first surface area 537 of the first major surface 403 and a second surface area 527 of the second major surface 405. In some embodiments, as shown, the first masked portion may include a third edge 415 of the strip 501. In some embodiments, the first masked portion may include a first edge portion of the first edge and / or a first edge portion of the second edge. A second mask 2001 may be disposed on a second portion 523 of the strip 501 to establish a second masked portion. The second masked portion may include a third surface area 539 of the first major surface 403 and a fourth surface area 529 of the second major surface 405. In some embodiments, as shown, the second masked portion may include a fourth edge 417 of the strip. In some embodiments, the second masked portion may include a second edge portion of the first edge and / or a second edge portion of the second edge.

[0213] In some embodiments, the first mask and / or the second mask may include one or more of silicon dioxide, aluminum oxide, titanium dioxide, aluminum nitride, silicon oxynitride, magnesium oxide, and zirconium oxide. In other embodiments, the first mask and / or the second mask may inhibit (e.g., prevent) ions from penetrating (e.g., diffusing) through the material of the mask. In other embodiments, masking the first portion and masking the second portion may each include: setting one or more of silicon dioxide, aluminum oxide, titanium dioxide, aluminum nitride, silicon oxynitride, magnesium oxide, and zirconium oxide. The first mask and / or the second mask may be set using a coating technique, such as physical vapor deposition (PVD), chemical vapor deposition (CVD), plasma enhanced chemical vapor deposition (PECVD), and atomic layer deposition (ALD). PVD techniques may include sputtering techniques, ion-assisted electron beam (IAD-EB), thermal evaporation, ion beam, and / or laser ablation. Mechanical polishing (e.g., grinding) and / or chemical etching may be used to remove the first mask. Chemical etching may include contacting the first mask and / or the second mask with one or more inorganic acids (e.g., HCl, HF, H2SO4, HNO3). In some embodiments, the first mask and / or the second mask may include a tape or a polymer. In other embodiments, the first mask and / or the second mask may be easily removed.

[0214] The method of processing a ribbon may include chemically strengthening a central portion of the first major surface 403 and a central portion 541 of the second major surface 405 after placing a first mask 2003 on the first portion 521 and placing a second mask 2001 on the second portion 523. Chemical strengthening of a ribbon (e.g., a glass-based ribbon, a ceramic-based ribbon) may be achieved by ion exchange, which occurs when a first cation within a certain depth in the outer surface of the glass-based ribbon is exchanged with a second cation having a larger radius than the first cation. For example, lithium cations within a certain depth in the surface of the glass-based ribbon may be exchanged with sodium cations or potassium cations. As a result, since the radius of the lithium cations is smaller than the radius of the sodium cations or potassium cations being exchanged, the surface of the glass-based ribbon is in a compressed state and is thereby chemically strengthened by the ion exchange process.

[0215] Chemically strengthening the central portion of the strip may obtain a first central compressive stress zone extending from the first major surface of the strip to a first central compression depth. Chemically strengthening the central portion of the strip may obtain a second central compressive stress zone extending from the second major surface of the strip to a second central compression depth. As described above, the central portion may include a width within the range described above with respect to the width of the central portion. As described above, the central portion may be located between the first portion and the second portion. The first central compression depth and / or the second central compression depth may be within the range described above with respect to the first central compression depth and / or the second central compression depth. The maximum compressive stress that the first central compressive stress zone may include and / or the maximum compressive stress that the second central compressive stress zone may achieve may be within the range described above with respect to the maximum compressive stress of the first central compressive stress zone and / or the second central compressive stress zone of the strip. In some embodiments, the maximum compressive stress of the first central compressive stress zone may be substantially equal to the maximum compressive stress of the second central compressive stress zone. In some embodiments, the maximum compressive stress of the first central compressive stress zone may be less than the maximum compressive stress of the second central compressive stress zone. In some embodiments, the maximum compressive stress of the first central compressive stress zone may be greater than the maximum compressive stress of the second central compressive stress zone. In some embodiments, as described above with respect to the first central compressive stress region and / or the second central compressive stress region, the first central compressive stress region and / or the second central compressive stress region may be enriched with sodium and / or potassium.

[0216] In a first exemplary method of processing a strip, as Figure 20-21As shown, before chemically strengthening the strip, a first mask 2003 is placed on the first portion and a second mask 2001 is placed on the second portion 523. Chemically strengthening the strip may include immersing the strip in a salt solution 1803 contained in a salt bath 1801. In some embodiments, the salt solution 1803 may be similar to the above-referenced methods in terms of composition, temperature, and / or the time that the foldable substrate (e.g., strip) can be in contact with the salt solution 1803. Fig.18 After the strip has been immersed in the salt solution 1803, as Fig.21 As shown, the strip may include a chemically strengthened center portion 541 between a masked (and therefore unstrengthened) first portion 521 and a second portion 523. The first exemplary method may also include demasking each of the first portion 521 and the second portion 523 by removing the first mask 2003 and the second mask 2001 to provide a Figure 4-7 and the strip 501 shown in 10-11.

[0217] In a second exemplary method of processing a strip, as Fig. 20 As shown, before chemically strengthening the strip 501, the first mask 2003 is set on the first portion 521 and the second mask 2001 is set on the second portion 523. Fig.23 As shown, chemically strengthening the strip 501 may include: disposing a salt solution 2303 from a source 2301 on a central portion 541 at the first major surface 403. The salt solution 2303 may be cured to produce a first salt deposit 2401. In addition, chemically strengthening the strip 501 may include: disposing a salt solution from a source 2301 on a central portion at the second major surface 405. The salt solution 2303 on the central portion at the second major surface 405 may be cured to produce a second salt deposit 2403 located opposite the first salt deposit 2401. In some embodiments, the source 2301 may include a conduit (e.g., a flexible tube, a micropipette, or a syringe), a nozzle, or a container (e.g., a beaker).

[0218] The salt solution 2303 may include an organic binder or solvent. The organic binder may include one or more of cellulose, cellulose derivatives, hydrophobically modified ethylene oxide polyurethane modifiers (HUER) and ethylene acrylic acid. Examples of cellulose derivatives include ethyl cellulose, methyl cellulose and AQUAZOL (poly 2 ethyl-2 oxazine). The solvent may include a polar solvent (e.g., water, alcohol, acetate, acetone, formic acid, dimethylformamide, acetonitrile, dimethyl sulfoxide, nitromethane, propylene carbonate, poly (ether ether ketone)) and / or a non-polar solvent (e.g., pentane, 1,4-dioxane, chloroform, dichloromethane, ether, hexane, heptane, benzene, toluene, xylene). In some embodiments, by removing the solvent and / or organic binder, the salt solution may be solidified to form the first salt deposit 2401 and / or the second salt deposit 2403. In other embodiments, the solvent and / or organic binder can be removed by drying the salt solution 2303 at room temperature (about 20° C. to about 30° C.) for 8 hours or more. In other embodiments, the solvent and / or organic binder can be removed by drying the salt solution 2303 at a temperature of about 100° C. to about 140° C., or about 100° C. to about 120° C. for about 8 minutes to about 30 minutes, or about 8 minutes to about 20 minutes, or about 8 minutes to about 15 minutes. In some embodiments, the salt solution 2303 may include one or more of potassium nitrate, potassium phosphate, potassium chloride, potassium sulfate, sodium chloride, sodium sulfate, and / or sodium nitrate. In other embodiments, the salt solution may include potassium nitrate and potassium phosphate.

[0219] In a second exemplary method of processing a strip, first portion 521 and second portion 523 may be unmasked by removing first mask 2003 and second mask 2001, leaving first salt deposit 2401 and second salt deposit 2403 on opposite surfaces (e.g., first major surface 403, second major surface 405) of central portion 541 of strip 501, as shown in FIG. Fig.24 The first portion 521 and the second portion 523 may be demasked and then Fig.25 The ribbon 501 is shown heated to establish a first central compressive stress region and / or a second central compressive stress region. In other embodiments, the mask may remain on during heating.

[0220] In some embodiments, Fig.25As shown, the strip 501 may be placed in the furnace 2501. In some embodiments, the strip 501 may be heated at a temperature of greater than or equal to about 300° C., greater than or equal to about 360° C., greater than or equal to about 400° C., less than or equal to about 500° C., less than or equal to about 460° C., or less than or equal to about 400° C. In some embodiments, the strip 501 may be heated at a temperature in the following ranges: about 300° C. to about 500° C., about 360° C. to about 500° C., about 400° C. to about 500° C., about 300° C. to about 460° C., about 360° C. to about 460° C., about 400° C. to about 460° C., about 300° C. to about 400° C., about 360° C. to about 400° C., or any range or sub-range therebetween. In some embodiments, the ribbon 501 may be heated for a duration of about 15 minutes or more, about 1 hour or more, about 3 hours or more, about 48 hours or less, about 24 hours or less, or about 8 hours or less. In some embodiments, a portion of the ribbon 501 may be heated for a duration in the range of about 15 minutes to about 48 hours, about 1 hour to about 48 hours, about 3 hours to about 48 hours, about 15 minutes to about 24 hours, about 1 hour to about 24 hours, about 3 hours to about 48 hours, about 3 hours to about 24 hours, about 3 hours to about 48 hours, about 3 hours to about 24 hours, about 3 hours to about 8 hours, or any range or sub-range therebetween.

[0221] After the strip is heated, Fig.26 As shown, the strip may include a chemically strengthened center portion 541 between the first portion 521 and the second portion 523. The second exemplary method may further include removing the first salt deposit 2401 and the second salt deposit 2403. In some embodiments, as Fig.26 As shown, removing the first salt deposit 2401 and the second salt deposit 2403 may include: sweeping the tool 2601 across the surface (e.g., the first major surface 403, the second major surface 405) in the direction 2603. In other embodiments, using the tool may include: scraping, grinding, pushing, etc. In some embodiments, the first salt deposit 2401 and the second salt deposit 2403 may be removed by washing the surface (e.g., the first major surface 403, the second major surface 405) with a solvent.

[0222] Example

[0223] Each embodiment is further illustrated by the following examples. Examples AJ all include a substrate or tape containing a glass-based material (Composition 1, in mole %, having the following nominal composition: 63.6SiO2; 15.7Al2O3; 10.8Na2O; 6.2Li2O; 1.16ZnO; .04SnO2 and 2.5P2O5). Example AE is prepared by ion exchanging the first portion, the second portion and the central portion to the compression depths of the first major surface, the central surface area and the second major surface described in Tables 1 and 2. Table 1 records the maximum compressive stress and the maximum tensile stress in the first portion of Example AE. Table 2 records the maximum compressive stress and the maximum tensile stress in the central portion of Example AE. Lower effective minimum bend radius values ​​are associated with increased foldability. Higher pen drop heights are associated with increased impact resistance. The experimental results of the pen drop test of Example AE were conducted in a region including the thickness of the substrate. Table 3 records the mechanical properties of Example AE. Table 4 presents the minimum bend radius obtained for different tape thicknesses of Example FG.

[0224] Example A includes a uniform thickness of 25 μm across the length and width of the glass-based substrate. Example A is chemically strengthened to achieve a uniform compression depth of 6 μm and an associated maximum tensile stress of 354 MPa. Example A exhibits an effective minimum bend radius of 1.2 mm and a pen drop height of 15 cm.

[0225] Example B includes a glass-based substrate of the same composition as Example A, and includes a uniform thickness of 50 μm across the length and width of the glass-based substrate. Example B is chemically strengthened to achieve a uniform compression depth of 9.7 μm and an associated maximum tensile stress of 235 MPa. Example B exhibits an effective minimum bend radius of 2.5 mm and a pen drop height of 10 cm.

[0226] Example C includes a glass-based substrate of the same composition as Example A, and includes a uniform thickness of 125 μm across the length and width of the glass-based substrate. Example C is chemically strengthened to achieve a uniform compression depth of 21.2 μm and an associated maximum tensile stress of 226 MPa. Example C exhibits an effective minimum bend radius of 6.2 mm and a pen drop height of 25 cm.

[0227] Example D includes a glass-based substrate having the same composition as Example A, which is manufactured according to an embodiment of the present disclosure. The first and second portions include a substrate thickness of 150 μm, while the center portion includes a center thickness of 30 μm. Example D is chemically strengthened to obtain a uniform compression depth of 5.5 μm, which corresponds to a maximum tensile stress of 37 MPa in the first portion and a maximum tensile stress of 223 MPa in the center portion. Example D exhibits an effective minimum bending radius of 1.7 mm and a pen drop height of 80 cm.

[0228] Example E includes a glass-based substrate made according to an embodiment of the present disclosure. The first and second portions include a substrate thickness of 150 μm, while the center portion includes a center thickness of 50 μm. Example E was chemically strengthened to obtain a uniform compression depth of 9.7 μm. Example E exhibited an effective minimum bend radius of 2.5 mm and a pen drop height of 80 cm.

[0229] Table 1: Properties of the first part of Examples AE

[0230]

[0231] Table 2: Properties of the central portion of Examples AE

[0232]

[0233] Table 3: Mechanical properties of Examples AE

[0234]

[0235]

[0236] Embodiments AC all include a first portion maximum tensile stress greater than or equal to about 200 MPa, i.e., 354 MPa, 235 MPa, and 226 MPa, respectively. Embodiments AC all have a high energy failure mode. In contrast, embodiment DE includes a first portion maximum tensile stress less than about 100 MPa, i.e., 37 MPa and 68 MPa, respectively. Embodiments DE have a low energy failure mode. Therefore, providing a first portion and / or second portion maximum tensile stress less than or equal to about 100 MPa can be associated with a low energy failure mode.

[0237] Examples AC demonstrate that increasing substrate thickness is associated with increasing the effective minimum bend radius. However, Example D includes an effective minimum bend radius of 1.7 mm, which is between the effective minimum bend radius of Example A (1.2 mm for a substrate thickness of 25 μm) and the effective minimum bend radius of Example B (2.5 μm for a substrate thickness of 50 μm). Example E achieves substantially the same effective minimum bend radius as Example B, and the substrate thickness of Example B is substantially equal to the center thickness of Example E. Therefore, by reducing the center thickness of a glass-based substrate while maintaining a predetermined substrate thickness, the effective minimum bend radius can be reduced. Providing a center thickness that is less than the substrate thickness can be associated with better bending performance (e.g., a lower effective minimum bend radius) than a glass-based substrate comprising a uniform thickness.

[0238] As described above, the impact resistance based on the pen drop height recorded in Table 3 is performed with the pen only dropping in an area (e.g., the first portion) that includes the thickness of the substrate. Therefore, locations within the center portion (e.g., the first transition portion, the center portion, the second transition portion) are not used for the data recorded in Table 3. Examples AC demonstrate a non-uniform trend in impact resistance. Examples AC still all have a pen drop height of less than or equal to about 25. In contrast, Example DE has a pen drop height of about 80 cm. This demonstrates that the thickness of the center portion does not significantly affect the impact resistance of the glass-based substrate when tested in an area that includes the thickness of the substrate. On the contrary, by increasing the substrate thickness while maintaining a constant center thickness, enhanced impact resistance can be obtained.

[0239] Example F includes a glass-based ribbon that has not been chemically strengthened. Therefore, the glass-based ribbon of Example F includes neither a compressive stress region at the first major surface nor a compressive stress region at the second major surface. As shown in Table 4, for a ribbon thickness of 50 μm or greater, the glass-based ribbon cannot achieve a minimum bend radius of 10 mm.

[0240] Example G includes chemically strengthening a central portion of a glass-based ribbon according to an embodiment of the present disclosure to include a first compressive stress region and a second compressive stress region, wherein the first compressive stress region includes a maximum compressive stress of about 1200 MPa and the second compressive stress region includes a maximum compressive stress of about 1200 MPa. As shown in Example G in Table 4, all ribbon thicknesses examined exhibited a minimum bend radius of about 1 mm to about 10 mm (e.g., about 1 mm to about 8 mm, about 1.2 mm to about 7.5 mm). Example G can achieve a minimum bend radius that is about 7 times to about 8 times smaller than the minimum bend radius that can be achieved by Example F. For example, at a ribbon thickness of 25 μm, Example G achieves a minimum bend radius of 1.2 mm, while Example F achieves a minimum bend radius of 9.3 mm (7.75 times larger than the minimum bend radius of Example G). Similarly, at a ribbon thickness of 150 μm, Example G achieves a minimum bend radius of 7.5 mm, while Example F achieves a minimum bend radius of 56 mm (7.46 times larger than the minimum bend radius of Example G). Thus, providing a glass-based ribbon including a central portion and the central portion including a compressive stress region can achieve a smaller minimum bend radius than a glass-based ribbon without such a compressive stress region.

[0241] Table 4: Minimum bending radius of glass-based ribbons

[0242]

[0243] Example H includes a glass-based ribbon that has been chemically strengthened such that the glass-based ribbon includes a first compressive stress region and a second compressive stress region, wherein the first compressive stress region includes the entire first major surface and the second compressive stress region includes the entire second major surface. The first compressive stress region includes a maximum compressive stress of 1,200 MPa. The second compressive stress region includes a maximum compressive stress of 1,200 MPa. The sample of Example H includes a thickness of either 50 μm or 100 μm.

[0244] Example I includes a sample according to Example G and including a thickness of either 50 μm or 100 μm. Example HI is analyzed using the above-described pen drop test. For a sample including a thickness of 100 μm, Example H includes a failed pen drop height that is about 30% of the failed pen drop height of Example I. For a sample including a thickness of 50 μm, Example H includes a failed pen drop height that is about 20% of the failed pen drop height of Example I. Without wishing to be bound by theory, chemically strengthening the entire first major surface and the entire second major surface may create and / or exacerbate surface defects and increase overall surface roughness. Comparison of Example HI demonstrates that chemically strengthening a portion of the first major surface outside the central region (e.g., the curved region) may be associated with reduced pen drop performance (e.g., impact resistance, puncture resistance). Therefore, providing a glass-based ribbon that is not chemically strengthened (e.g., stress-free, including a layer depth of 0% to about 5% of the ribbon thickness, including a surface roughness of less than or equal to about 0.3 nm) can provide a technical benefit of improved impact resistance and / or puncture resistance.

[0245] Example J includes a sample prepared according to Example G, the sample including a thickness of 100 μm, a length of 20 mm, and a maximum compressive stress value of the first compressive stress region and the second compressive stress region of either 7,00 MPa or 1,200 MPa. The maximum warp was measured using a simulated out-of-plane warp distribution. For the sample including a maximum compressive stress of 700 MPa, the maximum warp was measured to be about 0.4 μm. For the sample including a maximum compressive stress of 1,200 MPa, the maximum warp was shown to be about 0.6 μm. Therefore, the glass-based ribbon according to embodiments of the present disclosure can achieve a maximum warp of less than or equal to about 2 mm (e.g., about 10 nm to about 2 μm, about 100 nm to about 1 μm).

[0246] The above phenomena can be combined to provide a foldable device, which includes a foldable substrate having a low effective minimum bending radius, high impact resistance and low fracture energy failure. The foldable substrate and the tape can provide a small effective minimum bending radius, while providing excellent impact resistance and puncture resistance, and low energy fracture. The device of the present disclosure may include a first portion and a second portion and have a substrate thickness. The substrate thickness can be large enough (e.g., about 80 μm to about 2 mm) to provide excellent impact resistance and excellent puncture resistance.

[0247] The apparatus of the present disclosure may include attaching the first portion to the central portion of the second portion. In particular, embodiments of the present disclosure may provide a central portion including a central tensile stress region, which may be located between a first central compressive stress region and a second central compressive stress region. In some embodiments, the maximum tensile stress of the central tensile stress region may be greater than the maximum tensile stress of the first tensile stress region in the first portion and / or the maximum tensile stress of the second tensile stress region in the second portion. In some embodiments, the first portion and / or the second portion may be substantially unstrengthened (e.g., stress-free, chemically unstrengthened, thermally unstrengthened), and substantially have no tensile stress region or have a small magnitude of maximum tensile stress. The central maximum tensile stress provided is greater than the first maximum tensile stress of the first tensile stress region (if provided) and / or the second maximum tensile stress of the second tensile stress region (if provided), thereby making the fracture caused by impact in the first portion and / or the second portion a low energy fracture, while providing excellent folding performance. In some embodiments, the low energy fracture may be the result of a reduced thickness of the central portion, and for a given maximum tensile stress, the reduced thickness central portion stores less energy than a thicker glass portion. In some embodiments, the low energy fracture can be the result of fracture of the first portion and / or the second portion away from the central portion undergoing bending, wherein the first portion and / or the second portion comprises a lower maximum tensile stress than the central portion. Providing a central maximum tensile stress greater than the first maximum tensile stress of the first tensile stress region (if provided) and / or the second maximum tensile stress of the second tensile stress region (if provided) can provide excellent impact resistance and / or fracture resistance in the first portion and / or the second portion, which is indicated by excellent pen drop performance, as described below.

[0248] The device of the present disclosure may include a central portion attaching the first portion to the second portion. The central portion may include a central thickness that is less than the thickness of the substrate. The central thickness may be sufficiently small (e.g., about 10 μm to about 125 μm) to be in the bending region of the foldable device and to provide a low effective minimum bending radius (e.g., less than or equal to about 10 mm, or less than or equal to about 9 mm, or less than or equal to about 8 mm, or less than or equal to about 7 mm, or less than or equal to about 6 mm, or less than or equal to about 5 mm, or less than or equal to about 4 mm, or less than or equal to about 3 mm, less than or equal to about 2 mm, about 1 mm). As shown by Fig.14As indicated by the surprising results of the presented pen drop test, glass-based substrates comprising a thickness of less than or equal to about 50 μm provide excellent pen drop performance, while a thickness of about 50 μm to about 80 μm provides poor pen drop performance. Further, in some embodiments, providing a substantially uniform compression depth associated with a compressive stress region of a foldable substrate can simplify the manufacture of the article by avoiding the use of masking or other non-uniform ion exchange methods.

[0249] The strip according to the disclosed embodiments includes a center portion including a first center compressive stress zone extending to a first center compression depth, and a second center compressive stress zone extending to a second compression depth, the strip can achieve a small minimum bend radius (e.g., less than or equal to about 10 mm) because the compressive stress zone (e.g., from chemical strengthening) can counteract the bending-induced tensile forces. Further, providing a first center compression depth and / or a second center compression depth in the range of about 10% to about 30% of the thickness of the strip can achieve a small minimum bend radius. Similarly, a center portion including a first center layer depth and / or a second center layer depth greater than or equal to about 10% can achieve a small minimum bend radius. Providing a first edge portion of the center region having a compressive stress zone, compression depth, and / or layer depth and / or a second edge portion of the center region can further achieve a small minimum bend radius by reducing damage (e.g., fracture and / or cracking) due to bending-induced stresses. In some embodiments, the maximum compressive stress of the first central compressive stress region can be substantially equal to the maximum compressive stress of the second central compressive stress region, which can provide a ribbon with low warpage (e.g., less than or equal to about 2 nm, less than or equal to about 1 nm). In some embodiments, providing a central portion having a width of about 5 times the minimum bending radius (e.g., a width of about 5 mm to about 55 mm) can achieve a small minimum bending radius by reducing (e.g., avoiding) stress concentration and damage along the bending length of the ribbon when it is at or near the minimum bending radius. At the same time, the first portion and / or the second portion can achieve excellent impact resistance and / or puncture resistance. In some embodiments, the first portion and / or the second portion can include a surface roughness of less than or equal to about 0.3 nanometers at the first major surface and / or the second major surface. The smoothness of the surface in the first portion and / or the second portion (e.g., low surface roughness) can minimize defects in the surface, which can reduce the incidence of ribbon damage (e.g., fracture and / or cracking). In some embodiments, the first portion and / or the second portion may include a layer depth that is 0% to about 5% of the thickness of the glass-based tape from the first major surface and / or the second major surface. In some embodiments, the first portion and / or the second portion may include a stress-free area at the first major surface and / or the second major surface. The lack of significant chemical strengthening and / or compressive stress at the surface of the first portion and / or the second portion can minimize the occurrence of defects in the surface, which can reduce the incidence of damage to the tape (e.g., fractures and / or cracks). When the tape is part of a foldable device that includes an optically clear adhesive, matching the refractive index of the optically clear adhesive to the refractive index of the glass-based tape (e.g., within about 0.1) can minimize optical distortion in the foldable device.

[0250] Directional terms used herein—eg, up, down, left, right, front, back, top, bottom—are used only with reference to the drawings in which they are drawn and are not intended to imply an absolute orientation.

[0251] It should be understood that each disclosed embodiment may relate to features, elements or steps described in conjunction with the embodiments. It should also be understood that, although described in the form of one embodiment, features, elements or steps may be interchanged or combined with alternative embodiments in various unillustrated combinations or arrangements.

[0252] It should also be understood that the terms "the," "an," or "an" as used herein mean "at least one" and should not be limited to "only one" unless clearly indicated to the contrary. For example, reference to "a component" includes embodiments having two or more such components, unless the context clearly indicates otherwise. Similarly, "plurality" is intended to mean "more than one."

[0253] As used herein, the term "about" refers to that the amount, size, formula, parameter and other quantities and features are not precise and need not be precise, but may be approximate and / or larger or smaller as required, such as reflecting tolerances, conversion factors, rounding, measurement errors, etc., and other factors known to those skilled in the art. Herein, the range can be expressed as starting from "about" one specific value and / or ending at "about" another specific value. When expressing such a range, the embodiment includes starting from a specific value and / or ending at another specific value. Similarly, when the antecedent "about" is used to express a numerical value as an approximation, it should be understood that the specific value constitutes another embodiment. Regardless of whether the numerical value or endpoint of the range in the specification is stated using "about", the numerical value or endpoint of the range is intended to include two embodiments: one modified with "about" and the other not modified with "about". It should also be understood that the endpoint of each range is important in relation to and independently of the other endpoint.

[0254] As used herein, the terms "substantially," "substantially," and variations thereof are intended to mean that the feature being described is equal to or approximately equal to a value or description. For example, a "substantially planar" surface is intended to mean a planar or substantially planar surface. Additionally, as defined above, "substantially similar" is intended to mean that two values ​​are equal or approximately equal. In some embodiments, "substantially similar" can mean values ​​that are within about 10% of each other, such as within about 5% of each other, or within about 2% of each other.

[0255] Unless otherwise stated, it is not intended that any method described herein be construed as requiring that its steps be performed in a specific order. Therefore, when a method claim does not actually state that its steps follow a certain order or it does not specifically indicate in any other way in the claims or description that the steps are limited to a specific order, it is not intended to imply any particular order.

[0256] Although the use of the transitional term "comprising" may disclose various features, elements, or steps of a particular embodiment, it should be understood that this implies alternative embodiments including those that may be described using the transitional terms "consisting of" or "consisting essentially of." Thus, for example, implied alternative embodiments of a device comprising A+B+C include embodiments in which the device consists of A+B+C and embodiments in which the device consists essentially of A+B+C. Unless otherwise noted, the terms "comprising" and "including" and variations thereof as used herein should be interpreted as being synonymous and open ended.

[0257] The above embodiments and features of these embodiments are exemplary and may be provided alone or in any combination with any one or more features of other embodiments provided herein without departing from the scope of the present disclosure.

[0258] It is obvious to those skilled in the art that various modifications and changes can be made to the present disclosure without departing from the scope and spirit of the present disclosure. Therefore, the present disclosure is intended to cover modifications and changes of the embodiments herein, as long as these modifications and changes are within the scope of the appended claims and their equivalents.

Claims

1. A strip material, comprising: a strip thickness defined between a first major surface and a second major surface opposite the first major surface; a first portion, the first portion comprising a first layer depth from 0% to 5% of the strip thickness from the first major surface and a second layer depth from 0% to 5% of the strip thickness from the second major surface, wherein the first portion comprises the strip thickness; a second portion including a third layer depth from 0% to 5% of the strip thickness from the second major surface and a fourth layer depth from 0% to 5% of the strip thickness from the second major surface, wherein the second portion includes the strip thickness; and a central portion, the central portion comprising: a first central layer depth greater than or equal to 10% of the strip thickness from the first major surface, a first central compressive stress zone extending from the first major surface to the first central compression depth, a second central layer depth greater than or equal to 10% of the strip thickness from the second major surface, and a second central compressive stress zone extending from the second major surface to the second central compression depth, wherein the central portion is located between the first portion and the second portion in the direction of the strip length, wherein the central portion includes a first central surface area opposite the second major surface, wherein the central portion includes a central thickness defined between the first central surface area and the second major surface, and wherein the central thickness is less than the strip thickness.

2. The strip according to claim 1, wherein: The first central compression depth is 10% to 30% of the strip thickness.

3. The strip of claim 1 further comprising a width defined between a first edge of the strip and a second edge of the strip opposite the first edge, the first edge extending between the first major surface and the second major surface, the second edge extending between the first major surface and the second major surface, and the first central compressive stress zone and the second central compressive stress zone each extending from the first edge to the second edge.

4. The strip of claim 1, further comprising: a first tensile stress region between the first compressive stress region and the second compressive stress region, the first tensile stress region comprising a first maximum tensile stress; a second tensile stress region between the third compressive stress region and the fourth compressive stress region, the second tensile stress region comprising a second maximum tensile stress; as well as a central tensile stress region between the first central compressive stress region and the second central compressive stress region, the central tensile stress region comprising a central maximum tensile stress, The central maximum tensile stress is greater than the first maximum tensile stress, and the central maximum tensile stress is greater than the second maximum tensile stress.

5. The strip of any one of claims 1-4, further comprising a central tensile stress region between the first central compressive stress region and the second central compressive stress region, the central tensile stress region comprising a central maximum tensile stress of 10 MPa to 375 MPa.

6. The strip material according to any one of claims 1 to 4, wherein: The strip includes a minimum bend radius of less than 10 mm.

7. The strip according to claim 6, wherein The strip achieved a bending radius of 5 mm.

8. The strip according to claim 6, wherein The length of the center portion in the strip length direction is 5 times or more the minimum bending radius.

9. The strip material according to any one of claims 1 to 4, wherein: The length of the central portion in the length direction of the strip is in the range of 5 mm to 55 mm.

10. The strip material according to any one of claims 1 to 4, wherein: The strip thickness ranged from 25 microns to 150 microns.

11. The strip material according to any one of claims 1 to 4, wherein: The ribbon exhibits a warp of 10 nanometers to 2 micrometers relative to a first plane defined by the first major surface.

12. The strip material according to any one of claims 1 to 4, wherein: The ribbon includes a glass-based material.

13. The strip material according to any one of claims 1 to 4, wherein: The strip thickness is greater than 80 microns and less than or equal to 2 millimeters; and wherein the center thickness is in the range of 10 microns to 50 microns.

14. A foldable device comprising: The strip material according to any one of claims 1 to 4; Optically clear adhesives; and A release liner wherein the optically clear adhesive is located between the tape and the release liner.

15. A consumer electronic product comprising: a housing, the housing comprising a front surface, a rear surface and side surfaces; an electrical component at least partially located within the housing, the electrical component including a controller, a memory, and a display, the display being located at or near a front surface of the housing; as well as At least one of a cover substrate disposed above a display, a portion of a housing, or the cover substrate comprises the tape material according to any one of claims 1-4.

16. A method of processing a strip material, the strip material comprising a strip thickness defined between a first major surface and a second major surface opposite the first major surface, the method comprising: masking a first portion of the strip, the first portion comprising a first surface region of a first major surface of the strip and a second surface region of a second major surface of the strip opposite the first major surface, wherein the first portion comprises a thickness of the strip; masking a second portion of the tape, the second portion comprising a third surface region of the first major surface and a fourth surface region of the second major surface, wherein the second portion comprises a tape thickness; and A central portion of the strip is chemically strengthened to achieve a first central compressive stress zone extending from a central portion of the first major surface to a first central compression depth and a second central compressive stress zone extending from a central portion of the second major surface to a second central compression depth, wherein the central portion of the strip is located between the first portion and the second portion, and wherein the central portion includes a first central surface region opposite the second major surface, wherein the central portion includes a central thickness defined between the first central surface region and the second major surface, and wherein the central thickness is less than the strip thickness.

17. The method of claim 16, wherein: Chemical strengthening includes: disposing a saline solution on the central portion at the first major surface; disposing a saline solution on the central portion at the second major surface; and The strip is heated at a temperature of 300°C to 500°C for a period of 15 minutes to 12 hours.

18. The method of claim 17, wherein: Prior to heating the strip, each of the first portion and the second portion is demasked.

19. The method of claim 17, wherein: The salt solution includes an organic binder, potassium nitrate and potassium phosphate.

20. The method of any one of claims 16 to 19, wherein: The first central compression depth is 10% to 30% of the strip thickness.

21. The method of any one of claims 16 to 19, wherein: The length of the central portion of the strip in the strip length direction is in the range of 5 mm to 55 mm.

22. The method of any one of claims 16 to 19, wherein: The strip thickness is greater than 80 microns and less than or equal to 2 millimeters; and wherein the center thickness is in the range of 10 microns to 50 microns.