A densely graded extra-large particle size asphalt crushed stone mixture and pavement structure
By preparing a dense-graded extra-large aggregate asphalt macadam mixture with a nominal maximum particle size of 53mm, the problem of the limited thickness of the flexible base course in the existing technology has been solved, enabling large-thickness paving and efficient construction, and improving the overall quality and service life of the pavement structure.
Patent Information
- Application Number
- CN202210289475.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-03-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-03-23
AI Technical Summary
In existing technologies, the nominal maximum aggregate size of dense-graded asphalt stabilized crushed stone mixtures is limited, which means that when the thickness of the flexible base course exceeds 120mm, it needs to be laid in layers, increasing the bonding interface and construction time, and affecting construction efficiency and quality.
A dense-graded extra-large particle size asphalt macadam mixture is prepared by mixing binder, aggregate and filler. The nominal maximum particle size of the aggregate is 53mm, the gradation range of the mixture is the passing rate of a specific sieve, and the filler is limestone powder. It is suitable for the construction of flexible base courses with greater thickness.
It achieves a flexible base layer thickness of over 150mm in a single paving, reduces the bonding interface, improves construction efficiency, ensures the quality of asphalt pavement, and enhances the overall load-bearing capacity, fatigue resistance, and rutting resistance of the pavement through a multi-layer structure, thus extending its service life.
Smart Images

Figure CN114635328B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of road engineering, in particular to a dense-graded extra-large-size asphalt macadam mixture and a road surface structure. Background Art
[0002] The flexible base in the asphalt pavement structure is used to transfer the traffic load on the surface layer to the semi-rigid base or roadbed, and plays the role of transferring the upper load and modulus gradient transition. The most common flexible base is dense-graded asphalt mixture or dense-graded and semi-open-graded asphalt stabilized macadam mixture. Among the dense-graded asphalt stabilized macadam mixture, the maximum nominal particle size of the extra-coarse ATB-40 aggregate is the largest, which is 37.5mm. However, according to the requirement that the maximum paving thickness of the asphalt pavement structure layer does not exceed 3 times the nominal maximum particle size of the aggregate, even if the extra-coarse ATB-40 dense-graded asphalt stabilized macadam mixture is used as the flexible base, its paving thickness cannot exceed 120mm, resulting in the need for layered paving when the thickness of the flexible base is greater than 120mm, which increases the number of bonding interfaces and construction time, affecting the construction efficiency and the quality of the asphalt pavement structure. Since increasing the aggregate particle size will make it difficult to adjust the gradation, segregation is likely to occur during paving. Therefore, the prior art has not yet obtained an extra-large particle size asphalt stabilized macadam mixture with a larger nominal maximum particle size. Summary of the invention
[0003] The technical task of the present invention is to provide a dense-graded extra-large particle size asphalt crushed stone mixture to address the deficiencies of the above-mentioned prior art, which can achieve construction paving of greater thickness, reduce the bonding interface of the asphalt pavement structure and the construction period, and improve the overall quality of the flexible base.
[0004] A further technical task of the present invention is to provide a pavement structure.
[0005] The technical task of the present invention is achieved in the following way: a dense-graded extra-large particle size asphalt crushed stone mixture is formed by heating and mixing a binder, an aggregate and a filler, wherein the binder is 70# matrix asphalt or SBS modified asphalt; the nominal maximum particle size of the aggregate is 53mm, and the gradation range of the mixture is: the pass rate range of the standard sieve hole 63mm is 100%, the pass rate range of the standard sieve hole 53mm is 90-100%, the pass rate range of the standard sieve hole 37.5mm is 80-93%, the pass rate range of the standard sieve hole 31.5mm is 70-87%, the pass rate range of the standard sieve hole 26.5mm is 60-80%, the pass rate range of the standard sieve hole 19mm is 45-70%, and the pass rate range of the standard sieve hole 26.5mm is 60-80%. The pass rate of the standard sieve hole 16mm is 42-60%, the pass rate of the standard sieve hole 13.2mm is 35-54%, the pass rate of the standard sieve hole 9.5mm is 29-49%, the pass rate of the standard sieve hole 4.75mm is 20-40%, the pass rate of the standard sieve hole 2.36mm is 15-32%, the pass rate of the standard sieve hole 1.18mm is 10-25%, the pass rate of the standard sieve hole 0.6mm is 8-18%, the pass rate of the standard sieve hole 0.3mm is 5-14%, the pass rate of the standard sieve hole 0.15mm is 3-10%, and the pass rate of the standard sieve hole 0.075mm is 2-6%; the filler is lime ore powder and / or quicklime.
[0006] As a preferred range, the gradation of the mixture is: the pass rate of the standard sieve hole 63mm is 100%, the pass rate of the standard sieve hole 53mm is 93-98%, the pass rate of the standard sieve hole 37.5mm is 83-90%, the pass rate of the standard sieve hole 31.5mm is 74-82%, the pass rate of the standard sieve hole 26.5mm is 67-73%, the pass rate of the standard sieve hole 19mm is 52-62%, the pass rate of the standard sieve hole 16mm is 47-55%, the pass rate of the standard sieve hole 13.2mm is 40 ~50%, the pass rate of standard sieve hole 9.5mm ranges from 34 to 45%, the pass rate of standard sieve hole 4.75mm ranges from 25 to 35%, the pass rate of standard sieve hole 2.36mm ranges from 20 to 27%, the pass rate of standard sieve hole 1.18mm ranges from 13 to 21%, the pass rate of standard sieve hole 0.6mm ranges from 10 to 15%, the pass rate of standard sieve hole 0.3mm ranges from 7 to 12%, the pass rate of standard sieve hole 0.15mm ranges from 5 to 8%, and the pass rate of standard sieve hole 0.075mm ranges from 3 to 5.5%.
[0007] The 53mm standard sieve and 63mm standard sieve have the same structure as the existing standard sieves used in road engineering, the only difference is that the sieve hole sizes are 53mm and 63mm respectively.
[0008] Preferably, the aggregate of the present invention is limestone, basalt, or hard rock.
[0009] Preferably, the aggregate mix ratio is: aggregate with maximum particle size of 63mm: aggregate with maximum particle size of 43mm: aggregate with particle size of 15-20mm: aggregate with particle size of 10-15mm: aggregate with particle size of 5-10mm: aggregate with particle size of 3-5mm: aggregate with particle size of 0-3mm: mineral powder = (15-20): (12-17): (15-20): (10-15): (6-12): (3-7): (18-24): (1-3), particularly preferably (17-19): (14-16): (17-19): (11-13): (8-10): (4-6): (19-22): (1.5-2.5).
[0010] Preferably, the asphalt content of the mixture of the present invention is 3% to 4%, particularly preferably 3% to 3.5%.
[0011] Preferably, the void ratio of the mixture of the present invention is 3.7% to 4.4%, particularly preferably 3.9% to 4.2%; the mineral gap ratio is 10% to 11%, particularly preferably 10.5% to 11%; the asphalt saturation is 57% to 68%, particularly preferably 59% to 65%.
[0012] Preferably, the dynamic stability of the mixture of the present invention is greater than 25 kN, the rutting dynamic stability is greater than 5000 times / mm, and the freeze-thaw splitting strength ratio is greater than 60%.
[0013] A pavement structure is characterized in that a flexible base layer is paved with the dense-graded and extra-large-size asphalt macadam mixture of the present invention.
[0014] Preferably, the pavement structure consists of an anti-fatigue asphalt mixture structural layer, a flexible base layer, a high modulus asphalt mixture structural layer, and a steel slag asphalt mixture surface functional layer. The anti-fatigue asphalt mixture structural layer, the flexible base layer, the high modulus asphalt mixture structural layer, and the steel slag asphalt mixture surface functional layer are laid on the roadbed in sequence from bottom to top, and the flexible base layer is paved in a single layer with a thickness of 12-15 cm (particularly preferably 13-15 cm).
[0015] Preferably, the fatigue-resistant asphalt mixture structural layer adopts FAC-13 asphalt mixture with a thickness of 6 to 8 cm. Using continuous dense-graded asphalt mixture, the asphalt content of FAC-13 asphalt mixture is preferably 4.7-5.0%, the nominal maximum particle size is 13.2mm, the pass rate range of standard sieve hole 13.2mm is 90%-100%, the pass rate range of standard sieve hole 9.5mm is 70%-84%, the pass rate range of standard sieve hole 4.75mm is 40%-65%, the pass rate range of standard sieve hole 2.36mm is 25%-50%, the pass rate range of standard sieve hole 1.18mm is 15%-35%, the pass rate range of standard sieve hole 0.6mm is 10%-28%, the pass rate range of standard sieve hole 0.3mm is 10%-20%, the pass rate range of standard sieve hole 0.15mm is 5%-15%, the pass rate range of 0.075mm is 4%-8%, and the void ratio is preferably 2%-3%.
[0016] Preferably, the high modulus asphalt mixture structural layer adopts GAC-20 mixture, which is spread in two layers, with the lower layer thickness of 8 to 10 cm and the upper layer thickness of 5 to 8 cm. Using continuous dense-graded asphalt mixture, the asphalt content of GAC-20 mixture is preferably 4.6-4.8%, the nominal maximum particle size is 19mm, the pass rate of standard sieve hole 19mm ranges from 80% to 93%, the pass rate of standard sieve hole 16mm ranges from 75% to 90%, the pass rate of standard sieve hole 13.2mm ranges from 60% to 80%, the pass rate of standard sieve hole 9.5mm ranges from 55% to 75%, the pass rate of standard sieve hole 4.75mm ranges from 26% to 56%, the pass rate of standard sieve hole 2.36mm ranges from 15% to 45%, the pass rate of standard sieve hole 1.18mm ranges from 12% to 35%, the pass rate of standard sieve hole 0.6mm ranges from 8% to 22%, the pass rate of standard sieve hole 0.3mm ranges from 5% to 18%, the pass rate of standard sieve hole 0.15mm ranges from 4% to 13%, the pass rate of 0.075mm ranges from 3% to 7%, and the void ratio is preferably 3% to 3.5%.
[0017] Preferably, the surface functional layer of the steel slag asphalt mixture adopts SSMA-13 steel slag asphalt mixture with a thickness of 4 cm. A discontinuous graded asphalt horseshoe fat gravel mixture is adopted, and the asphalt content of the SSMA-13 steel slag asphalt mixture is preferably 5.8-6.0%, and the aggregate is a mixture of steel slag and limestone, and the mass ratio of steel slag to limestone is (18-30): (72-83), the nominal maximum particle size of the steel slag is 13.2 mm, and the standard sieve aperture of 13.2 mm steel slag has a pass rate range of 80%-100%, the standard sieve aperture of 9.5 mm steel slag has a pass rate range of 55%-65%, and the standard sieve aperture of 4.75 mm The pass rate range is 20% to 25%, the pass rate range of standard sieve hole 2.36mm is 20% to 25%, the pass rate range of standard sieve hole 1.18mm is 15% to 20%, the pass rate range of standard sieve hole 0.6mm is 10% to 28%, the pass rate range of standard sieve hole 0.3mm is 10% to 15%, the pass rate range of standard sieve hole 0.15mm is 8% to 12%, the pass rate range of 0.075mm is 7% to 10%, and the porosity is preferably 3.3% to 4.6%.
[0018] Compared with the prior art, the dense-graded extra-large particle size asphalt macadam mixture and pavement structure of the present invention have the following outstanding beneficial effects:
[0019] (1) The maximum nominal aggregate size is 53 mm. Within the aggregate size range of the present invention, the flexible base can be paved with a thickness of more than 150 mm at one time, thus avoiding the addition of redundant bonding interfaces, significantly saving construction time, improving construction efficiency, and ensuring the overall quality of the asphalt pavement;
[0020] (ii) In the pavement structure of the present invention, the main function of the anti-fatigue asphalt mixture FAC-13 structural layer is to enhance the anti-fatigue ability of the bottom of the asphalt layer, and improve its ability to resist cracks and failure of mechanical properties under repeated loads, mainly to resist fatigue cracks; the main function of the dense-graded extra-large particle size asphalt stabilized gravel mixture flexible base is to enhance the overall bearing capacity of the pavement structure. Through this thick structural layer, the level of load on the bending and tensile strain at the bottom of the entire structural layer is reduced, so that the anti-fatigue structural layer can work under a smaller strain; the main function of the high modulus asphalt mixture GAC-20 structural layer is to improve the rutting resistance of the pavement structure, that is, to enhance the ability of the structural layer to resist high-temperature shear, thereby ensuring the smoothness of the road surface. At the same time, these two layers of structure play the role of transferring load and improving bearing capacity. Together with the flexible base layer, they increase the thickness of the structural layer and reduce the bending and tensile strain level at the bottom of the overall structural layer. There is a certain modulus gradient between the anti-fatigue asphalt mixture FAC-13 structural layer, the flexible base layer, and the high modulus asphalt mixture GAC-20 structural layer. The modulus gradually decreases from bottom to top, which can achieve a uniform transition of the structural layer stiffness and avoid the effects of stress concentration caused by sudden changes in modulus. The main function of the surface functional layer of the steel slag asphalt mixture SSMA-13 is to provide better surface functionality, that is, anti-skid performance, to ensure that the road surface is still rough after repeated wear and tear under driving dynamic loads, providing sufficient friction to ensure driving safety. The combination of each structural layer can greatly increase the service life of the pavement structure and reduce the cost of pavement maintenance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Attached Figure 1 is a schematic diagram of a pavement structure of an embodiment;
[0022] Attached Figure 2 is a graph showing the relationship between the service life of a pavement structure and the number of axle loads in an embodiment;
[0023] Attached Figure 3 2. It is a relationship diagram between permanent deformation of pavement structure and axle load times in the embodiment. DETAILED DESCRIPTION
[0024] The dense-graded extra-large particle size asphalt macadam mixture of the present invention is described in detail below with reference to the accompanying drawings of the specification by way of specific embodiments.
[0025] Example:
[0026] 1. Determination of gradation interval of dense-graded extra-large particle size asphalt stabilized crushed stone mixture
[0027] Based on the nominal maximum aggregate size of 53mm, the screening pass rate of each grade of aggregate is determined, and the upper, middle and lower limits of the screening pass rate of dense-graded extra-large particle size asphalt stabilized crushed stone mixture aggregate are determined, see Table 1.
[0028] Table 1 Aggregate passing rate of each grade of dense graded extra-large particle size asphalt stabilized crushed stone mixture (%)
[0029]
[0030] 2. Aggregate mix ratio of dense-graded and extra-large particle size asphalt-stabilized crushed stone mixture
[0031] Aggregate mix ratio is: limestone with maximum particle size of 63mm: limestone with maximum particle size of 43mm: limestone with particle size of 15-20mm: limestone with particle size of 10-15mm: limestone with particle size of 5-10mm: limestone with particle size of 3-5mm: limestone with particle size of 0-3mm: mineral powder = 18:15:18:12:9:5:21:2. The aggregate gradation of dense-graded extra-large particle size asphalt-stabilized crushed stone mixture is determined in Table 2.
[0032] Table 2 Determination of gradation pass rate of dense graded extra-large particle size asphalt stabilized crushed stone mixture (%)
[0033]
[0034] 3. Asphalt content of dense graded extra large particle size asphalt stabilized crushed stone mixture
[0035] The optimum asphalt content of dense-graded extra-large particle size asphalt stabilized gravel mixture is 3.3%.
[0036] 4. Performance parameters of dense-graded extra-large particle size asphalt stabilized crushed stone mixture
[0037] The dynamic stability of dense-graded extra-large particle size asphalt stabilized crushed stone mixture is 28.23kN, the rutting dynamic stability is greater than 5727 times / mm, and the freeze-thaw splitting strength ratio is greater than 63.83%. The void ratio of dense-graded extra-large particle size asphalt stabilized crushed stone mixture is 4.1%, the mineral gap ratio is 10.9%, and the asphalt saturation is 62.2%.
[0038] 5. Design of pavement structure of dense-graded and extra-large particle size asphalt-stabilized crushed stone mixture
[0039] As attached Figure 1 As shown, on the treated roadbed 1, a 7 cm anti-fatigue asphalt mixture FAC-13 structural layer 2, a 15 cm dense-graded extra-large particle size asphalt stabilized gravel mixture flexible base layer 3, an 8 cm high modulus asphalt mixture GAC-20 structural layer 4, a 6 cm high modulus asphalt mixture GAC-20 structural layer 5, and a 4 cm steel slag asphalt mixture SSMA-13 surface functional layer 6 are laid in sequence from bottom to top.
[0040] Among them, the fatigue-resistant asphalt mixture FAC-13 adopts continuous dense-graded asphalt mixture. The asphalt content of FAC-13 asphalt mixture is 4.8%, the aggregate is limestone, the nominal maximum particle size is 13.2mm, the pass rate of standard sieve hole 13.2mm is 92%, the pass rate of standard sieve hole 9.5mm is 76%, the pass rate of standard sieve hole 4.75mm is 55%, the pass rate of standard sieve hole 2.36mm is 35%, the pass rate of standard sieve hole 1.18mm is 27%, the pass rate of standard sieve hole 0.6mm is 18%, the pass rate of standard sieve hole 0.3mm is 13%, the pass rate of standard sieve hole 0.15mm is 12%, the pass rate of 0.075mm is 7%, the void rate is 3%, and the fatigue times are greater than 1 million times of standard axle load.
[0041] The high modulus asphalt mixture GAC-20 adopts continuous dense graded asphalt mixture. The asphalt content of GAC-20 mixture is 4.6%. The aggregate is limestone. The nominal maximum particle size is 19mm, the pass rate of standard sieve hole 19mm is 93%, the pass rate of standard sieve hole 16mm is 80%, the pass rate of standard sieve hole 13.2mm is 65%, the pass rate of standard sieve hole 9.5mm is 63%, the pass rate of standard sieve hole 4.75mm is 42%, the pass rate of standard sieve hole 2.36mm is 35%, the pass rate of standard sieve hole 1.18mm is 18%, the pass rate of standard sieve hole 0.6mm is 12%, the pass rate of standard sieve hole 0.3mm is 13%, the pass rate of standard sieve hole 0.15mm is 10%, the pass rate of 0.075mm is 4%, the void ratio is 3%, and the uniaxial compression dynamic modulus is 12000MPa.
[0042] SSMA-13 steel slag asphalt mixture adopts discontinuous graded asphalt horseshoe fat crushed stone mixture. The asphalt content of SSMA-13 steel slag asphalt mixture is 5.9%. The aggregate is a mixture of steel slag and limestone with a mass ratio of 22:78. The nominal maximum particle size of the steel slag is 13.2mm. The pass rate of steel slag with a standard sieve hole of 13.2mm is 90%, the pass rate of steel slag with a standard sieve hole of 9.5mm is 58%, the pass rate of steel slag with a standard sieve hole of 4.75mm is 20%, the pass rate of standard sieve hole of 2.36mm is 22%, the pass rate of standard sieve hole of 1.18mm is 15%, the pass rate of standard sieve hole of 0.6mm is 18%, the pass rate of standard sieve hole of 0.3mm is 13%, the pass rate of standard sieve hole of 0.15mm is 10%, the pass rate of 0.075mm is 7%, and the void ratio is 3.5%.
[0043] 6. Verification of pavement structure of dense-graded and extra-large particle size asphalt-stabilized crushed stone mixture
[0044] (1) Traffic load parameters
[0045] According to the OD survey and analysis, the traffic volume of large buses and trucks in the section AADTT is 5717 vehicles / day, the annual traffic growth rate γ is 4.2%, the direction coefficient DDF is 55.0%, and the lane coefficient LDF is 80.0%. The vehicle type distribution coefficient is shown in Table 3.
[0046] Table 3 Vehicle type distribution coefficient
[0047] Vehicle Type Category 2 Category 3 Category 4 5 categories 6 categories 7 categories 8 categories 9 categories 10 categories 11 categories Model distribution coefficient (%) 6 7.6 19.8 0 0 0 0 53.3 13.3 0
[0048] Based on the investigation and analysis of the vehicle load conditions of adjacent highways in the road network and historical data, the proportion of underloaded and fully loaded vehicles of various types of vehicles was obtained, as shown in Table 4.
[0049] Table 4 Proportion of partially loaded vehicles and fully loaded vehicles (%)
[0050] Vehicle Type Category 2 Category 3 Category 4 5 categories 6 categories 7 categories 8 categories 9 categories 10 categories 11 categories Partially loaded vehicle ratio 80 85 60 70 50 65 40 45 45 60 Full load ratio 20 15 40 30 50 35 60 55 55 40
[0051] The design indicators corresponding to the pavement structure are fatigue cracking of the asphalt mixture layer, permanent deformation of the asphalt mixture layer, and vertical compressive strain on the top surface of the roadbed. The equivalent design axle load conversion coefficients of non-full-loaded vehicles and fully-loaded vehicles corresponding to each vehicle type under different design indicators are obtained, as shown in Table 5.
[0052] Table 5 Conversion coefficients of equivalent design axle loads for partially loaded vehicles and fully loaded vehicles
[0053]
[0054] The cumulative number of equivalent axle load actions corresponding to permanent deformation and fatigue cracking of the asphalt mixture layer is 57,304,064 times (see Figure 2 ). The cumulative number of equivalent axle load actions corresponding to the vertical compressive strain on the top surface of the roadbed is 121,057,777 times. The cumulative traffic volume of large passenger cars and trucks in the design lanes within the design service life of this pavement structure is 18,660,288, and the traffic level is heavy traffic.
[0055] (3) Preliminary pavement structure plan and material parameters
[0056] The preliminary proposed pavement structure is shown in Table 6.
[0057] Table 6 Preliminary pavement structure
[0058] Structural layer number Horizon Material Type Thickness(mm) Modulus (MPa) Poisson's ratio 1 Surface Asphalt mixture 40 12,000 0.25 2 Surface Asphalt mixture 60 14,000 0.25 3 Surface Asphalt mixture 80 14,000 0.25 4 Grassroots Asphalt mixture 150 11,000 0.25 5 Grassroots Asphalt mixture 70 10,000 0.25 6 Roadbed Soil foundation 162 0.4
[0059] The rebound modulus of the roadbed under standard conditions is 190MPa, the rebound modulus humidity adjustment coefficient Ks is 1, and the reduction coefficient Kη for dry-wet and freeze-thaw cycles is 0.85. The rebound modulus of the top surface of the roadbed after humidity adjustment and reduction for dry-wet and freeze-thaw cycles is 162MPa.
[0060] (4) Pavement structure verification
[0061] Permanent deformation calculation of asphalt mixture layer:
[0062] The benchmark equivalent temperature Tξ is 14.2℃, and the calculated equivalent temperature Tpef of the permanent deformation of the asphalt mixture layer is 20.6℃. The reliability coefficient β is 1.65. The asphalt mixture layer is divided into 8 layers, and the thickness of each layer (hi) is shown in Table 8. Using the elastic layered system theory, the vertical compressive stress (Pi) at the top of each layer under the design load is calculated respectively. The calculation results of the permanent deformation (Rai) are summarized in Table 7. The permanent deformation of each layer is accumulated to obtain the total permanent deformation of the asphalt mixture layer Ra=6.8 (mm), the allowable permanent deformation of the asphalt layer is 10 (mm), and the proposed pavement structure meets the requirements. The relationship between permanent change and axle load times is shown in Figure 3 .
[0063] Table 7 Calculation results of permanent deformation of asphalt layer
[0064] Layering Layer thickness Rutting test specimen thickness Permanent deformation of rutting test Vertical pressure Correction factor Permanent deformation 1 20 50 1.8 0.7 3.977 1.3 2 20 50 1.8 0.69 6.846 2.2 3 20 50 1 0.67 7.217 1.2 4 20 50 1 0.61 6.067 0.9 5 20 50 1 0.54 4.608 0.5 6 80 50 1 0.46 1.877 0.6 7 150 50 2.5 0.22 0.151 0.1 8 70 50 2 0.04 0.011 0.0 total 6.8
[0065] Fatigue cracking calculation of asphalt mixture layer:
[0066] According to the elastic layer system theory, the horizontal tensile strain at the bottom of the asphalt layer is calculated to be 25.300με. According to meteorological data, the freezing index F in the area is 900℃·day, and the adjustment coefficient ka in the seasonal frozen area is 0.79. According to the area, the temperature adjustment coefficient of the benchmark pavement structure (structural layer fatigue) is 0.98. According to the initial pavement structure and pavement structure layer material parameters, the temperature adjustment coefficient kT1 is calculated to be 1.283. The saturation of the asphalt layer is 90.0%.
[0067] Based on the above parameters, the fatigue cracking life of the asphalt layer Nf1 is calculated to be 98,244,718. According to the traffic parameter analysis, the cumulative number of equivalent design axle load actions corresponding to asphalt layer fatigue within the design service life is 57,304,064. The proposed pavement structure meets the requirements.
[0068] Compressive strain verification of soil foundation top surface:
[0069] According to the region, the temperature adjustment coefficient of the benchmark pavement structure (compressive strain on the top of the roadbed) is 0.87. According to the parameters of the preliminary pavement structure and the material parameters of the pavement structure layer, the temperature adjustment coefficient kT3 is calculated to be 1.669. According to the above parameters, when the cumulative number of equivalent design axle loads Ne4 is calculated to be 121,057,777, the allowable vertical compressive strain value [εz] on the top of the roadbed is 154.081με. Using the elastic layered system theory, the vertical compressive strain on the top of the roadbed is calculated to be 66.622με, which meets the allowable vertical compressive strain requirements on the top of the roadbed.
[0070] Calculation of low temperature cracking index of pavement:
[0071] According to the climate conditions, the low temperature design temperature T in the area is -25℃. The roadbed type parameter b=5, the stiffness modulus St of the surface asphalt in the bending beam rheological test at -10℃ is 300MPa, and the low temperature cracking index CI=0.002 is calculated. The low temperature cracking index requirement is 3. The selected pavement structure and materials meet the requirements of low temperature crack resistance.
[0072] Asphalt mixture penetration strength verification:
[0073] According to the climatic conditions in the area, there are 9 months with a monthly average temperature ≥ 0℃, and the cumulative number of design axle load actions for the design lane corresponding to the penetration strength verification is calculated to be Ne5 = 42,978,048. The average monthly average temperature Td of the months with a monthly average temperature ≥ 0℃ in the area is 16.1℃. According to the highway grade, the allowable permanent deformation of the asphalt mixture layer [Ra] is 10mm, and the pavement structure coefficient Ψg = 0.88 is calculated. The asphalt mixture penetration strength is 0.751, and the comprehensive penetration strength of the asphalt mixture of each layer of the pavement is Rτs = 1. The selected pavement structure and materials meet the requirements of the asphalt mixture penetration strength.
[0074] Acceptance deflection values of roadbed top surface and road surface:
[0075] The rebound modulus of the roadbed under standard conditions is 190MPa, and the rebound modulus humidity adjustment coefficient Ks is 1, then the rebound modulus E0 under the equilibrium humidity state is 190MPa, and the roadbed top surface acceptance deflection value lg is calculated by using the elastic half-space body theory to be 98.285 (0.01mm). Using the proposed pavement structure and the modulus values of each layer structure, the roadbed top surface rebound modulus is 190, which is the rebound modulus under the equilibrium humidity state multiplied by the modulus adjustment coefficient kl (kl = 1). According to the elastic layered system theory, the road surface acceptance deflection value la is 10.4 (0.01mm), and the road surface deflection humidity adjustment coefficient K is 1.
[0076] According to the elastic layer system theory, the theoretical deflection value of the second layer of asphalt binder is 11.3 (0.01mm). The theoretical deflection value of the third layer of asphalt binder is 13.2 (0.01mm). The theoretical deflection value of the fourth layer of asphalt binder is 17.6 (0.01mm). The theoretical deflection value of the fifth layer of asphalt binder is 39.3 (0.01mm).
[0077] In summary, the results of various calculations are summarized in Table 8:
[0078] Table 8 Summary of analysis results
[0079] Verification content Calculated Value Comparison value Is it satisfied? Asphalt layer rutting (mm) 6.801 10 yes Cumulative equivalent axial load corresponding to fatigue cracking of asphalt layer 98,244,718 57,304,064.189 yes Compressive strain on the top surface of soil foundation (micro strain) 66.622 154.081 yes Low temperature cracking index 0.002 3 yes Asphalt layer penetration strength 1 0.751 yes
[0080] The designed dense-graded extra-large-size asphalt-stabilized crushed stone mixture suitable for large-thickness paving and its pavement structure meet the use requirements.
[0081] 7. Determination of paving thickness of dense-graded extra-large particle size asphalt-stabilized crushed stone mixture
[0082] The nominal maximum aggregate size of the dense-graded extra-large particle size asphalt stabilized gravel mixture is 53 mm. According to the requirement that the paving thickness shall not exceed 3 times the nominal maximum aggregate size, the one-time paving thickness of the dense-graded extra-large particle size asphalt stabilized gravel mixture flexible base is 150 mm.
Claims
1. A pavement structure, characterized in that: It is composed of an anti-fatigue asphalt mixture structure layer, a flexible base layer, a high modulus asphalt mixture structure layer and a steel slag asphalt mixture surface functional layer. The anti-fatigue asphalt mixture structure layer, the flexible base layer, the high modulus asphalt mixture structure layer and the steel slag asphalt mixture surface functional layer are laid on the roadbed from bottom to top. The flexible base is paved with dense-graded and extra-large-size asphalt crushed stone mixture, with a single-layer paving thickness of 12-15 cm, a void ratio of 3.9% to 4.2%, a mineral gap ratio of 10.5% to 11%, an asphalt saturation of 59% to 65%, and an asphalt content of 3% to 3.5%. The dense-graded extra-large particle size asphalt crushed stone mixture is formed by heating and mixing a binder, an aggregate and a filler. The binder is 70# matrix asphalt or SBS modified asphalt. The nominal maximum particle size of the aggregate is 53mm. The mix ratio is: maximum particle size 63mm aggregate: maximum particle size 43mm aggregate: particle size 15-20mm aggregate: particle size 10-15mm aggregate: particle size 5-10mm aggregate: particle size 3-5mm aggregate: particle size 0-3 mm aggregate: mineral powder = (17-19): (14-16): (17-19): (11-13): (8-10): (4-6): (19-22): (1.5-2.5), the gradation range of the mixture is: the pass rate of the standard sieve hole 63mm is 100%, the pass rate of the standard sieve hole 53mm is 93-98%, the pass rate of the standard sieve hole 37.5mm is 83-90%, the pass rate of the standard sieve hole 31. The pass rate of the standard sieve hole of 5mm is 74-82%, the pass rate of the standard sieve hole of 26.5mm is 67-73%, the pass rate of the standard sieve hole of 19mm is 52-62%, the pass rate of the standard sieve hole of 16mm is 47-55%, the pass rate of the standard sieve hole of 13.2mm is 40-50%, the pass rate of the standard sieve hole of 9.5mm is 34-45%, the pass rate of the standard sieve hole of 4.75mm is 25-35%, the pass rate of the standard sieve hole of 2.36mm is 20-27%, the pass rate of the standard sieve hole of 1.18mm is 13-21%, the pass rate of the standard sieve hole of 0.6mm is 10-15%, the pass rate of the standard sieve hole of 0.3mm is 7-12%, the pass rate of the standard sieve hole of 0.15mm is 5-8%, and the pass rate of the standard sieve hole of 0.075mm is 3-5.5%, and the filler is lime ore powder and / or quicklime; The anti-fatigue asphalt mixture structural layer adopts FAC-13 asphalt mixture with a thickness of 6 to 8 cm, adopts continuous dense graded asphalt mixture, the asphalt content is 4.7 to 5.0%, the nominal maximum particle size is 13.2 mm, the pass rate of the standard sieve hole 13.2 mm is in the range of 90% to 100%, the pass rate of the standard sieve hole 9.5 mm is in the range of 70% to 84%, the pass rate of the standard sieve hole 4.75 mm is in the range of 40% to 65%, the pass rate of the standard sieve hole 2.36 mm is in the range of 25% to 50%, the pass rate of the standard sieve hole 1.18 mm is in the range of 15% to 35%, the pass rate of the standard sieve hole 0.6 mm is in the range of 10% to 28%, the pass rate of the standard sieve hole 0.3 mm is in the range of 10% to 20%, the pass rate of the standard sieve hole 0.15 mm is in the range of 5% to 15%, the pass rate of 0.075 mm is in the range of 4% to 8%, and the void ratio is 2% to 3%; The high modulus asphalt mixture structural layer adopts GAC-20 mixture, which is paved in two layers, with a lower layer thickness of 8 to 10 cm and an upper layer thickness of 5 to 8 cm. It adopts a continuous dense graded asphalt mixture, with an asphalt content of 4.6 to 4.8%, a nominal maximum particle size of 19 mm, a standard sieve hole of 19 mm, a pass rate range of 80% to 93%, a standard sieve hole of 16 mm, a pass rate range of 75% to 90%, a standard sieve hole of 13.2 mm, a pass rate range of 60% to 80%, and a standard sieve hole of 9.5 mm, a pass rate range of 5 5% to 75%, the pass rate of standard sieve hole 4.75mm is 26% to 56%, the pass rate of standard sieve hole 2.36mm is 15% to 45%, the pass rate of standard sieve hole 1.18mm is 12% to 35%, the pass rate of standard sieve hole 0.6mm is 8% to 22%, the pass rate of standard sieve hole 0.3mm is 5% to 18%, the pass rate of standard sieve hole 0.15mm is 4% to 13%, the pass rate of 0.075mm is 3% to 7%, and the void ratio is 3% to 3.5%; The surface functional layer of the steel slag asphalt mixture adopts SSMA-13 steel slag asphalt mixture with a thickness of 4 cm, adopts discontinuous graded asphalt horseshoe fat crushed stone mixture, and the asphalt content is 5.8-6.0%. The aggregate is a mixture of steel slag and limestone, and the mass ratio of steel slag to limestone is (18-30): (72-83). The maximum nominal particle size of the steel slag is 13.2 mm, and the passing rate of the steel slag with a standard sieve hole of 13.2 mm is in the range of 80%-100%, and the passing rate of the steel slag with a standard sieve hole of 9.5 mm is in the range of 55%-65%. %, the pass rate of standard sieve hole 4.75mm is 20% ~ 25%, the pass rate of standard sieve hole 2.36mm is 20% ~ 25%, the pass rate of standard sieve hole 1.18mm is 15% ~ 20%, the pass rate of standard sieve hole 0.6mm is 10% ~ 28%, the pass rate of standard sieve hole 0.3mm is 10% ~ 15%, the pass rate of standard sieve hole 0.15mm is 8% ~ 12%, the pass rate of 0.075mm is 7% ~ 10%, and the void ratio is 3.3% ~ 4.6%.