Separator for electrochemical device and electrochemical device including the separator
By coating the separator of a lithium-ion battery with a porous inorganic coating to control the uniform distribution of inorganic particles, the problem of insufficient discharge capacity and safety of lithium-ion batteries at low temperatures is solved, and the dielectric breakdown performance and adhesion are improved. , reduces the risk of short circuit and enhances battery safety.
Patent Information
- Application Number
- CN202080077958.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-11-19
- Filing Date
- 2020-11-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-11-17
AI Technical Summary
Existing lithium-ion batteries have insufficient discharge capacity at low temperatures and have safety issues. In particular, overheating may lead to thermal runaway or perforation of the separator, causing an explosion. In addition, the uneven distribution of inorganic particles in the inorganic coating leads to pressure-resistant defects.
Using a porous inorganic coating, a composition containing a high content of inorganic particles and a binder resin is coated on the surface of the porous substrate to control the aggregation of inorganic particles, ensure their uniform distribution and form low-content secondary particles, thereby improving dielectric breakdown Performance and adhesion.
It is achieved to reduce the risk of short circuit in lithium-ion batteries, improve the dielectric breakdown performance of the separator and the adhesion to the electrode, reduce the possibility of short circuit at high temperatures, and enhance the safety of the battery.
Smart Images

Figure CN114651367B_ABST
Abstract
Description
Technical Field
[0001] This application claims the priority of Korean Patent Application No. 10-2019-0148978 filed in Korea on November 19, 2019. The present disclosure relates to a separator for an electrochemical device, and an electrochemical device including the separator. Specifically, the present disclosure relates to a separator having a small thickness, excellent adhesion and improved dielectric breakdown performance, and an electrochemical device including the separator. Background Art
[0002] Energy storage technology has been gaining attention recently. As the application of energy storage technology has been extended to energy for mobile phones, cameras and notebook PCs, and even to energy for electric vehicles, efforts to develop electrochemical devices have been increasingly realized. In this context, electrochemical devices have attracted the most attention. Among these electrochemical devices, the development of rechargeable secondary batteries has been attracting attention. Recently, in the development of such batteries, research on designing new electrodes and cells has been actively conducted in order to improve capacity density and specific energy.
[0003] Among commercially available secondary batteries, lithium secondary batteries developed in the early 1990s have attracted attention because they have higher operating voltages and significantly higher energy densities than conventional batteries such as Ni-MH, Ni-Cd, and lead sulfate batteries using aqueous electrolytes. However, the disadvantages of these lithium ion batteries are that they have safety-related problems such as ignition and explosion caused by the use of organic electrolytes and require complex manufacturing processes.
[0004] Recently, lithium-ion polymer batteries have been regarded as one of the next-generation batteries due to the improvement of the above-mentioned disadvantages of lithium-ion batteries. However, lithium-ion polymer batteries have a relatively low capacity compared with lithium-ion batteries and show insufficient discharge capacity especially at low temperatures. Therefore, a solution that can improve the above-mentioned problems is urgently needed.
[0005] Although many production companies have produced such electrochemical devices, their safety characteristics show different signs. It is very important to evaluate and ensure the safety of these electrochemical devices. The most important consideration is that the electrochemical devices should not harm the user when they fail. For this purpose, safety standards strictly control the ignition and smoke exhaust in electrochemical devices. For the safety characteristics of electrochemical devices, great attention is paid to the explosion when the electrochemical device overheats and causes thermal runaway or perforation of the separator. In particular, at temperatures of 100°C or higher, the polyolefin-based porous substrate conventionally used as a separator for electrochemical devices exhibits severe thermal shrinkage behavior due to its material properties and characteristics including orientation during its manufacturing process, thereby causing a short circuit between the cathode and the anode.
[0006] In order to solve the above safety problems of electrochemical devices, a separator having a porous coating layer formed by coating a mixture containing inorganic particles and a binder polymer on at least one surface of a porous separator sheet (substrate) has been proposed. Since the inorganic particles contained in the inorganic coating layer have higher heat resistance than the polymer material, unlike a separator using a substrate including only a polymer material, an effect of preventing a short circuit between the positive electrode and the negative electrode can be obtained even when the electrochemical device is overheated. However, as Figure 1 As shown, there is a problem that during the preparation of the slurry for forming the inorganic coating layer, the inorganic particles introduced into the coating layer are not uniformly dispersed in the slurry, but are locally concentrated or agglomerated with each other. This inhibits the thin filmization of the separator and causes the generation of withstand voltage defects. Under these circumstances, it is increasingly necessary to develop a separator that is easy to thin filmize, reduces the generation of secondary particle aggregation, and has excellent dielectric breakdown performance. Summary of the invention
[0007] Technical issues
[0008] The present disclosure aims to solve the problems of the prior art, and thus the present disclosure aims to provide a separator for an electrochemical device, which has a low content of secondary particles, i.e., aggregates of inorganic particles, in an inorganic coating layer, and exhibits a high dielectric breakdown voltage to provide a low withstand voltage defect generation rate. The present disclosure also aims to provide a method for manufacturing the above-mentioned separator.
[0009] Technical Solution
[0010] According to a first embodiment of the present disclosure, there is provided a separator for an electrochemical device, comprising: a porous substrate having a plurality of pores; and a porous inorganic coating layer formed on at least one surface or both surfaces of the porous substrate and comprising a plurality of inorganic particles and a binder resin located on the entire or partial surfaces of the inorganic particles to connect and fix the inorganic particles to each other,
[0011] wherein the inorganic particles are present in an amount of 50 wt % or more based on 100 wt % of the total weight of the inorganic coating layer, and the separator has a ratio (A) of 70 % or more defined by the following Formula 1:
[0012] [Formula 1]
[0013] Ratio (A) (%) = [(initial dielectric breakdown voltage before compression - dielectric breakdown voltage after compression) / (initial dielectric breakdown voltage before compression)] × 100%,
[0014] The initial dielectric breakdown voltage before compression refers to the voltage at which a short circuit occurs when a direct current is applied to the partition so that the partition is pressurized at a predetermined rate, and the dielectric breakdown voltage after compression refers to the voltage at which a short circuit occurs when a direct current is applied to the partition so that the partition is pressurized at a predetermined ratio while the partition is pressurized in the range of 1MPa to 10MPa.
[0015] According to a second embodiment of the present disclosure, a separator for an electrochemical device as defined in the first embodiment is provided, wherein when observed from the surface of the inorganic coating, the separator has no secondary particles, or the diameter of the secondary particles observed from the surface of the inorganic coating is 50 μm or less, wherein the secondary particles are aggregates of multiple primary particles.
[0016] According to a third embodiment of the present disclosure, a separator for an electrochemical device as defined in the first or second embodiment is provided, wherein the separator has no secondary particles when observed from the surface of the inorganic coating, or the secondary particles observed from the surface of the inorganic coating have a diameter of 50 μm or less and protrude from the surface of the separator to a height of 3 μm or less, wherein the secondary particles are aggregates of multiple primary particles.
[0017] According to a fourth embodiment of the present disclosure, there is provided a separator for an electrochemical device as defined in any one of the first to third embodiments, the separator having an adhesion force to an electrode of 15 gf / 25 mm to 200 gf / 25 mm.
[0018] According to a fifth embodiment of the present disclosure, there is provided a separator for an electrochemical device as defined in any one of the first to fourth embodiments, wherein the binder resin includes a fluorinated binder resin, and the fluorinated binder resin includes any one selected from the group consisting of polyvinylidene fluoride homopolymer, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, and polyvinylidene fluoride-co-chlorotrifluoroethylene, or a mixture of two or more thereof.
[0019] According to a sixth embodiment of the present disclosure, there is provided the separator for an electrochemical device as defined in the fifth embodiment, wherein the molecular weight of the fluorinated binder resin is 200,000 to 1,500,000.
[0020] According to a seventh embodiment of the present disclosure, there is provided a separator for an electrochemical device as defined in the sixth embodiment, wherein the fluorinated binder resin is PVDF-HFP, and the substitution rate of HFP is 3 wt % to 30 wt %.
[0021] According to an eighth embodiment of the present disclosure, there is provided an electrochemical device including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the separator is the same as defined in any one of the first to seventh embodiments.
[0022] According to a ninth embodiment of the present disclosure, there is provided an electrochemical device as defined in the eighth embodiment, the electrochemical device being a lithium secondary battery.
[0023] According to a tenth embodiment of the present disclosure, there is provided a method for manufacturing a separator for an electrochemical device, comprising the steps of: preparing a composition for forming an inorganic coating layer comprising a solvent, inorganic particles and a binder resin; and applying the composition to a surface of a porous substrate and then drying, wherein the composition is prepared by introducing the inorganic particles and the binder resin into the solvent and then stirring, and the prepared composition comprises composite particles satisfying at least one of the following conditions: particle size (D 50 ) is 2.5 μm or less, and the particle size (D 99 ) is 35 μm or less, and the composite particles are floccules formed by aggregation of the inorganic particles and / or the binder resin in the composition.
[0024] According to an eleventh embodiment of the present disclosure, there is provided a method for manufacturing a separator for an electrochemical device as defined in the tenth embodiment, wherein the binder resin includes a fluorinated binder resin, and the fluorinated binder resin includes any one selected from the group consisting of polyvinylidene fluoride homopolymer, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, and polyvinylidene fluoride-co-chlorotrifluoroethylene, or a mixture of two or more thereof.
[0025] According to a twelfth embodiment of the present disclosure, there is provided a method for manufacturing a separator for an electrochemical device as defined in the eleventh embodiment, wherein the molecular weight of the fluorinated binder resin is 200,000 to 1,500,000.
[0026] According to a thirteenth embodiment of the present disclosure, there is provided a method for manufacturing a separator for an electrochemical device as defined in the twelfth embodiment, wherein the fluorinated binder resin is PVDF-HFP, and the substitution rate of HFP is 3 wt % to 30 wt %.
[0027] Beneficial Effects
[0028] The separator for an electrochemical device according to the present disclosure has a low content of secondary particles formed by the aggregation of inorganic particles in the inorganic coating. In particular, the separator has a low content of secondary particles protruding from the surface of the separator to a predetermined height or higher. Since the inorganic particles are not aggregated but evenly distributed in the inorganic coating, when the separator according to the present disclosure is applied to a battery and pressure is generated in the battery due to the charging / discharging of the battery, the separator according to the present disclosure allows the pressure to be evenly dispersed over the entire surface of the separator. In this way, the deformation of the separator can be minimized. At the same time, when a porous film made of a polymer material is used as a separator substrate, there is a low tendency to concentrate pressure from the secondary particles to a local part of the separator substrate, so the separator substrate is less damaged, thereby reducing the possibility of a short circuit. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] The accompanying drawings illustrate preferred embodiments of the present disclosure and are used together with the foregoing disclosure to provide a further understanding of the technical features of the present disclosure, and therefore, the present disclosure is not to be interpreted as being limited to the drawings. In addition, for the purpose of a clearer description, the shapes, sizes, proportions, or ratios of some constituent elements in the drawings may be magnified.
[0030] Figure 1 is a schematic diagram showing a cross section of a separator according to the related art, in which inorganic particles are aggregated with each other to form secondary particles remaining on the separator.
[0031] Figure 2 is a schematic diagram showing a cross section of a separator according to an embodiment of the present disclosure.
[0032] Figure 3 is a schematic diagram illustrating a cross section of a separator having an electrode bonding portion according to an embodiment of the present disclosure.
[0033] Figure 4 is a scanning electron microscope (SEM) image showing the surface of the separator according to Example 1.
[0034] Figure 5 is a scanning electron microscope (SEM) image showing the surface of the separator according to Comparative Example 1. DETAILED DESCRIPTION
[0035] Hereinafter, the preferred embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. Before the description, it should be understood that the terms used in the specification and the appended claims should not be interpreted as being limited to the general meaning and dictionary meaning, but should be interpreted according to the meaning and concept corresponding to the technical aspects of the present disclosure on the basis of the principle of allowing the inventor to appropriately define the terms for the best interpretation.
[0036] Throughout the specification, the expression "a portion includes an element" does not exclude the existence of any other elements but indicates that the portion may further include other elements.
[0037] As used herein, the terms "approximately," "substantially," and the like are used to indicate a meaning adjacent to the stated numerical value when acceptable manufacturing and material errors specific to the stated meaning are proposed, and are used to prevent unscrupulous infringers from improperly using the disclosure content including exact numerical values or absolute numerical values provided to assist in understanding the disclosure content.
[0038] As used herein, the expression "A and / or B" means "A, B, or both."
[0039] The present disclosure relates to a separator for an electrochemical device. According to the present disclosure, an electrochemical device refers to a device that converts chemical energy into electrical energy through an electrochemical reaction, and has the concept of covering primary batteries and secondary batteries (Secondary Battery). In addition, a secondary battery is a rechargeable battery, and has the concept of covering lithium-ion batteries, nickel-cadmium batteries, nickel-hydrogen batteries, etc. According to an embodiment of the present disclosure, the secondary battery can be a lithium-ion secondary battery.
[0040] In one aspect of the present disclosure, a separator for an electrochemical device is provided, comprising: a porous substrate having a plurality of pores; and a porous inorganic coating, the porous inorganic coating being formed on at least one surface or both surfaces of the porous substrate and comprising a plurality of inorganic particles and a binder resin located on the entire or a portion of the surface of the inorganic particles to connect and fix the inorganic particles to each other, wherein the inorganic particles are present in an amount of 50 wt % or more based on 100 wt % of the total weight of the inorganic coating.
[0041] In addition, according to the present disclosure, the separator is characterized in that it has a high dielectric breakdown voltage. According to an embodiment of the present disclosure, the separator has a ratio (A) of 70% or more defined by the following Formula 1. The ratio (A) may be calculated according to the following Formula 1.
[0042] [Formula 1]
[0043] Ratio (A) (%) = [(initial dielectric breakdown voltage before compression - dielectric breakdown voltage after compression) / (initial dielectric breakdown voltage before compression)] × 100%
[0044] The initial dielectric breakdown voltage before compression refers to the voltage at which a short circuit occurs when the separator being analyzed is ramped up at a predetermined rate by applying a direct current to the separator. The initial dielectric breakdown voltage before compression can be measured at a temperature of 70° C. to 90° C. In addition, a direct current of 0.1 mA or more can be applied, and the voltage can be ramped up at a rate of 10 V / s to 150 V / s. Here, the voltage can be 3 kV and the ramp up time can be 30 seconds.
[0045] In addition, the dielectric breakdown voltage after compression refers to a voltage at which a short circuit occurs when a direct current is applied to the separator to increase the pressure of the separator at a predetermined ratio while the separator is pressurized in the range of 1 MPa to 10 MPa. The dielectric breakdown voltage after compression can be measured at a temperature of 70° C. to 90° C. In addition, a direct current of 0.1 mA or more can be applied, and the voltage can be increased at a rate of 10 V / s to 150 V / s. Here, the voltage can be 3 kV and the ramp up time can be 30 seconds.
[0046] According to an embodiment of the present disclosure, the initial dielectric breakdown voltage before compression refers to a voltage at which a short circuit occurs when a 0.5 mA direct current is ramped up at a rate of 100 V / s at a temperature of 70° C. to 90° C. (voltage 3 kV, ramp up time 30 seconds). In addition, the dielectric breakdown voltage after compression refers to a voltage at which a short circuit occurs when a 0.5 mA direct current is ramped up at a rate of 100 V / s while the separator is pressurized in the range of 1 MPa to 10 MPa (voltage 3 kV, ramp up time 30 seconds).
[0047] Meanwhile, according to the present disclosure, dielectric breakdown voltage refers to the highest voltage that an insulator can withstand, and dielectric breakdown refers to that when a voltage is applied to an insulator, the insulator is destroyed and loses its dielectric properties at a specific voltage value or a higher voltage value. In other words, the withstand voltage of the partition can be determined by measuring the dielectric breakdown voltage of the partition. According to an embodiment of the present disclosure, the dielectric breakdown voltage can be determined by setting a partition as an insulator between two conductors and applying a voltage to the partition to measure the voltage at which dielectric breakdown occurs. For example, an AC / DC / IR withstand voltage (Hi-Pot) tester can be used to measure the dielectric breakdown voltage. Specifically, a porous substrate is set between an aluminum bottom fixture (jig) and a cylindrical electrode rod, a DC current is set to 0.5mA, and a ramp-up rate is set to 100V / s (voltage (voltage) 3kV, ramp-up time (ramp up time) 30 seconds). Once the test is started, the determination is completed when a short circuit occurs during the boost process, and the voltage at this time is defined as the dielectric breakdown voltage. Here, when determining the dielectric breakdown voltage after compression of the separator, as described above, a predetermined range of pressure may be applied to the separator.
[0048] Meanwhile, according to an embodiment of the present disclosure, the separator shows an adhesion force (adhesion force to the electrode) of 15 gf / 25 mm to 200 gf / 25 mm between the separator and the electrode.
[0049] The reason why the separator according to the present disclosure has a high dielectric breakdown voltage and / or the above-mentioned range of adhesion to the electrode even after compression is that the content of the secondary particles in the inorganic coating is controlled to a low level. In particular, since the protrusion of the secondary particles from the surface of the inorganic coating is controlled, the separator has a uniform surface.
[0050] According to an embodiment of the present disclosure, when observed from the surface of the inorganic coating, the partition has no secondary particles, or the diameter of the secondary particles observed from the surface of the inorganic coating is 50 μm or less. Preferably, when observed from the surface of the inorganic coating, the partition has no secondary particles, or the diameter of the secondary particles observed from the surface of the inorganic coating is 30 μm or less. More preferably, when observed from the surface of the inorganic coating, the partition has no secondary particles, or the diameter of the secondary particles observed from the surface of the inorganic coating is 10 μm or less. In other words, when the inorganic coating according to the present disclosure is observed from its surface, no secondary particles are observed, and if any secondary particles are present, the diameter of the secondary particles is 50 μm or less, preferably 30 μm or less, and more preferably 10 μm or less. Here, the diameter refers to the maximum diameter of each particle.
[0051] According to an embodiment of the present disclosure, when the partition is observed from the surface of the inorganic coating, the number of secondary particles having a base of 1.5×2 cm and a diameter of 50 μm or less, preferably 30 μm or less, and more preferably 10 μm or less observed from the surface of the inorganic coating is 30 or less, preferably 10 or less. In addition, when the partition is observed from the surface of the inorganic coating, no secondary particles are observed, or the secondary particles observed from the surface of the inorganic coating have a diameter controlled within the above range and protrude from the surface of the partition to a height of 3 μm or less. In other words, when the partition is observed from the surface of the inorganic coating, no secondary particles are observed, or the protruding height of the secondary particles observed from the surface of the inorganic coating is 3 μm or less.
[0052] According to an embodiment of the present disclosure, the surface of the inorganic coating can be observed by using an analyzer such as FESEM-optical profiler (×100 times) to determine the diameter and the protrusion height. The protrusion height of the secondary particles can be determined by measuring the highest-lowest height. During analysis using an optical profiler, the height of the secondary particles can be calculated based on the portion with the largest difference between the highest height and the lowest height.
[0053] According to the present disclosure, the secondary particle refers to an aggregate formed by aggregating two or more inorganic particles in the form of independent single primary particles, and is different from independent primary particles bonded to each other by a binder resin. Figure 1 is a schematic diagram showing a cross section of a separator according to the prior art, in which secondary particle type aggregates 123 formed by aggregation of inorganic particles remain. In contrast, Figure 2 1 is a schematic diagram of a separator according to an embodiment of the present disclosure, in which inorganic particles are not aggregated but are uniformly distributed in the state of primary particles 122 on the inorganic coating layer of the separator.
[0054] According to an embodiment of the present disclosure, in the inorganic coating, the inorganic particles are bonded to each other by a binder resin and integrated with each other, wherein the interstitial volume between the inorganic particles can form pores. As used herein, "interstitial volume" refers to the space defined by the inorganic particles that substantially face each other in a closed packed or densely packed structure of the inorganic particles.
[0055] Furthermore, according to the present disclosure, due to the characteristics of the method for manufacturing a separator described below, the inorganic coating layer is provided with the electrode bonding part 121 having a high binder resin content on the surface thereof. Figure 3is a schematic diagram showing a cross-sectional structure of a separator 100 according to an embodiment of the present disclosure. Figure 3 , a separator according to the present disclosure includes an inorganic coating 120 formed on the surface of a separator substrate 110, wherein a binder resin is distributed at a higher concentration at a top portion of the inorganic coating compared to other portions. For ease of description, the top portion where the binder resin is distributed at a higher concentration is hereinafter referred to as an "electrode bonding portion 121". According to an embodiment of the present disclosure, the electrode bonding portion is the result of the migration of the binder resin toward the top portion through a process such as humidification phase separation. Therefore, the electrode bonding portion is not a structure physically separated from the inorganic coating, but is integrally and inseparably bonded to the surface of the inorganic coating as a part of the inorganic coating. In addition, the thickness of the electrode bonding portion may be uneven because the electrode bonding portion is a product produced by humidification phase separation. According to an embodiment of the present disclosure, the electrode bonding portion may be defined as a portion having a binder resin content of 70% by weight or greater, preferably 85% by weight or greater, from the top in the thickness direction of the inorganic coating. In addition, each figure mark may be applied together Figures 1 to 3 .
[0056] Furthermore, according to the present disclosure, the total thickness of the porous coating layer may be appropriately controlled within a range of 2 μm to 10 μm based on both surfaces of the separator substrate.
[0057] Based on the total weight of the inorganic coating, the inorganic particles may be present in an amount of 50 wt % or more, preferably 70 wt % or more. At the same time, based on the total weight of the inorganic coating, the inorganic particles may be present in an amount of 97 wt % or less. When the inorganic particles are present in an amount of less than 50 wt %, there is an excess of binder resin in the pores of the inorganic coating, resulting in a decrease in pore size and porosity. At the same time, when the amount of binder resin is too small, the peeling resistance of the inorganic coating and / or the adhesion to the electrode will be reduced. Peeling resistance refers to the adhesion between the separator substrate and the inorganic coating, and the adhesion to the electrode refers to the adhesion between the separator and the electrode.
[0058] According to an embodiment of the present disclosure, the inorganic coating may include a fluorinated binder resin as a binder resin. Fluorinated binder resin may include polyvinylidene fluoride (PVDF) based polymers. This PVDF based polymer is not particularly limited, but its specific examples may include polyvinylidene fluoride homopolymer, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, polyvinylidene fluoride-co-chlorotrifluoroethylene, or the like. At least one selected from the above-mentioned PVDF based polymers may be used. In addition to PVdF based polymers, a PVdF based copolymer including a vinylidene fluoride repeating unit (A) and another repeating unit (B) copolymerizable with the repeating unit may also be used.
[0059] According to an embodiment of the present disclosure, the molecular weight (Mw) of the fluorinated binder is preferably 200,000 to 1,500,000. In addition, when the fluorinated binder is PVDF-HFP, it is a copolymer including a vinylidene fluoride repeating unit (A) and another repeating unit (B) copolymerizable with the repeating unit, such as hexafluoropropylene (HFP), and the HFP substitution degree of the copolymer may be 3 wt % to 30 wt %.
[0060] According to the present disclosure, the term "molecular weight" refers to the weight average molecular weight (Mw). According to an embodiment of the present disclosure, the molecular weight (Mw) can be determined by using gel permeation chromatography (GPC). For example, 200 mg of the polymer resin to be analyzed is diluted in 200 mL of a solvent such as tetrahydrofuran (THF) to prepare a sample with a concentration of about 1000 ppm, and the molecular weight can be determined by using an Agilent 1200 series GPC instrument at a flow rate of 1 mL / min through a refractive index (RI) detector. In addition, a Varian 500 MHz NMR can be used to determine the molecular weight. 1 H-NMR was used to determine the degree of substitution.
[0061] In addition, if necessary, in addition to the fluorinated binder, the inorganic coating may further include a second binder resin, such as an acrylate polymer having adhesive properties. Based on the total weight 100 weight % of the binder resin, the content of the second binder resin is preferably controlled within the range of 3 weight % to 20 weight %. For example, within the above-defined range, the amount of the second binder resin can be 5 weight % or more, or 10 weight % or more. Specific examples of the second binder resin may include polyacrylate, polymethylmethacrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, polyethylene oxide, polyarylate, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinylalchol, cyanoethylcellulose, cyanoethylsucrose, pullulan, carboxymethyl cellulose, or the like. At least one second binder resin selected from the above examples may be used.
[0062] According to the present disclosure, there is no particular limitation on inorganic particles, as long as they are electrochemically stable. In other words, the inorganic particles that can be used in this article are not particularly limited, as long as they do not cause oxidation and / or reduction within the operating voltage range of the applicable electrochemical device (e.g., 0-5V based on Li / Li+). Specifically, when inorganic particles with a high dielectric constant are used as inorganic particles, the ionic conductivity of the electrolyte can be improved by increasing the degree of dissociation of the electrolyte salt (such as a lithium salt) in the liquid electrolyte. Non-limiting examples of inorganic particles may include high dielectric constant inorganic particles with a dielectric constant of 5 or more, preferably 10 or more, inorganic particles with lithium ion transport capability, or mixtures thereof. According to an embodiment of the present disclosure, non-limiting examples of inorganic particles include BaTiO 3, Pb(Zr,Ti)O 3 (PZT), Pb 1-x La x Zr 1-y Ti y O 3 (PLZT), Pb(Mg 1 / 3 Nb 2 / 3 )O 3 PbTiO 3 (PMN-PT), hafnium dioxide (HfO 2 ), SrTiO 3 , SnO 2 , CeO 2 , MgO, NiO, CaO, ZnO, ZrO 2 , Y 2 O 3 , Al 2 O 3 , TiO 2 , AlOOH, Al(OH) 3 , SiC, or a mixture thereof. In addition, the inorganic particles may further include lithium phosphate (Li 3 PO 4 ); lithium titanium phosphate (Li x Ti y (PO 4 ), 0 < x < 2, 0 < y < 3); lithium aluminum titanium phosphate (Li 3 , 0 < x < 2, 0 < y < 1, 0 < z < 3); (LiAlTiP) x Al y Ti z (PO 4 ), 0 < x < 2, 0 < y < 1, 0 < z < 3); (LiAlTiP) 3 , 0 < x < 2, 0 < y < 1, 0 < z < 3); (LiAlTiP) x O y -based glass (1 < x < 4, 0 < y < 13); lithium lanthanum titanate (Li x La y TiO 3 , 0 < x < 2, 0 < y < 3); lithium germanium thiophosphate (Li x Ge y P z S w , 0 < x < 4, 0 < y < 1, 0 < z < 1, 0 < w < 5); lithium nitride; SiS 2 -based glass (Li x Si y S z , 0 < x < 3, 0 < y < 2, 0 < z < 4); and P 2 S 5 -based glass (Li x P y Sz , 0 < x < 3, 0 < y < 3, 0 < z < 7), or a mixture of two or more of them.
[0063] According to an embodiment of the present disclosure, the particle size (D 50 ) of the inorganic particles can be 0.2 - 3 μm. For example, the particle size (D 50 ) of the inorganic particles can be 0.3 μm or larger, or 0.5 μm or larger. In combination with or independent of this, the particle size (D 50 ) of the inorganic particles can be 2 μm or smaller, 1.5 μm or smaller, or 1 μm or smaller.
[0064] According to the present disclosure, the porous substrate can be a porous polymer film substrate or a porous polymer nonwoven substrate.
[0065] The porous polymer film substrate can be a porous polymer film, and the porous polymer film includes polyolefins such as polyethylene or polypropylene. Such a polyolefin porous polymer film substrate achieves a closing function at a temperature of 80°C to 130°C.
[0066] Here, the polyolefin porous polymer film can be formed of a polymer including a polyolefin polymer alone or in combination of two or more of them, and the polyolefin polymer such as polyethylene, polypropylene, polybutene, or polyisopentene including high - density polyethylene, linear low - density polyethylene, low - density polyethylene, and ultra - high - molecular - weight polyethylene.
[0067] In addition, the porous polymer film substrate can be obtained by molding various polymers such as polyester other than polyolefins into a film shape. In addition, the porous polymer film substrate can have a stacked structure of two or more film layers, and each film layer can be formed of a polymer including the above - mentioned polymers such as polyolefins or polyesters alone or in combination of two or more of them.
[0068] In addition, in addition to the above-mentioned polyolefins, the porous polymer film substrate and the porous nonwoven web substrate can also be formed by polymers including polyethylene terephthalate, polybutylene terephthalate, polyester, polyacetal, polyamide, polycarbonate, polyimide, polyetheretherketone, polyethersulfone, polyphenyleneoxide, polyphenylenesulfide, or polyethylenenaphthalene, alone or in combination.
[0069] Although there is no particular limitation on the thickness of the porous substrate, the thickness of the porous substrate is 1 μm to 100 μm, specifically 5 μm to 50 μm. Although there is no particular limitation on the size and porosity of the pores present in the porous substrate, the pore size and porosity may be 0.01 μm to 50 μm and 10% to 95%, respectively.
[0070] In addition to the above-mentioned inorganic particles and binder resin, the separator according to the present disclosure may further include other additives such as a flame retardant, a dispersant, etc. as a component of the inorganic coating layer, as needed.
[0071] The separator according to an embodiment of the present disclosure may be obtained by preparing a composition for forming an inorganic coating layer including inorganic particles and a binder resin, applying the composition to at least one surface of a porous substrate, and then drying.
[0072] First, a composition for forming an inorganic coating layer may be prepared by forming a polymer solution containing a binder resin dissolved in a solvent, adding inorganic particles to the polymer solution, and dispersing the inorganic particles therein.
[0073] The solvent is not particularly limited as long as it can be uniformly mixed with the binder resin. Non-limiting examples of solvents include cyclohexane, mesitylene, dimethylacetamide, dimethylsulfone, dimethyl carbonate, acetone, tetrahydrofuran, methylene chloride, chloroform, dimethylformamide, N-methyl-2-pyrrolidone (NMP), water, methyl ethyl ketone, methyl acetate, cyclohexanone or the like. According to an embodiment of the present disclosure, the solvent may include at least one selected from the above examples.
[0074] In addition, according to an embodiment of the present disclosure, inorganic particles may be added after being crushed to a predetermined average particle size in advance. In a variation, inorganic particles may be added to a polymer solution and then dispersed therein, while being controlled and crushed to a predetermined average particle size by a ball milling process, etc., thereby providing a composition for forming an inorganic coating. According to the present disclosure, the latter is more preferred because the primary particles in the composition are uniformly dispersed and the generation of secondary particles is reduced.
[0075] The solid content of the composition excluding the solvent can be controlled to be less than 30% by weight.
[0076] In addition, according to an embodiment of the present disclosure, the composition is a dispersed mixture including a binder resin and inorganic particles dispersed in a solvent, and composite particles as flocs formed by aggregation of the binder resin and / or the inorganic particles can be formed. According to the present disclosure, the particle size of the composite particles and the aggregated flocs is controlled to reduce the generation of secondary particles in the separator. According to an embodiment of the present disclosure, the particle size (D 50 ) is preferably 2.5 μm or less. In combination with or independently of this, the particle size (D 99 ) is preferably 35 μm or less. When preparing the composition, the stirring and dispersing steps of the composition can be performed while controlling the processing conditions, such as stirring time, stirring speed, stirring direction, choice of solvent, concentration of the composition, number of stirring times or the like.
[0077] According to an embodiment of the present disclosure, the slurry preferably has a stress energy (StressEnergy) of 0.1 mJ to 1.0 mJ and / or a stress number (StressNumber) of 10 or more.
[0078] According to an embodiment of the present disclosure, the particle size (D 50 ) and particle size (D 99 ) refers to the integral value from the smaller particle side calculated based on the particle size distribution results of particles measured after classification using a particle size analyzer. In other words, the integral value 50% corresponds to the particle size (D 50 ), the integral value 90% corresponds to the particle size (D 99 ). This particle size distribution can be determined by the diffraction or scattering intensity pattern produced when light contacts the particles. As a particle size distribution analyzer, a Microtrac 3000 or Microtrac HRA available from Nikkiso can be used. In addition, a cumulative size-distribution curve can be derived from the measurement results.
[0079] Although there is no particular restriction on the process of applying the composition for forming the inorganic coating to the porous substrate, it is preferred to use a slit coating or dip coating process. The slit coating process includes applying the composition supplied via a slit die to the entire surface of the substrate, and the thickness of the coating can be controlled depending on the flow rate supplied from the metering pump. In addition, the dip coating process includes dipping the substrate into a tank containing the composition to implement the coating, and the thickness of the coating can be controlled depending on the composition concentration and the rate at which the substrate is removed from the tank. Further, in order to more accurately control the coating thickness, post-metering can be implemented after dipping by a Mayer rod or the like.
[0080] Then, the porous substrate coated with the composition for forming an inorganic coating layer may be dried in an oven to form an inorganic coating layer on the surface of the porous substrate. The inorganic coating layer may be formed on at least one surface of the porous substrate or on both surfaces thereof.
[0081] At the same time, an electrode bonding portion can be formed on the surface of the inorganic coating. In order to form the electrode bonding portion, a drying step can be performed under humidification conditions. After the slurry is applied to the surface of the separator substrate, the resulting product is allowed to stand for a predetermined time at a relative humidity of about 30%-80% to solidify (dry) the binder resin. Here, phase separation of the binder resin is initiated. During the phase separation process, the solvent migrates to the surface portion of the inorganic coating, and the binder resin migrates to the surface portion of the inorganic coating as the solvent migrates. In this way, the content of the binder resin on the top layer portion of the porous coating increases. Then, the inorganic coating portion below the top layer portion of the porous coating has porosity, and the pores are formed by the interstitial volume between the inorganic particles.
[0082] In the inorganic coating layer, inorganic particles are bonded to each other by a binder while they are stacked and contact each other, thereby forming interstitial volumes between the inorganic particles, and the interstitial volumes between the inorganic particles become vacant spaces to form pores.
[0083] In other words, the binder resin attaches the inorganic particles to each other so that they can maintain their bonded state. For example, the binder resin connects the inorganic particles to each other and fixes them. In addition, the pores of the porous coating are pores formed by the interstitial volume between the inorganic particles becoming vacant space. The space can be limited by the inorganic particles that are substantially facing each other in the close packing or densely packed structure of the inorganic particles.
[0084] In addition, when the drying step is performed under a humidified condition as described above, the inorganic coating layer may further include an electrode binding part having a high content of the binder resin in a top layer portion thereof. Reference will be made to the above description regarding the electrode binding part.
[0085] In another aspect of the present disclosure, an electrochemical device is provided, including a cathode, an anode, and a separator interposed between the cathode and the anode, wherein the separator is the above-mentioned separator according to an embodiment of the present disclosure.
[0086] Electrochemical devices include any device that implements an electrochemical reaction, and specific examples thereof include all types of primary batteries, secondary batteries, fuel cells, solar cells, or capacitors such as supercapacitor devices. In particular, among secondary batteries, lithium secondary batteries including lithium metal secondary batteries, lithium ion secondary batteries, lithium polymer secondary batteries, or lithium ion polymer batteries are preferred.
[0087] The two electrodes, cathode and anode, used in combination with the separator according to the present disclosure are not particularly limited and can be obtained by bonding the electrode active material to the electrode current collector by methods generally known in the art. In the electrode active material, non-limiting examples of cathode active materials include conventional cathode active materials that can be used for cathodes of conventional electrochemical devices. In particular, lithium manganese oxide, lithium cobalt oxide, lithium nickel oxide, lithium iron oxide, or lithium composite oxides comprising a combination thereof are preferably used. Non-limiting examples of anode active materials include conventional anode active materials that can be used for anodes of conventional electrochemical devices. In particular, materials such as lithium metal or lithium alloys embedded with lithium, carbon, petroleum coke, activated carbon, graphite or other carbonaceous materials are preferably used. Non-limiting examples of cathode current collectors include foils made of aluminum, nickel, or a combination thereof. Non-limiting examples of anode current collectors include foils made of copper, gold, nickel, nickel alloys, or a combination thereof.
[0088] The electrolyte that can be used in the electrochemical device according to the present disclosure is one having A + B - A salt of the structure + Including such as Li + 、Na + , K + , or a combination thereof such as an alkali metal cation, B - Including PF 6 - , BF 4 - , Cl - Br - ,I - , ClO 4 - , AsF 6 - , CH 3 CO 2 - CF 3 SO 3 - 、N(CF 3 SO 2 ) 2 - , C(CF 2 SO 2 ) 3 -, or anions such as a combination thereof, the salt is dissolved or dissociated in an organic solvent including propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, tetrahydrofuran, N-methyl-2-pyrrolidone (NMP), ethyl methyl carbonate (EMC), gamma-butyrolactone (γ-butyrolactone), or its self-nucleus. However, the present disclosure is not limited thereto.
[0089] Depending on the manufacturing process of the final product and the properties required of the final product, the injection of electrolyte can be performed in a suitable step during the process for manufacturing the battery. That is, the injection of electrolyte can be performed before assembling the battery or in the final step of assembling the battery.
[0090] In another aspect of the present disclosure, a battery module is provided, the battery module including a battery including the electrode assembly as a unit cell; a battery pack including the battery module; and a device including the battery pack as a power source. Specific examples of the device include, but are not limited to: a power tool driven by an electric motor; an electric vehicle, including an electric vehicle (EV), a hybrid electric vehicle (HEV), a plug-in hybrid electric vehicle (PHEV), or the like; an electric two-wheeled vehicle, including an electric bicycle (E-bike) and an electric scooter (E-scooter); an electric golf cart; a power storage system; or the like.
[0091] Embodiments will be described more fully below so that the present disclosure can be easily understood. However, the following embodiments can be embodied in a variety of different forms and should not be construed as being limited to the exemplary embodiments set forth herein. On the contrary, these exemplary embodiments are provided so that the present disclosure will be thorough and complete, and will fully convey the scope of the present disclosure to those skilled in the art.
[0092] Manufacturing example
[0093] The separators according to Examples and Comparative Examples were obtained by the following method.
[0094] Polyvinylidene fluoride-co-hexafluoropropylene (PVDF-HFP, HFP substitution ratio: 12 wt %, Mw 400,000) as a binder resin was added to acetone and dissolved therein at 50° C. for about 12 hours to prepare a polymer solution. Then, the particle size (D 50) is 500nm aluminum oxide (Al 2 O 3 ) particles (powder) were added to the obtained polymer solution and dispersed therein to prepare a composition for inorganic coating. Here, the binder resin and the alumina particles were used in a weight ratio of 20:80, and the composition had a solid content of 20% by weight excluding acetone.
[0095] The obtained composition was coated on both surfaces of a polyethylene porous film (porosity 40%) having a thickness of 15 μm by a dip coating process and dried at 25° C. and 40% relative humidity to obtain a separator having an inorganic coating layer having a thickness of 6 μm. The thickness refers to the total thickness of the inorganic coating layer formed on both surfaces of the substrate.
[0096] Physical performance evaluation of separators
[0097] The surface properties, slurry particle size, and dielectric breakdown voltage of each separator according to Examples 1 to 6 and Comparative Examples 1 to 3 were measured. The results are shown in Table 1 below.
[0098] (1) Breathing time
[0099] Gurley air permeability values are obtained according to the method of ASTM D726-94. Herein, "Gurley" refers to the resistance to air flow and is determined by a Gurley densometer. Each Gurley air permeability value defined herein is determined by passing 100 mL of air through a 1 in. air filter at a pressure of 12.2 in. H2O. 2 The time (seconds) required for the cross section is expressed as the ventilation time.
[0100] (2) Particle size distribution of composite particles
[0101] In each composition according to Examples and Comparative Examples, the particle size distribution of the composite particles was measured by using Microtrac 3000.
[0102] (3) Observation of the partition surface
[0103] The surface of the inorganic coating in each separator according to the embodiment and the comparative example was observed by using an instrument such as FESEM-optical profiler (×100 times). Each separator was prepared to have a size of 1.5×2 cm. When the surface was analyzed using an optical profiler, the height of the secondary particles was calculated based on the portion where the height difference between the maximum height and the minimum height was the largest. In addition, the minimum height of the inorganic coating was taken as the surface portion of the inorganic coating, and the diameter of the inorganic particles was determined based on the maximum diameter of the secondary particles protruding from the surface portion.
[0104] Figure 4 is a scanning electron microscope (SEM) image showing the surface of the separator according to Example 1. Figure 4 It can be seen that secondary particles having a predetermined size are generated at a low ratio. Figure 5 is a scanning electron microscope (SEM) image showing the surface of the separator according to Comparative Example 1. Figure 5 It can be seen that through Figure 4 In contrast, secondary particles formed by the aggregation of primary particles protrude from the separator surface.
[0105] (4) Determination of dielectric breakdown voltage
[0106] A separator sample was prepared from each of the Examples and Comparative Examples, and the dielectric breakdown voltage of each separator sample was measured by using an AC / DC / IR withstand voltage tester (Hi-Pottester).
[0107] The initial dielectric breakdown voltage was determined by measuring the voltage at which a short circuit occurred when a direct current of 0.5 mA was ramped up at a rate of 100 V / s at a temperature of 80° C. (voltage 3 kV, ramp up time 30 seconds).
[0108] In addition, while the separator was pressurized within the range of 10 MPa, the dielectric breakdown voltage after compression was determined by measuring the voltage at which a short circuit occurred when a direct current of 0.5 mA was ramped up at a rate of 100 V / s at a temperature of 80°C (voltage 3 kV, ramp up time 30 seconds).
[0109] In addition, the ratio (A) is calculated according to the following formula 1.
[0110] [Formula 1]
[0111] Ratio (A) (%) = [(initial dielectric breakdown voltage before compression - dielectric breakdown voltage after compression) / (initial dielectric breakdown voltage before compression)] × 100%
[0112] (5) Determination of electrode adhesion
[0113] The negative electrode was prepared as follows. The negative electrode active material (graphite), the conductive material (super P) and the binder (CMC / SBR mixed in a weight ratio of 1: 1) were introduced into the solvent (water) at a weight ratio (wt %) of 97.5: 1.5: 1, and then mixed (2000rpm, 30 minutes) to prepare the negative electrode slurry. The prepared negative electrode slurry was coated on a copper film with a thickness of 20 μm using a scraper and dried overnight at 110 ° C. The thickness of the negative electrode was controlled to be about 100 μm to 110 μm, and a roller press was used to press the final thickness to about 60 μm to 70 μm. The prepared electrode was allowed to stand in a vacuum dryer at 80 ° C for 4 hours. Then, the separator obtained by each embodiment and comparative example was laminated with the negative electrode to prepare a separator-negative electrode laminated sample. Each laminated sample was prepared to have a size of 2.5 cm × 10 cm. A double-sided tape available from 3M Co. was attached to a glass slide, and each sample was attached to the glass slide in such a way that the spacer side of each sample could face the double-sided tape. A UTM (Universal Testing Machine) was used at a speed of 300 mm / min with a 10 N load cell and 180° mode.
[0114] [Table 1]
[0115]
[0116] As can be seen from Table 1, in the case of Examples 1 to 6, in which the particle size D of the composite particles is set to 50 and D 99 Controlled within the above-defined range, the diameter of the secondary particles formed in the inorganic coating layer in each separator is smaller than the diameter of the secondary particles in Comparative Examples 1 to 3. In the case of Examples 1 to 6, if any secondary particles are present in the inorganic coating layer, their diameter is 30 μm or less. In particular, in the case of Examples 1 to 3, if any secondary particles are present, their diameter is 10 μm or less. However, in the case of Comparative Examples 1 to 3, secondary particles having a diameter greater than 50 μm are observed. In addition, it can be seen that each of Examples 1 to 6 provides a dielectric breakdown voltage ratio before and after compression of 70% or more, i.e., A value, which is higher than that of Comparative Examples 1 to 3.
Claims
1. A separator for an electrochemical device, comprising: a porous substrate having a plurality of pores; and a porous inorganic coating layer formed on at least one surface or both surfaces of the porous substrate and comprising a plurality of inorganic particles and a binder resin located on the entire or a part of the surface of the inorganic particles to connect and fix the inorganic particles to each other, wherein the inorganic particles are present in an amount of 50 wt % or more based on 100 wt % of the total weight of the inorganic coating layer, The particle size D of the inorganic particles 50 0.2μm to 3μm; wherein the binder resin is a fluorinated binder resin, and the fluorinated binder resin is any one selected from the group consisting of polyvinylidene fluoride homopolymer, polyvinylidene fluoride-co-hexafluoropropylene, polyvinylidene fluoride-co-trichloroethylene, and polyvinylidene fluoride-co-chlorotrifluoroethylene, or a mixture of two or more thereof; wherein when observed from the surface of the inorganic coating layer, the diameter of the secondary particles observed from the surface of the inorganic coating layer is 10 μm or less and protrudes from the separator surface to a height of 3 μm or less, wherein the secondary particles are aggregates of primary particles of a plurality of the inorganic particles; And the separator has a ratio (A) of 70% or more defined by the following Formula 1: [Formula 1] Ratio (A) (%) = [(initial dielectric breakdown voltage before compression - dielectric breakdown voltage after compression) / (initial dielectric breakdown voltage before compression)] × 100%, The initial dielectric breakdown voltage before compression is determined by measuring the voltage at which a short circuit occurs when a direct current of 0.5 mA is applied at a rate of 100 V / s and a voltage of 3 kV is increased for 30 seconds at a temperature of 80°C, and the dielectric breakdown voltage after compression is determined by measuring the voltage at which a short circuit occurs when a direct current of 0.5 mA is applied at a rate of 100 V / s and a voltage of 3 kV is increased for 30 seconds at a temperature of 80°C while the partition is pressurized at 10 MPa. 2 . The separator for an electrochemical device according to claim 1 , wherein the separator has an adhesion force to an electrode of 15 gf / 25 mm to 200 gf / 25 mm. 3 . The separator for an electrochemical device according to claim 1 , wherein the molecular weight of the fluorinated binder resin is 200,000 to 1,500,000. 4 . The separator for an electrochemical device according to claim 3 , wherein the fluorinated binder resin is PVDF-HFP, and the substitution rate of HFP is 3 wt % to 30 wt %.
5. An electrochemical device comprising: A positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, wherein the separator is the same as the separator defined in any one of claims 1 to 4. The electrochemical device according to claim 5 , which is a lithium secondary battery.
7. A method for manufacturing a separator for an electrochemical device as defined in claim 1, comprising the steps of: preparing a composition for forming an inorganic coating layer including a solvent, the inorganic particles and the binder resin; as well as The composition is applied to the surface of a porous substrate and then dried, wherein the composition is prepared by introducing the inorganic particles and the binder resin into the solvent and then stirring, and the prepared composition includes composite particles that satisfy at least one of the following conditions: a particle size D 50 2.5 μm or less, and the particle size D 99 The composite particles are 35 μm or less, and are floccules formed by aggregation of the inorganic particles and / or the binder resin in the composition. 8 . The method for producing the separator for an electrochemical device according to claim 7 , wherein the molecular weight of the fluorinated binder resin is 200,000 to 1,500,000. 9 . The method for producing the separator for an electrochemical device according to claim 8 , wherein the fluorinated binder resin is PVDF-HFP, and a substitution rate of HFP is 3 wt % to 30 wt %.