Coated glass substrate

By using a specific layer sequence on the glass substrate, including oxynitride dielectric layers of aluminum, zinc and tin, the problem of complex layer sequences in the prior art that increase production costs and time is solved, and optical properties are achieved that are not affected by heat treatment. Variable and wear-resistant coated glass substrates, reducing manufacturing costs and increasing robustness.

CN114728841BActive Publication Date: 2024-10-01PILKINGTON GRP LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080078696.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-11-13
Filing Date
2020-11-13
Publication Date
2024-10-01
Estimated Expiration
2040-11-13

AI Technical Summary

Technical Problem

It is difficult to create heat-treatable coated glass substrates that meet automotive and architectural window performance requirements in glass manufacturing with existing technologies, and complex layer sequences increase production costs and time, and existing technologies fail to provide optical properties that remain unchanged upon heat treatment and coated glass substrates with high wear resistance.

Method used

A layer sequence composed of a glass substrate is used, including a lower anti-reflective layer, a silver-based functional layer, a barrier layer and an upper anti-reflective layer, wherein the upper anti-reflective layer contains at least 5 atomic % of aluminum, zinc and tin oxygen and nitrogen. Chemical dielectric layer, the dielectric layer can contain 10 to 45 atomic % aluminum, and the layers are deposited by magnetron cathode sputtering to reduce the number of coatings and improve mechanical robustness.

Benefits of technology

A coated glass substrate with unchanged or small changes in optical properties during heat treatment is achieved, with high light transmittance, low emissivity and good sunlight control, reducing manufacturing costs and improving the mechanical and chemical robustness of the coating. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114728841B_ABST
    Figure CN114728841B_ABST
Patent Text Reader

Abstract

The present invention relates to a coated glass substrate, a method for preparing the same and use thereof in a multi-layer glazing unit, the coated glass substrate comprising, starting from a glass substrate, in sequence at least: a lower antireflection layer; a silver-based functional layer; a barrier layer; and an upper antireflection layer, wherein the upper antireflection layer comprises a dielectric layer of oxynitrides of aluminum (Al), zinc (Zn) and tin (Sn) containing at least 5 atomic % of aluminum (Al).
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to coated glass substrates, and to methods of making the same. More particularly, the present invention relates to heat treatable coated glass substrates having a reduced number of layers in the coating, and further comprising a low-e and / or solar control coating.

[0002] Glass coatings that provide low emissivity (low-e) and / or solar control can be deposited, for example, by physical vapor deposition methods such as sputtering. Glass coatings deposited by sputtering are typically made by passing a glass substrate through one or more chambers with targets that are bombarded with ions or atoms. The bombarded targets release material that subsequently coats the glass substrate. Sputtered low emissivity and solar control coating stacks typically consist of a repeating sequence such as the following: "substrate / base antireflection layer sequence / [silver (Ag) / antireflection layer sequence] n ”, where each of the “n” anti-reflective layers does not necessarily have the same thickness or composition. The anti-reflective layer typically includes one or more dielectric layers.

[0003] The glass manufacturing industry is constantly demanding coated glass substrates that can meet the demanding performance requirements of automotive and architectural glazing, with the result that glass substrates are coated using increasingly complex layer sequences (or stacks) based on a range of dielectric materials. Therefore, it is becoming increasingly common in the glass manufacturing industry for "n" in the sequence to be greater than or equal to 2 or even 3 or 4.

[0004] Previously, depositing multiple coatings on glass substrates has been addressed by installing expensive extensions to coating lines in glass manufacturing plants to achieve a sufficient number of chambers to deposit the desired different coating materials in sufficient quantities, thicknesses, and sequences.

[0005] This has also led to the installation of additional pumping sections in the extensions to allow multiple reactive deposition processes to run in sequence. However, this can only be achieved at high expense and with lengthy interruptions, as the coating line typically needs to be stopped for long periods of time in order to complete the required engineering installations. Each additional chamber and pumping section also requires accompanying power supplies, vacuum pumps, conveying sections, services, instruments, and integration into the control system. Such changes often lead to the reconstruction of downstream logistics and may even lead to new civil engineering or building expansions. These problems continue to increase as the need for multiple metal layers and / or more complex coating stacks becomes more and more common.

[0006] Furthermore, dielectric layers are typically thicker and slower to deposit by sputtering than metal layers such as silver. This further increases the number of chambers required, as multiple chambers may be required to effectively deposit a single dielectric layer.

[0007] Architectural or automotive glazing also requires the provision of coated glass substrates which can be heat treated and thus toughened to provide safety properties and / or which can be bent into a desired shape.

[0008] It is known that for the thermal toughening and / or bending of glass substrates (also referred to as tempering in the glass industry), the glass sheet must be heat treated to a temperature close to or above the softening point of the glass and then rapidly cooled and / or bent with the aid of a suitable bending device. The toughening or bending of standard float glass of the soda-lime-silica type is usually achieved by heating the glass to a temperature in the region of 580 to 690° C., keeping the glass substrate in this temperature range for several minutes, and then starting the actual toughening and / or bending process.

[0009] "Heat treatment", "heat treated" and "heat treatable" in the following description and in the claims refer to heat bending and / or toughening processes (also known as tempering) and other thermal processes in which the coated glass substrate reaches a temperature of, for example, 580 to 690° C. for several minutes, for example, up to about 10 minutes. If the coated glass substrate undergoes heat treatment without significant damage, it is considered to be heat treatable. Examples of significant damage to the glass substrate caused by heat treatment include, for example, increased haze (or turbidity), pinholes or spots.

[0010] The use of coated glass substrates with coatings comprising doped metal oxide layers is known. For example, in US 2009 / 0197077, a transparent glass substrate provided with a thin-film multilayer is described, comprising a functional layer based on silver or on a silver-containing metal alloy and two coatings consisting of a plurality of dielectric layers, such that the silver functional layer is located between the two coatings. The functional layer is deposited on the wetting layer, itself deposited directly onto the coating below. The coating below comprises at least one nitride-based dielectric layer and at least one amorphous smoothing layer made of a mixed oxide in the form of zinc stannate doped with antimony, which is in contact with the wetting layer above.

[0011] In US 6541133, a layer stack for a surface coating of a transparent substrate is disclosed, which has at least one metal oxide composite layer produced by reactive cathode sputtering and contains zinc (Zn) oxide and tin (Sn) oxide. The metal oxide composite layer may also contain 0.5 to 6.5% by weight of one or more elements Al, Ga, In, B, Y, La, Ge, Si, P, As, Sb, Bi, Ce, Ti, Zr, Nb and Ta, relative to the total amount of metal.

[0012] In US 9315414, a method for forming a low emissivity (low-e) plate based on a transparent substrate is disclosed. A metal oxide layer is formed above the transparent substrate. The metal oxide layer includes oxygen, a first element, a second element, and a third element. The first element is tin or zinc. The second element is strontium and the third element is hafnium.

[0013] However, none of the above-mentioned prior art documents provides a heat-treatable coated glass substrate having a layer sequence according to the invention which is able to provide the optical properties as well as the abrasion and scratch resistance requirements required by the glass industry.

[0014] It is therefore an object of the present invention to provide an improved heat-treatable coated glass substrate whose optical properties do not change significantly or change to a reduced amount upon heat treatment. For example, the color change of the coated glass substrate caused by the heat treatment should preferably be such that, if desired, heat-treated and non-heat-treated coated glass substrates can be mounted (glazed) adjacent to each other without noticeable color differences in use.

[0015] It is also an object of the present invention to provide a heat treatable, low emissivity (low-e) and / or solar control coated glass substrate that is capable of withstanding everyday environmental influences during, for example, storage, transportation and use, before and after heat treatment. In addition, it is an object of the present invention to provide a heat treatable, low emissivity (low-e) and / or solar control coated glass substrate that is capable of withstanding the mechanical and chemical conditions acting on the coated glass substrate during normal handling and processing without incurring significant damage, as detailed below with respect to a series of tests.

[0016] The present invention also aims to provide a heat-treatable coated glass substrate having high light transmittance, low emissivity (corresponding to low sheet resistance) and / or good solar control properties. That is, the glass substrate has low solar transmittance and sufficiently high light transmittance. Another object of the present invention is to provide such a heat-treatable coated glass substrate having a reduced number of coatings compared to existing substrates, thereby reducing the investment costs required to manufacture such a coated substrate.

[0017] In summary, the present invention aims to solve the problems associated with the prior art methods and products as described in detail above, and attempts to provide a cost-effective and commercially acceptable coated glass substrate that meets the optical properties required by the glass industry (in terms of, for example, haze, light transmittance and color), and which is also robust enough to withstand thermal tempering.

[0018] According to a first aspect of the present invention, there is provided a coated glass substrate, which comprises, starting from a glass substrate, at least the following layers in order:

[0019] a lower anti-reflection layer;

[0020] Silver-based functional layer;

[0021] Barrier layer; and

[0022] Upper anti-reflection layer,

[0023] The upper anti-reflection layer comprises:

[0024] A dielectric layer of oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) containing at least 5 atomic % aluminum (Al).

[0025] In the coated glass substrate according to the first aspect of the present invention, the dielectric layer may include an oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) containing at least 10 atomic % of aluminum. Alternatively, the dielectric layer may include an oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) containing at least 15 atomic % of aluminum, or the dielectric layer may include an oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) containing at least 22 atomic % of aluminum.

[0026] Furthermore, with respect to the first aspect of the present invention, the dielectric layer preferably comprises an oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) containing up to 45 atomic % of aluminum. More preferably, the dielectric layer comprises an oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) containing up to 40 atomic % of aluminum. Alternatively, the dielectric layer may comprise an oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) containing up to 35 atomic % of aluminum.

[0027] Therefore, in a preferred embodiment of the present invention, the dielectric layer preferably comprises an oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) containing aluminum in the range of 5 atomic % aluminum to 45 atomic % aluminum. Alternatively, the dielectric layer may comprise an oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) containing aluminum in the range of 5 atomic % aluminum to 40 atomic % aluminum. The dielectric layer may also comprise an oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) containing aluminum in the range of 5 atomic % aluminum to 35 atomic % aluminum. In one embodiment of the present invention, the dielectric layer may comprise an oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) containing aluminum in the range of 10 atomic % aluminum to 35 atomic % aluminum. In an alternative embodiment of the present invention, the dielectric layer may comprise an oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) containing aluminum in the range of 20 atomic % aluminum to 35 atomic % aluminum. In yet another embodiment of the present invention, the dielectric layer may include an oxynitride of aluminum (Al), zinc (Zn), and tin (Sn) containing aluminum in the range of 20 atomic % aluminum to 30 atomic % aluminum. In a preferred embodiment of the present invention, the dielectric layer may include an oxynitride of aluminum (Al), zinc (Zn), and tin (Sn) containing aluminum in the range of 22 atomic % aluminum to 28 atomic % aluminum.

[0028] Preferably, the dielectric layer based on oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) contains at most 30 atomic % of zinc and at most 15 atomic % of tin.

[0029] The dielectric layer based on oxynitrides of aluminum (Al), zinc (Zn) and tin (Sn) may preferably include a thickness of at least 5 nm. Alternatively, the dielectric layer based on oxynitrides of aluminum (Al), zinc (Zn) and tin (Sn) may preferably include a thickness of 10 to 50 nm. More preferably, the dielectric layer based on oxynitrides of aluminum (Al), zinc (Zn) and tin (Sn) may preferably include a thickness of 20 to 40 nm. Even more preferably, the dielectric layer based on oxynitrides of aluminum (Al), zinc (Zn) and tin (Sn) may preferably include a thickness of 30 to 40 nm. Most preferably, the dielectric layer based on oxynitrides of aluminum (Al), zinc (Zn) and tin (Sn) preferably includes a thickness of 32 to 36 nm. Such thickness improves the mechanical robustness of the coated substrate. The aluminum (Al), zinc (Zn), and tin (Sn) oxynitride-based dielectric layer may preferably be in direct contact with the zinc (Zn) oxide-based layer in the upper dielectric layer.

[0030] The dielectric layer based on oxynitrides of aluminum (Al), zinc (Zn) and tin (Sn) preferably provides improved stability to the coated glass substrate, that is to say better protection during heat treatment, and may preferably act as a diffusion barrier. In addition, the dielectric layer based on oxynitrides of aluminum (Al), zinc (Zn) and tin (Sn) may preferably act as a protective layer, providing improved mechanical and / or chemical robustness, such as scratch resistance.

[0031] In addition, with respect to the present invention, the lower anti-reflection layer may preferably include, starting from the glass substrate, in order:

[0032] a layer based on oxides of zinc (Zn) and tin (Sn) or oxide of tin (Sn); and

[0033] A layer based on zinc (Zn) oxide.

[0034] The layer based on oxides of zinc (Zn) and tin (Sn) or oxide of tin (Sn) preferably has a thickness of 0.5 to 10 nm.

[0035] The lower anti-reflection layer may also preferably comprise one or more base layers based on (oxy)nitrides of silicon and / or aluminum and / or alloys of silicon and / or aluminum. In the lower anti-reflection layer, the one or more base layers based on (oxy)nitrides of silicon and / or aluminum and / or alloys of silicon and / or aluminum are preferably located between the glass substrate and the layer based on oxides of zinc (Zn) and tin (Sn) or oxides of tin (Sn). Preferably, the base layer comprises a thickness of 20 to 40 nm.

[0036] Furthermore, the base layer may preferably be in direct contact with a layer based on oxides of zinc (Zn) and tin (Sn) or oxide of tin (Sn).

[0037] Therefore, with regard to the present invention, the lower anti-reflection layer may preferably include, starting from the glass substrate, directly in sequence:

[0038] A base layer based on silicon and / or aluminum (oxy)nitrides and / or alloys of silicon and / or aluminum;

[0039] A layer based on oxides of zinc (Zn) and tin (Sn) or oxide of tin (Sn);

[0040] a separation layer based on: a metal oxide; and / or an (oxy)nitride of silicon and / or aluminum; and / or an alloy of silicon and / or aluminum; and

[0041] A layer based on zinc (Zn) oxide.

[0042] Alternatively, the lower anti-reflection layer may preferably comprise, starting directly from the glass substrate:

[0043] A base layer based on silicon and / or aluminum (oxy)nitrides and / or alloys of silicon and / or aluminum;

[0044] a layer based on oxides of zinc (Zn) and tin (Sn) or oxide of tin (Sn); and

[0045] A layer based on zinc (Zn) oxide.

[0046] That is, the lower anti-reflection layer may preferably include three or four layers in the above order.Whether the lower anti-reflection layer preferably includes three or four layers as described above will depend on the number of silver-based functional layers present in the coating sequence.

[0047] Preferably, when the coating sequence contains only a single silver-based coating, the lower antireflection layer preferably consists of four layers in the above order, including a separating layer. Alternatively, when the coating sequence contains more than one silver-based coating, the lower antireflection layer preferably consists of three layers in the above order, that is, there is no separating layer.

[0048] The base layer of the lower antireflection layer based on silicon and / or aluminum (oxy)nitride and / or silicon and / or aluminum alloy may preferably comprise a thickness of at least 5 nm. More preferably, the base layer comprises a thickness of 5 to 60 nm. Even more preferably, the base layer comprises a thickness of, for example, 10 to 50 nm; 15 to 45 nm; or 20 to 40 nm. Most preferably, the base layer of the lower antireflection layer comprises a thickness of 25 to 35 nm. One purpose of the base layer in the coated glass substrate of the present invention is to act as a glass-side diffusion barrier, that is, the barrier attempts to prevent, for example, sodium ions from migrating into the coating.

[0049] The term "silicon (oxy)nitride" includes silicon (Si) nitride (SiN x ) and silicon (Si) oxynitride (SiO x N y ), while the term "aluminum (oxy) nitride" includes aluminum (Al) nitride (AlN x ) and aluminum (Al) oxide nitride (AlO x N y The silicon nitride (Si), silicon oxynitride (Si), aluminum nitride (Al), and aluminum oxynitride (Al) layers are preferably substantially stoichiometric (e.g., in silicon nitride = Si3N4, SiN x =1.33), but may also be substoichiometric or even superstoichiometric, provided that the heat treatability of the coating is not adversely affected thereby. A preferred composition of the base layer of the lower antireflection layer based on silicon (oxy)nitride and / or aluminum (oxy)nitride is an essentially stoichiometric mixed nitride Si 90 Al 10 N x .

[0050] The layer of silicon (oxygen) nitride and / or aluminum (oxygen) nitride can be reactively sputtered from a target based on silicon (Si) and / or aluminum (Al) in a sputtering atmosphere containing nitrogen and argon, respectively. The oxygen content of the base layer based on silicon (oxygen) nitride and / or aluminum (oxygen) nitride can come from residual oxygen in the sputtering atmosphere or from an added oxygen of controlled content in the atmosphere. If the oxygen content of the (oxygen) nitride silicon and / or (oxygen) aluminum nitride is significantly lower than its nitrogen content, that is to say, if the atomic ratio O / N in the layer remains significantly lower than 1, this is generally preferred. It is most preferred to use silicon nitride and / or aluminum nitride with negligible oxygen content for the base layer of the lower antireflection layer. This feature can be controlled by ensuring that the refractive index of the layer is not significantly different from the refractive index of the oxygen-free silicon nitride and / or aluminum nitride layer.

[0051] It is within the scope of the present invention to use mixed silicon (Si) and / or aluminum (Al) targets or otherwise add metals or semiconductors to the silicon (Si) and / or aluminum (Al) components of the layer, as long as the basic barrier and protection properties of the base layer of the lower anti-reflective layer are not lost. For example, aluminum (Al) and silicon (Si) targets can be mixed, without excluding other mixed targets. The additional components are generally present in an amount of 10 to 15 weight percent. Aluminum is generally present in the mixed silicon target in an amount of 10 weight percent.

[0052] The layer based on zinc (Zn) and tin (Sn) oxide or tin (Sn) oxide of the lower anti-reflection layer preferably improves the stability during heat treatment by providing a dense and thermally stable layer, and also contributes to the reduction of haze after heat treatment. The layer based on zinc (Zn) and tin (Sn) oxide or tin (Sn) oxide of the lower anti-reflection layer may preferably have a thickness of at least 0.5 nm. Preferably, the layer based on zinc (Zn) and tin (Sn) oxide or tin (Sn) oxide of the lower anti-reflection layer may have the following thickness: 0.5 to 15 nm; or 0.5 to 13 nm; or 0.5 to 10 nm; or 1 to 12 nm. In addition, the layer based on zinc (Zn) and tin (Sn) oxide or tin (Sn) oxide of the lower anti-reflection layer may have the following thickness: 1 to 7 nm; or 2 to 6 nm; or 3 to 6 nm. Most preferably, for a coated glass substrate having a layer sequence comprising a single silver-based functional layer, the layer based on zinc (Zn) and tin (Sn) oxide or based on tin (Sn) oxide of the lower antireflection layer may have a thickness of 3 to 5 nm. An upper thickness limit in the region of 8 nm may also be preferred due to the optical interference conditions and the reduction in thermal processability due to the resulting reduction in the thickness of the base layer required to maintain the optical interference boundary conditions for the antireflection of the functional layer.

[0053] In an alternative embodiment of the first aspect of the present invention, when the coated glass substrate comprises more than one silver-based functional layer, the layer based on zinc (Zn) and tin (Sn) oxide or based on tin (Sn) oxide of the lower anti-reflection layer preferably has a thickness of at least 12 nm. More preferably, the layer based on zinc (Zn) and tin (Sn) oxide or based on tin (Sn) oxide of the lower anti-reflection layer has a thickness of 12 nm to 20 nm. Even more preferably, the layer based on zinc (Zn) and tin (Sn) oxide or based on tin (Sn) oxide of the lower anti-reflection layer has a thickness of 12 nm to 16 nm. However, most preferably, the layer based on zinc (Zn) and tin (Sn) oxide or based on tin (Sn) oxide of the lower anti-reflection layer has a thickness of 12 nm to 14 nm.

[0054] The layer based on zinc (Zn) and tin (Sn) oxide or based on tin (Sn) oxide of the lower antireflection layer is preferably located directly on a base layer based on silicon (oxy)nitride and / or aluminum (oxy)nitride and / or an alloy of silicon and / or aluminum.

[0055] When the zinc (Zn) and tin (Sn) oxide-based or tin (Sn) oxide-based layer of the lower antireflection layer is zinc (Zn) and tin (Sn) oxide-based (abbreviation: ZnSnO x), the layer may preferably contain: 10 to 90 wt% zinc (Zn) and 90 to 10 wt% tin (Sn); more preferably about 40 to 60 wt% zinc (Zn) and about 40 to 60 wt% tin (Sn); even more preferably about 50 wt% each of zinc (Zn) and tin (Sn), in wt% of the total metal content of the layer. In some preferred embodiments, the layer based on oxides of zinc (Zn) and tin (Sn) of the lower anti-reflective layer may contain: up to 18 wt% tin (Sn), more preferably up to 15 wt% tin (Sn), even more preferably up to 10 wt% tin (Sn). The layer based on oxides of Zn and Sn may preferably also be deposited by reactive sputtering of a mixed ZnSn target in the presence of O2.

[0056] Preferably, the lower anti-reflection layer further includes a separation layer between the layer based on oxides of zinc (Zn) and tin (Sn) or tin (Sn) oxide and the layer based on zinc (Zn) oxide.

[0057] The separation layer preferably contains a metal oxide; and / or a silicon (oxy)nitride and / or an aluminum (oxy)nitride; and / or an alloy of silicon and / or aluminum.

[0058] Furthermore, the separation layer may preferably have a thickness of at least 0.5 nm; or preferably 0.5 to 6 nm; more preferably 0.5 to 5 nm; even more preferably 0.5 to 4 nm; most preferably 0.5 to 3 nm. These preferred thicknesses can further improve the haze during heat treatment. The separation layer preferably provides protection during the deposition process and during subsequent heat treatment. The separation layer is preferably substantially completely oxidized immediately after deposition, or it is oxidized to a substantially fully oxidized layer during subsequent oxide layer deposition.

[0059] The separation layer may preferably comprise: a metal oxide; and / or (oxy)nitrides of silicon and / or aluminum; and / or alloys of silicon and / or aluminum. When the separation layer is based on a metal oxide, the separation layer may preferably comprise a layer based on the following oxides: Ti, Zn, NiCr, InSn, Zr, Al and / or Si.

[0060] When the separation layer is preferably based on a metal oxide, it can be formed using non-reactive sputtering from a ceramic target based on, for example, slightly substoichiometric titanium oxide, such as TiO 1.98 The target is deposited as a substantially stoichiometric or slightly substoichiometric oxide by reactive sputtering of a Ti-based target in the presence of O2, or by depositing a thin Ti-based layer which is subsequently oxidized. In the context of the present invention, "substantially stoichiometric oxide" means an oxide that is at least 95% but at most 100% stoichiometric, while "slightly substoichiometric oxide" means an oxide that is at least 95% but less than 100% stoichiometric.

[0061] In addition to the metal oxide and / or silicon and / or aluminum (oxy)nitride and / or silicon and / or aluminum alloy on which it is based, the separation layer may further comprise one or more other chemical elements selected from at least one of the following elements: Ti, V, Mn, Co, Cu, Zn, Zr, Hf, Al, Nb, Ni, Cr, Mo, Ta, Si, or an alloy based on at least one of these materials, for example as a dopant or alloying agent. Preferably, however, the separation layer based on metal oxide and / or silicon and / or aluminum (oxy)nitride does not comprise one or more other chemical elements.

[0062] In a preferred embodiment of the invention, the separation layer is preferably based on metal oxides which comprise oxides of zinc (Zn) and / or oxides of titanium (Ti).

[0063] When the glass-coated layer sequence comprises a silver-based functional layer, it is particularly preferred that the separating layer is based on titanium oxide.

[0064] Although the separating layer can also be based on titanium oxide when the layer sequence comprises more than one silver-based functional layer, it can also be preferred for the layer sequence or stack to contain no separating layer in the lower antireflection layer when the layer sequence or stack comprises more than one silver-based functional layer.

[0065] Furthermore, it is preferred that the separation layer has a thickness of 0.5 to 3 nm based on titanium oxide.

[0066] The zinc (Zn) oxide-based layer of the lower anti-reflection layer mainly acts as a growth-promoting layer for the subsequently deposited silver-based functional layer. The zinc (Zn) oxide-based layer is optionally mixed with a metal such as aluminum (Al) or tin (Sn) in an amount of up to about 10% by weight (weight % refers to the target metal content). The typical content of the metal such as aluminum (Al) or tin (Sn) is about 2% by weight, and aluminum (Al) is actually preferred. Zinc oxide (ZnO) and mixed zinc (Zn) oxides have been shown to be very effective as growth-promoting layers, and thus assist in achieving low sheet resistance at a given thickness of the subsequently deposited silver-based functional layer. The zinc (Zn) oxide-based layer of the lower anti-reflection layer is preferably sputtered by a zinc (Zn) target in the presence of oxygen (O2). Alternatively, the zinc (Zn) oxide-based layer of the lower anti-reflection layer can be deposited by sputtering, for example, a ceramic target based on ZnO:Al in an atmosphere containing zero or only a small amount of oxygen (i.e., usually not more than about 5% by volume of oxygen). The layer of the lower anti-reflection layer based on zinc (Zn) oxide may preferably have a thickness of at least 2 nm. More preferably, the layer of the lower anti-reflection layer based on zinc (Zn) oxide may preferably have a thickness of 2 to 15 nm; or 3 to 12 nm. Even more preferably, the layer of the lower anti-reflection layer based on zinc (Zn) oxide may preferably have a thickness of 4 to 10 nm. Most preferably, the layer of the lower anti-reflection layer based on zinc (Zn) oxide has a thickness of 5 to 8 nm.

[0067] In addition, with regard to the present invention, it is preferred that the layer based on zinc (Zn) oxide in the lower anti-reflection layer is in direct contact with the silver-based functional layer. Therefore, in a preferred embodiment of the present invention, the layer sequence between the glass substrate and the silver-based functional layer can consist of three layers or four layers of the above-mentioned lower anti-reflection layer.

[0068] The silver-based functional layer preferably consists essentially of silver, without any additives, as is usually the case in the area of ​​low-emissivity and / or solar control coatings. However, it is within the scope of the present invention to modify the properties of the silver-based functional layer by adding dopants, alloying additives, etc. or even adding very thin layers of metals or metal compounds, as long as the properties of the silver-based functional layer required to act as an IR-reflecting layer with high light transmission and low light absorption are not substantially impaired thereby.

[0069] The thickness of each silver-based functional layer is determined by its technical purpose. For typical low-emissivity and / or solar control purposes, the preferred layer thickness for a single silver-based layer may preferably be: 5 to 20 nm; more preferably 5 to 15 nm; even more preferably 5 to 13 nm or 8 to 12 nm; most preferably 9 to 11 nm. With such layer thicknesses, transmittance values ​​of higher than 86% and normal emissivity of lower than 0.05 after heat treatment can be easily achieved according to the invention for a single silver coating. If even better solar control properties are required, the thickness of the silver-based functional layer may be appropriately increased, or several spaced functional layers may be provided as further explained below.

[0070] Although the present invention relates to coated substrates having only one silver-based functional layer, it is within the scope of the present invention to apply the inventive concept to the preparation of low-emissivity and / or solar control coatings comprising two or more silver-based functional layers. When more than one silver-based functional layer is provided, all silver-based functional layers are separated by an intervening dielectric layer (collectively referred to herein as a "central antireflection layer") to form a Fabry-Perot interference filter, whereby the optical properties of the low-emissivity and / or solar control coating can be further optimized for the respective application.

[0071] Preferably, each silver-based functional layer is separated from the adjacent silver-based functional layer by an intervening central anti-reflection layer. The intervening central anti-reflection layer may comprise a combination of one or more of the following layers: a layer based on silicon (oxy)nitride and / or aluminum (oxy)nitride; a layer based on Zn and Sn oxides and / or Sn oxide; and a layer based on metal oxides such as Zn oxide.

[0072] In some preferred embodiments, each silver-based functional layer is separated from adjacent silver-based functional layers by an intervening central anti-reflection layer, wherein each central anti-reflection layer comprises, in order starting from the silver-based functional layer closest to the glass substrate, at least:

[0073] A layer based on (oxy)nitride of silicon and / or (oxy)nitride of aluminum; a layer based on oxides of Zn and Sn and / or oxide of Sn; and a layer based on metal oxide such as oxide of Zn.

[0074] The coated glass substrate according to the first aspect of the present invention preferably further comprises a barrier layer. The barrier layer is preferably in position in direct contact with the silver-based functional layer.

[0075] The barrier layer preferably comprises a NiCrO-based x or zinc (Zn) oxide layer. Based on zinc (Zn) oxide or NiCrO x The barrier layer preferably has a thickness of at least 0.5 nm. More preferably, the Zn-based oxide or NiCrO xThe barrier layer has a thickness of 0.5 to 10 nm. Most preferably, the Zn-based oxide or NiCrO x The barrier layer has a thickness of 1 to 10 nm.

[0076] However, when the barrier layer is based on NiCrO x When the layer is a layer of ethylene, it preferably has a thickness of 0.5 to 5 nm or 1.0 to 5 nm.

[0077] It has been found that excellent protection of the silver-based functional layer during the deposition process and high optical stability during heat treatment can be achieved if the barrier layer comprises a mixed metal oxide layer sputtered from a mixed metal oxide target. When the barrier layer is based on an oxide of zinc (Zn), the oxide can be a mixed metal oxide such as ZnO:Al. Good results are particularly achieved if the ZnO:Al-based layer is sputtered from a conductive ZnO:Al target. The ZnO:Al can be deposited fully oxidized, or in such a way that it is slightly suboxidized.

[0078] In addition, when the barrier layer comprises a layer based on zinc (Zn) oxide, it may be practical for the barrier layer to comprise a plurality of zinc oxide layers, such as layers based not only on mixed metal oxides such as ZnO:Al, but also on oxides of zinc (Zn) and tin (Sn). Suitable barrier layers may therefore be ZnO:Al, ZnS ... x , ZnO:Al. Such an arrangement of three barrier layers may preferably have a combined thickness of 3 to 12 nm.

[0079] The arrangement of the other three barrier layers can preferably be selected from the following layer combinations starting from the silver-based functional layer: ZnO:Al / TiO x / ZnO:Al, ZnO:Al / ZnSnO x / ZnO:Al、TiO x / ZnSnO x / ZnO:Al、TiO x / ZnO:Al / TiO x 、TiO x / ZnSnO x / TiO x and ZnO:Al / ZnSnO x / TiO x .

[0080] At least a portion of the barrier layer that is in direct contact with the silver-based functional layer is preferably deposited using non-reactive sputtering of an oxide target to avoid silver damage.

[0081] Furthermore, as an alternative to a barrier layer based on zinc (Zn) oxide, it has also been found that if the barrier layer comprises a mixed metal oxide based on nickel (Ni) and chromium (Cr), such as substoichiometric NiCrO x The NiCrO layer can also achieve adequate protection of the silver-based functional layer during the deposition process and high optical stability during thermal treatment. This is especially true when the coated glass substrate contains two or more silver-based functional layers, but when the coated glass substrate contains a single silver-based functional layer, substoichiometric NiCrO can also be used. x layer.

[0082] Therefore, for a coated glass substrate comprising two or more silver-based functional layers, it is preferred that each silver-based functional layer is separated from an adjacent silver-based functional layer by an intervening central anti-reflection layer, wherein each central anti-reflection layer comprises, in order starting from the silver-based functional layer closest to the glass substrate, at least:

[0083] a layer based on a mixed metal oxide comprising nickel (Ni) and chromium;

[0084] A layer based on zinc and aluminum based mixed metal oxides;

[0085] Layers based on silicon (oxy)nitride and / or aluminum (oxy)nitride;

[0086] a layer based on oxides of Zn and Sn or based on oxide of Sn; and

[0087] Layers based on metal oxides such as Zn oxide.

[0088] Also with respect to the first aspect of the present invention, the coated glass preferably comprises an upper anti-reflection layer. The upper anti-reflection layer preferably comprises:

[0089] i) a layer based on oxides of zinc (Zn) and tin (Sn) or based on oxide of tin (Sn); and

[0090] ii) A layer based on zinc (Zn) oxide.

[0091] The layer based on Zn and Sn oxide or Sn oxide in the upper antireflection layer may preferably have a thickness of at least 0.5 nm; more preferably at least 0.5 nm or 1 nm, or even at least 1.5 nm, but preferably less than 5 nm; more preferably at most 4 nm; even more preferably less than 4 nm; most preferably at most 3 nm; and especially 2 nm. These preferred thicknesses enable easier deposition and improved optical properties (such as haze) while maintaining mechanical durability.

[0092] The Zn oxide-based layer in the upper antireflection layer may preferably have a thickness of at least 0.5 nm, more preferably at least 0.5 nm or 1 nm; or even at least 1.5 nm; but preferably less than 5 nm; more preferably 4 nm. These preferred thicknesses enable easier deposition and improved optical properties (such as haze) while maintaining mechanical durability.

[0093] Preferably, the layers in the upper anti-reflection layer are based on substantially stoichiometric metal oxides. The use of substantially stoichiometric metal oxides rather than metallic or less than 95% stoichiometric layers in the upper anti-reflection layer results in extremely high optical stability of the coating during thermal treatment and effectively helps keep optical changes small during thermal treatment. In addition, the use of substantially stoichiometric metal oxide based layers provides benefits in terms of mechanical robustness.

[0094] In the context of the present invention, the term "non-reactive sputtering" includes sputtering an oxide target in a low oxygen atmosphere (ie having zero or at most 5 volume % oxygen) to provide a substantially stoichiometric oxide.

[0095] Also in the context of the present invention, when a layer is referred to as being "based on" a specific material or materials, this means that, unless stated otherwise, the layer predominantly comprises said material or materials in an amount of at least 50 atomic %.

[0096] When the layer is based on ZnSnO x When "ZnSnO x ” refers to mixed oxides of Zn and Sn as described and defined elsewhere in the specification.

[0097] In order to minimize any light absorption in the coating and reduce the increase in light transmittance during thermal treatment, all individual layers of the upper and lower antireflection layers are preferably deposited in a substantially stoichiometric composition.

[0098] In order to further optimize the optical properties of the coated substrate, the upper antireflection layer may comprise further partial layers consisting of materials generally known to be suitable for low-e and / or solar control coatings, in particular one or more selected from Sn, Ti, Zn, Nb, Ce, Hf, Ta, Zr, Al and / or Si oxides and / or Si and / or Al (oxy) nitrides or combinations thereof. However, when adding such further partial layers, it should be verified that the hot processability aimed at herein is not thereby impaired.

[0099] It is to be understood that any other layer may contain additives that modify its properties and / or facilitate its fabrication, such as dopants or reaction products of reactive sputtering gases. In the case of oxide-based layers, nitrogen may be added to the sputtering atmosphere, resulting in the formation of oxynitrides instead of oxides, and in the case of nitride-based layers, oxygen may be added to the sputtering atmosphere, also resulting in the formation of oxynitrides instead of nitrides.

[0100] The dielectric layer comprising oxynitrides of aluminum (Al), zinc (Zn) and tin (Sn) may be the outermost layer on the coated glass substrate. Alternatively, the coated glass substrate may further comprise at least one additional layer, such that the dielectric layer of oxynitrides of aluminum (Al), zinc (Zn) and tin (Sn) is between the at least one additional layer and the glass substrate. Preferably, the at least one additional layer comprises: a layer based on oxides of zinc (Zn) and tin (Sn) or based on oxide of tin (Sn); and / or a layer based on oxide of zirconium (Zr). Such additional layers may improve the durability of the coated substrate.

[0101] It is clear that the material, structure and thickness selection of any layer in the sequential stack is important and changes thereto may have a negative impact on the coating performance. It is therefore clear that when any further layers are added to the existing layer sequence described above for the present invention, the properties of the coating stack, such as high thermal stability, are not significantly compromised.

[0102] According to a second aspect of the present invention, there is provided a method for manufacturing a coated glass substrate according to the first aspect of the present invention, comprising:

[0103] i) providing a glass substrate;

[0104] ii) providing a lower anti-reflection layer;

[0105] iii) providing a silver-based functional layer;

[0106] iv) providing a barrier layer; and

[0107] v) providing an upper anti-reflection layer; and

[0108] vi) providing a dielectric layer comprising an oxynitride of aluminum (Al), zinc (Zn) and tin (Sn), wherein the dielectric layer comprises at least 5 atomic % aluminum; and wherein any portion of the barrier layer in direct contact with the silver-based functional layer is deposited by sputtering in an atmosphere containing less than 5 volume % oxygen.

[0109] The invention is not limited to a specific method of producing the coating. However, it is particularly preferred that at least one of the layers and most preferably all of the layers are applied by magnetron cathode sputtering in DC mode, in pulsed mode, in medium frequency mode or in any other suitable mode, whereby a metal or semiconductor target is sputtered reactively or non-reactively in a suitable sputtering atmosphere. Depending on the material to be sputtered, planar or rotating tubular targets can be used.

[0110] Layers based on oxides of Zn, Ti, ZnSn, InSn, Zr, Al, Sn and / or Si and / or (oxy)nitrides of Si and / or Al can be deposited by non-reactive sputtering. The layers can be sputtered from a ceramic target.

[0111] Layers based on oxides of Zn, Ti, ZnSn, InSn, Zr, Al, Sn and / or Si and / or (oxy)nitrides of Si and / or Al can also be deposited by reactive sputtering. The layers can be sputtered from one or more metal targets.

[0112] The coating process is preferably carried out by setting appropriate coating conditions so as to keep any oxygen (or nitrogen) defects of any oxide (or nitride) layer of the anti-reflective layer of the coating low to achieve high stability of the transmittance and color of the coated glass substrate during heat treatment.

[0113] The light transmittance values ​​mentioned in the specification are usually specified with reference to a coated glass substrate comprising a 4 mm thick standard float glass substrate which, without coating, has a light transmittance T in the 90% area. L .

[0114] While a neutral reflection and transmission color of the coated glass substrate is generally targeted, the color of the coated glass substrate according to the present invention can be varied widely by appropriate adjustment of the thickness of the individual layers, depending on the desired visual appearance of the product.

[0115] The thermal stability of the coated glass substrate according to the invention is reflected in the fact that the coated glass substrates after the heat treatment do not show unacceptable haze levels. If a large increase in haze values ​​(haze scan) is detected during the heat treatment, it indicates that the coating is beginning to be damaged. The mechanical durability of the coated glass substrate according to the invention can be illustrated by the performance in the oil friction test.

[0116] According to a third aspect of the present invention, there is provided a multiple glazing unit incorporating a coated glass substrate according to the first aspect of the present invention or prepared by a method according to the second aspect of the present invention. In addition, the multiple glazing unit according to the third aspect of the present invention may be a laminated glazing unit or an insulating glazing unit.

[0117] Furthermore, all features and preferences relating to the coated glass substrate and layer sequence of the first aspect of the invention, including for example but not limited to details of the lower anti-reflection layer, the upper anti-reflection layer, the silver-based functional layer, the barrier layer and the dielectric layer, are also preferred for the second and third aspects of the invention.

[0118] The invention will now be explained in more detail with reference to the following non-limiting examples.

[0119] Regarding the embodiments, Figure 1 The haze scan and scratch load values ​​of Examples 2 to 7 are relative to AlZnSnO x N y Graphical representation of the atomic % of Al in .

[0120] A series of experiments were conducted to evaluate the effect of using a dielectric layer comprising oxynitrides of aluminum (Al), zinc (Zn) and tin (Sn) containing at least 5 atomic % aluminum in a stack sequence deposited on a float glass substrate.

[0121] A series of coatings (referred to as a stack) is deposited on a float glass substrate. The coating includes at least one silver-based coating. The layers of the series are identified in Tables 1, 2 and 3.

[0122] For all examples, the coatings were deposited on 4 mm thick standard float glass substrates in the 90% transmittance region using single or dual magnetrons equipped with MF-AC and / or DC magnetron (or pulsed DC) power supplies.

[0123] Zinc and tin oxides (ZnSnO) were reactively sputtered from a zinc-tin target (Zn:Sn weight ratio of about 50:50) in an argon / oxygen (Ar / O2) sputtering atmosphere. x ) dielectric layer.

[0124] Titanium oxide (TiO) is deposited from a metallic titanium (Ti) target in an argon / oxygen (Ar / O2) sputtering atmosphere. x )layer.

[0125] The ZnO:Al growth-promoting top layer of the lower antireflection layer was sputtered from an Al-doped Zn target (aluminum (Al) content of about 2 wt %) in an Ar / O2 sputtering atmosphere containing less than 5 vol % oxygen.

[0126] Without any external oxygen and with a residual oxygen partial pressure below 10 -5 The functional layer consisting essentially of pure silver (Ag) in all examples was sputtered from a silver target in an Ar sputtering atmosphere at mbar.

[0127] Conductive ZnO in an Ar / O2 sputtering atmosphere containing less than 5% oxygen by volume x A barrier layer of Al-doped zinc oxide (ZnO:Al) is sputtered from an Al target above the silver-based functional layer.

[0128] In an argon / nitrogen (Ar / N2) sputtering atmosphere containing only residual oxygen, a mixed Si 90 Al 10 Target reactive sputtering of mixed silicon aluminum nitride (Si 90 Al 10 N x )layer.

[0129] The AlN layer was reactively sputtered from an Al target in an argon / nitrogen (Ar / N2) sputtering atmosphere containing only residual oxygen.

[0130] Two aluminum targets and a conductive ceramic mixed zinc tin oxide (ZnSnO x ) target to co-sputter a mixed aluminum, zinc, tin, and oxynitride layer.

[0131] Tables 1, 2 and 3 provide details of the coating sequence, wherein the geometric thickness of each layer is provided in nanometers (nm) in brackets. For the coated glass substrate comparative examples and the coated glass substrate examples according to the present invention, each example was tested to determine:

[0132] Outermost layer metal content, haze scan, oil friction test value, sliding angle test value, scratch load test value, T of glass substrate before heat treatment L %-Percentage (%) transmittance value, ΔT L - change in percent (%) transmittance after heat treatment, RsAD - sheet resistance before heat treatment, Rs HT - sheet resistance after heat treatment, ΔRs (ohms / square) - change in thermal resistance, and TΔE* - which is a measure of the change in transmission color after heat treatment.

[0133] For each example, the layers were deposited onto a glass substrate in the order shown, starting with the layer at the top of each column.

[0134] Table 1

[0135]

[0136] Table 2

[0137]

[0138] Table 3

[0139]

[0140] The methods used to collect the data in Tables 1, 2, and 3 are described below.

[0141] Oil rub test - The oil rub test is used to simulate the effect of the cutting oil used to cut the glass substrate on the mechanical robustness of the coating. Coated glass substrates that cannot withstand the oil rub test are difficult to process and are not suitable for most practical applications. A felt pad with an area of ​​1.2×1.2 cm immersed in microscope oil with a refractive index of 1.52 (1.515 to 1.517) is used to rub the coated samples defined in Tables 1, 2 and 3. The samples are subjected to 500 cycles with a load of 1,000 grams at a rate of 37 cycles per minute. The oil-rubbed samples are then evaluated on a perfection scale of 0 (perfect, no damage) to 9 (part of the coating stack is completely removed) using an internal evaluation system. Scores of 6 or less are preferred.

[0142] Thermal Treatability Test - Immediately after deposition of all coatings in each example, the coating stack parameters (such as haze scan, sheet resistance (Rs), transmittance (T L )) and color coordinates. The sample was then heat treated in a 650°C zone for 5 minutes. Thereafter, the haze scan values, sheet resistance (Rs), percent transmittance (T L ) and color coordinates, and calculate the change in transmittance after heat treatment (ΔT L ) and the change in transmittance color (TΔE*). The measured results are also provided in Tables 1, 2 and 3 above.

[0143] The percentage (%) change in light transmittance (ΔT) of the coated glass substrate in each example after heat treatment L ) are derived from measurements according to EN 140, the details of which are incorporated herein by reference.

[0144] Sheet Resistance / Change in Sheet Resistance - For Comparative Examples 1 and 8 and Examples 2 to 7 and 9 to 12, sheet resistance measurements were performed using a NAGYSRM-12. This device uses an inductor to generate eddy currents in a 100 mm x 100 mm coated sample. This generates a measurable magnetic field, the magnitude of which is related to the resistivity of the sample. Using this method, the sheet resistance can be calculated. The instrument was used to measure the sheet resistance of the sample before and after heat treatment at 650°C for 5 minutes.

[0145] Color Properties - The color properties of each sample in Tables 1, 2 and 3 were measured and reported using established CIE LAB L*, a*, b* coordinates (e.g., as described in paragraphs

[0030] and

[0031] of WO 2004 / 063111 A1, incorporated herein by reference). Change in Transmittance Color after Heat Treatment, TΔE* = ((Δa*) 2 +(Δb*) 2 +(ΔL*) 2 ) 1 / 2, where ΔL*, Δa* and Δb* are the differences in the color values ​​L*, a*, b* of the coated glass substrate, respectively, before and after the heat treatment. ΔE* values ​​of less than 3 (e.g. 2 or 2.5) are preferred for layer sequences with one silver-based functional layer and represent a low and practically insignificant color change caused by the heat treatment. For layer sequences comprising two or more silver-based functional layers, lower TΔE* values ​​indicate the stability of the sequence; the lower the TΔE* value, the better the result and appearance of the coated glass substrate.

[0146] Haze Scan - A haze scoring system was applied to each of the examples in Tables 1, 2, and 3. The quality assessment system described below was also used to more clearly distinguish the visual quality of the coatings under bright light conditions; properties not fully reflected by the standard haze value were measured according to ASTM D1003-61.

[0147] The evaluation system takes into account the more macroscopic effects of visible defects in the coating, which cause local color changes when the coating is damaged or imperfect (haze scans in Tables 1, 2 and 3). The evaluation analyzes light levels in images of heat-treated samples acquired using fixed lighting conditions and geometry.

[0148] In order to generate an image for calculating the haze scan value, the sample is placed in a black box 30 cm away from the camera lens. The standard 1200 lumen light irradiation sample is used with a brightness of 2400 to 2800 Lux (as measured at the sample position). The sample is then photographed using standard aperture size and exposure length. The grayscale of each pixel in the resulting image is then recorded, wherein a value of 0 represents black, and a value of 255 represents white. The statistical analysis of these values ​​is carried out to provide an overall assessment of the sample haze, referred to in this article as haze scan value. The lower the haze scan value recorded, the more excellent the result.

[0149] Sliding Angle Test – The sliding angle measurement provides an indication of the coefficient of friction of the outermost layer of the coating. To complete the test, the sample is placed on top of a flat steel bed and a block with two felt pads attached to the bottom is placed on top of the sample so that the pads are in contact with the sample. The angle of the plate is tilted until the block slides off the sample, creating the sliding angle.

[0150] Scratch Load Test – The scratch load test is a measure of a coating’s ability to resist scratching. The test is performed using a durometer with a tungsten carbide tip. The tip is dragged across the surface in multiple adjacent locations. The process is repeated with increasing loads applied to the durometer until three significant scratches are observed. Significant scratches are defined as continuous scratches or significant amounts of material removed from the coating. Higher loads indicate improved scratch resistance.

[0151] Summary of results

[0152] Comparative Example 1 includes an AlN layer in the upper antireflection layer located near the first silver-based functional layer. x and ZnSnO x Comparative Example 1 provides good results for haze scan values ​​and mechanical robustness tests. However, Comparative Example 1 has AlN in the upper antireflection layer. x Layer and ZnSnO x Comparative Example 1 therefore does not solve the object of the present invention, namely to reduce the number of coating layers in a stacking sequence and thereby to reduce the investment costs required to produce such a coating sequence.

[0153] Likewise, Comparative Example 8 includes a stack of layers, the topmost of which is ZnSnO x Dielectric layer but lack of AlN x Comparative Example 8 showed poor performance in terms of haze scan value, indicating that ZnSnO x The single layer is not the AlN in Comparative Example 1. x and ZnSnO x A suitable single layer alternative to a double layer.

[0154] Examples 2 to 7 and 9 to 12 according to the present invention contain AlZnSnO x N y The layer replaces the AlN of Comparative Example 1 x With ZnSnO x The amounts of aluminum (Al), zinc (Zn) and tin (Sn) in each of Examples 2 to 7 and 9 to 12 are different.

[0155] All examples according to the present invention showed acceptable optical properties, with transmission values ​​greater than 79%, a change in transmission value less than 3.5 after heat treatment, and a change in color value less than 3.5 after heat treatment. In addition, all examples showed acceptable electrical properties, with sheet resistance values ​​less than 7 ohms / square, and a change in sheet resistance value less than 2.5 after heat treatment.

[0156] Regarding the haze scan results, all Examples 2 to 7 and 9 to 12 according to the present invention provided acceptable values ​​of about 200 or less. Figure 1 As shown in , particular improvements in haze scans were observed for Examples 3 and 4 (relative to the values ​​obtained for Comparative Example 1 in Table 1), and Example 2 also provided acceptable haze scan values. Example 9 in Table 3 also provided acceptable haze scan values.

[0157] Figure 1 It is also shown that for the scratch load test, Example 2 exhibits particularly good mechanical durability, with a value of 1.0. Example 2 thus provides a good compromise, where durability is desired over a reduction in haze.

[0158] Therefore, it can be seen from the above results that the coated glass substrate of the present invention provides good heat treatability and mechanical durability, having AlZnSnO in the upper antireflection layer. x N y A single dielectric layer (wherein the amount of aluminum in the layer is at least 5 atomic %).

[0159] According to the test of simulating use, processing and handling conditions, the coated glass substrate of the present invention also shows low level of visible damage.In addition, the coated glass substrate shows high light transmittance and low emissivity and / or good solar control properties, and the optical properties remain stable even after heat treatment.

[0160] The coated glass substrate according to the present invention may be suitable for architectural glazing, such as in buildings, including insulating glazing units and facades. Alternatively, the coated glass substrate according to the present invention may be suitable for vehicle glazing, such as passenger cars, public transportation carriages and buses, trucks and ships or aircraft, including windshields, rear windows, top lights, side lights and side windows.

Claims

1. A coated glass substrate comprising at least the following layers in order starting from a glass substrate: a lower anti-reflection layer; Silver-based functional layer; Barrier layer; and Upper anti-reflection layer, The upper anti-reflection layer comprises: A dielectric layer of an oxynitride of aluminum (Al), zinc (Zn) and tin (Sn), containing at least 5 atomic % aluminum (Al). 2 . The coated glass substrate of claim 1 , wherein the dielectric layer of oxynitride of aluminum (Al), zinc (Zn), and tin (Sn) comprises up to 45 atomic % aluminum.

3. The coated glass substrate of claim 1 or claim 2, wherein the dielectric layer of oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) comprises a thickness of 10 to 50 nm.

4. The coated glass substrate of claim 1 or claim 2, wherein the dielectric layer of oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) comprises at most 30 atomic % zinc and at most 15 atomic % tin.

5. The coated glass substrate of claim 1 or claim 2, wherein the barrier layer is in direct contact with the silver-based functional layer.

6. The coated glass substrate of claim 1 or claim 2, wherein the barrier layer has a thickness of 1 to 10 nm and comprises a NiCrO-based x Or a layer of zinc (Zn) oxide.

7. The coated glass substrate of claim 1, wherein the lower anti-reflection layer comprises, in order from the glass substrate: a layer based on oxides of zinc (Zn) and tin (Sn) or oxide of tin (Sn); and A layer based on zinc (Zn) oxide. 8 . The coated glass substrate of claim 7 , wherein the layer based on zinc (Zn) and tin (Sn) oxide or tin (Sn) oxide has a thickness of 0.5 to 15 nm, or 12 to 20 nm. 9 . The coated glass substrate of claim 8 , wherein the lower anti-reflection layer further comprises a separation layer between the layer based on zinc (Zn) and tin (Sn) oxide or tin (Sn) oxide and the layer based on zinc (Zn) oxide. 10 . The coated glass substrate of claim 9 , wherein the separation layer has a thickness of 0.5 to 6 nm.

11. The coated glass substrate of claim 9 or claim 10, wherein the separation layer comprises: Metal oxides; and / or Silicon and / or aluminum nitrides, and / or silicon and / or aluminum oxynitrides; and / or Alloys of silicon and / or aluminium. 12 . The coated glass substrate of claim 11 , wherein when the separation layer is based on a metal oxide, the metal oxide comprises an oxide of zinc (Zn) and / or an oxide of titanium (Ti).

13. The coated glass substrate of claim 11, wherein the separation layer further comprises one or more other chemical elements selected from at least one of the following elements: Ti, V, Mn, Co, Cu, Zn, Zr, Hf, Al, Nb, Ni, Cr, Mo, Ta, Si, or an alloy based on at least one of these materials.

14. The coated glass substrate according to any one of claims 7 to 10 and 12, wherein the lower anti-reflection layer further comprises a base layer between the glass substrate and the layer based on zinc (Zn) and tin (Sn) oxide or tin (Sn) oxide, and wherein the base layer comprises: Silicon and / or aluminum nitrides, and / or silicon and / or aluminum oxynitrides; and / or Alloys of silicon and / or aluminium; and Wherein the base layer comprises a thickness of 20 to 40 nm. 15 . The coated glass substrate of claim 14 , wherein the base layer is in direct contact with a layer based on zinc (Zn) and tin (Sn) oxide or tin (Sn) oxide.

16. The coated glass substrate of any one of claims 7 to 10, 12 and 15, wherein the zinc (Zn) oxide-based layer in the lower anti-reflection layer comprises a thickness of 2 to 15 nm. 17 . The coated glass substrate according to claim 7 , wherein the zinc (Zn) oxide-based layer in the lower anti-reflection layer is in direct contact with the silver-based functional layer.

18. The coated glass substrate of any one of claims 1 to 2, 7 to 10, 12 and 15, wherein the silver-based functional layer has a thickness of 5 to 20 nm.

19. The coated glass substrate of any one of claims 1 to 2, 7 to 10, 12 and 15, wherein the upper anti-reflective layer comprises: i) a layer based on oxides of zinc (Zn) and tin (Sn) or oxide of tin (Sn); and ii) A layer based on zinc (Zn) oxide. 20 . The coated glass substrate of claim 19 , wherein the layer based on zinc (Zn) and tin (Sn) oxide or tin (Sn) oxide in the upper dielectric layer has a thickness of 1 to 10 nm. 21 . The coated glass substrate of claim 19 , wherein the zinc (Zn) oxide-based layer in the upper dielectric layer has a thickness of 1 to 10 nm.

22. The coated glass substrate of any one of claims 1 to 2, 7 to 10, 12, 15, 20 and 21, wherein the substrate comprises more than one silver-based functional layer, and wherein each silver-based functional layer is separated from an adjacent silver-based functional layer by an intervening central antireflective layer.

23. The coated glass substrate of any one of claims 1 to 2, 7 to 10, 12, 15, 20 and 21, further comprising at least one additional layer in the upper anti-reflection layer, wherein the at least one additional layer is located above or below the dielectric layer of oxynitride of aluminum (Al), zinc (Zn) and tin (Sn) containing at least 5 atomic % of aluminum (Al); and wherein the at least one additional layer comprises: a layer based on oxides of zinc (Zn) and tin (Sn) or an oxide of tin (Sn); and / or a layer based on oxide of zirconium (Zr).

24. A method of making a coated glass substrate according to any one of claims 1 to 23, comprising: i) providing a glass substrate; ii) providing a lower anti-reflection layer; iii) providing a silver-based functional layer; iv) providing a barrier layer; and v) providing an upper anti-reflection layer; and vi) providing a dielectric layer comprising an oxynitride of aluminum (Al), zinc (Zn) and tin (Sn), wherein the dielectric layer comprises at least 5 atomic % aluminum; and wherein any portion of the barrier layer in direct contact with the silver-based functional layer is deposited by sputtering in an atmosphere containing less than 5 volume % oxygen.

25. Multiple glazing unit comprising a coated glass substrate according to any one of claims 1 to 23 and / or produced by the method of claim 24.