Halogen-free flame retardant polymer composition

By using maleic anhydride grafting compatibilizer and crystalline block composite in HFFR cable sheath, the ESCR, tensile strength and elongation of break of HFFR cable sheath are improved, and traditional HFFR cable sheath is solved in non-existent Problem of insufficient mechanical characteristics in traditional applications.

CN114746501BActive Publication Date: 2024-12-06DOW GLOBAL TECHNOLOGIES LLC
View PDF 29 Cites 0 Cited by

Patent Information

Application Number
CN202080084338.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-12-18
Filing Date
2020-12-07
Publication Date
2024-12-06
Estimated Expiration
2040-12-07

AI Technical Summary

Technical Problem

Traditional HFFR cable sheath compositions are difficult to meet mechanical characteristics such as environmental stress cracking, moisture exposure and temperature fluctuations in non-traditional applications due to high filler loads.

Method used

By using maleic anhydride grafted compatible agent in the HFFR cable sheath, the polyolefin elastomer is compatible with the HFFR filler and combined with the crystalline block composite compatibilizer in the polypropylene and polyolefin elastomer to improve polymerization The compatibility and adhesion of the phases can improve ESCR, tensile strength, elongation of break and hot knife indentation characteristics.

Benefits of technology

Achieved that HFFR cable sheath exhibits ESCR of more than 1000 hours, less than 50% hot knife indentation, more than 70% elongation of break and tensile strength of 10MPa or greater under high packing load conditions, suitable for Applications outside conventional HFFR cable sheath.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003678586080000191
    Figure BDA0003678586080000191
  • Figure BDA0003678586080000211
    Figure BDA0003678586080000211
  • Figure BDA0003678586080000212
    Figure BDA0003678586080000212
Patent Text Reader

Abstract

The present invention discloses a polymer composition, which comprises, based on the weight percentage of the polymer composition: (a) 10 wt% to 30 wt% of a polyolefin elastomer; (b) 1 wt% to 20 wt% of a polypropylene-based polymer; (c) greater than 1 wt% to 20 wt% of a crystalline block composite; (d) 1 wt% to 10 wt% of a maleated polyolefin elastomer; and (e) 40 wt% to 80 wt% of a halogen-free flame retardant filler.
Need to check novelty before this filing date? Find Prior Art

Description

Background Art Technical Field

[0001] The present disclosure relates generally to polymer compositions, and more particularly to compatibilized polymer compositions including hydrated mineral fillers. Background Art

[0003] Halogen-free flame retardant (HFFR) cable jacket compositions based on polyolefins can be used in a variety of applications where flame retardancy of the insulation / jacket material is important. Flame retardancy is achieved by adding hydrated mineral fillers, which dilute the concentration of flammable polymer materials and decompose below the degradation temperature of the polymer when exposed to heat. The decomposition of the hydrated mineral filler releases water, thereby removing heat from the source of fire. Conventional HFFR cable jacket compositions are used indoors, in buildings, trains, cars, or anywhere people may be present.

[0004] There are many disadvantages to using hydrated mineral fillers in polyolefin wire and cable formulations, most of which are due to the relatively high levels of fillers required to meet flame retardant specifications. Filler loadings of 60 weight percent (wt%) or 65 wt% in polyolefins are not uncommon. This loading of filler affects the properties of HFFR cable jacket compositions and results in compounds with high density, limited flexibility, and reduced mechanical properties such as elongation at break.

[0005] Blends of different polymers must generally be used to allow such high filler loading to be incorporated while maintaining some mechanical properties. For example, polypropylene is generally used to increase the strength of cable jacket compositions, while polyolefin elastomers allow filler loading. Compatibilizers are used in systems where different polymers are blended together to increase the mixing and adhesion of polymers. For example, WO2017100175 utilizes ethylene-propylene diblock copolymers to make propylene and high-density polyethylene (HDPE) systems compatible. However, considering that the polymer phase of HFFR cable jackets is a minority phase, conventional attempts and understandings teach that compatibilization should involve increasing the compatibility and adhesion between the polymer phase and the hydrated mineral filler. For example, US20100319960A1 discloses HFFR, olefin multi-block interpolymers, which utilize compatibilizers based on polar monomers to couple HFFR and olefin multi-block interpolymers together. Other other multipolymer HFFR systems are considered to be advantages without polymer phase compatibilizers. For example, WO2011079457A1 explains that "advantageously, the compositions of the present invention do not require a compatibilizer (e.g., a functional polymer), and in embodiments, no such compatibilizer is included between the PP and thermoplastic elastomer components."

[0006] As the application of HFFR cable jackets begins to expand into non-traditional areas, mechanical properties that were once considered irrelevant to HFFR cable jackets have become relevant. For example, environmental stress cracking (ESCR) is a mechanical property associated with cable jackets exposed to moisture (e.g., outdoor and / or underground cables), lack of moisture (e.g., in desert environments), and wide temperature fluctuations. Therefore, in addition to other properties such as ESCR, mechanical properties (e.g., tensile strength and elongation at break), and total composition cost, traditional properties of HFFR cable jackets such as "hot press" or "hot knife" indentation tests must also be evaluated. Complicating this balance of properties is the fact that improvements in one property typically compromise another, making it difficult to achieve an acceptable balance of properties.

[0007] Thus, it is surprising to find cable jacket compositions having HFFR content of 40 wt% or greater that exhibit ESCR greater than 1000 hours, hot knife indentation less than 50%, elongation at break greater than 70%, and tensile strength of 10 MPa or greater. Summary of the invention

[0008] The present invention provides a polymer composition having a HFFR filler content of 40 wt% or more, which exhibits an ESCR of greater than 1000 hours, a hot knife indentation of less than 50%, an elongation at break of greater than 70%, and a tensile strength of 10 MPa or more. The present invention is particularly useful for cable jacketing.

[0009] The present invention is to find that although polymer phase is the minority phase in HFFR cable composition, the effective compatibility of multiple different polymer types in polymer phase effectively provides the result of the balance of the characteristics required for critical environment. By utilizing the compatibilizer grafted with maleic anhydride to make polyolefin elastomer compatible with HFFR filler, HFFR filler is attached to polymer phase. By using crystalline block composite compatibilizer in the polypropylene and polyolefin elastomer polymer phase of HFFR cable sheath, polyolefin elastomer is more effectively attached to polypropylene phase. Surprisingly, instead of simply improving the single characteristic of the resulting composition, ESCR, tensile strength, elongation at break and hot knife indentation characteristics are all improved. Therefore, HFFR cable sheath of the present invention can be used in applications beyond conventional HFFR cable sheath.

[0010] The invention is particularly useful in sheathing of cables.

[0011] According to a first feature of the present disclosure, the polymer composition comprises, by weight percentage of the polymer composition: (a) 10 wt% to 30 wt% of a polyolefin elastomer; (b) 1 wt% to 20 wt% of a polypropylene-based polymer; (c) greater than 1 wt% to 20 wt% of a crystalline block composite; (d) 1 wt% to 10 wt% of a maleated polyolefin elastomer; and (e) 40 wt% to 80 wt% of a halogen-free flame retardant filler. DETAILED DESCRIPTION

[0012] As used herein, the term "and / or," when used in a list of two or more items, means that any one of the listed items may be used alone, or any combination of two or more of the listed items may be used. For example, if a composition is described as comprising components A, B, and / or C, the composition may contain A alone; B alone; C alone; A and B in combination; A and C in combination; B and C in combination; or A, B, and C in combination.

[0013] Unless otherwise indicated, all ranges are inclusive.Subscript values ​​in polymer formulas refer to the molar average number of units per molecule of the designated component of the polymer.

[0014] Test methods refer to the most recent test methods as of the priority date of this document unless the date is expressed as a two-digit number with a hyphen in the test method number. Reference to a test method includes reference to both the testing association and the test method number. Test method organizations are referenced by one of the following abbreviations: ASTM refers to ASTM International (formerly the American Society for Testing and Materials); EN refers to European Standards; DIN refers to the German Institute for Standardization; ISO refers to the International Organization for Standardization, and IEC refers to the International Electrotechnical Commission.

[0015] As used herein, unless otherwise indicated, the term weight percent ("wt%") refers to the weight percent of a component based on the total weight of the polymer composition.

[0016] As used herein, an "elastomer" is a rubbery polymer having an elastic modulus of about 68.95 MPa (10,000 psi) or less and an elongation greater than 200% at 23°C using the method of ASTM D638-72 in the uncrosslinked state.

[0017] As used herein, the term "halogen-free" is an object or material containing 2000 mg / kg or less of halogen, as measured by ion chromatography (IC). Halogen content less than this amount is considered insignificant to the efficacy of the composition as a wire or cable covering and can therefore be referred to as "halogen-free".

[0018] Polymer composition

[0019] The polymer composition of the present invention comprises a polyolefin elastomer, a polypropylene-based polymer, a crystalline block composite, a maleated polyolefin elastomer; and a halogen-free flame retardant filler.

[0020] Polyolefin elastomer

[0021] Polyolefin elastomers are elastomers that may include ethylene-based elastomers / plastomers, ethylene block copolymers, and propylene-based elastomers.

[0022] The polyolefin elastomer may comprise an α-olefin block copolymer. An "olefin block copolymer" refers to a polymer comprising two or more chemically distinct regions or segments (referred to as "blocks") joined in a linear manner rather than in a pendant or grafted manner, i.e., a polymer comprising chemically distinct units joined end-to-end with respect to polymerized olefinic (preferably olefinic) functional groups. The blocks differ in the amount or type of comonomer incorporated, density, degree of crystallinity, crystallite size attributable to polymers of such composition, type or degree of stereoisomerism (isotactic or syndiotactic), regioregularity or regioirregularity, degree of branching (including long chain branching or hyperbranching), homogeneity, or any other chemical or physical property.

[0023] Suitable monomers for preparing olefin block copolymers may include olefin or diene comonomers. Examples of suitable comonomers include 2 to 30 straight or branched α-olefins. Suitable branched α-olefins may include ethylene, propylene, 1-butene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene and 1-eicosene; 3 to 30, preferably 3 to 20 carbon atoms of cyclic olefins such as cyclopentene, cycloheptene, norbornene, 5-methyl-2-norbornene, tetracyclododecene and 2-methyl-1,4,5,8-dimethanol-1,2,3,4,4a,5, 8,8a-octahydronaphthalene; dienes and polyolefins such as butadiene, isoprene, 4-methyl-1,3-pentadiene, 1,3-pentadiene, 1,4-pentadiene, 1,5-hexadiene, 1,4-hexadiene, 1,3-hexadiene, 1,3-octadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, 1,7-octadiene, ethylidene norbornene, vinyl norbornene, dicyclopentadiene, 7-methyl-1,6-octadiene, 4-ethylidene-8-methyl-1,7-nonadiene and 5,9-dimethyl-1,4,8-decatriene.

[0024] Examples of olefin block copolymers useful as polyolefin elastomers in the practice of the present invention are INFUSE TMD9100, D9500, D9507 or D9530 olefin block copolymers are commercially available from Dow Chemical Company, Midland, Michigan, USA.

[0025] The polyolefin elastomer may comprise an elastomeric ethylene homopolymer or an ethylene and alpha-olefin random copolymer. The alpha-olefin of ethylene and the alpha-olefin copolymer may have 3 to 12 carbon atoms, and preferably 3 to 8 carbon atoms. Preferably, the alpha-olefin is one or more of 1-butene, 1-hexene or 1-octene. The ethylene polymer used in the practice of the present invention may comprise units derived from three or more different monomers. For example, the third comonomer may be another alpha-olefin or diene, such as ethylidene norbornene, butadiene, 1,4-hexadiene or dicyclopentadiene.

[0026] Examples of ethylene polymers useful in the practice of the present invention include homogeneously branched linear ethylene / α-olefin copolymers such as TAFMER from Mitsui Petrochemicals Company Limited, New York, NY, USA. TM Copolymers and Exxon Chemical Company's EXACT TM Copolymers. Examples of homogeneously branched substantially linear ethylene and α-olefin polymers include AFFINITY TM Plastic, ENGAGE TM Elastomer and SEC 39001 ethylene-butene copolymer. The resin of such polyolefin elastomer can be prepared with at least one metallocene catalyst, or a blend of multiple elastomeric resins can be prepared with different metallocene catalysts. In some embodiments, the elastomer is a substantially linear ethylene polymer (SLEP). SLEP and other metallocene-catalyzed elastomers are known in the art, for example US 5,272,236.

[0027] The polyolefin elastomer may have a density of 0.86 grams per cubic centimeter (g / cc) or greater, or 0.87 g / cc or greater, or 0.88 g / cc or greater, or 0.89 g / cc or greater, or 0.90 g / cc or greater, or 0.91 g / cc or greater, or 0.92 g / cc or greater, or 0.93 g / cc or greater, or 0.94 g / cc or greater, or 0.95 g / cc or greater, or 0.96 g / cc or greater, as measured by ASTM D792. c or greater, while 0.97 g / cc or less, or 0.965 g / cc or less, or 0.96 g / cc or less, or 0.95 g / cc or less, or 0.94 g / cc or less, or 0.93 g / cc or less, or 0.92 g / cc or less, or 0.91 g / cc or less, or 0.90 g / cc or less, or 0.89 g / cc or less, or 0.88 g / cc or less, or 0.87 g / cc or less.

[0028] The polyolefin elastomer has a melt flow index (MFI) of 1 gram per ten minutes (g / 10 min) or more, or 2 g / 10 min or more, 3 g / 10 min or more, 4 g / 10 min or more, 5 g / 10 min or more, 6 g / 10 min or more, 7 g / 10 min or more, 8 g / 10 min or more, 9 g / 10 min or more, 10 g / 10 min or more, or 11 g / 10 min or more, or 12 g / 10 min or more, 13 g / 10 min or more, 14 g / 10 min or more, 15 g / 10 min or more, 16 g / 10 min or more, 17 g / 10 min or more, 18 g / 10 min or more, 1 g / 10 min or more, or less, or 10 g / 10 min or less, or 20 g / 10 min or less, or 19 g / 10 min or less, or 18 g / 10 min or less, or 17 g / 10 min or less, or 16 g / 10 min or less, or 15 g / 10 min or less, or 14 g / 10 min or less, or 13 g / 10 min or less, or 12 g / 10 min or less, or 11 g / 10 min or less, or 10 g / 10 min or less, or 9 g / 10 min or less, or 8 g / 10 min or less, or 7 g / 10 min or less, or 6 g / 10 min or less, or 5 g / 10 min or less, or 4 g / 10 min or less, or 3 g / 10 min or less, or 2 g / 10 min or less. MFI is measured according to ASTM D1238 at 190°C and 2.16 kg.

[0029] The polymer composition may comprise 10 wt % or greater, or 11 wt % or greater, or 12 wt % or greater, or 13 wt % or greater, or 14 wt % or greater, or 15 wt % or greater, or 16 wt % or greater, or 17 wt % or greater, or 18 wt % or greater, or 19 wt % or greater, or 20 wt % or greater, or 21 wt % or greater, or 22 wt % or greater, or 23 wt % or greater, or 24 wt % or greater, or 25 wt % or greater, or 26 wt % or greater, or 27 wt % or greater, or 28 wt % or greater, or 29 wt % or greater, while At the same time, 30 weight % or less, or 29 weight % or less, or 28 weight % or less, or 27 weight % or less, or 26 weight % or less, 25 weight % or less, or 24 weight % or less, or 23 weight % or less, or 22 weight % or less, or 21 weight % or less, or 20 weight % or less, or 19 weight % or less, or 18 weight % or less, or 17 weight % or less, or 16 weight % or less, 15 weight % or less, or 14 weight % or less, or 13 weight % or less, or 12 weight % or less, or 11 weight % or less, or less of polyolefin elastomer.

[0030] Polypropylene based polymers

[0031] The polymer composition comprises a propylene-based polymer. As used herein, a "propylene-based polymer" refers to a polymer containing more than 50% by weight of polymerized propylene monomer (based on the total amount of polymerizable monomers) and optionally may contain one or more comonomers. The terms "propylene-based polymer" and "polypropylene" are used interchangeably. Propylene-based polymers include propylene homopolymers and propylene copolymers (meaning units derived from propylene and one or more comonomers). As used herein, a "propylene homopolymer" means a polymer consisting only of polymerized propylene monomers or substantially all of polymerized propylene monomers. As used herein, a "propylene copolymer" means a polymer comprising a monomer derived from polymerized propylene and ethylene and / or one or more other unsaturated comonomers (such as C 4-20 Linear, branched or cyclic α-olefin) units. 4-20Examples of alpha-olefins include 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene and 1-octadecene. For propylene copolymers, the comonomer content is 10 wt % or less, or 5 wt % or less, or 3 wt % or less. Common forms of polypropylene known in the art include homopolymer polypropylene (hPP), random copolymer polypropylene (rcPP), impact copolymer polypropylene (hPP+at least one elastomeric impact modifier) ​​(ICPP) or high impact polypropylene (HIPP), high melt strength polypropylene (HMS-PP), isotactic polypropylene (iPP), syndiotactic polypropylene (sPP) and combinations thereof.

[0032] The polymer composition can include 1 wt % or greater, or 2 wt % or greater, or 3 wt % or greater, or 4 wt % or greater, or 5 wt % or greater, or 6 wt % or greater, or 7 wt % or greater, or 8 wt % or greater, or 9 wt % or greater, or 10 wt % or greater, or 11 wt % or greater, or 12 wt % or greater, or 13 wt % or greater, or 14 wt % or greater, or 15 wt % or greater, or 16 wt % or greater, or 17 wt % or greater, or 18 wt % or greater, or 19 wt % or greater. % or less, or 19 wt % or less, or 18 wt % or less, or 17 wt % or less, or 16 wt % or less, or 15 wt % or less, or 14 wt % or less, or 13 wt % or less, or 12 wt % or less, or 11 wt % or less, or 10 wt % or less, or 9 wt % or less, or 8 wt % or less, or 7 wt % or less, or 6 wt % or less, or 5 wt % or less, or 4 wt % or less, or 3 wt % or less, or 2 wt % or less of polypropylene.

[0033] The propylene-based polymer has an MFI of 1 g / 10 min or more, or 2 g / 10 min or more, 3 g / 10 min or more, 4 g / 10 min or more, 5 g / 10 min or more, 6 g / 10 min or more, 7 g / 10 min or more, 8 g / 10 min or more, 9 g / 10 min or more, 10 g / 10 min or more, or 11 g / 10 min or more, or 12 g / 10 min or more, 13 g / 10 min or more, 14 g / 10 min or more, 15 g / 10 min or more, 16 g / 10 min or more, 17 g / 10 min or more, 18 g / 10 min or more, or 19 g / 10 min or more, and at the same time 10min or less, or 20g / 10min or less, or 19g / 10min or less, or 18g / 10min or less, or 17g / 10min or less, or 16g / 10min or less, or 15g / 10min or less, or 14g / 10min or less, or 13g / 10min or less, or 12g / 10min or less, or 11g / 10min or less, or 10g / 10min or less, or 9g / 10min or less, or 8g / 10min or less, or 7g / 10min or less, or 6g / 10min or less, or 5g / 10min or less, or 4g / 10min or less, or 3g / 10min or less, or 2g / 10min or less. MFI is measured according to ASTM D1238 at 230°C and 2.16kg.

[0034] Polypropylene homopolymers useful in the practice of the present invention are commercially available as H700-12 polypropylene from The Dow Chemical Company, Midland, Michigan, USA or Braskem America, Philadelphia, Pennsylvania, USA. Copolymer polypropylenes (including random copolymer polypropylene resins) useful in the practice of the present invention are commercially available as DS6D82, 6D83K, and C715-12NHP polypropylenes from The Dow Chemical Company, Midland, Michigan, USA. Impact-modified propylene copolymers useful in the practice of the present invention are commercially available as C766-03, C7057-07, C7061-01N, and C706-21NA HP polypropylenes from The Dow Chemical Company, Midland, Michigan, USA.

[0035] Crystalline block composite

[0036] The polymer composition comprises a crystalline block composite. The term "crystalline block composite" ("CBC") refers to a polymer comprising three polymer components:

[0037] (i) a crystalline ethylene polymer (CEP), wherein the ethylene content of the CEP is greater than or equal to 90 mol %, based on the total moles of polymerized monomer units in the CEP;

[0038] (ii) a crystalline alpha-olefin based polymer (CAOP) having an alpha-olefin content greater than 90 mole percent based on the total moles of polymerized monomer units in the CAOP; and

[0039] (iii) a block copolymer comprising a crystalline ethylene block (CEB) and a crystalline α-olefin block (CAOB); and

[0040] wherein the crystalline ethylene block has a melting temperature (Tm) that is the same as or similar to that of the CEP of component (i), and

[0041] wherein the crystalline α-olefin block has a Tm that is the same as or similar to the CAOP of component (ii); and

[0042] Wherein the phrase "same or similar" means an absolute Tm difference of ≤ 5°C as measured using differential scanning calorimetry (DSC) at a temperature ramp rate of 0.1°C to 10°C.

[0043] Methods for preparing CBC and methods for analyzing CBC are described, for example, in U.S. Patent Application Publication Nos. 2011 / 0313106, 2011 / 0313108, and 2011 / 0313108 (all published on Dec. 22, 2011) and in PCT Publication No. WO2014 / 043522A1. Examples of suitable α-olefins include, for example, C3-C10 α-olefins, such as C3, C4, C5, C6, and C8 α-olefins. The α-olefin may be propylene.

[0044] A "crystalline ethylene polymer" ("CEP") contains 90 mole % or more of the polymerized monomer units in the CEP which are ethylene units, wherein any comonomer content is 10 mole % or less of the polymerized monomer units in the CEP.

[0045] "Crystalline alpha-olefin polymer" ("CAOP") is a crystalline polymer containing polymerized alpha-olefin units. The polymerized alpha-olefin units can be 1-propylene. The polymerized alpha-olefin units (e.g., propylene) are present in an amount of 90 mol% or greater, or 93 mol% or greater, or 95 mol% or greater, or 98 mol% or greater, based on the total weight of the crystalline alpha-olefin polymer (propylene). The comonomer can be ethylene. The comonomer content in the CAOP is 10 mol% or less. CAOP with propylene crystallinity has a melting point of 80°C or higher. The CAOP may contain all or substantially all propylene units.

[0046] Other suitable α-olefin units (besides propylene) that can be used in CAOP are those containing 4 to 10 carbon atoms, such as 1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene. Suitable dienes that can be used in CAOP include isoprene, butadiene, 1,4-pentadiene, 1,4-hexadiene, 1,5-hexadiene, 1,7-octadiene, 1,9-decadiene, dicyclopentadiene, methylene-norbornene, 5-ethylidene-2-norbornene, and the like, as well as combinations containing at least one of the foregoing α-olefin units.

[0047] The block copolymer of CBC contains CEB and crystalline alpha olefin block CAOB. In CEB, polymerized ethylene is present in an amount of 90 mol% or more based on the total moles of CEB. The CEB polymer may be polyethylene.

[0048] CAOB includes polypropylene blocks copolymerized with other α-olefin units containing 4 to 10 carbon atoms. The polypropylene is present in the CAOB in an amount of 90 mol% or more based on the total moles of CAOB. The comonomer content in the CAOB is 10 mol% or less based on the total moles of CAOB. CAOB having propylene crystallinity has a melting point of 80°C or higher. In an embodiment, CAOB contains all or substantially all propylene units.

[0049] The CBC may contain propylene, 1-butene or 4-methyl-1-pentene and one or more comonomers. The CBC may contain propylene and ethylene and / or one or more C4–20 α-olefin comonomers in polymerized form, and / or one or more additional copolymerizable comonomers, or the CBC contains 4-methyl-1-pentene and ethylene and / or one or more C4-20 α-olefin comonomers, or the CBC contains 1-butene and ethylene, propylene and / or one or more C5-20 α-olefin comonomers and / or one or more additional copolymerizable comonomers. Additional suitable comonomers are selected from dienes, cyclic olefins and cyclic dienes, halogenated vinyl compounds and vinylidene aromatic compounds. The monomer may be propylene and the comonomer may be ethylene.

[0050] In one embodiment, the CBC can be a propylene-based polymer containing greater than or equal to 50 weight percent of units derived from propylene, based on the total weight of the CBC. The comonomer content in the CBC can be measured using nuclear magnetic resonance (NMR) spectroscopy.

[0051] The MFI of CBC is 1 g / 10 min or more, or 2 g / 10 min or more, 3 g / 10 min or more, 4 g / 10 min or more, 5 g / 10 min or more, 6 g / 10 min or more, 7 g / 10 min or more, 8 g / 10 min or more, 9 g / 10 min or more, 9.5 g / 10 min or more, or 10 g / 10 min or more, or 11 g / 10 min or more, or 12 g / 10 min or more, 13 g / 10 min or more, 14 g / 10 min or more, 15 g / 10 min or more, 16 g / 10 min or more, 17 g / 10 min or more, 18 g / 10 min or more, 19 g / 10 min or more The MFI is measured according to ASTM D1238 at 230°C and 2.16 kg.

[0052] The weight average molecular weight (Mw) of CBC may be 10,000 g / mol or more, or 20,000 g / mol or more, or 30,000 g / mol or more, or 40,000 g / mol or more, or 50,000 g / mol or more, or 60,000 g / mol or more, or 70,000 g / mol or more, or 80,000 g / mol or more, or 90,000 g / mol or more, or 10 0,000 g / mol or more, or 110,000 g / mol or more, or 120,000 g / mol or more, or 130,000 g / mol or more, or 140,000 g / mol or more, or 150,000 g / mol or more, or 160,000 g / mol or more, or 170,000 g / mol or more, or 180,000 g / mol or more, or 190,000 g / mol or more ol or more, and at the same time 200,00 g / mol or less, or 190,000 g / mol or less, or 180,000 g / mol or less, or 170,000 g / mol or less, or 160,000 g / mol or less, or 150,000 g / mol or less, or 140,000 g / mol or less, or 130,000 g / mol or less, or 120,000 g / mol or less, or 110,000 g / mol or less, or 100,000 g / mol or less, or 90,000 g / mol or less, or 80,000 g / mol or less, or 70,000 g / mol or less, or 60,000 g / mol or less, or 50,000 g / mol or less, or 40,000 g / mol or less, or 30,000 g / mol or less, or 20,000 g / mol or less. The weight average molecular weight is measured using gel permeation chromatography.

[0053] The sum of the weight percentages of CEP, CAOP, and block copolymer in the CBC is equal to 100%. The CBC may be 0.5 wt% or more, or 1 wt% or more, or 5 wt% or more, or 10 wt% or more, or 20 wt% or more, or 30 wt% or more, or 40 wt% or more, or 50 wt% or more, or 60 wt% or more, or 70 wt% or more, or 80 wt% or more, while at the same time being 90 wt% or less, or 80 wt% or less, or 70 wt% or less, or 60 wt% or less, or 50 wt% or less, or 40 wt% or less, or 30 wt% or less, or 20 wt% or less, or 10 wt% or less of CEP.

[0054] The CBC may be 0.5 wt % or greater, or 1 wt % or greater, or 5 wt % or greater, or 10 wt % or greater, or 20 wt % or greater, or 30 wt % or greater, or 40 wt % or greater, or 50 wt % or greater, or 60 wt % or greater, or 70 wt % or greater, or 80 wt % or greater, while at the same time being 90 wt % or less, or 80 wt % or less, or 70 wt % or less, or 60 wt % or less, or 50 wt % or less, or 40 wt % or less, or 30 wt % or less, or 20 wt % or less, or 10 wt % or less of the CAOP.

[0055] The CBC may be 0.5 wt % or greater, or 1 wt % or greater, or 5 wt % or greater, or 10 wt % or greater, or 20 wt % or greater, or 30 wt % or greater, or 40 wt % or greater, or 50 wt % or greater, or 60 wt % or greater, or 70 wt % or greater, or 80 wt % or greater, while at the same time being 90 wt % or less, or 80 wt % or less, or 70 wt % or less, or 60 wt % or less, or 50 wt % or less, or 40 wt % or less, or 30 wt % or less, or 20 wt % or less, or 10 wt % or less of a block copolymer.

[0056] The block copolymers of CBC may contain 0.5 wt % or more, or 1 wt % or more, or 5 wt % or more, or 10 wt % or more, or 20 wt % or more, or 30 wt % or more, or 40 wt % or more, or 50 wt % or more, or 60 wt % or more, or 70 wt % or more, or 80 wt % or more, while at the same time having 90 wt % or less, or 80 wt % or less, or 70 wt % or less, or 60 wt % or less, or 50 wt % or less, or 40 wt % or less, or 30 wt % or less, or 20 wt % or less, or 10 wt % or less of crystalline ethylene blocks (CEB). The block copolymers of CBC may contain 0.5 wt % or more, or 1 wt % or more, or 5 wt % or more, or 10 wt % or more, or 20 wt % or more, or 30 wt % or more, or 40 wt % or more, or 50 wt % or more, or 60 wt % or more, or 70 wt % or more, or 80 wt % or more, while at the same time having 90 wt % or less, or 80 wt % or less, or 70 wt % or less, or 60 wt % or less, or 50 wt % or less, or 40 wt % or less, or 30 wt % or less, or 20 wt % or less, or 10 wt % or less of crystalline alpha-olefin blocks (CAOB).

[0057] The CBC may contain (i) CEP, which is a crystalline ethylene / propylene copolymer (CEP); (ii) CAOP, which is an isotactic crystalline propylene homopolymer (iPP); and (iii) a block copolymer containing an iPP block (CAOB) and an ethylene / propylene block (CEB); wherein the block copolymer comprises a diblock having formula (1):

[0058] (CEP)―(iPP) Formula (1).

[0059] The polymer composition can include 1 wt % or greater, or 2 wt % or greater, or 3 wt % or greater, or 4 wt % or greater, or 5 wt % or greater, or 6 wt % or greater, or 7 wt % or greater, or 8 wt % or greater, or 9 wt % or greater, or 10 wt % or greater, or 11 wt % or greater, or 12 wt % or greater, or 13 wt % or greater, or 14 wt % or greater, or 15 wt % or greater, or 16 wt % or greater, or 17 wt % or greater, or 18 wt % or greater, or 19 wt % or greater, While at the same time 20 wt % or less, or 19 wt % or less, or 18 wt % or less, or 17 wt % or less, or 16 wt % or less, 15 wt % or less, or 14 wt % or less, or 13 wt % or less, or 12 wt % or less, or 11 wt % or less, or 10 wt % or less, or 9 wt % or less, or 8 wt % or less, or 7 wt % or less, or 6 wt % or less, or 5 wt % or less, or 4 wt % or less, or 3 wt % or less, or 2 wt % or less of crystalline block composites.

[0060] Maleated polyolefin elastomer

[0061] The polymer composition comprises a maleated polyolefin elastomer. As used herein, the term "maleated" means an elastomer (e.g., a polyolefin elastomer) that has been modified to incorporate a maleic anhydride monomer. The maleated polyolefin elastomer can be formed by copolymerization of maleic anhydride monomer with ethylene and other monomers (if present) to prepare an interpolymer with maleic anhydride incorporated into the polymer backbone. Additionally or alternatively, maleic anhydride can be graft polymerized to the polyolefin elastomer. The maleated polyolefin elastomer can be any of the polyolefin elastomers previously discussed.

[0062] The maleated polyolefin elastomer may have a density of 0.86 g / cc or greater, or 0.87 g / cc or greater, or 0.88 g / cc or greater, or 0.89 g / cc or greater, or 0.90 g / cc or greater, or 0.91 g / cc or greater, or 0.92 g / cc or greater, or 0.93 g / cc or greater, or 0.94 g / cc or greater, or 0.95 g / cc or greater, or 0.96 g / cc or greater, as measured by ASTM D792. or greater, while at the same time 0.97 g / cc or less, or 0.965 g / cc or less, or 0.96 g / cc or less, or 0.95 g / cc or less, or 0.94 g / cc or less, or 0.93 g / cc or less, or 0.92 g / cc or less, or 0.91 g / cc or less, or 0.90 g / cc or less, or 0.89 g / cc or less, or 0.88 g / cc or less, or 0.87 g / cc or less.

[0063] The maleated polyolefin elastomer has an MFI of 1 g / 10 min or more, or 2 g / 10 min or more, 3 g / 10 min or more, 4 g / 10 min or more, 5 g / 10 min or more, 6 g / 10 min or more, 7 g / 10 min or more, 8 g / 10 min or more, 9 g / 10 min or more, 10 g / 10 min or more, or 11 g / 10 min or more, or 12 g / 10 min or more, 13 g / 10 min or more, 14 g / 10 min or more, 15 g / 10 min or more, 16 g / 10 min or more, 17 g / 10 min or more, 18 g / 10 min or more, or 19 g / 10 min or more, while the same 10min or less, or 20g / 10min or less, or 19g / 10min or less, or 18g / 10min or less, or 17g / 10min or less, or 16g / 10min or less, or 15g / 10min or less, or 14g / 10min or less, or 13g / 10min or less, or 12g / 10min or less, or 11g / 10min or less, or 10g / 10min or less, or 9g / 10min or less, or 8g / 10min or less, or 7g / 10min or less, or 6g / 10min or less, or 5g / 10min or less, or 4g / 10min or less, or 3g / 10min or less, or 2g / 10min or less. MFI is measured according to ASTM D1238 at 190°C and 2.16kg.

[0064] The maleic anhydride content of the maleated polyolefin elastomer may be 0.25 wt% or more, or 0.50 wt% or more, or 0.75 wt% or more, or 1.00 wt% or more, or 1.25 wt% or more, or 1.50 wt% or more, or 1.75 wt% or more, or 2.00 wt% or more, or 2.25 wt% or more, or 2.50 wt% or more, or 2.75 wt% or more, while 3.00 wt% or less, 2.75 wt% or less, or 2.50 wt% or less, or 2.25 wt% or less, or 2.00 wt% or less, or 1.75 wt% or less, or 1.50 wt% or less, or 1.25 wt% or less, or 1.00 wt% or less, or 0.75 wt% or less, or 0.5 wt% or less, based on the total weight of the maleated polyolefin elastomer. Maleic anhydride concentration is determined by titration analysis.By utilizing dry resin to carry out titration analysis, and use 0.02N KOH titration, to determine the amount of maleic anhydride.Dry polymer is titrated by dissolving 0.3 to 0.5 gram of maleated polymer in the refluxing xylene of about 150mL.After dissolving completely, deionized water (four drops) is added to the solution, and the solution is refluxed for 1 hour.Next, 1% thymol blue (several drops) is added to the solution, and the solution is excessively titrated with the ethanolic solution of 0.02N KOH, as shown in the purple formation.Then the solution is back titrated to the yellow end point with the isopropanol solution of 0.05N HCl.

[0065] The polymer composition may comprise 1 wt % or more, or 2 wt % or more, or 3 wt % or more, or 4 wt % or more, or 5 wt % or more, or 6 wt % or more, or 7 wt % or more, or 8 wt % or more, or 9 wt % or more, while at the same time 10 wt % or less, or 9 wt % or less, or 8 wt % or less, or 7 wt % or less, or 6 wt % or less, or 5 wt % or less, or 4 wt % or less, or 3 wt % or less, or 2 wt % or less of maleated polyolefin elastomer.

[0066] An example of a suitable commercially available maleated polyolefin elastomer is AMPLIFY TM GR216.

[0067] Halogen-free flame retardant (HFFR) filler

[0068] The halogen-free flame retardant of polymer composition can suppress, contain or delay flame generation.The example of the halogen-free flame retardant used in the composition according to the present disclosure includes but is not limited to metal hydroxide, red phosphorus, silicon dioxide, aluminum oxide, aluminum hydroxide, magnesium dihydroxide, aluminum trihydrate, aluminum hydroxide, titanium oxide, carbon nanotube, talcum, clay, organic modified clay, calcium carbonate, zinc borate, antimony trioxide, wollastonite, mica, ammonium octamolybdate, glass frit, hollow glass microsphere, expansion compound, expanded graphite, and their combination.In one embodiment, halogen-free flame retardant can be selected from the group consisting of aluminum hydroxide, magnesium hydroxide, calcium carbonate and their combination.Halogen-free flame retardant can optionally be surface treated (coated) with saturated or unsaturated carboxylic acid or metal salt of the acid with 8 to 24 carbon atoms or 12 to 18 carbon atoms. Exemplary surface treatments are described in US 4,255,303, US 5,034,442, US 7,514,489, US 2008 / 0251273 and WO2013 / 116283. Alternatively, the acid or salt may be added to the composition in similar amounts without using a surface treatment procedure. Other surface treatments known in the art may also be used, including silanes, titanates, phosphates and zirconates.

[0069] Commercially available examples of halogen-free flame retardants suitable for use in the compositions according to the present disclosure include, but are not limited to: APYRAL FR, available from Nabaltec AG. TM 40CD aluminum hydroxide, MAGNIFIN available from Magnifin Magnesiaprodukte GmbH & Co KG TM H5 magnesium hydroxide, and combinations thereof.

[0070] The polymer composition can have 40 wt % or greater, or 42 wt % or greater, or 44 wt % or greater, or 46 wt % or greater, or 48 wt % or greater, or 50 wt % or greater, or 52 wt % or greater, or 54 wt % or greater, or 56 wt % or greater, or 58 wt % or greater, or 60 wt % or greater, or 62 wt % or greater, or 64 wt % or greater, or 66 wt % or greater, or 68 wt % or greater, or 70 wt % or greater, or 72 wt % or greater, or 74 wt % or greater, or 76 wt % or greater, or 78 wt % or greater, based on the weight of the polymer composition. While at the same time 80 wt % or less, or 78 wt % or less, or 76 wt % or less, or 74 wt % or less, or 72 wt % or less, or 70 wt % or less, or 68 wt % or less, or 66 wt % or less, or 64 wt % or less, or 62 wt % or less, or 60 wt % or less, or 58 wt % or less, or 56 wt % or less, or 54 wt % or less, or 52 wt % or less, or 50 wt % or less, or 48 wt % or less, or 46 wt % or less, or 44 wt % or less, or 42 wt % or less concentration contains HFFR filler.

[0071] D of HFFR filler 50 The particle size may be 0.5 μm or more, or 0.6 μm or more, or 0.7 μm or more, or 0.8 μm or more, or 0.9 μm or more, or 1.0 μm or more, or 1.1 μm or more, or 1.2 μm or more, or 1.3 μm or more, or 1.4 μm or more, or 1.5 μm or more, or 1.6 μm or more, or 1.7 μm or more, or 1.8 μm or more, or 1.9 μm or more. , while at the same time 2.0 μm or less, or 1.9 μm or less, or 1.8 μm or less, or 1.7 μm or less, or 1.6 μm or less, or 1.5 μm or less, or 1.4 μm or less, or 1.3 μm or less, or 1.2 μm or less, or 1.1 μm or less, or 1.0 μm or less, or 0.9 μm or less, or 0.8 μm or less, or 0.7 μm or less, or 0.6 μm or less. The particle size of the HFFR filler can be determined using static laser scattering.

[0072] additive

[0073] The polymer composition may include additional additives in the form of antioxidants, crosslinking aids, curing accelerators and scorch retardants, processing aids, coupling agents, UV stabilizers (including UV absorbers), antistatic agents, additional nucleating agents, slip agents, lubricants, viscosity control agents, tackifiers, antiblocking agents, surfactants, extender oils, acid scavengers, flame retardants and metal deactivators. The polymer composition may include 0.01 wt% to 10 wt% of one or more additional additives.

[0074] UV light stabilizers may include hindered amine light stabilizers ("HALS") and UV light absorbers ("UVA") additives. Representative UVA additives include benzotriazole types such as TINUVIN 326 commercially available from Ciba, Inc. TM Light stabilizers and TINUVIN 328 TM Light Stabilizers: Blends of HAL and UVA additives are also effective.

[0075] Antioxidants may include hindered phenols such as tetrakis[methylene(3,5-di-tert-butyl-4-hydroxyhydro-cinnamate)]methane; bis[(β-(3,5-di-tert-butyl-4-hydroxybenzyl)methylcarboxyethyl)]-sulfide, 4,4'-thiobis(2-methyl-6-tert-butylphenol), 4,4'-thiobis(2-tert-butyl-5-methylphenol), 2,2'-thiobis(4-methyl-6-tert-butylphenol) and thiodiethylenebis(3,5-di-tert-butyl-4-hydroxy)-hydrocinnamate; phosphites and phosphonites , such as tris(2,4-di-tert-butylphenyl)phosphite and di-tert-butylphenyl-phosphite; thio compounds, such as dilaurylthiodipropionate, dimyristylthiodipropionate and distearylthiodipropionate; various siloxanes; polymeric 2,2,4-trimethyl-1,2-dihydroquinoline, n,n'-bis(1,4-dimethylpentyl-p-phenylenediamine), alkylated diphenylamine, 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, diphenyl-p-phenylenediamine, mixed diaryl-p-phenylenediamines and other hindered amine antidegradants or stabilizers.

[0076] Processing aids may include metal salts of carboxylic acids, such as zinc stearate or calcium stearate; fatty acids, such as stearic acid, oleic acid or erucic acid; fatty amides, such as stearamide, oleamide, erucamide or N,N'-ethylenebisstearamide; polyethylene waxes; oxidized polyethylene waxes; polymers of ethylene oxide; copolymers of ethylene oxide and propylene oxide; vegetable waxes; petroleum waxes; nonionic surfactants; silicone fluids and polysiloxanes.

[0077] Compounding and Cable Forming

[0078] The components of polymer composition can be added in batches or continuous mixers to form melt blended compositions. Components can be added in any order or one or more masterbatches can be first prepared to blend with other components. Melt blending can be carried out at a temperature higher than the highest molten polymer. The melt blended composition can then be transported to an extruder or injection molding machine, or molded into required goods through a die, or converted into pellets, tapes, strips or films or some other forms to be used for storage or preparation of materials supplied to the next forming or processing step. Optionally, if formed into pellets or some similar configurations, pellets etc. can be coated with a release agent so as to facilitate the processing when stored.

[0079] Examples of compounding equipment include internal batch mixers such as the BANBURY TM or BOLLING TM Internal mixer. Alternatively, a continuous single screw or twin screw mixer such as the FARRELL TM Continuous mixer, WERNER TM and PFLEIDERER TM Twin screw mixer or BUSS TM Kneading Continuous Extruder. The type of mixer utilized and the operating conditions of the mixer will affect the properties of the composition, such as viscosity, volume resistivity and extruded surface smoothness.

[0080] The polymer composition may be disposed on or positioned around a conductor to form a cable. As used herein, a "conductor" is one or more wires, or one or more fibers, used to conduct heat, light and / or electricity. The conductor may be a single wire / ray or multiple wires / rays and may be in strand form or in tubular form. Non-limiting examples of suitable conductors include carbon and various metals such as silver, gold, copper and aluminum. The conductor may also be an optical fiber made of glass or plastic. The polymer composition may be used as a protective sheath to form a cable. The polymer composition is then extruded onto the conductor to form the cable. The polymer composition may be

[0081] Polymer composition properties

[0082] The polymer composition may exhibit 10.0 MPa or more, or 10.5 MPa or more, or 11.0 MPa or more, or 11.5 MPa or more, or 12.0 MPa or more, or 12.5 MPa or more, or 13.0 MPa or more, or 13.5 MPa or more, or 14.0 MPa or more, or 14.5 MPa or more, or 15.0 MPa or more, or 15.5 MPa or more, or 16.0 MPa or more, or 16.5 MPa or more, or 17.0 MPa or more, or 17.5 MPa or more, or 18.0 MPa or more, or 18.5 MPa or more, or 19.0 MPa or more, or 19.5 MPa or more. , while at the same time a tensile strength of 20.0 MPa or less, or 19.5 MPa or less, or 19.0 MPa or less, or 18.5 MPa or less, or 18.0 MPa or less, or 17.5 MPa or less, or 17.0 MPa or less, or 16.5 MPa or less, or 16.0 MPa or less, or 15.5 MPa or less, or 15.0 MPa or less, or 14.5 MPa or less, or 14.0 MPa or less, or 13.5 MPa or less, or 13.0 MPa or less, or 12.5 MPa or less, or 12.0 MPa or less, or 11.5 MPa or less, or 11.0 MPa or less, or 10.5 MPa or less. The tensile strength is determined according to the procedure described in the Test Methods section below.

[0083] The polymer composition may exhibit an elongation at break of 70% or more, or 75% or more, or 80% or more, or 85% or more, or 90% or more, or 95% or more, or 100% or more, or 105% or more, or 110% or more, or 115% or more, or 120% or more, or 125% or more, while 130% or less, or 125% or less, or 120% or less, or 115% or less, or 110% or less, or 105% or less, or 100% or less, or 95% or less, or 90% or less, or 85% or less, or 80% or less, or 75% or less. The elongation at break modulus is determined according to the procedure described in the Test Methods section below.

[0084] The polymer composition may exhibit 200 MPa or more, or 210 MPa or more, or 220 MPa or more, or 230 MPa or more, or 240 MPa or more, or 250 MPa or more, or 260 MPa or more, or 270 MPa or more, or 280 MPa or more, or 290 MPa or more, or 300 MPa or more, or 310 MPa or more, or 320 MPa or more, or 330 MPa or more, or 340 MPa or more. , while having a flexural modulus of 350 MPa or less, or 340 MPa or less, or 330 MPa or less, or 320 MPa or less, or 310 MPa or less, or 300 MPa or less, or 290 MPa or less, or 280 MPa or less, or 270 MPa or less, or 260 MPa or less, or 250 MPa or less, or 240 MPa or less, or 230 MPa or less, or 220 MPa or less, or 210 MPa or less. The flexural modulus is determined according to the procedure described in the Test Methods section below.

[0085] The polymer composition can exhibit 1.0 g / min or more, or 1.1 g / min or more, or 1.2 g / min or more, or 1.3 g / min or more, or 1.4 g / min or more, or 1.5 g / min or more, or 1.6 g / min or more, or 1.7 g / min or more, or 1.8 g / min or more, or 1.9 g / min or more, 2.0 g / min or more, or 2.1 g / min or more, or 2.2 g / min or more, or 2.3 g / min or more, or 2.4 g / min or more, or 2.5 g / min or more, or 2.6 g / min or more, or 2.7 g / min or more, or 2.8 g / min or more, or 2.9 g / min or more, While at the same time an MFI of 3.0 g / min or less, or 2.9 g / min or less, or 2.8 g / min or less, or 2.7 g / min or less, or 2.6 g / min or less, or 2.5 g / min or less, or 2.4 g / min or less, or 2.3 g / min or less, or 2.2 g / min or less, or 2.1 g / min or less, or 2.0 g / 10 min or less, or 1.9 g / min or less, or 1.8 g / min or less, or 1.7 g / min or less, or 1.6 g / min or less, or 1.5 g / min or less, or 1.4 g / min or less, or 1.3 g / min or less, or 1.2 g / min or less, or 1.1 g / min or less. The MFI is determined according to the procedure described in the Test Methods section below.

[0086] The polymer composition exhibits a hot knife indentation value of 50% or less, or 45% or less, or 40% or less, or 35% or less, or 30% or less, or 25% or less, or 20% or less, or 15% or less, or 10% or less, or 15% or less, or 10% or less, or 5% or less. The hot knife indentation value is measured according to DIN EN 60811-3-1 at a thickness of 1.9 mm.

[0087] The polymer composition exhibits an ESCR value of 1000 hours or more, or 1100 hours or more, or 1200 hours or more, or 1300 hours or more, or 1400 hours or more, or 1500 hours or more, or 1600 hours or more, or 1700 hours or more, or 1800 hours or more, or 1900 hours or more, or 2000 hours or more. The ESCR value is measured according to ASTM D1693.

[0088] Example

[0089] Material

[0090] The following materials were used in the following examples.

[0091] LLDPE is a linear low-density polyethylene having a density of 0.92 g / cc and an MFI of 1 g / 10 min (190°C / 21.6 kg), and an example thereof is DOWLEX TM 2045G polyethylene resin is commercially available from The Dow Chemical Company, Midland, Michigan, USA.

[0092] Polypropylene (PP) is a polypropylene homopolymer having a melt flow index of 12 g / 10 min (230° C., 2.16 kg) and a melting temperature of 160° C., an example of which is available as PP H700-12 polypropylene from Braskem, Sao Paulo, Brazil. Paulo, Brazil).

[0093] POE is a polyolefin elastomer of ethylene and butene having a melt flow index of 4.5 g / 10 min (190°C / 21.6 kg), a density of 0.89 g / cc, and a melting temperature of 80°C, an example of which is commercially available from The Dow Chemical Company, Midland, Michigan, USA, under the trade name SEC 39001.

[0094] CBC is a crystalline block copolymer that is a diblock composite of polypropylene and polyethylene. As used herein, a diblock composite of polypropylene and polyethylene is a composite of: (i) CEP, which is a crystalline ethylene / propylene copolymer; (ii) CAOP, which is an isotactic crystalline propylene homopolymer (iPP); and (iii) a block copolymer containing an iPP block (CAOB) and an ethylene / propylene block (CEB) having the properties provided in Table 1:

[0095] Table 1 :

[0096]

[0097] • wt% PP - weight percentage of propylene polymer in the CBC as measured by high temperature liquid chromatography.

[0098] • Mw - weight average molecular weight of CBC in kg / mol, as determined by gel permeation chromatography, as described above.

[0099] • Mw / Mn—molecular weight distribution of the CBC, as determined by gel permeation chromatography, as described above.

[0100] Total wt% C2 - the weight percentage of ethylene in the CBC as determined by C13 NMR spectroscopy, with the remainder being propylene.

[0101] Tm (°C) Peak 1 (Peak 2) - Peak melting temperature as determined by the second heating curve of DSC. Peak 1 refers to the melting of CEB / CEP (for CBC) or EB / EP (for BC), while Peak 2 refers to the melting of CEB or CEP.

[0102] • Tc (°C) - peak crystallization temperature as determined by DSC cooling scan.

[0103] Suitable processes that can be used to produce CBC can be found, for example, in U.S. Patent Application Publication No. 2008 / 0269412. Specifically, it is desirable that the polymerization be conducted as a continuous polymerization, preferably a continuous solution polymerization, in which the catalyst components, monomers, and optional solvents, adjuvants, scavengers, and polymerization aids are continuously supplied to and the polymer product is continuously removed from one or more reactors or zones. Within the scope of the term "continuous" as used in this context are those methods in which the reactants are intermittently added and the product is removed at less regular or irregular time intervals so that over time, the overall process is substantially continuous. One or more chain shuttling agents may be added at any point during the polymerization, including in the first reactor or zone, at the outlet or slightly before the outlet of the first reactor, or between the first reactor or zone and the second or any subsequent reactor or zone. Due to monomer, temperature, pressure differences or other differences in polymerization conditions between at least two reactors or zones connected in series, polymer segments with different compositions, such as comonomer content, crystallinity, density, stereoisomerism, regioregularity or other chemical or physical differences in the same molecule are formed in different reactors or zones. The size of each segment or block is determined by the continuous polymer reaction conditions, and preferably the most probable distribution of polymer sizes. Exemplary catalysts and catalyst precursors for forming crystalline block composites include metal complexes as disclosed in International Publication No WO 2005 / 090426.

[0104] MAH-g-POE is a maleic anhydride grafted polyolefin elastomer having a density of 0.87 g / cc and a melt flow index of 1.25 g / 10 min, an example of which can be found under the trade name AMPLIFY TM GR 216 is commercially available from The Dow Chemical Company, Midland, Michigan, USA.

[0105] HFFR is magnesium hydroxide, an example of which can be found under the trade name MAGNIFIN TM H-5MV is commercially available from Albemarle Corporation Charlotte, NC, USA.

[0106] The stabilizer is a blend of: 4 wt% TiO2, 0.1 wt% IRGASTAB TM FS301FF stabilizer and 0.75 wt% CHIMASSORB TM 2020 Light Stabilizing Additives, the rest are ERSIFY TM 2300 Propylene-ethylene copolymer. IRGASTAB TM and CHIMASSORBTM is commercially available from BASF, Ludwigshafen, Germany, and VERSIFY TM Dow® 2300 is commercially available from The Dow Chemical Company, Midland, Michigan, USA.

[0107] PA is a processing aid, which can be included as MB50-313 TM The masterbatch was an ultra high molecular weight siloxane polymer commercially available from Dow Corning, Midland Michigan, USA.

[0108] Sample preparation

[0109] Inventive Examples ("IE") and Comparative Examples ("CE") were prepared according to the following steps. Each of the materials for IE and CE was loaded into a BUSS Model MDK / E 46. TM The materials were mixed in a kneader to homogenize the CE and IE samples. The samples of IE and CE were compression molded to form 2 mm test plaques for testing.

[0110] Test Method

[0111] The following test methods were used to determine the properties of the following compression molded plaques of the IE and CE samples.

[0112] Tensile strength and elongation at break

[0113] According to IEC 60811-512, INSTRON TM The tensile strength and elongation at break of the samples were tested in a 4202 tester at a speed of 25 mm / min, a preload of 3 Newtons (N), a yield sensitivity of 1%, a clamping distance of 50 mm and a 10,000 N load cell.

[0114] Flexural modulus

[0115] The compression molded samples were placed on the INSTRON TM 3-point flexure was performed in the flexure fixture of a 4202 tester using a 5.08 cm span and a crosshead speed of 0.127 cm / min. Flexural modulus was determined according to ISO 178 at the maximum flexural stress sustained during the test.

[0116] MFI

[0117] The melt flow index of the samples was measured according to ASTM D1238 at 190°C and 21.6 kg.

[0118] Hot Knife Indentation

[0119] The hot knife indentation values ​​were measured according to DIN EN 60811-3-1 on samples with a thickness of 1.9 mm.

[0120] ESCR

[0121] The ESCR values ​​of the samples were measured according to ASTM D1693.

[0122] result

[0123] Table 2 provides composition data for CE1-CE4 in weight percent.

[0124] Table 2 :

[0125]

[0126] Table 3 provides the composition and mechanical property data of IE1-IE4.

[0127] Table 3:

[0128]

[0129]

[0130] CE1-CE4 are similar in composition in that CE1-CE4 contain 1 wt% or less of crystalline block composites. It is apparent from the mechanical property data provided in Table 3 that CE1-CE4 exhibit acceptable cable jacket properties in some properties, but do not provide the balance of acceptable performance provided by IE1-IE4 in each mechanical property category. For example, although CE1, CE3, and CE4 meet the cable jacket properties of 10 MPa tensile strength and less than 50% hot knife indentation, they cannot meet 70% elongation at break or 1000 hours ESCR value. Similarly, although CE2 almost meets 10 MPa tensile strength and has less than 50% hot knife indentation, CE2 cannot meet 70% elongation at break or 1000 hours ESCR value.

[0131] IE1-IE4 are similar in composition in that IE1-IE4 include greater than 1 wt% crystalline block composites. Specifically, IE1-IE4 each include 4 wt% or greater crystalline block composites, particularly propylene and polyethylene copolymers. It is apparent from the mechanical property data provided in Table 3 that IE1-IE4 exhibit acceptable cable jacket properties in all mechanical property categories. It can be seen that each of IE1-IE4 meets or exceeds the cable jacket properties of 10 MPa tensile strength, 70% elongation at break, hot knife indentation less than 50%, and 1000 hour ESCR values.

Claims

1. A polymer composition, comprising, by weight percentage of the polymer composition: (a) 10 to 30 weight percent of a polyolefin elastomer, wherein the polyolefin elastomer is a random copolymer of ethylene and an α-olefin, wherein the α-olefin has 3 to 12 carbon atoms; (b) 1 wt% to 9 wt% of a propylene-based polymer, wherein the propylene-based polymer is a propylene homopolymer; (c) 2 to 20 wt% of a crystalline block composite, wherein the crystalline block composite is a diblock composite of polypropylene and polyethylene; (d) 1 to 10 wt % of a maleated polyolefin elastomer; and (e) 40 to 80 wt % of a halogen-free flame retardant filler.

2. The polymer composition according to claim 1, wherein the polymer composition comprises 50 wt% to 70 wt% of the halogen-free flame retardant filler, and the halogen-free flame retardant filler is magnesium hydroxide.

3. The polymer composition of claim 1, wherein the maleated polyolefin elastomer is a maleic anhydride grafted polyolefin elastomer, further wherein the polymer composition comprises 3 to 7 weight percent of the maleic anhydride grafted polyolefin elastomer.

4. The polymer composition according to claim 1, wherein the polymer composition comprises 15 wt % to 25 wt % of the polyolefin elastomer, and further wherein the density of the polyolefin elastomer is in the range of 0.87 g / cm 3 Up to 0.91g / cm 3 .

5. The polymer composition of claim 1, wherein the polymer composition comprises 4 to 8 wt% of the propylene-based polymer.

6. The polymer composition of claim 5, wherein the polymer composition comprises 4 to 12 wt% of the crystalline block composite.

7. The polymer composition according to any one of claims 1 to 6, wherein the polyolefin elastomer is a polyolefin elastomer of ethylene and butene.

8. The polymer composition according to any one of claims 1 to 6, wherein the density of the polypropylene and polyethylene diblock composite is in the range of 0.89 g / cm 3 Up to 0.92g / cm 3 .

9. The polymer composition of any one of claims 1 to 6, wherein the polypropylene and polyethylene diblock composite has a melt flow index at 230°C and 2.16 kg of 8 to 12 g / 10 min.

10. A cable, comprising: conductor; as well as A polymer composition according to any one of claims 1 to 9 positioned around the conductor.

Citation Information

Patent Citations

  • Plenum Cable Flame Retardant Layer / Component with Excellent Aging Properties

    US20080251273A1

  • Catalytic Olefin Block Copolymers with Controlled Block Sequence Distribution

    US20080269412A1

  • Halogen-free flame retardant formulations

    US20100319960A1

  • Crystalline block composites as compatibilizers

    US20110313106A1

  • Crystalline block composites as compatibilizers

    US20110313108A1